Gas barrier laminate
The gas barrier laminate with a roughened polyethylene base layer and integrated barrier layers addresses the deformation issues of polyethylene films, ensuring smooth processing and effective gas barrier performance.
Patent Information
- Application Number
- JP2024118549
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-08-19
AI Technical Summary
Conventional polyethylene films used in packaging laminates face issues with low melting point and easy deformation, leading to poor processability and wrinkle formation during roll conveyance, which hinders proper post-processing.
A gas barrier laminate with a polyethylene base layer having an arithmetic mean roughness of 3 μm or more on the surface opposite to the barrier layer, combined with a barrier layer that includes a gas barrier coating and an inorganic vapor deposited layer, enhances film transportability and reduces wrinkle formation.
The laminate achieves good processability and resistance to wrinkles, enabling efficient roll processing and maintaining high gas barrier properties.
Smart Images

Figure 2024144563000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a gas barrier laminate. [Background technology]
[0002] 2. Description of the Related Art Conventionally, a laminate including a biaxially oriented polyethylene terephthalate film having excellent heat resistance and toughness as a base film, and a sealant layer has been known as a gas barrier laminate (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-178357 A Summary of the Invention [Problem to be solved by the invention]
[0004] In recent years, however, there has been a demand for more efficient sorting and recovery of plastic materials and recycling due to growing environmental awareness triggered by the problem of marine plastic waste, etc. In other words, there is a demand for mono-materialization of packaging laminates, which have traditionally been made high-performance by combining various different materials.
[0005] To realize a mono-material laminate, the constituent films must be made of the same material. For example, polyethylene film, a type of polyolefin film, is widely used as a packaging material, and so there are hopes for a mono-material laminate using polyethylene film. However, one of the basic physical properties of polyethylene film is that it has a low melting point and is easily stretched and deformed even at low temperatures. Therefore, in the process of forming a barrier layer on a polyethylene film by a method such as deposition to impart high gas barrier properties, when the polyethylene film is wound up under tension, the roll transportability becomes poor, wrinkles occur in the film, and problems such as the inability to process the film properly in post-processing can often occur.
[0006] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a gas barrier laminate that is useful for realizing mono-materialization, has good processability, and is wrinkle-resistant. [Means for solving the problem]
[0007] The present invention provides a gas barrier laminate comprising a polyethylene-containing substrate layer and a barrier layer, the polyethylene-containing substrate layer having an arithmetic mean roughness a of 3 μm or more on the surface opposite to the barrier layer. Such a gas barrier laminate has good film transportability and is less prone to wrinkling when rolled.
[0008] When the arithmetic mean roughness of the surface of the polyethylene-containing substrate layer that contacts the barrier layer is designated as b, a / b may be 3 or more.
[0009] The substrate layer comprising polyethylene may comprise unoriented polyethylene.
[0010] The barrier layer may include a gas barrier coating layer, or may include an inorganic vapor deposition layer.
[0011] The barrier layer may include an undercoat layer, an inorganic vapor deposition layer, and a gas barrier coating layer in this order from the side of the polyethylene-containing substrate layer. Effect of the Invention
[0012] The present invention can provide a gas barrier laminate that is suitable for processing and is resistant to wrinkles. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a gas barrier laminate according to one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the drawings as needed. In the drawings, the same or corresponding parts are denoted by the same reference numerals, and duplicated explanations will be omitted. In addition, the dimensional ratios of the drawings are not limited to those shown in the drawings.
[0015] <Gas barrier laminate> Fig. 1 is a schematic cross-sectional view showing a gas barrier laminate according to one embodiment. The gas barrier laminate 10 shown in Fig. 1 includes a base layer 1 and a barrier layer 2. The base layer 1 contains polyethylene, and the arithmetic mean roughness a of the surface of the base layer opposite to the barrier layer is 3 µm or more.
[0016] [Base material layer] The base layer 1 is a film serving as a support and contains polyethylene. The content of polyethylene in the base layer 1 may be 50% by mass or more, 80% by mass or more, or 100% by mass based on the total amount of the base layer 1. The base layer 1 may contain a polyethylene film or may be made of a polyethylene film. In addition, the polyethylene may be an acid-modified polyethylene obtained by graft-modifying polyethylene with an unsaturated carboxylic acid, an acid anhydride of an unsaturated carboxylic acid, an ester of an unsaturated carboxylic acid, or the like.
[0017] The polyethylene contained in the base layer 1 is preferably high density polyethylene (HDPE). HDPE is preferable because it has excellent heat resistance, is less likely to stretch than other polyethylenes, and is more likely to be prevented from wrinkling. The density of the polyethylene contained in the base layer 1 is, for example, 0.94 g / cm 2 or more, and 2 It may be more than that.
[0018] The polyethylene contained in the base layer 1 may be stretched or unstretched, but is preferably unstretched. A base layer containing unstretched polyethylene can ensure the rigidity required for a packaging material and can easily prevent bags from falling off or breaking.
[0019] The arithmetic mean roughness a of the surface of the base layer 1 opposite to the barrier layer 2 is 3 μm or more. When the arithmetic mean roughness a is 3 μm or more, the roll transportability is excellent when the polyethylene film is wound up under tension, and the occurrence of wrinkles in the film can be suppressed. From this viewpoint, the arithmetic mean roughness a of the surface of the base layer 1 opposite to the barrier layer 2 is preferably 4 μm or more, and more preferably 5 μm or more. The upper limit of the arithmetic mean roughness a is not particularly limited, and may be, for example, 10 μm or less.
[0020] When the arithmetic mean roughness of the surface of the base layer 1 in contact with the barrier layer 2 is b, it is preferable that a / b is 3 or more. When a / b is 3 or more, it becomes easy to laminate the barrier layer 2 without impairing the barrier property. From this viewpoint, a / b is more preferably 3.5 or more, and even more preferably 4 or more. There is no particular upper limit for a / b, and it may be, for example, 100 or less. In this specification, the arithmetic mean roughness is measured by measuring the front and / or back surface three times using an optical interference surface measuring device, and the largest maximum projection height (μm) among the three measurements is defined as the arithmetic mean roughness of the film.
[0021] The base layer 1 may be appropriately multi-layered, taking into consideration, for example, the processing suitability, rigidity, strength, heat resistance, and powder fall during transportation of the film constituting the base layer 1. The base layer 1 may be, for example, a multi-layered structure including a plurality of layers (films) each containing polyethylene with different densities. The film constituting the base layer 1 may be appropriately selected from high density polyethylene (HDPE), medium density polyethylene, low density polyethylene, and the like. When the density of the base material for the base layer 1 was measured, the density was 0.94 g / cm. 2 More preferably, the above content is sufficient. In addition, when a slip agent, an antistatic agent, or the like is contained, the content of these agents may be changed in each layer. The base layer 1 having a plurality of layers can be laminated to form a film by extrusion coating, coextrusion coating, sheet molding, coextrusion blow molding, or the like.
[0022] The thickness of the base layer 1 may be, for example, 10 to 100 μm, or 15 to 50 μm.
[0023] The lamination surface of the base layer 1 may be subjected to various pretreatments such as corona treatment, plasma treatment, and flame treatment within the scope that does not impair the barrier performance, or a coating layer such as an easy-adhesion layer may be provided.
[0024] [Barrier layer] The barrier layer 2 is a layer capable of imparting gas barrier properties to the gas barrier laminate, and may include, for example, a gas barrier coating layer, an inorganic vapor deposition layer, etc. As shown in FIG. 1, the barrier layer 2 may include, from the substrate layer 1 side, an undercoat layer 3, an inorganic vapor deposition layer 4, and a gas barrier coating layer 5 in this order. The oxygen permeability of the barrier layer 2 is 20 cc / m 2 ·day·atm or less is preferable, and 10cc / m 2 ·day·atm is more preferable, and 5cc / m 2 ·day·atm or less is more preferable, and 2cc / m 2 By having the oxygen permeability within the above range, the gas barrier properties of the gas barrier laminate can be sufficiently ensured.
[0025] (subbing layer) The undercoat layer (anchor coat layer) 3 has the effects of improving the adhesion between the substrate layer 1 and the inorganic vapor deposition layer 4, improving the smoothness of the surface of the substrate layer 1, and suppressing the occurrence of cracks in the inorganic vapor deposition layer 4 due to elongation of the substrate layer 1. The improved smoothness makes it easier to form the inorganic vapor deposition layer 4 uniformly without defects, and makes it easier to exhibit high barrier properties. The undercoat layer 3 can be formed using a composition for forming an undercoat layer (anchor coat agent).
[0026] Examples of the anchor coating agent include acrylic resins, epoxy resins, acrylic urethane resins, polyester polyurethane resins, polyether polyurethane resins, etc. As the anchor coating agent, acrylic urethane resins and polyester polyurethane resins are preferred from the viewpoints of heat resistance and interlayer adhesive strength.
[0027] The thickness of the undercoat layer 3 is not particularly limited, but is, for example, preferably in the range of 0.01 to 5 μm, more preferably in the range of 0.03 to 3 μm, and even more preferably in the range of 0.05 to 2 μm. When the thickness of the undercoat layer 3 is equal to or greater than the above lower limit, more sufficient interlayer adhesive strength tends to be obtained, while when the thickness is equal to or less than the above upper limit, desired gas barrier properties are likely to be exhibited.
[0028] The method for applying the undercoat layer 3 onto the substrate layer 1 can be any known application method without any particular limitation, and examples of such methods include an immersion method (dipping method), a method using a spray, a coater, a printer, a brush, etc. Examples of the types of coaters and printers used in these methods and the application methods thereof include gravure coaters such as direct gravure method, reverse gravure method, kiss reverse gravure method, and offset gravure method, reverse roll coaters, microgravure coaters, coaters combined with chamber doctor, air knife coaters, dip coaters, bar coaters, comma coaters, die coaters, etc.
[0029] The coating amount of the undercoat layer 3 is 1 m after the anchor coating agent is applied and dried. 2 Mass per unit is 0.01 to 5 g / m 2 is preferably 0.03 to 3 g / m 2 It is more preferable that the thickness of the anchor coating agent is 1m after it is applied and dried. 2 When the mass per unit area is equal to or greater than the lower limit, the film tends to be sufficiently formed, whereas when the mass per unit area is equal to or less than the upper limit, the film tends to be sufficiently dried and the solvent is less likely to remain.
[0030] The method for drying the undercoat layer 3 is not particularly limited, and examples thereof include a method of natural drying, a method of drying in an oven set at a predetermined temperature, and a method using a dryer attached to the coater, such as an arch dryer, a floating dryer, a drum dryer, an infrared dryer, etc. Furthermore, the drying conditions can be appropriately selected depending on the drying method, and for example, in a method of drying in an oven, drying at a temperature of 60 to 100°C for about 1 second to 2 minutes is preferable.
[0031] A polyvinyl alcohol-based resin can be used instead of the above-mentioned resins for the undercoat layer 3. The polyvinyl alcohol-based resin may be any resin having a vinyl alcohol unit obtained by saponifying a vinyl ester unit, and examples thereof include polyvinyl alcohol (PVA) and ethylene-vinyl alcohol copolymer (EVOH).
[0032] Examples of PVA include resins obtained by homopolymerizing vinyl esters such as vinyl acetate, vinyl formate, vinyl propionate, vinyl valerate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl pivalate, and vinyl versatate, followed by saponification. PVA may be modified PVA that has been copolymerized or post-modified. Modified PVA can be obtained, for example, by copolymerizing a vinyl ester with an unsaturated monomer copolymerizable with the vinyl ester, followed by saponification. Examples of unsaturated monomers copolymerizable with vinyl ester include olefins such as ethylene, propylene, isobutylene, α-octene, α-dodecene, and α-octadecene; hydroxyl-containing α-olefins such as 3-buten-1-ol, 4-pentyn-1-ol, and 5-hexen-1-ol; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, maleic anhydride, itaconic acid, and undecylenic acid; nitriles such as acrylonitrile and methacrylonitrile; diacetone acrylamide, acrylonitrile, and methacrylonitrile; and the like. amides such as arylamide and methacrylamide; olefin sulfonic acids such as ethylene sulfonic acid, allyl sulfonic acid, and methallyl sulfonic acid; vinyl compounds such as alkyl vinyl ethers, dimethylallyl vinyl ketone, N-vinylpyrrolidone, vinyl chloride, vinyl ethylene carbonate, 2,2-dialkyl-4-vinyl-1,3-dioxirane, glycerin monoallyl ether, and 3,4-diacetoxy-1-butene; vinylidene chloride, 1,4-diacetoxy-2-butene, and vinylene carbonate.
[0033] The polymerization degree of PVA is preferably 300 to 3000. If the polymerization degree is less than 300, the barrier property is likely to decrease, and if it exceeds 3000, the viscosity is too high and the coating suitability is likely to decrease. The saponification degree of PVA is preferably 90 mol% or more, more preferably 95 mol% or more, and even more preferably 99 mol% or more. The saponification degree of PVA may be 100 mol% or less, or 99.9 mol% or less. The polymerization degree and saponification degree of PVA can be measured in accordance with the method described in JIS K 6726 (1994).
[0034] EVOH is generally obtained by saponifying a copolymer of ethylene and an acid vinyl ester such as vinyl acetate, vinyl formate, vinyl propionate, vinyl valerate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl pivalate, or vinyl versatate.
[0035] The degree of polymerization of EVOH is preferably 300 to 3000. If the degree of polymerization is less than 300, the barrier property is likely to decrease, and if it exceeds 3000, the viscosity is too high and the coating suitability is likely to decrease. The degree of saponification of the vinyl ester component of EVOH is preferably 90 mol % or more, more preferably 95 mol % or more, and even more preferably 99 mol % or more. The degree of saponification of EVOH may be 100 mol % or less, or may be 99.9 mol % or less. The degree of saponification of EVOH can be measured by nuclear magnetic resonance ( 1 H-NMR measurement is performed, and the peak area of the hydrogen atom contained in the vinyl ester structure and the peak area of the hydrogen atom contained in the vinyl alcohol structure are used to determine the molecular weight.
[0036] The ethylene unit content of EVOH is preferably 10 mol% or more, more preferably 15 mol% or more, even more preferably 20 mol% or more, and particularly preferably 25 mol% or more. The ethylene unit content of EVOH is preferably 65 mol% or less, more preferably 55 mol% or less, and even more preferably 50 mol% or less. When the ethylene unit content is 10 mol% or more, the gas barrier property or dimensional stability can be maintained well under high humidity. On the other hand, when the ethylene unit content is 65 mol% or less, the gas barrier property can be improved. The ethylene unit content of EVOH can be determined by NMR method.
[0037] When a polyvinyl alcohol-based resin is used as the undercoat layer 3, the undercoat layer 3 can be formed by coating a polyvinyl alcohol-based resin solution, multi-layer extrusion, or the like.
[0038] (Inorganic vapor deposited layer) Examples of materials constituting the inorganic vapor deposition layer 4 include inorganic oxides such as aluminum oxide, silicon oxide, magnesium oxide, and tin oxide. From the viewpoints of transparency and barrier properties, the inorganic oxide may be selected from the group consisting of aluminum oxide, silicon oxide, and magnesium oxide. From the viewpoint of excellent tensile extensibility during processing, it is preferable that the inorganic vapor deposition layer 4 is a layer using silicon oxide. By using the inorganic vapor deposition layer 4, high barrier properties can be obtained with a very thin layer that does not affect the recyclability of the gas barrier laminate.
[0039] The O / Si ratio of the inorganic vapor deposition layer 4 is preferably 1.7 or more. When the O / Si ratio is 1.7 or more, the content of metal Si is suppressed, and good transparency is easily obtained. In addition, the O / Si ratio is preferably 2.0 or less. When the O / Si ratio is 2.0 or less, the crystallinity of SiO is high, and the inorganic vapor deposition layer is prevented from becoming too hard, and good tensile resistance is obtained. This makes it possible to suppress the occurrence of cracks in the inorganic vapor deposition layer 4 when laminating the gas barrier coating layer 5. In addition, even after forming into a packaging bag, the base layer 1 may shrink due to heat during the boiling treatment, but when the O / Si ratio is 2.0 or less, the inorganic vapor deposition layer easily follows the above shrinkage, and the deterioration of the barrier property can be suppressed. From the viewpoint of obtaining these effects more fully, the O / Si ratio of the inorganic vapor deposition layer 4 is preferably 1.75 to 1.9, and more preferably 1.8 to 1.85.
[0040] The O / Si ratio of the inorganic vapor deposition layer 4 can be determined by X-ray photoelectron spectroscopy (XPS). For example, the measurement can be performed using an X-ray photoelectron spectrometer (manufactured by JEOL Ltd., product name: JPS-90MXV) as a measuring device, a non-monochromated MgKα (1253.6 eV) X-ray source, and an X-ray output of 100 W (10 kV-10 mA). For quantitative analysis to determine the O / Si ratio, relative sensitivity factors of 2.28 for O1s and 0.9 for Si2p can be used.
[0041] The thickness of the inorganic vapor deposition layer 4 is preferably 10 nm or more and 50 nm or less. If the thickness is 10 nm or more, sufficient gas barrier properties can be obtained. Furthermore, if the thickness is 50 nm or less, the occurrence of cracks due to deformation caused by internal stress in the thin film can be suppressed, and the deterioration of gas barrier properties can be suppressed. Note that if the thickness exceeds 50 nm, costs tend to increase due to an increase in the amount of material used and a longer film formation time, and this is not preferable from an economical point of view. From the same viewpoint as above, the thickness of the inorganic vapor deposition layer is more preferably 20 nm or more and 40 nm or less.
[0042] The inorganic vapor deposition layer 4 can be formed, for example, by vacuum film formation. In the vacuum film formation, physical vapor deposition or chemical vapor deposition can be used. Examples of physical vapor deposition include, but are not limited to, vacuum deposition, sputtering, and ion plating. Examples of chemical vapor deposition include, but are not limited to, thermal CVD, plasma CVD, and photo CVD.
[0043] In the vacuum film formation, the resistance heating vacuum deposition method, the EB (Electron Beam) heating vacuum deposition method, the induction heating vacuum deposition method, the sputtering method, the reactive sputtering method, the dual magnetron sputtering method, the plasma enhanced chemical vapor deposition method (PECVD method), and the like are particularly preferably used. However, in terms of productivity, the vacuum deposition method is currently the most excellent. As the heating means for the vacuum deposition method, it is preferable to use any one of the electron beam heating method, the resistance heating method, and the induction heating method.
[0044] (Gas barrier coating layer) The gas barrier coating layer 5 protects the inorganic vapor deposition layer 4 and prevents the inorganic oxide layer from cracking when bent.
[0045] The gas barrier coating layer 5 is a layer having gas barrier properties. By providing the gas barrier coating layer, the gas barrier properties of the gas barrier laminate can be improved.
[0046] The gas barrier coating layer 5 may be formed using a composition for forming a gas barrier coating layer (hereinafter also referred to as a coating agent) whose main component is an aqueous solution or a water / alcohol mixed solution containing at least one member selected from the group consisting of a hydroxyl group-containing polymer compound, a metal alkoxide, a silane coupling agent, and their hydrolysates.
[0047] Specific examples of hydroxyl group-containing polymer compounds include water-soluble polymers such as ethylene vinyl alcohol, polyvinyl alcohol, polyvinylpyrrolidone, starch, methyl cellulose, carboxymethyl cellulose, and sodium alkynate. Polyvinyl alcohol (PVA) is particularly preferred because of its excellent barrier properties.
[0048] The metal alkoxide is preferably formed from a composition containing at least one selected from the group consisting of metal alkoxides represented by the following general formula (1) and their hydrolysates or polymers. M(OR 1 ) m (R 2 ) n-m (1) In the above general formula (1), R 1 and R 2 are each independently a monovalent organic group having 1 to 8 carbon atoms, and are preferably an alkyl group such as a methyl group or an ethyl group. M represents an n-valent metal atom such as Si, Ti, Al, or Zr. m is an integer from 1 to n. 1 or R 2 If there are multiple, R 1 R 2 They may be the same or different.
[0049] Specific examples of metal alkoxides include tetraethoxysilane [Si(OC2H5)4] and triisopropoxyaluminum [Al(O-2'-C3H7)3]. Metal alkoxides are preferably tetraethoxysilane or triisopropoxyaluminum, since they are relatively stable in aqueous solvents after hydrolysis. Examples of hydrolyzates of metal alkoxides include silicic acid (Si(OH)4), which is a hydrolyzate of tetraethoxysilane, and aluminum hydroxide (Al(OH)3), which is a hydrolyzate of tripropoxyaluminum. These can be used alone or in combination.
[0050] The silane coupling agent includes a compound represented by the following general formula (2). Si(OR 11 ) p (R 12 ) 3-p R 13 (2) In the above general formula (2), R 11 represents an alkyl group such as a methyl group or an ethyl group, and R 12 represents a monovalent organic group such as an alkyl group, an aralkyl group, an aryl group, an alkenyl group, an alkyl group substituted with an acryloxy group, or an alkyl group substituted with a methacryloxy group, and R 13 represents a monovalent organic functional group, and p represents an integer of 1 to 3. 11 or R 12 If there are multiple, R 11 R 12 R may be the same or different. 13 Examples of the monovalent organic functional group represented by the formula (I) include a monovalent organic functional group containing a glycidyloxy group, an epoxy group, a mercapto group, a hydroxyl group, an amino group, an alkyl group substituted with a halogen atom, or an isocyanate group.
[0051] Specific examples of the silane coupling agent include vinyltrimethoxysilane, γ-chloropropylmethyldimethoxysilane, γ-chloropropyltrimethoxysilane, glycidoxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, and γ-methacryloxypropylmethyldimethoxysilane.
[0052] The silane coupling agent may also be a polymer formed by polymerizing the compound represented by the general formula (2). The polymer is preferably a trimer, and more preferably 1,3,5-tris(3-trialkoxysilylalkyl)isocyanurate. This is a condensation polymer of 3-isocyanate alkylalkoxysilane. It is known that the isocyanate moiety of this 1,3,5-tris(3-trialkoxysilylalkyl)isocyanurate has no chemical reactivity, but the reactivity is ensured by the polarity of the nurate moiety. In general, it is added to adhesives, etc., in the same manner as 3-isocyanate alkylalkoxysilane, and is known as an adhesion improver. Therefore, by adding 1,3,5-tris(3-trialkoxysilylalkyl)isocyanurate to a hydroxyl group-containing polymer compound, the water resistance of the gas barrier coating layer 5 can be improved by hydrogen bonding. 3-isocyanate alkyl alkoxy silanes are highly reactive and have low liquid stability, whereas 1,3,5-tris (3-trialkoxy silyl alkyl) isocyanurates are not water-soluble due to the polarity of the nurate moiety, but are easily dispersed in aqueous solutions and can maintain a stable liquid viscosity. In addition, the water resistance of 3-isocyanate alkyl alkoxy silanes is equivalent to that of 1,3,5-tris (3-trialkoxy silyl alkyl) isocyanurates.
[0053] 1,3,5-tris(3-trialkoxysilylalkyl)isocyanurate is produced by thermal condensation of 3-isocyanatepropylalkoxysilane, and may contain the raw material 3-isocyanatepropylalkoxysilane, but this does not cause any problem. More preferably, 1,3,5-tris(3-trialkoxysilylpropyl)isocyanurate is used, and more preferably, 1,3,5-tris(3-trimethoxysilylpropyl)isocyanurate is used. This methoxy group has a fast hydrolysis rate, and those containing propyl groups are relatively inexpensive and therefore 1,3,5-tris(3-trimethoxysilylpropyl)isocyanurate is advantageous in practical use.
[0054] Furthermore, known additives such as an isocyanate compound, a dispersant, a stabilizer, a viscosity adjuster, a colorant, and the like may be added to the coating agent as long as the gas barrier properties are not impaired.
[0055] The coating agent may contain water-swellable mica. Mica is a type of inorganic layered mineral in which extremely thin unit crystal layers overlap to form a layered particle. Micas include natural mica and synthetic mica. For example, muscovite, phlogopite, biotite, potassium phlogopite, potassium tetrasilicic mica, potassium taeniolite, potassium sodium fluorine tetrasilicic mica, fluorine tetrasilicic mica, sodium phlogopite, sodium tetrasilicic mica, sodium hectorite, etc. One of these micas may be used, or two or more different micas may be used in combination.
[0056] As the mica, those that swell and cleave in water are preferred, and among these, water-swellable mica that has swelling properties in water is particularly preferred. More specifically, it is a synthetic mica that has the property of absorbing and swelling water by coordinating it between the extremely thin unit crystal layers, and generally contains Si 4+ O 2- The layers are coordinated to form a tetrahedral structure, and the Al 3+ , Mg 2+ , Fe 2+ , and Fe 3+ Etc., O 2-and OH - The layers that form the octahedral structure are bonded to each other in a 1:1 or 2:1 ratio and stacked to form a layered structure. For example, sodium tetrasilicic fluoride mica is preferred.
[0057] When water-swellable mica is contained, the coating agent preferably contains a hydroxyl group-containing polymer compound. When the total mass of the gas barrier coating layer 5 is 100 parts by mass, the content of the water-swellable mica may be within the approximate range of, for example, 20 parts by mass to 50 parts by mass. In this case, the gas barrier coating layer 5 can be formed using a coating liquid containing, as solid contents, the hydroxyl group-containing polymer compound and the water-swellable mica. The solid content ratio of the water-swellable mica among the total solid contents of this coating liquid may be within the approximate range of, for example, 20% by mass to 50% by mass.
[0058] The area-average diameter of the water-swellable mica is, for example, within the approximate range of 0.5 μm to 5 μm, and may be within the approximate range of 1.5 μm to 2.5 μm. The aspect ratio of the water-swellable mica is, for example, within the approximate range of 10 to 200.
[0059] The thickness of the gas barrier coating layer 5 is preferably 50 to 1000 nm, and more preferably 100 to 500 nm. If the thickness of the gas barrier coating layer 5 is 50 nm or more, more sufficient gas barrier properties tend to be obtained, and if it is 1000 nm or less, sufficient flexibility tends to be maintained.
[0060] The coating agent for forming the gas barrier coating layer 5 can be applied by, for example, dipping, roll coating, gravure coating, reverse gravure coating, air knife coating, comma coating, die coating, screen printing, spray coating, gravure offset, etc. The coating film obtained by applying this coating agent can be dried by, for example, hot air drying, hot roll drying, high frequency irradiation, infrared irradiation, UV irradiation, or a combination thereof. Taking high speed processability into consideration, the coating film is most preferably dried by hot air drying.
[0061] The temperature and tension when drying the coating film may be, for example, a coating film surface temperature of 30 to 120° C. and a tension of 10 to 100 N / m, and preferably a coating film surface temperature of 40 to 70° C. and a tension of 10 to 70 N / m. By keeping the coating film surface temperature and tension during drying within the above ranges, the occurrence of cracks in the inorganic vapor deposition layer 4 and the gas barrier coating layer 5 can be further suppressed, and excellent barrier properties can be exhibited.
[0062] When the gas barrier coating layer 5 is formed by high speed processing, the temperature and tension when drying the coating film may be, for example, an oven temperature of 50 to 180° C. and a tension of 10 to 100 N / m, and preferably an oven temperature of 70 to 150° C. and a tension of 10 to 70 N / m. By keeping the oven temperature and tension during drying within the above ranges, the occurrence of cracks in the inorganic vapor deposition layer 4 and the gas barrier coating layer 5 can be further suppressed during high speed processing of 100 m / min or more over a wide width of 500 mm or more, and excellent barrier properties can be exhibited.
[0063] From the viewpoint of preventing cracking of the inorganic vapor deposition layer 4, it is preferable that the gas barrier coating layer 5 and the inorganic vapor deposition layer 4 are in direct contact (with no other layer interposed therebetween). For this reason, it is preferable to form the gas barrier coating layer 5 by applying the above-mentioned adhesive onto the inorganic vapor deposition layer 4, and drying and curing it. Similarly, from the viewpoint of preventing cracking of the inorganic vapor deposition layer 4, it is preferable that the inorganic vapor deposition layer 4 and the undercoat layer 3 are in direct contact (with no other layer interposed therebetween).
[0064] The gas barrier laminate according to this embodiment may include a sealant layer or a print layer on the barrier layer.
[0065] The sealant layer is a layer that imparts heat sealing properties to the gas barrier laminate. The sealant layer may contain a polyolefin, and the polyolefin may be polyethylene.
[0066] As the material for the sealant layer, polyolefin-based resins are generally used among thermoplastic resins, and specifically, ethylene-based resins such as low-density polyethylene resin (LDPE), medium-density polyethylene resin (MDPE), direct-locked low-density polyethylene resin (LLDPE), ethylene-vinyl acetate copolymer (EVA), ethylene-α-olefin copolymer, ethylene-(meth)acrylic acid copolymer, etc., blend resins of polyethylene and polybutene, polypropylene-based resins such as homopolypropylene resin (PP), propylene-ethylene random copolymer, propylene-ethylene block copolymer, propylene-α-olefin copolymer, etc. can be used. These thermoplastic resins can be appropriately selected depending on the application and temperature conditions such as boiling treatment.
[0067] The sealant layer may contain various additives such as a flame retardant, a slip agent, an antiblocking agent, an antioxidant, a light stabilizer, and a tackifier.
[0068] The thickness of the sealant layer is determined depending on the weight of the contents, the shape of the package, etc., but a thickness of about 30 to 150 μm is preferable.
[0069] The sealant layer can be formed by any of the known lamination methods, including a method in which a sealant layer on a film made of the above-mentioned thermoplastic resin is bonded with an adhesive for forming the above-mentioned gas barrier coating layer 5, a dry lamination method in which an adhesive such as a one-component curing or two-component curing urethane adhesive is used for bonding, a non-solvent dry lamination method in which a sealant layer on a film is bonded with a solvent-free adhesive, and an extrusion lamination method in which the above-mentioned thermoplastic resin is heated and melted, extruded into a curtain shape, and bonded together.
[0070] The printing layer is provided at a position visible from the outside of the gas barrier laminate for the purpose of displaying information about the contents, identifying the contents, or improving the design of the packaging bag. The printing method and printing ink are not particularly limited, and are appropriately selected from known printing methods and printing inks in consideration of printability on the film, design such as color tone, adhesion, safety as a food container, etc. Examples of printing methods that can be used include gravure printing, offset printing, gravure offset printing, flexographic printing, and inkjet printing. Among them, gravure printing can be preferably used from the viewpoints of productivity and high definition of the image.
[0071] In order to improve the adhesion of the printed layer, the surface of the layer on which the printed layer is formed may be subjected to various pretreatments such as corona treatment, plasma treatment, and frame treatment, or a coating layer such as an easy-adhesion layer may be provided.
[0072] As described above, the film constituting the gas barrier laminate according to this embodiment can be a mono-material packaging material that is excellent in recyclability. The gas barrier laminate can be suitably used for various applications such as packaging products such as containers and bags, sheet molded products such as decorative sheets and trays, optical films, resin plates, various label materials, lid materials, and laminate tubes, and is particularly suitable for use in packaging products. Examples of packaging products include pillow bags, standing pouches, three-side sealed bags, and four-side sealed bags.
[0073] <Packaging bag> The packaging bag is produced by forming the gas barrier laminate described above. The packaging bag may be produced by folding one gas barrier laminate in half so that the sealant layers face each other, and then heat-sealing three sides to form a bag shape, or may be produced by stacking two gas barrier laminates so that the sealant layers face each other, and then heat-sealing four sides to form a bag shape. The packaging bag can contain food, medicine, and other contents. The packaging bag can be subjected to a heat sterilization treatment such as boiling treatment.
[0074] The boiling treatment is a method of moist heat sterilization for preserving food, medicine, etc. Usually, although depending on the contents, a packaging bag in which food, etc. is packaged is subjected to moist heat sterilization treatment under conditions of 60 to 100°C, atmospheric pressure, and 10 to 120 minutes. The boiling treatment is usually performed using a hot water bath at 100°C or less. Methods include a batch type in which the bag is immersed in a hot water bath at a constant temperature and treated for a certain period of time, and then removed, and a continuous type in which the bag is passed through a tunnel-type hot water bath for treatment. The packaging bag of this embodiment can also be suitably used for applications in which a boiling treatment is performed.
[0075] The packaging bag may have a shape having a bent portion (folded portion) such as a standing pouch, etc. The packaging bag of the present embodiment can maintain high gas barrier properties even when it has a shape having a bent portion. EXAMPLES
[0076] The present invention will be described in more detail with reference to the following examples, but the present invention is not limited to these examples.
[0077] [Base material layer] Substrate A: GAP (Charter NEX, thickness: 32 μm, unstretched HDPE) Substrate B: SMUQ (Tokyo Ink Co., Ltd., thickness: 25 μm, stretched HDPE) Substrate C: UB-3 (manufactured by Tamapoly Co., Ltd., thickness: 40 μm, unstretched MDPE) Substrate D: JINDAL (manufactured by JINDAL, thickness: 25 μm, stretched HDPE)
[0078] <Measurement of arithmetic mean roughness of base layer> Using an optical interference surface measuring instrument (Vertscan R3300h Lite, manufactured by Ryoka Systems Co., Ltd.) and a 5x objective lens, the front and back surfaces were each measured three times, and the largest maximum protrusion height (μm) among the three measurements was taken as the protrusion height (arithmetic mean roughness) of the film.
[0079] [Preparation of composition for forming undercoat layer] Acrylic polyol and tolylene diisocyanate were mixed so that the number of NCO groups of tolylene diisocyanate was equal to the number of OH groups of the acrylic polyol, and diluted with ethyl acetate so that the total solid content (total amount of acrylic polyol and tolylene diisocyanate) was 5 mass%. β-(3,4 epoxycyclohexyl)trimethoxysilane was further added to the diluted mixed solution so that the amount was 5 mass parts per 100 mass parts of the total amount of acrylic polyol and tolylene diisocyanate, and these were mixed to prepare a composition for forming an undercoat layer (anchor coating agent).
[0080] [Preparation of composition for forming gas barrier coating layer (coating agent)] Composition A for forming gas barrier coating layer: A gas barrier coating layer A was prepared by mixing the following liquids A, B, and C in a mass ratio of 70 / 20 / 10. Liquid A: A hydrolysis solution with a solid content of 5 mass% (SiO2 equivalent) obtained by adding 72.1 g of 0.1N hydrochloric acid to 17.9 g of tetraethoxysilane (Si(OC2H5)4) and 10 g of methanol and stirring for 30 minutes. B liquid: 5% by mass of polyvinyl alcohol in water / methanol (water:methanol mass ratio is 95:5) Liquid C: A hydrolysis solution in which 1,3,5-tris(3-trialkoxysilylpropyl)isocyanurate was diluted with a mixture of water and isopropyl alcohol (water:isopropyl alcohol mass ratio 1:1) to a solid content of 5 mass%.
[0081] Composition B for forming gas barrier coating layer: The polyurethane resin, 5% PVA aqueous solution, and silane coupling agent were mixed in a solid content ratio of 60:35:5, and diluted with water and isopropanol to a solid content concentration of 5% to prepare gas barrier coating layer forming composition B. At this time, the amount of isopropanol was 10% of the total gas barrier coating layer forming composition B.
[0082] Composition C for forming a gas barrier coating layer: Polyvinyl alcohol resin (PVA, Selvol-325 (saponification degree: 98-99%, polymerization degree 1700), manufactured by Sekisui Specialty Chemicals America, LLC.) was used as the hydroxyl group-containing polymer compound. The polyvinyl alcohol resin and water were mixed and heated to 95°C to dissolve the polyvinyl alcohol resin in water. After cooling the mixture to room temperature, it was diluted with water and isopropanol (mass ratio 1:1) so that the final solid concentration was 5 mass%, to prepare component (A). Water-swellable synthetic mica (Somasif MEB-3, manufactured by Co-op Agri Co., Ltd.) was used as the water-swellable mica. The water-swellable synthetic mica was treated using a bead mill so that the area particle size was 2 μm. Then, water was mixed so that the final solid concentration was 8 mass %, and component (B) was prepared. Components (A) and (B) were diluted with water and methanol (mass ratio 1:1) so that the content of water-swellable synthetic mica in the final gas barrier coating layer was 15 mass % to prepare composition C for forming a gas barrier coating layer.
[0083] Example 1 The above-mentioned composition for forming the undercoat layer was applied by gravure roll coating onto the surface of the substrate A having the smallest maximum projection height, and then dried and cured at 60°C to obtain a coating amount of 0.1 g / m 2On the above-mentioned undercoat layer, a transparent inorganic deposition layer (silica deposition film) made of silicon oxide having a thickness of 30 nm was formed by a vacuum deposition apparatus using an electron beam heating method. As the silica deposition film, a deposition film having O / Si of 1.8 was formed by preparing a deposition material type. On the above-mentioned inorganic deposition layer, a composition A for forming a gas barrier coating layer was applied by a gravure roll coating method, and the composition was heated and dried in an oven under a tension of 20 N / n and under conditions that the temperature of the coated coating surface was 60°C, thereby forming a gas barrier coating layer having a thickness of 0.3 μm. The heat drying was performed by attaching a heat label (manufactured by Micron Co., Ltd.) to the coating surface before drying, checking the temperature after drying, and adjusting the oven temperature to an arbitrary temperature (60°C in this embodiment). As a result, a gas barrier laminate having a laminated structure of a base layer / undercoat layer / inorganic deposition layer / gas barrier coating layer was obtained.
[0084] Example 2 A gas barrier laminate was obtained in the same manner as in Example 1, except that composition B for forming a gas barrier coating layer was used instead of composition A for forming a gas barrier coating layer.
[0085] Example 3 A gas barrier laminate was obtained in the same manner as in Example 1, except that composition C for forming a gas barrier coating layer was used instead of composition A for forming a gas barrier coating layer.
[0086] Example 4 A gas barrier laminate was obtained in the same manner as in Example 1, except that the gas barrier coating layer was not formed.
[0087] Example 5 A gas barrier laminate was obtained in the same manner as in Example 3, except that no inorganic vapor deposition layer was formed on the undercoat layer.
[0088] Comparative Example 1 Substrate B was used instead of substrate A, and an undercoat layer, an inorganic vapor deposition layer and a gas barrier coating layer were formed on the surface having the greater maximum projection height in the same manner as in Example 1 to obtain a gas barrier laminate.
[0089] Comparative Example 2 Substrate C was used in place of substrate A, and an undercoat layer, an inorganic vapor deposition layer and a gas barrier coating layer were formed on the surface having the smaller maximum projection height in the same manner as in Example 1, to obtain gas barrier laminate G.
[0090] Comparative Example 3 Substrate D was used in place of substrate A, and an undercoat layer, an inorganic vapor deposition layer and a gas barrier coating layer were formed on the surface having the smaller maximum projection height in the same manner as in Example 1, to obtain gas barrier laminate H.
[0091] <Evaluation of processing suitability> When lamination was performed by laminating the gas barrier laminates A to H produced in Examples 1 to 5 and Comparative Examples 1 to 3 using a gravure coating machine in a roll-to-roll manner, those which could be laminated without any problems were marked as "Good", and those which had wrinkles during winding and the winding shape was deformed were marked as "Poor". The results are shown in Table 1.
[0092] <Evaluation of oxygen barrier properties> The oxygen barrier properties of the gas barrier laminates according to the examples, which had good processing suitability, were measured by JIS K7126, Method B (isobaric method). The measurement was performed using an OXTRAN 2 / 20 made by MOCON at a temperature of 30°C and a relative humidity of 70%. The results are shown in Table 1 (unit: cc / m 2 ·day·atm).
[0093] <Kinematic friction coefficient> The dynamic friction coefficients of the back surface of the base layer and the barrier layer opposite the base layer in the gas barrier laminates according to the examples with good processing suitability were measured under the following conditions, assuming that the gas barrier laminates would be wound up on a roll, etc. The dynamic friction coefficients are shown in Table 1. Measurement speed: 100mm / min Slider: 63 x 63 mm Slider mass: 200g Dynamic friction force: Average load from the start of relative shear movement between the contact surfaces up to 60 mm (N=3 times) Coefficient of kinetic friction: kinetic friction force divided by 1.96
[0094] [Table 1] [Explanation of symbols]
[0095] Reference Signs List 1: substrate layer, 2: barrier layer, 3: undercoat layer, 4: inorganic vapor deposition layer, 5: gas barrier coating layer, 10: gas barrier laminate.
Claims
1. A base layer made of a polyethylene film having a thickness of 15 μm to 50 μm and having a first surface and a second surface; an inorganic vapor deposition layer provided on the second surface side of the base layer; Equipped with The arithmetic mean roughness a of the first surface of the base layer is 3 μm to 10 μm, The inorganic deposition layer has a thickness of 10 nm to 50 nm; The gas barrier laminate for packaging bags further comprises an undercoat layer between the substrate layer and the inorganic vapor deposition layer.
2. The substrate layer has a density of 0.940 g / cm 3 2. The gas barrier laminate for packaging bags according to claim 1, which comprises the above polyethylene film.
3. 3. The gas barrier laminate for packaging bags according to claim 1, wherein the base layer is made of a multi-layered polyethylene film.
4. The gas barrier laminate for packaging bags according to any one of claims 1 to 3, wherein the undercoat layer comprises a polyvinyl alcohol-based resin.
5. The gas barrier laminate for packaging bags according to any one of claims 1 to 4, further comprising a sealant layer containing a polyethylene resin on the second surface side of the base material layer.
6. 6. The gas barrier laminate for packaging bags according to claim 5, wherein the sealant layer is a layer formed by an extrusion lamination method.
7. 6. The gas barrier laminate for packaging bags according to claim 5, wherein the sealant layer is a layer formed by a non-solvent lamination method.
Citation Information
Patent Citations
Gas barrier laminate
JP2010000743A
Polyethylene-based crosslinked shrink film
JP2015093885A
Laminate for packaging material and packaging material
JP2020037186A
Composite gas barrier laminate and method for producing same
WO2015115337A1
Packaging bag
JP2017178357A
Cited By
Gas barrier laminate
JP2025100875A
gas barrier laminate
JP7921356B2