Negative electrode material, electrochemical device, and electronic device

By controlling the distribution of silicon and carbon in the negative electrode material to a specific ratio (R≦0.5), the structural stability and cycle life of lithium ion batteries are improved through uniform stress distribution and efficient lithium desorption.

JP2024144079AActive Publication Date: 2024-10-11AESC JAPAN LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023212565
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2023-12-15
Publication Date
2024-10-11
Estimated Expiration
2043-12-15

AI Technical Summary

Technical Problem

The uneven distribution of silicon and carbon in existing silicon-carbon composite negative electrode materials leads to non-uniform stress distribution, reducing the structural stability and long cycle life of lithium ion batteries.

Method used

The negative electrode material is designed with a controlled distribution of elemental silicon and carbon, where the ratio R of elemental silicon to elemental carbon (R≦0.5) is maintained, ensuring uniform stress distribution and structural stability during charging and discharging processes.

Benefits of technology

This approach enhances the long cycle life of lithium ion batteries by maintaining structural integrity and improving the efficiency of lithium desorption processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144079000001_ABST
    Figure 2024144079000001_ABST
Patent Text Reader

Abstract

To provide a negative electrode material that improves the cycle life of an electrochemical device.SOLUTION: A negative electrode material includes: a carbon layer; and a silicon layer located on at least part of the surface of the carbon layer. Distribution degree R of silicon element to carbon element of the negative electrode material satisfies the relationship of R≤0.5, and R satisfies the following relationships. X1, X2, and Xn are respectively the ratios of the mass of silicon element to the mass of carbon element at the first point, the second point and the n-th point on a straight line, obtained by section-cutting a negative electrode sheet with an argon ion etching instrument through line scan analysis performed with an energy spectrometer, and n is the total number of points on the straight line.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the technical field of secondary batteries, and in particular to negative electrode materials, electrochemical devices and electronic devices. [Background technology]

[0002] Lithium-ion batteries are secondary batteries (rechargeable batteries) that rely mainly on the movement of lithium ions between the positive and negative electrodes. During the charging and discharging process, lithium ions shuttle between the positive and negative electrodes and are inserted or removed. During the charging process, lithium ions are removed from the positive electrode and inserted into the negative electrode through the electrolyte. Under this condition, the negative electrode is in a lithium-excess state, which changes inversely during the discharging process. The advantages of lithium ions include high energy density, high operating voltage, wide operating temperature range, long cycle life, low self-discharge efficiency, excellent safety performance, environmental friendliness, and no memory effect.

[0003] The negative electrode material is the main body that stores lithium ions and is an important part that directly determines the performance of the entire lithium-ion battery. Silicon is a commonly adopted lithium-ion negative electrode material, and its advantages lie in high theoretical capacity, low lithium insertion platform voltage, and abundant reserves. However, the volume expansion rate of silicon is very large. In the initial lithium insertion and desorption process, mechanical stress is often caused by the volume expansion effect, which reduces the contact points between the active material and the conductive agent and binder, causing the active material to fall off the electrode sheet. At the same time, when the SEI film on the surface of the silicon-based active material is destroyed and regrown, it is difficult to form a stable SEI film, and the continuous consumption of the electrolyte and lithium source will form a passivation layer, which will hinder the transport of lithium ions and electrons, making the irreversible capacity too high and the capacity rapidly decreasing. The low electrical conductivity of silicon affects the high-speed charge and discharge performance and rate performance of the battery, and these factors hinder the industrialization of silicon-based materials.

[0004] In order to solve the above technical problems, people have tried to use carbon to compound silicon. In the existing technology, the technology of covering the silicon surface with carbon material is common. For example, the patent document with publication number CN102709566A discloses a spherical silicon-carbon composite anode material for lithium-ion batteries and a manufacturing method thereof, in which silicon accounts for 5%-12%, graphite accounts for 68%-90%, and the rest is carbon material. Publication number CN102709566A adopts a constant temperature mixing technique to prepare a spherical precursor from silicon powder, flake graphite, and a carbon source material, and then the pellet is heat-treated at high temperature to prepare a spherical silicon-carbon composite anode electrode with anisotropically distributed flake / silicon surface carbon material as a core. The spherical silicon-carbon composite anode material has a reversible capacity of more than 480mAh / g, the initial continuous efficiency can reach more than 85%, and the capacity retention rate after 300 cycles is more than 87%. There is also a method of mechanically mixing with carbon materials to prepare silicon-carbon composite materials. For example, the patent document with publication number CN113871604A discloses a silicon-containing mineral-based porous silicon-carbon composite anode material and its manufacturing method. Publication number CN113871604A uses purified silicon-containing mineral samples, nanosilica powder, and carbon-coated silicon monoxide powder as silicon sources, and after solid-phase mixing, spray granulation and low-temperature pyrolysis, controls the HF concentration and reaction time to form micron-sized macropores as the primary buffer structure by etching a portion of SiO2. The introduced low-expansion carbon-coated silicon monoxide serves as the secondary buffer structure. Then, a porous silicon carbon precursor is obtained by thermal reduction of magnesium and pickling of the intermediate product to form mesopores and macropores, which are a three-layer buffer structure. Finally, an organic carbon source is uniformly coated on the surface of the precursor by vacuum impregnation to form a four-level buffer structure, thereby preparing a silicon-containing mineral-based porous silicon-carbon composite anode material with a core-shell structure with quadruple buffer protection. The initial efficiency of the prepared silicon-containing mineral-based porous silicon-carbon composite negative electrode material is 66.7%-70.2%, and the capacity retention rate after 100 cycles at 0.5° C. is 54.6%-68.7%.However, there is room for improvement in the long cycle life of lithium ion secondary batteries using a negative electrode sheet made of a silicon-carbon composite material produced by the above scheme. Summary of the Invention [Problem to be solved by the invention]

[0005] In view of the above, an object of the present invention is to provide a negative electrode material, an electrochemical device, and an electronic device for further improving the long cycle life of an electrochemical device including a negative electrode sheet made of a negative electrode material. [Means for solving the problem]

[0006] The inventors further studied the above scheme and found that the distribution of silicon and carbon in the negative electrode material prepared by the above method is non-uniform, and as a result, the electrochemical device made of the negative electrode sheet will have non-uniform stress distribution during the charge and discharge process, which will result in a decrease in the structural stability of the electrochemical device, and therefore a decrease in the long cycle life of the electrochemical device.

[0007] In order to realize the above solution, the solution of the present invention is as follows.

[0008] In a first aspect, the present invention provides an anode material comprising a carbon layer and a silicon layer overlying at least a portion of a surface of the carbon layer, the anode material satisfying the relationship R≦0.5, where R is the elemental silicon / elemental carbon distribution of the anode material, and R satisfies the following relationship:

number

[0009] During the ceremony,

number

[0010] In the formula, X1, X2 and X nEach of the ratios is the ratio of the mass content of elemental silicon to the mass content of elemental carbon at the first point, the second point, and the nth point on a line obtained by cutting a cross section of a negative electrode sheet made of a negative electrode material with an argon ion etching apparatus and performing line scanning analysis with an energy spectroscopic analyzer, where n is the total number of points on the line.

[0011] In the present invention, the elemental silicon / elemental carbon distribution degree R of the negative electrode material is controlled within a specific range (elemental silicon / elemental carbon distribution degree R≦0.5), thereby ensuring structural stability during the charge / discharge process (specifically, the lithium desorption process) of an electrochemical device comprising a negative electrode sheet made of a negative electrode material, and thereby improving the long cycle life of an electrochemical device comprising a negative electrode sheet made of a composite material.

[0012] In the present invention, when the distribution ratio R of elemental silicon / elemental carbon of the negative electrode material is ≧0.5, the elemental silicon and elemental carbon are distributed non-uniformly. The non-uniform distribution causes non-uniform stress distribution during the charge and discharge process of the electrochemical device composed of the negative electrode sheet made of the negative electrode material. As a result, the structural stability of the electrochemical device is reduced, and the long cycle life of the electrochemical device is reduced.

[0013] In some embodiments, the distribution ratio R of elemental silicon / elemental carbon in the negative electrode material satisfies the relationship R≦0.1.

[0014] In some embodiments, the pressed density of the negative electrode material is 0.5 g / cm 3 ~2.5g / cm 3 It is.

[0015] In some embodiments, the pressed density of the negative electrode material is 0.9 g / cm 3 ~2.5g / cm 3 It is.

[0016] In some embodiments, the specific surface area of ​​the negative electrode material is ≦15 m 2 / g.

[0017] In some embodiments, the specific surface area of ​​the negative electrode material is ≦8 m 2 / g.

[0018] In some embodiments, the silicon layer is comprised of a silicon-based material having a grain size of ≦200 nm. The silicon-based material includes elemental silicon, silicon oxide, or a mixture of both. The silicon oxide includes silicon monoxide, silicon dioxide, or a mixture of both.

[0019] In some embodiments, the carbon layer is comprised of a carbon-based material having a particle size of ≦200 nm, the carbon-based material including at least one of porous carbon, hard carbon, hollow carbon microspheres, and expanded graphite.

[0020] In addition, in the present invention, the manufacturing method of the negative electrode material is not particularly limited. As long as the above-mentioned specific indicators of the prepared negative electrode material are within the corresponding specific selected range, high temperature pyrolysis method, template method (for example, calcium carbonate is used as template), ball mill method, vapor deposition method, hydrothermal synthesis method, freeze-drying method, magnetron sputtering method, electrostatic self-assembly, etc. can be used.

[0021] In the present invention, the method for producing the negative electrode material is not particularly limited. For example, a vapor deposition method may be used.

[0022] In a second aspect, the present invention provides an electrochemical device including a negative electrode sheet. The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector. The negative electrode active material layer includes the negative electrode material described above.

[0023] The method for producing the electrochemical device is not particularly limited.

[0024] In a third aspect, the present invention provides an electronic device comprising an electrochemical device as described above. Effect of the Invention

[0025] As described above, the negative electrode material, electrochemical device, and electronic device of the present invention have the following advantages.

[0026] By controlling the elemental silicon / elemental carbon distribution degree R of the negative electrode material within a specific range (elemental silicon / elemental carbon distribution degree R≦0.5), the present invention can ensure structural stability during the charge / discharge process (specifically, the lithium desorption process) of an electrochemical device comprising a negative electrode sheet made of a negative electrode material, thereby improving the long cycle life of an electrochemical device comprising a negative electrode sheet made of a negative electrode material. [Brief description of the drawings]

[0027] [Figure 1] The structure of the negative electrode material prepared in Example 2. Here, 1 is the carbon layer (i.e., the carbon layer located in the inner layer), 2 is the silicon layer (i.e., the silicon layer located in the inner layer), and 3 is the carbon layer for surface coating. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] The present invention will be further described below with specific examples. However, the specific material ratios, process conditions and results described in the embodiments of the present invention are only used to explain the present invention, and should not be limited thereto. Any equivalent changes or modifications made based on the spirit and essence of the present invention shall be included in the protection scope of the present invention.

[0029] The present invention has a compressed density of 0.5 g / cm 3 ~2.5g / cm 3 and the specific surface area is ≦15m 2 / g. The negative electrode material includes a carbon layer made of a carbon-based material having a particle size of ≦200 nm. A silicon layer is located on at least a portion of a surface of the carbon layer. The silicon layer is made of a silicon-based material having a particle size of ≦200 nm.

[0030] The negative electrode material satisfies the relationship R≦0.5, where R is the elemental silicon / elemental carbon distribution degree of the negative electrode material, and R satisfies the following relationship:

number

[0031]

number

[0032] In the formula, X1, X2 and X n Each of the ratios is the ratio of the mass content of elemental silicon to the mass content of elemental carbon at the first point, the second point, and the nth point on a line obtained by cutting a cross section of a negative electrode sheet made of a negative electrode material with an argon ion etching apparatus and performing line scanning analysis with an energy spectroscopic analyzer, where n is the total number of points on the line.

[0033] Specifically, it indicates the distribution degree R of elemental silicon / elemental carbon in the negative electrode material, and the uniformity of the distribution of elemental silicon and elemental carbon in the negative electrode material. By controlling the distribution degree R of elemental silicon / elemental carbon in the negative electrode material within a specific range (distribution degree R of elemental silicon / elemental carbon≦0.5), it is possible to ensure structural stability in the charge / discharge process (specifically, the lithium desorption process) of an electrochemical device made of a negative electrode sheet made of a negative electrode material, thereby improving the long cycle life of an electrochemical device made of a negative electrode sheet made of a negative electrode material.

[0034] The compressed density of the negative electrode material is within a specific selection range (0.5g / cm 3 ~2.5g / cm 3 ), the skeletal strength of the negative electrode material can be secured, and this can further secure the structural stability during the charge and discharge process (specifically, the lithium desorption process) of the electrochemical device made of the negative electrode sheet made of the negative electrode material, thereby improving the long cycle life of the electrochemical device made of the negative electrode sheet made of the negative electrode material. At the same time, the compressed density of the negative electrode material can be controlled within a specific range (0.5 g / cm 3 ~2.5g / cm 3), it is possible to increase the volumetric energy density of a battery cell of an electrochemical device that includes a negative electrode sheet made of a negative electrode material.

[0035] The specific surface area of ​​the negative electrode material is within a specific range (≦15m 2 By controlling the efficiency within the range of 0.1 to 1.0 μm / g, it is possible to suppress the formation of a film on the surface of the negative electrode material, thereby ensuring the initial efficiency (i.e., efficiency in the first cycle) of an electrochemical device comprising a negative electrode sheet made of a negative electrode material, and therefore improving the cycle life of an electrochemical device comprising a negative electrode sheet made of a negative electrode material.

[0036] In some embodiments, the present invention further provides an electrochemical device comprising a negative electrode sheet, the negative electrode sheet including a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector. The negative electrode active material layer contains the above-mentioned negative electrode material.

[0037] The electrochemical device of the present invention includes any device that undergoes an electrochemical reaction. Specifically, it includes various primary batteries, secondary batteries, fuel cells, solar cells, capacitors, etc. The electrochemical device is a sodium metal battery, and the battery includes at least one of a soft-pack battery, a battery with a square aluminum housing, a battery with a square steel housing, a battery with a cylindrical aluminum housing, and a battery with a cylindrical steel housing.

[0038] In the following, a lithium ion secondary battery will be described as an example.

[0039] In some embodiments, the present invention provides an electronic device comprising the electrochemical device described above.

[0040] The application of the electrochemical device of the present invention is not particularly limited, and the electrochemical device can be used in any electronic device known in the art. In some embodiments, the electrochemical device of the present invention can be used in, but is not limited to, notebook computers, pen-input computers, mobile computers, electronic book players, mobile phones, portable fax machines, portable copy machines, portable printers, head-mounted stereo headphones, video recorders, liquid crystal televisions, portable cleaners, portable CD players, mini discs, transceivers, electronic notepads, calculators, memory cards, portable recorders, radios, backup power sources, motors, automobiles, motorcycles, power-assisted bicycles, bicycles, lighting equipment, toys, game consoles, watches, power tools, flashlights, cameras, large household batteries, energy storage, and sodium ion capacitors.

[0041] The present invention will be described in more detail below with reference to specific examples. It should also be understood that the following examples are only used to specifically explain the present invention and are not to be understood as limiting the scope of protection of the present invention. Any non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention all belong to the scope of protection of the present invention. The specific process parameters in the following examples are merely examples of suitable ranges, and those skilled in the art can select within the appropriate range through the description of this specification, and are not limited to the specific values ​​exemplified below.

[0042] In the present invention, the distribution degree R of elemental silicon and elemental carbon indicates the uniformity of the distribution of elemental silicon and elemental carbon in the negative electrode material, and is specifically tested by the following method. The prepared negative electrode material, polyacrylic acid, and conductive carbon black (SP) are mixed in a mass ratio of 8:1:1, and then the resulting mixture is added with deionized water as a solvent (the mass ratio of deionized water to the negative electrode material is 2:1), and then thoroughly stirred and mixed to obtain a negative electrode slurry. The negative electrode slurry is uniformly applied onto a negative electrode current collector copper foil, and a negative electrode sheet is obtained through drying, cold pressing, and slitting processes. The negative electrode sheet made of the negative electrode material is cross-cut with an argon ion etching device. By performing line scanning analysis with an energy spectroscopic analyzer, the ratio of the mass content of elemental silicon to the mass content of elemental carbon at the first point, second point, and nth point on the line can be obtained. n is the total number of points on the line. Next, the distribution degree R of elemental silicon / elemental carbon in the negative electrode material is calculated according to the following formula.

number

[0043] During the ceremony,

number

[0044] In the formula, X1, X2 and X n Each of the ratios is the ratio of the mass content of elemental silicon to the mass content of elemental carbon at the first point, the second point, and the nth point on a line obtained by cutting a cross section of a negative electrode sheet made of a negative electrode material with an argon ion etching apparatus and performing line scanning analysis with an energy spectroscopic analyzer, where n is the total number of points on the line.

[0045] In the present invention, the pressed density is tested according to "GB / T 24533-2019 Graphite negative electrode material for lithium ion batteries".

[0046] In the present invention, the specific surface area is tested according to the dynamic chromatography method of "GB / T 39713-2020 Test of the specific surface area of ​​ceramic powder-BET gas adsorption procedure".

[0047] In the present invention, the test steps for the initial efficiency and cycle life are as follows:

[0048] (1) Preparation of positive electrode sheet: Positive electrode material NCM811 (i.e., LiNi 0.8 Co 0.1 Mn 0.1 O2), conductive agent Super P (i.e., highly conductive carbon black), and polyvinylidene fluoride (PVDF) as a binder were mixed according to a weight ratio of 97:1.5:1.5 to obtain a mixture. N-methylpyrrolidone (i.e., NMP) as a solvent was added to the mixture. The mass ratio of NMP to the positive electrode material NCM811 was 1:1, and the mixture was thoroughly stirred and mixed to obtain a positive electrode slurry. The positive electrode slurry was applied onto a positive electrode current collector aluminum foil, and a positive electrode sheet was obtained through processes such as drying, cold pressing, and slitting.

[0049] (2) Preparation of negative electrode sheet: The sample, polyacrylic acid, and conductive carbon black (SP) were mixed in a mass ratio of 8:1:1, and then deionized water was added to the resulting mixture. The mass ratio of deionized water to the sample was 2:1, and the mixture was thoroughly stirred and mixed to obtain a negative electrode slurry. The negative electrode slurry was uniformly applied onto a negative electrode current collector copper foil, and the negative electrode sheet was obtained through processes such as drying, cold pressing, and slitting.

[0050] (3) Preparation of electrolyte:

[0051] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1:1 to obtain a mixed solvent. Then, lithium hexafluorophosphate (LiPF6) that had been thoroughly dried was dissolved in the mixed solvent to prepare an electrolyte solution with a concentration of 1 mol / L.

[0052] (4) Preparation of separator:

[0053] The separator used was a polyethylene (PE) porous film with a thickness of 11 μm, an air permeability of 280 s / 100 mL, and a porosity of 40%.

[0054] (5) Preparation of lithium-ion secondary battery:

[0055] The prepared positive electrode sheet, separator, and negative electrode sheet were stacked in order with the separator between the positive electrode sheet and the negative electrode sheet, and then separated. Next, the sheet was wrapped in an aluminum plastic film, dried, and then the electrolyte prepared above was poured in. After going through processes such as sealing, leaving, and chemical formation, a 3020-type button battery, which is a lithium-ion secondary battery, was assembled as the final product.

[0056] The initial efficiency and cycle performance of each of the fabricated lithium ion secondary batteries were tested. The specific steps are as follows: Cycles were performed with a charge-discharge program of charging at 0.1C to 1.5C and discharging at 0.1C to 5mV, and the initial efficiency and cycle performance were tested.

[0057] The initial efficiency was calculated according to the following formulas: initial efficiency = charge gram capacity at 1st cycle / discharge gram capacity at 1st cycle × 100%, charge gram capacity at 1st cycle = charge capacity at 1st cycle / (mass of negative electrode sheet × 0.8), discharge gram capacity at 1st cycle = discharge capacity at 1st cycle / (mass of negative electrode sheet × 0.8).

[0058] The cycle performance is as follows: When cycled to 80% SOH, the corresponding number of cycles is the cycle performance. 80% SOH is defined as: When the discharge capacity of the battery divided by the discharge capacity of the first cycle is 80%, the corresponding number of cycles is the cycle performance of the battery cell.

[0059] Example 1

[0060] This embodiment provides a method for producing a negative electrode material, the specific steps are as follows:

[0061] Step S1. Carbon and silicon were alternately deposited by vapor deposition. Specifically, in a sealed chamber under a protective gas (nitrogen) atmosphere, first, carbon source methane was introduced into the sealed chamber and heated until the atmospheric temperature in the sealed chamber reached 850°C. The carbon deposition temperature was 850°C, the carbon deposition time was 10 minutes, the nitrogen flow rate was 20 L / min, and the methane flow rate was 10 L / min, so the carbon deposition rate was 10 nm / min, and the unit size of carbon deposited in one step was 100 nm. Next, silane was introduced into the sealed chamber, the silicon deposition time was 2 minutes, and the silane flow rate was 5 L / min, so the ratio of the carbon deposition rate to the silicon deposition rate was 5:1, and the particle size of silicon deposited in one step was 4 nm (particle size of silicon deposited in one step = carbon deposition rate / (ratio of carbon deposition rate to silicon deposition rate) x silicon deposition time). The particle size of the carbon deposited in one step is 100 nm (particle size of the carbon deposited in one step = deposition rate of carbon x deposition time of carbon). In this manner, the alternate deposition process is performed, and the deposition rate and time are not changed during the alternate deposition process, and product A can be obtained.

[0062] Step S2: The product A obtained in step S1 is coarsely crushed, then crushed and classified by an airflow crusher. During the airflow crushing and classification process, the spindle speed is 3000 rpm, the output is 1000 W, and the compressor capacity is 20 m 3 / min, and product B having a D50 of 6 μm can be obtained.

[0063] Step S3: Product C is produced from product B obtained in step S2 using a liquid phase method. Specifically, product B is mixed with the carbon source glucose soluble matter in a mass ratio of 1:1, and then the mixture is heated to 60°C and reacted in a water bath at 60°C for 12 hours to crosslink the surface of product 2 with the carbon source. After washing, the product is vacuum dried at 100°C for 48 hours to obtain product C.

[0064] Step S4: Product 3 is pyrolyzed and carbonized at a temperature of 950° C. The pyrolysis and carbonization time is 4 hours, and a surface carbon layer is deposited and grown on the surface of Product C. The thickness of the surface carbon layer can be controlled within 30 nm to obtain a negative electrode material.

[0065] Example 2

[0066] A negative electrode material was prepared in the same manner as in Example 1 except for the following conditions.

[0067] Step S1. Carbon and silicon were alternately deposited by the deposition method. Specifically, in a sealed chamber under a protective gas (nitrogen) atmosphere, first, carbon source methane was introduced into the sealed chamber and heated until the atmospheric temperature in the sealed chamber reached 850°C. The carbon deposition temperature was 850°C, the carbon deposition time was 10 minutes, the nitrogen flow rate was 20 L / min, and the methane flow rate was 10 L / min, so the carbon deposition rate was 10 nm / min, and the unit size of carbon deposited in one step was 100 nm. Next, silane was introduced into the sealed chamber, the silicon deposition time was 2 minutes, and the silane flow rate was 12.5 L / min, so the ratio of the carbon deposition rate to the silicon deposition rate was 2:1, and the particle size of silicon deposited in one step was 10 nm (particle size of silicon deposited in one step = carbon deposition rate x carbon deposition rate / (ratio of carbon deposition rate to silicon deposition rate) x silicon deposition time). The particle size of the carbon deposited in one step is 100 nm (particle size of carbon deposited in one step = deposition rate of carbon x deposition time of carbon). In this manner, the alternate deposition process is performed, and the deposition rate and time are not changed during the alternate deposition process, and product A can be obtained.

[0068] The negative electrode material produced in this embodiment is shown in Figure 1. Here, 1 is the carbon layer, 2 is the silicon layer, and 3 is the surface-coating carbon layer.

[0069] Example 3

[0070] A negative electrode material was prepared in the same manner as in Example 1 except for the following conditions.

[0071] Step S1. Carbon and silicon were alternately deposited by the deposition method. Specifically, in a sealed chamber under a protective gas (nitrogen) atmosphere, first, the carbon source methane was introduced into the sealed chamber and heated until the atmospheric temperature in the sealed chamber reached 850°C. The carbon deposition temperature was 850°C, the carbon deposition time was 10 minutes, the nitrogen flow rate was 20L / min, and the methane flow rate was 10L / min, so the carbon deposition rate was 10nm / min, and the unit size of carbon deposited in one step was 100nm. Next, silane was introduced into the sealed chamber, the silicon deposition time was 2 minutes, and the silane flow rate was 25L / min, so the ratio of the carbon deposition rate to the silicon deposition rate was 1:1, and the particle size of silicon deposited in one step was 20nm (particle size of silicon deposited in one step = carbon deposition rate / (ratio of carbon deposition rate to silicon deposition rate) x silicon deposition time). The particle size of the carbon deposited in one step is 100 nm (particle size of carbon deposited in one step = deposition rate of carbon x deposition time of carbon). In this manner, the alternate deposition process is performed, and the deposition rate and time are not changed during the alternate deposition process, and product A can be obtained.

[0072] Example 4

[0073] A negative electrode material was prepared in the same manner as in Example 1 except for the following conditions.

[0074] Step S4: The product 3 is pyrolyzed and carbonized at a temperature of 700° C. The pyrolysis and carbonization time is 4 hours, and a surface carbon layer is deposited and grown on the surface of the product 3. The thickness of the surface carbon layer can be controlled within 2 nm to obtain a negative electrode material.

[0075] Comparative Example 1

[0076] This comparative example provides a method for producing a negative electrode material. The specific steps are as follows:

[0077] Step S1. Carbon was produced by the vapor deposition method. Specifically, in a sealed chamber with a protective gas atmosphere (nitrogen; doped with 2% ammonia gas by weight), carbon source methane is introduced into the sealed chamber, and the carbon source methane is introduced into the sealed chamber and heated until the atmospheric temperature in the sealed chamber reaches 850°C. The carbon deposition temperature is 850°C, the carbon deposition time is 3 hours, the nitrogen (ammonia gas doped, ammonia doping amount 2% by weight) flow rate is 20L / min, the flow rate is 20L / min, and the methane flow rate is 60L / min, so the carbon deposition rate is 60nm / min, and carbon element A1 can be obtained.

[0078] Silicon was prepared by the deposition method. Specifically, in a sealed chamber with a protective gas atmosphere (nitrogen; doped with 2 wt% ammonia gas), the carbon source methane was introduced into the sealed chamber and heated until the atmospheric temperature in the sealed chamber reached 850 ° C. Silicon was deposited at a temperature of 850 ° C for 3 hours, the flow rate of silane was 50 L / min, and the deposition rate of silicon was 100 nm / min, and elemental silicon A2 could be obtained.

[0079] Step S2: The silicon element A2 and carbon element A1 obtained in step S1 are coarsely crushed, then crushed and classified by an airflow crusher. During the airflow crushing and classification process, the spindle speed is 3000 rpm, the output is 1000 W, and the compressor capacity is 20 m 3 / min, and elemental silicon with a D50 of 6 μm and elemental carbon with a D50 of 6 μm can be obtained.

[0080] Step S3. The elemental silicon having a D50 of 6 μm and the elemental carbon having a D50 of 6 μm obtained in step S2 are mechanically mixed according to a mass ratio of 1:1.

[0081] Step S4. The mixture is pyrolyzed and carbonized at a temperature of 950° C. The pyrolysis and carbonization time is 4 hours to deposit and grow a surface carbon layer on the surface of the product 3. The thickness of the surface carbon layer can be controlled within 30 nm to obtain a negative electrode material.

[0082] Comparative Example 2

[0083] A negative electrode material was prepared in the same manner as in Example 1 except for the following conditions.

[0084] Step S1. Carbon and silicon were alternately deposited by the deposition method. Specifically, in a sealed chamber under a protective gas (nitrogen) atmosphere, first, the carbon source methane was introduced into the sealed chamber and heated until the atmospheric temperature in the sealed chamber reached 850°C. The carbon deposition temperature was 850°C, the carbon deposition time was 10 minutes, and the methane and gas flow rates were 10L / min, so the carbon deposition rate was 10nm / min, and the unit size of carbon deposited in one step was 100nm. Next, silane was introduced into the sealed chamber, the silicon deposition time was 2 minutes, the nitrogen flow rate was 20L / min, and the silane flow rate was 5L / min, so the ratio of the carbon deposition rate to the silicon deposition rate was 5:1, and the particle size of silicon deposited in one step was 4nm (particle size of silicon deposited in one step = carbon deposition rate / (ratio of carbon deposition rate to silicon deposition rate) x silicon deposition time). The particle size of the carbon deposited in one step is 100 nm (particle size of carbon deposited in one step = deposition rate of carbon x deposition time of carbon). In this manner, the alternate deposition process is performed, and the deposition rate and time are not changed during the alternate deposition process, and product A can be obtained.

[0085] During the deposition process, ammonium polyphosphate is added to the closed chamber at a rate of 0.1 mg / min.

[0086] Comparative Example 3

[0087] A negative electrode material was prepared in the same manner as in Example 1 except for the following conditions.

[0088] Step S1. Carbon and silicon were alternately deposited by the deposition method. Specifically, in a sealed chamber under a protective gas (nitrogen) atmosphere, first, carbon source methane was introduced into the sealed chamber and heated until the atmospheric temperature in the sealed chamber reached 850°C. The carbon deposition temperature was 850°C, the carbon deposition time was 10 minutes, the nitrogen flow rate was 20 L / min, and the methane flow rate was 10 L / min, so the carbon deposition rate was 10 nm / min, and the unit size of carbon deposited in one step was 100 nm. Next, silane was introduced into the sealed chamber, and the silicon deposition time was 2 minutes, the nitrogen flow rate was 20 L / min, and the silane flow rate was 5 L / min, so the ratio of the carbon deposition rate to the silicon deposition rate was 5:1, and the particle size of silicon deposited in one step was 4 nm (particle size of silicon deposited in one step = carbon deposition rate / (ratio of carbon deposition rate to silicon deposition rate) x silicon deposition time). The particle size of the carbon deposited in one step is 100 nm (particle size of carbon deposited in one step = deposition rate of carbon x deposition time of carbon). In this manner, the alternate deposition process is performed, and the deposition rate and time are not changed during the alternate deposition process, and product A can be obtained.

[0089] During the deposition process, the amount of ammonium polyphosphate added to the closed chamber is 0.5 mg / min.

[0090] Comparative Example 4

[0091] In this comparative example, a method for producing a negative electrode material is provided. The specific steps are as follows:

[0092] Step S1. Carbon and silicon were alternately deposited by the deposition method. Specifically, in a sealed chamber under a protective gas (nitrogen) atmosphere, first, the carbon source methane was introduced into the sealed chamber and heated until the atmospheric temperature in the sealed chamber reached 850°C. The carbon deposition temperature was 850°C, the carbon deposition time was 10 minutes, the nitrogen flow rate was 20 L / min, and the methane flow rate was 10 L / min, so the carbon deposition rate was 10 nm / min, and the unit size of carbon deposited in one step was 100 nm. Next, silane was introduced into the sealed chamber, the silicon deposition time was 10 minutes, and the silane flow rate was 100 L / min, so the ratio of the carbon deposition rate to the silicon deposition rate was 1:4, and the particle size of silicon deposited in one step was 400 nm (particle size of silicon deposited in one step = carbon deposition rate / (ratio of carbon deposition rate to silicon deposition rate) x silicon deposition time). The particle size of the carbon deposited in one step is 100 nm (particle size of carbon deposited in one step = deposition rate of carbon x deposition time of carbon). In this manner, the alternate deposition process is performed, and the deposition rate and time are not changed during the alternate deposition process, and product A can be obtained.

[0093] Comparative Example 5

[0094] A negative electrode material was prepared in the same manner as in Example 1 except for the following conditions.

[0095] Step S1: Carbon and silicon were alternately deposited by vapor deposition. Specifically, in a sealed chamber under a protective gas (nitrogen) atmosphere, first, the carbon source methane was introduced into the sealed chamber and heated until the atmospheric temperature in the sealed chamber reached 850°C. The carbon deposition temperature was 850°C, the carbon deposition time was 20 minutes, the carbon deposition time was 20 L / min, and the methane flow rate was 20 L / min, so the carbon deposition rate was 20 nm / min, and the unit size of carbon deposited at one time was 100 nm. Next, silane is introduced into the sealed chamber, and the deposition time of silicon is 2 minutes and the flow rate of silane is 5 L / min. Therefore, the ratio of the deposition rate of carbon to that of silicon is 5:1 and the particle diameter of silicon deposited in one step is 4 nm (particle diameter of silicon deposited in one step = (carbon deposition rate / (ratio of carbon deposition rate to silicon deposition rate) x silicon deposition time). The particle diameter of carbon deposited in one step is 400 nm (particle diameter of carbon deposited in one step = carbon deposition rate x carbon deposition time). In this way, the alternating deposition process is performed, and the deposition rate and time are not changed during the alternating deposition process, and product A can be obtained.

[0096] test

[0097] The distribution of elemental silicon / elemental carbon, compressed density, specific surface area, initial efficiency, and cycle life were tested for the negative electrode materials produced in Examples 1 to 4 and Comparative Examples 1 to 5. The test results are shown in Table 1. Test results

[0098] [Table 1]

[0099] As can be seen from Table 1, the initial efficiency of the lithium ion secondary battery comprising the negative electrode sheet made of the negative electrode material of Examples 1 to 4 is ≧87.1%, and the cycle life is ≧600. This result shows that the lithium ion secondary battery comprising the negative electrode sheet made of the negative electrode material of the present invention has excellent long cycle life performance.

[0100] From Table 1, it can be seen that the elemental silicon / elemental carbon distribution degree R of the negative electrode material of Comparative Example 1 is ≧0.5 (specifically, 0.6), and the cycle life of the lithium ion secondary battery made of the negative electrode sheet made of the negative electrode material is only 320 cycles. The elemental silicon / elemental carbon distribution degree R of the negative electrode materials of Examples 1 to 4 is <0.5, and the cycle life of the lithium ion secondary battery made of the negative electrode sheet made of the negative electrode material is 600 to 1000 cycles. This result shows that by controlling the elemental silicon / elemental carbon distribution degree R of the negative electrode material to a specific range (elemental silicon / elemental carbon distribution degree R≦0.5), it is possible to ensure structural stability in the charge / discharge process (specifically, lithium desorption / insertion process) of the lithium ion secondary battery made of the negative electrode sheet made of the negative electrode material, thereby improving the long cycle life of the lithium ion secondary battery made of the negative electrode sheet made of the negative electrode material.

[0101] From Table 1, the compressed density of the negative electrode material of Comparative Example 2 is 0.5 g / cm 3 Less than (specifically 0.3 g / cm 3 ) and it can be seen that the cycle life of a lithium ion secondary battery made of a negative electrode sheet made of the negative electrode material is only 330 cycles. The compressed density of the negative electrode materials of Examples 1 to 4 is 1.3 g / cm 3 ~1.5g / cm 3 The cycle life of a lithium ion secondary battery made of a negative electrode sheet made of the negative electrode material is 600 to 1000 cycles. This result is obtained when the compressed density of the negative electrode material is within a specific selected range (0.5 g / cm 3 ~2.5g / cm 3 ), it is possible to ensure the skeletal strength of the negative electrode material, which in turn makes it possible to better ensure the structural stability during the charge and discharge process (specifically, the lithium desorption process) of a lithium ion secondary battery made of a negative electrode sheet made of the negative electrode material, thereby improving the long cycle life of a lithium ion secondary battery made of a negative electrode sheet made of the negative electrode material.

[0102] From Table 1, the specific surface area of ​​the negative electrode materials of Comparative Example 3 and Comparative Example 5 is ≧15 m2 / g (specifically, 25.1m 2 / g and 20.2m 2 / g), and it can be seen that the cycle life of the lithium ion secondary battery comprising the negative electrode sheet made of the negative electrode material was 230 cycles and 480 cycles, respectively. In comparison, the specific surface area of ​​the negative electrode materials of Examples 1 to 4 was all <15 m 2 / g, and the cycle life of a lithium ion secondary battery made of a negative electrode sheet made of the negative electrode material is 600 to 1000 cycles. This result is obtained when the specific surface area of ​​the negative electrode material is within a specific selection range (≦15 m 2 / g), it is possible to suppress the formation of a film on the surface of the negative electrode material, thereby ensuring the initial efficiency (i.e., initial Coulombic efficiency) of a lithium-ion secondary battery made of a negative electrode sheet made of a negative electrode, and thereby improving the long cycle life of a lithium-ion secondary battery made of a negative electrode sheet made of a negative electrode material.

[0103] The above-mentioned embodiment is illustrative of the principle and effect of the present invention, but is not intended to limit the present invention. Anyone with ordinary skill in the art can modify or change the above-mentioned embodiment without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or changes made by a person with ordinary skill in the art without departing from the spirit and technical idea disclosed in the present invention are still intended to be included in the scope of the claims of the present invention. [Industrial Applicability]

[0104] The negative electrode material provided by the present invention can be applied to lithium ion batteries. [Explanation of symbols]

[0105] 1: Carbon layer 2: Silicon layer 3: Carbon layer for surface coating

Claims

1. 1. An anode material comprising: a carbon layer; and a silicon layer located on at least a portion of a surface of the carbon layer, wherein the anode material satisfies the relationship R≦0.5, where R is a distribution degree of elemental silicon / elemental carbon in the anode material, and R satisfies the relationship: [0010] During the ceremony, [0025] X 1 , X 2 and X n are the ratios of the mass content of the elemental silicon to the mass content of the elemental carbon at a first point, a second point, and an n-th point on a line obtained by cutting a cross section of a negative electrode sheet made of the negative electrode material with an argon ion etching apparatus and performing line scanning analysis with an energy spectroscopic analysis apparatus, respectively, where n is the total number of points on the line.

2. 2. The negative electrode material according to claim 1, wherein the distribution ratio R of elemental silicon / elemental carbon in the negative electrode material satisfies the relationship R≦0.

1.

3. The compressed density of the negative electrode material is 0.5 g / cm 3 ~2.5g / cm 3 The negative electrode material according to claim 1 ,

4. The compressed density of the negative electrode material is 0.9 g / cm 3 ~2.5g / cm 3 The negative electrode material according to claim 3 ,

5. The specific surface area of ​​the negative electrode material is ≦15 m 2 / g.

6. The specific surface area of ​​the negative electrode material is ≦8 m 2 / g.

7. 2. The negative electrode material of claim 1, wherein the silicon layer is made of a silicon-based material having a particle size of ≦200 nm.

8. 2. The negative electrode material of claim 1, wherein the carbon layer is made of a carbon-based material having a particle size of ≦200 nm.

9. An electrochemical device including a negative electrode sheet, The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector, and the negative electrode active material layer includes the negative electrode material according to any one of claims 1 to 8. An electrochemical device.

10. An electronic device comprising the electrochemical device according to claim 9.

Citation Information

Patent Citations

  • Spherical silicon carbon composite anode material of lithium ion battery and preparation method for spherical silicon carbon composite anode material

    CN102709566A

  • Silicon-based composite and preparation method thereof and lithium ion battery with silicon-based composite

    CN106159229A

  • Silicon-carbon anode material for lithium ion battery and preparation method thereof

    CN108288705A

  • Silicon-carbon anode material for lithium ion battery and preparation method thereof

    CN110400930A

  • Silicon-containing mineral-based porous silicon-carbon composite negative electrode material and preparation method thereof

    CN113871604A