Composition for polishing and method for producing the same, polishing method
The polishing composition with abrasive grains, hydrophobic medium, and specific surfactant addresses the issue of residual haze by minimizing residue adherence, ensuring a glossy finish on resin coatings.
Patent Information
- Application Number
- JP2023056494
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Conventional polishing compositions leave a white haze or cloudy residue on the surface of resin coatings that is difficult to remove, requiring rework even after prolonged periods before wiping.
A polishing composition comprising abrasive grains, a hydrophobic dispersion medium, water, and a specific surfactant with a polyoxyethylene alkyl ether structure, designed to minimize residue adherence.
The composition effectively prevents cloudy residues on the polished surface, ensuring a glossy finish without the need for rework, even after a long delay before wiping.
Smart Images

Figure 2024143701000002 
Figure 2024143701000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a polishing composition, a method for producing the same, and a polishing method. [Background technology]
[0002] Buff polishing is known as a processing method for smoothing and glossing the surface of a resin coating film coated on the surface of an automobile body, etc. Buff polishing is a processing method in which, for example, a cloth buff is pressed against an object to be polished (e.g., a resin coating film) while a polishing composition is interposed between the buff and the object to be polished, thereby polishing the surface.
[0003] The polishing composition used in the buff polishing process contains abrasive grains (abrasive material) and a surfactant, and the abrasive grains used are, for example, aluminum oxide (alumina) particles (see, for example, Patent Documents 1 to 3). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2008-255232 A [Patent Document 2] JP 2008-127456 A [Patent Document 3] JP 2007-277379 A Summary of the Invention [Problem to be solved by the invention]
[0005] After the buffing process is completed, it is necessary to wash the surface of the resin coating film and wipe off the polishing composition. In the buffing process using the conventional polishing composition, if a long time is left before wiping, a white haze tends to remain on the finished surface after washing. This white haze is difficult to remove even by repeated washing, so a rework such as buffing is required.
[0006] The present invention has been made in consideration of the above circumstances, and aims to provide a polishing composition that is less likely to leave a haze on the surface of an object to be polished even if a long period of time is allowed to pass before wiping, as well as a method for producing the same and a polishing method. [Means for solving the problem]
[0007] In order to solve the above problems, a polishing composition according to one aspect of the present invention includes an abrasive grain, a hydrophobic dispersion medium, water, and a surfactant. The surfactant is represented by the formula (i) RO-(C2H4O) n In the formula (i), R is a branched alkyl group having 12 to 20 carbon atoms, and n is the average number of moles of oxyethylene added and is 3 to 50. Effect of the Invention
[0008] According to one aspect of the present invention, it is possible to provide a polishing composition that is less likely to leave a haze on the surface of an object to be polished even if a long period of time is allowed to pass before wiping, and a method for producing the same and a polishing method. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a diagram showing an example of a polishing apparatus used in an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] An embodiment of the present invention will be described in detail. Note that the following embodiment shows an example of the present invention, and the present invention is not limited to the embodiment. In addition, various modifications or improvements can be made to the following embodiment, and such modifications or improvements can also be included in the present invention.
[0011] <Polishing composition> The polishing composition according to an embodiment of the present invention (hereinafter, the present embodiment) contains abrasive grains, a hydrophobic dispersion medium (organic solvent), water, and a surfactant. The surfactant is represented by the formula (i) RO-(C2H4O)n In the formula (i), R is a branched alkyl group having 12 to 20 carbon atoms, and n is the average number of moles of oxyethylene (C2H4O) added, which is 3 to 50.
[0012] The polishing composition having such a constitution can suppress the components of the polishing composition from adhering to the surface of the polishing composition even if a time is left before wiping off, and the surface of the object to be polished is less likely to become cloudy. It can suppress the remaining of the adhering matter that causes cloudiness on the surface of the object to be polished after polishing. It can suppress the inability to obtain sufficient gloss on the surface after polishing due to the adhering matter.
[0013] Hereinafter, each component contained in the polishing composition according to this embodiment will be described with examples. (1) Abrasive grain The polishing composition according to this embodiment contains abrasive grains. The abrasive grains have the effect of mechanically polishing the object to be polished. Specific examples of the abrasive grains used in this embodiment include metal oxides such as aluminum oxide (alumina), silicon oxide (silica), cerium oxide (ceria), zirconium oxide, titanium oxide (titania), tin oxide, and manganese oxide, metal carbides such as silicon carbide and titanium carbide, metal nitrides such as silicon nitride and titanium nitride, metal borides such as titanium boride and tungsten boride, silicate compounds such as zircon (ZrSiO4), and diamond. The abrasive grains may be used alone or in combination of two or more kinds. In addition, the abrasive grains may be commercially available or synthetic products.
[0014] Among these abrasive grains, from the viewpoint that grains having various particle sizes are easily available and an excellent polishing rate can be obtained, at least one selected from the group consisting of metal oxides and metal carbides is preferred, silicon carbide, silicon dioxide, or metal oxide is more preferred, at least one of aluminum oxide (alumina), cerium oxide, and zirconium oxide is further preferred, and aluminum oxide is particularly preferred. Also, a mixture of alumina and zircon can be preferably used. In this specification, the term "polishing rate" may be rephrased as the polishing removal rate.
[0015] Furthermore, among aluminum oxides, those containing α-phase or a transition state crystal phase, such as θ-phase, δ-phase, or γ-phase, which is a process of becoming α-phase, are suitable as abrasive grains. It is preferable to contain α-phase or θ-phase, and more preferably to contain α-phase. It is also considered that there is an optimal range for the α-phase depending on the degree of becoming α-phase.
[0016] In general, the crystal structure of the α phase is considered to be the hardest, but it is estimated that if the α phase is sintered sufficiently at high temperature to convert it to the α phase, the particle shape will change to a round shape and the polishing performance will decrease. The α phase ratio can be used as a reference value to indicate the degree of α phase contained in aluminum oxide. The preferred lower limit of the α phase ratio is 50% or more. The lower limit of the α phase ratio is more preferably 60% or more, more preferably 70% or more, particularly preferably 80% or more, and even more preferably 90% or more. Furthermore, the preferred upper limit of the α phase ratio is 100% or less. The upper limit of the α phase ratio is more preferably 98% or less. In other words, the α phase ratio of aluminum oxide is preferably 50% or more and 100% or less, and more preferably 60% or more and 98% or less.
[0017] By setting the alpha conversion rate within the above preferred range, it is expected that the polishing power, i.e., the scratch removal speed will be increased and the polishing rate will be improved. The alpha conversion rate of the aluminum oxide particles can be calculated from the integrated intensity ratio of the (113) plane diffraction line by X-ray diffraction measurement using an X-ray diffraction device (Ultima-IV, manufactured by Rigaku Corporation).
[0018] The lower limit of the volume average particle size (average secondary particle size) of the abrasive grains is preferably 0.05 μm or more, more preferably 0.1 μm or more, and even more preferably 0.2 μm or more. By having the volume average particle size (average secondary particle size) of the abrasive grains be 0.05 μm or more, the processing power can be improved and the object to be polished can be polished well in both rough polishing and finish polishing.
[0019] The upper limit of the volume average particle size (average secondary particle size) of the abrasive grains is preferably 15 μm or less, more preferably 10 μm or less, even more preferably 5 μm or less, particularly preferably 4 μm or less, and most preferably 3 μm or less. As the volume average particle size (average secondary particle size) of the abrasive grains becomes smaller, it becomes easier to obtain a surface with fewer defects and less roughness.
[0020] Therefore, by setting the volume average particle size (average secondary particle size) of the abrasive grains to 0.05 μm or more and 15 μm or less, it is possible to obtain a surface with fewer defects and less roughness while improving the processing power.
[0021] Abrasive grains that have a large particle size before polishing but become smaller at the interface between the buff and the object to be polished during polishing (abrasive grains in which secondary particles break down to primary particles during polishing) may be used. From the above, the volume average particle size (average secondary particle size) of the abrasive grains is preferably 0.05 μm or more and 15 μm or less, more preferably 0.1 μm or more and 10 μm or less, even more preferably 0.2 μm or more and 5 μm or less, particularly preferably 0.2 μm or more and 4 μm or less, and most preferably 0.2 μm or more and 3 μm or less. In one embodiment, the volume average particle size (average secondary particle size) of the abrasive grains is 0.05 μm or more and 10 μm or less, 0.2 μm or more and 4 μm or less, or 0.2 μm or more and 3 μm or less.
[0022] In this specification, the volume average particle size of the abrasive grains is defined as the cumulative 50% particle size (D50) based on the volume-based particle size distribution. That is, D50 is the particle size when the cumulative volume from the large particle size side (or the small particle size side) of the cumulative particle size distribution on a volume basis is 50%. The D50 of the abrasive grains can be measured using a commercially available particle size measuring device. Such a particle size measuring device may be based on any of the techniques such as dynamic light scattering, laser diffraction, laser scattering, or pore electrical resistance. As an example of the method and device for measuring D50, the measuring method and device described in the examples can be mentioned.
[0023] The lower limit of the content of the abrasive grains in the polishing composition is preferably 0.1 mass% or more, more preferably 1 mass% or more, even more preferably 5 mass% or more, particularly preferably 7 mass% or more, and most preferably 10 mass% or more, based on the total mass of the polishing composition. By having the content of the abrasive grains be 0.1 mass% or more, the processing force can be appropriately controlled, and the object to be polished can be polished well in both rough polishing and finish polishing.
[0024] The upper limit of the content of the abrasive grains in the polishing composition is preferably 50 mass% or less, more preferably 35 mass% or less, even more preferably 30 mass% or less, particularly preferably 20 mass% or less, and most preferably 15 mass% or less, based on the total mass of the polishing composition. By making the content of the abrasive grains 50 mass% or less, the manufacturing cost of the polishing composition can be reduced, and a surface with fewer defects and less roughness can be obtained.
[0025] In a preferred embodiment, the abrasive grains are contained in an amount of 5 mass % or more and 30 mass % or less based on the total mass of the polishing composition.
[0026] (2) Other examples of abrasive grains In the polishing composition according to the present embodiment, the abrasive grains are not limited to the examples described in (1) above. In the polishing composition according to the present embodiment, the abrasive grains may be other examples 1 or 2 shown below. (2.1) Another Example 1 The abrasive grains of this embodiment have a specific surface area (m 2 Abrasive grains having a shape parameter value, calculated by dividing the particle diameter D50 (μm) by the square of the particle diameter D50 (μm), of 0.6 or more and 60 or less, preferably 0.8 or more and 50 or less, and more preferably 1.0 or more and 40 or less may be used. In addition, abrasive grains having the above shape parameters may be used that have an average secondary particle diameter of 0.05 μm or more and 10 μm or less. This makes it possible to obtain a surface with fewer defects and less roughness while improving the processing power. In addition, in abrasive grains having the above shape parameters, the specific surface area (m 2 / g) is preferably 2.1 or more and 21 or less, more preferably 8 or more and 20 or less, and further preferably 12 or more and 15 or less. This makes it possible to provide a good finished surface after polishing of the object to be polished. Again, in this example, the abrasive grains may comprise, for example, aluminum oxide, and preferably comprise sintered alumina, which has a rougher surface than fused alumina.
[0027] By polishing the surface of an object to be polished with a polishing composition containing such abrasive grains, it is possible to improve both the polishing rate (μm / min) of the object to be polished and the scratch removal performance for the object to be polished (e.g., the performance of reducing the number of scratches and the performance of reducing the depth of scratches).
[0028] (2.2) Other Example 2 The abrasive grains of this embodiment have a particle size distribution width (D10-D90) / D50 of 0.4 or more and 2.0 or less, and a specific surface area (m 2 / g) of 12 or more and 20 or less may be used. Here, D10, D50, and D90 are particle sizes at which the cumulative volume from the large particle diameter side of the cumulative particle size distribution on a volume basis is 10%, 50%, and 90%, respectively. D10, D50, and D90 can be measured using a commercially available particle size measuring device.
[0029] In this example, the particle size distribution width (D10-D90) / D50 of the abrasive grains is preferably 0.4 to 1.8, more preferably 0.4 to 1.6. The specific surface area (m 2 / g) is preferably 12 to 18, more preferably 12 to 15. If the particle size distribution width of the abrasive grains is smaller than the lower limit of the particle size distribution width, the polishing rate is unlikely to be high, and if it is larger than the upper limit, scratches are likely to occur on the polished object after polishing. 2 When the specific surface area (g) is smaller than the lower limit, scratches are likely to occur on the object to be polished after polishing, and when it is larger than the upper limit, the polishing rate is difficult to increase. By setting both within the above ranges, the object to be polished can be polished at a high polishing rate, and the finished surface after polishing can be made good. In other words, the performance of the polishing composition can be improved. In addition to the above constitution, abrasive grains having an average secondary particle size of 0.05 μm or more and 10 μm or less may be used. In addition to the above, the specific surface area (m 2 Alternatively, abrasive grains having a shape parameter value of 0.6 or more and 60 or less, calculated by dividing the particle diameter D50 (μm) by the square of the particle diameter D50 (μm), may be used. In this example, the abrasive grains may also contain, for example, aluminum oxide. As the alumina oxide, it is preferable to use sintered alumina, which has a more uneven surface than fused alumina.
[0030] By polishing the surface of an object to be polished with a polishing composition containing such abrasive grains, it is possible to improve both the polishing rate (μm / min) of the object to be polished and the scratch removal performance for the object to be polished (e.g., the performance of reducing the number of scratches and the performance of reducing the depth of scratches).
[0031] (3) Hydrophobic dispersion medium The polishing composition according to the present embodiment includes a hydrophobic dispersion medium. The hydrophobic dispersion medium includes at least one selected from the group consisting of normal paraffinic hydrocarbons, isoparaffinic hydrocarbons, naphthenic hydrocarbons, and terpene hydrocarbons. The hydrophobic dispersion medium preferably has a vapor pressure of 0.004 kPa or more and 2 kPa or less at 20°C. The hydrophobic dispersion medium preferably has a flash point of 30°C or more and 100°C or less. By using such a hydrophobic dispersion medium, the processing efficiency (polishing removal rate) when buffing the resin coating film is improved. Hereinafter, the normal paraffinic hydrocarbons, isoparaffinic hydrocarbons, naphthenic hydrocarbons, and terpene hydrocarbons that may be included in the hydrophobic dispersion medium may be referred to as "organic solvent".
[0032] In the present embodiment, the hydrophobic dispersion medium and the organic solvent are preferably those which are not easily soluble in water. The hydrophobic dispersion medium and the organic solvent may be commercially available products or synthetic products.
[0033] The normal paraffinic hydrocarbons, isoparaffinic hydrocarbons, naphthenic hydrocarbons, and terpene hydrocarbons are preferably derived from mineral oil, and may be those obtained by extracting and refining components derived from mineral oil, or may be those synthesized using components derived from mineral oil as a raw material (synthetic hydrocarbons derived from mineral oil). The normal paraffinic hydrocarbons, isoparaffinic hydrocarbons, naphthenic hydrocarbons, and terpene hydrocarbons are more preferably synthetic hydrocarbons derived from mineral oil. These hydrophobic organic solvents are generally known to be less toxic than other halogen-based or benzene-based organic solvents, and more volatile than other polyethylene glycols, etc.
[0034] Examples of normal paraffin-based hydrocarbons include linear hydrocarbons having from 5 to 30 carbon atoms, liquid paraffin, kerosene, and diesel.
[0035] Examples of isoparaffinic hydrocarbons include branched hydrocarbons having about 5 to 40 carbon atoms, liquid isoparaffin, and the like.
[0036] Examples of naphthenic hydrocarbons include cyclic hydrocarbons having about 5 to 40 carbon atoms, such as monocyclic cycloparaffins, such as cyclohexane, cyclopentane, and cyclononane; polycyclic cycloparaffins, such as decalin; and alkylcycloparaffins, such as methylcyclopentane, methylcyclohexane, 1-methyl-4-isopropylcyclohexane, butylcyclohexane, and methyldecalin.
[0037] Examples of terpene hydrocarbons include chain terpene hydrocarbons such as myrcene, farnesene, and citral; and cyclic terpene hydrocarbons such as menthol, cineole, pinene, limonene, α-terpinene, γ-terpinene, camphene, phellandrene, terpinene, terpinolene, p-cymene, and cedrene.
[0038] The hydrophobic dispersion medium may further contain other organic solvents other than the above-mentioned hydrocarbons. Hereinafter, organic solvents other than normal paraffin-based hydrocarbons, isoparaffin-based hydrocarbons, naphthenic hydrocarbons, and terpene-based hydrocarbons are referred to as "other organic solvents". Examples of such other organic solvents include, for example, methyl alcohol, ethyl alcohol, isopropyl alcohol, acetone, diethyl ether, ethyl acetate, butyl acetate, triethyl citrate, acetyl tributyl citrate, and acetyl triethyl citrate.
[0039] Hydrophobic dispersion media (organic solvents) generally have a flash point. The flash point is the minimum temperature at which a liquid generates a sufficient concentration of vapor to instantly ignite when a flame is brought close to it after being heated at a constant temperature rise. The flash point can also be said to be the minimum temperature at which the hydrophobic dispersion medium evaporates and forms a flammable mixture with air. There are various methods for measuring flash points, depending on the purpose of the measurement and the properties of the sample. There are two methods for measuring flash points: the closed method and the open method. Examples of the closed method include the Tag closed method (JIS K 2265-1:2007), the Seta closed method (JIS K 2265-2:2007), and the Pensky-Martens closed method (JIS K 2265-3:2007). Examples of the open method include the Cleveland open method (JIS K 2265-4:2007).
[0040] (4)Water The polishing composition according to the present embodiment contains water. As the water, from the viewpoint of suppressing the inhibition of the action of other components, it is preferable that the water contains as few impurities as possible, and specifically, it is preferable that the water is pure water or ultrapure water which is obtained by removing impurity ions with an ion exchange resin and then removing foreign matter through a filter, or distilled water.
[0041] The lower limit of the water content in the polishing composition is preferably 1% by mass or more, more preferably 5% by mass or more, even more preferably 10% by mass or more, particularly preferably 15% by mass or more, and most preferably 20% by mass or more, based on the total mass of the polishing composition.The upper limit of the water content in the polishing composition is preferably 90% by mass or less, more preferably 85% by mass or less, even more preferably 80% by mass or less, particularly preferably 75% by mass or less, and most preferably 70% by mass or less, based on the total mass of the polishing composition.
[0042] That is, the water content in the polishing composition is preferably 1% by mass or more and 90% by mass or less, more preferably 5% by mass or more and 85% by mass or less, even more preferably 10% by mass or more and 80% by mass or less, particularly preferably 15% by mass or more and 75% by mass or less, and most preferably 20% by mass or more and 70% by mass or less. By having the water content in the above range, the processing power is improved, and the object to be polished can be polished well in both rough polishing and finish polishing.
[0043] (5) Surfactants The polishing composition according to this embodiment contains a surfactant. The surfactant disperses or emulsifies a hydrophobic dispersion medium or water. In addition, the surfactant imparts hydrophilicity to the polished surface after polishing, thereby improving the cleaning efficiency of the polished surface after polishing, and can also prevent adhesion of dirt to the polished surface. Furthermore, the surfactant according to this embodiment contributes to stability after emulsification.
[0044] As described above, the surfactant of the present embodiment is represented by the formula (i) RO-(C2H4O) n In the formula (i), R is a branched alkyl group having 12 to 20 carbon atoms, and n represents the average number of moles of oxyethylene added, which is 3 to 50. The average number of moles added, n, is more preferably 5 to 20, and even more preferably 5 to 15.
[0045] The surfactant of the present embodiment contains, as the polyoxyethylene alkyl ether represented by formula (i), at least one selected from the group consisting of polyoxyethylene alkyl ether (C12-14 secondary alcohol), polyoxyethylene octyldodecyl ether, and polyoxyethylene 2-hexyldecyl ether. C12-14 means that in the polyoxyethylene alkyl ether represented by formula (i), the number of carbon atoms in R is 12, 13, or 14, or a mixture of two or more of these (hereinafter the same).
[0046] The polyoxyethylene alkyl ether represented by formula (i) may be called polyoxyethylene secondary alcohol ether, secondary alcohol ethoxylate (secondary alcohol ethoxylate), polyoxyethylene alkyl ether (secondary alcohol), or polyoxyethylene secondary alkyl ether. In any case, it has the same structure as the polyoxyethylene alkyl ether represented by formula (i).
[0047] The content of surfactant in the polishing composition is preferably 0.01 mass% or more, more preferably 0.1 mass% or more, based on the total mass of the polishing composition.The content of surfactant in the polishing composition is preferably 3.0 mass% or less, more preferably 2.0 mass% or less, based on the total mass of the polishing composition.When the content of the surfactant is within the above range, the stability of the emulsion in the polishing composition is increased. For example, the HLB value, which indicates the affinity of a surfactant for water and oil, is 10 or more and 16 or less, and preferably 10 or more and 14 or less.
[0048] (6) Various additives The polishing composition according to the present embodiment may contain various additives such as a pH adjuster, a polishing accelerator, an oxidizing agent, a dispersant, a viscosity adjuster, a complexing agent, an anticorrosive agent, and an antifungal agent in order to improve its performance. Examples of additives that can be blended in the polishing composition according to the present embodiment will be described below.
[0049] (6.1) pH adjuster The polishing composition according to the present embodiment may contain a pH adjuster. The pH value of the polishing composition can be adjusted by adding a pH adjuster. The pH adjuster that is used as necessary to adjust the pH value of the polishing composition to a desired value may be either an acid or an alkali, and may be either an inorganic compound or an organic compound.
[0050] Specific examples of acids as pH adjusters include inorganic acids, carboxylic acids, and organic acids such as organic sulfuric acid. Specific examples of inorganic acids include sulfuric acid, nitric acid, boric acid, carbonic acid, hypophosphorous acid, phosphorous acid, and phosphoric acid. Specific examples of carboxylic acids include formic acid, acetic acid, propionic acid, butyric acid, valeric acid, 2-methylbutyric acid, n-hexanoic acid, 3,3-dimethylbutyric acid, 2-ethylbutyric acid, 4-methylpentanoic acid, n-heptanoic acid, 2-methylhexanoic acid, n-octanoic acid, 2-ethylhexanoic acid, benzoic acid, glycolic acid, salicylic acid, glyceric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, malic acid, tartaric acid, citric acid, and lactic acid. Specific examples of organic sulfuric acid include methanesulfonic acid, ethanesulfonic acid, and isethionic acid. These acids may be used alone or in combination of two or more.
[0051] Specific examples of bases as pH adjusters include alkali metal hydroxides or salts thereof, alkaline earth metal hydroxides or salts thereof, quaternary ammonium hydroxides or salts thereof, ammonia, amines, and the like.
[0052] Specific examples of alkali metals include potassium and sodium. Specific examples of alkaline earth metals include calcium and strontium. Specific examples of salts include carbonates, hydrogen carbonates, sulfates, acetates, etc. Specific examples of quaternary ammonium include tetramethylammonium, tetraethylammonium, tetrabutylammonium, etc.
[0053] The quaternary ammonium hydroxide compound includes quaternary ammonium hydroxide or a salt thereof, and specific examples thereof include tetramethylammonium hydroxide, tetraethylammonium hydroxide, and tetrabutylammonium hydroxide.
[0054] Further, specific examples of amines include methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, ethylenediamine, monoethanolamine, N-(β-aminoethyl)ethanolamine, hexamethylenediamine, diethylenetriamine, triethylenetetramine, anhydrous piperazine, piperazine hexahydrate, 1-(2-aminoethyl)piperazine, N-methylpiperazine, and guanidine. These bases may be used alone or in combination of two or more.
[0055] Among these bases, ammonia, ammonium salts, alkali metal hydroxides, alkali metal salts, quaternary ammonium hydroxide compounds, and amines are preferred, and ammonia, potassium compounds, sodium hydroxide, quaternary ammonium hydroxide compounds, ammonium hydrogen carbonate, ammonium carbonate, sodium hydrogen carbonate, and sodium carbonate are more preferred.
[0056] From the viewpoint of preventing metal contamination, the polishing composition further preferably contains a potassium compound as a base. Examples of the potassium compound include potassium hydroxide or potassium salt, specifically potassium hydroxide, potassium carbonate, potassium hydrogencarbonate, potassium sulfate, potassium acetate, potassium chloride, etc.
[0057] Alternatively, instead of or in combination with the above acids, salts of the above acids, such as ammonium salts or alkali metal salts, may be used as pH adjusters that act as buffers. In particular, when the above acids and buffers are combined with a weak acid and a strong base, a strong acid and a weak base, or a weak acid and a weak base, a pH buffering effect can be expected.
[0058] (6.2) Polishing accelerator (oxidizer) The polishing composition according to the present embodiment may contain a polishing accelerator. The polishing accelerator plays a role in chemically polishing the object to be polished, and acts on the outer surface of the resin coating film to significantly improve the processing efficiency.
[0059] Specific examples of the polishing accelerator include at least one salt selected from the group consisting of metal salts of inorganic acids, metal salts of organic acids, ammonium salts of inorganic acids, and ammonium salts of organic acids.
[0060] The inorganic acid may be any of nitric acid, sulfuric acid, and hydrochloric acid. The organic acid may be any of oxalic acid, lactic acid, acetic acid, formic acid, citric acid, tartaric acid, malic acid, gluconic acid, glycolic acid, and malonic acid. The metal salt may be any of aluminum salt, nickel salt, lithium salt, magnesium salt, sodium salt, and potassium salt.
[0061] These abrasion accelerators may be used alone or in combination of two or more.
[0062] An oxidizing agent may be added as a polishing accelerator. Specific examples of the oxidizing agent include hydrogen peroxide, peroxide, nitrate, iodate, periodate, hypochlorite, chlorite, chlorate, perchlorate, persulfate, dichromate, permanganate, ozone water, silver(II) salt, and iron(III) salt.
[0063] (6.3) Dispersants / Viscosity modifiers (thickeners) The polishing composition according to this embodiment may contain a dispersant or a thickener. The dispersant or the thickener disperses the abrasive grains (abrasive) uniformly in the liquid, so that the abrasive grains can act efficiently on the object to be polished. In addition, the presence of the dispersant or the thickener between the abrasive grains is expected to suppress caking of the abrasive grains. This suppresses the occurrence of scratches caused by agglomerated abrasive grains.
[0064] Specific examples of the dispersant include colloidal substances containing fine particles, such as colloidal alumina, colloidal silica, colloidal zirconia, colloidal titania, alumina sol, silica sol, zirconia sol, titania sol, fumed alumina, fumed silica, fumed zirconia, fumed titania, etc. Sodium phosphate, sodium hexametaphosphate, sodium pyrophosphate, etc., which are generally used as dispersants, may also be used.
[0065] Specific examples of the thickener include glycols such as propylene glycol polymers and ethylene glycol polymers, and polymeric compounds. More specifically, examples of the glycols include propylene glycol, ethylene glycol, dipropylene glycol, polypropylene glycol, diethylene glycol, and polyethylene glycol. Examples of the polymeric compounds include sodium polyacrylate, polyvinyl alcohol, and hydroxyethyl cellulose.
[0066] (6.4) Complexing agents The polishing composition according to the present embodiment may contain a chelating agent (complexing agent). The complexing agent traps metal ions and the like derived from the polishing device, the object to be polished, etc., and is expected to suppress metal contamination of the polished surface by metal ions and to obtain a good polished surface.
[0067] Examples of the complexing agent include organic acids, amino acids, nitrile compounds, and other chelating agents. Specific examples of the organic acid include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, malic acid, tartaric acid, and citric acid. Instead of or in combination with the organic acid, a salt such as an alkali metal salt of the organic acid may be used.
[0068] Specific examples of amino acids include glycine, α-alanine, β-alanine, N-methylglycine, N,N-dimethylglycine, 2-aminobutyric acid, norvaline, valine, leucine, norleucine, isoleucine, phenylalanine, proline, sarcosine, ornithine, lysine, taurine, serine, threonine, homoserine, tyrosine, bicine, tricine, 3,5-diiodo-tyrosine, β-(3,4-dihydroxyphenyl)-alanine, thyroxine, These include 4-hydroxy-proline, cysteine, methionine, ethionine, lanthionine, cystathionine, cystine, cysteic acid, aspartic acid, glutamic acid, S-(carboxymethyl)-cysteine, 4-aminobutyric acid, asparagine, glutamine, azaserine, arginine, canavanine, citrulline, delta-hydroxy-lysine, creatine, histidine, 1-methyl-histidine, 3-methyl-histidine, and tryptophan.
[0069] Specific examples of the nitrile compound include acetonitrile, aminoacetonitrile, propionitrile, butyronitrile, isobutyronitrile, benzonitrile, glutarodinitrile, and methoxyacetonitrile.
[0070] Specific examples of chelating agents other than these include iminodiacetic acid, nitrilotriacetic acid, diethylenetriaminepentaacetic acid, ethylenediaminetetraacetic acid, N,N,N-trimethylenephosphonic acid, ethylenediamine-N,N,N',N'-tetramethylenesulfonic acid, transcyclohexanediaminetetraacetic acid, 1,2-diaminopropanetetraacetic acid, glycol ether diaminetetraacetic acid, ethylenediamine orthohydroxyphenylacetic acid, ethylenediamine disuccinic acid (SS form), N-(2-carboxylate ethyl)-L-aspartic acid, β-alanine diacetic acid, 2-phosphonobutane-1,2,4-tricarboxylic acid, 1-hydroxyethylidene-1,1-diphosphonic acid, N,N'-bis(2-hydroxybenzyl)ethylenediamine-N,N'-diacetic acid, and 1,2-dihydroxybenzene-4,6-disulfonic acid. do. These complexing agents may be used alone or in combination of two or more.
[0071] (6.5) Corrosion inhibitors The polishing composition according to this embodiment may contain an anticorrosive agent. The anticorrosive agent forms a protective film on the metal surface, and is therefore expected to prevent corrosion of the polishing device, the object to be polished, the fixture, and the like.
[0072] The usable anticorrosive agent is not particularly limited, and may be, for example, a heterocyclic compound or a surfactant. The number of members of the heterocyclic ring in the heterocyclic compound is not particularly limited. The heterocyclic compound may be a monocyclic compound or a polycyclic compound having a condensed ring. The anticorrosive agent may be used alone or in a mixture of two or more kinds.
[0073] Specific examples of heterocyclic compounds that can be used as anticorrosive agents include nitrogen-containing heterocyclic compounds such as pyrrole compounds, pyrazole compounds, imidazole compounds, triazole compounds, tetrazole compounds, pyridine compounds, pyrazine compounds, pyridazine compounds, pyrindine compounds, indolizine compounds, indole compounds, isoindole compounds, indazole compounds, purine compounds, quinolizine compounds, quinoline compounds, isoquinoline compounds, naphthyridine compounds, phthalazine compounds, quinoxaline compounds, quinazoline compounds, cinnoline compounds, buteridine compounds, thiazole compounds, isothiazole compounds, oxazole compounds, isoxazole compounds, and furazan compounds.
[0074] (6.6) Mold inhibitors and preservatives The polishing composition according to this embodiment may contain a mildewproofing agent and a preservative. Specific examples of mildewproofing agents and preservatives include isothiazolinone preservatives (e.g., 2-methyl-4-isothiazolin-3-one, 5-chloro-2-methyl-4-isothiazolin-3-one), paraoxybenzoic acid esters, and phenoxyethanol. These mildewproofing agents and preservatives may be used alone or in combination of two or more.
[0075] <Method of manufacturing the polishing composition> The method for producing a polishing composition according to the present embodiment includes a step of producing a polishing composition by mixing abrasive grains, a hydrophobic dispersion medium, water, and a surfactant. The surfactant is represented by the formula (i) RO-(C2H4O) n In the formula (i), R is a branched alkyl group having 12 to 20 carbon atoms, and n is the average number of moles of oxyethylene added and is 3 to 50.
[0076] By using such a production method, it is possible to produce a polishing composition that is less likely to leave a haze on the surface of the object to be polished, even if a long time is left before wiping it off.
[0077] In the above-mentioned manufacturing method, it is preferable to mix the hydrophobic dispersion medium and the surfactant in advance, and then mix with water and abrasive grains.In addition, when the polishing composition of the present invention contains hydrophilic components such as thickeners and emulsion stabilizers, it is preferable to mix the hydrophobic dispersion medium and the surfactant in advance to prepare a hydrophobic mixture, and mix the water and the hydrophilic component to prepare a hydrophilic mixture, and then mix the hydrophobic mixture, the hydrophilic mixture, and the abrasive grains.
[0078] In addition, when the polishing composition of the present invention contains other components such as a pH adjuster, after mixing the hydrophobic dispersion medium, surfactant, water, and abrasive grains, other components such as the pH adjuster may be stirred and mixed, if necessary.
[0079] The temperature at which the components are mixed is not particularly limited, but is preferably, for example, from 10° C. to 40° C. The mixing time is not particularly limited.
[0080] (Specific example of a method for manufacturing abrasive grains) The method for producing the abrasive grains (secondary particles) will be further described with a specific example. As described above, in this embodiment, the abrasive grains may be aluminum oxide (alumina). The method for producing alumina is not particularly limited, but one example includes appropriately pulverizing and / or classifying a powder obtained by firing a starting material such as an aluminum oxide precursor powder. The shape of the abrasive grains, including the degree of surface roughness, can be controlled by the type of aluminum oxide starting material and the firing conditions.
[0081] The aluminum oxide precursor powder may be an aluminum hydroxide powder or an aluminum oxide powder containing a transitional aluminum oxide phase. The aluminum hydroxide powder may be gibbsite, boehmite, pseudoboehmite, diaspore, or any combination thereof. The aluminum oxide precursor powder may include gamma (γ), eta (η), theta (θ), chi (χ), (kappa) κ, and / or delta (δ) phase aluminum oxide.
[0082] The aluminum oxide precursor powder can be calcined to form aluminum oxide (alumina). The calcination method is not particularly limited, but a rotary kiln, a tunnel kiln, an electric furnace, a muffle furnace, an elevator kiln, or a pusher kiln can be used as an example. The calcination conditions are a calcination temperature of about 700 to 1600°C and a calcination time of about 1 to 48 hours. This makes it possible to obtain α-alumina having a suitable α-conversion rate. The higher the calcination temperature and the longer the calcination time, the smaller the surface unevenness, i.e., the smaller the specific surface area tends to be.
[0083] The calcined alumina powder can be crushed and classified to obtain alumina having a desired particle size distribution. Crushing and classification can be carried out by a wet or dry process.
[0084] As examples of the pulverization method, various devices including a roller mill, a jet mill, a high-speed rotary pulverizer, and a container-driven mill can be used. In each device, alumina having a desired particle size distribution can be obtained by changing the pulverization conditions such as the pulverization time.
[0085] Examples of classification methods include filtering, sieving, air classification, elutriation classification, weight classification, inertial classification, and centrifugal classification. Examples of filtering methods include rough filtration, precision filtration, ultrafiltration, and reverse osmosis. Examples of filters used for filtering include mesh filters, depth filters, and membrane filters. In filtering, the particle size distribution of the powder can be controlled by the filtration time, filtration speed, and filtration accuracy. For example, the filtration accuracy can be 0.1 to 300 μm.
[0086] By appropriately selecting and / or combining one or more of the above-mentioned firing methods, pulverizing methods, and classification / filtering methods and controlling the respective conditions, it is possible to obtain alumina having a desired particle size distribution and specific surface area.
[0087] <Object to be polished> The object to be polished according to the present embodiment is not particularly limited, but preferably includes at least one selected from the group consisting of alloy materials, resin materials, metals, semi-metals, metal oxides, metal carbides, metal nitrides, semi-metal oxides, semi-metal carbides, semi-metal nitrides, and glass materials, and may further be a composite material of these materials. In particular, a resin material (resin coating film) used for the painted surface of an automobile body or the like is preferable.
[0088] The type of the resin coating is not particularly limited, but the resin constituting the resin coating is preferably, for example, a urethane resin or an acrylic resin, and the type of the resin may be a single urethane resin or an acrylic resin, or a mixture thereof. Furthermore, the resin coating may be a transparent clear coating. The thickness of the resin coating is not particularly limited, but may be 100 μm or less, or may be 10 μm or more and 40 μm or less. The hardness of the resin can be adjusted by the drying temperature, and generally, the resin is soft at a drying temperature of about 60 ° C., and hard at a drying temperature of about 140 ° C. If the polishing composition according to this embodiment is applied to the buff polishing of such a resin coating, it is possible to improve the wiping property after polishing while improving the processing efficiency.
[0089] The polishing composition of this embodiment can be used to manufacture a coated member having a resin coating film on the surface of a substrate. By using the polishing composition of this embodiment to polish the outer surface of the resin coating film of a coated member, it is possible to manufacture a coated member having a resin coating film with beautiful luster that is unlikely to remain cloudy on the surface of the polished object even if a long time is left before wiping it off.
[0090] The type of painted member (i.e., the application of the resin coating film) is not limited to the body of an automobile. The type of painted member is not particularly limited, and examples thereof include railroad cars, aircraft, and resin members.
[0091] <Polishing method> The polishing method according to this embodiment includes a step of polishing an object to be polished with the polishing composition or the polishing composition obtained by the production method described above.
[0092] In the step of polishing an object to be polished, for example, a polishing composition is supplied to the surface of the resin coating film, which is the object to be polished, and the surface to which the polishing composition has been supplied is polished by contacting it with a polishing buff. As the polishing buff, for example, a wool buff or a sponge buff, or both, are used.
[0093] The configuration of the polishing device is not particularly limited, and may be a general polishing device such as a polisher that can be held by the operator (hereinafter also referred to as a hand polisher), a single-sided polisher, a double-sided polisher, a lens polisher, a vertical electric polisher, a grinder, or an automatic polishing device.
[0094] When using a hand polisher, an operator manually moves the hand polisher to polish the surface of an object to be polished (e.g., a resin coating). The driving means of the hand polisher is not particularly limited, but generally, single action, double action, gear action, etc. are used, and double action is preferred for polishing resin coatings.
[0095] When an automatic polishing device is used, the automatic polishing device moves a robot arm under the control of a controller to polish the surface of an object to be polished (for example, a resin coating).
[0096] <Polishing equipment> Fig. 1 is a diagram showing an example of a polishing device used in an embodiment of the present invention. The automatic polishing device 1 in Fig. 1 includes a robot arm 2, a polishing buff 10, a polishing tool 4, a pressing force detection unit 5, and a controller 7. The robot arm 2 has a plurality of joints 20, 21, and 22, and therefore can move a tip portion 23 to which the polishing buff 10, the polishing tool 4, and the pressing force detection unit 5 are attached in a plurality of directions. The object 90 to be polished is, for example, a vehicle body such as an automobile, the surface of which is covered with a resin coating film.
[0097] The polishing tool 4 is attached to the tip 23 via a pressing force detection unit 5, and the polishing buff 10 is rotated by a built-in driving means about a rotation axis perpendicular to the polishing surface 10a of the polishing buff 10. A controller 7 controls the behavior of the robot arm 2 and the rotation of the polishing buff 10 by the polishing tool 4. A polishing composition is supplied from a polishing composition supplying mechanism (not shown) between the polishing surface 10a of the polishing buff 10 and the resin-coated surface of the object 90 to be polished.
[0098] The controller 7 uses the robot arm 2 to press the polishing surface 10a of the polishing buff 10 against the resin-coated surface of the polishing object 90 and rotate the polishing buff 10 to polish the resin-coated surface. The pressing force detection unit 5 detects the pressing force of the polishing surface 10a of the polishing buff 10 against the resin-coated surface. The controller 7 may adjust the force pressing the polishing surface 10a against the resin-coated surface based on the pressing force detection result by the pressing force detection unit 5. Furthermore, the controller 7 may control the robot arm 2 based on the pressing force detection result by the pressing force detection unit 5 so that the polishing buff 10 moves over the resin-coated surface while keeping the pressing force of the polishing surface 10a against the resin-coated surface constant.
[0099] The material of the polishing buff 10 is not particularly limited, and general nonwoven fabric, suede, wool buff, woven fabric, polyurethane foam, polyethylene foam, porous fluororesin, etc. can be used without particular limitation. The polishing buff 10 that can be used has grooves on the polishing surface 10a for storing a liquid polishing composition.
[0100] <Example> The present invention will be described in more detail below with reference to examples and comparative examples. However, the technical scope of the present invention is not limited to the following examples. The following examples and comparative examples were carried out under the conditions of room temperature (20°C to 25°C) and relative humidity of 30% RH to 50% RH.
[0101] Table 1 shows the constitutions of the polishing compositions according to the examples of the present invention and the comparative examples, and the presence or absence of adherent matter on the resin coating film after polishing. (Preparation of Polishing Compositions of Examples 1 to 5 and Comparative Examples 1 to 6) A hydrophobic dispersion medium solution was prepared by adding 0.8 wt% of a surfactant to 16% by mass (hereinafter, wt%) of the hydrophobic dispersion medium. Next, 1.0 wt% of a polyacrylic acid-based polymer (thickener) and 2.0 wt% of glycerin (emulsion stabilizer) were mixed into water, and the solution was added to the hydrophobic dispersion medium solution and stirred at room temperature (25°C), and then 12 wt% of abrasive grains shown in Table 1 were added. A preservative was added to the obtained dispersion liquid, and sodium hydroxide was added as an alkali to adjust the pH to 9.0, to prepare polishing compositions of Examples 1 to 5 and Comparative Examples 1 to 6 of O / W type emulsion. In Table 1, the column marked with - means that there is no data.
[0102] In Table 1, the structure of the R portion indicates the structure of the alkyl ether portion in the polyoxyethylene alkyl ether, and corresponds to R in formula (i). In Table 1, the average number of moles added indicates the average number of moles added of oxyethylene (CHO) or oxyalkylene, and corresponds to n in formula (i). [Table 1]
[0103] In Examples 1 to 5 and Comparative Examples 1 to 6, the following abrasive grains and hydrophobic dispersion media were used.
[0104] (Abrasive grain) The abrasive grains have a composition of aluminum oxide, an alpha content of 95%, an average secondary particle diameter (D50) of 0.8 μm, (D10-D90) / D50 of 1.1, and a specific surface area of 14.1 m. 2 / g abrasive grains were used. The alpha conversion rate of the aluminum oxide particles was measured using an X-ray analyzer (Ultima-IV, Rigaku Corporation), and commercially available alpha alumina single crystal particles (alpha conversion rate: 100%) that had been fired at a sufficiently high temperature and had undergone sufficient alpha conversion were used as the reference material. The integrated intensity of the (113) diffraction line from X-ray diffraction measurements of the reference material and the target abrasive grains (aluminum oxide particles) was measured, and the alpha conversion rate of the target abrasive grains (aluminum oxide particles) was calculated from the integrated intensity ratio of the (113) diffraction line of the target abrasive grains to that of the reference material.
[0105] The average secondary particle diameter (D50), D10, and D90 of the abrasive grains were measured by the pore electrical resistance method using a Multisizer 3 (Beckman Coulter, Inc.). The specific surface area of the abrasive grains was measured by the BET method using a Macsorb HM model-1201 (Mountec Co., Ltd.).
[0106] (Hydrophobic Dispersion Medium) The hydrophobic dispersion medium used was a synthetic hydrocarbon (isoparaffinic hydrocarbon) derived from mineral oil, with a flash point of 63°C (closed method), a total content of benzene-based organic solvents and halogen-based organic solvents of 0.5% by mass or less, and a vapor pressure of 0.05 kPa (molecular weight 170). Note that the vapor pressure is the value at 20°C.
[0107] (Object to be polished) The object to be polished was a composite material having a clear coating film made of synthetic resin paint on the surface of a steel plate, which was baked at 60°C. The pencil hardness of the clear coating film after baking was F.
[0108] (polishing machine) The polishing machine used was a double action polisher LHR12E (manufactured by Rupes).
[0109] (polishing conditions) The polishing conditions are as follows. Polishing buff: Sponge buff Pressing load: 4kg Polisher speed: 5300 rpm ·Polishing linear speed: 200m / min Flow rate of polishing compound: 0.6g / 30sec ·Polishing time: 30 seconds ·Polishing area: 400×600mm (Washing, wiping)
[0110] In order to evaluate the wiping properties of the polishing compositions according to Examples 1 to 5 and Comparative Examples 1 to 6, cleaning treatment and wiping treatment were carried out in the following order of Steps 1 to 6. Then, the wiping properties were evaluated. Step 1 After polishing the surface of the object to be polished vertically under the above polishing conditions, leave it for 1 hour, and then pour water on it (just enough to wet it). Step 2 Lather up the 25x diluted cleaning solution in the container. Step 3 A soft woolen cloth is immersed in the container and thoroughly saturated with the cleaning solution. The cloth is then brought into contact with the surface of the object to be polished, and lightly rubbed while lathering the cleaning solution to lightly clean the surface of the object to be polished. Step 4 The surface of the object to be polished is washed with water to wash away the cleaning solution. Step 5 Air is blown onto the surface of the workpiece to remove moisture. Step 6 Gently wipe the surface of the object to be polished with a cloth.
[0111] (Evaluation of wiping ability) After performing the above steps 1 to 6, the inventors visually checked the presence or absence of white cloudiness (adhered matter) on the surface of the object to be polished, thereby evaluating the wiping properties. When no white cloudiness (adhered matter) was visually confirmed, it was determined that no adhering matter was present on the surface of the object to be polished (i.e., the clear coating film) (good: ◯). When white cloudiness (adhered matter) was visually confirmed, it was determined that there was adhering matter present on the surface of the object to be polished (i.e., the clear coating film) (poor: ×).
[0112] As shown in Table 1, in Examples 1 to 5, no adhered matter was found and the wiping ability was good: ◯. On the other hand, in Comparative Examples 1 to 6, adhered matter was found and the wiping ability was poor: ×.
[0113] (Stability evaluation) The present inventors performed an evaluation of the stability of the polishing compositions according to Examples 1 to 5, which had good results in the evaluation of the wiping property. Here, stability means that the polishing composition maintains a state in which water and oil are mixed uniformly (i.e., an emulsified state). If the emulsified state was visually maintained after a certain time had elapsed after the production of the polishing composition, it was judged to have stability (good: ◯), and if the emulsified state was not visually maintained (i.e., the water layer and the oil layer were separated), it was judged to have no stability (poor: ×).
[0114] As shown in Table 1, in all of Examples 1 to 5, the emulsified state was maintained and the stability was good (good: ◯).
[0115] <Other embodiments> As described above, the present technology has been described by the embodiments and examples, but the descriptions and drawings forming part of this disclosure should not be understood as limiting the present technology. From this disclosure, various alternative embodiments, examples, and operation techniques will be apparent to those skilled in the art. Of course, the present technology includes various embodiments not described here. At least one of various omissions, substitutions, and modifications of components can be made within the scope of the gist of the above-mentioned embodiments and examples. In addition, the effects described in this specification are merely examples and are not limited, and other effects may be present.
[0116] The present invention can also have the following configuration. (1) The method includes the steps of: The surfactant has the formula (i) RO-(CHO) n -H, In the above formula (i), R is a branched alkyl group having 12 to 20 carbon atoms, and n is the average number of moles of oxyethylene added and is 3 to 50. (2) The polishing composition according to (1) above, wherein the average number of added moles n is 5 or more and 15 or less. (3) The polishing composition according to (1) or (2), wherein the surfactant has an HLB value of 10 or more and 16 or less, the HLB value indicating the affinity of the surfactant for water and oil. (4) The polishing composition according to any one of (1) to (3), wherein the abrasive grains are contained in an amount of 5 mass % to 30 mass % based on the total mass of the polishing composition. (5) The polishing composition according to any one of (1) to (4), wherein the abrasive grains contain aluminum oxide. (6) The polishing composition according to (5) above, wherein the alpha conversion rate of the aluminum oxide is 50% or more and 100% or less. (7) The hydrophobic dispersion medium is At least one selected from the group consisting of normal paraffinic hydrocarbons, isoparaffinic hydrocarbons, naphthenic hydrocarbons, and terpene hydrocarbons, The polishing composition according to any one of (1) to (6), having a flash point of 30° C. or higher and 100° C. or lower. (8) The polishing composition according to any one of (1) to (7), wherein the hydrophobic dispersion medium has a vapor pressure at 20° C. of 0.004 kPa or more and 2 kPa or less. (9) A method for producing a polishing composition, comprising the step of producing a polishing composition by mixing an abrasive grain, a hydrophobic dispersion medium, water, and a surfactant, The surfactant has the formula (i) RO-(CHO) n -H, In the above formula (i), R is a branched alkyl group having 12 to 20 carbon atoms, and n is the average number of moles of oxyethylene added which is 3 to 50. (10) A polishing method comprising a step of polishing an object to be polished with the polishing composition according to any one of (1) to (8). (11) The polishing method according to (10), wherein the object to be polished includes at least one material selected from the group consisting of a resin material, an alloy material, and a glass material. (12) In the step of polishing the object to be polished, The polishing method according to (10) or (11), further comprising supplying the polishing composition to a surface of the object to be polished, and bringing a polishing buff into contact with the surface to which the polishing composition has been supplied, thereby polishing the surface. [Explanation of symbols]
[0117] 1 Automatic polishing device 2. Robot Arm 4 Polishing tools 5 Pressure detection unit 7 Controller 10 Polishing buff 10a Polished surface 20, 21, 22 Joints 23 Tip 90 Polishing object
Claims
1. The method includes the steps of: The surfactant has the formula (i) RO-(C 2 H 4 O) n Contains a polyoxyethylene alkyl ether represented by -H, In the above formula (i), R is a branched alkyl group having 12 to 20 carbon atoms, and n is the average number of moles of oxyethylene added and is 3 to 50.
2. The polishing composition according to claim 1 , wherein the average number of added moles n is 5 or more and 15 or less.
3. 3. The polishing composition according to claim 1, wherein the surfactant has an HLB value, which indicates affinity for water and oil, of 10 or more and 16 or less.
4. 3. The polishing composition according to claim 1, wherein the abrasive grains are contained in an amount of 5 mass % or more and 30 mass % or less based on the total mass of the polishing composition.
5. The polishing composition according to claim 1 , wherein the abrasive grains contain aluminum oxide.
6. 6. The polishing composition according to claim 5, wherein the aluminum oxide has an alpha conversion rate of 50% or more and 100% or less.
7. The hydrophobic dispersion medium is At least one selected from the group consisting of normal paraffinic hydrocarbons, isoparaffinic hydrocarbons, naphthenic hydrocarbons, and terpene hydrocarbons, 3. The polishing composition according to claim 1, having a flash point of 30° C. or higher and 100° C. or lower.
8. 3. The polishing composition according to claim 1, wherein the hydrophobic dispersion medium has a vapor pressure at 20°C of 0.004 kPa or more and 2 kPa or less.
9. A method for producing a polishing composition, comprising the step of producing a polishing composition by mixing an abrasive grain, a hydrophobic dispersion medium, water, and a surfactant, The surfactant has the formula (i) RO-(C 2 H 4 O) n Contains a polyoxyethylene alkyl ether represented by -H, In the above formula (i), R is a branched alkyl group having 12 to 20 carbon atoms, and n is an average number of moles of oxyethylene added which is 3 to 50.
10. A polishing method comprising a step of polishing an object to be polished with the polishing composition according to claim 1 or 2.
11. The polishing method according to claim 10 , wherein the object to be polished includes at least one material selected from the group consisting of a resin material, an alloy material, and a glass material.
12. In the step of polishing the object to be polished, 11. The polishing method according to claim 10, further comprising supplying the polishing composition to a surface of the object to be polished, and bringing a polishing buff into contact with the surface to which the polishing composition has been supplied, thereby polishing the object.
Citation Information
Patent Citations
Aqueous lapping liquid and aqueous lapping agent
JP2002114970A
POLISHING alpha-ALUMINA COMPOSITION, AND METHOD FOR PRODUCING THE SAME
JP2006124622A
Method for treating floor treated with wax
JP2010077182A
Alumina abrasive particles for use in automotive finishing compositions
JP2020510605A
Abrasive composition
US20170355880A1
Cited By
Lapping method and composition for lapping process
WO2026211581A1