Steel sheet, and method for manufacturing steel sheet
A high-strength steel plate with controlled carbon concentration and decarburized layers, achieved through precise annealing, addresses bendability issues in high-strength steel plates, ensuring excellent bendability and plating adhesion.
Patent Information
- Application Number
- JP2024022770
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-02-19
- Publication Date
- 2024-10-11
AI Technical Summary
High-strength steel plates, particularly those with tensile strengths of 980 MPa or higher, face challenges in achieving both high strength and excellent bendability due to issues with Si and Mn oxidation leading to poor plating adhesion and unplated areas during continuous annealing.
A steel plate with controlled carbon concentration profiles and decarburized layers formed through specific annealing processes, including oxidation and reduction treatments, to enhance bendability while maintaining high strength.
The steel plate achieves high tensile strength of 980 MPa or more with excellent bendability, ensuring good plating adhesion and reducing weight in vehicle bodies.
Smart Images

Figure 2024144148000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a steel sheet and a method for manufacturing the steel sheet, and more particularly to a high-tensile steel sheet having excellent bendability and a method for manufacturing the steel sheet. [Background technology]
[0002] There has been a demand for improved safety for vehicle occupants, and for this purpose, the strength of the materials used in vehicle bodies has been improved. On the other hand, against the background of the worsening of global warming and other issues, there has been an accelerating movement to improve the fuel efficiency of automobiles. It is known that reducing the weight of vehicle bodies is an effective way to improve fuel efficiency.
[0003] Addition of Si and Mn is effective in increasing the strength of steel sheets to reduce the weight of car bodies. However, during continuous annealing, Si and Mn oxidize even in a reducing atmosphere where Fe does not oxidize, and oxides of Si and Mn are formed on the outermost surface of the steel sheet. For example, during zinc-based plating treatment, oxides of Si and Mn reduce the wettability between molten zinc and the base steel sheet, so steel sheets to which Si and Mn have been added have problems such as frequent bare spots and poor plating adhesion.
[0004] In response to the above problems, Patent Document 1 discloses a method for producing a high-strength hot-dip galvanized steel sheet having excellent coating adhesion, workability, and fatigue resistance, which comprises the steps of: in a first stage, heating the steel sheet at a temperature of 400 to 750°C in an atmosphere with an O2 concentration of 1000 volume ppm or more and an H2O concentration of 1000 volume ppm or more; and in a second stage, heating at a temperature of 600 to 850°C in an atmosphere with an O2 concentration of less than 1000 volume ppm and an H2O concentration of 1000 volume ppm or more; It shows that the steel is heated to a temperature of 650 to 900°C at a heating rate of 0.1°C / sec or more in an atmosphere having an H2 concentration of 5 to 30% by volume, an H2O concentration of 10 to 1000 ppm by volume, and the balance being N2 and unavoidable impurities, and then reduction annealing is performed in a soaking zone in an atmosphere having an H2 concentration of 5 to 30% by volume, an H2O concentration of 500 to 5000 ppm by volume, and the balance being N2 and unavoidable impurities, with the temperature change in the soaking zone being within ±20°C, for 10 to 300 seconds. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2017-166057 A Summary of the Invention [Problem to be solved by the invention]
[0006] In manufacturing automobile parts, steel sheets are sometimes bent to form the part shape. However, there is a problem that it is difficult to bend high-strength steel sheets, for example, 980 MPa or more, or even 1180 MPa or more, satisfactorily to form the desired part shape, that is, it is difficult to ensure excellent bendability. Patent Document 1 does not consider improving the bendability of plated steel sheets. The present disclosure has been made in view of the above circumstances, and its purpose is to provide a steel sheet that is high in strength, can contribute to weight reduction of a vehicle body, and exhibits excellent bendability, and a method for easily manufacturing the steel sheet. [Means for solving the problem]
[0007] Aspect 1 of the present invention is In the plate thickness direction, The position where the carbon concentration (mass%) is 50% of the bulk carbon concentration is in a region that is 0.20% or more of the plate thickness from the steel plate surface, and The position where the carbon concentration (mass %) is 90% of the bulk carbon concentration is in a region of the steel plate that is 8.0% or less of the plate thickness from the surface of the steel plate.
[0008] Aspect 2 of the present invention is The maximum carbon concentration (mass%) in the region from the steel sheet surface to 20 μm in the sheet thickness direction is less than 70% of the bulk carbon concentration, and The amount of surface decarburization per 1 mm of plate thickness on one side of the steel plate is 0.045 mol / m 2 The steel sheet according to embodiment 1 is as follows:
[0009] Aspect 3 of the present invention is 3. The steel sheet according to claim 1 or 2, having a tensile strength of 980 MPa or more.
[0010] A fourth aspect of the present invention is The composition of the components is C: 0.08% by mass or more and 0.30% by mass or less Si: More than 0.5% by mass and 3.0% by mass or less Mn: 1.5% by mass or more and 3.0% by mass or less Cr: 0 mass% or more, 1.0 mass% or less P: More than 0% by mass and 0.1% by mass or less S: More than 0% by mass, 0.05% by mass or less Al: more than 0 mass% and 1.0 mass% or less, and N: More than 0% by mass and 0.01% by mass or less; The steel sheet according to any one of Aspects 1 to 3, wherein the balance is Fe and unavoidable impurities.
[0011] A fifth aspect of the present invention is The annealing process includes an oxidation process at an oxygen concentration of 0.1 to 2% and a temperature of 650 to 750°C, followed by a reduction process. The reduction treatment is a method for producing a steel sheet, which includes a first reduction treatment having a dew point of -35 to -15°C, followed by a second reduction treatment having a dew point of -25 to 0°C, which is higher than that of the first reduction treatment.
[0012] A sixth aspect of the present invention is In the method for producing a steel sheet according to aspect 5, the ultimate temperature in the first reduction treatment and the second reduction treatment is 800 to 920°C. Effect of the Invention
[0013] According to the present disclosure, there are provided a steel plate having high strength, capable of contributing to weight reduction of a vehicle body, and exhibiting excellent bendability, and a method for manufacturing the steel plate. [Brief description of the drawings]
[0014] [Figure 1-1]Figure 1-1 is a graph showing the relationship between the dew point at the center of the soaking zone and R / t during the second reduction treatment. [Figure 1-2] FIG. 1-2 is another graph showing the relationship between the dew point at the center of the soaking zone and R / t during the second reduction treatment. [Figure 2-1] FIG. 2-1 is a graph showing the relationship between the dew point at the center of the soaking zone during the second reduction treatment and the tensile strength TS. [Figure 2-2] FIG. 2-2 is another graph showing the relationship between the dew point at the center of the soaking zone and the tensile strength TS during the second reduction treatment. [Diagram 3] FIG. 3 is a diagram showing an example of a carbon concentration profile obtained in an example. [Figure 4-1] FIG. 4-1 is a graph showing the relationship between the position where the carbon concentration (mass %) in the sheet thickness direction is 50% of the bulk carbon concentration and R / t. [Figure 4-2] FIG. 4-2 is another graph showing the relationship between the position where the carbon concentration (mass %) in the sheet thickness direction is 50% of the bulk carbon concentration and R / t. [Figure 5-1] FIG. 5-1 is a graph showing the relationship between the position in the sheet thickness direction where the carbon concentration (mass %) is 90% of the bulk carbon concentration, and the tensile strength TS. [Figure 5-2] FIG. 5-2 is another graph showing the relationship between the position in the sheet thickness direction where the carbon concentration (mass %) is 90% of the bulk carbon concentration and the tensile strength TS. [Figure 6-1] FIG. 6-1 is a graph showing the relationship between the ratio of the maximum carbon concentration (mass %) in the region from the steel sheet surface to 20 μm deep, relative to the bulk carbon concentration, and R / t. [Figure 6-2] FIG. 6-2 is another graph showing the relationship between the ratio of the maximum carbon concentration (mass %) in the region from the steel sheet surface to 20 μm deep, relative to the bulk carbon concentration, and R / t. [Figure 7-1] Figure 7-1 is a graph showing the relationship between the amount of surface decarburization per mm of plate thickness and tensile strength TS. [Figure 7-2] Figure 7-2 is another graph showing the relationship between the amount of surface decarburization per mm of plate thickness and tensile strength TS. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present inventors have conducted extensive research to obtain a steel sheet that exhibits excellent bendability in bending even when it has high strength. As a result, they have found that by providing a decarburized layer within a predetermined range in the surface layer of the steel sheet, excellent bendability can be obtained while maintaining high strength. They have also found that in order to form a decarburized layer within a predetermined range in the surface layer of the steel sheet that can achieve both high strength and excellent bendability, it is sufficient to control the conditions when annealing the steel sheet. Hereinafter, the steel sheet of this embodiment will be first described.
[0016] [Steel plate] (Decarburized layer on the surface of steel plate) The steel plate according to this embodiment is (I) In the plate thickness direction, The position where the carbon concentration (mass%) is 50% of the bulk carbon concentration is in a region that is 0.20% or more of the plate thickness from the steel plate surface, and The position where the carbon concentration (mass %) is 90% of the bulk carbon concentration is in a region that is 8.0% or less of the sheet thickness from the steel sheet surface.
[0017] In the steel plate according to this embodiment, in the plate thickness direction, a position where the carbon concentration (mass %) is 50% of the bulk carbon concentration is in a region of 0.20% or more of the plate thickness from the surface of the steel plate. The position relates to the thickness of the decarburized layer that contributes to bendability. By ensuring that the position is in a region of 0.20% or more of the plate thickness from the surface of the steel plate and that the decarburized layer has a certain thickness or more that contributes to bendability, it is possible to reliably exhibit excellent bendability in bending. The position where the carbon concentration (mass %) is 50% of the bulk carbon concentration may be in a region of 0.5% or more, or even 1.0% or more of the plate thickness from the surface of the steel plate.
[0018] Furthermore, in the steel plate according to this embodiment, the position where the carbon concentration (mass%) is 90% of the bulk carbon concentration in the plate thickness direction is in a region of 8.0% or less of the plate thickness from the surface of the steel plate. Increasing the thickness of the decarburized layer improves bendability, but the strength is likely to decrease. However, the inventors have found through their studies that if the position where the carbon concentration (mass%) is 90% of the bulk carbon concentration is in a region of 8.0% or less of the plate thickness from the surface of the steel plate, the decrease in strength can be sufficiently suppressed. The position where the carbon concentration (mass%) is 90% of the bulk carbon concentration may be 6.0% or less of the plate thickness from the surface of the steel plate.
[0019] The steel plate according to this embodiment is (II) The maximum carbon concentration (mass%) in the region from the steel sheet surface to 20 μm in the sheet thickness direction is less than 70% of the bulk carbon concentration, and The amount of surface decarburization per 1 mm of plate thickness on one side of the steel plate is 0.045 mol / m 2 Less than or equal to 0.035 mol / m 2 It is also the following.
[0020] When the present inventors checked conventional steel sheets, they first found that there was a region in the surface layer of the steel sheet with a significantly high carbon concentration, which was the cause of the deterioration of bendability. Then, as described below, they investigated the manufacturing conditions of the steel sheet and found that excellent bendability can be obtained by promoting decarburization of the surface layer of the steel sheet and suppressing the carbon concentration in the surface layer of the steel sheet, specifically, by suppressing the maximum carbon concentration (mass%) in the region from the steel sheet surface to 20 μm in the sheet thickness direction to less than 70% of the bulk carbon concentration. The maximum carbon concentration is preferably 65% or less of the bulk carbon concentration, and more preferably 60% or less of the bulk carbon concentration.
[0021] In addition, the steel plate according to this embodiment has a surface decarburization amount of 0.045 mol / m per 1 mm of plate thickness on one side of the steel plate. 2 Less than or equal to 0.035 mol / m 2By suppressing the surface decarburization amount per mm of plate thickness to 0.030 mol / m or less, a high strength of tensile strength of 980 MPa or more, particularly 1180 MPa or more, can be ensured. 2 More preferably, it is 0.025 mol / m or less. 2 The following is the result.
[0022] From the viewpoint of achieving both high strength and excellent bendability, the steel sheet according to this embodiment only needs to satisfy at least one of the above (I) and (II), and preferably satisfies both of the above (I) and (II).
[0023] The "steel sheet surface" refers to the surface of the steel sheet in the case of a steel sheet obtained by annealing a cold-rolled steel sheet, and refers to the position of the interface between the coating layer and the base steel sheet in the case of a plated steel sheet. The position of the interface between the coating layer and the base steel sheet refers to the point where Zn constituting the coating layer is no longer detectable (the analysis value of Zn is 0) when Zn is analyzed from the surface of the coating layer in the thickness direction of the coating layer by GD-OES performed in the examples described later, for example, in the case of a zinc-based coating, and this point is defined as the starting point of the distance (depth) from the steel sheet surface.
[0024] The steel sheet according to the present embodiment has high strength and exhibits excellent bendability in bending. The strength can be, for example, a tensile strength TS of 980 MPa or more, preferably 1180 MPa or more. Furthermore, the steel sheet according to the present embodiment exhibits excellent bendability with a limit R / t of less than 2.5 when subjected to a bending test shown in the examples described later.
[0025] The thickness of the steel sheet according to the present embodiment is not limited, and may be, for example, 0.4 mm or more and 4 mm or less (in the case of a plated steel sheet, the thickness of the base steel sheet).
[0026] (Steel plate composition) To achieve high strength, the steel sheet according to the present embodiment may have a Si content of more than 0.5 mass% in its composition. The Si content is more preferably 1.0 mass% or more, even more preferably 1.1 mass% or more, and even more preferably 1.2 mass% or more. The upper limit of the Si content may be, for example, 3.0 mass%.
[0027] In one preferred embodiment, the composition of the steel sheet is C: 0.08% by mass or more, 0.30% by mass or less, Si: more than 0.5% by mass, 3.0% by mass or less, Mn: 1.5% by mass or more, 3.0% by mass or less, Cr: 0 mass% or more, 1.0 mass% or less, P: more than 0% by mass, 0.1% by mass or less, S: more than 0% by mass, 0.05% by mass or less, Al: more than 0 mass% and 1.0 mass% or less, and N: More than 0% by mass and 0.01% by mass or less; The balance is Fe and unavoidable impurities. Each element will be explained below.
[0028] [C: preferably 0.08% by mass or more and 0.30% by mass or less] C is an element effective in improving the strength of steel sheets, and is a particularly effective strengthening element for ensuring the tensile strength of the steel sheets to be 980 MPa or more, and even 1180 MPa or more, by being contained in the steel together with Si, and furthermore together with Mn as necessary. Furthermore, C is also an element necessary for ensuring the retained austenite and improving the workability. In order to effectively exert such an action, the C content is preferably 0.08 mass% or more, more preferably 0.11 mass% or more, and even more preferably 0.13 mass% or more. From the viewpoint of ensuring the strength of the steel sheets, it is preferable that the C content is high, but if the C content is too high, there is a risk of deterioration in corrosion resistance, spot weldability, and workability. Therefore, the C content is preferably 0.30 mass% or less, more preferably 0.25 mass% or less, and even more preferably 0.23 mass% or less.
[0029] [Mn: preferably 1.5% by mass or more and 3.0% by mass or less] Mn, like Si, is an inexpensive strengthening element for steel and is effective in improving the strength of steel sheets. Mn is a particularly effective strengthening element for ensuring the final tensile strength of steel sheets of 980 MPa or more, and even 1180 MPa or more, by being contained in steel together with Si and, if necessary, together with C. Furthermore, Mn is also an element that stabilizes austenite and contributes to improving the workability of steel sheets by the formation of retained austenite. In order to effectively exert such an action, the Mn content is preferably 1.5 mass% or more, more preferably 1.8 mass% or more, and even more preferably 2.0 mass% or more. However, if the Mn content is too high, the ductility of the steel sheet decreases, adversely affecting the workability of the steel sheet, and further, the weldability of the steel sheet may decrease. From these viewpoints, the Mn content is preferably 3.0 mass% or less, more preferably 2.8 mass% or less, and even more preferably 2.7 mass% or less.
[0030] [Si: more than 0.5 mass%, 3.0 mass% or less] Si is an inexpensive steel strengthening element and does not easily affect the workability of steel sheets. In addition, Si is an element that can suppress the decomposition of residual austenite, which is useful for improving the workability of steel sheets, to generate carbides. In order to effectively exert such an action, the Si content is more than 0.5 mass%, preferably 1.0 mass% or more, more preferably 1.1 mass% or more, and even more preferably 1.2 mass% or more. There is no particular upper limit for the Si content, but if the Si content is too high, the solid solution strengthening effect of Si becomes significant and the rolling load may increase. In addition, Si scale may be generated during hot rolling, causing surface defects in the steel sheet. Therefore, the Si content is preferably 3.0 mass% or less, more preferably 2.7 mass% or less, and even more preferably 2.5 mass% or less, from the viewpoint of manufacturing stability, for example.
[0031] [Cr: preferably 0 mass% or more and 1.0 mass% or less] Cr is an element effective in improving the strength of steel sheets. Furthermore, Cr is an element that improves the corrosion resistance of steel sheets, and has the effect of suppressing the generation of hydrogen due to corrosion of steel sheets. Specifically, Cr has the effect of promoting the generation of iron oxide (α-FeOOH). Iron oxide is said to be thermodynamically stable and protective among rusts that are generated in the atmosphere. By promoting the generation of such rust, it is possible to suppress the intrusion of the generated hydrogen into the steel sheet, and even when the steel sheet is used in a severe corrosive environment, for example, in the presence of chlorides, hydrogen-assisted cracking can be sufficiently suppressed. In addition, Cr, like B and Ti, is also an element that is effective in improving the delayed fracture resistance of steel sheets, so that it can be contained in an amount that does not affect the strength and workability, such as elongation, of the steel sheet. The Cr content may be 0% by mass, but in order to effectively exert these effects, the Cr content is preferably more than 0% by mass, more preferably 0.003% by mass or more, and even more preferably 0.01% by mass or more. On the other hand, if the Cr content is excessive, the workability, such as elongation, of the steel sheet may be deteriorated. Therefore, the Cr content is preferably 1.0 mass % or less, more preferably 0.8 mass % or less, and further preferably 0.6 mass % or less.
[0032] [P: preferably more than 0% by mass, 0.1% by mass or less] P is an element that is inevitably present as an impurity element. If the P content is excessive, it may deteriorate the weldability. Therefore, the P content is preferably controlled to 0.1 mass% or less, more preferably 0.08 mass% or less, and further preferably 0.05 mass% or less.
[0033] [S: preferably more than 0 mass% and 0.05 mass% or less] S is an element that is inevitably present as an impurity element. Usually, steel inevitably contains about 0.0005% by mass of S. If the S content is excessive, it may form sulfide-based inclusions, promote hydrogen absorption in a corrosive environment, deteriorate the delayed fracture resistance of the steel sheet, and deteriorate the weldability and workability of the steel sheet. Therefore, the S content is preferably suppressed to 0.05% by mass or less, more preferably 0.01% by mass or less, and further preferably 0.005% by mass or less.
[0034] [Al: preferably more than 0 mass% and 1.0 mass% or less] Al is an element having a deoxidizing effect. In order to effectively exert such an effect, the Al content is preferably more than 0 mass%, more preferably 0.005 mass% or more, and even more preferably 0.02 mass% or more. If the Al content is excessive, the amount of inclusions such as alumina increases, and the workability of the steel sheet may deteriorate. Therefore, the Al content is preferably 1.0 mass% or less, more preferably 0.8 mass% or less, and even more preferably 0.5 mass% or less.
[0035] [N: preferably more than 0% by mass and 0.01% by mass or less] N is an element that is inevitably present as an impurity element. If the N content is excessive, nitrides may be formed, which may deteriorate the workability of the steel sheet. In particular, when the steel sheet contains B to improve the hardenability, N combines with B to form BN precipitates, which inhibits the hardenability improving effect of B. Therefore, the N content is preferably suppressed to 0.01 mass% or less, more preferably 0.008 mass% or less, and further preferably 0.005 mass% or less.
[0036] [Remainder] The balance is Fe and unavoidable impurities. As unavoidable impurities, the inclusion of trace elements (e.g., As, Sb, Sn, etc.) that are brought in depending on the conditions of raw materials, materials, manufacturing equipment, etc. is permitted. Note that, as mentioned above, P, S, and N are generally preferable as their contents are lower, and therefore they can also be called unavoidable impurities. However, these elements are specified as above because the present invention can exert its effects by suppressing the contents of these elements to a specific range. For this reason, in this specification, the "unavoidable impurities" that make up the balance are a concept that excludes elements whose composition ranges are specified.
[0037] In addition to the above components, other well-known optional components may be further contained within the range that does not impair strength or sufficient bendability. Optional components include Cu, Ni, Ti, Nb, V, and B. These optional components are described below.
[0038] [Cu: preferably more than 0 mass% and 1.0 mass% or less] Like Cr, Cu is also effective in improving the strength of steel sheet and has the effect of suppressing hydrogen generation due to corrosion of the steel sheet, and is an element that improves the corrosion resistance of the steel sheet. Like Cr, Cu has the effect of promoting the formation of iron oxide. To effectively exert these effects, the Cu content is preferably more than 0 mass%, more preferably 0.003 mass% or more, and even more preferably 0.05 mass% or more. In addition, from the viewpoint of the workability of the steel sheet, the Cu content is preferably 1.0 mass% or less, more preferably 0.8 mass% or less, and even more preferably 0.5 mass% or less.
[0039] [Ni: preferably more than 0 mass% and 1.0 mass% or less] Ni, like Cr and Cu, is also effective in improving the strength of steel sheet and has the effect of suppressing hydrogen generation due to corrosion of the steel sheet, and is an element that improves the corrosion resistance of the steel sheet. Ni, like Cr and Cu, has the effect of promoting the formation of iron oxide. To effectively exert these effects, the Ni content is preferably more than 0 mass%, more preferably 0.003 mass% or more, and even more preferably 0.05 mass% or more. In addition, from the viewpoint of ensuring the workability of the steel sheet, the Ni content is preferably 1.0 mass% or less, more preferably 0.8 mass% or less, and even more preferably 0.5 mass% or less.
[0040] [Ti: preferably more than 0 mass% and 0.15 mass% or less] Ti, like Cr, Cu, and Ni, is also effective in improving the strength of steel sheets, and has the effect of suppressing hydrogen generation due to corrosion of steel sheets, and is an element that improves the corrosion resistance of steel sheets. Ti, like Cr, Cu, and Ni, has the effect of promoting the formation of iron oxide. In addition, Ti, like B and Cr, is also an element that is effective in improving the delayed fracture resistance of steel sheets, so it can be contained in an amount that does not affect the strength and workability, such as elongation, of the steel sheets. In order to effectively exert these effects, the Ti content is preferably more than 0 mass%, more preferably 0.003 mass% or more, and even more preferably 0.05 mass% or more. In addition, from the viewpoint of ensuring the workability of the steel sheets, the Ti content is preferably 0.15 mass% or less, more preferably 0.12 mass% or less, and even more preferably 0.10 mass% or less.
[0041] [Nb: preferably more than 0 mass% and 0.15 mass% or less] Nb is an element that is effective in improving the strength of steel plate and also acts to refine austenite grains after quenching, thereby improving the toughness of the steel plate. To effectively exert such an effect, the Nb content is preferably more than 0 mass%, more preferably 0.003 mass% or more, and even more preferably 0.005 mass% or more. On the other hand, if the Nb content is excessive, a large amount of carbides, nitrides, or carbonitrides may be formed, which may deteriorate the workability or delayed fracture resistance of the steel plate. Therefore, the Nb content is preferably 0.15 mass% or less, more preferably 0.12 mass% or less, and even more preferably 0.10 mass% or less.
[0042] [V: preferably more than 0% by mass, 0.15% by mass or less] Like Nb, V is also an element that is effective in improving the strength of steel sheet and refines austenite grains after quenching to improve the toughness of the steel sheet. To effectively exert such an effect, the V content is preferably more than 0 mass%, more preferably 0.003 mass% or more, and even more preferably 0.005 mass% or more. On the other hand, if the V content is excessive, like Nb, a large amount of carbides, nitrides, or carbonitrides may be formed, which may deteriorate the workability or delayed fracture resistance of the steel sheet. Therefore, the V content is preferably 0.15 mass% or less, more preferably 0.12 mass% or less, and even more preferably 0.1 mass% or less.
[0043] [B: preferably more than 0% by mass and 0.005% by mass or less] B is an element useful for improving the hardenability and weldability of steel sheets. In addition, like Ti and Cr, B is also an element effective for the delayed fracture resistance of steel sheets, so it can be contained in an amount that does not affect the strength and workability such as elongation of the steel sheets. In order to effectively exert these effects, the B content is preferably more than 0 mass%, more preferably 0.0002 mass% or more, even more preferably 0.0003 mass% or more, and particularly preferably 0.0004 mass% or more. On the other hand, if the B content is excessive, such effects may be saturated and the ductility may decrease, resulting in poor workability. Therefore, the B content is preferably 0.005 mass% or less, more preferably 0.004 mass% or less, and even more preferably 0.003 mass% or less.
[0044] Examples of the steel sheet include cold-rolled steel sheet, plated steel sheet, etc. The type of plated steel sheet is not limited, and may be, for example, a zinc-based plated steel sheet that is plated with a zinc-based coating such as Al-Zn coating, Ni-Zn coating, Fe-Zn coating, Cr-Zn coating, or Mg-Zn coating. Specific examples of the zinc-based plated steel sheet include hot-dip galvanized steel sheet (GI), alloyed hot-dip galvanized steel sheet (GA), and electrolytic galvanized steel sheet (EG).
[0045] [Steel plate manufacturing method] Next, a method for producing a high strength steel sheet according to the present invention, particularly a method for producing a steel sheet with excellent galvanizability, will be described.
[0046] The method for manufacturing a steel sheet according to this embodiment is as follows: The annealing process includes an oxidation process at an oxygen concentration of 0.1 to 2% and a temperature of 650 to 750°C, followed by a reduction process. The reduction treatment includes a first reduction treatment in which the dew point is −35 to −15° C., and then a second reduction treatment in which the dew point is −25 to 0° C., which is higher than the dew point of the first reduction treatment.
[0047] By subjecting the surface of the steel sheet to an oxidation treatment, an Fe oxide layer is formed on the surface of the steel sheet. Next, by performing a reduction treatment under a reducing atmosphere, a decarburized layer is formed on the surface layer of the steel sheet, while a reduced Fe layer capable of forming, for example, a good plating layer is formed. At this time, if water vapor is added throughout the reduction treatment, the amount of decarburization may become excessive, resulting in a decrease in strength. On the other hand, if a high dew point is used in the first half of the reduction treatment, decarburization occurs once, but carbon re-diffuses (recarbonizes) in the decarburized portion in the second half of the reduction treatment, and bending properties do not improve. The inventors of the present invention have therefore conducted research and found that by performing the oxidation treatment as described above, and by determining the ranges of the dew points of the first reduction treatment and the second reduction treatment in the reduction treatment, and by setting the dew point of the second reduction treatment higher than the dew point of the first reduction treatment, the decarburized state of the surface layer of the steel sheet described above, which can achieve both high strength and excellent bending properties, can be easily ensured. Each treatment of the oxidation treatment and the reduction treatment will be described below.
[0048] (Oxidation treatment) The oxidation treatment is performed under conditions of an oxygen concentration of 0.1 to 2%. Although the oxygen concentration can be performed under conditions of 0.0%, it is preferable to set the oxygen concentration to 0.1% or more from the viewpoint of obtaining an excellent plating appearance when obtaining a plated steel sheet. The oxygen concentration is more preferably 0.15% or more, and even more preferably 0.20% or more. On the other hand, if the oxygen concentration is too high, a defect called pickup is likely to occur, in which oxide scale adheres to the rolls in the furnace due to excessive oxidation and indentation occurs on the steel sheet. In order to suppress the occurrence of such defects, the oxygen concentration is set to 2% or less. The oxygen concentration is preferably 1.7% or less, and more preferably 1.5% or less. The concentrations of elements other than oxygen are not particularly limited, and examples thereof include a gas atmosphere containing CO2, N2, H2O, and other inevitable impurities in addition to the above-mentioned concentrations of oxygen. For example, the oxidation treatment can be carried out in a DFF (Direct Fired Furnace) type annealing furnace or the like in a gas atmosphere in which the concentration of unburned O2 is controlled in combustion gas such as coke oven gas (COG) or liquefied petroleum gas (LPG).
[0049] The oxidation treatment is carried out under the condition of an ultimate temperature of 650 to 750°C. For example, heating may be performed in an oxidation heating zone in a DFF type annealing furnace to an ultimate temperature of 650 to 750°C. By setting the ultimate temperature at 750°C or less, it is possible to suppress the reaction between SiO2 on the surface of the steel sheet near the width direction edge and FeO generated by the oxidation treatment. As a result, for example, when the steel sheet according to this embodiment is a plated steel sheet, good plating adhesion can be obtained.
[0050] In this specification, the "achieved temperature" during heating in the oxidation treatment means the maximum reached sheet temperature of the steel sheet that is heat-controlled in the oxidation heating zone.
[0051] The temperature reached in the oxidation treatment is preferably 730° C. or lower, more preferably 720° C. or lower, and further preferably 700° C. or lower. On the other hand, the steel sheet temperature in the oxidation treatment is set to 650° C. or higher from the viewpoint of forming an Fe oxide layer in the above gas atmosphere. The steel sheet temperature in the oxidation treatment is preferably 670° C. or higher.
[0052] The temperature rise time in the oxidation treatment is not particularly limited, and may be adjusted so that the oxidation treatment is not too long and, for example, a fayalite layer that adversely affects plating properties is not formed. Specifically, the temperature rise time in the oxidation treatment may be appropriately adjusted in consideration of the hot rolling conditions (particularly the coiling temperature), the annealing conditions before pickling, the pickling conditions, and the steel sheet temperature during heating in the oxidation treatment. For example, the temperature rise time in the oxidation treatment is preferably 10 seconds or more, more preferably 15 seconds or more. Also, for example, the temperature rise time in the oxidation treatment is preferably 120 seconds or less, more preferably 90 seconds or less. In the above, the case where the oxidation treatment is performed while raising the temperature has been described, but the aspect of the oxidation treatment is not limited to this, and the oxidation treatment may be performed by raising the temperature to the target temperature and holding the target temperature.
[0053] (Reduction treatment) In the reduction treatment, a desired decarburized layer is formed on the surface layer of the steel sheet. In addition, when the steel sheet is a plated steel sheet, for example, a reduced Fe layer capable of forming a good plated layer is formed. In the manufacturing method according to the present embodiment, the reduction treatment is performed by first reduction treatment having a dew point of -35 to -15°C, followed by second reduction treatment having a dew point of -25 to 0°C, which is higher than that of the first reduction treatment. Hereinafter, the first reduction treatment and the second reduction treatment will be described respectively. (First reduction treatment) In the first reduction treatment, the dew point is set in the range of -35 to -15°C. If the dew point exceeds -15°C, decarburization tends to proceed more than necessary, which tends to lead to a decrease in strength. In addition, the reduction treatment does not proceed easily, and iron oxide produced in the oxidation treatment adheres to the rolls, which tends to cause a defect called pickup, which causes pressure marks on the steel sheet. Therefore, the dew point is set to -15°C or lower. The dew point is preferably -20°C or lower. On the other hand, from the viewpoint of suppressing additional equipment and costs, the dew point in the first reduction treatment is set to -35°C or higher. The dew point is preferably -30°C or higher.
[0054] The dew point may be within the above range in the atmosphere at the center of the front stage of the reduction zone where the first reduction treatment is performed. The dew point in the first reduction treatment and the second reduction treatment described below can be controlled, for example, by introducing water vapor gas and mixing it with the atmospheric gas in a furnace, or by bubbling the atmospheric gas to mix water vapor therein.
[0055] The atmosphere of the first reduction treatment may be an atmosphere that satisfies the above dew point and contains N2, H2, CO, H2O, O2, and other inevitable impurities. In the first reduction treatment, after the temperature of the steel sheet reaches 800°C in the atmosphere, the temperature may be held in a temperature range of 800 to 920°C for, for example, 60 to 240 seconds. The "holding" may be at a constant temperature or may be varied within the temperature range.
[0056] (Second reduction treatment) Next, the dew point of the second reduction treatment will be described. Figure 1-1 (No. 1-16) and Figure 1-2 (No. 17-22) are graphs created using the examples described later, and are graphs showing the relationship between the dew point at the center of the soaking zone during the second reduction treatment and R / t. From these Figures 1-1 and 1-2, it can be seen that in order to achieve excellent bendability with R / t of less than 2.5 as shown by the arrows in the figures, it is necessary to set the dew point in the second reduction treatment to -25°C or higher. Also, Figure 2-1 (No. 1-16) and Figure 2-2 (No. 17-22) are graphs created using the examples described later, and are graphs showing the relationship between the dew point at the center of the soaking zone during the second reduction treatment and tensile strength TS. From these Figures 2-1 and 2-2, it can be seen that by setting the dew point to 0°C or lower, a high strength of tensile strength TS of 980MPa or higher, or even 1180MPa or higher, can be secured. The dew point in the second reduction treatment is preferably -15°C or lower.
[0057] The atmosphere for the second reduction treatment may be an atmosphere that satisfies the above dew point and contains N2, H2, CO, H2O, O2, and other unavoidable impurities. In the second reduction treatment, the steel sheet may be held in the above atmosphere for, for example, 60 to 240 seconds in a temperature range in which the steel sheet reaches a temperature of 800 to 920°C. The "holding" may be at a constant temperature or may be varied within the above temperature range.
[0058] The first reduction treatment and the second reduction treatment may be performed in separate atmospheres having different dew points as described above, and the specific embodiment is not limited thereto. For example, a reduction furnace may be provided for performing each of the first reduction treatment and the second reduction treatment. In addition, when the steel sheet is a plated steel sheet, a partition wall having an opening area ratio of 20% or less may be provided in the middle of the reduction zone of the continuous hot-dip galvanizing line to separate the first reduction treatment from the second reduction treatment.
[0059] Between the first reduction treatment and the second reduction treatment, as long as there is no adverse effect on ensuring the decarburized state of the steel sheet according to this embodiment, for example, a holding step for holding at least one of the conditions of the first reduction treatment (dew point, heating temperature), for example, a cooling step for cooling to a temperature between the heating temperature of the first reduction treatment and room temperature, etc. are allowed. It is preferable to carry out the second reduction treatment subsequent to the first reduction treatment.
[0060] The oxidation treatment and reduction treatment may be carried out using any one or more known facilities. Preferably, from the viewpoints of production efficiency, cost, and quality maintenance, a continuous hot-dip galvanizing line (CGL) facility is used. By using a continuous hot-dip galvanizing line, the oxidation treatment and reduction treatment by the oxidation-reduction method, and the hot-dip galvanizing treatment and alloying treatment when manufacturing, for example, a galvanized steel sheet as a steel sheet, can be continuously carried out in a series of production lines. More specifically, the oxidation treatment and reduction treatment by the oxidation-reduction method can be carried out using, for example, an annealing furnace in a DFF-type continuous hot-dip galvanizing line. The oxidation treatment can be carried out, for example, in a heating zone in a DFF-type annealing furnace as described above. The reduction treatment can be carried out, for example, in a soaking zone in a DFF-type annealing furnace.
[0061] The method for producing the steel sheet (original sheet) to be annealed is not particularly limited. The steel sheet (original sheet) to be annealed can be obtained by melting and casting steel in a conventional manner to obtain a steel slab, and then subjecting the steel slab to a rolling process (hot rolling, cold rolling) in a conventional manner.
[0062] The manufacturing method according to the present embodiment may include the annealing step, and other steps are not limited. The steel sheet according to the present embodiment may be a cold-rolled steel sheet that has been annealed without undergoing any steps after the annealing. Alternatively, a plating step, such as a hot-dip galvanizing step and further an alloying step, may be provided after the annealing to obtain, for example, a hot-dip galvanized steel sheet (GI) or an alloyed hot-dip galvanized steel sheet (GA) as the steel sheet according to the present embodiment. Alternatively, an electric galvanizing step may be provided to obtain, for example, an electric galvanized steel sheet (EG) as the steel sheet according to the present embodiment.
[0063] The method for forming a zinc plating layer on the surface of the steel sheet after the annealing is not particularly limited, and a known method can be used as appropriate. For example, the base material after the annealing step can be immersed in a plating bath. When immersing in the plating bath, the plating coating weight can be reduced to, for example, 20 g / m by gas wiping or the like. 2More than 200g / m 2 It is preferable to suppress it to the following value.
[0064] The plating bath may be used for binary or higher alloy plating containing Zn, such as Al-Zn plating, Fe-Zn plating, Ni-Zn plating, Cr-Zn plating, Mg-Zn plating, etc.
[0065] The plating may be performed by using a plating bath containing components other than zinc at a concentration of, for example, 0.01% by mass to 0.5% by mass, and impregnating the material at a temperature of, for example, 300° C. to 600° C. for, for example, 1 second to 30 seconds. The alloying treatment is also not particularly limited, and a known method may be used as appropriate. For example, the alloying treatment may be performed by reheating the material at an alloying temperature of 470° C. to 600° C. for 1 second to 100 seconds. EXAMPLES
[0066] The present invention will be described in more detail below with reference to examples. The present invention is not limited to the following examples, and can be practiced with appropriate modifications within the scope of the above and below-mentioned aims, and all such modifications are included in the technical scope of the present invention.
[0067] As the annealing samples, Nos. 1 to 11 were prepared with a component composition in terms of bulk carbon concentration, i.e., the C content of the steel sheet (original sheet) was 0.22 mass%, the Si content was 1.7 mass%, the Mn content was 2.0 mass%, the Cr content was 0.5 mass%, the Al content was 0.04 mass%, and the balance was Fe and unavoidable impurities (note that "unavoidable impurities" here includes P, S, and N in amounts within the above-mentioned ranges), and the structure was ferrite + pearlite, and the original sheet had a strength of 700 to 800 MPa. For Nos. 12 to 16, the bulk carbon concentration was 0.13 mass% (0.13 mass% C), the Si content was 0.9 mass%, the Mn content was 2.3 mass%, the Cr content was 0.57 mass%, the Al content was 0.02 mass%, the balance was Fe and unavoidable impurities (note that "unavoidable impurities" here includes P, S, and N in the above-mentioned ranges), the structure was ferrite + pearlite, and the strength was 700 to 800 MPa. For Nos. 17 to 22, the bulk carbon concentration was 0.21 mass% (0.21 mass% C), the Si content was 1.8 mass%, the Mn content was 2.3 mass%, the Al content was 0.45 mass%, the balance was Fe and unavoidable impurities (note that "unavoidable impurities" here includes P, S, and N in the above-mentioned ranges), the structure was ferrite + pearlite, and the strength was 600 to 700 MPa.
[0068] The annealing sample was subjected to oxidation treatment and reduction treatment in an actual machine. In detail, oxidation treatment was performed at the oxygen concentration and ultimate temperature shown in Table 1, and then the first reduction treatment (heating zone) and second reduction treatment (soaking zone) shown in Table 1 were performed in this order under each condition (ultimate temperature, dew point) shown in Table 1. The conditions of the "first reduction zone" in Table 1 indicate the conditions of the first reduction treatment, and the conditions of the "second reduction zone" indicate the conditions of the second reduction treatment.
[0069] The steel sheet after the second reduction treatment was cooled to 460°C and then immersed in an Al-Zn plating bath containing 0.08 to 0.13 mass% of Al (Al is effective Al%, plating bath temperature is 460 to 480°C) to perform zinc plating. The coating weight of the plating was 40 g / m by gas wiping. 2 More than 90g / m 2The temperature was controlled as follows, and then alloying treatment was carried out at 480 to 490° C. for 20 to 30 seconds to obtain a galvannealed steel sheet.
[0070] [Table 1]
[0071] The obtained galvannealed steel sheets were evaluated as follows.
[0072] [Method for measuring decarburization behavior: Carbon profile measurement by GD-OES] As described below, the carbon profile was measured by GD-OES (Glow Discharge Optical Emission Spectrometry) to investigate the decarburization behavior.
[0073] (Sample preparation) Materials measuring 50 mm x 40 mm x thickness or 30 mm x 30 mm x thickness were collected. After that, samples were prepared by degreasing in the usual manner. Then, using the samples, the mass% concentration of each element was measured by GD-OES under the following conditions.
[0074] (Measurement conditions) Equipment used: Horiba, Ltd. Marcus type radio frequency glow discharge optical emission surface analyzer (rf-GD-OES) GD-Profiler2 Sputtering method: Normal sputtering Measurement range: φ4mm Gas type: Ar Analyzed elements: B, C, O, Al, Si, Ti, Cr, Mn, Fe, Zn, P, S, N (In this example, the evaluation was performed on these elements, but if elements other than the above are contained in, for example, the plating layer or steel sheet, the other elements will also be analyzed.)
[0075] (Measurement method) GD-OES measurements were performed on the plated surface of the sample up to a depth of 150 μm in the plate thickness direction.
[0076] (Analysis method) Since the sputtering rate of the above-mentioned device is almost constant, the sputtering crater depth of the sample was measured after the analysis was completed, and the value (sputtering depth) was plotted on the horizontal axis.
[0077] The details of the calibration curve method for converting the measured emission intensity of each element into a concentration are shown below. Sputter weight of element i per unit time W i (g / sec) and luminescence intensity I i The relationship is expressed by the following formula (1) using the slope a and intercept b of the calibration curve. W i =aI i +b...Formula (1) The sputter weight W of the above element i per unit time i is the concentration C i (wt.%), density ρ(g / cm 3 ), and the sputtering rate Δd (cm / sec) of the reference sample are known. 2 ) and is calculated using the following formula (2). W i =C i ×ρ×Δd×S··························Formula (2)
[0078] W i Using two or more reference samples with known emission intensities I i The slope a and intercept b of the above formula (1) were determined, and a calibration curve was created with the emission intensity on the horizontal axis and the sputter weight on the vertical axis. The reference samples used are shown in Table 2 below. Using the created calibration curve, the sputter weight was determined from the emission intensity of each target element, and the concentration was converted from the weight ratio. The calibration curve used to convert the O concentration was corrected using SiO2 so that the concentration ratio of Si to O was 1:2.
[0079] [Table 2]
[0080] Then, a carbon profile was obtained using the results of the carbon analysis. An example is shown in FIG. 3. FIG. 3 shows No. 2, which is a comparative example, and No. 10, which is an example of the present invention. In FIG. 3, the carbon profile of each material has a carbon concentration peak within 20 μm of the surface layer (specifically, in the internal oxide layer). However, while the carbon concentration is higher than the bulk carbon concentration in the comparative example, the carbon concentration in the example of the present invention is sufficiently lower than the bulk carbon concentration. Note that the bulk carbon concentration of the sample used in this example is 0.22 mass%, so the upper limit of the maximum carbon concentration (mass%) (vertical axis) in the region from the steel sheet surface to 20 μm is 0.22 mass%×70%=0.15 mass%.
[0081] From the obtained carbon concentration profile in the sheet thickness direction, the position where the carbon concentration (mass%) was 50% of the bulk carbon concentration, the position where the carbon concentration (mass%) was 90% of the bulk carbon concentration, and the maximum carbon concentration (mass%) in the region from the steel sheet surface to 20 μm were obtained. Note that the bulk carbon concentration was corrected for analysis so that the carbon concentration at a sufficiently deep position (120 to 150 μm) measured by GD-OES was the value obtained by normal steel analysis. For example, when the steel analysis value was 0.22% and the GD-OES analysis value was 0.25%, the GD-OES analysis value was multiplied by 0.22 / 0.25 and used for analysis.
[0082] The amount of decarburized surface layer per mm of plate thickness on one side of the steel plate was calculated as follows. The amount of decarburized carbon was calculated from the difference between the bulk carbon concentration and the carbon concentration profile of the steel plate (after decarburization). 2 For a steel plate, the volume of decarburized iron (m 3 ) × density (specific gravity) of iron (7.87 × 10 6 g / m 3 The total amount of decarburization was calculated by multiplying the ratio of decarburized carbon in the iron of the decarburized part by the atomic weight of carbon (g / mol). The total amount of decarburization was then divided by the plate thickness to obtain the amount of surface decarburization per mm of plate thickness on one side of the steel plate (mol / m 2 ) was sought.
[0083] [Evaluation of limit bending strength (R / t)] The bendability of the steel sheet was evaluated by the following procedure. A test piece with a width of 40 mm and a length of 100 mm was prepared with the direction perpendicular to the rolling direction as the major axis, and a bending test was performed by the V-block method in accordance with JIS Z 2248:2014. In the bending test, the bending radius was changed from 0 to 7 mm to obtain the minimum bending radius at which the material could be bent without breaking, and the limit bending radius R (mm) / sheet thickness t (mm) was calculated using this limit bending radius R (mm). Then, when the limit bending radius R (mm) / sheet thickness t (mm) was less than 2.5, it was evaluated as having excellent bendability, and when it was 2.5 or more, it was evaluated as having poor bendability.
[0084] [Measurement of tensile strength (TS)] TS (tensile strength) was measured by taking a JIS No. 5 tensile test piece from the steel plate so that the direction perpendicular to the rolling direction of the steel plate was the longitudinal direction, according to the method specified in JIS Z 2241: 2011. TS (tensile strength) of 980 MPa or more was evaluated as high strength (preferably 1180 MPa or more is higher strength), and TS less than 980 MPa was evaluated as poor strength.
[0085] [Evaluation of plating properties] The appearance of the plated steel sheet samples was visually observed. If adhesion of dross due to the presence of selective oxides of Si and Mn, which have a detrimental effect on plating formation, was confirmed, the plateability was evaluated as poor (×), and if not, the plateability was evaluated as excellent (○). The results are shown in Table 3.
[0086] [Table 3]
[0087] Based on the results of Table 3 above, graphs showing the relationship between the position where the carbon concentration (mass%) in the thickness direction is 50% of the bulk carbon concentration and R / t are shown in Figure 4-1 (Nos. 1 to 16) and Figure 4-2 (Nos. 17 to 22). From Figures 4-1 and 4-2, it can be seen that in order to achieve excellent bendability with an R / t of less than 2.5, as shown by the arrows in the figures, it is sufficient to ensure that the position where the carbon concentration (mass%) in the thickness direction is 50% of the bulk carbon concentration is in a region 0.20% or more of the thickness from the steel sheet surface.
[0088] Based on the results of Table 3, graphs showing the relationship between the position where the carbon concentration (mass%) in the sheet thickness direction is 90% of the bulk carbon concentration and the tensile strength TS are shown in Figure 5-1 (Nos. 1 to 16) and Figure 5-2 (Nos. 17 to 22). It can be seen from Figures 5-1 and 5-2 that if the position where the carbon concentration (mass%) in the sheet thickness direction is 90% of the bulk carbon concentration is in a region 8.0% or less of the sheet thickness from the steel sheet surface, a high strength of tensile strength TS of 980 MPa or more, preferably 1180 MPa or more can be ensured.
[0089] Based on the results of Table 3 above, graphs showing the relationship between the ratio of the maximum carbon concentration (mass%) in the region from the steel sheet surface to 20 μm to the bulk carbon concentration and R / t are shown in Figure 6-1 (Nos. 1 to 16) and Figure 6-2 (Nos. 17 to 22). From Figures 6-1 and 6-2, it can be seen that in order to achieve excellent bendability with an R / t of less than 2.5, as shown by the arrows in the figures, it is preferable to set the ratio of the maximum carbon concentration (mass%) in the region from the steel sheet surface to 20 μm to the bulk carbon concentration to less than 70%.
[0090] Based on the results of Table 3 above, graphs showing the relationship between the amount of surface decarburization per mm of plate thickness on one side of the steel plate and the tensile strength TS are shown in Figure 7-1 (No. 1-16) and Figure 7-2 (No. 17-22). From Figure 7-1 and Figure 7-2, it can be seen that the amount of surface decarburization per mm of plate thickness is 0.045 mol / m 2 Less than or equal to 0.035 mol / m 2It can be seen that a high strength of tensile strength TS of 980 MPa or more, preferably 1180 MPa or more, can be ensured if the content is less than 0.028 mol / m 2 By making it so that the above-mentioned temperature is satisfied, a higher tensile strength TS of 1200 MPa or more can be achieved.
[0091] In Table 3, Nos. 1 to 4 and 22 did not have the surface layer of the steel plate defined in this embodiment and were poor in bendability. Nos. 5 to 21 had the surface layer of the steel plate defined in this embodiment and were able to achieve both high strength and excellent bendability. It can be seen that, in order to ensure excellent galvanizability as the properties of the steel plate in addition to high strength and excellent bendability, it is preferable to carry out an oxidation treatment under specified conditions in the manufacturing process, as in Nos. 9 to 21.
[0092] The disclosure of this specification may include the following aspects. Aspect 1 of the present invention is In the plate thickness direction, The position where the carbon concentration (mass%) is 50% of the bulk carbon concentration is in a region that is 0.20% or more of the plate thickness from the steel plate surface, and The position where the carbon concentration (mass %) is 90% of the bulk carbon concentration is in a region of the steel plate that is 8.0% or less of the plate thickness from the surface of the steel plate. Aspect 2 of the present invention is The maximum carbon concentration (mass%) in the region from the steel sheet surface to 20 μm in the sheet thickness direction is less than 70% of the bulk carbon concentration, and The amount of surface decarburization per 1 mm of plate thickness on one side of the steel plate is 0.035 mol / m 2 The steel sheet according to embodiment 1 is as follows: Aspect 3 of the present invention is 3. The steel sheet according to claim 1 or 2, having a tensile strength of 1180 MPa or more. A fourth aspect of the present invention is The composition of the components is C: 0.08% by mass or more and 0.30% by mass or less Si: More than 0.5% by mass and 3.0% by mass or less Mn: 1.5% by mass or more and 3.0% by mass or less Cr: more than 0 mass%, 1.0 mass% or less P: More than 0% by mass and 0.1% by mass or less S: More than 0% by mass, 0.05% by mass or less Al: more than 0 mass% and 1.0 mass% or less, and N: More than 0% by mass and 0.01% by mass or less; The steel sheet according to any one of Aspects 1 to 3, wherein the balance is Fe and unavoidable impurities. A fifth aspect of the present invention is The annealing process includes an oxidation process at an oxygen concentration of 0.1 to 2% and a temperature of 650 to 750°C, followed by a reduction process. The reduction treatment is a method for producing a steel sheet, which includes a first reduction treatment having a dew point of -35 to -15°C, followed by a second reduction treatment having a dew point of -25 to 0°C, which is higher than that of the first reduction treatment. A sixth aspect of the present invention is In the method for producing a steel sheet according to aspect 5, the ultimate temperature in the first reduction treatment and the second reduction treatment is 800 to 920°C.
Claims
1. In the plate thickness direction, The position where the carbon concentration (mass%) is 50% of the bulk carbon concentration is in a region that is 0.20% or more of the sheet thickness from the steel sheet surface, and A steel plate in which the position where the carbon concentration (mass %) is 90% of the bulk carbon concentration is in a region that is 8.0% or less of the plate thickness from the surface of the steel plate.
2. The maximum carbon concentration (mass%) in a region from the steel sheet surface to 20 μm in the sheet thickness direction is less than 70% of the bulk carbon concentration, and The amount of surface decarburization per 1 mm of plate thickness on one side of the steel plate is 0.045 mol / m 2 The steel sheet according to claim 1 , wherein:
3. The steel plate according to claim 1 or 2, having a tensile strength of 980 MPa or more.
4. The composition of the components is C: 0.08% by mass or more, 0.30% by mass or less, Si: more than 0.5 mass%, 3.0 mass% or less, Mn: 1.5% by mass or more, 3.0% by mass or less, Cr: 0 mass% or more, 1.0 mass% or less, P: more than 0 mass%, 0.1 mass% or less, S: more than 0 mass%, 0.05 mass% or less, Al: more than 0 mass% and 1.0 mass% or less, and N: more than 0 mass% and 0.01 mass% or less; The steel sheet according to claim 1 or 2, wherein the balance is Fe and unavoidable impurities.
5. The annealing process includes an oxidizing process under conditions of an oxygen concentration of 0.1 to 2% and an ultimate temperature of 650 to 750°C, followed by a reducing process. The reduction treatment includes a first reduction treatment having a dew point of −35 to −15° C., and then a second reduction treatment having a dew point of −25 to 0° C., which is higher than the dew point of the first reduction treatment.
6. The method for producing a steel sheet according to claim 5, wherein the temperature achieved in the first reduction treatment and the second reduction treatment is 800 to 920°C.
Citation Information
Patent Citations
Method of manufacturing high-strength hot-dip galvanized steel plate
JP2017166057A