Zeolite-based catalyst and method for producing synthesis gas
A silicon and aluminum-based zeolite catalyst with controlled transition metal content addresses the issue of hot spots in methane partial oxidation, ensuring high selectivity and stability for carbon monoxide and hydrogen production.
Patent Information
- Application Number
- JP2024031652
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-01
- Publication Date
- 2024-10-11
AI Technical Summary
Existing catalysts for methane partial oxidation suffer from rapid heating due to hot spots, leading to complete oxidation and catalyst deterioration, reducing the yield of carbon monoxide and causing metal agglomeration.
A zeolite catalyst composed of silicon and aluminum with minimal transition metals, having specific crystal structures and properties, is used to selectively partial oxidize methane, suppressing complete oxidation and maintaining catalyst stability.
The zeolite catalyst effectively suppresses complete oxidation, maintaining high selectivity for carbon monoxide and hydrogen production, preventing hot spots and catalyst degradation.
Smart Images

Figure 2024144183000001 
Figure 2024144183000002 
Figure 2024144183000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a zeolite catalyst and a method for producing synthesis gas, and more particularly to a method for producing carbon monoxide and hydrogen (synthesis gas) using methane as a raw material and a catalyst. [Background technology]
[0002] Methane (CH4) reforming is a technology that is often used to produce a mixed gas (synthetic gas) of carbon monoxide (CO) and hydrogen (H2). Among the methane reforming reactions, steam reforming of methane (CH4+H2O→3H2+CO, ΔH0=+206kJ) is the most commonly used technology, but this reaction is a large endothermic reaction, and the large energy consumption in the process is an issue. On the other hand, the partial oxidation of methane (2CH4 + O2 → 4H2 + 2CO, ΔH0 = -36 kJ) is an exothermic reaction, and therefore is attracting attention as a highly energy-efficient process that does not require external energy supply once the reaction begins.
[0003] For such partial oxidation of methane, catalytic materials containing transition metals such as Co, Ni, Ru, Rh, Pd, and Pt as active sites have been used. For example, Patent Document 1 discloses a partial oxidation catalyst for light hydrocarbons containing cobalt- and rhodium-supported zeolite. Patent Document 2 discloses a partial oxidation catalyst for light hydrocarbons in which zeolite supports at least one element selected from transition metals in Groups 8 to 11 of the periodic table and at least one element selected from metals in Groups 1 to 3 of the periodic table. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-181375 A [Patent Document 2] Patent Publication No. 2021-45722 Summary of the Invention [Problem to be solved by the invention]
[0005] When the catalytic materials disclosed in Patent Documents 1 and 2 are used, a part of methane is likely to be completely oxidized (CH4+2O2→2H2O+CO2, ΔH0=-803 kJ) simultaneously with the partial oxidation of methane. Since the heat generated by the complete oxidation is much larger than that generated during partial oxidation, the catalyst bed is rapidly heated as soon as the reaction starts, forming a hot spot. The formation of such a hot spot not only reduces the yield of carbon monoxide, but also causes aggregation of active metal species at the hot spot. When a hot spot is formed, even if the reaction is stopped and the partial oxidation reaction is resumed, the complete oxidation reaction is likely to occur again, and the aggregation of metals can also cause catalyst deterioration. Therefore, there is a demand for the development of a catalyst that suppresses the complete oxidation of methane and partially oxidizes methane highly selectively by reaction with oxygen.
[0006] The present invention is intended to solve the above problems, and has an object to provide a catalyst that suppresses complete oxidation of methane and partially oxidizes methane with high selectivity in the reaction of methane with oxygen. [Means for solving the problem]
[0007] The present inventors have conducted studies aimed at solving the above problems, and have found that by activating methane by utilizing the acidic properties of the zeolite surface, the methane can be converted into carbon monoxide and hydrogen, that is, that zeolite can convert methane to carbon monoxide with high selectivity in the partial oxidation of methane. The present invention was completed based on these findings.
[0008] The present invention includes the following gist. [1] A zeolite catalyst used for the partial oxidation of light hydrocarbons, containing silicon (Si) and aluminum (Al) as its constituent elements and with less than 0.1% by mass of elements from groups 8 to 10 of the periodic table. [2] The zeolite catalyst according to the above [1], wherein the molar ratio of silicon to aluminum (Si / Al) contained in the zeolite catalyst is 1 or more and 100 or less. [3] The zeolite catalyst according to the above [1] or [2], wherein the zeolite catalyst comprises at least one crystal structure selected from the group consisting of AEI, CHA, MFI, and BEA, as defined by the International Zeolite Association (IZA) codes. [4] The zeolite catalyst according to any one of the above [1] to [3], wherein the light hydrocarbons are hydrocarbons having 6 or less carbon atoms. [5] The zeolite catalyst according to any one of the above [1] to [4], wherein the light hydrocarbons are methane or contain methane as a main component. [6] A method for producing synthesis gas by partial oxidation of methane at a reaction temperature of 650°C or higher using a zeolite catalyst containing silicon (Si) and aluminum (Al) as its constituent elements and having a content of elements from groups 8 to 10 of the periodic table of less than 0.1 mass%. [7] The method for producing a synthesis gas according to the above [6], wherein a synthesis gas that is a product of the partial oxidation reaction of methane contains carbon monoxide, hydrogen, ethane, ethylene, carbon dioxide, and water, and the selectivity of carbon dioxide relative to methane is 30 mol % or less. [8] The method for producing a synthesis gas according to the above [6] or [7], wherein the partial oxidation reaction of methane is performed in a molar ratio of methane to oxygen (methane / oxygen) of 1 or more. [9] The method for producing a synthesis gas according to any one of the above [6] to [8], wherein the partial oxidation reaction of methane is carried out at 1000° C. or lower.
[10] The method for producing a synthesis gas according to any one of the above [6] to [9], wherein the molar ratio of silicon to aluminum (Si / Al) contained in the zeolite catalyst is 1 or more and 100 or less.
[11] The method for producing a synthesis gas according to any one of the above [6] to
[10] , wherein the zeolite in the zeolite-based catalyst has at least one crystal structure selected from the group consisting of AEI, CHA, MFI, and BEA, as defined by the International Zeolite Association (IZA) code. Effect of the Invention
[0009] According to the present invention, it is possible to provide a catalyst which suppresses complete oxidation of methane in the reaction of methane with oxygen and highly selectively partially oxidizes methane. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described in detail below. However, the description of the constituent elements described below is one example (representative example) of an embodiment of the present invention, and the present invention is not limited to these contents, and can be implemented in various modifications within the scope of the gist of the present invention.
[0011] [Zeolite catalyst] The zeolite catalyst of the present invention is a catalyst used for partial oxidation of light hydrocarbons, which contains silicon (Si) and aluminum (Al) as constituent elements and has a content of elements of Groups 8 to 10 of the periodic table of less than 0.1 mass%. Here, the light hydrocarbon is preferably a hydrocarbon having a carbon number of 6 or less. When the hydrocarbon has a carbon number of 6 or less, the zeolite catalyst of the present invention functions effectively as a partial oxidation catalyst. In particular, the hydrocarbon having a carbon number of 6 or less is preferably methane or a hydrocarbon containing methane as a main component.
[0012] <Zeolite> The zeolite used as the catalyst of the present invention contains silicon (Si) and aluminum (Al) as constituent elements. In addition to Si and Al, the constituent elements may contain one or more elements selected from boron (B), titanium (Ti), vanadium (V), iron (Fe), zinc (Zn), gallium (Ga), germanium (Ge), zirconium (Zr), and tin (Sn). Note that Al and the like forming the zeolite framework become acid sites and act as reaction sites for catalytic activity. The molar ratio of silicon to aluminum in these zeolites (hereinafter referred to as "Si / Al ratio") is not particularly limited as long as it is within a range in which the effects of the present invention can be achieved, but is preferably 1 or more and 100 or less. When the Si / Al ratio is 100 or less, the amount of acid becomes appropriate, and the partial oxidation reaction of methane can be promoted. From the above viewpoints, it is more preferable that the Si / Al ratio is 80 or less. On the other hand, when the Si / Al ratio is 1 or more, dealumination in the partial oxidation reaction of methane can be suppressed, and high activity can be maintained. From the above viewpoints, it is preferable that the Si / Al ratio is 3 or more, and more preferably 8 or more. The contents of Si, Al, etc. in the zeolite produced by the method of the present invention can usually be measured by inductively coupled plasma atomic emission spectrometry (ICP-AES), etc. The "Si / Al ratio" in the present invention is a value calculated from the value measured by ICP-AES for the produced zeolite, and is not the ratio of Si to Al calculated from the amount of raw material charged. The Si / Al ratio can be controlled by the SiO2 / Al2O3 ratio used in the production of zeolite, and can also be controlled by the production conditions. Furthermore, after the production of zeolite, the Si / Al ratio can also be controlled by desorbing Al and the like through a steaming process or the like.
[0013] The crystal structure of the zeolite according to the present invention is not particularly limited as long as it exhibits the effects of the present invention, and examples of the codes set by the International Zeolite Association (IZA) include AEI, AEL, AFI, AFX, APC, ATO, BEA, BRE, CDO, CHA, CON, DDR, EAB, EPI, ERI, ESV, EUO, FAU, FER, GIS, GME, HEU, ITH, KFI, LEV, LTA, LTL, MER, MEL, MFI, MON, MOR, MSE, MTF, MTT, MTW, MWW, NES, OFF, PAU, PHI, RHO, RTE, RTH, SOD, STI, STT, SZR, TON, TSC, TUN, UFI, VNI, WEI, YUG, etc. Among these, it is preferable to include one or more types selected from AEI, CHA, MFI, and BEA. These zeolites generate Al species that can exhibit Lewis acidity during the partial oxidation of methane, making them suitable reaction fields for the partial oxidation of methane, and therefore show better activity than MOR and FAU. The above zeolites may be used alone or in combination of two or more kinds. The formation of Lewis acid Al species can be confirmed by adsorption IR using CO molecules as a probe.
[0014] The pore size of the zeolite is not particularly limited, but is preferably 0.3 nm or more, more preferably 0.35 nm or more. It is also preferably 0.9 nm or less, more preferably 0.8 nm or less, and even more preferably 0.6 nm or less. The pore size referred to here indicates the crystallographic channel diameter defined by the International Zeolite Association (IZA). When the pore size of the zeolite is within the above range, the raw materials methane and oxygen easily enter the zeolite pores, and the reaction easily proceeds at the active sites in the pores. In addition, the product is easily desorbed, and there is no problem such as coking caused by excessive reaction in the pores.
[0015] The ion exchange sites of the zeolite are not particularly limited, and may be either H-type or those exchanged with alkali metal ions, alkaline earth metal ions, etc., with the H-type being preferred.
[0016] The BET specific surface area of the zeolite is not particularly limited as long as the effects of the present invention are achieved. For example, 2 The BET specific surface area of the zeolite is preferably 200 m 2 When the BET specific surface area of the zeolite is 250 m / g or more, sufficient adsorption sites for the raw material methane are secured, and the reaction efficiency can be improved. 2 / g or more is more preferable, and 300m 2 On the other hand, the BET specific surface area of the zeolite is preferably 2000 m 2 The BET specific surface area of the zeolite is preferably 2000 m 2 From the above viewpoints, the BET specific surface area of the zeolite is 1500 m 2 / g or less is more preferable, and 2 It is more preferable that the BET specific surface area is equal to or less than 1 / g. The BET specific surface area can be measured by a nitrogen adsorption method.
[0017] In addition, the pore volume of the zeolite according to the present invention is not particularly limited as long as the effects of the present invention are achieved, but is preferably 0.1 mL / g or more. When the pore volume of the zeolite is 0.1 mL / g or more, sufficient adsorption sites for the raw material methane are secured, and the reaction efficiency can be improved. From the above viewpoints, the pore volume of the zeolite is more preferably 0.2 mL / g or more, and even more preferably 0.3 mL / g or more. On the other hand, the pore volume of the zeolite is preferably 3 mL / g or less, and more preferably 2 mL / g or less. The average pore size of the zeolite may be the pore size value of each crystal structure published by IZA, and the pore volume can be measured by a nitrogen adsorption method.
[0018] The average primary particle size of the zeolite according to the present invention is not particularly limited as long as the effects of the present invention are achieved, but is preferably 10 μm or less. If the average primary particle size of the zeolite is 10 μm or less, it is advantageous in terms of the diffusion of the reaction substrate and the reaction product. From the above viewpoint, the average primary particle size of the zeolite is more preferably 3 μm or less, and further preferably 700 nm or less. On the other hand, the lower limit is not particularly limited as long as it is within the range in which the effects of the present invention can be obtained, and is usually 20 nm or more, preferably 40 nm or more.
[0019] The "average primary particle size" can be calculated using a scanning electron microscope (SEM). Here, the term "primary particle" refers to the smallest particle in which no grain boundary is observed. In the present invention, an SEM image of the zeolite catalyst is obtained, and the smallest particle in which no grain boundary is observed and which is a part corresponding to zeolite contained in the SEM image is determined as the "primary particle". In the present invention, the primary particle does not have to exist as a single particle, and may form a secondary particle by aggregation or the like. Even if a secondary particle is formed, the primary particle on the surface of the secondary particle can be distinguished in the SEM image. The "average primary particle size" refers to a measurement made as follows: 50 primary particles are randomly selected from the SEM image of the zeolite catalyst, the major axis (the longest straight line length when connecting one end of a primary particle with the other end of a straight line) is measured for each of the selected 50 primary particles, and the arithmetic mean of the major axes of the 50 particles is taken as the "average primary particle size." However, if the entire zeolite catalyst contains less than 50 primary particles, the major axis of each of the primary particles contained in the zeolite catalyst is measured, and the average value thereof is regarded as the "average primary particle diameter."
[0020] The average primary particle size can be set within a specific range, for example, by using zeolite having a small particle size as seed crystals, or by adding a surfactant to the raw material gel for zeolite synthesis in the zeolite production process.
[0021] The zeolite according to the present invention has a content of elements of Groups 8 to 10 of the periodic table of less than 0.1% by mass. When the content of elements of Groups 8 to 10 of the periodic table is less than 0.1% by mass, the complete oxidation reaction of methane is not induced. Therefore, the yield of carbon monoxide is not decreased, and the formation of hot spots is suppressed, which is preferable.
[0022] <Zeolite manufacturing method> The method for producing a zeolite of the present invention includes a step of hydrothermally synthesizing a raw material composition. More specifically, the method includes a step of preparing a raw material gel containing a silica source, an aluminum source, and an alkali metal, and a step of hydrothermally synthesizing the raw material gel at 10 to 240°C.
[0023] (Preparation of raw gel) The raw gel is prepared using a silica source, an aluminum source, and a compound containing an alkali metal. In the preparation of the raw gel, other components such as a compound containing an alkaline earth metal, an organic structure directing material, and a seed crystal may be further used as long as they do not significantly impair the effects of the present invention.
[0024] <<Raw materials, etc.>> The silica source refers to a raw material compound that becomes silicon atoms that constitute zeolite. Examples of silica sources include fumed silica, silica sol, colloidal silica, water glass, ethyl silicate, methyl silicate, etc., and one or more of these are used. Among these, fumed silica and colloidal silica are preferred because they are easy to handle and highly reactive.
[0025] The aluminum source refers to a raw material compound that becomes the aluminum atoms that constitute the zeolite. The aluminum source is usually an aluminum alkoxide such as pseudoboehmite, gibbsite, aluminum isopropoxide, aluminum triethoxide, etc.; aluminum hydroxide; alumina sol, sodium aluminate, etc., and one or more of these are used. Among these, aluminum hydroxide, aluminum isopropoxide, and pseudoboehmite are preferred because they are easy to handle and highly reactive.
[0026] The compound containing an alkali metal may be a hydroxide of an alkali metal such as NaOH or KOH. The type of alkali metal is not particularly limited, and typically includes Na, K, Li, and Rb, and preferably Na and K. Two or more types of compounds containing an alkali metal may be used in combination. In addition, a compound containing an alkaline earth metal may be used. As the compound containing an alkaline earth metal, Ca(OH)2 or the like may be used. The type of alkaline earth metal is not particularly limited, and typically includes Ca, Mg, Sr, and Ba. In addition, two or more types of compounds containing an alkaline earth metal may be used in combination.
[0027] The organic structure directing agent used in the synthesis of zeolite is usually amines, quaternary ammonium salts, etc. For example, when synthesizing CHA-type aluminosilicate, the organic templates described in U.S. Patent No. 4,544,538 and U.S. Patent Publication No. 2008 / 0075656 are preferred. Note that, depending on the composition of the obtained zeolite, the organic structure directing agent is not necessarily required.
[0028] The raw gel may be prepared using seed crystals, and zeolite is usually used as the seed crystals. If the zeolite to be produced is an aluminosilicate, the seed crystals are preferably aluminosilicate zeolite, more preferably aluminosilicate zeolite containing d6r as the CBU. The seed crystals may contain an amorphous component as a part thereof. In addition, the zeolite used as the seed crystals may or may not contain an organic structure-directing material. The method for producing the zeolite to be used as the seed crystals is not particularly limited, and the zeolite may be produced by the zeolite production method of the present invention, or may be produced by other methods, such as a general batch method using an autoclave. The amount of the seed crystals is preferably large in terms of the effect of promoting crystallization as the seed crystals being easily exhibited. On the other hand, it is preferable that the amount of the seed crystals is small in terms of the ease of dissolving the seed crystals and the ease of functioning as the seed crystals. Therefore, the amount of the seed crystals is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, even more preferably 1.0% by mass or more, and particularly preferably 2% by mass or more, relative to the silica source contained in the raw material composition. On the other hand, it is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 15% by mass or less, and particularly preferably 10% by mass or less.
[0029] (Hydrothermal synthesis of raw gel) The zeolite of the present invention can be produced by hydrothermal synthesis of the raw material gel described above. The hydrothermal synthesis temperature of the raw material gel is usually 10°C or higher, preferably 50°C or higher, and more preferably 70°C or higher. A high temperature is preferable in terms of facilitating the reaction. There is no particular upper limit to the temperature of the hydrothermal synthesis, and it is usually 240°C or lower, preferably 220°C or lower, and more preferably 200°C or lower.
[0030] <<Cation exchange>> The method for producing a zeolite of the present invention may further include a step of exchanging the cation type of the zeolite obtained by the above-mentioned hydrothermal synthesis. Zeolite obtained by hydrothermal synthesis can be cation-exchanged to a desired cation type as necessary. The cation exchange can be performed using, but is not limited to, nitrates such as NH4NO3, LiNO3, NaNO3, KNO3, RbNO3, CsNO3, Be(NO3)2, Ca(NO3)2, Mg(NO3)2, Sr(NO3)2, Ba(NO3)2, or salts of halide ions, sulfate ions, carbonate ions, hydrogen carbonate ions, acetate ions, phosphate ions, and hydrogen phosphate ions instead of the nitrate ions contained in these nitrates, and acids such as nitric acid and hydrochloric acid. The temperature of the cation exchange is not particularly limited as long as it is a general cation exchange temperature, but is usually 10°C or higher and 100°C or lower. Ammonium-type zeolite can also be converted to proton-type zeolite by calcining the zeolite.
[0031] After the raw gel is crystallized, the crystallized raw gel is filtered and washed, and the solid content is dried at 100 to 200°C and then calcined at 400 to 900°C to obtain zeolite powder.
[0032] [Method of producing synthetic gas] The synthesis gas production method of the present invention is a method for producing synthesis gas by a partial oxidation reaction of methane, and is characterized in that the synthesis gas is produced by the partial oxidation reaction of methane at a reaction temperature of 650°C or higher using a zeolite-based catalyst that contains silicon (Si) and aluminum (Al) as constituent elements and has a content of elements of Groups 8 to 10 of the periodic table of less than 0.1 mass %.
[0033] <Reaction conditions> The reaction temperature in the synthesis gas production method of the present invention must be at least 650° C. By setting the reaction temperature at 650° C. or higher, partial oxidation of methane progresses, and synthesis gas can be efficiently obtained. On the other hand, there is no particular upper limit to the reaction temperature, but in order to suppress complete oxidation of methane, it is preferably 1000°C or lower, and in order to stabilize the activity of the catalyst, it is more preferably 900°C or lower, even more preferably 850°C or lower, and most preferably 800°C or lower. From the above viewpoints, the reaction temperature in this reaction is preferably in the range of 650°C to 1000°C, more preferably in the range of 650°C to 900°C, further preferably in the range of 650°C to 850°C, and most preferably in the range of 650°C to 800°C. Since this reaction is an exothermic reaction, even if the reaction start temperature is 500°C, it may reach 650°C or higher if an adiabatic reaction vessel is used. Therefore, the reaction temperature here refers not to the inlet temperature of the reaction gas but to the temperature of the catalyst layer of the reactor. The temperature of the catalyst layer can usually be considered to be the same as the internal temperature (not the inlet temperature) of the reactor.
[0034] In addition, in the partial oxidation process of methane in the present invention, the molar ratio of methane to oxygen in the raw material (methane / oxygen) is preferably 1 or more. When this ratio is 1 or more, complete oxidation of methane can be easily suppressed, and partial oxidation of methane can be promoted. Furthermore, when the methane / oxygen (CH4 / O2) ratio is 1 or more, a sufficient reaction rate can be obtained. From the above viewpoints, the methane / oxygen (CH4 / O2) ratio in the raw material is preferably 1 or more, more preferably 1.5 or more, and most preferably 2 or more. On the other hand, there is no particular upper limit for the methane / oxygen (CH4 / O2) ratio, but from the standpoint of reaction efficiency, it is preferably 6 or less, and more preferably 3 or less.
[0035] As the reaction mode in this embodiment, a known gas phase reaction process using a fluidized bed reactor, a moving bed reactor, or a fixed bed reactor can be applied. A fixed bed reactor is advantageous in terms of the equipment cost including auxiliary equipment, catalyst cost, and operation management. The process may be carried out in any of a batch, semi-continuous or continuous manner, but is preferably carried out in a continuous manner, and may be a process using a single reactor or a process using multiple reactors arranged in series or parallel.
[0036] When the above-mentioned catalyst is packed into the fluidized bed reactor, in order to minimize the temperature distribution in the catalyst layer, granular materials inactive to the reaction, such as quartz sand, alumina, silica, silica-alumina, etc., may be mixed with the catalyst and packed. In this case, there is no particular restriction on the amount of granular materials inactive to the reaction, such as quartz sand, used. In addition, it is preferable that the granular materials have a particle size similar to that of the catalyst, from the viewpoint of uniform mixing with the catalyst. Furthermore, the reaction substrates (reaction raw materials) may be divided and fed to the reactor for the purpose of dispersing heat generated by the reaction.
[0037] In addition to methane and oxygen, other gases that can be present in the reactor include helium, argon, nitrogen, carbon monoxide, carbon dioxide, hydrogen, water, paraffins, aromatic compounds, and mixtures of these. Of these, the coexistence of water (water vapor) and / or carbon dioxide is preferred because it is expected to have the effect of suppressing carbon deposition on the catalyst. As such a diluent, impurities contained in the reaction raw materials may be used as they are, or a separately prepared diluent may be mixed with the reaction raw materials. The diluent may also be mixed with the reaction raw materials before being placed in the reactor, or may be supplied to the reactor separately from the reaction raw materials.
[0038] It is important that the lower limit of the reaction temperature is 650°C or higher. There is no upper limit to the reaction temperature as long as the effects of the present invention are achieved, but it is preferably 800°C or lower. If the reaction temperature is 650°C or higher, a sufficient reaction rate can be obtained. On the other hand, if the reaction temperature is 800°C or lower, the activity of the catalyst becomes stable.
[0039] The upper limit of the reaction pressure is preferably 3 MPa (absolute pressure, the same applies below). If the reaction pressure is 3 MPa or less, the production of undesirable by-products can be suppressed. From the above viewpoint, the reaction pressure is preferably 1 MPa or less. The lower limit of the reaction pressure is not particularly limited, but is usually 0.1 kPa or more, preferably 1 kPa or more, and more preferably 10 kPa or more. By keeping the reaction pressure at or above these lower limits, a sufficient reaction rate can be obtained.
[0040] The weight space velocity of the reactants is 0.1 hr -1 It is preferable that the time is 0.5 hours or more. -1 On the other hand, the weight hourly space velocity is preferably 10 hr -1 It is preferable that the time is less than 5 hours. -1 It is more preferable that the weight hourly space velocity is not more than 100%. If the weight hourly space velocity is within this range, it is advantageous for the partial oxidation reaction of methane.
[0041] According to the method of the present invention, the reaction products include, in addition to synthesis gas (CO+H2), hydrocarbons having a carbon number of 2 (by-products) such as ethane and ethylene, carbon dioxide, and water, and among these reaction products, the selectivity of carbon dioxide to the raw material methane can be set to 30 mol % or less, more preferably 25 mol % or less. In the present invention, the conversion rate of methane is 8 to 100%, and the selectivities of carbon monoxide and hydrogen are 60 to 90% and 8 to 25%, respectively. The mixed gas containing unreacted raw materials, by-products and diluent in the reactor outlet gas can be introduced into a known separation and purification facility and can be recovered, purified, recycled or discharged according to the components. EXAMPLES
[0042] The present invention will be described in more detail below with reference to examples, but the scope of the present invention is not limited to the following examples. (Evaluation method) (1) Physical properties of zeolite <Elemental analysis> Elemental analysis was performed by inductively coupled plasma atomic emission spectrometry (ICP-AES). <X-ray diffraction measurement> The crystal structure of each zeolite was determined by X-ray diffraction measurement (XRD). The measurement was carried out using "D2PHASER" manufactured by BRUKER. The crystal structure, Si / Al ratio, and elemental analysis results of the zeolites used in each example and comparative example are shown in Table 1.
[0043]
Table 1
[0044] (2) Reaction evaluation Using a fixed-bed gas-phase flow-type reactor, 100 mg of the catalyst of each example and comparative example was filled in the middle of a quartz glass reaction tube (catalyst layer part: outer diameter 8.0 mm, inner diameter 6.0 mm, others: outer diameter 6.0 mm, inner diameter 4.0 mm, total length 260 mm). The electric furnace was heated to 500 °C under N2 flow (10 ml / min). Then, CH4 was introduced at a flow rate of 5.0 ml / min, O2 at 2.5 ml / min, and N2 at 12.5 ml / min, and a partial oxidation reaction test of methane was carried out in the temperature range of 500 °C to 800 °C. Downstream of the reactor, heating at 100 °C by a ribbon heater and dilution of the reaction gas with N2 (100 ml / min) were carried out to prevent condensation of the generated water. The products were analyzed by a two-channel online Micro-GC (FUSION, manufactured by INFICON). In channel 1 of the Micro-GC, H2, O2, N2, CH4, and CO were quantified using a capillary column Moleculer Sieve 5A (trade name) with Ar as the carrier gas. In channel 2, CO2, C2H4, C2H6, and H2O were quantified using a capillary column Porapak (trade name) with He as the carrier gas. A TCD was used as the detector.
[0045] The conversion rate of the reactants and the yield of the products were calculated as follows. In the following equations, F means flow rate, in means inlet, and out means outlet. For example, F CH4,inmeans the inlet CH4 flow rate.
[0046]
number
[0047] In addition, the following relationship holds in the above formula:
[0048]
number
[0049] Example 1 Proton-type BEA zeolite (Zeolyst, Si / Al ratio = 13) was prepared as a methane partial oxidation catalyst. Reaction evaluation was performed using the above method. As shown in Table 2, the reaction results of proton-type BEA zeolite at 700°C were CH4 conversion 22%, O2 conversion 60%, CO selectivity 81%, H2 selectivity 20%, and carbon dioxide selectivity 19%.
[0050] Examples 2 to 21 and Comparative Examples 1 to 5 A partial oxidation reaction test of methane was carried out in the same manner as in Example 1, except that in Example 1, the catalyst shown in Table 1 was used and the reaction was carried out under the reaction conditions shown in Table 1. The results are shown in Table 2.
[0051] [Table 2]
[0052] From the results shown in Tables 1 and 2, it is possible to suppress the complete combustion reaction of methane and improve the selectivity of the partial oxidation of methane by using a zeolite composed of Si and Al and by setting the content of transition metals of groups 8 to 10 of the periodic table to less than 0.1 mass %. Specifically, the selectivity of CO2 generated by the complete oxidation of methane could be suppressed to 30% or less. It is also clear that, compared to MOR and FAU, CHA, MFI, and BEA, which have Al sites with Lewis acidity, are preferable. Furthermore, a comparison of each Example with Comparative Examples 4 and 5 shows that the methane conversion rate is low when the reaction temperature is 600° C. or lower. Therefore, it is essential in the present invention to set the reaction temperature to 650° C. or higher. [Industrial Applicability]
[0053] According to the production method of the present invention, methane can be partially oxidized with high selectivity, and synthesis gas (CO+H2) can be efficiently produced. Since synthesis gas is important as a raw material for various reactions, the present invention is a technology that can contribute to industry.
Claims
1. A zeolite catalyst used for partial oxidation of light hydrocarbons, which contains silicon (Si) and aluminum (Al) as constituent elements and has a content of elements from Groups 8 to 10 of the periodic table of less than 0.1 mass %.
2. 2. The zeolite catalyst according to claim 1, wherein the molar ratio of silicon to aluminum (Si / Al) contained in the zeolite catalyst is 1 or more and 100 or less.
3. 3. The zeolite catalyst according to claim 1 or 2, wherein the zeolite catalyst comprises at least one crystal structure selected from the group consisting of AEI, CHA, MFI, and BEA, as defined by the International Zeolite Association (IZA) code.
4. 2. The zeolite catalyst according to claim 1, wherein the light hydrocarbons are hydrocarbons having 6 or less carbon atoms.
5. 2. The zeolite-based catalyst of claim 1, wherein the light hydrocarbons are methane or predominantly methane.
6. A zeolite catalyst containing silicon (Si) and aluminum (Al) as constituent elements and having a content of elements of Groups 8 to 10 of the Periodic Table of less than 0.1 mass % is used as a catalyst; A method for producing synthesis gas by partial oxidation of methane at a reaction temperature of 650°C or higher.
7. 7. The method for producing synthesis gas according to claim 6, wherein the synthesis gas product of the partial oxidation reaction of methane comprises carbon monoxide, hydrogen, ethane, ethylene, carbon dioxide, and water, and the selectivity of carbon dioxide relative to methane is 30 mol % or less.
8. 8. The method for producing a synthesis gas according to claim 6, wherein the partial oxidation reaction of methane is performed at a molar ratio of methane to oxygen (methane / oxygen) of 1 or more.
9. The method for producing a synthesis gas according to claim 6 or 7, wherein the partial oxidation reaction of methane is carried out at 1000° C. or lower.
10. 8. The method for producing a synthesis gas according to claim 6 or 7, wherein a molar ratio of silicon to aluminum (Si / Al) contained in the zeolite-based catalyst is 1 or more and 100 or less.
11. 8. The method for producing a synthesis gas according to claim 6 or 7, wherein the zeolite in the zeolite-based catalyst comprises at least one crystal structure selected from the group consisting of AEI, CHA, MFI, and BEA, as defined by the International Zeolite Association (IZA) codes.
Citation Information
Patent Citations
Partial oxidation catalyst for light hydrocarbon and process for producing carbon monoxide using the same
JP2019181375A
Partial oxidation catalyst of light hydrocarbon, and method for producing carbon monoxide and hydrogen by the catalyst
JP2021045722A