Resin composition, laminate, and method for producing resin composition
The resin composition with controlled particle size polymer fine particles of a carboxylic acid metal salt and a binder resin addresses the need for high hiding properties in paints and inks, achieving comparable results to titanium oxide without its use, by optimizing light scattering and adhesion.
Patent Information
- Application Number
- JP2024045032
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-11
AI Technical Summary
Existing resin compositions used in paints and inks lack high hiding properties when expensive pigments like titanium oxide are not used or their use is reduced, and there is a need for alternatives that provide comparable white concealment.
A resin composition containing polymer fine particles of a carboxylic acid metal salt with an unsaturated bond and a binder resin, where the particle size is controlled to about half the wavelength of visible light, typically between 50 to 500 nm, and includes a solvent and optional additives for improved dispersibility and stability.
The resin composition achieves high white hiding properties comparable to titanium oxide, even when its use is minimized, through efficient light scattering and controlled particle size, enhancing concealment and substrate adhesion.
Smart Images

Figure 2024144251000001 
Figure 2024144251000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition having high hiding power and a laminate using the same. [Background technology]
[0002] White pigments used in paints and inks are required to have whiteness and a hiding power that does not transmit light. Titanium oxide (TiO2) has no absorption in the visible light region and a refractive index that is considerably higher than that of resins used in paints, and is therefore widely used for coloring plastic resins such as automobile parts materials, packaging container materials, and home appliance parts materials as a white pigment with excellent hiding power and coloring power. However, titanium oxide is expensive and there is concern that it may be carcinogenic, so there is a demand for alternatives. Potential alternative pigments include inexpensive inorganic substances such as zinc oxide (ZnO), magnesium oxide (MgO), and calcium carbonate (CaCO3), but these have a low refractive index and are limited in their use as pigments, so there have been reports of the use of titanium oxide in combination with various inorganic pigments (Patent Document 1). However, these pigments are surface-treated and contain titanium oxide, so they are not a complete substitute for titanium oxide used as a white pigment. Therefore, an object of the present invention is to provide a resin composition which can be used for paints and inks having good hiding power even if expensive pigments such as titanium oxide are not used or the amount of the pigment used is reduced. In addition to the refractive index, precise control of particle shape is also required for color pigments such as titanium dioxide. In general, it is said that the hiding power is high when the particle diameter is about half the wavelength of visible light, so it is considered preferable to use pigments with particle diameters of about 180 to 400 nm (Non-Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 06-093204 [Non-patent literature]
[0004] [Non-Patent Document 1] Journal of the Adhesion Society of Japan Vol.46No.9 P345-349(2010) Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention aims to provide a resin composition that can easily form a white coating film on a substrate such as a plastic film or paper without using, or by reducing the amount of, expensive pigments such as titanium oxide, and that can be used for paints or inks that can exhibit high white hiding power comparable to that of titanium oxide, a laminate using the same, and a method for producing the resin composition. [Means for solving the problem]
[0006] As a result of extensive research aimed at solving the above problems, the inventors discovered that by adopting a structure containing a metal salt of a carboxylic acid, it is possible to produce a resin composition having high white hiding power and in which the particle size is controlled to about half that of visible light, thereby arriving at the present invention.
[0007] That is, the present invention relates to a resin composition comprising polymer fine particles of a metal salt of a carboxylate having an unsaturated bond (A) and a binder resin (B).
[0008] Alternatively, the present invention relates to the above resin composition, wherein the metal carboxylate (A) having an unsaturated bond is a metal (meth)acrylate.
[0009] Alternatively, the present invention relates to the resin composition, wherein the metal carboxylate (A) having an unsaturated bond contains one or more metal ions selected from the group consisting of zinc ions, magnesium ions, calcium ions, aluminum ions and titanium ions.
[0010] Alternatively, the present invention relates to the above resin composition, wherein the metal salt of a carboxylate having an unsaturated bond (A) contains a zinc ion.
[0011] Alternatively, the present invention relates to the above resin composition, wherein the polymer fine particles have a particle size of 50 to 500 nm.
[0012] Alternatively, the present invention relates to the above resin composition, wherein the binder resin (B) is a polymer of vinyl alcohol and / or vinyl chloride.
[0013] Alternatively, the present invention relates to the resin composition, wherein the content of the polymer fine particles is 50 to 99 mass % in 100 mass % of the solid content of the resin composition.
[0014] Alternatively, the present invention relates to the resin composition, wherein the polymer of the polymer fine particles has a metal salt of a carboxylic acid in a side chain.
[0015] Alternatively, the present invention relates to the above resin composition, further comprising a solvent (C).
[0016] Alternatively, the present invention relates to the resin composition, which is a paint or ink.
[0017] Alternatively, the present invention relates to a laminate comprising a substrate and a resin layer formed by coating or printing the resin composition on the substrate.
[0018] Alternatively, the present invention relates to a method for producing a resin composition containing fine particles including a polymer of a metal salt of a carboxylate (A) having an unsaturated bond and a binder resin (B), characterized in that the polymer is produced by at least one polymerization reaction selected from the group consisting of EB irradiation, UV irradiation, and heating. Effect of the Invention
[0019] According to the present invention, it is possible to provide a resin composition and a laminate which are capable of exhibiting high white hiding power even when no titanium oxide is used or when the amount of titanium oxide used is reduced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Hereinafter, an embodiment of the present invention will be described.
[0021] The resin composition and laminate of the present invention are characterized in that they contain polymer fine particles of a metal salt of a carboxylate having an unsaturated bond and a binder resin.
[0022] [Polymer particles of metal carboxylates with unsaturated bonds] The polymer fine particles of a metal salt of a carboxylic acid having an unsaturated bond of the present invention are fine particles made of a polymer of a metal salt of a carboxylic acid having an unsaturated bond. In general, light scattering is thought to be affected by particle size, and it is known that light is most effectively scattered when the particle size is half the wavelength of light. By controlling the particle size according to the wavelength to be scattered, efficient scattering occurs and the concealment effect is also increased. On the other hand, if the particle size is too small, light is not easily scattered and passes through, resulting in reduced concealment. Also, if the particle size is too large, the light concealment efficiency is proportional to the cross-sectional area of the scattering particles, so the larger the particle size, the lower the light concealment efficiency. For this reason, the particle size of the polymer fine particles of the metal salt of a carboxylic acid having an unsaturated bond in the present invention is preferably 50 to 500 nm, more preferably 180 to 400 nm. The particle size of the polymer fine particles can be controlled by the composition and reaction conditions.
[0023] <Polymer of metal carboxylate having unsaturated bond> The polymer of the metal salt of a carboxylic acid having an unsaturated bond of the present invention can be synthesized by polymerizing a metal salt of a carboxylic acid having an unsaturated bond by a polymerization method described later, and may contain one or more metal salts of carboxylic acids. In addition, it may contain one or more optional copolymerizable monomers as long as the effects of the present invention are not impaired. The monomer referred to here is not particularly limited, but may be any of aliphatic, alicyclic, and aromatic, and examples thereof include carboxylic acid such as acrylic acid and methacrylic acid, aliphatic acrylic acid esters such as methyl acrylate and ethyl acrylate, alicyclic acrylic acid esters such as cyclohexyl acrylate and isobornyl acrylate, and aromatic acrylic acid esters such as phenyl acrylate and benzyl acrylate.
[0024] (Metal salt of carboxylate having unsaturated bond (A)) The metal salt of carboxylic acid having an unsaturated bond (A) in the present invention is a metal salt formed by a coordinate bond or ionic bond between a carboxylic acid having an unsaturated bond and a metal ion, specifically, a metal salt in which a negatively charged carboxylic acid moiety and a positively charged metal ion are strongly bound by a coordinate bond or ionic bond. The metal salt of carboxylic acid having an unsaturated bond may be a commercially available metal salt of carboxylic acid having an unsaturated bond, or may be a metal salt of carboxylic acid having an unsaturated bond produced by reacting a carboxylic acid having an unsaturated bond or a carboxylic acid salt having an unsaturated bond with a metal salt or a metal hydroxide, or may be a metal salt of carboxylic acid having an unsaturated bond produced by reacting a carboxylic acid with a metal oxide. In particular, a (meth)acrylic acid metal salt is preferred. Examples of metal salts of carboxylic acids having unsaturated bonds include, but are not limited to, zinc acrylate, zinc methacrylate, magnesium acrylate, magnesium methacrylate, calcium acrylate, magnesium methacrylate, aluminum acrylate, magnesium methacrylate, titanium acrylate, titanium methacrylate, copper acrylate, etc. Commercially available products of such metal salts of carboxylic acids include, for example, ZN-DA manufactured by Nippon Shokubai Co., Ltd., and ZDA-100, ZDA-90, M-CP, R-20S, R-MMA2, ZA30, MA35, CA25, etc. manufactured by Asada Chemical Industry Co., Ltd. Incidentally, (meth)acrylic acid means acrylic acid and / or methacrylic acid.
[0025] (Carboxylic acid having unsaturated bonds) The carboxylic acid having an unsaturated bond in the present invention is a polymerizable carboxylic acid, which may be a monocarboxylic acid, a dicarboxylic acid, or a polycarboxylic acid. More specifically, the carboxylic acid is an olefinically unsaturated carboxylic acid containing at least one activated carbon or double bond and at least one carboxyl group, i.e., an acid that is easily converted to an acid containing an olefinic double bond in the alpha or beta position relative to the carboxyl group of C=C-COOH, or as part of the methylene end group of CH2=C<. Furthermore, the carboxylic acid having an unsaturated bond in the present invention is characterized in that the carboxylic acid moiety functions as a ligand, specifically, crosslinking is possible by coordination of a negatively charged carboxylate ion with a metal ion.
[0026] Examples of carboxylic acids of this type include, but are not limited to, acrylic acid, methacrylic acid, ethacrylic acid, cyanoacrylic acid, crotonic acid, phenylacrylic acid, acryloxypropionic acid, cinnamic acid, chlorocinnamic acid, citraconic acid, mesaconic acid, glutaconic acid, aconitic acid, tricarboxyethylene, maleic anhydride, maleic acid, fumaric acid, itaconic acid, itaconic anhydride, 2-(trifluoromethyl)acrylic acid, mono(2-acryloyloxyethyl)succinate, mono-2-(methacryloyloxy)ethyl phthalate, monohydroxyethyl phthalate acrylate, monohydroxyethyl phthalate acrylate, ω-carboxy-polycaprolactone monoacrylate, 6-acrylamidohexanoic acid, 4-carboxystyrene, 4-methacryloyloxyphthalic acid, 4-methacryloxyethyl triacrylate, 1,2-dimethylphenyl ... Mellitic anhydride, 1,3,4-benzenetricarboxylic acid 4-[2-(methacryloyloxy) Examples include (oxy)ethyl.
[0027] (Metal ions) The metal ion species of the metal salt of a carboxylate having an unsaturated bond in the present invention is not particularly limited, but refers to a metal ion carrying a positive charge, and examples thereof include copper, zinc, nickel, iron, cobalt, gallium, chromium, vanadium, manganese, titanium, beryllium, aluminum, magnesium, calcium, strontium, scandium, potassium, sodium, and lithium.
[0028] The metal ions that can be used as the carboxylate metal salt of the present invention are not particularly limited, but divalent or higher metal ions are preferred because the carboxylic acid is more likely to form crosslinks by forming coordinate bonds with the metal ions. In addition, various colors can be developed by selecting the metal ion. For example, it is possible to develop a blue color when copper ions are used, a red color when iron ions are used, and a white color when zinc ions are used, and the coating material can be used as various colored coating materials by using different metal ions according to the desired color. Although not particularly limited, when white hiding power is to be expressed, metal ions or metal salts of carboxylates that do not absorb in the visible light region, such as zinc, magnesium, calcium, titanium, and aluminum, are preferred, and zinc is more preferred in terms of ease of coordinate bonds. The content of the metal ions or metal atoms in the solid content of the coating material is preferably 50% by mass or less, more preferably 25% or less, in terms of environmental consideration.
[0029] <Polymerization> The polymerization or polymerization reaction in the present invention is a method for preparing fine particles using the metal salt of the carboxylic acid having unsaturated bond, and proceeds by chemical reaction of the unsaturated bond site.The polymer in the present invention means a compound or polymer having a molecular weight of 1000 or more obtained by polymerization, but is not particularly limited.The polymerization method includes, but is not particularly limited to, a heating polymerization method, a UV irradiation polymerization method, and an EB irradiation polymerization method.
[0030] (Heating polymerization) Thermal polymerization is a polymerization in which a polymerization reaction occurs by heating a radically polymerizable compound containing a monomer and a chain transfer group in the presence of a thermal initiator (thermal radical polymerization initiator). By heating a mixture of the thermal initiator, a metal salt of a carboxylic acid having an unsaturated bond, and a solvent, a polymer is formed, and fine particles of 50 to 500 nm can be produced.
[0031] (UV irradiation polymerization) UV irradiation polymerization is a polymerization in which a radically polymerizable compound containing a monomer and a chain transfer group is irradiated with UV light in the presence of a photoinitiator (photoradical polymerization initiator) to generate radical active species, which then initiate a polymerization reaction. A mixture of a photoinitiator, a metal salt of a carboxylic acid having an unsaturated bond, a solvent, and a binder resin is applied to a substrate and then irradiated with UV light to generate fine particles of 50 to 500 nm, which can be used to create a colored coating. As a UV light source, ultraviolet lamps (UV lamps) such as low- or high-pressure mercury lamps, xenon lamps, and metal halide lamps are widely used, but an irradiation module using an ultraviolet light-emitting diode (UV-LED) as a light source may also be used.
[0032] In the present invention, the polymerization reaction is carried out by applying energy using active energy rays (ultraviolet rays, visible light, near-infrared rays, etc.) to obtain the desired polymer. As a light source for applying the energy, a light source having a dominant emission wavelength in the wavelength region of 250 nm to 450 nm is preferable. Examples of light sources having a dominant wavelength of light emission in the wavelength region of 250 nm to 450 nm include ultra-high pressure mercury lamps, high pressure mercury lamps, medium pressure mercury lamps, low pressure mercury lamps, mercury xenon lamps, metal halide lamps, high power metal halide lamps, xenon lamps, pulsed xenon lamps, carbon arc lamps, deuterium lamps, fluorescent lamps, argon ion lasers, helium cadmium lasers, helium neon lasers, krypton ion lasers, various semiconductor lasers, YAG lasers, light emitting diodes, CRT light sources, plasma light sources, ArF excimer lasers, KrF excimer lasers, F2 lasers, Nd-AG triple wave lasers, nitrogen lasers, Xe-Cl excimer lasers, Xe-F excimer lasers, and LED lamps.
[0033] (Electron beam (EB) irradiation polymerization) Electron beam irradiation polymerization is a method in which a radical polymerizable compound containing a monomer and a chain transfer group is irradiated with an electron beam (EB) instead of a UV light source to generate radicals without the use of a photoradical polymerization initiator, and decomposition or polymerization reaction is promoted. A mixed liquid of a metal salt of a carboxylic acid having an unsaturated bond, a solvent, and a binder resin is applied to a substrate, and then irradiated with an electron beam to generate fine particles of 50 to 500 nm, which can be used as a colored coating material. The method of electron beam irradiation is not particularly limited, and an electron beam irradiation device such as an area beam type, curtain beam type, scanning beam type, or vacuum tube type can be used. It is preferable to irradiate under an oxygen concentration of 10 to 000 ppm during irradiation. The acceleration voltage when extracting the electron beam is not particularly limited, but is preferably less than 200 kV. If the acceleration voltage is 200 kV or more, the energy of the electron beam becomes too high, which is not only poor in energy efficiency but also increases the risk of material deterioration, which is not preferable. In order to produce the desired effect at the electron beam irradiated site with high energy efficiency, the acceleration voltage is preferably 10 to 150 kV, and more preferably 30 to 120 kV.
[0034] <Initiator> The initiator that can be used in the present invention will be described in detail. As the initiator, for example, a conventionally known photoinitiator (photoradical polymerization initiator), a thermal initiator (thermal radical polymerization initiator), etc. can be used. For example, when a metal salt of a carboxylic acid having an unsaturated bond is polymerized by ultraviolet or UV light, a photoinitiator can be used, and when a metal salt of a carboxylic acid having an unsaturated bond is polymerized by heat, a thermal polymerization initiator can be used, and the polymerization can be appropriately selected. Among them, it is preferable to polymerize a metal salt of a carboxylic acid having an unsaturated bond by heat because the apparatus used is simple and is cost-effective, and the fine particles of the obtained polymer can be recovered as a pigment, making it easy to handle.
[0035] (Photoinitiator (F)) The photoinitiator (F) used in the present invention includes photoradical polymerization initiators and generally refers to compounds that generate radical active species that initiate a polymerization reaction by irradiation with light, and includes photoradical polymerization initiators as well as sensitizers. In the present invention, it is preferable to use an initiator that has a light absorption of 380 nm to 410 nm, and examples of such initiators include acylphosphine oxide-based, α-aminoacetophenone-based, benzophenone-based, and thioxanthone-based photoinitiators, and conventionally known photoinitiators can be used. Specifically, for example, diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, benzyl methyl ketal, 4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butane, oligo{2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone}, 2 acetophenones such as 1-hydroxy-1-{4-[4-(2-hydroxy-2-methylpropionyl)benzyl]phenyl}-2-methylpropan-1-one; benzoins such as benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether; phosphines such as 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide; and phenylglyoxylic methyl esters. More specifically, Omnirad 651, Omnirad 184, Omnirad 1173, Omnirad 2529, Omnirad 127, Omnirad 500, Omnirad 1000, Omnirad 2959, Omnirad 907, Omnirad 369, Omnirad 379, Omnirad TPO, Omnirad 819, Omnirad MBE, Omnirad 754, Omnirad 250, Omnirad 270, Omnirad 784 (IGM Examples of photoinitiators include, but are not limited to, Adeka Optomer N1414, Adeka Optomer N1717, and Esacure 1001M (manufactured by Lamberti Chemicals), but since the carboxylate metal salt used in the present invention is water-soluble, water-soluble photoinitiators such as Omnirad-1173 and Omnirad 2959 are preferred. These can be used alone or in combination, and can be mixed as desired depending on the properties required for the polymer. When using these photoinitiators, the amount used is in the range of 0.01 to 100 mass%, preferably 0.1 to 10, based on the total amount of the ink composition.
[0036] If the amount of photoinitiator used is less than 0.01, the amount of radicals, which are active species, generated by irradiation with active energy rays is insufficient, and the desired polymerization rate may not be obtained. On the other hand, if the amount of photoinitiator used is more than 200, the amount of low molecular weight components is too large, and the properties of the polymer after the polymerization reaction may be insufficient.
[0037] (Thermal Initiator (D)) The thermal initiator (D) in the present invention contains a thermal polymerization radical initiator and generates a radical active species for radically polymerizing a radically polymerizable compound by thermal decomposition. There are no particular limitations on the thermal polymerization radical initiator, and any initiator known to those skilled in the art can be used without limitation. Examples of the thermal polymerization initiator include aromatic ketones, onium salt compounds, organic peroxides, thio compounds, hexaarylbiimidazole compounds, ketoxime ester compounds, borate compounds, azinium compounds, metallocene compounds, active ester compounds, compounds having a carbon-halogen bond, azo compounds, and the like, and are not particularly limited. However, since the carboxylate metal salt used in the present invention is water-soluble, water-soluble thermal initiators such as ammonium persulfate and potassium persulfate are preferred. These can be used alone or in combination, and can be mixed as desired depending on the properties desired for the polymer. When using these thermal initiators, the amount used is in the range of 0.001 to 99 mass%, preferably 0.01 to 10 mass%, relative to 100 mass% of the solid content of the resin composition.
[0038] [Binder resin (B)] Examples of the binder resin (B) that can be used by mixing with the metal salt of a carboxylic acid having an unsaturated bond or the polymer microparticles of a metal salt of a carboxylic acid having an unsaturated bond of the present invention include polymers and copolymers such as polyacrylates, poly-α-alkyl acrylates, polyamides, polyvinyl acetals, polyformaldehydes, polyurethanes, polycarbonates, polystyrenes, and polyvinyl esters. More specifically, examples include polyvinyl alcohol, polyimide, polymethacrylate, polymethyl methacrylate, polyethyl methacrylate, polyamide, polystyrene, polyethylene, polyvinyl carbazole, polyvinyl pyrrolidone, polyurethane, polyvinyl butyral, polyvinyl acetate, phenoxy resin, polyvinyl acetate resin, polyvinyl chloride resin, ionomer resin, novolac resin, phenolic resin, epoxy resin, and alkyd resin. From the viewpoint of microparticle dispersibility, however, polyvinyl alcohol and / or vinyl chloride polymers are preferred.
[0039] [Resin composition] The resin composition of the present invention is characterized by containing polymer fine particles of a metal carboxylate (A) having an unsaturated bond, and a binder resin (B). From the viewpoint of a balance between substrate adhesion and whiteness, the content of the polymer fine particles contained in the resin composition of the present invention is preferably 50 to 99 mass%, more preferably 60 to 95 mass%, and even more preferably 70 to 90 mass%, when the total of the metal carboxylate (A) and the binder resin (B) is taken as 100 mass%, although it varies depending on the production method of the resin composition.
[0040] <Solvent (C)> The solvent (C) used in the resin composition of the present invention is preferably water from the viewpoint of solubility and fine particle dispersibility, but is not particularly limited, and organic solvents can be used as other solvents, for example, ester-based solvents such as methyl acetate, ethyl acetate, normal propyl acetate, normal butyl acetate, isobutyl acetate, propyl acetate, ethyl cellosolve acetate, normal propyl acetate, isopropyl acetate, isobutyl acetate, propylene glycol monoethyl ether acetate, and propylene glycol monomethyl ether acetate, alcohol-based solvents such as methyl alcohol, ethyl alcohol, isopropyl alcohol, normal propanol, normal butanol, normal propyl alcohol, propylene glycol monoethyl ether, and propylene glycol monomethyl ether, ketone-based solvents such as acetone, methyl ethyl ketone, cyclohexanone, and methyl isobutyl ketone, and hydrocarbon-based solvents such as toluene, benzene, cyclohexane, hexane, methylcyclohexane, and ethylcyclohexane, and other known solvents can be used. These can also be used as a solvent by combining one or more of them. The mass of the solvent when used is not particularly limited, but the content of the solvent (C) in the resin composition is preferably 0.1 to 99 mass%, more preferably 10 to 95 mass%, and even more preferably 40 to 90 mass%.
[0041] <Dispersant> The resin composition of the present invention is preferably added with a dispersant in order to improve the dispersibility and storage stability when using a solvent.As the dispersant, hydroxyl group-containing carboxylic acid ester, salt of long chain polyaminoamide and high molecular weight acid ester, salt of high molecular weight polycarboxylic acid, salt of long chain polyaminoamide and polar acid ester, high molecular weight unsaturated acid ester, polymer copolymer, modified polyurethane, modified polyacrylate, polyether ester type anionic activator, naphthalene sulfonic acid formalin condensate salt, aromatic sulfonic acid formalin condensate salt, polyoxyethylene alkyl phosphate ester, polyoxyethylene nonylphenyl ether, stearylamine acetate, etc. can be used. Specific examples of dispersants include Disperbyk-101, Disperbyk-107, Disperbyk-110, Disperbyk-111, Disperbyk-130, Disperbyk-161, Disperbyk-162, Disperbyk-163, Disperbyk-164, Disperbyk-165, Disperbyk-166, Disperbyk-167, Disperbyk-168, Disperbyk-170, Disperbyk-400, Bykumen, BYK-P104, P105, P104S, 240S, and Lactimon (manufactured by BYK Chemie). In addition, EFKA44, EF KA46, EFKA47, EFKA48, EFKA49, EFKA54, EFKA63, EFKA64, EFKA65, EFKA66, EFKA71, EFKA701, EFKA764, EFKA766, EFKAPOLYMER100, EFKAPOLYMER150, EFKAPOLYMER400, EFKAPOLYMER401, EFKAPOLYMER402, EFKAPOLYMER403, EFKAPOLYMER450, EFKAPOLYMER451, EFKAPOLYMER452, EFKAPOLYMER453, EFKAPOLYMER745 (manufactured by BASF), FLOWLEN TG-710, FLOWNON SH-290, SP-1000, POLYFLOW No.50E, POLYFLOW No.300 (manufactured by Kyoeisha Chemical Co., Ltd.), DISPARLON Examples include KS-860, Disparlon 873SN, Disparlon 874, Disparlon #2150, and Disparlon #7004 (manufactured by Kusumoto Chemicals Co., Ltd.). In addition, Homogenol L-18, Emulgen 920, Emulgen 930, Emulgen 931, Emulgen 935, Emulgen 950, Emulgen 985, Acetamine 24, Acetamine 86 (manufactured by Kao Corporation), Solsperse 5000, Solsperse 13940, Solsperse 17000, Solsperse 24000GR, Solsperse 32000, Solsperse 33000, Solsperse 39000, Solsperse 41000, Solsperse 53000, Solsperse 76400, Solsperse 76500, Solsperse J100 (manufactured by Lubrizol Corporation), Nikkor T106 (polyoxyethylene sorbitan monooleate), MYS-IEX (polyoxyethylene monostearate), Hexagline 4-0 (hexaglyceryl tetraoleate) (manufactured by Nikko Chemical Co., Ltd.), Ajisper PB821, Ajisper 822, Ajisper 824, Ajisper 827, Ajisper 711 (manufactured by Ajinomoto Fine-Techno Co., Ltd.), TEGO Disper 685 (manufactured by Tego Chemi Services Co., Ltd.), and the like. The amount of dispersant added is selected arbitrarily to ensure the desired stability. Excellent flow characteristics are obtained when the dispersant is 0.1 to 10% by mass relative to the polymer fine particles. This range is more preferable because it provides good dispersion stability.
[0042] <Other> Furthermore, the resin composition of the present invention may be further mixed with an oxygen scavenger such as a phosphine, a phosphonate or a phosphite, a reducing agent, a polymerization accelerator, an antifoggant, an anti-fading agent, an antihalation agent, a fluorescent brightening agent, a surfactant, a colorant, an extender, a plasticizer, a flame retardant, an antioxidant, an ultraviolet absorber, a foaming agent, an anti-mold agent, a thermal polymerization inhibitor, an antistatic agent, a dye, an organic or inorganic pigment, a dye precursor, a magnetic material or other additives that impart various properties, depending on the purpose.
[0043] <Application> The resin composition of the present invention can be used for coating materials, inks, colored molded products, colorants, light-shielding agents, and sensors, and can be particularly suitably used as white coating materials and white inks.
[0044] [Method of producing resin composition] The method for producing the resin composition of the present invention is not particularly limited, but examples thereof include a method (production method 1) in which a metal salt of a carboxylic acid having an unsaturated bond (A) is polymerized by the above-mentioned polymerization method to synthesize fine particles, and then the fine particles and binder resin (E) are dispersed or dissolved in a solvent (C) to produce a resin composition, and a method (production method 2) in which a metal salt of a carboxylic acid having an unsaturated bond (A) and a binder resin (E) are dissolved in a solvent to obtain an intermediate of a resin composition, and then the intermediate of a resin composition is coated on a substrate, and then the carboxylic acid metal salt (A) is polymerized on the substrate to generate fine particles, thereby producing a resin composition on a substrate.
[0045] From the viewpoint of a balance between substrate adhesion and whiteness, the content of the polymer fine particles contained in the resin composition of the present invention is preferably 60 to 90 mass % when the total of the carboxylate metal salt and the binder resin is taken as 100 mass %, because the dispersibility and adhesion of the fine particles are improved when the binder resin (E) is contained sufficiently in the production method 1. Moreover, in the production method 2, when the carboxylate metal salt is small and the binder resin is contained in a large amount, the fine particles may not be formed well, so the content is more preferably 70 to 100 mass %.
[0046] In the method for producing the resin composition of the present invention, the method for dissolving or dispersing the metal salt of the carboxylic acid having an unsaturated bond or the fine particles containing the polymer thereof, the binder resin, etc. in the solvent is not particularly limited. Processing may be performed using a kiln equipped with a stirrer such as a planetary mixer or a disperser, or a glass bottle, but as a method for dispersing the fine particles, it is preferable to apply a dispersion treatment using a ball mill, a bead mill, a roller mill, a pebble mill, an attritor, a sand mill, etc. In addition, the fine particles composed of a polymer of a metal carboxylate in the resin composition of the present invention can be synthesized by a polymerization reaction of a metal carboxylate. During the polymerization reaction, polymerization is carried out by applying active energy such as ultraviolet light, visible light, near infrared light, electron beams, heat, or the like, and the desired particulate polymer can be obtained.
[0047] [Laminate] The laminate of the present invention has a layer of a colored resin composition formed by coating a resin composition or an intermediate thereof on one or both sides of a substrate. The layer of the resin composition may contain a solvent or may not contain a solvent, but it is preferable that the layer does not contain a solvent. The coating method of the resin composition includes a printing method and is not particularly limited, and a known coating method described later can be utilized. The thickness of the layer of the resin composition is not particularly limited, but is preferably 0.2 to 200 μm in a dry state, more preferably 0.5 to 10 μm, for the purpose of suppressing crack generation when bending and for the purpose of improving concealment. In addition, the resin composition layer formed here may be laminated in one or more layers on one or both sides of the substrate. When multiple layers of the resin composition are provided, the compositions may be the same or different, but it is preferable that they are different. For example, after coating one side of the substrate with a white resin composition, a drying process may be performed, and a layer of a blue resin composition may be formed in the same process to form two layers, or layers of resin compositions of different colors may be formed to form three layers. Furthermore, since the laminate of the present invention is required to have high white hiding power equivalent to that of titanium oxide, the L value is preferably 70 or more, and more preferably 75 or more.
[0048] <Base film (G)> The substrate or substrate film is selected from the group consisting of resin sheets, paper, and aluminum sheets (aluminum foils). For example, the resin sheet may be a resin sheet formed from a resin such as polyester resins such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polycarbonate resins, polyarylate resins, acrylic resins, polyphenylene sulfide resins, polystyrene resins, vinyl resins, vinyl chloride resins, polyimide resins, epoxy resins, polyethylene, polypropylene (OPP, CPP), and polyolefin resins such as polynorbornene. In addition, the substrate may be a laminate in which a metal is laminated on these sheets, for example, a laminate in which a metal is laminated on a polyethylene terephthalate (PET) sheet. Among the substrates, polypropylene, polyethylene terephthalate, polyethylene, and the like are preferred because of their good stretchability, translucency, and rigidity. The substrate may contain one or more optional components within a range that does not impair the effects of the present invention. The substrate used in the present invention may contain an ultraviolet absorber, an antioxidant, an antistatic agent, a surfactant, a pigment, a fluorescent whitening agent, etc. The substrate may contain inorganic particles containing silica, calcium carbonate, titanium oxide, etc., or organic particles containing acrylic resin, styrene resin, etc.
[0049] [Method of manufacturing laminate] A method for producing a laminate of the present invention using the resin composition obtained by the above-mentioned production method 1 is not particularly limited, but includes a step of forming a laminate having a layer of the resin composition on one or both sides of a substrate by a coating method described below, and drying the laminate. A method for producing a laminate of the present invention using the resin composition obtained by the above-mentioned production method 2 is not particularly limited, but includes a step of coating an intermediate of the resin composition on one or both sides of a substrate by a coating method described below, forming a layer of the intermediate of the resin composition, and then forming a laminate having a layer of the resin composition by UV irradiation polymerization method or electron beam (EB) irradiation polymerization method, which generates active radical species and causes a polymerization reaction to proceed, or by heating, and further drying the laminate.
[0050] <Coating and printing methods> In the method for producing a laminate, the coating method of the resin composition or the intermediate of the resin composition is not particularly limited, and includes a printing method, and a laminate can be obtained by utilizing a known coating method. Specific coating methods include wire bar coating, die coat coating, cast coating, slot coating, omega coating, spiral coating, control seam coating, slot coating, dot coating, hot melt applicator coating, hot melt coater coating, blade coat coating, dip coating, gravure coat coating, microgravure coating, curtain spray coating, bead coating, hot melt roll coater coating, and spin coat coating, and printing methods include inkjet printing, spray printing, roll coat printing, doctor roll printing, doctor blade printing, curtain coat printing, slit coat printing, screen printing, reverse printing, push coat printing, slit coater printing, and offset printing.
[0051] After the resin composition or the intermediate of the resin composition is applied to the substrate by these methods, it may be dried by heating or under reduced pressure as necessary to remove the solvent or promote crosslinking. The drying conditions are not particularly limited as long as they do not deteriorate the substrate, depending on the film thickness, substrate, and selected solvent, but hot air heating at about 40 to 200°C is preferably used.
[0052] When the resin composition contains a metal salt of a carboxylate or other reactive monomer having an unreacted unsaturated bond, it is possible to form a polymer inside the coating film by inducing a polymerization reaction by the above-mentioned method. The thickness of the resin composition layer is not particularly limited, but for the purpose of preventing cracks from occurring when folded or for the purpose of enhancing hiding power, it is preferably 0.2 to 200 μm, more preferably 0.5 to 10 μm in a dry state. The resin composition layer formed here may be a laminate formed by laminating one or more layers on one or both sides of the substrate. When the resin composition layers of the laminate are provided, the compositions may be the same or different, but it is preferable that they are different. For example, after applying a white resin composition to one side of the substrate, a drying process may be performed, and a layer of a blue resin composition may be formed in the same process to form two layers, or layers of resin compositions of different colors may be formed to form three layers. EXAMPLES
[0053] The present invention will be described in detail below with reference to examples, but these examples are merely one embodiment of the present invention, and the present invention is not limited to these examples. In the tables, "parts" and "%" represent "parts by mass" and "% by mass", respectively. For solutions of commercially available raw materials dissolved in other solvents, the raw materials excluding the solvent were used in calculation. The abbreviations for the carboxylic acid metal salt (A), binder resin (B), solvent (C), thermal initiator (D), monomer (E), photoinitiator (F), substrate film (G), and other components and constituent elements described in the examples and Table 1 below are shown below.
[0054] <Metal salt of carboxylate having unsaturated bond (A)> A-1: Nippon Shokubai Co., Ltd. Product name: ZN-DA (zinc acrylate) A-2: Asada Chemical Industry Co., Ltd. Product name: R-20S (zinc methacrylate) A-3: Fujifilm Wako Pure Chemical Corporation Product name: Magnesium acrylate A-4: Fujifilm Wako Pure Chemical Corporation Product name: Calcium acrylate
[0055] <Binder resin (B)> B-1: Mitsubishi Chemical Corporation Product name: Gohsenol NL-05 (polyvinyl alcohol) B-2: Nissin Chemical Industry Co., Ltd. Product name: TA5R (vinyl chloride-vinyl acetate copolymer) B-3: Nippon Shokubai Co., Ltd. Product name: HL-415 (Polyacrylic acid)
[0056] <Solvent (C)> C-1: Ion-exchanged water C-2: A mixture of ion-exchanged water and isopropyl alcohol (mixture ratio 9:1) C-3: Fujifilm Wako Pure Chemical Corporation Product name: Ethyl acetate
[0057] <Thermal initiator (D)> D-1: Fujifilm Wako Pure Chemical Corporation Product name: Ammonium persulfate
[0058] <Monomer (E)> E-1: Fujifilm Wako Pure Chemical Corporation Product name: Acrylic acid E-2: Fujifilm Wako Pure Chemical Corporation Product name: Methacrylic acid
[0059] <Photoinitiator (F)> F-1: IGM Resins BV Product name: Omnirad-1173
[0060] <Base film (G)> G-1: Futamura Chemical Co., Ltd. Product name: FOH (30μm OPP film) G-2: Toyobo Co., Ltd. Product name: E5102 (25μm PET film)
[0061] <Synthesis of polymer particles> [Synthesis Example 1] (Synthesis of polymer microparticles 1) A reaction vessel was charged with 28 parts of a metal carboxylate (A-1) and 210 parts of a solvent (C-2), and heated to 70°C. At the same temperature, 40 parts of a solvent (C-2) containing 5 parts of a thermal initiator (D-1) was added dropwise over 1 hour while stirring in the reaction vessel. The precipitate was recovered and washed by filtration under reduced pressure, and dried under reduced pressure to obtain polymer microparticles 1.
[0062] [Synthesis Examples 2-7, 10-12] (Synthesis of polymer microparticles 2-7 and 10-12) As shown in Table 1, Synthesis Examples 2 to 7 and 10 to 12 were produced in the same manner as Synthesis Example 1, except that the carboxylic acid metal salt (A), the solvent (C), and the thermal initiator (D) were changed.
[0063] [Synthesis Example 8] A reaction vessel was charged with 15 parts of a metal carboxylate (A-1), 10 parts of a monomer (E-1), and 220 parts of a solvent (C-1), and heated to 70°C. At the same temperature, 50 parts of a solvent (C-1) containing 4 parts of a thermal initiator (D-1) was added dropwise over 1 hour while stirring in the reaction vessel. The precipitate was recovered and washed by filtration under reduced pressure, and dried under reduced pressure to obtain polymer microparticles 8.
[0064] [Synthesis Example 9] A reaction vessel was charged with 15 parts of a metal carboxylate (A-1), 10 parts of a monomer (E-2), and 220 parts of a solvent (C-1), and heated to 70°C. At the same temperature, 50 parts of a solvent (C-1) containing 4 parts of a thermal initiator (D-1) was added dropwise over 1 hour while stirring in the reaction vessel. The precipitate was recovered and washed by filtration under reduced pressure, and dried under reduced pressure to obtain polymer microparticles 9.
[0065] Next, the following tests were carried out using the synthesized microparticles, and the results are shown in Table 1. 1. Particle size evaluation The particle size of the synthesized microparticles was evaluated using SEM images observed under the following conditions. Measuring device: JSM-7800F, manufactured by JEOL Ltd. Measurement conditions: Accelerating voltage 5 kV Observation mode: Secondary electron observation Magnification: 10,000 to 50,000 times
[0066] [Table 1]
[0067] [Example 1] 75 parts of the polymer microparticles 1 obtained in Synthesis Example 1, 25 parts of the binder resin (B-1), and 315 parts of the solvent (C-2) were mixed and dispersed in a bead mill for 1 hour to obtain a resin composition 1. The resin composition 1 was applied onto a substrate (G-2) and dried at 70°C for 1 minute to obtain a laminate having a white resin composition layer (hereinafter, a white laminate).
[0068] [Examples 2 to 16, 23 to 25] Resin compositions were obtained in the same manner as in Example 1, except that the polymer microparticles obtained in Synthesis Examples 1 to 12, the commercially available microparticles, the resin (B), and the solvent (C) were changed as shown in Table 2. Furthermore, a white laminate was obtained by coating on a substrate (G) in the same manner as in Example 1.
[0069] [Example 17] 75 parts of the carboxylate metal salt (A-1), 1 part of the binder resin (B-1), 312 parts of the solvent (C-2), and 1 part of the photopolymerization initiator (F-1) were mixed and dispersed in a bead mill for 1 hour to obtain an intermediate resin composition. Next, the intermediate resin composition prepared above was applied onto a substrate (G-2), and the resulting coating was irradiated with 1000 (mJ / cm 2 ) of a high-pressure mercury lamp. 2 ) UV irradiation is used to create a white layer The particle diameter of the fine particles in the coating was 205 nm. The method for measuring the particle size of the fine particles in the coating film is the same as the method for measuring the particle size of the synthesized fine particles described above.
[0070] [Example 18] 80 parts of the carboxylate metal salt (A-2), 25 parts of the binder resin (B-1), 350 parts of the solvent (C-2), and 1 part of the photopolymerization initiator (F-1) were mixed and dispersed in a bead mill for 1 hour to obtain an intermediate resin composition. Next, the intermediate resin composition prepared above was applied onto a substrate (G-2), and the resulting coating was irradiated with 1000 (mJ / cm 2 ) of a high-pressure mercury lamp. 2 ) UV irradiation was performed to obtain a white laminate. The particle diameter of the fine particles in the coating film was 180 nm.
[0071] [Example 19] 81 parts of the carboxylate metal salt (A-1), 21 parts of the binder resin (B-1), 299 parts of the solvent (C-2), and 1 part of the photopolymerization initiator (F-1) were mixed and dispersed in a bead mill for 1 hour to obtain an intermediate resin composition. Next, the intermediate resin composition prepared above was applied onto a substrate (G-2), and the resulting coating was irradiated with 1000 (mJ / cm 2 ) of a high-pressure mercury lamp. 2 ) UV irradiation is used to create a white layer The particle diameter of the fine particles in the coating was 220 nm.
[0072] [Example 20] 68 parts of the carboxylate metal salt (A-1), 1 part of the binder resin (B-1), 312 parts of the solvent (C-2), and 1 part of the photopolymerization initiator (F-1) were mixed and dispersed in a bead mill for 1 hour to obtain an intermediate resin composition. Next, the intermediate resin composition prepared above was coated on a substrate (G-2), and the coating film obtained was irradiated with an electron beam of 4 Mrad (accelerating voltage 100 kV, current value 7 mA, conveyor speed 20 m / min) using an EB irradiation device to obtain a white laminate. The particle diameter of the fine particles in the coating film was 185 nm.
[0073] [Example 21] 86 parts of the carboxylate metal salt (A-2), 25 parts of the binder resin (B-1), and 300 parts of the solvent (C-2) were mixed and dispersed in a bead mill for 1 hour to obtain an intermediate resin composition. Next, the intermediate resin composition prepared above was coated on a substrate (G-2), and the coating film obtained was irradiated with an electron beam of 4 Mrad (accelerating voltage 100 kV, current value 7 mA, conveyor speed 20 m / min) using an EB irradiation device to obtain a white laminate. The particle diameter of the fine particles in the coating film was 190 nm.
[0074] [Example 22] 75 parts of the carboxylate metal salt (A-1), 24 parts of the binder resin (B-1), and 299 parts of the solvent (C-2) were mixed and dispersed in a bead mill for 1 hour to obtain an intermediate resin composition. Next, the intermediate resin composition prepared above was coated on a substrate (G-2), and the resulting coating was irradiated with an electron beam of 4 Mrad (accelerating voltage 100 kV, current value 7 mA, conveyor speed 20 m / min) using an EB irradiation device to obtain a white laminate. The particle diameter of the fine particles in the coating was 210 nm.
[0075] [Comparative Example 1] 75 parts of commercially available ZnO powder (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was mixed with 25 parts of binder resin (B-2) and 300 parts of solvent (C-2), and dispersed in a bead mill for 1 hour to obtain an intermediate resin composition. The intermediate resin composition prepared above was applied onto a substrate (G-2) and dried at 70°C for 1 minute to obtain a white laminate. The particle diameter of the fine particles in the coating was 170 nm.
[0076] Next, the following tests were carried out using the white laminate thus produced. 2. Concealment rate The hiding rate of the white laminate was measured by placing the resin composition coated side of the white laminate produced in Examples 1 to 22 and Comparative Example 1 on a black paper and placing the detection part of a spectrophotometer (X-rite eXact, manufactured by X-Rite, Inc.) from above (the coated side of the white laminate) to measure the L value, which indicates whiteness. The white hiding property was evaluated using the following three-level scale as the criterion. The evaluation results are shown in Table 2. The L value in a similar evaluation using titanium oxide was in the range of 84 or less and 75 or more. ◎: L value is 85 or more 〇: L value is 84 or less and 75 or more △: L value is 74 or less and 70 or more ×: L value is 69 or less
[0077] 3. Film Thickness For the white laminates produced in Examples 1 to 25 and Comparative Example 1, the film thickness of the resin composition layer not containing the substrate was measured using a length measuring machine. The results are shown in Table 2.
[0078] 4. Metal content The white laminates produced in Examples 1 to 25 and Comparative Example 1 were measured and evaluated for the content of metal components contained in the solid content of the resin composition layer not including the substrate after drying. Specifically, the ratio of metal atoms to the total solid content was calculated in mass %, and the content was evaluated into the following three levels. The results are shown in Table 2. ◎: Content is less than 28% ○: Content is 28% or more but less than 50% ×: Content is 50% or more
[0079] [Table 2]
Claims
1. A resin composition comprising polymer fine particles of a metal salt of a carboxylate having an unsaturated bond (A) and a binder resin (B).
2. 2. The resin composition according to claim 1, wherein the metal salt of a carboxylate having an unsaturated bond (A) is a metal salt of (meth)acrylic acid.
3. 2. The resin composition according to claim 1, wherein the metal salt of a carboxylate having an unsaturated bond (A) contains one or more metal ions selected from the group consisting of zinc ions, magnesium ions, calcium ions, aluminum ions and titanium ions.
4. 4. The resin composition according to claim 3, wherein the metal salt of a carboxylate having an unsaturated bond (A) contains a zinc ion.
5. 2. The resin composition according to claim 1, wherein the polymer fine particles have a particle size of 50 to 500 nm.
6. 2. The resin composition according to claim 1, wherein the binder resin (B) is a polymer of vinyl alcohol and / or vinyl chloride.
7. 2. The resin composition according to claim 1, wherein the content of said polymer fine particles is 50 to 99 mass % based on 100 mass % of the solid content of the resin composition.
8. 2. The resin composition according to claim 1, wherein the polymer has a metal salt of a carboxylic acid in a side chain.
9. The resin composition according to claim 1, further comprising a solvent (C).
10. 2. The resin composition according to claim 1, which is a paint or ink.
11. A laminate comprising a substrate and a resin composition layer formed by coating or printing the resin composition according to any one of claims 1 to 10 on the substrate.
12. A method for producing a resin composition containing fine particles consisting of a polymer of a metal salt of a carboxylate (A) having an unsaturated bond and a binder resin (B), characterized in that the polymer is obtained by at least one polymerization reaction selected from the group consisting of EB irradiation, UV irradiation, and heating.
Citation Information
Patent Citations
Production of highly masking white pigment
JP1994093204A