Polymer, copolymer, ink, ink container, image forming method, image forming device, and backsheet for solar cell

A polymer with a specific structural unit and copolymer with electrostatic repulsion improve the storage stability and redispersibility of colorants in inks, addressing settling issues and enhancing ink performance on non-paper media and solar cell backsheets.

JP2024144347APending Publication Date: 2024-10-11RICOH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024051698
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-27
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Conventional white inks using rutile titanium oxide for non-paper media suffer from storage stability and redispersibility issues due to settling and aggregation, leading to increased viscosity and reduced hiding power.

Method used

A polymer with a specific structural unit represented by general formula (1) is used to improve the dispersibility and stability of colorants like titanium oxide, incorporating a pyridyl group for enhanced adsorption and a copolymer with structural unit (2) for electrostatic repulsion, ensuring long-term stability and easy redispersion.

Benefits of technology

The polymer and copolymer achieve excellent storage stability and redispersibility of colorants, enabling the production of inks with improved performance on non-paper media and solar cell backsheets with enhanced weather resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144347000056
    Figure 2024144347000056
  • Figure 2024144347000057
    Figure 2024144347000057
  • Figure 2024144347000001
    Figure 2024144347000001
Patent Text Reader

Abstract

To provide a polymer with which a coloring material dispersion excellent in storage stability, an ink excellent in storage stability and redispersibility, and a solar cell backsheet excellent in weather resistance can be manufactured.SOLUTION: A polymer comprises a structural unit represented by general formula (1) in the figure. In general formula (1), R1 represents a hydrogen atom or a methyl group; L1 represents "-COO-", "-CONH-", or a bond; X represents a C2-10 hydrocarbon group or an oxygen-containing C2-10 hydrocarbon group; L2 represents "-O-" or "-NH-"; Y represents a C2-12 hydrocarbon group or a bond; and L3 represents "-OCO-", "-O-", "-(CH2)n-", or "-OCO-(CH2)n-", where n represents an integer from 1 to 3.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polymer, a copolymer, an ink, an ink container, an image forming method, an image forming apparatus, and a solar cell backsheet. [Background technology]

[0002] Inkjet printers are widely used as printers for printing on paper media. When printing on media other than paper media (for example, media such as transparent or colored plastic films and colored fabrics), a white ink with high hiding power is required in addition to black ink, yellow ink, magenta ink, and cyan ink.

[0003] Rutile-type titanium oxide, which has a high refractive index, is used as a pigment for white ink with high hiding power. As a dispersant for the titanium oxide, for example, a carboxyl group-containing AB block copolymer of an AB block type, which is composed of methacrylate containing an aliphatic cyclic alkyl group having at least 6 carbon atoms and methacrylic acid, has been proposed (for example, see Patent Document 1). Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide a colorant dispersion having excellent storage stability, an ink having excellent storage stability and redispersibility, and a polymer capable of producing a solar cell backsheet having excellent weather resistance. [Means for solving the problem]

[0005] The ink of the present invention as a means for solving the above problems is as follows. The polymer is characterized by having a structural unit represented by the following general formula (1). [ka] (In general formula (1), R1 is hydrogen or a methyl group, L1 is "-COO-", "-CONH-" or a bond, X is a hydrocarbon group having 2 to 10 carbon atoms or a hydrocarbon group containing oxygen and having 2 to 10 carbon atoms, L2 is "-O-" or "-NH-", Y is a hydrocarbon group having 2 to 12 carbon atoms or a bond, L3 is "-OCO-", "-O-", "-(CH2)n-" or "-OCO-(CH2)n-", and n is an integer of 1 to 3.) Effect of the Invention

[0006] According to the present invention, it is possible to provide a colorant dispersion having excellent storage stability, an ink having excellent storage stability and redispersibility, and a polymer capable of producing a solar cell backsheet having excellent weather resistance. [Brief description of the drawings]

[0007] [Figure 1] FIG. 1 is a schematic diagram showing an example of an image forming apparatus. [Diagram 2] FIG. 2 is a schematic diagram illustrating an example of an ink cartridge. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Rutile titanium dioxide used in conventional white inks with high hiding power has a specific gravity of 4.17 g / mL, and is known to settle in the ink over time and eventually separate. When using the white ink, there is no problem if the original dispersion state is restored by stirring or shaking, but there is a problem that titanium dioxide deposited in the lower layer of the ink aggregates and the dispersion state does not return to the original state. In addition, there are problems such as an increase in the viscosity of the ink, a decrease in the white hiding power, and ejection defects due to the ink not returning to the original dispersion state.

[0009] The conventional dispersants described in Patent Document 1 do not provide sufficient ink storage stability or colorant redispersibility, and further improvements are desired.

[0010] As a result of intensive research, the present inventors have found that by using a polymer having a structural unit represented by general formula (1) or a copolymer having a structural unit represented by general formula (1) and a structural unit represented by general formula (2), a colorant dispersion having excellent storage stability, and an ink having excellent storage stability and redispersibility can be obtained.

[0011] Furthermore, the inventors have discovered that a film in which a colorant such as titanium oxide is uniformly dispersed without aggregation can be obtained from an ink containing water, a colorant, and a polymer having a structural unit represented by general formula (1), or a copolymer having a structural unit represented by general formula (1) and a structural unit represented by general formula (2), and that by applying the obtained film to a solar cell backsheet as a protective layer, a solar cell backsheet with excellent weather resistance can also be obtained.

[0012] The present invention will now be described in detail.

[0013] (Polymer) The polymer of the present invention has a structural unit represented by general formula (1) and may contain other polymerizable monomers, if necessary. In this specification, the "structural unit represented by general formula (1)" may be referred to as the "first monomer". In this specification, the "polymer having a structural unit represented by formula (1)" may be referred to as a "polymer". In this specification, even if the polymer of the present invention contains other polymerizable monomers described later, it is described as a "polymer" for convenience.

[0014] <Structural unit represented by general formula (1)> [ka] (In general formula (1), R1 is hydrogen or a methyl group, L1 is "-COO-", "-CONH-" or a bond, X is a hydrocarbon group having 2 to 10 carbon atoms or a hydrocarbon group containing oxygen and having 2 to 10 carbon atoms, L2 is "-O-" or "-NH-", Y is a hydrocarbon group having 2 to 12 carbon atoms or a bond, L3 is "-OCO-", "-O-", "-(CH2)n-" or "-OCO-(CH2)n-", and n is an integer of 1 to 3.)

[0015] In the polymer having a structural unit represented by the general formula (1), the pyridyl group present at the terminal functions as a Lewis base, thereby improving the adsorptivity to the particle surfaces of titanium oxide, titanium oxide surface-treated with alumina, barium sulfate, and the like. In addition, since the pyridyl group in the structural unit represented by the general formula (1) is located away from the main chain of the polymer, it is less susceptible to the inhibition of adsorption to the colorant by other components involved in the (co)polymerization (such as the structural unit represented by the general formula (2)). Furthermore, the linking group X in the general formula (1) and the "-NH-CO-NH- group" or "-NH-COO- group" bonded to the linking group Y impart water solubility to the polymer. Therefore, the dispersion stability of the colorant can be improved, and an ink with high storage stability can be obtained. That is, when a colorant dispersion in which a colorant is dispersed in water is prepared as described below, a colorant dispersion with high dispersibility and long-term stability can be prepared by using the polymer of the present invention.

[0016] The weight average molecular weight (Mw) of the polymer of the present invention is preferably from 5,000 to 50,000, more preferably from 15,000 to 40,000, from the viewpoints of storage stability of the colorant dispersion and ink, and redispersibility of the ink. The method for measuring the weight average molecular weight (Mw) of the polymer is not particularly limited, but for example, it can be measured by the following method. [An example of how to measure weight average molecular weight (Mw)] Measurement was performed by GPC (Gel Permeation Chromatography) under the following conditions. Equipment: GPC-8320GPC (Tosoh Corporation) Column: TSK G2000HXL and G4000HXL (Tosoh Corporation) ·Temperature: 40℃ Solvent: THF (tetrahydrofuran) Flow rate: 0.6mL / min Inject 1 mL of a polymer with a concentration of 0.5% by mass into the apparatus, and calculate the weight average molecular weight Mw of the polymer from the molecular weight distribution of the polymer measured under the above conditions using a molecular weight calibration curve prepared from a monodisperse polystyrene standard sample.

[0017] The method for obtaining the structural unit represented by the general formula (1) is not particularly limited and can be appropriately selected depending on the purpose. For example, the following methods can be mentioned. [An example of a method for obtaining a structural unit represented by general formula (1)] Pyridyl carboxylic acid (A-1) is subjected to a condensation reaction with an excess amount of diol to obtain pyridine carboxylic acid hydroxyalkyl ester (A-2).

[0018] [ka]

[0019] Next, an isocyanate compound (A-3) having an acrylic group or the like is reacted with the (A-2) to obtain a monomer (A-4).

[0020] [ka]

[0021] Next, the polymer (A-5) is obtained by polymerization in the presence of a radical polymerization initiator.

[0022] [ka]

[0023] (copolymer) The copolymer of the present invention has a structural unit represented by the above general formula (1) and a structural unit represented by the following general formula (2), and may contain other polymerizable monomers as necessary. In this specification, the "structural unit represented by formula (2)" may be referred to as the "second monomer". In this specification, a "copolymer having a structural unit represented by general formula (1) and a structural unit represented by general formula (2)" may be referred to as a "copolymer".

[0024] <Structural unit represented by general formula (2)> [ka] (In the general formula (2), R2 is a hydrogen atom or a methyl group, X + is a proton, an organic cation, or an inorganic cation.)

[0025] The proton or cation in the general formula (2) induces electrostatic repulsion between the copolymer molecules, thereby suppressing aggregation of the colorant. Therefore, even if the colorant precipitates in the ink, it can be easily redispersed, and an ink with high redispersibility can be obtained. That is, when preparing a colorant dispersion in which a colorant is dispersed in water, as described below, the use of the copolymer of the present invention can improve the dispersibility, redispersibility, and storage stability of the colorant dispersion.

[0026] The proton or cation is not particularly limited and can be appropriately selected depending on the purpose. For example, a sodium ion, a potassium ion, a lithium ion, a tetramethylammonium ion, a tetraethylammonium ion, a tetrapropylammonium ion, a tetrabutylammonium ion, a tetrapentylammonium ion, a tetrahexylammonium ion, a triethylmethylammonium ion, a tributylmethylammonium ion, a trioctylmethylammonium ion, a 2-hydroxyethyltrimethylammonium ion, a tris(2-hydroxyethyl)methylammonium ion, a propyltrimethylammonium ion, a hexyltrimethylammonium ion, an octyltrimethylammonium ion, a nonyltrimethylammonium ion, a decyltrimethylammonium ion, a dodecyltrimethylammonium ion, a tetradecyltrimethylammonium ion, a hexadecyltrimethylammonium ion, an octadecyltrimethylammonium ion, a hex ... ammonium ion, didodecyldimethylammonium ion, ditetradecyldimethylammonium ion, dihexadecyldimethylammonium ion, dioctadecyldimethylammonium ion, ethylhexadecyldimethylammonium ion, ammonium ion, dimethylammonium ion, trimethylammonium ion, monoethylammonium ion, diethylammonium ion, triethylammonium ion, monoethanolammonium ion, diethanolammonium ion, triethanolammonium ion, methylethanolammonium ion, methyldiethanolammonium ion, dimethylethanolammonium ion, monopropanolammonium ion, dipropanolammonium ion, tripropanolammonium ion, isopropanolammonium ion, morpholinium ion, N-methylmorpholinium ion, N-methyl-2-pyrrolidinium ion, 2-pyrrolidinium ion, and the like.

[0027] The weight average molecular weight (Mw) of the copolymer of the present invention is preferably from 5,000 to 50,000, more preferably from 15,000 to 40,000, from the viewpoints of storage stability of the colorant dispersion and ink, and redispersibility of the ink. The method for measuring the weight average molecular weight (Mw) of the copolymer is not particularly limited, and examples thereof include the same method as [One example of the method for measuring the weight average molecular weight (Mw)] described in the above (Polymer) section.

[0028] The structure of the copolymer of the present invention is not particularly limited and can be appropriately selected depending on the purpose. Examples of the copolymer include random copolymers, graft copolymers, and block copolymers.

[0029] The method for synthesizing the copolymer of the present invention is not particularly limited and may be appropriately selected depending on the purpose. For example, there may be mentioned a method for obtaining a copolymer (A-7) by copolymerizing the monomer (A-4) described in the above section [One example of a method for obtaining a structural unit represented by general formula (1)] with methacrylic acid (A-6) in the presence of a radical polymerization initiator.

[0030] [ka]

[0031] <Other polymerizable monomers> The polymer or copolymer of the present invention may have other polymerizable monomers in addition to the structural unit represented by the general formula (1) and the structural unit represented by the general formula (2). The other polymerizable monomers are not particularly limited and may be appropriately selected depending on the purpose. Examples of the other polymerizable monomers include polymerizable hydrophobic monomers, polymerizable hydrophilic monomers, and polymerizable surfactants. In this specification, the "other polymerizable monomer" may be referred to as a "third monomer".

[0032] <<Polymerizable hydrophobic monomers>> The polymerizable hydrophobic monomer is not particularly limited and can be appropriately selected depending on the purpose. For example, it is possible to use unsaturated ethylene monomers having an aromatic ring, such as α-methylstyrene, 4-t-butylstyrene, and 4-chloromethylstyrene; methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, dimethyl maleate, dimethyl itaconate, dimethyl fumarate, lauryl (meth)acrylate (C12), tridecyl (meth)acrylate (C13), tetradecyl (meth)acrylate (C14), pentadecyl (meth)acrylate (C15), hexadecyl (meth)acrylate (C16), heptadecyl (meth)acrylate (C17), nonadecyl (meth)acrylate (C19), eicosyl (meth)acrylate (C20), (meth)acrylate (C21), (meth)acrylate (C22), (meth)acrylate (C23), (meth)acrylate (C24), (meth)acrylate (C25), (meth)acrylate (C26), (meth)acrylate (C27), (meth)acrylate (C28), (meth)acrylate (C29), (meth)acrylate (C30), (meth)acrylate (C31), (meth)acrylate (C32), (meth)acrylate (C33), (meth)acrylate (C34), (meth)acrylate (C35), (meth)acrylate (C36), (meth)acrylate (C37), (meth)acrylate (C38), (meth)acrylate (C39 ...9), (meth)acrylate (C39), (meth)acrylate (C39), (meth)acrylate (Meth)acrylic acid alkyl such as henoicosyl (C21) methacrylate and docosyl (meth)acrylate (C22); unsaturated ethylene monomers having an alkyl group such as 1-heptene, 3,3-dimethyl-1-pentene, 4,4-dimethyl-1-pentene, 3-methyl-1-hexene, 4-methyl-1-hexene, 5-methyl-1-hexene, 1-octene, 3,3-dimethyl-1-hexene, 3,4-dimethyl-1-hexene, 4,4-dimethyl-1-hexene, 1-nonene, 3,5,5-trimethyl-1-hexene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, 1-eicosene, and 1-docosene. These may be used alone or in combination of two or more.

[0033] <<Polymerizable hydrophilic monomer>> The polymerizable hydrophilic monomer is not particularly limited and can be appropriately selected depending on the purpose. Examples of the polymerizable hydrophilic monomer include anionic unsaturated ethylene monomers such as maleic acid or a salt thereof, monomethyl maleate, itaconic acid, monomethyl itaconate, fumaric acid, 4-styrenesulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, or unsaturated ethylene monomers containing phosphoric acid, phosphonic acid, alendronic acid, or etidronic acid; and nonionic unsaturated ethylene monomers such as 2-hydroxyethyl (meth)acrylate, diethylene glycol mono(meth)acrylate, triethylene glycol mono(meth)acrylate, tetraethylene glycol mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, (meth)acrylamide, N-methylol(meth)acrylamide, N-vinylformamide, N-vinylacetamide, N-vinylpyrrolidone, acrylamide, N,N-dimethylacrylamide, Nt-butylacrylamide, N-octylacrylamide, and Nt-octylacrylamide.

[0034] The content of the polymerizable hydrophobic monomer and the polymerizable hydrophilic monomer is not particularly limited and can be appropriately selected depending on the purpose. For example, the content of the polymerizable hydrophobic monomer and the polymerizable hydrophilic monomer can be 5% by mass or more and 100% by mass or less based on the total amount of the monomers forming the polymer having the structural unit represented by the general formula (1) or the copolymer having the structural unit represented by the general formula (1) and the structural unit represented by the general formula (2).

[0035] <<Polymerizable surfactants>> The polymerizable surfactant is a surfactant having at least one radically polymerizable unsaturated double bond group in the molecule, and examples thereof include anionic surfactants and nonionic surfactants.

[0036] -Anionic surfactants- The anionic surfactant is not particularly limited and can be appropriately selected depending on the purpose. For example, ammonium sulfate base (-SO3-NH4 +), etc., hydrocarbon compounds having sulfate groups and allyl groups (-CH2-CH=CH2), ammonium sulfate groups (-SO3-NH4 + ), etc., which have a sulfate group and a methacryl group (-CO-C(CH3)=CH2), or an ammonium sulfate group (-SO3-NH4 + ) and aromatic hydrocarbon compounds having a sulfate group and a 1-propenyl group (-CH=CH2CH3). Specific examples of the anionic surfactants include, by trade name, ELEMINOL JS-20, RS-300 (both manufactured by Sanyo Chemical Industries, Ltd.), AQUALON KH-10, AQUALON KH-1025, AQUALON KH-05, AQUALON HS-10, AQUALON HS-1025, AQUALON BC-0515, AQUALON BC-10, AQUALON BC-1025, AQUALON BC-20, and AQUALON BC-2020 (all manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.).

[0037] -Nonionic surfactants- The nonionic surfactant is not particularly limited and may be appropriately selected depending on the purpose, and examples thereof include a hydrocarbon compound or an aromatic hydrocarbon compound having a 1-propenyl group (-CH=CH2CH3) and a polyoxyethylene group (-(C2H4O)nH), where "n" in the polyoxyethylene group is an integer of 2 or more. Specific examples of the nonionic surfactants include trade names such as Aqualon RN-20, Aqualon RN-2025, Aqualon RN-30, and Aqualon RN-50 (all manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), Latemul PD-104, Latemul PD-420, Latemul PD-430, and Latemul PD-450 (all manufactured by Kao Corporation).

[0038] The content of the polymerizable surfactant is not particularly limited and can be appropriately selected depending on the purpose. For example, the content of the polymerizable surfactant can be from 0.1% by mass to 10% by mass relative to the total amount of monomers forming a polymer having a structural unit represented by the general formula (1) or a copolymer having a structural unit represented by the general formula (1) and a structural unit represented by the general formula (2).

[0039] A radical polymerization initiator may be used in the process of forming the polymers and copolymers of the present invention. The radical polymerization initiator is not particularly limited and may be appropriately selected depending on the purpose, and examples thereof include peroxyketals, hydroperoxides, dialkyl peroxides, diacyl peroxides, peroxydicarbonates, peroxyesters, cyano-based azobisisobutyronitrile, azobis(2-methylbutyronitrile), azobis(2,2'-isovaleronitrile), non-cyano-based dimethyl-2,2'-azobisisobutyrate, etc. Among these, organic peroxides and azo-based compounds are preferred, and azo-based compounds are more preferred, in terms of ease of molecular weight control and low decomposition temperature. The content of the radical polymerization initiator is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1% by mass or more and 10% by mass or less based on the total amount of polymerizable monomers. The polymerizable monomer refers to all of the monomers that form a polymer having a structural unit represented by the general formula (1), the monomers that form a copolymer having a structural unit represented by the general formula (1) and a structural unit represented by the general formula (2), and the other polymerizable monomers.

[0040] Chain transfer agents may be added to adjust the molecular weight of the polymers and copolymers of the present invention. The chain transfer agent is not particularly limited and can be appropriately selected depending on the purpose. Examples of the chain transfer agent include mercaptoacetic acid, mercaptopropionic acid, 2-propanethiol, 2-mercaptoethanol, thiophenol, dodecyl mercaptan, 1-dodecanethiol, and thioglycerol.

[0041] The polymerization temperature for forming the polymer or copolymer of the present invention is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 50°C or higher and 150°C or lower, more preferably 60°C or higher and 100°C or lower. The polymerization time for forming the polymer or copolymer of the present invention is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 3 hours or more and 48 hours or less.

[0042] The content of the structural unit represented by the general formula (1) in the polymer or copolymer is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 75% by mass or more and 95% by mass or less, and more preferably 80% by mass or more and 90% by mass or less, based on the total amount of the polymer or copolymer. When the content of the structural unit represented by the general formula (1) is within the above preferred range, the storage stability of the ink is further improved, which is advantageous.

[0043] The content of the structural unit represented by the general formula (2) in the polymer or copolymer is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 5.0 mass % or more and 35.0 mass % or less, and more preferably 15.0 mass % or more and 25.0 mass % or less, based on the total amount of the polymer or copolymer. When the content of the structural unit represented by the general formula (2) is within the above preferred range, it is preferable since the solubility in water and the dispersion stability become good.

[0044] The contents of the first monomer and the third monomer in the polymer of the present invention, and the contents of the first monomer, the second monomer, and the third monomer in the copolymer of the present invention are 1 H-NMR, 13 It can be determined by a combination of C-NMR, GC-MS, LC-MS, and LC-MS / MS. The second monomer in the copolymer of the present invention can be quantified by a neutralization titration method in which a solution containing a titration indicator such as phenolphthalein is added dropwise to a solution in which a certain amount of the copolymer of the present invention is dissolved.

[0045] (ink) The ink of the present invention contains water, a colorant, and a polymer having a structural unit represented by the general formula (1) or a copolymer having a structural unit represented by the general formula (1) and a structural unit represented by the general formula (2), and may contain other components as necessary. Here, the "polymer having a structural unit represented by the general formula (1)" and the "copolymer having a structural unit represented by the general formula (1) and a structural unit represented by the general formula (2)" are the same as those described above in the (polymer) and (copolymer) sections, and therefore will not be described here.

[0046] <Water> The water contained in the ink is not particularly limited and can be appropriately selected depending on the purpose. The water content is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of the drying property and ejection reliability of the ink, however, the water content is preferably from 10% by mass to 90% by mass, and more preferably from 20% by mass to 60% by mass, of the total amount of the ink.

[0047] <Coloring material> The coloring material contained in the ink of the present invention is not particularly limited and can be appropriately selected depending on the purpose, and for example, a pigment, a dye, etc. may be used. Mixed crystals may also be used.

[0048] <<Pigments>> The pigment is not particularly limited and can be appropriately selected depending on the purpose. For example, black pigments, yellow pigments, magenta pigments, cyan pigments, white pigments, green pigments, orange pigments, glossy pigments such as gold and silver pigments, metallic pigments, and the like can be used. Examples of the white pigment include titanium oxide, iron oxide, calcium carbonate, barium sulfate, and aluminum hydroxide.

[0049] As the pigment, inorganic pigments and organic pigments can be used. The inorganic pigment is not particularly limited and can be appropriately selected depending on the purpose. Examples of the inorganic pigment include titanium oxide, iron oxide, calcium carbonate, barium sulfate, aluminum hydroxide, barium yellow, cadmium red, and chrome yellow, as well as carbon black produced by a known method such as a contact method, a furnace method, or a thermal method. The organic pigment is not particularly limited and can be appropriately selected depending on the purpose. Examples of the organic pigment include azo pigments, polycyclic pigments (e.g., phthalocyanine pigments, perylene pigments, perinone pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, indigo pigments, thioindigo pigments, isoindolinone pigments, quinophthalone pigments, etc.), dye chelates (e.g., basic dye-type chelates, acid dye-type chelates, etc.), nitro pigments, nitroso pigments, aniline black, etc. Among these pigments, those having good affinity with the solvent are preferably used. In addition, resin hollow particles and inorganic hollow particles can also be used.

[0050] Specific examples of the pigment include the following: Examples of black pigments include carbon blacks (CI Pigment Black 7) such as furnace black, lamp black, acetylene black, and channel black; metals such as copper and iron (CI Pigment Black 11); and organic pigments such as aniline black (CI Pigment Black 1). Examples of white pigments include titanium oxide, titanium dioxide, and hollow resin particles. Color pigments include CI Pigment Yellow 1, CI Pigment Yellow 3, CI Pigment Yellow 12, CI Pigment Yellow 13, CI Pigment Yellow 14, CI Pigment Yellow 17, CI Pigment Yellow 24, CI Pigment Yellow 34, CI Pigment Yellow 35, CI Pigment Yellow 37, CI Pigment Yellow 42 (Yellow Iron Oxide), CI Pigment Yellow 53, CI Pigment Yellow 55, CI Pigment Yellow 74, CI Pigment Yellow 75, CI Pigment Yellow 76, CI Pigment Yellow 77, CI Pigment Yellow 78, CI Pigment Yellow 79, CI Pigment Yellow 80, CI Pigment Yellow 81, CI Pigment Yellow 82, CI Pigment Yellow 83, CI Pigment Yellow 84, CI Pigment Yellow 85, CI Pigment Yellow 86, CI Pigment Yellow 87, CI Pigment Yellow 88, CI Pigment Yellow 89, CI Pigment Yellow 90, CI Pigment Yellow 91, CI Pigment Yellow 92, CI Pigment Yellow 93, CI Pigment Yellow 94, CI Pigment Yellow 95, CI Pigment Yellow 96, CI Pigment Yellow 97, CI Pigment Yellow 98, CI Pigment Yellow 99, CI Pigment Yellow 100, CI Pigment Yellow 101, CI Pigment Yellow 102, CI Pigment Yellow 103, CI Pigment Yellow 104, CI Pigment Yellow 105, CI Pigment Yellow 106, CI Pigment Yellow 107, CI Pigment Yellow 108, CI Pigment Yellow 109, -81, CI Pigment Yellow 83, CI Pigment Yellow 95, CI Pigment Yellow 97, CI Pigment Yellow 98, CI Pigment Yellow 100, CI Pigment Yellow 101, CI Pigment Yellow 104, CI Pigment Yellow 108, CI Pigment Yellow 109, CI Pigment Yellow 110, CI Pigment Yellow 117, CI Pigment Yellow 120, CI Pigment Yellow 138, CI Pigment Yellow 150, CI Pigment Yellow 153, CI Pigment Yellow 155, CI Pigment Yellow 180, CI Pigment Yellow 185, CI Pigment Yellow 213, CI Pigment Orange 5, CI Pigment Orange 13, CI Pigment Orange 16, CI Pigment Orange 17, CI Pigment Orange 36, CI Pigment Orange 43, CI Pigment Orange 51, CI Pigment Red 1, CI Pigment Red 2, CI Pigment Red 3, CI Pigment Red 5, CI Pigment Red 17 , CI Pigment Red 22, CI Pigment Red 23, CI Pigment Red 31, CI Pigment Red 38, CI Pigment Red 48:2 (Permanent Red 2B (Ca)), CI Pigment Red 48:3, CI Pigment Red 48:4, CI Pigment Red 49:1, CI Pigment Red 52:2, CI Pigment Red 53:1, CI Pigment Red 57:1 (Brilliant Carmine 6B), CI Pigment Red 60:1, CI Pigment Red 63:1, C.I. Pigment Red 63:2, CI Pigment Red 64:1, CI Pigment Red 81, CI Pigment Red 83, CI Pigment Red 88, CI Pigment Red 101 (Red Flax), CI Pigment Red 104, CI Pigment Red 105, CI Pigment Red 106, CI Pigment Red 108 (Cadmium Red), CI Pigment Red 112, CI Pigment Red 114, CI Pigment Red 122 (Quinacridone Magenta), CI Pigment Red 1 23, CI Pigment Red 146, CI Pigment Red 149, CI Pigment Red 166, CI Pigment Red 168, CI Pigment Red 170, CI Pigment Red 172, CI Pigment Red 177, CI Pigment Red 178, CI Pigment Red 179, CI Pigment Red 184, CI Pigment Red 185, CI Pigment Red 190, CI Pigment Red 193, CI Pigment Red 202, CI Pigment Red 207, CI Pigment Red 208, CI Pigment Red 209, CI Pigment Red 213, CI Pigment Red 219, CI Pigment Red 224, CI Pigment Red 254, CI Pigment Red 264, CI Pigment Violet 1 (Rhodamine Lake), CI Pigment Violet 3, CI Pigment Violet 5:1, CI Pigment Violet 16, CI Pigment Violet 19, CI Pigment Violet 23, CI Pigment Violet 38, CI Pigment Blue Rue 1, CI Pigment Blue 2, CI Pigment Blue 15 (Phthalocyanine Blue), CI Pigment Blue 15:1, CI Pigment Blue 15:2, CI Pigment Blue 15:3, CI Pigment Blue 15:4 (Phthalocyanine Blue), CI Pigment Blue 16, CI Pigment Blue 17:1, CI Pigment Blue 56, CI Pigment Blue 60, CI Pigment Blue 63, CI Pigment Green 1, CI Pigment Green 4, CI Pigment Green 7, CIPigment Green 8, CI Pigment Green 10, CI Pigment Green 17, CI Pigment Green 18, CI Pigment Green 36, etc. Among these, CI Pigment Red 146, CI Pigment Red 202, CI Pigment Red 208, and CI Pigment Violet 19 are preferred as magenta pigments, and CI Pigment Yellow 17 and CI Pigment Yellow 180 are preferred as yellow pigments.

[0051] <<dye>> The dye is not particularly limited and may be appropriately selected depending on the purpose. For example, acid dyes, direct dyes, reactive dyes, and basic dyes may be used. These may be used alone or in combination of two or more.

[0052] Specific examples of the dyes include CI Acid Yellow 17, CI Acid Yellow 23, CI Acid Yellow 42, CI Acid Yellow 44, CI Acid Yellow 79, CI Acid Yellow 142, CI Acid Red 52, CI Acid Red 80, CI Acid Red 82, CI Acid Red 249, CI Acid Red 254, CI Acid Red 289, CI Acid Blue 9, CI Acid Blue 45, CI Acid Blue 249, CI Acid Black 1, CI Acid Black 2, CI Acid Black 24, CI Acid Black 94, CI Food Black 1, CI Food Black 2, CI Direct Yellow 1, CI Direct Yellow 12, CI Direct Yellow 24, CI Direct Yellow 33, CI Direct Yellow 50, CI Direct Yellow 55, CI Direct Yellow 58, CI Direct Yellow 86, CI Direct Yellow 132, CI Direct Yellow 142, CI Direct Yellow 144, CI Dye Direct Yellow 173, CI Direct Red 1, CI Direct Red 4, CI Direct Red 9, CI Direct Red 80, CI Direct Red 81, CI Direct Red 225, CI Direct Red 227, CI Direct Blue 1, CI Direct Blue 2, CI Direct Blue 15, CI Direct Blue 71, CI Direct Blue 86, CI Direct Blue 87, CI Direct Blue 98, CI Direct Blue 165, CI Direct Blue 199, CI Direct Blue 202, CI Directed Black 19, CI Directed Black 38, CI Directed Black 51, CI Directed Black 71, CI Directed Black 154, CI Directed Black 168, CI Directed Black 171, CI Directed Black 195, CI Reactive Red 14, CI Reactive Red 32, CI Reactive Red 55, CI Reactive Red 79, CI Reactive Red 249, CI Reactive Black 3, CIReactive Black 4, CI Reactive Black 35, etc.

[0053] As the coloring material in the present invention, a pigment is preferred because it has excellent adsorption ability to the polymer or copolymer, and excellent water resistance and weather resistance. In particular, when a white pigment is used as the coloring material, titanium oxide and barium sulfate are preferred from the viewpoint of excellent white hiding power, and titanium oxide is more preferred, and titanium oxide is preferred from the viewpoint of excellent storage stability of the coloring material dispersion, storage stability of the ink, and redispersibility of the ink.

[0054] The content of the colorant contained in the ink of the present invention is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of improving image density and obtaining good fixability and ejection stability, however, the content is preferably from 0.1% by mass to 15% by mass, and more preferably from 10% by mass to 15% by mass, based on the total amount of the ink.

[0055] <Other ingredients> The other components are not particularly limited and can be appropriately selected depending on the purpose. Examples of the other components include other resins (A), water, organic solvents, additives, radical polymerization initiators, and chain transfer agents.

[0056] <<Other resins (A)>> The ink of the present invention may contain another resin (A) different from the polymer and copolymer. The other resin (A) is not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include urethane resins, polyester resins, acrylic resins, vinyl acetate resins, styrene resins, butadiene resins, styrene-butadiene resins, vinyl chloride resins, acrylic styrene resins, and acrylic silicone resins. These may be used alone or in combination of two or more.

[0057] The resin particles made of the other resin (A) may be used as the other resin (A). The resin particles to be used may be appropriately synthesized or commercially available products.

[0058] The volume average particle diameter of the resin particles is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of obtaining good fixing property and high image hardness, the volume average particle diameter is preferably 10 nm or more and 1000 nm or less, more preferably 10 nm or more and 200 nm or less, and particularly preferably 10 nm or more and 100 nm or less. The volume average particle size of the resin particles can be measured, for example, using a particle size analyzer (Nanotrac Wave-UT151, manufactured by Microtrac-Bell Co., Ltd.).

[0059] <<Organic solvents>> The ink of the present invention may contain an organic solvent. Since the polymer and copolymer are water-soluble in the ink, they may be used in combination with a hydrophilic organic solvent. The organic solvent is not particularly limited and can be appropriately selected depending on the purpose. For example, ethylene glycol, diethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 3-methyl-1,3-butanediol, triethylene glycol, polyethylene glycol, polypropylene glycol, 1,2-pentanediol, 1,3-pentanediol, 1,4-pentanediol, 2,4-pentanediol, polyhydric alcohols such as 1,5-pentanediol, 1,2-hexanediol, 1,6-hexanediol, 1,3-hexanediol, 2,5-hexanediol, 1,5-hexanediol, glycerin, 1,2,6-hexanetriol, 2-ethyl-1,3-hexanediol, ethyl-1,2,4-butanetriol, 1,2,3-butanetriol, 2,2,4-trimethyl-1,3-pentanediol, and petriol; ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethyl ... Examples of the alkyl ethers include polyhydric alcohols such as ethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether, tetraethylene glycol monomethyl ether, and propylene glycol monoethyl ether; polyhydric alcohols such as ethylene glycol monophenyl ether and ethylene glycol monobenzyl ether; nitrogen-containing heterocyclic compounds such as 2-pyrrolidone, N-methyl-2-pyrrolidone, N-hydroxyethyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, ε-caprolactam, and γ-butyrolactone; amides such as formamide, N-methylformamide, N,N-dimethylformamide, 3-methoxy-N,N-dimethylpropionamide, and 3-butoxy-N,N-dimethylpropionamide; amines such as monoethanolamine, diethanolamine, and triethylamine; sulfur-containing compounds such as dimethyl sulfoxide, sulfolane, and thiodiethanol; propylene carbonate, and ethylene carbonate. When the organic solvent is used as the penetrant, it is preferable to use triethylene glycol monobutyl ether as the penetrant. By including triethylene glycol monobutyl ether in the ink, when printing on a fabric as a recording medium described later, the penetrability into the fabric can be adjusted to an appropriate level, and the problem of the ink penetrating too much into the fabric and failing to obtain a good image can be solved, which is preferable. When the organic solvent is used as a moisturizing agent, it is preferable to use ethylene glycol and glycerin as the moisturizing agent. The ethylene glycol is relatively inexpensive and has high moisturizing properties, and can improve the ejection properties of the ink. Furthermore, when a dispersant with high hydrophilicity is used, the storage stability of the ink can be improved. The glycerin has a higher boiling point than other organic solvents, and can improve the ejection stability of the ink.

[0060] The organic solvent not only functions as a wetting agent but also has good drying properties, so it is preferable to use an organic solvent having a boiling point of 250° C. or less.

[0061] When paper is used as the recording medium, polyol compounds having 8 or more carbon atoms and glycol ether compounds can be suitably used as the organic solvent from the viewpoint of improving the permeability of the ink. Specific examples of the polyol compound having 8 or more carbon atoms include 2-ethyl-1,3-hexanediol and 2,2,4-trimethyl-1,3-pentanediol.

[0062] The content of the organic solvent is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of the drying property and ejection reliability of the ink, the content is preferably from 10% by mass to 60% by mass, more preferably from 20% by mass to 70% by mass, and even more preferably from 45% by mass to 65% by mass.

[0063] <<Additives>> The additives are not particularly limited and may be appropriately selected depending on the purpose. Examples of the additives include surfactants, antifoaming agents, antiseptic and antifungal agents, rust inhibitors, and pH adjusters that are used as other components.

[0064] -Surfactants used as other ingredients- The surfactant used as the other component is not particularly limited and can be appropriately selected depending on the purpose. Examples of the surfactant include silicone-based surfactants, fluorine-based surfactants, amphoteric surfactants, nonionic surfactants, and anionic surfactants. In this specification, the term "surfactant used as another component" refers to a surfactant contained in the ink of the present invention as another component, and does not fall under the above-mentioned <other polymerizable monomers>.

[0065] --Silicone surfactants-- The silicone surfactant is not particularly limited and can be appropriately selected depending on the purpose, but it is preferable that the silicone surfactant does not decompose even at high pH (pH 11 to 14). Specific examples of silicone surfactants that do not decompose even at high pH (pH 11 to 14) include side-chain modified polydimethylsiloxane, both-end modified polydimethylsiloxane, one-end modified polydimethylsiloxane, side-chain both-end modified polydimethylsiloxane, etc. Among these, polyether-modified silicone surfactants having a polyoxyethylene group or a polyoxyethylene polyoxypropylene group as a modifying group are preferred from the viewpoint of improving hydrophilicity and increasing solubility in water. These may be used alone or in combination of two or more.

[0066] The polyether-modified silicone surfactant is not particularly limited and can be appropriately selected depending on the purpose. For example, it may be a surfactant in which a polyalkylene oxide structure represented by the general formula (S-1) is introduced into the Si part side chain of dimethylpolysiloxane.

[0067] [ka] (In the general formula (S-1), m, n, a, and b each independently represent an integer, R represents an alkylene group, and R' represents an alkyl group.)

[0068] The polyether-modified silicone surfactant may be appropriately synthesized or may be a commercially available product. Examples of commercially available polyether-modified silicone surfactants include KF-618, KF-642, KF-643 (all manufactured by Shin-Etsu Chemical Co., Ltd.), EMALEX-SS-5602, EMALEX-SS-1906EX (all manufactured by Nippon Emulsion Co., Ltd.), FZ-2105, FZ-2118, FZ-2154, FZ-2161, FZ-2162, FZ-2163, FZ-2164 (all manufactured by Toray Dow Corning Silicone Co., Ltd.), BYK-33, BYK-387 (all manufactured by Big Chemie Co., Ltd.), TSF4440, TSF4452, TSF4453 (all manufactured by Toshiba Silicon Co., Ltd.), etc.

[0069] The silicone surfactant may be a synthetic product or a commercially available product, such as those available from BYK Chemical Co., Ltd., Shin-Etsu Chemical Co., Ltd., Dow Corning Toray Silicone Co., Ltd., Nippon Emulsion Co., Ltd., Kyoeisha Chemical Co., Ltd., etc.

[0070] --Fluorosurfactants-- The fluorine-based surfactant is not particularly limited and can be appropriately selected depending on the purpose, but is preferably a compound having 2 to 16 fluorine-substituted carbon atoms, and more preferably a compound having 4 to 16 fluorine-substituted carbon atoms.

[0071] The fluorine-based surfactant is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of low foaming, however, perfluoroalkyl sulfonic acid compounds, perfluoroalkyl carboxylic acid compounds, perfluoroalkyl phosphate compounds, perfluoroalkyl ethylene oxide adducts, and polyoxyalkylene ether polymer compounds having a perfluoroalkyl ether group in the side chain are preferred. Examples of the perfluoroalkylsulfonic acid compound include perfluoroalkylsulfonic acid and perfluoroalkylsulfonate salts. Examples of the perfluoroalkyl carboxylic acid compound include perfluoroalkyl carboxylic acids and perfluoroalkyl carboxylates. Examples of the polyoxyalkylene ether polymer compound having a perfluoroalkyl ether group on the side chain include sulfate ester salts of polyoxyalkylene ether polymers having a perfluoroalkyl ether group on the side chain, and salts of polyoxyalkylene ether polymers having a perfluoroalkyl ether group on the side chain.

[0072] Furthermore, fluorine-based surfactants represented by the following general formulas (F-1) and (F-2) are more preferred.

[0073] [ka] In the compound represented by the general formula (F-1), m is preferably an integer of 0 to 10, and n is preferably an integer of 0 to 40 in order to impart water solubility.

[0074] [ka] In the compound represented by the general formula (F-2), Y is H or C m F 2m+1 m is an integer from 1 to 6, or CH2CH(OH)CH2-C m F 2m+1 m is an integer from 4 to 6, or C p H2p+1 where p is an integer from 1 to 19. n is an integer from 1 to 6. a is an integer from 4 to 14.

[0075] Counter ions of the salts in these fluorosurfactants include Li, Na, K, NH4, NH3CH2CH2OH, NH2(CH2CH2OH)2, NH(CH2CH2OH)3, and the like.

[0076] The fluorosurfactant may be a synthetic product or a commercially available product. Examples of commercially available fluorosurfactants include Surflon S-111, Surflon S-112, Surflon S-113, Surflon S-121, Surflon S-131, Surflon S-132, Surflon S-141, Surflon S-145 (all manufactured by AGC Inc.), Fullard FC-93, Fullard FC-95, Fullard FC-98, Fullard FC-129, Fullard FC-135, Fullard FC-170C, Fullard FC-430, Fullard FC-431 (all manufactured by Sumitomo 3M Limited), Megafac F-470, Megafac F-1405, Megafac F-474 (all manufactured by DIC Corporation), Zonyl TB, etc. S, FSP, FSA, FSN-100, FSN, FSO-100, FSO, FS-300, UR, Capstone FS-30, Capstone FS-31, Capstone FS-3100, Capstone FS-34, Capstone FS-35 (all manufactured by Chemours), FT-110, FT-250, FT-251, FT-400S, FT-150, FT-400SW (all manufactured by Neos Co., Ltd.), Polyfox PF-136A, Polyfox PF-156A, Polyfox PF-151N, Polyfox PF-154, Polyfox PF-159 (all manufactured by Omnova), Unidyne DSN-403N (manufactured by Daikin Industries, Ltd.), etc. Among these, FS-3100, FS-34, FS-300 (all manufactured by Chemours), FT-110, FT-250, FT-251, FT-400S, FT-150, FT-400SW (all manufactured by Neos Corporation), Polyfox PF-151N (all manufactured by Omnova), and Unidyne DSN-403N (all manufactured by Daikin Industries, Ltd.) are preferred because they provide good printing quality, particularly improved color development, penetration into paper, wettability, and dye uniformity.

[0077] --Amphoteric surfactants-- The amphoteric surfactant is not particularly limited and can be appropriately selected depending on the purpose. Examples of the amphoteric surfactant include lauryl aminopropionate, lauryl dimethyl betaine, stearyl dimethyl betaine, and lauryl dihydroxyethyl betaine. These may be used alone or in combination of two or more.

[0078] --Nonionic surfactants-- The nonionic surfactant is not particularly limited and can be appropriately selected depending on the purpose. Examples of the nonionic surfactant include polyoxyethylene alkylphenyl ethers, polyoxyethylene alkyl esters, polyoxyethylene alkylamines, polyoxyethylene alkylamides, polyoxyethylene propylene block polymers, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, and ethylene oxide adducts of acetylene alcohol. These may be used alone or in combination of two or more.

[0079] --Anionic surfactants-- The anionic surfactant is not particularly limited and can be appropriately selected depending on the purpose. Examples of the anionic surfactant include polyoxyethylene alkyl ether acetates, dodecylbenzene sulfonates, laurates, and polyoxyethylene alkyl ether sulfates. These may be used alone or in combination of two or more.

[0080] The content of the surfactant used as another component is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of excellent wettability and ejection stability and improved image quality, however, the content is preferably from 0.001% by mass to 5% by mass, and more preferably from 0.05% by mass to 5% by mass, relative to the total amount of ink.

[0081] - Defoaming agent - The surfactant used as the other component can be used as a defoaming agent. The defoaming agent is not particularly limited and may be appropriately selected depending on the purpose, and examples thereof include silicone-based defoaming agents, polyether-based defoaming agents, fatty acid ester-based defoaming agents, etc. Among these, silicone-based defoaming agents are preferred because of their excellent foam breaking effect. These may be used alone or in combination of two or more.

[0082] -Preservative and fungicidal agent- The antiseptic and antifungal agent is not particularly limited and can be appropriately selected depending on the purpose. For example, 1,2-benzisothiazolin-3-one and the like can be mentioned.

[0083] -pH adjuster- The pH adjuster is not particularly limited and may be appropriately selected depending on the purpose as long as it can adjust the pH to 7 or more, and examples thereof include amines such as diethanolamine and triethanolamine. Among these, triethanolamine, which is inexpensive, is preferable. The content of the pH adjuster is preferably 0.5% by mass or less based on the total amount of the ink, and more preferably 0.25% by mass or more and 0.5% by mass or less from the viewpoint of storage stability of the ink.

[0084] <<Radical polymerization initiator>> In the process of forming the copolymer in the present invention, a radical polymerization initiator may be used. The radical polymerization initiator is not particularly limited and may be appropriately selected depending on the purpose, and examples thereof include peroxyketals, hydroperoxides, dialkyl peroxides, diacyl peroxides, peroxydicarbonates, peroxyesters, cyano-based azobisisobutyronitrile, azobis(2-methylbutyronitrile), azobis(2,2'-isovaleronitrile), and non-cyano-based dimethyl-2,2'-azobisisobutyrate, etc. Among these, organic peroxides and azo-based compounds are preferred, and azo-based compounds are more preferred, in terms of ease of molecular weight control and low decomposition temperature.

[0085] The content of the radical polymerization initiator is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1% by mass or more and 10% by mass or less with respect to the total amount of the polymerizable monomers. Note that the "polymerizable monomer" refers to all monomers including the first monomer, the second monomer, and the third monomer.

[0086] <<Chain transfer agent>> In order to adjust the molecular weight of the copolymer in the present invention, a chain transfer agent may be added. The chain transfer agent is not particularly limited and can be appropriately selected depending on the purpose. Examples of the chain transfer agent include mercaptoacetic acid, mercaptopropionic acid, 2-propanethiol, 2-mercaptoethanol, thiophenol, dodecyl mercaptan, 1-dodecanethiol, and thioglycerol.

[0087] [Ink properties] The physical properties of the ink of the present invention are not particularly limited and can be appropriately set depending on the purpose. For example, it is preferable that the viscosity, surface tension, pH, etc. are within the following ranges. The viscosity of the ink of the present invention at 25°C is preferably from 5 mPa·s to 30 mPa·s, more preferably from 5 mPa·s to 25 mPa·s, in order to improve print density and character quality and to obtain good ejection properties. Here, the viscosity can be measured using, for example, a rotational viscometer (RE-80L manufactured by Toki Sangyo Co., Ltd.). The viscosity can be measured under the following conditions: 25°C, standard cone rotor (1°34'×R24), sample liquid volume 1.2 mL, rotation speed 50 rpm, and 3 minutes. The surface tension of the ink of the present invention is preferably 35 mN / m or less, and more preferably 32 mN / m or less at 25° C., from the viewpoints of suitably leveling the ink on a recording medium described below and shortening the drying time of the ink. The pH of the ink of the present invention is preferably from 7 to 12, and more preferably from 8 to 11, from the viewpoint of preventing corrosion of metal members that come into contact with the ink.

[0088] Methods for qualitatively and quantitatively analyzing the organic solvent, polymer, copolymer, pigment, and other components contained in the ink of the present invention include, for example, gas chromatography mass spectrometry (GC-MS). An example of a measuring device using gas chromatography mass spectrometry (GC-MS) is GCMS-QP2020NX (manufactured by Shimadzu Corporation). The amount of water contained in the ink can be measured by a general method such as quantifying the volatile components using gas chromatography mass spectrometry (GC-MS) or measuring mass fluctuations using thermogravimetry-differential thermal analysis (TG-DTA).

[0089] (Ink storage container) The ink of the present invention can be used by being contained in a container. In this specification, a container that contains the ink of the present invention is sometimes referred to as an "ink containing container." The ink container is not particularly limited, and examples thereof include known ink cartridges for inkjet printers. The ink storage container is easy to store, transport, and the like, and has excellent handleability, and can therefore be detachably attached to an ink cartridge, image forming apparatus, or the like, and used to replenish ink. The ink container is not particularly limited and can be appropriately selected from known containers, and examples thereof include a container having a container body and a cap.

[0090] The shape of the ink container is not particularly limited and may be appropriately selected depending on the purpose, but is preferably cylindrical. Furthermore, it is preferable that the inner peripheral surface is formed with a spiral irregularity so that the ink contained therein can move to the outlet side by rotating the container, and that a part or all of the spiral irregularity has a bellows function. The material of the ink container is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of good dimensional accuracy, however, resins such as polyester resin, polyethylene resin, polypropylene resin, polystyrene resin, polyvinyl chloride resin, polyacrylic acid, polycarbonate resin component ABS resin, and polyacetal resin are preferred. The structure and size of the ink container are not particularly limited and can be appropriately selected according to the purpose.

[0091] (Image forming apparatus and image forming method) The image forming apparatus of the present invention comprises an ink containing container that contains the ink of the present invention, and an ejection means that ejects the ink contained in the ink containing container onto a recording medium, and may also have other means as necessary. The image forming method of the present invention comprises a step of ejecting the ink of the present invention onto a recording medium to form an image, and may also comprise other steps as necessary. The image forming method can be suitably carried out by the image forming apparatus.

[0092] <Discharge Means and Discharge Process> The ejection means ejects the ink contained in the ink container onto a recording medium. The ejection step is a step of ejecting the ink contained in the ink container onto a recording medium. The ejection step can be suitably carried out by the ejection means. The ejection means is not particularly limited, and any known ink ejection means can be used, such as an inkjet system.

[0093] <Other means and other steps> The other means are not particularly limited and can be appropriately selected depending on the purpose. Examples of the other means include pre-treatment means, post-treatment means, heating means, drying means, and means related to feeding, transporting, and discharging of the recording medium. The other steps are not particularly limited and can be appropriately selected depending on the purpose. Examples of the other steps include a pre-treatment step, a post-treatment step, a heating step, a drying step, and steps related to feeding, transporting, and discharging a recording medium. The other steps can be suitably carried out by the other means.

[0094] -Pretreatment means and pretreatment process- The pretreatment means is a means for applying a pretreatment liquid to the recording medium before applying the ink. The pretreatment step is a step of applying a pretreatment liquid to the recording medium before applying the ink. The pretreatment step can be suitably carried out by the pretreatment means. One aspect of a pretreatment device equipped with the pretreatment means is to add a liquid storage section having the pretreatment liquid and a liquid ejection head, as in the case of inks such as black (K), cyan (C), magenta (M), yellow (Y), and white (W), and to eject the pretreatment liquid by an inkjet recording method. The pretreatment means is not particularly limited and can be appropriately selected depending on the purpose. Examples of the pretreatment means include a means in which the pretreatment liquid is stored in an ink storage means like a normal ink and applied to a recording medium by an inkjet method, a blade coating method, a roll coating method, a spray coating method, and the like.

[0095] The pretreatment liquid contains a flocculant, an organic solvent, and water, and may contain, as necessary, a surfactant, an antifoaming agent, a pH adjuster, an antiseptic / fungal agent, an antirust agent, and the like. The organic solvent, the surfactant, the defoaming agent, the pH adjuster, the preservative and antifungal agent, and the rust inhibitor can be similar to the materials used in the ink, and other materials used in known treatment liquids can be used. The type of the flocculant is not particularly limited and can be appropriately selected depending on the purpose. Examples of the flocculant include water-soluble cationic polymers, acids, and polyvalent metal salts.

[0096] -Post-processing means and post-processing process- The post-treatment unit is a unit that applies a post-treatment liquid to the recording medium after applying the ink. The pretreatment step is a step of applying a posttreatment liquid to the recording medium after applying the ink. The post-treatment step can be suitably carried out by the post-treatment means. One aspect of a post-processing device equipped with the post-processing means is to add a liquid storage section having the post-processing liquid and a liquid ejection head, as in the case of inks such as black (K), cyan (C), magenta (M), yellow (Y), and white (W), and to eject the post-processing liquid by an inkjet recording method. The post-treatment means is not particularly limited and can be appropriately selected depending on the purpose. Examples of the post-treatment means include a means in which the post-treatment liquid is stored in an ink storage means like a normal ink and applied to a recording medium by an inkjet method, a blade coating method, a roll coating method, a spray coating method, and the like.

[0097] The post-treatment liquid is not particularly limited as long as it can form a transparent layer. The post-treatment liquid is obtained by selecting and mixing organic solvents, water, resins, surfactants, defoamers, pH adjusters, antiseptics, antifungals, rust inhibitors, etc. as necessary. The post-treatment liquid may be applied to the entire recording area formed on the recording medium, or may be applied only to the area where an image is formed.

[0098] -Heating means and heating process, and drying means and drying process- The heating means includes, for example, a means for heating the print surface or the back surface of the recording medium. The heating step includes, for example, a step of heating the print surface and the back surface of the recording medium. The heating step can be suitably carried out by the heating means. The drying means includes, for example, a means for drying the printed surface and the back surface of the recording medium. The drying step includes, for example, a step of drying the printed surface and the back surface of the recording medium. The drying step can be suitably carried out by the drying means. The heating means and drying means are not particularly limited, and for example, a hot air heater, an infrared heater, etc. Heating and drying can be carried out before, during, or after printing.

[0099] The image forming apparatus and the image forming method are not limited to those that visualize meaningful images such as characters and figures with ink. For example, they also include those that form patterns such as geometric patterns and those that create three-dimensional images. Unless otherwise specified, the image forming apparatus includes both a serial type apparatus in which the ejection head is moved and a line type apparatus in which the ejection head is not moved. The image forming device includes not only desktop types, but also wide recording devices capable of printing on A0 size recording media, and continuous feed printers that can use continuous paper wound into a roll as a recording medium.

[0100] <Recording Media> The term "recording medium" used herein refers to an object on which recording is performed using the ink of the present invention. The recording medium also refers to an object on which the ink of the present invention and various treatment liquids can be attached, even if only temporarily. The recording medium is not particularly limited and can be appropriately selected depending on the purpose. For example, plain paper, glossy paper, special paper, cloth, film, OHP sheet, general-purpose printing paper, non-permeable substrate, etc. may be used. The non-permeable substrate is a substrate having a surface with low water permeability and low absorbency, and includes materials that have many cavities inside but are not open to the outside. More quantitatively, in the Bristow method, 1 / 2 Water absorption up to 10mL / m 2 The term "substrate" refers to a substrate that is: Examples of the non-permeable substrate include plastic films such as polyvinyl chloride resin films, polyethylene terephthalate (PET) films, polypropylene, polyethylene, and polycarbonate films.

[0101] The recording medium is not limited to those generally used as recording media, and may be appropriately used wallpaper, flooring, building materials such as tiles, cloth for clothing such as T-shirts, textiles, leather, etc. Also, by adjusting the configuration of the path for conveying the recording medium, ceramics, glass, metal, etc. may be used.

[0102] <Recordings> An image formed on the recording medium using the ink of the present invention can be considered as a recorded matter. The recorded matter can be obtained by recording using the image forming apparatus and image forming method.

[0103] Here, an example of the image forming apparatus of the present invention will be described with reference to Figs. 1 and 2. Fig. 1 is a perspective view of the apparatus. Fig. 2 is a perspective view of a main tank. The image forming apparatus 400 is a serial type image forming apparatus. A mechanism unit 420 is provided inside an exterior 401 of the image forming apparatus 400. Each ink storage unit 411 of the main tanks 410 (410k, 410c, 410m, 410y, 410w) for each color of black (K), cyan (C), magenta (M), yellow (Y), and white (W) is formed of a packaging material such as an aluminum laminate film. The ink storage unit 411 is stored in a storage container case 414 made of plastic, for example. As a result, the main tanks 410 are used as ink cartridges of each color. On the other hand, a cartridge holder 404 is provided at the back side of the opening when the cover 401c of the apparatus body is opened. A main tank 410 is detachably attached to the cartridge holder 404. This allows each ink outlet 413 of the main tank 410 to communicate with an ejection head 434 for each color via a supply tube 436 for each color, making it possible to eject ink from the ejection head 434 to a recording medium.

[0104] <Application> The ink of the present invention can be suitably used in various recording devices using the ink jet recording method, such as printers, facsimile machines, copying machines, printer / fax / copier combination machines, and three-dimensional modeling devices. The application of the ink of the present invention is not particularly limited and can be appropriately selected depending on the purpose, and can be applied to, for example, printed matter, paint, coating material, base, etc. Furthermore, it can be used not only to form two-dimensional characters and images, but also as a material for three-dimensional modeling to form three-dimensional solid images (three-dimensional objects). The three-dimensional object includes a three-dimensional object obtained by applying ink in layers, etc. Also included is a molded product obtained by processing a structure in which ink is applied onto a substrate such as a recording medium. The three-dimensional modeling device for forming the three-dimensional object can be a known one, and is not particularly limited, but can be, for example, one equipped with ink storage means, supply means, ejection means, drying means, etc. The molded products are, for example, products obtained by subjecting recorded matter or structures formed into a sheet or film shape to molding processes such as heat stretching or punching, and are suitably used for applications in which the surface is molded after decoration, such as meters and operation panel for automobiles, office automation equipment, electric and electronic equipment, cameras, etc.

[0105] (Solar cell backsheet) A polymer having a structural unit represented by the general formula (1) or a copolymer having a structural unit represented by the general formula (1) and a structural unit represented by the general formula (2) can also be used as a resin contained in a protective layer of a solar cell backsheet. In other words, the solar cell backsheet of the present invention is a solar cell backsheet having a protective layer, characterized in that the protective layer is a coating film made of the ink, and may contain other resins (B) as necessary. Note that the "ink" is the same as that described in the above (ink) section, and therefore the description is omitted. The solar cell backsheet of the present invention can improve weather resistance against light irradiation from the light-receiving surface side and the back surface side of the solar cell module, for example, by providing it on the back surface of the solar cell module.

[0106] The protective layer is preferably provided on a substrate film. The substrate film is not particularly limited and can be appropriately selected depending on the purpose, but is preferably a polyester film from the viewpoint of excellent mechanical strength, dimensional stability, and thermal stability, and more preferably a polyester film mainly composed of polyethylene terephthalate or polyethylene naphthalate.

[0107] The protective layer in the solar cell module may contain another resin (B). The other resin (B) is not particularly limited and may be appropriately selected depending on the purpose, but from the viewpoint of excellent mechanical strength and heat resistance, an acrylic resin is preferable, and an acrylic resin capable of being crosslinked with an isocyanate is more preferable.

[0108] The method for producing the solar cell backsheet is not particularly limited and can be appropriately selected depending on the purpose. For example, the solar cell backsheet can be produced by the following method (steps (1) to (4)). Step (1): The polymer or copolymer of the present invention is added to an organic solvent, and the solution is prepared by stirring and dissolving the polymer or copolymer. If necessary, a colorant is gradually added to the solution while stirring the solution, and the solution is stirred again. Step (2): After dispersing with a dispersing device, the contents are filtered with a membrane filter. If necessary, an adjusted amount of an organic solvent is added to prepare a protective layer forming liquid. Step (3): The protective layer forming liquid is applied to the surface of the substrate using a wire bar and dried until a desired thickness is reached, to form a protective layer (coating film). Step (4): The protective layer is aged to obtain a solar cell backsheet.

[0109] The organic solvent in step (1) is not particularly limited and can be appropriately selected depending on the purpose. For example, the organic solvents described in the above (Ink) section or hexamethylene diisocyanate can be suitably used. The coloring material used in step (1) is not particularly limited and can be appropriately selected depending on the purpose. For example, the coloring materials described in the above (ink) section can be suitably used. The dispersing device in step (2) is not particularly limited and can be appropriately selected depending on the purpose, for example, Big Rotor BR-2 (manufactured by AS ONE Corporation), etc. The conditions for the dispersion treatment are not particularly limited and can be appropriately selected depending on the purpose, for example, the rotation speed can be set to 90 rpm and the treatment time can be set to 5 days, etc. The substrate in step (3) is not particularly limited and can be appropriately selected depending on the purpose. For example, the recording media described in the above section (Image forming apparatus and image forming method) can be suitably used. The "any film thickness" in step (3) is not particularly limited and can be appropriately selected depending on the purpose, and can be, for example, 2 μm. The drying conditions in the step (3) are not particularly limited and can be appropriately selected depending on the purpose. For example, the drying temperature can be set to 150° C. and the drying time can be set to 5 minutes. The aging conditions in the step (4) are not particularly limited and can be appropriately selected depending on the purpose. For example, the treatment temperature can be set to 50° C. and the treatment time can be set to 3 days.

[0110] In this specification, the terms image formation, recording, printing, printing, etc. are all synonymous. In this specification, the terms recording medium, media, and printed matter are all synonymous. EXAMPLES

[0111] Examples of the present invention will be described below, but the scope of the present invention is not limited to these examples. In the following examples and comparative examples, "parts" and "%" are "parts by mass" and "% by mass" unless otherwise specified.

[0112] The molecular weights of the polymers and copolymers obtained in the Synthesis Examples, Examples, and Comparative Examples described below were measured by the following methods and conditions. [Method for measuring weight average molecular weight] Measurement was performed by GPC (Gel Permeation Chromatography) under the following conditions. Equipment: GPC-8320GPC (Tosoh Corporation) Column: TSK G2000HXL and G4000HXL (Tosoh Corporation) ·Temperature: 40℃ Solvent: THF (tetrahydrofuran) Flow rate: 0.6mL / min 1 mL of copolymer having a concentration of 0.5% by mass was injected into the above apparatus, and the weight average molecular weight Mw of the polymer and copolymer was calculated from the molecular weight distribution of the copolymer measured under the above conditions using a molecular weight calibration curve prepared from a monodisperse polystyrene standard sample.

[0113] (Synthesis Example 1) <Synthesis of Monomer M-1> 11.77g (120mmol) of concentrated sulfuric acid (Kokusan Kagaku) ​​was added little by little to 31.03g (500mmol) of ethylene glycol (Tokyo Kasei Co., Ltd.), and the mixture was heated to 50°C. 12.31g (100mmol) of isonicotinic acid (Tokyo Kasei Co., Ltd.) was added little by little with stirring, and the mixture was heated to 120°C and stirred for 5 hours. After cooling to room temperature, 4N aqueous sodium hydroxide solution (Kanto Kagaku Co., Ltd.) was added with stirring until the pH reached 7. The mixture was extracted twice with 150ml of ethyl acetate (Kanto Kagaku Co., Ltd.), and the isolated organic phase was washed twice with 150ml of water, and then the isolated organic phase was dried over magnesium sulfate (Kanto Kagaku Co., Ltd.). The solvent was distilled off from the organic phase, and the residue was purified by silica gel column chromatography using a mixed solvent of hexane (manufactured by Kanto Chemical Co., Ltd.) / ethyl acetate (manufactured by Kanto Chemical Co., Ltd.) (volume ratio 5 / 5 to 0 / 10) as an eluent to obtain 9.55 g of intermediate 1.

[0114] [ka]

[0115] Next, 8.36 g (50 mmol) of intermediate 1 was dissolved in 20 mL of dehydrated tetrahydrofuran (THF) (Kanto Chemical Co., Ltd.). A solution of 9.31 g (60 mmol) of 2-isocyanate ethyl methacrylate (Tokyo Chemical Industry Co., Ltd.) dissolved in 10 mL of dehydrated THF was added dropwise to this solution over 10 minutes, and then stirred at 35°C for 12 hours. The solvent was distilled off from the resulting reaction solution, and the residue was purified by silica gel column chromatography using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 0 / 10) as an eluent, to obtain 11.55 g of monomer M-1.

[0116] [ka]

[0117] (Synthesis Example 2) <Synthesis of Monomer M-2> 59.08g (500mmol) of 1,6-hexanediol (Tokyo Chemical Industry Co., Ltd.) was heated to 80°C, 11.77g (120mmol) of concentrated sulfuric acid was added in small portions, and then 12.31g (100mmol) of isonicotinic acid was added in small portions with stirring, and the mixture was heated to 120°C and stirred for 5 hours. After cooling to room temperature, 4N aqueous sodium hydroxide solution was added with stirring until the pH reached 7. Extraction was performed twice with 200ml of ethyl acetate, and the isolated organic phase was washed twice with 200ml of water, and then the isolated organic phase was dried over magnesium sulfate. The solvent was distilled off from the organic phase, and the residue was purified by column chromatography on silica gel using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 0 / 10) as an eluent to obtain 13.67g of intermediate 2.

[0118] [ka]

[0119] Next, 11.16 g (50 mmol) of intermediate 2 was dissolved in 20 mL of dehydrated THF. To this solution, a solution in which 9.31 g (60 mmol) of 2-isocyanate ethyl methacrylate was dissolved in 10 mL of dehydrated THF was dropped over 10 minutes, and then the mixture was stirred at 35°C for 12 hours. The solvent was distilled off from the resulting reaction solution, and the residue was purified by silica gel column chromatography using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 0 / 10) as an eluent, to obtain 13.34 g of monomer M-2.

[0120] [ka]

[0121] (Synthesis Example 3) <Synthesis of Monomer M-3> 11.16g (50mmol) of intermediate 2 was dissolved in 20mL of dehydrated THF. To this solution, 12.68g (60mmol) of methacrylic acid 6-isocyanate hexyl ester (manufactured by Hong Kong Chemhere Co., Ltd.) dissolved in 10mL of dehydrated THF was dropped over 10 minutes, and then stirred at 35°C for 12 hours. The solvent was distilled off from the resulting reaction solution, and the residue was purified by silica gel column chromatography using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 0 / 10) as an eluent, to obtain 13.34g of monomer M-3.

[0122] [ka]

[0123] (Synthesis Example 4) <Synthesis of Monomer M-4> 11.16g (50mmol) of intermediate 2 was dissolved in 20mL of dehydrated THF. To this solution, 16.05g (60mmol) of methacrylic acid (3-methyl-7,7-dimethyl-7-isocyanate) hexyl ester (manufactured by Hong Kong Chemhere Co., Ltd.) dissolved in 10mL of dehydrated THF was dropped over 10 minutes, and then stirred at 35°C for 12 hours. The solvent was distilled off from the resulting reaction solution, and the residue was purified by silica gel column chromatography using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 0 / 10) as an eluent, to obtain 17.47g of monomer M-4.

[0124] [ka]

[0125] (Synthesis Example 5) <Synthesis of Monomer M-5> 87.14g (500mmol) of 1,10-decanediol (Tokyo Chemical Industry Co., Ltd.) was heated to 80°C, 11.77g (120mmol) of concentrated sulfuric acid was added in small portions, and then 12.31g (100mmol) of isonicotinic acid was added in small portions with stirring, and the mixture was heated to 120°C and stirred for 5 hours. After cooling to room temperature, 4N aqueous sodium hydroxide solution was added with stirring until the pH reached 7. Extraction was performed twice with 200ml of ethyl acetate, and the isolated organic phase was washed twice with 200ml of water, and then the isolated organic phase was dried over magnesium sulfate. The solvent was distilled off from the organic phase, and the residue was purified by column chromatography on silica gel using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 0 / 10) as an eluent to obtain 14.55g of intermediate 3.

[0126] [ka]

[0127] Next, 13.97 g (50 mmol) of intermediate 3 was dissolved in 20 mL of dehydrated THF. To this solution, 16.05 g (60 mmol) of methacrylic acid (3-methyl-7,7-dimethyl-7-isocyanate) hexyl ester (manufactured by Hong Kong Chemhere Co., Ltd.) dissolved in 10 mL of dehydrated THF was dropped over 10 minutes, and then stirred at 35 ° C for 12 hours. The solvent was distilled off from the obtained reaction solution, and the residue was purified by silica gel column chromatography using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 0 / 10) as an eluent, to obtain 16.23 g of monomer M-5.

[0128] [ka]

[0129] (Synthesis Example 6) <Synthesis of Monomer M-6> 9.51 g (100 mmol) of 4-hydroxypyridine, 21.73 g (120 mmol) of 6-bromo-1-hexanol (Tokyo Chemical Industry Co., Ltd.), and 27.64 g (200 mmol) of potassium carbonate (Kanto Chemical Industry Co., Ltd.) were added to 50 mL of methyl ethyl ketone (Kanto Chemical Industry Co., Ltd.), and the mixture was refluxed for 18 hours. After cooling to room temperature, the mixture was filtered, and the solvent was distilled off from the filtrate. The residue was purified by silica gel column chromatography using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 0 / 10) as an eluent, and 15.12 g of intermediate 4 was obtained.

[0130] [ka]

[0131] Next, 9.77 g (50 mmol) of intermediate 4 was dissolved in 20 mL of dehydrated THF. To this solution, a solution of 8.47 g (60 mmol) of acrylic acid 2-isocyanate ethyl ester (Tokyo Chemical Industry Co., Ltd.) dissolved in 10 mL of dehydrated THF was dropped over 10 minutes, and then stirred at 35 ° C for 12 hours. The solvent was distilled off from the obtained reaction solution, and the residue was purified by silica gel column chromatography using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 0 / 10) as an eluent, to obtain 14.38 g of monomer M-6.

[0132] [ka]

[0133] (Synthesis Example 7) <Synthesis of Monomer M-7> 59.10g (500mmol) of 1,6-hexanediol was heated to 80°C, 11.77g (120mmol) of concentrated sulfuric acid was added in small portions, and then 15.12g (100mmol) of 3-(3-pyridyl)propionic acid was added in small portions with stirring, and the mixture was heated to 120°C and stirred for 5 hours. After cooling to room temperature, 4N aqueous sodium hydroxide solution was added with stirring until the pH reached 7. 250ml of ethyl acetate was added to extract the organic matter, washed with 300ml of water, and dried over magnesium sulfate. The solvent was distilled off, and the residue was purified by column chromatography on silica gel using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 0 / 10) as an eluent to obtain 15.88g of intermediate 5.

[0134] [ka]

[0135] Next, 12.57 g (50 mmol) of intermediate 5 was dissolved in 20 mL of dehydrated THF. To this solution, a solution in which 8.47 g (60 mmol) of acrylic acid 2-isocyanate ethyl ester was dissolved in 10 mL of dehydrated THF was dropped over 10 minutes, and then the mixture was stirred at 35°C for 12 hours. The solvent was distilled off from the resulting reaction solution, and the residue was purified by silica gel column chromatography using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 0 / 10) as an eluent, to obtain 14.62 g of monomer M-7.

[0136] [ka]

[0137] (Synthesis Example 8) <Synthesis of Monomer M-8> 6.68g (50mmol) of 4-pyridinepropanol (Tokyo Chemical Industry Co., Ltd.) was dissolved in 10mL of dehydrated THF. A solution of 8.47g (60mmol) of acrylic acid 2-isocyanate ethyl ester dissolved in 10mL of dehydrated THF was added dropwise to this solution over 10 minutes, and then stirred at 35°C for 12 hours. The solvent was distilled off from the resulting reaction solution, and the residue was purified by silica gel column chromatography using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 0 / 10) as an eluent, to obtain 9.87g of monomer M-8.

[0138] [ka]

[0139] (Synthesis Example 9) <Synthesis of Monomer M-9> 5.41g (50mmol) of 4-(aminomethyl)pyridine (Tokyo Chemical Industry Co., Ltd.) was dissolved in 10mL of dehydrated THF. A solution of 8.47g (60mmol) of acrylic acid 2-isocyanate ethyl ester dissolved in 10mL of dehydrated THF was added dropwise to this solution over 10 minutes, and then stirred at 35°C for 12 hours. The solvent was distilled off from the resulting reaction solution, and the residue was purified by silica gel column chromatography using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 0 / 10) as an eluent, to obtain 8.91g of monomer M-9.

[0140] [ka]

[0141] (Synthesis Example 10) <Synthesis of Monomer M-10> 6.11g (50mmol) of 4-(2-aminoethyl)pyridine (Tokyo Chemical Industry Co., Ltd.) was dissolved in 10mL of dehydrated THF. A solution of 8.47g (60mmol) of acrylic acid 2-isocyanate ethyl ester dissolved in 10mL of dehydrated THF was added dropwise to this solution over 10 minutes, and then stirred at 35°C for 12 hours. The solvent was distilled off from the resulting reaction solution, and the residue was purified by silica gel column chromatography using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 0 / 10) as an eluent, to obtain 9.87g of monomer M-10.

[0142] [ka]

[0143] (Synthesis Example 11) <Synthesis of Monomer M-11> 11.16g (50mmol) of intermediate 2 was dissolved in 20mL of dehydrated THF. To this solution, 9.25g (60mmol) of N-(3-isocyanatepropyl)acrylamide (manufactured by Chemieliva Pharmaceutical Co.,Ltd.) dissolved in 10mL of dehydrated THF was dropped over 10 minutes, and then stirred at 35°C for 12 hours. The solvent was distilled off from the resulting reaction solution, and the residue was purified by silica gel column chromatography using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 0 / 10) as an eluent, to obtain 14.22g of monomer M-11.

[0144] [ka]

[0145] (Synthesis Example 12) <Synthesis of Monomer M-12> 9.76 g (50 mmol) of intermediate 4 was dissolved in 20 mL of dehydrated THF. To this solution, a solution of 9.25 g (60 mmol) of N-(3-isocyanatepropyl)acrylamide dissolved in 10 mL of dehydrated THF was added dropwise over 10 minutes, and then stirred at 35°C for 12 hours. The solvent was distilled off from the resulting reaction solution, and the residue was purified by silica gel column chromatography using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 0 / 10) as an eluent, to obtain 12.80 g of monomer M-12.

[0146] [ka]

[0147] (Synthesis Example 13) <Synthesis of Monomer M-13> 12.57g (50mmol) of intermediate 5 was dissolved in 20mL of dehydrated THF. A solution of 9.25g (60mmol) of N-(3-isocyanatepropyl)acrylamide dissolved in 10mL of dehydrated THF was added dropwise to this solution over 10 minutes, and then stirred at 35°C for 12 hours. The solvent was distilled off from the resulting reaction solution, and the residue was purified by silica gel column chromatography using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 0 / 10) as an eluent, to obtain 15.22g of monomer M-13.

[0148] [ka]

[0149] (Synthesis Example 14) <Synthesis of Monomer M-14> 6.86g (50mmol) of 4-pyridinepropanol was dissolved in 10mL of dehydrated THF. A solution of 9.25g (60mmol) of N-(3-isocyanatepropyl)acrylamide dissolved in 10mL of dehydrated THF was added dropwise to this solution over 10 minutes, and then stirred at 35°C for 12 hours. The solvent was distilled off from the resulting reaction solution, and the residue was purified by silica gel column chromatography using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 0 / 10) as an eluent, to obtain 10.89g of monomer M-14.

[0150] [ka]

[0151] (Synthesis Example 15) <Synthesis of Monomer M-15> 5.41g (50mmol) of 4-(aminomethyl)pyridine was dissolved in 10mL of dehydrated THF. To this solution, 9.25g (60mmol) of N-(3-isocyanatepropyl)acrylamide was dissolved in 10mL of dehydrated THF and added dropwise over 10 minutes, followed by stirring at 35°C for 12 hours. The solvent was removed from the resulting reaction solution, and the residue was purified by silica gel column chromatography using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 0 / 10) as an eluent to obtain 9.87g of monomer M-15.

[0152] [ka]

[0153] (Synthesis Example 16) <Synthesis of Monomer M-16> 11.16g (50mmol) of intermediate 2 was dissolved in 20mL of dehydrated THF. To this solution, 11.95g (60mmol) of methacrylic acid 2-(2-isocyanate ethoxy) ethyl ester (manufactured by Chemieliva Pharmaceutical Co., Ltd.) dissolved in 10mL of dehydrated THF was dropped over 10 minutes, and then stirred at 35°C for 12 hours. The solvent was distilled off from the resulting reaction solution, and the residue was purified by silica gel column chromatography using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 0 / 10) as an eluent, to obtain 15.44g of monomer M-16.

[0154] [ka]

[0155] (Synthesis Example 17) <Synthesis of Monomer M-17> 9.76 g (50 mmol) of intermediate 4 was dissolved in 20 mL of dehydrated THF. To this solution, 11.95 g (60 mmol) of methacrylic acid 2-(2-isocyanate ethoxy) ethyl ester was dissolved in 10 mL of dehydrated THF, and then the solution was dropped over 10 minutes, followed by stirring at 35°C for 12 hours. The solvent was removed from the resulting reaction solution, and the residue was purified by silica gel column chromatography using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 0 / 10) as an eluent, to obtain 14.18 g of monomer M-17.

[0156] [ka]

[0157] (Synthesis Example 18) <Synthesis of Monomer M-18> 12.57g (50mmol) of intermediate 5 was dissolved in 20mL of dehydrated THF. To this solution, 11.95g (60mmol) of methacrylic acid 2-(2-isocyanate ethoxy) ethyl ester was dissolved in 10mL of dehydrated THF, and then the solution was dropped over 10 minutes, followed by stirring at 35°C for 12 hours. The solvent was distilled off from the resulting reaction solution, and the residue was purified by silica gel column chromatography using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 0 / 10) as an eluent, to obtain 16.45g of monomer M-18.

[0158] [ka]

[0159] (Synthesis Example 19) <Synthesis of Monomer M-19> 6.86g (50mmol) of 4-pyridinepropanol was dissolved in 10mL of dehydrated THF. To this solution, 11.95g (60mmol) of methacrylic acid 2-(2-isocyanate ethoxy) ethyl ester was dissolved in 10mL of dehydrated THF, and then the solution was dropped over 10 minutes, followed by stirring at 35°C for 12 hours. The solvent was removed from the resulting reaction solution, and the residue was purified by silica gel column chromatography using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 0 / 10) as an eluent, to obtain 12.45g of monomer M-19.

[0160] [ka]

[0161] (Synthesis Example 20) <Synthesis of Monomer M-20> 5.41g (50mmol) of 4-(2-aminomethyl)pyridine was dissolved in 10mL of dehydrated THF. To this solution, 11.95g (60mmol) of methacrylic acid 2-(2-isocyanate ethoxy) ethyl ester was dissolved in 10mL of dehydrated THF, and then the solution was dropped over 10 minutes, followed by stirring at 35°C for 12 hours. The solvent was distilled off from the resulting reaction solution, and the residue was purified by silica gel column chromatography using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 0 / 10) as an eluent, to obtain 11.35g of monomer M-20.

[0162] [ka]

[0163] The structures of the monomers M-1 to M-20 obtained in Monomer Synthesis Examples 1 to 20 are shown in Tables 1 to 2.

[0164] [Table 1]

[0165] [Table 2]

[0166] (Comparative Synthesis Example 1) <Synthesis of Comparative Monomer RM-1> 13.01g (100mmol) of 2-hydroxyethyl methacrylate was dissolved in 50mL of dimethylacetamide (Kanto Chemical Co., Ltd.), and 16.81g (100mmol) of hexamethylene diisocyanate was added dropwise over 30 minutes, followed by stirring at room temperature for 4 hours. Next, a solution of 12.31g (100mmol) of 2-(2-hydroxyethyl)pyridine dissolved in 20mL of dimethylacetamide was added, followed by stirring at room temperature for 4 hours. 300mL of water was added to the resulting reaction solution, and the mixture was extracted twice with 200mL of ethyl acetate. The isolated organic phase was dried over magnesium sulfate, and the solvent was distilled off. The residue was purified by silica gel column chromatography using a mixed solvent of hexane / ethyl acetate (volume ratio 4 / 6 to 0 / 10) as an eluent, to obtain 22.73g of comparative monomer RM-1.

[0167] [ka]

[0168] (Comparative Synthesis Example 2) <Synthesis of Comparative Monomer RM-2> 59.08g (500mmol) of 1,6-hexanediol was heated to 80°C, 1.96g (20mmol) of concentrated sulfuric acid was added in small portions, and then 12.22g (100mmol) of benzoic acid was added in small portions with stirring, and the mixture was heated to 120°C and stirred for 5 hours. After cooling to room temperature, 4N aqueous sodium hydroxide solution was added with stirring until the pH reached 7. Extraction was performed twice with 200ml of ethyl acetate, and the isolated organic phase was washed twice with 200ml of water, and then the isolated organic phase was dried over magnesium sulfate. The solvent was distilled off from the organic phase, and the residue was purified by column chromatography on silica gel using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 0 / 10) as an eluent to obtain 13.81g of benzoic acid 6-hydroxyhexyl ester. Next, 11.12 g (50 mmol) of benzoic acid 6-hydroxyhexyl ester was dissolved in 20 mL of dehydrated THF. To this solution, a solution of 9.31 g (60 mmol) of methacrylic acid 2-isocyanate ethyl dissolved in 10 mL of dehydrated THF was dropped over 10 minutes, and then stirred at room temperature for 12 hours. The solvent was distilled off from the resulting reaction solution, and the residue was purified by silica gel column chromatography using a mixed solvent of hexane / ethyl acetate (volume ratio 5 / 5 to 1 / 9) as an eluent, to obtain 14.38 g of comparative monomer RM-2.

[0169] [ka]

[0170] Example 1 <Synthesis of copolymer CP-1> 25.0 parts by mass of acrylic acid (AA, manufactured by Tokyo Chemical Industry Co., Ltd.), 75.0 parts by mass of monomer M-1, and 0.95 parts by mass of 2,2'-azoiso(butyronitrile) (AIBN, manufactured by Tokyo Chemical Industry Co., Ltd.) were dissolved in 252 parts by mass of dimethylformamide (DMF) (manufactured by Kanto Chemical Co., Ltd.). This solution was added dropwise to 28 parts by mass of DMF heated to 80°C under a nitrogen stream over 1 hour, and then stirred at 80°C for 5 hours. The reaction solution was cooled to room temperature and dropped into 500 mL of water. The precipitate was filtered and dried under reduced pressure to obtain 97.7 parts by mass of copolymer CP-1 (weight average molecular weight (Mw): 17,800).

[0171] Example 2 <Synthesis of copolymer CP-2> 98.1 parts by mass of copolymer CP-2 (Mw: 23,300) was obtained in the same manner as in Example 1, except that 20.0 parts by mass of acrylic acid, 80.0 parts by mass of monomer M-2, and 0.72 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0172] Example 3 <Synthesis of copolymer CP-3> 97.2 parts by mass of copolymer CP-3 (Mw: 29,200) was obtained in the same manner as in Example 1, except that 15.0 parts by mass of acrylic acid, 85.0 parts by mass of monomer M-3, and 0.54 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0173] Example 4 <Synthesis of copolymer CP-4> 97.9 parts by mass of copolymer CP-4 (Mw: 35,700) was obtained in the same manner as in Example 1, except that 10.0 parts by mass of acrylic acid, 90.0 parts by mass of monomer M-4, and 0.37 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0174] Example 5 <Synthesis of copolymer CP-5> 98.2 parts by mass of copolymer CP-5 (Mw: 47,100) was obtained in the same manner as in Example 1, except that 5.0 parts by mass of acrylic acid, 95.0 parts by mass of monomer M-5, and 0.24 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0175] Example 6 <Synthesis of copolymer CP-6> 20.0 parts by mass of acrylic acid, 80.0 parts by mass of monomer M-2, and 0.20 parts by mass of 2,2'-azoiso(butyronitrile) were dissolved in 216 parts by mass of DMF. This solution was added dropwise to 24 parts by mass of DMF heated to 80°C under a nitrogen stream over 1 hour, and then stirred at 80°C for 5 hours. The reaction solution was cooled to room temperature and dropped into 500 mL of water. The precipitate was filtered and dried under reduced pressure to obtain 97.1 parts by mass of copolymer CP-6 (Mw: 51,300).

[0176] Example 7 <Synthesis of copolymer CP-7> 20.0 parts by mass of acrylic acid, 80.0 parts by mass of monomer M-2, 1.61 parts by mass of 2,2'-azoiso(butyronitrile), and 0.26 parts by mass of 3-mercaptopropionic acid (3MPA, manufactured by Tokyo Chemical Industry Co., Ltd.) were dissolved in 252 parts by mass of DMF. This solution was added dropwise to 28 parts by mass of DMF heated to 80°C under a nitrogen stream over 1 hour, and then stirred at 80°C for 5 hours. The reaction solution was cooled to room temperature and dropped into 500 mL of water. The precipitate was filtered and dried under reduced pressure to obtain 97.0 parts by mass of copolymer CP-7 (Mw: 4,100).

[0177] Example 8 <Synthesis of copolymer CP-8> 20.0 parts by mass of 2-acrylamido-2'-methylpropanesulfonic acid (AAMS, manufactured by Tokyo Chemical Industry Co., Ltd.), 80.0 parts by mass of monomer M-2, and 0.25 parts by mass of 2,2'-azoiso(butyronitrile) were dissolved in 252 parts by mass of DMF. This solution was added dropwise to 28 parts by mass of DMF heated to 80°C under a nitrogen stream over 1 hour, and then stirred at 80°C for 5 hours. The reaction solution was cooled to room temperature and dropped into 500 mL of water. The precipitate was filtered and dried under reduced pressure to obtain 98.5 parts by mass of copolymer CP-8 (Mw: 41,600).

[0178] Example 9 <Synthesis of copolymer CP-9> 20.0 parts by mass of 2-acrylamido-2'-methylpropanesulfonic acid, 80.0 parts by mass of monomer M-2, and 0.13 parts by mass of 2,2'-azoiso(butyronitrile) were dissolved in 216 parts by mass of DMF. This solution was added dropwise to 24 parts by mass of DMF heated to 80°C under a nitrogen stream over 1 hour, and then stirred at 80°C for 5 hours. The reaction solution was cooled to room temperature and dropped into 500 mL of water. The precipitate was filtered and dried under reduced pressure to obtain 97.0 parts by mass of copolymer CP-9 (Mw: 52,200).

[0179] Example 10 <Synthesis of copolymer CP-10> 20.0 parts by mass of 2-acrylamido-2'-methylpropanesulfonic acid, 80.0 parts by mass of monomer M-2, 1.01 parts by mass of 2,2'-azoiso(butyronitrile), and 0.16 parts by mass of 3-mercaptopropionic acid were dissolved in 252 parts by mass of DMF. This solution was added dropwise to 28 parts by mass of DMF heated to 80°C under a nitrogen stream over 1 hour, and then stirred at 80°C for 5 hours. The reaction solution was cooled to room temperature and dropped into 500 mL of water. The precipitate was filtered and dried under reduced pressure to obtain 97.0 parts by mass of copolymer CP-10 (Mw: 4,300).

[0180] Example 11 <Synthesis of copolymer CP-11> 98.2 parts by mass of copolymer CP-11 (Mw: 18,100) was obtained in the same manner as in Example 1, except that 25.0 parts by mass of acrylic acid, 75.0 parts by mass of monomer M-6, and 0.88 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0181] Example 12 <Synthesis of copolymer CP-12> 98.4 parts by mass of copolymer CP-12 (Mw: 24,600) was obtained in the same manner as in Example 1, except that 20.0 parts by mass of acrylic acid, 80.0 parts by mass of monomer M-7, and 0.71 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0182] Example 13 <Synthesis of copolymer CP-13> 98.5 parts by mass of copolymer CP-13 (Mw: 30,100) was obtained in the same manner as in Example 1, except that 15.0 parts by mass of acrylic acid, 85.0 parts by mass of monomer M-8, and 0.67 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0183] Example 14 <Synthesis of copolymer CP-14> 98.0 parts by mass of copolymer CP-14 (Mw: 36,200) was obtained in the same manner as in Example 1, except that 10.0 parts by mass of acrylic acid, 90.0 parts by mass of monomer M-9, and 0.57 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0184] Example 15 <Synthesis of copolymer CP-15> 98.5 parts by mass of copolymer CP-15 (Mw: 46,900) was obtained in the same manner as in Example 1, except that 5.0 parts by mass of acrylic acid, 95.0 parts by mass of monomer M-10, and 0.35 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0185] (Example 16) <Synthesis of copolymer CP-16> 98.5 parts by mass of copolymer CP-16 (Mw: 53,400) was obtained in the same manner as in Example 6, except that 20.0 parts by mass of acrylic acid, 80.0 parts by mass of monomer M-8, and 0.28 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0186] (Example 17) <Synthesis of copolymer CP-17> 98.0 parts by mass of copolymer CP-17 (Mw: 4,100) was obtained in the same manner as in Example 7, except that 20.0 parts by mass of acrylic acid, 80.0 parts by mass of monomer M-8, 1.86 parts by mass of 2,2'-azoiso(butyronitrile), and 0.30 parts by mass of 3-mercaptopropionic acid were used.

[0187] (Example 18) <Synthesis of copolymer CP-18> 98.8 parts by mass of copolymer CP-18 (Mw: 42,600) was obtained in the same manner as in Example 8, except that 20.0 parts by mass of 2-acrylamido-2-methylpropanesulfonic acid, 80.0 parts by mass of monomer M-8, and 0.32 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0188] (Example 19) <Synthesis of copolymer CP-19> 98.0 parts by mass of copolymer CP-19 (Mw: 52,800) was obtained in the same manner as in Example 9, except that 20.0 parts by mass of 2-acrylamido-2-methylpropanesulfonic acid, 80.0 parts by mass of monomer M-8, and 0.16 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0189] (Example 20) <Synthesis of copolymer CP-20> 98.7 parts by mass of copolymer CP-20 (Mw: 4,500) was obtained in the same manner as in Example 10, except that 20.0 parts by mass of 2-acrylamido-2-methylpropanesulfonic acid, 80.0 parts by mass of monomer M-8, 1.26 parts by mass of 2,2'-azoiso(butyronitrile), and 0.20 parts by mass of 3-mercaptopropionic acid were used.

[0190] Example 21 <Synthesis of copolymer CP-21> 98.4 parts by mass of copolymer CP-21 (Mw: 19,700) was obtained in the same manner as in Example 1, except that 25.0 parts by mass of acrylic acid, 75.0 parts by mass of monomer M-11, and 0.90 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0191] Example 22 <Synthesis of copolymer CP-22> 98.8 parts by mass of copolymer CP-22 (Mw: 23,900) was obtained in the same manner as in Example 1, except that 20.0 parts by mass of acrylic acid, 80.0 parts by mass of monomer M-12, and 0.75 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0192] (Example 23) <Synthesis of copolymer CP-23> 98.1 parts by mass of copolymer CP-23 (Mw: 29,800) was obtained in the same manner as in Example 1, except that 15.0 parts by mass of acrylic acid, 85.0 parts by mass of monomer M-13, and 0.55 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0193] (Example 24) <Synthesis of copolymer CP-24> 98.6 parts by mass of copolymer CP-24 (Mw: 35,100) was obtained in the same manner as in Example 1, except that 10.0 parts by mass of acrylic acid, 90.0 parts by mass of monomer M-14, and 0.51 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0194] (Example 25) <Synthesis of copolymer CP-25> 98.0 parts by mass of copolymer CP-25 (Mw: 43,800) was obtained in the same manner as in Example 1, except that 5.0 parts by mass of acrylic acid, 95.0 parts by mass of monomer M-15, and 0.35 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0195] (Example 26) <Synthesis of copolymer CP-26> 97.7 parts by mass of copolymer CP-26 (Mw: 54,100) was obtained in the same manner as in Example 6, except that 20.0 parts by mass of acrylic acid, 80.0 parts by mass of monomer M-12, and 0.21 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0196] Example 27 <Synthesis of copolymer CP-27> 98.4 parts by mass of copolymer CP-27 (Mw: 4,600) was obtained in the same manner as in Example 7, except that 20.0 parts by mass of acrylic acid, 80.0 parts by mass of monomer M-12, 1.68 parts by mass of 2,2'-azoiso(butyronitrile), and 0.27 parts by mass of 3-mercaptopropionic acid were used.

[0197] (Example 28) <Synthesis of copolymer CP-28> 98.0 parts by mass of copolymer CP-28 (Mw: 40,900) was obtained in the same manner as in Example 8, except that 20.0 parts by mass of 2-acrylamido-2-methylpropanesulfonic acid, 80.0 parts by mass of monomer M-12, and 0.27 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0198] (Example 29) <Synthesis of copolymer CP-29> 98.6 parts by mass of copolymer CP-29 (Mw: 56,200) was obtained in the same manner as in Example 9, except that 20.0 parts by mass of 2-acrylamido-2-methylpropanesulfonic acid, 80.0 parts by mass of monomer M-12, and 0.13 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0199] (Example 30) <Synthesis of copolymer CP-30> 97.7 parts by mass of copolymer CP-30 (Mw: 4,700) was obtained in the same manner as in Example 10, except that 20.0 parts by mass of 2-acrylamido-2-methylpropanesulfonic acid, 80.0 parts by mass of monomer M-12, 1.68 parts by mass of 2,2'-azoiso(butyronitrile), and 0.17 parts by mass of 3-mercaptopropionic acid were used.

[0200] (Example 31) <Synthesis of copolymer CP-31> 25.0 parts by mass of methacrylic acid (MA, manufactured by Tokyo Chemical Industry Co., Ltd.), 75.0 parts by mass of monomer M-16, and 0.77 parts by mass of 2,2'-azoiso(butyronitrile) were dissolved in 252 parts by mass of DMF. This solution was added dropwise to 28 parts by mass of DMF heated to 80°C under a nitrogen stream over 1 hour, and then stirred at 80°C for 5 hours. The reaction solution was cooled to room temperature and dropped into 500 mL of water. The precipitate was filtered and dried under reduced pressure to obtain 98.2 parts by mass of copolymer CP-31 (Mw: 18,800).

[0201] Example 32 <Synthesis of copolymer CP-32> 98.1 parts by mass of copolymer CP-32 (Mw: 23,000) was obtained in the same manner as in Example 31, except that 20.0 parts by mass of methacrylic acid, 80.0 parts by mass of monomer M-17, and 0.64 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0202] (Example 33) <Synthesis of copolymer CP-33> 98.9 parts by mass of copolymer CP-33 (Mw: 30,100) was obtained in the same manner as in Example 31, except that 15.0 parts by mass of methacrylic acid, 85.0 parts by mass of monomer M-18, and 0.48 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0203] (Example 34) <Synthesis of copolymer CP-34> 98.2 parts by mass of copolymer CP-34 (Mw: 35,900) was obtained in the same manner as in Example 31, except that 10.0 parts by mass of methacrylic acid, 90.0 parts by mass of monomer M-19, and 0.44 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0204] Example 35 <Synthesis of copolymer CP-35> 98.9 parts by mass of copolymer CP-35 (Mw: 45,700) was obtained in the same manner as in Example 31, except that 5.0 parts by mass of methacrylic acid, 95.0 parts by mass of monomer M-20, and 0.30 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0205] (Example 36) <Synthesis of copolymer CP-36> 20.0 parts by mass of methacrylic acid, 70.0 parts by mass of monomer M-3, 10.0 parts by mass of styrene (St, manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.49 parts by mass of 2,2'-azoiso(butyronitrile) were dissolved in 252 parts by mass of DMF. This solution was added dropwise to 28 parts by mass of DMF heated to 80°C under a nitrogen stream over 1 hour, and then stirred at 80°C for 5 hours. The reaction solution was cooled to room temperature and dropped into 500 mL of water. The precipitate was filtered and dried under reduced pressure to obtain 98.3 parts by mass of copolymer CP-36 (Mw: 37,900).

[0206] (Example 37) <Synthesis of copolymer CP-37> 20.0 parts by mass of methacrylic acid, 70.0 parts by mass of monomer M-3, 10.0 parts by mass of dodecyl methacrylate (DdMA, manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.43 parts by mass of 2,2'-azoiso(butyronitrile) were dissolved in 252 parts by mass of DMF. This solution was added dropwise to 28 parts by mass of DMF heated to 80°C under a nitrogen stream over 1 hour, and then stirred at 80°C for 5 hours. The reaction solution was cooled to room temperature and dropped into 500 mL of water. The precipitate was filtered and dried under reduced pressure to obtain 98.6 parts by mass of copolymer CP-37 (Mw: 38,600).

[0207] (Example 38) <Synthesis of copolymer CP-38> 20.0 parts by mass of 2-acrylamido-2-methylpropanesulfonic acid, 70.0 parts by mass of monomer M-3, 10.0 parts by mass of styrene, and 0.35 parts by mass of 2,2'-azoiso(butyronitrile) were dissolved in 252 parts by mass of DMF. This solution was added dropwise to 28 parts by mass of DMF heated to 80°C under a nitrogen stream over 1 hour, and then stirred at 80°C for 5 hours. The reaction solution was cooled to room temperature and dropped into 500 mL of water. The precipitate was filtered and dried under reduced pressure to obtain 98.3 parts by mass of copolymer CP-38 (Mw: 39,900).

[0208] (Example 39) <Synthesis of copolymer CP-39> 20.0 parts by mass of 2-acrylamido-2-methylpropanesulfonic acid, 70.0 parts by mass of monomer M-3, 10.0 parts by mass of styrene, and 0.15 parts by mass of 2,2'-azoiso(butyronitrile) were dissolved in 216 parts by mass of DMF. This solution was added dropwise to 24 parts by mass of DMF heated to 80°C under a nitrogen stream over 1 hour, and then stirred at 80°C for 5 hours. The reaction solution was cooled to room temperature and dropped into 500 mL of water. The precipitate was filtered and dried under reduced pressure to obtain 98.8 parts by mass of copolymer CP-39 (Mw: 55,500).

[0209] (Example 40) <Synthesis of copolymer CP-40> 20.0 parts by mass of 2-acrylamido-2-methylpropanesulfonic acid, 70.0 parts by mass of monomer M-3, 10.0 parts by mass of styrene, 1.18 parts by mass of 2,2'-azoiso(butyronitrile), and 0.19 parts by mass of 3-mercaptopropionic acid were dissolved in 252 parts by mass of DMF. This solution was added dropwise to 28 parts by mass of DMF heated to 80°C under a nitrogen stream over 1 hour, and then stirred at 80°C for 5 hours. The reaction solution was cooled to room temperature and dropped into 500 mL of water. The precipitate was filtered and dried under reduced pressure to obtain 97.5 parts by mass of copolymer CP-40 (Mw: 4,000).

[0210] Comparative Example 1 <Synthesis of comparative copolymer RCP-1> In the same manner as in Example 1, except that 25.0 parts by mass of acrylic acid, 75.0 parts by mass of comparative monomer RM-1, and 0.52 parts by mass of 2,2'-azoiso(butyronitrile) were used, 98.5 parts by mass of comparative copolymer RCP-1 (Mw: 34,900) was obtained.

[0211] Comparative Example 2 <Synthesis of comparative copolymer RCP-2> In the same manner as in Example 1, except that 15.0 parts by mass of acrylic acid, 85.0 parts by mass of comparative monomer RM-1, and 0.40 parts by mass of 2,2'-azoiso(butyronitrile) were used, 98.0 parts by mass of comparative copolymer RCP-2 (Mw: 35,300) was obtained.

[0212] Comparative Example 3 <Synthesis of comparative copolymer RCP-3> 97.5 parts by mass of comparative copolymer RCP-3 (Mw: 36,200) was obtained in the same manner as in Example 1, except that 5.0 parts by mass of acrylic acid, 95.0 parts by mass of comparative monomer RM-1, and 0.29 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0213] Comparative Example 4 <Synthesis of comparative copolymer RCP-4> The same procedure as in Example 8 was repeated except that 20.0 parts by mass of 2-acrylamido-2-methylpropanesulfonic acid, 80.0 parts by mass of comparative monomer RM-1, and 0.28 parts by mass of 2,2'-azoiso(butyronitrile) were used to obtain 98.5 parts by mass of comparative copolymer RCP-4 (Mw: 36,300).

[0214] Comparative Example 5 <Synthesis of comparative copolymer RCP-5> The procedure of Example 9 was repeated except that 20.0 parts by mass of 2-acrylamido-2-methylpropanesulfonic acid, 80.0 parts by mass of comparative monomer RM-1, and 0.12 parts by mass of 2,2'-azoiso(butyronitrile) were used, to obtain 98.8 parts by mass of copolymer RCP-5 (Mw: 56,100).

[0215] Comparative Example 6 <Synthesis of comparative copolymer RCP-6> 98.0 parts by mass of comparative copolymer RCP-6 (Mw: 4,600) was obtained in the same manner as in Example 10, except that 20.0 parts by mass of 2-acrylamido-2-methylpropanesulfonic acid, 80.0 parts by mass of comparative monomer RM-1, 0.94 parts by mass of 2,2'-azoiso(butyronitrile), and 0.15 parts by mass of 3-mercaptopropionic acid were used.

[0216] Comparative Example 7 <Synthesis of comparative copolymer RCP-7> 98.3 parts by mass of comparative copolymer RCP-7 (Mw: 36,900) was obtained in the same manner as in Example 36, except that 25.0 parts by mass of methacrylic acid, 70.0 parts by mass of comparative monomer RM-2, 5.0 parts by mass of styrene, and 0.52 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0217] Comparative Example 8 <Synthesis of comparative copolymer RCP-8> 98.8 parts by mass of comparative copolymer RCP-8 (Mw: 37,100) was obtained in the same manner as in Example 37, except that 5.0 parts by mass of methacrylic acid, 70.0 parts by mass of comparative monomer RM-2, 5.0 parts by mass of dodecyl methacrylate, and 0.34 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0218] Comparative Example 9 <Synthesis of comparative copolymer RCP-9> 98.9 parts by mass of comparative copolymer RCP-9 (Mw: 35,900) was obtained in the same manner as in Example 38, except that 20.0 parts by mass of 2-acrylamide-2-methylpropanesulfonic acid, 70.0 parts by mass of comparative monomer RM-2, 10.0 parts by mass of styrene, and 0.37 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0219] Comparative Example 10 <Synthesis of comparative copolymer RCP-10> 98.1 parts by mass of comparative copolymer RCP-10 (Mw: 53,700) was obtained in the same manner as in Example 39, except that 20.0 parts by mass of 2-acrylamido-2-methylpropanesulfonic acid, 70.0 parts by mass of comparative monomer RM-2, 10.0 parts by mass of styrene, and 0.16 parts by mass of 2,2'-azoiso(butyronitrile) were used.

[0220] Comparative Example 11 <Synthesis of comparative copolymer RCP-11> 97.7 parts by mass of comparative copolymer RCP-11 (Mw: 3,900) was obtained in the same manner as in Example 40, except that 20.0 parts by mass of 2-acrylamido-2-methylpropanesulfonic acid, 70.0 parts by mass of comparative monomer RM-2, 10.0 parts by mass of styrene, 1.24 parts by mass of 2,2'-azoiso(butyronitrile), and 0.20 parts by mass of 3-mercaptopropionic acid were used.

[0221] The compositions, parts by mass, and weight average molecular weights (Mw) of copolymers CP-1 to CP-40 synthesized in Examples 1 to 40 and copolymers RCP-1 to RCP-11 synthesized in Comparative Examples 1 to 11 are summarized in Tables 3 and 4.

[0222] [Table 3]

[0223] [Table 4]

[0224] (Example 41) <Preparation of pigment dispersion PD-1> 40.0 parts by mass of ion-exchanged water and 5.0 parts by mass of ethylene glycol (manufactured by Tokyo Chemical Industry Co., Ltd.) were placed in a glass container, and after stirring, 1.16 parts by mass of (2-hydroxyethyl)dimethylamine (manufactured by Tokyo Chemical Industry Co., Ltd.) and 3.75 parts by mass of copolymer CP-1 prepared in Example 1 were added and dissolved. Next, 50.0 parts by mass of titanium oxide JR-405 (manufactured by Teika Co., Ltd.) were added little by little while stirring, and then stirred for 6 hours. 540.0 parts by mass of zirconia beads with a diameter of 2 mm were added, and the mixture was dispersed for 48 hours at a rotation speed of 90 rpm using a Big Rotor BR-2 (manufactured by AS ONE Co., Ltd.). The contents were filtered through a membrane filter with a pore size of 10 μm, and an adjusted amount of ion-exchanged water was added to obtain 100.0 parts by mass of pigment dispersion PD-1 (pigment solid content concentration: 50%).

[0225] <Preparation of Water-Based Ink-1> 20.0 parts by mass of pigment dispersion PD-1, 18.0 parts by mass of ethylene glycol, 4.0 parts by mass of 3-methoxy-N,N-dimethylpropionamide (manufactured by Tokyo Chemical Industry Co., Ltd.), 1.0 part by mass of Zonyl FS-300 (manufactured by Dupont, fluorosurfactant, solids content 40%), 0.3 parts by mass of triethanolamine (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.8 parts by mass of 1,2-benzothiazolin-3-one (manufactured by Tokyo Chemical Industry Co., Ltd.), and 56.0 parts by mass of ion-exchanged water were mixed and stirred for 1 hour, and then filtered through a membrane filter having a pore size of 5.0 μm to obtain ink Ink-1.

[0226] (Example 42) <Preparation of Water-Based Ink Ink-2> A pigment dispersion PD-2 and an ink Ink-2 were obtained in the same manner as in Example 41, except that the copolymer CP-2 prepared in Example 2 was used instead of the copolymer CP-1 used in Example 41, and 0.93 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of the 1.16 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 41.

[0227] (Example 43) <Preparation of Water-Based Ink-3> A pigment dispersion PD-3 and an ink Ink-3 were obtained in the same manner as in Example 41, except that the copolymer CP-3 prepared in Example 3 was used instead of the copolymer CP-1 used in Example 41, and 0.70 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of the 1.16 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 41.

[0228] (Example 44) <Preparation of Water-Based Ink-4> A pigment dispersion PD-4 and an ink Ink-4 were obtained in the same manner as in Example 41, except that the copolymer CP-4 prepared in Example 4 was used instead of the copolymer CP-1 used in Example 41, and 0.46 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of the 1.16 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 41.

[0229] (Example 45) <Preparation of Water-Based Ink-5> A pigment dispersion PD-5 and an ink Ink-5 were obtained in the same manner as in Example 41, except that the copolymer CP-5 prepared in Example 5 was used instead of the copolymer CP-1 used in Example 41, and 0.23 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of the 1.16 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 41.

[0230] (Example 46) <Preparation of Water-Based Ink-6> Pigment dispersion PD-6 and ink Ink-6 were obtained in the same manner as in Example 41, except that copolymer CP-6 prepared in Example 6 was used instead of copolymer CP-1 used in Example 41, and 0.93 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of 1.16 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 41.

[0231] (Example 47) <Preparation of Water-Based Ink-7> Pigment dispersion PD-7 and ink Ink-7 were obtained in the same manner as in Example 41, except that copolymer CP-7 prepared in Example 7 was used instead of copolymer CP-1 used in Example 41, and 0.93 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of 1.16 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 41.

[0232] (Example 48) <Preparation of Water-Based Ink-8> Pigment dispersion PD-8 and ink Ink-8 were obtained in the same manner as in Example 41, except that copolymer CP-8 prepared in Example 8 was used instead of copolymer CP-1 used in Example 41, and 0.32 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of 1.16 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 41.

[0233] (Example 49) <Preparation of Water-Based Ink-9> A pigment dispersion PD-9 and an ink Ink-9 were obtained in the same manner as in Example 41, except that the copolymer CP-9 prepared in Example 9 was used instead of the copolymer CP-1 used in Example 41, and 0.32 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of the 1.16 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 41.

[0234] (Example 50) <Preparation of Water-Based Ink Ink-10> A pigment dispersion PD-10 and an ink Ink-10 were obtained in the same manner as in Example 41, except that the copolymer CP-10 prepared in Example 10 was used instead of the copolymer CP-1 used in Example 41, and 0.32 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of the 1.16 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 41.

[0235] (Example 51) <Preparation of Water-Based Ink Ink-11> A pigment dispersion PD-11 and an ink Ink-11 were obtained in the same manner as in Example 41, except that 2.50 parts by mass of the copolymer CP-11 prepared in Example 11 were used instead of the 3.75 parts by mass of the copolymer CP-1 used in Example 41, and 0.77 parts by mass of (2-hydroxyethyl)dimethylamine were used instead of the 1.16 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 41.

[0236] (Example 52) <Preparation of Water-Based Ink Ink-12> A pigment dispersion PD-12 and an ink Ink-12 were obtained in the same manner as in Example 41, except that 2.50 parts by mass of the copolymer CP-12 prepared in Example 12 were used instead of the 3.75 parts by mass of the copolymer CP-1 used in Example 41, and 0.62 parts by mass of (2-hydroxyethyl)dimethylamine were used instead of the 1.16 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 41.

[0237] (Example 53) <Preparation of Water-Based Ink Ink-13> A pigment dispersion PD-13 and an ink Ink-13 were obtained in the same manner as in Example 41, except that 2.50 parts by mass of the copolymer CP-13 prepared in Example 13 were used instead of the 3.75 parts by mass of the copolymer CP-1 used in Example 41, and 0.46 parts by mass of (2-hydroxyethyl)dimethylamine were used instead of the 1.16 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 41.

[0238] (Example 54) <Preparation of Water-Based Ink Ink-14> A pigment dispersion PD-14 and an ink Ink-14 were obtained in the same manner as in Example 41, except that 2.50 parts by mass of the copolymer CP-14 prepared in Example 14 were used instead of the 3.75 parts by mass of the copolymer CP-1 used in Example 41, and 0.31 parts by mass of (2-hydroxyethyl)dimethylamine were used instead of the 1.16 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 41.

[0239] (Example 55) <Preparation of Water-Based Ink Ink-15> Pigment dispersion PD-15 and ink Ink-15 were obtained in the same manner as in Example 41, except that 2.50 parts by mass of copolymer CP-15 prepared in Example 15 were used instead of 3.75 parts by mass of copolymer CP-1 used in Example 41, and 0.15 parts by mass of (2-hydroxyethyl)dimethylamine were used instead of 1.16 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 41.

[0240] (Example 56) <Preparation of Water-Based Ink Ink-16> A pigment dispersion PD-16 and an ink Ink-16 were obtained in the same manner as in Example 41, except that 2.50 parts by mass of the copolymer CP-16 prepared in Example 16 were used instead of the 3.75 parts by mass of the copolymer CP-1 used in Example 41, and 0.62 parts by mass of (2-hydroxyethyl)dimethylamine were used instead of the 1.16 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 41.

[0241] (Example 57) <Preparation of Water-Based Ink-17> Pigment dispersion PD-17 and ink Ink-17 were obtained in the same manner as in Example 41, except that 2.50 parts by mass of copolymer CP-17 prepared in Example 17 were used instead of 3.75 parts by mass of copolymer CP-1 used in Example 41, and 0.62 parts by mass of (2-hydroxyethyl)dimethylamine were used instead of 1.16 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 41.

[0242] (Example 58) <Preparation of Water-Based Ink-18> Pigment dispersion PD-18 and ink Ink-18 were obtained in the same manner as in Example 41, except that 2.50 parts by mass of copolymer CP-18 prepared in Example 18 were used instead of 3.75 parts by mass of copolymer CP-1 used in Example 41, and 0.22 parts by mass of (2-hydroxyethyl)dimethylamine were used instead of 1.16 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 41.

[0243] (Example 59) <Preparation of Water-Based Ink-19> A pigment dispersion PD-19 and an ink Ink-19 were obtained in the same manner as in Example 41, except that 2.50 parts by mass of the copolymer CP-19 prepared in Example 19 were used instead of the 3.75 parts by mass of the copolymer CP-1 used in Example 41, and 0.22 parts by mass of (2-hydroxyethyl)dimethylamine were used instead of the 1.16 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 41.

[0244] (Example 60) <Preparation of Water-Based Ink Ink-20> A pigment dispersion PD-20 and an ink Ink-20 were obtained in the same manner as in Example 41, except that 2.50 parts by mass of the copolymer CP-20 prepared in Example 20 were used instead of 3.75 parts by mass of the copolymer CP-1 used in Example 41, and 0.22 parts by mass of (2-hydroxyethyl)dimethylamine were used instead of 1.16 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 41.

[0245] (Example 61) <Preparation of pigment dispersion PD-21> 40.0 parts by mass of ion-exchanged water and 5.0 parts by mass of ethylene glycol (manufactured by Tokyo Kasei Co., Ltd.) were placed in a glass container, and after stirring, 0.52 parts by mass of sodium hydroxide (manufactured by Kanto Chemical Co., Ltd.) and 3.75 parts by mass of copolymer CP-21 prepared in Example 21 were added and dissolved. Next, 50.0 parts by mass of titanium oxide JR-405 (manufactured by Teika Co., Ltd.) were added little by little while stirring, and then stirred for 6 hours. 540.0 parts by mass of zirconia beads with a diameter of 2 mm were added, and the mixture was dispersed for 48 hours at a rotation speed of 90 rpm using a Big Rotor BR-2 (manufactured by AS ONE Co., Ltd.). The contents were filtered through a membrane filter with a pore size of 10 μm, and an adjusted amount of ion-exchanged water was added to obtain 100.0 parts by mass of pigment dispersion PD-21 (pigment solid content concentration: 50%).

[0246] <Preparation of Water-Based Ink Ink-21> An ink Ink-21 was obtained in the same manner as in Example 41, except that the pigment dispersion PD-21 was used instead of the pigment dispersion PD-1 used in Example 41.

[0247] (Example 62) A pigment dispersion PD-22 and an ink Ink-22 were obtained in the same manner as in Example 61, except that the copolymer CP-22 prepared in Example 22 was used instead of the copolymer CP-21 used in Example 61, and 0.42 parts by mass of sodium hydroxide was used instead of the 0.52 parts by mass of sodium hydroxide used in Example 61.

[0248] (Example 63) A pigment dispersion PD-23 and an ink Ink-23 were obtained in the same manner as in Example 61, except that the copolymer CP-23 prepared in Example 23 was used instead of the copolymer CP-21 used in Example 61, and 0.31 parts by mass of sodium hydroxide was used instead of the 0.52 parts by mass of sodium hydroxide used in Example 61.

[0249] (Example 64) A pigment dispersion PD-24 and an ink Ink-24 were obtained in the same manner as in Example 61, except that the copolymer CP-24 prepared in Example 24 was used instead of the copolymer CP-21 used in Example 61, and 0.21 parts by mass of sodium hydroxide was used instead of the 0.52 parts by mass of sodium hydroxide used in Example 61.

[0250] (Example 65) A pigment dispersion PD-25 and an ink Ink-25 were obtained in the same manner as in Example 61, except that the copolymer CP-25 prepared in Example 25 was used instead of the copolymer CP-21 used in Example 61, and 0.10 parts by mass of sodium hydroxide was used instead of the 0.52 parts by mass of sodium hydroxide used in Example 61.

[0251] (Example 66) A pigment dispersion PD-26 and an ink Ink-26 were obtained in the same manner as in Example 61, except that the copolymer CP-26 prepared in Example 26 was used instead of the copolymer CP-21 used in Example 61, and 0.42 parts by mass of sodium hydroxide was used instead of the 0.52 parts by mass of sodium hydroxide used in Example 61.

[0252] (Example 67) Pigment dispersion PD-27 and ink Ink-27 were obtained in the same manner as in Example 61, except that the copolymer CP-27 prepared in Example 27 was used instead of the copolymer CP-21 used in Example 61, and 0.42 parts by mass of sodium hydroxide was used instead of the 0.52 parts by mass of sodium hydroxide used in Example 61.

[0253] (Example 68) Pigment dispersion PD-28 and ink Ink-28 were obtained in the same manner as in Example 61, except that the copolymer CP-28 prepared in Example 28 was used instead of the copolymer CP-21 used in Example 61, and 0.14 parts by mass of sodium hydroxide was used instead of the 0.52 parts by mass of sodium hydroxide used in Example 61.

[0254] (Example 69) A pigment dispersion PD-29 and an ink Ink-29 were obtained in the same manner as in Example 61, except that the copolymer CP-29 prepared in Example 29 was used instead of the copolymer CP-21 used in Example 61, and 0.14 parts by mass of sodium hydroxide was used instead of the 0.52 parts by mass of sodium hydroxide used in Example 61.

[0255] (Example 70) A pigment dispersion PD-30 and an ink Ink-30 were obtained in the same manner as in Example 61, except that the copolymer CP-30 prepared in Example 30 was used instead of the copolymer CP-21 used in Example 61, and 0.14 parts by mass of sodium hydroxide was used instead of the 0.52 parts by mass of sodium hydroxide used in Example 61.

[0256] (Example 71) Pigment dispersion PD-31 and ink Ink-31 were obtained in the same manner as in Example 61, except that 2.50 parts by mass of copolymer CP-31 prepared in Example 31 was used instead of 3.75 parts by mass of copolymer CP-21 used in Example 61, and 0.29 parts by mass of sodium hydroxide was used instead of 0.52 parts by mass of sodium hydroxide used in Example 61.

[0257] (Example 72) A pigment dispersion PD-32 and an ink Ink-32 were obtained in the same manner as in Example 61, except that 2.50 parts by mass of the copolymer CP-32 prepared in Example 32 were used instead of 3.75 parts by mass of the copolymer CP-21 used in Example 61, and 0.23 parts by mass of sodium hydroxide were used instead of 0.52 parts by mass of the sodium hydroxide used in Example 61.

[0258] (Example 73) Pigment dispersion PD-33 and ink Ink-33 were obtained in the same manner as in Example 61, except that 2.50 parts by mass of copolymer CP-33 prepared in Example 33 were used instead of 3.75 parts by mass of copolymer CP-21 used in Example 61, and 0.17 parts by mass of sodium hydroxide were used instead of 0.52 parts by mass of sodium hydroxide used in Example 61.

[0259] (Example 74) Pigment dispersion PD-34 and ink Ink-34 were obtained in the same manner as in Example 61, except that 2.50 parts by mass of copolymer CP-34 prepared in Example 34 were used instead of 3.75 parts by mass of copolymer CP-21 used in Example 61, and 0.12 parts by mass of sodium hydroxide were used instead of 0.52 parts by mass of sodium hydroxide used in Example 61.

[0260] (Example 75) Pigment dispersion PD-35 and ink Ink-35 were obtained in the same manner as in Example 61, except that 2.50 parts by mass of copolymer CP-35 prepared in Example 35 were used instead of 3.75 parts by mass of copolymer CP-21 used in Example 61, and 0.06 parts by mass of sodium hydroxide were used instead of 0.52 parts by mass of sodium hydroxide used in Example 61.

[0261] (Example 76) Pigment dispersion PD-36 and ink Ink-36 were obtained in the same manner as in Example 61, except that 2.50 parts by mass of copolymer CP-36 prepared in Example 36 were used instead of 3.75 parts by mass of copolymer CP-21 used in Example 61, and 0.23 parts by mass of sodium hydroxide were used instead of 0.52 parts by mass of sodium hydroxide used in Example 61.

[0262] (Example 77) Pigment dispersion PD-37 and ink Ink-37 were obtained in the same manner as in Example 61, except that 2.50 parts by mass of copolymer CP-37 prepared in Example 37 were used instead of 3.75 parts by mass of copolymer CP-21 used in Example 61, and 0.23 parts by mass of sodium hydroxide were used instead of 0.52 parts by mass of sodium hydroxide used in Example 61.

[0263] (Example 78) Pigment dispersion PD-38 and ink Ink-38 were obtained in the same manner as in Example 61, except that 2.50 parts by mass of copolymer CP-38 prepared in Example 38 were used instead of 3.75 parts by mass of copolymer CP-21 used in Example 61, and 0.10 parts by mass of sodium hydroxide were used instead of 0.52 parts by mass of sodium hydroxide used in Example 61.

[0264] (Example 79) Pigment dispersion PD-39 and ink Ink-39 were obtained in the same manner as in Example 61, except that 2.50 parts by mass of copolymer CP-39 prepared in Example 39 was used instead of 3.75 parts by mass of copolymer CP-21 used in Example 61, and 0.10 parts by mass of sodium hydroxide was used instead of 0.52 parts by mass of sodium hydroxide used in Example 61.

[0265] (Example 80) A pigment dispersion PD-40 and an ink Ink-40 were obtained in the same manner as in Example 61, except that 2.50 parts by mass of the copolymer CP-40 prepared in Example 40 were used instead of 3.75 parts by mass of the copolymer CP-21 used in Example 61, and 0.10 parts by mass of sodium hydroxide were used instead of 0.52 parts by mass of the sodium hydroxide used in Example 61.

[0266] (Example 81) <Preparation of pigment dispersion PD-41> 40.0 parts by mass of ion-exchanged water and 5.0 parts by mass of ethylene glycol were placed in a glass container, and after stirring, 0.77 parts by mass of (2-hydroxyethyl)dimethylamine and 2.50 parts by mass of the copolymer CP-1 prepared in Example 1 were added and dissolved. Next, 50.0 parts by mass of barium sulfate TS-2 (manufactured by Takehara Chemical Industry Co., Ltd.) were added little by little while stirring, and then stirred for 6 hours. 540.0 parts by mass of zirconia beads with a diameter of 2 mm were added, and the mixture was dispersed for 48 hours at a rotation speed of 90 rpm using a Big Rotor BR-2 (manufactured by AS ONE Corporation). The contents were filtered through a membrane filter with a pore size of 10 μm, and an adjusted amount of ion-exchanged water was added to obtain 100.0 parts by mass of pigment dispersion PD-41 (pigment solid content concentration: 50%).

[0267] <Preparation of Water-Based Ink Ink-41> An ink Ink-41 was obtained in the same manner as in Example 41, except that the pigment dispersion PD-41 was used instead of the pigment dispersion PD-1 used in Example 41.

[0268] (Example 82) A pigment dispersion PD-42 and an ink Ink-42 were obtained in the same manner as in Example 81, except that the copolymer CP-2 prepared in Example 2 was used instead of the copolymer CP-1 used in Example 81, and 0.62 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of 0.77 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 81.

[0269] (Example 83) A pigment dispersion PD-43 and an ink Ink-43 were obtained in the same manner as in Example 81, except that the copolymer CP-3 prepared in Example 3 was used instead of the copolymer CP-1 used in Example 81, and 0.46 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of 0.77 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 81.

[0270] (Example 84) A pigment dispersion PD-44 and an ink Ink-44 were obtained in the same manner as in Example 81, except that the copolymer CP-4 prepared in Example 4 was used instead of the copolymer CP-1 used in Example 81, and 0.31 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of 0.77 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 81.

[0271] (Example 85) Pigment dispersion PD-45 and ink Ink-45 were obtained in the same manner as in Example 81, except that copolymer CP-5 prepared in Example 5 was used instead of copolymer CP-1 used in Example 81, and 0.15 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of 0.77 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 81.

[0272] (Example 86) Pigment dispersion PD-46 and ink Ink-46 were obtained in the same manner as in Example 81, except that copolymer CP-6 prepared in Example 6 was used instead of copolymer CP-1 used in Example 81, and 0.62 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of 0.77 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 81.

[0273] (Example 87) Pigment dispersion PD-47 and ink Ink-47 were obtained in the same manner as in Example 81, except that copolymer CP-7 prepared in Example 7 was used instead of copolymer CP-1 used in Example 81, and 0.62 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of 0.77 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 81.

[0274] (Example 88) Pigment dispersion PD-48 and ink Ink-48 were obtained in the same manner as in Example 81, except that copolymer CP-8 prepared in Example 8 was used instead of copolymer CP-1 used in Example 81, and 0.77 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of 0.77 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 81.

[0275] (Example 89) Pigment dispersion PD-49 and ink Ink-49 were obtained in the same manner as in Example 81, except that copolymer CP-9 prepared in Example 9 was used instead of copolymer CP-1 used in Example 81, and 0.22 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of 0.77 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 81.

[0276] (Example 90) A pigment dispersion PD-50 and an ink Ink-50 were obtained in the same manner as in Example 81, except that the copolymer CP-10 prepared in Example 10 was used instead of the copolymer CP-1 used in Example 81, and 0.22 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of 0.77 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 81.

[0277] Comparative Example 12 <Preparation of Comparative Water-Based Ink Rink-1> A comparative pigment dispersion RPD-1 and a comparative ink Rink-1 were obtained in the same manner as in Example 41, except that the comparative copolymer RCP-1 prepared in Comparative Example 1 was used instead of the copolymer CP-1 used in Example 41, and 1.16 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of the 1.16 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 41.

[0278] Comparative Example 13 <Preparation of Comparative Water-Based Ink Rink-2> A comparative pigment dispersion RPD-2 and a comparative ink Rink-2 were obtained in the same manner as in Example 41, except that the comparative copolymer RCP-2 prepared in Comparative Example 2 was used instead of the copolymer CP-1 used in Example 41, and 0.70 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of the 1.16 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 41.

[0279] (Comparative Example 14) <Preparation of Comparative Water-Based Ink Rink-3> A comparative pigment dispersion RPD-3 and a comparative ink Rink-3 were obtained in the same manner as in Example 41, except that the comparative copolymer RCP-3 prepared in Comparative Example 3 was used instead of the copolymer CP-1 used in Example 41, and 0.23 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of the 1.16 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 41.

[0280] Comparative Example 15 <Preparation of Comparative Water-Based Ink Rink-4> A comparative pigment dispersion RPD-4 and a comparative ink Rink-4 were obtained in the same manner as in Example 41, except that the comparative copolymer RCP-4 prepared in Comparative Example 4 was used instead of the copolymer CP-1 used in Example 41, and 0.32 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of the 1.16 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 41.

[0281] Comparative Example 16 <Preparation of Comparative Water-Based Ink Rink-5> Comparative pigment dispersion RPD-5 and comparative ink Rink-5 were obtained in the same manner as in Example 41, except that the comparative copolymer RCP-5 prepared in Comparative Example 5 was used instead of the copolymer CP-1 used in Example 41, and 0.32 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of the 1.16 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 41.

[0282] Comparative Example 17 <Preparation of Comparative Water-Based Ink Rink-6> A comparative pigment dispersion RPD-6 and a comparative ink Rink-6 were obtained in the same manner as in Example 41, except that the comparative copolymer RCP-6 prepared in Comparative Example 6 was used instead of the copolymer CP-1 used in Example 41, and 0.32 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of the 1.16 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 41.

[0283] (Comparative Example 18) <Preparation of Comparative Water-Based Ink Rink-7> A comparative pigment dispersion RPD-7 and a comparative ink Rink-7 were obtained in the same manner as in Example 61, except that 2.50 parts by mass of the comparative copolymer RCP-7 prepared in Comparative Example 7 were used instead of 3.75 parts by mass of the copolymer CP-21 used in Example 61, and 0.29 parts by mass of sodium hydroxide were used instead of 0.52 parts by mass of the sodium hydroxide used in Example 61.

[0284] Comparative Example 19 <Preparation of Comparative Water-Based Ink Rink-8> Comparative pigment dispersion RPD-8 and comparative ink Rink-8 were obtained in the same manner as in Example 61, except that 2.50 parts by mass of comparative copolymer RCP-8 prepared in Comparative Example 8 were used instead of 3.75 parts by mass of copolymer CP-21 used in Example 61, and 0.06 parts by mass of sodium hydroxide were used instead of 0.52 parts by mass of sodium hydroxide used in Example 61.

[0285] Comparative Example 20 <Preparation of Comparative Water-Based Ink Rink-9> A comparative pigment dispersion RPD-9 and a comparative ink Rink-9 were obtained in the same manner as in Example 61, except that 2.50 parts by mass of the comparative copolymer RCP-9 prepared in Comparative Example 9 was used instead of 3.75 parts by mass of the copolymer CP-21 used in Example 61, and 0.10 parts by mass of sodium hydroxide was used instead of 0.52 parts by mass of the sodium hydroxide used in Example 61.

[0286] Comparative Example 21 <Preparation of Comparative Water-Based Ink Rink-10> A comparative pigment dispersion RPD-10 and a comparative ink Rink-10 were obtained in the same manner as in Example 61, except that 2.50 parts by mass of the comparative copolymer RCP-10 prepared in Comparative Example 10 was used instead of 3.75 parts by mass of the copolymer CP-21 used in Example 61, and 0.10 parts by mass of sodium hydroxide was used instead of 0.52 parts by mass of the sodium hydroxide used in Example 61.

[0287] Comparative Example 22 <Preparation of Comparative Water-Based Ink Rink-11> A comparative pigment dispersion RPD-11 and a comparative ink Rink-11 were obtained in the same manner as in Example 61, except that 2.50 parts by mass of the comparative copolymer RCP-11 prepared in Comparative Example 11 was used instead of 3.75 parts by mass of the copolymer CP-21 used in Example 61, and 0.10 parts by mass of sodium hydroxide was used instead of 0.52 parts by mass of the sodium hydroxide used in Example 61.

[0288] (Comparative Example 23) <Preparation of Comparative Water-Based Ink Rink-12> A pigment dispersion RPD-12 and a comparative ink Rink-12 were obtained in the same manner as in Example 81, except that the comparative copolymer RCP-1 prepared in Comparative Example 1 was used instead of the copolymer CP-1 used in Example 81, and 0.62 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of 0.77 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 81.

[0289] Comparative Example 24 <Preparation of Comparative Water-Based Ink Rink-13> A pigment dispersion RPD-13 and a comparative ink Rink-13 were obtained in the same manner as in Example 81, except that the comparative copolymer RCP-2 prepared in Comparative Example 2 was used instead of the copolymer CP-1 used in Example 81, and 0.62 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of 0.77 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 81.

[0290] Comparative Example 25 <Preparation of Comparative Water-Based Ink Rink-14> A pigment dispersion RPD-14 and a comparative ink Rink-14 were obtained in the same manner as in Example 81, except that the comparative copolymer RCP-3 prepared in Comparative Example 3 was used instead of the copolymer CP-1 used in Example 81, and 0.62 parts by mass of (2-hydroxyethyl)dimethylamine was used instead of 0.77 parts by mass of (2-hydroxyethyl)dimethylamine used in Example 81.

[0291] (Evaluation of storage stability of pigment dispersion) Each pigment dispersion was filled into a glass container and stored at 70°C for 2 weeks, and the rate of change in viscosity after storage relative to the viscosity before storage was calculated using the following formula and evaluated according to the following criteria. A viscometer (RE80L, manufactured by Toki Sangyo Co., Ltd.) was used to measure the viscosity at 25°C at 50 revolutions. Viscosity change rate (%) = 100 x (viscosity of pigment dispersion after storage - viscosity of pigment dispersion before storage) / viscosity of pigment dispersion before storage [Evaluation Criteria] A: Viscosity change rate is within ±5% B: Viscosity change rate exceeds ±5% and is within ±8% C: Viscosity change rate exceeds ±8% and is within ±10% D: Viscosity change rate exceeds ±10% and is within ±30%

[0292] (Evaluation of ink storage stability) Each ink was filled into an ink cartridge and stored at 70°C for one week, and the rate of change in viscosity after storage relative to the viscosity before storage was calculated using the following formula and evaluated according to the following criteria. A viscometer (RE80L, manufactured by Toki Sangyo Co., Ltd.) was used to measure the viscosity at 25°C at 50 revolutions. Viscosity change rate (%) = 100 x (viscosity of ink after storage - viscosity of ink before storage) / viscosity of ink before storage [Evaluation Criteria] A: Viscosity change rate is within ±5% B: Viscosity change rate exceeds ±5% and is within ±8% C: Viscosity change rate exceeds ±8% and is within ±10% D: Viscosity change rate exceeds ±10% and is within ±30%

[0293] (Evaluation of ink redispersibility) Sedimentation of the ink components by leaving the ink still requires leaving the ink for a long time, so a centrifuge was used to accelerate the sedimentation of the ink components. First, the ink was poured into a test tube PYREX (registered trademark) IWAKI TE-32 (16.5 mm x 105 mm, manufactured by AGC) to a depth of 45 mm, and the tube was covered with a silicone stopper to prepare an evaluation sample. Next, in order to define the initial state of the evaluation sample, immediately after the evaluation sample was prepared, the tip of a 2-3 mm pipette was immersed in the ink liquid surface to collect about 0.02 mL (about 20 mg) of ink. Of the collected ink, 4-10 mg was placed in a 50 mL sample bottle and diluted 4000 times with ion-exchanged water. The sample bottle was placed on the stand of a mix rotor VMR-5R (manufactured by AS ONE) and rotated at a rotation speed of 60 rpm for 10 minutes or more, and then immediately the absorption spectrum of UV-VIS (Ultraviolet-Visible Absorption Spectroscopy) was measured using an ultraviolet-visible-near infrared spectrophotometer V-680 (manufactured by JASCO Corporation) to prepare a reference spectrum before accelerated sedimentation. The measurement conditions are as follows. -UV-VIS measurement conditions- Wavelength range: 350~800nm Cell length: 3mm Measurement conditions: UV / VIS band width 2.0 nm, NIR band width 4.0 nm, response FAST, scanning speed 400 nm / min Next, the evaluation sample was placed in an inverter hematocrit centrifuge 3220 (KUBOTA) and accelerated sedimentation was performed at 300 rpm for 14 hours. The evaluation sample was gently turned sideways and gently placed on a mix rotor VMR-5R and rotated at 60 rpm for 1, 2, 3, or 4 minutes, after which the evaluation sample was immediately returned to its original vertical orientation, and a sample was taken from the ink surface in the same manner as above, and the absorption spectrum was measured, and the redispersion spectrum was obtained after 1, 2, 3, or 4 minutes. The redispersibility of the ink was evaluated according to the following criteria by calculating the rate of change of the redispersion spectrum relative to the reference spectrum from the following formula. Redispersibility (%) = 100 x (absorbance at peak wavelength of redispersion spectrum / absorbance at peak wavelength of reference spectrum) [Evaluation Criteria] A: Redispersion spectrum after 1 minute shows redispersion rate of 90% or more B: Redispersion spectrum after 2 minutes shows redispersion rate of 90% or more C: Redispersion spectrum after 3 minutes shows redispersion rate of 90% or more D: Redispersion spectrum after 4 minutes shows redispersion rate of 90% or more E: Redispersion spectrum after 4 minutes shows redispersion rate of 89% or less

[0294] The results of storage stability and redispersibility of pigment dispersions PD-1 to PD-50 and inks Ink-1 to Ink-50 of Examples 41 to 90, and comparative pigment dispersions RPD-1 to RPD-14 and comparative inks RInk-1 to RInk-14 of Comparative Examples 12 to 25 are summarized in Tables 5 and 6.

[0295] [Table 5]

[0296] [Table 6]

[0297] (Example 91) <Preparation of solar cell backsheet BS-1> -Preparation of protective layer forming solution PC-1- 45 parts of dimethylformamide (Kanto Chemical Co., Ltd.) and 36 parts of the copolymer CP-5 obtained in Example 5 were added to a glass container and dissolved by stirring. Next, 10 parts of titanium oxide JR-405 were added little by little while stirring, and then stirred for 6 hours. 540.0 parts of 1 mm diameter zirconia beads were added, and the mixture was dispersed for 2 days at a rotation speed of 90 rpm using a Big Rotor BR-2 (As One Corporation). The contents were filtered through a membrane filter with a pore size of 10 μm, and an adjusted amount of dimethylformamide (Kanto Chemical Co., Ltd.) and 4.0 parts of hexamethylene diisocyanate (Tokyo Chemical Industry Co., Ltd.) were added to obtain 100.0 parts of protective layer forming solution PC-1 (pigment solid content concentration: 10%).

[0298] -Preparation of solar cell backsheet BS-1- The protective layer forming liquid PC1 was applied to the surface of a 75 μm thick white polyethylene terephthalate film (Lumirror MX11, manufactured by Toray Industries, Inc.) using a wire bar, and dried at 150°C for 5 minutes to provide a protective layer with an average film thickness of 2 μm. The film was then aged at 50°C for 3 days to obtain a solar cell backsheet BS-1.

[0299] (Example 92) <Preparation of solar cell backsheet BS-2> A protective layer forming liquid PC-2 and a solar cell back sheet BS-2 were obtained in the same manner as in Example 91, except that the copolymer CP-15 prepared in Example 15 was used instead of the copolymer CP-5 used in Example 91.

[0300] (Example 93) <Preparation of solar cell backsheet BS-3> A protective layer forming liquid PC-3 and a solar cell back sheet BS-3 were obtained in the same manner as in Example 91, except that the copolymer CP-25 prepared in Example 25 was used instead of the copolymer CP-5 used in Example 91.

[0301] (Example 94) <Preparation of solar cell backsheet BS-4> A protective layer forming liquid PC-4 and a solar cell back sheet BS-4 were obtained in the same manner as in Example 91, except that the copolymer CP-35 prepared in Example 35 was used instead of the copolymer CP-5 used in Example 91.

[0302] Comparative Example 26 <Preparation of comparative solar cell backsheet RBS-1> A comparative protective layer forming liquid RPC-1 and a comparative solar cell back sheet RBS-1 were obtained in the same manner as in Example 91, except that the comparative copolymer RCP-3 prepared in Comparative Example 3 was used instead of the copolymer CP-5 used in Example 91.

[0303] (Comparative Example 27) <Preparation of comparative solar cell backsheet RBS-2> A comparative protective layer forming liquid RPC-2 and a comparative solar cell back sheet RBS-2 were obtained in the same manner as in Example 91, except that the copolymer RCP-8 prepared in Comparative Example 8 was used instead of the copolymer CP-5 used in Example 91.

[0304] (Weather resistance evaluation) -Measurement of initial breaking elongation Es- Each of the produced solar cell backsheets was cut into a size of 1 cm x 10 cm, and the breaking elongation of the solar cell backsheet was measured based on ASTM-D882 (ANNUAL BOOK OF ASTM STANDARDS 1999 edition), and the result was taken as the initial breaking elongation Es.

[0305] -Measurement of breaking elongation Ee after aging- Using a Super Xenon Weather Meter SX75 (manufactured by Suga Test Instruments), the black panel temperature was 65°C, the relative humidity was 50%, and the illuminance was 180W / m 2 Under the condition of UV irradiation (wavelength range: 300-400 nm), a solar cell backsheet test piece of 10 cm x 20 cm was repeatedly irradiated with UV rays for 108 minutes and then irradiated with UV rays while spraying water for 12 minutes (without humidity control) for a total of 3000 hours. The test piece was then cut into a size of 1 cm x 10 cm, and the breaking elongation was measured by the above method, and the result was defined as the breaking elongation after aging Ee.

[0306] -Weather resistance evaluation- As an index of weather resistance, the breaking elongation retention rate (%)=(Ee / Es)×100 was calculated, and the weather resistance was evaluated as follows based on the following evaluation criteria. [Evaluation Criteria] A: Breaking elongation retention is 50% or more B: Breaking elongation retention rate is 30% or more and less than 50% C: Breaking elongation retention is less than 30%

[0307] Table 7 shows the results of weather resistance of the solar cell backsheets BS-1 to BS-4 of Examples 91 to 94 and the comparative solar cell backsheets RBS1 to RBS2 of Comparative Examples 26 to 27.

[0308] [Table 7]

[0309] For example, aspects of the present invention are as follows. <1> The polymer is characterized by having a structural unit represented by the following general formula (1). [ka] (In general formula (1), R1 is hydrogen or a methyl group, L1 is "-COO-", "-CONH-" or a bond, X is a hydrocarbon group having 2 to 10 carbon atoms or a hydrocarbon group containing oxygen and having 2 to 10 carbon atoms, L2 is "-O-" or "-NH-", Y is a hydrocarbon group having 2 to 12 carbon atoms or a bond, L3 is "-OCO-", "-O-", "-(CH2)n-" or "-OCO-(CH2)n-", and n is an integer of 1 to 3.) <2> The copolymer is characterized by having a structural unit represented by the following general formula (1) and a structural unit represented by the following general formula (2). [ka] (In general formula (1), R1 is hydrogen or a methyl group, L1 is "-COO-", "-CONH-" or a bond, X is a hydrocarbon group having 2 to 10 carbon atoms or a hydrocarbon group containing oxygen and having 2 to 10 carbon atoms, L2 is "-O-" or "-NH-", Y is a hydrocarbon group having 2 to 12 carbon atoms or a bond, L3 is "-OCO-", "-O-", "-(CH2)n-" or "-OCO-(CH2)n-", and n is an integer of 1 to 3.) [ka] (In the general formula (2), R2 is a hydrogen atom or a methyl group, X + is a proton, an organic cation, or an inorganic cation.) <3> Water, Color material and A polymer having a structural unit represented by the following general formula (1), or a copolymer having a structural unit represented by the above general formula (1) and a structural unit represented by the following general formula (2), The ink is characterized by comprising: [ka] (In general formula (1), R1 is hydrogen or a methyl group, L1 is "-COO-", "-CONH-" or a bond, X is a hydrocarbon group having 2 to 10 carbon atoms or a hydrocarbon group containing oxygen and having 2 to 10 carbon atoms, L2 is "-O-" or "-NH-", Y is a hydrocarbon group having 2 to 12 carbon atoms or a bond, L3 is "-OCO-", "-O-", "-(CH2)n-" or "-OCO-(CH2)n-", and n is an integer of 1 to 3.) [ka] (In the general formula (2), R2 is a hydrogen atom or a methyl group, X + is a proton, an organic cation, or an inorganic cation.) <4> The weight average molecular weight of the polymer or copolymer is 5,000 or more and 50,000 or less. <3> The ink is as described in <5> The coloring material is titanium oxide. <3> From the above <4> The ink according to any one of claims 1 to 5, <6> The above <3> From the above <5> 1 is an ink container that contains the ink according to any one of the above items. <7> The above <3> From the above <5> and discharging the ink according to any one of claims 1 to 5 onto a recording medium to form an image. <8> The above <6> an ink container according to a discharge means for discharging the ink contained in the ink container onto a recording medium; The image forming apparatus is characterized by comprising: <9> A solar cell backsheet having a protective layer, The protective layer is <3> From the above <5> 2. A solar cell back sheet comprising a coating film made of the ink according to any one of claims 1 to 11.

[0310] The above <1> From the above <5> The ink according to any one of the preceding claims. <6> The ink container according to the <7> The image forming method according to the <8> and the image forming apparatus according to the above. <9> According to the solar cell backsheet described above, the conventional problems can be solved and the object of the present invention can be achieved. [Explanation of symbols]

[0311] 400 Image forming device 401 Exterior of image forming device 401c Device body cover 404 Cartridge Holder 410 Main Tank 410k, 410c, 410m, 410y, 410w Main tanks for each color: Black (K), Cyan (C), Magenta (M), Yellow (Y), and White (W) 411 Ink storage unit 413 Ink outlet 414 Storage container case 420 Mechanism Department 434 Discharge Head 436 Supply Tube [Prior art documents] [Patent documents]

[0312] [Patent Document 1] Patent No. 5863600

Claims

1. A polymer having a structural unit represented by the following general formula (1): 【Chemistry 1】 (In general formula (1), R 1 is a hydrogen atom or a methyl group, L 1 is "-COO-", "-CONH-" or a bond, X is a hydrocarbon group having 2 to 10 carbon atoms or a hydrocarbon group containing oxygen having 2 to 10 carbon atoms, L 2 is "-O-" or "-NH-", Y is a hydrocarbon group or bond having 2 to 12 carbon atoms, L 3 is "-OCO-", "-O-", "-(CH 2 )n-" or "-OCO-(CH 2 ) n-", where n is an integer from 1 to 3.

2. A copolymer having a structural unit represented by the following general formula (1) and a structural unit represented by the following general formula (2): 【Chemistry 2】 (In general formula (1), R 1 is a hydrogen atom or a methyl group, L 1 is "-COO-", "-CONH-" or a bond, X is a hydrocarbon group having 2 to 10 carbon atoms or a hydrocarbon group containing oxygen having 2 to 10 carbon atoms, L 2 is "-O-" or "-NH-", Y is a hydrocarbon group or bond having 2 to 12 carbon atoms, L 3 is "-OCO-", "-O-", "-(CH 2 )n-" or "-OCO-(CH 2 ) n-", where n is an integer from 1 to 3. 【Chemistry 3】 (In general formula (2), R 2 is hydrogen or a methyl group, X + is a proton, an organic cation, or an inorganic cation.)

3. Water, Color material and A polymer having a structural unit represented by the following general formula (1), or a copolymer having a structural unit represented by the above general formula (1) and a structural unit represented by the following general formula (2), An ink comprising: 【Chemistry 4】 (In general formula (1), R 1 is a hydrogen atom or a methyl group, L 1 is "-COO-", "-CONH-" or a bond, X is a hydrocarbon group having 2 to 10 carbon atoms or a hydrocarbon group containing oxygen having 2 to 10 carbon atoms, L 2 is "-O-" or "-NH-", Y is a hydrocarbon group or bond having 2 to 12 carbon atoms, L 3 is "-OCO-", "-O-", "-(CH 2 )n-" or "-OCO-(CH 2 ) n-", where n is an integer from 1 to 3. 【Chemistry 5】 (In general formula (2), R 2 is hydrogen or a methyl group, X + is a proton, an organic cation, or an inorganic cation.)

4. The ink according to claim 3 , wherein the weight average molecular weight of the polymer or copolymer is 5,000 or more and 50,000 or less.

5. The ink according to claim 3 , wherein the colorant is titanium oxide.

6. An ink container comprising the ink according to any one of claims 3 to 5.

7. 6. An image forming method comprising discharging the ink according to claim 3 onto a recording medium to form an image.

8. The ink container according to claim 6 , a discharge means for discharging the ink contained in the ink container onto a recording medium; An image forming apparatus comprising:

9. A solar cell backsheet having a protective layer, A solar cell backsheet, wherein the protective layer is a coating film made of the ink according to any one of claims 3 to 5.