Epoxy resin composition, cured product, and damping material
The epoxy resin composition with a (meth)acrylic graft copolymer and curing agent achieves superior vibration damping performance from -40°C to 70°C by formulating a tan δ peak of 0.15 or more, addressing the inadequacies of existing compositions.
Patent Information
- Application Number
- JP2024050114
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-11
AI Technical Summary
Existing epoxy resin compositions do not adequately satisfy vibration damping performance across the general temperature range of -40°C to 70°C.
An epoxy resin composition containing a (meth)acrylic graft copolymer, an epoxy resin, and a curing agent, with optional inclusion of a curing accelerator, formulated to achieve a tan δ peak of 0.15 or more in the temperature range of -40°C to 70°C, enhancing vibration damping properties.
The composition yields a cured product with excellent vibration damping performance across the required temperature range, effectively dissipating mechanical energy as thermal energy.
Smart Images

Figure 2024144318000001 
Figure 2024144318000002 
Figure 2024144318000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an epoxy resin composition, a cured product, and a vibration damping material. [Background technology]
[0002] Epoxy resins have excellent rigidity, heat resistance, electrical properties, durability, etc., and are therefore used in components, molding materials, fiber-reinforced plastics, etc. for civil engineering and construction applications, vehicle applications, electronic materials applications, industrial applications, etc. In recent years, there has been a demand for these applications to function as vibration-damping materials to reduce noise and vibration, and in order to impart vibration-damping properties to epoxy resins, polymers that have a low glass transition temperature and are rubber-like at room temperature are being blended into them.
[0003] For example, Patent Document 1 proposes a vibration-damping thermosetting resin composition containing a thermosetting resin and a graft copolymer, and describes that the thermoplastic elastomer constituting the graft copolymer has excellent vibration-damping properties due to viscoelasticity over a wide temperature range including room temperature, and therefore the cured product of the vibration-damping thermosetting resin composition exhibits vibration-damping performance. Furthermore, Patent Document 2 proposes a prepreg in which reinforcing fibers are impregnated with an epoxy resin composition, and describes that by including an acrylic block copolymer with high vibration damping properties in the epoxy resin composition, a molded product obtained by curing the prepreg exhibits excellent vibration damping performance.
[0004] Patent Document 3 proposes a composite resin composition containing a non-polar polymer and a viscoelastic polymer such as an acrylic resin, and discloses that the viscoelastic polymer having vibration damping properties forms a bicontinuous phase structure in the composite resin composition, thereby achieving highly satisfactory vibration damping performance. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2002-3819 A [Patent Document 2] JP 2020-50833 A [Patent Document 3] JP 2003-105060 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, the resin compositions described in Patent Documents 1 to 3 do not necessarily have satisfactory vibration damping performance.
[0007] An object of the present invention is to provide an epoxy resin composition which can give a cured product having excellent vibration-damping performance in the general temperature range of -40°C to 70°C where vibration-damping performance is required, and a cured product thereof, and a vibration-damping material. [Means for solving the problem]
[0008] The present invention has the following aspects. [1] An epoxy resin composition comprising a (meth)acrylic graft copolymer (A), an epoxy resin (B) and a curing agent (C), wherein a cured product of the epoxy resin composition has a tan δ peak intensity of 0.15 or more in a temperature range of -40°C to 70°C. [2] The epoxy resin composition according to [1], further comprising a curing accelerator (D). [3] The epoxy resin composition according to [1] or [2], wherein a cured product of the epoxy resin composition has a tan δ peak at 100°C or higher. [4] The epoxy resin composition according to any one of [1] to [3], wherein the (meth)acrylic graft copolymer (A) contains a structural unit derived from a macromonomer (M) and a structural unit derived from a vinyl radically polymerizable monomer (a1). [5] The epoxy resin composition according to [4], wherein the macromonomer (M) has a structure represented by the following formula (1):
[0009] [ka]
[0010] (In formula (1), X 1 ~X n-1 are each independently a hydrogen atom, a methyl group, or CHOH; Y 1 ~Y n each independently represents X bonded to a vinyl group of the vinyl radical polymerizable monomer (a2) which is a monomer constituent unit of the macromonomer (M). 1 ~X n-1 Z is a terminal group, and n is an integer of 2 to 10,000. [6] A cured product of the epoxy resin composition according to any one of [1] to [5]. [7] A vibration-damping material comprising the cured product described in [6]. Effect of the Invention
[0011] According to the present invention, it is possible to provide an epoxy resin composition capable of giving a cured product having excellent vibration-damping performance in the general temperature range of -40°C to 70°C where vibration-damping performance is required, and a cured product thereof, and a vibration-damping material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described in detail below. The following embodiments are merely examples for explaining the present invention, and are not intended to limit the present invention to these embodiments. The present invention can be implemented in various forms without departing from the spirit of the present invention. In the present invention, "(meth)acrylic" is a general term for "acrylic" and "methacrylic". "(meth)acrylate" is a general term for "acrylate" and "methacrylate". "(meth)acryloyl group" is a general term for "acryloyl group" and "methacryloyl group", and is a group represented by CH2=C(R)-C(=O)- (R is a hydrogen atom or a methyl group). The term "macromonomer" refers to a compound having a radical polymerizable group or an addition-reactive functional group. The number average molecular weight (Mn) is usually 1,000 to 1,000,000. The term "vinyl radically polymerizable monomer" refers to a monomer having an ethylenically unsaturated bond that is not a macromonomer. The "cured product" refers to a cured product of the epoxy resin composition of the present invention.
[0013] [Epoxy resin composition] The epoxy resin composition of the present invention contains a (meth)acrylic graft copolymer (A) (hereinafter also referred to as "component (A)"), an epoxy resin (B) (hereinafter also referred to as "component (B)"), and a curing agent (C) (hereinafter also referred to as "component (C)"). The epoxy resin composition of the present invention may further contain a curing accelerator (D) (hereinafter also referred to as "component (D)"). In addition, the epoxy resin composition may contain components other than components (A) to (D) (hereinafter also referred to as "optional components") as necessary, within the scope of not impairing the effects of the present invention.
[0014] <Component (A)> The component (A) is a graft copolymer in which at least a part of the constituent units is derived from a (meth)acrylic monomer. The component (A) may further contain a constituent unit derived from a vinyl radical polymerizable monomer (such as styrene) other than the (meth)acrylic monomer.
[0015] Component (A) is a graft copolymer composed of a main chain polymer structure and a side chain polymer structure (branch polymer structure) chemically bonded to the main chain polymer structure (trunk polymer structure). In this specification, a "graft copolymer" is a polymer having one or more types of blocks connected as side chain polymer structures to the main chain polymer structure. The structures of the main chain polymer and the side chain polymer may be different or the same.
[0016] The method for producing the graft copolymer is not particularly limited, and examples thereof include a method in which a macromonomer having a radically polymerizable double bond at an end is produced as a side chain polymer structure, and then radically polymerized with a monomer that becomes a constituent unit of the main chain polymer; a method in which a main chain polymer having a reactive site and a macromonomer having a reactive site are produced in advance, and then reacted with each other; and a method in which, after the production of the main chain polymer, a radical is generated on the main chain polymer using an initiator having a hydrogen abstraction ability, and then a monomer that becomes a constituent unit of the side chain polymer is reacted to produce a side chain polymer structure.
[0017] The component (A) preferably contains a structural unit derived from a vinyl radically polymerizable monomer (a1) (hereinafter also referred to as "component (a1)") and a structural unit derived from a macromonomer (M) (hereinafter also referred to as "component (M)").
[0018] Examples of the (a1) component include monofunctional (meth)acrylates, polyfunctional (meth)acrylates, and vinyl compounds other than monofunctional (meth)acrylates and polyfunctional (meth)acrylates (hereinafter also referred to as "other vinyl compounds").
[0019] Specific examples of monofunctional (meth)acrylates include (meth)acrylic acid, (meth)acryloyloxyethyl succinate, 2-(meth)acryloyloxyethyl maleate, 2-(meth)acryloyloxyethyl phthalate, and 2-(meth)acryloyloxyethyl hexahydrophthalate, and other (meth)acrylates containing a carboxyl group; methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, and i-propyl (meth)acrylate. Pyr(meth)acrylate, i-butyl(meth)acrylate, t-butyl(meth)acrylate, s-butyl(meth)acrylate, n-pentyl(meth)acrylate, n-hexyl(meth)acrylate, n-heptyl(meth)acrylate, n-octyl(meth)acrylate, n-nonyl(meth)acrylate, n-decyl(meth)acrylate, n-undecyl(meth)acrylate, n-dodecyl(meth)acrylate, n-tridecyl(meth)acrylate, n-tetradecyl(meth)acrylate Acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, behenyl (meth)acrylate, i-amyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, i-nonyl (meth)acrylate, i-decyl (meth)acrylate, 3-i-propylheptyl (meth)acrylate, i-undecyl (meth)acrylate, 2-t-butylheptyl (meth)acrylate, i-dodecyl (meth)acrylate, i-tridecyl (meth)acrylate, i-tetradecyl (meth)acrylates having an alkyl group, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, glycerin mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, and polypropylene glycol mono(meth)acrylate;(Meth)acrylates having a cycloalkyl group such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenoxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, adamantyl (meth)acrylate, and 1,4-cyclohexanedimethanol monoacrylate; phenyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, nonylphenoxypolyethylene glycol (meth)acrylate, phenoxypolypropylene glycol (meth)acrylate, phenylphenyl (meth)acrylate, phenylphenoxyethyl (meth)acrylate, (Meth)acrylates having an aryl group, such as phenoxybenzyl (meth)acrylate, phenylbenzyl (meth)acrylate, naphthyl (meth)acrylate, and (1-naphthyl)methyl (meth)acrylate; (meth)acrylates having a cyclic ether group, such as tetrahydrofurfuryl (meth)acrylate, glycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, (meth)acryloylmorpholine, (3,4-epoxycyclohexyl)methyl (meth)acrylate, β-methylglycidyl (meth)acrylate, (3-ethyloxetan-3-yl)methyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl) (meth)acrylate, and (5-ethyl-1,3-dioxan-5-yl)methyl (meth)acrylate;Methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, 2-ethylhexyloxyethyl (meth)acrylate, methoxyethylethylene glycol (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, butoxydiethylene glycol (meth)acrylate, 2-ethylhexyloxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate, and other alkoxy (meth)acrylates; 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 2-(meth)acryloyloxyethyl acid phosphate, trifluoroethyl (meth)acrylate, heptadecafluorodecyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, (meth)acrylamide, and the like. These monofunctional (meth)acrylates may be used alone or in combination of two or more kinds.
[0020] Specific examples of polyfunctional (meth)acrylates include ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate, polybutylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, polycarbonate diol di(meth)acrylate, polyester diol di(meth)acrylate, bisphenol A ethylene oxide adduct di(meth)acrylate, bisphenol A dimeth ... Examples of the functional (meth)acrylate include difunctional (meth)acrylates such as propylene oxide adduct di(meth)acrylate of terephthalic acid A, polyurethane di(meth)acrylate, and 9,9-bis[4-(2-(meth)acryloyloxyethoxy)phenyl]fluorene; trifunctional (meth)acrylates such as trimethylolpropane tri(meth)acrylate, ethoxylated isocyanuric acid tri(meth)acrylate, and ε-caprolactone-modified tris((meth)acryloxyethyl)isocyanurate; tetrafunctional (meth)acrylates such as ditrimethylolpropane tetra(meth)acrylate; pentafunctional (meth)acrylates such as dipentaerythritol penta(meth)acrylate; and hexafunctional (meth)acrylates such as dipentaerythritol hexa(meth)acrylate. These polyfunctional (meth)acrylates may be used alone or in combination of two or more kinds.
[0021] The other vinyl-based compound is not particularly limited as long as it is copolymerizable with the monofunctional (meth)acrylate and the polyfunctional (meth)acrylate, and examples thereof include styrene or styrene derivatives such as styrene, α-methylstyrene, pt-butylstyrene, vinyltoluene, etc.; acrylamides such as N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, etc.; unsaturated carboxylic acids such as itaconic acid, maleic acid, fumaric acid, etc.; unsaturated nitriles such as (meth)acrylonitrile, etc.; unsaturated carboxylic acid esters such as diethyl maleate, dibutyl maleate, dibutyl fumarate, diethyl itaconate, dibutyl itaconate, etc.; and vinyl esters such as vinyl acetate, vinyl propionate, etc. These other vinyl compounds may be used alone or in combination of two or more.
[0022] As the (a1) component, from the viewpoint of achieving good vibration-damping characteristics at -40°C to 70°C, a (meth)acrylate having an alkyl group with 1 to 8 carbon atoms is preferred, a (meth)acrylate having an alkyl group with 1 to 4 carbon atoms is more preferred, a methacrylate having an alkyl group with 1 to 4 carbon atoms is even more preferred, and i-butyl methacrylate is particularly preferred.
[0023] From the viewpoints of improving the solubility of component (A) in component (B) and of improving vibration damping properties, the structural unit derived from component (a1) is preferably contained in an amount of 50 to 99 mass%, more preferably 70 to 98 mass%, and even more preferably 85 to 97 mass% or more, relative to 100 mass% of the total amount of component (A).
[0024] The component (M) is a high molecular weight compound (macromonomer) having a radically polymerizable group or an addition-reactive functional group. The component (M) is not particularly limited as long as it is a high molecular weight compound having a radically polymerizable group or an addition-reactive functional group, but from the standpoint of high degree of design for the solubility of the component (A) in the component (B), it is preferably a compound containing a structural unit derived from vinyl radically polymerizable monomer (a2) (hereinafter also referred to as "component (a2)"), and more preferably a compound containing two or more structural units derived from the component (a2) and having a radically polymerizable group at its terminal.
[0025] As the (a2) component, from the viewpoint of improving the solubility of the (A) component in the (B) component, a (meth)acrylate having a cyclic ether group is preferable, a (meth)acrylate having an epoxy group is more preferable, glycidyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate glycidyl ether are further preferable, and glycidyl (meth)acrylate is particularly preferable. The component (M) may be used alone or in combination of two or more types.
[0026] From the viewpoints of improving the solubility of the component (A) in the component (B) and of improving vibration damping properties, the structural unit derived from the component (M) is preferably contained in an amount of 1 to 50 mass%, more preferably 2 to 30 mass%, and even more preferably 3 to 15 mass%, relative to 100 mass% of the total amount of the component (A).
[0027] The component (M) preferably has a structure represented by the following general formula (1) from the viewpoint of excellent radical polymerizability with the component (a1).
[0028] [ka]
[0029] In formula (1), X 1 ~X n-1 are each independently a hydrogen atom, a methyl group, or CHOH; Y 1 ~Y neach independently represents X bonded to a vinyl group of the vinyl radical polymerizable monomer (a2) which is a monomer constituent unit of the macromonomer (M). 1 ~X n-1 Z is a terminal group, and n is an integer of 2 to 10,000. In addition, "-···-" in formula (1) represents a state in which the monomer units are polymerized.
[0030] X 1 ~X n-1 are each independently a hydrogen atom, a methyl group, or CHOH, and a methyl group is preferred. From the viewpoint of ease of synthesis, X 1 ~X n-1 It is preferable that at least half of the groups are methyl groups. Y 1 ~Y n each independently represents X bonded to a vinyl group of the vinyl radical polymerizable monomer (a2) which is a monomer constituent unit of the macromonomer (M). 1 ~X n-1 Examples of such substituents include OR 1 , halogen atom, COR 2 , COOR 3 , C.N., C.O.N. 4 R 5 , N.H.C.O.R. 6 , or R 7 In addition, R 1 ~R 7 are each independently a hydrogen atom, an alkyl group, a cycloalkyl group, a cyclic ether group, an aryl group, a heteroaryl group, or the like. Z is a terminal group. The terminal group may be a hydrogen atom or a group derived from a radical polymerization initiator, similar to the terminal groups of polymers obtained by known radical polymerization. The symbol n represents the number of monomer units in one molecule of the component (M), and is an integer from 2 to 10,000, preferably an integer from 5 to 1,000, and more preferably an integer from 10 to 500.
[0031] The number average molecular weight (Mn) of the component (M) is preferably from 300 to 30000, more preferably from 500 to 20000, and even more preferably from 1000 to 10000. When the number average molecular weight of the component (M) is within the above range, the solubility in the component (B) is improved. The mass average molecular weight (Mw) of the component (M) is preferably from 500 to 100000, more preferably from 1000 to 50000, and even more preferably from 2000 to 30000. When the mass average molecular weight of the component (M) is within the above range, the solubility in the component (B) is improved. The Mw / Mn of the component (M) is preferably from 1 to 5, and more preferably from 1.5 to 3. When the Mw / Mn of the component (M) is within the above range, the solubility in the component (B) is improved. The number average molecular weight (Mn) and weight average molecular weight (Mw) of the component (M) are each values calculated as polystyrene equivalents measured by gel permeation chromatography (GPC).
[0032] The component (M) may be one produced by a known method, or a commercially available product. Examples of methods for producing the component (M) include a production method using a cobalt chain transfer agent (U.S. Patent No. 4,680,352, etc.), a method using an α-substituted unsaturated compound such as α-bromomethylstyrene as a chain transfer agent (WO 1988 / 04304), a method in which a polymerizable group is chemically bonded (JP-A-60-133007 and U.S. Patent No. 5,147,952, etc.), and a method using thermal decomposition (JP-A-11-240854, etc.). The method of producing component (M) is preferably a method using a cobalt chain transfer agent, since it requires fewer production steps and uses a catalyst with a high chain transfer constant. Because the cobalt chain transfer agent has a high chain transfer constant, it is possible to obtain component (M) with a controlled molecular weight by adding a small amount of the agent.
[0033] As the cobalt chain transfer agent, a known cobalt complex can be used. The amount of the cobalt chain transfer agent used is preferably 0.00001 to 0.1 parts by mass, more preferably 0.00005 to 0.05 parts by mass, and even more preferably 0.0001 to 0.02 parts by mass, based on 100 parts by mass of the components (a1) and (a2).
[0034] The component (A) and the macromonomer (M) can be produced, for example, by solution polymerization, suspension polymerization, emulsion polymerization, or the like. The polymerization can be carried out by a known method such as polymerization or redox polymerization.
[0035] The mass average molecular weight (Mw) of component (A) is preferably 10,000 to 1,000,000, more preferably 20,000 to 800,000, and even more preferably 30,000 to 600,000. When the mass average molecular weight of component (A) is within the above range, the solubility of component (A) in component (B) becomes better. The number average molecular weight (Mn) of the component (A) is preferably from 3,000 to 300,000, more preferably from 50,000 to 200,000, and even more preferably from 10,000 to 100,000. When the number average molecular weight of the component (A) is within the above range, the solubility of the component (A) in the component (B) is improved. The Mw / Mn of component (A) is preferably from 1 to 20, and more preferably from 1.5 to 15. When the Mw / Mn of component (A) is within the above range, the solubility of component (A) in component (B) becomes better. The number average molecular weight (Mn) and weight average molecular weight (Mw) of the component (A) are each values calculated as polystyrene equivalents measured by gel permeation chromatography (GPC). These components (A) may be used alone or in combination of two or more.
[0036] <(B) component> Component (B) is an epoxy resin. Examples of the component (B) include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AD type epoxy resins, bisphenol E type epoxy resins, naphthalene type epoxy resins, biphenyl type epoxy resins, dicyclopentadiene type epoxy resins, phenol novolac type epoxy resins, alicyclic epoxy resins, and glycidylamine type epoxy resins. Examples of the component (B) include prepolymers of the above-mentioned epoxy resins, copolymers of the above-mentioned epoxy resins with other polymers, such as polyether-modified epoxy resins and silicone-modified epoxy resins, and those in which a portion of the above-mentioned epoxy resins has been substituted with a reactive diluent having an epoxy group.
[0037] Examples of reactive diluents include monoglycidyl compounds such as resorcinol glycidyl ether, t-butylphenyl glycidyl ether, 2-ethylhexyl glycidyl ether, allyl glycidyl ether, phenyl glycidyl ether, 3-glycidoxypropyl trimethoxysilane, 3-glycidoxypropyl methyl dimethoxysilane, 1-(3-glycidoxypropyl)-1,1,3,3,3-pentamethylsiloxane, and N-glycidyl-N,N-bis[3-(trimethoxysilyl)propyl]amine; and monoalicyclic epoxy compounds such as 2-(3,4)-epoxycyclohexyl)ethyltrimethoxysilane. These reactive diluents may be used alone or in combination of two or more. Among these, bisphenol A type epoxy resins and bisphenol F type epoxy resins are preferred as component (B) because they are liquid and easy to handle, and because they have high glass transition temperatures and thus improve the heat resistance of the cured product. These components (B) may be used alone or in combination of two or more.
[0038] <(C) component> The component (C) cures the component (B) and is used to adjust the curability of the epoxy resin composition and the properties of the cured product. As the component (C), known compounds can be used, such as acid anhydrides, amine compounds, phenol compounds, and latent hardeners.
[0039] Specific examples of the component (C) include acid anhydrides such as phthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, hexahydrophthalic anhydride, tetrahydrophthalic anhydride, trialkyltetrahydrophthalic anhydride, methylhimic anhydride, methylcyclohexene dicarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, benzophenone tetracarboxylic anhydride, ethylene glycol bistrimellitate, glycerol tristrimellitate, dodecenylsuccinic anhydride, polyazelaic anhydride, and poly(ethyloctadecanedioic) anhydride;2,5(2,6)-bis(aminomethyl)bicyclo[2,2,1]heptane, isophoronediamine, ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, diethylaminopropylamine, bis(4-amino-3-methyldicyclohexyl)methane, diaminodicyclohexylmethane, bis(aminomethyl)cyclohexane, bis(aminomethyl)norbornane, bis(4-aminocyclohexyl)methane, metaphenylenediamine, diaminodiphenylmethane, diaminodiphenylsulfone, diaminodiethyldiphenylmethane, diethyltoluenediamine, diaminodiphenylsulfones such as 3,3'-diaminodiphenylsulfone (3,3'-DDS), 4,4'-diaminodiphenylsulfone (4,4'-DDS), diaminodiphenylether (DADPE), bisaniline, dimethylaniline, triethylenediamine, dimethylbenzylamine, 2,4,6-tris(dimethylaminomethyl) amine compounds such as phenol, benzyldimethylaniline, 3,3'-dichloro-4,4'-diaminodiphenylmethane (MOCA), 4,4'-diaminodiphenylmethane, 2,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 2,2'-diaminobiphenyl, 3,3'-diaminobiphenyl, 2,4-diaminophenol, 2,5-diaminophenol, o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, m-xylylenediamine, 2,3-tolylenediamine, 2,4-tolylenediamine, 2,5-tolylenediamine, 2,6-tolylenediamine, 3,4-tolylenediamine, methylthiotoluenediamine, diethyltoluenediamine, and dicyandiamide; phenol compounds such as phenol novolac resin, cresol novolac resin, bisphenol A, bisphenol F, bisphenol AD, and diallylated derivatives of these bisphenols;Carbohydrazide, oxalic acid dihydrazide, malonic acid dihydrazide, succinic acid dihydrazide, iminodiacetic acid dihydrazide, adipic acid dihydrazide, pimelic acid dihydrazide, suberic acid dihydrazide, azelaic acid dihydrazide, sebacic acid dihydrazide, dodecane dihydrazide, hexadecane dihydrazide, maleic acid dihydrazide, fumaric acid dihydrazide, diglycol Examples of hydrazide compounds include carboxylic acid dihydrazide, tartaric acid dihydrazide, malic acid dihydrazide, isophthalic acid dihydrazide, terephthalic acid dihydrazide, 2,6-naphthoic acid dihydrazide, 4,4'-bisbenzenedihydrazide, 1,4-naphthoic acid dihydrazide, Amicure VDH, Amicure UDH (all trade names, manufactured by Ajinomoto Co., Inc.), and citric acid trihydrazide;
[0040] Among these, from the viewpoint of improving the storage stability of the epoxy resin composition, the component (C) is preferably an amine compound or a hydrazide compound, and more preferably dicyandiamide or a hydrazide compound. These components (C) may be used alone or in combination of two or more.
[0041] <(D) component> The epoxy resin composition of the present invention may contain a curing accelerator (D). As the component (D), a known catalyst used as a thermosetting catalyst for epoxy resins can be used, such as 3-(3,4-dichlorophenyl)-1,1-dimethylurea (DCMU), 2-methylimidazole, 2-ethyl-4-methylimidazole, adducts of imidazole compounds and epoxy resins, triphenylphosphine, tetraphenylphosphine tetraphenylborate, and diazabicycloundecene (DBU).
[0042] Among these, 3-(3,4-dichlorophenyl)-1,1-dimethylurea (DCMU) is preferred as component (D) because it can provide good storage stability to the epoxy resin composition and sufficient curability to obtain a cured product. These components (D) may be used alone or in combination of two or more.
[0043] <Optional ingredients> Optional components include, for example, 2,6-di-t-butylphenol, 2,6-di-t-butyl-p-cresol, n-octadecyl-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate, tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane, triethylene glycol bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], triethyl phosphite, tri(2-ethylhexyl)phosphite, tridecyl phosphite, triphenyl phosphite, trisisodecyl phosphite, tristridecyl phosphite, tris(2,4-di-t-butylphenyl)phosphite, dihexyl antioxidants such as rufide, dilauryl-3,3'-thiodipropionate, ditridecyl-3,3'-thiodipropionate, dimyristyl-3,3'-thiodipropionate, distearic-3,3'-thiodipropionate, pentaerythritol tetrakis (β-laurylthiopropionate); release agents such as silicone oil, natural wax, and synthetic wax; fillers such as glass beads, crystalline silica, fused silica, calcium silicate, alumina, and calcium carbonate; fibers such as glass fiber, carbon fiber, alumina fiber, and cellulose nanofiber; flame retardants such as antimony trioxide; halogen trapping agents such as hydrotalcite and rare earth oxides; colorants such as carbon black and red iron oxide; silane coupling agents; rubber materials such as NBR, SBR, and polymers having a core-shell structure; defoamers; rheology adjusters: pigments; and dyes. These optional components may be used alone or in combination of two or more.
[0044] <Content> When the total mass of the components (A) to (D) is taken as 100 mass %, the preferred content of each component is as follows. The content of the component (A) is preferably 1 to 60 mass%, more preferably 5 to 55 mass%, and even more preferably 10 to 50 mass%, because this allows the epoxy resin composition to have a low viscosity with good workability while further improving the vibration damping properties of the cured product. The content of the (B) component is preferably 20 to 90 mass %, more preferably 30 to 80 mass %, and even more preferably 40 to 70 mass %, because this allows the epoxy resin composition to have a low viscosity and good workability. The content of the (C) component is preferably 0.1 to 10 mass%, more preferably 0.5 to 9 mass%, and even more preferably 1 to 8 mass%, because this provides sufficient curability to obtain a cured product while improving the storage stability of the epoxy resin composition. The content of the (D) component is preferably 0 to 5 mass%, more preferably 0.01 to 3 mass%, and even more preferably 0.05 to 1 mass%, because this provides sufficient curability to obtain a cured product while improving the storage stability of the epoxy resin composition.
[0045] <Manufacturing method> The method for producing the epoxy resin composition is not particularly limited, and known methods can be used. For example, the (A), (B) and (C) components, and optionally the (D) component and optional components may be mixed simultaneously, or some of the components (e.g., the (A) and (B) components) may be mixed in advance, and the mixture may be mixed with the remaining components. The mixing method is not particularly limited, and a known mixer such as a planetary centrifugal mixer, a three-roll mill, or a kneader can be used.
[0046] [Cured product] The cured product of the present invention is obtained by curing the above-mentioned epoxy resin composition of the present invention. The method for curing the epoxy resin composition is not particularly limited, and any known method can be used, such as a thermal curing method. When the epoxy resin composition is cured by a heat curing method, the optimal conditions vary depending on the type and amount of the component (C) contained in the epoxy resin composition, but it is preferable to cure the epoxy resin composition under heating conditions of, for example, 50 to 250°C for about 0.1 to 10 hours.
[0047] <Dynamic viscoelasticity measurement> The cured product of the present invention has a tan δ peak with a peak intensity of 0.15 or more in the general temperature range of −40° C. to 70° C. where vibration-damping performance is required. If the tan δ peak intensity is high, the mechanical energy imparted by the viscoelastic behavior can be dissipated as thermal energy, and the energy can be attenuated more effectively. The peak intensity of tan δ is more preferably 0.20 or more, further preferably 0.25 or more, and particularly preferably 0.30 or more.
[0048] The cured product of the present invention preferably has a tan δ peak in the range of -20°C to 70°C, more preferably in the range of 0°C to 70°C, even more preferably in the range of 10°C to 70°C, and particularly preferably in the range of 20°C to 70°C.
[0049] In order to provide good rigidity and heat resistance, the cured product of the present invention preferably has a peak tan δ at 100°C or higher, more preferably has a peak tan δ at 110°C or higher, even more preferably has a peak tan δ at 120°C or higher, and particularly preferably has a peak tan δ at 130°C or higher.
[0050] <Action and effect> The epoxy resin composition of the present invention described above contains the above-mentioned components (A), (B) and (C), and optionally contains component (D) and optional components. Therefore, a cured product obtained by curing the epoxy resin composition has a peak intensity of tan δ of 0.15 or more at −40° C. to 70° C. as determined by dynamic viscoelasticity measurement, and has excellent vibration damping properties.
[0051] <Application> INDUSTRIAL APPLICABILITY The epoxy resin composition of the present invention is useful as a vibration damping material since it gives a cured product having high vibration damping properties. The use of the epoxy resin composition of the present invention is not limited to the above. The epoxy resin composition of the present invention can also be used for other purposes, for example, for various purposes in which thermosetting resins such as epoxy resins are used. Examples of such uses include paints, coating agents, insulating materials, sealants, etc. The vibration damping material containing the epoxy resin composition of the present invention will be described below.
[0052] [Vibration damping material] The vibration damping material of the present invention comprises a cured product of the above-mentioned epoxy resin composition of the present invention. The vibration-damping material may be in the form of a sheet, film, coating, fiber-reinforced plastics obtained by impregnating fibers with the epoxy resin composition of the present invention and curing the fibers, etc. The applications of the vibration-damping material include, for example, vibration-damping materials for civil engineering and construction, vibration-damping materials for vehicles, vibration-damping materials for electronic materials, etc. EXAMPLES
[0053] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention. In each of the following examples, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".
[0054] [Measurement and evaluation method] <Measurement of molecular weight of macromonomer (M)> The molecular weight of the (M) component was measured using a gel permeation chromatograph (GPC apparatus) (manufactured by Tosoh Corporation, product name "HLC-8320") as follows. The component (M) was dissolved in tetrahydrofuran (THF) to a concentration of 0.2% by mass to prepare a THF solution (1). 10 μL of the above THF solution (1) was injected into a GPC apparatus equipped with columns manufactured by Tosoh Corporation (TSKgel SuperHZM-M (inner diameter 4.6 mm, length 15 cm) x 1, HZM-M (inner diameter 4.6 mm, length 15 cm) x 1, HZ-2000 (inner diameter 4.6 mm, length 15 cm) x 1, TSKguardcolumn SuperHZ-L (inner diameter 4.6 mm, length 3.5 cm) x 1), and measurements were performed under the following conditions: flow rate: 0.35 mL / min, eluent: THF containing dibutylhydroxytoluene (BHT) as a stabilizer, column temperature: 40°C, and the mass average molecular weight (Mw) and number average molecular weight (Mn) were calculated in terms of standard polystyrene.
[0055] <Measurement of Molecular Weight of (Meth)acrylic Graft Copolymer (A)> The molecular weight of the (meth)acrylic graft copolymer (A) was measured using a gel permeation chromatograph (GPC apparatus) (manufactured by Tosoh Corporation, product name "HLC-8320") as follows. The (meth)acrylic graft copolymer (A) was dissolved in tetrahydrofuran (THF) to a concentration of 0.2% by mass to prepare a THF solution (2). 10 μL of the above THF solution (2) was injected into a GPC apparatus equipped with columns manufactured by Tosoh Corporation (2 TSKgel SuperHZM-H (inner diameter 6.0 mm, length 15 cm), 1 TSKguardcolumn SuperHZ-H (inner diameter 4.6 mm, length 3.5 cm)), and measurement was performed under the conditions of a flow rate of 0.5 mL / min, eluent: THF containing BHT as a stabilizer, and column temperature: 40° C., and the mass average molecular weight (Mw) and number average molecular weight (Mn) were calculated in terms of standard polystyrene.
[0056] <Evaluation of vibration damping characteristics> The epoxy resin composition was heated at 180°C for 30 minutes to obtain a flat-plate-shaped cured product with a width of 5 mm, length of 30 mm, and thickness of 0.5 mm. A dynamic viscoelasticity measuring device (manufactured by UBM, product name "Reogel-E4000") was used to measure at a frequency of 1 Hz and at temperatures ranging from -100°C to 200°C. The peak strength of tan δ of the obtained cured product at temperatures ranging from -40°C to 70°C was obtained to evaluate the vibration damping properties. A higher peak strength of tan δ at temperatures ranging from -40°C to 70°C indicates better vibration damping properties.
[0057] [Dispersant] <Synthesis Example 1: Synthesis of Dispersant (1)> In a polymerization apparatus equipped with a stirrer, a cooling tube, a thermometer, and a nitrogen gas inlet tube, 900 parts of deionized water, 60 parts of 2-sulfoethyl sodium methacrylate, 10 parts of potassium methacrylate, and 12 parts of methyl methacrylate (MMA) were placed and stirred, and the temperature was raised to 50°C while replacing the inside of the polymerization apparatus with nitrogen. 0.08 parts of 2,2'-azobis(2-methylpropionamidine) dihydrochloride were added thereto as a polymerization initiator, and the temperature was further raised to 60°C. After the temperature was raised, MMA was continuously dropped at a rate of 0.24 parts / min for 75 minutes using a dropping pump. The reaction solution was kept at 60°C for 6 hours, and then cooled to room temperature to obtain a transparent aqueous solution of dispersant (1) with a solid content of 10%.
[0058] [Chain transfer agent] <Synthesis Example 2: Synthesis of Chain Transfer Agent (1)> In a synthesis apparatus equipped with a stirrer, 1.00 g of cobalt (II) acetate tetrahydrate, 1.93 g of diphenylglyoxime, and 80 mL of diethyl ether previously deoxygenated by nitrogen bubbling were placed under a nitrogen atmosphere and stirred at room temperature for 30 minutes. Next, 10 mL of boron trifluoride diethyl ether complex was added and stirred for an additional 6 hours. The mixture was filtered, the solid was washed with diethyl ether, and vacuum dried for 15 hours to obtain 2.12 g of chain transfer agent (1) as a reddish brown solid.
[0059] <Production Example 1: Production of Macromonomer (m1)> In a polymerization apparatus equipped with a stirrer, a cooling tube, a thermometer, and a nitrogen gas inlet tube, 145 parts of deionized water, 0.1 parts of sodium sulfate, and 0.25 parts of dispersant (1) (solid content 10%) were added and stirred to obtain a uniform aqueous solution. Next, 50 parts of MMA as a vinyl radical polymerizable monomer (a2), 50 parts of glycidyl methacrylate (GMA) which is a (meth)acrylate having a cyclic ether group, 0.0040 parts of a chain transfer agent (1), and 2 parts of 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate (manufactured by NOF Corporation, trade name "Perocta O") as a polymerization initiator were added to obtain an aqueous suspension. Next, the inside of the polymerization apparatus was replaced with nitrogen, the temperature was raised to 80°C and the reaction was carried out for 3.5 hours, and in order to further increase the polymerization rate, the temperature was raised to 90°C and maintained for 1 hour. Thereafter, the reaction liquid was cooled to 40°C to obtain an aqueous suspension containing the macromonomer. This aqueous suspension was filtered through a filter, and the residue remaining on the filter was washed with deionized water, dehydrated, and dried at 40°C for 16 hours to obtain a macromonomer (m1). The molecular weight of the resulting macromonomer (m1) was measured, and the results are shown in Table 1.
[0060] [Table 1]
[0061] The abbreviations in Table 1 are as follows. MMA: Methyl methacrylate (manufactured by Mitsubishi Chemical, product name "Acryester M"). GMA: Glycidyl methacrylate (manufactured by Mitsubishi Chemical, product name "Acryester G"). Chain transfer agent (1): The chain transfer agent synthesized in Synthesis Example 2. Perocta O: 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate (manufactured by NOF Corporation, trade name "Perocta O").
[0062] <Production Example 2: Production of (meth)acrylic graft copolymer (A-1)> In a four-neck flask equipped with a stirrer, a thermometer, a cooling tube and a nitrogen gas inlet, 55 parts of methyl ethyl ketone (MEK) as an initial charge solvent and 5 parts of macromonomer (m1) as an (M) component were placed, and the external temperature was raised to 85°C under nitrogen gas aeration. After the external temperature reached 85°C and the internal temperature stabilized, a mixture consisting of 20 parts of MEK, 48 parts of methyl acrylate as an (a1) component, 47 parts of i-butyl methacrylate, and 0.13 parts of benzoyl peroxide (manufactured by NOF Corp., trade name: "Niper BMT-K40") as a polymerization initiator was added dropwise over 4 hours. After holding for 1 hour after the end of the dropwise addition, a mixture consisting of 0.5 parts of 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate (manufactured by NOF Corp., trade name "Perocta O") as a polymerization initiator and 10 parts of MEK was added over 1 hour. After that, after keeping for 2 hours, MEK was added so that the solid content (the ratio of the amount of monomer charged to the amount of (monomer + solvent charged)) became 50%, and then the mixture was cooled to room temperature to obtain a (meth)acrylic graft copolymer (A-1) solution. The molecular weight of the resulting (meth)acrylic graft copolymer (A-1) was measured, and the results are shown in Table 2.
[0063] <Production Examples 3 to 10: Production of (meth)acrylic graft copolymers (A-2) to (A-9)> Solutions of (meth)acrylic graft copolymers (A-2) to (A-9) were obtained in the same manner as in Production Example 2, except that the types and amounts of the (M) component and the (a1) component, and the types and amounts of the initially charged solvents were changed to the values shown in Table 2. The molecular weights of the resulting (meth)acrylic graft copolymers (A-2) to (A-9) were measured, and the results are shown in Table 2.
[0064] [Table 2]
[0065] The abbreviations in Table 2 are as follows. m1: the macromonomer produced in Production Example 1. ·MA: Methyl acrylate (manufactured by Mitsubishi Chemical Corporation, trade name "Methyl acrylate"). · EA: Ethyl acrylate (manufactured by Mitsubishi Chemical Corporation, trade name "Ethyl acrylate"). · n-BA: n-Butyl acrylate (manufactured by Mitsubishi Chemical Corporation, trade name "butyl acrylate"). · i-BMA: i-Butyl methacrylate (manufactured by Mitsubishi Chemical Corporation, product name "Acrylic Ester IB"). GMA: Glycidyl methacrylate (manufactured by Mitsubishi Chemical, product name "Acryester G"). IBXA: Isobornyl acrylate (manufactured by Osaka Organic Chemical Industry Ltd., product name "IBXA"). ·MEK: Methyl ethyl ketone. ·IPA: Isopropyl alcohol.
[0066] [Example 1] 100 parts of the (meth)acrylic graft copolymer (A-1) solution obtained in Production Example 2 was mixed with 50 parts of bisphenol A type epoxy resin (manufactured by Mitsubishi Chemical Corporation, product name "jER828"), and MEK and IPA were distilled off under reduced pressure using a vacuum dryer to obtain a (meth)acrylic graft copolymer-containing epoxy resin containing 50 parts of the (meth)acrylic graft copolymer (A-1). To a mixing vessel were added 70 parts of a (meth)acrylic graft copolymer-containing epoxy resin as components (A) and (B) (breakdown: 35 parts of (meth)acrylic graft copolymer (A-1) and 35 parts of jER828) as component (B), 24 parts of jER828 as component (B), 5 parts of dicyandiamide (manufactured by Mitsubishi Chemical Corporation, product name "DICY7") as component (C), and 1 part of 3-(3,4-dichlorophenyl)-1,1-dimethylurea (manufactured by Hodogaya Chemical Co., Ltd., product name "DCMU") as a curing accelerator, and mixed using a stirring and degassing apparatus (manufactured by Thinky Corporation, product name "Awatori Rentaro") to prepare an epoxy resin composition. The obtained epoxy resin composition was used to evaluate vibration damping properties, and the results are shown in Table 3.
[0067] [Examples 2 to 8, Comparative Examples 1 to 2] Epoxy resin compositions were prepared in the same manner as in Example 1, except that the type of component (A) and the amount of each component were changed to those shown in Tables 3 and 4. The obtained epoxy resin composition was used to evaluate vibration damping properties, and the results are shown in Tables 3 and 4.
[0068] [Example 9] 100 parts of the (meth)acrylic graft copolymer (A-1) solution obtained in Production Example 2 was mixed with 50 parts of bisphenol A type epoxy resin (manufactured by Mitsubishi Chemical Corporation, product name "jER828"), and MEK and IPA were distilled off under reduced pressure using a vacuum dryer to obtain a (meth)acrylic graft copolymer-containing epoxy resin containing 50 parts of the (meth)acrylic graft copolymer (A-1). Into a mixing vessel, 70 parts of a (meth)acrylic graft copolymer-containing epoxy resin as components (A) and (B) (breakdown: 35 parts of (meth)acrylic graft copolymer (A-1) and 35 parts of jER828) as component (B), 24 parts of jER828 as component (B), 5 parts of dicyandiamide (manufactured by Mitsubishi Chemical Corporation, product name "DICY7") as component (C), 1 part of 3-(3,4-dichlorophenyl)-1,1-dimethylurea (manufactured by Hodogaya Chemical Co., Ltd., product name "DCMU") as a curing accelerator, and 17.9 parts of calcium carbonate (manufactured by Shiraishi Calcium Co., Ltd., product name "Whiten B") as a filler were added and mixed using a stirring degassing device (manufactured by Thinky Corporation, product name "Awatori Rentaro") to prepare an epoxy resin composition. The vibration damping properties of the obtained epoxy resin composition were evaluated, and the results are shown in Table 4.
[0069] [Example 10] An epoxy resin composition was prepared in the same manner as in Example 9, except that the type of component (A) and the amount of each component were changed to those shown in Table 4. The vibration damping properties of the obtained epoxy resin composition were evaluated, and the results are shown in Table 4.
[0070] [Example 11] 100 parts of the (meth)acrylic graft copolymer (A-1) solution obtained in Production Example 2 was mixed with 50 parts of bisphenol A type epoxy resin (manufactured by Mitsubishi Chemical Corporation, product name "jER828"), and MEK and IPA were distilled off under reduced pressure using a vacuum dryer to obtain a (meth)acrylic graft copolymer-containing epoxy resin containing 50 parts of the (meth)acrylic graft copolymer (A-1). To a mixing vessel were added 70 parts of a (meth)acrylic graft copolymer-containing epoxy resin as component (A) and component (B) (breakdown: 35 parts of (meth)acrylic graft copolymer (A-1) and 35 parts of jER828) as component (B), 24 parts of jER828 as component (B), and 5 parts of dicyandiamide (manufactured by Mitsubishi Chemical Corporation, product name "DICY7") as component (C), and mixed using a stirring degassing apparatus (manufactured by Thinky Corporation, product name "Awatori Rentaro") to prepare an epoxy resin composition. The vibration damping properties of the obtained epoxy resin composition were evaluated, and the results are shown in Table 4.
[0071] [Examples 12 to 13] An epoxy resin composition was prepared in the same manner as in Example 11, except that the type of component (A) and the amount of each component were changed to those shown in Table 4. The vibration damping properties of the obtained epoxy resin composition were evaluated, and the results are shown in Table 4.
[0072] [Example 14] 100 parts of the (meth)acrylic graft copolymer (A-6) solution obtained in Production Example 7 was mixed with 50 parts of bisphenol A type epoxy resin (manufactured by Mitsubishi Chemical Corporation, product name "jER828"), and MEK and IPA were distilled off under reduced pressure using a vacuum dryer to obtain a (meth)acrylic graft copolymer-containing epoxy resin containing 50 parts of the (meth)acrylic graft copolymer (A-6). Into a mixing vessel, 50 parts of a (meth)acrylic graft copolymer-containing epoxy resin as components (A) and (B) (breakdown: 25 parts of (meth)acrylic graft copolymer (A-1) and 25 parts of jER828) as component (B), 19 parts of jER828 as component (B), 5 parts of dicyandiamide (manufactured by Mitsubishi Chemical Corporation, trade name "DICY7") as component (C), 1 part of 3-(3,4-dichlorophenyl)-1,1-dimethylurea (manufactured by Hodogaya Chemical Co., Ltd., trade name "DCMU") as a curing accelerator, and 25 parts of Kaneka Corporation's trade name "Kane Ace MX154" (breakdown: 10 parts of a polymer having a core-shell structure and 15 parts of a bisphenol A type epoxy resin) were added and mixed using a stirring degassing device (manufactured by Thinky Corporation, product name "Awatori Rentaro") to prepare an epoxy resin composition. The vibration damping properties of the obtained epoxy resin composition were evaluated, and the results are shown in Table 4.
[0073] [Table 3]
[0074] [Table 4]
[0075] The abbreviations in Tables 3 and 4 are as follows. A-1 to A-9: (meth)acrylic graft copolymers (A) produced in Production Examples 2 to 10. · jER828: Bisphenol A type epoxy resin (manufactured by Mitsubishi Chemical Corporation, product name "jER828"). Bisphenol A epoxy: A bisphenol A type epoxy resin contained in the Kaneka Corporation product "Kane Ace MX154." DICY: Dicyandiamide (manufactured by Mitsubishi Chemical Corporation, product name "DICY7"). DCMU: 3-(3,4-dichlorophenyl)-1,1-dimethylurea (manufactured by Hodogaya Chemical Industry Co., Ltd., trade name "DCMU"). · Whiten B: Calcium carbonate (manufactured by Shiraishi Calcium Co., Ltd., product name "Whiten B"). Polymer having a core-shell structure: A polymer having a core-shell structure included in the product name "Kane Ace MX154" manufactured by Kaneka Corporation.
[0076] As is clear from Tables 3 and 4, the cured products of the epoxy resin compositions obtained in Examples 1 to 14 had high peak intensities of tan δ at −40° C. to 70° C. and were excellent in vibration damping properties. On the other hand, the cured products of the epoxy resin compositions obtained in the respective Comparative Examples were poor in vibration damping properties. [Industrial Applicability]
[0077] From the epoxy resin composition of the present invention, a cured product having excellent vibration-damping properties can be obtained, and therefore the epoxy resin composition of the present invention is useful, for example, as a vibration-damping material for civil engineering and construction, a vibration-damping material for vehicles, a vibration-damping material for electronic materials, etc.
Claims
1. An epoxy resin composition comprising a (meth)acrylic graft copolymer (A), an epoxy resin (B) and a curing agent (C), wherein a cured product of the epoxy resin composition has a tan δ peak having an intensity of 0.15 or more in a temperature range of -40°C to 70°C.
2. The epoxy resin composition according to claim 1, further comprising a curing accelerator (D).
3. 2. The epoxy resin composition according to claim 1, wherein a cured product of the epoxy resin composition has a tan δ peak at 100° C. or higher.
4. 2. The epoxy resin composition according to claim 1, wherein the (meth)acrylic graft copolymer (A) contains a structural unit derived from a macromonomer (M) and a structural unit derived from a vinyl radically polymerizable monomer (a1).
5. The epoxy resin composition according to claim 4, wherein the macromonomer (M) has a structure represented by the following formula (1): 【Chemistry 1】 (In formula (1), X 1 ~X n-1 are each independently a hydrogen atom, a methyl group, or CH 2 OH and Y 1 ~Y n each independently represents X bonded to a vinyl group of the vinyl radical polymerizable monomer (a2) which is a monomer constituent unit of the macromonomer (M). 1 ~X n-1 Z is a terminal group, and n is an integer from 2 to 10,000.
6. A cured product of the epoxy resin composition according to any one of claims 1 to 5.
7. A vibration damping material comprising the cured product according to claim 6.
Citation Information
Patent Citations
Vibration-damping thermosetting resin composition and its cured material
JP2002003819A
Thermosetting resin composition having vibration-damping properties and adhesive using the same
JP2003105060A
Prepreg and molded article thereof
JP2020050833A