Honeycomb structure

The combination of crosslinked starch and acrylic polymer as pore-forming materials addresses the strength and extrusion pressure issues in manufacturing thin-walled, high-porosity honeycomb structures, ensuring high productivity and performance in filters and catalyst carriers.

JP2024144042AActive Publication Date: 2024-10-11NGK CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023187959
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-11-01
Publication Date
2024-10-11
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

Honeycomb structures with thin walls and high porosity face challenges in maintaining sufficient strength and require reduced extrusion pressure during manufacturing, making it difficult to meet stringent PM emission standards and catalyst carrier requirements.

Method used

A manufacturing method involving the use of a combination of crosslinked starch and acrylic polymer as pore-forming materials in the clay composition, with controlled P content, to produce honeycomb structures with thicknesses between 50 μm and 210 μm, porosity of 45% to 60%, and isostatic fracture strength of 1.0 MPa or more.

Benefits of technology

The method enables the production of honeycomb structures with high productivity, suitable for filters and catalyst carriers, achieving high PM collection efficiency and rapid temperature increase, without overburdening the extrusion molding machine.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144042000001_ABST
    Figure 2024144042000001_ABST
Patent Text Reader

Abstract

To provide a honeycomb structure that is formed in thinner wall and higher porosity, and has excellent strength.SOLUTION: A honeycomb structure has: an outer peripheral side wall; and a partition wall which is disposed on an inner peripheral side of the outer peripheral side wall, and partitions a plurality of cells forming flow channels from a first bottom face to a second bottom face, where the thickness of the partition wall is 50 μm or more and 210 μm or less, the porosity of the partition wall is 45% to 60%, P content in the honeycomb structure is 0.01 mass% or more and less than 0.2 mass%, and the isostatic strength is 1.0 MPa or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a honeycomb structure and a manufacturing method thereof. [Background technology]

[0002] 2. Description of the Related Art Honeycomb structures are used as filters that collect particulate matter in exhaust gas emitted from internal combustion engines such as diesel engines, and as supports for catalysts that purify toxic gas components such as CO, HC, and NOx.

[0003] In general, a honeycomb structure has an outer peripheral side wall and partition walls disposed on the inner peripheral side of the outer peripheral side wall and partitioning a plurality of cells that form a flow path from the first bottom surface to the second bottom surface. The honeycomb structure can be manufactured by kneading a raw material composition obtained by appropriately adding various additives to a ceramic raw material, a pore-forming material, a binder, and a dispersion medium to form a clay, extruding the mixture through a die that defines a predetermined cell structure to produce a honeycomb molded body, cutting the honeycomb molded body to a predetermined length, drying it, and then firing it.

[0004] In recent years, with the strengthening of exhaust gas regulations, stricter PM emission standards (PN regulations: Particle Matter number regulations) have been introduced, and filters are required to have high PM collection performance (high PN collection efficiency). In addition, catalyst carriers are also required to be able to quickly heat up to the catalyst activation temperature by reducing their heat capacity. On the other hand, honeycomb structures are also required to have low pressure loss when exhaust gas is passed through them, and the development of filters that can meet market demands is becoming more difficult. In order to obtain a honeycomb structure that meets these required performance requirements, studies are being conducted on "thinning the walls" by reducing the thickness of the partition walls of the honeycomb structure, as well as "increasing the porosity" by further increasing the porosity of the partition walls compared to conventional methods (Patent Document 1).

[0005] However, as the wall of a honeycomb structure becomes thinner, the extrusion pressure required to extrude the clay through a very narrow die slot also increases, reaching the limit of the extrusion molding machine. For this reason, a technology for reducing the extrusion pressure is also required. In this regard, Patent Document 2 describes that a high amylose ratio in the starch added to the raw material composition improves the fluidity and reduces the molding pressure, and in particular, it discloses that the extrusion pressure can be reduced when the ratio of amylose:amylopectin is 40:60 to 80:20. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Special Publication No. 2007-507667 [Patent Document 2] International Publication No. 2017 / 095916 Summary of the Invention [Problem to be solved by the invention]

[0007] Starch is useful as a component for obtaining a honeycomb structure with high porosity. Therefore, when manufacturing a honeycomb structure with thin walls and high porosity, it was considered effective to add starch in the blending ratio of amylose and amylopectin described in Patent Document 2. However, even if the extrusion molding pressure can be reduced by adding starch with an adjusted blending ratio of amylose and amylopectin to the raw material composition in this way, the strength of the honeycomb structure manufactured by this method is insufficient. In particular, since honeycomb structures with thin walls and high porosity are prone to strength reduction, it would be advantageous if this problem could be solved.

[0008] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a method for manufacturing a honeycomb structure having thin walls, high porosity, and excellent strength without placing an excessive burden on an extrusion molding machine, and to provide a honeycomb structure having thin walls, high porosity, and excellent strength, in one embodiment. [Means for solving the problem]

[0009] The present inventors have conducted extensive research to solve the above problems and have found that it is effective to use a combination of an acrylic polymer and crosslinked starch as a pore-forming material. The present invention was completed based on this finding and is exemplified below.

[0010] (1. Manufacturing method of honeycomb structure) [Aspect 1] A method for manufacturing a honeycomb structure having an outer peripheral side wall and partition walls disposed on an inner peripheral side of the outer peripheral side wall and partitioning a plurality of cells forming a flow path from a first bottom surface to a second bottom surface, a step of extruding a clay containing a ceramic raw material, a pore former, a binder, and a dispersion medium through a die that defines an opening shape of the plurality of cells to produce a honeycomb formed body; A step of drying the honeycomb formed body to obtain a dried honeycomb body; a step of firing the honeycomb dried body to obtain a honeycomb fired body having a partition wall thickness of 50 μm or more and 210 μm or less and a partition wall porosity of 45% to 60%; Including, The pore-forming material in the clay contains crosslinked starch and an acrylic polymer, The clay contains 1.0 part by mass or more of crosslinked starch, with a P content of less than 0.2 part by mass per 100 parts by mass of ceramic raw material. Manufacturing method. [Aspect 2] The method according to embodiment 1, wherein the clay contains 1.0 part by mass or more of crosslinked starch, with a P content of 0.1 part by mass or less per 100 parts by mass of the ceramic raw material. [Aspect 3] The method according to embodiment 1, wherein the clay contains 1.0 part by mass or more of crosslinked starch, with the P content being 0.05 part by mass or less, per 100 parts by mass of the ceramic raw material. [Aspect 4] The manufacturing method according to any one of aspects 1 to 3, wherein the honeycomb structure has a P content of less than 0.2 mass %. [Aspect 5] The manufacturing method according to any one of aspects 1 to 3, wherein the honeycomb structure has a P content of 0.1 mass % or less. [Aspect 6] The manufacturing method according to any one of aspects 1 to 3, wherein the honeycomb structure has a P content of 0.05% by mass or less. [Aspect 7] 7. The method according to any one of Aspects 1 to 6, wherein the clay contains 0.5 parts by mass or more of an acrylic polymer with respect to 100 parts by mass of the ceramic raw material. [Aspect 8] The method according to any one of Aspects 1 to 7, wherein the ceramic raw material is a cordierite-forming raw material.

[0011] (2. Honeycomb structure) [Aspect 1] A honeycomb structure having an outer peripheral side wall and partition walls disposed on an inner peripheral side of the outer peripheral side wall and partitioning a plurality of cells forming a flow path from a first bottom surface to a second bottom surface, The thickness of the partition wall is 50 μm or more and 210 μm or less, The porosity of the partition wall is 45% to 60%. The P content in the honeycomb structure is 0.01 mass% or more and less than 0.2 mass%, Isostatic fracture strength is 1.0MPa or more. Honeycomb structure. [Aspect 2] 2. The honeycomb structure according to embodiment 1, wherein the upper limit of the P content in the honeycomb structure is 0.1% by mass or less. [Aspect 3] 2. The honeycomb structure according to embodiment 1, wherein the upper limit of the P content in the honeycomb structure is 0.05% by mass or less. [Aspect 4] The honeycomb structure according to any one of aspects 1 to 3, wherein the outer peripheral side wall and the partition walls contain cordierite. Effect of the Invention

[0012] According to one embodiment of the present invention, a honeycomb structure having thin walls, high porosity, and excellent strength can be manufactured with high productivity without placing an excessive burden on an extrusion molding machine. The honeycomb structure can be suitably used as a filter or a catalyst carrier, and is particularly useful as a filter requiring high collection performance (high PN collection efficiency) or a catalyst carrier requiring a high heating rate. [Brief description of the drawings]

[0013] [Figure 1] FIG. 2 is a perspective view showing a typical wall-through type honeycomb structure. [Diagram 2] FIG. 2 is a schematic cross-sectional view of a wall-through type honeycomb structure observed in a cross section parallel to the cell extension direction. [Diagram 3] FIG. 1 is a perspective view showing a schematic view of a wall-flow type honeycomb structure. [Figure 4] FIG. 2 is a schematic cross-sectional view of a wall-flow type honeycomb structure observed in a cross section parallel to the cell extension direction. [Diagram 5] FIG. 2 is a schematic partial enlarged view of a partition wall of a wall-flow type honeycomb structure observed in a cross section perpendicular to the cell extension direction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Next, an embodiment of the present invention will be described in detail with reference to the drawings. It should be understood that the present invention is not limited to the following embodiment, and that appropriate changes and improvements in the design may be made based on the ordinary knowledge of a person skilled in the art without departing from the spirit of the present invention.

[0015] <1. Honeycomb structure> In one embodiment, the honeycomb structure according to the present invention is provided as a wall-through type or wall-flow type honeycomb structure. The use of the honeycomb structure is not particularly limited. For example, it is used for various industrial applications such as heat sinks, filters (e.g. GPF, DPF), catalyst carriers, sliding parts, nozzles, heat exchangers, electrical insulating members, and parts for semiconductor manufacturing equipment. In particular, it can be suitably used as a filter for collecting particulate matter contained in exhaust gas from an internal combustion engine, a boiler, etc., and a catalyst carrier for an exhaust gas purification catalyst. In particular, the porous honeycomb structure can be suitably used as an exhaust gas filter and / or a catalyst carrier for an automobile.

[0016] 1 and 2 are schematic perspective and cross-sectional views, respectively, of a honeycomb structure 100 applicable as a wall-through type exhaust gas filter and / or catalyst carrier for an automobile. The honeycomb structure 100 includes an outer peripheral side wall 102 and partition walls 112 disposed on the inner peripheral side of the outer peripheral side wall 102 and partitioning a plurality of parallel cells 108 that form a fluid flow path from a first bottom surface 104 to a second bottom surface 106. The outer surface of the outer peripheral side wall 102 forms a side surface 103 of the honeycomb structure 100. In the honeycomb structure 100, both ends of each cell 108 are open, and exhaust gas that flows into one cell 108 from the first bottom surface 104 is purified while passing through the cell, and flows out from the second bottom surface 106. Here, the first bottom surface 104 is defined as the upstream side of the exhaust gas, and the second bottom surface 106 is defined as the downstream side of the exhaust gas. However, the distinction between the first bottom surface and the second bottom surface is for convenience, and the second bottom surface 106 may be defined as the upstream side of the exhaust gas, and the first bottom surface 104 may be defined as the downstream side of the exhaust gas.

[0017] 3 and 4 are schematic perspective and cross-sectional views, respectively, of a honeycomb structure 200 applicable as a wall-flow type exhaust gas filter for automobiles and / or a catalyst carrier. The honeycomb structure 200 includes an outer peripheral side wall 202 and partition walls 212 disposed on the inner peripheral side of the outer peripheral side wall 202 and partitioning a plurality of cells 208a, 208b that form a fluid flow path from a first bottom surface 204 to a second bottom surface 206. The outer surface of the outer peripheral side wall 202 forms a side surface 203 of the honeycomb structure 200.

[0018] In the honeycomb structure 200, the multiple cells 208a, 208b can be classified into multiple parallel first cells 208a extending from the first bottom surface 204 to the second bottom surface 206, opening at the first bottom surface 204 and having plugging portions 209 at the second bottom surface 206, and multiple parallel second cells 208b disposed inside the outer peripheral side wall 202, extending from the first bottom surface 204 to the second bottom surface 206, having plugging portions 209 at the first bottom surface 204, and opening at the second bottom surface 206. In this honeycomb structure 200, the first cells 208a and the second cells 208b are alternately adjacently arranged with the partition walls 212 interposed therebetween.

[0019] When exhaust gas containing particulate matter such as soot is supplied to the first bottom surface 204 on the upstream side of the honeycomb structure 200, the exhaust gas is introduced into the first cells 208a and proceeds downstream inside the first cells 208a. Since the first cells 208a have plugged portions 209 on the second bottom surface 206 on the downstream side, the exhaust gas passes through the partition walls 212 that separate the first cells 208a and the second cells 208b and flows into the second cells 208b. Since the particulate matter cannot pass through the partition walls 212, it is collected and accumulated inside the first cells 208a. After the particulate matter is removed, the clean exhaust gas that has flowed into the second cells 208b proceeds downstream inside the second cells 208b and flows out from the second bottom surface 206 on the downstream side. Here, the first bottom surface 204 is defined as the upstream side of the exhaust gas, and the second bottom surface 206 is defined as the downstream side of the exhaust gas, but the distinction between the first bottom surface and the second bottom surface is for convenience, and the second bottom surface 206 may be defined as the upstream side of the exhaust gas, and the first bottom surface 204 may be defined as the downstream side of the exhaust gas.

[0020] The outer shape of the honeycomb structure may be, for example, a columnar shape. The bottom shape of the honeycomb structure is not limited, and may be, for example, a round shape such as a circle, an ellipse, a racetrack shape, or an oval shape, a polygonal shape such as a triangle or a square, or other irregular shape. The honeycomb structure shown in the figure has a circular bottom shape and is cylindrical as a whole.

[0021] The height of the honeycomb structure (the length from the first bottom surface to the second bottom surface) is not particularly limited, and may be appropriately set depending on the application and required performance. The height of the honeycomb structure may be, for example, 40 mm to 450 mm. There is also no particular limit to the relationship between the height of the honeycomb structure and the maximum diameter of each bottom surface (the maximum length of the diameters passing through the center of gravity of each bottom surface of the honeycomb structure). Therefore, the height of the honeycomb structure may be longer than the maximum diameter of each bottom surface, or the height of the honeycomb structure may be shorter than the maximum diameter of each bottom surface.

[0022] The cell density of the honeycomb structure (the number of cells per unit cross-sectional area perpendicular to the cell extension direction) is not particularly limited, but is, for example, 6 to 2000 cells / square inch (0.9 to 311 cells / cm). 2 ), more preferably 50 to 1000 cells / in2 (7.8 to 155 cells / cm2). 2 ), and particularly preferably 100 to 600 cells / square inch (15.5 to 92.0 cells / cm 2 Here, the cell density is calculated by dividing the total number of cells on one side of the bottom surface of the honeycomb structure excluding the peripheral side wall (if plugged cells are present, the calculation is performed assuming that the cells are not plugged) by the bottom area of ​​the one side of the bottom surface.

[0023] The thickness of the partition walls in the honeycomb structure is preferably 210 μm or less, more preferably 150 μm or less, and even more preferably 100 μm or less, from the viewpoint of reducing pressure loss and heat capacity by thinning the walls, and is preferably 50 μm or more, more preferably 60 μm or more, and even more preferably 70 μm or more, from the viewpoint of ensuring strength.

[0024] 5 shows a schematic partial enlarged view of the partition walls 212 of the wall-flow type honeycomb structure 200 observed in a cross section perpendicular to the cell extension direction. The thickness of the partition wall refers to the length of a line segment N that crosses the partition wall when the line segment N connects the centers of gravity C of adjacent cells in a cross section perpendicular to the cell extension direction (height direction of the honeycomb structure).

[0025] The porosity of the partition walls is preferably 45% or more, more preferably 50% or more, from the viewpoint of suppressing pressure loss and reducing heat capacity by increasing the porosity. The upper limit of the porosity of the partition walls is preferably 60% or less, more preferably 55% or less, from the viewpoint of ensuring the strength of the honeycomb structure with thin walls. Therefore, the porosity of the partition walls is preferably, for example, 45 to 60%, more preferably 50 to 55%. The porosity is measured by mercury intrusion porosimetry using a mercury porosimeter. The mercury intrusion porosimetry is specified in JIS R1655:2003. In this specification, a partition wall sample (a cube of length x width x height = about 13 mm x about 13 mm x about 13 mm) of the honeycomb structure is taken from two locations, near the center in the radial direction of the center in the height direction and near the outer periphery, and the porosity is measured by mercury intrusion porosimetry, and the average value is taken as the measured value.

[0026] Materials constituting the partition walls and the outer peripheral side walls of the honeycomb structure include, but are not limited to, porous ceramics. Types of ceramics include cordierite, mullite, zirconium phosphate, aluminum titanate, silicon carbide (SiC), silicon-silicon carbide composites (e.g., Si-bonded SiC), cordierite-silicon carbide composites, zirconia, spinel, indialite, sapphirine, corundum, titania, silicon nitride, and the like. These ceramics may contain one type alone or two or more types.

[0027] The partition walls and the outer peripheral side walls of the honeycomb structure preferably contain cordierite because of their high thermal shock resistance. The mass ratio of cordierite in the honeycomb structure is preferably 50 mass% or more, preferably 70 mass% or more, and preferably 90 mass% or more. The mass ratio of cordierite in the porous honeycomb structure containing cordierite can be substantially 100 mass% excluding unavoidable impurities.

[0028] Raw materials mixed in the raw material composition may remain in the honeycomb structure. As described later, a crosslinking agent containing P (phosphorus) may be used in the crosslinked starch, but if the amount of the crosslinking agent containing P is large, agglomerates are formed in the clay, which tends to increase the extrusion molding pressure. Therefore, if the P content in the crosslinked starch used as the pore-forming material is low, the extrusion molding pressure can be reduced, and the P concentration remaining in the honeycomb structure is also low.

[0029] Therefore, in one embodiment, the P content in the honeycomb structure is less than 0.2 mass%, preferably 0.1 mass% or less, and more preferably 0.05 mass% or less. From the viewpoint of enhancing the effect of reducing the extrusion molding pressure, the P content in the honeycomb structure may be 0.01 mass% or less, or even 0. However, starch crosslinked with a crosslinking agent containing P has a high effect of suppressing cell deformation during extrusion molding, and as a result, the strength of the honeycomb structure is highly improved. Therefore, in terms of the balance with the effect of reducing the extrusion molding pressure, the P content in the honeycomb structure is preferably 0.01 mass% or more and less than 0.2 mass%, and more preferably 0.01 mass% or more and 0.05 mass% or less.

[0030] The P content in the honeycomb structure is measured by the following method. First, partition wall samples (0.5 to 5.0 g) are collected from the honeycomb structure from two locations, namely, near the center in the radial direction at the center in the height direction and near the outer periphery. Sulfuric acid is added to each partition wall sample, and the sample solution is prepared by heating, incineration, and dissolving in hydrochloric acid. The sample solution is sprayed into high-temperature argon plasma generated by high-frequency energy, and the emission intensity of the characteristic wavelength of excited P atoms is measured by a sequential inductively coupled plasma optical emission spectroscope (ICP-OES / AES) and converted into the P content in the honeycomb structure. The average value of the P content in the honeycomb structure obtained from each partition wall sample is taken as the measured value.

[0031] One measure of the mechanical strength of a honeycomb structure is its isostatic fracture strength. In measuring the isostatic fracture strength of a honeycomb structure, a test is conducted in which the honeycomb structure is submerged in water in a pressure vessel, and the water pressure is gradually increased to apply isotropic pressure to the honeycomb structure. As the water pressure in the pressure vessel gradually increases, destruction eventually occurs in the partition walls and outer peripheral side walls of the honeycomb structure. The value of the pressure (destruction strength) at which destruction occurs is the isostatic fracture strength. Isostatic fracture strength is measured based on the automobile standard (JASO M505-87) issued by the Automotive Engineering Society of Japan.

[0032] In one embodiment, the honeycomb structure can have an isostatic fracture strength of 1.0 MPa or more, even though it has thin walls and high porosity. The isostatic fracture strength of the honeycomb structure is preferably 1.5 MPa or more, and more preferably 2.0 MPa or more. There is no particular upper limit set for the isostatic fracture strength, but it is usually 3.0 MPa or less, and typically 2.5 MPa or less.

[0033] When the honeycomb structure is used as a catalyst carrier, the surface of the partition wall can be coated with a catalyst according to the purpose. The catalyst may be used alone or in combination of two or more types. Examples of the catalyst include, but are not limited to, an oxidation catalyst (DOC) for increasing the exhaust gas temperature by oxidizing and burning hydrocarbons (HC) and carbon monoxide (CO), a PM combustion catalyst for assisting the combustion of PM such as soot, an SCR catalyst and an NSR catalyst for removing nitrogen oxides (NOx), and a three-way catalyst capable of simultaneously removing hydrocarbons (HC), carbon monoxide (CO), and nitrogen oxides (NOx). The catalyst may appropriately contain, for example, precious metals (Pt, Pd, Rh, etc.), alkali metals (Li, Na, K, Cs, etc.), alkaline earth metals (Mg, Ca, Ba, Sr, etc.), rare earths (Ce, Sm, Gd, Nd, Y, La, Pr, etc.), transition metals (Mn, Fe, Co, Ni, Cu, Zn, Sc, Ti, Zr, V, Cr, etc.), etc.

[0034] <2. Manufacturing method of honeycomb structure> A method for manufacturing a honeycomb structure according to an embodiment of the present invention will be described below by way of example.

[0035] (2-1. Preparation of honeycomb molded body) First, a raw material composition containing ceramic raw materials, a pore former, a binder, and a dispersion medium is kneaded to form a clay, and then the clay is extruded through a die that defines the opening shape of a plurality of cells to produce an outer peripheral side wall and a honeycomb molded body that is disposed on the inner peripheral side of the outer peripheral side wall, extends from the first bottom surface to the second bottom surface, and has openings on both the first bottom surface and the second bottom surface. Additives such as a dispersant may be blended into the raw material composition as necessary. A die having the desired overall shape, cell shape, partition wall thickness, cell density, etc. can be used for extrusion molding.

[0036] The ceramic raw material remains after firing and is a raw material of a part that constitutes the skeleton of the honeycomb structure as ceramics. As the ceramic raw material, a raw material that can form the above-mentioned ceramics after firing can be used. The ceramic raw material can be provided in the form of, for example, powder. As the ceramic raw material, raw materials for obtaining ceramics such as cordierite, mullite, zircon, aluminum titanate, silicon carbide, silicon nitride, zirconia, spinel, indialite, sapphirine, corundum, and titania can be mentioned. Specific examples of the ceramic raw material include, but are not limited to, silica, talc, alumina, kaolin, serpentine, pyroferrite, brucite, boehmite, mullite, magnesite, and aluminum hydroxide. The ceramic raw material may be used alone or in combination of two or more types.

[0037] Cordierite can be suitably used as the ceramic. In this case, a cordierite-forming raw material can be used as the ceramic raw material. The cordierite-forming raw material is a raw material that becomes cordierite by firing. As the cordierite-forming raw material, talc, kaolin, alumina, aluminum hydroxide, silica, etc. can be used, and the cordierite-forming raw material preferably has a chemical composition of 30 to 45 mass % alumina (Al2O3) (including the aluminum hydroxide converted to alumina), 11 to 17 mass % magnesia (MgO), and 42 to 57 mass % silica (SiO2).

[0038] Since the ceramic raw materials, including the cordierite raw materials, affect the strength of the honeycomb structure, it is preferable to use raw materials whose particle size has been adjusted by crushing, sieving, or the like. Specifically, in the cumulative particle size distribution based on volume measured by a laser diffraction / scattering method, the lower limit of the cumulative 50% particle diameter (D50) from the small particle side of each ceramic raw material is preferably 0.1 μm or more, more preferably 0.5 μm or more, and even more preferably 1.0 μm or more. In addition, the upper limit of the cumulative 50% particle diameter (D50) from the small particle side of each ceramic raw material is preferably 30 μm or less, more preferably 20 μm or less, and even more preferably 15 μm or less. Therefore, for example, the cumulative 50% particle diameter (D50) of each ceramic raw material is preferably 0.1 μm or more and 30 μm or less, more preferably 0.5 μm or more and 20 μm or less, and even more preferably 1.0 μm or more and 15 μm or less.

[0039] When crosslinked starch and acrylic polymer are used in combination as a pore former, the fluidity of the clay is significantly improved. This improves moldability and suppresses cell deformation that is likely to occur during molding, resulting in increased strength of the honeycomb structure. In order to make the honeycomb structure thinner, it is necessary to extrude the clay through an extremely narrow die slot, and this, combined with an increase in extrusion molding pressure, tends to cause distortion of the cell shape (cell deformation). The reason why cell deformation is suppressed by using crosslinked starch and acrylic polymer in combination as a pore former is not necessarily clear. Although it is not intended that the present invention be limited by theory, it is presumed that the water retention properties of crosslinked starch and acrylic polymer lead to improved moldability. Compared to using only one of crosslinked starch and acrylic polymer, the combined use of both can provide a significant effect.

[0040] In crosslinked starch, some hydroxyl groups between starch molecules are crosslinked by using one or more crosslinking agents such as formalin, epichlorohydrin, and phosphate. Examples of crosslinked starch include acetylated adipate crosslinked starch, acetylated phosphate crosslinked starch, hydroxypropylated phosphate crosslinked starch, phosphate monoesterified phosphate crosslinked starch, and phosphate crosslinked starch. The crosslinked starch may be used alone or in combination of two or more types.

[0041] Thus, crosslinked starch may contain phosphorus (P). Furthermore, crosslinked starch containing P is preferable from the viewpoint of achieving high porosity while improving the strength of the honeycomb structure. However, if the P content in the crosslinked starch is high, the screen used to remove impurities during extrusion molding of the clay may become clogged, causing an increase in the extrusion molding pressure, so it is desirable to control the P content in the clay to a range in which screen clogging does not occur.

[0042] The extrusion molding pressure when extruding the clay is preferably 15 MPa or less, more preferably 10 MPa or less. Although a lower extrusion molding pressure is preferable, from the viewpoint of ensuring strength, a clay that can be extruded at an excessively low extrusion molding pressure cannot be used. Therefore, the extrusion molding pressure is preferably 1 MPa or more, more preferably 3 MPa or more. Therefore, the extrusion molding pressure is, for example, preferably 1 to 15 MPa, more preferably 3 to 10 MPa.

[0043] Therefore, it is desirable that the clay contains an acrylic polymer and crosslinked starch under the condition that the P content is less than 0.2 parts by mass, preferably 0.1 parts by mass or less, more preferably 0.05 parts by mass or less, relative to 100 parts by mass of ceramic raw materials. The P content in the clay may be 0.01 parts by mass or less, or even 0 parts by mass, relative to 100 parts by mass of ceramic raw materials. From the viewpoint of achieving high porosity while obtaining the strength improvement effect of the honeycomb structure, the lower limit of the content of the crosslinked starch in the clay is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and even more preferably 10 parts by mass or more, relative to 100 parts by mass of ceramic raw materials, while satisfying the above-mentioned suitable condition of the P content. From the viewpoint of suppressing the occurrence of cracks due to heat generation during firing, the upper limit of the content of the crosslinked starch in the clay is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 20 parts by mass or less, relative to 100 parts by mass of ceramic raw materials.

[0044] When using starch crosslinked with a crosslinking agent containing P, even if the content of crosslinked starch in the clay is the same, the higher the crosslinking degree, the higher the P content, so the P content can be used as an index of the crosslinking degree. For example, the crosslinked starch may have a P content of 0.01 parts by mass or more and less than 0.20 parts by mass per 10 parts by mass. The P content of the crosslinked starch per 10 parts by mass is preferably 0.01 parts by mass or more and less than 0.15 parts by mass, more preferably 0.01 parts by mass or more and less than 0.1 parts by mass.

[0045] The P content in the clay is measured by the following method. First, a sample (0.5 to 5.0 g) is taken from the clay. Sulfuric acid is added to each partition wall sample, and the sample is heated, incinerated, and then dissolved in hydrochloric acid to prepare a sample solution. The sample solution is sprayed into high-temperature argon plasma generated by high-frequency energy, and the emission intensity of the characteristic wavelength of excited P atoms is measured using a sequential inductively coupled plasma optical emission spectrometer (ICP-OES / AES), and converted into the P content in the clay.

[0046] From the viewpoint of achieving high porosity while obtaining the strength improvement effect of the honeycomb structure, the clay preferably contains 0.5 parts by mass or more of acrylic polymer relative to 100 parts by mass of ceramic raw material, more preferably contains 0.7 parts by mass or more of acrylic polymer, and even more preferably contains 1.0 parts by mass or more of acrylic polymer. Also, from the viewpoint of fluidity, the clay preferably contains 10.0 parts by mass or less of acrylic polymer relative to 100 parts by mass of ceramic raw material, more preferably contains 7.0 parts by mass or less of acrylic polymer, and even more preferably contains 5.0 parts by mass or less of acrylic polymer. Therefore, for example, the clay preferably contains 0.5 parts by mass or more and 10 parts by mass or less of acrylic polymer relative to 100 parts by mass of ceramic raw material, more preferably contains 0.7 to 7.0 parts by mass of acrylic polymer, and even more preferably contains 1.0 to 5.0 parts by mass of acrylic polymer.

[0047] The types of acrylic polymers include, but are not limited to, polyacrylic acid, polymethacrylic acid, polyacrylic acid esters, polymethacrylic acid esters, etc., and polymethyl methacrylate (PMMA) is a particularly suitable type of acrylic polymer. The acrylic polymer may be crosslinked. The acrylic polymer may be used alone or in combination of two or more types.

[0048] One or more of other known pore-forming materials may be appropriately added to the clay, such as wheat flour, expanded resin, water-absorbent resin, non-crosslinked starch, porous silica, carbon (e.g., graphite), ceramic balloons, polyethylene, polystyrene, polypropylene, nylon, polyester, and phenol.

[0049] Since the pore formers such as crosslinked starch and acrylic polymer affect the strength of the honeycomb structure, it is preferable to use those whose particle size has been adjusted by crushing, sieving, etc. Specifically, in the cumulative particle size distribution based on volume measured by the laser diffraction scattering method, the lower limit of the cumulative 50% particle diameter (D50) from the small particle side of each pore former is preferably 0.1 μm or more, more preferably 1.0 μm or more, and even more preferably 5.0 μm or more. In addition, the upper limit of the cumulative 50% particle diameter (D50) from the small particle side of each pore former is preferably 30.0 μm or less, more preferably 20.0 μm or less, and even more preferably 15.0 μm or less. Therefore, for example, the cumulative 50% particle diameter (D50) from the small particle side of each pore former is preferably 0.1 to 30.0 μm, more preferably 1.0 to 20.0 μm, and even more preferably 5.0 to 15.0 μm.

[0050] Examples of the binder include organic binders such as methyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl cellulose, carboxymethyl cellulose, and polyvinyl alcohol. In particular, it is preferable to use methyl cellulose and hydroxypropyl methyl cellulose in combination. In addition, the content of the binder in the clay is preferably 4 parts by mass or more, more preferably 5 parts by mass or more, and even more preferably 6 parts by mass or more, relative to 100 parts by mass of the ceramic raw material, from the viewpoint of increasing the strength of the honeycomb molded body. The content of the binder in the clay is preferably 9 parts by mass or less, more preferably 8 parts by mass or less, and even more preferably 7 parts by mass or less, relative to 100 parts by mass of the ceramic raw material, from the viewpoint of suppressing the occurrence of cracks due to abnormal heat generation in the firing process. The binder may be used alone or in combination of two or more types.

[0051] Examples of the dispersion medium include water or a mixed solvent of water and an organic solvent such as alcohol, and water is particularly preferably used. The content of the dispersion medium in the clay is preferably 30 to 70 parts by mass, more preferably 35 to 65 parts by mass, and even more preferably 40 to 60 parts by mass, relative to 100 parts by mass of the ceramic raw material. When the content of the dispersion medium in the clay is 30 parts by mass or more relative to 100 parts by mass of the ceramic raw material, the advantage that the quality of the honeycomb formed body is easily stabilized is easily obtained. When the content of the dispersion medium in the clay is 70 parts by mass or less relative to 100 parts by mass of the ceramic raw material, the shrinkage amount during drying is small, and deformation can be suppressed. In this specification, the water content of the clay refers to a value measured by a loss on drying method.

[0052] The dispersant may be ethylene glycol, dextrin, fatty acid soap, polyether polyol, etc. The dispersant may be used alone or in combination of two or more. The content of the dispersant in the clay is preferably 0 to 2 parts by mass per 100 parts by mass of the ceramic raw material.

[0053] (2-2. Drying of honeycomb formed body) Next, the honeycomb molded body is dried to obtain a dried honeycomb body. In the drying step, for example, a conventionally known drying method such as hot air drying, microwave drying, dielectric drying, reduced pressure drying, vacuum drying, freeze drying, etc., can be used. Among them, a drying method combining hot air drying with microwave drying or dielectric drying is preferred in that the entire molded body can be dried quickly and uniformly. In addition, a batch type dryer or a continuous type dryer may be used.

[0054] When forming plugging portions, the plugging portions are formed at predetermined positions on the first and second bottom faces of the dried honeycomb formed body, and then the plugging portions are dried. The method for plugging the first and second bottom faces of the honeycomb formed body is not particularly limited, and a known method can be adopted. The material of the plugging portions is not particularly limited, but is preferably ceramics from the viewpoint of strength and heat resistance. As the ceramics, it is preferable that the ceramic material contains at least one selected from the group consisting of cordierite, mullite, zircon, aluminum titanate, silicon carbide, silicon nitride, zirconia, spinel, indialite, sapphirine, corundum, and titania. It is even more preferable that the plugging portions have the same material composition as the main body of the honeycomb formed body, since the expansion coefficient during firing can be made the same, which leads to improved durability.

[0055] (2-3. Firing of dried honeycomb body) After drying the honeycomb formed body, degreasing and firing are performed to manufacture a columnar honeycomb structure. The conditions for the degreasing and firing processes may be known conditions according to the material composition of the honeycomb formed body, and no particular explanation is required, but examples of specific conditions are given below.

[0056] The debinding process will be described. The combustion temperature of the binder is about 200°C, and the combustion temperature of the pore former is about 300 - 1000°C. Therefore, the debinding process can be carried out by heating the honeycomb formed body in the range of about 200 - 1000°C. The heating time is not particularly limited, but is usually about 10 - 100 hours. The honeycomb formed body after the debinding process is called a calcined body.

[0057] The firing process can be carried out, for example, by heating the calcined body to 1350 - 1600°C and holding it for 3 - 10 hours, depending on the material composition of the honeycomb formed body.

[0058] When the honeycomb structure is used as a catalyst carrier, a catalyst can be supported on the partition walls. There is no particular limitation on the method of supporting the catalyst on the porous partition walls, and a known method can be adopted. For example, a method of contacting the porous partition walls with a catalyst composition slurry and then drying and firing can be mentioned. The catalyst composition slurry preferably contains one or a combination of two or more appropriate catalysts according to its use.

Examples

[0059] Examples for better understanding of the present invention and its advantages are illustrated below, but the present invention is not limited to the examples.

[0060] <A. Manufacture of honeycomb structures according to Examples and Comparative Examples> (1) Raw materials As raw materials for cordierite formation, talc, kaolin, alumina, aluminum hydroxide, and silica were prepared. The volume-based cumulative 50% particle diameter (D50) measured by the laser diffraction / scattering method for these is shown in Table 1. As pore formers, acrylic polymer, low-crosslinked starch, medium-crosslinked starch, and high-crosslinked starch were prepared. As the acrylic polymer, polyacrylic acid was used. The low-crosslinked starch, medium-crosslinked starch, and high-crosslinked starch are all starches crosslinked with a phosphoric acid-based crosslinking agent but have different degrees of crosslinking. The volume-based cumulative 50% particle diameter (D50) measured by the laser diffraction / scattering method for these is shown in Table 1. As auxiliaries, a binder, a dispersant, and water were prepared. Methyl cellulose was used as the binder, and ethylene glycol was used as the dispersant.

[0061] (2) Preparation of honeycomb formed body The cordierite-forming raw material, pore-forming material, and auxiliary agent described above were kneaded to form raw material compositions compounded at the mass ratios shown in Table 1 according to the numbers of the examples and comparative examples, thereby forming the green compacts according to the examples and comparative examples, respectively. Table 1 shows the P content with respect to 100 parts by mass of the ceramic raw material in the green compact measured according to the method described above.

[0062] Thereafter, each green compact was put into an extrusion molding machine and extruded through a die of a predetermined shape to obtain a columnar honeycomb formed body. The pressure (extrusion molding pressure) during extrusion molding was measured by a pressure sensor. The results are shown in Table 1. After the obtained honeycomb formed body was dielectrically dried and hot air dried, both bottom surfaces were cut so as to have a predetermined dimension, and further hot air dried under the conditions of 70°C × 2 hours.

[0063] (3) Firing Next, heat degreasing was performed at about 200°C in an air atmosphere, and further firing was performed at 1400°C for 10 hours in an air atmosphere to obtain the honeycomb structures according to the examples and comparative examples. The required number of honeycomb structures for the following tests was manufactured.

[0064] (4) Specifications of honeycomb structure The specifications of the obtained honeycomb structure are as follows. Overall shape: Columnar with a diameter of 100 mm and a height of 100 mm Cell shape in a cross-section perpendicular to the flow path direction of the cell: Square Thickness of partition wall (nominal value based on the die specifications): Described in Table 1 Cell density (number of cells per unit cross-sectional area): Described in Table 1 (cpsi: cells / square inch)

[0065] <B. Characteristic evaluation> Various characteristic evaluations were performed on each of the honeycomb structures according to the examples and comparative examples obtained above.

[0066] (1) Porosity Partition wall samples (cubic shape of length x width x height = about 13 mm x about 13 mm x about 13 mm) of each honeycomb structure were taken from two places, near the center in the radial direction of the center in the height direction and near the outer periphery, and the porosity was measured by mercury intrusion porosimetry, and the average value was taken as the measured value. The results are shown in Table 1.

[0067] (2) Measurement of isostatic fracture strength The isostatic fracture strength of each honeycomb structure was measured based on the automobile standard (JASO M505-87) issued by the Automotive Engineers Association of Japan. The results are shown in Table 1.

[0068] (3) Measurement of P content The P content in each honeycomb structure was measured according to the above-mentioned measuring method, and the results are shown in Table 1.

[0069] [Table 1]

[0070] (4) Discussion All the honeycomb structures according to the examples and comparative examples had thin walls and high porosity. Comparative Examples 1 to 6 were all examples in which only one of acrylic polymer and crosslinked starch was used as the pore-forming material. The strength of the honeycomb structures in Comparative Examples 1 to 4 was insufficient. Comparative Examples 5 and 6, which used highly crosslinked starch, had excellent strength, but the P content was high and the extrusion molding pressure was too high, resulting in a significant decrease in the extrusion speed and an excessive burden on the molding machine. On the other hand, in Examples 1 to 16, by using an acrylic polymer and crosslinked starch in combination as a pore-forming material, it was possible to produce honeycomb structures with thin walls, high porosity, and excellent strength without placing excessive strain on the extrusion molding machine (extrusion molding pressure of 15 MPa or less). [Explanation of symbols]

[0071] 100: Honeycomb structure 102: Outer wall 103: Side 104: First bottom surface 106:Second bottom surface 108: Cell 112: Bulkhead 200: Honeycomb structure 202: Outer wall 203: Side 204: First bottom surface 206: Second bottom surface 208a: First cell 208b: Second cell 209: Plugging part 212: Bulkhead

Claims

1. A honeycomb structure having an outer peripheral side wall and partition walls disposed on an inner peripheral side of the outer peripheral side wall and partitioning a plurality of cells forming a flow path from a first bottom surface to a second bottom surface, The thickness of the partition wall is 50 μm or more and 210 μm or less, The porosity of the partition wall is 45% to 60%, The P content in the honeycomb structure is 0.01 mass% or more and less than 0.2 mass%, The isostatic fracture strength is 1.0 MPa or more. Honeycomb structure.

2. 2. The honeycomb structure according to claim 1, wherein the upper limit of the P content in the honeycomb structure is 0.1 mass % or less.

3. 2. The honeycomb structure according to claim 1, wherein the upper limit of the P content in the honeycomb structure is 0.05 mass % or less.

4. 4. The honeycomb structure according to claim 1, wherein the outer peripheral side wall and the partition walls contain cordierite.

Citation Information

Patent Citations

  • Porous ceramic and its production

    JP1998167856A

  • Method of producing porous ceramic material

    JP2003238271A

  • Ceramics porous body and method for producing the same, and dust collection filter

    JP2020164408A

  • Shear binder agglomerates enabling high porosity in ceramic honeycomb bodies

    US20210155555A1

  • Aluminum titanate ceramic forming batch mixtures and green bodies including PORE former combinations and methods of manufacturing and firing same

    WO2006130759A2