Glass substrate for light guide plate of transparent display with holding part

A glass wafer with a holding part and specific properties supports precise formation of diffractive optical elements, addressing flatness and positioning issues in light guide plates, enhancing the quality and reproducibility of image display devices.

JP2024144229APending Publication Date: 2024-10-11HOYA CORPORATION
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024042412
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-18
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The production of diffractive optical elements for light guide plates in smart glasses faces challenges such as reduced flatness and precision due to the handling of glass wafers during electron beam lithography, leading to inaccuracies in forming and positioning of these elements, which affect the quality and reproducibility of the light guide plates.

Method used

A glass wafer with a holding part on the outer edge, having a thin plate shape, specific Young's modulus, and polished surface, which maintains flatness and allows precise formation of diffractive optical elements through methods like electron beam lithography and photolithography, reducing warpage and damage during handling and processing.

Benefits of technology

The solution enables high-precision formation of diffractive optical elements, ensuring accurate positioning and reducing the occurrence of chips and cracks, thereby improving the quality and reproducibility of light guide plates for image display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144229000001_ABST
    Figure 2024144229000001_ABST
Patent Text Reader

Abstract

To provide a glass wafer capable of inhibiting deterioration of flatness during formation of a diffraction optical element; a light guide plate obtainable from the glass wafer; and an image display device including the light guide plate.SOLUTION: A glass wafer for manufacturing a light guide plate includes a holding part on an outer edge thereof and has a thin plate shape whose one main surface has an area of 1950 mm2 or more and whose thickness is 3.0 mm or less. The glass wafer has a Young's modulus of 100 GPa or more.SELECTED DRAWING: Figure 7
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a glass wafer, a light guide plate, and an image display device. [Background technology]

[0002] In recent years, with the advancement of AR (Augmented Reality), MR (Mixed Reality), and VR (Virtual Reality) technologies, display devices such as head-mounted displays have been developed as AR devices, MR devices, and VR devices. Among them, glasses-type wearable terminals called smart glasses, as disclosed in Patent Document 1, have attracted attention.

[0003] In smart glasses, light emitted from an image light source is guided to the front of the wearer's eyes by a light guide plate, which corresponds to a spectacle lens, and is displayed as an image.

[0004] Specifically, light emitted from the image light source is incident on the inside of the light guide plate by a diffractive optical element formed on the surface of the light guide plate. The light that has entered the inside of the light guide plate travels while repeatedly being totally reflected inside the light guide plate, and is emitted in the direction of the wearer's pupil by a diffractive optical element provided in front of the wearer's pupil.

[0005] Here, the light guide plate used in smart glasses etc. is manufactured using semiconductor circuit manufacturing equipment. In the mass production process of semiconductor circuits, a large number of integrated circuits are formed on the surface of a silicon wafer, and the silicon wafer on which the large number of integrated circuits are formed is cut and separated by dicing to manufacture a large number of semiconductor circuit elements.

[0006] The light guide plate can be manufactured using the same process as the mass production of semiconductor circuits. That is, a large number of diffractive optical elements are formed on the surface of a thin glass plate such as a glass wafer, and then the plate is cut and separated by dicing to manufacture a large number of light guide plates. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2016-139174 A Summary of the Invention [Problem to be solved by the invention]

[0008] In the production of semiconductor circuit elements, fine circuit patterns are formed by photolithography. In photolithography, a photomask equivalent to the master of the circuit pattern is used, and the mask pattern is transferred to a photoresist by exposure and development. After development, the film formed on the wafer is selectively removed by etching to form the circuit pattern. This method is suitable for mass production of semiconductor circuit elements, since once a photomask is produced, the mask pattern can be transferred onto many silicon wafers by repeatedly using the photomask. For mass production of light guide plates, it is also preferable to apply photolithography to the formation of diffractive optical elements.

[0009] On the other hand, it is not desirable in terms of cost, labor, etc. to prepare a photomask corresponding to the uneven pattern of the diffractive optical element every time the design of the diffractive optical element is changed or adjusted at the prototype stage of the light guide plate. Therefore, after forming a film of titanium oxide, silicon nitride, silicon carbide, etc. on the main surface of a glass wafer, an electron beam resist is applied, the resist is selectively exposed by electron beam lithography, and the diffractive optical element is fabricated through the steps of development and etching.

[0010] Here, when moving from prototype to mass production of light guide plates, it is required to reproduce the performance confirmed in the prototype with high accuracy in mass production. Therefore, it is desirable that the glass wafer used for the prototype of the light guide plate and the glass wafer used for mass production are the same in material, shape, size, etc. In the electron beam lithography at the prototype stage, the glass wafer with electron beam resist applied on one main surface is fixed in a vacuum chamber, and the electron beam resist on the glass wafer is irradiated and scanned with an electron beam to selectively expose the resist. In the series of processes, the glass wafer needs to be handled so as not to scratch both main surfaces. That is, in the vacuum chamber, the glass wafer cannot be fixed by suction on the back surface (one of the main surfaces) with a vacuum chuck or the like, and is fixed by holding the outer edge of the glass wafer. At this time, the glass wafer may be slightly distorted by its own weight, and the flatness of the main surface may decrease.

[0011] The formation of diffractive optical elements requires precision on the order of submicrons, and the inventors have found that a problem occurs in that diffractive optical elements cannot be formed with high precision on a glass wafer with reduced flatness of the main surface, even by electron beam lithography.

[0012] As described above, after the diffractive optical elements are formed, the glass wafer is cut and separated by dicing to manufacture a large number of light guide plates, but due to misalignment of the diffractive optical elements on the wafer, the positional accuracy of the diffractive optical elements in each light guide plate decreases. As a result, a shift occurs in the direction of light diffraction, and when assembling an image display device, a correction operation for this shift is required, and if the amount of misalignment is large, the quality of the displayed image decreases. In addition, due to the above problem, there is a problem that reproducibility of the prototype cannot be obtained in mass production.

[0013] Therefore, there is a demand for a glass wafer that allows diffractive optical elements to be formed with high precision in both prototype and mass production.

[0014] The present invention has been made in consideration of the above-described circumstances, and has an object to provide a glass wafer capable of suppressing a decrease in flatness during the formation of a diffractive optical element, a light guide plate obtained from the glass wafer, and an image display device including the light guide plate. [Means for solving the problem]

[0015] The gist of the present invention is as follows.

[0016] (1) A holder is provided on an outer edge of the holder. The area of ​​one main surface is 1950 mm 2 or more, and has a thin plate shape with a thickness of 3.0 mm or less, Young's modulus is 100 GPa or more. A glass wafer for manufacturing light guide plates.

[0017] (2) The glass wafer according to (1), having a diffractive optical element portion on a main surface thereof.

[0018] (3) The glass wafer according to (1), wherein the holding part has a polishing surface.

[0019] (4) A method for producing a light guide plate, comprising the step of separating the glass wafer described in (2) above. Effect of the Invention

[0020] According to the present invention, it is possible to provide a glass wafer capable of suppressing a decrease in flatness during the formation of a diffractive optical element, a light guide plate obtained from the glass wafer, and an image display device including the light guide plate. [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 is a schematic diagram of a glass wafer according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing the shape of a holding portion in a cross section of a glass wafer according to one embodiment of the present invention. [Diagram 3]FIG. 3 is a schematic diagram showing the shape of a holding portion in a cross section of a glass wafer according to one embodiment of the present invention. [Figure 4] FIG. 4 is a schematic diagram showing the shape of a holding portion in a cross section of a glass wafer according to one embodiment of the present invention. [Diagram 5] FIG. 5 is a diagram showing a schematic shape of a holding portion in a cross section of a glass wafer according to one embodiment of the present invention. [Figure 6] FIG. 6 is a schematic diagram showing the shape of a holding portion in a cross section of a glass wafer according to one embodiment of the present invention. [Figure 7] FIG. 7 is a schematic diagram showing the shape of a holding portion in a cross section of a glass wafer according to one embodiment of the present invention. [Figure 8] FIG. 8 is a schematic diagram showing the shape of a holding portion in a cross section of a glass wafer according to one embodiment of the present invention. [Figure 9] FIG. 9 is a schematic diagram showing the shape of a holding portion in a cross section of a glass wafer according to one embodiment of the present invention. [Figure 10] FIG. 10 is a schematic diagram showing the shape of a holding portion in a cross section of a glass wafer according to one embodiment of the present invention. [Figure 11] FIG. 11 is a diagram showing a schematic configuration of a head mounted display using a light guide plate according to one embodiment of the present invention. [Figure 12] FIG. 12 is a side view that illustrates a schematic configuration of a head mounted display that uses a light guide plate according to one embodiment of the present invention. [Figure 13] 13 is an SEM image of the cross section of the glass wafer obtained in the example, showing the shape of the holding part. The numerical values ​​in the figure are the angles between the holding part and the main surface. [Figure 14] FIG. 14 is a diagram showing a schematic diagram of a method for measuring the BOW. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] In this specification, unless otherwise specified, the refractive index refers to the refractive index nd at the d line of helium (wavelength 587.56 nm).

[0023] The Abbe number νd is used as a value representing the properties related to dispersion, and is expressed by the following formula: Here, nF is the refractive index at the F line (wavelength 486.13 nm) of blue hydrogen, and nC is the refractive index at the C line (656.27 nm) of red hydrogen. νd=(nd-1) / (nF-nC)

[0024] In the present invention, the glass composition is expressed on an oxide basis unless otherwise specified. Here, "glass composition on an oxide basis" refers to a glass composition obtained by converting the glass raw materials into oxides that are all decomposed during melting and exist in the glass. The total content of all glass components expressed on an oxide basis (excluding Sb (Sb2O3) and Ce (CeO2) added as fining agents) is 100 mass%. Each glass component is conventionally expressed as SiO2, TiO2, etc. The content and total content of glass components are on a mass basis unless otherwise specified, and "%" means "mass%".

[0025] The content of the glass component can be quantified by known methods, such as inductively coupled plasma atomic emission spectrometry (ICP-AES), inductively coupled plasma mass spectrometry (ICP-MS), etc. In the present invention, the content of a component being 0% means that the component is substantially not contained, and it is acceptable for the component to be contained at an unavoidable impurity level.

[0026] An embodiment of the present invention will be described below.

[0027] Glass Wafer The glass wafer according to this embodiment has a holding portion on its outer edge. The glass wafer according to this embodiment can be processed and used as a spectacle lens in smart glasses or the like. Therefore, the glass wafer is handled so as not to scratch both main surfaces (front and back) so as not to impair the function as a spectacle lens. For example, even in the manufacturing process of smart glasses, the glass wafer is fixed and processed with minimal contact with its main surfaces (front and back). By having the holding portion on the outer edge of the glass wafer, it becomes easier to hold the glass wafer by a robot arm or the like when transporting the glass wafer or forming a diffractive optical element on the glass wafer, and it is also possible to prevent the robot arm or the like from contacting the main surfaces (front and back) of the glass wafer. Furthermore, even when performing electron beam drawing in a vacuum chamber during prototyping, the glass wafer can be held without damaging the main surface.

[0028] 1 is a schematic diagram of a glass wafer 10 according to the present embodiment, and the glass wafer 10 has a main surface 11 and a holding portion 12 indicated by hatched portions. Note that the glass wafer according to the present embodiment may have any shape as long as it has a thin plate shape, and is not limited to the disk shape shown in FIG.

[0029] The shape of the holding part 12 is not particularly limited, but examples thereof include shapes as shown in Figures 2 to 10. Figures 2 to 10 are diagrams that typically show the shape of the holding part 12 in a cross section of the glass wafer 10 according to this embodiment. Figures 2 to 10 will be described below.

[0030] As shown in FIG. 2, the holding portion 12 may be a plane perpendicular to the main surface 11 in the cross section of the glass wafer 10. As shown in FIG. 3 and FIG. 4, the holding portion 12 may have a shape with one corner chamfered. As shown in FIG. 5 to FIG. 7 and FIG. 10, the holding portion 12 may have a shape with two corners chamfered. As shown in FIG. 3, FIG. 7, FIG. 9 and FIG. 10, the holding portion 12 may be chamfered to an angle θ, as shown in FIG. 4 and FIG. 5, the holding portion 12 may have a chamfered portion with an angle θ and a chamfered portion with a rounded corner, as shown in FIG. 6. The angle θ is not particularly limited, but may be about 45 degrees. The holding portion 12 has a chamfered shape, which can reduce chipping and cracking starting from the outer edge of the glass wafer.

[0031] When the glass wafer 10 has a holding portion 12 as shown in Fig. 7, the lengths of C and D in the holding portion 12 can be adjusted so that the ratio of the length of C to the length of D [C / D] is 0.2 to 0.45. By setting the ratio of the length of C to the length of D [C / D] within the above range, it is possible to reduce chipping or cracking of the glass wafer, and it becomes easier to hold the glass wafer by a robot arm or the like in the manufacturing process. In Fig. 7, the sum of twice the length of C and the length of D [C x 2 + D] is the thickness of the glass wafer 10.

[0032] The holding portion 12 may have a rounded shape. For example, as shown in Fig. 8, the holding portion 12 may have a semicircular shape with a radius R in the cross section of the glass wafer 10. In this case, the radius R is 1 / 2 the thickness of the glass wafer 10.

[0033] The retaining portion 12 may have a shape having a rounded portion. For example, the retaining portion 12 may have a rounded shape with one main surface side linearly chamfered as shown in Fig. 9, or may have a shape with two main surface sides linearly chamfered and a rounded center portion as shown in Fig. 10.

[0034] In the glass wafer according to this embodiment, the holding part preferably has a polished surface. Fine scratches and the like are removed from the polished surface. By having the holding part have a polished surface, when a robot arm or the like holds the glass wafer, it is possible to reduce the occurrence of chipping or cracking originating from the outer edge of the glass wafer. The entire surface of the holding part may be a polished surface, or a part of the holding part may be a polished surface. The larger the area of ​​the polished surface of the holding part, the more it is possible to reduce the occurrence of chipping or cracking originating from the outer edge of the glass wafer, and the greater the strength of the glass wafer.

[0035] (shape) The glass wafer according to the present embodiment has a thin plate shape. Preferably, the glass wafer has a disk shape. The glass wafer may also have a thin plate shape in which the main surface has a polygonal, square or rectangular shape. When the glass wafer has such a thin plate shape, a light guide plate can be manufactured from the glass wafer using normal semiconductor circuit manufacturing equipment.

[0036] (area) In the glass wafer according to this embodiment, the area of ​​one main surface is 1950 mm 2 More than 4400mm, preferably 4400mm 2 More preferably, 7850 mm 2 More preferably, 17670 mm 2 More preferably, 70690 mm 2 That is all. By increasing the area of ​​the main surface, the number of light guide plates that can be obtained per unit area can be increased. There is no particular upper limit to the area of ​​the main surface, but from the viewpoint of using ordinary semiconductor circuit manufacturing equipment, it is usually 159050 mm 2 It is.

[0037] (Diameter of inscribed circle) In the glass wafer according to this embodiment, the size can also be evaluated by the size of a circle virtually inscribed in the shape of the main surface. That is, the diameter of the circle virtually inscribed in the shape of the main surface is preferably 50 mm or more, more preferably 75 mm or more, even more preferably 100 mm or more, and even more preferably 150 mm or more. By increasing the diameter of the inscribed circle, the number of light guide plates obtained per unit area can be increased. The upper limit of the diameter of the inscribed circle is not particularly limited, but is usually 450 mm from the viewpoint of using normal semiconductor circuit manufacturing equipment.

[0038] (diameter) When the glass wafer according to the present embodiment is disk-shaped, its diameter is preferably 50 mm or more, more preferably 75 mm or more, even more preferably 100 mm or more, and even more preferably 150 mm or more. By increasing the diameter, the number of light guide plates obtained per unit area can be increased. The upper limit of the diameter is not particularly limited, but is usually 450 mm from the viewpoint of using ordinary semiconductor circuit manufacturing equipment.

[0039] (Thickness) In the glass wafer according to this embodiment, the thickness is 3.0 mm or less, preferably 1.0 mm or less, more preferably 0.8 mm or less, and even more preferably 0.5 mm or less. The lower limit of the thickness is not particularly limited, but is usually 0.2 mm, preferably 0.25 mm. By setting the thickness within the above range, a light guide plate that can be used as a lens for smart glasses can be manufactured, and the light guide plate can be manufactured from the glass wafer using ordinary semiconductor circuit manufacturing equipment.

[0040] (Young's Modulus) In the glass wafer according to this embodiment, the Young's modulus is 100 GPa or more, preferably 110 GPa or more, more preferably 120 GPa or more. The upper limit of the Young's modulus is not particularly limited, but is usually 150 GPa, preferably 140 GPa. By setting the Young's modulus within the above range, when the outer edge of the glass wafer is held and fixed, the distortion due to its own weight can be reduced, and the decrease in flatness on the main surface can be suppressed.

[0041] Here, as described below, a diffractive optical element portion can be formed on the main surface of the glass wafer. Submicron precision is required for the formation of the diffractive optical element portion. However, when forming the diffractive optical element portion on the surface of the glass wafer, the glass wafer may be heated to 100°C or higher. Conventionally, this heating causes warping of the glass wafer, which causes a problem that the diffractive optical element portion cannot be formed with high precision. Specifically, this is as follows.

[0042] The diffractive optical element part is made of inorganic materials such as titanium oxide, silicon nitride, and silicon carbide, or organic materials such as transparent resin. When an inorganic material is used, a film of the inorganic material is first formed on the surface of a glass wafer. In the prototype stage, an electron beam resist is applied onto the inorganic material film, and the wafer is heated on a hot plate to perform pre-baking to evaporate the solvent of the photoresist. Next, the wafer is placed in a vacuum chamber, the chamber is depressurized, and a pattern of the diffractive optical element is drawn on the resist by electron beam irradiation. After electron beam drawing, the wafer is removed from the vacuum chamber, and in order to thermally crosslink the resist, the wafer is placed on a hot plate and heated (post-baked) to about 120 to 150°C. Next, the resist is developed, and then fine irregularities are formed in the film by etching to form the diffractive optical element part. Since the glass wafer cannot be fixed by suction in the vacuum chamber, it is held by a holder on the outer edge of the wafer. However, since the Young's modulus of the glass wafer is large, electron beam drawing can be performed while maintaining flatness. It is preferable to evaluate the performance of the prototype light guide plate and move to mass production.

[0043] In mass production, the pattern of the diffractive optical element is formed by photolithography instead of electron beam drawing. For example, the inorganic material film is formed on the main surface of a glass wafer. Next, a photoresist is applied to the surface on which the film is formed, and the wafer is heated on a hot plate and pre-baked to evaporate the solvent of the photoresist. Next, the pattern of the photomask is transferred to the photoresist by ultraviolet light exposure. After exposure, the wafer is placed on a hot plate and heated (post-baked) to about 120 to 150°C in order to thermally crosslink the photoresist. Next, the photoresist is developed, and then fine irregularities are formed in the film by etching to form a diffractive optical element portion. When an organic material is used, a resin such as a transparent ultraviolet curable resin is applied to the main surface of the glass wafer to form a coating film, and the fine irregularity pattern of the diffractive optical element portion is pressed with a mold having an inverted shape to transfer the pattern to the coating film. Then, the wafer is placed on a hot plate and heated to about 125°C to bake it, forming the diffractive optical element portion.

[0044] Regardless of whether the material is inorganic or organic, warping occurs when a glass wafer is heated on a hot plate. Glass has a relatively low thermal conductivity, and when heated on a hot plate, a large temperature difference occurs between the main surface facing the hot plate, i.e., the main surface facing downward, and the main surface on the opposite side, i.e., the main surface facing upward. The amount of expansion of the high-temperature main surface facing downward is greater than the amount of expansion of the low-temperature main surface facing upward, so the glass wafer warps into a downward convex shape. The peripheral portion of the warped glass wafer is separated from the hot plate, so the central portion of the main surface is hotter than the peripheral portion. In this state, thermal crosslinking of the photoresist and baking of the organic material are performed, so that even after heating is completed, the fine pattern of the diffractive optical element portion is misaligned. A similar phenomenon also occurs in the preforming and post-baking of electron beam resist.

[0045] By setting the Young's modulus of the glass wafer within the above range, the diffractive optical element portion can be formed with high accuracy without using pattern formation methods such as electron beam drawing and photolithography. In addition, when the diffractive optical element portion is formed on the main surface of the glass wafer by heating it as described above, the warp of the glass wafer can be reduced, and the diffractive optical element portion can be formed with high accuracy. Furthermore, by setting the Young's modulus within the above range, damage during transportation of the glass wafer can be reduced. In addition, damage during insertion and removal of the glass wafer from a wafer cassette (e.g., a multiple wafer vertical case) and damage during processing can also be reduced.

[0046] Young's modulus is measured and calculated in accordance with JIS R 1602-1995. Specifically, a glass sample made of the same material as the glass wafer, measuring 20 mm in length, 20 mm in width, and 100 mm in height, is fully annealed and placed in a temperature-controlled chamber, and the longitudinal wave velocity (Vl) and shear wave velocity (Vs) of 5 MHz ultrasound are measured, and Young's modulus (E) and rigidity modulus (G) are calculated using the following formulas. E=(4G 2 -3G×Vl 2 ×ρ) / (G-Vl 2 ×ρ) G=Vs 2 ×ρ Here, ρ is the density of the glass sample, and the value of the specific gravity can be used. The density (specific gravity) of the glass sample at room temperature and the density (specific gravity) of the glass wafer at room temperature are assumed to be the same. In other words, the density at room temperature is calculated by multiplying the specific gravity by the unit g / cm. 3 It is expressed by adding .

[0047] (Average linear expansion coefficient α at -30℃ to 70℃ n ) In the glass wafer according to this embodiment, the average linear expansion coefficient α n is preferably 80 x 10 -6 K -1 More preferably, it is 75×10 or less. -6 K -1 The average linear expansion coefficient α at -30℃ to 70℃ is as follows. n The lower limit is not particularly limited, but is usually 60×10 -6K -1 The average linear expansion coefficient α at -30℃ to 70℃ n By setting the thickness within the above range, even when the glass wafer is heated from one side on a hot plate during the formation of the diffractive optical element portion, the difference in expansion between the two main surfaces of the glass wafer can be reduced, and warping can be reduced.

[0048] Average linear expansion coefficient α at -30℃ to 70℃ n is measured using an interferometric dilatometer and calculated according to the following formula: α n =dL n / (L×dT n ) Here, dT n is the temperature difference from -30 to 70°C (K), L is the initial length of the glass sample (mm), dL n is the change in sample length (mm) in the temperature range of -30 to 70°C.

[0049] (Refractive index nd) In the glass wafer according to this embodiment, the refractive index nd is preferably 1.9 or more, more preferably 1.95 or more, and even more preferably 2.00 or more. The upper limit of the refractive index nd is not particularly limited, but is usually 2.2. From the viewpoint that the light incident on the glass wafer travels inside the glass wafer while repeating total reflection and emerges at a sufficient viewing angle, it is preferable that the refractive index of the glass wafer is within the above range.

[0050] (Abbe number νd) In the glass wafer according to this embodiment, the upper limit of the Abbe number vd can be 40, or can be 35 or 30. The lower limit of the Abbe number vd is not particularly limited, but is usually 15.

[0051] (glass transition temperature Tg) In the glass wafer according to this embodiment, the glass transition temperature Tg is preferably 600° C. or higher, more preferably 630° C. or higher, and further preferably 650° C. or higher. The upper limit of the glass transition temperature Tg is not particularly limited, but is usually 780° C., and preferably 760° C. When the glass wafer is heated to form a diffractive optical element portion on its main surface, it is preferable to set the glass transition temperature Tg within the above range from the viewpoint of reducing warpage of the glass wafer and from the viewpoint of maintaining good thermal stability of the glass wafer while maintaining a desired refractive index.

[0052] (internal transmittance) The glass wafer according to this embodiment has light transmittance for visible light. The light transmittance can be evaluated by the internal transmittance at wavelengths of 420 nm to 800 nm for a glass sample having a thickness of 10.0 mm±0.1 mm. The internal transmittance is the transmittance excluding the surface reflection loss on the entrance side and exit side of the glass sample. The internal transmittance τ for a thickness of 10.0±0.1 mm at a specific wavelength can be calculated by measuring the transmittances (external transmittances) T1 and T2 including the surface reflection loss of two glass samples made of the same type of glass and having different thicknesses d1 and d2, respectively, and using the following formula. logτ=-[(logT1-logT2)×10] / Δd Here, d2>d1, Δd=d2-d1, and log is the common logarithm.

[0053] The internal transmittance of a glass sample having a thickness of 10.0 mm±0.1 mm and made of the same material as the glass wafer, i.e., the internal transmittance of the glass wafer converted to a thickness of 10.0 mm±0.1 mm, is preferably 78% or more over the wavelength range of 420 nm to 800 nm, more preferably 83% or more, and even more preferably 90% or more.

[0054] The minimum value of the internal transmittance in the wavelength range of 420 nm to 800 nm is preferably the internal transmittance at the wavelength of 420 nm, which is the short wavelength end of the wavelength range. That is, the internal transmittance of a glass sample having a thickness of 10.0 mm±0.1 mm and made of the same material as the glass wafer at a wavelength of 420 nm (the internal transmittance of the glass wafer converted to a thickness of 10.0 mm±0.1 mm) is preferably 78% or more, more preferably 83% or more, and even more preferably 90% or more.

[0055] (specific gravity) In the glass wafer according to the present embodiment, the specific gravity is preferably 5.5 or less, more preferably 5.4 or less, and even more preferably 5.3 or less. The lower limit of the specific gravity is not particularly limited, but is usually 4.3. When used as a spectacle lens for smart glasses, it is preferable to set the specific gravity of the glass wafer within the above range in order to reduce discomfort caused by the weight of the lens when worn.

[0056] (Specific elastic modulus) In the glass wafer according to this embodiment, the specific elastic modulus is preferably 24.0 MN / Kg or more, more preferably 24.5 MN / Kg or more, and even more preferably 25.0 MN / Kg or more. The upper limit of the specific elastic modulus is not particularly limited, but is approximately 30 MN / Kg as a guide. From the viewpoint of reducing warpage of the glass wafer when the glass wafer is heated to form a diffractive optical element portion on its main surface, it is preferable that the specific elastic modulus of the glass wafer is within the above range.

[0057] (material) The material of the glass wafer according to the present embodiment is not particularly limited as long as it satisfies the above Young's modulus. For example, the material of the glass wafer may be optical glass. The glass wafer is preferably made of optical glass.

[0058] Specifically, the glass wafer material can be exemplified by glass having a B-La system composition. Therefore, non-limiting examples of B-La system glass compositions are shown below. Note that the glass wafer material is not limited to the glass having the B-La system composition shown below, and any material can be used as long as it can provide a glass wafer that can suppress the decrease in flatness during the formation of a diffractive optical element.

[0059] The glass wafer according to this embodiment preferably has the following glass composition (expressed in mass %). The total content of B2O3 and SiO2 [B2O3+SiO2] is preferably 5 to 25%. The total content of La2O3, Gd2O3, Y2O3, and Yb2O3 [La2O3+Gd2O3+Y2O3+Yb2O3] is preferably 25 to 68%. The total content of TiO2, Nb2O5, Ta2O5, and WO3 [TiO2+Nb2O5+Ta2O5+WO3] is preferably 5 to 40%. The total content of MgO, CaO, SrO and BaO [MgO+CaO+SrO+BaO] is preferably 0 to 20%. The total content of Li2O, Na2O and K2O [Li2O+Na2O+K2O] is preferably 0 to 5%. The content of ZrO2 is preferably 0 to 12%. The ZnO content is preferably 0 to 10%. The content of B2O3 is preferably 3 to 20%. The SiO2 content is preferably 0 to 15%. The content of La2O3 is preferably 25 to 60%. The content of Gd2O3 is preferably 0 to 30%. The content of Y2O3 is preferably 0 to 16%. The content of Yb2O3 is preferably 0 to 5%. The TiO content is preferably 0 to 28%. The content of Nb2O5 is preferably 0 to 15%. The content of Ta2O5 is preferably 0 to 10%. The content of WO3 is preferably 0 to 6%. The content of MgO is preferably 0 to 5%. The CaO content is preferably 0 to 5%. The content of SrO is preferably 0 to 5%. The content of BaO is preferably 0 to 20%. The content of Li2O is preferably 0 to 5%. The Na2O content is preferably 0 to 5%. The content of K2O is preferably 0 to 5%. The content of Sb2O3 is preferably 0 to 1%. The content of Lu2O3 is preferably 0 to 1%. The content of Sc2O3 is preferably 0 to 1%. The content of Ga2O3 is preferably 0 to 1%. The GeO2 content is preferably 0 to 1%.

[0060] In the glass wafer according to the present embodiment, from the viewpoint of increasing the Young's modulus, it is preferable that the total content [La2O3+Gd2O3+Y2O3+Yb2O3], the content of ZrO2, and the content of TiO are within the above ranges. Also, from the viewpoint of suppressing an increase in the average linear expansion coefficient, it is preferable that the total content [MgO+CaO+SrO+BaO] and the total content [Li2O+Na2O+K2O] are within the above ranges.

[0061] It is preferable that the glass wafer does not contain Pb, Te, Cd, Th, Tl, V, Cr, Ni, Fe, U, Nd, Cu, Er, Eu, etc.

[0062] <Diffractive optical element> The glass wafer according to the present embodiment may have a diffractive optical element portion on the main surface. The diffractive optical element portion is not particularly limited as long as it includes a portion that functions as a diffraction grating. For example, the diffractive optical element portion includes a diffraction grating that functions to diffract light (image) incident from an image light source into the glass wafer, i.e., a diffractive optical element for light incidence, or a diffraction grating that functions to diffract light traveling through the glass wafer by total reflection and emit it to the outside, i.e., a diffractive optical element for light emission. In this case, the glass wafer is cut by dicing, and a diffractive optical element for incidence and a diffractive optical element for emission are formed in each region that will become a light guide plate after separation. Since the light beam before entering the light guide plate is thin, the area of ​​the diffractive optical element for incidence may be relatively small. On the other hand, the diffractive optical element for emission has a relatively large area because it displays an image in an enlarged manner in front of the pupil of the person wearing the image display device. The larger the viewing angle, the larger the area of ​​the diffractive optical element for emission.

[0063] The shape of the diffraction grating in the diffractive optical element part is not particularly limited. Therefore, the diffraction grating may be a diffraction grating having a grooved shape, or may be a so-called holographic diffraction grating using holography. For example, the diffractive optical element part may have a periodic uneven structure as a diffraction grating. In this case, from the viewpoint that the light (image) incident from the image light source travels while repeating total reflection inside the glass wafer, and from the viewpoint that the light is emitted at a sufficient viewing angle, the period of the uneven structure is preferably 500 nm or less, more preferably 400 nm or less, and may be 280 nm or less.

[0064] The material of the diffractive optical element is not particularly limited, and may be an inorganic material or an organic material. From the viewpoint of maintaining the light transmittance as a spectacle lens of smart glasses, a transparent material is preferable. Examples of inorganic materials include, but are not limited to, titanium oxide, silicon nitride, and silicon carbide. In addition, in films of titanium oxide, silicon nitride, silicon carbide, etc., the molar ratio of elements such as Ti, Si, O, N, and C is not necessarily an integer ratio (non-stoichiometric). Therefore, in this specification, the inorganic material of the diffractive optical element will be described as titanium oxide, silicon nitride, silicon carbide, etc., including those that are in a stoichiometric ratio and those that are not in a stoichiometric ratio. Examples of organic materials include transparent resins, and may be, for example, ultraviolet-curable resins.

[0065] light guide plate A large number of light guide plates can be manufactured by cutting and separating the above-mentioned glass wafer having the diffractive optical element portion on the main surface by dicing. That is, the light guide plate according to this embodiment is obtained by cutting and separating the above-mentioned glass wafer. Therefore, the light guide plate according to this embodiment has a glass portion corresponding to the cut and separated glass wafer and a diffractive optical element portion on its main surface.

[0066] The light guide plate according to this embodiment inherits the properties of the glass wafer as is, and the properties of the glass wafer and the diffractive optical element portion can be directly used as the properties of the glass portion and the diffractive optical element portion in the light guide plate.

[0067] That is, in the light guide plate according to this embodiment, the thickness of the glass portion, Young's modulus, and average linear expansion coefficient α n , refractive index nd, Abbe number νd, glass transition temperature Tg, internal transmittance, specific gravity, specific elastic modulus, and material, as well as the type, shape, diffraction grating period, and material of the diffractive optical element part, can be the same as those of the glass wafer and the diffractive optical element part.

[0068] Image display device The image display device according to this embodiment includes the above-mentioned light guide plate.

[0069] Hereinafter, a light guide plate according to one embodiment of the present invention and an image display device using the same will be described in detail with reference to the drawings. In the drawings, the same or corresponding parts are designated by the same reference characters and their description will not be repeated.

[0070] FIG. 11 is a diagram showing a configuration example of a head mounted display 1 (hereinafter, abbreviated as "HMD1") using a light guide plate 10 according to one embodiment of the present invention, in which FIG. 11(a) is a front perspective view of the HMD1, and FIG. 11(b) is a rear perspective view of the HMD1. As shown in FIG. 11(a) and FIG. 11(b), a spectacle lens 3 is attached to the front part of a spectacle-type frame 2 worn on the head of a user. A backlight 4 for illuminating an image is attached to a mounting part 2a of the spectacle-type frame 2. A signal processing device 5 for projecting an image and a speaker 6 for reproducing sound are provided on the temple part of the spectacle-type frame 2. Flexible printed circuits (FPCs) 7 constituting wiring drawn from the circuit of the signal processing device 5 are wired along the spectacle-type frame 2. A display element unit (e.g., a liquid crystal display element) 20 is wired to the center position of both eyes of the user by the FPC 7, and is held so that the approximate center of the display element unit 20 is located on the optical axis of the backlight 4. The imager unit 20 is fixed relative to the light guide plate 10 so as to be located approximately at the center of the light guide plate 10. Holographic optical elements (HOEs) 32R and 32L (first diffractive optical elements) are formed on the first surface 10a of the light guide plate 10 at positions in front of the user's eyes. HOEs 52R and 52L are formed on the second surface 10b of the light guide plate 10 at positions facing the imager unit 20 across the light guide plate 10.

[0071] FIG. 12 is a side view showing a schematic configuration of an HMD 1 according to an embodiment of the present invention. In FIG. 12, in order to clarify the drawing, only the main parts of the image display device are shown, and the eyeglass-type frame 2 and the like are omitted. As shown in FIG. 12, the HMD 1 has a bilaterally symmetrical structure with respect to a center line X connecting the center of the image display element 24 and the light guide plate 10. Furthermore, the light of each wavelength incident on the light guide plate 10 from the image display element 24 is divided into two and guided to the right eye and the left eye of the user, as described later. The optical paths of the light of each wavelength guided to each eye are also approximately bilaterally symmetrical with respect to the center line X.

[0072] As shown in FIG. 12, the backlight 4 has a laser light source 21, a diffusion optical system 22, and a microlens array 23. The display element unit 20 is an image generating unit having an image display element 24, and is driven, for example, by a field sequential method. The laser light source 21 has laser light sources corresponding to the wavelengths of R (wavelength 633 nm), G (wavelength 546 nm), and B (wavelength 436 nm), and sequentially irradiates light of each wavelength at high speed. The light of each wavelength is incident on the diffusion optical system 22 and the microlens array 23, and is converted into a uniform, highly directional parallel light beam without unevenness in the amount of light, and is incident perpendicularly on the display panel surface of the image display element 24.

[0073] The image display element 24 is, for example, a transmissive liquid crystal (LCDT-LCOS) panel driven by a field sequential method. The image display element 24 modulates the light of each wavelength according to an image signal generated by an image engine (not shown) of the signal processing device 5. The light of each wavelength modulated by the pixels in the effective area of ​​the image display element 24 is incident on the light guide plate 10 with a predetermined light beam cross section (approximately the same shape as the effective area). The image display element 24 can also be replaced with other types of display elements, such as a DMD (Digital Mirror Device), a reflective liquid crystal (LCOS) panel, a MEMS (Micro Electro Mechanical Systems), an organic EL (Electro-Luminescence), or an inorganic EL.

[0074] The image generating unit of the image display element 20 is not limited to a field sequential type image display element, but may be a simultaneous type image display element (a display element having a predetermined arrangement of RGB color filters in front of the emission surface). In this case, for example, a white light source is used as the light source.

[0075] As shown in Fig. 12, the light of each wavelength modulated by the image display element 24 is sequentially incident on the inside of the light guide plate 10 from the first surface 10a. HOEs 52R and 52L (second diffractive optical elements) are formed on the second surface 10b of the light guide plate 10. The HOEs 52R and 52L are, for example, reflective volume phase HOEs having a rectangular shape, and are configured by laminating three photopolymer sheets on which interference fringes corresponding to the light of each wavelength of R, G, and B are recorded. In other words, the HOEs 52R and 52L are configured to have a wavelength selection function that diffracts the light of each wavelength of R, G, and B and transmits the light of the other wavelengths.

[0076] The HOEs 32R and 32L are also reflective volume phase type HOEs and have the same layer structure as the HOEs 52R and 52L. The HOEs 32R and 32L and the HOEs 52R and 52L may have, for example, approximately the same pitch of the interference fringe patterns.

[0077] The HOEs 52R and 52L are stacked with their centers aligned and with their interference fringe patterns inverted by 180 degrees. They are formed on the second surface 10b of the light guide plate 10 so that their centers aligned with the center line X when stacked. Light of each wavelength modulated by the image display element 24 is sequentially incident on the HOEs 52R and 52L via the light guide plate 10.

[0078] The HOEs 52R and 52L each diffract the light of each wavelength incident sequentially at a predetermined angle to guide it to the right eye and the left eye. The light of each wavelength diffracted by the HOEs 52R and 52L is repeatedly totally reflected at the interface between the light guide plate 10 and the air, propagates inside the light guide plate 10, and is incident on the HOEs 32R and 32L. Here, the HOEs 52R and 52L give the same diffraction angle to the light of each wavelength. Therefore, all the light of wavelengths that are incident at approximately the same position on the light guide plate 10 (or, in other words, emitted from approximately the same coordinates within the effective area of ​​the image display element 24) propagate through approximately the same optical path within the light guide plate 10 and are incident on approximately the same position on the HOEs 32R and 32L. From another perspective, the HOEs 52R and 52L diffract the light of each wavelength of RGB so that the pixel positional relationship within the effective area of ​​the image displayed in the effective area of ​​the image display element 24 is faithfully reproduced on the HOEs 32R and 32L.

[0079] Thus, in one aspect of the present invention, HOEs 52R and 52L each diffract light of all wavelengths emitted from approximately the same coordinates within the effective area of ​​image display element 24 so that it is incident on approximately the same position on HOEs 32R and 32L. Alternatively, HOEs 52R and 52L may be configured to diffract light of all wavelengths that originally constitute the same pixel but are relatively shifted within the effective area of ​​image display element 24 so that it is incident on approximately the same position on HOEs 32R and 32L.

[0080] The light of each wavelength incident on the HOEs 32R and 32L is diffracted by the HOEs 32R and 32L and sequentially emitted from the second surface 10b of the light guide plate 10 in a substantially perpendicular direction to the outside. The light of each wavelength emitted as substantially parallel light in this manner is imaged on the right and left retina of the user as a virtual image I of the image generated by the image display element 24. In addition, a condenser effect may be given to the HOEs 32R and 32L so that the user can observe the virtual image I of the enlarged image. That is, the light incident on the peripheral area of ​​the HOEs 32R and 32L may be emitted at an angle closer to the center of the pupil and imaged on the user's retina. Alternatively, in order to allow the user to observe the virtual image I of the enlarged image, the HOEs 52R and 52L may diffract the light of each wavelength of RGB so that the pixel positional relationship on the HOEs 32R and 32L forms an enlarged similar shape to the pixel positional relationship within the effective area of ​​the image displayed in the effective area of ​​the image display element 24.

[0081] Since the air-equivalent optical path length of light traveling inside the light guide plate 10 becomes shorter as the refractive index increases, the use of the light guide plate according to this embodiment having a glass wafer with a high refractive index makes it possible to increase the apparent viewing angle relative to the width of the image display element 24. Furthermore, in this embodiment, although the refractive index of the glass wafer is high, the specific gravity is kept low, making it possible to provide a light guide plate that is lightweight yet provides the above-mentioned effects.

[0082] In the above, a head mounted display has been described as an example of an image display device, but the image display device according to the present embodiment may be a pair of eyeglass-type smart glasses. Alternatively, the image display device may be another image display device. Alternatively, the diffractive optical element may be a diffraction grating having a fine concave-convex periodic structure instead of a holographic diffraction grating. In the above example, a light guide plate for both eyes has been described, but it is also possible to use separate light guide plates for displaying images to the left eye and the right eye.

[0083] <Glass Wafer Manufacturing> The glass wafer according to this embodiment can be manufactured, for example, by using a glass molded body. The manufacture of a glass molded body made of optical glass will be exemplarily described below.

[0084] Optical glass may be manufactured by blending glass raw materials to obtain a predetermined composition, and using the blended glass raw materials according to a known glass manufacturing method. For example, a plurality of compounds may be blended and thoroughly mixed to obtain batch raw materials, which are then placed in a quartz crucible or platinum crucible to be roughly melted (rough melt). The molten material obtained by rough melting is quenched and crushed to produce cullet. The cullet is then placed in a platinum crucible, heated, and remelted (remelt) to obtain molten glass, which is then clarified and homogenized, molded, and slowly cooled to obtain a glass molded body made of optical glass. Known methods may be used to mold and slowly cool the molten glass.

[0085] In addition, as long as a desired glass component can be introduced into the glass in a desired content, the compound used when preparing the batch raw materials is not particularly limited. Examples of such compounds include oxides, carbonates, nitrates, hydroxides, fluorides, etc.

[0086] The glass wafer can be produced by a method including a step of processing a glass molded body into a thin plate shape having a holding portion on the outer edge. Examples of the processing include cutting, cutting, rough grinding, fine grinding, polishing, etc.

[0087] Alternatively, the glass wafer can be produced, for example, by the following method.

[0088] Glass raw materials are melted to a predetermined composition by a known method to produce molten glass, and this molten glass is poured into a mold and formed into a plate shape to produce a glass material made of optical glass. The obtained glass material is appropriately cut, ground, and polished to produce cut pieces of a size and shape suitable for press molding. The cut pieces are heated and softened, and press molded (reheat press) by a known method to produce a glass blank that is similar in shape to the glass wafer. The glass blank is annealed, and ground and polished by a known method to process it into a thin plate shape with a holding portion on the outer edge, to produce a glass wafer.

[0089] A diffractive optical element portion can be formed on the main surface of the glass wafer. The method for forming the diffractive optical element portion is not particularly limited. The diffractive optical element portion can be formed by electron beam lithography. When forming the diffractive optical element portion by electron beam lithography, a known method may be used. In addition, the following examples are given of the case where the diffractive optical element portion is formed from an organic material and the case where it is formed from an inorganic material. When the diffractive optical element portion is a holographic diffraction grating, it may be formed by a known method.

[0090] When using an organic material, the organic material is applied to one of the main surfaces of the glass wafer to form a coating film, and a mold having an inverted shape of the diffraction grating pattern of the diffractive optical element part is transferred to the coating film. The glass wafer is then heated and baked at about 125°C to produce a glass wafer having a diffractive optical element part formed at a predetermined position on the main surface. The organic material is not particularly limited, but may be a transparent resin, such as an ultraviolet-curable resin.

[0091] When using an inorganic material, an inorganic material film is formed on one of the main surfaces of a glass wafer in a vacuum chamber by sputtering, deposition, or chemical vapor deposition (CVD). After the film is formed, the wafer is removed from the vacuum chamber, photoresist is applied, pre-baked, the resist is exposed to ultraviolet light to transfer the pattern of the photomask, post-baked (at about 120 to 150°C), developed, and then etched to form a diffraction grating pattern. This allows the manufacture of a glass wafer having a diffractive optical element portion formed at a predetermined position on the main surface. Examples of inorganic materials include, but are not limited to, titanium oxide, silicon nitride, and silicon carbide.

[0092] <Manufacture of light guide plates> The method for manufacturing the light guide plate is not particularly limited, and the light guide plate can be manufactured by a known method. For example, a glass wafer on which a diffractive optical element portion is formed as described above is cut and separated by dicing to manufacture a plurality of light guide plates. When cutting and separating the glass wafer, an anti-reflection film may be formed on the main surface of the wafer, a protective sheet may be attached thereon with an ultraviolet peelable adhesive to protect the main surface of the wafer, and the protective sheet may be peeled off by irradiating ultraviolet light after cutting and separating.

[0093] <Manufacture of image display devices> The manufacturing method of the image display device is not particularly limited, and the image display device can be manufactured by a known method. For example, in the case of a glasses-type image display device, the light guide plate is incorporated into a head-mounted display 1 shown in Fig. 12, that is, the light guide plate is mounted on a frame together with a light source and an optical system, and the image display device can be manufactured. EXAMPLES

[0094] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the embodiments shown in the examples.

[0095] Example 1 Glass wafers made of glass A, B, or C shown in Table 1 were prepared by the following procedure, and various evaluations were carried out.

[0096] [Preparation of glass samples] Compound raw materials corresponding to the constituent components of the glass wafer, i.e., raw materials such as oxides and carbonates, were weighed and thoroughly mixed to prepare a blended raw material. The blended raw material was placed in a platinum crucible, heated to 1000 to 1350°C in an air atmosphere or a water vapor atmosphere to melt, and homogenized and clarified by stirring to obtain a molten glass. The molten glass was cast into a mold to be molded, and slowly cooled to obtain a glass sample. The glass melted in a water vapor atmosphere was heat-treated in air for a long period of time to increase the transmittance in the visible range.

[0097] [Optical property measurements] The obtained glass samples were measured for refractive index nd, Abbe number νd, glass transition temperature Tg, Young's modulus, and average linear expansion coefficient α by the following methods. n The specific gravity, specific elastic modulus, and internal transmittance at wavelengths of 420 nm and 800 nm (converted value at a thickness of 10.0 mm) were measured. The results are shown in Table 1.

[0098] [Refractive index nd and Abbe number νd] The refractive indices nd, ng, nF, and nC were measured according to the refractive index measurement method of JIS B 7071-1, and the Abbe number vd was calculated according to the following formula. νd=(nd-1) / (nF-nC)

[0099] [Glass transition temperature Tg] The glass transition temperature Tg was measured using a differential scanning calorimeter (DSC3300SA) manufactured by NETZSCH JAPAN at a heating rate of 10° C. / min.

[0100] [Young's Modulus] The Young's modulus was measured and calculated in accordance with JIS R 1602-1995. Specifically, a glass sample was processed to a size of 20 mm in length, 20 mm in width, and 100 mm in height, sufficiently annealed, and placed in a temperature-controlled chamber. The longitudinal wave velocity (Vl) and shear wave velocity (Vs) of 5 MHz ultrasound were measured, and the Young's modulus (E) and rigidity modulus (G) were calculated by the following formulas. E=(4G 2 -3G×Vl 2 ×ρ) / (G-Vl 2 ×ρ) G=Vs 2 ×ρ Here, ρ is the density of the glass sample, and the value of the specific gravity is used.

[0101] [Average linear expansion coefficient α at -30℃ to 70℃ n 〕 Average linear expansion coefficient α at -30℃ to 70℃ n was measured using an interferometric dilatometer and calculated according to the following formula: α n =dL n / (L×dT n ) Here, dT n is the temperature difference from -30 to 70°C (K), L is the initial length of the glass sample (mm), dL n is the change in sample length (mm) in the temperature range of -30 to 70°C.

[0102] 〔specific gravity〕 The specific gravity was measured by the Archimedes method.

[0103] [Specific elastic modulus] The specific elastic modulus was calculated by dividing the Young's modulus by the density at room temperature. The density at room temperature is expressed in units of specific gravity (g / cm 3 ) is added.

[0104] [Internal transmittance] The glass samples were processed to have a thickness of 10 mm ± 0.1 mm and parallel, optically polished flat surfaces, and the internal transmittances at wavelengths of 420 nm and 800 nm were measured. The internal transmittance τ was calculated using the following formula by measuring the transmittances (external transmittances) T1 and T2, including the surface reflection loss, of two glass samples made of the same glass sample but with different thicknesses d1 and d2. logτ=-[(logT1-logT2)×10] / Δd Here, d2>d1, Δd=d2-d1, and log is the common logarithm.

[0105] [Table 1]

[0106] [Preparation of glass wafer] The above glass sample was cut, ground, and polished to produce a disk-shaped glass wafer with a holder on its outer edge. The area, diameter, and thickness of one main surface of the glass wafer are shown in Table 2. Figure 13 shows the shape of the holder using an SEM image of the cross section of the glass wafer. The flatness of the glass wafer before the formation of the diffractive optical element was evaluated using a BOW.

[0107] [Flatness before forming diffractive optical element (BOW)] The flatness was evaluated by the BOW. The BOW can be measured by a known method, for example, a non-contact BOW measuring device, and the standard for measuring the BOW in the American Society for Testing and Materials standard ASTM F534 can be applied. Specifically, the glass wafer was supported at three points arranged at equal intervals (120° intervals) on the circumference of an imaginary circle with a diameter slightly smaller than the diameter of the glass wafer. At this time, the center of the glass wafer and the center of the imaginary circle were aligned vertically, and the glass wafer was not fixed (clamped). The deviation of the center point of the central surface of the glass wafer from an imaginary plane (called the central surface reference plane) including the three points supporting the glass wafer was defined as the BOW.

[0108] Here, as shown in Figure 14, the central surface is an imaginary surface that is equidistant from the two main surfaces of the glass wafer and is inside the glass wafer. When the center point of the central surface of the glass wafer is above the central surface reference plane, the BOW has a positive value. On the other hand, when the center point of the central surface of the glass wafer is below the central surface reference plane, the BOW has a negative value. The larger the absolute value of BOW, the greater the curvature of the glass wafer.

[0109] A diffractive optical element was formed on a glass wafer by the following method. For the obtained glass wafer, the period of the uneven structure of the diffraction grating and the height difference between the convex and concave portions of the diffraction grating were measured. The results are shown in Table 2.

[0110] [Formation by electron beam lithography] A titanium oxide film was formed by sputtering on one of the main surfaces of the glass wafer in a vacuum chamber. After the film formation, a diffractive optical element portion was formed on the glass wafer by electron beam drawing. In the electron beam drawing, the glass wafer was coated with an electron beam resist, pre-baked, and placed in a vacuum chamber to reduce the pressure. At this time, a vacuum chuck was not used in the vacuum chamber, and the glass wafer was held at points at the holding portion on the outer edge and at several points near the outer edge of the back surface where the diffractive optical element portion was not formed. The held glass wafer was not distorted, and the diffractive optical element portion was formed with high precision while maintaining the flatness of the glass wafer. A glass wafer was obtained in which a diffractive optical element portion of the size shown in Table 2 was formed at a predetermined position on the main surface. It was confirmed that the fabrication of the diffractive optical element portion by electron beam drawing was suitable for prototyping. It was also confirmed that the performance of the prototype could be reproduced with high precision in mass production by using the same glass, material of the diffractive optical element portion, shape and size of the wafer in the prototype and mass production, and further using glass with a predetermined Young's modulus.

[0111] [Formation using organic materials] A siloxane polymer was applied as an organic material to one of the main surfaces of the glass wafer to form a coating film, and a mold having an inverted shape of the diffraction grating pattern of the diffractive optical element portion was transferred to the coating film. It was then heated and baked at about 125°C to obtain a glass wafer having a diffractive optical element portion of the size shown in Table 2 formed at a predetermined position on the main surface.

[0112] [Formation using inorganic materials] In a vacuum chamber, a titanium oxide film, a silicon nitride film, or a silicon carbide film was formed on one of the main surfaces of a glass wafer by sputtering. After the film formation, the glass wafer was removed from the vacuum chamber, and a photoresist liquid was uniformly applied to the main surface of the glass wafer on which the film was formed. Next, the glass wafer was heated to evaporate the solvent of the photoresist (pre-baking), and a photomask having a pattern corresponding to the periodic fine structure pattern of the diffractive optical element was used to transfer the pattern of the photomask to the photoresist on the surface of the glass wafer by ultraviolet irradiation (exposure). After exposure, the photoresist was selectively removed using a developer (development), and the glass wafer was heated to about 120 to 150°C to thermally crosslink the photoresist (post-baking). Next, the film on the main surface of the glass wafer was selectively etched to form a diffractive optical element portion. As a result, a glass wafer was obtained in which a diffractive optical element portion having the size shown in Table 2 was formed at a predetermined position on the main surface.

[0113] [Periodicity (pitch) of the uneven structure of the diffraction grating] The measurements were carried out using a scanning electron microscope (SEM).

[0114] [Height difference between convex and concave portions of the diffraction grating] The measurements were performed using an atomic force microscope (AFM).

[0115] Example 2 Each glass wafer produced by each method in Example 1, i.e., a glass wafer on which a diffractive optical element portion was formed by electron beam lithography, and a glass wafer on which a diffractive optical element portion was formed by organic or inorganic material, was cut and separated by dicing to produce a plurality of light guide plates. The size and number of light guide plates obtained from one glass wafer are shown in Table 2.

[0116] Example 3 The light guide plate produced in Example 2 was incorporated into a head-mounted display. That is, the light guide plates produced in Example 2 were mounted on a frame together with a light source and an optical system to produce a glasses-type image display device. When this image display device was worn and images were displayed, high-quality images with a wide FOV could be displayed in all cases, providing a sufficient sense of immersion.

[0117] [Table 2(1)]

[0118] [Table 2(2)]

[0119] [Table 2(3)]

[0120] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of the present invention is defined by the claims, not the above description, and is intended to include all modifications within the meaning and scope of the claims.

[0121] For example, by adjusting the composition as described in the specification to the glass compositions exemplified above, an optical glass according to one aspect of the present invention can be produced. Furthermore, it is of course possible to arbitrarily combine two or more of the items described in the specification as examples or preferred ranges.

Claims

1. A retaining portion is provided on the outer edge. The area of ​​one main surface is 1950 mm 2 or more, and has a thin plate shape with a thickness of 3.0 mm or less, Young's modulus is 100 GPa or more. A glass wafer for manufacturing light guide plates.

2. The glass wafer according to claim 1 , further comprising a diffractive optical element portion on a main surface thereof.

3. 2. The glass wafer according to claim 1, wherein the holding part has a polished surface.

4. A method for manufacturing a light guide plate, comprising the step of separating the glass wafer according to claim 2.

Citation Information

Patent Citations

  • Head-mount display, control method of head-mount display, and control program

    JP2016139174A