Composition for forming polarizing film, polarizing film, polarizing plate, and manufacturing method thereof

A composition with controlled solvent evaporation and polymerization initiator molecular weight addresses polymerization initiator sublimation issues, resulting in a polarizing film with enhanced transferability and reduced blocking.

JP2024144145APending Publication Date: 2024-10-11SUMITOMO CHEM CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024022193
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-04
Filing Date
2024-02-16
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The use of high boiling point solvents in polarizing film formation leads to polymerization initiator sublimation, resulting in insufficient curing and reduced transferability and increased blocking of the polarizing film.

Method used

A composition comprising a polymerizable liquid crystal compound with smectic liquid crystal properties, specific organic solvents with controlled boiling points, and a polymerization initiator with a molecular weight of 400 or more, ensuring proper solvent evaporation and polymerization, thereby enhancing transferability and reducing blocking.

Benefits of technology

The composition forms a polarizing film with excellent transferability and reduced blocking, maintaining high orientational order and polarization performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144145000001
    Figure 2024144145000001
  • Figure 2024144145000002
    Figure 2024144145000002
  • Figure 2024144145000003
    Figure 2024144145000003
Patent Text Reader

Abstract

To provide a composition for forming a polarizing film capable of forming a polarizing film with excellent transferability and low blocking.SOLUTION: The composition for forming a polarizing film contains a polymerizable liquid crystal compound exhibiting smectic liquid crystallinity, a dichroic dye, a polymerization initiator, and at least two types of organic solvents. The composition for forming polarizing film contains an organic solvent A in which the molecular weight of the polymerization initiator is 400 or more, and the organic solvent has a boiling point that is -20°C to 50°C higher than the isotropic phase transition temperature of the polymerizable liquid crystal compound, and an organic solvent B that has a boiling point that is 50°C higher than the isotropic phase transition temperature of the polymerizable liquid crystal compound.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition for forming a polarizing film, a polarizing film, a polarizing plate, and a method for producing the same. [Background technology]

[0002] Conventionally, polarizing plates are used in flat panel displays (FPDs) by being attached to image display elements such as liquid crystal cells and organic EL display elements. As such polarizing plates, thin polarizing plates using a polarizing film obtained by applying a polymerizable liquid crystal compound to a substrate and polymerizing the compound are widely known. Such polarizing films formed from polymerizable liquid crystal compounds are generally produced through a process of applying a composition for forming a polarizing film, which contains a polymerizable liquid crystal compound and a dichroic dye together with a solvent, to a substrate such as a resin film to form a coating film, and then heating and drying the coating film to cause a phase transition of the polymerizable liquid crystal compound to a liquid crystal state (for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-139222 A Summary of the Invention [Problem to be solved by the invention]

[0004] The above-mentioned Patent Document 1 discloses the use of a high-boiling point solvent as a solvent in a composition for forming a polarizing film in order to suppress missing dots and alignment defects caused by the precipitation of microcrystals that may occur during the curing of the composition for forming a polarizing film. The present inventors have found that when a polarizing film is formed from a composition for forming a polarizing film containing such a high-boiling point solvent, the polymerization initiator may be sublimated together with the solvent depending on the drying conditions for removing the high-boiling point solvent. If the polymerization initiator is sublimated during the process of forming the polarizing film, it becomes difficult to obtain a sufficiently cured polarizing film, which may cause a decrease in the transferability of the obtained polarizing film and the occurrence of blocking.

[0005] An object of the present invention is to provide a composition for forming a polarizing film, which is capable of forming a polarizing film having excellent transferability and which is less likely to cause blocking. [Means for solving the problem]

[0006] The present inventors have conducted intensive research to solve the above problems and have completed the present invention. That is, the present invention provides the following preferred embodiments. [1] A polymerizable liquid crystal compound exhibiting smectic liquid crystallinity, a dichroic dye, a polymerization initiator, and at least two organic solvents; The molecular weight of the polymerization initiator is 400 or more, The organic solvent includes an organic solvent A having a boiling point that is -20°C or more and 50°C or less higher than the isotropic phase transition temperature of the polymerizable liquid crystal compound, and an organic solvent B having a boiling point that is more than 50°C higher than the isotropic phase transition temperature of the polymerizable liquid crystal compound. [2] The composition for forming a polarizing film according to [1] above, wherein the content of organic solvent A is 51 to 99 parts by mass and the content of organic solvent B is 1 to 49 parts by mass, relative to 100 parts by mass of all organic solvents contained in the composition for forming a polarizing film. [3] The composition for forming a polarizing film according to the above [1] or [2], wherein the organic solvent A is a ketone-based solvent or an aromatic solvent. [4] The composition for forming a polarizing film according to any one of the above [1] to [3], wherein the organic solvent B is a ketone-based solvent or a lactone-based solvent. [5] The composition for forming a polarizing film according to any one of the above [1] to [4], wherein the organic solvent B is a cyclic ketone solvent or a lactone solvent. [6] The composition for forming a polarizing film according to any one of the above [1] to [5], wherein the content of the polymerization initiator having a molecular weight of 400 or more is 1 to 10 parts by mass per 100 parts by mass of the polymerizable liquid crystal compound. [7] A polarizing film which is a cured product of the composition for forming a polarizing film according to any one of the above [1] to [6], in which a polymerizable liquid crystal compound and / or a polymer thereof is oriented in a smectic liquid crystal state. [8] The polarizing film according to [7] above, which exhibits a Bragg peak in X-ray diffraction measurement. [9] A polarizing plate comprising the polarizing film according to [7] or [8] above and a substrate. Effect of the Invention

[0007] According to the present invention, there can be provided a composition for forming a polarizing film, which is capable of forming a polarizing film that has excellent transferability and is less likely to cause blocking. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, the embodiments of the present invention will be described in detail. Note that the scope of the present invention is not limited to the embodiments described here, and various modifications can be made without departing from the spirit of the present invention.

[0009] <Polarizing film forming composition> The polarizing film forming composition of the present invention contains a polymerizable liquid crystal compound having at least one polymerizable group exhibiting smectic liquid crystal properties (hereinafter, also referred to as "polymerizable liquid crystal compound (A)"). By using a polymerizable liquid crystal compound exhibiting smectic liquid crystal properties, a polarizing film having a high degree of alignment order can be formed. The liquid crystal state exhibited by the polymerizable liquid crystal compound (A) is preferably a smectic phase (smectic liquid crystal state). From the viewpoint of realizing a higher degree of alignment order, a high-order smectic phase (high-order smectic liquid crystal state) is more preferable. Here, the high-order smectic phase means a smectic B phase, a smectic D phase, a smectic E phase, a smectic F phase, a smectic G phase, a smectic H phase, a smectic I phase, a smectic J phase, a smectic K phase, and a smectic L phase. Among these, the smectic B phase, the smectic F phase, and the smectic I phase are more preferable. The liquid crystal property may be thermotropic or lyotropic, but thermotropic liquid crystal is preferred because it allows precise control of the film thickness. The polymerizable liquid crystal compound may be a monomer, or may be an oligomer or polymer in which a polymerizable group is polymerized.

[0010] The polymerizable liquid crystal compound (A) is a liquid crystal compound having at least one polymerizable group. Here, the polymerizable group refers to a group that can participate in a polymerization reaction by a reactive species generated from a polymerization initiator, such as an active radical or an acid. The polymerizable group of the polymerizable liquid crystal compound (A) is preferably a photopolymerizable group, such as a vinyl group, a vinyloxy group, a 1-chlorovinyl group, an isopropenyl group, a 4-vinylphenyl group, an acryloyloxy group, a methacryloyloxy group, an oxiranyl group, an oxetanyl group, etc. Among them, a radical polymerizable group is preferable, an acryloyloxy group, a methacryloyloxy group, a vinyl group, a vinyloxy group are more preferable, and an acryloyloxy group and a methacryloyloxy group are more preferable.

[0011] The polymerizable liquid crystal compound (A) is not particularly limited as long as it is a polymerizable liquid crystal compound exhibiting smectic liquid crystallinity, and any known polymerizable liquid crystal compound can be used. Examples of such polymerizable liquid crystal compounds include a compound represented by formula (A1) (hereinafter, also referred to as "polymerizable liquid crystal compound (A1)"). U 1 -V 1 -W 1 -(X 1 -Y 1 ) n -X 2 -W 2 -V 2 -U 2 (A1)

[0012] In formula (A1), X 1 and X 2 represent, independently of each other, a divalent aromatic group or a divalent alicyclic hydrocarbon group, in which a hydrogen atom contained in the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with a substituent selected from the group consisting of a halogen atom, an alkyl group having 1 to 4 carbon atoms, a fluoroalkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, and a nitro group, and a carbon atom constituting the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with an oxygen atom, a sulfur atom, or a nitrogen atom. 1 and X 2At least one of the groups is a 1,4-phenylene group which may have the above-mentioned substituent, or a cyclohexane-1,4-diyl group which may have the above-mentioned substituent. Y 1 is a single bond or a divalent linking group. n is 1 to 3. If n is 2 or more, multiple X 1 may be the same or different. X 2 is multiple X 1 In addition, when n is 2 or more, a plurality of Y 1 may be the same as or different from each other. From the viewpoint of liquid crystallinity, n is preferably 2 or more. U 1 represents a hydrogen atom or a polymerizable group. U 2 represents a polymerizable group. W 1 and W 2 are each independently a single bond or a divalent linking group. V 1 and V 2 each independently represents an alkanediyl group having 1 to 20 carbon atoms which may have a substituent, and -CH2- constituting the alkanediyl group may be replaced by -O-, -CO-, -S- or NH-.

[0013] In the polymerizable liquid crystal compound (A1), X 1 and X 2 are each independently preferably an optionally substituted 1,4-phenylene group or an optionally substituted cyclohexane-1,4-diyl group; X 1 and X 2At least one of the groups is a 1,4-phenylene group which may have a substituent, or a cyclohexane-1,4-diyl group which may have a substituent, and is preferably a trans-cyclohexane-1,4-diyl group. Examples of the optional substituent of the 1,4-phenylene group which may have a substituent, or the cyclohexane-1,4-diyl group which may have a substituent, include an alkyl group having 1 to 4 carbon atoms such as a methyl group, an ethyl group, and a butyl group, a cyano group, and a halogen atom such as a chlorine atom or a fluorine atom. It is preferably unsubstituted.

[0014] The polymerizable liquid crystal compound (A1) is a compound represented by the formula (A1-1): -(X 1 -Y 1 ) n -X 2 - (A1-1) [In the formula, X 1 , Y 1 , X 2 and n have the same meanings as above. [hereinafter referred to as partial structure (A1-1)] is preferably asymmetric in that smectic liquid crystallinity is easily exhibited. Examples of the polymerizable liquid crystal compound (A1) in which the partial structure (A1-1) is an asymmetric structure include n is 1 and one X 1 and X 2 and (A1) are different structures from each other. n is 2 and there are two Y 1 A compound in which two Xs are the same structure. 1 are identical in structure to each other, and one X 2 These two X 1 A polymerizable liquid crystal compound (A1) having a structure different from that of Two X's 1 Of the W 1 X binds to 1 But the other X 1 and X 2 The structure is different from that of the other X 1 and X 2and the polymerizable liquid crystal compound (A1) each having the same structure. n is 3 and there are three Y 1 A compound in which three Xs are the same structure as each other. 1 and one X 2 The polymerizable liquid crystal compound (A1) includes any one of the following three structures different from all of the other three structures.

[0015] Y 1 are -CH2CH2-, -CH2O-, -CH2CH2O-, -COO-, -OCOO-, single bond, -N=N-, -CR a =CR b -, -C≡C-, -CR a =N- or -CO-NR a - is preferred. a and R b each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 1 is more preferably -CH2CH2-, -COO- or a single bond, 1 If present, X 2 Y that binds to 1 is more preferably -CH2CH2- or CH2O-. 1 and X 2 When all of Y are the same structure, two or more Y 1 It is preferable that there is a plurality of Y 1 When the compound has a structure of asymmetric structure, the compound tends to exhibit smectic liquid crystallinity.

[0016] U 2 is a polymerizable group. 1 is a hydrogen atom or a polymerizable group, and is preferably a polymerizable group. 1 and U 2 Preferably, both are polymerizable groups, and preferably both are radically polymerizable groups. Examples of the polymerizable group include the same groups as those exemplified above as the polymerizable group contained in the polymerizable liquid crystal compound (A). 1 and a polymerizable group represented by U 2The polymerizable groups represented by may be different from each other, but are preferably the same type of group. The polymerizable groups may be in a polymerized state or an unpolymerized state, but are preferably in an unpolymerized state.

[0017] V 1 and V 2 Examples of the alkanediyl group represented by the formula (I) include a methylene group, an ethylene group, a propane-1,3-diyl group, a butane-1,3-diyl group, a butane-1,4-diyl group, a pentane-1,5-diyl group, a hexane-1,6-diyl group, a heptane-1,7-diyl group, an octane-1,8-diyl group, a decane-1,10-diyl group, a tetradecane-1,14-diyl group, and an icosane-1,20-diyl group. 1 and V 2 is preferably an alkanediyl group having 2 to 12 carbon atoms, and more preferably an alkanediyl group having 6 to 12 carbon atoms.

[0018] Examples of the substituent that the alkanediyl group may have include a cyano group and a halogen atom. The alkanediyl group is preferably unsubstituted, and more preferably an unsubstituted linear alkanediyl group.

[0019] W 1 and W 2 are each independently preferably a single bond, -O-, -S-, -COO- or -OCOO-, more preferably a single bond or -O-.

[0020] As a structure that is likely to exhibit smectic liquid crystal properties, it is preferable that the polymerizable liquid crystal compound has an asymmetric molecular structure in the molecular structure, and specifically, a polymerizable liquid crystal compound having a structure represented by the following formulae (Aa) to (Ai) is likely to exhibit smectic liquid crystal properties and is suitable as the polymerizable liquid crystal compound (A). Furthermore, from the viewpoint of being likely to exhibit high-order smectic liquid crystal properties, it is more preferable that the polymerizable liquid crystal compound has a structure represented by formula (Aa), formula (Ab) or formula (Ac). In the following formulae (Aa) to (Ai), * represents a bond (single bond).

[0021] [ka]

[0022] Specific examples of the polymerizable liquid crystal compound (A1) include compounds represented by formulae (A-1) to (A-25). When the polymerizable liquid crystal compound (A1) has a cyclohexane-1,4-diyl group, the cyclohexane-1,4-diyl group is preferably a trans isomer.

[0023] [ka]

[0024] [ka]

[0025] [ka]

[0026] Among these, at least one selected from the group consisting of compounds represented by formula (A-2), formula (A-3), formula (A-4), formula (A-5), formula (A-6), formula (A-7), formula (A-8), formula (A-13), formula (A-14), formula (A-15), formula (A-16) and formula (A-17) is preferred. As the polymerizable liquid crystal compound (A1), one type may be used alone, or two or more types may be used in combination.

[0027] The polymerizable liquid crystal compound (A1) can be produced by a known method such as that described in Lub et al., Recl. Trav. Chim. Pays-Bas, 115, 321-328 (1996) or Japanese Patent No. 4,719,156.

[0028] The polarizing film-forming composition of the present invention may contain a polymerizable liquid crystal compound other than the polymerizable liquid crystal compound (A) as long as the effect of the present invention is not impaired. From the viewpoint of obtaining a polarizing film with a high degree of orientation order, the proportion of the polymerizable liquid crystal compound (A) to the total mass of all polymerizable liquid crystal compounds in the polarizing film-forming composition is preferably 51 mass % or more, more preferably 70 mass % or more, and even more preferably 90 mass % or more of the polymerizable liquid crystal compounds are the polymerizable compound (A), and all (100 mass %) may be the polymerizable liquid crystal compound (A).

[0029] When the composition for forming a polarizing film of the present invention contains two or more polymerizable liquid crystal compounds (A), it is preferable that at least one of them is the polymerizable liquid crystal compound (A1), and all of the compounds contained in the composition for forming a polarizing film may be the polymerizable liquid crystal compound (A1).

[0030] The content of the polymerizable liquid crystal compound in the composition for forming a polarizing film of the present invention is preferably 40 to 99.9 mass %, more preferably 60 to 99.9 mass %, and further preferably 70 to 99 mass %, based on the solid content of the composition for forming a polarizing film. When the content of the polymerizable liquid crystal compound is within the above range, the orientation of the polymerizable liquid crystal compound tends to be high. In this specification, the solid content refers to the total amount of components excluding the solvent from the composition for forming a polarizing film.

[0031] The polarizing film forming composition of the present invention contains a dichroic dye. Here, the dichroic dye means a dye having different absorbance in the long axis direction and absorbance in the short axis direction of the molecule. The dichroic dye that can be used in the present invention is not particularly limited as long as it has the above-mentioned properties, and may be a dye or a pigment. Two or more dyes or pigments may be used in combination, or a dye and a pigment may be used in combination. The dichroic dye may be used alone or in combination, but in order to obtain absorption in the entire visible light range, it is preferable to combine two or more dichroic dyes, and more preferably to combine three or more dichroic dyes. In particular, by mixing two or more dichroic dyes having different absorption wavelengths, polarizing films of various hues can be produced, and a polarizing film having absorption in the entire visible light range can be obtained.

[0032] The dichroic dye preferably has the property of absorbing visible light, and has a maximum absorption wavelength (λ ) in the range of 300 to 700 nm. MAX ) is preferred. Examples of such dichroic dyes include acridine dyes, oxazine dyes, cyanine dyes, naphthalene dyes, azo dyes, and anthraquinone dyes. Among these, azo dyes are preferred.

[0033] Examples of azo dyes include monoazo dyes, bisazo dyes, trisazo dyes, tetrakisazo dyes, and stilbene azo dyes. Bisazo dyes and trisazo dyes are preferred, and examples thereof include a compound represented by formula (I) (hereinafter also referred to as "compound (I)").

[0034] K 1 (-N=NK 2 ) p -N=NK 3 (I) [In formula (I), K 1 and K. 3 each independently represents a phenyl group which may be substituted, a naphthyl group which may be substituted, a phenyl benzoate group which may be substituted, or a monovalent heterocyclic group which may be substituted. 2represents a p-phenylene group which may have a substituent, a naphthalene-1,4-diyl group which may have a substituent, a 4,4'-stilbenylene group which may have a substituent, or a divalent heterocyclic group which may have a substituent. p represents an integer of 0 to 4. When p is an integer of 2 or more, a plurality of K 2 may be the same or different. The -N=N- bond may be replaced with a -C=C-, -COO-, -NHCO-, or -N=CH- bond as long as the compound exhibits absorption in the visible region.

[0035] Examples of monovalent heterocyclic groups include groups in which one hydrogen atom has been removed from a heterocyclic compound such as quinoline, thiazole, benzothiazole, thienothiazole, imidazole, benzimidazole, oxazole, benzoxazole, etc. Examples of divalent heterocyclic groups include groups in which two hydrogen atoms have been removed from the above-mentioned heterocyclic compounds.

[0036] K 1 and K. 3 Phenyl, naphthyl, phenyl benzoate and monovalent heterocyclic groups in 2 In the above formula, examples of the substituents that the p-phenylene group, the naphthalene-1,4-diyl group, the 4,4'-stilbenylene group, and the divalent heterocyclic group may optionally have include an alkyl group having 1 to 20 carbon atoms, an alkyl group having 1 to 20 carbon atoms and having a polymerizable group, an alkenyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, such as a methoxy group, an ethoxy group, or a butoxy group, an alkoxy group having 1 to 20 carbon atoms and having a polymerizable group, a fluorinated alkyl group having 1 to 4 carbon atoms, such as a trifluoromethyl group, Examples of the amino group include an ano group, a nitro group, a halogen atom, and a substituted or unsubstituted amino group such as an amino group, a diethylamino group, or a pyrrolidino group (the substituted amino group means an amino group having one or two alkyl groups having 1 to 6 carbon atoms, an amino group having one or two alkyl groups having 1 to 6 carbon atoms and a polymerizable group, or an amino group in which two substituted alkyl groups are bonded to each other to form an alkanediyl group having 2 to 8 carbon atoms. An unsubstituted amino group is -NH2). Examples of the polymerizable group include a (meth)acryloyl group and a (meth)acryloyloxy group.

[0037] Among the compounds (I), compounds represented by any one of the following formulas (I-1) to (I-8) are preferred. [ka] [In the formulas (I-1) to (I-8), B 1 ~B 30 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, a nitro group, a substituted or unsubstituted amino group (the substituted amino group and the unsubstituted amino group are defined above), a chlorine atom, or a trifluoromethyl group. n1 to n4 each independently represent an integer of 0 to 3. If n1 is 2 or more, multiple B 2 may be the same or different, If n2 is 2 or more, multiple B 6 may be the same or different, If n3 is 2 or more, multiple B 9 may be the same or different, If n4 is 2 or more, multiple B 14 may be the same or different.]

[0038] The anthraquinone dye is preferably a compound represented by formula (I-9). [ka] [In formula (I-9), R 1 ~R 8 are each independently a hydrogen atom, -R x , -NH2, -NHR x , -NR x 2, -SR x Or a halogen atom. R x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.

[0039] The oxazone dye is preferably a compound represented by formula (I-10). [ka] [In formula (I-10), R 9 ~R 15 are each independently a hydrogen atom, -R x , -NH2, -NHR x , -NR x 2, -SR x Or a halogen atom. R x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.

[0040] The acridine dye is preferably a compound represented by formula (I-11). [ka] [In formula (I-11), R 16 ~R 23 are each independently a hydrogen atom, -R x , -NH2, -NHR x , -NR x 2, -SR x Or a halogen atom. R x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms. In formula (I-9), formula (I-10) and formula (I-11), R x Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, and a hexyl group, and examples of the aryl group having 6 to 12 carbon atoms include a phenyl group, a toluyl group, a xylyl group, and a naphthyl group.

[0041] As the cyanine dye, the compounds represented by formula (I-12) and formula (I-13) are preferred. [ka] [In formula (I-12), D 1 and D. 2 represent, independently of each other, a group represented by any one of formulae (I-12a) to (I-12d). [ka] n5 represents an integer from 1 to 3. [ka] [In formula (I-13), D 3 and D. 4 each independently represents a group represented by any one of formulas (1-13a) to (1-13h). [ka] n6 represents an integer from 1 to 3.

[0042] The content of the dichroic dye in the composition for forming a polarizing film of the present invention can be appropriately determined depending on the type of the dichroic dye used, and is preferably 1 to 60 mass %, more preferably 1 to 20 mass %, and further preferably 1 to 15 mass % based on the solid content of the composition for forming a polarizing film. When the content of the dichroic dye is within the above range, the orientation of the polymerizable liquid crystal compound is unlikely to be disturbed, and a polarizing film having a high degree of orientation order can be obtained.

[0043] The polarizing film forming composition of the present invention contains at least two kinds of organic solvents. The two kinds of organic solvents include at least an organic solvent A having a boiling point that is -20°C to 50°C higher than the isotropic phase transition temperature of the polymerizable liquid crystal compound, and an organic solvent B having a boiling point that is more than 50°C higher than the isotropic phase transition temperature of the polymerizable liquid crystal compound. The process of forming a polarizing film usually includes a step of heating and drying a coating film of the polarizing film forming composition to cause a phase transition of the polymerizable liquid crystal compound to a liquid crystal state (hereinafter, also referred to as a "heat drying step"). In this step, if the solvent evaporates from the coating film before the polymerizable liquid crystal compound undergoes a phase transition to a liquid crystal state, the polymerizable liquid crystal compound is likely to precipitate as microcrystals. If microcrystals are precipitated, it is difficult to obtain a good mixed and inclusive state of the polymerizable liquid crystal compound and the dichroic dye in the subsequent heat drying step, which causes dot missing in the obtained polarizing film. Such precipitation of microcrystals is considered to be due to the fact that smectic liquid crystals have a structure closer to crystals than general nematic liquid crystals, and may be particularly problematic in polarizing films formed from polymerizable liquid crystal compounds exhibiting smectic liquid crystallinity. The polarizing film-forming composition of the present invention contains at least two organic solvents having different boiling points, which can prevent the organic solvent from volatilizing before the heat-drying step, and can facilitate the removal of the organic solvent in the heat-drying step. This can suppress the occurrence of missing dots even when using a polymerizable liquid crystal compound exhibiting smectic liquid crystallinity, and can also suppress uneven drying in the heat-drying step. When the polarizing film-forming composition of the present invention contains two or more polymerizable liquid crystal compounds, the organic solvents A and B are selected based on the isotropic phase transition temperatures of the polymerizable liquid crystal compounds contained in the polarizing film-forming composition in a mixed state.

[0044] The organic solvent A usually dissolves the polymerizable liquid crystal compound, the dichroic dye, and the polymerization initiator, and facilitates the formation of a good mixed inclusion state of the polymerizable liquid crystal compound and the dichroic dye in the coating film, and also functions to adjust the solid content concentration and viscosity of the composition for forming a polarizing film. In particular, compounds exhibiting smectic liquid crystallinity generally tend to have high viscosity, and the inclusion of the organic solvent A in the composition for forming a polarizing film improves the handleability of the composition, which results in the formation of a polarizing film. In order to suppress the organic solvent from volatilizing from the coating film before the heat drying process of the coating film of the composition for forming a polarizing film, the boiling point of the organic solvent A is higher by −20° C. to 50° C. than the isotropic phase transition temperature of the polymerizable liquid crystal compound contained in the composition for forming a polarizing film, preferably higher by 0° C. to 50° C., more preferably higher by 10° C. to 50° C., and even more preferably higher by 20° C. to 40° C. If the boiling point of the organic solvent A is lower than the isotropic phase transition temperature of the polymerizable liquid crystal compound by more than -20°C, the organic solvent is likely to volatilize before the heat drying process, and the microcrystals of the polymerizable liquid crystal compound are likely to precipitate. If the boiling point of the organic solvent A is higher than the isotropic phase transition temperature of the polymerizable liquid crystal compound by more than 50°C, the solvent is unlikely to volatilize in the heat drying process, and alignment defects and drying unevenness are likely to occur. At the same time, if the boiling point of the organic solvent A is within a preferred range, the amount of solvent remaining after the heat drying process can be reduced, and therefore the decrease in transferability and the occurrence of blocking due to the remaining solvent can be suppressed. The organic solvent A may be used alone or in combination of two or more.

[0045] The organic solvent B is a high boiling point solvent, and has a function of providing a moisturizing effect to the coating film before the heat drying process. From the viewpoint of suppressing volatilization from the coating film before the heat drying process, the boiling point of the organic solvent B is higher than the isotropic phase transition temperature of the polymerizable liquid crystal compound contained in the composition for forming a polarizing film by more than 50°C, preferably 55°C or higher, and preferably 150°C or lower, more preferably 60°C or higher and 150°C or lower, more preferably 60°C or higher and 130°C or lower, even more preferably 60°C or higher and 120°C or lower, and particularly preferably 60°C or higher and 110°C or lower. By including the organic solvent B having a boiling point higher than the isotropic phase transition temperature of the polymerizable liquid crystal compound in the above range, it is possible to effectively suppress the organic solvent from volatilizing from the coating film before the heat drying process, and it is possible to maintain a good mixed and inclusive state of the polymerizable liquid crystal compound and the dichroic dye in the coating film. This effectively suppresses the occurrence of missing dots in the obtained polarizing film. In addition, by selecting an organic solvent having a boiling point equal to or lower than the upper limit in relation to the isotropic phase transition temperature of the polymerizable liquid crystal compound as organic solvent B, the removability of organic solvent B in the heat drying step is improved, so that drying unevenness is unlikely to occur, and the transferability and blocking suppression effect of the obtained polarizing film can be improved. Organic solvent B may be used alone or in combination of two or more.

[0046] The difference between the boiling point of organic solvent A and the boiling point of organic solvent B is preferably 20° C. or more, more preferably 30° C. or more, and preferably 120° C. or less, more preferably 100° C. or less, and even more preferably 90° C. or less. When the boiling points of organic solvents A and B satisfy the above relationship, it is easy to achieve a balance between the effect of suppressing the generation of microcrystals of the polymerizable liquid crystal compound before the heat drying step of the coating film of the composition for forming a polarizing film and the effect of facilitating removal of the solvent in the heat drying step, so that the resulting polarizing film is less likely to have defects such as missing dots, and the effect of suppressing drying unevenness and the transferability and blocking suppression effect of the resulting polarizing film can be further improved.

[0047] The organic solvents A and B can be appropriately selected from known organic solvents capable of dissolving each component constituting the composition for forming a polarizing film, based on the isotropic phase transition temperature of the polymerizable liquid crystal compound, depending on the polymerizable liquid crystal compound, dichroic dye, polymerization initiator, etc. used. Examples of the organic solvent include the following solvents: Ketone solvents such as methyl isobutyl ketone (116°C), cyclohexanone (156°C), cyclopentanone (131°C), cycloheptanone (180°C), methyl amyl ketone (151°C), isophorone (215°C), piperitone (235°C), etc.; Lactone solvents such as gamma-butyrolactone (GBL) (204°C); Aromatic solvents such as o-xylene (144°C), m-xylene (139°C), p-xylene (138°C), mesitylene (165°C), cumene (152°C), ethylbenzene (136°C), anisole (154°C), aniline (184°C), benzaldehyde (178°C), benzyl alcohol (205°C), methyl benzoate (199°C), ethyl benzoate (213°C), propyl benzoate (230°C), butyl benzoate (250°C), nitrobenzene (211°C), and tetralin (207°C); Long-chain hydrocarbon solvents such as octane (125°C), nonane (151°C), decane (174°C), undecane (196°C), and dodecane (216°C); Ethylene glycol monomethyl ether (124°C), ethylene glycol monoethyl ether (202°C), ethylene glycol-n-propyl ether (151°C), ethylene glycol-i-propyl ether (141°C), ethylene glycol-n-butyl ether (171°C), ethylene glycol monomethyl ether (124°C), diethylene glycol dimethyl ether (162°C), diethylene glycol diethyl ether (189°C), dipropylene glycol dimethyl ether (171°C), diethylene glycol monomethyl ether (194°C), diethylene glycol monoethyl ether (202°C), diethylene glycol monobutyl ether (230°C), diethylene glycol ethyl methyl ether (176°C), diethylene glycol butyl methyl ether (212°C), propylene glycol monomethyl ether glycol solvents such as propylene glycol dimethyl ether (120°C), dipropylene glycol monomethyl ether (188°C), dipropylene glycol dimethyl ether (171°C), propylene glycol dimethyl ether (97°C), tripropylene glycol dimethyl ether (215°C), triethylene glycol monomethyl ether (249°C), triethylene glycol dimethyl ether (216°C), tetraethylene glycol dimethyl ether (276°C), propylene glycol monomethyl ether acetate (146°C), ethylene glycol monomethyl ether acetate (145°C), ethylene glycol monomethyl ether acetate (145°C), diethylene glycol monoethyl ether acetate (217°C), and diethylene glycol monobutyl ether acetate (245°C); Ester solvents such as propyl acetate (102°C), butyl acetate (126°C), amyl acetate (149°C), ethyl lactate (155°C), methyl methoxypropionate (143°C), ethyl ethoxypropionate (170°C), isoamyl propionate (156°C), isoamyl isobutyrate (179°C), ethyl butyrate (121°C), propyl butyrate (143°C), butyl butyrate (165°C), ethylene carbonate (244°C), and propylene carbonate (242°C); Amide solvents such as N,N-dimethylformamide (153°C), N,N-dimethylacetamide (165°C), N-methylpyrrolidone (202°C), and γ-butyrolactam (245°C); and Halogen-based solvents such as chlorobenzene (131°C) and 1,1,2,2-tetrachloroethane (147°C).

[0048] It is more advantageous to select an organic solvent A having high solubility for the polymerizable liquid crystal compound, the dichroic dye, and the polymerization initiator. In a preferred embodiment of the present invention, the organic solvent A is preferably a ketone solvent or an aromatic solvent, and more preferably an aromatic solvent.

[0049] As the organic solvent B, it is more advantageous to select one having a high boiling point relative to the isotropic phase transition temperature of the polymerizable liquid crystal compound and high solubility in the polymerizable liquid crystal compound, the dichroic dye, and the polymerization initiator. In a preferred embodiment of the present invention, the organic solvent B is preferably a ketone solvent or a lactone solvent, more preferably a cyclic ketone solvent or a lactone solvent. When a ketone solvent or an aromatic solvent, preferably an aromatic solvent, is used as the organic solvent A, and a ketone solvent or a lactone solvent, preferably a cyclic ketone solvent or a lactone solvent, is used as the organic solvent B, it is easy to balance the effect of suppressing the generation of microcrystals of the polymerizable liquid crystal compound before the heat drying process of the coating film of the polarizing film forming composition and the effect of easiness of removal of the solvent in the heat drying process. This can further expect the effect of suppressing the generation of drying unevenness, missing dots, and / or blocking, and the effect of improving transferability.

[0050] The content of organic solvent A in the polarizing film-forming composition of the present invention is preferably higher than the content of organic solvent B. The content of organic solvent A is preferably 51 to 99 parts by mass, more preferably 60 parts by mass or more, even more preferably 70 parts by mass or more, particularly preferably 80 parts by mass or more, and more preferably 95 parts by mass or less, and even more preferably 90 parts by mass or less, relative to 100 parts by mass of all organic solvents contained in the polarizing film-forming composition. The content of organic solvent B is preferably 1 to 49 parts by mass, more preferably 5 parts by mass or more, even more preferably 10 parts by mass or more, and more preferably 40 parts by mass or less, even more preferably 30 parts by mass or less, and especially preferably 20 parts by mass or less, relative to 100 parts by mass of all organic solvents contained in the polarizing film-forming composition. When the organic solvents A and B are contained within the above content ranges, the evaporation of the solvent is suppressed in the coating film before the heat drying process, so that a good mixed inclusion state of the polymerizable liquid crystal compound and the dichroic dye can be obtained, and the heat drying process does not require excessive heating, and the solvent can be sufficiently removed even at a temperature near the phase transition temperature of the polymerizable liquid crystal compound. This makes it difficult for missing dots to occur, and also suppresses the occurrence of drying unevenness and blocking, thereby improving transferability. When two or more types of organic solvent A and / or organic solvent B are contained, the above content means the total amount of organic solvent A and / or organic solvent B. The polarizing film forming composition of the present invention may contain organic solvents other than organic solvents A and B, as long as the effect of the present invention is not impaired.

[0051] The composition for forming a polarizing film of the present invention preferably contains an organic solvent in an amount such that the solid content is 5 to 40% by mass. In other words, the content of the organic solvent in the composition for forming a polarizing film of the present invention (the total amount of organic solvents A and B, and other organic solvents if contained) is preferably 60 to 95% by mass based on the total mass of the composition for forming a polarizing film. When the content of the organic solvent is within the above range, it is possible to suppress the volatilization of the solvent in the coating film before heat drying, and in the heat drying step, it is easy to dry and remove the solvent without heating more than necessary, and the amount of residual solvent can be reduced. This can further improve the effects of the present invention.

[0052] The composition for forming a polarizing film of the present invention contains a polymerization initiator having a molecular weight of 400 or more. The present inventors have found that when the composition for forming a polarizing film contains a high-boiling point solvent as described above, the polymerization initiator can be sublimated in the same manner as the organic solvent under the heating and drying conditions (drying temperature and time) for removing the high-boiling point solvent. If the polymerization initiator is sublimated during the process of forming the polarizing film, the polymerization of the polymerizable liquid crystal compound does not proceed sufficiently, making it difficult to obtain a polarizing film that is sufficiently cured. This causes a decrease in the transferability of the obtained polarizing film and the occurrence of blocking during storage in a rolled state or the like. As described above, by adjusting the combination of organic solvent A and organic solvent B, it is possible to suppress uneven drying caused by the remaining amount of organic solvents, particularly organic solvent B, which is a high-boiling point solvent, during the heating and drying process. However, it was difficult to sufficiently improve the transferability of the polarizing film and suppress blocking by only adjusting the combination of organic solvent A and organic solvent B. The present inventors have found that by including organic solvent A and organic solvent B having different boiling points in relation to the isotropic phase transition temperature of the polymerizable liquid crystal compound and controlling the molecular weight of the polymerization initiator, it is possible to obtain a high transferability and blocking suppression effect that is difficult to achieve by only selecting a combination of organic solvents. The reason for obtaining such an effect is not necessarily limited to this, but it is considered that a relatively large polymerization initiator such as one having a molecular weight of 400 or more is difficult to sublimate even at high temperatures, and it is possible to retain a necessary and sufficient polymerization initiator from the coating of the polarizing film-forming composition to obtaining a cured film (polarizing film), and the polymerization of the polymerizable liquid crystal compound proceeds sufficiently to obtain a firmly cured polarizing film. A polarizing film-forming composition using such a polymerization initiator having a molecular weight of 400 or more is also advantageous in that a sufficiently cured polarizing film can be obtained without increasing the amount of the polymerization initiator. The molecular weight of the polymerization initiator is preferably 2000 or less, more preferably 1500 or less, and even more preferably 1000 or less. If the weight-average molecular weight of the polymerization initiator exceeds the upper limit and becomes too large, it becomes difficult to align with the polymerizable liquid crystal compound, and the dichroic dye present in a state of being included in the polymerizable liquid crystal compound tends to be easily denatured. If the weight-average molecular weight of the polymerization initiator is equal to or less than the upper limit, the orientation disorder of the polymerizable liquid crystal compound caused by the polymerization initiator can be suppressed, and a polarizing film having excellent polarization performance and maintaining a high degree of orientation order can be obtained.

[0053] In the present invention, the polymerization initiator has an important feature of having a molecular weight of 400 or more, and a photopolymerization initiator is preferred because it can initiate a polymerization reaction under lower temperature conditions. Specifically, photopolymerization initiators capable of generating active radicals or acids under the action of light are included, and among these, photopolymerization initiators that generate radicals under the action of light are preferred. The polymerization initiators can be used alone or in combination of two or more kinds.

[0054] The polymerization initiator is not particularly limited as long as it has a molecular weight of 400 or more, and a known polymerization initiator can be appropriately selected and used. For example, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (molecular weight 419), 1,2-octanedione, 1-[4-(phenylthio)-,2-(O-benzoyloxime)] (molecular weight 446), ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-,1-(O-acetyloxime) (molecular weight 413), etc. can be mentioned. In addition, a commercially available polymerization initiator may be used, for example, Esacure one, Esacure KIP150, Esacure 1001M, Omnirad 819 (all manufactured by IGM Resins), Irgacure OXE-01, Irgacure OXE-02 (both manufactured by BASF Japan), etc. can be used.

[0055] The upper limit of the molecular weight of the polymerization initiator is not particularly limited, and may be, for example, 1000 or less. In addition, in this specification, when the polymerization initiator is a polymer (oligomer or polymer), its "molecular weight" means a weight average molecular weight. In this specification, the molecular weight of the polymerization initiator is a value calculated from the structure of the polymerization initiator, and when the molecular weight is a weight average molecular weight, it means a weight average molecular weight in terms of polystyrene measured by gel permeation chromatography, or when a commercially available product is used as the polymerization initiator, the molecular weight described in the product specification, catalog, etc. may be used.

[0056] In the composition for forming a polarizing film of the present invention, the content of the polymerization initiator having a molecular weight of 400 or more is preferably 1 to 10 parts by mass, more preferably 1.5 to 8 parts by mass, and even more preferably 2 to 5 parts by mass, based on 100 parts by mass of the polymerizable liquid crystal compound. When the content of the polymerization initiator having a molecular weight of 400 or more is within the above range, a polarizing film having excellent transferability and little blocking even during storage in a rolled state or the like can be formed. In addition, the polymerization reaction of the polymerizable liquid crystal compound can be carried out without significantly disturbing the orientation of the polymerizable liquid crystal compound, and a polarizing film having excellent polarization performance while maintaining a high degree of orientation order can be obtained.

[0057] The polarizing film-forming composition of the present invention may contain other polymerization initiators having a molecular weight of less than 400 (hereinafter, also referred to as "other polymerization initiators"), so long as the effects of the present invention are not impaired. As the other polymerization initiators, polymerization initiators having a molecular weight of less than 400 that have been conventionally used in the field can be used. For example, as photopolymerization initiators that generate active radicals, self-cleavage type benzoin compounds, acetophenone compounds, hydroxyacetophenone compounds, α-aminoacetophenone compounds, oxime ester compounds, acylphosphine oxide compounds, etc. and azo-based compounds; hydrogen-abstraction-type photopolymerization initiators such as benzophenone-based compounds, benzoin ether-based compounds, benzyl ketal-based compounds, dibenzosuberone-based compounds, anthraquinone-based compounds, xanthone-based compounds, thioxanthone-based compounds, halogenoacetophenone-based compounds, dialkoxyacetophenone-based compounds, halogenobisimidazole-based compounds, halogenotriazine-based compounds, and triazine-based compounds; and acid-generating photopolymerization initiators such as iodonium salts and sulfonium salts.

[0058] In the composition for forming a polarizing film of the present invention, the content of the polymerization initiator other than the polymerization initiator having a molecular weight of 400 or more is preferably 2 parts by mass or less, more preferably 1 part by mass or less, and even more preferably 0.5 parts by mass or less, relative to 100 parts by mass of the polymerizable liquid crystal compound, so as to ensure the above-mentioned effect obtained by blending a polymerization initiator having a molecular weight of 400 or more and to maintain high alignment order of the polymerizable liquid crystal compound, and it is particularly preferable that no other polymerization initiator is contained. When the composition for forming a polarizing film of the present invention contains other polymerization initiators, it is preferable that the total content of the polymerization initiators is within the range described above as the suitable range for the content of the polymerization initiator having a molecular weight of 400 or more.

[0059] The polarizing film-forming composition of the present invention may contain a leveling agent. The leveling agent is a component that adjusts the fluidity of the polarizing film-forming composition and functions to make the coating film obtained by applying the polarizing film-forming composition flatter. Specifically, a surfactant can be mentioned. As the leveling agent, at least one selected from the group consisting of leveling agents mainly composed of a polyacrylate compound and leveling agents mainly composed of a fluorine atom-containing compound is preferable. The leveling agents can be used alone or in combination of two or more kinds.

[0060] Examples of leveling agents containing a polyacrylate compound as a main component include "BYK-350", "BYK-352", "BYK-353", "BYK-354", "BYK-355", "BYK-358N", "BYK-361N", "BYK-380", "BYK-381" and "BYK-392" (BYK Chemie).

[0061] Leveling agents containing a fluorine atom-containing compound as a main component include "Megafac (registered trademark) R-08", "R-30", "R-90", "F-410", "F-411", "F-443", "F-445", "F-470", "F-471", "F-477", "F-479", "F-482" and "F-483" (DIC Corporation); "Surflon (registered trademark) S-381" and "S-38 2”, “S-383”, “S-393”, “SC-101”, “SC-105”, “KH-40”, and “SA-100” (AGC Seimi Chemical Co., Ltd.); “E1830”, “E5844” (Daikin Fine Chemical Research Institute Ltd.); “F-TOP EF301”, “F-TOP EF303”, “F-TOP EF351”, and “F-TOP EF352” (Mitsubishi Materials Electronic Chemicals Co., Ltd.).

[0062] The content of the leveling agent in the composition for forming a polarizing film of the present invention is preferably 0.05 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, based on 100 parts by mass of the polymerizable liquid crystal compound. When the content of the leveling agent is within the above range, the polymerizable liquid crystal compound is easily horizontally aligned, and unevenness is unlikely to occur, so that a smoother polarizing film tends to be obtained.

[0063] The polarizing film forming composition may further contain a photosensitizer. The use of the photosensitizer can further promote the polymerization reaction of the polymerizable liquid crystal compound. Examples of the photosensitizer include xanthone compounds such as xanthone and thioxanthone (2,4-diethylthioxanthone, 2-isopropylthioxanthone, etc.); anthracene compounds such as anthracene and alkoxy group-containing anthracene (dibutoxyanthracene, etc.); phenothiazine, rubrene, etc. The photosensitizer can be used alone or in combination of two or more kinds.

[0064] The content of the photosensitizer in the composition for forming a polarizing film of the present invention may be appropriately determined depending on the types and amounts of the photopolymerization initiator and the polymerizable liquid crystal compound, and is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound.

[0065] In order to make the polymerization reaction of the composition for forming a polarizing film proceed more stably, the composition may contain an appropriate amount of a polymerization inhibitor, which makes it easier to control the degree of progress of the polymerization reaction of the polymerizable liquid crystal compound.

[0066] Examples of the polymerization inhibitor include radical scavengers such as hydroquinone, alkoxy group-containing hydroquinone, alkoxy group-containing catechol (for example, butylcatechol, etc.), pyrogallol, and 2,2,6,6-tetramethyl-1-piperidinyloxy radical; thiophenols; β-naphthylamines, and β-naphthols.

[0067] When the composition for forming a polarizing film contains a polymerization inhibitor, the content thereof can be appropriately adjusted depending on the type and amount of the polymerizable liquid crystal compound, the amount of the photosensitizer used, etc., but is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound. If the content of the polymerization inhibitor is within this range, the polymerizable liquid crystal compound can be polymerized without disturbing the alignment.

[0068] The polarizing film-forming composition may contain additives other than the leveling agent, the photosensitizer, and the polymerization inhibitor. Examples of the additives include antioxidants, release agents, stabilizers, colorants such as bluing agents, flame retardants, and lubricants. When the polarizing film-forming composition contains other additives, the content of the additives is preferably more than 0% by mass and not more than 20% by mass, more preferably more than 0% by mass and not more than 10% by mass, based on the solid content of the polarizing film-forming composition.

[0069] The solid content of the composition for forming a polarizing film of the present invention is preferably 5 to 40% by mass. When the solid content concentration of the composition for forming a polarizing film is equal to or more than the lower limit, the solvent is prevented from volatilizing before the heat drying process of the coating film of the composition for forming a polarizing film, which prevents the precipitation of microcrystals of the polymerizable liquid crystal compound, and the occurrence of missing dots in the polarizing film can be suppressed. When the solid content is equal to or less than the upper limit, the organic solvent is easily removed in the heat drying process, and drying unevenness is unlikely to occur. Furthermore, since compounds that exhibit smectic liquid crystallinity generally have high viscosity, there is also an advantage that the coating becomes easier by setting the solid content concentration within the above range, and as a result, the polarizing film is easily formed. In the present invention, the solid content of the composition for forming a polarizing film is more preferably 10% by mass or more, even more preferably 15% by mass or more, particularly preferably 20% by mass or more, more preferably 38% by mass or less, and even more preferably 35% by mass or less. The solid content concentration can be adjusted mainly by the amount of the organic solvent and the polymerizable liquid crystal compound blended.

[0070] The composition for forming a polarizing film of the present invention can usually be prepared by mixing and stirring the polymerizable liquid crystal compound, the dichroic dye, the polymerization initiator, and the organic solvent, and, if necessary, the above-mentioned additives.

[0071] The composition for forming a polarizing film of the present invention is capable of producing a polarizing film that is unlikely to cause drying unevenness or missing dots and has excellent transferability. In addition, since it has an excellent effect of suppressing the occurrence of blocking, it is possible to produce a polarizing film that can be stored for a long period of time, for example, in a rolled state. Therefore, the present invention also includes a polarizing film obtained by curing the composition for forming a polarizing film of the present invention (i.e., a cured product of the composition for forming a polarizing film). In the polarizing film of the present invention, the polymerizable liquid crystal compound and / or its polymer that forms the polarizing film is preferably aligned in a smectic liquid crystal state. By being aligned in a smectic liquid crystal state, the polarizing film of the present invention exhibits a high degree of orientation order.

[0072] A polarizing film having a high degree of orientation order exhibits a Bragg peak derived from a higher-order structure such as a hexatic phase or a crystalline phase in X-ray diffraction measurement. The Bragg peak means a peak derived from the planar periodic structure of molecular orientation. A polarizing film formed from the composition for forming a polarizing film of the present invention preferably exhibits a Bragg peak in X-ray diffraction measurement, and more preferably has a "horizontal orientation" in which the polymerizable liquid crystal compound and / or its polymer are molecularly oriented in the direction in which light is absorbed. In the present invention, a polarizing film having a planar periodic spacing of molecular orientation of 3.0 to 6.0 Å is preferred.

[0073] The polarizing film of the present invention can be produced, for example, according to a method for forming a polarizing film in the method for producing a polarizing plate of the present invention described below.

[0074] The present invention is also directed to a polarizing plate comprising the polarizing film of the present invention. In one embodiment of the present invention, the polarizing plate of the present invention includes a substrate in addition to the polarizing film of the present invention. In another embodiment of the present invention, the polarizing film of the present invention includes a layer formed from a composition for forming a polarizing film and an alignment film, and in particular, it is preferable that the polarizing film includes a layer formed from a composition for forming a polarizing film and a photo-alignment film.

[0075] The polarizing plate of the present invention can be produced, for example, by forming a coating film of the composition for forming a polarizing film of the present invention; the coating film is dried by heating to a temperature close to a nematic-isotropic phase transition temperature of the polymerizable liquid crystal compound contained in the composition for forming a polarizing film, and then cooled to cause a phase transition of the polymerizable liquid crystal compound to a smectic liquid crystal phase (smectic liquid crystal state); and The polymerizable liquid crystal compound is polymerized while maintaining the smectic liquid crystal phase (smectic liquid crystal state) to form a polarizing film. The composition can be produced by a method comprising the steps of:

[0076] The coating film of the composition for forming a polarizing film can be formed, for example, by applying the composition for forming a polarizing film onto a substrate, an alignment film described later, etc. In addition, when the polarizing plate of the present invention includes a retardation film or the like, the composition for forming a polarizing film may be directly applied onto the retardation film.

[0077] The substrate is usually a transparent substrate. When the substrate is not placed on the display surface of a display element, for example, when a laminate obtained by removing the substrate from a polarizing film is placed on the display surface of a display element, the substrate does not have to be transparent. The transparent substrate means a substrate having transparency capable of transmitting light, particularly visible light, and the transparency means a property in which the transmittance for light rays having a wavelength of 380 to 780 nm is 80% or more. Specific examples of transparent substrates include light-transmitting resin substrates. Examples of resins constituting the light-transmitting resin substrate include polyolefins such as polyethylene and polypropylene; cyclic olefin resins such as norbornene-based polymers; polyvinyl alcohol; polyethylene terephthalate; polymethacrylic acid esters; polyacrylic acid esters; cellulose esters such as triacetyl cellulose, diacetyl cellulose, and cellulose acetate propionate; polyethylene naphthalate; polycarbonate; polysulfone; polyether sulfone; polyether ketone; polyphenylene sulfide, polyphenylene oxide, and the like. From the viewpoint of availability and transparency, polyethylene terephthalate, polymethacrylic acid ester, cellulose ester, cyclic olefin resin, or polycarbonate is preferred. Cellulose ester is a material in which a part or all of the hydroxyl groups contained in cellulose are esterified, and is easily available on the market. Cellulose ester substrates are also easily available on the market. Commercially available cellulose ester substrates include "FUJITAC FILM" (Fuji Photo Film Co., Ltd.); "KC8UX2M", "KC8UY" and "KC4UY" (Konica Minolta Opto Co., Ltd.).

[0078] If the substrate is too thin, the strength decreases and the processability tends to be poor, so the thickness is usually 5 to 300 μm, preferably 20 to 200 μm, and more preferably 20 to 100 μm.

[0079] Examples of a method for applying the composition for forming a polarizing film to a substrate or the like include known methods such as application methods such as spin coating, extrusion, gravure coating, die coating, bar coating, and applicator methods, and printing methods such as flexography.

[0080] Next, the coating film obtained from the composition for forming a polarizing film is heated to a temperature close to the isotropic phase transition temperature of the polymerizable liquid crystal compound contained in the composition for forming a polarizing film, the solvent is dried and removed, and at the same time, the polymerizable liquid crystal compound is phase-transitioned to a liquid phase, and then the temperature is lowered to cause the polymerizable liquid crystal compound to phase-transition to a smectic phase (smectic liquid crystal state).

[0081] The heating temperature of the coating film can be appropriately determined in consideration of the polymerizable liquid crystal compound used and the material of the film such as the substrate on which the coating film is formed. In order to sufficiently remove the organic solvent and to make the polymerizable liquid crystal compound in an isotropic state while suppressing the influence of heating on the polymerization initiator, the heating temperature in the present invention is preferably at least −7° C. higher than the isotropic phase transition temperature of the polymerizable liquid crystal compound, more preferably at least −5° C. higher, and even more preferably at least −3° C. higher. The upper limit of the heating temperature is preferably 150° C. or lower, more preferably 130° C. or lower, in order to avoid volatilization of the polymerization initiator and damage to the coating film and substrate due to excessive heating.

[0082] The heating time can be appropriately determined depending on the heating temperature, the type of polymerizable liquid crystal compound used, the type and boiling point of the organic solvent, and the amount thereof, but is usually 0.5 to 10 minutes, and preferably 1 to 5 minutes.

[0083] Before heating to the vicinity of the isotropic phase transition temperature of the polymerizable liquid crystal compound, a preliminary drying step may be provided to adequately remove the solvent in the coating film obtained from the film-forming composition under conditions in which the polymerizable liquid crystal compound contained in the coating film does not polymerize. By providing the drying step, the orientation of the polymerizable liquid crystal compound can be improved. Examples of the drying method include natural drying, ventilation drying, heat drying, and reduced pressure drying. The drying temperature (heating temperature) in the drying step can be appropriately determined depending on the type of polymerizable liquid crystal compound used, the type of organic solvent, the boiling point and the amount thereof, etc., but is usually 30 to 150°C, preferably 50 to 130°C, from the viewpoint of suppressing the precipitation of microcrystals of the polymerizable liquid crystal compound. The drying time can be appropriately determined depending on the drying temperature and the type of organic solvent used, etc., but is usually 0.1 to 5 minutes, preferably 0.1 to 3 minutes.

[0084] Next, in the dried coating film obtained by the above heat drying, the polymerizable liquid crystal compound is polymerized while maintaining the smectic liquid crystal state of the polymerizable liquid crystal compound, thereby forming a cured film of the composition for forming a polarizing film as a polarizing film. The polymerization method is preferably a photopolymerization method. In the photopolymerization, the light to be irradiated to the dried coating film is appropriately selected according to the type of photopolymerization initiator contained in the dried coating film, the type of polymerizable liquid crystal compound (particularly, the type of polymerizable group possessed by the polymerizable liquid crystal compound) and the amount thereof. Specific examples thereof include one or more types of light selected from the group consisting of visible light, ultraviolet light, infrared light, X-rays, α-rays, β-rays and γ-rays, and active electron beams. Among them, ultraviolet light is preferred in terms of ease of controlling the progress of the polymerization reaction and the ability to use photopolymerization devices that are widely used in this field, and it is preferable to select the types of polymerizable liquid crystal compound and photopolymerization initiator contained in the composition for forming a polarizing film so that they can be photopolymerized by ultraviolet light. In addition, the polymerization temperature can also be controlled by irradiating light while cooling the dried coating film with an appropriate cooling means during polymerization. By adopting such a cooling means, the polymerization of the polymerizable liquid crystal compound can be carried out at a lower temperature, so that a polarizing film can be appropriately formed even if a substrate having a relatively low heat resistance is used. During photopolymerization, a patterned polarizing film can also be obtained by performing masking and development.

[0085] Examples of the light source of the active energy rays include a low-pressure mercury lamp, a medium-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a xenon lamp, a halogen lamp, a carbon arc lamp, a tungsten lamp, a gallium lamp, an excimer laser, an LED light source emitting light in the wavelength range of 380 to 440 nm, a chemical lamp, a black light lamp, a microwave-excited mercury lamp, and a metal halide lamp.

[0086] The UV irradiation intensity is usually 10 to 3,000 mW / cm 2 The ultraviolet irradiation intensity is preferably an intensity in a wavelength region effective for activating a photopolymerization initiator. The time for light irradiation is usually 0.1 seconds to 10 minutes, preferably 0.1 seconds to 5 minutes, more preferably 0.1 seconds to 3 minutes, and further preferably 0.1 seconds to 1 minute. When irradiating once or multiple times with such ultraviolet irradiation intensity, the integrated light amount is 10 to 3,000 mJ / cm. 2 , preferably 50 to 2,000 mJ / cm 2 , more preferably 100 to 1,000 mJ / cm 2 It is.

[0087] By carrying out photopolymerization, the polymerizable liquid crystal compound is polymerized while maintaining the liquid crystal state of the smectic phase, preferably the high-order smectic phase, to form a polarizing film. The polarizing film obtained by polymerizing the polymerizable liquid crystal compound while maintaining the liquid crystal state of the smectic phase has an advantage of having a higher polarization performance due to the action of the dichroic dye, compared to conventional host-guest type polarizing films, i.e., polarizing films made of a liquid crystal state of a nematic phase. Furthermore, it has an advantage of having superior strength compared to films coated with only a dichroic dye or a lyotropic liquid crystal.

[0088] The thickness of the polarizing film can be appropriately selected depending on the display device to which it is applied, and is preferably 0.5 to 10 μm, more preferably 1 to 5 μm, and further preferably 1 to 3 μm.

[0089] The coating of the polarizing film-forming composition is preferably formed on an alignment film. The alignment film has an alignment regulating force that aligns the polymerizable liquid crystal compound in a desired direction. The alignment film is preferably one that has solvent resistance that does not dissolve in the organic solvent contained in the polarizing film-forming composition, and also has heat resistance in a heat treatment for removing the solvent and orienting the polymerizable liquid crystal compound. Examples of such alignment films include an alignment film containing an alignment polymer, a photo-alignment film formed from a composition containing a polymer that generates an alignment regulating force by light and a solvent, a groove alignment film having a concave-convex pattern or a plurality of grooves on the surface, and a stretched film stretched in the alignment direction. A photo-alignment film is preferable from the viewpoint of being less likely to generate static electricity or foreign matter and being excellent in quality as an optical film.

[0090] Examples of the oriented polymer include polyamides and gelatins having an amide bond in the molecule, polyimides having an imide bond in the molecule, and polyamic acids, which are hydrolyzates thereof, polyvinyl alcohol, alkyl-modified polyvinyl alcohol, polyacrylamide, polyoxazole, polyethyleneimine, polystyrene, polyvinylpyrrolidone, polyacrylic acid, and polyacrylic acid esters. Among these, polyvinyl alcohol is preferred. The oriented polymers can be used alone or in combination of two or more kinds.

[0091] An alignment film containing an alignment polymer is usually obtained by applying a composition in which an alignment polymer is dissolved in a solvent (hereinafter, sometimes referred to as an "alignment polymer composition") to a substrate and removing the solvent, or by applying an alignment polymer composition to a substrate, removing the solvent, and rubbing (rubbing method). Examples of the solvent include the same organic solvents as those exemplified above as those usable in the composition for forming a polarizing film.

[0092] The concentration of the orienting polymer in the orienting polymer composition may be within a range in which the orienting polymer material can be completely dissolved in the solvent, and is preferably 0.1 to 20% in terms of solid content relative to the solution, and more preferably about 0.1 to 10%.

[0093] As the oriented polymer composition, a commercially available alignment film material may be used as it is. Examples of commercially available alignment film materials include Sunever (registered trademark, manufactured by Nissan Chemical Industries, Ltd.) and Optomer (registered trademark, manufactured by JSR Corporation).

[0094] The method for applying the orientable polymer composition to a substrate may be the same as those exemplified as the method for applying the composition for forming a polarizing film to a substrate.

[0095] Methods for removing the solvent contained in the orientable polymer composition include natural drying, ventilation drying, heat drying, and reduced pressure drying.

[0096] In order to impart an alignment control force to the alignment film, a rubbing treatment can be carried out as necessary (rubbing method).

[0097] An example of a method for imparting an orientation control force by a rubbing method is to bring an oriented polymer film formed on the surface of a substrate by applying an oriented polymer composition to the substrate and annealing the composition into contact with a rotating rubbing roll wrapped with a rubbing cloth.

[0098] The photo-alignment film can be formed by applying a composition (hereinafter also referred to as "photo-alignment film forming composition") containing a polymer or monomer having a photoreactive group and generating an alignment regulating force by light and a solvent onto a film such as a substrate to form a coating film, drying and removing the solvent from the resulting coating film, and then irradiating the resulting dried coating film with polarized ultraviolet light. The photo-alignment film is more preferable in that the direction of the alignment regulating force can be arbitrarily controlled by selecting the polarization direction of the irradiated polarized ultraviolet light.

[0099] The photoreactive group refers to a group that generates liquid crystal alignment ability by irradiation with light. Specifically, it includes groups involved in photoreactions that induce molecular alignment or are the origin of liquid crystal alignment ability, such as isomerization reaction, dimerization reaction, photocrosslinking reaction, or photodecomposition reaction, caused by irradiation with light. Among them, groups involved in dimerization reaction or photocrosslinking reaction are preferred in terms of excellent alignment ability. As the photoreactive group, a group having an unsaturated bond, particularly a double bond, is preferred, and a group having at least one selected from the group consisting of a carbon-carbon double bond (C=C bond), a carbon-nitrogen double bond (C=N bond), a nitrogen-nitrogen double bond (N=N bond), and a carbon-oxygen double bond (C=O bond) is particularly preferred.

[0100] Examples of photoreactive groups having a C=C bond include vinyl groups, polyene groups, stilbene groups, stilbazolyl groups, stilbazolium groups, chalcone groups, and cinnamoyl groups. Examples of photoreactive groups having a C=N bond include groups having structures such as aromatic Schiff bases and aromatic hydrazones. Examples of photoreactive groups having an N=N bond include azobenzene groups, azonaphthalene groups, aromatic heterocyclic azo groups, bisazo groups, formazan groups, and groups having an azoxybenzene structure. Examples of photoreactive groups having a C=O bond include benzophenone groups, coumarin groups, anthraquinone groups, and maleimide groups. These groups may have substituents such as alkyl groups, alkoxy groups, aryl groups, allyloxy groups, cyano groups, alkoxycarbonyl groups, hydroxyl groups, sulfonic acid groups, and halogenated alkyl groups.

[0101] Among them, photoreactive groups involved in photodimerization are preferred, and cinnamoyl and chalcone groups are preferred because the amount of polarized light irradiation required for photoalignment is relatively small and a photoalignment film having excellent thermal stability and stability over time is easily obtained. As the polymer having a photoreactive group, one having a cinnamoyl group such that the terminal of the polymer side chain has a cinnamic acid structure is particularly preferred.

[0102] A photo-alignment-inducing layer can be formed on a substrate by applying the composition for forming a photo-alignment film on the substrate. The solvent contained in the composition can be the same as the organic solvents exemplified above as those usable in the composition for forming a polarizing film, and can be appropriately selected depending on the solubility of the polymer or monomer having a photoreactive group.

[0103] The content of the polymer or monomer having a photoreactive group in the composition for forming a photo-alignment film can be appropriately determined depending on the type of polymer or monomer and the thickness of the desired photo-alignment film, but is preferably at least 0.2% by mass, more preferably in the range of 0.3 to 10% by mass, based on the total mass of the composition for forming a photo-alignment film. The composition for forming a photo-alignment film may contain a polymer material such as polyvinyl alcohol or polyimide, or a photosensitizer, within a range that does not significantly impair the properties of the photo-alignment film.

[0104] The method for applying the composition for forming a photo-alignment film to a substrate may be the same as the method for applying the composition for forming a polarizing film to a substrate. Methods for removing the solvent from the applied composition for forming a photo-alignment film may include natural drying, ventilation drying, heat drying, and reduced pressure drying.

[0105] The temperature for drying and removing the solvent can be appropriately determined depending on the type and amount of the solvent used, but is usually 30 to 150° C., and preferably 60 to 130° C. The time for drying and removing the solvent is usually 0.1 to 10 minutes, and preferably 0.5 to 5 minutes.

[0106] The polarized light may be irradiated by removing the solvent from the photo-alignment film forming composition applied on the substrate, or by irradiating the polarized UV light from the substrate side and transmitting the polarized UV light. It is particularly preferable that the polarized UV light is substantially parallel light. The wavelength of the polarized UV light to be irradiated is preferably in a wavelength range in which the photoreactive group of the polymer or monomer having a photoreactive group can absorb light energy. Specifically, UV light having a wavelength of 250 to 400 nm is particularly preferable. Examples of light sources used for the polarized light irradiation include xenon lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, and ultraviolet lasers such as KrF and ArF, and high-pressure mercury lamps, ultra-high-pressure mercury lamps, and metal halide lamps are more preferable. Among these, high-pressure mercury lamps, ultra-high-pressure mercury lamps, and metal halide lamps are preferable because they have a high emission intensity of UV light with a wavelength of 313 nm. The light from the light source can be irradiated by passing through an appropriate polarizer. As such a polarizer, a polarizing filter, a polarizing prism such as a Glan-Thompson or Glan-Taylor type polarizer, or a wire grid type polarizer can be used.

[0107] If masking is performed during rubbing or polarized light irradiation, a plurality of regions (patterns) in which the liquid crystal alignment directions are different can be formed.

[0108] A groove alignment film is a film that has a concave-convex pattern or multiple grooves on the film surface. When a polymerizable liquid crystal compound is applied to a film with multiple equally spaced linear grooves, the liquid crystal molecules are aligned in the direction along the grooves.

[0109] Methods for obtaining a groove alignment film include a method in which the surface of a photosensitive polyimide film is exposed to light through an exposure mask having slits in a pattern shape, followed by development and rinsing to form an uneven pattern; a method in which a layer of uncured UV-curable resin is formed on a plate-shaped master having grooves on its surface, the formed resin layer is transferred to a substrate and then cured; and a method in which a roll-shaped master having multiple grooves is pressed against an uncured UV-curable resin film formed on a substrate to form unevenness, followed by curing.

[0110] The thickness of the alignment film (alignment film containing an alignment polymer or photoalignment film) is usually in the range of 10 to 10,000 nm, preferably in the range of 10 to 1000 nm, more preferably 500 nm or less, further preferably 10 to 200 nm, and particularly preferably 30 to 150 nm.

[0111] The polarizing plate of the present invention may include, in addition to the polarizing film and the substrate of the present invention, a hard coat layer or an overcoat layer for protecting the polarizing film, etc. The hard coat layer or the overcoat layer can be formed by appropriately selecting conventionally known materials or components and by conventionally known methods.

[0112] The thickness of the polarizing plate of the present invention is preferably from 10 to 300 μm, more preferably from 20 to 200 μm, and further preferably from 25 to 100 μm, from the viewpoints of flexibility and visibility of the display device.

[0113] The polarizing film and polarizing plate of the present invention have excellent polarization performance and can be suitably used in various display devices. A display device is a device having a display mechanism, and includes a light-emitting element or a light-emitting device as a light source. Examples of the display device include a liquid crystal display device, an organic electroluminescence (EL) display device, an inorganic electroluminescence (EL) display device, a touch panel display device, an electron emission display device (field emission display device (FED, etc.), surface field emission display device (SED)), electronic paper (display device using electronic ink or electrophoretic element), a plasma display device, a projection type display device (grating light valve (GLV) display device, display device having digital micromirror device (DMD), etc.), and a piezoelectric ceramic display, etc., and organic EL display devices and touch panel display devices are particularly preferred, and organic EL display devices are particularly preferred. A display device including the polarizing plate of the present invention can be obtained by attaching the polarizing plate of the present invention to the surface of a display device via a pressure-sensitive adhesive or adhesive. EXAMPLES

[0114] The present invention will be described in more detail below with reference to examples. In the examples, "%" and "parts" are by mass % and parts by mass unless otherwise specified.

[0115] 1. Example 1 (1) Preparation of composition for forming polarizing film The following components were mixed and stirred at 80° C. for 1 hour to obtain a polarizing film-forming composition (1). The polymerizable liquid crystal compounds (A-6) and (A-7) are polymerizable liquid crystal compounds produced according to the method described in Lub et al., Recl. Trav. Chim. Pays-Bas, 115, 321-328 (1996), and have the structures shown below. The dichroic dyes (Ia) to (Ic) are azo dyes described in the examples of JP2013-101328A, and have the structures shown below.

[0116] <Constituents of the composition for forming a polarizing film> ·Polymerizable liquid crystal compound (A-6): 75 parts ·Polymerizable liquid crystal compound (A-7): 25 parts Dichroic dye (Ia): 2.5 parts ·Dichroic dye (Ib): 2.5 parts ·Dichroic dye (Ic): 2.5 parts Polymerization initiator [Esacure ONE (IGM Resins BV), molecular weight 435]: 2.5 parts Leveling agent [polyacrylate compound (BYK-361N; manufactured by BYK-Chemie)]: 1.2 parts Organic solvent [o-xylene:isophorone mixed solvent (90:10, mass ratio)]: 250 parts

[0117] Polymerizable liquid crystal compound (A-6): [ka] Polymerizable liquid crystal compound (A-7): [ka]

[0118] Dichroic dye (Ia): [ka] Dichroic dye (Ib): [ka] Dichroic dye (Ic): [ka]

[0119] (2) Preparation of composition for forming photoalignment film The following components described in JP 2013-033249 A were mixed, and the resulting mixture was stirred at 80° C. for 1 hour to obtain a composition for forming a photoalignment film. Photo-aligned polymer with the structure shown below: 2 parts (Weight average molecular weight: 50000) [ka] Solvent [o-xylene]: 98 parts

[0120] (3) Preparation of Water-Soluble Polymer Aqueous Solution According to the synthesis scheme below, a water-soluble polymer consisting of the following structural units was obtained. [ka]

[0121] 20 g of polyvinyl alcohol (manufactured by Wako Pure Chemical Industries, Ltd.) having a weight average molecular weight of 1000, 0.55 mg of N,N-dimethyl-4-aminopyridine as a nucleophile, and 4.6 g of triethylamine were dissolved in 400 g of dimethyl sulfoxide, and the temperature was raised to 60 ° C. while stirring. Next, a solution in which 10.5 g of methacrylic anhydride was dissolved in 50 g of dimethyl sulfoxide was dropped over 1 hour, and the mixture was reacted by heating and stirring at a temperature of 60 ° C. for 14 hours. After cooling the resulting reaction solution to room temperature, 481 g of methanol was added to the reaction solution and stirred to completely mix, so that the ratio (mass) of the reaction solution and methanol was adjusted to 1:1. The water-soluble polymer was crystallized by a crystallization method by gradually adding 1500 mL of acetone to this solution. The resulting solution containing white crystals was filtered, thoroughly washed with acetone, and then vacuum dried to obtain 20.2 g of water-soluble polymer. The resulting water-soluble polymer was dissolved in water to prepare a 3 mass% water-soluble polymer aqueous solution.

[0122] (4) Preparation of HC layer forming composition The following components were mixed and stirred at 50° C. for 4 hours to obtain a composition for forming a hard coat (HC) layer. Acrylate monomer with the structure shown below: 70 parts [ka] - Urethane acrylate resin [EBECRYL4858 (manufactured by Daicel Allnex Corporation)]: 30 parts Polymerization initiator [Omnirad907 (manufactured by IGM Resins BV)]: 3 parts Organic solvent [methyl ethyl ketone]: 10 parts

[0123] <Measurement of phase transition temperature> (i) Formation of alignment film The phase transition temperature of the polymerizable liquid crystal compound in the polarizing film-forming composition (1) was measured according to the following method. A 2% by mass aqueous solution of polyvinyl alcohol (polyvinyl alcohol 1000 fully saponified type, manufactured by Wako Pure Chemical Industries, Ltd.) was applied onto a glass substrate by spin coating, and after drying, a film having a thickness of 100 nm was formed. Subsequently, an alignment film was formed by subjecting the surface of the obtained film to a rubbing treatment. The rubbing treatment was performed using a semi-automatic rubbing device (trade name: LQ-008 type, manufactured by Joyo Engineering Co., Ltd.) with a cloth (trade name: YA-20-RW, manufactured by Yoshikawa Kako Co., Ltd.) under the conditions of a pressing amount of 0.15 mm, a rotation speed of 500 rpm, and 16.7 mm / s.

[0124] (ii) Measurement of phase transition temperature 75 parts by mass of polymerizable liquid crystal compound (A-6) and 25 parts by mass of polymerizable liquid crystal compound (A-7) were added to 400 parts by mass of chloroform and stirred at 80°C for 1 hour to obtain a homogeneously mixed mixed composition. The obtained composition was applied to the glass substrate with the alignment film by spin coating, and the solvent chloroform was removed by heating and drying on a hot plate at 130°C for 3 minutes. The obtained coating film was then quickly cooled to room temperature to obtain a dried film of the polymerizable liquid crystal compound. The dried film was again heated to 130°C on a hot plate, and then cooled to 23°C at a rate of 5°C / min. The phase transition temperature was measured by observing with a polarizing microscope. As a result, it was confirmed that the phase transition occurred to a nematic liquid crystal phase at 111.6°C, to a smectic A phase at 109.2°C, to a smectic B phase at 93.9°C, and the smectic B phase was maintained until the temperature reached 23°C. In the above process, the isotropic phase transition temperature was confirmed to be 111.6°C.

[0125] (6) Preparation of polarizing plate with substrate layer The HC layer-forming composition obtained above was continuously applied to the release-treated surface of a release polyethylene terephthalate (PET) film ("FF-50" manufactured by Unitika Ltd., one-sided release-treated PET film (support substrate thickness: 50 μm)) using a slot die coater, and dried at a temperature of 100° C. for 2 minutes to form an HC layer (first protective layer) having a thickness of 2.00 μm. This resulted in a film in which an HC layer was laminated on the release-treated surface of the one-sided release-treated PET film, and this was used as the first substrate layer (1).

[0126] After subjecting the HC layer of the first base layer (1) to plasma treatment, the composition for forming a photoalignment film prepared above was applied using a slot die coater to form a coating layer in a 600 mm wide range at the center of the one-sided release-treated PET film. The coating layer on the HC layer was then dried by transporting the film through a ventilated drying oven set at a temperature of 100° C. for 2 minutes to remove the solvent. Thereafter, the dried coating layer was irradiated with 20 mJ / cm of polarized UV light in a direction 90° to the length direction of the one-sided release-treated PET film. 2 An alignment control force was imparted by irradiating the HC layer with light having an intensity of 313 nm (based on 313 nm), and a photo-alignment film (1) was formed on the HC layer. The thickness of the photo-alignment film (1) was about 50 nm.

[0127] The polarizing film-forming composition (1) prepared above was applied onto the photoalignment film (1) formed on the first base layer (1) using a slot die coater to form a coating layer in a 600 mm wide range at the center of the first base layer (1). The coating layer was then transported for 2 minutes through a ventilated drying oven set at a temperature of 110°C to remove the solvent, and the coating layer on the first base layer (1) was dried. After that, ultraviolet light of 1000 mJ / cm was applied using a high-pressure mercury lamp. 2(365 nm standard) was irradiated to cure the polymerizable liquid crystal compound contained in the above coating layer after drying, thereby forming a cured layer of the composition for forming a polarizing film, and a polarizing film (1) with a substrate layer was obtained in which a photo-alignment film (1) and a cured layer (together, a polarizing film) were formed in this order on a first substrate layer (1). The polarizing film with a substrate layer (1) had an absorption axis at 90° to the length direction. The cured layer had a thickness of 3 μm. In addition, as a result of performing X-ray diffraction measurement on the obtained polarizing film, a Bragg peak was obtained, and it was confirmed that a structure reflecting a high-order smectic phase was formed.

[0128] Next, the cured layer side of the polarizing film (1) with the substrate layer was subjected to plasma treatment, and then the water-soluble polymer aqueous solution prepared above was continuously applied using a slot die coater and dried for 2 minutes at a temperature of 100° C. to form an overcoat layer (second protective layer) with a thickness of 2 μm. This resulted in a long polarizing plate (1) with a substrate layer, which was provided with the first substrate layer (1) (one-sided release-treated PET film / HC layer) / polarizing film (photoalignment film (1) / cured layer) / overcoat layer in this order.

[0129] (7) Evaluation of polarizing film The polarizing films were evaluated according to the methods described below. The evaluation results are shown in Table 1. <Evaluation of Drying Unevenness> The state of the coating surface of the obtained polarizing plate (1) with a substrate layer was visually observed on a backlight on which a linear polarizing plate was set, and evaluated according to the following criteria. [Evaluation criteria for uneven drying] ◯: No visible unevenness. △: Some unevenness is visible. ×: Unevenness is visible overall.

[0130] <Evaluation of dead pixels> The polarizing film (1) with the substrate layer was observed through a microscope at 200x magnification. In addition, the polarizing film was observed under a polarizing microscope at 200x magnification with crossed Nicols so that the absorption axis (molecular orientation direction) of the polarizing film was at 45°. From the above observation results, it was confirmed that there were no regions (missing dots) in the liquid crystal domains where the dichroic dye was not included. In addition, when circular color loss of approximately 200 to 800 μm was observed by visual observation, it was evaluated as having dot loss confirmed by visual observation, and when color loss was not observed by visual observation but minute circular color loss was observed by polarizing microscope observation, it was evaluated as having dot loss confirmed by microscope observation.

[0131] [Dead pixel evaluation criteria] ◯: Not observed visually, and not observed under the above microscope. Δ: Not observed visually, but observed in the above microscope observation. ×: Observed visually and also observed under the microscope.

[0132] <Evaluation of blocking properties> The polarizing plate (1) with the base layer was cut out to prepare five pieces with a size of 10 cm x 10 cm. The five cut pieces were stacked on the glass so that the base layer side of the cut pieces faced the glass side, the four corners were secured with Kapton tape, and the cut pieces were placed in an oven at a temperature of 90°C and held for five minutes. After holding, the area of ​​the cut pieces (100 cm 2 ) was calculated and evaluated according to the following criteria. [Blocking evaluation criteria] ○: The area of ​​adhesion is 20% or less △: The area of ​​adhesion is more than 20% and less than 40%. ×: Adhered area is more than 40% and less than 100%

[0133] <Evaluation of transferability> The obtained polarizing plate (1) with the substrate layer was cut into a square of 40 mm × 40 mm in size. The overcoat layer side was attached to an alkali-free glass plate (manufactured by Corning Incorporated, product name "Eagle-XG") using an acrylic adhesive having a thickness of 25 μm (manufactured by Lintec Corporation, product name "P-3132"), and then the one-sided release-treated PET film was peeled off. [Transferability evaluation criteria] 〇: Transfer is possible over the entire surface (peel occurs between the PET film and the HC layer) △: Part of the polarizer remains on the one-sided release-treated PET film. ×: Almost no transfer possible

[0134] 2. Examples 2 to 8 and 10 Polarizing film-forming compositions (2) to (8) and (10) were prepared and polarizing plates (2) to (8) and (10) with base layer were obtained in the same manner as in Example 1, except that the type and mixing ratio of the organic solvent used were changed as shown in Table 1. The obtained polarizing plates (2) to (8) and (10) with base layer were evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0135] 3. Examples 9 and 11, Comparative Examples 1, 2, and 5 Polarizing film-forming compositions (9), (11), (12), (15) and (16) were prepared in the same manner as in Example 1, except that the polymerization initiator was changed as shown in Table 1, and polarizing plates with base layer (9), (11), (12), (15) and (16) were obtained. The obtained polarizing plates with base layer (9), (11), (12), (15) and (16) were evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0136] 4. Comparative Examples 3 and 4 Polarizing film-forming compositions (13) and (14) were prepared in the same manner as in Examples, except that the organic solvent was o-xylene alone or isophorone alone, and polarizing plates (13) and (14) with a base layer were obtained. The obtained polarizing plates (13) and (14) with a base layer were evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0137] [Table 1]

Claims

1. The liquid crystal composition includes a polymerizable liquid crystal compound exhibiting smectic liquid crystallinity, a dichroic dye, a polymerization initiator, and at least two organic solvents, The molecular weight of the polymerization initiator is 400 or more, The organic solvent includes an organic solvent A having a boiling point that is −20° C. or more and 50° C. or less higher than the isotropic phase transition temperature of the polymerizable liquid crystal compound, and an organic solvent B having a boiling point that is more than 50° C. higher than the isotropic phase transition temperature of the polymerizable liquid crystal compound.

2. 2. The composition for forming a polarizing film according to claim 1, wherein the content of organic solvent A is 51 to 99 parts by mass and the content of organic solvent B is 1 to 49 parts by mass, relative to 100 parts by mass of all organic solvents contained in the composition for forming a polarizing film.

3. 3. The composition for forming a polarizing film according to claim 1, wherein the organic solvent A is a ketone solvent or an aromatic solvent.

4. 3. The composition for forming a polarizing film according to claim 1, wherein the organic solvent B is a ketone-based solvent or a lactone-based solvent.

5. 3. The composition for forming a polarizing film according to claim 1, wherein the organic solvent B is a cyclic ketone solvent or a lactone solvent.

6. 3. The composition for forming a polarizing film according to claim 1, wherein the content of the polymerization initiator having a molecular weight of 400 or more is 1 to 10 parts by mass based on 100 parts by mass of the polymerizable liquid crystal compound.

7. 2. A polarizing film comprising a cured product of the composition for forming a polarizing film according to claim 1, in which the polymerizable liquid crystal compound and / or its polymer are oriented in a smectic liquid crystal state.

8. 8. The polarizing film according to claim 7, which exhibits a Bragg peak in X-ray diffraction measurement.

9. A polarizing plate comprising the polarizing film according to claim 7 or 8 and a substrate.

Citation Information

Patent Citations

  • Composition for forming polarization film, polarization film, polarization plate, and method for manufacturing the same

    JP2019139222A