Plated steel sheet, and method for manufacturing the same
A plated steel sheet with a specific composition and controlled cooling process addresses the complexity of existing manufacturing methods, achieving high strength and workability, contributing to reduced vehicle weight and improved safety.
Patent Information
- Application Number
- JP2024022773
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-02-19
- Publication Date
- 2024-10-11
AI Technical Summary
Existing plated steel sheets for automobile bodies require complex manufacturing methods to achieve high strength and workability, leading to potential instability in production and room for improvement in strength and workability.
A plated steel sheet with a specific composition and metal structure, including C, Si, Mn, Cr, Ti, and B, and controlled cooling rates during manufacturing, resulting in a steel plate with a tensile strength of 1150 MPa or more and high workability, achieved through controlled cooling rates and a metal structure comprising bainite, tempered martensite, retained austenite, and limited polygonal ferrite and bainitic ferrite.
The solution enables the production of a plated steel sheet with high strength, improved workability, and reduced weight, facilitating easier manufacturing and enhanced vehicle body performance.
Smart Images

Figure 2024144150000007 
Figure 2024144150000008 
Figure 2024144150000009
Abstract
Description
[Technical field]
[0001] The present disclosure relates to plated steel sheets and methods for producing the same. [Background technology]
[0002] There has been a demand for improved safety for vehicle occupants, and for this purpose, the strength of the materials used in vehicle bodies has been improved. On the other hand, against the background of the worsening of global warming and other issues, there has been an accelerating movement to improve the fuel efficiency of automobiles. It is known that reducing the weight of vehicle bodies is an effective way to improve fuel efficiency.
[0003] Galvanized steel sheets used in automobile bodies are required to have high strength (e.g., tensile strength of 1150 MPa or more) in order to reduce the weight of the vehicle body. Furthermore, because the plated steel sheets need to be processed into the shape of parts, the plated steel sheets are required to have high formability (high elongation EL, high hole expansion ratio λ, etc.).
[0004] Patent Documents 1 and 2 disclose plated steel sheets that contain C, Si, and Mn as essential components and have a specified metal structure, thereby exhibiting high ductility and high strength. Patent Document 3 discloses a plated steel sheet that contains at least one selected from C, Si, Mn, Al, and V, Mo, Ti, and Nb as essential components and has a predetermined metal structure, thereby exhibiting high ductility and high workability (high λ, etc.). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. WO2020 / 080402 [Patent Document 2] International Publication No. WO2020 / 080401 [Patent Document 3] International Publication No. WO2019 / 159771 Summary of the Invention [Problem to be solved by the invention]
[0006] In Patent Documents 1 to 3, the manufacturing method, particularly the cooling after reheating after hot rolling (and after cold rolling), is strictly controlled in order to obtain the desired performance. For example, in Patent Document 1, it is necessary to control or maintain the cooling rate within at least six temperature ranges (810 to 700°C, 700 to 490°C, 490 to 405°C, 405 to 310°C, 315 to 255°C, and 255°C to the cooling stop temperature (254 to 220°C). In Patent Document 2, the cooling rate needs to be controlled or maintained in at least five temperature ranges (810 to 650°C, 650 to 505°C, 505 to 405°C, 405 to 315°C, and 315 to the cooling stop temperature (310 to 255°C)). In Patent Document 3, the cooling rate needs to be controlled or maintained in at least four temperature ranges (830 to 550° C. or less, Ac1+60° C. to 550° C., 550 to 400° C., and 375 to 150° C.). As described above, in the plated steel sheets disclosed in Patent Documents 1 to 3, the manufacturing methods for achieving high strength and high formability are complicated, and there is a concern that, for example, stable production cannot be achieved, etc. Furthermore, there is room for improvement in terms of strength and formability.
[0007] The present invention has been made in view of the above circumstances, and one of its objectives is to provide a plated steel sheet that can be produced more easily, has high strength, can contribute to weight reduction of a vehicle body, and exhibits high formability, and a method for producing the same. [Means for solving the problem]
[0008] Aspect 1 of the present invention is A plated steel sheet comprising a steel sheet and a plating layer disposed on a surface of the steel sheet, the plated steel sheet having a tensile strength of 1150 MPa or more, The steel sheet included in the plated steel sheet is C: 0.150~0.250% by mass, Si: 0.80~2.20% by mass, Mn: 1.50~2.80% by mass, Cr:0.15~1.50% by mass, Ti:0.012~0.100% by mass, B:0.0015~0.0100% by mass, P: 0.100% by mass or less (including 0% by mass), S: 0.050% by mass or less (including 0% by mass), Al: 0.005~1.000% by mass, N: 0.0100% by mass or less (including 0% by mass), and The balance is composed of iron and inevitable impurities, and The metal structure has a total of bainite and tempered martensite of 95% by area or less, retained austenite of 5% by volume or more, a total of polygonal ferrite and bainitic ferrite of 5% by area or less, and a remaining structure of 5% by area or less. It is plated steel sheet.
[0009] Aspect 2 of the present invention is In the plate thickness direction, In the plated steel sheet according to aspect 1, the position where the carbon concentration (mass %) is 50% of the bulk carbon concentration is in a region that is 0.2% or more of the sheet thickness from the surface of the steel sheet.
[0010] Aspect 3 of the present invention is A plated steel sheet according to aspect 1 or 2, wherein a maximum carbon concentration (mass %) in a region extending from the surface of the steel sheet to 20 μm in the sheet thickness direction is less than 70% of a bulk carbon concentration.
[0011] A fourth aspect of the present invention is The retained austenite is Contains 10 to 50 volume % of first retained austenite having a solute C content of 0.9 mass % or less, and The plated steel sheet according to any one of Aspects 1 to 3, comprising 10 to 50 volume % of second retained austenite having a solute C content of more than 0.9 mass % and not more than 1.1 mass %.
[0012] A fifth aspect of the present invention is A step of hot rolling a steel having the composition according to embodiment 1 to obtain a rolled plate; Heating the rolled plate to a first heating temperature of 850° C. or more; After the heating step, maintaining the first heating temperature for 50 seconds or more; After the holding step, a step of cooling to a cooling stop temperature of 200 to 350 ° C., wherein the average cooling rate from the first heating temperature to 550 ° C. is 5 ° C. / sec or more, and the average cooling rate from 550 ° C. to the cooling stop temperature is 1 ° C. / sec or more; After the cooling step, a step of heating to a second heating temperature of 300°C to 450°C and holding the temperature for 50 to 1000 seconds to obtain a steel sheet; forming a plating layer on the steel sheet; The method for producing the plated steel sheet according to any one of aspects 1 to 4 includes the steps of:
[0013] A sixth aspect of the present invention is After the step of obtaining the rolled plate, an oxidation treatment is performed under conditions of an oxygen concentration of 0.1 to 2% and an ultimate temperature of 650 to 750 ° C., The production method according to aspect 5, wherein the holding step includes a first reduction treatment having a dew point of −35 to −15° C., followed by a second reduction treatment having a dew point of −25 to 0° C., which is higher than the dew point of the first reduction treatment.
[0014] A seventh aspect of the present invention is In the method according to aspect 5 or 6, the cooling step is performed at an average cooling rate of 400° C. / sec or less from 400° C. to the cooling stop temperature. Effect of the Invention
[0015] According to the embodiments of the present invention, it is possible to provide a plated steel sheet that can be manufactured more easily, has high strength, contributes to weight reduction of a vehicle body, and exhibits high formability, and a manufacturing method thereof. [Brief description of the drawings]
[0016] [Figure 1]FIG. 1 is a graph showing the relationship between the dew point at the center of the soaking zone and R / t during the second reduction treatment. [Diagram 2] FIG. 2 is a schematic diagram of an X-ray diffraction pattern. [Diagram 3] FIG. 3 is a diagram showing an example of a carbon concentration profile obtained in an example. [Figure 4] FIG. 4 is a graph showing the relationship between R / t and the position where the carbon concentration (mass %) in the sheet thickness direction is 50% of the bulk carbon concentration. [Diagram 5] FIG. 5 is a graph showing the relationship between the ratio of the maximum carbon concentration (mass %) in the region from the steel sheet surface to 20 μm deep, relative to the bulk carbon concentration, and R / t. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The present inventors have conducted research from various angles in order to realize a plated steel sheet that can be more easily manufactured and exhibits high strength (tensile strength TS of 1150 MPa or more, yield stress YS of 850 MPa or more) and high formability (elongation EL of 14% or more, hole expansion ratio λ of 30% or more). As a result, a plated steel sheet exhibiting high strength and high formability has been realized by using a steel sheet containing a predetermined component composition, particularly Cr, Ti and B in predetermined amounts as essential components, and further having a predetermined metal structure. At the same time, the inventors have also found that the plated steel sheet can be manufactured by an easier manufacturing method in which the cooling rate is controlled within two temperature ranges (first heating temperature to 550°C, 550°C to cooling stop temperature) in cooling after reheating after hot rolling (and cold rolling) which is fewer than that of the conventional technology. The following provides details of each requirement stipulated by the embodiment of the present invention.
[0018] <1. Plated steel sheet> The plated steel sheet according to the embodiment of the present invention includes a steel sheet and a plating layer disposed on the surface of the steel sheet. The plating layer may be a zinc-based plating layer such as a hot-dip galvanized layer, a galvannealed hot-dip galvanized layer or an electrogalvanized layer, or an aluminum plating layer such as a hot-dip aluminum plating layer. The zinc-based plating layer may be a zinc-based alloy plating layer such as zinc-Ni, zinc-Fe, or zinc-Al. The plating layer may be formed on at least one surface (e.g., a rolled surface) of the steel sheet, may be formed on both opposing surfaces, or may be formed on the entire surface of the steel sheet. Specific examples of the plated steel sheet including the zinc-based plating layer include hot-dip galvanized steel sheet (GI), alloyed hot-dip galvanized steel sheet (GA), and electrogalvanized steel sheet (EG).
[0019] <2. Composition of steel sheets contained in plated steel sheets> The steel sheet included in the plated steel sheet according to an embodiment of the present invention (which may be, for example, a portion of the plated steel sheet excluding the plating layer) preferably contains C: 0.150 to 0.250 mass%, Si: 0.80 to 2.20 mass%, Mn: 1.50 to 2.80 mass%, Cr: 0.15 to 1.50 mass%, Ti: 0.012 to 0.100 mass%, B: 0.0015 to 0.0100 mass%, P: 0.100 mass% or less (including 0 mass%), S: 0.050 mass% or less (including 0 mass%), Al: 0.005 to 1.000 mass%, N: 0.0100 mass% or less (including 0 mass%), with the remainder being iron and unavoidable impurities. Each component will be described in detail below.
[0020] (C:0.150~0.250% by mass) C is an important element for improving the strength of steel. C is also an important element for stabilizing austenite and securing residual γ. Furthermore, C also has the effect of suppressing the formation of polygonal ferrite during cooling from high temperature. In order to exert this effect, the C content is 0.150 mass% or more, preferably 0.170 mass% or more, and more preferably 0.190 mass% or more. On the other hand, since an excessive C content deteriorates the weldability, the C content is 0.250 mass% or less, preferably 0.240 mass% or less, and more preferably 0.230 mass% or less.
[0021] (Si:0.80~2.20% by mass) Si is an element that contributes to increasing the strength of steel as a solid solution strengthening element. Si also has the effect of improving temper softening resistance and suppressing the softening of martensite during tempering. In addition, Si has the effect of suppressing the generation of carbides, condensing and stabilizing C in austenite, and is an important element for securing residual γ. In order to exert this effect, the Si content is 0.80 mass% or more, preferably 1.00 mass% or more, and more preferably 1.20 mass% or more. On the other hand, if Si is contained excessively, a large amount of scale is formed during hot rolling, and the surface condition is deteriorated, such as scale marks on the steel sheet surface. Therefore, the Si content is 2.20 mass% or less, preferably 2.00 mass% or less, and more preferably 1.80 mass% or less.
[0022] (Mn:1.50~2.80% by mass) Mn is an important element that not only increases the strength of steel but also directly contributes to the stabilization of austenite. It is also an element that improves hardenability and has the effect of suppressing the formation of polygonal ferrite. In order to achieve this effect, the Mn content is 1.50 mass% or more, preferably 1.70 mass% or more, and more preferably 1.90 mass% or more. On the other hand, if Mn is contained excessively, it causes adverse effects such as the occurrence of cracks in the cast slab, so the Mn content is 2.80 mass% or less, preferably 2.70 mass% or less, more preferably 2.60 mass% or less, and even more preferably 2.20 mass% or less.
[0023] (Cr:0.15~1.50% by mass) Cr is an element that suppresses the formation of polygonal ferrite and vetic ferrite during cooling from high temperature. Furthermore, Cr is one of the important elements because it improves tempering softening resistance and also has the effect of suppressing the softening of martensite during tempering and the decomposition of residual γ during alloying treatment. In order to achieve the above-mentioned effect, the Cr content is 0.15 mass% or more, preferably 0.17 mass% or more, and more preferably 0.20 mass% or more. On the other hand, if Cr is contained excessively, not only the effect is saturated but also the formability is deteriorated, so the Cr content is 1.50 mass% or less, preferably 1.20 mass% or less, and more preferably 1.00 mass% or less.
[0024] (Ti:0.012~0.100% by mass) Ti refines the metal structure and contributes to improving the strength and toughness of the steel sheet. Furthermore, it is one of the important elements that binds with solute N to prevent the formation of BN. In order to achieve the above-mentioned effects, the Ti content is set to 0.012 mass% or more, preferably 0.014 mass% or more, and more preferably 0.016 mass% or more. On the other hand, if Ti is contained excessively, not only the above-mentioned effects are saturated, but also the yield ratio increases and shape fixability deteriorates, so the Ti content is set to 0.100 mass% or less, preferably 0.080 mass% or less, and more preferably 0.060 mass% or less.
[0025] (B:0.0015~0.0100% by mass) B is one of the important elements that suppresses the formation of polygonal ferrite and vetic ferrite during cooling from high temperature. In order to exert the above-mentioned effect, the B content is 0.0015 mass% or more, preferably 0.0017 mass% or more, and more preferably 0.0020 mass% or more. On the other hand, if B is contained excessively, not only the effect is saturated but also the formability is deteriorated, so the B content is 0.0100 mass% or less, preferably 0.0080 mass% or less, and more preferably 0.0060 mass% or less.
[0026] (P: 0.100% by mass or less (including 0% by mass)) P is an element that is inevitably present as an impurity element. P is an element that promotes grain boundary embrittlement due to grain boundary segregation and deteriorates formability. Therefore, the less P, the better, and the P content is 0.100 mass% or less, preferably 0.080 mass% or less, and more preferably 0.050 mass% or less. In this specification, "including 0 mass%" means that it includes embodiments in which it is not added intentionally, i.e., the content is below the unavoidable impurity level (it does not exclude the case where it is added intentionally).
[0027] (S: 0.050% by mass or less (including 0% by mass)) S is an element that is inevitably present as an impurity element. S is an element that forms sulfide-based inclusions such as MnS, which become the starting point of cracks and deteriorate the formability. Therefore, the less S, the better, and the S content is 0.050 mass% or less, preferably 0.030 mass% or less, and more preferably 0.020 mass% or less.
[0028] (Al: 0.005~1.000% by mass) Al is an element that acts as a deoxidizer, and in order to exert this effect, the Al content is set to 0.005% by mass or more, preferably 0.010% by mass or more, more preferably 0.020% by mass or more, and further preferably 0.030% by mass or more. On the other hand, if Al is contained excessively, a large amount of inclusions such as alumina is generated in the steel sheet, deteriorating the formability, so the Al content is set to 1.000% by mass or less, preferably 0.800% by mass or less, and more preferably 0.500% by mass or less.
[0029] (N: 0.0100% by mass or less (including 0% by mass)) N is an element that is inevitably present as an impurity element. N forms nitrides, which become the starting point of cracks and deteriorate the formability. Therefore, the less N, the better, and the N content is 0.0100 mass% or less, preferably 0.0080 mass% or less, and more preferably 0.0060 mass% or less.
[0030] The steel sheet included in the plated steel sheet according to the embodiment of the present invention preferably contains the above-mentioned composition, and in one embodiment of the present invention, the balance is preferably iron and inevitable impurities. As inevitable impurities, the inclusion of elements brought in due to the conditions of raw materials, materials, manufacturing facilities, etc. is permitted. Note that, for example, there are elements such as P, S, and N, which are usually preferable to have a lower content and therefore are inevitable impurities, but whose composition ranges are separately specified as above. For this reason, in this specification, the "unavoidable impurities" that constitute the balance are a concept that excludes elements whose composition ranges are separately specified.
[0031] <3. Metal structure of steel sheets contained in plated steel sheets> The metal structure of the steel sheet included in the plated steel sheet according to the embodiment of the present invention has a total of 95 area % or less of bainite and tempered martensite, 5 volume % or more of retained austenite, 5 area % or less of the total of polygonal ferrite and bainitic ferrite, and 5 area % or less of the remaining structure. Each structure will be described below.
[0032] (The total area % of bainite and tempered martensite is 95% or less) Bainite and tempered martensite are metal structures necessary for ensuring strength. However, if these metal structures are contained in excess, workability such as elongation decreases, so the total of bainite and tempered martensite is set to 95 area % or less, preferably 92 area % or less, and more preferably 90 area % or less. The lower limit of the total of these structures is preferably 50 area % or more, more preferably 60 area % or more, and even more preferably 70 area % or more.
[0033] (Residual austenite is 5% or more by volume) Retained austenite (hereinafter sometimes referred to as "retained γ") is mainly present between the laths in the metal structure, but can also exist in the form of clumps in aggregates of lath-like structures (e.g., blocks or packets) and on the grain boundaries of prior γ. This retained γ exhibits high workability such as high elongation by transforming into martensite when the steel sheet is strained and deformed. In other words, the inclusion of retained γ promotes hardening of the parts that are strained and deformed, and prevents strain concentration. These effects are generally called the TRIP effect, and contribute to the realization of a balance between high strength and high workability. In order to exert the TRIP effect, the residual γ is 5 volume % or more, preferably 6 volume % or more, and more preferably 7 volume % or more, relative to the entire metal structure. The upper limit of the structure is not particularly limited, but may be 40 area % or less, 30 area % or less, or 20 area % or less.
[0034] The amount of solute C in the residual γ can be an index that affects the stability of martensitic transformation of the residual γ during deformation, and by containing a predetermined amount of both the residual γ with a relatively low amount of solute C and the residual γ with a relatively high amount of solute C, it becomes easier to achieve a desired elongation. According to one embodiment of the present invention, the residual γ preferably contains 10 to 50 volume % of the residual γ with a solute C amount of 0.9 mass % or less (hereinafter also referred to as "first residual γ") and 10 to 50 volume % of the residual γ with a solute C amount of more than 0.9 mass % and 1.1 mass % or less (hereinafter also referred to as "second residual γ"). More preferably, the residual γ contains 15 to 50 volume % of both the first residual γ and the second residual γ.
[0035] (The total of polygonal ferrite and bainitic ferrite is 5% or less by area) Polygonal ferrite and bainitic ferrite are soft structures that can cause a decrease in strength and, in some cases, can also reduce the hole expansion ratio λ. Therefore, the total of these structures is 5 area % or less, preferably 3 area % or less, and more preferably 1 area % or less, relative to the entire metal structure. The lower limit of the total of these structures is not particularly limited and may be 0 area %.
[0036] (Residual tissue is less than 5% by area) In order to ensure high strength and high workability, the remaining structure, such as fresh martensite and pearlite, must be 5% by area or less in total. There is no particular lower limit for the remaining structure, and it may be 0% by area.
[0037] The method for measuring the area ratio (or volume ratio) of the metal structure is the method described in the Examples below.
[0038] <4. Mechanical properties of plated steel sheets> The plated steel sheet according to the present embodiment can exhibit high strength (high tensile strength, high yield stress) and high workability (high elongation, high hole expansion ratio). In this specification, a plated steel sheet having a tensile strength TS of 1150 MPa or more and a yield stress YS of 850 MPa or more is defined as a high-strength plated steel sheet. In addition, in this specification, a plated steel sheet having an elongation EL of 14% or more and a hole expansion ratio λ of 30% or more is defined as a high-workability plated steel sheet. The tensile strength is preferably 1180 MPa or more. The yield stress is preferably 900 MPa or more. The elongation EL is preferably 15% or more. The hole expansion ratio λ is preferably 35% or more.
[0039] The thickness of the steel sheet included in the plated steel sheet according to the present embodiment is not particularly limited. The thickness of the steel sheet included in the plated steel sheet according to the present embodiment may be, for example, 0.8 mm or more and 2.3 mm or less. The coating weight of the plated steel sheet according to the present embodiment is not particularly limited, and may be, for example, 10 to 100 g / m per side. 2 The extent of the problem can be mentioned as follows.
[0040] <5. Decarburized layer on the surface of plated steel sheets> The steel sheet included in the plated steel sheet according to this embodiment is (I) In the sheet thickness direction, the position where the carbon concentration (mass %) is 50% of the bulk carbon concentration is preferably in a region of 0.2% or more of the sheet thickness from the surface of the steel sheet. The position relates to the thickness of the decarburized layer that contributes to bendability. By ensuring that the position is in a region of 0.2% or more of the sheet thickness from the surface of the steel sheet and that the decarburized layer that contributes to bendability has a certain thickness or more, it is possible to reliably exhibit excellent bendability in bending. The position where the carbon concentration (mass %) is 50% of the bulk carbon concentration may be in a region of 0.5% or more, or even 1.0% or more of the sheet thickness from the surface of the steel sheet.
[0041] The steel sheet included in the plated steel sheet according to this embodiment is (II) The maximum carbon concentration (mass%) in the region from the steel sheet surface to 20 μm in the sheet thickness direction is preferably less than 70% of the bulk carbon concentration. When the present inventors checked steel sheets included in conventional plated steel sheets, they first found that there is a region with a significantly high carbon concentration in the surface layer of the steel sheet, which is the cause of deterioration of bendability. Then, as described below, they investigated the manufacturing conditions of the steel sheet and found that excellent bendability can be obtained by promoting decarburization of the surface layer of the steel sheet to suppress the carbon concentration in the surface layer of the steel sheet, specifically, by suppressing the maximum carbon concentration (mass%) in the region from the steel sheet surface to 20 μm in the sheet thickness direction to less than 70% of the bulk carbon concentration. The maximum carbon concentration is preferably 65% or less of the bulk carbon concentration, and more preferably 60% or less of the bulk carbon concentration.
[0042] From the viewpoint of exhibiting excellent bendability, the plated steel sheet according to this embodiment preferably satisfies at least one of the above (I) and (II), and more preferably satisfies both of the above (I) and (II).
[0043] The "surface of the steel sheet" refers to the position of the interface between the plating layer and the steel sheet. In the case of a zinc-based plating, for example, the position of the interface between the plating layer and the steel sheet refers to the point where Zn constituting the plating layer is no longer detectable (the analytical value of Zn is 0) when Zn is analyzed from the surface of the plating layer in the thickness direction of the plating layer by GD-OES measured in the examples described later, and this point is defined as the starting point of the distance (depth) from the steel sheet surface.
[0044] The plated steel sheet according to this embodiment has high tensile strength (1150 MPa or more), high yield stress (850 MPa or more), high elongation (14% or more), and high hole expansion ratio (30% or more), and further, when subjected to a bending test shown in the examples described later, can exhibit excellent bendability with R / t of less than 2.5.
[0045] <6. Manufacturing method of plated steel sheets> A method for producing a plated steel sheet according to an embodiment of the present invention includes: (A) hot rolling a steel having the above-mentioned composition to obtain a rolled plate; (B) heating the rolled plate to a first heating temperature of 850°C or higher; (C) maintaining the first heating temperature for 50 seconds or more; (D) after the holding step, a step of cooling to a cooling stop temperature of 200 to 350 ° C., wherein the average cooling rate from the first heating temperature to 550 ° C. is 5 ° C. / sec or more, and the average cooling rate from 550 ° C. to the cooling stop temperature is 1 ° C. / sec or more; (E) after the cooling step, a step of heating to a second heating temperature of 300°C to 450°C and holding the temperature for 50 to 1000 seconds to obtain a steel sheet; (F) forming a plating layer on the steel sheet; Each step will be described in detail below.
[0046] (A) Process for obtaining rolled plate The steel having the above-mentioned composition is melted and cast by a commonly used method, and the steel (steel slab) is subjected to a hot rolling process by a commonly used method to obtain a rolled plate. As an example, the steel (steel slab) having the above-mentioned composition cast by a continuous casting method, an ingot method, a thin slab casting method, or the like may be reheated to about 1150 to 1300°C, hot rolled to a finish rolling temperature of about 850 to 950°C, and coiled at about 500 to 700°C to obtain a rolled plate.
[0047] If necessary, the rolled plate may be pickled by a conventional method to remove surface scale, and if necessary, the rolled plate may be further subjected to cold rolling by a conventional method.
[0048] (B) A step of heating the rolled plate to a first heating temperature The rolled sheet is heated to a first heating temperature of 850° C. or more. By setting the first heating temperature at 850° C. or more, recrystallization can be promoted and the metal structure can be homogenized. The upper limit of the first heating temperature is not particularly limited, but may be, for example, 1000° C. or less.
[0049] (C) maintaining the first heating temperature. The rolled sheet is held at the first heating temperature for 50 seconds or more. By holding at the first heating temperature for 50 seconds or more, recrystallization can be promoted and the metal structure can be homogenized. The upper limit of the holding time is not particularly limited, and may be, for example, 30 minutes or less from the viewpoint of productivity.
[0050] After step (A), the method preferably includes an oxidation treatment (hereinafter also referred to as "step (B1)") under conditions of an oxygen concentration of 0.1 to 2% and an ultimate temperature of 650 to 750°C, and the method preferably includes a reduction treatment (hereinafter also referred to as "step (C1)") in which the first reduction treatment is performed at a dew point of -35 to -15°C, and then the second reduction treatment is performed at a dew point of -25 to 0°C, which is higher than the dew point of the first reduction treatment. For example, the oxidation treatment in step (B1) may be performed after step (A) and before step (B), or may be performed during the temperature rise to the first heating temperature in step (B) (i.e., step (B) may include the oxidation treatment in step (B1)). The reduction treatment in step (C1) may be performed during the holding at the first heating temperature in step (C).
[0051] By subjecting the surface of the steel sheet to the oxidation treatment in step (B1), an Fe oxide layer can be formed on the surface of the steel sheet. Then, by performing the reduction treatment in step (C1) in a reducing atmosphere, a decarburized layer can be formed on the surface layer of the steel sheet, while a reduced Fe layer capable of forming, for example, a good plating layer can be formed. The inventors have conducted research and found that, by performing the oxidation treatment as described above and determining the ranges of the dew points of the first reduction treatment and the second reduction treatment in the reduction treatment, and setting the dew point of the second reduction treatment higher than the dew point of the first reduction treatment, the carbon concentration of the surface layer of the steel sheet described above, which can realize not only high tensile strength, high yield stress, high elongation and high hole expansion ratio, but also excellent bendability, can be easily ensured. Each step of the oxidation treatment and the reduction treatment will be described below.
[0052] (B1) Oxidation treatment The oxidation treatment is preferably carried out under conditions of an oxygen concentration of 0.1 to 2%. From the viewpoint of obtaining an excellent coating appearance, the oxygen concentration is preferably 0.1% or more, more preferably 0.15% or more, and even more preferably 0.2% or more. On the other hand, if the oxygen concentration is too high, excessive oxidation causes oxide scale to adhere to the rolls in the furnace, which causes indentation marks on the steel sheet, and this is prone to cause defects known as pick-up. From the viewpoint of suppressing the occurrence of such defects, the oxygen concentration is preferably 2% or less, more preferably 1.7% or less, and even more preferably 1.5% or less. The concentrations of elements other than oxygen are not particularly limited. For example, together with the above-mentioned concentrations of oxygen, CO 2 , N 2 , H 2 For example, oxidation treatment is carried out in a direct fired furnace (DFF) type annealing furnace or the like, in a combustion gas such as coke oven gas (COG) or liquefied petroleum gas (LPG), with unburned O 2 The treatment can be carried out in a gas atmosphere having a controlled concentration.
[0053] The oxidation treatment is preferably performed under the condition of an ultimate temperature of 650 to 750° C. For example, heating may be performed in an oxidation heating zone in a DFF type annealing furnace to an ultimate temperature of 650 to 750° C. By achieving an ultimate temperature of 750° C. or less, the SiO 2 This can suppress the reaction between FeO and the steel sheet caused by the oxidation treatment, thereby improving the adhesion between the steel sheet and the plating layer.
[0054] In this specification, the "achieved temperature" during heating in the oxidation treatment step means the maximum reached sheet temperature of the rolled sheet that is heat-controlled in the oxidation heating zone.
[0055] The temperature reached in the oxidation treatment is more preferably 730° C. or lower, further preferably 720° C. or lower, and even more preferably 700° C. or lower. On the other hand, the steel sheet temperature in the oxidation treatment is preferably 650° C. or higher from the viewpoint of forming an Fe oxide layer in the above gas atmosphere. The steel sheet temperature in the oxidation treatment is more preferably 670° C. or higher.
[0056] The temperature rise time in the oxidation treatment is not particularly limited, and may be adjusted so that the oxidation treatment is too long and does not form a fayalite layer that adversely affects, for example, plating. Specifically, the temperature rise time in the oxidation treatment may be appropriately adjusted in consideration of the hot rolling conditions (particularly the coiling temperature), the annealing conditions before pickling, the pickling conditions, and the steel sheet temperature during heating in the oxidation treatment. For example, the temperature rise time in the oxidation treatment is preferably 10 seconds or more, more preferably 15 seconds or more. Also, for example, the temperature rise time in the oxidation treatment is preferably 120 seconds or less, more preferably 90 seconds or less. In the above, the case where the oxidation treatment is performed while increasing the temperature has been described, but the aspect of the oxidation treatment is not limited to this, and the oxidation treatment may be performed by increasing the temperature to the target temperature and holding the target temperature.
[0057] (C1) Reduction treatment In the reduction treatment, a decarburized layer is formed on the surface layer of the steel sheet, while a reduced Fe layer capable of favorably forming, for example, a plating layer is formed. In the manufacturing method according to this embodiment, the reduction treatment is preferably performed by first reduction treatment having a dew point of -35 to -15°C, followed by second reduction treatment having a dew point of -25 to 0°C, which is higher than that of the first reduction treatment. Hereinafter, the first reduction treatment and the second reduction treatment will be described respectively.
[0058] (C1a) First reduction treatment In the first reduction treatment, the dew point is preferably set in the range of -35 to -15°C. If the dew point exceeds -15°C, decarburization may proceed more than necessary, which may result in a decrease in strength. In addition, the reduction treatment may be difficult to proceed, and a defect called pickup may occur in which iron oxide produced in the oxidation treatment adheres to the rolls and causes pressure marks on the steel sheet. Therefore, the dew point is preferably set to -15°C or lower. The dew point is more preferably set to -20°C or lower. On the other hand, from the viewpoint of suppressing additional equipment and costs, the dew point in the first reduction treatment is preferably set to -35°C or higher. The dew point is more preferably set to -30°C or higher.
[0059] The dew point may be within the above range in the atmosphere at the center of the front stage of the reduction zone where the first reduction treatment is performed. The dew point in the first reduction treatment and the second reduction treatment described below can be controlled, for example, by introducing water vapor gas and mixing it with the atmospheric gas in a furnace, or by bubbling the atmospheric gas to mix water vapor therein.
[0060] The atmosphere of the first reduction treatment satisfies the above dew point and contains N 2 , H 2 , CO, H 2 O, O 2 and other unavoidable impurities. In the first reduction treatment, after the steel sheet reaches a temperature of 800°C in the atmosphere, the steel sheet is heated in a temperature range of 850 to 920°C for, for example, 60 to 240 seconds. The "holding" mentioned above includes not only a constant temperature but also a temperature change within the above temperature range.
[0061] (C1b) Second reduction treatment Next, the dew point in the second reduction treatment will be described. FIG. 1 is a graph created using a reference example described later, which shows the relationship between the dew point at the center of the soaking zone during the second reduction treatment and R / t. It can be seen from FIG. 1 that in order to achieve excellent bendability with R / t of less than 2.5, the dew point in the second reduction treatment needs to be -25°C or higher. On the other hand, the upper limit of the dew point in the second reduction treatment is preferably 0°C or lower from the viewpoint of exhibiting higher strength. The dew point in the second reduction treatment is more preferably -15°C or lower.
[0062] The atmosphere of the second reduction treatment satisfies the above dew point and contains N 2 , H 2 , CO, H 2 O, O 2 and other unavoidable impurities. In the second reduction treatment, the steel sheet is heated in the above atmosphere within a temperature range of 850 to 920°C for, for example, 60 to 240 seconds. The "holding" includes not only a constant temperature but also a temperature change within the above temperature range.
[0063] The first reduction treatment and the second reduction treatment may be performed in separate atmospheres having different dew points as described above, and the specific embodiment is not limited thereto. For example, a reduction furnace may be provided for performing each of the first reduction treatment and the second reduction treatment. In addition, when the steel sheet is a plated steel sheet, a partition wall having an opening area ratio of 20% or less may be provided in the middle of the reduction zone of the continuous hot-dip galvanizing line to separate the first reduction treatment from the second reduction treatment.
[0064] Between the first reduction treatment and the second reduction treatment, for example, a holding step for holding at least one of the conditions (dew point, etc.) of the first reduction treatment may be inserted as long as it does not adversely affect the decarburization state of the steel sheet according to the present embodiment. Preferably, the second reduction treatment is performed following the first reduction treatment.
[0065] The oxidation treatment and reduction treatment may be carried out using any one or more known facilities. Preferably, from the viewpoints of production efficiency, cost, and quality maintenance, a continuous hot-dip galvanizing line (CGL) facility is used. By using a continuous hot-dip galvanizing line, the oxidation treatment and reduction treatment by the oxidation-reduction method, and the hot-dip galvanizing treatment and alloying treatment when manufacturing, for example, a galvanized steel sheet as a steel sheet, can be continuously carried out in a series of production lines. More specifically, the oxidation treatment and reduction treatment by the oxidation-reduction method can be carried out using, for example, an annealing furnace in a DFF-type continuous hot-dip galvanizing line. The oxidation treatment can be carried out, for example, in a heating zone in a DFF-type annealing furnace as described above. The reduction treatment can be carried out, for example, in a soaking zone in a DFF-type annealing furnace.
[0066] (D) After step (C), a step of cooling to a cooling stop temperature. After the step (C), the material is cooled to a cooling stop temperature of 200 to 350°C at a predetermined cooling rate. First, the average cooling rate from the first heating temperature to 550°C (hereinafter also referred to as "first average cooling rate") is 5°C / sec or more. If the first average cooling rate is less than 5°C / sec, there is a risk of excessive generation of polygonal ferrite. The first average cooling rate is preferably 7°C / sec or more. There is no particular upper limit to the first average cooling rate, but from the viewpoint of ease of control, it may be, for example, 100°C / sec or less.
[0067] Next, the average cooling rate from 550°C to the cooling stop temperature (200 to 350°C) (hereinafter also referred to as "second average cooling rate") is 1°C / sec or more. If the second average cooling rate is less than 1°C / sec, there is a risk of excessive generation of bainitic ferrite. The second average cooling rate is preferably 2°C / sec or more. The upper limit of the second average cooling rate is not particularly limited, but from the viewpoint of ease of control, it may be, for example, 100°C / sec or less. In addition, if the cooling stop temperature is less than 200°C, the amount of martensite becomes excessive, and there is a risk that the amount of retained austenite cannot be sufficiently secured, and if it exceeds 350°C, there is a risk that the amount of martensite cannot be sufficiently secured, and the remaining structure such as fresh martensite and pearlite becomes excessive.
[0068] Furthermore, the average cooling rate from 400°C to the cooling stop temperature (hereinafter also referred to as the "third average cooling rate") is preferably 40°C / sec or less. This promotes C concentration in untransformed austenite due to bainite transformation, stabilizing the residual γ and making it easier to ensure a predetermined amount of the first residual γ, which has a relatively low amount of solute C.
[0069] (E) After step (D), a step of heating to a second heating temperature to obtain a steel sheet. After step (D), the steel sheet is heated (reheated) to a second heating temperature of 300°C to 450°C and held for 50 to 1000 seconds to obtain a steel sheet used for the plated steel sheet according to the embodiment of the present invention. This step advances the bainite transformation and promotes C concentration in untransformed austenite, thereby ensuring a sufficient amount of retained austenite and further making it easier to ensure a predetermined amount of second retained γ having a relatively stable high amount of dissolved C. If the second heating temperature is outside the above temperature range or the holding time is less than 50 seconds, there is a risk that a sufficient amount of retained austenite cannot be ensured. On the other hand, if the holding time is too long, the above effects will saturate, so it is preferable to set the holding time to 1000 seconds or less. The metal structure defined in the embodiment of the present invention is obtained mainly through steps (D) and (E).
[0070] (F) A step of forming a plating layer on the steel sheet The above-mentioned plating layer is formed on the surface of the steel sheet. The conditions for forming the plating layer are not particularly limited, and a conventional plating process can be adopted. For example, when forming a hot-dip galvanized layer, the hot-dip galvanizing process may be performed by immersing the steel sheet in a hot-dip galvanizing bath at 300°C or more and 550°C or less. The plating time may be appropriately adjusted so as to ensure a desired coating weight, and is preferably, for example, 1 to 10 seconds.
[0071] In the case of alloying hot-dip galvanizing, alloying treatment may be performed after the above-mentioned hot-dip galvanizing. The alloying temperature is not particularly limited, but if the alloying temperature is too low, alloying does not proceed sufficiently, so it is preferably 450°C or higher, more preferably 460°C or higher, and even more preferably 480°C or higher. However, if the alloying temperature is too high, alloying proceeds excessively, the Fe concentration in the plating layer becomes excessive, and plating adhesion deteriorates. From this viewpoint, the alloying temperature is preferably 550°C or lower, more preferably 540°C or lower, and even more preferably 530°C or lower. The alloying time is not particularly limited, and may be adjusted so that the hot-dip galvanizing is alloyed. The alloying time is, for example, 10 to 60 seconds.
[0072] The method for producing a plated steel sheet according to the embodiment of the present invention may include other processes without departing from the scope of the present disclosure. EXAMPLES
[0073] The following examples are provided to more specifically describe the embodiments of the present invention. The embodiments of the present invention are not limited to the following examples, and may be modified as appropriate within the scope of the above and below-described aims, and all of these are included in the technical scope of the embodiments of the present invention.
[0074] Steel (steel slab) having the chemical composition shown in Table 1 was heated at 1250°C for 30 minutes, then hot-rolled to a reduction of about 90% and a finish rolling temperature of 920°C, cooled to 660°C, coiled, and then cooled to room temperature to obtain a rolled plate having a thickness of 1.8 to 2.6 mm. The obtained rolled plate was pickled to remove surface scale, and then cold-rolled to a thickness of 1.0 to 1.6 mm. In Table 1, "-" indicates that the ingredient was not added intentionally. In the following tables, values marked with * indicate that the ingredient is outside the scope of the embodiment of the present invention.
[0075] [Table 1]
[0076] The above-mentioned rolled sheet was subjected to the above-mentioned step (B1) and steps (B) to (F) to obtain plated steel sheets of Test Nos. 1 to 17. The conditions of each step are shown in Table 2. Although not shown in Table 2, in Test Nos. 11 to 14, step (B1) was performed during the temperature rise to the first heating temperature in step (B), with an oxygen concentration of 0.1 to 2%, an ultimate temperature of 650 to 750°C, and a temperature rise time in the oxidation treatment of 10 to 120 seconds. Step (C) includes a reduction step (C1) in which a first reduction treatment (C1a) having a dew point of -35 to -15°C is followed by a second reduction treatment (C1b) having a dew point higher than that of the first reduction treatment, and the heating times (retention times) of the first reduction treatment and the second reduction treatment were each 60 seconds or more. Furthermore, although not shown in Table 2, in Test Nos. 1 to 17, in step (F), an alloyed hot-dip galvanized layer was formed by a known method. Specifically, in step (F), the steel sheet was immersed in a hot-dip galvanizing bath at 300°C or higher and 550°C or lower to perform hot-dip galvanizing treatment (plating time 1 to 10 seconds), and then alloying treatment was performed, with the alloying treatment temperature being 480 to 500°C and the alloying treatment time being 20 to 25 seconds.
[0077] [Table 2]
[0078] The steel sheets of Test Nos. 1 to 17 described above were subjected to the following evaluations.
[0079] <Metal structure evaluation> A test piece was taken from the center in the direction perpendicular to the rolling direction and thickness direction (sheet width direction), and a cross section parallel to the rolling direction and sheet width direction and located 1 / 4 of the sheet thickness from the steel sheet surface was exposed from the test piece by electrolytic polishing or the like. The cross section was observed by SEM, and the area ratios of polygonal ferrite, bainitic ferrite, MA, and pearlite were measured. The sum of the area ratios of bainite and tempered martensite was calculated by subtracting the sum of the area ratios of polygonal ferrite, bainitic ferrite, MA, and pearlite from 100 area %.
[0080] The volume fraction of the retained γ in the metal structure constituting the steel sheet was measured by X-ray diffraction. Specifically, an X-ray diffraction pattern was obtained from the above cross section using an X-ray source: Co-Kα, and the volume fraction of the retained γ relative to the entire metal structure was measured based on a known method (ISIJ Int. Vol. 33. (1993), No. 7, p. 776).
[0081] The area ratio of fresh martensite in the remaining structure was calculated by subtracting the volume ratio of the above-mentioned retained γ (≒area ratio) from the area ratio of MA, assuming that the volume ratio of the above-mentioned retained γ is the area ratio. The ratios of the first retained γ and the second retained γ to the total retained γ were calculated as follows.
[0082] First, the carbon concentration distribution of the residual γ was determined using the three diffraction peaks of (200)γ, (220)γ, and (311)γ measured by the above-mentioned X-ray diffractometer. Figure 2 is a schematic diagram of an X-ray diffraction pattern. As shown in Figure 2, for the three diffraction peaks of (200)γ, (220)γ, and (311)γ, the 2θ (2θ avg (hkl)) and its half-width Δ2θ(hkl) were calculated, where (hkl) means (200), (220) or (311) (hereinafter the same).
[0083] Next, the above 2θ avg From (hkl), the Bragg condition: λ = 2d sinθ (d: lattice plane Using the above formula (1), d(hkl) was calculated using the distance (λ) between the laser beam and the target laser, and λ is the wavelength of Co-Kα radiation. d(hkl)=λ / {2sin(2θ avg (hkl) / 2)} ···(1)
[0084] Each lattice constant a0(hkl) was calculated by the following formula (2), and the lattice constant a0 was determined by arithmetic average. a0(hkl)=d(hkl)√(h 2 +k 2 +l 2 ) ···(2)
[0085] Carbon concentration (%) C is calculated using the following formula (3): avg (unit: mass%) was calculated. %C avg =(1 / 0.033)×(a0-3.572) ···(3)
[0086] Next, the half-value width Δ%C of the carbon concentration distribution of the residual γ was obtained by the following procedure.
[0087] First, the diffraction angles at the upper and lower limits of the half-width Δ2θ(hkl) of the diffraction angle 2θ(hkl) of each peak were calculated using the following formulas (4) and (5) (see FIG. 2). 2θL(hkl)=2θ avg (hkl)-Δ2θ(hkl) / 2 (4) 2θH(hkl)=2θ avg (hkl)+Δ2θ(hkl) / 2 (5)
[0088] Using the above 2θL(hkl) and 2θH(hkl), the upper and lower limits %CL and %CH of the half-width of the carbon concentration distribution were calculated using the Bragg condition and the above formulas (1) to (3) in the same manner as above. Then, the half-width Δ%C of the carbon concentration distribution was calculated using the following formula (6). Δ%C = %CH - %CL (6)
[0089] Assuming that the carbon concentration distribution is a normal distribution, the standard deviation σ%C was calculated from the half-width Δ%C as follows. That is, the probability density function f(x) of the normal distribution is expressed by the following formula (7) using the mean value u and the standard deviation σ. f(x)={1 / √(2πσ 2 )}×exp{-(xu) 2 / (2σ 2 )}···(7)
[0090] The probability f(u) at the average value was calculated using the following formula (8) by substituting x=u into the above formula (7). f(u)=1 / √(2πσ 2 ) ···(8)
[0091] Average value u=%C avg The value shifted up or down by 1 / 2 of the half-width Δ%C from ±Δ%C / 2) probability density f(%C avg ±Δ%C / 2) is the average value u=%C avg The probability of f(u)=f(%C avg ), so from the above equations (7) and (8), the relationship in the following equation (9) can be obtained. {1 / √(2πσ%C 2 )}×exp{-(Δ%C / 2) 2 / (2σ%C 2 )}=1 / {2 √(2πσ%C 2 )} ···(9)
[0092] By transforming the above formula (9), the following formula (10) is derived as the formula for obtaining the standard deviation σ%C from the half-width Δ%C. Thus, the standard deviation σ%C was calculated by substituting the half-width Δ%C into this formula (10). σ%C = √{(Δ%C / 2) 2 / (2ln2)} ···(10)
[0093] Using the average value %C of the carbon concentration distribution in the remaining γ obtained as described above avg and the standard deviation σ%C, the following formula (12) was derived as the formula for obtaining the volume fraction VγR(C≤1.0%) of the remaining γ with a carbon concentration of 1.0 mass% or less with respect to the entire metal structure using the cumulative distribution function g(x) shown in the following formula (11). Then, VγR(C≤1.0%) was calculated using this formula (12). g(x) = (1 / 2)×[1 + erf{(x - u) / √(2σ 2 )}]···(11) VγR(C≤1.0%) = VγR×g(1.0) = VγR×(1 / 2)×[1 + erf{(1.0 - %C avg ) / √(2σ%C 2 )}] ···(12)
[0094] Using the average value %C of the carbon concentration distribution in the remaining γ obtained as described above avg and the standard deviation σ%C, the following formulas (13) and (14) were respectively derived as the formulas for obtaining the volume fractions VγR(C≤0.9%) and VγR(0.9% < C≤1.1%) of the remaining γ with a carbon concentration of 0.9 mass% or less and more than 0.9 mass% and 1.1 mass% or less with respect to the entire metal structure using the cumulative distribution function g(x) shown in the above formula (11). After calculating VγR(C≤0.9%) using these formulas (13) and (14), the ratios with respect to the total remaining γ volume fraction were obtained respectively. VγR(C≤0.9%) = VγR×g(0.9) = VγR×(1 / 2)×[1 + erf{(0.9 - %C avg ) / √(2σ%C 2 )}]···(13) VγR(0.9% <C≦1.1%)=VγR×g(1.2)-VγR(C≦0.9%)=VγR×(1 / 2)×[1+erf{(1.1-%C avg ) / √(2σ%C 2 )}]-VγR×(1 / 2)×[1+erf{(0.9-%C avg ) / √(2σ%C 2 )}]···(14)
[0095] Regarding the remaining structure, no structure other than fresh martensite and pearlite was observed.
[0096] <Method for measuring decarburization behavior: Carbon profile measurement by GD-OES> As described below, the carbon profile was measured by GD-OES (glow discharge optical emission spectrometry) to investigate the decarburization behavior.
[0097] (Sample Preparation) Materials measuring 50 mm x 40 mm x thickness or 30 mm x 30 mm x thickness were collected. After that, samples were prepared by degreasing in the usual manner. Then, using the samples, the mass% concentration of each element was measured by GD-OES under the following conditions.
[0098] (Measurement conditions) Equipment used: Horiba, Ltd. Marcus type radio frequency glow discharge optical emission surface analyzer (rf-GD-OES) GD-Profiler2 Sputtering method: Normal sputtering Measurement range: φ4mm Gas type: Ar Analyzed elements: B, C, O, Al, Si, Ti, Cr, Mn, Fe, Zn, P, S, N (In this embodiment, the evaluation was performed on these elements, but if elements other than the above are contained in, for example, the plating layer and / or the steel sheet, the elements other than the above will also be analyzed.)
[0099] (Measurement method) GD-OES measurements were performed on the plated surface of the sample up to a depth of 150 μm in the plate thickness direction.
[0100] (Analysis method) Since the sputtering rate of the above-mentioned device is almost constant, the sputtering crater depth of the sample after the analysis was completed was measured, and the value (sputtering depth) was plotted on the horizontal axis.
[0101] The details of the calibration curve method for converting the measured emission intensity of each element into a concentration are shown below.
[0102] Sputter weight of element i per unit time W i (g / sec) and luminescence intensity I i The relationship is expressed by the following formula (15) using the slope a and intercept b of the calibration curve. W i =aI i +b...(15) The sputter weight W of the above element i per unit time i is the concentration C i (wt.%), density ρ(g / cm 3 ), and the sputtering rate Δd (cm / sec) of the reference sample are known. 2 ) and is calculated using the following formula (16). W i =C i ×ρ×Δd×S (16)
[0103] W i Using two or more reference samples with known emission intensities I i The slope a and intercept b of the above formula (15) were determined, and a calibration curve was created with the emission intensity on the horizontal axis and the sputter weight on the vertical axis. The reference samples used are shown in Table 3 below. Using the created calibration curve, the sputter weight was calculated from the emission intensity of each target element, and the concentration was converted from the weight ratio. The calibration curve used to convert the O concentration was SiO 2 The concentration ratio of Si and O was adjusted to 1:2 using the formula:
[0104] [Table 3]
[0105] Then, the carbon analysis results were used to obtain a carbon profile, an example of which is shown in Figure 3. Figure 3 shows the carbon profiles of Test No. 12 and Test No. 14. In FIG. 3 above, the carbon profiles of all materials have a carbon concentration peak within the surface layer of 20 μm (more specifically, in the internal oxide layer). However, in Test No. 14, the carbon concentration is higher than the bulk carbon concentration, whereas in Test No. 12, the carbon concentration is kept sufficiently lower than the bulk carbon concentration.
[0106] From the obtained carbon concentration profile in the sheet thickness direction, the position where the carbon concentration (mass%) was 50% of the bulk carbon concentration and the maximum carbon concentration (mass%) in the region from the steel sheet surface to 20 μm were obtained. The bulk carbon concentration was corrected for analysis so that the carbon concentration at a sufficiently deep position (120 to 150 μm) measured by GD-OES was the value obtained by normal steel analysis. For example, when the steel analysis value was 0.22% and the GD-OES analysis value was 0.25%, the GD-OES analysis value was multiplied by 0.22 / 0.25 and used for analysis.
[0107] <Evaluation of tensile strength, yield stress and elongation> JIS No. 5 test pieces (plate-shaped test pieces) were taken so that the longitudinal direction of the test pieces was perpendicular to the rolling direction in a plane parallel to the cold-rolled rolling surface of the steel plate. Tensile tests were conducted using the test pieces to measure the tensile strength TS, yield stress YS, and elongation EL. Examples with a tensile strength TS of 1150 MPa or more were evaluated as sufficient, and examples with a tensile strength TS of less than 1150 MPa were evaluated as insufficient. Examples with a yield stress YS of 850 MPa or more were evaluated as sufficient, and examples with an elongation EL of less than 850 MPa were evaluated as insufficient. Examples with an elongation EL of 14% or more were evaluated as sufficient, and examples with an elongation EL of less than 14% were evaluated as insufficient.
[0108] <Hole expansion ratio evaluation> Test pieces measuring 90 mm x 90 mm x thickness were taken from the cold-rolled steel sheets. Using the test pieces, a hole expansion test was performed based on JIS Z 2256:2010 to measure the hole expansion ratio λ. Examples with a hole expansion ratio λ of 30% or more were evaluated as sufficient, and examples with a hole expansion ratio λ of less than 30% were evaluated as insufficient.
[0109] <Bending property (R / t) evaluation> The bendability of the steel plate was evaluated by the following procedure. A test piece with a width of 40 mm and a length of 100 mm was prepared with the major axis taken perpendicular to the rolling direction, and a bending test was performed using the V-block method in accordance with JIS Z 2248:2014. The bending radius was varied from 0 to 7 mm to determine the minimum bending radius at which the material could be bent without breaking, and this was taken as the bending radius R (mm) to calculate the bending radius R (mm) / sheet thickness t (mm). Examples with a bending radius R (mm) / sheet thickness t (mm) of less than 2.5 were evaluated as having excellent bendability (◯), and examples with a bending radius R (mm) / sheet thickness t (mm) of 2.5 or more were evaluated as having poor bendability (×).
[0110] The results are shown in Table 4. In Table 4, "PF+BF" is the sum of the area ratio of polygonal ferrite and the area ratio of bainitic ferrite, "B+M" is the sum of the area ratio of bainite and the area ratio of tempered martensite, "residual γ" is the volume ratio of all retained austenite, "first residual γ / residual γ" is the ratio (volume %) of the first residual γ to the total residual γ, "second residual γ / residual γ" is the ratio (volume %) of the second residual γ to the total residual γ, "residual structure" is the area ratio of the residual structure, and "maximum value of surface layer carbon concentration" is the maximum value of the carbon concentration (mass %) in the region from the surface of the steel sheet to 20 μm in the sheet thickness direction. The composition of the components shown in Table 4 is a part of the composition of the components shown in Table 1 to clarify the differences between Test Nos. 1 to 17. The remaining structure was fresh martensite and pearlite.
[0111] [Table 4]
[0112] From the results in Table 4, the following can be considered. Test Nos. 1 to 14 in Table 4 all satisfied the requirements defined in the embodiment of the present invention, and were easier to manufacture, and exhibited high strength and high processability. Furthermore, when comparing Test Nos. 11 to 14, Test Nos. 11 to 13 satisfied the preferable requirements defined in the embodiment of the present invention, and were excellent in bendability. On the other hand, all of Test Nos. 15 to 17 in Table 4 did not satisfy the requirements stipulated in the embodiment of the present invention, and the strength and / or processability were insufficient.
[0113] In Test No. 15, the Si content was less than 0.80 mass % and the residual γ was less than 5 volume %, so the tensile strength was less than 1150 MPa and the elongation was less than 14%.
[0114] In Test No. 16, the Cr content was less than 0.15 mass % and the total of polygonal ferrite and bainitic ferrite exceeded 5 area %, so the tensile strength was less than 1150 MPa.
[0115] Test No. 17 did not contain B, and the total of polygonal ferrite and bainitic ferrite exceeded 5 area %, so the tensile strength was less than 1150 MPa, the yield stress was less than 850 MPa, and the hole expansion ratio λ was less than 30%.
[0116] [Reference example] Below, a description will be given of a reference example in which the above requirements (I) and (II) and their relationship with bendability have been investigated in more detail. As a sample for annealing, a raw sheet was prepared having a component composition in which the bulk carbon concentration, i.e., the C content of the steel sheet (original sheet) was 0.22 mass% (0.22 mass% C), the Si content was 1.7 mass%, the Mn content was 2.0 mass%, the Cr content was 0.5 mass%, the Al content was 0.04 mass%, and the balance was Fe and unavoidable impurities (note that "unavoidable impurities" here can include P: more than 0 mass% and 0.1 mass% or less, S: more than 0 mass% and 0.05 mass% or less, and N: more than 0 mass% and 0.01 mass% or less), with a structure of ferrite + pearlite and a strength of 700 to 800 MPa.
[0117] The annealing sample was subjected to oxidation treatment and reduction treatment in an actual machine. In detail, the oxidation treatment was performed at the oxygen concentration and ultimate temperature shown in Table 5, and then the first reduction treatment (heating zone) and the second reduction treatment (soaking zone) shown in Table 5 were performed in this order under each condition (ultimate temperature, dew point) shown in Table 5.
[0118] The steel sheet after the second reduction treatment was cooled to 460°C and then immersed in an Al-Zn plating bath containing 0.08 to 0.13 mass% of Al (Al is effective Al%, plating bath temperature is 460 to 480°C) to perform zinc plating. The coating weight of the plating was 40 g / m by gas wiping. 2 More than 90g / m 2 The temperature was controlled as follows, and then alloying treatment was carried out at 480 to 490° C. for 20 to 30 seconds to obtain a galvannealed steel sheet.
[0119] [Table 5]
[0120] The carbon profile of the obtained plated steel sheet was measured by the above-mentioned GD-OES. From the obtained carbon concentration profile in the sheet thickness direction, the position where the carbon concentration (mass%) was 50% of the bulk carbon concentration and the maximum carbon concentration (mass%) in the region from the steel sheet surface to 20 μm were obtained. The bulk carbon concentration was corrected for analysis so that the carbon concentration at a sufficiently deep position (120 to 150 μm) measured by GD-OES was the value obtained by normal steel analysis. For example, when the steel analysis value was 0.22% and the GD-OES analysis value was 0.25%, the GD-OES analysis value was multiplied by 0.22 / 0.25 and used for analysis.
[0121] Furthermore, the resulting plated steel sheets were evaluated for limit bending property (R / t) as described below.
[0122] [Evaluation of limit bending strength (R / t)] The bendability of the steel sheet was evaluated by the following procedure. A test piece with a width of 40 mm and a length of 100 mm was prepared with the direction perpendicular to the rolling direction as the major axis, and a bending test was performed by the V-block method in accordance with JIS Z 2248:2014. In the bending test, the bending radius was changed from 0 to 7 mm to obtain the minimum bending radius at which the material could be bent without breaking, and the limit bending radius R (mm) / sheet thickness t (mm) was calculated using this limit bending radius R (mm). Then, when the limit bending radius R (mm) / sheet thickness t (mm) was less than 2.5, it was evaluated as having excellent bendability, and when it was 2.5 or more, it was evaluated as having poor bendability.
[0123] [Table 6]
[0124] Based on the results of Table 6 above, a graph showing the relationship between the position where the carbon concentration (mass %) in the sheet thickness direction is 50% of the bulk carbon concentration and R / t is shown in Figure 4. It can be seen from Figure 4 that in order to achieve excellent bendability with an R / t of less than 2.5, it is sufficient to ensure that the position where the carbon concentration (mass %) in the sheet thickness direction is 50% of the bulk carbon concentration is in a region that is 0.20% or more of the sheet thickness from the steel sheet surface.
[0125] Based on the results of Table 6 above, a graph showing the relationship between R / t and the ratio of the maximum carbon concentration (mass%) in the region from the steel sheet surface to 20 μm, relative to the bulk carbon concentration, is shown in Figure 5. It can be seen from Figure 5 that in order to achieve excellent bendability with an R / t of less than 2.5, it is best to set the ratio of the maximum carbon concentration (mass%) in the region from the steel sheet surface to 20 μm, relative to the bulk carbon concentration, to less than 70%.
Claims
1. A plated steel sheet comprising a steel sheet and a plating layer disposed on a surface of the steel sheet, the plated steel sheet having a tensile strength of 1150 MPa or more, The steel sheet included in the plated steel sheet is C: 0.150 to 0.250% by mass, Si: 0.80 to 2.20% by mass, Mn: 1.50 to 2.80% by mass, Cr: 0.15 to 1.50% by mass, Ti: 0.012 to 0.100% by mass, B: 0.0015 to 0.0100% by mass, P: 0.100% by mass or less (including 0% by mass), S: 0.050% by mass or less (including 0% by mass), Al: 0.005 to 1.000% by mass, N: 0.0100% by mass or less (including 0% by mass), and The balance is composed of iron and inevitable impurities, and The metal structure has a total of bainite and tempered martensite of 95% by area or less, retained austenite of 5% by volume or more, a total of polygonal ferrite and bainitic ferrite of 5% by area or less, and a remaining structure of 5% by area or less. Galvanized steel sheet.
2. In the plate thickness direction, 2. The plated steel sheet according to claim 1, wherein a position where the carbon concentration (mass %) is 50% of the bulk carbon concentration is in a region that is 0.2% or more of the sheet thickness from the surface of the steel sheet.
3. 2. The plated steel sheet according to claim 1, wherein a maximum carbon concentration (mass%) in a region extending from the surface of the steel sheet to 20 μm in the sheet thickness direction is less than 70% of a bulk carbon concentration.
4. The retained austenite is Contains 10 to 50 volume % of first retained austenite having a solute C content of 0.9 mass % or less, and The plated steel sheet according to claim 1, comprising 10 to 50 volume % of second retained austenite having a solute C content of more than 0.9 mass % and not more than 1.1 mass %.
5. A step of hot rolling a steel having the composition according to claim 1 to obtain a rolled plate; Heating the rolled plate to a first heating temperature of 850° C. or more; After the heating step, maintaining the first heating temperature for 50 seconds or more; After the holding step, a step of cooling to a cooling stop temperature of 200 to 350 ° C., wherein the average cooling rate from the first heating temperature to 550 ° C. is 5 ° C. / sec or more, and the average cooling rate from 550 ° C. to the cooling stop temperature is 1 ° C. / sec or more; After the cooling step, a step of heating to a second heating temperature of 300° C. to 450° C. and holding the temperature for 50 to 1000 seconds to obtain a steel sheet; forming a plating layer on the steel sheet; The method for producing a plated steel sheet according to any one of claims 1 to 4, comprising:
6. After the step of obtaining the rolled plate, an oxidation treatment is performed under conditions of an oxygen concentration of 0.1 to 2% and an ultimate temperature of 650 to 750° C., The holding step includes a first reduction treatment having a dew point of −35 to −15° C., followed by a second reduction treatment having a dew point of −25 to 0° C., which is higher than the dew point of the first reduction treatment. The manufacturing method according to claim 5.
7. The method according to claim 5, wherein the cooling step is performed at an average cooling rate of 400° C. / sec or less from 400° C. to the cooling stop temperature.
Citation Information
Patent Citations
High-strength steel sheet and manufacturing method therefor
WO2019159771A1
Steel sheet and manufacturing method therefor
WO2020080401A1
Steel sheet and manufacturing method therefor
WO2020080402A1