Resin film, composite sheet, and manufacturing method for processed workpiece

A composite sheet with a laminated structure of a second resin layer and a resin film, containing a soluble resin and an energy ray-curable compound, addresses the inefficiencies of separate sheets by allowing flexible use as a die bonding or dicing sheet through controlled curing, improving storage and process efficiency.

JP2024144243APending Publication Date: 2024-10-11LINTEC CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024044155
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-19
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Conventional methods require separate die bonding sheets, protective film forming sheets, and dicing sheets, leading to inefficiencies in storage and management, as these sheets have different uses depending on whether the resin film is peeled off or not.

Method used

A composite sheet with a laminated structure of a second resin layer and a resin film containing a soluble resin and an energy ray-curable compound, allowing the resin film to be used as either a die bonding sheet or a protective film forming sheet by controlling its curing with energy rays, thereby simplifying storage and use.

Benefits of technology

The composite sheet can be used flexibly as either a die bonding sheet or a dicing sheet, reducing the need for multiple types of sheets and enhancing process efficiency by controlling peeling forces through energy ray curing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144243000001_ABST
    Figure 2024144243000001_ABST
Patent Text Reader

Abstract

To provide a composite sheet having a laminated structure of a second resin layer and a resin film of a type different from the second resin layer, which can be used as either a die bonding sheet or a dicing sheet, and to provide the resin film.SOLUTION: A resin film 11 includes a soluble resin (a) and an energy ray curable compound (b) different from the soluble resin (a), where 13 g or more of the soluble resin (a) is soluble in 100 g of toluene at a temperature condition of 23°C. A composite sheet 1 includes the resin film 11 and a second resin layer 12 provided on one surface 11a of the resin film 11.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a resin film, a composite sheet, and a workpiece. [Background technology]

[0002] A semiconductor chip is usually die-bonded to the circuit surface of a substrate by a film-like adhesive (sometimes called a "die-bonding film") provided on the back surface of the semiconductor chip. Then, if necessary, one or more semiconductor chips are stacked on the semiconductor chip, wire bonding is performed, the film-like adhesive is thermally cured, and the whole obtained is sealed with resin to produce a semiconductor package. The semiconductor package is then used to manufacture the desired semiconductor device.

[0003] The film-like adhesive is, for example, in the form of a die bonding sheet having a release film (sometimes called a "separator") on one side, and the other side (i.e., the side opposite the one side) is attached to the back side of a semiconductor wafer (see, for example, Patent Document 1). Next, after the release film is peeled off from the film-like adhesive, a dicing sheet is attached to the surface of the film-like adhesive on which the release film was provided. The dicing sheet may be, for example, a composite sheet comprising a base material and a pressure-sensitive adhesive layer. In this case, the pressure-sensitive adhesive layer is attached to the film-like adhesive (for example, see Patent Document 2). Next, the semiconductor wafer is diced (divided) together with the film adhesive to produce a semiconductor chip with a film adhesive, the semiconductor chip comprising a semiconductor chip and the film adhesive after cutting provided on the back surface of the semiconductor chip. The semiconductor chip with the film-like adhesive is then peeled off from the dicing sheet and, as described above, is die-bonded to the circuit surface of the substrate by the film-like adhesive. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 7155245 [Patent Document 2] JP 2009-064975 A Summary of the Invention [Problem to be solved by the invention]

[0005] Furthermore, as with the film-like adhesive, a protective film-forming film for protecting a semiconductor wafer or semiconductor chip is used by laminating it with a release film and provided on the back surface of the semiconductor wafer or semiconductor chip. The protective film-forming film is also, for example, in the state of a protective film-forming sheet having a release film on one surface thereof, and the other surface is attached to the back surface of the semiconductor wafer. The protective film-forming film includes those that have a curing property and form a protective film by curing, and those that function as a protective film without curing. If the protective film-forming film has a curing property, it is cured at some stage during use. The protective film-forming film is also used in the same manner as the film-like adhesive, and in that case, a semiconductor chip with a protective film-forming film or a semiconductor chip with a protective film is produced, which comprises a semiconductor chip and a protective film-forming film or a protective film after cutting provided on the back surface of the semiconductor chip, and these are peeled off from the dicing sheet.

[0006] In the manufacturing process of the semiconductor device as described above, the film-like adhesive in the die bonding sheet and the pressure-sensitive adhesive layer in the dicing sheet may be used as a resin layer containing a resin component (sometimes referred to as the "second resin layer" in this specification). When the resin layer is capable of forming a protective film, the protective film-forming film in the protective film-forming sheet may be used as the resin layer (second resin layer). When the film-like adhesive in the die bonding sheet and the protective film-forming film in the protective film-forming sheet are used, the release film is peeled off. On the other hand, the pressure-sensitive adhesive layer in the dicing sheet has the base material on one side thereof, and this state is maintained even when the dicing sheet is used. That is, the die bonding sheet, the protective film-forming sheet, and the dicing sheet are all common in that they are composite sheets having a laminated structure of a second resin layer and a resin film of a type different from the second resin layer, but the usage methods thereof differ from each other in terms of whether or not the resin film is peeled off. Therefore, naturally, conventionally, the die bonding sheet, the protective film forming sheet, and the dicing sheet are used separately.

[0007] However, if a composite sheet could be realized that could be used as both a die bonding sheet or a sheet for forming a protective film, and a dicing sheet, it would be extremely useful, as it would eliminate the need to keep die bonding sheets or sheets for forming a protective film, and dicing sheets in stock separately. In contrast, no such composite sheet is known among the conventional composite sheets, including those disclosed in Patent Documents 1 and 2.

[0008] Although the above description has been given taking semiconductor wafers and semiconductor chips as examples, the same can be said for workpieces other than semiconductor wafers used in the manufacture of semiconductor devices, and their processed products.

[0009] The present invention aims to provide a composite sheet having a laminated structure of a second resin layer and a resin film of a different type from the second resin layer, which can be used as either a die bonding sheet or a sheet for forming a protective film, or a dicing sheet, and the resin film. [Means for solving the problem]

[0010] In order to solve the above problems, the present invention employs the following configuration. [1] A resin film comprising a soluble resin (a) and an energy ray-curable compound (b) different from the soluble resin (a), wherein 13 g or more of the soluble resin (a) is soluble in 100 g of toluene at a temperature of 23°C. [2] The resin film according to [1], further comprising a photopolymerization initiator (c).

[0011] [3] The resin film according to [1] or [2], wherein the soluble resin (a) is an ethylene-vinyl acetate copolymer. [4] The resin film and an acrylic resin film are bonded together to prepare a test piece (s11), and an illuminance of 230 mW / cm 2 is applied to the test piece (s11). 2 , light intensity 190mJ / cm 2 A test piece (s12) was prepared by irradiating ultraviolet rays to ultraviolet-cur the test piece under the above conditions. A peel force P1 was measured when the resin film was peeled from the acrylic resin film in the test piece (s11) at a peel speed of 300 mm / min in an environment of a temperature of 23° C. and a relative humidity of 50%, so that the surfaces of the resin film and the acrylic resin film that had been in contact with each other formed an angle of 180°. A peel force P2 was measured when the ultraviolet-cured product of the resin film was peeled from the acrylic resin film in the test piece (s12) at a peel speed of 300 mm / min in an environment of a temperature of 23° C. and a relative humidity of 50%, so that the surfaces of the ultraviolet-cured product of the resin film and the acrylic resin film that had been in contact with each other formed an angle of 180°. The peel force P2 was calculated based on the following formula P(0): P2 / P1×100 P(0) The resin film according to any one of [1] to [3], wherein the peel strength ratio calculated by the following formula is 15000% or more.

[0012] [5] A composite sheet comprising the resin film according to any one of [1] to [4] and a second resin layer provided on one surface of the resin film. [6] A method for producing a workpiece, the workpiece being obtained by processing a workpiece, the method comprising: a bonding step of bonding a surface of the second resin layer in the composite sheet described in [5] opposite to the resin film side to one surface of the workpiece to produce a workpiece with the composite sheet; and a peeling step (I) of peeling the resin film from the second resin layer in the workpiece with the composite sheet after the bonding step; and a processing step (I) of processing the workpiece with the second resin layer after the peeling step (I), to produce the workpiece; or the method for producing a workpiece, comprising: a hardening step (II) of hardening the resin film in the composite sheet with energy rays after the attaching step, thereby producing a workpiece with a hardened composite sheet, in which the composite sheet in the workpiece with the composite sheet becomes a hardened composite sheet; a processing step (II) of processing the workpiece in the workpiece with the hardened composite sheet after the hardening step (II), thereby producing the workpiece; and a pick-up step (II) of separating the workpiece from the second resin layer in the hardened composite sheet and picking it up after the processing step (II). [7] A method for manufacturing a workpiece as described in [6], further comprising, after the curing step (II) and before the processing step (II), a peeling step (III) of peeling the cured composite sheet from the workpiece in the workpiece with the cured composite sheet, and, after the peeling step (III), a re-attaching step (II) of producing a workpiece with a cured composite sheet by re-attaching the surface of the second resin layer in the peeled cured composite sheet opposite the energy ray cured product side of the resin film to one surface of the workpiece. Effect of the Invention

[0013] According to the present invention, there is provided a composite sheet having a laminated structure of a second resin layer and a resin film of a different type from the second resin layer, which can be used as either a die bonding sheet or a sheet for forming a protective film, or a dicing sheet, and the resin film. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a cross-sectional view illustrating an example of a composite sheet and a resin film according to an embodiment of the present invention. [Diagram 2] 1A to 1C are cross-sectional views for illustrating a method of using a composite sheet according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] ◇Resin film A resin film according to one embodiment of the present invention contains a soluble resin (a) and an energy ray-curable compound (b) different from the soluble resin (a), and at a temperature of 23°C, 13 g or more of the soluble resin (a) can be dissolved in 100 g of toluene. The resin film of the present embodiment contains the soluble resin (a) and the energy ray-curable compound (b), and thus has energy ray-curability.

[0016] The resin film of the present embodiment can be laminated with a second resin layer to form a composite sheet, as described below. In the composite sheet, the peel strength between the resin film and the second resin layer varies depending on whether or not the resin film is cured with energy rays. More specifically, when the resin film in the composite sheet is energy ray cured, i.e., in a cured composite sheet comprising an energy ray cured product of the resin film and a second resin layer provided on one side of the energy ray cured product, the peel force between the energy ray cured product and the second resin layer (sometimes referred to in this specification as "post-curing peel force") is significantly greater than the peel force between the resin film and the second resin layer in the composite sheet (sometimes referred to in this specification as "pre-curing peel force").

[0017] Therefore, in a composite sheet in which the resin film has not been cured by energy rays, the resin film can be easily peeled off from the second resin layer, so that the second resin layer is suitable as a film-like adhesive or a protective film-forming film, and the composite sheet is suitable as a die bonding sheet or a sheet for forming a protective film. On the other hand, in the cured composite sheet in which the resin film is energy ray cured, the energy ray cured product of the resin film cannot be easily peeled off from the second resin layer, but rather the cured composite sheet can be easily peeled off from the attachment (e.g., a film-like adhesive, a workpiece, etc.) attached to the second resin layer therein. Therefore, the second resin layer is suitable as a pressure-sensitive adhesive layer, and the composite sheet is suitable as a dicing sheet.

[0018] In this specification, the mere description of "resin film" means the resin film of this embodiment which contains the soluble resin (a) and the energy ray-curable compound (b) and is not cured by energy rays. In this specification, the mere description of a "composite sheet" means a composite sheet in which the resin film is not cured with energy rays.

[0019] In this specification, the term "energy rays" refers to electromagnetic waves or charged particle beams that have an energy quantum. Examples of energy rays include ultraviolet rays, radiation, and electron beams. Ultraviolet rays can be irradiated by using, for example, a high-pressure mercury lamp, a fusion lamp, a xenon lamp, a black light, or an LED lamp as an ultraviolet ray source. Electron beams can be irradiated by generating them using an electron beam accelerator or the like. In this specification, the term "energy ray curable" refers to a property of being cured by irradiation with energy rays.

[0020] <<Probe tack value T1 of resin film>> The probe tack value T1 of a resin film (a resin film that has not been cured with energy rays) (sometimes referred to in this specification as the "probe tack value T1 before curing" or simply as "T1") is an indicator of the peel force between the resin film and the second resin layer in the composite sheet described below. The probe tack value T1 before curing is 1.96mN / cm 2 (0.2gf / cm 2 ) or more, for example, 2.16 mN / cm 2 (0.22gf / cm 2 When T1 is equal to or greater than the lower limit, the peel strength between the resin film and the second resin layer becomes greater within an appropriate range, and a composite sheet including such a resin film, which will be described later, is suitable as a die bonding sheet. On the other hand, the upper limit of T1 is not particularly limited. For example, if T1 is 10 mN / cm 2 (1.02gf / cm 2 ) or less can be more easily manufactured. In one embodiment, T1 is, for example, 1.96 to 10 mN / cm 2 (0.2~1.02gf / cm 2 ), and 2.16 to 10 mN / cm 2 (0.22~1.02gf / cm 2 ) However, these are just examples of T1.

[0021] The pre-curing probe tack value T1 can be measured by the following method. That is, a test piece (s21) having a diameter of 10 mm is cut out from the resin film to be measured, and the probe tack value is measured for one surface of the test piece (s21) under a temperature condition of 23° C. At this time, a stainless steel probe having a diameter of 5 mm is used as the probe, and a tack value of 9.80665 N / cm 2 (1000gf / cm 2 It is preferable that the load of (s21) is applied for 1 second, and then the probe is peeled off from the test piece (s21) at a peeling speed of 10 mm / sec. When determining T1, it is preferable to determine the maximum probe tack value at any point in the test piece (s21) in this manner, determine such maximum probe tack values ​​at two or more different points in the test piece (s21), and use the minimum value of the multiple maximum values ​​thus obtained as the pre-cured probe tack value T1.

[0022] The pre-curing probe tack value T1 can be adjusted by adjusting the types or amounts of the components contained in the resin film, which will be described later. In particular, the pre-curing probe tack value T1 can be more easily adjusted by adjusting the types or amounts of the soluble resin (a) and the energy ray curable compound (b), which will be described later.

[0023] <<Probe tack value T2 of UV-cured resin film>> The probe tack value T2 of the UV-cured resin film (sometimes referred to in this specification as the "post-cured probe tack value T2" ​​or simply as "T2") is an indicator of the peel force between the energy ray-cured resin film and the second resin layer in the cured composite sheet described below. After curing, the probe tack value T2 is 0.88mN / cm 2 (0.09gf / cm 2 ) or less, for example, 0.69 mN / cm 2 (0.07gf / cm 2 ) or less, and 0.49mN / cm 2 (0.05gf / cm2 When T2 is equal to or less than the upper limit, the peel strength between the energy ray-cured product of the resin film and the second resin layer becomes larger, and a composite sheet including such a resin film, which will be described later, is suitable as a dicing sheet. On the other hand, the lower limit of T2 is not particularly limited. For example, when T2 is 0.05 mN / cm 2 (0.005gf / cm 2 ) or more can be produced more easily. In one embodiment, T2 is, for example, 0.05 to 0.88 mN / cm 2 (0.005~0.09gf / cm 2 ), 0.05~0.69mN / cm 2 (0.005~0.07gf / cm 2 ), and 0.05 to 0.49 mN / cm 2 (0.005~0.05gf / cm 2 ) However, these are just examples of T2.

[0024] The post-curing probe tack value T2 can be measured by the following method. That is, a test piece (s21) was prepared, and this test piece (s21) was irradiated with an ultraviolet ray irradiation device equipped with a high-pressure mercury lamp under air at an illuminance of 230 mW / cm 2 , light intensity 190mJ / cm 2 The test piece (s21) is cured by irradiating ultraviolet rays under the above conditions, and the obtained one is called a test piece (s22). Then, for the test piece (s22), the post-curing probe tack value T2 is measured in the same manner as for the test piece (s21).

[0025] The post-cure probe tack value T2 can be adjusted in the same manner as the pre-cure probe tack value T1 described above.

[0026] <<Probe tack value of resin film after curing>> Using the pre-cure probe tack value T1 and the post-cure probe tack value T2, the following formula (T0): T2 / T1×100 (T0) The post-curing ratio of the probe tack value of the resin film calculated by (sometimes referred to herein as "post-curing ratio of the probe tack value" or simply "post-curing ratio") is preferably 50% or less, more preferably 40% or less, and may be, for example, either 30% or less or 20% or less. The smaller the post-curing ratio of the probe tack value, the smaller the ratio of the probe tack value T2 of the ultraviolet-cured product of the resin film to the probe tack value T1 of the resin film, and the larger the fluctuation range of the probe tack value of the resin film before and after its energy ray curing. A composite sheet having such a resin film is more preferable in terms of the characteristic that it can be used as either a die bonding sheet or a dicing sheet. On the other hand, the lower limit of the probe tack value after curing is not particularly limited. For example, a resin film having a probe tack value after curing of 8% or more can be produced more easily. In one embodiment, the post-cure ratio of the probe tack value may be, for example, any one of 8 to 50%, 8 to 40%, 8 to 30%, and 8 to 20%, although these are only examples of the post-cure ratio of the probe tack value.

[0027] <<Gel fraction G1 of resin film>> The gel fraction G1 of a resin film (a resin film that has not been cured with energy rays) (sometimes referred to in this specification as the "pre-cured gel fraction G1" or simply as "G1") is an indicator of the peel force between the resin film and the second resin layer in the composite sheet described below. The gel fraction G1 before curing is preferably less than 30%, more preferably 20% or less, and even more preferably 10% or less, and may be, for example, 7% or less. When G1 is in such a range, the peel force between the resin film and the second resin layer becomes larger within an appropriate range, and a composite sheet having such a resin film, which will be described later, is suitable as a die bonding sheet. On the other hand, the lower limit of G1 is not particularly limited. For example, a resin film having a G1 of 1% or more can be produced more easily. In one embodiment, G1 may be, for example, any one of 1% or more and less than 30%, 1 to 20%, 1 to 10%, and 1 to 7%, although these are just examples of G1.

[0028] When the resin film contains a solid material such as a filler that is insoluble in a solvent (e.g., toluene) at room temperature, the gel fraction G1 before curing is the gel fraction of the components other than the solid material of the resin film. The gel fraction G1 before curing means the degree of gelation when the components in the resin film gel. Since the solid material among the components in the resin film does not contribute to gelation, when the resin film contains a solid material, the gel fraction G1 before curing is the gel fraction of the components other than the solid material of the resin film.

[0029] In this specification, "room temperature" means a temperature that is neither particularly cooled nor heated, that is, an ordinary temperature, and examples thereof include temperatures of 15 to 25°C.

[0030] In this specification, unless otherwise specified, the term "solvent" is a concept that encompasses both a component that is liquid at room temperature and that dissolves a solute, and a component that is liquid at room temperature and that functions as a dispersion medium for dispersing a dispersoid.

[0031] The gel fraction G1 before curing can be measured by a known method. For example, G1 can be measured with high accuracy by the following method. That is, the resin film is cut into a size of 50 mm x 100 mm to prepare a sample (s310), and the sample (s310) is wrapped in a nylon mesh sheet with a size of 100 mm x 150 mm and a mesh size of 200, and the resultant is fastened with a staple or other fastener to prepare a test piece (s31). The mass M of the test piece (s31) 11The mass M of the test piece (s31) after immersion in toluene (500 mL) at 25°C for 24 hours was measured, and the insoluble matter of the sample (s310), the nylon mesh sheet, and the fasteners were all removed, and these were dried at 90°C for 3 hours, and then left to stand for 1 hour under conditions of 23°C and a relative humidity of 50% for humidity conditioning. 51 (i.e., the total mass of the insoluble matter of the sample (s310), the mass of the nylon mesh sheet, and the mass of the fastener) was measured, and the M 51 , mass M of the test piece (s31) 11 Using the mass M2 of the nylon mesh sheet, the mass M3 of the fastener, and the solid matter content M4 of the resin film, the following formula G(01): (M 51 -M2-M3-M4) / (M 11 -M2-M3-M4) x 100 G(01) The gel fraction before curing G1 can be calculated by the above. In addition, when the resin film contains inorganic components such as a filler, the content of the inorganic components in the resin film can be determined by burning the gel after measuring the gel fraction G1 and measuring the amount of the resulting residue.

[0032] The gel fraction G1 before curing can be adjusted by adjusting the types or amounts of the components contained in the resin film, which will be described later. In particular, the gel fraction G1 before curing can be more easily adjusted by adjusting the types or amounts of the soluble resin (a) and the energy ray curable compound (b), which will be described later.

[0033] <<Gel fraction G2 of UV-cured resin film>> The gel fraction G2 of the UV-cured resin film (sometimes referred to in this specification as the "post-cured gel fraction G2" or simply as "G2") is an indicator of the peel force between the energy ray-cured resin film and the second resin layer in the cured composite sheet described below. The gel fraction G2 after curing is preferably 30% or more, more preferably 40% or more, and may be, for example, 50% or more. When G2 is equal to or more than the lower limit, the peel force between the energy ray-cured product of the resin film and the second resin layer becomes larger, and a composite sheet including such a resin film, which will be described later, is suitable as a dicing sheet. On the other hand, the upper limit of G2 is not particularly limited. For example, a resin film having a G2 of 70% or less can be produced more easily. In one embodiment, G2 may be, for example, any one of 30 to 70%, 40 to 70%, and 50 to 70%, although these are just examples of G2.

[0034] When the UV-cured resin film contains a solid such as a filler that is insoluble in a solvent (e.g., toluene) at room temperature, the gel fraction G2 after curing is the gel fraction of the components other than the solid matter in the UV-cured resin film. The gel fraction G2 after curing means the degree of gelation when the components in the UV-cured resin film are gelled. Since the solid matter among the components in the UV-cured resin film does not contribute to gelation, when the UV-cured resin film contains a solid matter, the gel fraction G2 after curing is the gel fraction of the components other than the solid matter in the UV-cured resin film.

[0035] The gel fraction G2 after curing can be measured by a known method. For example, G2 can be measured with high accuracy by the following method. That is, a resin film was exposed to ultraviolet light at an illuminance of 230 mW / cm under air using an ultraviolet light irradiation device equipped with a high-pressure mercury lamp. 2 , light intensity 190mJ / cm 2 The composition is cured by irradiating it with ultraviolet light under the above conditions. Using the obtained UV-cured resin film, a test piece (s32) is prepared in the same manner as the above test piece (s31), and the gel fraction is measured. More specifically, the UV-cured resin film is cut into a size of 50 mm x 100 mm to prepare a sample (s320), and the sample (s320) is wrapped in a nylon mesh sheet with a size of 100 mm x 150 mm and a mesh size of 200, and the resulting product is fastened with a fastener such as a stapler pin to prepare a test piece (s32). The mass M of the test piece (s32) is 12 The mass M of the test piece (s32) after immersion in toluene (500 mL) at 25°C for 24 hours was measured, and the insoluble matter of the sample (s320), the nylon mesh sheet, and the fasteners were all removed, and these were dried at 90°C for 3 hours, and then allowed to stand for 1 hour under conditions of 23°C and a relative humidity of 50% for humidity conditioning. 52 (i.e., the total mass of the insoluble matter of the sample (s320), the mass of the nylon mesh sheet, and the mass of the fastener) was measured, and the M 52 , mass of test piece (s32) M 12 Using the mass M2 of the nylon mesh sheet, the mass M3 of the fastener, and the solid content M4 of the UV-cured resin film, the following formula G(02): (M 52 -M2-M3-M4) / (M 12 -M2-M3-M4) x 100 G(02) The gel fraction G2 after curing can be calculated by the above.

[0036] The post-cure gel fraction G2 can be adjusted in the same manner as in the pre-cure gel fraction G1 described above.

[0037] <<Gel fraction of resin film after curing>> Using the gel fraction before curing G1 and the gel fraction after curing G2, the following formula (G0): G2 / G1×100 (G0) The post-curing gel fraction ratio of the resin film calculated by (sometimes referred to herein as "post-curing gel fraction ratio" or simply "post-curing ratio") is preferably 400% or more, more preferably 700% or more, and may be, for example, 1000% or more. The higher the post-curing gel fraction ratio, the higher the ratio of the gel fraction G2 of the UV-cured resin film to the gel fraction G1 of the resin film, and the larger the variation range of the gel fraction of the resin film before and after its energy ray curing. A composite sheet having such a resin film is more preferable in terms of its characteristic that it can be used as either a die bonding sheet or a dicing sheet. On the other hand, there is no particular upper limit to the post-curing gel fraction ratio. For example, a resin film having a post-curing probe tack value ratio of 1500% or less can be produced more easily. In one embodiment, the post-curing ratio of the probe tack value may be, for example, any one of 400 to 1500%, 700 to 1500%, and 1000 to 1500%, although these are only examples of the post-curing ratio of the gel fraction.

[0038] <<Peel force P1 between resin film and acrylic resin film>> After a resin film (a resin film that has not been cured by energy rays) is laminated to an acrylic resin film, the peel force P1 (sometimes referred to in this specification as the "pre-curing peel force P1" or simply "P1") observed when peeling the resin film from the acrylic resin film is an indicator of the peel force between the resin film and the second resin layer in the composite sheet described below. The pre-curing peel strength P1 is preferably 100 mN / 25 mm or less, more preferably 50 mN / 25 mm or less, and even more preferably 30 mN / 25 mm or less. By making P1 equal to or less than the upper limit, the peel strength between the resin film and the second resin layer becomes smaller within an appropriate range, and a composite sheet having such a resin film, which will be described later, is suitable as a die bonding sheet or a sheet for forming a protective film. On the other hand, the lower limit of P1 is not particularly limited. For example, a resin film having P1 of 8 mN / 25 mm or more can be produced more easily. In one embodiment, P1 may be, for example, any one of 8 to 100 mN / 25 mm, 8 to 50 mN / 25 mm, and 8 to 30 mN / 25 mm, although these are merely examples of P1.

[0039] When measuring the pre-curing peel force P1, the acrylic resin constituting the acrylic resin film is a resin having structural units that can be considered to be derived from a (meth)acrylic acid ester, and preferably a resin having only structural units that can be considered to be derived from a (meth)acrylic acid ester.

[0040] In this specification, the term "(meth)acrylic acid" is a concept that encompasses both "acrylic acid" and "methacrylic acid." The same applies to terms similar to (meth)acrylic acid, such as a (meth)acryloyl group.

[0041] The pre-curing peel strength P1 can be measured by the following method. That is, a test piece (s110) is prepared by bonding a resin film to be measured and an acrylic resin film while heating them at a temperature of 35 to 45° C. Furthermore, a piece having a width of 25 mm is cut out from this test piece (s110), and this piece is used as a test piece (s11). After this, the test piece (s11) is preferably left to stand for 30 minutes in an environment of a temperature of 23° C. and a relative humidity of 50%. Next, in an environment of 23°C temperature and 50% relative humidity, the peeling speed is set to 300 mm / min, and the resin film is peeled off from the acrylic resin film so that the surfaces of the resin film and the acrylic resin film in the test piece (s11) that were in contact with each other form an angle of 180° (180° peeling is performed). Then, the peeling force at this time is measured and is defined as the peeling force P1. It is preferable to calculate the average value of the peeling forces measured at this time and adopt this average value as the peeling force P1. Then, it is more preferable to calculate the average value of the peeling forces measured from when the length of the peeled part of the resin film exceeds 30 mm until the peeling is completed, and adopt this average value as the peeling force P1 of the resin film before curing. When measuring the peeling force, it is preferable to attach the entire exposed surface of the second resin layer in the test piece (s11) to the surface of a hard support via a double-sided tape, and measure the peeling force using the laminate obtained in this way. In this way, the peeling force P1 can be measured with higher accuracy.

[0042] The acrylic resin film to which the resin film is to be bonded may be, for example, a second resin layer constituting a composite sheet. That is, the test piece (s110) may be the composite sheet, and the test piece (s11) may be a slice of the composite sheet.

[0043] The peel strength P1 before curing can be adjusted by adjusting the types or amounts of the components contained in the resin film, which will be described later. In particular, the peel strength P1 before curing can be more easily adjusted by adjusting the types or amounts of the soluble resin (a) and the energy ray curable compound (b), which will be described later.

[0044] <<Peel force P2 between UV-cured resin film and acrylic resin film>> In an adhesive obtained by laminating a resin film (a resin film that has not been energy ray-cured) to an acrylic resin film, after curing the resin film with ultraviolet light, the peel force P2 (sometimes referred to in this specification as "post-curing peel force P2" or simply "P2") when peeling the ultraviolet-cured resin film from the acrylic resin film is an indicator of the peel force between the energy ray-cured resin film and the second resin layer in the cured composite sheet described below. The post-curing peel strength P2 is preferably 3500 mN / 25 mm or more, more preferably 4500 mN / 25 mm or more, and even more preferably 5500 mN / 25 mm or more. When P2 is equal to or more than the lower limit, the peel strength between the energy ray-cured resin film and the second resin layer becomes larger, and a composite sheet including such a resin film, which will be described later, is suitable as a dicing sheet. On the other hand, there is no particular upper limit for P2. For example, a resin film having P2 of 10000 mN / 25 mm or less can be produced more easily. In one embodiment, P2 may be, for example, any one of 3500 to 10000 mN / 25 mm, 4500 to 10000 mN / 25 mm, and 5500 to 10000 mN / 25 mm, although these are merely examples of P2.

[0045] The post-curing peel strength P2 can be measured by the following method. That is, a test piece (s11) was prepared, and this test piece (s11) was irradiated with an ultraviolet ray irradiation device equipped with a high-pressure mercury lamp under air at an illuminance of 230 mW / cm. 2 , light intensity 190mJ / cm 2 The test piece (s11) is cured by irradiating ultraviolet rays under the above conditions, and the obtained one is called a test piece (s12). Then, for the test piece (s12), the post-curing peel force P2 is measured in the same manner as for the test piece (s11).

[0046] The post-cure release force P2 can be adjusted in the same manner as the pre-cure release force P1 described above.

[0047] <<Resin film peel strength after curing>> Using the peel force before curing P1 and the peel force after curing P2, the following formula (P0): P2 / P1×100 (P0) The post-curing ratio of the peel strength of the resin film calculated by (sometimes referred to as "post-curing ratio of peel strength" or simply "post-curing ratio" in this specification) is preferably 15000% or more, more preferably 25000% or more, and even more preferably 35000% or more. The higher the post-curing ratio of the peel strength, the higher the ratio of the post-curing peel strength P2 of the ultraviolet-cured product of the resin film to the pre-curing peel strength P1 of the resin film, and the larger the fluctuation range of the peel strength of the resin film before and after its energy ray curing. A composite sheet having such a resin film is more preferable in terms of the characteristic that it can be used as either a die bonding sheet or a sheet for forming a protective film, or a dicing sheet. On the other hand, there is no particular upper limit to the post-curing ratio of peel strength. For example, a resin film having a post-curing ratio of peel strength of 100,000% or less can be produced more easily. In one embodiment, the post-curing ratio of the peel strength may be, for example, any one of 15000 to 100000%, 25000 to 100000%, and 35000 to 100000%, although these are merely examples of the post-curing ratio of the peel strength.

[0048] As an example of a preferable resin film of the present embodiment, a test piece (s11) is prepared by bonding the resin film and an acrylic resin film, The illuminance of the test piece (s11) was 230 mW / cm 2 , light intensity 190mJ / cm 2 The test piece is irradiated with ultraviolet light under the conditions of (a) to (c), thereby curing the test piece with ultraviolet light, thereby preparing a test piece (s12); The peel force P1 was measured when the resin film was peeled from the acrylic resin film in the test piece (s11) at a peel speed of 300 mm / min under an environment of a temperature of 23° C. and a relative humidity of 50% such that the surfaces of the resin film and the acrylic resin film in the test piece (s11) that had been in contact with each other formed an angle of 180°; When a peel force P2 is measured at a peel speed of 300 mm / min under an environment of a temperature of 23°C and a relative humidity of 50%, such that the surfaces of the UV-cured product of the resin film and the acrylic resin film in the test piece (s12) that were in contact with each other form an angle of 180°, the peel force P2 is measured. Examples of the resin film include those in which the peel force ratio calculated by the formula P(0) is 15,000% or more.

[0049] <<Resin composition>> The resin film of the present embodiment can be manufactured using a resin composition containing its constituent materials. For example, the resin composition can be applied to a surface to be formed with the resin film, and dried as necessary to form the resin film at a desired location. The ratio of the contents of the components that do not vaporize at room temperature in the resin composition is usually the same as the ratio of the contents of the components in the resin film.

[0050] In the resin film, the ratio of the total content of one or more components contained in the resin film, which will be described later, to the total mass of the resin film does not exceed 100 mass %. Similarly, in the resin composition, the proportion of the total content of one or more components contained in the resin composition, which will be described later, relative to the total mass of the resin composition does not exceed 100 mass %.

[0051] The resin composition may be applied by a known method, for example, a method using various coaters such as an air knife coater, a blade coater, a bar coater, a gravure coater, a roll coater, a roll knife coater, a curtain coater, a die coater, a knife coater, a screen coater, a Mayer bar coater, or a kiss coater.

[0052] The drying conditions for the resin composition are not particularly limited, but when the resin composition contains a solvent described below, it is preferable to heat-dry the resin composition. The resin composition containing the solvent is preferably dried, for example, at 70 to 130° C. for 10 seconds to 5 minutes. The components of the resin film and the resin composition will be described in detail below.

[0053] The resin composition and the resin film contain a soluble resin (a) and an energy ray-curable compound (b), and are energy ray-curable. The resin composition and the resin film preferably contain a soluble resin (a), an energy ray-curable compound (b), and a photopolymerization initiator (c).

[0054] <Soluble resin (a)> The soluble resin (a) is a component for imparting film-forming properties to the resin film. The soluble resin (a) has solubility in a solvent at room temperature. More specifically, 13 g or more of the soluble resin (a) can be dissolved in 100 g of toluene under a temperature condition of 23° C. Since the soluble resin (a) has such solubility, a resin film can be produced by coating the resin composition.

[0055] The soluble resin (a) is preferably a resin other than an acrylic resin. The soluble resin (a) may, for example, be ethylene-vinyl acetate copolymer (EVA), and ethylene-vinyl acetate copolymer is a particularly preferred soluble resin (a).

[0056] In an ethylene-vinyl acetate copolymer, the ratio of the amount (parts by mass) of structural units derived from vinyl acetate to the total amount (parts by mass) of structural units ([amount (parts by mass) of structural units derived from vinyl acetate in ethylene-vinyl acetate copolymer] / [total amount (parts by mass) of structural units in ethylene-vinyl acetate copolymer]×100, sometimes referred to as the "vinyl acetate content" in this specification) is preferably 10 to 40% by mass, more preferably 10 to 30% by mass. By using such an ethylene-vinyl acetate copolymer, the difference in the properties of the composite sheet depending on whether or not the resin film is cured with energy rays becomes clearer.

[0057] The weight average molecular weight of the ethylene-vinyl acetate copolymer is preferably 45,000 to 65,000, and may be, for example, 50,000 to 60,000. By using such an ethylene-vinyl acetate copolymer, the difference in the properties of the composite sheet depending on whether or not the resin film is cured with energy rays becomes clearer.

[0058] The resin composition and the resin film may contain only one type of soluble resin (a), or two or more types. When there are two or more types, the combination and ratio thereof can be arbitrarily selected depending on the purpose.

[0059] In the resin composition, the ratio of the content of the soluble resin (a) to the total content of all components other than the solvent ([content of the soluble resin (a) in the resin composition (parts by mass)] / [total content of all components other than the solvent in the resin composition (parts by mass)]×100) is preferably 60 to 90% by mass, and may be, for example, any one of 60 to 75% by mass, 75 to 90% by mass, and 65 to 80% by mass. When the ratio is equal to or greater than the lower limit, the film shape of the resin film becomes more stable. When the ratio is equal to or less than the upper limit, the effects obtained by containing components other than the soluble resin (a), such as higher energy ray curability of the resin film, become greater.

[0060] The above is equivalent to saying that in the resin film, the ratio of the content of soluble resin (a) to the total mass of the resin film ([content of soluble resin (a) in resin film (parts by mass)] / [total mass of resin film (parts by mass)]×100) is preferably 60 to 90% by mass, and may be, for example, any one of 60 to 75% by mass, 75 to 90% by mass, and 65 to 80% by mass. This is based on the fact that in the process of removing the solvent from a resin composition containing a solvent (not limited to the resin composition for producing the resin film) to form a resin film, the amount of components other than the solvent usually does not change, and the content ratio of the components other than the solvent is the same between the resin composition and the resin film. Therefore, in this specification, not only in the case of a resin film, but also in the case of the resin film, the content of the components other than the solvent is mainly described as the content in the resin film obtained by removing the solvent from the resin composition.

[0061] <Energy ray curable compound (b)> The energy ray-curable compound (b) is a component for imparting energy ray-curability to the resin film. The energy ray-curable compound (b) is a component that does not fall under the category of the soluble resin (a), and may be either a resin component or a non-resin component. The energy ray-curable compound (b) may, for example, be a compound having at least one polymerizable double bond (energy ray-curable group) in the molecule, and is preferably an acrylate-based compound having a (meth)acryloyl group.

[0062] The energy ray-curable compound (b) which is a resin component may be either an oligomer having energy ray curability or a polymer having energy ray curability. The energy ray-curable compound (b), which is a non-resin component, is a monomer having energy ray curability (a low molecular weight compound having an energy ray-curable group).

[0063] Examples of the acrylate-based compound include trimethylolpropane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol monohydroxypenta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate, 1,4-butylene glycol di(meth)acrylate, and 1,6-hexanediol di(meth)acrylate. Examples of the (meth)acrylates include (meth)acrylates containing a chain aliphatic skeleton such as those mentioned above; (meth)acrylates containing a cyclic aliphatic skeleton such as dicyclopentanyl di(meth)acrylate and tricyclodecane dimethylol diacrylate; polyalkylene glycol (meth)acrylates such as polyethylene glycol di(meth)acrylate; oligoester (meth)acrylates; urethane (meth)acrylate oligomers; epoxy-modified (meth)acrylates; polyether (meth)acrylates other than the above-mentioned polyalkylene glycol (meth)acrylates; and itaconic acid oligomers.

[0064] The weight average molecular weight of the energy ray-curable compound (b) which is a resin component may be, for example, 300 to 30,000. The molecular weight of the energy ray-curable compound (b), which is a non-resin component, may be, for example, 60 to 500.

[0065] In this specification, the term "weight average molecular weight", not limited to the case of the energy ray-curable compound (b), unless otherwise specified, is a polystyrene-equivalent value measured by gel permeation chromatography (GPC).

[0066] The energy ray-curable compound (b) contained in the resin composition and resin film may be one type or two or more types, and when there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0067] In the resin film, the ratio of the content of the energy ray curable compound (b) to the total mass of the resin film ([content of energy ray curable compound (b) in the resin film (parts by mass)] / [total mass of the resin film (parts by mass)]×100) is preferably 10 to 38 mass%, and may be, for example, any one of 10 to 24 mass%, 24 to 38 mass%, and 18 to 32 mass%. When the ratio is equal to or more than the lower limit, the energy ray curability of the resin film becomes higher. When the ratio is equal to or less than the upper limit, the effect obtained by containing components other than the energy ray curable compound (b), such as a more stable film shape of the resin film, becomes higher.

[0068] <Photopolymerization initiator (c)> The photopolymerization initiator (c) is a component for efficiently promoting the polymerization reaction (energy ray curing) of the energy ray curable compound (b). The photopolymerization initiator (c) may be a known one.

[0069] Examples of the photopolymerization initiator (c) include benzoin compounds such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzoin benzoic acid, benzoin methyl benzoate, and benzoin dimethyl ketal; acetophenone compounds such as acetophenone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, and 2,2-dimethoxy-1,2-diphenylethane-1-one; and acylphosphine oxides such as bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide and 2,4,6-trimethylbenzoyldiphenylphosphine oxide. compounds; sulfide compounds such as benzyl phenyl sulfide and tetramethylthiuram monosulfide; α-ketol compounds such as 1-hydroxycyclohexyl phenyl ketone; azo compounds such as azobisisobutyronitrile; titanocene compounds such as titanocene; thioxanthone compounds such as thioxanthone; peroxide compounds; diketone compounds such as diacetyl; benzyl; dibenzyl; benzophenone; 2,4-diethylthioxanthone; 1,2-diphenylmethane; 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone; quinone compounds such as 1-chloroanthraquinone and 2-chloroanthraquinone, etc. Examples of the photopolymerization initiator (h) include photosensitizers such as amines.

[0070] The photopolymerization initiator (c) contained in the resin composition and the resin film may be one type or two or more types, and when there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0071] When the photopolymerization initiator (c) is used, the content of the photopolymerization initiator (c) in the resin composition and the resin film is preferably 1 to 20 parts by mass, more preferably 3 to 16 parts by mass, and particularly preferably 5 to 12 parts by mass, relative to 100 parts by mass of the content of the energy ray curable compound (b). When the content is equal to or more than the lower limit, the effect obtained by using the photopolymerization initiator (c) is enhanced. When the content is equal to or less than the upper limit, excessive use of the photopolymerization initiator (c) is suppressed.

[0072] <Solvent> The resin composition preferably further contains a solvent. A resin composition containing a solvent has good handleability. The solvent is not particularly limited, and examples of the solvent include water and organic solvents. Preferred examples of the organic solvent include hydrocarbons such as toluene and xylene; alcohols such as methanol, ethanol, 2-propanol, isobutyl alcohol (2-methylpropan-1-ol), and 1-butanol; esters such as ethyl acetate; ketones such as acetone and methyl ethyl ketone; ethers such as tetrahydrofuran; and amides (compounds having an amide bond) such as dimethylformamide and N-methylpyrrolidone.

[0073] The resin composition may contain only one type of solvent, or two or more types. When two or more types are contained, the combination and ratio of the solvents can be selected arbitrarily.

[0074] The content of the solvent in the resin composition is not particularly limited and may be appropriately selected depending on, for example, the types of components other than the solvent.

[0075] <Other ingredients> The resin composition and the resin film may or may not contain other components that do not fall under any of the soluble resin (a), the energy ray curable compound (b), the photopolymerization initiator (c), and the solvent.

[0076] The other components contained in the resin composition and the resin film may be one type only, or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0077] Examples of the other components contained in the resin composition and the resin film include an antistatic agent, a tackifier, and silicone oil. The antistatic agent is a component for imparting antistatic properties to the resin film. The tackifier is a component for increasing the adhesive strength of the resin film. The silicone oil is a component for reducing the adhesive strength of the resin film.

[0078] In the resin film, the ratio of the total content of the soluble resin (a), the energy ray curable compound (b), and the photopolymerization initiator (c) to the total mass of the resin film ([total content (parts by mass) of the soluble resin (a), the energy ray curable compound (b), and the photopolymerization initiator (c) in the resin film] / [total mass (parts by mass) of the resin film]×100) is preferably 90 to 100% by mass, and may be, for example, any of 95 to 100% by mass, 97 to 100% by mass, and 99 to 100% by mass. When the ratio is equal to or more than the lower limit, a composite sheet including such a resin film is more preferable in terms of the property that it can be used as either a die bonding sheet or a dicing sheet. When the resin film does not contain the photopolymerization initiator (c), the content of the photopolymerization initiator (c) in the resin film is 0 part by mass.

[0079] <<Other configurations of resin film>> The resin film may be made of one layer (single layer) or may be made of two or more layers. When the resin film is made of multiple layers, these multiple layers may be the same or different from each other, and the combination of these multiple layers is not particularly limited.

[0080] In this specification, not only in the case of a resin film, "multiple layers may be the same or different" means "all layers may be the same, all layers may be different, or only some layers may be the same", and further, "multiple layers are different" means "at least one of the constituent materials and thicknesses of each layer is different from each other".

[0081] In the thickness direction of the resin film, the content of one or two selected from the group consisting of the energy ray curable compound (b), the photopolymerization initiator (c) and the other components may vary (be non-uniform). In this way, when the content of the components in the resin film varies in the thickness direction of the resin film, the content of the components is preferably higher in the region near one or both sides of the resin film than in other regions, and more preferably higher only in the region near one side of the resin film than in other regions. Furthermore, the components whose content varies in the thickness direction of the resin film are preferably the energy ray curable compound (b) and the photopolymerization initiator (c) other than the soluble resin (a). With a smaller content of these components (one or two selected from the group consisting of the energy ray curable compound (b), the photopolymerization initiator (c) and the other components), such a resin film can be imparted with the property that it can be used as either a die bonding sheet or a sheet for forming a protective film, or a dicing sheet, for the composite sheet described below.

[0082] The thickness of the resin film can be appropriately adjusted depending on the purpose. The thickness of the resin film is preferably 3 to 200 μm, more preferably 5 to 150 μm, and even more preferably 10 to 120 μm. When the thickness of the resin film is equal to or more than the lower limit, the strength of the resin film is increased. When the thickness of the resin film is equal to or less than the upper limit, the thickness of the resin film and its cured product can be prevented from becoming excessive. Here, the "thickness of the resin film" means the thickness of the entire resin film. For example, the thickness of a resin film consisting of multiple layers means the total thickness of all layers constituting the resin film.

[0083] In this specification, the term "thickness", not limited to that of resin films, means, unless otherwise specified, a value expressed as the average of thicknesses measured at five randomly selected points on the object, and can be obtained using a constant pressure thickness gauge in accordance with JIS K7130.

[0084] <<Method of manufacturing resin composition>> The resin composition can be obtained by blending the respective components constituting the resin composition. The order of addition of the components when blending is not particularly limited, and two or more components may be added simultaneously. When a solvent is used, the solvent may be used by mixing it with any of the other ingredients to pre-dilute the ingredients, or the solvent may be used by mixing it with any of the other ingredients without pre-diluting the ingredients.

[0085] The method for mixing the components during blending is not particularly limited, and may be appropriately selected from known methods such as a method of mixing by rotating a stirrer or stirring blades, a method of mixing using a mixer, a method of mixing by adding ultrasound, etc. The temperature and time during addition and mixing of each component are not particularly limited as long as the components do not deteriorate, and may be adjusted appropriately. A temperature of 15 to 30°C is preferred.

[0086] ◇Composite sheet A composite sheet according to one embodiment of the present invention includes the resin film according to the above-mentioned one embodiment of the present invention, and a second resin layer provided on one surface of the resin film. The composite sheet of this embodiment includes the resin film, and therefore can be used as either a die bonding sheet or a protective film forming sheet, or a dicing sheet, as described above.

[0087] <<Second resin layer>> The second resin layer functions, for example, as any one of a film-like adhesive, a protective film-forming film, and a pressure-sensitive adhesive layer. Which of these functions it serves is determined by the components contained in the second resin layer and whether or not the resin film laminated with the second resin layer is cured by energy rays.

[0088] <<Composition for second resin layer>> The second resin layer can be formed using a composition for the second resin layer containing the constituent materials thereof. For example, the composition for the second resin layer can be applied to the surface on which the second resin layer is to be formed, and dried as necessary, to form the second resin layer at the desired location. The ratio of the contents of the components that do not vaporize at room temperature in the composition for the second resin layer is usually the same as the ratio of the contents of the components in the second resin layer.

[0089] The composition for the second resin layer can be handled in the same manner as the resin composition described above, and the composition for the second resin layer can be applied and dried in the same manner as the application and drying of the resin composition. Hereinafter, the second resin layer and the components contained in the composition for the second resin layer will be described in detail, taking as an example a case where the second resin layer is a film-like adhesive or pressure-sensitive adhesive layer.

[0090] The second resin layer and the composition for the second resin layer preferably contain a polymer component (A).

[0091] <Polymer component (A)> The polymer component (A) contained in the second resin layer and the composition for the second resin layer may be, for example, a resin that itself has adhesive properties, or a resin that exhibits adhesive properties or bonding properties when used in combination with other components.

[0092] The polymer component (A) contained in the second resin layer and the composition for the second resin layer may be only one type, or may be two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0093] Examples of the polymer component (A) include acrylic resins, aryl resins, urethane resins, and rubbers.

[0094] The acrylic resin is a polymer of one or more kinds of monomers, and examples of the monomers include (meth)acrylic acid esters and monomers other than (meth)acrylic acid esters. Examples of the (meth)acrylic acid ester include (meth)acrylic acid alkyl esters, in which the alkyl group constituting the alkyl ester has 1 to 18 carbon atoms; Examples of such reactive functional group-containing (meth)acrylic acid esters include those in which the alkyl group constituting the alkyl ester in the (meth)acrylic acid alkyl ester has a reactive functional group capable of bonding with other compounds, such as a hydroxyl group, a vinyl group, a (meth)acryloyl group, an amino group, a carboxy group, or an isocyanate group. However, the (meth)acrylic acid esters are not limited to these.

[0095] The acrylic resin having a structural unit derived from the reactive functional group-containing (meth)acrylic acid ester can undergo a crosslinking reaction at the reactive functional group therein by using a crosslinking agent, which will be described later, in combination.

[0096] In this specification, the reactive functional group-containing (meth)acrylic acid ester is given a name corresponding to the name of the reactive functional group. For example, a reactive functional group-containing (meth)acrylic acid ester having a hydroxyl group as a reactive functional group is called a hydroxyl group-containing (meth)acrylic acid ester.

[0097] The weight average molecular weight (Mw) of the polymer component (A) is preferably 10,000 to 2,000,000, and may be, for example, any one of 10,000 to 1,000,000, 1,000,000 to 2,000,000, and 200,000 to 1,200,000. When the weight average molecular weight of the polymer component (A) is within such a range, it becomes easy to adjust the tacky adhesive strength of the second resin layer to a preferred range.

[0098] The second resin layer and the composition for the second resin layer containing the polymer component (A) may or may not contain components other than the polymer component (A), as described later.

[0099] The content of the polymer component (A) in the second resin layer can be appropriately adjusted depending on the application of the second resin layer, the type of the polymer component (A), and the like. In the second resin layer, the ratio of the content of polymer component (A) to the total mass of the second resin layer ([content of polymer component (A) in second resin layer (parts by mass)] / [total mass of second resin layer (parts by mass)]×100) is preferably 15 to 100% by mass, and may be, for example, any one of 40 to 100% by mass, 65 to 100% by mass, and 90 to 100% by mass, any one of 15 to 75% by mass, 15 to 50% by mass, and 15 to 25% by mass, or may be 40 to 75% by mass.

[0100] <Solvent> The second resin layer composition preferably further contains a solvent, which improves the handleability of the second resin layer composition. The solvent contained in the second resin layer composition may be the same as the solvent contained in the resin composition. The solvent contained in the composition for the second resin layer may be only one type, or may be two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0101] The content of the solvent in the composition for the second resin layer is not particularly limited, and may be appropriately selected depending on, for example, the types of components other than the solvent.

[0102] <Other ingredients> The second resin layer and the composition for the second resin layer may or may not contain other components that do not fall under either the polymer component (A) or the solvent. The other components contained in the second resin layer and the composition for the second resin layer may be either a resin component or a non-resin component.

[0103] Examples of the other components include crosslinking agents, energy ray curable resins, energy ray curable compounds, photopolymerization initiators, plasticizers, antistatic agents, thermosetting resins such as epoxy resins and phenolic resins, heat curing agents, curing accelerators, coupling agents, fillers, colorants, etc. However, the other components are not limited to these.

[0104] The other components contained in the second resin layer and the composition for the second resin layer may be one type only, or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0105] For example, the second resin layer containing an epoxy resin as the other component is suitable as a thermosetting film-like adhesive for constituting a die bonding sheet as a composite sheet. As the other components, the second resin layer containing an epoxy resin preferably further contains a heat curing agent having two or more functional groups in one molecule that can react with an epoxy group, and a curing accelerator, and may or may not further contain one or more types selected from the group consisting of a filler, a coupling agent, a crosslinking agent, an energy ray curable resin, a photopolymerization initiator, a colorant, and a general-purpose additive that does not fall into any of the above categories (filler to colorant).

[0106] For example, a second resin layer containing an energy ray-curable compound as the other component is suitable as an energy ray-curable adhesive layer for constituting a dicing sheet as a composite sheet, regardless of whether or not the polymer component (A) is energy ray-curable.

[0107] The content of the other components in the second resin layer can be appropriately adjusted depending on the application of the second resin layer, the type of the other components, etc., and is not particularly limited.

[0108] The second resin layer contains an acrylic resin as the polymer component (A) and does not contain any components other than the polymer component (A) (in other words, consists of the polymer component (A), the same applies below), and is suitable, for example, as a film-like adhesive for forming a die bonding sheet as a composite sheet. The second resin layer contains, as the polymer component (A), an energy ray-curable adhesive resin having a structure in which an acrylic resin having the reactive functional group has reacted with an unsaturated group-containing compound having an energy ray-polymerizable unsaturated group at the reactive functional group, and does not contain any component other than the polymer component (A).The second resin layer is suitable, for example, as an energy ray-curable adhesive layer for constituting a dicing sheet as a composite sheet.

[0109] When the second resin layer is energy ray curable, the resin film and the second resin layer in the composite sheet are simultaneously energy ray cured, whereby the peel force between the energy ray cured product of the resin film and the energy ray cured product of the second resin layer is increased, and the adhesion between these cured products is increased. Such a composite sheet in which the second resin layer is also energy ray curable is particularly suitable as a dicing sheet.

[0110] In addition, the composite sheet usable as a dicing sheet can also be used as an adhesive sheet for adhering and fixing any member used in the field, such as adhering a hard support in a hard support process in the manufacturing process of a semiconductor device, instead of a dicing sheet. When such an adhesive sheet is used, unlike when a liquid adhesive is used, the adhesive force in the surface direction of the adhesive area is highly uniform, and therefore the adhesive strength is advantageously stabilized.

[0111] <Other configurations of the second resin layer> The second resin layer may be one layer (single layer) or may be two or more layers. When the second resin layer is made of multiple layers, these multiple layers may be the same or different from each other, and the combination of these multiple layers is not particularly limited.

[0112] The thickness of the second resin layer can be adjusted appropriately depending on the purpose. The thickness of the second resin layer is preferably 1 to 50 μm, more preferably 3 to 40 μm, and particularly preferably 5 to 30 μm. When the thickness of the second resin layer is equal to or greater than the lower limit, the strength of the second resin layer is increased. When the thickness of the second resin layer is equal to or less than the upper limit, the thickness of the second resin layer is prevented from becoming excessive. Here, "the thickness of the second resin layer" means the thickness of the entire second resin layer, and for example, the thickness of a second resin layer consisting of multiple layers means the total thickness of all layers that make up the second resin layer.

[0113] <<Other layers>> The composite sheet of the present embodiment may include another layer that does not fall under either the resin film or the second resin layer, so long as the effect of the present invention is not impaired. The type and number of the other layers, as well as the arrangement positions of the other layers in the composite sheet, can be arbitrarily selected depending on the purpose, and are not particularly limited. The other layer may be one layer (single layer) or two or more layers. When the other layer is a multi-layer structure, the multi-layer structure may be the same or different from each other, and the combination of the multi-layer structure is not particularly limited.

[0114] An example of the other layer is another resin film that is provided on the surface of the resin film opposite to the second resin layer side and contains a soluble resin (a). For example, when the other resin film does not contain the energy ray curable compound (b) or the content of the energy ray curable compound (b) in the other resin film is less than the content of the energy ray curable compound (b) in the resin film, the laminated film which is a laminate of the resin film and the other resin film is equivalent to a single layer film in which the content of the soluble resin (a) and the energy ray curable compound (b) varies in the thickness direction of these two layers (resin film, other resin film). And when the interface between these two layers cannot be recognized, it is the same as the resin film described above in which the content of the soluble resin (a) and the energy ray curable compound (b) varies (is non-uniform) in the thickness direction of the resin film.

[0115] Here, the energy ray curable compound (b) is taken as an example for explanation, but the same applies to the photopolymerization initiator (c) and the other components. That is, when the other resin film does not contain one or more selected from the group consisting of the energy ray curable compound (b), the photopolymerization initiator (c), and the other components, or when the content of one or more selected from the group consisting of the energy ray curable compound (b), the photopolymerization initiator (c), and the other components in the other resin film is less than the content of the component in the resin film, it is equivalent to a monolayer film in which the content of the component varies in the thickness direction in these two layers (resin film, other resin film). And, it is preferable that the other resin film does not contain any of the energy ray curable compound (b), the photopolymerization initiator (c), and the other components, or when the content of all of the energy ray curable compound (b), the photopolymerization initiator (c), and the other components in the other resin film is less than the content of these components in the resin film. In this way, a composite sheet in which the content of one or more components selected from the group consisting of the energy ray curable compound (b), the photopolymerization initiator (c), and the other components in the other resin film is lower than the content of these components in the resin film has the advantage, as explained above, that it can be used as either a die bonding sheet or a dicing sheet with a lower content of these components (one or two components selected from the group consisting of the energy ray curable compound (b), the photopolymerization initiator (c), and the other components).

[0116] The other layer can be formed by a known method. For example, the other resin film can be formed by the same method as the resin film, except that a composition for forming the other resin film is used that is different from the resin composition for forming the resin film.

[0117] <<Peel force P between the resin film and the second resin layer 11 >> When measuring the peel force P1, the resin film is peeled from the second resin layer in the composite sheet of this embodiment in the same manner as the resin film is peeled from the acrylic resin film. 11 (In this specification, the term "pre-curing peel strength P 11 ") may be the same as the peel force P1. That is, the peel strength before curing P 11 is preferably 100 mN / 25 mm or less, more preferably 50 mN / 25 mm or less, and even more preferably 30 mN / 25 mm or less. 11 By being equal to or less than the upper limit, the peel force between the resin film and the second resin layer becomes smaller within an appropriate range, and a composite sheet having such a resin film is suitable as a die bonding sheet or a sheet for forming a protective film. On the other hand, P 11 The lower limit of is not particularly limited. For example, P 11 Resin films with a strength of 8 mN / 25 mm or more can be manufactured more easily. In one embodiment, P11 may be, for example, any one of 8 to 100 mN / 25 mm, 8 to 50 mN / 25 mm, and 8 to 30 mN / 25 mm. 11 This is an example.

[0118] <<Peel strength P between the UV-cured resin film and the second resin layer 21 >> When measuring the peel force P2, the peel force P2 is measured by the same method as the method for peeling the ultraviolet-cured resin film from the acrylic resin film in the composite sheet of this embodiment. 21 (In this specification, the term "post-curing peel strength P 21 ") may be the same as the peel force P2. That is, the peel strength after curing P 21 is preferably 3500 mN / 25 mm or more, more preferably 4500 mN / 25 mm or more, and even more preferably 5500 mN / 25 mm or more. 21 When the peel strength between the energy ray-cured resin film and the second resin layer is greater, a composite sheet including such a resin film is suitable as a dicing sheet. On the other hand, P 21 The upper limit of is not particularly limited. For example, 21 Resin films with a strength of 10,000 mN / 25 mm or less can be produced more easily. In one embodiment, P 21 may be, for example, any one of 3500 to 10000 mN / 25 mm, 4500 to 10000 mN / 25 mm, and 5500 to 10000 mN / 25 mm. 21 This is an example.

[0119] <<Ratio of peel strength of resin film after curing in composite sheet>> Peeling force before curing P 11 and peel force P after curing 21 Using the following formula (P01): P21 / P 11 ×100 (P01) The post-curing ratio of the peel strength of the resin film in the composite sheet calculated by (sometimes referred to in this specification as the "post-curing ratio of the peel strength" or simply as the "post-curing ratio") may be the same as the post-curing ratio of the peel strength calculated by the formula (P0). That is, the post-curing ratio of the peel strength of the composite sheet is preferably 15000% or more, more preferably 25000% or more, and even more preferably 35000% or more. The higher the post-curing ratio of the peel strength of the composite sheet, the higher the pre-curing peel strength P 11 The peel strength P of the UV-cured resin film after curing 21 The ratio of is large, and the resin film has a large variation in peel strength before and after energy ray curing. A composite sheet having such a resin film is more preferable in terms of its characteristic that it can be used as either a die bonding sheet or a sheet for forming a protective film, or a dicing sheet. On the other hand, there is no particular upper limit to the post-curing ratio of the peel strength in the composite sheet. For example, a resin film having a post-curing ratio of the peel strength of 100,000% or less can be produced more easily. In one embodiment, the post-curing ratio of the peel strength in the composite sheet may be, for example, any one of 15000 to 100000%, 25000 to 100000%, and 35000 to 100000%, although these are merely examples of the post-curing ratio of the peel strength.

[0120] <<Manufacturing method of composite sheet>> The composite sheet of the present embodiment can be manufactured by laminating the above-mentioned layers so that they are in a corresponding positional relationship, and adjusting the shapes of some or all of the layers as necessary. The method of forming each layer is as described above.

[0121] For example, the resin composition is applied onto a release film and dried as necessary to form the resin film on the release film. Separately, a composition for the second resin layer is applied onto the release film and dried as necessary to form a second resin layer on the release film. Then, the exposed surface of the resin film (the surface opposite to the release film side) and the exposed surface of the second resin layer (the surface opposite to the release film side) are bonded together to laminate the resin film and the second resin layer, thereby producing a composite sheet. The release film provided on the resin film and the release film provided on the second resin layer can be peeled off at any stage before the composite sheet is used.

[0122] The resin film and the second resin layer are preferably attached to each other while heating at a temperature of 35 to 45°C.

[0123] When manufacturing a composite sheet having the other layer, for example, the other layer may be formed in advance by a method appropriate for the type of the other layer, and then the other layer may be laminated on any of the layers constituting the composite sheet at any appropriate timing in the above-mentioned method so that the other layer is appropriately positioned in the composite sheet.

[0124] <<An example of a composite sheet>> FIG. 1 is a cross-sectional view that illustrates an example of the composite sheet of the present embodiment together with an example of a resin film. In addition, the figures used in the following explanation may show key parts enlarged for convenience in order to make the features of the present invention easier to understand, and the dimensional ratios of each component may not necessarily be the same as the actual ones.

[0125] The composite sheet 1 shown here is composed of a resin film 11 and a second resin layer 12 provided on one side 11a of the resin film 11 (sometimes referred to as the "first side" in this specification). The composite sheet 1 further includes a release film 13 provided on a surface 12a of the second resin layer 12 opposite to the resin film 11 side (sometimes referred to as the "first surface" in this specification). The release film 13 has an optional configuration, and the composite sheet 1 may or may not include the release film 13. The release film 13 may be a known film. As explained above, the release film 13 may be the release film used when the composite sheet 1 is manufactured (more specifically, when the second resin layer 12 is formed).

[0126] The resin film 11 contains a soluble resin (a) and an energy ray-curable compound (b).

[0127] FIG. 2 is a cross-sectional view for illustrating a typical method of using the composite sheet 1. As shown in FIG. In FIG. 2, the same components as those shown in FIG. 1 are denoted by the same reference numerals as in FIG. 1, and detailed description thereof will be omitted.

[0128] When using the composite sheet 1, the release film 13 is peeled off from the second resin layer 12, and the first surface 12a of the second resin layer 12 newly exposed thereby is attached to one surface 9a of an object 9 to which the composite sheet 1 is to be attached (hereinafter, may be simply referred to as "object to be attached"). In this way, the composite sheet 1 is attached to the object 9 to which the composite sheet 1 is to be attached.

[0129] Next, when the composite sheet 1, more specifically the resin film 11, is irradiated with energy rays to turn the resin film 11 into an energy ray-cured product 11' of the resin film and turn the composite sheet 1 into a cured composite sheet 1', the peel force (post-curing peel force) between the energy ray-cured product 11' of the resin film and the second resin layer 12 becomes significantly greater than the peel force (pre-curing peel force) between the resin film 11 and the second resin layer 12 in the composite sheet 1. Then, when an operation is performed to peel the energy ray-cured product 11' of the resin film from the object 9 to which it is to be attached, the energy ray-cured product 11' of the resin film does not peel from the second resin layer 12 but remains integral with the second resin layer 12, and the cured composite sheet 1' peels from the object 9 to which it is to be attached. That is, in this case, the second resin layer 12 is suitable as a pressure-sensitive adhesive layer, and the composite sheet 1 is suitable as a dicing sheet.

[0130] In contrast, when the composite sheet 1, more specifically the resin film 11, is not irradiated with energy rays and is left unirradiated, the peel force (pre-curing peel force) between the resin film 11 and the second resin layer 12 remains small within an appropriate range. When the resin film 11 is peeled off from the object 9, the second resin layer 12 remains integral with the object 9, and the resin film 11 peels off from the second resin layer 12. That is, in this case, the second resin layer 12 is suitable as a film-like adhesive, and the composite sheet 1 is suitable as a die-bonding sheet.

[0131] The composite sheet of the present embodiment has an advantageous effect in that only a portion of the resin film therein is cured by energy rays, so that the composite sheet has both areas that remain as resin film and areas that are energy ray-cured of the resin film.

[0132] For example, when a wafer with a film-like adhesive, which includes a wafer and a film-like adhesive provided on the back surface of the wafer, is diced with a blade on a dicing sheet to produce a chip with a film-like adhesive provided on the back surface of the chip, chip pieces that do not have the desired shape and are formed in an area corresponding to the vicinity of the outer periphery of the wafer may peel off from the dicing sheet and scatter during or after dicing. In addition, the film-like adhesive protruding from the outer periphery of the wafer may be cut, and the resulting adhesive pieces may scatter during or after dicing. These scattered chip pieces or adhesive pieces may adhere to the inside of the device or the target chip with the film-like adhesive, thereby contaminating them. In response to this, by using the composite sheet of this embodiment and curing the region of the resin film therein where the vicinity of the outer periphery of the wafer is located (the region that overlaps with the vicinity of the outer periphery of the wafer in a planar view) with energy rays, the peel force (post-curing peel force) between the energy ray-cured resin film and the second resin layer in this region can be increased, thereby preventing the above-mentioned chip pieces or adhesive pieces from scattering, while in the region where the resin film has not been energy ray-cured, dicing and subsequent chip pick-up can be performed normally.

[0133] Also, for example, a method is known for manufacturing chips with a film-like adhesive by using a dicing sheet to which a large number of aligned chips with a film-like adhesive are attached, and expanding the sheet in a direction parallel to the surface at a low temperature to cut the film-like adhesive along the periphery of the chip. In this method, unintended cutting of the film-like adhesive is usually likely to occur, particularly near the periphery, and the resulting adhesive fragments may scatter and adhere to the inside of the device or the intended chips with the film-like adhesive, thereby contaminating them. In response to this problem, by using the composite sheet of this embodiment and curing the vicinity of the outer periphery of the resin film therein with energy rays, scattering of adhesive fragments can be suppressed in the same manner as described above.

[0134] On the other hand, some dicing sheets or die bonding sheets are so-called precut, that is, cut in advance on a release film so that the shape and size of the sheet match the shape and size of the wafer to be attached. However, when precutting is performed, the process becomes complicated, and the obtained dicing sheet or die bonding sheet tends to be expensive. In response to this, the resin film of this embodiment is formed on a release film, and cuts are formed in the resin film so that a region of the desired shape and size is formed. The resin film is then bonded to the second resin layer in a dicing sheet prepared separately, to produce a composite sheet of this embodiment with a release film. Using such a composite sheet, the resin film in the non-target region (region not of the desired shape and size) that is not to be attached to the wafer is cured with energy rays, and the peel force (post-curing peel force) between the energy-ray cured product of the resin film and the second resin layer in this region is increased, and the non-target region is peeled off from the release film as a whole. As a result, not only the non-target region but also the layer corresponding to the dicing sheet including the second resin layer in the region where the resin film is not cured with energy rays is peeled off from the release film as a whole. As a result, only the resin film that has been cut in advance to fit the shape and size of the wafer to be attached remains on the release film, and a sheet similar to a pre-cut dicing sheet or die bonding sheet can be produced without pre-cutting.

[0135] On the other hand, some conventional dicing die bonding sheets have a laminate of a substrate and an adhesive layer as a dicing sheet, and a film-like adhesive is provided on the surface of the adhesive layer opposite to the substrate. In such a dicing die bonding sheet, the adhesive layer in the region having the chip is cured with energy rays to reduce the adhesive force to the film-like adhesive, thereby making it possible to pick up the chip with the film-like adhesive from the laminate after energy ray curing. Some conventional dicing die bonding sheets further have an intermediate release layer between the adhesive layer and the film-like adhesive. In such a dicing die bonding sheet, even if the adhesive force of the adhesive layer is not sufficiently reduced, the adhesive force of the intermediate release layer to the film-like adhesive is small, making it possible to pick up the chip with the film-like adhesive from the laminate of the substrate, the adhesive layer, and the intermediate release layer. However, the shape and size of the intermediate release layer must be cut in advance to fit the shape and size of the wafer to be attached, just like the film-like adhesive, and a dicing die bonding sheet with such an intermediate release layer is likely to be expensive. In contrast, by using the composite sheet of this embodiment and curing the area of ​​the resin film in the vicinity of the outer periphery that does not have a chip with energy rays, thereby increasing the peel force (post-curing peel force) between the energy ray-cured resin film and the second resin layer in this area, and then performing an operation to separate the chip with the film-like adhesive from the dicing sheet in the area of ​​the resin film that has not been energy ray-cured, the chip with the film-like adhesive can be picked up normally even without an intermediate release layer.

[0136] Up to this point, the process of dividing a wafer into chips has been used as an example to explain the process, but the composite sheet of this embodiment is not limited to this and can be applied to all processes of dividing a workpiece into workpieces. In that case, even if the workpiece is something other than a wafer, it will have the same effect as dividing a wafer into chips.

[0137] ◇ Manufacturing method of workpiece In a method for manufacturing a workpiece according to an embodiment of the present invention, the workpiece is obtained by processing a workpiece, The manufacturing method includes a bonding step of bonding a surface of the second resin layer in the composite sheet according to one embodiment of the present invention opposite to the resin film side to one surface of the workpiece, thereby producing a workpiece with a composite sheet, Further, after the attaching step, a peeling step (I) of peeling the resin film from the second resin layer in the workpiece with the composite sheet, and after the peeling step (I), a processing step (I) of processing the workpiece with the second resin layer to produce the workpiece, or The method includes a hardening step (II) following the attaching step, in which the resin film in the composite sheet is hardened with energy rays to produce a workpiece with a hardened composite sheet, in which the composite sheet in the workpiece with the composite sheet becomes a hardened composite sheet, a processing step (II) following the hardening step (II) in which the workpiece in the workpiece with the hardened composite sheet is processed to produce the workpiece, and a pick-up step (II) following the processing step (II) in which the workpiece is separated from the second resin layer in the hardened composite sheet and picked up.

[0138] In the manufacturing method for a workpiece having the peeling step (I) and the processing step (I) (sometimes referred to in this specification as manufacturing method (I)), the resin film functions as a film-like adhesive, and the composite sheet functions as a die bonding sheet. In the manufacturing method for a workpiece (sometimes referred to as manufacturing method (II) in this specification) having the curing step (II), the processing step (II), and the pick-up step (II), the resin film functions as an adhesive layer, and the composite sheet functions as a dicing sheet.

[0139] The production method (I) and the production method (II) share the bonding step.

[0140] In this embodiment, the workpiece may be, for example, a wafer, a semiconductor device panel, or the like.

[0141] Examples of the wafer include semiconductor wafers made of elemental semiconductors such as silicon, germanium, and selenium, and compound semiconductors such as GaAs, GaP, InP, CdTe, ZnSe, and SiC; and insulating wafers made of insulators such as sapphire and glass. A circuit is formed on one surface of the workpiece, typically a wafer, and the surface opposite to the circuit surface is the back surface. The wafer is divided into chips by dicing or other means. The surface of the chip on which the circuit is formed is also called the circuit surface, and the surface of the chip opposite to the circuit surface is also called the back surface. It is preferable that the circuit surface of each workpiece is provided with protruding electrodes such as bumps, pillars, etc. The protruding electrodes are preferably made of solder.

[0142] The semiconductor device panel is handled during the manufacturing process of a semiconductor device, and a specific example thereof is a configuration in which a semiconductor device in which one or more electronic components are sealed with sealing resin is used, and multiple such semiconductor devices are arranged in a planar manner within an area of ​​a circular, rectangular, or other shape.

[0143] In this embodiment, the workpiece is obtained by processing the workpiece. For example, if the workpiece is a wafer, the workpiece may be a chip, and if the workpiece is a semiconductor wafer, the workpiece may be a semiconductor chip.

[0144] <<Manufacturing method (I)>> The attachment step in the production method (I) can be carried out by a known method. By the manufacturing method (I), for example, as shown in FIG. 2, a workpiece with a composite sheet is obtained, which includes a workpiece (corresponding to the object to be affixed 9) and a composite sheet (corresponding to the composite sheet 1) provided on one side of the workpiece, and the surface (corresponding to the first surface 12a of the second resin layer 12) of the composite sheet opposite to the resin film (corresponding to the resin film 11) side of the second resin layer (corresponding to the second resin layer 12) is bonded to one side of the workpiece.

[0145] The peeling step (I) of the production method (I) can be carried out by a known method. The resin film is peeled off from the second resin layer without irradiating the composite sheet (more specifically, the resin film) with energy rays. By the peeling process (I), for example, as shown in FIG. 2, a workpiece with a second resin layer is obtained, which comprises an object to be affixed 9 having a second resin layer 12 but no resin film 11, the object to be affixed comprising a workpiece (corresponding to the object to be affixed 9) and a second resin layer (corresponding to the second resin layer 12) provided on one side of the workpiece, and no resin film (corresponding to the resin film 11).

[0146] The processing step (I) of the production method (I) can be carried out by a known method. For example, when the work is a semiconductor wafer and semiconductor chips are produced by dicing the work, the work can be processed by various dicing methods such as blade dicing using a blade, laser dicing by irradiating laser light, or water dicing by spraying water containing an abrasive. At this time, the second resin layer can also be cut at the same time. As a result, a workpiece with a second resin layer (an example of which is a semiconductor chip with a second resin layer) is obtained, which includes a workpiece (corresponding to the processed workpiece 9 to be attached, an example of which is a semiconductor chip) and a second resin layer (corresponding to the second resin layer 12 after cutting) provided on one side of the workpiece. The workpiece with a second resin layer corresponds to, for example, the workpiece 9 to be attached having the second resin layer 12 shown in FIG. 2, which is processed by cutting the second resin layer 12.

[0147] The workpiece with the second resin layer obtained by the manufacturing method (I) is then mounted on the circuit surface of a substrate to manufacture a target product such as a semiconductor device.

[0148] <<Manufacturing method (II)>> The attachment step in the production method (II) is the same as the attachment step in the production method (I).

[0149] The curing step (II) of the production method (II) can be carried out by a known method. For example, when irradiating a composite sheet (resin film) with energy rays, the illuminance of the energy rays is 60 to 320 mW / cm 2 The light amount of the energy beam may be 100 to 1000 mJ / cm 2 It may be. The curing step (II) provides a workpiece with a cured composite sheet, which includes a workpiece (corresponding to the attachment object 9) and a cured composite sheet (corresponding to the cured composite sheet 1') provided on one side of the workpiece, and the surface (corresponding to the first surface 12a of the second resin layer 12) of the second resin layer (corresponding to the second resin layer 12) opposite to the energy ray cured product of the resin film (corresponding to the energy ray cured product of the resin film 11') is bonded to one side of the workpiece. The workpiece with a cured composite sheet corresponds to, for example, the composite sheet 1 attached to the attachment object 9 has become the cured composite sheet 1' (the resin film 11 has become the energy ray cured product 11') as shown in FIG. 2.

[0150] The processing step (II) of the production method (II) can be carried out by a known method, for example, by the same method as in the processing step (I) of the production method (I). By the processing step (II), a workpiece with a second resin layer (an example of which is a semiconductor chip with a second resin layer) is obtained, which includes a workpiece (corresponding to the workpiece of the attachment object 9, an example of which is a semiconductor chip) and a second resin layer (corresponding to the second resin layer 12) provided on one surface of the workpiece. The workpiece with a second resin layer obtained here differs from the case of the processing step (I) in that the second resin layer does not need to be cut. The laminate of the energy ray cured product of the resin film and the workpiece with the second resin layer obtained here corresponds to, for example, the laminate of the composite sheet 1 and the attachment object 9 (the laminate of the resin film 11, the second resin layer 12, and the attachment object 9) shown in FIG. 2, in which the composite sheet 1 becomes the cured composite sheet 1' (the resin film 11 becomes the energy ray cured product of the resin film 11') and the attachment object 9 becomes the processed product.

[0151] The pick-up step (II) of the production method (II) can be carried out by a known method. By the pick-up step (II), for example, in place of the object 9 to be attached which has been peeled off from the cured composite sheet 1' as shown in FIG. 2, a processed product of the object 9 to be attached is obtained.

[0152] The manufacturing method (II) may further include, after the curing step (II) and before the processing step (II), a peeling step (III) of peeling the cured composite sheet from the workpiece in the workpiece with the cured composite sheet, and a re-attaching step (II) of producing a workpiece with the cured composite sheet by re-attaching, after the peeling step (III), the surface of the second resin layer in the peeled cured composite sheet opposite to the energy ray cured product side of the resin film to one surface of the workpiece. If there is a defect in the attachment of the composite sheet in the workpiece with the composite sheet obtained in the attachment step, the above defect can be eliminated by performing the peeling step (III) and the re-attaching step (II) after the curing step (II).

[0153] The peeling step (III) of the production method (II) can be carried out by a known method. The peeling process (III) produces a cured composite sheet (corresponding to the hardened composite sheet 1') peeled from the workpiece (corresponding to the object 9 to be attached), for example, as shown in FIG. 2, as a cured composite sheet 1' peeled from the object 9 to be attached.

[0154] The reattaching step (II) of the production method (II) can be carried out by a known method. The re-attaching step (II) can be carried out, for example, in the same manner as in the attaching step. EXAMPLES

[0155] The present invention will be described in more detail below with reference to specific examples, although the present invention is not limited to the examples shown below.

[0156] <Components of resin film> The components contained in the resin films used in the present examples and comparative examples are shown below. Soluble resin (a)-1: ethylene-vinyl acetate copolymer (EVA), "Ultrathene 684" manufactured by Tosoh Corporation, vinyl acetate content 20% by mass, weight average molecular weight 55,000; 20 g can be dissolved in 100 g of toluene at a temperature of 23°C. Energy ray curable compound (b)-1: Tricyclodecane dimethylol diacrylate, "KAYARAD R-684" manufactured by Nippon Kayaku Co., Ltd., molecular weight 304.4 Photopolymerization initiator (c)-1: 1-hydroxycyclohexyl phenyl ketone, BASF "Irgacure 184"

[0157] <Components contained in the second resin layer> The components contained in the second resin layer used in the present examples and comparative examples are shown below. Polymer component (A)-1: An acrylic resin (weight average molecular weight 370,000, glass transition temperature 6° C.) obtained by copolymerizing methyl acrylate (85 parts by mass) and 2-hydroxyethyl acrylate (15 parts by mass).

[0158] [Example 1] <<Production of resin film>> <Production of Resin Composition> Soluble resin (a)-1 (70 parts by mass), energy ray curable compound (b)-1 (28 parts by mass) and photopolymerization initiator (c)-1 (2 parts by mass) were dissolved in toluene and stirred at 23° C. to produce an energy ray curable resin composition having a total concentration of 15% by mass of all components other than the solvent. Note that the amounts of all components other than toluene shown here are the amounts of the target product not including the solvent.

[0159] <Production of resin film> A release film (second release film, "SP-PET502150" manufactured by Lintec Corporation, thickness 50 μm) made of polyethylene terephthalate film, one side of which had been subjected to a release treatment by silicone treatment, was used. The resin composition obtained above was coated on the release-treated surface, dried at 100°C for 5 minutes, and this coating and drying process was then repeated once more to produce an energy ray-curable resin film having a thickness of 80 μm. Furthermore, a release-treated surface of a separate release film (first release film, "SP-PET381031" manufactured by Lintec Corporation, thickness 38 μm) was bonded to the exposed surface of the obtained resin film that did not have the second release film, thereby producing a resin film with a release film comprising a resin film, a first release film provided on one surface of the resin film, and a second release film provided on the other surface of the resin film.

[0160] <<Manufacturing of composite sheets>> A coating liquid containing polymer component (A)-1 and ethyl acetate as a solvent and having a solid content concentration of 35% by mass was prepared. The coating liquid was applied to the release-treated surface of the second release film and dried at 100° C. for 5 minutes to form a second resin layer having a thickness of 20 μm. The first release film was removed from the resin film with a release film obtained above. The exposed surface of the resin film that had the first release film was bonded to the exposed surface of the second resin layer to produce a composite sheet with a release film. The bonding was performed by heating the resin film and the second resin layer to 40°C. This composite sheet is configured by laminating the resin film (thickness 80 μm) and the second resin layer (thickness 20 μm) in the thickness direction.

[0161] <<Evaluation of resin film>> <Measurement of probe tack value T1 before curing> A piece having a diameter of 10 mm was cut out from the resin film obtained above, and the first release film and the second release film were peeled off to obtain a test piece (s21). Using a probe tack tester (TE-6001 manufactured by Tester Sangyo Co., Ltd.), the probe tack value was measured for one surface of the test piece (s21) at a temperature of 23°C, and the maximum value was calculated. The conditions for measuring the probe tack value at this time were as follows. That is, a stainless steel probe having a diameter of 5 mm was used as the probe, and a tack strength of 9.80665 N / cm was applied to the test piece (s21). 2(1000gf / cm 2 The load of s21 was applied for 1 second. The speed at which the probe was peeled off from the test piece (s21) was 10 mm / sec. Such a probe tack value measurement was performed at 10 different points on the test piece (s21), and the minimum value among the 10 maximum values ​​obtained was adopted as the probe tack value T1 before curing of the resin film. The results are shown in Table 1.

[0162] <Measurement of probe tack value T2 after curing> Separately, the test piece (s21) was prepared, and this test piece (s21) was irradiated with an ultraviolet ray irradiation device equipped with a high-pressure mercury lamp ("RAD-2000 m / 12" manufactured by Lintec Corporation) at an illuminance of 230 mW / cm in air. 2 , light intensity 190mJ / cm 2 The test piece (s21) was cured by irradiating ultraviolet rays under the above conditions to obtain a test piece (s22). For this test piece (s22), the probe tack value T2 after curing of the resin film was determined in the same manner as for the above test piece (s21). The results are shown in Table 1.

[0163] <Calculation of Probe Tack Value After Curing> Using the above-obtained probe tack value T1 before curing and the above-obtained probe tack value T2 after curing, the post-curing ratio of the resin film to the probe tack value was calculated according to the above formula (T0). The results are shown in Table 1.

[0164] <Measurement of gel fraction G1 before curing> The resin film obtained above was cut into a size of 50 mm x 100 mm to prepare a sample (s310), and the sample (s310) was wrapped in a nylon mesh sheet (mesh size 200) with a size of 100 mm x 150 mm and stapled to prepare a test piece (s31). The mass M of the test piece (s31) was measured using a precision balance. 11 The mass of the nylon mesh sheet, M2, and the mass of the staples, M3, were weighed. Next, the test piece (s31) was immersed in toluene (500 mL) at 25°C for 24 hours, and then the insoluble matter of the sample (s310), the nylon mesh sheet, and the staples were all removed and dried at 90°C for 3 hours, and then left to stand for 1 hour under conditions of 23°C and a relative humidity of 50% to condition the humidity. Next, the mass M of the test piece (s31) after immersion and drying 51 (That is, the total mass of the insoluble matter of the sample (s310), the mass of the nylon mesh sheet, and the mass of the staples) was weighed using a precision balance. Then, the gel fraction G1 before curing of the resin film was calculated using the above formula G(01). The results are shown in Table 1.

[0165] <Measurement of gel fraction G2 after curing> The resin film obtained above was exposed to ultraviolet light at an illuminance of 230 mW / cm under air using an ultraviolet irradiator equipped with a high-pressure mercury lamp ("RAD-2000 m / 12" manufactured by Lintec Corporation). 2 , light intensity 190mJ / cm 2 The sample was irradiated with ultraviolet light under the following conditions. Next, a sample (s320) measuring 50 mm × 100 mm was prepared using the resin film after ultraviolet irradiation (ultraviolet-cured resin film), and a test piece (s32) was prepared in the same manner as in the case of the resin film not irradiated with ultraviolet rays, and its mass M 12 , and the mass M of the test piece (s32) after immersion, drying and humidity conditioning 52 The gel fraction G2 of the resin film after curing was calculated by the above-mentioned formula G(02). The results are shown in Table 1.

[0166] <Calculation of gel fraction after curing> Using the gel fraction G1 before curing and the gel fraction G2 after curing of the resin film obtained above, the gel fraction of the resin film after curing was calculated according to the above formula (G0). The results are shown in Table 1.

[0167] <<Evaluation of composite sheets>> <Measurement of peel strength P1 before curing> A piece having a width of 25 mm and a length of 250 mm was cut out from the composite sheet obtained above and used as the test piece (s11). The entire exposed surface of the second resin layer in the test piece (s11) was attached to the surface of a hard support made of polymethylmethacrylate via a double-sided tape. That is, the hard support, the double-sided tape, the second resin layer, and the resin film were stacked in this order. Furthermore, in an environment of a temperature of 23°C and a relative humidity of 50%, a 2 kg rubber roller was rolled back and forth once on the upper surface of the stack on the side of the test piece (s11), i.e., on the exposed surface of the resin film, to sufficiently attach the test piece (s11) to the hard support via the double-sided tape. Next, this laminate of the hard support, the double-sided tape and the test piece (s11) was allowed to stand for 30 minutes in an environment at a temperature of 23° C. and a relative humidity of 50%. Next, the resin film was peeled off from the second resin layer in the test piece (s11) of the laminate after standing still using a tensile tester (Imada's universal tensile tester "Tensilon"). At this time, the peeling speed was set to 300 mm / min, and the resin film was peeled off from the second resin layer so that the surfaces of the resin film and the second resin layer that had been in contact with each other formed an angle of 180° (180° peeling was performed). Then, the average value of the peeling force measured from when the length of the peeled part of the resin film exceeded 30 mm until the peeling was completed was calculated, and this average value was adopted as the peeling force P1 of the resin film before curing. The results are shown in Table 1.

[0168] <Measurement of peel strength P2 after curing> Separately, the test piece (s11) was prepared, and this test piece (s11) was irradiated with an ultraviolet ray at an illuminance of 230 mW / cm in air using an ultraviolet ray irradiation device equipped with a high-pressure mercury lamp ("RAD-2000 m / 12" manufactured by Lintec Corporation). 2 , light intensity 190mJ / cm 2 The test piece (s11) was cured by irradiating ultraviolet rays under the above conditions to obtain a test piece (s12). Using this test piece (s12), the peel strength was measured in the same manner as in the case of the above test piece (s11), and the peel strength P2 after curing of the resin film was calculated. The results are shown in Table 1.

[0169] The peel strength P1 before curing obtained here is the peel strength P 11 Also corresponds to the peel strength P2 after curing, and the peel strength P 21 This also applies to the other examples and comparative examples described below.

[0170] <Calculation of peel strength after curing> The peel strength P1 before curing and the peel strength P2 after curing of the resin film obtained above were used to calculate the post-curing ratio of the peel strength of the resin film according to the above formula (P0). The results are shown in Table 1.

[0171] <Evaluation of suitability as a die bonding sheet> [Manufacturing of composite sheets] A second resin layer having a thickness of 30 μm was formed in the same manner as above, except that the coating amount of the coating liquid containing polymer component (A)-1 and ethyl acetate was increased. A composite sheet with a release film was produced in the same manner as above, except for using this second resin layer. That is, this composite sheet was constructed by laminating a resin film (thickness 80 μm) and a second resin layer (thickness 30 μm) in the thickness direction.

[0172] [Manufacturing of hardened composite sheets] Separately, a composite sheet similar to the above was produced. Next, the specimen was exposed to ultraviolet light at an illuminance of 230 mW / cm under air using an ultraviolet irradiator equipped with a high-pressure mercury lamp ("RAD-2000 m / 12" manufactured by Lintec Corporation). 2 , light intensity 190mJ / cm 2 The resin film was cured by irradiating the resin film side of the composite sheet with ultraviolet light under the conditions of 1. As a result, a cured composite sheet was obtained in which the resin film was cured with ultraviolet light (thickness: 80 μm) and the second resin layer (thickness: 30 μm) were laminated in the thickness direction.

[0173] [Evaluation of the suitability of composite sheets] An 8-inch silicon wafer (thickness 350 μm) with one surface polished to #2000 was prepared. Using a bonding device ("RAD-2500 m / 12" manufactured by Lintec Corporation), the second resin layer in the composite sheet obtained above was bonded to the #2000 polished surface (polished surface) of the silicon wafer. The bonding was performed under a temperature condition of 23° C. The composite sheet used had a surface that was larger than the polished surface of the silicon wafer to be bonded to the silicon wafer, and the surface of the composite sheet was bonded to the entire surface of the polished surface of the silicon wafer. That is, in the obtained laminate of the silicon wafer and the composite sheet, the composite sheet was allowed to protrude from the silicon wafer. Next, this laminate of the silicon wafer and the composite sheet was left to stand for 20 minutes in an environment at a temperature of 23° C. and a relative humidity of 50%.

[0174] Next, in the laminate after standing, a cut was made in the composite sheet from the second resin layer side along the outer periphery of the silicon wafer, and a cut was also made in the resin film, but the resin film was not cut across its entire thickness. Next, the resin film was peeled off by hand from the second resin layer in the composite sheet in an environment of 23°C temperature and 50% relative humidity. At this time, the resin film was peeled off from the second resin layer so that the surfaces of the resin film and the second resin layer that had been in contact with each other formed an angle of 180° (180° peeling was performed). Then, after peeling off the resin film, the presence or absence of the second resin layer remaining on the polished surface of the silicon wafer was confirmed. If the adhesive strength of the second resin layer to the polished surface of the silicon wafer is sufficiently large, the second resin layer attached to the polished surface of the silicon wafer will not peel off together with the resin film, but if the adhesive strength of the second resin layer to the polished surface of the silicon wafer is insufficient, the second resin layer attached to a partial area or the entire area of ​​the polished surface of the silicon wafer will peel off together with the resin film. From the results at this time, the suitability of the composite sheet as a die bonding sheet was evaluated according to the following criteria. The results are shown in Table 1. (Evaluation Criteria) A: The second resin layer remains on the entire polished surface of the silicon wafer, making the composite sheet highly suitable for use as a die bonding sheet. B: The second resin layer does not remain on a part or all of the polished surface of the silicon wafer, and the composite sheet is not suitable as a die bonding sheet.

[0175] [Evaluation of suitability of hardened composite sheet] The cured composite sheet obtained above was evaluated for suitability as a die bonding sheet in the same manner as for the composite sheet described above. The results are shown in Table 1.

[0176] <Evaluation of suitability as a dicing sheet> [Production of composite sheets and hardened composite sheets] Separately, the same composite sheet and cured composite sheet as described above (when evaluating suitability as a die bonding sheet) were produced.

[0177] [Evaluation of the suitability of composite sheets] (Prevents chips from scattering) An 8-inch silicon wafer (thickness 350 μm) with one surface polished to #2000 was prepared. Of the second resin layer in the composite sheet obtained above, the area near the center in the width direction was attached to the #2000 polished surface (polished surface) of the silicon wafer, and the area surrounding the attachment area to the silicon wafer was attached to a ring frame. At this time, the attachment of the second resin layer to the silicon wafer and ring frame was performed under a temperature condition of 23°C. Next, this laminate of the silicon wafer, the composite sheet, and the ring frame was left to stand for 20 minutes in an environment at a temperature of 23° C. and a relative humidity of 50%.

[0178] Next, the silicon wafer in the stack was diced using a dicing device (DISCO Corp.'s "DFD6361") to produce a large number of silicon chips measuring 5 mm x 5 mm. At this time, a DISCO Corp.'s "Z05-SD2000-D1-90 CC" dicing blade was used, with a blade rotation speed of 3000 rpm, a blade feed speed of 50 mm / min, and a blade height of 0.06 mm. Dicing was performed while spraying water (cleaning water). After dicing, the composite sheet was checked for the presence or absence of scattering of silicon chips of normal shape measuring 5 mm x 5 mm, except for the silicon chips having an abnormal shape formed in the peripheral area of ​​the silicon wafer. The chip scattering prevention effect (i.e., the suitability of the composite sheet as a dicing sheet) was evaluated according to the following criteria. The results are shown in Table 1. (Evaluation Criteria) A: No properly shaped silicon chips were scattered from the composite sheet, showing that the composite sheet is highly effective at preventing chips from scattering. B: One or more properly shaped silicon chips have been scattered from the composite sheet, and the composite sheet's ability to prevent chips from scattering is insufficient.

[0179] (Adhesion between chip and composite sheet) Furthermore, when evaluating the chip shattering prevention effect, the presence or absence of water infiltration from the dicing line between the composite sheet (more specifically, the second resin layer in the composite sheet) and the silicon chip was simultaneously confirmed through the composite sheet. Then, the adhesion between the chip and the composite sheet (i.e., the suitability of the composite sheet as a dicing sheet) was evaluated according to the following criteria. The results are shown in Table 1. (Evaluation Criteria) A: No water penetration was observed between any of the chips and composite sheet evaluated, and the chips and composite sheet were in close contact. B: Water penetration was observed between at least some of the chips and the composite sheet to be evaluated, and the adhesion between the chips and the composite sheet was low.

[0180] [Evaluation of suitability of hardened composite sheet] The cured composite sheet obtained above was evaluated for suitability as a dicing sheet in the same manner as for the composite sheet described above. The evaluation criteria were as follows. The results are shown in Table 1. (Evaluation criteria for chip scattering prevention effect) A: No properly shaped silicon chips were scattered from the cured composite sheet, and the cured composite sheet had a high chip scattering prevention effect. B: One or more properly shaped silicon chips have been scattered from the cured composite sheet, and the cured composite sheet is insufficient in preventing chip scattering. (Evaluation criteria for adhesion between chip and cured composite sheet) A: No water was observed to have penetrated between any of the chips evaluated and the hardened composite sheet, and the chips and the hardened composite sheet were in close contact with each other. B: Water penetration was observed between at least some of the chips and the cured composite sheet, and the adhesion between the chips and the cured composite sheet was poor.

[0181] <<Production and evaluation of resin films, and production and evaluation of composite sheets>> [Example 2] A resin film and a composite sheet were produced and evaluated in the same manner as in Example 1, except that the amount of the soluble resin (a)-1 was changed from 70 parts by mass to 76 parts by mass, and the amount of the energy ray curable compound (b)-1 was changed from 28 parts by mass to 22 parts by mass during the production of the resin composition. The results are shown in Table 1.

[0182] [Comparative Example 1] A resin film was produced and evaluated, and a composite sheet was produced and evaluated in the same manner as in Example 1, except that the energy ray curable compound (b)-1 and the photopolymerization initiator (c)-1 were not blended. The results are shown in Table 1.

[0183] [Comparative Example 2] <<Production of resin film>> <Production of Resin Composition> A urethane acrylate oligomer (Arkema's "CN9021 NS") (65 parts by mass), isobornyl acrylate (25 parts by mass) and dodecyl acrylate (10 parts by mass) were mixed, and a photopolymerization initiator (BASF's "Irgacure 1173") (3.4 parts by mass) was mixed with the total amount (100 parts by mass) of the mixture obtained from this, to produce an energy ray curable resin composition. Note that the amounts of each component shown here are the amounts of the target product not including the solvent.

[0184] <Production of resin film> A release film ("SP-PET381031", manufactured by Lintec Corporation, thickness 38 μm) made of polyethylene terephthalate film, one side of which had been treated for release by silicone treatment, was used, and the resin composition obtained above was applied to the release-treated surface by a fountain die method to form a coating film. Next, a belt conveyor type ultraviolet irradiation device (Eye Graphics "ECS-401GGX") and a high pressure mercury lamp (Eye Graphics "H04-L41") were used to illuminate the sample at an intensity of 112 mW / cm. 2 , light intensity 177mJ / cm 2 Under the above conditions, the exposed surface of the coating film was irradiated with ultraviolet light to form a semi-cured layer. Next, one side of a polyethylene terephthalate (PET) film (Toyobo Co., Ltd., "Cosmoshine A4100", thickness 50 μm) was attached to the exposed surface of the semi-cured layer. Using the same ultraviolet irradiation device and high-pressure mercury lamp as above, the illuminance was 271 mW / cm 2 , light intensity 1200mJ / cm 2 Under the above conditions, the semi-cured layer was irradiated with ultraviolet rays through the PET film to completely cure the semi-cured layer, thereby forming an ultraviolet-cured layer having a thickness of 30 μm. As a result of the above, a comparative two-layer resin film was obtained, which was configured to include a PET film (thickness: 50 μm) and an ultraviolet-cured layer (thickness: 30 μm) provided on one surface of the PET film.

[0185] <<Manufacturing of composite sheets>> In the same manner as in Example 1, a second resin layer having a thickness of 20 μm was formed. Next, a composite sheet with a release film was produced in the same manner as in Example 1, except that the resin film with a release film obtained above was used instead of the resin film with a release film. At this time, the exposed surface of the second resin layer was attached to the exposed surface of the ultraviolet cured material layer in the resin film with a two-layer structure. That is, this composite sheet is configured by laminating a PET film (thickness 50 μm), an ultraviolet cured material layer (thickness 30 μm), and a second resin layer (thickness 20 μm) in this order in the thickness direction.

[0186] <<Evaluation of resin films and composite sheets>> The resin film and composite sheet obtained above were evaluated in the same manner as in Example 1. The results are shown in Table 1. In this comparative example, the composite sheet obtained above already had an ultraviolet-cured layer, and was therefore treated as being the same as the cured composite sheets in the other examples. On the other hand, the coating film of the resin composition before UV irradiation (in other words, before the formation of the semi-cured layer) is liquid and cannot be made into a film. Therefore, the pre-cured probe tack value T1, pre-cured gel fraction G1, and pre-cured peel force P1 were all unmeasurable, and the suitability as a die bonding sheet before UV irradiation and the suitability as a dicing sheet before UV irradiation were all unevaluable. Therefore, the post-cured ratio of the probe tack value, the post-cured ratio of the gel fraction, and the post-cured ratio of the peel force were all uncalculatable. The post-cure probe tack value T2, post-cure gel fraction G2, and post-cure peel strength P2 of the resin film were all measured for the UV-cured layer in the two-layered resin film.

[0187] <<Production and evaluation of resin films, and production and evaluation of composite sheets>> [Comparative Example 3] A resin film was produced in the same manner as in Example 1. Next, this resin film was exposed to ultraviolet light at an illuminance of 230 mW / cm in air using an ultraviolet irradiator equipped with a high-pressure mercury lamp ("RAD-2000 m / 12" manufactured by Lintec Corporation). 2 , light intensity 190mJ / cm 2 The sample was irradiated with ultraviolet light under the following conditions. Next, a composite sheet was produced in the same manner as in Example 1, except that this resin film after ultraviolet ray irradiation (in other words, the ultraviolet ray cured resin film) was used instead of the resin film that had not been irradiated with ultraviolet ray. This composite sheet was then evaluated in the same manner as in Example 1. However, since the resin film in the composite sheet before evaluation obtained here had already been cured by ultraviolet light, it was not possible to evaluate the suitability of the composite sheet before curing. The results are shown in Table 1.

[0188] [Table 1]

[0189] As is clear from the above results, the composite sheets of Examples 1 and 2 had suitability as a die bonding sheet before curing, and had suitability as a dicing sheet after curing (as cured composite sheets). That is, the properties of the composite sheets of Examples 1 and 2 changed appropriately before and after curing of the resin film, and they could be used as either a die bonding sheet or a dicing sheet.

[0190] In the composite sheets of Examples 1 and 2, P1 was 14 mN / 25 mm or less (12 to 14 mN / 25 mm), while P2 was 6000 mN / 25 mm, and the post-curing ratio of the peel force was 42857% or more (42857 to 50000%), which was significantly larger. This post-curing ratio of the peel force supported that the composite sheet had two types of suitability as described above.

[0191] Furthermore, in the composite sheets of Examples 1 and 2, T1 was 2.06 mN / cm 2 or more (2.06~2.26mN / cm 2) while T2 is 0.78mN / cm 2 Below (0.29~0.78mN / cm 2 ) and the post-curing ratio of probe tack value was significantly smaller, less than 34.8% (14.3-34.8%). Furthermore, in the composite sheets of Examples 1 and 2, G1 was 5% or less (4-5%), while G2 was 46% or more (46-55%), and the gel fraction after curing was 920% or more (920-1375%), which was significantly larger. These changes in the physical properties of the composite sheet supported the above-mentioned post-curing ratios of peel force.

[0192] In Examples 1 and 2, the resin film contained a soluble resin (a) and an energy ray-curable compound (b) and was energy ray-curable.

[0193] In contrast, the composite sheet of Comparative Example 1 had no suitability as a dicing sheet either before or after curing. In the composite sheet of Comparative Example 1, the post-curing percentage of peel force, the post-curing percentage of probe tack value, and the post-curing percentage of gel fraction were all 100%. In Comparative Example 1, the resin film did not contain the energy ray-curable compound (b) and did not have energy ray-curability.

[0194] The composite sheet of Comparative Example 2 could not be formed into a film without irradiation with ultraviolet light, and was completely different from the composite sheet of the present embodiment. The components contained in the semi-cured layer and the ultraviolet-cured layer in Comparative Example 2 both had low solubility in toluene, and the semi-cured layer and the ultraviolet-cured layer were clearly different from the resin film of the present embodiment. Furthermore, the composite sheet of Comparative Example 2 was not suitable as a die bonding sheet, and was also insufficient in suitability as a dicing sheet.

[0195] The composite sheet of Comparative Example 3 appears similar to the cured composite sheet of Example 1, but since the ultraviolet-cured product is laminated with the second resin layer instead of the resin film during the production of the composite sheet, the advantageous effect of irradiating the laminate of the resin film and the second resin layer with ultraviolet rays (energy rays) was not obtained. In other words, the composite sheet of Comparative Example 3 was not suitable as a dicing sheet. [Industrial Applicability]

[0196] The present invention can be used in the manufacture of semiconductor devices. [Explanation of symbols]

[0197] 1. Composite sheet, 11: resin film; 11a: one surface (first surface) of the resin film; 11'... Energy ray cured resin film, 12: second resin layer; 12a: a surface (first surface) of the second resin layer opposite to the resin film side; 9. Object to be affixed

Claims

1. A resin film, The resin film contains a soluble resin (a) and an energy ray-curable compound (b) different from the soluble resin (a), A resin film, in which 13 g or more of the soluble resin (a) can be dissolved in 100 g of toluene under a temperature condition of 23°C.

2. The resin film according to claim 1 , further comprising a photopolymerization initiator (c).

3. 3. The resin film according to claim 1, wherein the soluble resin (a) is an ethylene-vinyl acetate copolymer.

4. The resin film and the acrylic resin film are bonded together to prepare a test piece (s11); The test piece (s11) had an illuminance of 230 mW / cm 2 , light intensity 190mJ / cm 2 The test piece is irradiated with ultraviolet light under the conditions of (a) to (c), thereby curing the test piece with ultraviolet light to prepare a test piece (s12); The peel force P when the resin film was peeled from the acrylic resin film in the test piece (s11) at a peel speed of 300 mm / min under an environment of a temperature of 23° C. and a relative humidity of 50%, so that the surfaces of the resin film and the acrylic resin film in the test piece (s11) that had been in contact with each other formed an angle of 180° was measured. 1 Measure The peel force P was measured when the ultraviolet-cured resin film was peeled from the acrylic resin film in the test piece (s12) at a peel speed of 300 mm / min under an environment of a temperature of 23° C. and a relative humidity of 50%, so that the surfaces of the ultraviolet-cured resin film and the acrylic resin film in the test piece (s12) that were in contact with each other formed an angle of 180°. 2 When the measurement was performed, the following formula P(0): P 2 / P 1 ×100 P(0) The resin film according to claim 1 or 2, wherein the peel strength ratio calculated by the following formula is 15,000% or more.

5. A composite sheet comprising the resin film according to claim 1 or 2 and a second resin layer provided on one surface of the resin film.

6. A method for manufacturing a workpiece, comprising: The workpiece is obtained by machining a workpiece, The manufacturing method includes a bonding step of bonding a surface of the second resin layer in the composite sheet according to claim 5 opposite to the resin film side to one surface of the workpiece, thereby producing a workpiece with the composite sheet, Further, after the attaching step, a peeling step (I) of peeling the resin film from the second resin layer in the workpiece with the composite sheet, and after the peeling step (I), a processing step (I) of processing the workpiece with the second resin layer to produce the workpiece, or The method for manufacturing a workpiece includes a hardening step (II) of hardening the resin film in the composite sheet with energy rays after the attaching step, thereby producing a workpiece with a hardened composite sheet, in which the composite sheet in the workpiece with the composite sheet becomes a hardened composite sheet, a processing step (II) of processing the workpiece in the workpiece with the hardened composite sheet after the hardening step (II), and a pick-up step (II) of separating the workpiece from the second resin layer in the hardened composite sheet and picking it up after the processing step (II).

7. 7. The method for manufacturing a workpiece according to claim 6, further comprising, after the curing step (II) and before the processing step (II), a peeling step (III) of peeling the cured composite sheet from the workpiece in the workpiece with the cured composite sheet, and, after the peeling step (III), a re-attaching step (II) of producing a workpiece with the cured composite sheet by re-attaching a surface of the second resin layer in the peeled cured composite sheet opposite to the energy ray cured product side of the resin film to one surface of the workpiece.

Citation Information

Patent Citations

  • Dicing adhesive sheet and dicing method

    JP2009064975A

  • Die bonding film, dicing die bonding sheet, and method for manufacturing semiconductor chips

    JP7155245B2