Organometallic complex, catalyst for polymerization, method for producing olefin polymer and method for producing olefin-cyclic olefin copolymer
A novel organometallic complex with specific metal and ligand structures addresses the inefficiencies of conventional catalysts by enhancing polymerization activity and copolymerizability, facilitating efficient production of olefin and olefin/cyclic olefin copolymers with improved stability and reduced energy use.
Patent Information
- Application Number
- JP2023215858
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2023-12-21
- Publication Date
- 2024-10-11
AI Technical Summary
Conventional organometallic complexes exhibit limitations in polymerization activity, molecular weight of copolymers, and copolymerizability with cyclic olefins, particularly when producing olefin and olefin/cyclic olefin copolymers, leading to inefficiencies and environmental concerns due to unreacted comonomer recovery.
A novel organometallic complex represented by specific formulas, featuring a titanium, zirconium, or hafnium atom with specific ligand structures, which enhances polymerization activity and copolymerizability by allowing easier access and stability during monomer insertion, even at high temperatures.
The novel organometallic complex demonstrates superior polymerization activity and copolymerizability, enabling efficient production of olefin and olefin/cyclic olefin copolymers with improved stability and reduced energy consumption for comonomer recovery.
Smart Images

Figure 2024144088000001 
Figure 2024144088000002 
Figure 2024144088000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an organometallic complex, a polymerization catalyst, a method for producing an olefin polymer, and a method for producing an olefin-cyclic olefin copolymer. [Background technology]
[0002] Conventionally, catalysts comprising a metallocene compound and a cocatalyst such as an organoaluminum oxy compound or a borate have been known as catalysts for producing olefin polymers such as ethylene and ethylene-α-olefin copolymers. Among these, metallocene complexes in which one cyclopentadienyl group is coordinated to a metal are called half-metallocene complexes, and it has been reported that they can be used to obtain copolymers of ethylene and α-olefins by taking advantage of their excellent copolymerizability with α-olefins (see, for example, Patent Documents 1 to 3).
[0003] When using a comonomer with a high boiling point, the copolymerizability of the comonomer is particularly important. For example, if a large amount of unreacted comonomer remains in the polymerization vessel, a large amount of energy is required to recover the comonomer, which can be problematic in terms of economy and environmental load. Among copolymers, polymers having ethylene and cyclic olefin monomers in the molecular chain have excellent optical properties and are used for optical lens applications, and are a development field that is being vigorously researched. On the other hand, when producing such polymers by coordination polymerization, the catalyst is required to have high copolymerizability that can efficiently polymerize cyclic olefins, and there are currently only a limited number of reports of such catalysts (see, for example, Patent Document 4 and Non-Patent Documents 1 to 3). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] European Patent No. 0416815 [Patent Document 2] International Publication No. 2003 / 024983 [Patent Document 3] Special Publication No. 2008-527050 [Patent Document 4] Patent No. 7175426 [Non-patent literature]
[0005] [Non-Patent Document 1] Organometallics, 2016, 35, 1895-1905 [Non-Patent Document 2] Polym. Chem. 2021, 12, 4372. [Non-Patent Document 3] Coord.Chem. Rev. 2006, 250, 212-241 Summary of the Invention [Problem to be solved by the invention]
[0006] Conventional organometallic complexes have room for further improvement in the production of olefins and olefin-cyclic olefin copolymers in terms of polymerization activity, molecular weight of the resulting copolymers, and copolymerizability with cyclic olefins.
[0007] The problem to be solved by one embodiment of the present invention is to provide a novel organometallic complex. Also, the problem to be solved by one embodiment of the present invention is to provide a polymerization catalyst containing the novel organometallic complex, and a method for producing an olefin polymer and a method for producing an olefin-cyclic olefin copolymer using the polymerization catalyst. [Means for solving the problem]
[0008] Means for solving the above problems include the following aspects. <1> An organometallic complex (A) represented by the following formula (1):
[0009] [ka]
[0010] In formula (1), M represents a titanium atom, a zirconium atom, or a hafnium atom; X's each independently represent a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a diene-based divalent derivative group; Y is a carbon atom or a silicon atom; R 1 ~R 7 and R 51 ~R 54 each independently represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group, R 1 ~R 7 and R 51 ~R 54 Two or more of these groups may be bonded to each other to form a ring structure.
[0011] <2> In the formula (1), R 1 ~R 7 In the above, two groups bonded to adjacent ring members are bonded to each other to form a ring structure. <1> The organometallic complex (A) according to the above. <3> In the formula (1), R 3 ~R 6 In the above, two groups bonded to adjacent ring members are bonded to each other to form a ring structure. <1> or <2> The organometallic complex (A) according to the above. <4> The formula (1) is represented by the following formula (2): <1> ~ <3> The organometallic complex (A) according to any one of the above.
[0012] [ka]
[0013] In formula (2), M is a titanium atom, a zirconium atom, or a hafnium atom; X's each independently represent a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a diene-based divalent derivative group; Y is a carbon atom or a silicon atom; R 1 , R 2 , R 7 and R 51 ~R 54 each independently represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group; R 55 ~R 58 each independently represents a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group; R 1 , R 2 , R 7 and R 55 ~R 58 Two or more groups selected from the following may be bonded to each other to form a ring structure. 51 ~R 54 Two or more of these groups may be bonded to each other to form a ring structure. <5> The formula (1) is represented by the following formula (3): <1> ~ <4> The organometallic complex (A) according to any one of the above.
[0014] [ka]
[0015] In formula (3), M is a titanium atom, a zirconium atom, or a hafnium atom; each X is independently a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a diene-based divalent derivative group; R 5 ~R 7 and R 51 ~R 54each independently represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group, R 5 ~R 7 and R 51 ~R 54 Two or more of the groups may be bonded to each other to form a ring structure, Ar represents an aromatic ring, R Ar each independently represents a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group, and n represents an integer from 0 to the maximum number of substituents on Ar minus 2. <6> In the formula (1) or (3), R 5 and R 6 and R 7 and the ring structure formed by bonding with each other is a pyrrole ring or an indole ring. <1> ~ <5> The organometallic complex (A) according to any one of the above. <7> In the formula (1) or (2), R 7 is an aryl group or a substituted aryl group; <1> ~ <4> The organometallic complex (A) according to any one of the above. <8> In the formula (1) or (2), M is a titanium atom. <1> ~ <4> The organometallic complex (A) according to any one of the above. <9> In the formula (1) or (2), R 51 ~R 54 is a hydrogen atom <1> ~ <4> The organometallic complex (A) according to any one of the above. <10> In the formula (1) or (2), R 51 ~R 54 is a hydrogen atom, M is a titanium atom, and R 7 is an aryl group or a substituted aryl group; <1> ~ <4> The organometallic complex (A) according to any one of the above. <11> The formula (1) is represented by the following formula (4): <1> ~ <10> The organometallic complex (A) according to any one of the above.
[0016] [ka]
[0017] In formula (4), M is a titanium atom; X's each independently represent a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a diene-based divalent derivative group; Y is a carbon atom or a silicon atom; R 1 and R 2 each independently represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group; R 55 ~R 58 and R 59 ~R 63 each independently represents a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group; R 55 ~R 58 Two or more groups selected from the group consisting of may be bonded to each other to form a ring structure, and R 59 ~R 63 Two or more groups selected from the above may be bonded to each other to form a ring structure.
[0018] <12> <1> ~ <11> An organometallic complex (A) according to any one of the above items (1) to (4), A polymerization catalyst comprising at least one compound (B) selected from the group consisting of an organometallic compound (B-1), an organoaluminum oxy compound (B-2), and a compound (B-3) that reacts with the organometallic complex (A) to form an ion pair. <13> <12> 13. A process for producing an olefin polymer, comprising polymerizing an olefin in the presence of the polymerization catalyst according to claim 12. <14> <12> A method for producing an olefin-cyclic olefin copolymer, comprising copolymerizing an olefin with a cyclic olefin compound in the presence of the polymerization catalyst according to claim 1. Effect of the Invention
[0019] According to one embodiment of the present invention, there is provided a novel organometallic complex. Also, according to one embodiment of the present invention, there are provided a polymerization catalyst containing the novel organometallic complex, and a method for producing an olefin polymer and a method for producing an olefin-cyclic olefin copolymer using the polymerization catalyst. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The present invention will be described in detail below. The following description of the components may be based on a representative embodiment of the present invention, but the present invention is not limited to such an embodiment. In this specification, the term "polymer" is a concept including homopolymers and copolymers. In this specification, the use of "to" indicating a numerical range means that the numerical values before and after it are included as the lower limit and upper limit. In this specification, the use of "to" indicating a numerical range means that the units written before or after it indicate the same units, unless otherwise specified. As used herein, a combination of two or more preferred embodiments is a more preferred embodiment. The present invention will now be described in further detail.
[0021] (Organometallic Complex (A)) The organometallic complex (A) according to the present invention is a novel compound represented by the following formula (1). When the organometallic complex (A) is used as a polymerization catalyst, it can exhibit excellent polymerization activity. Although the reason for this is not clear, the following mechanism is presumed. For example, when ethylene is polymerized with a bulky monomer, a complex having a wide space around the central metal (such as in the comparative example) is used, and the bulky monomer can easily approach, so that better polymerization activity and copolymerizability can be expected. On the other hand, when considering the polymerization mechanism, when the bulky monomer approaches the central metal at the moment of polymerization, the catalyst structure is slightly distorted from the stable structure (to avoid steric repulsion of the approaching monomer with the ligand), which enables polymerization. From the viewpoint of the ease of distortion of the complex, the organometallic complex (A) according to the present invention is a structure in which the ring structure consisting of a cyclopentadienyl group, a metal atom, a nitrogen atom, and a carbon atom has a six-membered ring, and therefore, it is considered to have a structure with less distortion than, for example, a complex having a wide space around the central metal shown in the comparative example described later. Therefore, at first glance, the coordination space of organometallic complex (A) appears to be narrower than that of complexes that have a wider space around the central metal. However, from the viewpoint of the ease of strain of the catalyst, the catalyst is more likely to be strained during monomer insertion (compared to complexes that have a larger strain to begin with), and as a result, the monomer can more easily approach the catalyst. This is thought to result in superior polymerization activity, for example, copolymerization ability between olefins and cyclic olefins. In addition, it is presumed that the structural stability of the organometallic complex (A) according to the present invention as described above contributes to the stability of the catalyst at high temperatures. Therefore, when the organometallic complex (A) is used as a catalyst, the catalyst has excellent stability and polymerization activity even under temperature conditions of, for example, 75°C or higher, and also has excellent polymerizability of bulky monomers. The organometallic complex (A) will be described in detail below.
[0022] The organometallic complex (A) according to the present invention is represented by the following formula (1).
[0023] [ka]
[0024] In formula (1), M is a titanium atom, a zirconium atom, or a hafnium atom; X's each independently represent a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a diene-based divalent derivative group; Y is a carbon atom or a silicon atom; R 1 ~R 7 and R 51 ~R 54 each independently represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group, R 1 ~R 7 and R 51 ~R 54 Two or more of these groups may be bonded to each other to form a ring structure.
[0025] <m> The above M is a titanium atom, a zirconium atom, or a hafnium atom. From the viewpoint of exhibiting excellent polymerization activity in the copolymerization of ethylene and a cyclic olefin when used as a catalyst, M is preferably a titanium atom.
[0026] In the organometallic complex (A) according to the present invention, the above-mentioned excellent polymerization activity can be obtained regardless of whether a titanium atom, a zirconium atom, or a hafnium atom is used. However, when comparing the complex structures having each of the above-mentioned metal atoms, it is presumed that there are slight structural differences depending on the type of central metal atom. For example, since titanium, zirconium, and hafnium atoms have different ionic radii, it is assumed that the bond distance between the nitrogen atom and the metal atom in the organometallic complex (A) and the bond distance between the cyclopentadienyl group and the metal atom will differ depending on the type of metal element contained in the organometallic complex (A). In particular, since titanium atoms have a smaller ionic radius than zirconium and hafnium atoms, the bond distances between the nitrogen atom and the cyclopentadienyl group and the titanium atom will be smaller than those of zirconium and hafnium atoms, and it is believed that the space around the central metal atom during the polymerization reaction is strongly influenced by the ligand structure. In addition, since organometallic complexes are usually unstable compounds against moisture and oxygen, organoaluminum compounds (sometimes called "scavengers") are often added during polymerization reactions to remove moisture and oxygen. A complex consisting of a metal atom and a ligand containing one cyclopentadienyl group (hereinafter sometimes called "half metallocene"), such as the organometallic complex (A) according to the present invention, has a wide coordination space around the central metal atom, so that the catalyst may be deactivated by reacting with compounds other than the monomer, such as organoaluminum reagents, moisture, oxygen, etc. Considering such a catalyst deactivation process, it is presumed that a complex having a titanium atom as the central metal can have a structure in which the metal atom is protected by the ligand compared to complexes having a zirconium atom and a hafnium atom, and therefore excellent polymerization activity can be expected as a result.
[0027] <x> The X's each independently represent a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a diene-based divalent derivative group. The atoms and functional groups that X may represent will be described in detail below.
[0028] <<Halogen atoms>> The halogen atom is not particularly limited, and examples thereof include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom, preferably a chlorine atom or a bromine atom, and particularly preferably a chlorine atom.
[0029] <<Hydrocarbon group>> The hydrocarbon group is not particularly limited, and may be a straight-chain, branched-chain or cyclic hydrocarbon group, may be a saturated or unsaturated hydrocarbon group, or may be substituted with a hydrogen atom. The substituent may be a group in which one or more hydrogen atoms of the hydrocarbon group are substituted with a substituent selected from an aryl group, a silicon-containing group, a nitrogen-containing group, an oxygen-containing group, a phosphorus-containing group, a halogen atom, and a halogen-containing group. The number of carbon atoms of the hydrocarbon group is preferably 1 to 20, more preferably 1 to 10, and even more preferably 1 to 8. Examples of the cyclic hydrocarbon group include an alicyclic hydrocarbon group having 3 to 20 carbon atoms and an aromatic hydrocarbon group having 6 to 20 carbon atoms (i.e., an aryl group). The alicyclic hydrocarbon group may be a cycloalkyl group, a cycloalkenyl group, an adamantyl group, a norbornyl group, or the like, with a cycloalkyl group being preferred. The aryl group may be a heteroaryl group containing a heteroatom, but preferably does not contain a heteroatom. The aryl group may have a hydrogen atom substituted. Examples of the aryl group include a group in which one or more hydrogen atoms of the aryl group are substituted with a substituent selected from a hydrocarbon group having 1 to 10 carbon atoms, a silicon-containing group, a nitrogen-containing group, an oxygen-containing group, a phosphorus-containing group, a halogen atom, and a halogen-containing group. Examples of the aryl group include a phenyl group and a naphthyl group. Suitable examples of the hydrocarbon group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isopropyl group, a benzyl group, and a phenyl group. When two Xs are linked to form a ring, examples of the hydrocarbon group include a butylene group, a pentamethylene group, and a hexamethylene group.
[0030] <<Halogen-containing groups>> Examples of the halogen-containing group include groups in which a hydrogen atom of a hydrocarbon group having 1 to 20 carbon atoms described below is substituted with a halogen atom. Examples of the halogen atom contained in the halogen-containing group include the halogen atoms described above, and preferably a fluorine atom or a chlorine atom. Examples of the halogen-containing group include halogenated hydrocarbon groups having 1 to 20 carbon atoms, such as a trifluoromethyl group, a tribromomethyl group, a pentafluoroethyl group, a pentafluorophenyl group, and a chlorophenyl group.
[0031] <<Silicon-containing groups>> The silicon-containing group is a group in which a carbon atom in the above-mentioned hydrocarbon group having 1 to 20 carbon atoms is replaced with a silicon atom. Examples of the silicon-containing group include alkylsilyl groups such as trimethylsilyl group, triethylsilyl group, t-butyldimethylsilyl group, and triisopropylsilyl group; arylsilyl groups such as dimethylphenylsilyl group, methyldiphenylsilyl group, and t-butyldiphenylsilyl group; pentamethyldisilanyl group, and trimethylsilylmethyl group. The alkylsilyl group preferably has 1 to 10 carbon atoms, and more preferably has 1 to 5 carbon atoms. The arylsilyl group preferably has 6 to 18 carbon atoms, and more preferably has 6 to 12 carbon atoms.
[0032] <<Oxygen-containing group>> Examples of the oxygen-containing group include a hydroxyl group, a group in which the -CH2- structural unit in the above-mentioned hydrocarbon group having 1 to 20 carbon atoms, silicon-containing group or nitrogen-containing group is replaced with an oxygen atom or a carbonyl group, or a group in which the -CH3 structural unit is replaced with an oxygen atom bonded to a hydrocarbon group having 1 to 20 carbon atoms, such as a methoxy group, ethoxy group, t-butoxy group, phenoxy group, trimethylsiloxy group, methoxyethoxy group, hydroxymethyl group, methoxymethyl group, ethoxymethyl group, t-butoxymethyl group, 1-hydroxymethyl group, 1-hydroxyethyl ... Examples of such an alkyl group include an aryl group, an aryloxyethyl group, a 1-methoxyethyl group, a 1-ethoxyethyl group, a 2-hydroxyethyl group, a 2-methoxyethyl group, a 2-ethoxyethyl group, an n-2-oxabutylene group, an n-2-oxapentylene group, an n-3-oxapentylene group, an aldehyde group, an acetyl group, a propionyl group, a benzoyl group, a trimethylsilylcarbonyl group, a carbamoyl group, a methylaminocarbonyl group, a carboxy group, a methoxycarbonyl group, a carboxymethyl group, an ethoxymethyl group, and a carbamoylmethyl group. The oxygen-containing group is preferably an alkoxy group having 1 to 10 carbon atoms, more preferably an alkoxy group having 1 to 5 carbon atoms, even more preferably an alkoxy group having 1 to 3 carbon atoms, and particularly preferably a methoxy group.
[0033] <<Sulfur-containing groups>> Examples of sulfur-containing groups include alkylthio groups, arylthio groups, thioester groups, sulfone ester groups, and sulfonamide groups. Specific examples of alkylthio groups include methylthio and ethylthio. Specific examples of arylthio groups include phenylthio, methylphenylthio, and naphthylthio. Specific examples of thioester groups include acetylthio, benzoylthio, methylthiocarbonyl, and phenylthiocarbonyl. Specific examples of sulfone ester groups include methyl sulfonate, ethyl sulfonate, and phenyl sulfonate. Specific examples of sulfonamide groups include phenylsulfonamide, N-methylsulfonamide, and N-methyl-p-toluenesulfonamide.
[0034] <<Nitrogen-containing group>> Examples of the nitrogen-containing group include an amino group, a nitro group, an N-morpholinyl group, and a dimethylamino group, which is a group in which the =CH- structural unit in the above-mentioned hydrocarbon group having 1 to 20 carbon atoms or silicon-containing group is replaced with a nitrogen atom, a group in which the -CH2- structural unit is replaced with a nitrogen atom to which a hydrocarbon group having 1 to 20 carbon atoms is bonded, or a group in which the -CH3 structural unit is replaced with a nitrogen atom to which a hydrocarbon group having 1 to 20 carbon atoms is bonded or a nitrile group, such as a dimethylamino group, a diethylamino group, or a dimethylaminomethyl group. More specifically, examples of the nitrogen-containing group include an amino group; an alkylamino group, such as a methylamino group, a dimethylamino group, a diethylamino group, a dipropylamino group, a dibutylamino group, or a dicyclohexylamino group; an arylamino group, such as a phenylamino group, a diphenylamino group, a ditolylamino group, a dinaphthylamino group, or a methylphenylamino group, or an alkylarylamino group. The nitrogen-containing group is preferably a dimethylamino group.
[0035] <<Phosphorus-containing group>> Examples of the phosphorus-containing group include trialkylphosphine groups such as a trimethylphosphine group, a tributylphosphine group, and a tricyclohexylphosphine group; triarylphosphine groups such as a triphenylphosphine group and a tritolylphosphine group; phosphite groups (phosphido groups) such as a methylphosphine group, an ethylphosphine group, and a phenylphosphine group; phosphonic acid groups; and phosphinic acid groups.
[0036] <<Boron-containing groups>> Examples of boron-containing groups include boranediyl, boranetriyl, diboranyl, as well as groups such as alkyl-, aryl-, and alkyl-substituted boron, boron halides, and alkyl-substituted boron halides.
[0037] Examples of the alkyl group-substituted boron include groups represented by (Et)B-, (iPr)B-, (iBu)B-, (Et)B, (iPr)B, or (iBu)B. Examples of the aryl group-substituted boron include groups represented by (C6H5)2B-, (C6H5)3B, (C6F5)3B, or (3,5-(CF3)2C6H3)3B. Examples of boron halides include groups represented by BCl2- or BCl3. Examples of the alkyl group-substituted boron halide include groups represented by (Et)BCl-, (iBu)BCl-, and (C6H5)2BCl. Trisubstituted boron may be in a coordinate bond. Here, Et stands for ethyl, iPr for isopropyl, and iBu for isobutyl.
[0038] <<Aluminum-containing group>> Examples of the aluminum halide include alkyl group-substituted aluminum, aryl group-substituted aluminum, and alkyl group-substituted aluminum halide groups. Examples of the aluminum halide group include (Et)2Al-, (iPr)2Al-, (iBu)2Al-, (Et)3Al, (iPr)3Al, and (iBu)3Al. Examples of the aluminum halide group include (C6H5)2Al-. Examples of the aluminum halide group include AlCl2- and AlCl3. Examples of the aluminum halide group include (Et)AlCl- and (iBu)AlCl-. Here, Et is an ethyl group, iPr is an isopropyl group, and iBu is an isobutyl group. Tri-substituted aluminum may be in a coordinate bond state.
[0039] <<Divalent Diene Derivative Group>> The diene divalent derivative group is a hydrocarbon group capable of coordinating with M in the above formula (1) via a lone electron pair, and examples thereof include a 1,3-butadienyl group, an isoprenyl group (2-methyl-1,3-butadienyl group), a piperylenyl group (1,3-pentadienyl group), a 2,4-hexadienyl group, a 1,4-diphenyl-1,3-pentadienyl group, a cyclopentadienyl group, a metallocyclopentenyl group, and a 1,5-cyclooctadienyl group.
[0040] From the viewpoint of exhibiting polymerization activity, X is more preferably a halogen atom, a hydrocarbon group or an alkylamino group.
[0041] Here, the active species of the polymerization catalyst refers to a state in which an ion pair is formed by reaction between an organometallic complex (A) (preferably X in the complex) and at least one compound (B) selected from the group consisting of an organometallic compound (B-1), an organoaluminum oxy compound (B-2), and a compound (B-3) that reacts with the organometallic complex (A) to form an ion pair, which will be described later. Therefore, from the viewpoint of the expression of the active species, the ease of generation of the active species, that is, the ease of reaction between at least one compound (B) selected from the group consisting of organometallic compounds (B-1), (B-2), and (B-3) and X of the organometallic complex (A) is important, and from this viewpoint, among the groups that X can take, a hydrocarbon group is suitable because it is a group that easily reacts with a compound (B) that will be described later. In addition, a halogen atom is also one of the suitable groups for X. The halogen atom bonded to M, which is a metal atom in the organometallic complex (A), easily reacts with the organoaluminum compound, and the halogen atom is substituted for a hydrocarbon group in the organoaluminum compound. As a result, the reaction with at least one compound (B) selected from the group consisting of the organometallic compounds (B-1), (B-2), and (B-3) proceeds easily, which is favorable for the generation of active species.
[0042] <y> Y represents a carbon atom or a silicon atom. From the viewpoint of exhibiting excellent polymerization activity, Y is preferably a carbon atom.
[0043] <R 1 ~R 7 and R 51 ~R 54 > R 1 ~R 7 and R 51 ~R 54 each independently represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group; R 1 ~R 7 and R 51 ~R 54 Two or more of these groups may be bonded to each other to form a ring structure.
[0044] <<Hydrocarbon group with 1 to 20 carbon atoms>> The above-mentioned hydrocarbon group is not particularly limited, and may be a straight-chain, chain-like or cyclic hydrocarbon group, may be a saturated or unsaturated hydrocarbon group, and may be substituted with a hydrogen atom. The above hydrocarbon group preferably has 1 to 10 carbon atoms, more preferably 2 to 8, even more preferably 3 to 8, still more preferably 4 to 8, and particularly preferably 4 to 6 carbon atoms. Examples of the linear or branched hydrocarbon group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a hexyl group, a heptyl group, an octyl group, a 2-ethylhexyl group, a decyl group, a dodecyl group, a tetradecyl group, a hexadecyl group, an octadecyl group, and an eicosyl group.
[0045] The cyclic hydrocarbon group may be an alicyclic hydrocarbon group having 3 to 20 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms (that is, an aryl group). The cyclic hydrocarbon group is not particularly limited and may be a single ring, a condensed ring, or a spiro ring. The number of ring members of the cyclic hydrocarbon group is not particularly limited and is preferably 1 to 4, more preferably 1 to 3, and further preferably 1 or 2.
[0046] The alicyclic hydrocarbon group may be a cycloalkyl group, a cycloalkenyl group, an adamantyl group, a norbornyl group, or the like. The alicyclic hydrocarbon group may also contain a heteroatom. Examples of the cycloalkyl group include cyclopropyl, cyclobutyl, cyclopentyl, and cyclohexyl groups. Examples of the heterocycloalkyl group include morpholino and piperidino groups. Examples of the cycloalkenyl group include cyclopropenyl, cyclobutenyl, and 2-cyclopenten-1-yl groups. The alicyclic hydrocarbon group may have a hydrogen atom substituted therein. Examples of the substituent include a group in which one or more hydrogen atoms of the alicyclic hydrocarbon group are substituted with a substituent selected from a hydrocarbon group having 1 to 20 carbon atoms, an aryl group, a silicon-containing group, a nitrogen-containing group, an oxygen-containing group, a phosphorus-containing group, a halogen atom, and a halogen-containing group.
[0047] The aryl group may be a heteroaryl group containing a heteroatom. The aryl group may have a hydrogen atom substituted therein. Examples of the heteroatom include an oxygen atom, a nitrogen atom, and a sulfur atom. The aryl group may contain two or more heteroatoms. The substituted aryl group will be described later. Examples of the aryl group include a phenyl group, a naphthyl group, an indenyl group, a biphenylyl group, an anthryl group, and a phenanthryl group. Examples of the heteroaryl group include a furanyl group, a pyrrolidinyl group, a piperidinyl group, a pyridinyl group, a benzpyrazolyl group, a thienyl group, and a furyl group. The aryl group is preferably an aryl group having 6 to 20 carbon atoms, more preferably an aryl group having 6 to 18 carbon atoms, and even more preferably an aryl group having 6 to 10 carbon atoms.
[0048] Among these, preferred examples of the hydrocarbon group having 1 to 20 carbon atoms include linear or chain hydrocarbon groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, and tert-butyl groups, and substituted or unsubstituted aryl groups such as phenyl.
[0049] R 1 ~R 7 and R 51 ~R 54 The halogen atom, halogen-containing group, silicon-containing group, oxygen-containing group, nitrogen-containing group, sulfur-containing group, and phosphorus-containing group in have the same meaning as the halogen atom, halogen-containing group, silicon-containing group, oxygen-containing group, nitrogen-containing group, sulfur-containing group, and phosphorus-containing group in X described above, and preferred embodiments are also the same.
[0050] <<Ring structure>> R 1 ~R 7 and R 51 ~R 54 Examples of the ring structure formed by bonding two or more groups among the above include ring structures such as an alicyclic ring having 3 to 20 carbon atoms and an aromatic ring having 6 to 20 carbon atoms. Examples of the alicyclic ring having 3 to 20 carbon atoms include a cyclopentane ring, a cyclohexane ring, a cycloheptane ring, a piperidine ring, and a morpholine ring. Examples of the aromatic ring having 6 to 20 carbon atoms include a benzene ring, a naphthalene ring, an indazole ring, an indole ring, and a quinoline ring. The ring structure may have hydrogen atoms substituted therein. Examples of the substituent include groups in which one or more hydrogen atoms in the ring structure are substituted with a substituent selected from a hydrocarbon group having 1 to 20 carbon atoms, an aryl group, a silicon-containing group, a nitrogen-containing group, an oxygen-containing group, a phosphorus-containing group, a halogen atom, and a halogen-containing group.
[0051] [R 1 and R 2 〕 R 1 and R 2 are each independently preferably a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, more preferably a hydrogen atom or a hydrocarbon group having 1 to 5 carbon atoms, and further preferably a hydrocarbon group having 1 to 3 carbon atoms; R 1 and R 2 It is particularly preferable that each of these is a methyl group.
[0052] [R 51 ~R 54 〕 R 51 ~R 54 are each independently preferably a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, or a silicon-containing group, more preferably a hydrogen atom, a hydrocarbon group having 1 to 5 carbon atoms, or an alkylsilyl group having 1 to 10 carbon atoms, further preferably a hydrogen atom, or a linear or branched hydrocarbon group having 1 to 5 carbon atoms, and particularly preferably a hydrogen atom. Also, R 51 ~R 54 When R forms a ring structure, 51 ~R 54 It is preferable that two adjacent groups among R are bonded to each other to form a ring structure, 51 and R 52 , R 52 and R 53 , and / or R 53 and R 54 more preferably, R 51 and R 52 and R 53 and R 54 More preferably, R 51 and R 52 and R 53 and R 54 are particularly preferably bonded to each other to form a benzene ring. Note that the ring structure may have a hydrogen atom substituted therein. R 51 ~R 54 It is preferable that does not form a ring structure.
[0053] R 51 ~R 54 From the viewpoint of ease of synthesis of organometallic compounds, R 51 ~R 54 Of these, R 51 and R 53 is a hydrogen atom or R 52 and R 54 is preferably a hydrogen atom, and R 51 , R 52 and R 54 is a hydrogen atom or R 51 , R 53 and R 54 is more preferably a hydrogen atom, and from the viewpoint of superior copolymerizability, R 51 ~R 54 It is particularly preferable that all of are hydrogen atoms.
[0054] In formula (1), R 1 ~R 7 It is preferred that two groups bonded to adjacent ring members are bonded to each other to form a ring structure. R 3 ~R 6 It is preferred that two groups bonded to adjacent ring members are bonded to each other to form a ring structure, and R 3 or R 4 and R 5 or R 6 and more preferably combine with each other to form a ring structure. Also, R 1 ~R 4 Two groups bonded to adjacent ring members are bonded to each other to form a ring structure, and / or R 5 ~R 7 It is more preferable that two groups bonded to adjacent ring members are bonded to each other to form a ring structure. Examples of the ring structure include the ring structures described above.
[0055] The formula (1) is preferably represented by the following formula (2).
[0056] [ka]
[0057] In formula (2), M is a titanium atom, a zirconium atom, or a hafnium atom; X's each independently represent a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a diene-based divalent derivative group; Y is a carbon atom or a silicon atom; R 1 , R 2 , R 7 and R 51 ~R 54 each independently represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group; R 55 ~R 58 are each independently a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group, provided that R 55 ~R 58 The total number of carbon atoms in R must not exceed 10. 1 , R 2 , R 7 and R 55 ~R 58 Two or more groups selected from the following may be bonded to each other to form a ring structure. 51 ~R 54 Two or more of these groups may be bonded to each other to form a ring structure.
[0058] M, X, Y, and R in formula (2) 1 , R 2 , R 7 and R 51 ~R 54 are M, X, Y, and R in formula (1). 1 , R 2 , R 7 and R 51 ~R 54 The same applies to the preferred embodiments.
[0059] < <R 55 ~R 58 >> R 55 ~R 58 In the above formula (1), the halogen atom, halogen-containing group, silicon-containing group, oxygen-containing group, nitrogen-containing group, sulfur-containing group, and phosphorus-containing group are exemplified as the halogen atom, halogen-containing group, silicon-containing group, oxygen-containing group, nitrogen-containing group, sulfur-containing group, and phosphorus-containing group. 55 ~R 58 It is preferred that the total number of carbon atoms in each of the groups does not exceed 10. R 55 ~R 58 The hydrocarbon group having 1 to 10 carbon atoms in is not particularly limited and may be a linear, chain, or cyclic hydrocarbon group, may be a saturated or unsaturated hydrocarbon group, and may be substituted with a hydrogen atom. The above hydrocarbon group preferably has 1 to 8 carbon atoms, more preferably 1 to 6 carbon atoms, further preferably 1 to 5 carbon atoms, and particularly preferably 1 to 4 carbon atoms. The cyclic hydrocarbon group may be an alicyclic hydrocarbon group having 3 to 10 carbon atoms, or an aromatic hydrocarbon group (aryl group) having 6 to 10 carbon atoms. The above-mentioned alicyclic hydrocarbon group having 3 to 10 carbon atoms and aromatic hydrocarbon group having 6 to 10 carbon atoms (aryl group) have the same meaning as the alicyclic hydrocarbon group having 3 to 10 carbon atoms and aromatic hydrocarbon group having 6 to 10 carbon atoms (aryl group) in the alicyclic hydrocarbon group having 3 to 20 carbon atoms and aromatic hydrocarbon group having 6 to 20 carbon atoms (aryl group) in the above formula (1). Among these, preferred examples of the hydrocarbon group having 1 to 10 carbon atoms include linear or chain-like hydrocarbon groups such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, and a tert-butyl group, as well as substituted or unsubstituted aryl groups such as a phenyl group.
[0060] <<Ring structure in formula (2)>> In formula (2), R 51 ~R 58 It is preferable that two or more groups selected from the group consisting of R 55 ~R 58 It is more preferable that two or more groups selected from the group consisting of are bonded to each other to form a ring structure. R in Equation (2) 1 , R 2 , R 7 and R 51 ~R 58 Examples of the ring structure formed by bonding two or more groups selected from the above include R 1 ~R 7 and R 51 ~R 54 The meaning is the same as the ring structure formed by bonding two or more groups among the above, and the preferred embodiments are also the same.
[0061] In the formula (1) or (2), R 7 is preferably an aryl group or a substituted aryl group. The aryl group has the same meaning as the aryl group in the above formula (1), and preferred embodiments are also the same. Examples of the substituted aryl group include the above-mentioned aryl group in which one or more hydrogen atoms are substituted with a substituent selected from a hydrocarbon group having 1 to 20 carbon atoms, an aryl group, a silicon-containing group, a nitrogen-containing group, an oxygen-containing group, a phosphorus-containing group, a halogen atom, and a halogen-containing group. Examples of the substituted aryl group include a 3-methylphenyl group (m-tolyl group), a 4-methylphenyl group (p-tolyl group), a 3-ethylphenyl group, a 4-ethylphenyl group, a 3,4-dimethylphenyl group, a 3,5-dimethylphenyl group, a biphenylyl group, a 4-(trimethylsilyl)phenyl group, a 4-aminophenyl group, a 4-(dimethylamino)phenyl group, a 4-(diethylamino)phenyl group, a 4-morpholinylphenyl group, a 4-methoxyphenyl group, a 4-ethoxyphenyl group, a 4-phenoxyphenyl group, a 3,4-dimethoxyphenyl group, a 3,5-dimethoxyphenyl group, a 3-methyl-4-methoxyphenyl group, a 3,5-dimethyl-4-methoxyphenyl group, a 3-(trifluoromethyl)phenyl group, a 4-(trifluoromethyl)phenyl group, a 3-chlorophenyl group, a 4-chlorophenyl group, a 3-fluorophenyl group, a 4-fluorophenyl group, a 5-methylnaphthyl group, and a 2-(6-methyl)pyridyl group.
[0062] In the formula (1) or the formula (2), R 51 ~R 54 are each independently preferably a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, or a silicon-containing group, more preferably a hydrogen atom, a hydrocarbon group having 1 to 5 carbon atoms, or an alkylsilyl group having 1 to 10 carbon atoms, and even more preferably a hydrogen atom.
[0063] In the formula (1) or (2), R 51 ~R 54 is a hydrogen atom, M is a titanium atom, and R 7 is preferably an aryl group or a substituted aryl group.
[0064] The formula (1) is preferably represented by the following formula (3).
[0065] [ka]
[0066] In formula (3), M is a titanium atom, a zirconium atom, or a hafnium atom; each X is independently a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a diene-based divalent derivative group; R 5 ~R 7 and R 51 ~R 54 each independently represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group; R 5 ~R 7 and R 51 ~R 54 Two or more of the groups may be bonded to each other to form a ring structure, Ar represents an aromatic ring, R Ar each independently represents a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group, and n represents an integer from 0 to the maximum number of substituents on Ar minus 2.
[0067] In formula (3), M, X, R 5 ~R 7 and R 51 ~R 54 are M, X, and R in formula (1). 5 ~R 7 and R 51 ~R 54 The same applies to the preferred embodiments.
[0068] < <ar>> The aromatic ring represented by Ar is not particularly limited and may be a monocyclic ring, a polycyclic ring, or a monocyclic or polycyclic ring and a condensed ring thereof. The aromatic ring may be an aromatic heterocycle. Examples of the aromatic ring include a benzene ring, a naphthalene ring, an anthracene ring, a pyridine ring, a thiophene ring, a furan ring, an indazole ring, an indole ring, etc. Among these, the aromatic ring is preferably a benzene ring or a naphthalene ring, and more preferably a benzene ring.
[0069] < <R Ar >> R Ar The hydrocarbon group having 1 to 10 carbon atoms, the halogen atom, the halogen-containing group, the silicon-containing group, the oxygen-containing group, the nitrogen-containing group, the sulfur-containing group, and the phosphorus-containing group in the formula (1) have the same meanings as the hydrocarbon group having 1 to 10 carbon atoms, the halogen atom, the halogen-containing group, the silicon-containing group, the oxygen-containing group, the nitrogen-containing group, the sulfur-containing group, and the phosphorus-containing group in the formula (1), and the preferred embodiments are also the same. Ar is preferably a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, more preferably a hydrogen atom or a hydrocarbon group having 1 to 5 carbon atoms, even more preferably a hydrogen atom or a hydrocarbon group having 1 to 3 carbon atoms, and particularly preferably a hydrogen atom or a methyl group.
[0070] < <n>> In formula (3), n represents an integer of from 0 to the maximum number of substituents on Ar minus 2, and is preferably 0 to 2, more preferably 0 or 1, and further preferably 0.
[0071] <<Ring structure in formula (3)>> R 5 ~R 7 and R 51 ~R 54 Examples of the ring structure formed by bonding two or more groups include R 1 ~R 7 and R 51 ~R 54 is synonymous with a ring structure formed by bonding two or more groups among the above.
[0072] In formula (3), R 5 ~R 7 It is preferred that two or more of the groups are bonded to each other to form a ring structure, and R 5 and R 6 and R 7 and more preferably bond together to form a ring structure, 5 and R 6 and R 7 It is further preferred that these are bonded together to form an aromatic heterocycle. R 5 and R 6 and R 7 The ring structure formed by bonding with each other is preferably an aromatic heterocycle, more preferably a pyrrole ring or an indole ring.
[0073] The above formula (1) is preferably represented by the following formula (4).
[0074] [ka]
[0075] In formula (4), M is a titanium atom; X's each independently represent a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a diene-based divalent derivative group; Y is a carbon atom or a silicon atom; R 1 and R 2 each independently represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group; R 55 ~R 58 and R 59 ~R 63 are each independently a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group, and R 55 ~R 58 The total number of carbon atoms in R 59 ~R 63 The total number of carbon atoms in each of these groups must not exceed 10. 55 ~R 58 Two or more groups selected from the group consisting of may be bonded to each other to form a ring structure, and R 59 ~R 63 Two or more groups selected from the above may be bonded to each other to form a ring structure.
[0076] X, Y, and R in formula (4) 1 and R 2 are M, X, Y, and R in formula (1). 1 and R 2 The same applies to the preferred embodiments. 55 ~R 58 is R in the above formula (2). 55 ~R 58 The same applies to the preferred embodiments.
[0077] < <R 59 ~R 63 >> R in Equation (4) 59 ~R 63 The hydrocarbon group having 1 to 10 carbon atoms, the halogen atom, the halogen-containing group, the silicon-containing group, the oxygen-containing group, the nitrogen-containing group, the sulfur-containing group, and the phosphorus-containing group represented by the formula (2) are R 55 ~R 58 These groups have the same meanings as the hydrocarbon group having 1 to 10 carbon atoms, the halogen atom, the halogen-containing group, the silicon-containing group, the oxygen-containing group, the nitrogen-containing group, the sulfur-containing group, and the phosphorus-containing group represented by the following formula (I), and preferred embodiments are also the same.
[0078] Specific examples of the metal complex compound (A) are shown below, but the present invention is not limited to these specific examples.
[0079] [ka]
[0080] [ka]
[0081] [ka]
[0082] [ka]
[0083] [ka]
[0084] [ka]
[0085] [ka]
[0086] [ka]
[0087] [ka]
[0088] [ka]
[0089] [ka]
[0090] [ka]
[0091] [ka]
[0092] In the present invention, the organometallic complex (A) may be one type alone or two or more types in combination.
[0093] <<Method for producing organometallic complex (A)>> The method for producing the organometallic complex (A) is not particularly limited, and for example, the "Synthesis Example" in the Examples described later can be used. The organometallic complex (A) may also be synthesized using a known reaction. The organometallic complex (A) may also be synthesized by synthesizing each part by a known synthesis method and bonding them by a known method. Examples of the synthesis method of the organometallic complex (A) include the methods shown below, but the present invention is not limited to these synthesis methods.
[0094] [ka]
[0095] The method for synthesizing the organometallic complex (A) may, for example, be a reaction in which the ligand is dissolved in a solvent, reacted with two equivalents of an organolithium reagent, and then reacted with a metal chloride. Preferred solvents for the reaction include hydrocarbon solvents such as hexane, heptane, cyclohexane, toluene, etc., or diethyl ether, cyclopentyl methyl ether, tetrahydrofuran, tert-butyl methyl ether, etc.
[0096] [ka]
[0097] Another synthesis method is, for example, the synthesis of a ligand and a transition metal amide complex (M(NR 64 2) and 4). In the above synthesis method, a complex in which X in the formula (1) is a dialkylamino group can be synthesized. 64 Suitable examples of the substituted amide complex include methyl and ethyl groups. Specific examples of the amide complex having such a substituent include tetrakisdimethylamidotitanium, tetrakisdimethylamidozirconium, and tetrakisdimethylamidohafnium. The obtained amide complex may be used as it is in the polymerization reaction, or may be reacted with a chlorinating agent to convert X in the formula (1) to a chlorine atom, if necessary. The chlorinating agent is not particularly limited, and any known reagent may be used. An example of the chlorinating agent is R 65 n SiCl 4-n (R 65 represents an alkyl group having 1 to 3 carbon atoms, and n is an integer of 0 to 3. Examples of such compounds include SiCl4, Me2SiCl2, and Me3SiCl.
[0098] [ka]
[0099] Alternatively, for example, the organometallic complex (A) may be synthesized by reacting a ligand with an alkyl metal complex. 66 is not particularly limited as long as it is a hydrocarbon group, and examples thereof include a methyl group, an ethyl group, a benzyl group, etc. According to the above synthesis method, it is possible to synthesize an organometallic complex (A) in which X in the formula (1) is a hydrocarbon group.
[0100] [ka]
[0101] An example of a method for introducing a hydrocarbon group into X in the formula (1) is a method for introducing a hydrocarbon group into X by reacting an organometallic complex (A) in which X is a chlorine atom with a Grignard reagent or an organolithium reagent. Furthermore, the compound in which a hydrocarbon group has been introduced into X in the formula (1) may be reacted with a compound having an OH group to introduce an oxygen-containing group or a substituted aryl group. The above synthesis scheme is an example of a method for introducing a hydrocarbon group into X in formula (1). R in the synthesis scheme is not limited as long as it is a hydrocarbon group. Examples of Grignard reagents include methyl magnesium bromide, ethyl magnesium bromide, phenyl magnesium bromide, and benzyl magnesium bromide. Grignard reagents having a chlorine atom or an iodine atom, such as methyl magnesium chloride and methyl magnesium iodide, may also be used. Examples of organolithium reagents include methyl lithium, ethyl lithium, phenyl lithium, and benzyl lithium. In the above synthesis, different reagents may also be used in combination to introduce different Rs.
[0102] (polymerization catalyst) The polymerization catalyst according to the present invention contains the organometallic complex (A) according to the present invention described above, and at least one compound (B) selected from the group consisting of organometallic compounds (B-1), organoaluminum oxy compounds (B-2), and compounds (B-3) that react with the organometallic complex to form an ion pair.
[0103] <Organometallic compound (B-1)> Examples of the organometallic compound (B-1) include compounds containing at least one element from Groups 1, 2, 12, and 13 of the periodic table, which are specifically represented by the following general formulas (B-1a) to (B-1c): R a p Al(ОR b ) q H r Y s ···(B-1a) (In the general formula (B-1a), R a and R b may be the same or different from each other and represent a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms. Y represents a halogen atom, p is a number where 0 < p ≤ 3, q is a number where 0 ≤ q < 3, r is a number where 0 ≤ r < 3, s is a number where 0 ≤ s < 3, and m + n + p + q = 3.) An organoaluminum compound represented by M 3 AlR c 4···(B-1b) (In the general formula (B-1b), M 3 represents Li, Na, or K, and R c represents a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms.) A complex alkyl compound of an alkali metal from Group 1 of the periodic table and aluminum represented by R d R e M 4 ···(B-1c) (In the general formula (B-1c), R d and R e may be the same or different from each other and represent a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms. M 4 is Mg, Zn, or Cd.) A dialkyl compound of an alkaline earth metal from Group 2 of the periodic table or a metal from Group 12 and a metal represented by
[0104] Examples of the organoaluminum compound belonging to the general formula (B-1a) include the following compounds. R a p Al(ОR b ) 3-p ···(B-1a-1) (In formula (B-1a-1), R a and R b may be the same as or different from each other, and represent a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms, and p is preferably a number satisfying 1.5 ≦ p ≦ 3.) An organoaluminum compound represented by R a p AlY 3-p ···(B-1a-2) (In formula (B-1a-2), R a represents a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms, Y represents a halogen atom, and p is preferably a number satisfying 0 < p < 3.) An organoaluminum compound represented by R a p AlH 3-p ···(B-1a-3) (In formula (B-1a-3), R a represents a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms, and p is preferably a number satisfying 2 ≦ p < 3.) An organoaluminum compound represented by R a p Al(ОR b ) q Y s ···(B-1a-4) (In formula (B-1a-4), R a and R b may be the same as or different from each other, and represent a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms, Y represents a halogen atom, p is a number satisfying 0 < p ≦ 3, q is a number satisfying 0 ≦ q < 3, s is a number satisfying 0 ≦ s < 3, and p + q + s = 3.) An organoaluminum compound represented by
[0105] More specifically, as the organoaluminum compound belonging to the general formula (B-1a), tri-n-alkylaluminums such as trimethylaluminum, triethylaluminum, tri-n-butylaluminum, tripropylaluminum, tripentylaluminum, trihexylaluminum, trioctylaluminum, tridecylaluminum; tri-branched alkylaluminums such as triisopropylaluminum, triisobutylaluminum, trisec-butylaluminum, tritert-butylaluminum, tri2-methylbutylaluminum, tri3-methylbutylaluminum, tri2-methylpentylaluminum, tri3-methylpentylaluminum, tri4-methylpentylaluminum, tri2-methylhexylaluminum, tri3-methylhexylaluminum, and tri2-ethylhexylaluminum; Tricycloalkylaluminums such as tricyclohexylaluminum and tricyclooctylaluminum; Triarylaluminum such as triphenylaluminum and tritolylaluminum; dialkylaluminum hydrides such as diisobutylaluminum hydride; (i-C4H9) x Al y (C5H 10 ) z (wherein x, y and z are positive numbers, and z≧2x), and other trialkenylaluminums, such as triisoprenylaluminum; Alkyl aluminum alkoxides such as isobutyl aluminum methoxide, isobutyl aluminum ethoxide, and isobutyl aluminum isopropoxide; Dialkylaluminum alkoxides such as dimethylaluminum methoxide, diethylaluminum ethoxide, and dibutylaluminum butoxide; Alkyl aluminum sesquialkoxides such as ethyl aluminum sesquiethoxide, butyl aluminum sesquibutoxide; R a 2.5 Al(OR b ) 0.5 Partially alkoxylated alkylaluminum having an average composition represented by the formula: a and R b may be the same or different and represent a hydrocarbon group having 1 to 15, preferably 1 to 4, carbon atoms; dialkylaluminum aryloxides such as diethylaluminum phenoxide, diethylaluminum (2,6-di-t-butyl-4-methylphenoxide), ethylaluminum bis(2,6-di-t-butyl-4-methylphenoxide), diisobutylaluminum (2,6-di-t-butyl-4-methylphenoxide), and isobutylaluminum bis(2,6-di-t-butyl-4-methylphenoxide); Dialkylaluminum halides such as dimethylaluminum chloride, diethylaluminum chloride, dibutylaluminum chloride, diethylaluminum bromide, and diisobutylaluminum chloride; Alkyl aluminum sesquihalides such as ethyl aluminum sesquichloride, butyl aluminum sesquichloride, and ethyl aluminum sesquibromide; partially halogenated alkylaluminums, such as alkylaluminum dihalides, such as ethylaluminum dichloride, propylaluminum dichloride, butylaluminum dibromide, and the like; Dialkylaluminum hydrides such as diethylaluminum hydride and dibutylaluminum hydride; Other partially hydrogenated alkylaluminums, such as alkylaluminum dihydrides, such as ethylaluminum dihydride, propylaluminum dihydride, etc.; Examples of the aluminum compounds include partially alkoxylated and halogenated alkylaluminum compounds such as ethylaluminum ethoxy chloride, butylaluminum butoxy chloride, and ethylaluminum ethoxy bromide.
[0106] Compounds similar to the general formula (B-1a) can also be used in the present invention, such as organoaluminum compounds in which two or more aluminum compounds are bonded via nitrogen atoms, such as (C2H5)2AlN(C2H5)Al(C2H5)2.
[0107] The compounds belonging to the general formula (B-1b) include LiAl(C2H5)4, LiAl(C7H 15 )4 can be mentioned as examples. Examples of the compound belonging to the general formula (B-1c) include dimethylmagnesium, diethylmagnesium, dibutylmagnesium, butylethylmagnesium, dimethylzinc, diethylzinc, diphenylzinc, di-n-propylzinc, diisopropylzinc, di-n-butylzinc, diisobutylzinc, bis(pentafluorophenyl)zinc, dimethylcadmium, and diethylcadmium.
[0108] In addition, as the organometallic compound (B-1), methyllithium, ethyllithium, propyllithium, butyllithium, methylmagnesium bromide, methylmagnesium chloride, ethylmagnesium bromide, ethylmagnesium chloride, propylmagnesium bromide, propylmagnesium chloride, butylmagnesium bromide, butylmagnesium chloride, etc. can also be used.
[0109] Furthermore, a compound that forms the above-mentioned organoaluminum compound in the polymerization system, such as a combination of an aluminum halide and an alkyllithium, or a combination of an aluminum halide and an alkylmagnesium, can also be used as the organometallic compound (B-1).
[0110] Among the organometallic compounds (B-1), organoaluminum compounds are preferred from the standpoint of catalytic activity. The organometallic compounds (B-1) as described above may be used singly or in combination of two or more kinds.
[0111] <Organoaluminum oxy compound (B-2)> The organoaluminum oxy compound (B-2) used in the present invention may be a conventionally known aluminoxane, or may be a benzene-insoluble organoaluminum oxy compound such as those exemplified in JP-A-2-78687. Conventionally known aluminoxanes can be produced, for example, by the following method, and are usually obtained as a solution in a hydrocarbon solvent.
[0112] (1) A method in which an organoaluminum compound such as trialkylaluminum is added to a hydrocarbon medium suspension of a compound containing adsorbed water or a salt containing water of crystallization, such as magnesium chloride hydrate, copper sulfate hydrate, aluminum sulfate hydrate, nickel sulfate hydrate, or cerous chloride hydrate, to react the adsorbed water or the water of crystallization with the organoaluminum compound. (2) A method in which water, ice or water vapor is allowed to act directly on an organoaluminum compound such as trialkylaluminum in a medium such as benzene, toluene, ethyl ether or tetrahydrofuran. (3) A method in which an organoaluminum compound such as trialkylaluminum is reacted with an organotin oxide such as dimethyltin oxide or dibutyltin oxide in a medium such as decane, benzene, or toluene.
[0113] The aluminoxane may contain a small amount of an organometallic component. After the solvent or unreacted organoaluminum compound is removed by distillation from the recovered aluminoxane solution, the resulting aluminoxane may be redissolved in a solvent or suspended in a poor solvent for the aluminoxane.
[0114] Specific examples of the organoaluminum compound used in preparing the aluminoxane include the same organoaluminum compounds as those exemplified as the organoaluminum compounds belonging to the general formula (B-1a) above.
[0115] Of these, trialkylaluminum and tricycloalkylaluminum are preferred, with trimethylaluminum being particularly preferred. The above organoaluminum compounds may be used singly or in combination of two or more.
[0116] Examples of the solvent used in the preparation of aluminoxane include aromatic hydrocarbons such as benzene, toluene, xylene, cumene, and cymene; aliphatic hydrocarbons such as pentane, hexane, heptane, octane, decane, dodecane, hexadecane, and octadecane; alicyclic hydrocarbons such as cyclopentane, cyclohexane, cyclooctane, and methylcyclopentane; petroleum fractions such as gasoline, kerosene, and diesel; and halides of the above aromatic hydrocarbons, aliphatic hydrocarbons, and alicyclic hydrocarbons, especially chlorinated and brominated hydrocarbons. Furthermore, ethers such as ethyl ether and tetrahydrofuran can also be used. Among these solvents, aromatic hydrocarbons or aliphatic hydrocarbons are particularly preferred. These solvents can be used alone or in combination.
[0117] The organoaluminum oxy compound (B-2) may be at least one selected from aluminoxanes having a structure represented by the following general formula (B-2a) or (B-2b), and aluminoxanes having a structure comprising a repeating unit represented by the following general formula (B-2c) and a repeating unit represented by the following general formula (B-2d).
[0118] [ka]
[0119] In the general formula, R c are each independently a hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 4 carbon atoms. Specific examples of hydrocarbon groups include a methyl group, an ethyl group, a propyl group, an isopropyl group, an isopropenyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a hexyl group, an octyl group, a decyl group, a dodecyl group, a tridecyl group, a tetradecyl group, a hexadecyl group, an octadecyl group, an eicosyl group, a cyclohexyl group, a cyclooctyl group, a phenyl group, a tolyl group, and an ethylphenyl group. Among these examples, a methyl group, an ethyl group, and an isobutyl group are preferable, and a methyl group is particularly preferable. In the general formulae (B-2a), (B-2b), and (B-2c), R c may be partially substituted with halogen atoms such as chlorine and bromine atoms, and the halogen content may be 40 mass % or less.
[0120] In the general formulae (B-2a) and (B-2b), r represents an integer of 2 to 500, preferably 6 to 300, and particularly preferably 10 to 100. In the general formulae (B-2c) and (B-2d), s and t each represent an integer of 1 or more.
[0121] The aluminoxane having a repeating unit represented by the general formula (B-2c) and a repeating unit represented by the general formula (B-2d) preferably has a molecular weight in the range of 200 to 2000 as measured by cryoscopic method in benzene.
[0122] The benzene-insoluble organoaluminum oxy-compound is preferably one in which the Al component dissolved in benzene at 60°C is usually 10% or less, preferably 5% or less, and particularly preferably 2% or less, calculated as Al atom, i.e., one which is insoluble or poorly soluble in benzene.
[0123] The organoaluminum oxy compound (B-2) may be an organoaluminum oxy compound containing boron represented by the following general formula (B-2e).
[0124] [ka]
[0125] In general formula (B-2e), R 15 represents a hydrocarbon group having 1 to 10 carbon atoms, and four R 16 may be the same or different and each independently represents a hydrogen atom, a halogen atom, or a hydrocarbon group having 1 to 10 carbon atoms.
[0126] The boron-containing organoaluminum oxy compound represented by the general formula (B-2e) may be produced by reacting an alkylboronic acid represented by the following general formula (B-2f) with an organoaluminum compound in an inert solvent under an inert gas atmosphere at a temperature of −80° C. to room temperature for 1 minute to 24 hours.
[0127] R 15 -B(OH)2···(B-2f) In general formula (B-2f), R 15 is R in the general formula (B-2e) 15 represents the same group as
[0128] Specific examples of the alkylboronic acid represented by the general formula (B-2f) include methylboronic acid, ethylboronic acid, isopropylboronic acid, n-propylboronic acid, n-butylboronic acid, isobutylboronic acid, n-hexylboronic acid, cyclohexylboronic acid, phenylboronic acid, 3,5-difluoroboronic acid, pentafluorophenylboronic acid, and 3,5-bis(trifluoromethyl)phenylboronic acid. Among these, methylboronic acid, n-butylboronic acid, isobutylboronic acid, 3,5-difluorophenylboronic acid, and pentafluorophenylboronic acid are preferred. These are used alone or in combination of two or more.
[0129] Specific examples of the organoaluminum compound to be reacted with such an alkylboronic acid include the same organoaluminum compounds as those exemplified as the organoaluminum compounds belonging to the above general formula (B-1a).
[0130] The organoaluminum compound is preferably a trialkylaluminum or a tricycloalkylaluminum, more preferably a trimethylaluminum, a triethylaluminum or a triisobutylaluminum, which may be used alone or in combination of two or more.
[0131] When an organoaluminum oxy compound (B-2) such as methylaluminoxane is used as a cocatalyst component in addition to the organometallic complex (A), extremely high polymerization activity for olefin compounds is exhibited. The organoaluminum oxy compounds (B-2) may be used singly or in combination of two or more kinds.
[0132] <Compound (B-3) that reacts with organometallic complex (A) to form an ion pair> Examples of the compound (B-3) (hereinafter referred to as "ionized ionic compound") that reacts with the organometallic complex (A) to form an ion pair include Lewis acids, ionic compounds, borane compounds, and carborane compounds described in JP-T-1-501950, JP-T-1-502036, JP-A-3-179005, JP-A-3-179006, JP-A-3-207703, JP-A-3-207704, and US-5321106. Further examples include heteropoly compounds and isopoly compounds.
[0133] Specifically, the Lewis acid includes a compound represented by BR3 (R is fluorine or a phenyl group which may have a substituent such as fluorine, a methyl group, or a trifluoromethyl group), such as trifluoroboron, triphenylboron, tris(4-fluorophenyl)boron, tris(3,5-difluorophenyl)boron, tris(4-fluoromethylphenyl)boron, tris(pentafluorophenyl)boron, tris(p-tolyl)boron, tris(o-tolyl)boron, and tris(3,5-dimethylphenyl)boron.
[0134] The ionic compound includes, for example, a compound represented by the following general formula (B-3a).
[0135] [ka]
[0136] In general formula (B-3a), R 17 H + , a carbonium cation, an oxonium cation, an ammonium cation, a phosphonium cation, a cycloheptyltrienyl cation or a ferrocenium cation having a transition metal, and R 18 ~R 21 may be the same or different and are organic groups, preferably aryl groups or substituted aryl groups.
[0137] Specific examples of the carbonium cation include tri-substituted carbonium cations such as triphenylcarbonium cation, tri(methylphenyl)carbonium cation, and tri(dimethylphenyl)carbonium cation.
[0138] Specific examples of the ammonium cation include trialkylammonium cations such as trimethylammonium cation, triethylammonium cation, tripropylammonium cation, tributylammonium cation, and tri(n-butyl)ammonium cation; N,N-dialkylanilinium cations such as N,N-dimethylanilinium cation, N,N-diethylanilinium cation, and N,N-2,4,6-pentamethylanilinium cation; and dialkylammonium cations such as di(isopropyl)ammonium cation and dicyclohexylammonium cation.
[0139] Specific examples of the phosphonium cation include triarylphosphonium cations such as triphenylphosphonium cation, tri(methylphenyl)phosphonium cation, and tri(dimethylphenyl)phosphonium cation.
[0140] R 17 As the cation, a carbonium cation and an ammonium cation are preferred, and in particular, a triphenylcarbonium cation, an N,N-dimethylanilinium cation, and an N,N-diethylanilinium cation are preferred.
[0141] Further, examples of the ionic compound include trialkyl-substituted ammonium salts, N,N-dialkylanilinium salts, dialkylammonium salts, and triarylphosphonium salts.
[0142] Specific examples of the trialkyl-substituted ammonium salt include triethylammonium tetra(phenyl)boron, tripropylammonium tetra(phenyl)boron, tri(n-butyl)ammonium tetra(phenyl)boron, trimethylammonium tetra(p-tolyl)boron, trimethylammonium tetra(o-tolyl)boron, tri(n-butyl)ammonium tetra(pentafluorophenyl)boron, tripropylammonium tetra(o,p-dimethylphenyl)boron, tri(n-butyl)ammonium tetra(m,m-dimethylphenyl)boron, tri(n-butyl)ammonium tetra(p-trifluoromethylphenyl)boron, tri(n-butyl)ammonium tetra(3,5-ditrifluoromethylphenyl)boron, and tri(n-butyl)ammonium tetra(o-tolyl)boron.
[0143] Specific examples of the N,N-dialkylanilinium salt include N,N-dimethylanilinium tetra(phenyl)boron, N,N-diethylanilinium tetra(phenyl)boron, and N,N,2,4,6-pentamethylanilinium tetra(phenyl)boron.
[0144] Specific examples of the dialkylammonium salt include di(1-propyl)ammonium tetra(pentafluorophenyl)boron, dicyclohexylammonium tetra(phenyl)boron, and the like.
[0145] Further examples of the ionic compound include triphenylcarbenium tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, ferrocenium tetra(pentafluorophenyl)borate, triphenylcarbenium pentaphenylcyclopentadienyl complex, N,N-diethylanilinium pentaphenylcyclopentadienyl complex, and boron compounds represented by the following formula (B-3b) or (B-3c).
[0146] [ka]
[0147] In formula (B-3b), Et represents an ethyl group.
[0148] [ka]
[0149] In formula (B-3c), Et represents an ethyl group.
[0150] Specific examples of the borane compound, which is an example of the ionizable ionic compound (compound (B-3)), include decaborane; Salts of anions such as bis[tri(n-butyl)ammonium]nonaborate, bis[tri(n-butyl)ammonium]decaborate, bis[tri(n-butyl)ammonium]undecaborate, bis[tri(n-butyl)ammonium]dodecaborate, bis[tri(n-butyl)ammonium]decachlorodecaborate, and bis[tri(n-butyl)ammonium]dodecachlorododecaborate; Examples of the salt include salts of metal borane anions such as tri(n-butyl)ammonium bis(dodecahydride dodecaborate) cobaltate(III) and bis[tri(n-butyl)ammonium]bis(dodecahydride dodecaborate) nickelate(III).
[0151] Specific examples of carborane compounds, which are examples of ionized ionic compounds, include 4-carbanonaborane, 1,3-dicarbanonaborane, 6,9-dicarbadecaborane, dodecahydride-1-phenyl-1,3-dicarbanonaborane, dodecahydride-1-methyl-1,3-dicarbanonaborane, undecahydride-1,3-dimethyl-1,3-dicarbanonaborane, 7,8-dicarbaundecaborane, 2,7-dicarbaundecaborane, and undecahydride-7,8-dimethyl-1,3-dicarbanonaborane. 1-methyl-7,8-dicarboxylic acid borane, dodecahydride-11-methyl-2,7-dicarboxylic acid borane, tri(n-butyl)ammonium 1-carbadecaborate, tri(n-butyl)ammonium 1-carbaundecaborate, tri(n-butyl)ammonium 1-carbadodecaborate, tri(n-butyl)ammonium 1-trimethylsilyl-1-carbadecaborate, tri(n-butyl)ammonium bromo-1-carbadodecaborate, tri(n-butyl)ammonium ammonium 6-carbadecaborate, tri(n-butyl)ammonium 6-carbadecaborate, tri(n-butyl)ammonium 7-carbaundecaborate, tri(n-butyl)ammonium 7,8-dicaundecaborate, tri(n-butyl)ammonium 2,9-dicaundecaborate, tri(n-butyl)ammonium dodecahydride-8-methyl-7,9-dicaundecaborate, tri(n-butyl)ammonium undecahydride-8-ethyl-7,9-dicaundecaborate Salts of anions such as undecahydride, tri(n-butyl)ammonium undecahydride-8-butyl-7,9-dicarboxaborate, tri(n-butyl)ammonium undecahydride-8-allyl-7,9-dicarboxaborate, tri(n-butyl)ammonium undecahydride-9-trimethylsilyl-7,8-dicarboxaborate, tri(n-butyl)ammonium undecahydride-4,6-dibromo-7-carbaundecaborate; Tri(n-butyl)ammonium bis(nonahydride-1,3-dicarbanonaborate)cobaltate(III), tri(n-butyl)ammonium bis(undecahydride-7,8-dicarbandecaborate)ferrate(III), tri(n-butyl)ammonium bis(undecahydride-7,8-dicarbandecaborate)cobaltate(III), tri(n-butyl)ammonium bis(undecahydride-7,8-dicarbandecaborate)nickelate(III), tri(n-butyl)ammonium bis(undecahydride-7,8-dicarbandecaborate)cuprate(III), tri(n-butyl)ammonium bis(undecahydride-7,8-dicarbandecaborate)aurate(III), tri(n-butyl)ammonium bis(nonahydride-7,8-dimethyl-7,8-dicarbandecaborate)ferrate salt (III), tri(n-butyl)ammonium bis(nonahydride-7,8-dimethyl-7,8-dicarboxaborate)chromate (III), tri(n-butyl)ammonium bis(tribromooctahydride-7,8-dicarboxaborate)cobaltate (III), tris[tri(n-butyl)ammonium]bis(undecahydride-7-carbowndecaborate)chromate (III), bis[tri(n-butyl)ammonium]bis(undecahydride-7-carbowndecaborate)manganate (IV), bis[tri(n-butyl)ammonium]bis(undecahydride-7-carbowndecaborate)cobaltate (III), bis[tri(n-butyl)ammonium]bis(undecahydride-7-carbowndecaborate)nickelate (IV), and the like.
[0152] Heteropoly compounds, which are examples of ionized ionic compounds, are compounds that contain an atom selected from silicon, phosphorus, titanium, germanium, arsenic and tin, and one or more atoms selected from vanadium, niobium, molybdenum and tungsten.Specific examples include, but are not limited to, phosphovanadic acid, germanovanadic acid, arsenic vanadic acid, phosphoniobic acid, germanoniobic acid, siliconomybdic acid, phosphomolybdic acid, titanomolybdic acid, germanomolybdic acid, arsenic molybdic acid, tinmolybdic acid, phosphotungstic acid, germanotungstic acid, tintungstic acid, phosphomolybdovanadic acid, phosphotungstovanadic acid, germanotungstovanadic acid, phosphomolybdotungstovanadic acid, germanomolybdotungstovanadic acid, phosphomolybdotungstic acid, phosphomolybdoniobic acid, and the salts of these acids. Examples of the salts include salts of the acids with, for example, alkali metals of Group 1 or alkaline earth metals of Group 2 of the periodic table, specifically, lithium, sodium, potassium, rubidium, cesium, beryllium, magnesium, calcium, strontium, barium, etc., and organic salts such as triphenylethyl salts.
[0153] Isopoly compounds, which are examples of ionized ionic compounds, are compounds composed of metal ions of one type of atom selected from vanadium, niobium, molybdenum, and tungsten, and can be considered to be molecular ion species of metal oxides.Specific examples include, but are not limited to, vanadic acid, niobic acid, molybdic acid, tungstic acid, and salts of these acids.Furthermore, examples of the salts include salts of the acids with metals of Group 1 or 2 of the periodic table, specifically, lithium, sodium, potassium, rubidium, cesium, beryllium, magnesium, calcium, strontium, barium, etc., and organic salts such as triphenylethyl salts.
[0154] The above-mentioned ionizing ionic compound (compound (B-3) which reacts with the organometallic complex (A) to form an ion pair) may be used alone or in combination of two or more kinds. The polymerization catalyst according to the present invention may contain the above-mentioned organometallic complex (A) (hereinafter may be abbreviated as "component (A)"), and at least one compound (B) (hereinafter may be abbreviated as "component (B)") selected from the group consisting of organometallic compounds (B-1), organoaluminum oxy compounds (B-2), and ionizing ionic compounds (B-3), and may also contain the following carrier (C) as necessary.
[0155] ((C) Carrier) The carrier (C) is not particularly limited, and may be an inorganic or organic compound, and may be a granular or fine particle solid. When the above-mentioned organometallic complex (A) and compound (B) are supported on the carrier (C), a polymer with good morphology is obtained.
[0156] The inorganic compound is preferably a porous oxide, a solid aluminoxane compound, an inorganic halide, clay, a clay mineral, or an ion-exchangeable layered compound. Specifically, the porous oxide may be SiO2, Al2O3, MgO, ZrO, TiO2, B2O3, CaO, ZnO, BaO, ThO2, etc., or a composite or mixture containing these, and further may be, for example, natural or synthetic zeolite, SiO2-MgO, SiO2-Al2O3, SiO2-TiO2, SiO2-V2O5, SiO2-Cr2O3, SiO2-TiO2-MgO, etc. Among these, the porous oxide is preferably one containing SiO2 and / or Al2O3 as the main component.
[0157] The porous oxide may contain small amounts of carbonates, sulfates, nitrates, and oxides such as Na2CO3, K2CO3, CaCO3, MgCO3, Na2SO4, Al2(SO4)3, BaSO4, KNO3, Mg(NO3)2, Al(NO3)3, Na2O, K2O, and Li2O.
[0158] The properties of such porous oxides vary depending on the type and manufacturing method, but the porous oxides preferably used in the present invention have a particle size of 10 to 300 μm, preferably 20 to 200 μm, and a specific surface area of 50 to 1000 m. 2 / g, preferably 100 to 700m 2 / g and the pore volume is 0.3-3.0 cm 3 / g range. Such a porous oxide is calcined at 100 to 1000°C, preferably 150 to 700°C, as required, before use.
[0159] The solid aluminoxane compound may be at least one selected from the aluminoxanes shown in (B-2a) to (B-2d) above. The solid aluminoxane used in the present invention differs from conventionally known olefin polymerization catalyst supports in that it does not contain inorganic solid components such as silica or alumina or organic polymer components such as polyethylene or polystyrene, but is a solidified product containing an alkylaluminum compound as the main component. As used herein, "solid state" means that the aluminoxane remains in a substantially solid state in the reaction environment employed. More specifically, for example, when the solid catalyst component for olefin polymerization is prepared by contacting the component (A) with the component (B) as described below, the component (B) is in a solid state in an inert hydrocarbon solvent such as hexane or toluene used in the reaction under a specific temperature and pressure environment. In addition, for example, when suspension polymerization is performed using the solid catalyst component for olefin polymerization prepared using the component (B) as described below, it is also a necessary requirement that the component (B) contained in the catalyst component is in a solid state in a hydrocarbon solvent such as hexane, heptane, or toluene under a specific temperature and pressure environment. The same is true for bulk polymerization in which polymerization is performed in a liquefied monomer instead of a solvent, and gas-phase polymerization in which polymerization is performed in a monomer gas.
[0160] The easiest method to check whether component (B) is in a solid state under the above environment is to check visually, but it is often difficult to check visually, for example, during polymerization. In that case, it can be judged, for example, from the properties of the polymer powder obtained after polymerization and the state of adhesion to the reactor. Conversely, if the properties of the polymer powder are good and there is little adhesion to the reactor, even if a part of component (B) is eluted to some extent under the polymerization environment, it does not deviate from the gist of the present invention. Examples of indices for judging the properties of the polymer powder include bulk density, particle shape, surface shape, and the degree of presence of amorphous polymers, but from the viewpoint of quantitativeness, polymer bulk density is preferred. The bulk density in the present invention is usually 0.01 to 0.9, preferably 0.05 to 0.6, and more preferably 0.1 to 0.5.
[0161] The solubility of the solid aluminoxane in n-hexane maintained at a temperature of 25° C. generally falls within the range of 0 to 40 mol %, preferably 0 to 20 mol %, and particularly preferably 0 to 10 mol %.
[0162] The solubility of the solid aluminoxane in n-hexane was determined by adding 2 g of the solid aluminoxane carrier to 50 mL of n-hexane kept at 25°C, stirring for 2 hours, separating the solution using a G-4 glass filter, and measuring the aluminum concentration in the filtrate. Therefore, the solubility is determined as the ratio of aluminum atoms present in the filtrate to the amount of aluminum atoms equivalent to 2 g of the aluminoxane used.
[0163] The solid aluminoxane can be any known solid aluminoxane without any restrictions. Known production methods include, for example, those disclosed in JP-B-7-42301, JP-A-6-220126, JP-A-6-220128, JP-A-11-140113, JP-A-11-310607, JP-A-2000-38410, JP-A-2000-95810, and WO2010 / 55652.
[0164] The average particle size of the solid aluminoxane is generally in the range of 0.01 to 50,000 μm, preferably 1 to 1,000 μm, and particularly preferably 1 to 200 μm. The average particle size of solid aluminoxane is determined by observing the particles with a scanning electron microscope, measuring the particle size of 100 or more particles, and averaging the weights. The particle size of solid aluminoxane was determined by measuring the maximum length of the Pythagorean method from the particle image. That is, the length of the particle image sandwiched between two parallel lines in both the horizontal and vertical directions was measured, and the particle size was calculated using the following formula. Particle size = ((horizontal length) 2 +(Vertical length) 2 ) 0.5
[0165] The weight average particle diameter of the solid aluminoxane is calculated from the particle diameter calculated above according to the following formula. Average particle size=Σnd 4 / Σnd 3 (where n is the number of particles and d is the particle size)
[0166] The solid aluminoxane preferably has a specific surface area of 50 to 1000 m 2 / g, more preferably 100 to 800m 2 / g, and the pore volume is preferably 0.1 to 2.5 cm 3 / g.
[0167] As the inorganic halide, MgCl2, MgBr2, MnCl2, MnBr2, etc. can be used. The inorganic halide can be used as it is, or can be used after being pulverized by a ball mill or a vibration mill. In addition, the inorganic halide can be dissolved in a solvent such as alcohol, and then precipitated into fine particles by a precipitating agent.
[0168] The clay is usually composed mainly of clay minerals. The ion-exchangeable layered compound is a compound having a crystal structure in which the planes formed by ionic bonds are stacked in parallel with each other with weak bonding force, and the ions contained therein are exchangeable. Most clay minerals are ion-exchangeable layered compounds. These clays, clay minerals, and ion-exchangeable layered compounds are not limited to natural products, and artificial synthetic products can also be used.
[0169] Examples of the clay, clay mineral, or ion-exchangeable layered compound include ionic crystalline compounds having layered crystal structures such as hexagonal close packing type, antimony type, CdCl2 type, and CdI2 type.
[0170] Furthermore, examples of clay and clay minerals include kaolin, bentonite, kibushi clay, gairome clay, allophane, hisingerite, pyrophyllite, ummo group, montmorillonite group, vermiculite, ryokudeite group, palygorskite, kaolinite, nacrite, dickite, halloysite, etc. Ion-exchangeable layered compounds include crystalline acid salts of polyvalent metals, such as α-Zr(HAsO4)2·H2O, α-Zr(HPO4)2, α-Zr(KPO4)2·3H2O, α-Ti(HPO4)2, α-Ti(HAsO4)2·H2O, α-Sn(HPO4)2·H2O, γ-Zr(HPO4)2, γ-Ti(HPO4)2, and γ-Ti(NH4PO4)2·H2O.
[0171] Such clay, clay mineral, or ion-exchangeable layered compound preferably has a pore volume of 0.1 cc / g or more, particularly preferably 0.3 to 5 cc / g, having a radius of 20 Å or more, as measured by mercury intrusion porosimetry, where the pore volume is measured for a pore radius range of 20 to 30,000 Å by mercury intrusion porosimetry using a mercury porosimeter. When a support having a pore volume of less than 0.1 cc / g and a radius of 20 Å or more is used, it tends to be difficult to obtain high polymerization activity.
[0172] It is also preferable to subject clay and clay minerals to chemical treatment. As the chemical treatment, any of surface treatments that remove impurities attached to the surface and treatments that affect the crystalline structure of the clay can be used. Specific examples of chemical treatments include acid treatment, alkali treatment, salt treatment, and organic treatment. In addition to removing impurities from the surface, acid treatment increases the surface area by eluting cations such as Al, Fe, and Mg in the crystalline structure. In alkali treatment, the crystalline structure of the clay is destroyed, resulting in a change in the structure of the clay. In addition, salt treatment and organic treatment form ion complexes, molecular complexes, organic derivatives, etc., which can change the surface area and interlayer distance.
[0173] The ion-exchangeable layered compound may be a layered compound in which the space between layers is expanded by utilizing the ion exchangeability and exchanging the exchangeable ions between layers with other large bulky ions. Such bulky ions play a role of supporting the layered structure and are usually called pillars. The introduction of another substance between layers of a layered compound in this way is called intercalation. Examples of guest compounds to be intercalated include cationic inorganic compounds such as TiCl4 and ZrCl4, metal alkoxides such as Ti(OR)4, Zr(OR)4, PO(OR)3, and B(OR)3 (R is a hydrocarbon group, etc.), [Al 13 O4(OH) 24 ] 7+ , [Zr4(OH) 14 ] 2+ , [Fe3O(OCOCH3)6] + Metal hydroxide ions such as these can be used. These compounds can be used alone or in combination of two or more. When intercalating these compounds, polymers obtained by hydrolysis of metal alkoxides (R indicates a hydrocarbon group, etc.) such as Si(OR)4, Al(OR)3, Ge(OR)4, and colloidal inorganic compounds such as SiO2 can also be used. Examples of pillars include oxides produced by intercalating the above metal hydroxide ions between layers and then dehydrating them with heat.
[0174] The clay, clay mineral, and ion-exchangeable layered compound may be used as is, or after treatment such as ball milling or sieving. They may also be used after adding and adsorbing new water or after heat dehydration treatment. Furthermore, they may be used alone or in combination of two or more kinds. Of these, clay or clay minerals are preferred, and montmorillonite, vermiculite, pectolite, taeniolite and synthetic mica are particularly preferred.
[0175] When the carrier (C) is an organic compound, the organic compound may be a granular or fine particle solid having a particle size in the range of 10 to 300 μm.Specific examples of the organic compound include (co)polymers mainly composed of α-olefins having 2 to 14 carbon atoms, such as ethylene, propylene, 1-butene, and 4-methyl-1-pentene, or (co)polymers mainly composed of vinylcyclohexane and styrene, and modified products thereof.
[0176] The polymerization catalyst may contain the above-mentioned organometallic complex (A), the above-mentioned compound (B), and, if necessary, the support (C), as well as the following specific organic compound component (D), if necessary.
[0177] <<(D) Organic compound component>> The organic compound component (D) is used, if necessary, for the purpose of improving the polymerization performance of the polymerization catalyst and the physical properties of the resulting polymer (for example, the molecular weight of the resulting polymer) (increasing the molecular weight). Examples of such organic compounds include, but are not limited to, alcohols, phenolic compounds, carboxylic acids, phosphorus compounds, and sulfonates.
[0178] The alcohols and phenolic compounds are generally selected from the group consisting of R 22 The formula represented by -OH is used, where R 22 represents a hydrocarbon group having 1 to 50 carbon atoms (6 to 50 carbon atoms in the case of phenols) or a halogenated hydrocarbon group having 1 to 50 carbon atoms (6 to 50 carbon atoms in the case of phenols).
[0179] Alcohols include R 22 The phenolic compound is preferably one in which the α,α'-positions of the hydroxyl group are substituted with a hydrocarbon having 1 to 20 carbon atoms.
[0180] The carboxylic acid is usually R 23 The one represented by -COOH is used. 23 represents a hydrocarbon group having 1 to 50 carbon atoms or a halogenated hydrocarbon group having 1 to 50 carbon atoms, and is particularly preferably a halogenated hydrocarbon group having 1 to 50 carbon atoms.
[0181] As the phosphorus compound, phosphoric acids having a P-O-H bond, phosphates having a P-OR or P=O bond, and phosphine oxide compounds are preferably used. The sulfonate salt includes those represented by the following general formula (Da).
[0182] [ka]
[0183] In the general formula (Da), M 5 is an atom in groups 1 to 14 of the periodic table, and R 24 represents hydrogen, a hydrocarbon group having 1 to 20 carbon atoms, or a halogenated hydrocarbon group having 1 to 20 carbon atoms; Z represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, or a halogenated hydrocarbon group having 1 to 20 carbon atoms; t represents an integer of 1 to 7; u represents an integer of 1 to 7; and tu is 1 or greater.
[0184] [Method for producing olefin polymer] The method for producing an olefin polymer according to the present invention includes a step of polymerizing an olefin in the presence of the polymerization catalyst. The method for producing an olefin-cyclic olefin copolymer according to the present invention includes a step of polymerizing an olefin and a cyclic olefin in the presence of the polymerization catalyst. As described above, the term "olefin" as used herein refers to any compound having a polymerizable double bond.
[0185] In the polymerization, the components constituting the catalyst of the present invention may be used in any manner and added in any order to a polymerization vessel. Examples of the manner include the following. (1) A method in which the organometallic complex (A) is added alone to a polymerization reactor. (2) A method in which the organometallic complex (A) and the compound (B) are added to a polymerization reactor in any order. (3) A method in which a catalyst component in the form of an organometallic complex (A) supported on a carrier (C) and a compound (B) are added to a polymerization reactor in any order. (4) A method in which a catalyst component in which the compound (B) is supported on a carrier (C) and an organometallic complex (A) are added to a polymerization reactor in any order. (5) A method in which a catalyst component in which an organometallic complex (A) and a compound (B) are supported on a carrier (C) is added to a polymerization reactor. (6) A method in which a catalyst component in which an organometallic complex (A) and a compound (B) are supported on a carrier (C), and the compound (B) are added to a polymerization vessel in any order. In this case, the compound (B) supported on the carrier (C) and the compound (B) added alone may be the same or different. (7) A method in which a catalyst component in which the compound (B) is supported on a carrier (C), and an organometallic complex (A) are added to a polymerization reactor in any order. (8) A method in which the catalyst component in which compound (B) is supported on carrier (C), organometallic complex (A), and compound (B) are added to a polymerization vessel in any order. In this case, compound (B) supported on carrier (C) and compound (B) added alone may be the same or different. (9) A method in which an organometallic complex (A) supported on a carrier (C) and a compound (B) supported on a carrier (C) are added to a polymerization reactor in any order. (10) A method of adding a component in which an organometallic complex (A) is supported on a carrier (C), a component in which a compound (B) is supported on a carrier (C), and a compound (B) to a polymerization vessel in any order. In this case, the compound (B) supported on the carrier (C) and the compound (B) added alone may be the same or different. (11) A method in which the organometallic complex (A), the compound (B), and the organic compound component (D) are added to a polymerization reactor in any order. (12) A method in which the compound (B) and the organic compound component (D) which have been contacted in advance, and the organometallic complex (A) are added to a polymerization reactor in any order. (13) A method in which the compound (B), the organic compound component (D) supported on the carrier (C), and the organometallic complex (A) are added to a polymerization reactor in any order. (14) A method in which a catalyst component in which an organometallic complex (A) and a compound (B) have been contacted in advance, and an organic compound component (D) are added to a polymerization reactor in any order. (15) A method in which a catalyst component in which an organometallic complex (A) is contacted with a compound (B) in advance, compound (B), and an organic compound component (D) are added to a polymerization reactor in any order. (16) A method in which a catalyst component in which an organometallic complex (A) is contacted with a compound (B) in advance, and a component in which a compound (B) is contacted with an organic compound component (D) in advance are added to a polymerization vessel in any order. In this case, the compound (B) contacted with the organometallic complex (A) and the compound (B) contacted with the organic compound component (D) may be the same or different. (17) A method in which an organometallic complex (A) supported on a carrier (C), a compound (B), and an organic compound component (D) are added to a polymerization reactor in any order. (18) A method in which an organometallic complex (A) supported on a carrier (C) and a compound (B) previously contacted with an organic compound component (D) are added to a polymerization reactor in any order. (19) A method in which a catalyst component prepared by previously contacting an organometallic complex (A), a compound (B) and an organic compound component (D) in any order is added to a polymerization reactor. (20) A method in which a catalyst component in which an organometallic complex (A), a compound (B) and an organic compound component (D) have been contacted in advance, and compound (B) are added to a polymerization vessel in any order. In this case, compound (B) that is contacted with organometallic complex (A) and organic compound component (D) and compound (B) that is added alone may be the same or different. (21) A method of adding a catalyst comprising an organometallic complex (A), a compound (B) and an organic compound component (D) supported on a carrier (C) to a polymerization reactor. (22) A method of adding a catalyst component in which an organometallic complex (A), a compound (B) and an organic compound component (D) are supported on a carrier (C), and component (B) to a polymerization vessel in any order. In this case, the compound (B) supported on the carrier (C) and the compound (B) added alone may be the same or different.
[0186] In the solid catalyst component having the organometallic complex (A) supported on the support (C) and the solid catalyst component having the organometallic complex (A) and the compound (B) supported on the support (C), an olefin may be prepolymerized, or a catalyst component may be further supported on the prepolymerized solid catalyst component.
[0187] In the method for producing an olefin polymer according to the present invention, the (co)polymerization can be carried out by either a liquid phase polymerization method such as solution polymerization or suspension polymerization, or a gas phase polymerization method. Specific examples of the inert hydrocarbon medium used in the liquid phase polymerization method include aliphatic hydrocarbons such as propane, butane, pentane, hexane, heptane, octane, decane, dodecane, and kerosene; alicyclic hydrocarbons such as cyclopentane, cyclohexane, and methylcyclopentane; aromatic hydrocarbons such as benzene, toluene, and xylene; halogenated hydrocarbons such as ethylene chloride, chlorobenzene, and dichloromethane, and mixtures thereof. The olefin itself to be subjected to the (co)polymerization can also be used as a solvent.
[0188] When olefin polymerization is carried out using the above polymerization catalyst, the organometallic complex (A) is usually used in an amount of 1×10 -12 ~1×10 -2 Molar, preferably 1 x 10 -10 ~1×10 -3 It is used in molar amounts.
[0189] The organometallic compound (B-1) is used in an amount such that the molar ratio [(B-1) / M] of the organometallic compound (B-1) to the total transition metal atoms (M) in the organometallic complex (A) is usually 0.01-100,000, preferably 0.05-50,000. The organoaluminum oxy compound (B-2) is used in an amount such that the molar ratio [(B-2) / M] of the aluminum atoms in the organoaluminum oxy compound (B-2) to the total transition metals (M) in the organometallic complex (A) is usually 10-500,000, preferably 20-100,000. The compound (ionizing ionic compound) (B-3) that reacts with the organometallic complex (A) to form an ion pair is used in an amount such that the molar ratio [(B-3) / M] of the ionizing ionic compound (B-3) to the transition metal atoms (M) in the organometallic complex (A) is usually 1-10, preferably 1-5.
[0190] The organic compound component (D) is used in an amount such that the molar ratio [(D) / (B-1)] to the organometallic compound (B-1) is usually 0.01 to 10, preferably 0.1 to 5. The organic compound component (D) is used in an amount such that the molar ratio [(D) / (B-2)] to the organoaluminum oxy compound (B-2) is usually 0.001 to 2, preferably 0.005 to 1. The organic compound component (D) is used in an amount such that the molar ratio [(D) / (B-3)] to the ionizing ionic compound (B-3) is usually 0.01 to 10, preferably 0.1 to 5.
[0191] The polymerization temperature of the olefin using such an olefin polymerization catalyst is usually in the range of −50 to +200° C., preferably 0 to 170° C. The polymerization pressure is usually normal pressure to 100 kg / cm. 2 -G, preferably normal pressure to 50 kg / cm 2 Under the conditions of -G, the polymerization reaction can be carried out in any of batch, semi-continuous and continuous modes. Furthermore, the polymerization can be carried out in two or more stages with different reaction conditions.
[0192] The molecular weight of the resulting olefin polymer can be adjusted by adding hydrogen to the polymerization system or by changing the polymerization temperature. It can also be adjusted by the amount of compound (B) used. When hydrogen is added, the appropriate amount is about 0.001 to 5,000 NL per kg of the resulting copolymer.
[0193] In the process for producing an olefin polymer, the olefin to be subjected to the polymerization reaction may be a linear or branched α-olefin, and is preferably an olefin defined by the following (Z-1).
[0194] In the method for producing an olefin-cyclic olefin copolymer, the olefin to be subjected to the polymerization reaction may, for example, be a linear or branched α-olefin, and preferably, the olefin defined in (Z-1) and the cyclic olefin defined in (Z-2) below.
[0195] <<(Z-1) Linear or branched α-olefins with 2 to 30 carbon atoms>> The linear or branched α-olefin may be a linear or branched α-olefin (Z-1) having 2 to 30 carbon atoms.
[0196] The α-olefin (Z-1) preferably has 2 to 20 carbon atoms, more preferably 2 to 10 carbon atoms, and further preferably 2 to 5 carbon atoms. Specific examples of the α-olefin (Z-1) include ethylene, propylene, 1-butene, 2-butene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene. Linear olefins are more preferred, and ethylene is particularly preferred.
[0197] <<(Z-2) Cyclic Olefins>> The cyclic olefin may be at least one cyclic olefin (Z-2) selected from the group consisting of compounds represented by the following general formula [ZI], general formula [Z-II], general formula [Z-III], general formula [Z-IV] or general formula [ZV].
[0198] [ka]
[0199] In the general formula [ZI], u is 0 or 1; v is 0 or a positive integer, w is 0 or 1, R 61 ~R 78 And R a1 and R b1 are each independently selected from a hydrogen atom, a halogen atom, and a hydrocarbon group; R 75 ~R 78 may be bonded to each other to form a monocyclic or polycyclic ring, and the monocyclic or polycyclic ring may have a double bond; 75 and R 76 With or R 77 and R 78 and may form an alkylidene group.
[0200] [ka]
[0201] In the general formula [Z-II], x and d are 0 or an integer of 1 or more, y and z are 0, 1 or 2; R 81 ~R 99 are each independently selected from a hydrogen atom, a halogen atom, and a hydrocarbon group; R 89 and R 90 and the carbon atom to which R is bonded. 93 or the carbon atom to which R is bonded 91 may be bonded directly or via an alkylene group having 1 to 3 carbon atoms, and when y=z=0, R 95 and R 92 or R 95 and R 99 may be bonded to each other to form a monocyclic or polycyclic aromatic ring.
[0202] [ka]
[0203] In the general formula [Z-III], R 100 and R 101 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 5 carbon atoms, and f is 1≦f≦18.
[0204] [ka]
[0205] In the general formula [Z-IV], x is 0 or an integer of 1 or more, R 111 ~R 118 are each independently selected from a hydrogen atom, a halogen atom, and a hydrocarbon group; R 121 ~R 124 are each independently selected from a hydrogen atom, a halogen atom, and a hydrocarbon group, and two adjacent groups may be bonded to each other to form a monocyclic or polycyclic aromatic ring.
[0206] [ka]
[0207] In the general formula [ZV], n and m are each independently 0, 1 or 2, q is 1, 2 or 3, and R 18 ~R 31 each independently represents a hydrogen atom, a halogen atom other than a fluorine atom, or a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom other than a fluorine atom, and when q=1, R 28 and R 29 , R 29 and R 30 , R 30 and R 31 may be bonded to each other to form a monocyclic or polycyclic ring, and when q=2 or 3, R 28 and R 28 , R 28 and R 29 , R 29 and R 30 , R 30 and R 31 , R 31 and R 31 may be bonded to each other to form a monocycle or polycycle, the monocycle or polycycle may have a double bond, and the monocycle or polycycle may be an aromatic ring.
[0208] General formula [ZI], general formula [Z-II], general formula [Z-III], general formula [Z-IV], general formula [ZV], and general formula [Z-VI] are described in detail below.
[0209] <<General formula [ZI]>> In the general formula [ZI], u is 0 or 1, v is 0 or a positive integer, and w is 0 or 1. When w is 1, the ring represented by w is a 6-membered ring, and when w is 0, the ring is a 5-membered ring.
[0210] R 61 ~R 78 And R a1 and R b1 may be the same or different and are a hydrogen atom, a halogen atom, or a hydrocarbon group. Here, the halogen atom is a fluorine atom, a chlorine atom, a bromine atom or an iodine atom.
[0211] Examples of the hydrocarbon group include linear or branched alkyl groups having 1 to 30 carbon atoms, preferably 1 to 20 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, neopentyl, and n-hexyl; linear or branched alkenyl groups having 2 to 30 carbon atoms, more preferably 2 to 20 carbon atoms, such as vinyl, allyl, and isopropenyl; linear or branched alkynyl groups having 2 to 30 carbon atoms, preferably 2 to 20 carbon atoms, such as ethynyl and propargyl; cyclopropyl, cyclobutyl, cyclopentyl, and cyclohexyl. cycloalkyl groups having 3 to 30 carbon atoms, preferably 3 to 20 carbon atoms, such as cyclooctyl, adamantyl, norbornyl, and tetracyclododecyl; cyclic unsaturated hydrocarbon groups having 5 to 30 carbon atoms, such as cyclopentadienyl, indenyl, and fluorenyl; aryl groups having 6 to 30 carbon atoms, preferably 6 to 20 carbon atoms, such as phenyl, benzyl, naphthyl, biphenyl, terphenyl, phenanthryl, and anthracenyl; and alkyl-substituted aryl groups, such as tolyl, isopropylphenyl, t-butylphenyl, dimethylphenyl, and di-t-butylphenyl.
[0212] The above-mentioned hydrocarbon group may have a hydrogen atom substituted with a halogen, and examples thereof include monotrifluoromethyl, ditrifluoromethyl, monofluorophenyl, difluorophenyl, trifluorophenyl, pentafluorophenyl, and chlorophenyl, which have 1 to 30 carbon atoms, and are preferably halogenated alkyl or aryl groups having 1 to 20 carbon atoms.
[0213] The above-mentioned hydrocarbon groups may be substituted with other hydrocarbon groups, for example, aryl-substituted alkyl groups such as benzyl and cumyl groups. Further, the above-mentioned hydrocarbon group may be a heterocyclic compound residue; an oxygen-containing group such as an alkoxy group, an aryloxy group, an ester group, an ether group, an acyl group, a carboxy group, a carbonate group, a hydroxy group, a peroxy group, or a carboxylic anhydride group; a nitrogen-containing group such as an amino group, an imino group, an amido group, an imido group, a hydrazino group, a hydrazono group, a nitro group, a nitroso group, a cyano group, an isocyano group, a cyanate ester group, an amidino group, a diazo group, or an amino group in the form of an ammonium salt; a boranediyl group, a boranetriyl group, a diboranyl group, or the like. The compound may have a uridine-containing group; a sulfur-containing group such as a mercapto group, a thioester group, a dithioester group, an alkylthio group, an arylthio group, a thioacyl group, a thioether group, a thiocyanate group, an isocyanate group, a sulfone ester group, a sulfonamide group, a thiocarboxyl group, a dithiocarboxyl group, a sulfo group, a sulfonyl group, a sulfinyl group, or a sulfenyl group; a phosphorus-containing group such as a phosphido group, a phosphoryl group, a thiophosphoryl group, or a phosphite group; a silicon-containing group; a germanium-containing group; or a tin-containing group.
[0214] Preferred examples of the hydrocarbon group include linear or branched alkyl groups having 1 to 30, preferably 1 to 20, carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, t-butyl, neopentyl, and n-hexyl; cycloalkyl groups having 3 to 30, preferably 3 to 20, carbon atoms, such as cyclopropyl, cyclobutyl, cyclohexyl, cycloheptyl, cyclooctyl, adamantyl, norbornyl, and tetracyclododecyl; aryl groups having 6 to 30, preferably 6 to 20, carbon atoms, such as phenyl, naphthyl, biphenyl, terphenyl, phenanthryl, and anthracenyl; and substituted aryl groups in which these aryl groups are substituted with 1 to 5 substituents, such as halogen atoms, alkyl groups or alkoxy groups having 1 to 30, preferably 1 to 20, carbon atoms, or aryl groups or aryloxy groups having 6 to 30, preferably 6 to 20, carbon atoms.
[0215] Furthermore, in the above general formula [ZI], R 75 and R 76 But, R 77 and R 78 But, R 75 and R 77 But, R 76 and R 78 But, R 75 and R 78 Toga or R 76 and R 77 and may be bonded together (together with each other) to form a monocyclic or polycyclic group, and the monocyclic or polycyclic group thus formed may have a double bond. Specific examples of the monocyclic or polycyclic group formed here include the following:
[0216] [ka]
[0217] In the above examples, the carbon atoms numbered 1 and 2 correspond to R 75 (R 76 ) or R 77 (R 78 ) represents the carbon atom to which the atom is bonded. Also, R 75 and R 76 With or R 77 and R 78 and the like may form an alkylidene group. Such an alkylidene group is usually an alkylidene group having 2 to 20 carbon atoms, and specific examples of such an alkylidene group include ethylidene, propylidene, and isopropylidene.
[0218] <<General formula [Z-II]>> In the general formula [Z-II], x and d are 0 or a positive integer, and y and z are 0, 1, or 2.
[0219] Also, R 81 ~R 99 may be the same or different and are a hydrogen atom, a halogen atom, or a hydrocarbon group. Examples of the halogen atom and the hydrocarbon group include the same as those in the above general formula [ZI].
[0220] Here, R 89 and R 90 and the carbon atom to which R is bonded. 93 or the carbon atom to which R is bonded 91 The carbon atom to which R is bonded may be bonded directly or via an alkylene group having 1 to 3 carbon atoms. In other words, when the above two carbon atoms are bonded via an alkylene group, R 89 and R 93 Or, R 90 and R 91 and combine with each other to form an alkylene group which is either a methylene group (-CH2-), an ethylene group (-CH2CH2-), or a propylene group (-CH2CH2CH2-).
[0221] Furthermore, when y=z=0, R 95 and R 92 or R 95 and R 99 may be bonded to each other to form a monocyclic or polycyclic aromatic ring. Specifically, when y=z=0, R 95 and R 92 Examples of aromatic rings formed by the above formula include the following aromatic rings:
[0222] [ka]
[0223] Here, l is the same as d in the above general formula [Z-II].
[0224] <<General formula [Z-III]>> In the general formula [Z-III], R 100 and R 101 may be the same or different and are a hydrogen atom or a hydrocarbon group having 1 to 5 carbon atoms, and f is 1≦f≦18.
[0225] The hydrocarbon group having 1 to 5 carbon atoms is preferably an alkyl group, a halogenated alkyl group, or a cycloalkyl group. Specific examples of these are R 61 ~R 78 This is similar to the specific example above.
[0226] <<General formula [Z-IV]>> In the general formula [Z-IV], x is 0 or an integer of 1 or more. R 111 ~R 118 and R 121 ~R 124 are selected from a hydrogen atom, a halogen atom, and a hydrocarbon group, and may be the same or different.
[0227] Examples of the halogen atom and the hydrocarbon group include the same as those in the above general formula [ZI]. Also, R 121 ~R 124 Two adjacent groups may be bonded to each other to form a monocyclic or polycyclic aromatic ring. 121 and R 122 Specific examples of cyclic olefins in which an aromatic ring is formed by bonding include the following structures.
[0228] [ka]
[0229] [ka]
[0230] Also, R 122 and R 123 Specific examples of cyclic olefins in which an aromatic ring is formed by bonding include the following structures.
[0231] [ka]
[0232] [ka]
[0233] Also, R 121 and R 122 , R 123 and R 124 Specific examples of cyclic olefins in which an aromatic ring is formed by bonding include the following structures.
[0234] [ka]
[0235] Examples also include cyclic olefins in which the aromatic ring is substituted with a substituent selected from a halogen atom, an alkyl group, and an aryl group.
[0236] <<General formula [ZV]>> In the general formula [ZV], m and n are 0, 1 or 2; R 18 ~R 31 each independently represents a hydrogen atom, a halogen atom other than a fluorine atom, or a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom other than a fluorine atom; R 28 and R 29 , R 29 and R 30 , R 30 and R 31 may be bonded to each other to form a monocyclic ring, and the monocyclic ring may have a double bond.
[0237] In the general formula [ZV], m is preferably 0 or 1, and more preferably 1. n is preferably 0 or 1, and more preferably 0. R 18 ~R 31 is preferably a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, and more preferably a hydrogen atom.
[0238] Examples of the hydrocarbon group having 1 to 20 carbon atoms include, independently, an alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 15 carbon atoms, and an aromatic hydrocarbon group. More specifically, examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, an amyl group, a hexyl group, an octyl group, a decyl group, a dodecyl group, and an octadecyl group. Examples of the cycloalkyl group include a cyclohexyl group. Examples of the aromatic hydrocarbon group include an aryl group or an aralkyl group such as a phenyl group, a tolyl group, a naphthyl group, a benzyl group, and a phenylethyl group. These hydrocarbon groups may be substituted with a halogen atom other than a fluorine atom.
[0239] <<General formula [Z-VI]>>
[0240] [ka]
[0241] In the above general formula (Z-VI), n and q each independently represent 0, 1, or 2. 1 ~R 17 each independently represents a hydrogen atom, a halogen atom other than a fluorine atom, or a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom other than a fluorine atom; R 10 ~R 17 One of them is a bond. Also, when q=0, R 10 and R 11 , R 11 and R 12 , R 12 and R 13 , R 13 and R 14 , R 14 and R 15 , R 15 and R 10 may be bonded to each other to form a monocyclic or polycyclic ring. When q=1 or 2, R 10 and R 11 , R 11 and R 17 , R 17 and R 12 , R 12 and R 13 , R 13 and R 14 , R 14 and R 15 , R 15 and R 16 , R 16 and R 16 , R 17 and R 17 , R 16 and R 10 may be bonded to each other to form a monocycle or polycycle, and the monocycle or polycycle may have a double bond, or the monocycle or polycycle may be an aromatic ring.
[0242] Preferred specific examples of the cyclic olefins represented by the above general formula [ZI], [Z-II], [Z-III], [Z-IV], [ZV] or [Z-VI] include tetracyclo[4.4.0.1 2,5 .1 7,10
[0176] to
[0207] of JP2011-122146A, such as 1,4-dihydro-1,4-methanonaphthalene (benzonorbornadiene: BNBD) and 1,4-methano-1,4,4a,9a-tetrahydrofluorene are also preferred cyclic olefins.
[0243] These cyclic olefins (Z-2) represented by the general formula [ZI], [Z-II], [Z-III], [Z-IV], [ZV], or [Z-VI] may be used alone or in combination of two or more.
[0244] In the method for producing an olefin polymer of the present invention, olefins other than the above-mentioned (Z-1) and (Z-2) may be subjected to the polymerization reaction. Examples of such olefins include conjugated / non-conjugated polyenes and vinylcyclohexane. Among these, cyclic ones may be used as comonomers in the method for producing an olefin-cyclic olefin copolymer of the present invention.
[0245] The conjugated / non-conjugated polyenes include cyclic or chain hydrocarbons having 4 to 30, preferably 4 to 20, carbon atoms and two or more double bonds. Specific examples thereof include butadiene, isoprene, 4-methyl-1,3-pentadiene, 1,3-pentadiene, 1,4-pentadiene, 1,5-hexadiene, 1,4-hexadiene, 1,3-hexadiene, 1,3-octadiene, 1,4-octadiene, 1,5-octadiene, 1,6-octadiene, 1,7-octadiene, ethylidenenorbornene (ENB), vinylnorbornene, dicyclopentadiene, 7-methyl-1,6-octadiene, 4-ethylidene-8-methyl-1,7-nonadiene, and 5,9-dimethyl-1,4,8-decatrienebutadiene, which are exemplified in paragraph
[0211] of JP2011-122146A.
[0246] In the method for producing an olefin-cyclic olefin copolymer, a polymerizable compound other than an olefin may be polymerized together with the above-mentioned olefin. Examples of such a polymerizable compound include a compound having a polar group and a polymerizable unsaturated bond, an aromatic vinyl compound, and a functional group-containing styrene derivative.
[0247] Specific examples of the compound having a polar group and a polymerizable unsaturated bond include the compounds exemplified as unsaturated hydrocarbons having a polar group in paragraphs
[0208] to
[0211] of JP2011-122146A.
[0248] Specific examples of the aromatic vinyl compound and the functional group-containing styrene derivative include the compounds exemplified in paragraph
[0211] of JP-A-2011-122146. Preferred embodiments of the production method of the present invention include a copolymerization of the α-olefin (Z-1) with the cyclic olefin (Z-2) and a copolymerization of the α-olefin (Z-1) with a cyclic conjugated / non-conjugated polyene. In this embodiment, the α-olefin (Z-1) is preferably ethylene, and the cyclic olefin (Z-2) is preferably tetracyclo[4.4.0.1 2,5 .1 7,10 ]-3-dodecene, 1,4-dihydro-1,4-methanonaphthalene (benzonorbornadiene: BNBD), 1,4-methano-1,4,4a,9a-tetrahydrofluorene, bicyclo[2,2,1]hept-2-ene, and methylphenylnorbornene are preferred. As the cyclic conjugated / non-conjugated polyene, ethylidenenorbornene (ENB) is preferred.
[0249] In copolymerizing the α-olefin (Z-1) and the cyclic olefin (Z-2), the pressure of the α-olefin (Z-1) and the concentration of the cyclic olefin (Z-2) can be set arbitrarily and are not particularly limited. The pressure of the α-olefin (Z-1) is preferably the polymerization pressure, and the concentration of the cyclic olefin (Z-2) is 0.001 to 100 mol / L, preferably 0.001 to 10 mol / L, more preferably 0.001 to 1 mol / L.
[0250] [Physical properties of olefin polymers and olefin-cyclic olefin copolymers] -Molecular weight- The molecular weight of the olefin polymer and the olefin-cyclic olefin copolymer is determined from the intrinsic viscosity measured in decalin at 135° C. and is preferably 0.1 to 10.0. The lower limit is more preferably 0.2, and even more preferably 0.4. On the other hand, the upper limit is more preferably 8.0, and even more preferably 7.0. As long as the intrinsic viscosity of the olefin polymer and olefin-cyclic olefin copolymer is within the above range, they will have a good balance of moldability, strength, transparency, etc., and can be suitably used in cases where strength (toughness) is required as a mechanical property.
[0251] The weight average molecular weight (Mw) of the olefin polymer and the olefin-cyclic olefin copolymer is preferably 1,000 to 5,000,000, and more preferably 5,000 to 2,000,000. The molecular weight distribution (Mw / Mn) of the olefin polymer and the olefin-cyclic olefin copolymer is preferably 1.5 to 10.0, and more preferably 1.8 to 6.0. The weight average molecular weight (Mw) and the molecular weight distribution (Mw / Mn) are determined by the measurement methods described in the Examples section below.
[0252] -Glass transition temperature (Tg)- The glass transition temperature (Tg) of the olefin polymer and olefin-cyclic olefin copolymer is preferably in the range of, for example, 100° C. to 250° C. The lower limit is preferably 110° C. On the other hand, the upper limit is more preferably 230° C., and further preferably 220° C., from the viewpoint of the heat resistance stability of the polymer during melt molding. The glass transition temperature can be determined by the method described in the examples below. EXAMPLES
[0253] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.
[0254] [Measurement method] The organometallic complex (A) is 1 H-NMR spectra (400 MHz, JEOL Ltd., model number: JNM-ECZ400S / L1 or 500 MHz, Bruker Biospin, model: AVANCE NEO cryo-500), FD-mass (hereafter referred to as FD-MS) spectra (JEOL Ltd., model number: JMS-T200GC), etc. were measured and identified.
[0255] The physical properties of the ethylene / propylene copolymer and ethylene / 5-ethylidene-2-norbornene (ENB) copolymer synthesized below were measured by the following methods.
[0256] [Propylene and ENB content] The comonomer content of the copolymer was measured by FT-IR (model FT-IR410 infrared spectrophotometer, manufactured by JASCO Corporation).
[0257] (FT-IR measurement method) For FT-IR, the polymer obtained in the examples was heated to 135°C, melt-stretched in a hot press, and then cooled under pressure at room temperature to obtain a film, which was used as a measurement sample, and the 1-octene structural unit content was measured using a calibration curve. The ethylene / 1-octene copolymer sample used for creating the calibration curve was measured under the same conditions as above. 13 The comonomer content was determined by C-NMR measurement.
[0258] The physical properties of the ethylene / tetracyclododecene (TD) copolymer and the ethylene / benzonorbornadiene (BNBD) copolymer were measured by the following methods.
[0259] [Polymer glass transition temperature (Tg)] DSC measurement was carried out under the following conditions to determine the Tg of the polymer. Using a differential scanning calorimeter (Hitachi High-Tech Science Co., Ltd., model number: DSC7020AS-3D), approximately 5.0 mg of a polymer sample was heated from 30°C to 250°C at a heating rate of 10°C / min under a nitrogen atmosphere and held at that temperature for 5 minutes. The sample was then cooled to -20°C at a heating rate of 10°C / min, held at that temperature for 5 minutes, and then heated to 250°C at a heating rate of 10°C / min. During this second heating, the DSC curve was bent due to a change in specific heat, and the baseline was sensed as moving in parallel, so the temperature at the intersection of the tangent of the baseline lower than this bending and the tangent of the point where the slope at the bending part is maximum was determined as the glass transition temperature (Tg).
[0260] [Polymer intrinsic viscosity [η]] The intrinsic viscosity [η] (dl / g) of the olefin polymer was measured in decalin at 135° C. in accordance with the method of JIS K7367 standard.
[0261] [Weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn)] The weight average molecular weight (Mw) and number average molecular weight (Mn) of the ethylene / propylene / ENB copolymer were determined by gel permeation chromatography (GPC). They were calculated from the molecular weight distribution curve obtained by a gel permeation chromatograph (high temperature size exclusion chromatograph) "HLC-8321 GPC / HT type" manufactured by Tosoh Corporation, and the operating conditions were as follows:
[0262] <Apparatus and conditions used> Measuring device: Gel permeation chromatograph HLC-8321 GPC / HT type (Tosoh Corporation) Analysis software: Chromatography Data System Empower (registered trademark), manufactured by Waters Column: TSKgel GMH6-HT x 2 + TSKgel GMH6-HT x 2 (inner diameter 7.5 mm x length 30 cm, (Tosoh Corporation) Mobile phase: o-dichlorobenzene [ODCB] Detector: Differential refractometer (built into the device) Column temperature: 140°C Flow rate; 1.0mL / min Injection volume: 400μL Sampling time interval: 1 second Sample concentration: 0.15% (w / v) Molecular weight calibration: Monodisperse polystyrene (Tosoh Corporation) / Molecular weight #3 std set
[0263] <<Synthesis of organometallic complex F>> A thermometer and a three-way cock were attached to a thoroughly dried 300mL three-neck flask. Under a nitrogen atmosphere, 0.51 grams of palladium dibenzylideneacetonepalladium (0), 1.02 grams of 4,5-bis(diphenylphosphino)-9,9-dimethylxanthene, 11.9 grams of sodium t-butoxide, and 130mL of dehydrated toluene were added. 11.1mL of 1-bromo-2-iodobenzene was added dropwise while stirring at room temperature, and then 8.1mL of aniline was slowly added dropwise. A condenser was attached to the flask, and the mixture was heated and refluxed under a nitrogen atmosphere for 2 hours. The mixture was cooled to room temperature to obtain a slurry containing insoluble matter. An adapter with a side tube was attached to a 500mL eggplant flask, a glass filter was attached to the top of the adapter, and a vacuum line was attached to the side tube of the adapter. Silica gel was added to the glass filter, and toluene was added and stirred to suspend the mixture. The flask was depressurized and the toluene was sucked out. While reducing the pressure in the flask, the slurry after the reaction was slowly added onto the silica gel and insoluble matter was filtered. After filtration, toluene was added onto the silica gel and suction filtered. This suction filtration was repeated several times to extract the soluble matter. The toluene solution in the flask was concentrated using a rotary evaporator to obtain 24.0 grams of crude product. The crude product was purified by silica gel column chromatography to obtain 21.5 grams (yield 98%) of compound A. 1 HNMR(400MHz,CDCl3,297K,δinppm)δ6.08(brs,1H),6.73(t,J=7.3Hz,1H),7.04(t,J=7.3Hz,1H),7.10-7.39(m,6H),7.52(d,J=8.0Hz,1H)
[0264] [ka]
[0265] A thermometer and a three-way cock were attached to a thoroughly dried 300mL three-neck flask. Under a nitrogen atmosphere, 11.0 grams of compound A, 90mL of dehydrated toluene, and 1.68 grams of 4-dimethylaminopyridine were added. 14.5mL of di-tert-butyl dicarbonate was slowly added while stirring at room temperature. A condenser was attached to the flask, and the mixture was heated and refluxed overnight. The mixture was cooled to room temperature, and the flask was cooled in an ice bath. 100mL of water was slowly added dropwise and stirred. The organic layer and the aqueous layer were separated using a separatory funnel. The organic layer was washed with saturated saline, and then the aqueous layer and the organic layer were separated again. Magnesium sulfate was added to the organic layer to dry it, and the magnesium sulfate was removed by filtration. The organic layer was concentrated using a rotary evaporator to obtain 20.2 grams of crude product. The crude product was purified by silica gel column chromatography to obtain 15.1 grams (98% yield) of compound B. 1 H NMR(400 MHz, CDCl3, 298 K, δ in ppm) δ1.44 (s, 9 H), 7.08-7.19 (m, 2 H), 7.24-7.32 (m, 6 H), 7.65 (d, J = 7.8 Hz, 1 H)
[0266] [ka]
[0267] A thermometer, a three-way cock, and a dropping funnel were attached to a thoroughly dried 2000mL three-neck flask. 101 grams of cyclopentadiene obtained by pyrolysis of dicyclopentadiene was dissolved in 800mL of dehydrated methanol, and then 102mL of dehydrated acetone was added. The mixture was cooled until the internal temperature reached -10°C, and 144mL of pyrrolidine was slowly added. After heating to room temperature and stirring for 2 hours, 50mL of acetic acid was added dropwise and stirred, and the reaction liquid was poured into 2L of ice water and stirred. After adding hexane and stirring, the organic layer and the aqueous layer were separated using a separatory funnel. The organic layer was washed with saturated saline and then dried over magnesium sulfate. The magnesium sulfate was removed by filtration, and the filtrate was concentrated using a rotary evaporator to obtain 126.4 grams of crude product. The crude product was distilled under reduced pressure (24 torr, distillation temperature 59°C) to obtain 6,6'-dimethylfulvene (compound C). 1 H NMR(400 MHz, CDCl3, 298 K, δ in ppm) δ2.20 (s, 6 H), 6.50 (m, 4 H).
[0268] [ka]
[0269] A thermometer and a three-way cock were attached to a thoroughly dried 100mL three-neck flask. Under a nitrogen atmosphere, 15.1 grams of compound B and 50mL of dehydrated diethyl ether were added. The solution was thoroughly cooled in a dry ice-acetone bath, and 29.9mL of n-butyllithium hexane solution (1.6M) was slowly added dropwise and stirred for 1 hour. 10.5mL of 6,6-dimethylfulvene was slowly added dropwise and stirred overnight while cooling. The next day, the internal temperature was adjusted to -20°C to -40°C and stirred for 6 hours. Another flask containing water was prepared, and the reaction solution was pressure-fed by a cannula to quench the reaction. Ethyl acetate was added to the quenched reaction solution to extract the soluble matter, and the organic layer and aqueous layer were separated using a separatory funnel. The organic layer was washed with water and a saturated aqueous ammonium chloride solution, respectively, and the organic layer was separated from the aqueous layer. Magnesium sulfate was added to the organic layer to dry it, and the magnesium sulfate was removed by filtration. The organic layer was concentrated using a rotary evaporator to obtain 18.0 grams of crude product. The crude product was purified by silica gel column chromatography to obtain 12.1 g (74% yield) of compound D (light yellow liquid) as a mixture of isomers of cyclopentadienyl groups. 1 H NMR(400 MHz, CDCl3, 298 K, δ in ppm) δ1.22-1.63 (m, 15 H), 2.51-2.93 (m, 2 H), 5.88-6.35 (m, 3 H), 6.95-7.41 (m, 9 H)
[0270] [ka]
[0271] A thermometer and a three-way cock were attached to a thoroughly dried 500mL three-neck flask. Under a nitrogen atmosphere, 11.1 grams of compound D, 220mL of dehydrated dichloromethane, and 3.35 grams of dehydrated pyridine were added and stirred while cooling in an ice bath. 7.85 grams of trimethylsilyl trifluoromethanesulfonate were slowly dripped in, and after the dripping, the temperature was raised to room temperature and stirred for 2 hours. The flask was cooled again in an ice bath and a saturated aqueous solution of sodium bicarbonate was slowly dripped in. The reaction mixture was added to a separatory funnel, and ethyl acetate was added to extract the soluble matter and separate the organic layer and the aqueous layer. The organic layer was washed with water and separated from the aqueous layer. This operation was repeated, and the organic layer was washed with water a total of four times. The organic layer was washed with saturated saline and separated from the aqueous layer. Potassium carbonate was added to the organic layer and dried, and then the potassium carbonate was filtered off. The filtrate was concentrated with a rotary evaporator to obtain a concentrated liquid. Toluene was added to the concentrated liquid, and then it was concentrated with a rotary evaporator. This procedure was repeated three times to obtain 9.3 g of crude product as a mixture of cyclopentadienyl isomers. Compound E was used in the next step without further purification. 1 H NMR(400 MHz, CD3COCD3, 299 K, δ in ppm) δ1.48-1.64 (m, 6H), 2.75-3.23 (m, 2 H, CH-CH2-CH), 5.88-6.08 (m, 1 H, NH), 6.15-6.56 (m, 3 H), 6.66-6.84 (m, 3H), 6.92-7.06(m, 1H), 7.09-7.31(m, 4H), 7.44-7.58(m, 1H)
[0272] [ka]
[0273] A thermometer and a three-way cock were attached to a thoroughly dried 100mL three-neck flask. Under a nitrogen atmosphere, 284.9mg of tetrakisdimethylamidotitanium(IV) and 50mL of dehydrated toluene were added. Under a nitrogen atmosphere, 350mg of compound E was weighed and dissolved in 10mL of dehydrated toluene. The toluene solution of compound E was added to the tetrakisdimethylamidotitanium(IV) solution, and after the addition, the mixture was stirred overnight at 80°C. The flask was brought into a glove box, and the solvent was distilled off using a rotary evaporator to obtain 0.5806 grams of a viscous red oil. The obtained compound F was used in the next step without further purification. The obtained product was analyzed by NMR, and the organometallic complex F (compound F) having the structure shown below was confirmed. 1 H NMR(400 MHz, CDCl3, 295 K, δ in ppm) δ1.67 (s, 6H), 2.96 (s, 12H), 5.56 (t, J = 2.7 Hz, 2H), 6.04 (t, J = 2.7 Hz, 2H), 6.53 (dd, J = 1.4, 7.9 Hz, 1H), 6.80 (tt, J = 1.1, 7.3 Hz, 1H), 6.88 (dd, J = 1.4, 7.3 Hz, 1H), 6.93-7.01 (m, 3H), 7.08-7.15 (m, 2H), 7.44 (dd, J = 1.6, 7.7, 1H).
[0274] [ka]
[0275] <<Synthesis of organometallic complex G>> A thermometer and a three-way cock were attached to a thoroughly dried 100mL three-neck flask. Under a nitrogen atmosphere, 398mg of compound F and 25mL of dehydrated toluene were added and stirred at room temperature. 627mg of dimethyldichlorosilane was added and stirred overnight at 60℃ using an oil bath under a nitrogen atmosphere. The flask was brought into a glove box and low boiling points were removed using a rotary evaporator. The solid was washed with hexane and dried under reduced pressure to obtain a reddish brown solid (compound G) (yield 87%). The obtained product was analyzed by NMR, and the organometallic complex G (compound G) having the structure shown below was confirmed. 1 H NMR(400 MHz, CDCl3, 300 K, δ in ppm) δ1.73 (s, 6H), 6.08 (t, J = 2.7 Hz, 2H), 6.16 (dd, J = 1.5, 8.0 Hz, 2H), 6.73 (t, J = 2.7 Hz, 1H), 7.02-7.07 (m, 1H), 7.11 (td, J = 1.5, 7.3 Hz, 1H), 7.36-7.41 (m, 1H), 7.44-7.53 (m, 4H), 7.59 (dd, J = 1.7, 7.8, 1H).FD-MS m / z 391.1
[0276] [ka]
[0277] <<Synthesis of organometallic complex H>> A thermometer and a three-way cock were attached to a thoroughly dried 100mL three-neck flask. Under a nitrogen atmosphere, 97.1mg of tetrakisdimethylamido zirconium(IV), 20mL of dehydrated toluene, and 100mg of compound E were added. Under a nitrogen atmosphere, the mixture was stirred overnight at 90℃ using an oil bath. The mixture was cooled to room temperature and used directly in the next step. 0.6mL of the solution was sampled, and the solvent was distilled off. The resulting product was analyzed by NMR, confirming that it was organometallic complex H (compound H) having the structure shown below. 1 H NMR(400 MHz, CDCl3, 298 K, δ in ppm) δ1.66 (s, 6H), 2.76 (s, 12H), 5.81 (t, J = 2.7 Hz, 2H), 6.16 (t, J = 2.7 Hz, 2H), 6.66-6.70 (m, 1H), 6.75-6.82 (m, 3H), 6.88-6.94 (m, 1H), 7.02-7.07 (m, 1H), 7.11-7.18 (m, 2H), 7.50 (dd, J = 1.5, 8.0, 1H).
[0278] [ka]
[0279] <<Synthesis of organometallic complex I>> 225 mg of dimethyldichlorosilane was added to the toluene solution obtained in the previous experiment under a nitrogen atmosphere. The mixture was heated and stirred at 60°C overnight, resulting in the formation of a precipitate. The flask was brought into a glove box and filtered through a membrane filter with a pore size of 3 μm. The solid matter obtained was washed with hexane and then dried under reduced pressure to obtain 0.1 g of compound I as a yellow powder. The product obtained was analyzed by NMR, and the organometallic complex H (compound H) having the structure shown below was confirmed. 1 H NMR(400 MHz, CDCl3, 298 K, δ in ppm) δ1.70 (s, 6H), 6.00 (t, J = 2.7 Hz, 2H), 6.40 (dd, J = 1.7, 7.6 Hz, 1H), 6.64 (t, J = 2.7 Hz, 2H), 7.07 (m, 2H), 7.51-7.59 (m, 3H), 7.38-7.45 (m, 3H).
[0280] [ka]
[0281] <<Synthesis of organometallic complex J>> In a thoroughly dried 30 mL Schlenk flask, 143 mg of tetrakisdimethylamidohafnium (IV) was weighed out and dissolved in 15 mL of dehydrated toluene under a nitrogen atmosphere, and then 111 mg of compound E was added. Under a nitrogen atmosphere, the mixture was stirred overnight at 90°C using an oil bath. The resulting solution was used directly in the next step without further purification. 0.6 mL of the solution was sampled and the solvent was distilled off in a glove box. The resulting product was analyzed by NMR, confirming the organometallic complex J (compound J) having the structure shown below. 1 H NMR(400 MHz, CDCl3, 298 K, δ in ppm) δ1.69 (s, 6H), 2.81 (s, 12H), 5.79 (t, J = 2.7 Hz, 2H), 6.15 (t, J = 2.7 Hz, 2H), 6.71 (dd, J = 1.5, 8.0 Hz, 1H), 6.75-6.85 (m, 3H), 6.90-6.96 (m, 1H), 7.03-7.09 (m, 1H), 7.11-7.17 (m, 2H), 7.50 (dd, J = 1.7, 7.8, 1H).
[0282] [ka]
[0283] <<Synthesis of organometallic complex K>> 0.26 grams of dimethyldichlorosilane was added to the toluene solution of compound J prepared above, and the mixture was heated and stirred at 60°C overnight. After the reaction, the flask was brought into a glove box and filtered through a membrane filter with a pore size of 3 μm. The filtrate was concentrated, and the resulting solid was washed with toluene, and the supernatant was removed by decantation. The remaining solid was dried under reduced pressure to obtain 134.6 mg of compound K as a white solid (yield 64%). The obtained product was analyzed by NMR, and the organometallic complex K (compound K) having the structure shown below was confirmed. 1 H NMR(400 MHz, CDCl3, 299 K, δ in ppm) δ1.73 (s, 6H), 5.96 (t, J = 2.7 Hz, 2H), 6.43 (dd, J = 1.5, 8.0 Hz, 1H), 6.54 (t, J = 2.7 Hz, 2H), 6.98-7.04 (m, 1H), 7.06-7.12 (m, 1H), 7.28-7.40 (m, 3H), 7.43-7.49 (m, 2H), 7.54 (dd, J = 1.7, 7.8 Hz, 1H). FD-MS m / z:523.0
[0284] [ka]
[0285] <<Synthesis of organometallic complex O>> A thermometer and a three-way cock were attached to a thoroughly dried 200mL three-neck flask. Under a nitrogen atmosphere, 10 grams of 1-adamantylcyclopentadiene, 4.8mL of dehydrated acetone, and 60mL of dehydrated methanol were added and stirred. The solution was cooled to -10°C, and then 7mL of pyrrolidine was slowly added dropwise. After the dropwise addition, the temperature was raised to room temperature over 1 hour and stirring was continued overnight at room temperature. 5.7mL of acetic acid was slowly added dropwise, and after stirring for about 10 minutes, the reaction solution was poured into 2L of cold water and stirred. After adding tert-butyl dimethyl ether and stirring, the organic layer and the aqueous layer were separated using a separatory funnel. The organic layer was washed with water and saturated saline, and the organic layer was concentrated using a rotary evaporator to obtain 11.6 grams of compound L (yield 97%). The obtained product was used in the next step without further purification. 1 H NMR(400 MHz, CDCl3, 297 K, δ in ppm) δ1.66-2.29 (m, 21H), 6.11 (s, 1H), 6.47-6.62 (m, 2H).
[0286] [ka]
[0287] A thermometer and a three-way cock were attached to a thoroughly dried 500 mL three-neck flask. Under a nitrogen atmosphere, 200 mL of dehydrated diethyl ether and 14.3 g of compound B were added and stirred. The solution was cooled in a dry ice acetone bath and stirred for a while, after which the solution was diluted to 1.6 mol / L. n 18.3 mL of BuLi hexane solution was slowly added dropwise. After the addition, the temperature was raised to -20°C and stirring was continued for 1 hour. 10.9 grams of compound L was weighed and added to the reaction solution. Stirring was continued at -20°C for 4 hours and the temperature was gradually raised to room temperature. Water was added to quench the mixture, and then ethyl acetate was added and stirred. The organic layer and the aqueous layer were separated using a separatory funnel. This operation was repeated, and the organic layer was washed with water a total of four times. The organic layer was washed with a saturated aqueous ammonium chloride solution and saturated saline, and then dried with magnesium sulfate. The magnesium sulfate was filtered off, and the filtrate was concentrated with a rotary evaporator to obtain 24.4 grams of crude product. The crude product was purified by silica gel column chromatography to obtain 12.9 grams of compound M as a mixture of isomers of cyclopentadienyl groups (yield 62%). 1 H NMR(400 MHz, CDCl3, 298 K, δ in ppm) δ1.20-2.17 (m, 30H), 2.36-2.79 (m, 2H), 5.60-6.32 (m, 2H), 6.93-7.34 (m, 9H).
[0288] [ka]
[0289] A thermometer and a three-way cock were attached to a thoroughly dried 200mL three-neck flask. Under a nitrogen atmosphere, 12.9 grams of compound M, 100mL of dehydrated dichloromethane, and 2.9 grams of dehydrated pyridine were added and stirred while cooling in an ice bath. 6.7 grams of trimethylsilyl trifluoromethanesulfonate were slowly dripped in, and the mixture was warmed to room temperature and stirred for 2 hours. The flask was cooled again in an ice bath, and a saturated aqueous solution of sodium bicarbonate was slowly dripped in. The reaction mixture was added to a separatory funnel, ethyl acetate was added to extract the soluble matter, and the organic layer and the aqueous layer were separated. Water was added to the organic layer to wash the organic layer, and the organic layer and the aqueous layer were separated. This operation was repeated four times. The organic layer was washed with saturated saline and separated from the aqueous layer. Potassium carbonate was added to the organic layer to dry it, and the potassium carbonate was filtered off. The filtrate was concentrated using a rotary evaporator, and then toluene was added and concentrated again. This operation was repeated three times, and 10.2 grams of crude product was obtained as a mixture of isomers of cyclopentadienyl groups. Compound N was used in the next step without further purification. 1 H NMR(400 MHz, CD3COCD3, 299 K, δ in ppm) δ1.10-1.99 (m, 21H), 2.68-3.18 (m, 2H), 5.30-6.42 (m, 3H), 6.56-7.56 (m, 9H).
[0290] [ka]
[0291] A thermometer and a three-way cock were attached to a thoroughly dried 200mL three-neck flask. Under a nitrogen atmosphere, 292mg of tetrakisdimethylamidotitanium(IV) and 60mL of dehydrated toluene were added. Under a nitrogen atmosphere, 490mg of compound N was weighed and dissolved in 10mL of dehydrated toluene. The toluene solution of compound N was added to the tetrakisdimethylamidotitanium(IV) solution, and after the addition, the mixture was stirred overnight at 80°C. The flask was brought into a glove box, and the solvent was removed using a rotary evaporator to obtain a reddish-brown product. Hexane was added and stirred well, and the insoluble matter was filtered through a membrane filter with a pore size of 3μm. The filtrate was concentrated to obtain 594mg of a product containing a reddish-brown amide complex. A thermometer and a three-way cock were attached to a thoroughly dried 100mL three-neck flask. The previously synthesized amide complex was dissolved in 45mL of dehydrated toluene and added to the flask, and then 4.6mL of dichlorodimethylsilane was added. After the addition, the mixture was heated and stirred at 60℃ overnight. The toluene was distilled off under reduced pressure in a glove box. 10mL of toluene was added and stirred well, and insoluble matter was removed using a membrane filter with a pore size of 3μm. The filtrate was concentrated once, 20mL of dehydrated hexane was added and stirred, and insoluble matter was removed using a membrane filter with a pore size of 3μm. The filtrate was concentrated, 10mL of dehydrated cyclohexane was added and stirred, and insoluble matter was similarly removed. After concentrating the filtrate, dehydrated cyclohexane was added until the product was dissolved. About four times the amount of dehydrated hexane added was added, and the mixture was left to stand in a nitrogen atmosphere in a freezer at -10℃ for two days. The supernatant was collected by decantation. A small amount of hexane was added to the remaining insoluble matter and allowed to stand, after which the supernatant was collected by decantation and combined with the previous supernatant. The supernatant was concentrated, and a small amount of dehydrated hexane was added to the precipitated solid, which was stirred and allowed to stand. The supernatant was removed by decantation, and 90 mg of compound O was obtained as an orange solid (yield 14%). The obtained product was analyzed by NMR, and the organometallic complex O (compound O) having the structure shown below was confirmed. 1 H NMR(500 MHz, CDCl3, 323 K, δ in ppm) δ1.56 (s, 3H), 1.69-1.78 (m, 6H), 1.84 (s, 3H), 1.96-2.10 (m, 9H), 5.46 (dd, J = 3.3, 2.4 Hz, 1H), 6.17 (dd, J = 7.9, 1.2 Hz, 1H), 6.37 (t, J = 3.3 Hz, 1H), 6.60 (dd, J = 3.3, 2.4 Hz, 1H), 7.00-7.04 (m, 1H), 7.08 (td, J = 7.6, 1.5 Hz, 1H), 7.28-7.57 (m, 6H)FD-MS m / z 525.2
[0292] [ka]
[0293] <<Synthesis of organometallic complex S>> A thermometer and a three-way cock were attached to a thoroughly dried 200mL three-neck flask. Under a nitrogen atmosphere, 9.2 grams of tert-butylcyclopentadiene, 7.2 mL of dehydrated acetone, and 60 mL of dehydrated methanol were added and stirred. The solution was cooled to -10°C, and then 10.7 mL of pyrrolidine was slowly added dropwise. After the dropwise addition, the temperature was raised to room temperature over more than one hour, and stirring was continued at room temperature overnight. 8.6 mL of acetic acid was slowly added dropwise, and after stirring for about 10 minutes, the reaction solution was poured into 2 L of cold water and stirred. After adding tert-butyl dimethyl ether and stirring, the organic layer and the aqueous layer were separated using a separatory funnel. The aqueous layer was extracted again with tert-butyl dimethyl ether and added to the previous organic layer. The organic layer was washed with water and saturated saline, and the organic layer was concentrated using a rotary evaporator to obtain 13.1 grams of crude product. The obtained product was purified by silica gel column chromatography to obtain 8.2 grams of compound P (yield 67%). 1 H NMR(400 MHz, CDCl3, 297 K, δ in ppm) δ1.2 (m, 9H), 2.15 (s, 3H), 2.16 (s, 3H), 6.14 (s, 1H), 6.53(s, 2H).
[0294] [ka]
[0295] A thermometer and a three-way cock were attached to a thoroughly dried 500 mL three-neck flask. Under a nitrogen atmosphere, 200 mL of dehydrated diethyl ether and 15.9 g of compound B were added and stirred. The solution was cooled in a dry ice acetone bath and stirred for a while, after which a 1.6 mol / L solution was added. n 31.4 mL of BuLi hexane solution was slowly added dropwise. After the addition, the internal temperature was raised to -20°C and stirring was continued for 1 hour, and then 8.15 g of compound P was weighed and added to the reaction solution. Stirring was continued at -20°C for 4 hours and the temperature was gradually raised to room temperature. After adding water to quench, ethyl acetate was added and stirred, and the organic layer and the aqueous layer were separated using a separatory funnel. The organic layer was washed with water, a saturated aqueous ammonium chloride solution, and saturated saline, and then dried over magnesium sulfate. The magnesium sulfate was filtered off, and the organic layer was concentrated using a rotary evaporator to obtain a crude product. The crude product was purified by silica gel column chromatography to obtain 8.7 g of compound Q as a mixture of isomers of cyclopentadienyl groups (yield 44%). 1 H NMR(400 MHz, CDCl3, 298 K, δ in ppm) δ0.98-1.60 (m, 24H), 2.38-2.78 (m, 2H), 5.59-6.23 (m, 2H), 6.92-7.35 (m, 9H).
[0296] [ka]
[0297] A thermometer and a three-way cock were attached to a thoroughly dried 200mL three-neck flask. Under a nitrogen atmosphere, 8.5 grams of compound Q, 100mL of dehydrated dichloromethane, and 2.24 grams of dehydrated pyridine were added and stirred while cooling in an ice bath. 5.3 grams of trimethylsilyl trifluoromethanesulfonate were slowly dripped in, and the mixture was warmed to room temperature and stirred for 2 hours. The flask was cooled again in an ice bath, and a saturated aqueous solution of sodium bicarbonate was slowly dripped in. The reaction mixture was added to a separatory funnel, ethyl acetate was added to extract the soluble matter, and the organic layer and the aqueous layer were separated. The organic layer was washed with water to separate the organic layer and the aqueous layer. This operation was repeated, and the organic layer was washed with water a total of four times. The organic layer was washed with saturated saline and separated from the aqueous layer. Potassium carbonate was added to the organic layer to dry it, and the potassium carbonate was filtered off. The organic layer was concentrated using a rotary evaporator, and then toluene was added and concentrated again. This operation was repeated three times, and 5.89 grams of crude product was obtained as a mixture of isomers of cyclopentadienyl groups. Compound R was used in the next step without further purification (no NMR data).
[0298] [ka]
[0299] A thermometer and a three-way cock were attached to a thoroughly dried 200mL three-neck flask. Under a nitrogen atmosphere, 338mg of tetrakisdimethylamidotitanium(IV) and 75mL of dehydrated toluene were added. Under a nitrogen atmosphere, 549mg of compound R was weighed and dissolved in 20mL of dehydrated toluene. The toluene solution of compound R was added to the tetrakisdimethylamidotitanium(IV) solution, and after the addition, the mixture was stirred overnight at 80°C. The flask was brought into a glove box, and the solvent was removed using a rotary evaporator to obtain a reddish-brown liquid. Hexane was added and stirred well, and the insoluble matter was filtered through a membrane filter with a pore size of 3μm. The filtrate was concentrated to obtain 704.3mg of a product containing a reddish-brown amide complex. A thermometer and a three-way cock were attached to a thoroughly dried 100mL three-neck flask. The previously synthesized amide complex was dissolved in 50mL of dehydrated toluene and added to the flask, and then 1.4mL of dichlorodimethylsilane was added. After the addition, the mixture was heated and stirred at 60°C overnight. Toluene was distilled off under reduced pressure in a glove box. 10mL of toluene was added and stirred well, and insoluble matter was removed using a membrane filter with a pore size of 3μm. The filtrate was concentrated once, dehydrated toluene was added to dissolve the product, and dehydrated hexane was slowly dropped. The precipitate was removed using a membrane filter with a pore size of 3μm, and a dark brown solid was obtained. Dehydrated cyclohexane was added to the obtained solid, stirred, and allowed to stand. The supernatant was removed by decantation. Dehydrated cyclohexane was added again, stirred, allowed to stand, and the supernatant was removed by decantation. A solvent was prepared by mixing equal amounts of dehydrated cyclohexane and dehydrated hexane, and added to the solid, followed by stirring and standing, and then the supernatant was removed by decantation. Washing was performed once more using a mixed solvent of dehydrated cyclohexane and dehydrated hexane. The remaining solid was dried under reduced pressure to obtain 192 mg of compound S as a brown powder (yield 26%). Analysis of the obtained product by NMR confirmed that it was organometallic complex S (compound S) having the structure shown below. 1 H NMR(400 MHz, CDCl3, 323 K, δ in ppm) δ1.39 (s, 9H), 1.58 (s, 3H), 1.85 (s, 3H), 5.48 (dd, J = 3.2, 2.4 Hz, 1H), 6.16 (dd, J = 8.0, 1.5 Hz, 1H), 6.37 (t, J = 2.4 Hz, 1H), 6.60 (dd, J = 3.3, 2.4 Hz, 1H), 6.99-7.04 (m, 1H), 7.08 (td, J = 7.3, 1.5 Hz 1H), 7.27-7.56 (m, 6H)FD-MS m / z 447.1
[0300] [ka]
[0301] <<Synthesis of organometallic complex X>> A thermometer and a three-way cock were attached to a thoroughly dried 500mL three-neck flask. Under a nitrogen atmosphere, 0.58 grams of palladium dibenzylideneacetone palladium (0), 1.16 grams of 4,5-bis(diphenylphosphino)-9,9-dimethylxanthene, 4.8 grams of sodium t-butoxide, and 200mL of dehydrated toluene were added. 28.3 grams of 1-bromo-2-iodobenzene were added dropwise while stirring at room temperature, and then 15.4 grams of 4-isopropylaniline were slowly added dropwise. A condenser was attached to the flask, and the mixture was heated under reflux overnight under a nitrogen atmosphere. 0.58 grams of palladium dibenzylideneacetone palladium (0), 1.16 grams of 4,5-bis(diphenylphosphino)-9,9-dimethylxanthene, and 2.4 grams of sodium t-butoxide were added, and the mixture was heated under reflux for another 6 hours. The mixture was cooled to room temperature to obtain a slurry containing insoluble matter. An adapter with a side tube was attached to a 500 mL eggplant flask, a glass filter was attached to the top of the adapter, and a vacuum line was attached to the side tube of the adapter. Silica gel was added to the glass filter, and toluene was added to suspend it. The flask was depressurized and the toluene was sucked out. While the flask was depressurized, the slurry after the reaction was slowly added onto the silica gel and insoluble matter was filtered out. After filtration, toluene was added onto the silica gel and suction filtered, and this suction filtration was repeated several times. The toluene solution in the flask was concentrated with a rotary evaporator to obtain 41.4 grams of crude product. The crude product was purified by silica gel column chromatography to obtain 28.4 grams (yield 93%) of compound T. 1 H NMR(400 MHz, CDCl3, 299 K, δ in ppm) δ1.34 (d, J = 5.8, 6 H), 4.51 (septet, J = 5.8 Hz, 1 H), 5.94 (s, 1 H), 6.64 (t, J = 7.6, 1 H), 6.88 (d, J = 8.8 Hz, 2H), 6.95 (d, J = 7.8 Hz, 1H), 7.05-7.17 (m, 3H), 7.47 (d, J = 7.8 Hz, 1H)
[0302] [ka]
[0303] A thermometer and a three-way cock were attached to a thoroughly dried 500mL three-neck flask. Under a nitrogen atmosphere, 28.3 grams of compound T, 200mL of dehydrated toluene, and 3.39 grams of 4-dimethylaminopyridine were added. 31.8 grams of di-tert-butyl dicarbonate were slowly added while stirring at room temperature. A condenser was attached to the flask, and the mixture was heated and refluxed overnight. The mixture was cooled to room temperature, and the flask was cooled in an ice bath. 100mL of water was slowly added dropwise and stirred. The resulting solution was added to a separatory funnel to separate the organic layer and the aqueous layer. The organic layer was washed with saturated saline, and then the aqueous layer and the organic layer were separated again. Magnesium sulfate was added to the organic layer to dry it, and the magnesium sulfate was filtered off. The organic layer was concentrated using a rotary evaporator to obtain 51.8 grams of crude product. The crude product was purified by silica gel column chromatography to obtain 37.2 grams (99% yield) of compound U. 1 H NMR(400 MHz, CDCl3, 300 K, δ in ppm) δ1.30 (d, J = 5.8 Hz, 6 H), 1.43 (s, 9 H), 4.47 (septet, J = 5.8 Hz, 1 H), 6.79 (d, J = 8.5 Hz, 2 H), 7.08-7.35 (m, 5H), 7.62 (d, J = 7.8 Hz, 1H)
[0304] [ka]
[0305] A thermometer and a three-way cock were attached to a thoroughly dried 100 mL three-neck flask. Under a nitrogen atmosphere, 20 mL of dehydrated diethyl ether and 5.0 g of compound U were added and stirred. The solution was cooled in a dry ice acetone bath and stirred for a while, after which the solution was diluted to 1.6 mol / L. n 8.5mL of BuLi hexane solution was slowly added dropwise and stirred for 1 hour. 2.79mL of 6,6'-dimethylfulvene was added and the temperature was gradually raised to room temperature. The reaction solution was poured into chilled water to quench, then ethyl acetate was added and stirred, and the organic layer and the aqueous layer were separated using a separatory funnel. The organic layer was washed with water, a saturated aqueous ammonium chloride solution, and saturated saline, and then dried over magnesium sulfate. The organic layer was concentrated using a rotary evaporator to obtain 6.1g of a crude product. The crude product was purified by silica gel column chromatography to obtain 3.6g of compound V as a mixture of isomers of cyclopentadienyl groups (yield 68%). 1 H NMR(400 MHz, CDCl3, 296 K, δ in ppm) δ1.21-1.59 (m, 21H), 2.50-2.93 (m, 2H), 4.45 (septet, J = 5.9 Hz, 1H), 5.88-6.38 (m, 3H), 6.67-6.81 (m, 2H), 6.99-7.16 (m, 3H), 7.20-7.34 (m, 3H).
[0306] [ka]
[0307] A thermometer and a three-way cock were attached to a thoroughly dried 100mL three-neck flask. Under a nitrogen atmosphere, 3.6 grams of compound V, 25mL of dehydrated dichloromethane, and 0.93 grams of dehydrated pyridine were added and stirred while cooling in an ice bath. 2.2 grams of trimethylsilyl trifluoromethanesulfonate was dissolved in 5mL of dehydrated dichloromethane and slowly dropped. After dropping, the temperature was raised to room temperature and stirred for 2 hours. The flask was cooled again in an ice bath, and a saturated aqueous solution of sodium bicarbonate was slowly dropped. The reaction mixture was added to a separatory funnel, ethyl acetate was added to extract the soluble matter, and the organic layer and the aqueous layer were separated. The organic layer was washed with water to separate the organic layer and the aqueous layer. This operation was repeated, and the organic layer was washed with water a total of four times. The organic layer was washed with saturated saline and separated from the aqueous layer. Potassium carbonate was added to the organic layer to dry it, and the potassium carbonate was filtered off. The filtrate was concentrated with a rotary evaporator, and then toluene was added and concentrated again. This procedure was repeated three times to obtain 2.85 g of a crude product as a mixture of cyclopentadienyl group isomers. Compound W was used in the next step without further purification. 1 H NMR(400 MHz, CD3COCD3, 296 K, δ in ppm) δ1.25 (d, J = 5.8 Hz, 6H), 1.54-1.66 (m, 6H), 2.73-3.22 (m, 2H), 4.40-4.56 (m, 1H), 5.78-6.03 (m, 1H), 6.15-6.55 (m, 3H), 6.63-7.28 (m, 7H), 7.37-7.52 (m, 1H).
[0308] [ka]
[0309] A thermometer and a three-way cock were attached to a thoroughly dried 200mL three-neck flask. Under a nitrogen atmosphere, 363mg of tetrakisdimethylamidotitanium(IV) and 65mL of dehydrated toluene were added. Under a nitrogen atmosphere, 529mg of compound W was weighed and dissolved in 10mL of dehydrated toluene. The toluene solution of compound W was added to the tetrakisdimethylamidotitanium(IV) solution, and after the addition, the mixture was stirred overnight at 80°C. The flask was brought into a glove box, and the solvent was distilled off using a rotary evaporator to obtain a reddish-brown liquid. Hexane was added and stirred well, and the insoluble matter was filtered through a membrane filter with a pore size of 3μm. The filtrate was concentrated to obtain 435mg of a reddish-brown oil containing an amide complex (compound X). When the obtained product was analyzed by NMR, organometallic complex X (compound X) having the structure shown below was confirmed (NMR data not available).
[0310] [ka]
[0311] <<Synthesis of organometallic complex Y>> A thermometer and a three-way cock were attached to a thoroughly dried 100mL three-neck flask. 430mg of the previously synthesized amide complex was dissolved in 50mL of dehydrated toluene and added to the flask, and then 0.6mL of dichlorodimethylsilane was added. After the addition, the mixture was heated and stirred at 60°C overnight. Toluene was distilled off under reduced pressure in a glove box. 10mL of toluene was added and stirred well, and insoluble matter was removed using a membrane filter with a pore size of 3μm. The filtrate was concentrated once, dehydrated cyclohexane was added and stirred. The precipitate was filtered through a membrane filter with a pore size of 3μm, the powder remaining on the filter was washed with dehydrated cyclohexane and dehydrated hexane, and the solvent was filtered. The powder remaining on the filter was dried under reduced pressure to obtain 178mg of compound Y as a dark brown powder (yield 25%). The obtained product was analyzed by NMR, and the organometallic complex Y (compound Y) having the structure shown below was confirmed. 1 1H NMR (400 MHz, CDCl3, 296 K, δ in ppm) δ 1.38 (dd, J = 6.1 Hz, 6H), 1.70 (s, 6H), 4.63 (septet, J = 6.1 Hz, 1H), 6.07 (t, J = 2.7 Hz, 2H), 6.17 (dd, J = 8.0, 1.5 Hz, 1H), 6.71 (t, J = 2.7 Hz, 2H), 6.98 - 7.03 (m, 2H), 7.05 (td, J = 7.8, 1.5 Hz, 1H), 7.10 (td, J = 7.8, 1.5 Hz, 1H), 7.30 - 7.37 (m, 2H), 7.59 (dd, J = 7.6, 1.7 Hz, 1H). FD-MS m / z 449.1
[0312] [Chemical formula]
[0313] [Synthesis of Organometallic Complex AD] A thermometer and a three-way cock were attached to a thoroughly dried 500mL three-neck flask. Under a nitrogen atmosphere, 0.87 grams of palladium dibenzylideneacetonepalladium (0), 1.76 grams of 4,5-bis(diphenylphosphino)-9,9-dimethylxanthene, 20.5 grams of sodium t-butoxide, and 200mL of dehydrated toluene were added. 43 grams of 1-bromo-2-iodobenzene were added dropwise while stirring at room temperature, and then 25 grams of 4-aminobenzotrifluoride were slowly added dropwise. A condenser was attached to the flask, and the mixture was heated under reflux overnight under a nitrogen atmosphere. An adapter with a side tube was attached to a 500mL eggplant flask, a glass filter was attached to the top of the adapter, and a vacuum line was attached to the side tube of the adapter. Silica gel was added to the glass filter, and toluene was added to suspend it. The flask was vacuumed to aspirate the toluene. While the flask was vacuumed, the slurry after the reaction was slowly added to the silica gel, and insoluble matter was filtered out. After filtration, toluene was added onto the silica gel and suction filtered, and this suction filtration was repeated several times. The toluene solution in the flask was concentrated using a rotary evaporator to obtain 75.8 g of a crude product. The crude product was purified by silica gel column chromatography to obtain 0.96 g (yield 2%) of compound Z. 1 H NMR(400 MHz, CDCl3, 296 K, δ in ppm) δ6.19 (s, 1 H), 6.88 (t, J = 7.6 Hz, 1 H), 7.14 (d, J = 8.3 Hz, 2 H), 7.20-7.30 (m, 1 H), 7.37 (d, J = 8.0 Hz, 1H), 7.52 (d, J = 8.3 Hz, 2H), 7.58 (d, J = 8.0 Hz, 1H).
[0314] [ka]
[0315] A thermometer and a three-way cock were attached to a thoroughly dried 50mL three-neck flask. Under a nitrogen atmosphere, 0.96 grams of compound Z, 10mL of dehydrated toluene, and 0.19 grams of 4-dimethylaminopyridine were added. 1.0 grams of di-tert-butyl dicarbonate was slowly added while stirring at room temperature. A condenser was attached to the flask, and the mixture was heated and refluxed overnight. The mixture was cooled to room temperature, and the flask was cooled in an ice bath. 100mL of water was slowly added dropwise and stirred. The resulting solution was added to a separatory funnel to separate the organic layer and the aqueous layer. Saturated saline was added to the organic layer, the organic layer was washed, and the aqueous layer and the organic layer were separated again. Magnesium sulfate was added to the organic layer to dry it, and the magnesium sulfate was filtered off. The organic layer was concentrated using a rotary evaporator to obtain 1.7 grams of crude product. The crude product was purified by silica gel column chromatography to obtain 1.2 grams (95% yield) of compound AA. 1 H NMR(400 MHz, CDCl3, 297 K, δ in ppm) δ1.44 (s, 9 H), 7.19-7.29 (m, 2 H), 7.33-7.40(m, 3H), 7.52 (d, J = 8.5 Hz, 2 H), 7.68 (d, J = 8.0 Hz, 1 H).
[0316] [ka]
[0317] In a thoroughly dried 30 mL Schlenk flask, 5 mL of dehydrated diethyl ether and 1.2 g of compound AA were added under a nitrogen atmosphere and stirred. The solution was cooled in a dry ice acetone bath and stirred for a while, after which it was diluted with 1.6 mol / L n 2.0 mL of BuLi hexane solution was slowly added dropwise and stirred for 1 hour. 0.38 mL of 6,6'-dimethylfulvene was added and the temperature was gradually raised to room temperature. The reaction solution was poured into chilled water to quench, then ethyl acetate was added and stirred, and the organic layer and aqueous layer were separated using a separatory funnel. The organic layer was washed with water, a saturated aqueous ammonium chloride solution, and saturated saline, and then dried over magnesium sulfate. The organic layer was concentrated using a rotary evaporator to obtain 1.2 g of a crude product. The crude product was purified by silica gel column chromatography to obtain 0.70 g of compound AB as a mixture of isomers of cyclopentadienyl groups (yield 55%). 1 H NMR(400 MHz, CDCl3, 296 K, δ in ppm) δ1.34-1.58 (m, 15H), 2.41-2.99 (m, 2H), 5.81-6.37(m, 3H), 7.02-7.75(m, 8H).
[0318] [ka]
[0319] In a thoroughly dried 30 mL Schlenk flask, 0.66 grams of compound AB, 5 mL of dehydrated dichloromethane, and 0.17 grams of dehydrated pyridine were added under a nitrogen atmosphere and stirred while cooling in an ice bath. 0.4 grams of trimethylsilyl trifluoromethanesulfonate was dissolved in 2 mL of dehydrated dichloromethane and slowly dropped into the flask. After dropping, the temperature was raised to room temperature and stirred for 2 hours. The Schlenk flask was cooled again in an ice bath, and a saturated aqueous solution of sodium bicarbonate was slowly dropped into the flask. The reaction mixture was added to a separatory funnel, ethyl acetate was added to extract the soluble matter, and the organic layer and the aqueous layer were separated. The organic layer was washed with water to separate the organic layer and the aqueous layer. The organic layer was washed with water a total of four times. The organic layer was washed with saturated saline, potassium carbonate was added to the organic layer to dry it, and the potassium carbonate was filtered off. The organic layer was concentrated using a rotary evaporator, and then toluene was added and concentrated again. This operation was repeated three times to obtain 0.50 grams of crude product as a mixture of isomers of cyclopentadienyl groups. Compound AC was used in the next step without further purification. 1 H NMR(400 MHz, CD3COCD3, 296 K, δ in ppm) δ 1.49-1.60 (m, 6H), 2.75-3.22 (m, 2H), 6.15-6.44 (m, 4H), 6.72-6.88 (m, 2H), 7.11-7.34 (m, 3H), 7.38-7.48 (m, 2H), 7.54-7.63 (m, 1H).
[0320] [ka]
[0321] A thermometer and a three-way cock were attached to a thoroughly dried 200mL three-neck flask. Under a nitrogen atmosphere, 313mg of tetrakisdimethylamidotitanium(IV) and 65mL of dehydrated toluene were added. Under a nitrogen atmosphere, 479mg of compound AC was weighed and dissolved in 10mL of dehydrated toluene. The toluene solution of compound AC was added to the tetrakisdimethylamidotitanium(IV) solution, and after the addition, the mixture was stirred overnight at 80°C. The flask was brought into a glove box, and the solvent was distilled off using a rotary evaporator to obtain a reddish-brown liquid. Hexane was added and stirred well, and the insoluble matter was filtered through a membrane filter with a pore size of 3μm. The filtrate was concentrated to obtain 665mg of a reddish-brown amide complex (compound AD). The obtained product was analyzed by NMR, and the organometallic complex AD (compound AD) having the structure shown below was confirmed. 1 H NMR(400 MHz, CDCl3, 296 K, δ in ppm) δ1.62 (s, 6H), 3.06 (s, 12H), 5.60-5.67 (m, 2H), 6.06-6.11 (m, 2H), 6.58 (d, J = 7.6 Hz, 1H), 6.78 (d, J = 8.8 Hz, 2H), 6.96 (t, J = 7.6 Hz, 1H), 7.04 (t, J = 7.6 Hz, 1H), 7.22-7.34 (m, 2H), 7.47 (d, J = 7.6 Hz, 1H).
[0322] [ka]
[0323] <<Synthesis of organometallic complex AE>> A thermometer and a three-way cock were attached to a thoroughly dried 100mL three-neck flask. 600mg of the previously synthesized amide complex was dissolved in 50mL of dehydrated toluene and added to the flask, and then 0.75mL of dichlorodimethylsilane was added. After the addition, the mixture was heated and stirred at 60°C overnight. Toluene was distilled off under reduced pressure in a glove box. 10mL of toluene was added and stirred well, and insoluble matter was removed using a membrane filter with a pore size of 3μm. The filtrate was concentrated once, and dehydrated cyclohexane was added and stirred. The precipitate was filtered through a membrane filter with a pore size of 3μm, and the powder remaining on the filter was washed twice with dehydrated cyclohexane and once with dehydrated hexane. The powder remaining on the filter was dried under reduced pressure to obtain 304mg of compound AE as an orange powder (yield 47%). The obtained product was analyzed by NMR, and the organometallic complex AE (compound AE) having the structure shown below was confirmed. 1 H NMR(400 MHz, CDCl3, 296 K, δ in ppm) δ1.74 (s, 6H), 6.06-6.18 (m, 3H), 6.73-6.83 (m, 2H), 7.07 (t, J = 7.3 Hz, 1H), 7.15 (t, J = 7.3 Hz, 1H), 7.52-7.64 (m, 3H), 7.72(d, J = 7.8, 2H).FD-MS m / z 459.0
[0324] [ka]
[0325] <<Synthesis of organometallic complex AI>> A thermometer, a three-way cock, and a dropping funnel were attached to a thoroughly dried 500mL three-neck flask. 15g of methylcyclopentadiene obtained by pyrolysis of methylcyclopentadiene dimer was dissolved in 125mL of dehydrated methanol, and then 13.8mL of dehydrated acetone was added. The flask was cooled in an ice bath, and 38.7mL of pyrrolidine was slowly added. After warming to room temperature and stirring for 2 hours, 32mL of acetic acid was added dropwise, and after stirring for 10 minutes, water was added. tert-Butyl methyl ether was added and stirred, and the organic layer and the aqueous layer were separated using a separatory funnel. The organic layer was washed with water and saturated saline, and then dried over magnesium sulfate. The magnesium sulfate was removed by filtration, and the filtrate was concentrated using a rotary evaporator to obtain a crude product. The crude product was distilled under reduced pressure (15 torr, distillation temperature 57°C) to obtain 11.4 grams of compound AF as an orange liquid. 1 H NMR(400 MHz, CDCl3, 296K, δ in ppm) δ2.06 (s, 6H), 2.13 (s, 3H), 2.14(s, 3H), 6.17 (s, 1H), 6.32 (d, J = 4.1 Hz, 1H), 6.29 (d, J = 4.1 Hz, 1H).
[0326] [ka]
[0327] A thermometer and a three-way cock were attached to a thoroughly dried 200mL three-neck flask. Under a nitrogen atmosphere, 11.0 g of compound B and 100 mL of dehydrated diethyl ether were added. The solution was thoroughly cooled using a dry ice-acetone bath, and 21.7 mL of n-butyllithium hexane solution (1.6 M) was slowly added dropwise. After the dropwise addition, the mixture was stirred for 1 hour while cooling. 4.18 g of compound AF was slowly added dropwise, and the mixture was stirred overnight while cooling. The next day, the internal temperature was adjusted to -20°C to -40°C, and the mixture was stirred for 6 hours. Another flask was prepared with water added, and the reaction solution was pressure-fed into the water using a cannula to quench the reaction. Ethyl acetate was added to the quenched reaction solution to extract the soluble matter, and the organic layer and the aqueous layer were separated using a separatory funnel. The organic layer was washed with water and a saturated aqueous ammonium chloride solution, respectively, and the organic layer was separated from the aqueous layer. Magnesium sulfate was added to the organic layer to dry it, and the magnesium sulfate was filtered off. The organic layer was concentrated using a rotary evaporator to obtain 14.2 g of a crude product, which was then purified by silica gel column chromatography to obtain 4.9 g (40% yield) of compound AG as a mixture of cyclopentadienyl group isomers. 1 H NMR(400 MHz, CDCl3, 297 K, δ in ppm) δ1.22-1.76 (m, 15 H), 1.89 (s, 3H), 2.33-2.89 (m, 2 H), 5.60-6.12 (m, 2 H), 6.90-7.42 (m, 9 H).
[0328] [ka]
[0329] A thermometer and a three-way cock were attached to a thoroughly dried 100mL three-neck flask. Under a nitrogen atmosphere, 4.92 grams of compound AG, 50mL of dehydrated dichloromethane, and 1.44 grams of dehydrated pyridine were added and stirred while cooling in an ice bath. 3.37 grams of trimethylsilyl trifluoromethanesulfonate were slowly dripped in, and after the dripping, the temperature was raised to room temperature and stirred for 2 hours. The flask was cooled again in an ice bath, and a saturated aqueous solution of sodium bicarbonate was slowly dripped in. The reaction mixture was added to a separatory funnel, ethyl acetate was added to extract the soluble matter, and the organic layer and the aqueous layer were separated. Water was added to the organic layer to wash the organic layer, and the organic layer and the aqueous layer were separated. This operation was repeated four times. The organic layer was washed with saturated saline and separated from the aqueous layer. Potassium carbonate was added to the organic layer to dry it, and the potassium carbonate was removed by filtration. The organic layer was concentrated with a rotary evaporator to obtain a concentrated liquid. Toluene was added to the concentrated liquid, and then it was concentrated with a rotary evaporator. This procedure was repeated three times to obtain 9.3 g of crude product as a mixture of cyclopentadienyl isomers. Compound AH was used in the next step without further purification.
[0330] [ka]
[0331] A thermometer and a three-way cock were attached to a thoroughly dried 100mL three-neck flask. Under a nitrogen atmosphere, 272mg of tetrakisdimethylamidotitanium(IV) and 40mL of dehydrated toluene were added. Under a nitrogen atmosphere, 351mg of compound AH was weighed and dissolved in 10mL of dehydrated toluene. The toluene solution of compound AH was added to the tetrakisdimethylamidotitanium(IV) solution, and after the addition, the mixture was stirred overnight at 80°C. The flask was brought into a glove box, and the solvent was distilled off using a rotary evaporator. Hexane was added and stirred well, and the insoluble matter was filtered through a membrane filter with a pore size of 3μm. The filtrate was concentrated to obtain a reddish brown liquid. The obtained product was used in the next step as it was without further purification. A thermometer and a three-way cock were attached to a thoroughly dried 100mL three-neck flask. The reddish brown liquid obtained in the previous reaction was dissolved in 40mL of dehydrated toluene and added to the flask, and then 0.64mL of dichlorodimethylsilane was added. After the addition, the mixture was heated and stirred overnight at 60°C. After toluene was distilled off under reduced pressure in a glove box, 10 mL of toluene was added and stirred thoroughly, and insoluble matter was removed using a membrane filter with a pore size of 3 μm. The filtrate was concentrated once, and dehydrated cyclohexane was added and stirred. The precipitate was filtered through a membrane filter with a pore size of 3 μm, and the powder remaining on the filter was washed twice with dehydrated cyclohexane and once with dehydrated hexane. The powder remaining on the filter was dried under reduced pressure to obtain 199 mg of compound AI as a brown powder (yield 40%). The obtained product was analyzed by NMR, and the organometallic complex AI (compound AI) having the structure shown below was confirmed. 1 1H NMR (400 MHz, CDCl3, 296 K, δ in ppm) δ 1.67 (s, 3H), 1.74 (s, 3H), 2.38 (s, 3H), 5.86 (dd, J = 3.2, 2.5 Hz 1H), 5.96 (t, J = 2.5 Hz, 1H), 6.16 (dd, J = 8.0, 1.5 Hz, 1H), 6.49 (m, 1H), 7.02 - 7.07 (m, 1H), 7.08 - 7.13 (m, 1H), 7.35 - 7.40 (m, 1H), 7.40 - 7.45 (m, 2H), 7.56 - 7.52 (m, 2H), 7.57 (dd, J = 7.6, 1.5 Hz 1H). FD-MS m / z 405.0
[0332]
Chem.
[0333] <<Synthesis of Organometallic Complex AJ>> The organometallic complex AJ (Compound AJ) was synthesized by the method described in JP-A-11-12289.
[0334]
Chem.
[0335] <<Synthesis of Organometallic Complex AO>> A thermometer and a three-way cock were attached to a thoroughly dried 500mL three-neck flask. Under a nitrogen atmosphere, 0.58 grams of palladium dibenzylideneacetonepalladium (0), 1.16 grams of 4,5-bis(diphenylphosphino)-9,9-dimethylxanthene, 4.81 grams of sodium t-butoxide, and 200mL of dehydrated toluene were added. 12.5mL of 1-bromo-2-iodobenzene was added dropwise while stirring at room temperature, and then 15.32 grams of 3,5-dimethoxyaniline was added. A condenser was attached to the flask, and the mixture was heated under reflux overnight under a nitrogen atmosphere. After cooling to room temperature, the organic layer and the aqueous layer were separated using a separatory funnel. The organic layer was washed with saturated saline, and the aqueous layer and the organic layer were separated again. Magnesium sulfate was added to the organic layer to dry it, and the magnesium sulfate was removed by filtration. The organic layer was concentrated using a rotary evaporator and purified by silica gel column chromatography to obtain 28.3 grams (yield 92%) of compound AK. 1 H NMR(400MHz, CDCl3, 297K, δin ppm)δ3.77(s,6H)6.04(brs,1H),6.16(s,1H),6.30(s,2H),6.76(t,J=7.4 Hz,1H),7.18(t,J=7.6Hz,1H),7.33(d,J=8.4Hz,1H),7.52(d,J=8.0Hz,1H)
[0336] [ka]
[0337] A thermometer and a three-way cock were attached to a thoroughly dried 500mL three-neck flask. Under a nitrogen atmosphere, 28.3 grams of compound AK, 200mL of dehydrated toluene, and 3.36 grams of 4-dimethylaminopyridine were added. 33.2mL of di-tert-butyl dicarbonate was slowly added while stirring at room temperature. A condenser was attached to the flask, and the mixture was heated and refluxed overnight. The mixture was cooled to room temperature, and the flask was cooled in an ice bath. 100mL of water was slowly added dropwise and stirred. The organic layer and the aqueous layer were separated using a separatory funnel. The organic layer was washed with saturated saline, and the aqueous layer and the organic layer were separated again. Magnesium sulfate was added to the organic layer to dry it, and the magnesium sulfate was removed by filtration. The organic layer was concentrated using a rotary evaporator to obtain 50.0 grams of crude product. The crude product was purified by silica gel column chromatography to obtain 30.7 grams (82% yield) of compound AL. 1 H NMR(400MHz,CDCl3,298K,δ in ppm) δ1.44(s,9H),3.74(s,6H),6.25(s,1H),6.48(s,2H),7.16(t,J=7.6Hz,1H),7.27-7.33(m,2H),7.64(d,J=7.8Hz,1H)
[0338] [ka]
[0339] A thermometer and a three-way cock were attached to a thoroughly dried 300mL three-neck flask. Under a nitrogen atmosphere, 10.0 g of compound AL and 100 mL of dehydrated diethyl ether were added. The solution was thoroughly cooled in a dry ice-acetone bath, and 16.8 mL of n-butyllithium hexane solution (1.6 M) was slowly added dropwise and stirred for 1 hour. 2.9 g of 6,6-dimethylfulvene was slowly added dropwise and stirred overnight while cooling. Another flask containing water was prepared, and the reaction solution was pressure-fed by a cannula to quench the reaction. Ethyl acetate was added to the quenched reaction solution to extract the soluble matter, and the organic layer and aqueous layer were separated using a separatory funnel. The organic layer was washed with water and a saturated aqueous ammonium chloride solution, respectively, and the organic layer was separated from the aqueous layer. Magnesium sulfate was added to the organic layer to dry it, and the magnesium sulfate was removed by filtration. The organic layer was concentrated using a rotary evaporator to obtain 10.8 g of a crude product. The crude product was purified by silica gel column chromatography to obtain 6.0 g (yield 56%) of compound AM as a mixture of isomers of cyclopentadienyl groups. 1 H NMR(400MHz CDCl3298K,δ in ppm) δ1.30-1.55(m,15H),2.55-2.93(m,2H),3.70(s,6H),5.96-6.41(m,6H),7.07(s,1H)7.23-7.29(m, 3H)
[0340] [ka]
[0341] A thermometer and a three-way cock were attached to a thoroughly dried 300mL three-neck flask. Under a nitrogen atmosphere, 5.9 grams of compound AM, 60mL of dehydrated dichloromethane, and 1.53 grams of dehydrated pyridine were added and stirred while cooling in an ice bath. 3.59 grams of trimethylsilyl trifluoromethanesulfonate were slowly dripped in, and after the dripping, the temperature was raised to room temperature and stirred for 2 hours. The flask was cooled again in an ice bath and a saturated aqueous solution of sodium bicarbonate was slowly dripped in. The reaction mixture was added to a separatory funnel, and ethyl acetate was added to extract the soluble matter and separate the organic layer and the aqueous layer. The organic layer was washed with water and separated from the aqueous layer. This operation was repeated, and the organic layer was washed with water a total of four times. The organic layer was washed with saturated saline and separated from the aqueous layer. Potassium carbonate was added to the organic layer and dried, and then the potassium carbonate was filtered off. The filtrate was concentrated with a rotary evaporator to obtain a concentrated liquid. Toluene was added to the concentrated liquid, and then it was concentrated with a rotary evaporator. This procedure was repeated three times to obtain 5.6 g of crude product as a mixture of cyclopentadienyl isomers. Compound AN was used in the next step without further purification. 1 H NMR(400MHz,CD3COCD3, 299 K, δ in ppm) δ1.55-1.57(m,6H),2.31-3.18(m,2H),3.69(s,6 H), 5.88-6.48(m,6H),7.05-7.06(m,1H),7.18-7.26(m,3H),7.49-7.53(m,1H)
[0342] [ka]
[0343] A thermometer and a three-way cock were attached to a thoroughly dried 200mL three-neck flask. Under a nitrogen atmosphere, 447.8mg of tetrakisdimethylamidotitanium(IV) and 80mL of dehydrated toluene were added. Under a nitrogen atmosphere, 670mg of compound AN was weighed and dissolved in 10mL of dehydrated toluene. The toluene solution of compound AN was added to the tetrakisdimethylamidotitanium(IV) solution, and after the addition, the mixture was stirred overnight at 80°C. The flask was brought into a glove box, the solvent was removed using a rotary evaporator, hexane was added and stirred well, and the insoluble matter was filtered through a membrane filter with a pore size of 3μm. The filtrate was concentrated to obtain 606mg of a product containing a reddish-brown amide complex. A thermometer and a three-way cock were attached to a thoroughly dried 100mL three-neck flask. Under a nitrogen atmosphere, 500mg of the amide complex and 40mL of dehydrated toluene were added and stirred at room temperature. 0.64mL of dimethyldichlorosilane was added and stirred overnight at 60℃ using an oil bath under a nitrogen atmosphere. The flask was brought into a glove box and light boiling points were removed using a rotary evaporator. The mixture was washed with toluene and dried under reduced pressure to obtain 73mg of a reddish brown solid (compound AO) (yield 15%). The washed toluene solution was concentrated under reduced pressure, and cyclohexane was added to remove unnecessary substances. The filtrate was concentrated under reduced pressure, redissolved in 6mL of toluene, and about 12mL of hexane was added to obtain a solid, which was filtered and dried under reduced pressure to obtain 216mg of a reddish brown solid (compound AO) (yield 45%). The obtained product was analyzed by NMR, and the organometallic complex AO (compound AO) having the structure shown below was confirmed. 1 H NMR(400MHz,CDCl3,300K,δ in ppm) δ3.79(s, 6H),6.04(s,2H),6.30(d,J=8.0Hz,1H),6.46(s, 1H),6.66(s,2H),6.74(s,2H),7.05-7.14(m,2H), 7.57(d,J=7.2Hz,1H)
[0344] [ka]
[0345] <<Synthesis of organometallic complex AT>> A thermometer and a three-way cock were attached to a thoroughly dried 500mL three-neck flask. Under a nitrogen atmosphere, 0.58 grams of palladium dibenzylideneacetonepalladium (0), 1.16 grams of 4,5-bis(diphenylphosphino)-9,9-dimethylxanthene, 4.81 grams of sodium t-butoxide, and 200mL of dehydrated toluene were added. 12.5mL of 1-bromo-2-iodobenzene was added dropwise while stirring at room temperature, and then 13.62 grams of 4-dimethylaminoaniline was added. A condenser was attached to the flask, and the mixture was heated under reflux overnight under a nitrogen atmosphere. After cooling to room temperature, the organic layer and the aqueous layer were separated using a separatory funnel. The organic layer was washed with saturated saline, and the aqueous layer and the organic layer were separated again. Magnesium sulfate was added to the organic layer to dry it, and the magnesium sulfate was removed by filtration. The organic layer was concentrated using a rotary evaporator and purified by silica gel column chromatography to obtain 26.0 grams (89% yield) of compound AP. 1 H NMR(400MHz,CDCl3,298K,δ in ppm)δ2.95(s, 6H),5.90(s,1H),6.60(t,J=7.2Hz,1H),6.75(d,J=8.4Hz,2H),6.86(d,J=8.0Hz,1H),7.05-7.11(m,3H),7.46(d,J=7.6Hz,1H)
[0346] [ka]
[0347] A thermometer and a three-way cock were attached to a thoroughly dried 500mL three-neck flask. Under a nitrogen atmosphere, 25.9 grams of compound AP, 200mL of dehydrated toluene, and 3.26 grams of 4-dimethylaminopyridine were added. 32.3mL of di-tert-butyl dicarbonate was slowly added while stirring at room temperature. A condenser was attached to the flask, and the mixture was heated and refluxed overnight. The mixture was cooled to room temperature, and the flask was cooled in an ice bath. 100mL of water was slowly added dropwise and stirred. The organic layer and the aqueous layer were separated using a separatory funnel. The organic layer was washed with saturated saline, and then the aqueous layer and the organic layer were separated again. Magnesium sulfate was added to the organic layer to dry it, and the magnesium sulfate was removed by filtration. The organic layer was concentrated using a rotary evaporator to obtain 50.2 grams of crude product. The crude product was purified by silica gel column chromatography to obtain 25.0 grams (72% yield) of compound AQ. 1 H NMR (400 MHz, CDCl3,299K, δ in ppm) δ1.43(s,9H),2.90(s,6H),6.64(d,J=8.8Hz,2H),7.08-7.12(m,1H),7.20(d,J=7.2Hz,2H),7.27-7.29(m,2H),7.61(d,J=7.6Hz,1H)
[0348] [ka]
[0349] A thermometer and a three-way cock were attached to a thoroughly dried 300mL three-neck flask. Under a nitrogen atmosphere, 7.0 grams of compound AQ and 70mL of dehydrated diethyl ether were added. The solution was thoroughly cooled in a dry ice-acetone bath, and 12.3mL of n-butyllithium hexane solution (1.6M) was slowly added dropwise and stirred for 1 hour. 2.1 grams of 6,6-dimethylfulvene was slowly added dropwise and stirred overnight while cooling. Another flask containing water was prepared, and the reaction solution was pressure-fed by a cannula to quench the reaction. Ethyl acetate was added to the quenched reaction solution to extract the soluble matter, and the organic layer and aqueous layer were separated using a separatory funnel. The organic layer was washed with water and a saturated aqueous ammonium chloride solution, respectively, and the organic layer was separated from the aqueous layer. Magnesium sulfate was added to the organic layer to dry it, and the magnesium sulfate was removed by filtration. The organic layer was concentrated using a rotary evaporator to obtain 7.1 grams of crude product. The crude product was purified by silica gel column chromatography to obtain 3.6 g (48% yield) of the compound AR as a mixture of isomers of the cyclopentadienyl group. 1 H NMR(400MHz CDCl3298K,δ in ppm) δ1.27-1.64(m,15H),2.58-3.04(m,8H),5.91-6.36(m,3H),6.60(d,J=9.2Hz,2H)7.04-7.27(m,6H)
[0350] [ka]
[0351] A thermometer and a three-way cock were attached to a thoroughly dried 200mL three-neck flask. Under a nitrogen atmosphere, 3.5 grams of compound AR, 40mL of dehydrated dichloromethane, and 0.96 grams of dehydrated pyridine were added and stirred while cooling in an ice bath. 2.24 grams of trimethylsilyl trifluoromethanesulfonate were slowly dripped in, and after the dripping, the temperature was raised to room temperature and stirred for 2 hours. The flask was cooled again in an ice bath and a saturated aqueous solution of sodium bicarbonate was slowly dripped in. The reaction mixture was added to a separatory funnel, and ethyl acetate was added to extract the soluble matter and separate the organic layer and the aqueous layer. The organic layer was washed with water and separated from the aqueous layer. This operation was repeated, and the organic layer was washed with water a total of four times. The organic layer was washed with saturated saline and separated from the aqueous layer. Potassium carbonate was added to the organic layer and dried, and then the potassium carbonate was filtered off. The filtrate was concentrated with a rotary evaporator to obtain a concentrated liquid. Toluene was added to the concentrated liquid, and then it was concentrated with a rotary evaporator. This procedure was repeated three times to obtain 2.79 g of crude product as a mixture of cyclopentadienyl group isomers. Compound AS was used in the next step without further purification.
[0352] [ka]
[0353] A thermometer and a three-way cock were attached to a thoroughly dried 200mL three-neck flask. Under a nitrogen atmosphere, 449.1mg of tetrakisdimethylamidotitanium(IV) and 80mL of dehydrated toluene were added. Under a nitrogen atmosphere, 638mg of compound AS was weighed and dissolved in 10mL of dehydrated toluene. A toluene solution of compound AN was added to the tetrakisdimethylamidotitanium(IV) solution, and the mixture was stirred overnight at 80°C. The flask was brought into a glove box, the solvent was removed using a rotary evaporator, hexane was added and stirred well, and the insoluble matter was filtered through a membrane filter with a pore size of 3μm. The filtrate was concentrated to obtain 606mg of a product containing a reddish-brown amide complex. A thermometer and a three-way cock were attached to a thoroughly dried 100mL three-neck flask. Under a nitrogen atmosphere, 883mg of the amide complex and 80mL of dehydrated toluene were added and stirred at room temperature. 1.17mL of dimethyldichlorosilane was added and stirred overnight at 60℃ using an oil bath under a nitrogen atmosphere. The flask was brought into a glove box and low boiling points were removed using a rotary evaporator. Insoluble matter was removed by washing with toluene. The filtrate was concentrated under reduced pressure and cyclohexane was added for washing. Insoluble matter was washed with toluene and hexane, and the filtrate was concentrated and dried under reduced pressure to obtain 61mg of a reddish brown solid (yield 7%). The obtained product was analyzed by NMR, and the organometallic complex AT (compound AT) having the structure shown below was confirmed. 1 H NMR(400MHz,CDCl3,300K,δ in ppm) δ1.69(s, 6H),3.08(s,6H),6.05(t,J=2.4Hz,2H),6.17(d,J=7.6Hz,1H),6.68(t,J=2.4Hz,2H), 6.82(d,J=9.2Hz,2H),7.03-7.10(m,2H),7.26(d,J=8.8Hz,2H),7.59(d,J=7.2Hz,1H)
[0354] [ka]
[0355] <Production of ethylene polymer> [Polymerization Example 1-1] 250 mL of toluene was charged into a glass reactor with an internal volume of 500 mL, which had been thoroughly substituted with nitrogen, and ethylene was passed through at 100 L / hr to saturate the liquid phase and the gas phase. Then, 0.05 mmol of triisobutylaluminum in terms of aluminum atom, 0.0125 μmol of the compound G synthesized above, and 0.05 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were added to start polymerization. Ethylene was continuously fed at 100 L / hr, and polymerization was carried out for 5 minutes at normal pressure and an internal temperature of 25°C, after which polymerization was terminated by adding a small amount of methanol. After polymerization was completed, the reactant was added to 750 mL of methanol containing a small amount of hydrochloric acid to precipitate a polymer. After washing with the same solvent, it was dried under reduced pressure at 80°C for 10 hours to obtain 0.863 grams of ethylene polymer. The physical properties of the obtained polymer are shown in Table 1.
[0356] [Polymerization Example 1-2] Polymerization was carried out in the same manner as in Polymerization Example 1-1, except that the polymerization was carried out at an internal temperature of 50° C., to obtain 1.303 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0357] [Polymerization Example 1-3] Polymerization was carried out in the same manner as in Polymerization Example 1-1, except that the polymerization was carried out at an internal temperature of 75° C., to obtain 1.267 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0358] [Polymerization Examples 1-4] 250 mL of toluene was charged into a glass reactor with a capacity of 500 mL, which had been thoroughly substituted with nitrogen, and 100 L / hr of ethylene and 0.24 L / hr of hydrogen were passed through to saturate the liquid and gas phases. Then, 0.05 mmol of triisobutylaluminum was added in terms of aluminum atoms, 0.0125 μmol of compound G, and 0.05 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were added to initiate polymerization. Ethylene was continuously supplied at 100 L / hr and hydrogen at 0.24 L / hr, and polymerization was carried out for 5 minutes at normal pressure and an internal temperature of 50°C, after which polymerization was terminated by adding a small amount of methanol. After polymerization was completed, the reactant was added to 750 mL of methanol containing a small amount of hydrochloric acid to precipitate a polymer. After washing with the same solvent, it was dried under reduced pressure at 80°C for 10 hours to obtain 0.405 grams of ethylene polymer. The physical properties of the obtained polymer are shown in Table 1.
[0359] [Polymerization Examples 1-5] Polymerization was carried out in the same manner as in Polymerization Example 1-1, except that 0.1 μmol of compound O was used instead of compound G, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.4 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, to obtain 1.246 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0360] [Polymerization Examples 1-6] Polymerization was carried out in the same manner as in Polymerization Example 1-1, except that 0.1 μmol of compound O was used instead of compound G, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.4 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, and the internal temperature was set to 50° C., to obtain 1.244 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0361] [Polymerization Examples 1-7] Polymerization was carried out in the same manner as in Polymerization Example 1-1, except that 0.1 μmol of compound O was used instead of compound G, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.4 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, and the internal temperature was set at 75° C., to obtain 0.707 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0362] [Polymerization Examples 1-8] Polymerization was carried out in the same manner as in Polymerization Example 1-4, except that 0.1 μmol of compound O was used instead of compound G, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.4 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, to obtain 1.521 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0363] [Polymerization Examples 1-9] Polymerization was carried out in the same manner as in Polymerization Example 1-1, except that 0.1 μmol of compound S was used instead of compound G, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.4 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, to obtain 0.982 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0364] [Polymerization Examples 1-10] Polymerization was carried out in the same manner as in Polymerization Example 1-1, except that 0.1 μmol of compound S was used instead of compound G, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.4 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, and polymerization was carried out at an internal temperature of 50° C., to obtain 0.477 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0365] [Polymerization Example 1-11] Polymerization was carried out in the same manner as in Polymerization Example 1-1, except that 0.1 μmol of compound S was used instead of compound G, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.4 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, and the internal temperature was set at 75° C., to obtain 0.122 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0366] [Polymerization Examples 1-12] Polymerization was carried out in the same manner as in Polymerization Example 1-4, except that 0.1 μmol of Compound S was used instead of Compound G, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.4 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, to obtain 0.486 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0367] [Polymerization Example 1-13] Polymerization was carried out in the same manner as in Polymerization Example 1-1, except that 0.02 μmol of compound Y was used instead of compound G, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.08 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, to obtain 0.618 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0368] [Polymerization Example 1-14] Polymerization was carried out in the same manner as in Polymerization Example 1-1, except that 0.01 μmol of compound Y was used instead of compound G, 0.1 mmol of triisobutylaluminum in terms of aluminum atom, and 0.04 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, and the internal temperature was set to 50° C., to obtain 0.917 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0369] [Polymerization Example 1-15] Polymerization was carried out in the same manner as in Polymerization Example 1-1, except that 0.01 μmol of compound Y was used instead of compound G, 0.1 mmol of triisobutylaluminum in terms of aluminum atom, and 0.04 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, and the internal temperature was set at 75° C., to obtain 0.867 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0370] [Polymerization Example 1-16] Polymerization was carried out in the same manner as in Polymerization Example 1-4, except that 0.05 μmol of compound Y was used instead of compound G, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.2 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, to obtain 0.324 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0371] [Polymerization Example 1-17] Polymerization was carried out in the same manner as in Polymerization Example 1-1, except that 0.02 μmol of Compound AE was used instead of Compound G, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.08 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, to obtain 0.488 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0372] [Polymerization Example 1-18] Polymerization was carried out in the same manner as in Polymerization Example 1-1, except that 0.02 μmol of Compound AE was used instead of Compound G, 0.1 mmol of triisobutylaluminum in terms of aluminum atom, and 0.08 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, and the internal temperature was set to 50° C., to obtain 1.093 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0373] [Polymerization Example 1-19] Polymerization was carried out in the same manner as in Polymerization Example 1-1, except that 0.02 μmol of Compound AE was used instead of Compound G, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.08 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, and the internal temperature was set at 75° C., to obtain 1.425 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0374] [Polymerization Example 1-20] Polymerization was carried out in the same manner as in Polymerization Example 1-4, except that 0.02 μmol of Compound AE, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.08 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used instead of Compound G, to obtain 0.079 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0375] [Polymerization Example 1-21] Polymerization was carried out in the same manner as in Polymerization Example 1-1, except that 0.02 μmol of compound AI was used instead of compound G, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.08 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, to obtain 0.898 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0376] [Polymerization Example 1-22] Polymerization was carried out in the same manner as in Polymerization Example 1-1, except that 0.005 μmol of compound AI was used instead of compound G, 0.05 mmol of triisobutylaluminum in terms of aluminum atom, and 0.02 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, and the internal temperature was set to 50° C., to obtain 0.897 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0377] [Polymerization Example 1-23] Polymerization was carried out in the same manner as in Polymerization Example 1-1, except that 0.2 μmol of compound AI was used instead of compound G, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.8 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, and the internal temperature was set at 75° C., to obtain 1.488 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0378] [Polymerization Example 1-24] Polymerization was carried out in the same manner as in Polymerization Example 1-4, except that 0.05 μmol of compound AI was used instead of compound G, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.2 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, to obtain 1.065 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0379] [Polymerization Example 1-25] Polymerization was carried out in the same manner as in Polymerization Example 1-1, except that 0.05 μmol of Compound AO was used instead of Compound G, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.2 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, to obtain 0.123 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0380] [Polymerization Example 1-26] Polymerization was carried out in the same manner as in Polymerization Example 1-1, except that 0.05 μmol of Compound AO was used instead of Compound G, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.2 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, and the internal temperature was set to 50° C., to obtain 0.324 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0381] [Polymerization Example 1-27] Polymerization was carried out in the same manner as in Polymerization Example 1-1, except that 0.05 μmol of Compound AO was used instead of Compound G, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.2 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, and polymerization was carried out at an internal temperature of 75° C., to obtain 0.783 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0382] [Polymerization Example 1-28] Polymerization was carried out in the same manner as in Polymerization Example 1-4, except that 0.05 μmol of Compound AO was used instead of Compound G, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.2 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, to obtain 0.137 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0383] [Polymerization Example 1-29] Polymerization was carried out in the same manner as in Polymerization Example 1-1, except that 0.05 μmol of compound AT was used instead of compound G, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.2 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, to obtain 0.255 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0384] [Polymerization Example 1-30] Polymerization was carried out in the same manner as in Polymerization Example 1-1, except that 0.05 μmol of compound AT was used instead of compound G, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.2 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, and the internal temperature was set to 50° C., to obtain 0.806 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0385] [Polymerization Example 1-31] Polymerization was carried out in the same manner as in Polymerization Example 1-1, except that 0.05 μmol of compound AT was used instead of compound G, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.2 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, and the internal temperature was set at 75° C., to obtain 1.331 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0386] [Polymerization Example 1-32] Polymerization was carried out in the same manner as in Polymerization Example 1-4, except that 0.05 μmol of compound AT, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.2 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used instead of compound G, to obtain 1.148 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0387] [Comparative Polymerization Example 1-1] Polymerization was carried out in the same manner as in Polymerization Example 1-1, except that 0.05 μmol of compound AJ was used instead of compound G, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.2 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, and the internal temperature was set to 50° C., to obtain 0.779 g of an ethylene polymer. The physical properties of the polymer are shown in Table 1.
[0388] [Comparative Polymerization Example 1-2] Polymerization was carried out in the same manner as in Polymerization Example 1-1 except that 0.05 μmol of compound AJ, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 0.2 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used instead of compound G, and the polymerization was carried out at an internal temperature of 75° C. However, only a trace amount of polymer was obtained.
[0389] [Table 1]
[0390] [Polymerization Example 2-1] 250 mL of toluene was charged into a glass reactor with an internal volume of 500 mL, which had been thoroughly purged with nitrogen, and ethylene was passed through at 100 L / hr to saturate the liquid and gas phases. Then, 0.5 mmol of methylaluminoxane (calculated as aluminum atoms) and 0.05 μmol of compound G were added to initiate polymerization. Ethylene was continuously fed at 100 L / hr, and polymerization was carried out for 5 minutes at normal pressure and an internal temperature of 25°C, after which polymerization was terminated by adding a small amount of methanol. After polymerization was completed, the reactant was added to 750 mL of methanol containing a small amount of hydrochloric acid to precipitate a polymer. After washing with the same solvent, it was dried under reduced pressure at 80°C for 10 hours, and 0.553 grams of an ethylene polymer was obtained. The physical properties of the obtained polymer are shown in Table 2.
[0391] [Polymerization Example 2-2] Polymerization was carried out in the same manner as in Polymerization Example 2-1, except that 0.25 μmol of compound G and 0.25 mmol of methylaluminoxane (calculated as aluminum atom) were used and the polymerization was carried out at an internal temperature of 50° C., to obtain 0.357 g of an ethylene polymer. The physical properties of the polymer are shown in Table 2.
[0392] [Polymerization Example 2-3] Polymerization was carried out in the same manner as in Polymerization Example 2-1, except that the polymerization was carried out at an internal temperature of 75° C., to obtain 1.439 g of an ethylene polymer. The physical properties of the polymer are shown in Table 2.
[0393] [Polymerization Example 2-4] 250mL of toluene was charged into a glass reactor with a capacity of 500mL, which had been thoroughly substituted with nitrogen, and 100L / hr of ethylene and 0.24L / hr of hydrogen were passed through to saturate the liquid and gas phases. Then, 0.25mmol of methylaluminoxane in terms of aluminum atom and 0.25μmol of compound G were added to start polymerization. Ethylene was continuously fed at 100L / hr and 0.24L / hr, and polymerization was carried out at normal pressure and an internal temperature of 50°C for 5 minutes, after which polymerization was stopped by adding a small amount of methanol. After polymerization was completed, the reactant was added to 750mL of methanol containing a small amount of hydrochloric acid to precipitate the polymer. After washing with the same solvent, it was dried under reduced pressure at 80°C for 10 hours, and 0.464 grams of ethylene polymer was obtained. The physical properties of the obtained polymer are shown in Table 2.
[0394] [Polymerization Example 2-5] Polymerization was carried out in the same manner as in Polymerization Example 2-1, except that 0.2 μmol of compound O was used instead of compound G, 0.2 mmol of methylaluminoxane was used in terms of aluminum atom, and the polymerization was carried out at an internal temperature of 50° C., to obtain 0.338 g of an ethylene polymer. The physical properties of the polymer are shown in Table 2.
[0395] [Polymerization Example 2-6] Polymerization was carried out in the same manner as in Polymerization Example 2-1, except that 0.2 μmol of compound O was used instead of compound G, 0.2 mmol of methylaluminoxane was used in terms of aluminum atom, and the polymerization was carried out at an internal temperature of 75° C., to obtain 0.407 g of an ethylene polymer. The physical properties of the polymer are shown in Table 2.
[0396] [Polymerization Example 2-7] Polymerization was carried out in the same manner as in Polymerization Example 2-1, except that 0.1 μmol of Compound S and 0.1 mmol of methylaluminoxane in terms of aluminum atom were used instead of Compound G, to obtain 0.068 g of an ethylene polymer. The physical properties of the polymer are shown in Table 2.
[0397] [Polymerization Example 2-8] Polymerization was carried out in the same manner as in Polymerization Example 2-1, except that 0.1 μmol of compound O was used instead of compound G, 0.1 mmol of methylaluminoxane was used in terms of aluminum atom, and the polymerization was carried out at an internal temperature of 50° C., to obtain 0.209 g of an ethylene polymer. The physical properties of the polymer are shown in Table 2.
[0398] [Polymerization Example 2-9] Polymerization was carried out in the same manner as in Polymerization Example 2-1, except that 0.1 μmol of compound O was used instead of compound G, 0.1 mmol of methylaluminoxane was used in terms of aluminum atom, and the polymerization was carried out at an internal temperature of 75° C., to obtain 0.131 g of an ethylene polymer. The physical properties of the polymer are shown in Table 2.
[0399] [Polymerization Example 2-10] Polymerization was carried out in the same manner as in Polymerization Example 2-4, except that 0.1 μmol of compound O and 0.1 mmol of methylaluminoxane in terms of aluminum atom were used instead of compound G, to obtain 0.06 g of an ethylene polymer. The physical properties of the polymer are shown in Table 2.
[0400] [Polymerization Example 2-11] Polymerization was carried out in the same manner as in Polymerization Example 2-1, except that 0.1 μmol of compound Y was used instead of compound G, 0.2 mmol of methylaluminoxane was used in terms of aluminum atom, and the polymerization was carried out at an internal temperature of 50° C., to obtain 0.258 g of an ethylene polymer. The physical properties of the polymer are shown in Table 2.
[0401] [Polymerization Example 2-12] Polymerization was carried out in the same manner as in Polymerization Example 2-1, except that 0.1 μmol of compound Y was used instead of compound G, 0.2 mmol of methylaluminoxane was used in terms of aluminum atom, and the polymerization was carried out at an internal temperature of 75° C., to obtain 1.467 g of an ethylene polymer. The physical properties of the polymer are shown in Table 2.
[0402] [Polymerization Example 2-13] Polymerization was carried out in the same manner as in Polymerization Example 2-1, except that 0.2 μmol of Compound AE and 0.2 mmol of methylaluminoxane in terms of aluminum atom were used instead of Compound G, to obtain 0.082 g of an ethylene polymer. The physical properties of the polymer are shown in Table 2.
[0403] [Polymerization Example 2-14] Polymerization was carried out in the same manner as in Polymerization Example 2-1, except that 0.2 μmol of Compound AE and 0.2 mmol of methylaluminoxane in terms of aluminum atom were used instead of Compound G, and the polymerization was carried out at an internal temperature of 50° C., to obtain 0.28 g of an ethylene polymer. The physical properties of the polymer are shown in Table 2.
[0404] [Polymerization Example 2-15] Polymerization was carried out in the same manner as in Polymerization Example 2-1, except that 0.2 μmol of Compound AE and 0.2 mmol of methylaluminoxane in terms of aluminum atom were used instead of Compound G, and the polymerization was carried out at an internal temperature of 75° C., to obtain 0.472 g of an ethylene polymer. The physical properties of the polymer are shown in Table 2.
[0405] [Polymerization Example 2-16] Polymerization was carried out in the same manner as in Polymerization Example 2-4, except that 0.2 μmol of Compound AE and 0.2 mmol of methylaluminoxane in terms of aluminum atom were used instead of Compound G, to obtain 0.151 g of an ethylene polymer. The physical properties of the polymer are shown in Table 2.
[0406] [Polymerization Example 2-17] Polymerization was carried out in the same manner as in Polymerization Example 2-1, except that 0.1 μmol of Compound AI and 0.2 mmol of methylaluminoxane in terms of aluminum atom were used instead of Compound G, to obtain 0.056 g of an ethylene polymer. The physical properties of the polymer are shown in Table 2.
[0407] [Polymerization Example 2-18] Polymerization was carried out in the same manner as in Polymerization Example 2-1, except that 0.1 μmol of compound AI was used instead of compound G, 0.2 mmol of methylaluminoxane was used in terms of aluminum atom, and the polymerization was carried out at an internal temperature of 50° C., to obtain 0.167 g of an ethylene polymer. The physical properties of the polymer are shown in Table 2.
[0408] [Polymerization Example 2-19] Polymerization was carried out in the same manner as in Polymerization Example 2-1, except that 0.1 μmol of compound AI was used instead of compound G, 0.2 mmol of methylaluminoxane was used in terms of aluminum atom, and the polymerization was carried out at an internal temperature of 75° C., to obtain 0.242 g of an ethylene polymer. The physical properties of the polymer are shown in Table 2.
[0409] [Polymerization Example 2-20] Polymerization was carried out in the same manner as in Polymerization Example 2-4, except that 0.1 μmol of Compound AI and 0.2 mmol of methylaluminoxane in terms of aluminum atom were used instead of Compound G, to obtain 0.156 g of an ethylene polymer. The physical properties of the polymer are shown in Table 2.
[0410] [Polymerization Example 2-21] Polymerization was carried out in the same manner as in Polymerization Example 2-1, except that 0.5 μmol of Compound AO was used instead of Compound G, 0.5 mmol of methylaluminoxane was used in terms of aluminum atom, and the polymerization was carried out at an internal temperature of 50° C., to obtain 0.064 g of an ethylene polymer. The physical properties of the polymer are shown in Table 2.
[0411] [Polymerization Example 2-22] Polymerization was carried out in the same manner as in Polymerization Example 2-1, except that 1.0 μmol of Compound AO was used instead of Compound G, 1.0 mmol of methylaluminoxane was used in terms of aluminum atom, and the polymerization was carried out at an internal temperature of 75° C., to obtain 0.099 g of an ethylene polymer. The physical properties of the polymer are shown in Table 2.
[0412] [Polymerization Example 2-23] Polymerization was carried out in the same manner as in Polymerization Example 2-1, except that 0.2 μmol of Compound AT was used instead of Compound G, 0.2 mmol of methylaluminoxane was used in terms of aluminum atom, and the polymerization was carried out at an internal temperature of 50° C., to obtain 0.086 g of an ethylene polymer. The physical properties of the polymer are shown in Table 2.
[0413] [Polymerization Example 2-24] Polymerization was carried out in the same manner as in Polymerization Example 2-1, except that 0.2 μmol of Compound AT was used instead of Compound G, 0.2 mmol of methylaluminoxane was used in terms of aluminum atom, and the polymerization was carried out at an internal temperature of 75° C., to obtain 0.096 g of an ethylene polymer. The physical properties of the polymer are shown in Table 2.
[0414] [Comparative Polymerization Example 2-1] Polymerization was carried out in the same manner as in Polymerization Example 2-1 except that 1.0 μmol of compound AJ and 1.0 mmol of methylaluminoxane in terms of aluminum atom were used instead of compound G and the polymerization was carried out at an internal temperature of 50° C., but only a trace amount of resin was obtained.
[0415] [Comparative Polymerization Example 2-2] Polymerization was carried out in the same manner as in Polymerization Example 2-1 except that 1.0 μmol of compound AJ and 1.0 mmol of methylaluminoxane in terms of aluminum atom were used instead of compound G and the polymerization was carried out at an internal temperature of 75° C. However, only a trace amount of resin was obtained.
[0416] [Table 2]
[0417] <Production of ethylene-propylene copolymer> [Polymerization Example 3-1] 250mL of toluene was charged into a glass reactor with an internal volume of 500mL, which had been thoroughly substituted with nitrogen, and 100L / hr of ethylene and 100L / hr of propylene were passed through to saturate the liquid and gas phases. Then, 0.2mmol of triisobutylaluminum in terms of aluminum atom, 0.0625μmol of compound G, and 0.25μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were added to initiate polymerization. Ethylene was continuously supplied at 100L / hr and 100L / hr of propylene, and polymerization was carried out for 10 minutes at normal pressure and an internal temperature of 50°C, after which a small amount of methanol was added to terminate the polymerization. After the polymerization was completed, the toluene solution containing the polymer was transferred to a separatory funnel. An aqueous hydrochloric acid solution was prepared by adding 2mL of concentrated hydrochloric acid to 200mL of water, and the organic layer was washed by adding it to a separatory funnel, and the organic layer was separated from the aqueous layer. The organic layer was washed again with an aqueous hydrochloric acid solution, and then washed with 200mL of distilled water, and the organic layer was separated from the aqueous layer. The organic layer was concentrated using a rotary evaporator, and the resulting polymer was dried under reduced pressure at 80°C for 10 hours to obtain 0.893 g of an ethylene-propylene polymer. The physical properties of the resulting polymer are shown in Table 3.
[0418] [Polymerization Example 3-2] 250mL of toluene was charged into a glass reactor with an internal volume of 500mL, which had been thoroughly substituted with nitrogen, and ethylene was passed through at 50L / hr and propylene at 100L / hr to saturate the liquid and gas phases. Then, 0.2mmol of triisobutylaluminum was added in terms of aluminum atom, 0.0625μmol of compound G, and 0.25μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were added to initiate polymerization. Ethylene was continuously supplied at 100L / hr and propylene at 100L / hr, and polymerization was carried out for 10 minutes at an internal temperature of 50°C under normal pressure, after which a small amount of methanol was added to terminate the polymerization. After the polymerization was completed, the toluene solution containing the polymer was transferred to a separatory funnel. An aqueous hydrochloric acid solution was prepared by adding 2mL of concentrated hydrochloric acid to 200mL of water, and the organic layer was washed by adding it to a separatory funnel, and the organic layer was separated from the aqueous layer. The organic layer was washed again with an aqueous hydrochloric acid solution, and then washed with 200mL of distilled water, and the organic layer was separated from the aqueous layer. The organic layer was concentrated using a rotary evaporator, and the resulting polymer was dried under reduced pressure at 80°C for 10 hours to obtain 0.606 g of an ethylene-propylene polymer. The physical properties of the resulting polymer are shown in Table 3.
[0419] [Polymerization Example 3-3] Polymerization was carried out in the same manner as in Polymerization Example 3-1, except that 5 μmol of compound O, 0.5 mmol of triisobutylaluminum in terms of aluminum atom, and 20 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used instead of compound G, to obtain 0.358 g of ethylene-propylene copolymer. The physical properties of the obtained polymer are shown in Table 3.
[0420] [Polymerization Example 3-4] Polymerization was carried out in the same manner as in Polymerization Example 3-2, except that 5 μmol of compound O, 0.5 mmol of triisobutylaluminum in terms of aluminum atom, and 20 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used instead of compound G, to obtain 0.131 g of ethylene-propylene copolymer. The physical properties of the obtained polymer are shown in Table 3.
[0421] [Polymerization Example 3-5] Polymerization was carried out in the same manner as in Polymerization Example 3-1, except that 4 μmol of compound S was used instead of compound G, 0.4 mmol of triisobutylaluminum (calculated as aluminum atom), and 16 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, to obtain 0.461 g of ethylene-propylene copolymer. The physical properties of the obtained polymer are shown in Table 3.
[0422] [Polymerization Examples 3-6] Polymerization was carried out in the same manner as in Polymerization Example 3-2, except that 4 μmol of compound S was used instead of compound G, 0.4 mmol of triisobutylaluminum (calculated as aluminum atom), and 16 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used, and 0.142 g of ethylene-propylene copolymer was obtained. The physical properties of the obtained polymer are shown in Table 3.
[0423] [Polymerization Examples 3-7] Polymerization was carried out in the same manner as in Polymerization Example 3-1, except that 0.05 μmol of compound Y, 0.2 mmol of triisobutylaluminum (calculated as aluminum atom), and 0.2 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used instead of compound G, to obtain 0.186 g of ethylene-propylene copolymer. The physical properties of the obtained polymer are shown in Table 3.
[0424] [Polymerization Example 3-8] Polymerization was carried out in the same manner as in Polymerization Example 3-2, except that 0.25 μmol of compound Y, 0.2 mmol of triisobutylaluminum (calculated as aluminum atom), and 1.0 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used instead of compound G, to obtain 0.565 g of ethylene-propylene copolymer. The physical properties of the obtained polymer are shown in Table 3.
[0425] [Polymerization Example 3-9] Polymerization was carried out in the same manner as in Polymerization Example 3-1, except that 0.05 μmol of compound AE, 0.2 mmol of triisobutylaluminum (calculated as aluminum atom), and 0.2 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used instead of compound G, to obtain 0.155 g of ethylene-propylene copolymer. The physical properties of the obtained polymer are shown in Table 3.
[0426] [Polymerization Example 3-10] Polymerization was carried out in the same manner as in Polymerization Example 3-1, except that 0.2 μmol of compound AE, 0.2 mmol of triisobutylaluminum (calculated as aluminum atom), and 0.8 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used instead of compound G, to obtain 0.484 g of ethylene-propylene copolymer. The physical properties of the obtained polymer are shown in Table 3.
[0427] [Polymerization Example 3-11] Polymerization was carried out in the same manner as in Polymerization Example 3-1, except that 0.05 μmol of compound AI, 0.2 mmol of triisobutylaluminum (calculated as aluminum atom), and 0.2 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used instead of compound G, to obtain 0.234 g of ethylene-propylene copolymer. The physical properties of the obtained polymer are shown in Table 3.
[0428] [Polymerization Example 3-12] Polymerization was carried out in the same manner as in Polymerization Example 3-1, except that 0.1 μmol of compound AI, 0.2 mmol of triisobutylaluminum (calculated as aluminum atom), and 0.4 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used instead of compound G, to obtain 0.201 g of ethylene-propylene copolymer. The physical properties of the obtained polymer are shown in Table 3.
[0429] [Polymerization Example 3-13] Polymerization was carried out in the same manner as in Polymerization Example 3-1, except that 1.0 μmol of Compound AO, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 4.0 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used instead of Compound G, to obtain 3.85 g of ethylene-propylene copolymer. The physical properties of the obtained polymer are shown in Table 3.
[0430] [Polymerization Example 3-14] Polymerization was carried out in the same manner as in Polymerization Example 3-1, except that 1.0 μmol of Compound AO, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 4.0 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used instead of Compound G, to obtain 1.68 g of ethylene-propylene copolymer. The physical properties of the obtained polymer are shown in Table 3.
[0431] [Polymerization Example 3-15] Polymerization was carried out in the same manner as in Polymerization Example 3-1, except that 0.5 μmol of compound AT, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 2.0 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used instead of compound G, to obtain 1.48 g of ethylene-propylene copolymer. The physical properties of the obtained polymer are shown in Table 3.
[0432] [Polymerization Example 3-16] Polymerization was carried out in the same manner as in Polymerization Example 3-1, except that 0.5 μmol of compound AT, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, and 2.0 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used instead of compound G, to obtain 0.613 g of ethylene-propylene copolymer. The physical properties of the obtained polymer are shown in Table 3.
[0433] [Table 3]
[0434] <Production of ethylene / propylene / ENB copolymer> [Polymerization Example 4-1] 250mL of toluene was charged into a 500mL glass reactor that had been thoroughly purged with nitrogen, 0.1mL of 5-ethylidene-2-norbornene (ENB) was added, and 100L / hr of ethylene and 100L / hr of propylene were passed through to saturate the liquid and gas phases. Polymerization was initiated by adding 0.2mmol of triisobutylaluminum in terms of aluminum atom, 0.1μmol of compound G, and 0.4μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate. Ethylene was continuously supplied at 100L / hr and 100L / hr of propylene, and polymerization was carried out for 10 minutes at normal pressure and an internal temperature of 50°C. The polymerization was then terminated by adding a small amount of methanol. A solution was prepared by adding 2mL of concentrated hydrochloric acid to a 1L solution of methanol and acetone mixed in a 1:2 ratio, and the toluene solution containing the polymer was poured into the solution and stirred. The precipitated polymer was filtered off and washed with a small amount of acetone. The resulting polymer was dried under reduced pressure at 130° C. for 10 hours to obtain 0.893 g of an ethylene / propylene / ENB copolymer. The physical properties of the resulting polymer are shown in Table 4.
[0435] [Polymerization Example 4-2] Polymerization was carried out in the same manner as in Example 4-1, except that 0.5 μmol of compound Y and 2.0 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used instead of compound G, to obtain 1.185 g of ethylene / propylene / ENB copolymer. The physical properties of the obtained polymer are shown in Table 4.
[0436] [Polymerization Example 4-3] Polymerization was carried out in the same manner as in Example 4-1, except that 0.5 μmol of compound AE and 2.0 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used instead of compound G, to obtain 0.913 g of an ethylene / propylene / ENB copolymer. The physical properties of the obtained polymer are shown in Table 4.
[0437] [Comparative Polymerization Example 4-1] 250mL of toluene was charged into a 500mL glass reactor that had been thoroughly purged with nitrogen, 0.3mL of 5-ethylidene-2-norbornene (ENB) was added, and 140L / hr of ethylene and 20L / hr of propylene were passed through to saturate the liquid and gas phases. Polymerization was initiated by adding 0.2mmol of triisobutylaluminum in terms of aluminum atom, 0.2μmol of compound AJ, and 0.8μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate. Ethylene was continuously fed at 140L / hr and 20L / hr of propylene, and polymerization was carried out for 10 minutes at normal pressure and an internal temperature of 50°C. The polymerization was then terminated by adding a small amount of methanol. A solution was prepared by adding 2mL of concentrated hydrochloric acid to 1L of a solution in which methanol and acetone were mixed in a 1:2 ratio, and the toluene solution containing the polymer was poured into the solution and stirred. The precipitated polymer was filtered off and washed with a small amount of acetone. The resulting polymer was dried under reduced pressure at 130° C. for 10 hours to obtain 0.518 g of an ethylene / propylene / ENB copolymer. The physical properties of the resulting polymer are shown in Table 4.
[0438] [Table 4]
[0439] As shown in Table 4, the complexes (compounds G, Y, and AE) used in Examples 4-1 to 4-3 had 1 / 3 the amount of ENB added compared to the complex (compound AJ) used in Comparative Example 4-1, but when the complexes of Examples 4-2 to 4-3 were used, polymers with the same ENB content as the complex (compound AJ) used in Comparative Example 4-1 were obtained, and when the complex of Example 4-1 was used, a polymer containing an even higher amount of ENB was obtained. It can be seen that the complexes used in Examples 4-1 to 4-3 have better copolymerizability with cyclic olefin (ENB) in the resulting polymers than the complex (compound AJ) used in Comparative Example 4-1.
[0440] <Production of ethylene / tetracyclododecene copolymer> [Polymerization Example 5-1] In a glass reactor with a volume of 500 mL, 216 mL of cyclohexane and 24 mL of hexane were placed, and 9.8 mL of tetracyclododecene (hereinafter also referred to as "TD") was added. Ethylene was passed through at 50 L / hr to saturate the liquid phase and the gas phase. Polymerization was started by adding 0.2 mmol of triisobutylaluminum in terms of aluminum atom, 1.0 μmol of compound G, and 4.0 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate. Ethylene was continuously fed at 50 L / hr, and polymerization was carried out for 10 minutes at an internal temperature of 50°C under normal pressure, and then a small amount of methanol was added to terminate the polymerization. A solution was prepared by adding 300 mL of methanol, 900 mL of acetone, and 2 mL of concentrated hydrochloric acid, and the solution containing the polymer was poured in and stirred. The precipitated polymer was filtered off and washed with a small amount of acetone. The obtained polymer was dried under reduced pressure at 130°C for 10 hours, and 0.145 grams of ethylene / tetracyclododecene copolymer was obtained. The physical properties of the obtained polymer are shown in Table 5.
[0441] [Polymerization Example 5-2] Polymerization was carried out in the same manner as in Polymerization Example 5-1, except that 4.9 mL of tetracyclododecene was added, to obtain 0.499 g of an ethylene / tetracyclododecene copolymer. The physical properties of the obtained polymer are shown in Table 5.
[0442] [Polymerization Example 5-3] The polymerization was carried out in the same manner as in Polymerization Example 5-1, except that 108 mL of cyclohexane, 12 mL of hexane, and 1.25 mL of tetracyclododecene were added, and 0.5 μmol of compound G and 2.0 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were added, to obtain 0.407 g of an ethylene / tetracyclododecene copolymer. The physical properties of the obtained polymer are shown in Table 5.
[0443] [Polymerization Example 5-4] Polymerization was performed in the same manner as in Polymerization Example 5-1, except that 2.0 μmol of compound Y and 8.0 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used instead of compound G, to obtain 0.098 g of an ethylene / tetracyclododecene copolymer. The physical properties of the obtained polymer are shown in Table 5.
[0444] [Polymerization Example 5-5] Polymerization was performed in the same manner as in Polymerization Example 5-1, except that 2.0 μmol of Compound AE and 8.0 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used instead of Compound G, to obtain 0.13 g of an ethylene / tetracyclododecene copolymer. The physical properties of the obtained polymer are shown in Table 5.
[0445] [Polymerization Example 5-6] Polymerization was performed in the same manner as in Polymerization Example 5-1, except that 2.0 μmol of Compound AI and 8.0 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used instead of Compound G, to obtain 0.60 g of an ethylene / tetracyclododecene copolymer. The physical properties of the obtained polymer are shown in Table 5.
[0446] [Comparative Polymerization Example 5-1] Polymerization was performed in the same manner as in Polymerization Example 5-1, except that 0.5 μmol of Compound AJ and 2.0 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were used instead of Compound G, to obtain 0.127 g of an ethylene / tetracyclododecene copolymer. The physical properties of the obtained polymer are shown in Table 5.
[0447] [Table 5]
[0448] In Examples 5-1 to 5-6 and Comparative Example 5-1, Tg (glass transition temperature) was used as an index of the TD (tetracyclododecene) content in the polymer, since the higher the TD content in the polymer, the higher the Tg tends to be. In addition, since the amount of solvent used during synthesis in each Example 5-1 to 5-6 and Comparative Example 5-1 is different, the TD concentration during polymerization was calculated from the amount of solvent used in the Examples and Comparative Examples and the amount of TD added at that time, and the copolymerizability was evaluated based on the TD concentration. Note that the higher the Tg value of the obtained polymer, the more TD is incorporated into the polymer, and therefore it can be judged that the copolymerizability between α-olefin and TD is excellent.
[0449] As shown in Table 5, Examples 5-1, 5-4, 5-5 and 5-6, which were polymerized under the condition of a TD concentration of 3.9%, all have higher Tg values and more TD is incorporated than Comparative Example 5-1. This shows that the use of the complexes of the Examples results in excellent copolymerization properties. Examples 5-1 to 5-3 are examples in which the amount of TD used during polymerization was changed (therefore, the concentration of TD in the solvent also decreased with the decrease in the amount of TD added). When the concentration of TD used was decreased, the amount of TD incorporated in the polymer decreased, and the Tg value also decreased. In Example 5-3, a Tg of 125°C was obtained when polymerization was performed under conditions of a TD concentration of 1.0%, whereas in Comparative Example 5-1, a Tg of 115°C was obtained under conditions of a TD concentration of 3.9%. In Example 5-3, a high Tg was obtained despite the TD concentration being about 1 / 4 of that in Comparative Example 5-1. This shows that when polymerization was performed using the complex of the Examples, the copolymerization of α-olefin with cyclic olein was excellent. In addition, when comparing the activities of Example 5-3 and Comparative Example 5-1, which have relatively close Tg values, it is found that Example 5-3 exhibits higher polymerization activity than Comparative Example 5-1, and is also superior in polymerization activity.
[0450] [Polymerization Example 6-1] In a glass reactor with a volume of 500 mL, 108 mL of cyclohexane and 12 mL of hexane were placed, and 8.9 mL of benzonorbornadiene (hereinafter also referred to as "BNBD") was added. Ethylene was passed through at 50 L / hr to saturate the liquid phase and the gas phase. Polymerization was started by adding 0.2 mmol of triisobutylaluminum in terms of aluminum atom, 1.0 μmol of compound G, and 4.0 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate. Ethylene was continuously fed at 50 L / hr, and polymerization was carried out for 10 minutes at normal pressure and an internal temperature of 50°C. The polymerization was then terminated by adding a small amount of methanol. A solution was prepared by adding 300 mL of methanol, 900 mL of acetone, and 2 mL of concentrated hydrochloric acid, and the solution containing the polymer was poured in and stirred. The precipitated polymer was filtered off and washed with a small amount of acetone. The obtained polymer was dried under reduced pressure at 130°C for 10 hours to obtain 0.32 grams of ethylene / BNBD copolymer. The physical properties of the obtained polymer are shown in Table 6.
[0451] [Polymerization Example 6-2] Polymerization was carried out in the same manner as in Polymerization Example 6-1, except that 0.2 μmol of compound G, 0.8 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate, and 4.45 mL of BNBD were added, to obtain 0.043 g of an ethylene / BNBD copolymer. The physical properties of the obtained polymer are shown in Table 6.
[0452] [Polymerization Example 6-3] Polymerization was carried out in the same manner as in Polymerization Example 6-1, except that 0.2 μmol of compound G, 0.8 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate, and 2.25 mL of BNBD were added, to obtain 0.111 g of an ethylene / BNBD copolymer. The physical properties of the obtained polymer are shown in Table 6.
[0453] [Polymerization Example 6-4] In a 500mL glass reactor that had been thoroughly purged with nitrogen, 108mL of cyclohexane and 12mL of hexane were placed, 8.9mL of BNBD was added, and ethylene was passed through at 50L / hr to saturate the liquid and gas phases. Polymerization was initiated by adding 0.2mmol of MMAO (modified methylaluminoxane) (Tosoh Finechem Co., Ltd.) in terms of aluminum atom, 1.0μmol of compound G, and 4.0μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate. Ethylene was continuously fed at 50L / hr, and polymerization was carried out for 10 minutes at normal pressure and an internal temperature of 50℃, after which polymerization was terminated by adding a small amount of methanol. A solution was prepared by adding 300mL of methanol, 900mL of acetone, and 2mL of concentrated hydrochloric acid, and the solution containing the polymer was poured in and stirred. The precipitated polymer was filtered off and washed with a small amount of acetone. The obtained polymer was dried under reduced pressure at 130℃ for 10 hours, yielding 1.16g of ethylene / BNBD copolymer. The physical properties of the obtained polymer are shown in Table 6.
[0454] [Polymerization Example 6-5] Polymerization was carried out in the same manner as in Polymerization Example 6-4, except that 4.45 mL of BNBD was added, to obtain 0.842 g of an ethylene / BNBD copolymer. The physical properties of the obtained polymer are shown in Table 6.
[0455] [Polymerization Example 6-6] Polymerization was carried out in the same manner as in Polymerization Example 6-4 except that 0.5 μmol of compound G, 2.0 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate, and 2.25 mL of BNBD were added, to obtain 1.10 g of an ethylene / BNBD copolymer. The physical properties of the obtained polymer are shown in Table 6.
[0456] [Polymerization Examples 6-7] Polymerization was carried out in the same manner as in Polymerization Example 6-4, except that 1.0 μmol of compound Y, 4.0 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate, and 8.9 mL of BNBD were added, to obtain 0.14 g of an ethylene / BNBD copolymer. The physical properties of the obtained polymer are shown in Table 6.
[0457] [Polymerization Examples 6-8] Polymerization was carried out in the same manner as in Polymerization Example 6-4, except that 1.0 μmol of compound Y, 4.0 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate, and 4.45 mL of BNBD were added, to obtain 0.24 g of an ethylene / BNBD copolymer. The physical properties of the obtained polymer are shown in Table 6.
[0458] [Polymerization Examples 6-9] Polymerization was carried out in the same manner as in Polymerization Example 6-4, except that 1.0 μmol of compound AE, 4.0 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate, and 8.9 mL of BNBD were added, to obtain 0.09 g of an ethylene / BNBD copolymer. The physical properties of the obtained polymer are shown in Table 6.
[0459] [Polymerization Examples 6-10] Polymerization was carried out in the same manner as in Polymerization Example 6-4, except that 1.0 μmol of compound AE, 4.0 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate, and 4.45 mL of BNBD were added, to obtain 0.16 g of an ethylene / BNBD copolymer. The physical properties of the obtained polymer are shown in Table 6.
[0460] [Comparative Polymerization Example 6-1] Polymerization was carried out in the same manner as in Polymerization Example 6-1 except that 1.0 μmol of Compound AJ was used, but no polymer was obtained.
[0461] [Table 6]
[0462] As shown in Table 6, the progress of the polymerization reaction was not confirmed in the complex of Comparative Example 6-1. It can be seen that the complex of Example 6-1 exhibits superior activity compared to the complex of Comparative Example 6-1. It can also be seen that the polymerization reaction proceeds even in Examples 6-4 to 6-10, in which MMAO was used as the scavenger instead of TiBAL.
[0463] [Polymerization Example 7-1] <Preparation of solid aluminoxane (S)> The solid aluminoxane was prepared according to the method described in International Publication WO 2010 / 055652 (Preliminary Experiment 1 and Example 5). However, in consideration of the safety of trimethylaluminum, such as ignition, the preparation was carried out at a concentration about 1 / 6 of the conditions disclosed in the document.
[0464] Specifically, 100 mL of a toluene solution of triethylaluminum adjusted to 0.5 mol / L was charged into a glass reactor equipped with a stirrer. The solution was cooled to 15°C, and 2.18 g of benzoic acid was slowly added to it at a rate such that the temperature of the solution was 25°C or less. Then, heat aging was performed at 50°C for 1 hour. At this time, the molar ratio of oxygen atoms of trimethylaluminum and benzoic acid was 1.40. The reaction solution was heated at 70°C for 4 hours, then heated at 60°C for 6 hours, and then cooled to room temperature once. Then, it was heated at 100°C for 8 hours to precipitate solid aluminoxane. After cooling the solution to 30°C or less, 100 mL of n-hexane was added under stirring for washing. After standing for 30 minutes, 150 mL of the supernatant was removed, and 150 mL of n-hexane was added under stirring. After standing for 15 minutes, 150 mL of the supernatant was removed, and 150 mL of n-hexane was added with stirring. Finally, after standing for 15 minutes, 180 mL of the supernatant was removed, and n-hexane was added to a total volume of 42 mL. A part of the hexane slurry of the obtained solid aluminoxane was sampled and the concentration was examined, which was found to be 14.2 g / L and Al concentration 0.202 mol / L. In addition, when the particles of the obtained solid aluminoxane were observed with a scanning electron microscope, the average particle diameter was 6.8 μm and the specific surface area was 18.1 m. 2 / mmol-Al.
[0465] <Preparation of olefin polymerization catalyst [G-1]> A 30 mL glass vessel equipped with a magnetic stirrer and thoroughly purged with nitrogen was charged with 21.29 mL of dehydrated toluene and 1.27 mL (1.71 mmol in terms of Al atoms) of the hexane slurry of the solid aluminoxane (S) prepared above was charged. Next, 2.44 mL (0.0122 mmol in terms of Ti atoms) of the toluene solution of the compound G synthesized above was dropped and reacted at room temperature for 2 hours. After leaving it to stand for more than 1 hour, 20 mL of the supernatant was removed and 20 mL of hexane was added. This operation was repeated three times to obtain an olefin polymerization catalyst [G-1].
[0466] <Ethylene polymerization> 500mL of purified heptane was placed in a 1L SUS autoclave that had been thoroughly purged with nitrogen, and ethylene was passed through to saturate the liquid and gas phases with ethylene. 0.25mmol of triisobutylaluminum n-decane solution (Al=1.0mol / L) and 10.0mg of olefin polymerization catalyst [G-1] were charged in solid component equivalent, and then the temperature was raised to 75°C using ethylene / hydrogen mixed gas with a hydrogen concentration of 1.25vol%, and ethylene / hydrogen mixed gas was continuously fed to 0.65MPaG, and polymerization reaction was carried out for 60 minutes. The obtained polymer was filtered and then vacuum dried at 80°C for 10 hours to obtain 13.2g of ethylene polymer. The physical properties of the obtained polymer are shown in Table 7.
[0467] [Polymerization Example 7-2] Polymerization was carried out in the same manner as in Polymerization Example 7-1, except that a mixed gas of ethylene and hydrogen with a hydrogen concentration of 0.45 vol% was used, to obtain 9.1 g of an ethylene polymer. The physical properties of the obtained polymer are shown in Table 7.
[0468] [Polymerization Example 7-3] Polymerization was carried out in the same manner as in Polymerization Example 7-1, except that ethylene gas was used, to obtain 5.6 g of an ethylene polymer. The physical properties of the obtained polymer are shown in Table 7.
[0469] [Polymerization Example 7-4] <Preparation of olefin polymerization catalyst [Y-1]> A 30 mL glass vessel equipped with a magnetic stirrer and thoroughly purged with nitrogen was charged with 21.29 mL of dehydrated toluene and 1.27 mL (1.71 mmol in terms of Al atoms) of the hexane slurry of the solid aluminoxane (S) prepared above was charged. Next, 2.44 mL (0.0122 mmol in terms of Ti atoms) of the toluene solution of the compound Y synthesized above was dropped and reacted at room temperature for 2 hours. After leaving it to stand for more than 1 hour, 20 mL of the supernatant was removed and 20 mL of hexane was added. This operation was repeated three times to obtain an olefin polymerization catalyst [Y-1].
[0470] <Ethylene polymerization> 500mL of purified heptane was placed in a 1L SUS autoclave that had been thoroughly purged with nitrogen, and ethylene was passed through to saturate the liquid and gas phases with ethylene. 0.25mmol of triisobutylaluminum n-decane solution (Al=1.0mol / L) and 10.0mg of olefin polymerization catalyst [Y-1] were charged in this autoclave in terms of solid components, and then the temperature was raised to 75°C using an ethylene / hydrogen mixed gas with a hydrogen concentration of 1.25vol%, and ethylene / hydrogen mixed gas was continuously fed to 0.65MPaG, and polymerization reaction was carried out for 60 minutes. The obtained polymer was filtered and then vacuum dried at 80°C for 10 hours to obtain 50.6g of ethylene polymer. The physical properties of the obtained polymer are shown in Table 7.
[0471] [Polymerization Example 7-5] Polymerization was carried out in the same manner as in Polymerization Example 7-4, except that a mixed gas of ethylene and hydrogen with a hydrogen concentration of 0.45 vol% was used, to obtain 52.9 g of an ethylene polymer. The physical properties of the obtained polymer are shown in Table 7.
[0472] [Polymerization Example 7-6] Polymerization was carried out in the same manner as in Polymerization Example 7-4, except that ethylene gas was used, to obtain 49.1 g of an ethylene polymer. The physical properties of the obtained polymer are shown in Table 7.
[0473] [Polymerization Example 7-7] <Preparation of olefin polymerization catalyst [AE-1]> A 30 mL glass vessel equipped with a magnetic stirrer and thoroughly purged with nitrogen was charged with 21.29 mL of dehydrated toluene and 1.27 mL (1.71 mmol in terms of Al atoms) of the hexane slurry of the solid aluminoxane (S) prepared above was then charged. Next, 2.44 mL (0.0122 mmol in terms of Ti atoms) of the toluene solution of the compound AE synthesized above was added dropwise and reacted at room temperature for 2 hours. After leaving to stand for 1 hour or more, 20 mL of the supernatant was removed and 20 mL of hexane was added. This operation was repeated three more times to obtain an olefin polymerization catalyst [AE-1].
[0474] <Ethylene polymerization> 500mL of purified heptane was placed in a 1L SUS autoclave that had been thoroughly purged with nitrogen, and ethylene was passed through to saturate the liquid and gas phases with ethylene. 0.25mmol of triisobutylaluminum n-decane solution (Al=1.0mol / L) and 10.0mg of olefin polymerization catalyst [AE-1] were charged in solid component equivalent, and then the temperature was raised to 75°C using ethylene / hydrogen mixed gas with a hydrogen concentration of 1.25vol%, and ethylene / hydrogen mixed gas was continuously fed to 0.65MPaG, and polymerization reaction was carried out for 60 minutes. The obtained polymer was filtered and then vacuum dried at 80°C for 10 hours to obtain 25.0g of ethylene polymer. The physical properties of the obtained polymer are shown in Table 7.
[0475] [Polymerization Examples 7-8] Polymerization was carried out in the same manner as in Polymerization Example 7-7, except that a mixed gas of ethylene and hydrogen with a hydrogen concentration of 0.45 vol% was used, to obtain 20.1 g of an ethylene polymer. The physical properties of the obtained polymer are shown in Table 7.
[0476] [Polymerization Examples 7-9] Polymerization was carried out in the same manner as in Polymerization Example 7-7, except that ethylene gas was used, to obtain 16.4 g of an ethylene polymer. The physical properties of the obtained polymer are shown in Table 7.
[0477] [Polymerization Examples 7-10] <Preparation of olefin polymerization catalyst [AI-1]> A 30 mL glass vessel equipped with a magnetic stirrer and thoroughly purged with nitrogen was charged with 21.29 mL of dehydrated toluene and 1.27 mL (1.71 mmol in terms of Al atoms) of the hexane slurry of the solid aluminoxane (S) prepared above was charged. Next, 2.44 mL (0.0122 mmol in terms of Ti atoms) of the toluene solution of the compound AI synthesized above was dropped and reacted at room temperature for 2 hours. After leaving it to stand for more than 1 hour, 20 mL of the supernatant was removed and 20 mL of hexane was added. This operation was repeated three more times to obtain an olefin polymerization catalyst [AI-1].
[0478] <Ethylene polymerization> 500mL of purified heptane was placed in a 1L SUS autoclave that had been thoroughly purged with nitrogen, and ethylene was passed through to saturate the liquid and gas phases with ethylene. 0.25mmol of triisobutylaluminum n-decane solution (Al=1.0mol / L) and 10.0mg of olefin polymerization catalyst [AI-1] were charged in solid component equivalent, and then the temperature was raised to 75°C using an ethylene / hydrogen mixed gas with a hydrogen concentration of 1.25vol%, and ethylene / hydrogen mixed gas was continuously fed to 0.65MPaG, and polymerization reaction was carried out for 60 minutes. The obtained polymer was filtered and then vacuum dried at 80°C for 10 hours to obtain 14.9g of ethylene polymer. The physical properties of the obtained polymer are shown in Table 7.
[0479] [Polymerization Examples 7-11] Polymerization was carried out in the same manner as in Polymerization Example 7-10, except that a mixed gas of ethylene and hydrogen with a hydrogen concentration of 0.45 vol% was used, to obtain 14.3 g of an ethylene polymer. The physical properties of the obtained polymer are shown in Table 7.
[0480] [Polymerization Examples 7-12] Polymerization was carried out in the same manner as in Polymerization Example 7-10, except that ethylene gas was used, to obtain 12.3 g of an ethylene polymer. The physical properties of the obtained polymer are shown in Table 7.
[0481] [Comparative Polymerization Example 7-1] <Preparation of olefin polymerization catalyst [AJ-1]> A 30 mL glass vessel equipped with a magnetic stirrer and thoroughly purged with nitrogen was charged with 20.11 mL of dehydrated toluene and 2.40 mL (3.57 mmol in terms of Al atoms) of the hexane slurry of the solid aluminoxane (S) prepared above. Next, 2.49 mL (0.0249 mmol in terms of Ti atoms) of the toluene solution of the compound AJ synthesized above was added dropwise and reacted at room temperature for 2 hours. After leaving it to stand for more than 1 hour, 20 mL of the supernatant was removed and 20 mL of hexane was added. This operation was repeated three times to obtain an olefin polymerization catalyst [AJ-1].
[0482] <Ethylene polymerization> 500mL of purified heptane was placed in a 1L SUS autoclave that had been thoroughly purged with nitrogen, and ethylene was passed through to saturate the liquid and gas phases with ethylene. 0.25mmol of triisobutylaluminum n-decane solution (Al=1.0mol / L) and 20.0mg of olefin polymerization catalyst [AJ-1] were charged in solid component equivalent, and then the temperature was raised to 75°C using ethylene / hydrogen mixed gas with a hydrogen concentration of 1.25vol%, and ethylene / hydrogen mixed gas was continuously fed to 0.65MPaG, and polymerization reaction was carried out for 60 minutes. The obtained polymer was filtered and then vacuum dried at 80°C for 10 hours to obtain 0.06g of ethylene polymer. The physical properties of the obtained polymer are shown in Table 7.
[0483] [Comparative Polymerization Example 7-2] Polymerization was carried out in the same manner as in Comparative Polymerization Example 7-1, except that a mixed gas of ethylene and hydrogen with a hydrogen concentration of 0.45 vol% was used, to obtain 0.08 g of an ethylene polymer. The physical properties of the obtained polymer are shown in Table 7.
[0484] [Comparative Polymerization Example 7-3] Polymerization was carried out in the same manner as in Comparative Polymerization Example 7-1, except that ethylene gas was used, to obtain 0.33 g of an ethylene polymer. The physical properties of the obtained polymer are shown in Table 7.
[0485] [Table 7]
[0486] [Polymerization Example 8-1] 500mL of purified heptane was placed in a 1L SUS autoclave that had been thoroughly purged with nitrogen, and ethylene was passed through to saturate the liquid and gas phases with ethylene. 0.25mmol of triisobutylaluminum n-decane solution (Al=1.0mol / L), 3mL of dehydrated 1-hexene, and 10.0mg of olefin polymerization catalyst [G-1] were charged in this autoclave in terms of solid components, and then the temperature was raised to 75°C using an ethylene / hydrogen mixed gas with a hydrogen concentration of 0.10vol%, and ethylene / hydrogen mixed gas was continuously fed to 0.65MPaG, and polymerization reaction was carried out for 60 minutes. The obtained polymer was filtered and then vacuum dried at 80°C for 10 hours to obtain 9.80g of ethylene polymer. The physical properties of the obtained polymer are shown in Table 8.
[0487] [Polymerization Example 8-2] Polymerization was carried out in the same manner as in Polymerization Example 8-1, except that 6 mL of dehydrated 1-hexene was used, to obtain 9.51 g of an ethylene polymer. The physical properties of the obtained polymer are shown in Table 8.
[0488] [Polymerization Example 8-3] Polymerization was carried out in the same manner as in Polymerization Example 8-1, except that the olefin polymerization catalyst [Y-1] was used, to obtain 91.78 g of an ethylene polymer. The physical properties of the obtained polymer are shown in Table 8.
[0489] [Polymerization Example 8-4] Polymerization was carried out in the same manner as in Polymerization Example 8-1, except that the olefin polymerization catalyst [Y-1] and 6 mL of dehydrated 1-hexene were used, to obtain an ethylene polymer of 91.80 g. The physical properties of the obtained polymer are shown in Table 8.
[0490] [Polymerization Example 8-5] Polymerization was carried out in the same manner as in Polymerization Example 8-1, except that the olefin polymerization catalyst [AE-1] was used, to obtain 32.69 g of an ethylene polymer. The physical properties of the obtained polymer are shown in Table 8.
[0491] [Polymerization Example 8-6] Polymerization was carried out in the same manner as in Polymerization Example 8-1, except that the olefin polymerization catalyst [AE-1] and 6 mL of dehydrated 1-hexene were used, to obtain 29.42 g of an ethylene polymer. The physical properties of the obtained polymer are shown in Table 8.
[0492] [Polymerization Example 8-7] Polymerization was carried out in the same manner as in Polymerization Example 8-1, except that the olefin polymerization catalyst [AI-1] was used, to obtain 23.38 g of an ethylene polymer. The physical properties of the obtained polymer are shown in Table 8.
[0493] [Polymerization Example 8-8] Polymerization was carried out in the same manner as in Polymerization Example 8-1, except that the olefin polymerization catalyst [AI-1] and 6 mL of dehydrated 1-hexene were used, to obtain 22.31 g of an ethylene polymer. The physical properties of the obtained polymer are shown in Table 8.
[0494] [Table 8]
[0495] It is seen that the polymerization catalyst containing the organometallic complex of the Example has superior polymerization activity compared to the polymerization catalyst containing the organometallic complex of the Comparative Example, even when the polymerization reaction is carried out under the condition of 75°C. In particular, it is seen that excellent polymerization activity is exhibited even in the copolymerization of ethylene and cyclic olefin. It is seen that when the polymerization catalyst containing the organometallic complex of the Example is used as a catalyst for copolymerization of ethylene and cyclic olefin, in particular, an olefin-cyclic olefin copolymer having a higher cyclic olefin content is obtained compared to the polymerization catalyst containing the organometallic complex of the Comparative Example.< / n> < / ar> < / y> < / x> < / m>
Claims
1. An organometallic complex (A) represented by the following formula (1): 【Chemistry 1】 (In formula (1), M represents a titanium atom, a zirconium atom, or a hafnium atom; X's each independently represent a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a diene-based divalent derivative group; Y is a carbon atom or a silicon atom; R 1 ~R 7 and R 51 ~R 54 each independently represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group; R 1 ~R 7 and R 51 ~R 54 Two or more of the groups may be bonded to each other to form a ring structure.
2. In the formula (1), R 1 ~R 7 The organometallic complex (A) according to claim 1, wherein two groups bonded to adjacent ring members among the above are bonded to each other to form a ring structure.
3. In the formula (1), R 3 ~R 6 The organometallic complex (A) according to claim 1, wherein two groups bonded to adjacent ring members among the above are bonded to each other to form a ring structure.
4. The organometallic complex (A) according to claim 1, wherein the formula (1) is represented by the following formula (2): 【Chemistry 2】 (In formula (2), M is a titanium atom, a zirconium atom, or a hafnium atom; X's each independently represent a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a diene-based divalent derivative group; Y is a carbon atom or a silicon atom; R 1 , R 2 , R 7 and R 51 ~R 54 each independently represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group; R 55 ~R 58 are each independently a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group; R 1 , R 2 , R 7 and R 55 ~R 58 Two or more groups selected from the following may be bonded to each other to form a ring structure. 51 ~R 54 Two or more of the groups may be bonded to each other to form a ring structure.
5. The organometallic complex (A) according to claim 1, wherein the formula (1) is represented by the following formula (3): 【Chemistry 3】 In formula (3), M is a titanium atom, a zirconium atom, or a hafnium atom; each X is independently a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a diene-based divalent derivative group; R 5 ~R 7 and R 51 ~R 54 each independently represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group; R 5 ~R 7 and R 51 ~R 54 Two or more of the groups may be bonded to each other to form a ring structure, Ar represents an aromatic ring, R Ar are each independently a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group, and n represents an integer from 0 to the maximum number of substituents on Ar minus 2.
6. In the formula (1) or (3), R 5 and R 6 and R 7 6. The organometallic complex (A) according to claim 1 or 5, wherein the ring structure formed by bonding together is a pyrrole ring or an indole ring.
7. In the formula (1) or (2), R 7 The organometallic complex (A) according to claim 1 or 4, wherein is an aryl group or a substituted aryl group.
8. 5. The organometallic complex (A) according to claim 1 or 4, wherein in the formula (1) or the formula (2), M is a titanium atom.
9. In the formula (1) or (2), R 51 ~R 54 The organometallic complex (A) according to claim 1 or 4, wherein is a hydrogen atom.
10. In the formula (1) or (2), R 51 ~R 54 is a hydrogen atom, M is a titanium atom, and R 7 The organometallic complex (A) according to claim 1 or 4, wherein is an aryl group or a substituted aryl group.
11. The organometallic complex (A) according to claim 1, wherein the formula (1) is represented by the following formula (4): 【Chemistry 4】 (In formula (4), M is a titanium atom; X's each independently represent a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a diene-based divalent derivative group; Y is a carbon atom or a silicon atom; R 1 and R 2 each independently represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group; R 55 ~R 58 and R 59 ~R 63 are each independently a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group; R 55 ~R 58 Two or more groups selected from the following may be bonded to each other to form a ring structure; R 59 ~R 63 Two or more groups selected from may be bonded to each other to form a ring structure.
12. An organometallic complex (A) according to any one of claims 1 to 5, at least one compound (B) selected from the group consisting of an organometallic compound (B-1), an organoaluminum oxy compound (B-2), and a compound (B-3) that reacts with the organometallic complex (A) to form an ion pair; A catalyst for polymerization comprising:
13. A method for producing an olefin polymer, comprising polymerizing an olefin in the presence of the polymerization catalyst according to claim 12.
14. A method for producing an olefin-cyclic olefin copolymer, comprising copolymerizing an olefin with a cyclic olefin compound in the presence of the polymerization catalyst according to claim 12.
Citation Information
Patent Citations
Constrained geometry addition polymerization catalysts, processes for their preparation, precursors therefor, methods of use, and novel polymers formed therewith
EP0416815A2
Transition metal compound, catalyst composition containing the same, and olefin polymerization using the same
JP2008527050A
Method for producing cyclic olefin copolymer
JP7175426B2
Transition metal complex, catalyst for olefin polymerization, and process for producing olefin polymer with the same
WO2003024983A1
Cited By
Image processing method, image processing apparatus, image pickup apparatus, and computer-readable program
EP4704025A1