Low-expansion high-elasticity glass substrate for light guide plate of transparent display
A glass wafer with high Young's modulus and low expansion coefficient minimizes warpage during diffractive optical element formation, ensuring precise manufacturing of light guide plates for improved image display devices.
Patent Information
- Application Number
- JP2024042297
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-18
- Publication Date
- 2024-10-11
AI Technical Summary
Conventional glass wafers warp during the formation of diffractive optical elements due to thermal expansion differences, leading to misalignment and reduced precision, which affects the quality of light guide plates used in AR, MR, and VR devices.
A glass wafer with specific properties, including a thin plate shape, high Young's modulus, low average linear expansion coefficient, and high refractive index, designed to minimize warpage during the formation of diffractive optical elements, allowing for precise manufacturing of light guide plates.
The solution reduces warpage and enhances the precision of diffractive optical elements, improving the quality and accuracy of light guide plates used in image display devices, such as smart glasses, by maintaining dimensional and positional accuracy.
Smart Images

Figure 2024144226000005 
Figure 2024144226000006 
Figure 2024144226000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a glass wafer, a light guide plate, and an image display device. [Background technology]
[0002] In recent years, with the advancement of AR (Augmented Reality), MR (Mixed Reality), and VR (Virtual Reality) technologies, display devices such as head-mounted displays have been developed as AR devices, MR devices, and VR devices. Among them, glasses-type wearable terminals called smart glasses, as disclosed in Patent Document 1, have attracted attention.
[0003] In smart glasses, light emitted from an image light source is guided to the front of the wearer's eyes by a light guide plate, which corresponds to a spectacle lens, and is displayed as an image.
[0004] Specifically, light emitted from the image light source is incident on the inside of the light guide plate by a diffractive optical element formed on the surface of the light guide plate. The light that has entered the inside of the light guide plate travels while repeatedly being totally reflected inside the light guide plate, and is emitted in the direction of the wearer's pupil by a diffractive optical element provided in front of the wearer's pupil.
[0005] The light guide plate used in smart glasses is manufactured using semiconductor circuit manufacturing equipment. In the mass production process of semiconductor circuits, a large number of integrated circuits are formed on the surface of a silicon wafer by lithography technology or the like. Then, the silicon wafer on which the large number of integrated circuits are formed is cut and separated by dicing to manufacture a large number of semiconductor circuit elements.
[0006] The light guide plate can be manufactured using the same process as the mass production of semiconductor circuits. That is, a large number of diffractive optical elements are formed on the surface of a thin glass plate such as a glass wafer, and then the plate is cut and separated by dicing to manufacture a large number of light guide plates. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2016-139174 A Summary of the Invention [Problem to be solved by the invention]
[0008] Submicron precision is required for the formation of diffractive optical elements. However, for example, when forming diffractive optical elements on the surface of a glass wafer, the glass wafer is heated to 100°C or higher. The inventors have found that with conventional glass wafers, the heating causes the glass wafer to warp, resulting in a problem that the diffractive optical elements cannot be formed with high precision. Specifically, the problem is as follows.
[0009] The material of the diffractive optical element is an inorganic material such as titanium oxide, silicon nitride, silicon carbide, or an organic material such as a transparent resin. When an inorganic material is used, a film of the inorganic material is formed on the surface of a glass wafer, and the film is finely processed by photolithography to form a diffractive optical element. In photolithography, a photoresist is applied to the film-formed surface of the glass wafer, and the wafer is heated on a hot plate and pre-baked to evaporate the solvent of the photoresist. Next, the pattern of the photomask is transferred to the photoresist by ultraviolet light exposure. After exposure, the wafer is placed on a hot plate and heated (post-baked) to about 120 to 150°C to thermally crosslink the photoresist. Next, the photoresist is developed, and then fine irregularities are formed in the film by etching to form a diffractive optical element. When an organic material is used, a resin such as a transparent ultraviolet curable resin is applied to the main surface of the glass wafer to form a coating film, and the fine irregularity pattern of the diffractive optical element is pressed with a mold having an inverted shape to transfer the pattern to the coating film. The wafer is then placed on a hot plate and heated to around 125° C. to bake it, forming a diffractive optical element.
[0010] Regardless of whether the material is inorganic or organic, warping of the glass wafer occurs when the glass wafer is heated on a hot plate. Glass has a relatively low thermal conductivity, and when heated on a hot plate, a large temperature difference occurs between the main surface facing the hot plate, i.e., the main surface facing downward, and the main surface on the opposite side, i.e., the main surface facing upward. The amount of expansion of the high-temperature main surface facing downward is greater than the amount of expansion of the low-temperature main surface facing upward, so the glass wafer warps into a downward convex shape. The periphery of the warped glass wafer is separated from the hot plate, so the center of the main surface is hotter than the periphery. In this state, thermal crosslinking of the photoresist and baking of the organic material are performed, so that even after heating is completed, the fine pattern of the diffractive optical element is misaligned.
[0011] As described above, after the diffractive optical elements are formed, the glass wafer is cut and separated by dicing to manufacture a large number of light guide plates, but the positional accuracy of the diffractive optical elements in each light guide plate decreases due to misalignment of the diffractive optical elements on the wafer. As a result, a shift occurs in the direction of light diffraction, and when assembling an image display device, a correction operation for this shift is required, or if the amount of misalignment is large, the quality of the displayed image decreases.
[0012] Therefore, there is a demand for a glass wafer on which diffractive optical elements can be formed with high precision.
[0013] The present invention has been made in consideration of the above-described circumstances, and has an object to provide a glass wafer in which warping during formation of a diffractive optical element is reduced, a light guide plate obtained from the glass wafer, and an image display device including the light guide plate. [Means for solving the problem]
[0014] The gist of the present invention is as follows.
[0015] (1) A glass portion having a thin plate shape and a diffractive optical element portion on a main surface thereof; The area of one of the main glass surfaces is 1950 mm 2 That's all. The thickness of the glass part is 3.0 mm or less, The Young's modulus of the glass portion is 100 GPa or more, The average linear expansion coefficient of the glass part at -30℃ to 70℃ is 80×10 -6 K -1 Below is the A glass wafer for manufacturing light guide plates.
[0016] (2) The glass wafer according to (1), wherein the diffractive optical element portion has a periodic uneven structure, and the period of the uneven structure is 500 nm or less.
[0017] (3) The glass wafer according to (1), wherein the refractive index nd of the glass portion is 1.9 or more.
[0018] (4) A glass portion and a diffractive optical element portion on a main surface thereof; The Young's modulus of the glass portion is 100 GPa or more, The average linear expansion coefficient of the glass part at -30℃ to 70℃ is 80×10 -6 K -1 Below is a light guide plate.
[0019] (5) The light guide plate according to (4), wherein the diffractive optical element portion has a periodic uneven structure, and the period of the uneven structure is 500 nm or less.
[0020] (6) The light guide plate according to (4), wherein the refractive index nd of the glass portion is 1.9 or more.
[0021] (7) An image display device comprising the light guide plate according to (4) above.
[0022] (8) The image display device according to (7), which is of a glasses type. Effect of the Invention
[0023] According to the present invention, it is possible to provide a glass wafer in which warping during formation of a diffractive optical element is reduced, a light guide plate obtained from the glass wafer, and an image display device including the light guide plate. [Brief description of the drawings]
[0024] [Figure 1] FIG. 1 is a diagram showing a schematic configuration of a head mounted display using a light guide plate according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a side view that illustrates a schematic configuration of a head mounted display that uses a light guide plate according to one embodiment of the present invention. [Diagram 3] FIG. 3 is a diagram showing a schematic diagram of a method for measuring the BOW. [Figure 4] FIG. 4 is a diagram showing a schematic view of the glass portion when viewed from above, and illustrates a method for evaluating the warpage of the glass portion. [Figure 5(1)] FIG. 5(1) is a schematic diagram showing a cross section of a glass portion, and illustrates a method for evaluating the warpage of the glass portion. [Figure 5 (2)] FIG. 5(2) illustrates a method for evaluating the warpage of the glass portion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] In this specification, unless otherwise specified, the refractive index refers to the refractive index nd at the d line of helium (wavelength 587.56 nm).
[0026] The Abbe number νd is used as a value representing the properties related to dispersion, and is expressed by the following formula: Here, nF is the refractive index at the F line (wavelength 486.13 nm) of blue hydrogen, and nC is the refractive index at the C line (656.27 nm) of red hydrogen. νd=(nd-1) / (nF-nC)
[0027] In the present invention, unless otherwise specified, the glass composition is expressed on an oxide basis. Here, the term "glass composition on an oxide basis" refers to a glass composition obtained by converting the glass raw materials into glass that are all decomposed during melting and exist as oxides in the glass. All glass components expressed on an oxide basis (Sb (Sb 2 O 3 ) and Ce(CeO 2The total content of each glass component is 100 mass %. 2 , TiO 2 The contents and total contents of glass components are based on mass unless otherwise specified, and "%" means "mass %".
[0028] The content of the glass component can be quantified by known methods, such as inductively coupled plasma atomic emission spectrometry (ICP-AES), inductively coupled plasma mass spectrometry (ICP-MS), etc. In the present invention, the content of a component being 0% means that the component is substantially not contained, and it is acceptable for the component to be contained at an unavoidable impurity level.
[0029] An embodiment of the present invention will be described below.
[0030] Glass Wafer The glass wafer according to this embodiment has a thin glass portion and a diffractive optical element portion on the main surface thereof.
[0031] <Glass Department> (shape) In the glass wafer according to this embodiment, the glass portion has a thin plate shape. Preferably, the glass portion has a disk shape. The glass portion may have a thin plate shape in which the main surface has a polygonal, square, or rectangular shape. When the glass portion has such a thin plate shape, a light guide plate can be manufactured from the glass wafer using ordinary semiconductor circuit manufacturing equipment.
[0032] (area) In the glass wafer according to this embodiment, the area of one main surface of the glass portion is 1950 mm 2 More than 4400mm, preferably 4400mm 2 More preferably, 7850 mm 2 More preferably, 17670 mm 2 More preferably, 70690 mm 2That is all. By increasing the area of the main surface of the glass portion, the number of light guide plates that can be obtained per unit area can be increased. There is no particular upper limit to the area of the main surface of the glass portion, but from the viewpoint of using ordinary semiconductor circuit manufacturing equipment, it is usually 159050 mm 2 It is.
[0033] (Diameter of inscribed circle) In the glass wafer according to this embodiment, the size of the glass part can also be evaluated by the size of a circle virtually inscribed in the shape of the main surface of the glass part. That is, the diameter of the circle virtually inscribed in the shape of the main surface of the glass part is preferably 50 mm or more, more preferably 75 mm or more, even more preferably 100 mm or more, and even more preferably 150 mm or more. By increasing the diameter of the inscribed circle, the number of light guide plates obtained per unit area can be increased. The upper limit of the diameter of the inscribed circle is not particularly limited, but is usually 450 mm from the viewpoint of using normal semiconductor circuit manufacturing equipment.
[0034] (diameter) In the glass wafer according to this embodiment, when the glass portion is disk-shaped, the diameter of the glass portion is preferably 50 mm or more, more preferably 75 mm or more, even more preferably 100 mm or more, and even more preferably 150 mm or more. By increasing the diameter of the glass portion, the number of light guide plates obtained per unit area can be increased. The upper limit of the diameter of the glass portion is not particularly limited, but is usually 450 mm from the viewpoint of using ordinary semiconductor circuit manufacturing equipment.
[0035] (Thickness) In the glass wafer according to this embodiment, the thickness of the glass portion is 3.0 mm or less, preferably 1.0 mm or less, more preferably 0.8 mm or less, and even more preferably 0.5 mm or less. The lower limit of the thickness of the glass portion is not particularly limited, but is usually 0.2 mm, preferably 0.25 mm. By setting the thickness of the glass portion within the above range, a light guide plate that can be used as a lens for smart glasses can be manufactured, and the light guide plate can be manufactured from the glass wafer using ordinary semiconductor circuit manufacturing equipment.
[0036] (Young's Modulus) In the glass wafer according to this embodiment, the Young's modulus of the glass part is 100 GPa or more, preferably 110 GPa or more, more preferably 120 GPa or more. The upper limit of the Young's modulus of the glass part is not particularly limited, but is usually 150 GPa, preferably 140 GPa. By setting the Young's modulus of the glass part within the above range, warping of the glass part can be reduced when the glass part is heated to form a diffractive optical element part on its main surface, and the diffractive optical element part can be formed with high accuracy. In addition, by setting the Young's modulus of the glass part within the above range, breakage during transport of the glass wafer can be reduced. In addition, breakage during insertion and removal of the glass wafer or glass part from the wafer cassette and breakage during processing can also be reduced.
[0037] Young's modulus is measured and calculated in accordance with JIS R 1602-1995. Specifically, a glass sample made of the same material as the glass part, measuring 20 mm in length, 20 mm in width and 100 mm in height, is fully annealed and placed in a temperature-controlled chamber, and the longitudinal wave velocity (Vl) and shear wave velocity (Vs) of 5 MHz ultrasound are measured, and Young's modulus (E) and rigidity modulus (G) are calculated using the following formulas. E=(4G 2 -3G×Vl 2 ×ρ) / (G-Vl 2 ×ρ) G=Vs 2 ×ρ Here, ρ is the density of the glass sample, and the value of specific gravity can be used. The density (specific gravity) of the glass sample at room temperature and the density (specific gravity) of the glass part at room temperature are assumed to be the same. In other words, the density at room temperature is calculated by multiplying the specific gravity by the unit g / cm. 3 It is expressed by adding .
[0038] (Average linear expansion coefficient α at -30℃ to 70℃ n ) In the glass wafer according to this embodiment, the average linear expansion coefficient α of the glass portion at −30° C. to 70° C. n is 80 x 10 -6 K -1 or less, preferably 75×10-6 K -1 The average linear expansion coefficient α of the glass part at -30℃ to 70℃ is as follows. n The lower limit is not particularly limited, but is usually 60×10 -6 K -1 The average linear expansion coefficient α of the glass part at -30℃ to 70℃ n By setting the thickness within the above range, even when the diffractive optical element portion is heated from one side on a hot plate during formation, the difference in expansion between the two main surfaces of the glass portion can be reduced, and warping of the glass portion can be reduced.
[0039] Average linear expansion coefficient α at -30℃ to 70℃ n is measured using an interferometric dilatometer and calculated according to the following formula: α n =dL n / (L×dT n ) Here, dT n is the temperature difference from -30 to 70°C (K), L is the initial length of the glass sample (mm), dL n is the change in sample length (mm) in the temperature range of -30 to 70°C.
[0040] (Refractive index nd) In the glass wafer according to this embodiment, the refractive index nd of the glass portion is preferably 1.9 or more, more preferably 1.95 or more, and even more preferably 2.00 or more. The upper limit of the refractive index nd of the glass portion is not particularly limited, but is usually 2.2. From the viewpoint that the light incident on the glass portion travels inside the glass portion while repeating total reflection and exits at a sufficient viewing angle, it is preferable that the refractive index of the glass portion is within the above range.
[0041] (Abbe number νd) In the glass wafer according to this embodiment, the upper limit of the Abbe number vd of the glass portion can be 40, or can be 35 or 30. The lower limit of the Abbe number vd of the glass portion is not particularly limited, but is usually 15.
[0042] (glass transition temperature Tg) In the glass wafer according to this embodiment, the glass portion has a glass transition temperature Tg of preferably 600° C. or higher, more preferably 630° C. or higher, and even more preferably 650° C. or higher. The upper limit of the glass transition temperature Tg of the glass portion is not particularly limited, but is usually 780° C., and preferably 760° C. When the glass portion is heated to form a diffractive optical element portion on its main surface, it is preferable to set the glass transition temperature Tg of the glass portion within the above range from the viewpoint of reducing warping of the glass portion and from the viewpoint of maintaining good thermal stability of the glass portion while maintaining a desired refractive index.
[0043] (internal transmittance) In the glass wafer according to this embodiment, the glass portion has light transmittance to visible light. The light transmittance can be evaluated by the internal transmittance at wavelengths of 420 nm to 800 nm in a glass sample having a thickness of 10.0 mm±0.1 mm. The internal transmittance is the transmittance excluding the surface reflection loss on the entrance side and the exit side of the glass sample. The internal transmittance τ at a specific wavelength for a thickness of 10.0±0.1 mm can be calculated by measuring the transmittances (external transmittances) T1 and T2 including the surface reflection loss of two glass samples made of the same type of glass and having different thicknesses d1 and d2, respectively, and using the following formula. logτ=-[(logT1-logT2)×10] / Δd Here, d2>d1, Δd=d2-d1, and log is the common logarithm.
[0044] The internal transmittance of a glass sample having a thickness of 10.0 mm±0.1 mm and made of the same material as the glass part, i.e., the internal transmittance of the glass part converted to a thickness of 10.0 mm±0.1 mm, is preferably 78% or more over the wavelength range of 420 nm to 800 nm, more preferably 83% or more, and even more preferably 90% or more.
[0045] The minimum value of the internal transmittance in the wavelength range of 420 nm to 800 nm is preferably the internal transmittance at the wavelength of 420 nm, which is the short wavelength end of the wavelength range. That is, the internal transmittance at a wavelength of 420 nm of a glass sample having a thickness of 10.0 mm±0.1 mm and made of the same material as the glass part (the internal transmittance of the glass part converted into a thickness of 10.0 mm±0.1 mm) is preferably 78% or more, more preferably 83% or more, and even more preferably 90% or more.
[0046] (specific gravity) In the glass wafer according to this embodiment, the specific gravity of the glass portion is preferably 5.5 or less, more preferably 5.4 or less, and even more preferably 5.3 or less. The lower limit of the specific gravity of the glass portion is not particularly limited, but is usually 4.3. When used as a spectacle lens for smart glasses, it is preferable to set the specific gravity of the glass portion within the above range in order to reduce discomfort caused by the weight of the lens when worn.
[0047] (Specific elastic modulus) In the glass wafer according to this embodiment, the specific elastic modulus of the glass part is preferably 24.0 MN / Kg or more, more preferably 24.5 MN / Kg or more, and even more preferably 25.0 MN / Kg or more. The upper limit of the specific elastic modulus of the glass part is not particularly limited, but is approximately 30 MN / Kg as a guide. From the viewpoint of reducing warpage of the glass part when the glass part is heated to form a diffractive optical element part on its main surface, it is preferable that the specific elastic modulus of the glass part is within the above range.
[0048] (material) In the glass wafer according to this embodiment, the material of the glass portion has the above-mentioned Young's modulus and the average linear expansion coefficient α n There is no particular limitation as long as it satisfies the above. Examples of the material of the glass portion include optical glass. The glass portion is preferably made of optical glass.
[0049] Specifically, the material of the glass portion can be, for example, a glass having a B-La system composition. Therefore, non-limiting examples of B-La system glass compositions are shown below. Note that the material of the glass portion is not limited to the glass having the B-La system composition shown below, and any material can be used as long as it can provide a glass wafer that can reduce warping during the formation of a diffractive optical element.
[0050] The glass portion preferably has the following glass composition (expressed in mass %). B 2 O 3 and SiO 2 The total content of [B 2 O 3 +SiO 2 ] is preferably 5 to 25%. La 2 O 3 , Gd 2 O 3 , Y 2 O 3 , and Yb 2 O 3 The total content of [La 2 O 3 +Gd 2 O 3 +Y 2 O 3 +Yb 2 O 3 ] is preferably 25 to 68%. TiO 2 , Nb 2 O 5 , Ta 2 O 5 , and W.O. 3 The total content [TiO 2 +Nb 2 O 5 +Ta 2 O 5 +WO 3 ] is preferably 5 to 40%. The total content of MgO, CaO, SrO and BaO [MgO+CaO+SrO+BaO] is preferably 0 to 20%. Li 2 O, Na 2 O, and K 2Total O content [Li 2 O+Na 2 O+K 2 O] is preferably 0 to 5%. ZrO 2 The content is preferably 0 to 12%. The ZnO content is preferably 0 to 10%. B 2 O 3 The content is preferably 3 to 20%. SiO 2 The content is preferably 0 to 15%. La 2 O 3 The content is preferably 25 to 60%. Gd 2 O 3 The content is preferably 0 to 30%. Y 2 O 3 The content is preferably 0 to 16%. Yb 2 O 3 The content is preferably 0 to 5%. The TiO content is preferably 0 to 28%. Nb 2 O 5 The content is preferably 0 to 15%. Ta 2 O 5 The content is preferably 0 to 10%. WO 3 The content is preferably 0 to 6%. The content of MgO is preferably 0 to 5%. The CaO content is preferably 0 to 5%. The content of SrO is preferably 0 to 5%. The content of BaO is preferably 0 to 20%. Li 2 The O content is preferably 0 to 5%. Na 2 The O content is preferably 0 to 5%. K 2The O content is preferably 0 to 5%. Sb 2 O 3 The content is preferably 0 to 1%. Lu 2 O 3 The content is preferably 0 to 1%. Sc 2 O 3 The content is preferably 0 to 1%. Ga 2 O 3 The content is preferably 0 to 1%. GeO 2 The content is preferably 0 to 1%.
[0051] In order to increase the Young's modulus in the glass portion, the total content [La 2 O 3 +Gd 2 O 3 +Y 2 O 3 +Yb 2 O 3 ], ZrO 2 In order to suppress an increase in the average linear expansion coefficient, it is preferable that the total content [MgO+CaO+SrO+BaO] and the total content [Li 2 O+Na 2 O+K 2 O] is preferably within the above range.
[0052] It is preferable that the glass portion does not contain Pb, Te, Cd, Th, Tl, V, Cr, Ni, Fe, U, Nd, Cu, Er, Eu, etc.
[0053] <Diffractive optical element> The glass wafer according to this embodiment has a diffractive optical element portion on the main surface of the glass portion. The diffractive optical element portion is not particularly limited as long as it includes a portion that functions as a diffraction grating. For example, the diffractive optical element portion includes a diffraction grating that functions to diffract light (image) incident from an image light source into the glass portion, i.e., a diffractive optical element for light incidence, or a diffraction grating that functions to diffract light traveling through the glass portion by total reflection and emit it to the outside, i.e., a diffractive optical element for light emission. In this case, the glass wafer is cut by dicing, and a diffractive optical element for incidence and a diffractive optical element for emission are formed in each region that will become a light guide plate after separation. Since the light beam before entering the light guide plate is thin, the area of the diffractive optical element for incidence may be relatively small. On the other hand, the diffractive optical element for emission has a relatively large area because it displays an image in an enlarged manner in front of the pupil of the person wearing the image display device. The larger the viewing angle, the larger the area of the diffractive optical element for emission.
[0054] In the glass wafer according to this embodiment, the shape of the diffraction grating in the diffractive optical element part is not particularly limited. Therefore, the diffraction grating may be a diffraction grating having a grooved shape, or may be a so-called holographic diffraction grating using holography. For example, the diffractive optical element part may have a periodic uneven structure as a diffraction grating. In this case, from the viewpoint that the light (image) incident from the image light source travels while repeating total reflection inside the glass part, and from the viewpoint that the light is emitted at a sufficient viewing angle, the period of the uneven structure is preferably 500 nm or less, more preferably 400 nm or less, and may be 280 nm or less.
[0055] The material of the diffractive optical element is not particularly limited, and may be an inorganic material or an organic material. From the viewpoint of maintaining the light transmittance as a spectacle lens of smart glasses, a transparent material is preferable. Examples of inorganic materials include, but are not limited to, titanium oxide, silicon nitride, and silicon carbide. In addition, in films of titanium oxide, silicon nitride, silicon carbide, etc., the molar ratio of elements such as Ti, Si, O, N, and C is not necessarily an integer ratio (non-stoichiometric). Therefore, in this specification, the inorganic material of the diffractive optical element will be described as titanium oxide, silicon nitride, silicon carbide, etc., including those that are in a stoichiometric ratio and those that are not in a stoichiometric ratio. Examples of organic materials include transparent resins, and may be, for example, ultraviolet-curable resins.
[0056] A large number of light guide plates can be manufactured by cutting and separating the glass wafer according to this embodiment by dicing.
[0057] light guide plate The light guide plate according to this embodiment has a glass portion and a diffractive optical element portion on the main surface thereof.
[0058] The light guide plate according to this embodiment inherits the characteristics of the glass wafer as is, and the characteristics of the glass portion and the diffractive optical element portion in the glass wafer can be directly used as the characteristics of the glass portion and the diffractive optical element portion in the light guide plate.
[0059] In particular, in the light guide plate according to this embodiment, the Young's modulus of the glass portion is 100 GPa or more, preferably 110 GPa or more, and more preferably 120 GPa or more. The upper limit of the Young's modulus of the glass portion is not particularly limited, but is usually 150 GPa, and preferably 140 GPa.
[0060] In the light guide plate according to this embodiment, the average linear expansion coefficient α of the glass portion at −30° C. to 70° C. n is 80 x 10 -6 K -1 or less, preferably 75×10 -6 K -1The average linear expansion coefficient α of the glass part at -30℃ to 70℃ is as follows. n The lower limit is not particularly limited, but is usually 60×10 -6 K -1 It is.
[0061] In the glass portion and the diffractive optical element portion of the light guide plate according to this embodiment, characteristics other than those described above, i.e., the thickness, refractive index nd, Abbe number νd, glass transition temperature Tg, internal transmittance, specific gravity, specific elasticity, and material of the glass portion, as well as the type, shape, diffraction grating period, and material of the diffractive optical element portion, can be made similar to those of the glass portion and the diffractive optical element portion of the glass wafer.
[0062] Image display device The image display device according to this embodiment includes the above-mentioned light guide plate.
[0063] Hereinafter, a light guide plate according to one embodiment of the present invention and an image display device using the same will be described in detail with reference to the drawings. In the drawings, the same or corresponding parts are designated by the same reference characters and their description will not be repeated.
[0064] FIG. 1 is a diagram showing an example of the configuration of a head mounted display 1 (hereinafter, abbreviated as "HMD1") using a light guide plate 10 according to an embodiment of the present invention, in which FIG. 1(a) is a front perspective view of the HMD1, and FIG. 1(b) is a rear perspective view of the HMD1. As shown in FIG. 1(a) and FIG. 1(b), a spectacle lens 3 is attached to the front part of a spectacle-type frame 2 worn on the head of a user. A backlight 4 for illuminating an image is attached to a mounting part 2a of the spectacle-type frame 2. A signal processing device 5 for projecting an image and a speaker 6 for reproducing sound are provided on the temple part of the spectacle-type frame 2. Flexible printed circuits (FPCs) 7 constituting wiring drawn from the circuit of the signal processing device 5 are wired along the spectacle-type frame 2. A display element unit (e.g., a liquid crystal display element) 20 is wired to the center position of both eyes of the user by the FPC 7, and is held so that the approximate center of the display element unit 20 is located on the optical axis of the backlight 4. The imager unit 20 is fixed relatively to the light guide plate 10 so as to be located approximately at the center of the light guide plate 10. Holographic optical elements (HOEs) 32R and 32L (first optical elements) are formed on the first surface 10a of the light guide plate 10 at positions in front of the user's eyes. HOEs 52R and 52L are formed on the second surface 10b of the light guide plate 10 at positions facing the imager unit 20 across the light guide plate 10.
[0065] FIG. 2 is a side view showing a schematic configuration of an HMD 1 according to an embodiment of the present invention. In FIG. 2, in order to clarify the drawing, only the main parts of the image display device are shown, and the eyeglass-type frame 2 and the like are omitted. As shown in FIG. 2, the HMD 1 has a bilaterally symmetrical structure with respect to a center line X connecting the center of the image display element 24 and the light guide plate 10. Furthermore, the light of each wavelength incident on the light guide plate 10 from the image display element 24 is divided into two and guided to the right eye and the left eye of the user, as described later. The optical paths of the light of each wavelength guided to each eye are also approximately bilaterally symmetrical with respect to the center line X.
[0066] As shown in FIG. 2, the backlight 4 has a laser light source 21, a diffusion optical system 22, and a microlens array 23. The display element unit 20 is an image generating unit having an image display element 24, and is driven, for example, by a field sequential method. The laser light source 21 has laser light sources corresponding to the wavelengths of R (wavelength 633 nm), G (wavelength 546 nm), and B (wavelength 436 nm), and sequentially irradiates light of each wavelength at high speed. The light of each wavelength is incident on the diffusion optical system 22 and the microlens array 23, and is converted into a uniform, highly directional parallel light beam without unevenness in the amount of light, and is incident perpendicularly on the display panel surface of the image display element 24.
[0067] The image display element 24 is, for example, a transmissive liquid crystal (LCDT-LCOS) panel driven by a field sequential method. The image display element 24 modulates the light of each wavelength according to an image signal generated by an image engine (not shown) of the signal processing device 5. The light of each wavelength modulated by the pixels in the effective area of the image display element 24 is incident on the light guide plate 10 with a predetermined light beam cross section (approximately the same shape as the effective area). The image display element 24 can also be replaced with other types of display elements, such as a DMD (Digital Mirror Device), a reflective liquid crystal (LCOS) panel, a MEMS (Micro Electro Mechanical Systems), an organic EL (Electro-Luminescence), or an inorganic EL.
[0068] The image generating unit of the image display element 20 is not limited to a field sequential type image display element, but may be a simultaneous type image display element (a display element having a predetermined arrangement of RGB color filters in front of the emission surface). In this case, for example, a white light source is used as the light source.
[0069] As shown in Fig. 2, the light of each wavelength modulated by the image display element 24 is sequentially incident on the inside of the light guide plate 10 from the first surface 10a. HOEs 52R and 52L (second diffractive optical elements) are formed on the second surface 10b of the light guide plate 10. The HOEs 52R and 52L are, for example, reflective volume phase HOEs having a rectangular shape, and are configured by laminating three photopolymer sheets on which interference fringes corresponding to the light of each wavelength of R, G, and B are recorded. In other words, the HOEs 52R and 52L are configured to have a wavelength selection function that diffracts the light of each wavelength of R, G, and B and transmits the light of the other wavelengths.
[0070] The HOEs 32R and 32L are also reflective volume phase type HOEs and have the same layer structure as the HOEs 52R and 52L. The HOEs 32R and 32L and the HOEs 52R and 52L may have, for example, approximately the same pitch of the interference fringe patterns.
[0071] The HOEs 52R and 52L are stacked with their centers aligned and with their interference fringe patterns inverted by 180 degrees. They are formed on the second surface 10b of the light guide plate 10 so that their centers aligned with the center line X when stacked. Light of each wavelength modulated by the image display element 24 is sequentially incident on the HOEs 52R and 52L via the light guide plate 10.
[0072] The HOEs 52R and 52L each diffract the light of each wavelength incident sequentially at a predetermined angle to guide it to the right eye and the left eye. The light of each wavelength diffracted by the HOEs 52R and 52L is repeatedly totally reflected at the interface between the light guide plate 10 and the air, propagates inside the light guide plate 10, and is incident on the HOEs 32R and 32L. Here, the HOEs 52R and 52L give the same diffraction angle to the light of each wavelength. Therefore, all the light of wavelengths that are incident at approximately the same position on the light guide plate 10 (or, in other words, emitted from approximately the same coordinates within the effective area of the image display element 24) propagate through approximately the same optical path within the light guide plate 10 and are incident on approximately the same position on the HOEs 32R and 32L. From another perspective, the HOEs 52R and 52L diffract the light of each wavelength of RGB so that the pixel positional relationship within the effective area of the image displayed in the effective area of the image display element 24 is faithfully reproduced on the HOEs 32R and 32L.
[0073] Thus, in one aspect of the present invention, HOEs 52R and 52L each diffract light of all wavelengths emitted from approximately the same coordinates within the effective area of image display element 24 so that it is incident on approximately the same position on HOEs 32R and 32L. Alternatively, HOEs 52R and 52L may be configured to diffract light of all wavelengths that originally constitute the same pixel but are relatively shifted within the effective area of image display element 24 so that it is incident on approximately the same position on HOEs 32R and 32L.
[0074] The light of each wavelength incident on the HOEs 32R and 32L is diffracted by the HOEs 32R and 32L and sequentially emitted from the second surface 10b of the light guide plate 10 in a substantially perpendicular direction to the outside. The light of each wavelength emitted as substantially parallel light in this manner is imaged on the right and left retina of the user as a virtual image I of the image generated by the image display element 24. In addition, a condenser effect may be given to the HOEs 32R and 32L so that the user can observe the virtual image I of the enlarged image. That is, the light incident on the peripheral area of the HOEs 32R and 32L may be emitted at an angle closer to the center of the pupil and imaged on the user's retina. Alternatively, in order to allow the user to observe the virtual image I of the enlarged image, the HOEs 52R and 52L may diffract the light of each wavelength of RGB so that the pixel positional relationship on the HOEs 32R and 32L forms an enlarged similar shape to the pixel positional relationship within the effective area of the image displayed in the effective area of the image display element 24.
[0075] Since the air-equivalent optical path length of light traveling inside the light guide plate 10 becomes shorter as the refractive index increases, by using the light guide plate according to this embodiment having a glass portion with a high refractive index, it is possible to increase the apparent viewing angle relative to the width of the image display element 24. Furthermore, in this embodiment, although the refractive index of the glass portion is high, the specific gravity is kept low, so that it is possible to provide a light guide plate that is lightweight yet provides the above-mentioned effects.
[0076] In the above, a head mounted display has been described as an example of an image display device, but the image display device according to the present embodiment may be a pair of eyeglass-type smart glasses. Alternatively, the image display device may be another image display device. Alternatively, the diffractive optical element may be a diffraction grating having a fine concave-convex periodic structure instead of a holographic diffraction grating. In the above example, a light guide plate for both eyes has been described, but it is also possible to use separate light guide plates for displaying images to the left eye and the right eye.
[0077] <Glass Wafer Manufacturing> The glass wafer according to this embodiment can be manufactured by producing a glass portion and forming a diffractive optical element portion on the main surface thereof.
[0078] The glass portion can be manufactured by using, for example, a glass molded body. The manufacture of a glass molded body made of optical glass will be described below as an example.
[0079] Optical glass may be manufactured by blending glass raw materials to obtain a predetermined composition, and using the blended glass raw materials according to a known glass manufacturing method. For example, a plurality of compounds may be blended and thoroughly mixed to obtain batch raw materials, which are then placed in a quartz crucible or platinum crucible to be roughly melted (rough melt). The molten material obtained by rough melting is quenched and crushed to produce cullet. The cullet is then placed in a platinum crucible, heated, and remelted (remelt) to obtain molten glass, which is then clarified and homogenized, molded, and slowly cooled to obtain a glass molded body made of optical glass. Known methods may be used to mold and slowly cool the molten glass.
[0080] As long as a desired glass component can be introduced into the glass in a desired content, the compound used when preparing the batch raw materials is not particularly limited. Examples of such compounds include oxides, carbonates, nitrates, hydroxides, and fluorides.
[0081] The glass portion can be produced by a method including a step of processing a glass molded body, for example, cutting, milling, rough grinding, fine grinding, polishing, etc.
[0082] The glass portion can also be produced, for example, by the following method.
[0083] Glass raw materials are melted to a predetermined composition by a known method to produce molten glass, which is then poured into a mold and formed into a plate to produce a glass material made of optical glass. The glass material obtained is appropriately cut, ground, and polished to produce cut pieces of a size and shape suitable for press molding. The cut pieces are heated and softened, and press molded (reheat pressed) by a known method to produce a glass blank that approximates the shape of the glass portion. The glass blank is annealed, and then ground and polished by a known method to produce the glass portion.
[0084] The glass wafer can be manufactured by forming a diffractive optical element portion on the main surface of the glass portion. The method of forming the diffractive optical element portion is not particularly limited. For example, the following will exemplify the case where the diffractive optical element portion is formed from an organic material and the case where the diffractive optical element portion is formed from an inorganic material. Note that, when the diffractive optical element portion is a holographic diffraction grating, it may be formed by a known method.
[0085] When using an organic material, the organic material is applied to one of the main surfaces of the glass portion to form a coating film, and a mold having an inverted shape of the diffraction grating pattern of the diffractive optical element portion is transferred to the coating film. The glass wafer is then heated and baked at about 125°C to produce a glass wafer having the diffractive optical element portion formed at a predetermined position on the main surface of the glass portion. The organic material is not particularly limited, but may be a transparent resin, such as an ultraviolet-curable resin.
[0086] When using an inorganic material, an inorganic material film is formed on one of the main surfaces of the glass portion in a vacuum chamber by sputtering, deposition, or chemical vapor deposition (CVD). After the film is formed, the glass is removed from the vacuum chamber, a photoresist is applied, pre-baked, exposed, post-baked (at about 120 to 150° C.), developed, and then etched to form a diffraction grating pattern. This allows the manufacture of a glass wafer having a diffractive optical element portion formed at a predetermined position on the main surface of the glass portion. Examples of inorganic materials include, but are not limited to, titanium oxide, silicon nitride, and silicon carbide.
[0087] <Manufacture of light guide plates> The method for manufacturing the light guide plate is not particularly limited, and the light guide plate can be manufactured by a known method. For example, a glass wafer on which a diffractive optical element portion is formed as described above is cut and separated by dicing to manufacture a plurality of light guide plates. When cutting and separating the glass wafer, an anti-reflection film may be formed on the main surface of the wafer, a protective sheet may be attached thereon with an ultraviolet peelable adhesive to protect the main surface of the wafer, and the protective sheet may be peeled off by irradiating ultraviolet light after cutting and separating.
[0088] <Manufacture of image display devices> The manufacturing method of the image display device is not particularly limited, and the image display device can be manufactured by a known method. For example, in the case of a glasses-type image display device, the light guide plate is incorporated into a head-mounted display 1 shown in Fig. 2, that is, the light guide plate is mounted on a frame together with a light source and an optical system, and the image display device can be manufactured. EXAMPLES
[0089] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the embodiments shown in the examples.
[0090] Example 1 Glass wafers including glass portions made of Glass A, B, or C shown in Table 1 were prepared by the following procedure, and various evaluations were carried out.
[0091] [Preparation of glass samples] Compound raw materials corresponding to the components of the glass portion, i.e., raw materials such as oxides and carbonates, were weighed and thoroughly mixed to prepare a blended raw material. The blended raw material was placed in a platinum crucible, heated to 1000 to 1350°C in an air atmosphere or a water vapor atmosphere to melt, and homogenized and clarified by stirring to obtain a molten glass. The molten glass was cast into a mold to be molded, and slowly cooled to obtain a glass sample. The glass melted in a water vapor atmosphere was heat-treated in air for a long period of time to increase the transmittance in the visible range.
[0092] [Optical property measurements] The obtained glass samples were measured for refractive index nd, Abbe number νd, glass transition temperature Tg, Young's modulus, and average linear expansion coefficient α by the following methods. n The specific gravity, specific elastic modulus, and internal transmittance at wavelengths of 420 nm and 800 nm (converted value at a thickness of 10.0 mm) were measured. The results are shown in Table 1.
[0093] [Refractive index nd and Abbe number νd] The refractive indices nd, ng, nF, and nC were measured according to the refractive index measurement method of JIS B 7071-1, and the Abbe number vd was calculated according to the following formula. νd=(nd-1) / (nF-nC)
[0094] [Glass transition temperature Tg] The glass transition temperature Tg was measured using a differential scanning calorimeter (DSC3300SA) manufactured by NETZSCH JAPAN at a heating rate of 10° C. / min.
[0095] [Young's Modulus] The Young's modulus was measured and calculated in accordance with JIS R 1602-1995. Specifically, a glass sample was processed to a size of 20 mm in length, 20 mm in width, and 100 mm in height, sufficiently annealed, and placed in a temperature-controlled chamber. The longitudinal wave velocity (Vl) and shear wave velocity (Vs) of 5 MHz ultrasound were measured, and the Young's modulus (E) and rigidity modulus (G) were calculated by the following formulas. E=(4G 2 -3G×Vl 2 ×ρ) / (G-Vl 2 ×ρ) G=Vs 2 ×ρ Here, ρ is the density of the glass sample, and the value of the specific gravity is used.
[0096] [Average linear expansion coefficient α at -30℃ to 70℃ n 〕 Average linear expansion coefficient α at -30℃ to 70℃ n was measured using an interferometric dilatometer and calculated according to the following formula: α n =dL n / (L×dT n ) Here, dT n is the temperature difference from -30 to 70°C (K), L is the initial length of the glass sample (mm), dL n is the change in sample length (mm) in the temperature range of -30 to 70°C.
[0097] 〔specific gravity〕 The specific gravity was measured by the Archimedes method.
[0098] [Specific elastic modulus] The specific elastic modulus was calculated by dividing the Young's modulus by the density at room temperature. The density at room temperature is expressed in units of specific gravity (g / cm 3 ) is added.
[0099] [Internal transmittance] The glass samples were processed to have a thickness of 10 mm ± 0.1 mm and parallel, optically polished flat surfaces, and the internal transmittances at wavelengths of 420 nm and 800 nm were measured. The internal transmittance τ was calculated using the following formula by measuring the transmittances (external transmittances) T1 and T2, including the surface reflection loss, of two glass samples made of the same glass sample but with different thicknesses d1 and d2. logτ=-[(logT1-logT2)×10] / Δd Here, d2>d1, Δd=d2-d1, and log is the common logarithm.
[0100] [Table 1]
[0101] [Preparation of glass wafer] The glass sample was cut, ground, and polished to produce a disk-shaped glass part. The area, diameter, and thickness of one main surface of the glass part are shown in Table 2. The flatness of the glass part before the diffractive optical element part was formed was evaluated by BOW. It was also confirmed that the warping of the glass part was reduced when the diffractive optical element part was formed.
[0102] [Flatness before forming diffractive optical element (BOW)] The flatness was evaluated by the BOW. The BOW was measured using a flatness measuring instrument, Flat Master MSP300, manufactured by Tropel. The BOW can be measured using a known method, for example, a non-contact BOW measuring instrument, and the standard for measuring the BOW in the American Society for Testing and Materials standard ASTM F534 can be applied. Specifically, the glass part was supported at three points arranged at equal intervals (120° intervals) on the circumference of a virtual circle with a diameter slightly smaller than the diameter of the glass part. At this time, the center of the glass part and the center of the virtual circle were aligned vertically, and the glass part was not fixed (clamped). The deviation of the center point of the central surface of the glass part from a virtual plane (called the central surface reference plane) including the three points supporting the glass part was taken as the BOW.
[0103] As shown in Figure 3, the central surface is an imaginary surface that is equidistant from the two main surfaces of the glass part and is inside the glass part. When the center point of the central surface of the glass part is above the central surface reference plane, the BOW has a positive value. On the other hand, when the center point of the central surface of the glass part is below the central surface reference plane, the BOW has a negative value. The larger the absolute value of BOW, the greater the curvature of the glass part.
[0104] [Evaluation of warpage of glass part during formation of diffractive optical element part] When multiple diffractive optical element sections are formed simultaneously on the main surface of the glass section, it is required that the dimensional accuracy and positional accuracy of all diffractive optical element sections be within an acceptable range. Warping of the glass section is a factor that reduces the above-mentioned dimensional accuracy and positional accuracy. Below, we will explain the effect that warping of the glass section has on the dimensional accuracy and positional accuracy of the diffractive optical element section. The bow value is used to quantitatively express the warping (flatness) of the glass section.
[0105] The disk-shaped glass part having a diameter Φ (mm) will be described. The area on the main surface of the glass part where the diffractive optical element part is formed is called the effective area. As shown in Figure 4, the effective area is the area surrounded by circle A with a radius of [(Φ / 2)-5 mm] from the center.
[0106] As shown in Figures 5(1) and (2), assuming a central surface reference plane for circle A, [(Φ / 2)-5mm] is the effective range length c. In other words, the effective range length c is expressed by the following equation. c=(Φ / 2)-5mm When the glass part is viewed in a plane from the direction of the central axis, the distance from the center of the glass part to the circumference of circle A is called the effective length b. The following equation holds between the BOW value a, execution length b, and effective range length c. a 2 +b 2 =c 2 From the above, the following equation holds: b=[c 2 -a 2 ] 1 / 2 =[{(Φ / 2)-5mm} 2 -a 2 ] 1 / 2 That is, the difference (deviation amount) between the effective range length c and the execution length b is expressed as follows. cb = [(Φ / 2)-5mm]-[{(Φ / 2)-5mm} 2 -a 2 ] 1 / 2
[0107] When multiple diffractive optical element sections are formed on the main surface of the glass section by photolithography, the BOW value is maximized near the circumference of circle A, which indicates the effective range, and as a result, the positional deviation is maximized. This positional deviation causes an error in the period (pitch) of the uneven structure of the diffraction grating contained in the diffractive optical element section.
[0108] To maintain the performance of the diffractive optical element, it is necessary to suppress the error in the period of the uneven structure of the diffraction grating to within ±5%. Note that the smaller the period of the uneven structure of the diffraction grating, the more difficult it becomes to suppress the error.
[0109] For example, when the period of the uneven structure of the diffraction grating is 150 nm, 5% of that is 7.5 nm. In other words, "7.5 nm" is the maximum allowable error in the period of the uneven structure of the diffraction grating. Even if the glass part is warped, if the above-mentioned deviation amount [cb] is within "7.5 nm", the error in the period of the uneven structure of the diffraction grating can be suppressed to within ±5%. On the other hand, if the above-mentioned deviation amount [cb] exceeds "7.5 nm", the error in the period of the uneven structure of the diffraction grating exceeds ±5%. In such a glass part with a large warp, it is not possible to form the diffractive optical element part with high precision.
[0110] The following is a specific example of the amount of deviation when the period of the uneven structure of the diffraction grating is 150 nm. When the diameter of the glass part is 200 mm and the BOW value is 44 μm, the amount of deviation [cb] exceeds 7.5 nm, so the error in the period of the uneven structure of the diffraction grating included in the diffractive optical element part near the circumference of circle A exceeds the maximum allowable value. With such a glass part, it is not possible to form the diffractive optical element part with high precision.
[0111] Similarly, if the diameter of the glass portion is 250 mm and the BOW value is 55 μm, or if the diameter of the glass portion is 300 mm and the BOW value is 66 μm, the deviation amount [cb] exceeds 7.5 nm in both cases, and the error in the period of the uneven structure of the diffraction grating contained in the diffractive optical element portion near the circumference of circle A exceeds the maximum allowable value. With such a glass portion, it is not possible to form the diffractive optical element portion with high precision.
[0112] As shown in Tables 2(1) to (3), before the diffractive optical element portion is formed, the BOW value is 10 to 30 μm, so the error in the period of the concave-convex structure of the diffraction grating can be suppressed to within ±5%.
[0113] A diffractive optical element portion was formed on the prepared glass portion by the following method to obtain a glass wafer. At this time, the warping of the glass portion during heating was sufficiently small. In addition, the BOW value of the glass wafer after the diffractive optical element portion was formed was also sufficiently small to suppress the error in the period of the uneven structure of the diffraction grating to within ±5%. In other words, it was confirmed that the diffractive optical element portion could be formed with high precision over the entire effective range of the glass portion. For the glass wafer obtained by forming the diffractive optical element portion, the period of the uneven structure of the diffraction grating and the height difference between the convex and concave portions of the diffraction grating were measured. The results are shown in Table 2.
[0114] [Formation with organic materials] A siloxane polymer was applied as an organic material to one of the main surfaces of the glass portion to form a coating film, and a mold having an inverted shape of the diffraction grating pattern of the diffractive optical element portion was transferred to the coating film. It was then heated and baked at about 125°C to obtain a glass wafer having a diffractive optical element portion of the size shown in Table 2 formed at a predetermined position on the main surface of the glass portion.
[0115] [Formation using inorganic materials] In a vacuum chamber, a titanium oxide film, a silicon nitride film, or a silicon carbide film was formed on one of the main surfaces of the glass part by sputtering. After the film was formed, it was removed from the vacuum chamber, and a photoresist liquid was uniformly applied to the main surface of the glass part on which the film was formed. Next, the glass part was heated to evaporate the solvent of the photoresist (pre-baking), and a photomask having a pattern corresponding to the periodic fine structure pattern of the diffractive optical element was used to transfer the pattern of the photomask to the photoresist on the surface of the glass part by ultraviolet irradiation (exposure). After exposure, the photoresist was selectively removed using a developer (development), and the glass part was heated to about 120 to 150 ° C. to thermally crosslink the photoresist (post-baking). Next, the film on the main surface of the glass part was selectively etched to form a diffractive optical element part. As a result, a glass wafer was obtained in which a diffractive optical element part having the size shown in Table 2 was formed at a predetermined position on the main surface of the glass part.
[0116] [Periodicity (pitch) of the uneven structure of the diffraction grating] The measurements were carried out using a scanning electron microscope (SEM).
[0117] [Height difference between convex and concave portions of the diffraction grating] The measurements were performed using an atomic force microscope (AFM).
[0118] Example 2 The glass wafer produced in Example 1 was cut and separated by dicing to produce a plurality of light guide plates. Table 2 shows the size and number of light guide plates obtained from one glass wafer.
[0119] Example 3 The light guide plate produced in Example 2 was incorporated into a head-mounted display. That is, the light guide plate produced in Example 2 was mounted on a frame together with a light source and an optical system to produce a glasses-type image display device. When this image display device was worn and an image was displayed, a high-quality image with a wide FOV could be displayed, providing a sufficient sense of immersion.
[0120] [Table 2(1)]
[0121] [Table 2(2)]
[0122] [Table 2(3)]
[0123] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of the present invention is defined by the claims, not the above description, and is intended to include all modifications within the meaning and scope of the claims.
[0124] For example, by adjusting the composition as described in the specification to the glass compositions exemplified above, an optical glass according to one aspect of the present invention can be produced. Furthermore, it is of course possible to arbitrarily combine two or more of the items described in the specification as examples or preferred ranges.
Claims
1. A glass portion having a thin plate shape and a diffractive optical element portion on a main surface thereof, The area of one of the main surfaces of the glass part is 1950 mm 2 That's all. The thickness of the glass portion is 3.0 mm or less, The Young's modulus of the glass portion is 100 GPa or more, The average linear expansion coefficient of the glass part at -30°C to 70°C is 80 x 10 -6 K -1 Below is the A glass wafer for manufacturing light guide plates.
2. 2. The glass wafer according to claim 1, wherein the diffractive optical element portion has a periodic uneven structure, the period of the uneven structure being 500 nm or less.
3. 2. The glass wafer according to claim 1, wherein the refractive index nd of the glass portion is 1.9 or more.
4. A glass portion and a diffractive optical element portion on a main surface thereof, The Young's modulus of the glass portion is 100 GPa or more, The average linear expansion coefficient of the glass part at -30°C to 70°C is 80 x 10 -6 K -1 Below is a light guide plate.
5. 5. The light guide plate according to claim 4, wherein the diffractive optical element portion has a periodic uneven structure, and the period of the uneven structure is 500 nm or less.
6. The light guide plate according to claim 4 , wherein the refractive index nd of the glass portion is 1.9 or more.
7. An image display device comprising the light guide plate according to claim 4.
8. The image display device according to claim 7 , which is of a glasses type.
Citation Information
Patent Citations