Semiconductor substrate and manufacturing method of the same
By forming a graphene layer and stress layer on SiC substrates to facilitate peeling, the method addresses the high cost and defect issues in SiC semiconductor production, achieving low-cost, high-quality substrates with improved yield and reduced manufacturing complexity.
Patent Information
- Application Number
- JP2024018156
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-02-08
- Publication Date
- 2024-10-11
AI Technical Summary
The high cost and defects in bonding interfaces of SiC semiconductor substrates, along with the difficulty in processing SiC using conventional methods, hinder the production of low-cost, high-quality semiconductor devices.
A method involving the formation of a graphene layer on a SiC single crystal substrate, followed by a stress layer to facilitate peeling, and subsequent epitaxial growth layers, allowing for the separation and reuse of the SiC single crystal substrate, reducing manufacturing costs and defects.
This approach enables the production of low-cost, high-quality SiC-based semiconductor substrates with reduced defects and improved yield, utilizing remote epitaxial growth and avoiding expensive processes like ion implantation delamination.
Smart Images

Figure 2024144132000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a semiconductor substrate and a method for manufacturing the same. [Background technology]
[0002] Conventionally, SiC devices such as Schottky barrier diodes (SBDs), metal-oxide-semiconductor field effect transistors (MOSFETs), and insulated gate bipolar transistors (IGBTs) have been provided for power control applications. In order to reduce manufacturing costs and provide desired physical properties, SiC semiconductor substrates on which such SiC devices are formed have been fabricated by bonding a single-crystal SiC semiconductor substrate to a polycrystalline SiC semiconductor substrate. Patent Document 1 describes a technique for bonding a single-crystal SiC semiconductor substrate to a polycrystalline SiC semiconductor substrate without defects in order to grow an epitaxial layer on the single-crystal SiC semiconductor substrate bonded to the polycrystalline SiC semiconductor substrate.
[0003] Silicon carbide (SiC) is one of the semiconductor materials that has attracted the most attention recently, and SiC-based power devices such as Schottky barrier diodes (SBD), metal-oxide-semiconductor field effect transistors (MOSFET), and insulated gate bipolar transistors (IGBT) are being provided for power control applications. Power devices fabricated on SiC wafers can reduce internal losses by an order of magnitude compared to current silicon-based devices, and are therefore expected to have a variety of applications as energy-saving power devices that can make effective use of limited energy.
[0004] The single crystal SiC semiconductor wafers on which such devices are formed are sometimes fabricated by bonding a single crystal SiC semiconductor layer to a polycrystalline SiC semiconductor substrate in order to reduce manufacturing costs and provide the desired physical properties. In addition, since a large current flows through a power device, a large amount of Joule heat is generated due to the electrical resistance of the substrate, etc. As a countermeasure, it was necessary to reduce the electrical resistance and thermal resistance by thinning the wafer by one-third to less than 100 μm by back grinding. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] U.S. Patent No. 8,916,451 [Patent Document 2] International Publication No. 2022 / 158078 [Patent Document 3] International Publication No. 2022 / 158085 Summary of the Invention [Problem to be solved by the invention]
[0006] However, the polishing process required to ensure the surface roughness required for bonding a single crystal SiC semiconductor substrate to a polycrystalline SiC semiconductor substrate by room temperature bonding or diffusion bonding is expensive, and defects occurring at the bonding interface can reduce yields. In addition, because SiC has a hardness second only to diamond, it is difficult to process it efficiently using conventional mechanical processing methods such as grinding and polishing, and the backside thinning process requires high processing costs, which has been an obstacle to practical use.
[0007] The present disclosure has been proposed in view of the above-mentioned circumstances, and has an object to provide a low-cost, high-quality semiconductor substrate and a manufacturing method thereof. It also has an object to provide a low-cost, high-quality SiC-based semiconductor substrate and semiconductor device, and a manufacturing method thereof. [Means for solving the problem]
[0008] According to one aspect of the present disclosure, a method for manufacturing a semiconductor substrate includes the steps of forming a graphene layer on a Si-face of a SiC single crystal substrate, forming a SiC epitaxial growth layer on the graphene layer, forming a stress layer on the SiC epitaxial growth layer, attaching a temporary substrate onto the stress layer, peeling off the graphene layer and the SiC epitaxial growth layer, forming a SiC polycrystalline growth layer on a C-face of the SiC epitaxial growth layer from which the graphene layer has been peeled off, and removing the temporary substrate, wherein the stress layer generates stress between the graphene layer and the SiC epitaxial growth layer to facilitate peeling.
[0009] According to another aspect of the present disclosure, a semiconductor substrate includes a SiC single crystal substrate, a graphene layer disposed on a Si face of the SiC single crystal substrate, a SiC epitaxial growth layer disposed above the SiC single crystal substrate via the graphene layer, and a stress layer disposed on the Si face of the SiC epitaxial growth layer, wherein the stress layer generates stress between the graphene layer and the SiC epitaxial growth layer that facilitates peeling.
[0010] A manufacturing method for a semiconductor substrate according to another aspect of the present disclosure includes the steps of forming a SiC epitaxial growth layer on a Si face of a SiC single crystal substrate, attaching the Si face of the SiC epitaxial growth layer to a temporary substrate, removing the SiC epitaxial growth layer from the SiC single crystal substrate, forming a first SiC polycrystalline growth layer on the C face of the SiC epitaxial growth layer attached to the temporary substrate, forming a graphene layer on the first SiC polycrystalline growth layer, forming a second SiC polycrystalline growth layer on the graphene layer, and removing the temporary substrate.
[0011] A semiconductor substrate according to another embodiment of the present disclosure includes a SiC epitaxial growth layer, a first SiC polycrystalline layer disposed on a Si face of the SiC epitaxial growth layer, a graphene layer disposed on the first SiC polycrystalline growth layer, and a second SiC polycrystalline layer disposed on the graphene layer. Effect of the Invention
[0012] According to the present disclosure, it is possible to provide a low-cost, high-quality semiconductor substrate and a manufacturing method thereof, and also to provide a low-cost, high-quality SiC-based semiconductor substrate. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 shows a cross-sectional view of a SiC single crystal substrate. [Figure 2A] FIG. 2A shows a plan view illustrating the crystal planes of a SiC wafer. [Figure 2B] FIG. 2B shows a side view illustrating the crystal planes of a SiC wafer. [Figure 3A] FIG. 3A shows an overhead view of a unit cell of a 4H—SiC crystal. [Figure 3B] FIG. 3B shows a schematic diagram of the two-layer portion of a 4H—SiC crystal. [Figure 3C] FIG. 3C shows a schematic diagram of a four-layer portion of a 4H—SiC crystal. [Figure 4] FIG. 4 shows a configuration diagram of the unit cell of the 4H—SiC crystal shown in FIG. 3A, viewed from directly above the (0001) plane. [Diagram 5] FIG. 5 shows a cross-sectional view of a structure in which a graphene layer is formed on a SiC single crystal substrate. [Figure 6] FIG. 6 shows an overhead view of an example of a graphene layer having a multi-layer stacked configuration. [Figure 7] FIG. 7 shows a cross-sectional view of a structure in which a SiC epitaxial growth layer is formed on a graphene layer. [Figure 8] FIG. 8 shows a cross-sectional view of a structure in which a stress layer is formed on a SiC epitaxial growth layer. [Figure 9A] FIG. 9A is an explanatory diagram of the mechanism of stress generation, and shows an explanatory diagram of a delamination mode in a cross-sectional structure in which a stress layer is formed. [Figure 9B] FIG. 9B is an explanatory diagram of the mechanism of stress generation, and shows an explanatory diagram of another interlayer peeling mode in a cross-sectional structure in which a stress layer is formed. [Figure 9C]FIG. 9C is an explanatory diagram of the mechanism of stress generation, and shows an explanatory diagram of the peeling mode or the fracture mode in a cross-sectional structure in which a stress layer is formed. [Figure 10] FIG. 10 is an explanatory diagram of the mechanism by which stress is generated, showing the relationship between the distance from the surface of the peeled or crushed portion and the stress. [Figure 11] FIG. 11 shows a cross-sectional view of a structure in which a graphite substrate is bonded onto a stress layer via an adhesive layer. [Figure 12A] FIG. 12A shows a cross-sectional view of the SiC epitaxial growth layer side of the structure in FIG. 11, which is peeled off at the interface between the graphene layer and the SiC epitaxial growth layer. [Figure 12B] FIG. 12B shows a cross-sectional view of the graphene layer side of the structure shown in FIG. 11, in which the structure is peeled off at the interface between the graphene layer and the SiC epitaxial growth layer. [Figure 13] FIG. 13 shows a cross-sectional view of a structure in which the peelable structure of FIG. 12A is attached to both sides of a graphite substrate and the adhesive layers are carbonized by annealing. [Figure 14] FIG. 14 shows a cross-sectional view of a structure in which a SiC polycrystalline growth layer is formed by the CVD method. [Figure 15] FIG. 15 shows a cross-sectional view of a structure in which part of the outer periphery of the SiC polycrystalline growth layer has been ground off. [Figure 16] FIG. 16 shows a cross-sectional view of the structure after annealing to remove the graphite substrate and the carbonized adhesive layer. [Figure 17] FIG. 17 is a cross-sectional view of the structure of FIG. 14 in which the temporary substrate is cut along the plane indicated by the line AA and separated into upper and lower portions. [Figure 18] FIG. 18 shows a cross-sectional view of the structure after removing the peripheral SiC polycrystalline growth layer and stress layer. [Figure 19] FIG. 19 shows a cross-sectional view of a SiC composite substrate. [Figure 20] FIG. 20 shows an overhead view of a SiC composite substrate (wafer). [Figure 21] FIG. 21 shows a cross-sectional view of a structure having a highly doped layer at the interface between a SiC epitaxial growth layer and a SiC polycrystalline growth layer. [Figure 22]FIG. 22 shows a cross-sectional view of a Schottky barrier diode. [Figure 23] FIG. 23 shows a cross-sectional view of a trench-gate TMOSFET. [Figure 24] FIG. 24 shows a cross-sectional view of a planar gate MOSFET. [Diagram 25] FIG. 25 shows a cross-sectional view of a SiC single crystal substrate. [Figure 26A] FIG. 26A shows a plan view illustrating the crystal planes of a SiC wafer. [Figure 26B] FIG. 26B shows a side view illustrating the crystal planes of a SiC wafer. [Figure 27A] FIG. 27A shows an overhead view of a unit cell of a 4H—SiC crystal. [Figure 27B] FIG. 27B shows a schematic diagram of a two-layer portion of a 4H—SiC crystal. [Figure 27C] FIG. 27C shows a schematic diagram of a four-layer portion of a 4H—SiC crystal. [Figure 28] FIG. 28 shows a configuration diagram of the unit cell of the 4H—SiC crystal shown in FIG. 27A viewed from directly above the (0001) plane. [Figure 29] FIG. 29 shows a cross-sectional view of a structure in which a first graphene layer is formed on a SiC single crystal substrate. [Diagram 30] FIG. 30 shows an overhead view of an example of a graphene layer having a multi-layer stacked configuration. [Diagram 31] FIG. 31 shows a cross-sectional view of a structure in which a SiC epitaxial growth layer is formed on a first graphene layer. [Diagram 32] FIG. 32 shows a cross-sectional view of a structure in which a stress layer is formed on a SiC epitaxial growth layer. [Figure 33A] FIG. 33A is an explanatory diagram of the mechanism of stress generation, and shows an explanatory diagram of a layer peeling mode in a cross-sectional structure in which a stress layer is formed. [Figure 33B] FIG. 33B is an explanatory diagram of the mechanism of stress generation, and shows an explanatory diagram of another interlayer peeling mode in a cross-sectional structure in which a stress layer is formed. [Figure 33C]FIG. 33C is an explanatory diagram of the mechanism of stress generation, and shows an explanatory diagram of the peeling mode or the crushing mode in a cross-sectional structure in which a stress layer is formed. [Diagram 34] FIG. 34 shows a cross-sectional view of a structure in which a graphite substrate is bonded onto a stress layer via an adhesive layer. [Figure 35A] FIG. 35A shows a cross-sectional view of the SiC epitaxial growth layer side of a structure in which a graphite substrate is bonded onto a stress layer via an adhesive layer, and the SiC epitaxial growth layer and the first graphene layer are peeled off at the interface between them. [Figure 35B] FIG. 35B shows a cross-sectional view of the first graphene layer side of a structure in which a graphite substrate is bonded onto a stress layer via an adhesive layer, and the SiC epitaxial growth layer and the first graphene layer are peeled off at the interface between them. [Diagram 36] FIG. 36 shows a cross-sectional view of a structure in which the peelable structure of FIG. 11A is attached to both sides of a graphite substrate and the adhesive layers are carbonized by annealing treatment. [Figure 37] FIG. 37 shows a cross-sectional view of a structure in which a first SiC polycrystalline growth layer is formed by the CVD method. [Figure 38] FIG. 38 shows a cross-sectional view of the structure after the second graphene layer is formed. [Figure 39] FIG. 39 shows a cross-sectional view of a structure in which a second SiC polycrystalline growth layer is formed by the CVD method. [Diagram 40] FIG. 40 shows a cross-sectional view of a structure in which part of the periphery of the second SiC polycrystalline growth layer, the second graphene layer, and the first SiC polycrystalline growth layer is ground away. [Diagram 41] FIG. 41 shows a cross-sectional view of the structure after removal of the graphite substrate and carbonized adhesive layer by combustion. [Diagram 42] FIG. 42 shows a cross-sectional view of the structure of FIG. 39 in which the temporary substrate is cut along the plane indicated by the line AA and separated into upper and lower portions. [Diagram 43] FIG. 43 shows a cross-sectional view of a SiC composite substrate structure obtained by removing the peripheral second SiC polycrystalline growth layer, the second graphene layer, the first SiC polycrystalline growth layer, and the stress layer. [Diagram 44] FIG. 44 shows a cross-sectional view of a structure in which a stress layer is bonded to the bottom of a countersunk hole in a graphite substrate via an adhesive layer. [Diagram 45] FIG. 45 shows a cross-sectional view of the structure after peeling off the SiC single crystal substrate and the first graphene layer. [Figure 46] FIG. 46 shows a cross-sectional view of a structure in which a first SiC polycrystalline growth layer is formed by the CVD method. [Figure 47] FIG. 47 shows a cross-sectional view of the structure after the second graphene layer is formed. [Figure 48] FIG. 48 shows a cross-sectional view of a structure in which a second SiC polycrystalline growth layer is formed by the CVD method. [Figure 49] FIG. 49 shows a cross-sectional view of a structure in which the outer peripheral second SiC polycrystalline growth layer, the second graphene layer, and the first SiC polycrystalline growth layer are ground. [Figure 50] FIG. 50 shows a cross-sectional view of a SiC composite substrate. [Figure 51] FIG. 51 shows an overhead view of a SiC composite substrate (wafer). [Figure 52] FIG. 52 shows a cross-sectional view of a structure having a highly doped layer at the interface between the SiC epitaxial growth layer and the first SiC polycrystalline growth layer. [Figure 53] FIG. 53 shows a cross-sectional view of a semiconductor device that constitutes a part of a Schottky barrier diode. [Figure 54] FIG. 54 shows a cross-sectional view of a semiconductor device constituting a part of a trench-gate MOSFET. [Figure 55] FIG. 55 shows a cross-sectional view of a semiconductor device constituting a part of a planar gate type MOSFET. [Figure 56] FIG. 56 is a cross-sectional view showing a state in which the second graphene layer and the second SiC polycrystalline growth layer are peeled off. [Figure 57] FIG. 57 is a cross-sectional view showing a method for forming crack starting points between the second graphene layer and the second SiC polycrystalline growth layer. [Figure 58] FIG. 58 is a cross-sectional view showing another method for forming crack starting points between the second graphene layer and the second SiC polycrystalline growth layer. [Figure 59] FIG. 59 is a cross-sectional view showing a method of propagating a crack between the second graphene layer and the second SiC polycrystalline growth layer. [Figure 60] FIG. 60 is a cross-sectional view showing another method for propagating a crack between the second graphene layer and the second SiC polycrystalline growth layer. [Figure 61] FIG. 61 shows a cross-sectional view of a Schottky barrier diode. [Figure 62] FIG. 62 shows a cross-sectional view of a trench-gate MOSFET. [Figure 63] FIG. 63 shows a cross-sectional view of a planar gate type MOSFET. [Figure 64] FIG. 64 shows a cross-sectional view of a structure in which a hydrogen ion implanted layer is formed on the Si surface of a SiC single crystal substrate. [Figure 65] FIG. 65 shows a cross-sectional view of a structure in which a thin single-crystal SiC layer is formed by weakening the hydrogen ion implanted layer through annealing, and then a SiC epitaxial growth layer is formed on the Si surface of the thin single-crystal SiC layer. [Figure 66] Figure 66 shows a cross-sectional view of a structure in which a graphite substrate is attached to the Si surface of a SiC epitaxial growth layer via an adhesive layer. [Figure 67] FIG. 67 shows a cross-sectional view of a structure that has been peeled off and separated from a SiC single crystal substrate via a thin single crystal SiC layer formed by embrittlement annealing. [Figure 68] Figure 68 shows a cross-sectional view of the structure in which the peeled surface of the thinned single crystal SiC layer has been smoothed. [Figure 69] FIG. 69 shows a cross-sectional view of a structure in which a first SiC polycrystalline growth layer is formed by the CVD method. [Figure 70] FIG. 70 shows a cross-sectional view of the structure after the second graphene layer is formed. [Figure 71] FIG. 71 shows a cross-sectional view of a structure in which a second SiC polycrystalline growth layer is formed by the CVD method. [Figure 72] FIG. 72 shows a cross-sectional view of a structure in which the outer peripheral second SiC polycrystalline growth layer, the second graphene layer, and the first SiC polycrystalline growth layer are ground. [Figure 73] FIG. 73 shows a cross-sectional view of the SiC composite substrate obtained after removing the adhesive layer and the graphite substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Next, an embodiment will be described with reference to the drawings. In the description of the drawings described below, the same or similar parts are given the same or similar reference numerals. The drawings are schematic. Furthermore, the embodiment shown below is an example of an apparatus or method for embodying a technical idea, and does not specify the material, shape, structure, arrangement, etc. of parts. Various modifications can be made to the embodiment.
[0015] (First embodiment) First, a first embodiment will be described. In the first embodiment, a stress layer is laminated on a SiC epitaxial growth layer formed on a SiC single crystal substrate via a graphene layer, and the stress layer generates a stress between the graphene layer and the SiC epitaxial growth layer that facilitates peeling.
[0016] (Method of manufacturing semiconductor substrate) A method for manufacturing a semiconductor substrate according to a first embodiment will be described. Fig. 1 is a cross-sectional view of a SiC single crystal substrate (SiCSB) 11 serving as a seed substrate. The SiC single crystal substrate 11 is, for example, a 4H-SiC substrate, and has a thickness of, for example, about 300 µm to 600 µm. In Fig. 1, [C] indicates the C-face of SiC, and [S] indicates the Si-face of SiC. The same applies to the following figures.
[0017] Fig. 2 is a diagram illustrating the crystal planes of a SiC wafer 100 applicable as a SiC single crystal substrate 11. The plan view of Fig. 2A shows a Si surface 103 of a SiC wafer 100 on which a primary orientation flat 101 and a secondary orientation flat 102 are formed. In the side view of Fig. 2B seen from the [-1100] orientation, a Si surface 103 with a
[0001] orientation is formed on the upper surface, and a C surface 104 with a [000-1] orientation is formed on the lower surface.
[0018] A schematic overhead configuration of a unit cell of a 4H-SiC crystal applicable to the first embodiment is shown in Fig. 3A, a schematic configuration of a two-layer portion of the 4H-SiC crystal is shown in Fig. 3B, and a schematic configuration of a four-layer portion of the 4H-SiC crystal is shown in Fig. 3C. Moreover, a schematic configuration of the unit cell of the 4H-SiC crystal structure shown in Fig. 3A viewed from directly above the (0001) plane is shown in Fig. 4.
[0019] As shown in FIG. 3A to FIG. 3C, the crystal structure of 4H-SiC can be approximated by a hexagonal system, in which one Si atom is bonded to four C atoms. The four C atoms are located at the four vertices of a regular tetrahedron with a Si atom at the center. Of these four C atoms, one Si atom is located in the
[0001] axial direction relative to the C atom, and the other three C atoms are located on the [000-1] axial side relative to the Si atom. In FIG. 3A, the off-angle θ is, for example, about 4 degrees or less.
[0020] The
[0001] and [000-1] axes are aligned along the axial direction of the hexagonal prism, and the surface (top surface of the hexagonal prism) normalized to the
[0001] axis is the (0001) surface (Si surface). Meanwhile, the surface (bottom surface of the hexagonal prism) normalized to the [000-1] axis is the (000-1) surface (C surface). In addition, the directions perpendicular to the
[0001] axis and passing through non-adjacent vertices of the hexagonal prism when viewed from directly above the (0001) surface are the a1 axis [2-1-10], a2 axis [-12-10], and a3 axis [-1-120], respectively.
[0021] As shown in FIG. 4, the direction passing through the vertex between the a1 axis and the a2 axis is the [11-20] axis, the direction passing through the vertex between the a2 axis and the a3 axis is the [-2110] axis, and the direction passing through the vertex between the a3 axis and the a1 axis is the [1-210] axis. Between each of the six axes passing through each vertex of the hexagonal prism, the axes inclined at an angle of 30° to the axes on both sides and normal to each side of the hexagonal prism are, in order clockwise from between the a1 axis and the [11-20] axis, the [10-10] axis, the [1-100] axis, the [0-110] axis, the [-1010] axis, the [-1100] axis, and the [01-10] axis. Each face (side face of the hexagonal prism) having these axes as normals is a crystal face perpendicular to the (0001) and (000-1) faces.
[0022] 5, a graphene layer (GR) 12 of up to several molecular layers is formed on the (0001) Si surface of the SiC single crystal substrate 11. The graphene layer 12 can be formed by pyrolysis on the Si surface of the SiC single crystal substrate 11 by, for example, annealing the SiC single crystal substrate 11 at about 1700° C. in an argon gas atmosphere at atmospheric pressure. The graphene layer 12 may also be formed by stacking on the SiC single crystal substrate 11 by CVD.
[0023] The graphene layer 12 applicable to the first embodiment is shown in FIG. 6. The graphene layer 12 has a laminated structure of graphite sheets 121·122·123·...12n. The graphite sheets 121·122·123·...12n on each surface of the n-layer structure have a large number of hexagonal carbon (C) covalent bonds in one laminated crystal structure, and the graphite sheets 121·122·123·...12n on each surface are bonded by van der Waals forces. In the first embodiment, the graphene layer 12 may have a 0 layer or a single layer structure as a buffer layer.
[0024] As shown in Fig. 7, a SiC epitaxial growth layer (SiC-epi) 13 is formed on a graphene layer 12. The SiC epitaxial growth layer 13 is formed by remote epitaxial growth on the graphene layer 12 formed on the Si surface of a SiC single crystal substrate 11. The SiC epitaxial growth layer 13 is a single crystal SiC thin film. The surface of the SiC epitaxial growth layer 13 in contact with the graphene layer 12 is the C-plane, and the surface of the SiC epitaxial growth layer 13 is the Si-plane.
[0025] 8, a stress layer 14 is formed on the SiC epitaxial growth layer 13. The stress layer 14 generates stress between the graphene layer 12 and the SiC epitaxial growth layer 13, making it easier to peel the graphene layer 12 from the SiC epitaxial growth layer 13.
[0026] The stress layer 14 in the first embodiment is made of a carbon film or a silicon nitride film. The carbon film is made of a polycrystalline diamond film or a diamond-like carbon film. The carbon film is obtained by a microwave chemical vapor deposition (CVD) device or the like in the case of a polycrystalline diamond film, and by an RF plasma chemical vapor deposition (CVD) device or the like in the case of a diamond-like carbon film. In addition, when forming either film, a negative potential is applied to the film formation substrate side in the initial stage of film formation, and the film is formed while being bombarded with ions, thereby obtaining the necessary film adhesion.
[0027] Table 1 below shows typical physical properties of the carbon film or silicon nitride film of the stress layer 14, the SiC single crystal substrate 11, and other layers. The material of the stress layer 14 used in the first embodiment needs to have heat resistance of 1500° C. or more because it will be subjected to a process of forming the SiC polycrystalline growth layer 16 in a later process.
[0028] [Table 1]
[0029] The mechanism by which the stress layer 14 generates stress will be described with reference to Figures 9A to 9C. In the example shown in Figures 9A to 9C, the internal stress T0 of the stress layer is a tensile stress, and the magnitude of the internal stress T0 gradually increases from Figure 9A to Figure 9B to Figure 9C. In the first embodiment, the internal stress T0 generated by the stress layer 14 includes three types of components: a true stress generated by the characteristics of each material during film formation, a thermal stress generated by the difference in thermal expansion coefficient between the SiC single crystal substrate 11 and the stress layer 14, and a stress due to a change in film quality of the stress layer 14, such as a change in film density due to hydrogen desorption in the film during heat treatment after film formation. Whether the internal stress T0 of the stress layer 14 is a compressive stress or a tensile stress and how large it is is based on these three types of components.
[0030] The true stress depends on the film thickness and temperature during film formation. In addition, the film density changes due to the release of hydrogen in the film caused by heat treatment after the stress layer 14 is formed, and the compressive stress is relaxed and the tensile stress is increased. The stress generated by the stress layer also depends on the layered structure of the SiC single crystal substrate 11, the graphene layer 12, the SiC epitaxial growth layer 13, the stress layer 14, and further the adhesive layer 15 and the graphite substrate 19 described later.
[0031] FIG. 10 is an explanatory diagram of the mechanism by which the stress layer 14 generates stress, showing the relationship between the distance from the surface of the part that may be peeled off or crushed and the stress. In FIG. 10, the horizontal axis indicates the magnitude of stresses T1, T2, and T3 at the positions where the SiC epitaxial growth layer 13, the graphene layer 12, or the SiC single crystal substrate 11 may be peeled off or crushed in FIG. 9A, FIG. 9B, and FIG. 9C, respectively, and the vertical axis indicates the distance from the surface of the peeled off or crushed part, respectively. These stresses T1, T2, and T3 are tensile stresses caused by the internal stress T0 of the stress layer 14, and increase according to the internal stress T0 that increases as we proceed from FIG. 9A to FIG. 9B to FIG. 9C. In addition, the manner of peeling or fracture is gradually becoming more severe, from an interlayer peeling mode at the interface between the stress layer 14 and the SiC epitaxial growth layer 13, to another interlayer peeling mode at the interface between the SiC epitaxial growth layer 13 and the graphene layer 12, to a peeling or fracture mode within the SiC single crystal substrate 11.
[0032] In the first embodiment, the stress generated by the internal stress T0 of the stress layer 14 is adjusted to be close to the adhesion energy between the graphene layer 12 and the SiC epitaxial growth layer 13. As shown in FIG. 9B, a stress T2 is generated at the interface between the graphene layer 12 and the SiC epitaxial growth layer 13 such that the graphene layer 12 and the SiC epitaxial growth layer 13 peel off. For this reason, the stress layer 14 is made of a specific material such as a carbon film or a silicon nitride film made of a polycrystalline diamond film or a diamond carbon film, and the film formation conditions such as the film thickness and the film formation temperature are adjusted to form the stress layer 14, thereby appropriately setting the internal stress T0 in the stress layer 14. In this way, in the first embodiment, the stress generated by the stress layer 14 is set to be close to the adhesion energy between the graphene layer 12 and the SiC epitaxial growth layer 13, thereby facilitating the peeling of the graphene layer 12 and the SiC epitaxial growth layer 13.
[0033] Next, as shown in FIG. 11, an adhesive layer 15 is formed on the stress layer 14, and the applied surface of the adhesive layer 15 is attached to one or both sides of a graphite substrate 19, which is a temporary substrate having an outer size slightly larger than that of the SiC single crystal substrate 11, to form a first composite (11 (SiCSB), 12 (GR), 13 (SiC-epi), 14, 15, 19). For example, a carbon adhesive may be used for the adhesive layer 15. The carbon adhesive is an adhesive that contains phenol resin and can maintain its bonding strength even at high temperatures by carbonizing the adhesive itself. As a temporary substrate having an outer size slightly larger than that of the SiC single crystal substrate 11, for example, if the SiC single crystal substrate 11 has a diameter of about 10 cm, a graphite substrate 19 having an outer size of about 11 cm is used, which is about 10 mm larger than that of the SiC single crystal substrate 11. For example, if the SiC single crystal substrate 11 has a diameter of about 15 cm, a graphite substrate 19 having an outer size of about 16 cm is used. The temporary substrate (graphite substrate 19), which is slightly larger than the SiC single crystal substrate 11, has the advantage that when inserted into the wafer boat groove of the batch-type vertical CVD furnace and aligned, the marks of the wafer boat supports are outside the effective substrate area.
[0034] The first composite is then heated in a vacuum annealing furnace or the like to dry and harden the adhesive layer 15. The graphite substrate 19 may have a glassy carbon coating on its surface. The glassy carbon coating has strong adhesive strength with the carbon adhesive, so that the SiC epitaxial growth layer 13 can be easily peeled off from the graphene layer 12 and the SiC single crystal substrate 11, and the yield can be improved. Note that, although FIG. 11 shows an example in which the adhesive layer 15 is attached to one side of the graphite substrate 19 to form the first composite, the adhesive layer 15 may be attached to both sides of the graphite substrate 19 to form the first composite.
[0035] As shown in Fig. 12, after the first composite of Fig. 11 is cured, the SiC epitaxial growth layer 13 is physically peeled off and separated from the graphene layer 12 interface on one or both sides of the first composite using an adhesive peeling tape, a debonder device, or the like. Fig. 12A is a cross-sectional view of a structure peeled off from the first composite shown in Fig. 11 to the SiC epitaxial growth layer 13 side, and Fig. 12B is a cross-sectional view of a structure peeled off to the graphene layer 12 side. The peeled structure on the SiC epitaxial growth layer 13 side shown in Fig. 12A forms a second composite (13 (SiC-epi), 14, 15, 19). In the first embodiment, the graphene layer 12 is bonded by van der Waals forces, and the stress generated by the stress layer 14 is adjusted to a magnitude that approximates the adhesion energy between the graphene layer 12 and the SiC epitaxial growth layer 13. Therefore, by applying a force in the shear direction, peeling can be easily caused at the interface between the graphene layer 12 and the SiC epitaxial growth layer 13.
[0036] In the structure shown in FIG. 12B where the graphene layer 12 is peeled off, the graphene layer 12 on the SiC single crystal substrate 11 is removed by etching or polishing. In the etching process of the graphene layer 12, for example, a plasma asher using oxygen plasma can be applied. Since the Si surface of the SiC single crystal substrate 11 from which the graphene layer 12 has been etched by oxygen plasma is oxidized, wet etching using hydrogen fluoride (HF) is performed. In the polishing process of the graphene layer 12, the graphene layer 12 is removed by, for example, chemical mechanical polishing (CMP). Here, the Si surface of the SiC single crystal substrate 11 has an average surface roughness Ra of, for example, about 1 nm or less due to the above-mentioned wet etching process. As a result, the SiC single crystal substrate 11 becomes reusable.
[0037] 13 shows an example in which the release structure of FIG. 12A is attached to both sides of a graphite substrate 19, and SiC epitaxial growth layers 131, 132 are formed on both sides. In this case, the second composite (131 (SiC-epi), 141, 151, 19, 152, 142, 132 (SiC-epi)) is heated in a vacuum thermal annealing furnace to form carbonized adhesion layers 151, 152.
[0038] As shown in FIG. 14, a SiC polycrystalline growth layer 16 is formed on the (000-1) C plane of the SiC epitaxial growth layers 131 and 132 provided on one or both sides of the second composite body. The SiC polycrystalline growth layer 16 can be formed by, for example, CVD technology. The SiC polycrystalline growth layer 16 has a 3C (cubic) structure. The SiC polycrystalline growth layer 16 is formed on the C plane of the SiC epitaxial growth layers 131 and 132 to form a substrate layer of the device wafer structure. The C plane of the SiC epitaxial growth layers 131 and 132 becomes the back surface of the device wafer structure, so the flatness of the surface is not required very much. Therefore, the SiC polycrystalline growth layer 16 can be formed by a simple polishing process.
[0039] The SiC polycrystalline growth layer 16 is deposited to a thickness that provides the mechanical strength required for the substrate of the SiC-based semiconductor device, forming a third composite (16 (SiC-poly CVD), 131 (SiC-epi), 141, 151, 19, 152, 142, 132 (SiC-epi), 16 (SiC-poly CVD)). The thickness of the SiC polycrystalline growth layer 16 is preferably about 150 μm to 500 μm, and the thickness of the completed SiC composite substrate (SiC polycrystalline growth layer 16 + SiC epitaxial growth layers 131, 132) is adjusted to about 150 μm to 500 μm as required. By reducing the thickness of the SiC polycrystalline growth layer 16, the thermal conductivity is improved. In addition, the deposition temperature of the SiC polycrystalline growth layer 16 is preferably in the range of 1300 ° C to 1600 ° C.
[0040] As shown in FIG. 15, the SiC polycrystalline growth layer 16 protruding from the outer periphery of the third composite and unnecessary portions of the graphite substrate 19 of the temporary substrate are ground and removed using an outer periphery grinding device to expose the temporary substrate (graphite substrate 19).
[0041] As shown in Fig. 16, the third composite shown in Fig. 15, whose periphery has been ground, is placed in a thermal annealing furnace in an air or oxygen atmosphere to remove the graphite substrate 19 and the carbonized adhesive layers 151 and 152 inside the third composite by oxidative combustion. When the stress layers 141 and 142 are made of carbon films such as polycrystalline diamond films or diamond-like carbon films, the stress layers 141 and 142 are also removed by oxidative combustion, and the fourth composite (16 (SiC-poly CVD), 131 (siC-epi), 132 (SiC-epi), 16 (SiC-poly CVD)) is taken out. Fig. 16 shows the fourth composite from which the stress layers 141 and 142 made of carbon films have been removed.
[0042] When the stress layers 141 and 142 are made of silicon nitride, the stress layers 141 and 142 remain after removing the graphite substrate 19 and the carbonized adhesive layers 151 and 152. Therefore, they are taken out as a fourth composite (16 (SiC-poly CVD), 131 (siC-epi), 141, 142, 132 (siC-epi), 16 (SiC-poly CVD)).
[0043] As shown in Fig. 17, instead of removing the unnecessary SiC polycrystalline growth layer 16 and graphite substrate 19 protruding from the periphery of the third composite by an outer periphery grinding device, the temporary substrate (graphite substrate 19) may be cut into two on a plane parallel to the main surface shown by the line AA in Fig. 15 to separate the third composite into upper and lower parts, and the cut surface of the temporary substrate (graphite substrate 19) may be exposed. As a separation technique, for example, a wire saw or a diamond wire saw may be used. In this case, the graphite substrate 19 and the carbonized adhesive layers 151 and 152 inside the third composite may be removed by oxidative combustion, and the fourth composite as shown in Fig. 16 may be taken out.
[0044] As shown in Fig. 18, the SiC polycrystalline growth layer 16 on the periphery of the fourth composite is removed by grinding and polishing. If the stress layers 141, 142 made of silicon nitride shown in Fig. 16 remain in the fourth composite, they are removed by dry etching with a carbon fluoride gas plasma or wet etching with hot phosphoric acid. Furthermore, the SiC composite substrate 10 is processed to the required dimensions and surface condition.
[0045] Fig. 19 shows a cross-sectional view of the SiC composite substrate 10. This SiC composite substrate 10 is obtained as upper and lower blocks by processing the fourth composite as shown in Fig. 18. Fig. 20 shows an overhead view of the SiC composite substrate 10. The SiC composite substrate 10 includes a SiC epitaxial growth layer 13 and a SiC polycrystalline growth layer 16 disposed on the C-plane of the SiC epitaxial growth layer 13.
[0046] In the SiC composite substrate 10, the surface of the SiC epitaxial growth layer 13 is a Si face of 4H-SiC with a
[0001] orientation, and the C face is a face of 4H-SiC with a [000-1] orientation. The thickness of the SiC polycrystalline growth layer 16 is, for example, about 150 μm to about 500 μm, and the thickness of the SiC epitaxial growth layer 13 is, for example, about 4 μm to about 100 μm.
[0047] 21, in the SiC epitaxial growth layer 13, a highly doped layer 13a may be formed toward the C-face of the SiC epitaxial growth layer 13 in contact with the SiC polycrystalline growth layer 16. The highly doped layer 13a suppresses the spread of a depletion layer in the SiC epitaxial growth layer 13, and also makes it possible to easily form an ohmic contact with the SiC polycrystalline growth layer 16 formed on the C-face of the SiC epitaxial growth layer 13.
[0048] The highly doped layer 13a can be formed, for example, by using a high-dose ion implantation technique. For example, in the case of an n-type semiconductor, the highly doped layer 13a is formed by high-dose phosphorus (P) ion implantation. When formed by P ion implantation, there is an effect on the crystallinity of the P ion-implanted C-face of the SiC epitaxial growth layer 13, but the Si face that becomes the device face has already been formed, and the crystallinity of the Si face is preserved.
[0049] The highly doped layer 13a may be formed by forming a highly nitrogen (N) doped epitaxial growth layer in the early stage of forming the SiC epitaxial growth layer (SiC-epi) 13 shown in Fig. 7. Although the highly nitrogen (N) doped epitaxial growth layer has an effect on crystallinity due to mismatch of lattice constants, the process is simple since it is formed by autodoping in the early stage of epitaxial growth.
[0050] (Semiconductor Substrate) 8, the semiconductor substrate according to the first embodiment includes a SiC single crystal substrate (SiCSB) 11, a graphene layer (GR) 12 disposed on the Si surface of the SiC single crystal substrate 11, a SiC epitaxial growth layer (SiC-epi) 13 disposed above the SiC single crystal substrate 11 via the graphene layer 12, and a stress layer 14 disposed on the Si surface of the SiC epitaxial growth layer 13. The stress layer 14 generates stress between the graphene layer 12 and the SiC epitaxial growth layer 13, facilitating peeling of the graphene layer 12 and the SiC epitaxial growth layer 13.
[0051] The stress layer 14 is made of a carbon film or a silicon nitride film. The carbon film is made of a polycrystalline diamond film or a diamond-like carbon film. The stress layer 14 is adjusted so that the stress generated by the internal stress is close to the adhesion energy between the graphene layer 12 and the SiC epitaxial growth layer 13. The stress generated by the stress layer also depends on the laminated structure of the SiC single crystal substrate 11, the graphene layer 12, the SiC epitaxial growth layer 13, the stress layer 14, and further the adhesive layer 15 and the temporary substrate 19 described later. The stress layer 14 is made of a specific material such as a carbon film or a silicon nitride film made of a polycrystalline diamond film or a diamond carbon film, and is formed by adjusting the film formation conditions such as the film thickness and the film formation temperature, thereby appropriately setting the internal stress in the stress layer 14. This makes it easy to peel off the graphene layer 12 from the SiC epitaxial growth layer 13.
[0052] 11, the semiconductor substrate according to the first embodiment may further include a graphite substrate 19 as a temporary substrate disposed on the stress layer 14. The graphite substrate 19 has an outer size slightly larger than that of the SiC single crystal substrate 11. The graphite substrate 19 is connected to the stress layer 14 via an adhesive layer 15 made of a carbon adhesive. The carbon adhesive contains a phenol resin, and is an adhesive that can maintain its bonding strength even at high temperatures by carbonizing the adhesive itself.
[0053] The graphite substrate 19 may have a glassy carbon coating on the surface. The glassy carbon coating has strong adhesive strength with a carbon adhesive, and therefore can easily peel off the SiC epitaxial growth layer 13 from the graphene layer 12 and the SiC single crystal substrate 11. As shown in Fig. 13, the semiconductor substrate according to the first embodiment may have a configuration in which the semiconductor substrate shown in Fig. 12A is disposed on both sides of a graphite substrate 19GS.
[0054] The semiconductor substrate of the first embodiment may have a SiC polycrystalline growth layer 16 formed on the C-face of the SiC epitaxial growth layers 131 and 132 as shown in FIG. 14. The SiC epitaxial growth layers 131 and 132 are transferred to the SiC polycrystalline growth layer 16. As shown in FIG. 19, the SiC epitaxial growth layer 13 may have a high-concentration doped layer 13a formed toward the C-face of the SiC epitaxial growth layer 13 in contact with the SiC polycrystalline growth layer 16. As shown in FIG. 6, the graphene layer 12 may have a stacked structure, or may have a zero layer as a buffer layer or a single-layer structure.
[0055] (Semiconductor element) The SiC composite substrate 10 manufactured by the semiconductor substrate manufacturing method according to the first embodiment or the SiC composite substrate 10 manufactured from the semiconductor substrate according to the first embodiment can be used, for example, in the manufacture of various SiC-based semiconductor elements. In the following, as examples thereof, a SiC-SBD, a SiC trench gate (T: Trench) type TMOSFET, and a SiC planar gate type MOSFET will be described.
[0056] (SiC-SBD) As shown in FIG. 22, the SiC-SBD 21, which is a semiconductor device fabricated using a SiC composite substrate, includes a SiC composite substrate 10 consisting of a SiC polycrystalline growth layer (SiC-poly CVD) 16 and a SiC epitaxial growth layer (SiC-epi) 13. A highly doped layer 13a may be interposed between the SiC polycrystalline growth layer 16 and the SiC epitaxial growth layer 13. The highly doped layer 13a suppresses the spread of a depletion layer in the SiC epitaxial growth layer 13, and easily forms an ohmic contact with the SiC polycrystalline growth layer 16 formed on the C-face of the SiC epitaxial growth layer 13. The SiC epitaxial growth layer 13 serves as a drift layer, the highly doped layer 13a serves as a buffer layer, and the SiC polycrystalline growth layer 16 serves as a substrate layer.
[0057] The SiC polycrystalline growth layer 16 is +type (impurity density is, for example, about 1×10 18 cm -3 ~Approx. 1×10 21 cm -3 ) and the SiC epitaxial growth layer 13 is doped with n - type (impurity density is, for example, about 5×10 14 cm -3 ~Approx. 5×10 16 cm -3 The heavily doped layer 13a is doped to a higher concentration than the SiC epitaxial growth layer 13.
[0058] Furthermore, the SiC epitaxial growth layer 13 may have any one of the crystal structures of 4H-SiC, 6H-SiC, or 2H-SiC.
[0059] As the n-type doping impurity, for example, N (nitrogen), P (phosphorus), As (arsenic), etc. can be used.
[0060] As the p-type doping impurity, for example, B (boron), Al (aluminum) or the like can be used.
[0061] The back surface ((000-1) C surface) of the SiC polycrystalline growth layer 16 is provided with a cathode electrode 21 so as to cover the entire area.
[0062] In addition, a surface 13b (e.g., a (0001) Si surface) of the SiC epitaxial growth layer 13 has a contact hole 23 that exposes a portion of the SiC epitaxial growth layer 13 as an active region 22, and a field insulating film 25 is formed in a field region 24 surrounding the active region 22.
[0063] The field insulating film 25 is made of SiO2 (silicon oxide), but may be made of other insulators such as silicon nitride (SiN). An anode electrode 26 is formed on the field insulating film 25, and the anode electrode 26 is connected to an anode terminal A.
[0064] A p-type JTE (Junction Termination Extension) structure 27 is formed in the vicinity of the surface 13b (surface layer portion) of the SiC epitaxial growth layer 13 so as to be in contact with the anode electrode 26. The JTE structure 27 is formed along the contour of the contact hole 23 so as to straddle the inside and outside of the contact hole 23 of the field insulating film 25.
[0065] (SiC-TMOSFET) As a semiconductor device fabricated using the SiC composite substrate 10 according to the first embodiment, a trench-gate TMOSFET 30 includes a SiC composite substrate 10 including a SiC polycrystalline growth layer 16 and a SiC epitaxial growth layer 13, as shown in FIG. 23. A highly doped layer 13a may be interposed between the SiC polycrystalline growth layer 16 and the SiC epitaxial growth layer 13. The highly doped layer 13a suppresses the spread of a depletion layer in the SiC epitaxial growth layer 13, and easily forms an ohmic contact with the SiC polycrystalline growth layer 16 formed on the C-face of the SiC epitaxial growth layer 13. The SiC epitaxial growth layer 13 serves as a drift layer, the highly doped layer 13a serves as a buffer layer, and the SiC polycrystalline growth layer 16 serves as a substrate layer.
[0066] The SiC polycrystalline growth layer 16 is + type (impurity density is, for example, about 1×10 18 cm -3 ~Approx. 1×10 21 cm -3 ) and the SiC epitaxial growth layer 13 is doped with n - type (impurity density is, for example, about 5×10 14 cm -3 ~Approx. 5×10 16 cm -3 The heavily doped layer 13a is doped to a higher concentration than the SiC epitaxial growth layer 13.
[0067] Furthermore, the SiC epitaxial growth layer 13 may have any one of the crystal structures of 4H-SiC, 6H-SiC, or 2H-SiC.
[0068] As the n-type doping impurity, for example, N (nitrogen), P (phosphorus), As (arsenic), etc. can be used.
[0069] As the p-type doping impurity, for example, B (boron), Al (aluminum) or the like can be used.
[0070] The back surface ((000-1) C surface) of the SiC polycrystalline growth layer 16 is provided with a drain electrode 31 so as to cover the entire area.
[0071] In the vicinity (surface layer portion) of the surface 13b ((0001) Si surface) of the SiC epitaxial growth layer 13, p-type (impurity density is, for example, about 1×10 16 cm -3 ~Approx. 1×10 19 cm -3 In the SiC epitaxial growth layer 13, the portion on the SiC polycrystalline growth layer 16 side with respect to the body region 32 is maintained in the state of the SiC epitaxial growth layer 13, i.e., n - The drain region 33(13) is of the type.
[0072] A gate trench 34 is formed in the SiC epitaxial growth layer 13. The gate trench 34 penetrates the body region 32 from the surface 13b of the SiC epitaxial growth layer 13, and its deepest portion reaches the drain region 33 (13).
[0073] A gate insulating film 35 is formed on the inner surface of the gate trench 34 and on the surface 13b of the SiC epitaxial growth layer 13 so as to cover the entire inner surface of the gate trench 34. The inside of the gate insulating film 35 is filled with, for example, polysilicon, so that a gate electrode 36 is embedded in the gate trench 34. A gate terminal G is connected to the gate electrode 36.
[0074] The surface layer of the body region 32 includes n-type GaN layers that form part of the side surface of the gate trench 34.+ A source region 37 is formed.
[0075] The SiC epitaxial growth layer 13 has p + type (impurity density is, for example, about 1×10 18 cm -3 ~Approx. 1×10 21 cm -3 ) a body contact region 38 is formed.
[0076] An interlayer insulating film 41 made of SiO2 is formed on the SiC epitaxial growth layer 13. A source electrode 43 is connected to the source region 37 and the body contact region 38 via a contact hole 42 formed in the interlayer insulating film 41. A source terminal S is connected to the source electrode 43.
[0077] By applying a predetermined voltage (a voltage equal to or higher than the gate threshold voltage) to the gate electrode 36 while a predetermined potential difference is generated between the source electrode 43 and the drain electrode 31 (between the source and drain), a channel can be formed in the body region 32 near the interface with the gate insulating film 35 by the electric field from the gate electrode 36. This allows a current to flow between the source electrode 43 and the drain electrode 31, turning the SiC-TMOSFET 31 on.
[0078] (SiC planar gate MOSFET) As shown in FIG. 24, a planar gate MOSFET 50, which is a semiconductor device fabricated using a SiC composite substrate 10, includes a SiC composite substrate 10 including a SiC polycrystalline growth layer 16 and a SiC epitaxial growth layer 13. A highly doped layer 13a may be interposed between the SiC polycrystalline growth layer 16 and the SiC epitaxial growth layer 13. The highly doped layer 13a suppresses the spread of a depletion layer in the SiC epitaxial growth layer 13, and easily forms an ohmic contact with the SiC polycrystalline growth layer 16 formed on the C-face of the SiC epitaxial growth layer 13. The SiC epitaxial growth layer 13 serves as a drift layer, the highly doped layer 13a serves as a buffer layer, and the SiC polycrystalline growth layer 16 serves as a substrate layer.
[0079] The SiC polycrystalline growth layer 16 is + type (impurity density is, for example, about 1×10 18 cm -3 ~Approx. 1×10 21 cm -3 ) and the SiC epitaxial growth layer 13 is doped with n - type (impurity density is, for example, about 5×10 14 cm -3 ~Approx. 5×10 16 cm -3 ) is doped.
[0080] Furthermore, the SiC epitaxial growth layer 13 may have any one of the crystal structures of 4H-SiC, 6H-SiC, or 2H-SiC.
[0081] As the n-type doping impurity, for example, N (nitrogen), P (phosphorus), As (arsenic), etc. can be used.
[0082] As the p-type doping impurity, for example, B (boron), Al (aluminum) or the like can be used.
[0083] A drain electrode 51 is formed on the back surface ((000-1) C surface) of the SiC composite substrate 10 so as to cover the entire area, and a drain terminal D is connected to the drain electrode 51.
[0084] In the vicinity (surface layer portion) of the surface 13b ((0001) Si surface) of the SiC epitaxial growth layer 13, p-type (impurity density is, for example, about 1×10 16 cm -3 ~Approx. 1×10 19 cm -3 The body region 52 of the SiC epitaxial growth layer 13 is formed in a well shape. The portion of the SiC epitaxial growth layer 13 on the SiC composite substrate 10 side with respect to the body region 52 is maintained in the state after the epitaxial growth, i.e., n - The drain region 53(13) is of the type.
[0085] The surface layer of the body region 52 is + A source region 54 of the type is formed in spaced relation to the periphery of the body region 52 .
[0086] Inside the source region 54, p + type (impurity density is, for example, about 1×10 18 cm -3 ~Approx. 1×10 21 cm -3 ) is formed in the body contact region 55. The body contact region 55 penetrates the source region 54 in the depth direction and is connected to the body region 52.
[0087] A gate insulating film 56 is formed on the surface 13b of the SiC epitaxial growth layer 13. The gate insulating film 56 covers a portion of the body region 52 surrounding the source region 54 (the peripheral portion of the body region 52) and the outer periphery of the source region 54.
[0088] A gate electrode 57 made of, for example, polysilicon is formed on the gate insulating film 56. The gate electrode 57 faces the peripheral edge of the body region 52 with the gate insulating film 56 interposed therebetween. A gate terminal G is connected to the gate electrode 57.
[0089] An interlayer insulating film 58 made of SiO2 is formed on the SiC epitaxial growth layer 13. A source electrode 62 is connected to the source region 54 and the body contact region 55 via a contact hole 61 formed in the interlayer insulating film 58. A source terminal S is connected to the source electrode 62.
[0090] By applying a predetermined voltage (a voltage equal to or higher than the gate threshold voltage) to the gate electrode 57 while a predetermined potential difference is generated between the source electrode 62 and the drain electrode 51 (between the source and drain), a channel can be formed in the body region 52 near the interface with the gate insulating film 56 by the electric field from the gate electrode 57. This allows a current to flow between the source electrode 62 and the drain electrode 51, turning the planar gate MOSFET 50 on.
[0091] As described above, according to the first embodiment, before forming SiC polycrystalline growth layer 16 by CVD, SiC single crystal substrate 11 is separated and replaced with a temporary substrate made of highly heat-resistant graphite substrate 19, thereby preventing unnecessary adhesion of polycrystalline SiC to SiC single crystal substrate 11 and maximizing the reusability of SiC single crystal substrate 11, thereby enabling further cost reduction.
[0092] According to the first embodiment, the stress layer 14 is formed of a carbon-based film (polycrystalline diamond film or diamond-like carbon film) or a silicon nitride film, and the internal stress and thermal stress of the film are utilized to make it easy to peel off the SiC epitaxial growth layer 13 from the graphene layer 12. This also makes it possible to avoid metal contamination, which is a problem when using a metal stressor film. The carbon-based film or silicon nitride film has the advantages of good adhesion to the base, excellent heat resistance, and the ability to obtain large stress.
[0093] According to the first embodiment, by making the graphite substrate 19 one size larger than the SiC single crystal substrate 11, it becomes possible to perform single-sided or double-sided epitaxial growth using an epitaxial growth apparatus such as a batch-type vertical tubular furnace, and high throughput and low-cost production can be realized without unduly increasing the growth rate. In addition, the graphite substrate 19 and the carbonized adhesive layer 15 can be removed at low cost simply by firing them in an oxidation furnace or the like.
[0094] According to the first embodiment, remote epitaxial growth of SiC is performed via graphene formed on a SiC single crystal substrate, and a SiC polycrystalline growth layer is formed directly thereon by CVD, eliminating the need for substrate bonding and eliminating defects caused by substrate bonding. In addition, since the epitaxial growth layer is formed via graphene, it is easy to separate the SiC single crystal substrate and the epitaxial growth layer, simplifying the process, and eliminating the need for expensive processes such as ion implantation delamination.
[0095] According to the first embodiment, after the SiC single crystal substrate is removed, the highly heat-resistant handle substrate is placed in a high-temperature LP-CVD apparatus, and a SiC polycrystalline growth layer is grown directly on the epitaxial growth layer. This eliminates the steps of transporting the epitaxial growth layer having a thickness of several μm from the handle substrate to the support substrate and bonding it to the support substrate, thereby making it possible to avoid defects such as wrinkles, crystal transitions, and voids caused by thin film transportation and bonding.
[0096] According to the first embodiment, the graphene layer formed on the SiC single crystal substrate 11 is not transferred, but epitaxial growth is performed directly on the graphene layer. This makes it possible to avoid defects such as wrinkles and cracks caused by the transfer of graphene.
[0097] According to the first embodiment, since the SiC single crystal substrate 11 is used as a base, hexagonal SiC with little deterioration in crystallinity can be obtained. In addition, the SiC single crystal substrate 11 is expensive and difficult to remove by polishing or etching, but by using remote epitaxial growth via the graphene layer 12, the obtained SiC epitaxial growth layer 13, which is a high-performance single crystal, can be easily separated, making removal by polishing or etching unnecessary. Since the expensive SiC single crystal substrate 11 can be reused after separation, a large cost advantage is obtained.
[0098] Although the first embodiment has been described above, other embodiments may be used. For example, although not shown, a MOS capacitor may be manufactured using the SiC composite substrate 10. In the MOS capacitor, the yield and reliability can be improved.
[0099] Although not shown, a bipolar transistor can also be manufactured using the SiC composite substrate 10. The SiC composite substrate 10 according to the first embodiment can also be used to manufacture SiC-pn diodes, SiCIGBTs, SiC complementary MOSFETs, etc. The SiC composite substrate 1 can also be applied to other types of devices, such as LEDs (light emitting diodes) and semiconductor optical amplifiers (SOAs).
[0100] The SiC epitaxial growth layer 13 may include at least one type or a plurality of types selected from the group consisting of Group IV element semiconductors, Group III-V compound semiconductors, and Group II-VI compound semiconductors.
[0101] Furthermore, the SiC composite substrate 10 and the SiC epitaxial growth layer 13 may be made of any one of 4H-SiC, 6H-SiC, and 2H-SiC materials.
[0102] Furthermore, the SiC single crystal substrate 11 and the SiC epitaxial growth layer 13 may comprise, as a material other than SiC, at least one selected from the group consisting of GaN, BN, AlN, Al2O3, Ga2O3, diamond, carbon, and graphite.
[0103] A semiconductor device including the SiC composite substrate 10 may include any of GaN-, AlN-, and gallium oxide-based IGBTs, diodes, MOSFETs, and thyristors other than SiC-based.
[0104] A semiconductor device including a SiC composite substrate 10 may have any of the following configurations: a one-in-one module, a two-in-one module, a four-in-one module, a six-in-one module, a seven-in-one module, an eight-in-one module, a twelve-in-one module, or a fourteen-in-one module.
[0105] With the SiC composite substrate 10, for example, a low-cost SiC polycrystalline growth layer 16 can be used as the substrate material instead of the high-cost SiC single crystal substrate 11.
[0106] (Second embodiment) Next, a second embodiment will be described. The second embodiment uses a remote epitaxial method that forms an SiC epitaxial growth layer on the surface of a SiC single crystal substrate serving as a seed crystal via a graphene layer, thereby enabling the separation of the SiC epitaxial growth layer transferred via the graphene layer.
[0107] (Method of manufacturing semiconductor substrate) FIG. 25 is a cross-sectional view of a SiC single crystal substrate (SiCSB) 11 serving as a seed substrate. In the second embodiment, the SiC single crystal substrate 11 will be described taking a 4H-SiC substrate as an example, but it may be either a hexagonal (4H, 6H) or cubic (3C) substrate. The thickness of the SiC single crystal substrate 11 may be, for example, about 300 μm to 600 μm. In FIG. 25, [C] indicates the C-face of SiC, and [S] indicates the Si-face of SiC. The same applies to the following figures.
[0108] Figures 26A and 26B are diagrams for explaining the crystal planes of a SiC wafer 110 applicable as a SiC single crystal substrate 11. The plan view of Figure 26A shows a Si surface 113 of a SiC wafer 110 on which a primary orientation flat 111 and a secondary orientation flat 112 are formed. In the side view of Figure 26B seen from the [-1100] orientation, a Si surface 113 with a
[0001] orientation is formed on the upper surface, and a C surface 114 with a [000-1] orientation is formed on the lower surface.
[0109] A schematic overhead configuration of a unit cell of a 4H-SiC crystal is shown as in Fig. 27A, a schematic configuration of a two-layer portion of a 4H-SiC crystal is shown as in Fig. 27B, and a schematic configuration of a four-layer portion of a 4H-SiC crystal is shown as in Fig. 27C. Moreover, a schematic configuration of the unit cell of the 4H-SiC crystal structure shown in Fig. 27A viewed from directly above the (0001) plane is shown as in Fig. 28.
[0110] As shown in Fig. 27A to Fig. 27C, the crystal structure of 4H-SiC can be approximated by a hexagonal system, in which one Si atom is bonded to four C atoms. The four C atoms are located at the four vertices of a regular tetrahedron with a Si atom at the center. Of these four C atoms, one Si atom is located in the
[0001] axial direction relative to the C atom, and the other three C atoms are located on the [000-1] axial side relative to the Si atom. In Fig. 27A, the off angle θ is, for example, about 4 degrees or less.
[0111] The
[0001] and [000-1] axes are aligned along the axial direction of the hexagonal prism, and the surface (top surface of the hexagonal prism) normalized to the
[0001] axis is the (0001) surface (Si surface). Meanwhile, the surface (bottom surface of the hexagonal prism) normalized to the [000-1] axis is the (000-1) surface (C surface). In addition, the directions perpendicular to the
[0001] axis and passing through non-adjacent vertices of the hexagonal prism when viewed from directly above the (0001) surface are the a1 axis [2-1-10], a2 axis [-12-10], and a3 axis [-1-120], respectively.
[0112] As shown in FIG. 28, the direction passing through the vertex between the a1 axis and the a2 axis is the [11-20] axis, the direction passing through the vertex between the a2 axis and the a3 axis is the [-2110] axis, and the direction passing through the vertex between the a3 axis and the a1 axis is the [1-210] axis. Between each of the six axes passing through each vertex of the hexagonal prism, the axes inclined at an angle of 30° to the axes on both sides and normal to each side of the hexagonal prism are, in order clockwise from between the a1 axis and the [11-20] axis, the [10-10] axis, the [1-100] axis, the [0-110] axis, the [-1010] axis, the [-1100] axis, and the [01-10] axis. Each face (side face of the hexagonal prism) having these axes as normals is a crystal face perpendicular to the (0001) and (000-1) faces.
[0113] 29, a first graphene layer (GR) 12 of up to several molecular layers is formed on the (0001) Si surface of the SiC single crystal substrate 11. The first graphene layer 12 can be formed by pyrolysis on the Si surface of the SiC single crystal substrate 11 by annealing the SiC single crystal substrate 11 at about 1700° C. in an argon gas atmosphere at atmospheric pressure. The first graphene layer 12 may also be formed by stacking on the SiC single crystal substrate 11 by CVD.
[0114] The first graphene layer 12 is shown in Fig. 30. The first graphene layer 12 has a laminated structure of graphite sheets 121·122·123·...12n. The graphite sheets 121·122·123·...12n on each side, which are made up of n layers, have a large number of hexagonal carbon (C) covalent bonds in one laminated crystal structure, and the graphite sheets 121·122·123·...12n on each side are bonded together by van der Waals forces. The first graphene layer 12 may be a 0 layer as a buffer layer, or a single layer structure.
[0115] As shown in Fig. 31, a SiC epitaxial growth layer (SiC-epi) 13 is formed on a first graphene layer 12. The SiC epitaxial growth layer 13 is formed by remote epitaxial growth on the first graphene layer 12 formed on the Si surface of a SiC single crystal substrate 11. The SiC epitaxial growth layer 13 is a single crystal SiC thin film. The surface of the SiC epitaxial growth layer 13 in contact with the first graphene layer 12 is the C-plane, and the surface of the SiC epitaxial growth layer 13 is the Si-plane.
[0116] As shown in FIG. 32, a stress layer 14 is formed on a SiC epitaxial growth layer 13. The stress layer 14 is made of a nickel (Ni) thin film. The nickel thin film may be formed by vapor deposition or plating. The stress layer 14 generates stress between the first graphene layer 12 and the SiC epitaxial growth layer 13 by internal stress within the layer, making it easier to peel the first graphene layer 12 and the SiC epitaxial growth layer 13 from each other.
[0117] The mechanism by which the stress layer 14 generates stress will be described with reference to Figures 33A to 33C. In the example shown in Figures 33A to 33C, the internal stress T0 of the stress layer is a tensile stress, and the magnitude of the internal stress T0 gradually increases from Figure 33A to Figure 33B to Figure 33C. As the internal stress T0 increases, peeling occurs at the interface between the stress layer 14 and the SiC epitaxial growth layer 13 in Figure 33A, peeling occurs at the interface between the SiC epitaxial growth layer 13 and the first graphene layer 12 in Figure 33B, and fracture occurs within the SiC single crystal substrate 11 in Figure 33C. By appropriately adjusting the internal stress T0 of the stress layer, peeling can be achieved at the interface between the SiC epitaxial growth layer 13 and the first graphene layer 12 as shown in Figure 33B.
[0118] Next, as shown in FIG. 34, an adhesive layer 15 is formed on the stress layer 14, and the applied surface of the adhesive layer 15 is attached to one or both sides of a graphite substrate 19, which is a temporary substrate having an outer size slightly larger than that of the SiC single crystal substrate 11, to form a first composite (11 (SiCSB), 12 (GR), 13 (SiC-epi), 14, 15, 19). For example, a carbon adhesive may be used for the adhesive layer 15. The carbon adhesive is an adhesive that contains phenol resin and can maintain its bonding strength even at high temperatures by carbonizing the adhesive itself. The graphite substrate 19 may be in the form of a disk or a rectangular plate. The graphite substrate 19 having an outer size slightly larger than that of the SiC single crystal substrate 11 may have an outer size of 1 mm or more larger than that of the SiC single crystal substrate 11. For example, if the SiC single crystal substrate 11 has a diameter of about 10 cm, a graphite substrate 19 having an outer size approximately 10 mm larger than that of the SiC single crystal substrate 11 may have a diameter of about 11 cm. For example, if the SiC single crystal substrate 11 has a diameter of about 15 cm, a graphite substrate 19 having an outer diameter of about 16 cm may be used.
[0119] Then, the first composite is heated in an inert gas atmosphere in a thermal annealing furnace or the like to carbonize the adhesive layer 15. At this time, by gradually heating with a temperature gradient that allows the gas generated when the carbon adhesive of the adhesive layer 15 decomposes to be gradually removed, the adhesive surface is prevented from peeling off when the adhesive layer 15 is carbonized. The graphite substrate 19 may have a glassy carbon coating on its surface. Since the glassy carbon coating has a strong adhesive force with the carbon adhesive of the adhesive layer 15, it is possible to easily peel off the SiC epitaxial growth layer 13 from the first graphene layer 12 and the SiC single crystal substrate 11, and the yield can be improved. Note that, in FIG. 34, an example in which the adhesive layer 15 is attached to one side of the graphite substrate 19 to form the first composite is shown, but the adhesive layer 15 may be attached to both sides of the graphite substrate 19 to form the first composite.
[0120] As shown in Fig. 35, after the first composite of Fig. 34 is carbonized, the SiC epitaxial growth layer 13 is physically peeled off and separated from the interface with the first graphene layer 12 on one or both sides of the first composite using an adhesive peeling tape, a debonder device, or the like. Fig. 35A is a cross-sectional view of a structure peeled off to the SiC epitaxial growth layer 13 side from the first composite shown in Fig. 34, and Fig. 35B is a cross-sectional view of a structure peeled off to the first graphene layer 12 side. The peeled structure on the SiC epitaxial growth layer 13 side shown in Fig. 35A forms a second composite (13 (SiC-epi), 14, 15, 19). The first graphene layer 12 is bonded by van der Waals forces, and the stress generated by the stress layer 14 is adjusted to a magnitude that facilitates peeling between the first graphene layer 12 and the SiC epitaxial growth layer 13. Therefore, by applying a force in the shear direction, peeling can be easily caused at the interface between the first graphene layer 12 and the SiC epitaxial growth layer 13.
[0121] In the structure shown in FIG. 35B where the first graphene layer 12 is peeled off, the first graphene layer 12 on the SiC single crystal substrate 11 is removed by etching or polishing. In the etching process of the first graphene layer 12, for example, a plasma asher using oxygen plasma can be applied. Since the Si surface of the SiC single crystal substrate 11 from which the first graphene layer 12 has been etched by oxygen plasma is oxidized, wet etching using hydrogen fluoride (HF) is performed. In addition, in the polishing process of the first graphene layer 12, the first graphene layer 12 is removed by, for example, chemical mechanical polishing (CMP). Here, the Si surface of the SiC single crystal substrate 11 has an average surface roughness Ra of, for example, about 1 nm or less due to the above-mentioned wet etching process. As a result, the SiC single crystal substrate 11 becomes reusable.
[0122] 36 shows an example in which the release structure of FIG. 35A is attached to both sides of a graphite substrate 19, and SiC epitaxial growth layers 131, 132 are formed on both sides. In this case, the second composite (131 (SiC-epi), 141, 151, 19, 152, 142, 132 (SiC-epi)) is heated in a thermal annealing furnace to carbonize the adhesive layers 151, 152.
[0123] As shown in FIG. 37, the first SiC polycrystalline growth layer 16 is formed on the (000-1) C plane of the SiC epitaxial growth layers 131, 132 provided on one or both sides of the second complex. The first SiC polycrystalline growth layer 16 can be formed by CVD technology. After the second complex is placed in a CVD furnace, the furnace is evacuated and heated to about 1400°C to 1500°C. Then, the material gases, for example, SiCl4 (silicon tetrachloride) gas, CH4 (methane) gas, and H2 (hydrogen) gas, are simultaneously flowed and the pressure is adjusted to deposit the first SiC polycrystalline growth layer 16. The first SiC polycrystalline growth layer 16 has a 3C (cubic) structure. The temporary substrate (graphite substrate 19) that is one size larger than the SiC single crystal substrate 11 has the advantage that the traces of the wafer boat support pillars are outside the substrate effective area when the substrate is inserted into the wafer boat groove of the batch-type vertical CVD furnace and aligned.
[0124] The thickness of the first SiC polycrystalline growth layer 16 is set to the thickness of the SiC composite substrate to be thinned. For example, when the thickness of the entire wafer after thinning is to be 100 μm, if the thickness of the SiC epitaxial growth layer 13 is 10 μm, the volume thickness of the first polycrystalline SiC bulk layer is set to 90 μm.
[0125] As shown in Fig. 38, a second graphene layer (GR) 17 of up to several molecular layers is formed on the (000-1) C plane of the SiC epitaxial growth layers 131, 132 of the second composite body on which the first SiC polycrystalline growth layer 16 has been formed. The second graphene layer 17 may be formed by stacking using CVD or may be formed by a thermal decomposition method. In the case of the thermal decomposition method, the second composite body on which the first SiC polycrystalline growth layer 16 has been deposited is placed in a thermal annealing furnace, and, for example, 1 x 10 -5 After performing a high vacuum of about Pascal to thoroughly remove atmospheric components, high-purity argon gas of about 6N was introduced and 5×10 -5 Pascal to 1×10 +5 The pressure is adjusted to between 1000 and 10000 Pascals, and then the mixture is heated to a range of 1250°C to 1750°C to form a second graphene layer 17 on the surface of the first SiC polycrystalline growth layer 16. The second graphene layer 17 has a stacked structure of graphite sheets, similar to the first graphene layer 12 shown in Fig. 30, and the graphite sheets on each surface are bonded together by van der Waals forces. The second graphene layer 17 may be a 0-layer as a buffer layer, or may have a single-layer structure.
[0126] As shown in FIG. 39, a second SiC polycrystalline growth layer 18 is further formed on the (000-1) C plane of the SiC epitaxial growth layers 131, 132 of the second composite in which the first SiC polycrystalline growth layer 16 and the second graphene layer 17 are laminated. The second SiC polycrystalline growth layer 18 can also be formed by the CVD technique, similar to the first SiC polycrystalline growth layer 16. In the case of using the CVD technique, the second composite in which the first SiC polycrystalline growth layer 16 and the second graphene layer 17 are laminated is placed in a CVD furnace, and then the furnace is sufficiently evacuated and heated to about 1400°C to 1500°C. Then, the second SiC polycrystalline growth layer 18 is deposited by simultaneously flowing, as material gas, for example, SiCl4 (silicon tetrachloride) gas, CH4 (methane) gas, and H2 (hydrogen) gas and adjusting the pressure. At this time, the thickness of the film to be deposited is set according to the thickness of the SiC composite substrate 10 in its final form. For example, when the overall thickness of the SiC composite substrate 10 is to be 350 μm, if the thickness of the SiC epitaxial growth layer 13 is 10 μm and the deposited thickness of the first SiC polycrystalline growth layer 16 is 90 μm, then the deposited thickness of the second SiC polycrystalline growth layer 18 should be set to 250 μm.
[0127] A first SiC polycrystalline growth layer 16, a second graphene layer 17 and a second SiC polycrystalline growth layer 18 are deposited on the second complex to form a third complex (18 (2nd SiC-poly CVD), 17, 16 (1st SiC-poly CVD), 131 (SiC-epi), 141, 151, 19, 152, 142, 132 (SiC-epi), 16 (1st SiC-poly CVD), 17, 18 (2nd SiC-poly CVD)).
[0128] As shown in Figure 40, unnecessary portions of the second SiC polycrystalline growth layer 18, the second graphene layer 17, the first SiC polycrystalline growth layer 16, and the graphite substrate 19 of the temporary substrate protruding from the outer periphery of the third composite are ground and removed using an outer periphery grinding device to expose the temporary substrate (graphite substrate 19).
[0129] As shown in Fig. 41, the third composite having its outer periphery ground as shown in Fig. 40 is heated to about 900°C to 1000°C in an atmospheric furnace capable of heating in an atmospheric atmosphere while flowing air, so that the graphite substrate 19 and the carbonized adhesive layers 151 and 152 inside the third composite are burned and completely removed. Then, the fourth composite (181 (2nd SiC-poly CVD), 171, 161 (1st SiC-poly CVD), 131 (siC-epi), 141, 142, 132 (SiC-epi), 162 (1st SiC-poly CVD), 172, 182 (2nd SiC-poly CVD)) is taken out.
[0130] Instead of removing the unnecessary second SiC polycrystalline growth layer 18, the second graphene layer 17, the first SiC polycrystalline growth layer 16, and the graphite substrate 19 protruding from the periphery of the third composite by the periphery grinding device, the temporary substrate (graphite substrate 19) may be cut into two on a plane parallel to the main surface of the graphite substrate 19 shown by the line AA in FIG. 39 to separate the third composite into upper and lower parts, and the cut surface of the temporary substrate (graphite substrate 19) may be exposed, as shown in FIG. 42. As a separation technique, for example, a wire saw or a diamond wire saw may be used. In this case, the graphite substrate 19 and the carbonized adhesive layers 151 and 152 inside the third composite may be removed by oxidative combustion, and the fourth composite as shown in FIG. 41 may be taken out.
[0131] As shown in Fig. 43, the second SiC polycrystalline growth layers 181, 182, the second graphene layers 171, 172, and the first SiC polycrystalline growth layers 161, 162 on the periphery of the fourth composite are removed by grinding and polishing with a beveling device, and the stress layers 141, 142 are removed by etching or polishing, thereby obtaining a SiC composite substrate 10 configured by stacking the second SiC polycrystalline growth layer 181, the second graphene layer 171, the first SiC polycrystalline growth layer 161, and the SiC epitaxial growth layer 131, and a SiC composite substrate 10 configured by stacking the SiC epitaxial growth layer 132, the first SiC polycrystalline growth layer 162, the second graphene layer 172, and the second SiC polycrystalline growth layer 182. Furthermore, these SiC composite substrates 10 are processed to the required dimensions and surface state. (Modification) Here, a modified example of the method for manufacturing a semiconductor substrate according to the second embodiment will be described. The manufacturing method of the modified example is the same as that of the second embodiment up to the step of forming a stack in which a stress layer 14 is stacked on a SiC epitaxial growth layer 13 as shown in FIG. 32, but is different from that of the second embodiment in the step of fitting and fixing the stack into a graphite substrate 19 having a countersunk hole formed on one side. The following describes the step of fitting the stack into the countersunk hole of the graphite substrate 19, which is different from that of the second embodiment. Note that the configuration of each layer formed in the modified example is the same as that of the second embodiment, and therefore the points common to the second embodiment may be omitted.
[0132] As shown in FIG. 44, the laminate in which the adhesive layer 15 is formed on the stress layer 14 is fitted into a countersunk hole in a graphite substrate 19, which is a temporary substrate having an outer size slightly larger than that of the SiC single crystal substrate 11, and the coated surface of the adhesive layer 15 is laminated and attached to the bottom surface of the countersunk hole to form a fifth composite (19, 15, 14, 13 (SiC-epi), 12 (GR), 11 (SiCSB)). In the fifth composite, the adhesive layer 15, the stress layer 14, and the SiC epitaxial growth layer 13 are in the countersunk hole of the graphite substrate 19, and the first graphene layer 12 and the SiC single crystal substrate 11 are outside the surface of the graphite substrate 19. A carbon adhesive is used for the adhesive layer 15 as in the second embodiment. Then, the fifth composite is heated in a thermal annealing furnace or the like to carbonize the adhesive layer 15. As in the second embodiment, the graphite substrate 19 may have a glassy carbon coating on its surface.
[0133] As shown in FIG. 45, after carbonizing the adhesive layer 15 of the fifth composite of FIG. 44, the SiC single crystal substrate 11 and the first graphene layer 12 are peeled off and removed using an adhesive peeling tape, a debonder device, or the like to form a sixth composite (19, 15, 14, 13 (SiC-epi)). The first graphene layer 12 is bonded by van der Waals forces, and the stress generated by the stress layer 14 is adjusted to a magnitude that facilitates peeling of the first graphene layer 12 and the SiC epitaxial growth layer 13. Therefore, peeling can be easily caused at the interface between the first graphene layer 12 and the SiC epitaxial growth layer 13 by applying a force in the shear direction. The structure consisting of the removed SiC single crystal substrate 11 and first graphene layer 12 is made into a reusable SiC single crystal substrate 11 by removing the first graphene layer 12 by etching or polishing.
[0134] As shown in Fig. 46, a first SiC polycrystalline growth layer 16 is formed on the (000-1) C plane of the SiC epitaxial growth layer 13 fitted into the countersunk hole of the sixth composite body. The first SiC polycrystalline growth layer 16 can be formed by, for example, a CVD technique. The first SiC polycrystalline growth layer 16 has a 3C (cubic) structure.
[0135] 47, a second graphene layer (GR) 17 of up to several molecular layers is formed on the (000-1) C plane of the SiC epitaxial growth layer 13 of the sixth composite body on which the first SiC polycrystalline growth layer 16 is formed. The second graphene layer 17 may be formed by stacking by CVD or by thermal decomposition.
[0136] 48, a second SiC polycrystalline growth layer 18 is further formed on the (000-1) C plane of the SiC epitaxial growth layer 13 of the sixth composite in which the first SiC polycrystalline growth layer 16 and the second graphene layer 17 are laminated. The second SiC polycrystalline growth layer 18 can also be formed by the CVD technique, similar to the first SiC polycrystalline growth layer 16. The second SiC polycrystalline growth layer 18 has a 3C (cubic) structure, similar to the first SiC polycrystalline growth layer 16.
[0137] As shown in FIG. 49, the second SiC polycrystalline growth layer 18, the second graphene layer 17, and the first SiC polycrystalline growth layer 16 on the periphery of the sixth composite are removed by grinding and polishing. Furthermore, the graphite substrate 19 and the adhesive layer 15 are burned and completely removed. When the stress layer 14 is removed by etching or polishing, a SiC composite substrate is obtained in which the SiC epitaxial growth layer 13, the first SiC polycrystalline growth layer 161, the first SiC polycrystalline growth layer 162, and the second graphene layer 171 are laminated. Note that the laminate of the first SiC polycrystalline growth layer 16, the second graphene layer 17, and the second SiC polycrystalline growth layer 18 separated by removing the graphite substrate 19 and the adhesive layer 15 has the same shape and size as the SiC composite substrate 10, and can be used as a dummy substrate.
[0138] (Semiconductor Substrate) A description will now be given of a SiC composite substrate 10 which is a semiconductor substrate according to the second embodiment. The SiC composite substrate 10 is fabricated by the method for fabricating a semiconductor substrate according to the second embodiment as described above.
[0139] As shown in FIG. 50, the SiC composite substrate 10 is configured by stacking a second SiC polycrystalline growth layer (2nd SiC-poly CVD) 18, a second graphene layer 17, a first SiC polycrystalline growth layer (1st SiC-poly CVD) 16, and a SiC epitaxial growth layer (SiC-epi) 13. FIG. 51 is a schematic bird's-eye view of the SiC composite substrate (wafer) 10. In the SiC composite substrate 10, the surface of the SiC epitaxial growth layer 13 may be a Si surface of 4H-SiC with a
[0001] orientation, and the surface in contact with the first SiC polycrystalline growth layer 16 may be a C surface of 4H-SiC with a [000-1] orientation. As shown in FIG. 30, the second graphene layer 17 has a single-layer structure or a multi-layer laminated structure of graphene, which facilitates peeling of the second graphene layer 17 and the second SiC polycrystalline growth layer 18.
[0140] 52, in the SiC epitaxial growth layer 13, a highly doped layer 13a may be formed toward the C-face of the SiC epitaxial growth layer 13 in contact with the first SiC polycrystalline growth layer 16. The highly doped layer 13a suppresses the spread of a depletion layer in the SiC epitaxial growth layer 13, and also makes it possible to easily form an ohmic contact with the first SiC polycrystalline growth layer 16 formed on the C-face of the SiC epitaxial growth layer 13.
[0141] The highly doped layer 13a can be formed, for example, by using a high-dose ion implantation technique. For example, in the case of an n-type semiconductor, the highly doped layer 13a is formed by high-dose phosphorus (P) ion implantation. When formed by P ion implantation, there is an effect on the crystallinity of the P ion-implanted C-face of the SiC epitaxial growth layer 13, but the Si face that becomes the device face has already been formed, and the crystallinity of the Si face is preserved.
[0142] The highly doped layer 13a may be formed by forming a highly nitrogen (N) doped epitaxial growth layer in the early stage of forming the SiC epitaxial growth layer (SiC-epi) 13 shown in Fig. 31. Although the highly nitrogen (N) doped epitaxial growth layer has an effect on crystallinity due to mismatch of lattice constants, the process is simple since it is formed by autodoping in the early stage of epitaxial growth.
[0143] (Semiconductor Device) The SiC composite substrate 10, which is a semiconductor substrate according to the second embodiment, can be provided as a semiconductor device in which a part of the structure of a semiconductor element, such as the main part of various SiC-based semiconductor elements, is formed on the Si surface of the SiC epitaxial growth layer 13, which is the device surface. Such a semiconductor device can be formed into a semiconductor element by forming an electrode or the like on the surface of the first SiC polycrystalline growth layer 16 after removing the second SiC polycrystalline growth layer 18 and the second graphene layer 17, as described below. In the following, as examples of such a semiconductor device, semiconductor devices in which the main parts of a SiC-SBD, a SiC trench gate (T: Trench) type TMOSFET, and a SiC planar gate type MOSFET are configured will be described.
[0144] (SiC-SBD) A semiconductor device 120 having a SiC-SBD structure in which the structure of the main part of the SiC-SBD is formed on a SiC composite substrate 10 includes a SiC composite substrate 10 including a second SiC polycrystalline growth layer (2nd SiC-poly CVD) 18, a second graphene layer (GR) 17, a first SiC polycrystalline growth layer (1st SiC-poly CVD) 16, and a SiC epitaxial growth layer (SiC-epi) 13, as shown in FIG. 53. A highly doped layer 13a may be interposed between the first SiC polycrystalline growth layer 16 and the SiC epitaxial growth layer 13. The highly doped layer 13a suppresses the spread of a depletion layer in the SiC epitaxial growth layer 13, and easily forms an ohmic contact with the first SiC polycrystalline growth layer 16 formed on the C-face of the SiC epitaxial growth layer 13. The SiC epitaxial growth layer 13 serves as a drift layer, the highly doped layer 13a serves as a buffer layer, and the first SiC polycrystalline growth layer 16 serves as a substrate layer.
[0145] The first SiC polycrystalline growth layer 16 is n + type (impurity density is, for example, about 1×10 18 cm -3 ~Approx. 1×10 21 cm -3 ) and the SiC epitaxial growth layer 13 is doped with n - type (impurity density is, for example, about 5×1014 cm -3 ~Approx. 5×10 16 cm -3 The heavily doped layer 13a is doped to a higher concentration than the SiC epitaxial growth layer 13.
[0146] Furthermore, the SiC epitaxial growth layer 13 may have any one of the crystal structures of 4H-SiC, 6H-SiC, or 2H-SiC.
[0147] As the n-type doping impurity, for example, N (nitrogen), P (phosphorus), As (arsenic), etc. can be used.
[0148] As the p-type doping impurity, for example, B (boron), Al (aluminum) or the like can be used.
[0149] In addition, a surface 100 (e.g., a (0001) Si surface) of the SiC epitaxial growth layer 13 has a contact hole 23 that exposes a portion of the SiC epitaxial growth layer 13 as an active region 22, and a field insulating film 25 is formed in a field region 24 surrounding the active region 22.
[0150] The field insulating film 25 is made of SiO2 (silicon oxide), but may be made of other insulators such as silicon nitride (SiN), etc. On this field insulating film 25, an anode electrode 26 is formed.
[0151] A p-type JTE (Junction Termination Extension) structure 27 is formed in the vicinity of the surface 13b (surface layer portion) of the SiC epitaxial growth layer 13 so as to be in contact with the anode electrode 26. The JTE structure 27 is formed along the contour of the contact hole 23 so as to straddle the inside and outside of the contact hole 23 of the field insulating film 25.
[0152] (SiC-TMOSFET) A semiconductor device 130 having a trench-gate type TMOSFET structure in which the main part of the trench-gate type TMOSFET is configured on a SiC composite substrate 10 includes a SiC composite substrate 10 including a second SiC polycrystalline growth layer (2nd SiC-poly CVD) 18, a second graphene layer (GR) 17, a first SiC polycrystalline growth layer (1st SiC-poly CVD) 16, and a SiC epitaxial growth layer (SiC-epi) 13, as shown in FIG. 54. A high-concentration doped layer 13a may be interposed between the first SiC polycrystalline growth layer 16 and the SiC epitaxial growth layer 13. Here, the high-concentration doped layer 13a suppresses the spread of the depletion layer in the SiC epitaxial growth layer 13, and easily forms an ohmic contact with the first SiC polycrystalline growth layer 16 formed on the C-face of the SiC epitaxial growth layer 13. The SiC epitaxial growth layer 13 serves as a drift layer, the highly doped layer 13a serves as a buffer layer, and the first SiC polycrystalline growth layer 16 serves as a substrate layer.
[0153] The first SiC polycrystalline growth layer 16 is n + type (impurity density is, for example, about 1×10 18 cm -3 ~Approx. 1×10 21 cm -3 ) and the SiC epitaxial growth layer 13 is doped with n - type (impurity density is, for example, about 5×10 14 cm -3 ~Approx. 5×10 16 cm -3 The heavily doped layer 13a is doped to a higher concentration than the SiC epitaxial growth layer 13.
[0154] Furthermore, the SiC epitaxial growth layer 13 may have any one of the crystal structures of 4H-SiC, 6H-SiC, or 2H-SiC.
[0155] As the n-type doping impurity, for example, N (nitrogen), P (phosphorus), As (arsenic), etc. can be used.
[0156] As the p-type doping impurity, for example, B (boron), Al (aluminum) or the like can be used.
[0157] In the vicinity (surface layer portion) of the surface 13b ((0001) Si surface) of the SiC epitaxial growth layer 13, p-type (impurity density is, for example, about 1×10 16 cm -3 ~Approx. 1×10 19 cm -3 In the SiC epitaxial growth layer 13, the portion on the first SiC polycrystalline growth layer 16 side with respect to the body region 32 is maintained in the state of the SiC epitaxial growth layer 13, i.e., n - The drain region 33(13) is of the type.
[0158] A gate trench 34 is formed in the SiC epitaxial growth layer 13. The gate trench 34 penetrates the body region 32 from the surface 13b of the SiC epitaxial growth layer 13, and its deepest portion reaches the drain region 33 (13).
[0159] A gate insulating film 35 is formed on the inner surface of the gate trench 34 and on the surface 13b of the SiC epitaxial growth layer 13 so as to cover the entire inner surface of the gate trench 45. Then, the inside of the gate insulating film 35 is filled with, for example, polysilicon, so that a gate electrode 36 is embedded in the gate trench 34.
[0160] The surface layer of the body region 32 includes n-type GaN layers that form part of the side surface of the gate trench 34. + A source region 37 is formed.
[0161] The SiC epitaxial growth layer 13 has p + type (impurity density is, for example, about 1×10 18 cm -3 ~Approx. 1×10 21 cm -3 ) a body contact region 38 is formed.
[0162] An interlayer insulating film 41 made of SiO2 is formed on the SiC epitaxial growth layer 13. A source electrode 43 is connected to the source region 37 and the body contact region 38 via a contact hole 42 formed in the interlayer insulating film 41.
[0163] (SiC planar gate MOSFET) A semiconductor device 150 having a planar gate MOSFET structure in which the structure of the main part of the planar gate MOSFET is formed on a SiC composite substrate 10 includes a SiC composite substrate 10 including a second SiC polycrystalline growth layer (2nd SiC-poly CVD) 18, a second graphene layer (GR) 17, a first SiC polycrystalline growth layer (1st SiC-poly CVD) 16, and a SiC epitaxial growth layer (SiC-epi) 13, as shown in FIG. 55. A highly doped layer 13a may be interposed between the first SiC polycrystalline growth layer 16 and the SiC epitaxial growth layer 13. The highly doped layer 13a suppresses the spread of the depletion layer in the SiC epitaxial growth layer 13, and easily forms an ohmic contact with the first SiC polycrystalline growth layer 16 formed on the C-face of the SiC epitaxial growth layer 13. The SiC epitaxial growth layer 13 serves as a drift layer, the highly doped layer 13a serves as a buffer layer, and the first SiC polycrystalline growth layer 16 serves as a substrate layer.
[0164] The first SiC polycrystalline growth layer 16 is n + type (impurity density is, for example, about 1×10 18 cm -3 ~Approx. 1×10 21 cm -3 ) and the SiC epitaxial growth layer 13 is doped with n - type (impurity density is, for example, about 5×10 14 cm -3 ~Approx. 5×10 16 cm -3 ) is doped.
[0165] Furthermore, the SiC epitaxial growth layer 13 may have any one of the crystal structures of 4H-SiC, 6H-SiC, or 2H-SiC.
[0166] As the n-type doping impurity, for example, N (nitrogen), P (phosphorus), As (arsenic), etc. can be used.
[0167] As the p-type doping impurity, for example, B (boron), Al (aluminum) or the like can be used.
[0168] In the vicinity (surface layer) of the surface 100 ((0001) Si surface) of the SiC epitaxial growth layer 13, p-type (impurity density is, for example, about 1×10 16 cm -3 ~Approx. 1×10 19 cm -3 The body region 52 of the SiC epitaxial growth layer 13 is formed in a well shape. The portion of the SiC epitaxial growth layer 13 on the SiC composite substrate 10 side with respect to the body region 52 is maintained in the state after the epitaxial growth, i.e., n - The drain region 53(13) is of the type.
[0169] The surface layer of the body region 52 is + A source region 54 of the type is formed in spaced relation to the periphery of the body region 52 .
[0170] Inside the source region 54, p + type (impurity density is, for example, about 1×10 18 cm -3 ~Approx. 1×10 21 cm -3 ) is formed in the body contact region 55. The body contact region 55 penetrates the source region 54 in the depth direction and is connected to the body region 52.
[0171] A gate insulating film 56 is formed on a surface 100 of the SiC epitaxial growth layer 13. The gate insulating film 56 covers a portion of the body region 52 surrounding the source region 54 (the peripheral portion of the body region 52) and the outer periphery of the source region 54.
[0172] A gate electrode 57 made of, for example, polysilicon is formed on the gate insulating film 56. The gate electrode 57 faces the peripheral edge of the body region 52 with the gate insulating film 56 interposed therebetween.
[0173] An interlayer insulating film 58 made of SiO2 is formed on the SiC epitaxial growth layer 13. A source electrode 62 is connected to the source region 54 and the body contact region 55 via a contact hole 61 formed in the interlayer insulating film 58.
[0174] (Removal of second SiC polycrystalline growth layer and second graphene layer) As shown in FIG. 56, in the SiC composite substrate 10, the second SiC polycrystalline growth layer 18 can be removed from the SiC composite substrate 10 by peeling off the interface between the second graphene layer 17 and the second SiC polycrystalline growth layer 18. As shown in FIG. 30, the second graphene layer 17 has a stacked structure of graphite sheets, and the graphite sheets on each surface are bonded by van der Waals forces, so that it can be peeled off. After removing the second SiC polycrystalline growth layer 18, the second graphene layer 17 is removed by etching or polishing to obtain a thinned SiC composite substrate 70 in which the first SiC polycrystalline growth layer 16 and the SiC epitaxial growth layer 13 are stacked.
[0175] In order to peel off the second graphene layer and the second SiC polycrystalline growth layer, a starting point of a crack between the second graphene layer and the second SiC polycrystalline growth layer is formed. As shown in FIG. 57, a heating body 191 such as a hot plate is brought into contact with the surface of the second SiC polycrystalline growth layer 18 of the SiC composite substrate 10. Then, by rapidly heating the second graphene layer 17 at the end of the SiC composite substrate 10 with the heating body 191, stress concentration due to thermal stress is generated at the interface between the second graphene layer 17 and the second SiC polycrystalline growth layer 18, and a starting point of a crack can be generated. Instead of the heating body 191 such as a hot plate, the second SiC polycrystalline growth layer 18 may be heated by irradiating light from a halogen lamp or the like.
[0176] 58, the surface of the second SiC polycrystalline growth layer 18 of the SiC composite substrate 10 may be cooled with a coolant 193 such as liquid nitrogen, and the thermal stress generated by the rapid cooling may be concentrated at the interface between the second graphene layer 17 at the end of the SiC composite substrate 10 and the second SiC polycrystalline growth layer 18, causing cracks to start. At this time, a heat-retaining plate 192 may be brought into contact with the surface of the SiC epitaxial growth layer 13 of the SiC composite substrate 10 to keep the surface of the SiC epitaxial growth layer 13 warm, thereby ensuring a temperature gradient within the SiC composite substrate 10.
[0177] As shown in FIG. 59, in the SiC composite substrate 10 in which the starting point of the crack is formed at the interface between the second graphene layer 17 and the second SiC polycrystalline growth layer 18 at the end surface, the surface of the second SiC polycrystalline growth layer 18 is scanned with an ultrasonic oscillator 194. The heated area caused by the focus of the ultrasonic waves converged along the interface between the second graphene layer 17 and the second SiC polycrystalline growth layer 18 moves, and the crack advances from the starting point of the crack along the interface between the second graphene layer 17 and the second SiC polycrystalline growth layer 18 due to thermal stress caused by heating. At this time, the oscillation energy of the ultrasonic oscillator may be set to a minimum value that advances the crack, thereby suppressing the occurrence of defects at the interface and warping of the substrate. In addition, a heat retention plate 192 may be brought into contact with the surface of the SiC epitaxial growth layer 13 of the SiC composite substrate 10 to keep the SiC epitaxial growth layer 13 warm, and a temperature gradient may be ensured within the SiC composite substrate 10. Instead of using the ultrasonic oscillator 194, the surface of the second SiC polycrystalline growth layer 18 of the SiC composite substrate 10 may be scanned with laser light to move the heated area to the interface between the second graphene layer 17 and the second SiC polycrystalline growth layer 18.
[0178] 60, in a SiC composite substrate 10 in which a crack origin is formed at the interface between the second graphene layer 17 and the second SiC polycrystalline growth layer 18 on the end surface, a cleavage blade 196 may be pushed into the crack origin on the end surface so that the crack mechanically advances from the crack origin along the interface between the second graphene layer 17 and the second SiC polycrystalline growth layer 18. At this time, the surface of the SiC epitaxial growth layer 13 of the SiC composite substrate 10 may be placed on a vacuum suction stage 195 and suctioned to fix the SiC composite substrate 10.
[0179] (Semiconductor element) In the semiconductor device of the second embodiment, as described above, the structure of the main part of the SiC-based semiconductor element is formed on the Si surface of the SiC epitaxial growth layer 13 in the SiC composite substrate 10. Therefore, as described above, the second SiC polycrystalline growth layer 18 and the second graphene layer 17 are removed from the SiC composite substrate 10 constituting the semiconductor device to obtain a thinned SiC composite substrate 70, and then a semiconductor element can be obtained by performing processing such as forming an electrode on the surface of the first SiC polycrystalline growth layer 16. In the following, a SiC-SBD, a SiC trench-gate type TMOSFET, and a SiC planar-gate type MOSFET, which are given as examples of the semiconductor device, will be described.
[0180] (SiC-SBD) Fig. 61 shows a SiC-SBD of a semiconductor element. The second SiC polycrystalline growth layer 18 and the second graphene layer 17 are removed from the SiC composite substrate 10 constituting the semiconductor device 120 having the SiC-SBD structure shown in Fig. 53 to form a thinned SiC composite substrate 70. Then, a cathode electrode 21 is formed on the back surface ((000-1) C surface) of the first SiC polycrystalline growth layer 16 of the thinned SiC composite substrate 70 so as to cover the entire area, and the cathode electrode 21 is connected to a cathode terminal K. Also, the anode electrode 26 is connected to an anode terminal A. In this manner, a SiC-SBD 20 as shown in Fig. 61 can be formed.
[0181] (SiC-TMOSFET) Fig. 62 shows a SiC-TMOSFET 30. The second SiC polycrystalline growth layer 18 and the second graphene layer 17 are removed from the SiC composite substrate 10 constituting the semiconductor device 130 having the SiC-TMOSFET structure shown in Fig. 54 to form a thinned SiC composite substrate 70. Then, a drain electrode 31 is formed on the back surface ((000-1) C surface) of the first SiC polycrystalline growth layer 16 of the thinned SiC composite substrate 70 so as to cover the entire area, and the drain electrode 31 is connected to a drain terminal D. In addition, the gate electrode 36 is connected to a gate terminal G, and the source electrode 43 is connected to a source terminal S. In this manner, a SiC-TMOSFET 30 as shown in Fig. 62 can be formed.
[0182] In the SiC-TMOSFET 30, by applying a predetermined voltage (a voltage equal to or higher than the gate threshold voltage) to the gate electrode 36 while a predetermined potential difference is generated between the source electrode 43 and the drain electrode 31 (between the source and drain), a channel can be formed in the body region 32 near the interface with the gate insulating film 35 by the electric field from the gate electrode 36. This allows a current to flow between the source electrode 43 and the drain electrode 31, turning the SiC-TMOSFET 30 into an on state.
[0183] (SiC planar gate MOSFET) Fig. 63 shows a SiC planar gate MOSFET 50. The second SiC polycrystalline growth layer 18 and the second graphene layer 17 are removed from the SiC composite substrate 10 constituting the semiconductor device 150 shown in Fig. 55 to form a thinned SiC composite substrate 70. Then, a drain electrode 51 is formed on the back surface ((000-1) C surface) of the first SiC polycrystalline growth layer 16 of the thinned SiC composite substrate 70 so as to cover the entire area. The drain electrode 51 is connected to a drain terminal D, and the gate electrode 57 is connected to a gate terminal G. In this manner, a SiC planar gate MOSFET 50 as shown in Fig. 63 can be formed.
[0184] In the SiC planar gate MOSFET 50, by applying a predetermined voltage (a voltage equal to or higher than the gate threshold voltage) to the gate electrode 57 while a predetermined potential difference is generated between the source electrode 62 and the drain electrode 51 (between the source and drain), a channel can be formed in the body region 52 near the interface with the gate insulating film 56 by the electric field from the gate electrode 57. This allows a current to flow between the source electrode 62 and the drain electrode 51, and the SiC planar gate MOSFET 50 can be turned on.
[0185] As described above, according to the second embodiment, a starting point for peeling is formed at the interface between the second graphene layer 17 and the second SiC polycrystalline growth layer 18 on the end face of the SiC composite substrate 10, and then by performing mechanical and / or thermal operations, the crack is propagated along the interface, thereby extending the crack across the entire interface in the SiC composite substrate 10, and the second graphene layer 17 and the second SiC polycrystalline growth layer 18 can be easily peeled off.
[0186] In addition, in the thinned SiC composite substrate 70 in which the second graphene layer 17 and the second SiC polycrystalline growth layer 18 are peeled off to remove the second SiC polycrystalline growth layer 18, the surface of the first SiC polycrystalline growth layer 16 on which the second graphene layer 17 is laminated maintains the surface roughness at the time of film formation, and can proceed directly to the next step unless special flattening processing by polishing or the like is required. In this case, the graphene remaining on the surface may be removed by oxygen plasma or the like. When thinning is performed by other technical methods, the thinned processed surface inevitably becomes rough, so flattening processing by polishing or the like is required to a certain extent. However, the thinning operation according to the second embodiment does not require polishing after thinning, and there is no processing loss of the expensive single crystal SiC layer at all, so the total cost of the SiC composite substrate can be further reduced. In addition, the peeled second SiC polycrystalline growth layer 18 can be reused as a dummy substrate or the like, which is economical. Similarly, the laminate of the first SiC polycrystalline growth layer 16, the second graphene layer 17, and the second SiC polycrystalline growth layer 18 generated in the modified example can also be reused as a dummy substrate.
[0187] Furthermore, according to the second embodiment, before forming first SiC polycrystalline growth layer 16 by CVD, SiC single crystal substrate 11 is separated and replaced with graphite substrate 19, which is a highly heat-resistant temporary substrate, thereby preventing unnecessary adhesion of SiC polycrystals to SiC single crystal substrate 11, improving the reusability of SiC single crystal substrate 11, and enabling cost reduction.
[0188] According to the second embodiment, by using graphite substrate 19, which is a highly heat-resistant temporary substrate one size larger than SiC single crystal substrate 11, it becomes possible to perform single-sided or double-sided epitaxial growth using an epitaxial growth apparatus such as a batch-type vertical tubular furnace, and it is possible to realize high-throughput and low-cost production without increasing the growth rate.
[0189] According to the second embodiment, by carbonizing a highly heat-resistant substrate such as graphite substrate 19 and an adhesive layer, the semiconductor substrate structures formed on both sides of graphite substrate 19 can be separated at low cost simply by baking them in an oxidation furnace or the like.
[0190] According to the second embodiment, remote epitaxial growth of SiC is performed via graphene formed on the SiC single crystal substrate 11, and the first SiC polycrystalline growth layer 16 and the like are formed directly thereon by CVD, making substrate bonding unnecessary and eliminating defects caused by substrate bonding. In addition, since the epitaxial growth layer is formed via the first graphene layer 12, separation of the SiC single crystal substrate 11 and the SiC epitaxial growth layer 13 becomes easy, simplifying the process steps.
[0191] According to the second embodiment, after the SiC single crystal substrate is removed, the graphite substrate 19, which is a highly heat-resistant handle substrate, is placed in a high-temperature LP-CVD apparatus, and the first SiC polycrystalline growth layer 16 and the like are grown directly on the SiC epitaxial growth layer 13. This eliminates the steps of transporting the epitaxial growth layer having a thickness of several μm from the handle substrate to a support substrate and bonding it to the support substrate, thereby making it possible to avoid defects such as wrinkles, crystal transitions, and voids that are caused by thin film transportation and bonding.
[0192] According to the second embodiment, the first graphene layer 12 formed on the SiC single crystal substrate 11 is not transferred, but epitaxial growth is performed directly on the first graphene layer 12. This makes it possible to avoid defects such as wrinkles and cracks caused by the transfer of graphene.
[0193] According to the second embodiment, since the SiC single crystal substrate 11 is used as a base, hexagonal SiC with little deterioration in crystallinity can be obtained. In addition, the SiC single crystal substrate 11 is expensive and difficult to remove by polishing or etching, but by using remote epitaxial growth via the first graphene layer 12, the obtained high-performance single crystal layer can be easily separated, making removal by polishing or etching unnecessary. Since the expensive SiC single crystal substrate 11 can be reused after separation, a large cost advantage can be obtained.
[0194] Although the second embodiment has been described above, it is also possible to implement the present invention in other aspects. For example, although not shown in the drawings, it is also possible to manufacture a MOS capacitor using the SiC composite substrate 10. In the MOS capacitor, the yield and reliability can be improved.
[0195] Although not shown, a bipolar transistor can also be manufactured using the SiC composite substrate 10. The SiC composite substrate 10 according to the second embodiment can also be used to manufacture SiC-pn diodes, SiCIGBTs, SiC complementary MOSFETs, etc. The semiconductor composite substrate 1 can also be applied to other types of devices, such as LEDs (light emitting diodes) and semiconductor optical amplifiers (SOAs).
[0196] The SiC epitaxial growth layer 13 may include at least one type or a plurality of types selected from the group consisting of Group IV element semiconductors, Group III-V compound semiconductors, and Group II-VI compound semiconductors.
[0197] Furthermore, the SiC single crystal substrate 11 and the SiC epitaxial growth layer 13 may be made of any one of 4H-SiC, 6H-SiC, and 2H-SiC materials.
[0198] Furthermore, the SiC single crystal substrate 11 and the SiC epitaxial growth layer 13 may comprise, as a material other than SiC, at least one selected from the group consisting of GaN, BN, AlN, Al2O3, Ga2O3, diamond, carbon, and graphite.
[0199] A semiconductor device including the SiC composite substrate 10 may include any of GaN-, AlN-, and gallium oxide-based IGBTs, diodes, MOSFETs, and thyristors other than SiC-based.
[0200] A semiconductor device including a SiC composite substrate 10 may have any of the following configurations: a one-in-one module, a two-in-one module, a four-in-one module, a six-in-one module, a seven-in-one module, an eight-in-one module, a twelve-in-one module, or a fourteen-in-one module.
[0201] The SiC composite substrate 10 uses a low-cost first SiC polycrystalline growth layer 16 and a second SiC polycrystalline growth layer 18 instead of a high-cost SiC single crystal substrate 11 on the Si surface that serves as the device surface.
[0202] (Third embodiment) Next, the third embodiment will be described. The third embodiment uses a hydrogen ion implantation delamination method that implants hydrogen ions into a SiC single crystal substrate to form an embrittled layer, thereby enabling the delamination of a thinned layer on the surface. The third embodiment is similar to the second embodiment except that the hydrogen ion implantation delamination method is used in the manufacturing method of the semiconductor substrate, so in the following third embodiment, only the manufacturing method of the semiconductor substrate will be described. The SiC composite substrate 10 manufactured by the semiconductor manufacturing method of the third embodiment can be applied to semiconductor devices and semiconductor elements, as in the second embodiment. For simplicity, in the following description of the third embodiment, the same reference numbers are used for members common to the second embodiment, and their description may be omitted.
[0203] (Method of manufacturing semiconductor substrate) Hydrogen ions are implanted into the Si surface of the SiC single crystal substrate (SiCSB) 11 shown in Fig. 25 for the ion implantation delamination method to form a hydrogen ion implanted layer 11c having a specified depth (for example, about 1 µm). Fig. 64 shows the SiC single crystal substrate 11 on which the hydrogen ion implanted layer 11c has been formed. Here, the ion implantation conditions are, for example, an acceleration energy of about 100 keV and a dose of about 2.0 × 10 17 / cm 2 The hydrogen ion implanted layer 11c is then subjected to a high temperature treatment to embrittle the hydrogen ion implanted layer 11c. After the hydrogen ion implantation, embrittlement thermal annealing is required to generate hydrogen microbubbles and make the hydrogen ion implanted layer 11c easier to break.
[0204] As shown in Fig. 65, a SiC epitaxial growth layer 13 is formed by CVD on the Si surface of the hydrogen ion implanted layer 11c. Then, as shown in Fig. 66, a graphite substrate 19 serving as a temporary substrate is attached to the Si surface of the SiC epitaxial growth layer 13 via an adhesive layer 15 made of a carbon adhesive, and the adhesive layer 15 is carbonized by heating in a thermal annealing furnace or the like.
[0205] The embrittled hydrogen ion implanted layer 11c is divided along the separation surface indicated by the line BB in FIG. 66, and the SiC single crystal substrate 11 is removed. As shown in FIG. 67, the side of the divided hydrogen ion implanted layer 11c in contact with the SiC epitaxial growth layer 13 forms a thinned SiC single crystal layer 11d formed by thinning the SiC single crystal substrate 11. Meanwhile, the uneven structure formed by separation on the Si surface of the main body of the SiC single crystal substrate 11 divided by the hydrogen ion implanted layer 11c is smoothed by mechanical polishing, mechanical chemical polishing, or the like. The average surface roughness Ra of the Si surface of the SiC single crystal substrate 11 is reduced to, for example, about 1 nm or less by the above process. As a result, the SiC single crystal substrate 11 becomes reusable.
[0206] As shown in Fig. 68, the peeled surface of the laminate of the thinned SiC single crystal layer 11d and the SiC epitaxial growth layer 13 bonded to the graphite substrate 19 has an uneven structure smoothed out by mechanical polishing, mechanical chemical polishing, etc. The structure shown in Fig. 68 forms a seventh composite (19, 15, 13 (SiC-epi), 11d).
[0207] As shown in Fig. 69, a first SiC polycrystalline growth layer 16 is formed by CVD on the C-face of the thinned SiC single crystal layer 11d of the seventh complex. As shown in Fig. 70, a second graphene layer (GR) 17 is formed on the C-face of the thinned SiC single crystal layer 11d of the seventh complex on which the first SiC polycrystalline growth layer 16 has been formed. As shown in Fig. 71, a second SiC polycrystalline growth layer 18 is further formed on the C-face of the thinned SiC single crystal layer 11d of the seventh complex on which the first SiC polycrystalline growth layer 16 and the second graphene layer 17 are laminated.
[0208] As shown in Fig. 72, the second SiC polycrystalline growth layer 18, the second graphene layer 17, and the first SiC polycrystalline growth layer 16 on the periphery of the seventh composite in which the first SiC polycrystalline growth layer 16, the second graphene layer 17, and the second SiC polycrystalline growth layer 18 shown in Fig. 71 are laminated are ground and polished to remove them. The structure shown in Fig. 72 forms an eighth composite (18 (2nd SiC-poly SVD), 17 (GR), 16 (1st SiC-poly SVD), 19, 15, 13 (SiC-epi), 11c, 16 (1st SiC-poly SVD), 17 (GR), 18 (2nd SiC-poly SVD)).
[0209] 73, the graphite substrate 19 and the carbonized adhesive layer 15 inside the eighth composite are removed by oxidative combustion to obtain a SiC composite substrate 10 in which a SiC epitaxial growth layer 13, a thinned SiC single crystal layer 11d, a first SiC polycrystalline growth layer 16, a second graphene layer 17, and a second SiC polycrystalline growth layer 18 are laminated. The SiC composite substrate 10 of the second embodiment is similar to the SiC composite substrate 10 of the second embodiment except that the thinned SiC single crystal layer 11d is interposed between the SiC epitaxial growth layer 13 and the first SiC polycrystalline growth layer.
[0210] Here, since the SiC epitaxial growth layer 13 has the same crystal structure as the SiC single crystal substrate 11, the SiC composite substrate 10 of the third embodiment shown in Fig. 73 has the same structure as the SiC composite substrate 10 of the second embodiment. Note that, by oxidatively burning the graphite substrate 19 and the adhesive layer 15, a laminate of the second SiC polycrystalline growth layer 18, the second graphene layer 17, and the first SiC polycrystalline growth layer 16 is obtained. This laminate has the same shape and size as the SiC composite substrate 10, and can therefore also be used as a dummy substrate.
[0211] As described above, the method for manufacturing a semiconductor substrate according to the third embodiment can produce a SiC composite substrate 10 in the same manner as in the second embodiment. Therefore, the second embodiment can also produce the same effects as in the second embodiment. Furthermore, in the third embodiment, epitaxial growth is performed directly on the Si surface of the SiC single crystal substrate 11 without an intervening graphene layer, so that a SiC epitaxial growth layer 13 having a good crystal structure can be formed. Furthermore, according to the third embodiment, a dummy substrate can be produced simultaneously with the SiC composite substrate 10.
[0212] (Other embodiments) As described above, several embodiments have been described, but the descriptions and drawings forming part of the disclosure are illustrative and should not be understood as limiting. From this disclosure, various alternative embodiments, examples and operating techniques will become apparent to those skilled in the art. Thus, the embodiments include various embodiments not described herein.
[0213] (Appendix 1) The manufacturing method of the SiC composite substrate 10, which is a semiconductor substrate, includes the steps of forming a graphene layer 12 on the Si surface of the SiC single crystal substrate 11, forming a SiC epitaxial growth layer 13 on the graphene layer 12, forming a stress layer 14 on the SiC epitaxial growth layer 13, attaching a graphite substrate 19 of a temporary substrate on the stress layer 14, peeling the graphene layer 12 and the SiC epitaxial growth layer 13, forming a SiC polycrystalline growth layer 16 on the C surface of the SiC epitaxial growth layer 13 from which the graphene layer 12 has been peeled off, and removing the graphite substrate 19. The stress layer 14 generates stress between the graphene layer 12 and the SiC epitaxial growth layer 13 to facilitate peeling. This facilitates peeling between the graphene layer 12 and the SiC epitaxial growth layer 13.
[0214] (Appendix 2) In the method for manufacturing a semiconductor substrate according to Appendix 1, the stress layer 14 generates a stress between the graphene layer 12 and the SiC epitaxial growth layer 13 that is similar to the adhesion energy between the graphene layer 12 and the SiC epitaxial growth layer 13. This enables peeling at the interface between the graphene layer 12 and the SiC epitaxial growth layer 13.
[0215] (Appendix 3) In the method for manufacturing a semiconductor substrate described in Appendix 2, the stress layer 14 generates stress for peeling off the graphene layer 12 and the SiC epitaxial growth layer 13 by a stacked structure of the SiC single crystal substrate 11, the graphene layer 12, the SiC epitaxial growth layer 13, the stress layer 14, and the graphite substrate 19. The magnitude of the generated stress can be adjusted.
[0216] (Appendix 4) In the method for manufacturing a semiconductor substrate according to any one of claims 1 to 3, the stress layer 14 includes a carbon film or a silicon nitride film. Since the stress layer 14 does not include a metal, contamination by a metal can be avoided.
[0217] (Appendix 5) In the method for manufacturing a semiconductor substrate according to appended claim 4, the carbon film includes a polycrystalline diamond film or a diamond-like carbon film. It can be formed relatively easily and can withstand high heat.
[0218] (Appendix 6) The method for manufacturing a semiconductor substrate according to any one of claims 1 to 3 further comprises removing the stress layer 14 by burning or grinding. The stress layer 14 can be easily removed.
[0219] (Appendix 7) In the method for manufacturing a semiconductor substrate according to appended claim 1, the graphite substrate 19 serving as a temporary substrate is made of graphite. This enables the graphite substrate 19 serving as a temporary substrate to be removed by burning.
[0220] (Appendix 8) In the method for manufacturing a semiconductor substrate according to appended claim 7, the graphite substrate 19 has an outer size larger than that of the SiC single crystal substrate 11. When the graphite substrate 19 is inserted into a wafer boat groove in a batch-type vertical CVD furnace and aligned, the marks of the wafer boat support pillars can be made to be outside the effective area of the substrate.
[0221] (Appendix 9) In the method for producing a semiconductor substrate according to Appendix 7, graphite substrate 19 includes a glassy carbon coating formed on the surface thereof. Since the glassy carbon coating has a strong adhesive force with the carbon adhesive of adhesive layer 15, graphene layer 12 and SiC epitaxial growth layer 13 can be easily peeled off from each other.
[0222] (Appendix 10) In the method for manufacturing a semiconductor substrate according to any one of Supplementary Note 7 to 9, the step of removing the graphite substrate 19 removes the graphite substrate 19 by burning it. The graphite substrate 19 can be removed by burning it in an air atmosphere or the like.
[0223] (Appendix 11) In the method for manufacturing a semiconductor substrate described in Appendix 1, the step of attaching the graphite substrate 19 onto the stress layer 14 attaches the stress layer 14 and the graphite substrate 19 via an adhesive layer made of a carbon adhesive. The carbon adhesive is capable of maintaining its bonding strength even at high temperatures by carbonizing the adhesive itself.
[0224] (Appendix 12) The method for producing a semiconductor substrate according to claim 11 further includes a step of burning and removing the adhesive layer 15. The adhesive layer 15 can be burned and removed together with the graphite substrate 19 in an air atmosphere or the like.
[0225] (Appendix 13) The method for manufacturing a semiconductor substrate according to Appendix 1 further includes, prior to the step of removing the graphite substrate 19, a step of grinding and removing the SiC polycrystalline growth layer 16 and the graphite substrate 19 protruding from the outer periphery of the composite including the graphite substrate 19, the stress layer 14, and the SiC epitaxial growth layer 13 in the step of forming the SiC polycrystalline growth layer 16, thereby exposing the outer periphery of the graphite substrate 19. This enables the graphite substrate 19 to be removed by burning.
[0226] (Appendix 14) The method for manufacturing a semiconductor substrate according to Appendix 1 further includes, prior to the step of removing the graphite substrate 19, a step of cutting the graphite substrate 19 in two along a plane parallel to its main surface together with the SiC polycrystalline growth layer 16 protruding from the outer periphery of the graphite substrate 19 in the step of forming the SiC polycrystalline growth layer 16, thereby exposing the cut surfaces of the graphite substrate 19. This enables the graphite substrate 19 to be removed by burning.
[0227] (Appendix 15) The method for manufacturing a semiconductor substrate according to Appendix 1 further includes a step of forming a highly-doped layer 13a having a higher impurity concentration than the SiC epitaxial growth layer 13 on a C-face of the SiC epitaxial growth layer 13 that is in contact with the SiC polycrystalline growth layer 16. The highly-doped layer 13a suppresses the spread of a depletion layer in the SiC epitaxial growth layer 13, and easily forms an ohmic contact with the SiC polycrystalline growth layer 16 formed on the C-face of the SiC epitaxial growth layer 13.
[0228] (Appendix 16) In the method for manufacturing a semiconductor substrate according to appendix 15, the step of forming the highly doped layer 13a includes an ion implantation step or an autodoping step of epitaxial growth. The highly doped layer 13a can be easily formed.
[0229] (Appendix 17) The SiC composite substrate 10, which is a semiconductor substrate, includes a SiC single crystal substrate 11, a graphene layer 12 arranged on the Si surface of the SiC single crystal substrate 11, a SiC epitaxial growth layer 13 arranged above the SiC single crystal substrate 11 via the graphene layer 12, and a stress layer 14 arranged on the Si surface of the SiC epitaxial growth layer 13, and the stress layer 14 generates stress between the graphene layer 12 and the SiC epitaxial growth layer 13 to facilitate peeling. The stress layer 14 facilitates peeling between the graphene layer 12 and the SiC epitaxial growth layer 13.
[0230] (Appendix 18) In the semiconductor substrate according to Appendix 17, the stress layer 14 generates a stress between the graphene layer 12 and the SiC epitaxial growth layer 13 that is similar to the adhesion energy between the graphene layer 12 and the SiC epitaxial growth layer 13. This enables peeling at the interface between the graphene layer 12 and the SiC epitaxial growth layer 13.
[0231] (Appendix 19) In the semiconductor substrate according to claim 17 or 18, the stress layer 14 includes a carbon film or a silicon nitride film. Since the stress layer 14 does not include a metal, contamination by a metal can be avoided.
[0232] (Appendix 20) 20. The semiconductor substrate according to claim 19, wherein the carbon film includes a polycrystalline diamond film or a diamond-like carbon film. The carbon film can be formed relatively easily and can withstand high heat.
[0233] (Appendix 21) 18. The semiconductor substrate of claim 17, further comprising a graphite substrate 19 disposed on the stress layer 14. The stress layer 14 may be fixed to the graphite substrate 19.
[0234] (Appendix 22) In the semiconductor substrate according to appendix 21, the graphite substrate 19 serving as a temporary substrate is made of graphite. The graphite substrate 19 serving as a temporary substrate can be removed by burning.
[0235] (Appendix 23) In the semiconductor substrate according to Appendix 22, the stress layer 14 and the graphite substrate 19 are attached to each other by an adhesive layer 15 made of a carbon adhesive. Since the carbon adhesive has a strong adhesive force, the graphene layer 12 and the SiC epitaxial growth layer 13 can be easily peeled off from each other.
[0236] (Appendix 24) In the semiconductor substrate according to Appendix 22, the graphite substrate 19 includes a glassy carbon coating formed on the surface thereof. The glassy carbon coating has a strong adhesive force with the carbon adhesive of the adhesive layer 15, so that the graphene layer 12 and the SiC epitaxial growth layer 13 can be easily peeled off from each other.
[0237] (Appendix 25) In the semiconductor substrate according to any one of appendices 22 to 24, the graphite substrate 19 has an outer size larger than that of the SiC single crystal substrate. When the graphite substrate 19 is inserted into a wafer boat groove of a batch-type vertical CVD furnace and aligned, the wafer boat support marks can be positioned outside the effective substrate area.
[0238] (Appendix 26) The semiconductor substrate according to claim 17, further comprising a SiC polycrystalline growth layer 16 disposed on the C-plane of the SiC epitaxial growth layer 13. The SiC polycrystalline growth layer 16 can be easily formed by CVD.
[0239] (Appendix 27) In the semiconductor substrate according to Appendix 26, the SiC epitaxial growth layer 13 further has a highly doped layer 13a having a higher impurity concentration than the SiC epitaxial growth layer 13 on a surface in contact with the SiC polycrystalline growth layer 16. The highly doped layer 13a suppresses the spread of a depletion layer in the SiC epitaxial growth layer 13, and easily forms an ohmic contact with the SiC polycrystalline growth layer 16 formed on the C-face of the SiC epitaxial growth layer 13.
[0240] (Appendix 28) In the semiconductor substrate according to Appendix 17, the graphene layer 12 has a single-layer structure or a multi-layer stacked structure of graphene. The graphene layer 12 can be peeled off.
[0241] (Appendix 29) The manufacturing method of the SiC composite substrate 10, which is a semiconductor substrate, includes the steps of forming a SiC epitaxial growth layer 13 on the Si surface of the SiC single crystal substrate 11, attaching the Si surface of the SiC epitaxial growth layer 13 to a graphite substrate 19, which is a temporary substrate, removing the SiC epitaxial growth layer 13 from the SiC single crystal substrate 11, forming a first SiC polycrystalline growth layer 16 on the C surface of the SiC epitaxial growth layer 13 attached to the graphite substrate 19, forming a second graphene layer 17, which is a graphene layer, on the first SiC polycrystalline growth layer 16, forming a second SiC polycrystalline growth layer 18 on the second graphene layer 17, and removing the graphite substrate 19. The second graphene layer 17 and the second SiC polycrystalline growth layer 18 can be peeled off.
[0242] (Appendix 30) The method for producing a semiconductor substrate according to Appendix 29 further includes a step of forming a first graphene layer 12 as another graphene layer on a Si surface of the SiC single crystal substrate 11, and the step of forming the SiC epitaxial growth layer 13 forms the SiC epitaxial growth layer 13 on the Si surface of the SiC single crystal substrate 11 via the first graphene layer 12. This makes it possible to peel off the first graphene layer 12 and the SiC epitaxial growth layer 13.
[0243] (Appendix 31) In the method for producing a semiconductor substrate according to Appendix 30, the step of removing the SiC epitaxial growth layer 13 from the SiC single crystal substrate 11 peels the SiC epitaxial growth layer 13 from the first graphene layer 12. The first graphene layer can be peeled off because the graphite sheets are bonded by van der Waals forces.
[0244] (Appendix 32) The method for producing a semiconductor substrate according to Appendix 31 further includes a step of forming a stress layer 14 on a Si face of the SiC epitaxial growth layer 13, the stress layer 14 generating a stress for peeling the SiC epitaxial growth layer 13 from the first graphene layer 12, and the step of attaching the Si face of the SiC epitaxial growth layer 13 to the graphite substrate 19 attaches the Si face of the SiC epitaxial growth layer 13 to the graphite substrate 19 via the stress layer 14. The graphite substrate 19 can fix a stack including the SiC epitaxial growth layer 13 and the SiC single crystal substrate 11.
[0245] (Appendix 33) The method for manufacturing a semiconductor substrate according to Appendix 29 further includes a step of forming a hydrogen ion implanted layer 11c at a predetermined depth from the Si face of the SiC single crystal substrate 11, and the step of removing the SiC epitaxial growth layer 13 from the SiC single crystal substrate 11 embrittles the hydrogen ion implanted layer 11c to peel off the SiC epitaxial growth layer 13 together with the thinned SiC single crystal layer 11d separated by the hydrogen ion implanted layer 11c from the SiC single crystal substrate 11. Separation is made possible by embrittling the hydrogen ion implanted layer 11c of the SiC single crystal substrate 11.
[0246] (Appendix 34) The method for manufacturing a semiconductor substrate according to claim 33 further includes a step of polishing a C-face of the thinned SiC single crystal layer 11d peeled off together with the SiC epitaxial growth layer 13. This makes it possible to smooth out the uneven structure formed by the division of the hydrogen ion implanted layer 11c.
[0247] (Appendix 35) In the method for producing a semiconductor substrate according to appended claim 29, the graphite substrate 19 serving as a temporary substrate is made of graphite. This enables the graphite substrate 19 serving as a temporary substrate to be removed by burning.
[0248] (Appendix 36) In the method for manufacturing a semiconductor substrate according to Appendix 35, the graphite substrate 19 has an outer size larger than that of the SiC single crystal substrate 11. When the graphite substrate 19 is inserted into a wafer boat groove in a batch-type vertical CVD furnace and aligned, the marks of the wafer boat support pillars can be made to be outside the effective area of the substrate.
[0249] (Appendix 37) In the method for producing a semiconductor substrate according to Appendix 35, graphite substrate 19 includes a glassy carbon coating formed on a surface thereof. Since the glassy carbon coating has a strong adhesive force with the carbon adhesive of adhesive layer 15, first graphene layer 12 and SiC epitaxial growth layer 13 can be reliably peeled off from each other.
[0250] (Appendix 38) In the method for manufacturing a semiconductor substrate according to any one of appendices 35 to 37, the step of removing the graphite substrate 19 removes the graphite substrate 19 by burning it. The graphite substrate 19 can be removed by burning it in an air atmosphere or the like.
[0251] (Appendix 39) In the method for manufacturing a semiconductor substrate according to Appendix 38, in the step of attaching the graphite substrate 19 to the C-face of the SiC epitaxial growth layer 13, the SiC epitaxial growth layer 13 and the graphite substrate 19 are attached via an adhesive layer made of a carbon adhesive. Since the carbon adhesive has a strong adhesive force, the first graphene layer 12 and the SiC epitaxial growth layer 13 can be reliably peeled off.
[0252] (Appendix 40) In the method for producing a semiconductor substrate according to Appendix 39, the step of removing the graphite substrate 19 includes burning and removing the adhesive layer 15 together with the graphite substrate 19. The adhesive layer 15 can be burned and removed together with the graphite substrate 19 in the air atmosphere or the like.
[0253] (Appendix 41) The method for manufacturing a semiconductor substrate according to Appendix 29 further includes a step of forming a highly-doped layer 13a having a higher impurity concentration than the SiC epitaxial growth layer 13 on a C-face of the SiC epitaxial growth layer 13 in contact with the first SiC polycrystalline growth layer 16. The highly-doped layer 13a suppresses the spread of a depletion layer in the SiC epitaxial growth layer 13, and easily forms an ohmic contact with the first SiC polycrystalline growth layer 16 formed on the C-face of the SiC epitaxial growth layer 13.
[0254] (Appendix 42) In the method for manufacturing a semiconductor substrate according to claim 41, the step of forming the highly doped layer 13a includes an ion implantation step or an autodoping step of epitaxial growth. The highly doped layer 13a can be reliably formed.
[0255] (Appendix 43) A method for manufacturing a semiconductor device including the method for manufacturing a semiconductor substrate described in Appendix 29, further comprising a step of forming at least a part of a structure constituting a semiconductor element on the C-face of the SiC epitaxial growth layer 13 of the SiC composite substrate 10. By peeling off the second SiC polycrystalline growth layer 18, the SiC composite substrate 10 can be easily thinned.
[0256] (Appendix 44) In the method for manufacturing a semiconductor device according to claim 43, the semiconductor element includes at least one of a SiC Schottky barrier diode, a SiC-MOSFET, a SiC bipolar transistor, a SiC diode, a SiC thyristor, and a SiC insulated gate bipolar transistor. Various useful SiC-based semiconductor elements can be provided.
[0257] (Appendix 45) The method for manufacturing a semiconductor device according to claim 43 further includes a step of peeling off the second SiC polycrystalline growth layer 18 from the graphene layer in the SiC composite substrate 10 on which a semiconductor element structure has been formed. The thinning of the SiC composite substrate 10 can be achieved by peeling off the second SiC polycrystalline growth layer 18 without grinding.
[0258] (Appendix 46) In the method for manufacturing a semiconductor device according to Appendix 45, the step of peeling off the second SiC polycrystalline growth layer 18 from the second graphene layer 17 further includes a step of heating the Si face of the second SiC polycrystalline growth layer 18. Heating can be easily performed using a hot plate.
[0259] (Appendix 47) In the method for manufacturing a semiconductor device according to Appendix 45, the step of peeling off the second SiC polycrystalline growth layer 18 from the second graphene layer 17 further includes a step of cooling the Si face of the second SiC polycrystalline growth layer 18. Cooling can be easily achieved using liquid nitrogen or the like.
[0260] (Appendix 48) In the method for manufacturing a semiconductor device according to Appendix 45, the step of peeling off the second SiC polycrystalline growth layer 18 from the second graphene layer 17 further includes the step of scanning the Si surface of the second SiC polycrystalline growth layer 18 with an ultrasonic oscillator. The position where the crack is generated can be controlled by adjusting the focus of the ultrasonic wave irradiated by the ultrasonic oscillator.
[0261] (Appendix 49) In the method for manufacturing a semiconductor device according to Appendix 45, the step of peeling off the second SiC polycrystalline growth layer 18 from the second graphene layer 17 further includes a step of forcing a cleavage blade 106 between the second graphene layer 17 and the second SiC polycrystalline growth layer 18 to cause cleavage. The occurrence of mechanical cleavage by the cleavage blade 106 can be reliably controlled.
[0262] (Appendix 50) The SiC composite substrate 10, which is a semiconductor substrate, includes a SiC epitaxial growth layer 13, a first SiC polycrystalline growth layer 16 disposed on the Si face of the SiC epitaxial growth layer 13, a second graphene layer 17 disposed on the first SiC polycrystalline growth layer 16, and a second SiC polycrystalline growth layer 18 disposed on the second graphene layer 17. By peeling off the second SiC polycrystalline growth layer 18, the SiC composite substrate 10 can be easily thinned.
[0263] (Appendix 51) In the SiC composite substrate 10 described in Appendix 50, the second graphene layer 17 has a single-layer structure or a multi-layer structure of graphene. The second graphene layer 17 can be peeled off because the graphite sheets are bonded by van der Waals forces.
[0264] (Appendix 52) In the SiC composite substrate 10 described in Appendix 50, the SiC epitaxial growth layer 13 further has a highly-doped layer 13a on the C-face having a higher impurity concentration than the SiC epitaxial growth layer 13. The highly-doped layer 13a suppresses the spread of a depletion layer in the SiC epitaxial growth layer 13, and easily forms an ohmic contact with the first SiC polycrystalline growth layer 16 formed on the C-face of the SiC epitaxial growth layer 13.
[0265] (Appendix 53) A semiconductor device comprising the SiC composite substrate 10 according to claim 50, and a semiconductor element structure formed on the C-face of the SiC epitaxial growth layer 13. The SiC composite substrate 10 can be easily thinned, which facilitates the fabrication of the semiconductor element.
[0266] (Appendix 54) In the SiC composite substrate 10 described in Appendix 50, the semiconductor element includes at least one of a SiC Schottky barrier diode, a SiC-MOSFET, a SiC bipolar transistor, a SiC diode, a SiC thyristor, and a SiC insulated gate bipolar transistor. Various useful SiC-based semiconductor elements can be provided. [Industrial Applicability]
[0267] The present disclosure can be used in various semiconductor module technologies, such as IGBT modules, diode modules, and MOS modules (SiC, GaN, AlN, gallium oxide), and can be applied to a wide range of application fields, such as power modules for inverter circuits that drive electric motors used as power sources for electric vehicles (including hybrid vehicles), trains, industrial robots, etc., and power modules for inverter circuits that convert power generated by solar cells, wind turbines, and other power generation devices (especially private power generation devices) into power from commercial power sources. [Explanation of symbols]
[0268] 10 SiC composite substrate 11 SiC single crystal substrate 11c Hydrogen ion implantation layer 11d Thinned SiC single crystal layer 12 Graphene layer, first graphene layer 13. SiC epitaxial growth layer 14 Stress Layer 15 Adhesive layer 16 SiC polycrystalline growth layer, 1st SiC polycrystalline growth layer 17 Second graphene layer 18 2nd SiC polycrystalline growth layer 19 Graphite Substrate
Claims
1. forming a graphene layer on a Si surface of a SiC single crystal substrate; forming a SiC epitaxial growth layer on the graphene layer; forming a stress layer on the SiC epitaxial growth layer; attaching a temporary substrate onto the stress layer; peeling off the graphene layer and the SiC epitaxial growth layer; forming a SiC polycrystalline growth layer on a C-face of the SiC epitaxial growth layer from which the graphene layer has been peeled off; removing the temporary substrate; Including, The stress layer generates stress between the graphene layer and the SiC epitaxial growth layer such that peeling is facilitated.
2. 2. The method for manufacturing a semiconductor substrate according to claim 1, wherein the stress layer generates a stress between the graphene layer and the SiC epitaxial growth layer that is similar to an adhesion energy between the graphene layer and the SiC epitaxial growth layer.
3. 3. The method for manufacturing a semiconductor substrate according to claim 2, wherein the stress layer generates a stress that peels off the graphene layer and the SiC epitaxial growth layer by a stacked structure of the SiC single crystal substrate, the graphene layer, the SiC epitaxial growth layer, the stress layer, and the temporary substrate.
4. The method for manufacturing a semiconductor substrate according to claim 1 , wherein the stress layer includes a carbon film or a silicon nitride film.
5. The method for manufacturing a semiconductor substrate according to claim 4 , wherein the carbon film includes a polycrystalline diamond film or a diamond-like carbon film.
6. The method for manufacturing a semiconductor substrate according to claim 1 , further comprising the step of removing the stress layer by burning or grinding.
7. The method for manufacturing a semiconductor substrate according to claim 1 , wherein the temporary substrate is made of graphite.
8. The method for manufacturing a semiconductor substrate according to claim 7 , wherein the temporary substrate has an outer size larger than that of the SiC single crystal substrate.
9. The method for manufacturing a semiconductor substrate according to claim 7 , wherein the temporary substrate includes a glassy carbon coating formed on a surface thereof.
10. The method for manufacturing a semiconductor substrate according to claim 7 , wherein the step of removing the temporary substrate comprises burning the temporary substrate to remove it.
11. 2 . The method for manufacturing a semiconductor substrate according to claim 1 , wherein the step of attaching the temporary substrate onto the stress layer comprises attaching the stress layer and the temporary substrate via an adhesive layer made of a carbon adhesive.
12. The method for manufacturing a semiconductor substrate according to claim 11, further comprising the step of burning off the adhesion layer.
13. 2. The method for manufacturing a semiconductor substrate according to claim 1, further comprising the step of grinding and removing the SiC polycrystalline growth layer and the temporary substrate that protrude to the outer periphery of a composite including the temporary substrate, the stress layer, and the SiC epitaxial growth layer in the step of forming the SiC polycrystalline growth layer, to expose the outer periphery of the temporary substrate, prior to the step of removing the temporary substrate.
14. 2. The method for manufacturing a semiconductor substrate according to claim 1, further comprising the step of cutting the temporary substrate in two along a plane parallel to its main surface together with the SiC polycrystalline growth layer protruding to the outer periphery of the temporary substrate in the step of forming the SiC polycrystalline growth layer, prior to the step of removing the temporary substrate, to expose the cut surfaces of the temporary substrate.
15. 2. The method for manufacturing a semiconductor substrate according to claim 1, further comprising the step of forming a highly doped layer having a higher impurity concentration than the SiC epitaxial growth layer on a C-face of the SiC epitaxial growth layer in contact with the SiC polycrystalline growth layer.
16. The method for manufacturing a semiconductor substrate according to claim 15, wherein the step of forming the highly doped layer includes an ion implantation step or an autodoping step in epitaxial growth.
17. A SiC single crystal substrate; A graphene layer disposed on a Si surface of the SiC single crystal substrate; a SiC epitaxial growth layer disposed above the SiC single crystal substrate via the graphene layer; a stress layer disposed on the Si surface of the SiC epitaxial growth layer; Including, The stress layer generates stress between the graphene layer and the SiC epitaxial growth layer to facilitate peeling.
18. forming a SiC epitaxial growth layer on the Si surface of the SiC single crystal substrate; attaching a Si surface of the SiC epitaxial growth layer to a temporary substrate; removing the SiC epitaxial growth layer from the SiC single crystal substrate; forming a first SiC polycrystalline growth layer on a C-face of the SiC epitaxial growth layer attached to the temporary substrate; forming a graphene layer on the first SiC polycrystalline growth layer; forming a second SiC polycrystalline growth layer on the graphene layer; removing the temporary substrate; A method for manufacturing a semiconductor substrate comprising the steps of:
19. 20. The method for producing a semiconductor substrate according to claim 18, further comprising the step of forming another graphene layer on a Si surface of the SiC single crystal substrate, wherein the step of forming the SiC epitaxial growth layer forms the SiC epitaxial growth layer on the Si surface of the SiC single crystal substrate via the another graphene layer.
20. The method for manufacturing a semiconductor substrate according to claim 19 , wherein the step of removing the SiC epitaxial growth layer from the SiC single crystal substrate comprises peeling the SiC epitaxial growth layer from the other graphene layer.
21. 21. The method for manufacturing a semiconductor substrate according to claim 20, further comprising the step of forming a stress layer on a Si surface of the SiC epitaxial growth layer, the stress layer generating a stress that peels the SiC epitaxial growth layer from the other graphene layer, and the step of attaching the Si surface of the SiC epitaxial growth layer to the temporary substrate includes attaching the Si surface of the SiC epitaxial growth layer to the temporary substrate via the stress layer.
22. 20. The method for manufacturing a semiconductor substrate according to claim 18, further comprising the step of forming a hydrogen ion implanted layer at a predetermined depth from a Si-face of the SiC single crystal substrate, and the step of removing the SiC epitaxial growth layer from the SiC single crystal substrate comprises embrittling the hydrogen ion implanted layer to peel off the SiC epitaxial growth layer together with the thinned SiC single crystal layer divided by the hydrogen ion implanted layer from the SiC single crystal substrate.
23. The method for producing a semiconductor substrate according to claim 22 , further comprising the step of polishing a C-plane of the thinned SiC single crystal layer that has been peeled off together with the SiC epitaxial growth layer.
24. The method for manufacturing a semiconductor substrate according to claim 18 , wherein the temporary substrate is made of graphite.
25. The method for manufacturing a semiconductor substrate according to claim 24 , wherein the temporary substrate has an outer size larger than that of the SiC single crystal substrate.
26. The method for manufacturing a semiconductor substrate according to claim 24 , wherein the temporary substrate includes a glassy carbon coating formed on a surface thereof.
27. The method for manufacturing a semiconductor substrate according to claim 24 , wherein the step of removing the temporary substrate comprises burning the temporary substrate to remove it.
28. 28. The method for manufacturing a semiconductor substrate according to claim 27, wherein the step of attaching the temporary substrate to the C surface of the SiC epitaxial growth layer includes attaching the SiC epitaxial growth layer and the temporary substrate via an adhesive layer made of a carbon adhesive.
29. The method for manufacturing a semiconductor substrate according to claim 28 , wherein the step of removing the temporary substrate includes burning and removing the adhesive layer together with the temporary substrate.
30. 20. The method for manufacturing a semiconductor substrate according to claim 18, further comprising the step of forming a highly doped layer having a higher impurity concentration than the SiC epitaxial growth layer on a C-face of the SiC epitaxial growth layer in contact with the first SiC polycrystalline growth layer.
31. The method for manufacturing a semiconductor substrate according to claim 30, wherein the step of forming the highly doped layer includes an ion implantation step or an autodoping step in epitaxial growth.
32. The method for manufacturing a semiconductor substrate according to claim 18, forming at least a part of a structure constituting a semiconductor element on a C-face of the SiC epitaxial growth layer of the semiconductor substrate; The method for manufacturing a semiconductor device further comprises:
33. 33. The method for manufacturing a semiconductor device according to claim 32, wherein the semiconductor element includes at least one of a SiC Schottky barrier diode, a SiC MOSFET, a SiC bipolar transistor, a SiC diode, a SiC thyristor, and a SiC insulated gate bipolar transistor.
34. The method for manufacturing a semiconductor device according to claim 32 , further comprising the step of peeling off the second SiC polycrystalline growth layer from the graphene layer in the semiconductor substrate on which the semiconductor element structure has been formed.
35. 35. The method for manufacturing a semiconductor device according to claim 34, wherein the step of peeling off the second SiC polycrystalline growth layer from the graphene layer further includes the step of heating a Si-face of the second SiC polycrystalline growth layer.
36. 35. The method for manufacturing a semiconductor device according to claim 34, wherein the step of peeling off the second SiC polycrystalline growth layer from the graphene layer further includes the step of cooling a Si-face of the second SiC polycrystalline growth layer.
37. 35. The method for manufacturing a semiconductor device according to claim 34, wherein the step of peeling off the second SiC polycrystalline growth layer from the graphene layer further includes the step of scanning a Si-face of the second SiC polycrystalline growth layer with an ultrasonic oscillator.
38. 35. The method for manufacturing a semiconductor device according to claim 34, wherein the step of peeling off the second SiC polycrystalline growth layer from the graphene layer further includes the step of forcing a cleavage blade between the graphene layer and the second SiC polycrystalline growth layer to cause cleavage.
39. A SiC epitaxial growth layer; a first SiC polycrystalline growth layer disposed on a Si face of the SiC epitaxial growth layer; a graphene layer disposed on the first SiC polycrystalline growth layer; a second SiC polycrystalline growth layer disposed on the graphene layer; A semiconductor substrate comprising:
40. The semiconductor wafer according to claim 39 , wherein the graphene layer has a single-layer structure or a multi-layer laminate structure of graphene.
41. The semiconductor wafer of claim 39 , wherein the SiC epitaxial growth layer further includes a highly doped layer on a C-plane having a higher impurity concentration than the SiC epitaxial growth layer.
42. A semiconductor device having a semiconductor element structure formed on a C surface of the SiC epitaxial growth layer of the semiconductor substrate according to claim 39.
43. 43. The semiconductor device according to claim 42, wherein the semiconductor element includes at least one of a SiC Schottky barrier diode, a SiC MOSFET, a SiC bipolar transistor, a SiC diode, a SiC thyristor, and a SiC insulated gate bipolar transistor.
Citation Information
Patent Citations
Thin film wafer transfer and structure for electronic devices
US8916451B2
Semiconductor substrate and method for producing same
WO2022158078A1
Semiconductor substrate and method for producing same, and semiconductor device