Composite molded body, method of manufacturing the same, and fiber composition
The composite molded body with cellulose fine fibers and an organic filler, using a crosslinking agent, addresses the agglomeration issue, enabling uniform dispersion and improved mechanical properties in thick members.
Patent Information
- Application Number
- JP2024120359
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-04-03
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing technologies face challenges in uniformly dispersing cellulose fine fibers in members with large thickness dimensions due to their tendency to agglomerate, leading to non-uniform distribution and reduced mechanical properties.
A composite molded body comprising cellulose fine fibers and an organic filler, with controlled fiber diameters and content, along with a crosslinking agent to form a stable three-dimensional network, ensuring uniform dispersion and improved mechanical properties.
The solution enables the formation of members with uniformly dispersed cellulose fine fibers, enhancing strength and stability while allowing for various shapes and improved resin impregnation, thus achieving high-quality composite molded products.
Smart Images

Figure 2024144619000004 
Figure 2024144619000005 
Figure 2024144619000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite molded body, a manufacturing method thereof, and a fiber composition. [Background technology]
[0002] In recent years, from the viewpoint of environmental protection, it has been proposed to manufacture various components using materials that have a small environmental impact during manufacture, use, and disposal. For example, components made of materials mainly composed of organic fibers have advantages such as light weight and low disposal costs. In particular, components obtained using fine organic fibers can have unique properties in mechanical strength, heat resistance, dimensional stability, air permeability, etc., and therefore various material designs have been carried out. For example, cellulose fine fibers (also called cellulose nanofibers, etc.) are lightweight and have excellent elastic modulus, heat resistance, dimensional stability, etc., and therefore can be suitably incorporated into various components.
[0003] Patent Document 1 discloses a fabric with a basis weight of 5 g / m 2 More than 100g / m 2 The present invention relates to a cellulose microfibril composition having a number average fiber diameter of 2 nm to 300 nm (component A) and one or more filler materials (component B) selected from the group consisting of inorganic fibers and polymeric fibers, the proportion of component A being 30% by weight to 90% by weight, and the composition having a density of 10 g / m 2 A composite molding material is described, which is characterized in that the air resistance equivalent to the basis weight is 10s / 100cc or more and 2,000s / 100cc or less.
[0004] Patent Document 2 describes a composite in which a resin is impregnated into a nonwoven fabric containing first fibers having a number average fiber width of 2 nm or more and less than 1000 nm and second fibers having a number average fiber width of 1000 nm or more and 100,000 nm or less and a number average fiber length of 0.1 to 20 mm, and describes that the first fibers may be cellulose fibers.
[0005] Patent Document 3 describes a composite including synthetic pulp having a Canadian freeness of 300 ml to 740 ml, the synthetic pulp being composed of microfibril fibers having an average fiber length of 0.05 mm to 50 mm, a minimum fiber diameter of 0.5 μm, and a maximum fiber diameter of 50 μm, the microfibril fibers being made of a resin having an MFR of 0.1 g / 10 min to 200 g / 10 min, and the Canadian freeness being 300 ml to 740 ml, and cellulose nanofibers captured in the synthetic pulp. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2010-202987 A [Patent Document 2] JP 2015-25033 A [Patent Document 3] JP 2018-204147 A Summary of the Invention [Problem to be solved by the invention]
[0007] It is generally difficult to mold cellulose fine fibers alone into a component, but they can be molded into various shapes by combining them with other materials (e.g., other fibers, etc.). However, since cellulose fine fibers are highly susceptible to aggregation due to strong hydrogen bonds caused by hydroxyl groups in cellulose molecules, it is difficult to uniformly disperse cellulose fine fibers in a component. The techniques described in Patent Documents 1 to 3 aim to provide sheet-like products with improved desired properties such as mechanical properties and printability while maintaining the advantages of cellulose fine fibers, and although they may be useful for relatively thin sheets, they do not enable uniform dispersion of cellulose fine fibers even in components with large thickness dimensions (i.e., the minimum dimension in the shape of the product) (thick film sheets, components of various other shapes).
[0008] The present invention aims to solve the above-mentioned problems and provide a composite molded body, a manufacturing method thereof, and a fiber composition which enable the formation of a component having a large thickness dimension while having cellulose fine fibers uniformly dispersed therein. [Means for solving the problem]
[0009] The present invention includes the following aspects. [1] A composite molding containing cellulose fine fibers and an organic filler, The average fiber diameter of the cellulose fine fibers is 5 nm or more and 2 μm or less, The content of the cellulose fine fibers in the composite molded body is 3% by mass or more and 90% by mass or less, The composite molding has a basis weight of 50 g / m 2 More than 1000g / m 2 is as follows: The average air resistance of the composite molded body is 0.5 sec / 100 mL or more and 100,000 sec / 100 mL or less, The coefficient of variation of air resistance, which is the standard deviation of the air resistance of the composite molded body divided by the average air resistance, is 0.5 or less; The average minor axis diameter of the organic filler is 0.1 μm or more and 100 μm or less, The thickness of the composite molded body is 100 μm or more and 10,000 μm or less. Composite molded body. [2] The composite molded body according to the above aspect 1, having a tensile strength of 0.1 kg / 15 mm or more and 40 kg / 15 mm or less. [3] The composite molded body according to the above-mentioned embodiment 1 or 2, wherein the organic filler is a fibrillated cut fiber. [4] A reactant derived from a crosslinking agent is uniformly distributed between the cellulose fine fibers, between the organic filler, and / or between the cellulose fine fibers and the organic filler in the composite molded body in a planar direction of the composite molded body, The composite molded body according to any one of the above aspects 1 to 3, wherein a mass ratio of the reactant is 0.1 to 100 mass % relative to a total mass of the cellulose fine fibers and the organic filler (100 mass %). [5] The composite molded body according to claim 4, wherein the reactant contains a urethane bond. [6] The composite molded body according to any one of the above aspects 1 to 5, wherein the organic filler is made of a thermoplastic resin. [7] The composite molded body according to claim 6, wherein the thermoplastic resin comprises at least one selected from the group consisting of polyolefins, polyesters, polyamides, acrylic polymers, polyvinyl alcohols, polylactic acids, polyphenylene ethers, polyoxymethylenes, and polyphenylene sulfides. [8] The composite molded body according to aspect 6 or 7, wherein the melting point of the thermoplastic resin is 50°C or higher and 500°C or lower. [9] The composite molded body according to any one of the above embodiments 1 to 8, which is a sheet.
[10] The composite molded body according to any one of the above embodiments 1 to 9, which is a curved molded body, a box-shaped molded body, or a cone-shaped molded body.
[11] A method for producing the composite molded body according to any one of the above aspects 1 to 10, comprising the steps of: A slurry preparation step of preparing a slurry containing cellulose fine fibers, an organic filler, and a liquid medium containing water; A concentrating step of dehydrating the slurry by a papermaking method to obtain a wet molded body; and a solidification step of at least drying the wetted molded body to obtain a composite molded body; A method comprising:
[12] The method according to claim 11, wherein the solid content of the slurry is 0.2% by mass to 1.5% by mass.
[13] The slurry further comprises a reactive crosslinker; The method according to aspect 11 or 12, wherein in the slurry preparation step, or simultaneously with or after the drying step, the reactive crosslinking agent is reacted to crosslink between the cellulose fine fibers, between the organic filler particles, and / or between the cellulose fine fibers and the organic filler.
[14] The reactive crosslinker is a blocked polyisocyanate; The method of claim 13, wherein the reaction is carried out at a temperature equal to or higher than the deblocking temperature of the blocked polyisocyanate.
[15] The method of claim 14, wherein the blocked polyisocyanate is a cationic blocked polyisocyanate.
[16] The method according to any one of the above-mentioned aspects 13 to 15, wherein the drying is carried out at 80° C. or more and 120° C. or less, and the reaction is carried out at 130° C. or more and 220° C. or less.
[17] The method according to any one of Aspects 13 to 16, wherein in the slurry preparation step, a premix is prepared by mixing cellulose fine fibers, a reactive crosslinking agent, and a liquid medium, and then the premix is mixed with an organic filler to obtain the slurry.
[18] The method according to any one of Aspects 13 to 16, wherein in the slurry preparation step, a premix is prepared by mixing cellulose fine fibers, an organic filler, and a liquid medium, and then the premix is mixed with a reactive crosslinking agent to obtain the slurry.
[19] A fiber composition, which is a shredded product of the composite molding according to any one of the above embodiments 1 to 10.
[20] The fiber composition of claim 19, wherein the shredded material is granular.
[21] The fiber composition of claim 19, wherein the shredded material is a pellet.
[22] A method for producing a resin molded product containing cellulose fine fibers and a resin, comprising: A mixing step of mixing the fiber composition according to any one of the above aspects 19 to 21 with a resin to obtain a mixture; and a molding step of molding the mixture; A method comprising:
[23] The organic filler in the fiber composition comprises a thermoplastic resin, the resin comprises a thermoplastic resin, 23. The method of claim 22, wherein the fiber composition and the resin are melt mixed in the mixing step.
[24] The method according to any one of claims 22 to 23, wherein the molding is selected from the group consisting of extrusion molding and injection molding.
[25] A method for producing a resin molded product containing cellulose fine fibers and a resin, comprising: A composite molded body forming step of forming a composite molded body containing cellulose fine fibers and an organic filler containing a thermoplastic resin by the method according to any one of the above-mentioned aspects 11 to 18; and a molding step of molding the composite molded body at a temperature equal to or higher than the melting point of the thermoplastic resin in the organic filler; A method comprising:
[26] A method for producing a resin molded product containing cellulose fine fibers and a resin, comprising: A composite molded body forming step of forming a composite molded body containing cellulose fine fibers and an organic filler by the method according to any one of the above-mentioned aspects 11 to 18; and a molding step of impregnating the composite molded body with a resin and then solidifying the resin; A method comprising:
[27] The method according to claim 26, wherein the resin to be impregnated is a heated and melted thermoplastic resin, and the solidification is performed by cooling.
[28] The organic filler comprises a thermoplastic resin; 28. The method of claim 27, wherein the impregnated resin is a hot melt of a thermoplastic resin having a melting point lower than that of the thermoplastic resin in the organic filler.
[29] The method according to claim 26, wherein the resin to be impregnated is an uncured or semi-cured thermosetting resin or photocurable resin, and the solidification is curing.
[30] The method according to any one of the above-mentioned aspects 25 to 29, wherein the molding step is carried out by mold pressing.
[31] The method according to any one of Aspects 25 to 30, wherein the resin molded article is an automobile part.
[32] A sound-absorbing material comprising the composite molded body according to any one of aspects 1 to 10.
[33] An air filter comprising the composite molded body according to any one of the first to tenth aspects.
[34] An automobile part material comprising the composite molded body according to any one of the first to tenth embodiments. Effect of the Invention
[0010] According to the present invention, it is possible to form a component having a large thickness dimension while having cellulose fine fibers uniformly dispersed therein, and since a decrease in strength resulting from uneven distribution of the component composition is unlikely to occur in a composite molded body and a resin molded body in which said composite molded body is further compounded with a resin, a composite molded body with higher strength and more stable quality, a manufacturing method thereof, and a fiber composition can be provided. [Brief description of the drawings]
[0011] [Figure 1] 13 is an explanatory diagram of a method for calculating the IR index 1730 and the IR index 1030. FIG. [Diagram 2] FIG. 2 is an explanatory diagram of a method for calculating the average substitution degree of hydroxyl groups in cellulose. [Diagram 3] FIG. 13 is a diagram showing the results of sound absorption coefficient measurement in Example 4. [Figure 4] FIG. 13 is a diagram showing the results of sound absorption coefficient measurement in Example 9. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, exemplary embodiments of the present invention will be described, but the present invention is not limited to these embodiments.
[0013] ≪Composite molded body≫ One aspect of the present invention provides a composite molded body containing cellulose fine fibers and an organic filler. In one aspect, the average fiber diameter of the cellulose fine fibers is 5 nm or more and 2 μm or less. In one aspect, the content of the cellulose fine fibers in the composite molded body is 3 mass % or more and 90 mass % or less. In one aspect, the basis weight of the composite molded body is 50 g / m 2 More than 1000g / m 2In one embodiment, the composite molded body has an average air resistance of 0.5 seconds / 100 mL or more and 100,000 seconds / 100 mL or less. In one embodiment, the coefficient of variation of air resistance, which is the standard deviation of the air resistance of the composite molded body divided by the average air resistance, is 0.5 or less. In one embodiment, the average minor axis diameter of the organic filler is 0.1 μm or more and 100 μm or less. In one embodiment, the composite molded body has a thickness of 100 μm or more and 10,000 μm or less.
[0014] The present inventors have found that by using a composite molded body containing cellulose fine fibers, which has a high basis weight, is porous and excellent in resin impregnation, and has a uniform fiber dispersion state, a member having a large thickness dimension and in which the cellulose fine fibers are uniformly dispersed can be manufactured with high efficiency and high quality. The air resistance variation coefficient can be regarded as an index reflecting the homogeneity of the composite molded body. With a small air resistance variation coefficient, the strength of the composite molded body as a whole can be improved due to less strength variation caused by defects, and physical properties such as strength and resin impregnation can be stably expressed, so that high quality can be ensured. Furthermore, by impregnating such a composite molded body with resin or pressing the composite molded body, members of various shapes can be formed with high efficiency and high quality.
[0015] The composite molded body may have various shapes, for example, a sheet shape (the surface may be flat, curved, or a combination thereof), or various part shapes (for example, a curved molded body, a box-shaped molded body, a cone-shaped molded body, etc.). In one embodiment, the composite molded body is a sheet. Specific examples of each component of the composite molded body will be described below.
[0016] <Cellulose microfibers> The composite molded body of the present embodiment contains cellulose fine fibers. The content of the cellulose fine fibers in the composite molded body is 3% by mass or more, preferably 9% by mass or more, 15% by mass or more, or 25% by mass or more, in one aspect, from the viewpoint of obtaining the advantages of using the cellulose fine fibers and the homogeneity of the composite molded body, and is 90% by mass or less, preferably 85% by mass or less, 82% by mass or less, or 75% by mass or less, in one aspect, from the viewpoint of ease of production of the composite molded body. If the content of the cellulose fine fibers in the composite molded body is less than 3% by mass, the self-supporting property of the composite molded body (strength that allows handling as a structure) is not guaranteed, which is not preferable. Also, if the content of the cellulose fine fibers in the composite molded body is more than 90% by mass, for example, the filtration time by papermaking becomes significantly longer, and the basis weight of the composite molded body of the present invention becomes 50 g / m 2 This is also undesirable since it becomes practically difficult to achieve the above.
[0017] The raw material for cellulose fine fibers includes so-called wood pulp such as coniferous pulp and hardwood pulp, and non-wood pulp. Examples of non-wood pulp include cotton-derived pulp such as cotton linter pulp, hemp-derived pulp, bagasse-derived pulp, kenaf-derived pulp, bamboo-derived pulp, and straw-derived pulp. Cotton-derived pulp, hemp-derived pulp, bagasse-derived pulp, kenaf-derived pulp, bamboo-derived pulp, and straw-derived pulp respectively refer to purified pulp obtained from raw materials such as cotton lint or cotton linter, hemp-based abaca (for example, many of which are produced in Ecuador or the Philippines), zaisal, bagasse, kenaf, bamboo, and straw through delignification by cooking treatment, and a refining process and a bleaching process for the purpose of removing hemicellulose. In addition, purified products such as seaweed-derived cellulose and sea squirt cellulose can also be used as raw materials for cellulose fine fibers. Furthermore, cut yarns of regenerated cellulose fibers and cut yarns of cellulose derivative fibers can also be used as raw materials for cellulose fine fibers, and cut yarns of ultrafine yarns of regenerated cellulose or cellulose derivatives obtained by electrospinning can also be used as raw materials for cellulose fine fibers or as cellulose fine fibers themselves. Among these, refined pulp derived from cotton lint or cotton linter, hemp-based abaca, zaisal, bagasse, kenaf, bamboo, straw, etc. is particularly preferred because it is easy to obtain cellulose fine fibers with long fiber length and has a high reinforcing effect as a filler due to entanglement.
[0018] The above-mentioned raw material can be refined to obtain cellulose fine fibers. In one embodiment, the refinement is carried out through a pretreatment step, a beating step, and a refinement step. In the pretreatment step, it is effective to make the raw pulp in a state that is easy to refine by autoclaving under water immersion at a temperature of 100 to 150°C, enzyme treatment, or a combination of these. These pretreatments not only reduce the load of the refinement treatment, but also discharge impurity components such as lignin and hemicellulose present on the surfaces and gaps of the microfibrils constituting the cellulose fibers into the aqueous phase, thereby increasing the α-cellulose purity of the finely refined fibers, and therefore may be effective in improving the heat resistance of the cellulose fine fibers.
[0019] In the beating process, the raw pulp is dispersed in water to a solids concentration of 0.5% to 4% by mass, preferably 0.8% to 3% by mass, more preferably 1.0% to 2.5% by mass, and fibrillation is highly promoted using a beating device such as a beater or a disc refiner (double disc refiner). When using a disc refiner, if the clearance between the discs is set as narrow as possible (for example, 0.1 mm or less), an extremely high degree of beating (fibrillation) will proceed, and this may be effective in alleviating the conditions for fine refining using a high-pressure homogenizer or the like.
[0020] A preferred degree of beating is defined as follows. In a study by the present inventors, it was confirmed that the CSF value (indicating the degree of beating of cellulose, evaluated by the Canadian Standard Freeness Test Method for Pulp defined in JIS P 8121) decreases over time as the beating process is performed, and once it reaches near zero, it increases again as the beating process is continued. In order to prepare the cellulose fine fibers that are the raw material of the composite molded body of this embodiment, it was found that it is preferable to beat the cellulose fine fibers as a pretreatment until the CSF value increases after the CSF value reaches near zero once. In the present disclosure, the CSF value in the process of decreasing the CSF value from unbeaten is expressed as ***↓, and the CSF value in the process of increasing after reaching zero is expressed as ***↑. In the beating process, the CSF value is preferably at least zero, and more preferably CSF30↑. In an aqueous dispersion prepared to such a degree of beating, fibrillation progresses to a high degree, and homogeneous cellulose fine fibers having a number average fiber diameter of 2 μm or less, for example 1 μm or less, are obtained. The cellulose microfibers obtained also tend to improve the tensile strength of the composite molded product. This is presumably due to the increase in the number of adhesion points between the cellulose microfibrils. Furthermore, highly beaten aqueous dispersions with a CSF value of at least zero or a value of ***↑ that subsequently increases have high uniformity, which has the advantage of reducing clogging during the subsequent micronization process using a high-pressure homogenizer, etc., in terms of production efficiency.
[0021] Following the above-mentioned beating process, a micronization process may be carried out using a high-pressure homogenizer, an ultra-high-pressure homogenizer, a grinder, etc. In this case, the solid content concentration in the aqueous dispersion is preferably 0.5% by mass or more and 4% by mass or less, more preferably 0.8% by mass or more and 3% by mass or less, and even more preferably 1.0% by mass or more and 2.5% by mass or less, in accordance with the above-mentioned beating process. When the solid content concentration is within this range, clogging does not occur, and efficient micronization process can be achieved.
[0022] Examples of high-pressure homogenizers include the NS-type high-pressure homogenizer from Nilo Soavi (Italy), the Lanier-type (R model) pressure homogenizer from SMT Co., Ltd., and the high-pressure homogenizer from Sanwa Machine Co., Ltd.; examples of ultra-high-pressure homogenizers include high-pressure collision type micronization machines such as the Microfluidizer from Mizuho Kogyo Co., Ltd., the Nanomizer from Yoshida Kikai Kogyo Co., Ltd., and the Starburst from Sugino Machine Co., Ltd.; examples of grinder-type micronization devices include stone mill-type grinding devices such as the Pure Fine Mill from Kurita Machinery Works Ltd. and the Super Mass Colloider from Masuko Sangyo Co., Ltd., but other devices may also be used as long as they perform micronization using a mechanism similar to that of these devices.
[0023] In one embodiment, two or more types of cellulose fine fibers having different raw materials, degrees of fibrillation, chemical treatments, etc. may be combined in any ratio.
[0024] The average fiber diameter of the cellulose fine fibers can be controlled by the conditions of the fine-fining treatment using a high-pressure homogenizer or the like (selection of the type of equipment, operating pressure, number of passes, etc.) or the conditions of the pretreatment prior to the fine-fining treatment (e.g., autoclave treatment, enzyme treatment, beating treatment, etc.).
[0025] The cellulose fine fibers may be produced without being defibrated under high shear using a homogenizer, etc. Cellulose fine fibers that have not been defibrated under high shear tend to have a relatively large amount of branched structure portions and large fiber diameter portions, and such cellulose fine fibers can also be suitably used in the composite molded product of the present disclosure.
[0026] In addition, for example, cellulose fine fibers in which the hydroxyl group at the 6-position is oxidized to a carboxyl group (including acid type and salt type) by a TEMPO (2,2,6,6-tetramethylpiperidinooxy radical) oxidation catalyst, or cellulose fine fibers whose surface is phosphoric acid esterified, may be used. According to these methods, homogeneous cellulose fine fibers can be obtained without using a high-energy-requiring microfiber processing device such as a high-pressure homogenizer. For example, as described in a literature (A. Isogai et al., Biomacromolecules, 7, 1687-1691 (2006)), a TEMPO catalyst and an alkyl halide are made to coexist, an oxidizing agent such as hypochlorous acid is added thereto, and the reaction is allowed to proceed for a certain period of time. This allows cellulose fine fibers to be obtained very easily by performing purification treatment such as washing with water and then performing a normal mixer treatment.
[0027] From the viewpoint of obtaining a composite molded product having excellent physical properties due to the contribution of the cellulose fine fibers, the number average fiber diameter of the cellulose fine fibers is 5 nm or more in one embodiment, and preferably 15 nm or more, or 20 nm or more, or 40 nm or more, or 60 nm or more. From the viewpoint of uniformly distributing the cellulose fine fibers between the organic fillers, the number average fiber diameter is 2 μm or less in one embodiment, and preferably 1.5 μm or less, or 1 μm or less, or 500 nm or less, or 450 nm or less, or 400 nm or less, or 350 nm or less, or 300 nm or less, or 250 nm or less.
[0028] From the viewpoint of satisfactorily improving the mechanical properties of a composite molded article containing the cellulose fine fibers with a small amount of the cellulose fine fibers, the average L / D of the cellulose fine fibers is preferably 20 or more, or 50 or more, or 80 or more, or 100 or more, or 150 or more. The upper limit is not particularly limited, but from the viewpoint of handleability, it is preferably 5000 or less.
[0029] In the present disclosure, the length, diameter, and L / D ratio of each of the cellulose fine fibers are determined by diluting an aqueous dispersion of the cellulose fine fibers with a water-soluble solvent (e.g., water, ethanol, tert-butanol, etc.) to 0.01 to 0.1% by mass, dispersing the fibers using a high-shear homogenizer (e.g., IKA, product name "Ultra Turrax T18") under processing conditions: rotation speed 25,000 rpm x 5 minutes, casting the resulting material on mica, and air-drying the resulting material as a measurement sample, and measuring the length (L) and diameter (D) of 100 randomly selected fibrous substances in an observation field where the magnification is adjusted so that at least 100 fibrous substances are observed, and calculating the ratio (L / D). The number average value of the length (L), the number average value of the diameter (D), and the number average value of the ratio (L / D) of the cellulose fine fibers are calculated. In the case of cellulose fine fibers having a branched structure, the number of fibers of the fibrous material is counted by separately counting the stem portion and the branch portion.
[0030] The length, diameter, and L / D ratio of the cellulose fine fibers in the composite molded body or a composite containing the composite molded body can be confirmed by using the composite molded body or composite as a measurement sample, or by dissolving components other than the cellulose fine fibers from the composite molded body or composite in an organic or inorganic solvent that can dissolve these components to separate the cellulose fine fibers, thoroughly washing with the solvent, and then replacing with a water-soluble solvent (e.g., water, ethanol, tert-butanol, etc.) to prepare a 0.01 to 0.1 mass% dispersion, which is then redispersed using a high-shear homogenizer (e.g., IKA, product name "Ultra Turrax T18"). The redispersed liquid is cast on mica and air-dried to obtain a measurement sample, which can be measured using the above-mentioned measurement method.
[0031] The crystallinity of the cellulose fine fibers is preferably 55% or more. When the crystallinity is within this range, the mechanical properties (strength, dimensional stability) of the cellulose fine fibers themselves are high, and therefore the strength and dimensional stability of the composite molded body tend to be high. A more preferred lower limit of the crystallinity is 60%, 70%, or 80%. There is no particular upper limit for the crystallinity of the cellulose fine fibers, and the higher the better, but from the viewpoint of production, a preferred upper limit is 99%.
[0032] Alkali-soluble polysaccharides such as hemicellulose and acid-insoluble components such as lignin are present between the microfibrils of plant-derived cellulose and between the microfibril bundles. Hemicellulose is a polysaccharide composed of sugars such as mannan and xylan, and plays a role in binding the microfibrils together by hydrogen bonding with cellulose. Lignin is a compound having an aromatic ring, and is known to be covalently bonded to hemicellulose in the cell walls of plants. If there is a large amount of impurities such as lignin remaining in the cellulose fine fibers, discoloration may occur due to heat during processing. Therefore, from the viewpoint of suppressing discoloration of the composite molded body during extrusion processing and molding processing, it is desirable to set the crystallinity of the cellulose fine fibers within the above-mentioned range.
[0033] The degree of crystallinity here, when the cellulose fine fibers are cellulose type I crystals (derived from natural cellulose), is calculated from the diffraction pattern (2θ / deg. is 10 to 30) obtained by measuring the sample by wide-angle X-ray diffraction using the Segal method, according to the following formula: Crystallinity (%) = ([diffraction intensity due to the (200) plane at 2θ / deg. = 22.5] - [diffraction intensity due to amorphous matter at 2θ / deg. = 18]) / [diffraction intensity due to the (200) plane at 2θ / deg. = 22.5] × 100
[0034] When the cellulose fine fibers are cellulose type II crystals (derived from regenerated cellulose), the degree of crystallinity can be calculated from the absolute peak intensity h0 at 2θ=12.6° assigned to the (110) plane peak of the cellulose type II crystals in wide-angle X-ray diffraction and the peak intensity h1 from the baseline at this interplanar spacing, according to the following formula: Crystallinity (%) =h1 / h0 ×100
[0035] Known cellulose crystal forms include type I, type II, type III, and type IV, of which type I and type II are particularly widely used, and type III and type IV are obtained on a laboratory scale but are not widely used on an industrial scale. As the cellulose fine fibers of the present disclosure, cellulose fine fibers containing cellulose type I crystals or cellulose type II crystals are preferred, since they have relatively high structural mobility, a lower linear expansion coefficient, and provide a composite molded product with superior strength and elongation during tensile and bending deformation, and cellulose fine fibers containing cellulose type I crystals and having a crystallinity of 55% or more are more preferred.
[0036] In addition, the degree of polymerization of the cellulose fine fibers is preferably 250 or more, or 300 or more, or 400 or more, or 500 or more, or 600 or more, or 700 or more, because the tensile strength and elastic modulus of the cellulose fine fibers are good, and therefore a composite molded body having good mechanical strength and handleability can be formed.From the viewpoint of easy availability of the cellulose fine fibers, the degree of polymerization is preferably 12,000 or less, and from the viewpoint of handleability, it is more preferably 8,000 or less, or 6,000 or less.
[0037] From the viewpoint of processability and mechanical property expression, it is desirable that the polymerization degree of the cellulose fine fibers is within the above-mentioned range. From the viewpoint of processability, it is preferable that the polymerization degree is not too high, and from the viewpoint of mechanical property expression, it is desirable that the polymerization degree is not too low.
[0038] The degree of polymerization of the cellulose fine fibers means the average degree of polymerization measured according to the reduced specific viscosity method using a copper ethylenediamine solution described in the Verification Test (3) of the "15th Revised Japanese Pharmacopoeia Commentary (published by Hirokawa Shoten)."
[0039] In one embodiment, the weight average molecular weight (Mw) of the cellulose fine fibers is preferably 100,000 or more, or 200,000 or more. The ratio (Mw / Mn) of the weight average molecular weight to the number average molecular weight (Mn) is preferably 6 or less, or 5.4 or less. The larger the weight average molecular weight, the fewer the number of terminal groups of the cellulose molecules. In addition, since the ratio (Mw / Mn) of the weight average molecular weight to the number average molecular weight represents the width of the molecular weight distribution, the smaller the Mw / Mn, the fewer the number of terminals of the cellulose molecules. Since the terminals of the cellulose molecules are the starting points of thermal decomposition, when the cellulose molecules of the cellulose fine fibers have a large weight average molecular weight and a narrow molecular weight distribution width at the same time, a particularly high heat-resistant cellulose fine fiber and a composite molded product can be obtained. The weight average molecular weight (Mw) of the cellulose fine fibers may be, for example, 600,000 or less, or 500,000 or less, from the viewpoint of the availability of the cellulose raw material. From the viewpoint of ease of production of cellulose fine fibers, the ratio (Mw / Mn) of the weight average molecular weight to the number average molecular weight (Mn) may be, for example, 1.5 or more, or 2 or more. Mw can be controlled within the above range by selecting a cellulose raw material having an Mw appropriate for the purpose, performing a physical treatment and / or a chemical treatment on the cellulose raw material appropriately within a moderate range, and the like. Mw / Mn can also be controlled within the above range by selecting a cellulose raw material having an Mw / Mn appropriate for the purpose, performing a physical treatment and / or a chemical treatment on the cellulose raw material appropriately within a moderate range, and the like. In both the control of Mw and the control of Mw / Mn, examples of the physical treatment include dry or wet grinding using a microfluidizer, ball mill, disk mill, etc., physical treatment that applies mechanical forces such as impact, shear, shear, and friction using a crusher, homomixer, high-pressure homogenizer, ultrasonic device, etc., and examples of the chemical treatment include digestion, bleaching, acid treatment, and conversion to regenerated cellulose.
[0040] The weight average molecular weight and number average molecular weight of cellulose referred to here are values determined by dissolving cellulose in N,N-dimethylacetamide containing added lithium chloride and then subjecting the cellulose to gel permeation chromatography using N,N-dimethylacetamide as a solvent.
[0041] Methods for controlling the degree of polymerization (i.e., average degree of polymerization) or molecular weight of cellulose fine fibers include mechanical defibration treatment and hydrolysis treatment. Hydrolysis treatment advances the depolymerization of amorphous cellulose inside the cellulose fine fibers, decreasing the average degree of polymerization. At the same time, hydrolysis treatment removes impurities such as hemicellulose and lignin in addition to the above-mentioned amorphous cellulose, making the inside of the fibers more porous.
[0042] The hydrolysis method is not particularly limited, and examples thereof include acid hydrolysis, alkali hydrolysis, hydrothermal decomposition, steam explosion, and microwave decomposition. These methods may be used alone or in combination of two or more. In the acid hydrolysis method, for example, α-cellulose obtained as pulp from a fibrous plant is used as a cellulose raw material, and this is dispersed in an aqueous medium, and an appropriate amount of a protonic acid, a carboxylic acid, a Lewis acid, a heteropoly acid, etc. is added, and the mixture is heated while stirring, so that the average degree of polymerization can be easily controlled. The reaction conditions at this time, such as temperature, pressure, and time, vary depending on the cellulose type, cellulose concentration, acid type, acid concentration, etc., and are appropriately adjusted so that the desired average degree of polymerization is achieved. For example, a condition in which cellulose is treated for 10 minutes or more at 100°C or higher under pressure using an aqueous mineral acid solution of 2% by mass or less can be exemplified. Under these conditions, the catalyst component such as acid penetrates into the inside of the cellulose fine fibers, promoting hydrolysis, reducing the amount of catalyst component used, and making subsequent purification easier. The dispersion of the cellulose raw material during hydrolysis may contain, in addition to water, a small amount of an organic solvent within a range that does not impair the effects of the present invention.
[0043] Alkali-soluble polysaccharides that may be contained in cellulose fine fibers include hemicellulose, β-cellulose, and γ-cellulose. Alkali-soluble polysaccharides are understood by those skilled in the art as components obtained as the alkali-soluble portion of holocellulose obtained by solvent extraction and chlorine treatment of plants (e.g., wood) (i.e., components obtained by removing α-cellulose from holocellulose). Alkali-soluble polysaccharides are polysaccharides containing hydroxyl groups and have poor heat resistance, and may cause inconveniences such as decomposition when exposed to heat, yellowing during heat aging, and a decrease in strength of cellulose fine fibers. Therefore, it is preferable that the content of alkali-soluble polysaccharides in cellulose fine fibers is low.
[0044] In one embodiment, the average content of alkali-soluble polysaccharides in the cellulose fine fibers is preferably 20% by mass or less, 18% by mass or less, 15% by mass or less, or 12% by mass or less, based on 100% by mass of the cellulose fine fibers, from the viewpoint of obtaining good dispersibility of the cellulose fine fibers. The content may be 1% by mass or more, 2% by mass or more, or 3% by mass or more, from the viewpoint of ease of production of the cellulose fine fibers.
[0045] The average alkali-soluble polysaccharide content can be determined by the method described in the non-patent literature (Wood Science Experiment Manual, edited by the Japan Wood Research Society, pages 92-97, 2000), by subtracting the α-cellulose content from the holocellulose content (Wise method). This method is understood in the industry as a method for measuring the amount of hemicellulose. The alkali-soluble polysaccharide content is calculated three times for each sample, and the number average of the calculated alkali-soluble polysaccharide contents is taken as the average alkali-soluble polysaccharide content.
[0046] In one embodiment, the average content of acid-insoluble components in the cellulose fine fibers is preferably 10% by mass or less, 5% by mass or less, or 3% by mass or less, based on 100% by mass of the cellulose fine fibers, from the viewpoint of avoiding a decrease in heat resistance of the cellulose fine fibers and the associated discoloration. From the viewpoint of ease of production of the cellulose fine fibers, the above content may be 0.1% by mass or more, 0.2% by mass or more, or 0.3% by mass or more.
[0047] The average acid-insoluble content is determined as a quantitative determination of the acid-insoluble content using the Clason method described in the non-patent literature (Wood Science Experiment Manual, edited by the Japan Wood Research Society, pages 92-97, 2000). This method is understood in the industry as a method for measuring the amount of lignin. The sample is stirred in a sulfuric acid solution to dissolve cellulose, hemicellulose, etc., and then filtered through a glass fiber filter paper, and the resulting residue corresponds to the acid-insoluble content. The acid-insoluble content is calculated from the weight of the acid-insoluble content, and the number average of the acid-insoluble content calculated for the three samples is taken as the average acid-insoluble content.
[0048] The cellulose fine fibers may be a combination of fibers obtained by two or more types of fiber pulverization means, such as a mixture of cellulose fine fibers obtained by acid hydrolysis and cellulose fine fibers obtained by mechanical defibration treatment.
[0049] The cellulose fine fibers may be chemically modified, for example, cellulose esters (acetate esters, nitrate esters, sulfate esters, etc.), ethers (alkyl ethers such as methyl ether, carboxy ethers such as carboxymethyl ether, cyano ethers such as cyanoethyl ether), etc. The chemical modification can be carried out using a modifying agent according to the desired modifying group. The modifying agent can be a compound that reacts with the hydroxyl groups of cellulose, and includes an esterifying agent (e.g., a silylating agent) and an etherifying agent. In a preferred embodiment, the chemical modification is acylation using an esterifying agent. As the esterifying agent, acid halides, acid anhydrides, vinyl carboxylates, and carboxylic acids are preferred.
[0050] The acid halide may be at least one selected from the group consisting of compounds represented by the following formula (1). R 1 -C(=O)-X (1) (In the formula, R 1 represents an alkyl group having 1 to 24 carbon atoms, an alkenyl group having 2 to 24 carbon atoms, a cycloalkyl group having 3 to 24 carbon atoms, or an aryl group having 6 to 24 carbon atoms, and X is Cl, Br, or I. Specific examples of acid halides include, but are not limited to, acetyl chloride, acetyl bromide, acetyl iodide, propionyl chloride, propionyl bromide, propionyl iodide, butyryl chloride, butyryl bromide, butyryl iodide, benzoyl chloride, benzoyl bromide, and benzoyl iodide. Among them, acid chlorides can be preferably used in terms of reactivity and handling. In addition, in the reaction of acid halides, one or more alkaline compounds may be added to act as a catalyst and neutralize the by-product acidic substances. Specific examples of alkaline compounds include, but are not limited to, tertiary amine compounds such as triethylamine and trimethylamine; and nitrogen-containing aromatic compounds such as pyridine and dimethylaminopyridine.
[0051] As the acid anhydride, any suitable acid anhydride can be used. For example, Saturated aliphatic monocarboxylic acid anhydrides, such as acetic acid, propionic acid, (iso)butyric acid, and valeric acid; unsaturated aliphatic monocarboxylic acid anhydrides, such as (meth)acrylic acid and oleic acid; Alicyclic monocarboxylic acid anhydrides such as cyclohexanecarboxylic acid and tetrahydrobenzoic acid; Aromatic monocarboxylic acid anhydrides such as benzoic acid and 4-methylbenzoic acid; Examples of dibasic carboxylic acid anhydrides include saturated aliphatic dicarboxylic acid anhydrides such as succinic anhydride and adipic acid, unsaturated aliphatic dicarboxylic acid anhydrides such as maleic anhydride and itaconic anhydride, alicyclic dicarboxylic acid anhydrides such as 1-cyclohexene-1,2-dicarboxylic acid anhydride, hexahydrophthalic anhydride and methyltetrahydrophthalic anhydride, and aromatic dicarboxylic acid anhydrides such as phthalic anhydride and naphthalic anhydride; Examples of polybasic carboxylic acid anhydrides having three or more bases include polycarboxylic acids (anhydrides) such as trimellitic anhydride and pyromellitic anhydride. In addition, in the reaction of an acid anhydride, one or more types of acidic compounds such as sulfuric acid, hydrochloric acid, phosphoric acid, etc., or Lewis acids (for example, Lewis acid compounds represented by MYn, where M represents a semimetal element such as B, As, Ge, etc., or a base metal element such as Al, Bi, In, etc., or a transition metal element such as Ti, Zn, Cu, etc., or a lanthanoid element, n is an integer corresponding to the atomic valence of M and represents 2 or 3, and Y represents a halogen atom, OAc, OCOCF3, ClO4, SbF6, PF6, or OSO2CF3(OTf)), or alkaline compounds such as triethylamine, pyridine, etc. may be added as a catalyst.
[0052] The vinyl carboxylate may be represented by the following formula (1): R-COO-CH=CH2…Formula (1) Preferred is a vinyl carboxylate represented by the formula: {wherein R is any one of an alkyl group having 1 to 24 carbon atoms, an alkenyl group having 2 to 24 carbon atoms, a cycloalkyl group having 3 to 16 carbon atoms, and an aryl group having 6 to 24 carbon atoms.} The vinyl carboxylate is more preferably at least one selected from the group consisting of vinyl acetate, vinyl propionate, vinyl butyrate, vinyl caproate, vinyl cyclohexanecarboxylate, vinyl caprylate, vinyl caprate, vinyl laurate, vinyl myristate, vinyl palmitate, vinyl stearate, vinyl pivalate, vinyl octylate, divinyl adipate, vinyl methacrylate, vinyl crotonate, vinyl pivalate, vinyl octylate, vinyl benzoate, and vinyl cinnamate. In the esterification reaction with a vinyl carboxylate, one or more catalysts selected from the group consisting of alkali metal hydroxides, alkaline earth metal hydroxides, alkali metal carbonates, alkaline earth metal carbonates, alkali metal hydrogencarbonates, primary to tertiary amines, quaternary ammonium salts, imidazole and derivatives thereof, pyridine and derivatives thereof, and alkoxides may be added.
[0053] Examples of the alkali metal hydroxides and alkaline earth metal hydroxides include sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide, barium hydroxide, etc. Examples of the alkali metal carbonates, alkaline earth metal carbonates, and alkali metal hydrogen carbonates include lithium carbonate, sodium carbonate, potassium carbonate, cesium carbonate, magnesium carbonate, calcium carbonate, barium carbonate, lithium hydrogen carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, cesium hydrogen carbonate, etc.
[0054] The primary, secondary and tertiary amines refer to primary, secondary and tertiary amines, and specific examples thereof include ethylenediamine, diethylamine, proline, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethyl-1,3-propanediamine, N,N,N',N'-tetramethyl-1,6-hexanediamine, tris(3-dimethylaminopropyl)amine, N,N-dimethylcyclohexylamine and triethylamine.
[0055] Examples of imidazole and its derivatives include 1-methylimidazole, 3-aminopropylimidazole, and carbonyldiimidazole.
[0056] Examples of pyridine and its derivatives include N,N-dimethyl-4-aminopyridine and picoline.
[0057] Examples of the alkoxide include sodium methoxide, sodium ethoxide, and potassium t-butoxide.
[0058] The carboxylic acid may be at least one selected from the group consisting of compounds represented by the following formula (1). R-COOH …(1) (In the formula, R represents an alkyl group having 1 to 16 carbon atoms, an alkenyl group having 2 to 16 carbon atoms, a cycloalkyl group having 3 to 16 carbon atoms, or an aryl group having 6 to 16 carbon atoms.)
[0059] Specific examples of carboxylic acids include at least one selected from the group consisting of acetic acid, propionic acid, butyric acid, caproic acid, cyclohexane carboxylic acid, caprylic acid, capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, pivalic acid, methacrylic acid, crotonic acid, pivalic acid, octylic acid, benzoic acid, and cinnamic acid.
[0060] Among these carboxylic acids, at least one selected from the group consisting of acetic acid, propionic acid, and butyric acid, and particularly acetic acid, is preferred from the viewpoint of reaction efficiency. In addition, in the reaction of carboxylic acid, one or more types of acidic compounds such as sulfuric acid, hydrochloric acid, phosphoric acid, etc., or Lewis acids (for example, Lewis acid compounds represented by MYn, where M represents a semimetal element such as B, As, Ge, etc., or a base metal element such as Al, Bi, In, etc., or a transition metal element such as Ti, Zn, Cu, etc., or a lanthanoid element, n is an integer corresponding to the atomic valence of M and represents 2 or 3, and Y represents a halogen atom, OAc, OCOCF3, ClO4, SbF6, PF6, or OSO2CF3(OTf)), or alkaline compounds such as triethylamine, pyridine, etc. may be added as a catalyst.
[0061] Among these esterification reactants, at least one selected from the group consisting of acetic anhydride, propionic anhydride, butyric anhydride, vinyl acetate, vinyl propionate, vinyl butyrate, and acetic acid, and among these, acetic anhydride and vinyl acetate are preferred from the viewpoint of reaction efficiency.
[0062] The degree of modification of the chemically modified cellulose fine fibers of this embodiment is expressed as the average degree of substitution of hydroxyl groups (also referred to as DS, the average number of hydroxyl groups substituted per glucose, which is the basic structural unit of cellulose). In one aspect, the DS of the chemically modified cellulose fine fibers is preferably 0.01 or more and 2.0 or less. If the DS is 0.01 or more, a composite molded body containing chemically modified fine cellulose with a high thermal decomposition onset temperature can be obtained. On the other hand, if the DS is 2.0 or less, an unmodified cellulose skeleton remains in the chemically modified fine cellulose, so that a composite molded body containing chemically modified fine cellulose having both high tensile strength and dimensional stability derived from cellulose and high thermal decomposition onset temperature derived from chemical modification can be obtained. The DS is more preferably 0.05 or more, or 0.1 or more, or 0.2 or more, or 0.3 or more, and more preferably 1.8 or less, or 1.5 or less, or 1.2 or less, or 1.0 or less.
[0063] When the modifying group of the chemically modified cellulose fine fiber is an acyl group, the degree of acyl substitution (DS) can be calculated from the peak intensity ratio of the peak derived from the acyl group to the peak derived from the cellulose skeleton from the reflection type infrared absorption spectrum of the esterified cellulose fine fiber. The peak of the absorption band of C=O based on the acyl group is at 1730 cm -1 The absorption band of CO based on the cellulose backbone appears at 1030 cm -1 The DS of esterified cellulose fine fibers was calculated by plotting a correlation graph between the DS obtained from solid-state NMR measurements of esterified cellulose fine fibers (described later) and the modification ratio (IR index 1030), which is defined as the ratio of the peak intensity of the absorption band of C=O based on the acyl group to the peak intensity of the absorption band of CO in the cellulose backbone chain, and then calculating the calibration curve from the correlation graph. Degree of substitution DS = 4.13 × IR index (1030) It can be found by using
[0064] The method for calculating the DS of esterified cellulose microfibers using solid-state NMR is as follows: 13 C solid-state NMR measurement was performed, and the intensity can be calculated using the area intensity (Inf) of a signal assigned to one carbon atom derived from the modifying group relative to the total area intensity (Inp) of signals assigned to carbons C1-C6 derived from the pyranose ring of cellulose, which appear in the range from 50 ppm to 110 ppm, using the following formula. DS = (Inf) x 6 / (Inp) For example, when the modifying group is an acetyl group, the signal at 23 ppm assigned to -CH3 may be used. Use 13 The conditions for the C solid-state NMR measurement are, for example, as follows: Equipment:Bruker Biospin Avance500WB Frequency: 125.77MHz Measurement method: DD / MAS method Waiting time: 75sec NMR sample tube: 4mmφ Accumulation times: 640 times (approx. 14 hours) MAS: 14,500Hz Chemical shift reference: glycine (external reference: 176.03 ppm)
[0065] The DS heterogeneity ratio (DSs / DSt), defined as the ratio of the degree of modification (DSs) of the fiber surface to the degree of modification (DSt) of the entire fiber of the chemically modified cellulose fine fiber (which is synonymous with the above-mentioned degree of acyl substitution (DS)), is preferably 1.05 or more. The larger the value of the DS heterogeneity ratio, the more pronounced the heterogeneous structure resembling a sheath-core structure (i.e., a structure in which the fiber surface layer is highly chemically modified while the fiber center maintains a structure close to the original unmodified cellulose structure), and while having high tensile strength and dimensional stability derived from cellulose, it is possible to improve the affinity with other components (organic fillers, resins, etc.) when composited with the other components, and to improve the dimensional stability of composite molded bodies. The DS heterogeneity ratio is more preferably 1.1 or more, or 1.2 or more, or 1.3 or more, or 1.5 or more, or 2.0 or more, and from the viewpoint of ease of production of the chemically modified cellulose fine fiber, is preferably 30 or less, or 20 or less, or 10 or less, or 6 or less, or 4 or less, or 3 or less. The value of DSs varies depending on the degree of modification of the esterified cellulose, but for example, it is preferably 0.1 or more, or 0.2 or more, or 0.3 or more, or 0.5 or more, and preferably 3.0 or less, or 2.5 or less, or 2.0 or less, or 1.5 or less, or 1.2 or less, or 1.0 or less. The preferred range of DSt is as described above for the acyl substituent (DS).
[0066] The smaller the coefficient of variation (CV) of the DS heterogeneity ratio of the chemically modified cellulose fine fibers, the smaller the variation in various physical properties of the composite molded body, and therefore the more preferable it is. The coefficient of variation is preferably 50% or less, or 40% or less, or 30% or less, or 20% or less. For example, the coefficient of variation can be further reduced in a method in which a cellulose raw material is defibrated and then chemically modified to obtain chemically modified cellulose fine fibers (i.e., a sequential method), whereas it can be increased in a method in which defibration and chemical modification of the cellulose raw material are performed simultaneously (i.e., a simultaneous method). Although the mechanism of this action is not clear, it is considered that in the simultaneous method, chemical modification is more likely to proceed in the thin fibers generated in the early stage of defibration, and when hydrogen bonds between cellulose microfibrils are reduced by chemical modification, defibration proceeds further, resulting in an increase in the coefficient of variation of the DS heterogeneity ratio.
[0067] The coefficient of variation (CV) of the DS heterogeneity ratio is calculated by taking 100 g of an aqueous dispersion of chemically modified cellulose fine fiber (solid content of 10 mass% or more) and freeze-pulverizing 10 g each to prepare measurement samples, calculating the DS heterogeneity ratio from the DSt and DSs of the 10 samples, and then using the standard deviation (σ) and arithmetic mean (μ) of the DS heterogeneity ratio among the obtained 10 samples, using the following formula. DS heterogeneity ratio = DSs / DSt Coefficient of variation (%) = standard deviation σ / arithmetic mean μ × 100
[0068] The DSs is calculated as follows. That is, the esterified cellulose powdered by freeze-pulverization is placed on a dish-shaped sample stage with a diameter of 2.5 mm, the surface is pressed down to make it flat, and then measurement is performed by X-ray photoelectron spectroscopy (XPS). The XPS spectrum reflects the constituent elements and chemical bond state of only the surface layer of the sample (typically about a few nm). Peak separation is performed on the obtained C1s spectrum, and DSs can be calculated by the following formula based on the area intensity (Ixf) of the peak assigned to one carbon atom derived from the modifying group relative to the area intensity (Ixp) of the peak (289 eV, CC bond) assigned to carbons C2-C6 derived from the pyranose ring of cellulose. DSs = (Ixf) x 5 / (Ixp) For example, if the modifying group is an acetyl group, after peak separation of the C1s spectrum at 285 eV, 286 eV, 288 eV, and 289 eV, the peak at 289 eV can be used for Ixp and the peak derived from the O-C=O bond of the acetyl group (286 eV) can be used for Ixf. The conditions for the XPS measurement are as follows, for example: Equipment used: ULVAC-Phi VersaProbe II Excitation source: mono.AlKα 15kV×3.33mA Analysis size: Approx. 200 μm φ Photoelectron extraction angle: 45° Capture Area Narrow scan: C 1s, O 1s Pass Energy: 23.5eV
[0069] In one embodiment, a mixture of non-chemically modified cellulose fine fibers and the above-mentioned chemically modified cellulose fine fibers can be used. When such a mixture is used, the above-mentioned value of the degree of substitution may be the value of only the chemically modified cellulose fine fibers in one embodiment, or may be the average value of the entire mixture in one embodiment.
[0070] <Organic filler> The composite molded body of the present embodiment includes an organic filler in addition to the cellulose fine fibers. The organic filler of the present disclosure is a component different from the cellulose fine fibers, and in one embodiment is cut fibers, irregular particles, or spherical particles, or a mixture of two or more of these. The average minor axis diameter of the organic filler is 0.1 μm or more in one embodiment, preferably 0.3 μm or more, or 0.5 μm or more, or 1.0 μm or more in one embodiment. The average minor axis diameter is 100 μm or less in one embodiment, preferably 80 μm or less, or 60 μm or less. The average minor axis diameters of the cut fibers, irregular particles, and spherical particles as the organic filler are defined as described below.
[0071] The organic filler may be obtained by recycling in terms of effective use of waste. Recycling here refers to material recycling or chemical recycling. For example, cut fibers made of polyethylene terephthalate obtained by recycling PET bottles, amorphous particles obtained by recovering and pulverizing foams used as industrial materials such as building materials, etc. can be used.
[0072] In one embodiment, the organic filler may be composed of a thermoplastic resin. The thermoplastic resin preferably includes at least one selected from the group consisting of polyolefin, polyester, polyamide, acrylic polymer, polyvinyl alcohol, polylactic acid, polyphenylene ether, polyoxymethylene, and polyphenylene sulfide. More specific examples of the thermoplastic resin will be described later for each of cut fibers, irregular particles, and spherical particles.
[0073] The melting point of the thermoplastic resin is preferably 50° C. or higher, or 100° C. or higher, or 140° C. or higher from the viewpoint of imparting good properties to the composite molded body, and is preferably 500° C. or lower, or 400° C. or lower, or 280° C. or lower, or 230° C. or lower from the viewpoint of ease of production of the composite molded body. Note that the melting point in the present disclosure refers to the peak top temperature of the endothermic peak (when multiple endothermic peaks appear, the endothermic peak on the highest temperature side) measured using a differential scanning calorimeter at a heating rate of 10° C. / min.
[0074] [Cut fiber] In one embodiment, the cut fibers have an average fiber length of 20 mm or less. The cut fibers may preferably be fibrillated cut fibers. Examples of fibrillated cut fibers include fibrillated fibers obtained by fibrillating fibers cut after spinning by beating treatment, and fibrillated fibers obtained by spinning fibers having a multi-branched structure obtained by spinning by flash spinning or electrospinning, and then cutting the fibers.
[0075] When the organic filler is cut fibers, the average minor axis diameter means the average fiber diameter of the cut fibers. The average fiber diameter of the cut fibers is preferably 0.1 μm or more, or 0.3 μm or more, or 1.0 μm or more from the viewpoint of availability of the cut fibers, and is preferably 50 μm or less, or 40 μm or less, or 25 μm or less from the viewpoint of uniform blending with cellulose fine fibers and easy formation of a homogeneous composite molded body. When the cut fibers have a relatively small average fiber diameter (for example, 10 μm or less), the difference in fiber diameter between the cellulose fine fibers and the cut fibers is small, so the air resistance variation coefficient is low and the uniformity of the structure within the composite molded body is good. On the other hand, when the cut fibers have a relatively large average fiber diameter (for example, more than 40 μm), the difference in fiber diameter between the cellulose fine fibers and the cut fibers is large, and there is a tendency for the structure within the composite molded body to vary widely, but the composite molded body of the present disclosure has a high basis weight and can exhibit a sufficiently low air resistance variation coefficient.
[0076] From the viewpoint of obtaining a composite molded body having good mechanical properties, the average fiber length of the cut fibers is preferably 0.5 mm or more, or 1.0 mm or more, or 1.5 mm or more, and from the viewpoint of facilitating uniform dispersion of the cellulose fine fibers among the cut fibers, the average fiber length is preferably 20 mm or less, or 15 mm or less, or 10 mm or less.
[0077] The average fiber diameter and average fiber length of the cut fibers are determined by measuring the cut fibers with an optical microscope. Specifically, the fiber diameter and fiber length of 20 randomly selected cut fibers are measured in an observation field in which the magnification is adjusted so that at least 20 cut fibers are observed, and the number average of the 20 fibers is calculated as the average fiber diameter and average fiber length. When the cut fibers are fibrillated fibers, the fiber diameter is defined as the maximum fiber diameter among all the trunk fibers and branch fibers that can be confirmed for each fibrillated fiber when observed with an optical microscope in a state in which the fibers are broken apart by a dry grinding process, and the number average of at least 20 (20 in one embodiment) fibrillated fibers is defined as the average fiber diameter. Similarly, when the cut fibers are fibrillated fibers, the fiber length is defined as the length of the trunk fiber having the maximum fiber diameter in the irregular shape of each fibrillated fiber when observed with an optical microscope in a state in which the fibers are broken apart by a dry grinding process, and the average fiber length is defined as the number average value for at least 20 fibrillated fibers (20 in one embodiment). When the fiber diameter or fiber length of the cut fibers is difficult to measure with the above-mentioned optical microscope due to resolution issues, a scanning electron microscope (SEM) may be used.
[0078] As the cut fibers, any of natural fibers, synthetic fibers, and semi-synthetic fibers can be used. Examples of polymers constituting the cut fibers include thermoplastic resins such as polyolefins, polyesters, polyamides (aromatic or aliphatic), acrylic polymers, polyvinyl alcohol, polylactic acid, polyphenylene ether, polyoxymethylene, and polyphenylene sulfide, and thermosetting resins such as epoxy resins, thermosetting modified polyphenylene ether resins, thermosetting polyimide resins, urea resins, allyl resins, silicon resins, benzoxazine resins, phenolic resins, unsaturated polyester resins, bismaleimide triazine resins, alkyd resins, furan resins, melamine resins, polyurethane resins, and aniline resins. In a preferred embodiment, the cut fibers are composed of a thermoplastic resin. In a preferred embodiment, the thermoplastic resin includes at least one selected from the group consisting of polyolefin (polyethylene, polypropylene, etc.), polyester (polyethylene terephthalate, etc.), polyamide (PA6, PA66, PA4, PA12, aromatic polyamide, etc.), polyacrylonitrile, polymethyl methacrylate, polystyrene, polyvinyl alcohol, polylactic acid, polyphenylene ether, polyoxymethylene, and polyphenylene sulfide. Preferred polymers are polyamide, polyester, polyoxymethylene, polylactic acid, polyacrylonitrile, etc., because they have high affinity with cellulose fine fibers and are easy to mix uniformly. Polyphenylene sulfide, polyphenylene ether, polyester, aromatic polyamide, etc. are suitable for applications requiring heat resistance. When the cut fibers include a thermoplastic resin, the composite molded product may be heated (for example, melt press, etc.) to melt a part or all of the thermoplastic resin, and then solidified to form a resin molded product described below. The thermoplastic resin can be impregnated between the cellulose fine fibers by such melting and solidification. The cut fibers in such a resin molded product (i.e., the heat-treated composite molded product) may still retain a fibrous shape in one embodiment, or may not retain a fibrous shape in one embodiment. The melting point of the thermoplastic resin may be preferably 50° C. or higher, or 100° C. or higher, or 140° C. or higher, and may be preferably 500° C. or lower, or 400° C. or lower, or 280° C. or lower.
[0079] [Irregular shaped particles and spherical particles] (irregular particles) In one embodiment, the irregular particles have an average minor axis diameter of 100 μm or less. The irregular particles may be irregular particles obtained by, for example, pulverizing a foam-like molded body. When the organic filler is an irregular particle, the average minor axis diameter is determined by observing the irregular particles with an optical microscope, approximating each irregular particle with an ellipse that completely fits the outer periphery of the particle and has the smallest area, defining the minor axis diameter of the ellipse as the minor axis diameter of the particle, and defining the number average value of the minor axis diameters of at least 20 particles (20 in one embodiment) as the average minor axis diameter of the irregular particles. Similarly, the outer periphery of each irregular particle is approximated with an ellipse that completely fits the outer periphery of the particle and has the smallest area, defining the major axis diameter of the ellipse as the major axis diameter of the particle, and defining the number average value of the major axis diameters of at least 20 particles (20 in one embodiment) as the average major axis diameter of the irregular particles.
[0080] The average minor axis diameter of the irregular particles is preferably 0.1 μm or more, or 0.3 μm or more, or 1.0 μm or more from the viewpoint of increasing the thickness dimension of the composite molded body, and is preferably 100 μm or less, or 80 μm or less, or 60 μm or less from the viewpoint of uniform blending with the cellulose fine fibers and facilitating the formation of a homogeneous composite molded body. When the irregular particles have a relatively small average minor axis diameter (for example, 10 μm or less), the difference in the minor axis diameter between the cellulose fine fibers and the irregular particles is small, so that the coefficient of variation of air resistance is low and the uniformity of the structure within the composite molded body is good. On the other hand, when the irregular particles have a relatively large average minor axis diameter (for example, more than 50 μm), a composite molded body with a larger thickness dimension is obtained. When the difference in minor axis diameter between the cellulose fine fibers and the irregular particles is large, the structural variation within the composite molded body tends to become greater; however, the composite molded body of the present disclosure has a high basis weight and can exhibit a sufficiently low coefficient of variation of air resistance.
[0081] The average major axis diameter of the irregular particles is preferably 0.2 μm or more, or 0.6 μm or more, or 2.0 μm or more from the viewpoint of obtaining a composite molded body with a large thickness dimension, and is preferably 500 μm or less, or 250 μm or less, or 100 μm or less from the viewpoint of obtaining a composite molded body with good mechanical properties.
[0082] In measuring the average minor axis diameter and the average major axis diameter of irregular particles, when measurement by the above-mentioned optical microscope is difficult due to resolution problems, a scanning electron microscope (SEM) may be used.
[0083] (spherical particles) In one embodiment, the spherical particles have an average minor axis diameter of 50 μm or less. When the organic filler is a spherical particle, the average minor axis diameter refers to the average particle diameter of the spherical particles.
[0084] The average particle diameter of the spherical particles is preferably 0.1 μm or more, or 0.3 μm or more, or 1.0 μm or more from the viewpoint of increasing the thickness dimension of the composite molded body, and is preferably 50 μm or less, or 40 μm or less, or 25 μm or less from the viewpoint of uniform blending with cellulose fine fibers and facilitating the formation of a homogeneous composite molded body. When the spherical particles have a relatively small average particle diameter (for example, 10 μm or less), the difference in diameter between the cellulose fine fibers and the spherical particles is small, so that the coefficient of variation of air resistance is low and the uniformity of the structure within the composite molded body is good. On the other hand, when the spherical particles have a relatively large average particle diameter (for example, more than 25 μm), a composite molded body with a larger thickness dimension is obtained. When the difference in diameter between the cellulose fine fibers and the spherical particles is large, the structure within the composite molded body tends to vary more, but the composite molded body of the present disclosure has a high basis weight and can exhibit a sufficiently low coefficient of variation of air resistance.
[0085] The average particle size of spherical particles is determined by measuring the spherical particles with an optical microscope. Specifically, the particle sizes of 20 randomly selected spherical particles are measured in an observation field where the magnification is adjusted so that at least 20 spherical particles are observed, and the number average value of the 20 particles is calculated as the average particle size. If it is difficult to measure with the optical microscope due to resolution issues, a scanning electron microscope (SEM) may be used.
[0086] (Materials for forming irregular particles and spherical particles) For each of the amorphous particles and the spherical particles, for example, naturally occurring or synthetic polymer particles can be used. For each of the amorphous particles and the spherical particles, the polymers constituting the amorphous particles and the spherical particles can be exemplified by thermoplastic resins and thermosetting resins, and more specifically, can be exemplified by naturally occurring polymers such as cellulose and cellulose derivatives, thermoplastic resins such as polyolefins, polyesters, polyamides (aromatic or aliphatic), acrylic polymers, polyvinyl alcohols, polylactic acids, polyphenylene ethers, polyoxymethylenes, and polyphenylene sulfides, thermosetting resins such as epoxy resins, thermosetting modified polyphenylene ether resins, thermosetting polyimide resins, urea resins, allyl resins, silicon resins, benzoxazine resins, phenolic resins, unsaturated polyester resins, bismaleimide triazine resins, alkyd resins, furan resins, melamine resins, polyurethane resins, and aniline resins. When the amorphous particles and / or the spherical particles contain a thermoplastic resin, the composite molded body may be heated (e.g., melt-pressed, etc.) to melt a part or all of the thermoplastic resin, and then solidified to form a resin molded body described below. Such melting and solidification can impregnate the thermoplastic resin between the cellulose fine fibers. In one embodiment, each of the amorphous particles and the spherical particles in such a resin molded body (i.e., the heat-treated composite molded body) may still retain a particle shape, or may not retain a particle shape in one embodiment. The melting point of the thermoplastic resin may be preferably 50°C or higher, or 100°C or higher, or 140°C or higher, and may be preferably 500°C or lower, or 400°C or lower, or 280°C or lower.
[0087] In one aspect, the mass ratio of the cellulose fine fibers to the total mass of the cellulose fine fibers and the organic filler in the composite molded body may be, from the viewpoint of obtaining the advantages of using the cellulose fine fibers, preferably 9 mass% or more, or 15 mass% or more, or 26 mass% or more, and from the viewpoint of ease of manufacturing the composite molded body, preferably 93 mass% or less, or 88 mass% or less, or 84 mass%.
[0088] The total mass of the cellulose fine fibers and the organic filler in the composite molding may be, in one embodiment, 80% by mass or more, or 85% by mass or more, or 90% by mass or more, and in one embodiment, 100% by mass or less, or 99% by mass or less, or 98% by mass or less.
[0089] <Crosslinking agent and crosslinking structure> In one embodiment, the reactants derived from the crosslinking agent are distributed between the cellulose fine fibers, between the organic fillers, and / or between the cellulose fine fibers and the organic fillers in the composite molded body. By using the crosslinking agent, the mechanical properties of the composite molded body and various members formed using the same can be significantly improved. In addition, the cellulose fine fibers are essentially hydrophilic, and the composite molded body can be hydrophobized by crosslinking the hydroxyl groups of the cellulose molecules, and the composite molded body can be suitably used in member applications requiring water resistance. Furthermore, hydrophobization of the composite molded body may also provide the advantage of improving the resin impregnation into the composite molded body. The crosslinking mode can be selected according to the functional groups possessed by each of the cellulose fine fibers and the organic filler. In view of good reactivity with the hydroxyl groups possessed by cellulose and excellent crosslinking effect, urethane bonds, ether bonds, ester bonds, amide bonds, silyl ether bonds, etc. are preferred, and urethane bonds are particularly preferred. Therefore, in a preferred embodiment, the reactants derived from the crosslinking agent include the bonds exemplified above. The crosslinking agent is preferably a reactive crosslinking agent such as blocked polyisocyanate, polyisocyanate, epichlorohydrin, formaldehyde, etc. Blocked polyisocyanate is preferred because it has a particularly good crosslinking effect on cellulose fine fibers.
[0090] Blocked polyisocyanates are compounds having a structure in which the isocyanate groups of polyisocyanates (i.e., polyfunctional compounds having two or more isocyanate groups per molecule) are blocked with blocking groups, and while they are substantially non-reactive at room temperature (specifically, below 30°C), they generate two or more free isocyanate groups per molecule at temperatures above the blocking group elimination temperature, and form a crosslinked structure by reaction with a functional group reactive with the isocyanate group (e.g., a functional group having active hydrogen). Cellulose fine fibers have hydroxyl groups, which are functional groups reactive with isocyanate groups, but since blocked polyisocyanates retain blocking groups, they do not react with cellulose fine fibers and are adsorbed to the cellulose fine fibers, functioning as a dispersant for the cellulose fine fibers and contributing to uniform dispersion of the cellulose fine fibers among the organic fillers. In the solidification process, when the mixture is heated to a temperature equal to or higher than the desorption temperature of the blocking group, the polyisocyanates and the cellulose fine fibers and the polyisocyanate are chemically bonded to each other to form crosslinked structures between the polyisocyanate and the polyisocyanate and between the polyisocyanate and the cellulose fine fibers. When the organic filler has a functional group having active hydrogen, a crosslinked structure between the polyisocyanate and the organic filler is also formed. Due to the crosslinked structure formed by the use of the blocked polyisocyanate, the cellulose fine fibers form a stable three-dimensional network while maintaining their fine structure in the composite molded body (i.e., while preventing aggregation of the cellulose fine fibers), and furthermore, the composite molded body is made water-resistant by the reduction of hydroxyl groups (due to the reaction with the isocyanate groups), so that the physical properties of the composite molded body can be improved more significantly.
[0091] In the crosslinked composite molded body, the cellulose fine fibers and / or organic filler are not only simply dispersed but also form a three-dimensional network by a crosslinked structure derived from the blocked polyisocyanate. Such a composite molded body can be molded into a desired shape and has good mechanical strength, water resistance, and solvent resistance. Therefore, the composite molded body can be used to form members of various shapes (for example, curved molded bodies, box-shaped molded bodies, cone-shaped molded bodies, etc.).
[0092] The blocked polyisocyanate is selected from compounds obtained by substituting the isocyanate group of a polyisocyanate (i.e., a compound having two or more isocyanate groups in a molecule) with a blocking group. Examples of the basic skeleton of the polyisocyanate include aromatic polyisocyanate, alicyclic polyisocyanate, and aliphatic polyisocyanate. Among them, alicyclic polyisocyanate and aliphatic polyisocyanate are more preferable from the viewpoint of less yellowing.
[0093] Examples of aromatic polyisocyanates include aromatic diisocyanates such as 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate and mixtures thereof (TDI), diphenylmethane-4,4'-diisocyanate (MDI), naphthalene-1,5-diisocyanate, 3,3-dimethyl-4,4-biphenylene diisocyanate, crude TDI, polymethylene polyphenyl diisocyanate, crude MDI, phenylene diisocyanate, and xylylene diisocyanate. Examples of the alicyclic polyisocyanate include alicyclic diisocyanates such as 1,3-cyclopentane diisocyanate, 1,3-cyclopentene diisocyanate, and cyclohexane diisocyanate. Examples of the aliphatic polyisocyanate include aliphatic diisocyanates such as trimethylene diisocyanate, 1,2-propylene diisocyanate, butylene diisocyanate, pentamethylene diisocyanate, and hexamethylene diisocyanate.
[0094] Examples of polyisocyanate derivatives as the basic skeleton of the blocked polyisocyanate include the above-mentioned polyisocyanate polymers (e.g., dimers, trimers, pentamers, heptamers, etc.) as well as reaction products obtained by reacting one or more active hydrogen-containing compounds. Examples of the reaction products include allophanate modified products (e.g., allophanate modified products produced by the reaction of polyisocyanate with alcohols), polyol modified products (e.g., polyol modified products (alcohol adducts) produced by the reaction of polyisocyanate with alcohols), biuret modified products (e.g., biuret modified products produced by the reaction of polyisocyanate with water or amines), urea modified products (e.g., urea modified products produced by the reaction of polyisocyanate with diamines), oxadiazinetrione modified products (e.g., oxadiazinetrione produced by the reaction of polyisocyanate with carbon dioxide), carbodiimide modified products (carbodiimide modified products produced by decarboxylation condensation reaction of polyisocyanate), uretdione modified products, uretonimine modified products, and the like.
[0095] Examples of active hydrogen-containing compounds include monovalent to hexavalent hydroxyl group-containing compounds (e.g., polyester polyols, polyether polyols, etc.), amino group-containing compounds, thiol group-containing compounds, carboxyl group-containing compounds, etc. Water, carbon dioxide, etc. present in the air or in the reaction site can also be active hydrogen-containing compounds.
[0096] Examples of the monohydric to hexahydric alcohol include non-polymerized alcohol and polymerized alcohol. The non-polymerized alcohol is an alcohol that has not undergone polymerization, and the polymerized alcohol is an alcohol obtained by polymerizing a monomer.
[0097] Examples of non-polymerized alcohols include monoalcohols, diols, triols, tetraols, etc. Examples of monoalcohols include, but are not limited to, methanol, ethanol, n-propanol, i-propanol, n-butanol, i-butanol, s-butanol, n-pentanol, n-hexanol, n-octanol, n-nonanol, 2-ethylbutanol, 2,2-dimethylhexanol, 2-ethylhexanol, cyclohexanol, methylcyclohexanol, and ethylcyclohexanol. The diols are not particularly limited, but examples thereof include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 2-methyl-1,2-propanediol, 1,5-pentanediol, 2-methyl-2,3-butanediol, 1,6-hexanediol, 1, Examples of the triols include, but are not limited to, 2-hexanediol, 2,5-hexanediol, 2-methyl-2,4-pentanediol, 2,3-dimethyl-2,3-butanediol, 2-ethyl-hexanediol, 1,2-octanediol, 1,2-decanediol, 2,2,4-trimethylpentanediol, 2-butyl-2-ethyl-1,3-propanediol, 2,2-diethyl-1,3-propanediol, phloroglucin, pyrogallol, catechol, hydroquinone, bisphenol A, bisphenol F, and bisphenol S. Examples of the triols include, but are not limited to, glycerin, trimethylolpropane, and the like. Examples of the tetraols include, but are not limited to, pentaerythritol, 1,3,6,8-tetrahydroxynaphthalene, and 1,4,5,8-tetrahydroxyanthracene.
[0098] The polymerized alcohol is not particularly limited, but examples thereof include polyols such as polyester polyols, polyether polyols, acrylic polyols, and polyolefin polyols.
[0099] The polyester polyol is not particularly limited, but examples thereof include polyester polyols obtained by a condensation reaction of a dicarboxylic acid, such as succinic acid, adipic acid, sebacic acid, dimer acid, maleic anhydride, phthalic anhydride, isophthalic acid, or terephthalic acid, alone or in a mixture, with a polyhydric alcohol, such as ethylene glycol, propylene glycol, diethylene glycol, neopentyl glycol, trimethylolpropane, or glycerin, alone or in a mixture; and polycaprolactones obtained by ring-opening polymerization of ε-caprolactone using a polyhydric alcohol.
[0100] The polyether polyol is not particularly limited, but examples thereof include polyether polyols obtained by randomly or block-adding a single or mixture of alkylene oxides such as ethylene oxide, propylene oxide, butylene oxide, cyclohexene oxide, and styrene oxide to a single or mixture of polyvalent hydroxy compounds using hydroxides of lithium, sodium, potassium, etc., alcoholates, strong basic catalysts such as alkylamines, metal porphyrins, and composite metal cyanide complexes such as zinc hexacyanocobaltate complexes, and polyether polyols obtained by reacting alkylene oxides with polyamine compounds such as ethylenediamines. Also included are so-called polymer polyols obtained by polymerizing acrylamide or the like using these polyethers as a medium.
[0101] The polyhydric alcohol compound may be (1) For example, diglycerin, ditrimethylolpropane, pentaerythritol, dipentaerythritol, etc. (2) Sugar alcohol compounds, such as erythritol, D-threitol, L-arabinitol, ribitol, xylitol, sorbitol, mannitol, galactitol, and rhamnitol; (3) Monosaccharides, such as arabinose, ribose, xylose, glucose, mannose, galactose, fructose, sorbose, rhamnose, fucose, and ribosaccharides; (4) Disaccharides such as trehalose, sucrose, maltose, cellobiose, gentiobiose, lactose, and melibiose; (5) Trisaccharides such as raffinose, gentianose, melezitose, etc. (6) Tetrasaccharides, such as stachyose, etc.
[0102] Examples of acrylic polyols include acrylic esters having active hydrogen, such as 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, and 2-hydroxybutyl acrylate; monoesters of glycerin or methacrylic acid; monoesters of trimethylolpropane or methacrylic acid; and methacrylic esters having active hydrogen, such as 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 2-hydroxybutyl methacrylate, 3-hydroxypropyl methacrylate, and 4-hydroxybutyl methacrylate. The acrylic polyols include acrylic esters having active hydrogen, such as methyl acrylate, ethyl acrylate, isopropyl acrylate, n-butyl acrylate, and 2-ethylhexyl acrylate. Examples of the acrylic polyol include methacrylic acid esters such as methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-hexyl methacrylate, and lauryl methacrylate; unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, and itaconic acid; unsaturated amides such as acrylamide, N-methylolacrylamide, and diacetone acrylamide; and vinyl monomers having a hydrolyzable silyl group such as glycidyl methacrylate, styrene, vinyl toluene, vinyl acetate, acrylonitrile, dibutyl fumarate, vinyl trimethoxysilane, vinyl methyl dimethoxysilane, and γ-methacryloxypropyl methoxysilane.
[0103] Examples of polyolefin polyols include polybutadiene having two or more hydroxyl groups, hydrogenated polybutadiene, polyisoprene, hydrogenated polyisoprene, etc. Furthermore, monoalcohol compounds having 50 or less carbon atoms, such as isobutanol, n-butanol, and 2-ethylhexanol, can be used in combination.
[0104] Examples of the amino group-containing compound include monohydrocarbylamines having 1 to 20 carbon atoms [alkylamines (butylamine, etc.), benzylamine, aniline, etc.], aliphatic polyamines having 2 to 20 carbon atoms (ethylenediamine, hexamethylenediamine, diethylenetriamine, etc.), alicyclic polyamines having 6 to 20 carbon atoms (diaminocyclohexane, dicyclohexylmethanediamine, isophoronediamine, etc.), aromatic polyamines having 2 to 20 carbon atoms (phenylenediamine, tolylenediamine, diphenylmethanediamine, etc.), and aromatic polyamines having 2 to 20 carbon atoms (phenylenediamine, tolylenediamine, diphenylmethanediamine, etc.). Examples of the heterocyclic polyamines include 20 heterocyclic polyamines (piperazine and N-aminoethylpiperazine, etc.), alkanolamines (monoethanolamine, diethanolamine, triethanolamine, etc.), polyamidepolyamines obtained by condensation of dicarboxylic acids with an excess of polyamines, polyetherpolyamines, hydrazines (hydrazine and monoalkylhydrazine, etc.), dihydrazides (succinic acid dihydrazide and terephthalic acid dihydrazide, etc.), guanidines (butylguanidine and 1-cyanoguanidine, etc.), and dicyandiamide.
[0105] Examples of thiol group-containing compounds include monovalent thiol compounds having 1 to 20 carbon atoms (alkylthiols such as ethylthiol, phenylthiol, and benzylthiol) and polyvalent thiol compounds (ethylenedithiol, 1,6-hexanedithiol, and the like).
[0106] Examples of the carboxyl group-containing compound include monovalent carboxylic acid compounds (alkyl carboxylic acids such as acetic acid, aromatic carboxylic acids such as benzoic acid) and polyvalent carboxylic acid compounds (alkyl dicarboxylic acids such as oxalic acid and malonic acid, aromatic dicarboxylic acids such as terephthalic acid, etc.).
[0107] The blocking group is added to the isocyanate group of the polyisocyanate compound to block it. This blocking group is stable at room temperature, but when heated to a specific desorption temperature (usually about 100 to about 200° C.), the blocking group is desorbed and the free isocyanate group can be regenerated.
[0108] Examples of blocking agents that provide blocking groups that satisfy these requirements include (1) Alcohols such as methanol, ethanol, 2-propanol, n-butanol, sec-butanol, 2-ethyl-1-hexanol, 2-methoxyethanol, 2-ethoxyethanol, and 2-butoxyethanol; (2) Alkylphenols: mono- and di-alkylphenols having an alkyl group having 4 or more carbon atoms as a substituent, such as monoalkylphenols such as n-propylphenol, isopropylphenol, n-butylphenol, sec-butylphenol, t-butylphenol, n-hexylphenol, 2-ethylhexylphenol, n-octylphenol, and n-nonylphenol; dialkylphenols such as di-n-propylphenol, diisopropylphenol, isopropyl cresol, di-n-butylphenol, di-t-butylphenol, di-sec-butylphenol, di-n-octylphenol, di-2-ethylhexylphenol, and di-n-nonylphenol; (3) Phenol-based: phenol, cresol, ethylphenol, styrenated phenol, hydroxybenzoic acid ester, etc. (4) Active methylene compounds: dimethyl malonate, diethyl malonate, methyl acetoacetate, ethyl acetoacetate, acetylacetone, etc. (5) Mercaptans: butyl mercaptan, dodecyl mercaptan, etc. (6) Acid amides: acetanilide, acetic acid amide, ε-caprolactam, δ-valerolactam, γ-butyrolactam, etc. (7) Acid imide series: succinimide, maleimide, etc. (8) Imidazoles: imidazole, 2-methylimidazole, 3,5-dimethylpyrazole, 3-methylpyrazole, etc. (9) Urea-based: urea, thiourea, ethyleneurea, etc. (10) Oximes: formaldoxime, acetaldoxime, acetoxime, methyl ethyl ketoxime, cyclohexanone oxime, etc. (11) Amines: diphenylamine, aniline, carbazole, di-n-propylamine, diisopropylamine, isopropylethylamine, etc. These blocking agents can be used alone or in combination of two or more.
[0109] The blocked polyisocyanate may be anionic, nonionic, or cationic, but is preferably a cationic blocked polyisocyanate. The cationic blocked polyisocyanate is advantageous in that it is easily adsorbed to cellulose fine fibers and / or organic fillers by electrostatic interaction. That is, since it is known that the surface of general cellulose fibers is anionic (zeta potential in distilled water is -30 to -20 mV) (Non-Patent Document 1, J. Brandrup (editor) and EH Immergut (editor), "Polymer Handbook 3rd edition", V-153 to V-155), it is preferable in terms of electrostatic interaction that the blocked polyisocyanate is cationic.
[0110] However, even if the blocked polyisocyanate is nonionic, it is possible to favorably adsorb the blocked polyisocyanate onto the cellulose fine fibers and / or organic fillers by adjusting the polymer chain length, rigidity, etc. of the hydrophilic group of the blocked polyisocyanate. Furthermore, even if the blocked polyisocyanate is an anionic blocked polyisocyanate, which is more difficult to adsorb due to electrostatic repulsion with the cellulose fine fibers and / or organic fillers, it is possible to adsorb the blocked polyisocyanate onto the cellulose fine fibers and / or organic fillers by using a generally known cationic adsorption aid or cationic polymer.
[0111] In the composite molded body, the amount of reactants derived from the crosslinking agent is preferably 0.1% by mass or more, or 0.3% by mass or more, or 0.5% by mass or more, or 1% by mass or more, or 3% by mass or more, based on the total of 100% by mass of the cellulose fine fibers and the organic filler, from the viewpoint of obtaining the advantages of using the crosslinking agent well, and from the viewpoint of reducing the amount of unreacted crosslinking agent remaining in the composite molded body and well preventing inconveniences such as crack generation in the member formed using the composite molded body, it is preferably 100% by mass or less, or 90% by mass or less, or 80% by mass or less. The amount of reactants derived from the crosslinking agent can be confirmed by TOF-SIMS (time-of-flight secondary ion mass spectrometry) of the composite molded body.
[0112] In one embodiment, the composite molded body may be an uncrosslinked one that contains a reactive crosslinking agent in a pre-reaction state (for example, as a blocked polyisocyanate). For example, the composite molded body may contain the reactive crosslinking agent in an amount of preferably 0.1% by mass or more, or 0.3% by mass or more, or 0.5% by mass or more, or 1% by mass or more, or 3% by mass or more, based on 100% by mass of the total of the cellulose fine fibers and the organic filler, and may contain the reactive crosslinking agent in an amount of preferably 100% by mass or less, or 90% by mass or less, or 85% by mass or less.
[0113] In one embodiment, the crosslinking agent or a reactant derived therefrom is uniformly distributed in the planar direction of the composite molded body. In this disclosure, "the crosslinking agent or a reactant derived therefrom is uniformly distributed in the planar direction of the composite molded body" is defined as follows. The uniformity in the planar direction means that the ratio (W1 / W2) of the amount of crosslinking agent or reactant derived therefrom (W1) to the amount of cellulose (W2) at any point on the surface of the composite molded body is always constant. Here, "always constant" means that when four areas of 1 cm x 1 cm are selected on the surface of the composite molded body, the variation in W1 / W2 at any four points has a coefficient of variation of 50% or less.
[0114] The coefficient of variation in the planar direction of the distribution of the crosslinking agent or a reactant derived therefrom is preferably 50% or less, or 30% or less, or 20% or less. When the coefficient of variation is 50% or less, the physical properties such as tensile strength (dry and wet) and biodegradability resistance are better than those of a composite molded body containing the same amount of crosslinking agent or a reactant derived therefrom and having a coefficient of variation of more than 50%. The coefficient of variation is a value that represents relative variation and can be calculated by the following formula: coefficient of variation (CV) = (standard deviation / arithmetic mean) x 100. The smaller the coefficient of variation, the more desirable it is, but from the viewpoint of ease of production of the composite molded body, it may be, for example, 1% or more, 2% or more, or 4% or more.
[0115] In the composite molded body, the ratio of the amount of the crosslinking agent or the reactant derived therefrom (W1) to the amount of cellulose (W2) can be obtained, for example, by a three-dimensional composition analysis using TOF-SIMS accompanied by sputter etching. TOF-SIMS can analyze the elemental composition and chemical structure of the extreme surface of a sample. When a primary ion beam is irradiated onto a sample under ultra-high vacuum, secondary ions are emitted from the extreme surface (1-3 nm) of the sample. By introducing the secondary ions into a time-of-flight (TOF) mass spectrometer, a mass spectrum of the extreme surface of the sample can be obtained. By keeping the amount of primary ion irradiation low, the surface components can be detected as molecular ions that maintain their chemical structure and partially cleaved fragments, and information on the elemental composition and chemical structure in the planar direction of the extreme surface can be obtained. In addition, by repeating sputter etching using a sputter etching gun and measurement of secondary ions using a primary ion gun, information on the elemental composition and chemical structure in the depth direction can be obtained, and three-dimensional composition and chemical structure analysis can be performed.
[0116] Calculation of W1 / W2 by TOF-SIMS is performed, for example, as follows. Samples of 0.5 cm square are taken from four equally divided locations in a 1 cm x 1 cm composite molding. 3D TOF-SIMS composition analysis is performed on the four samples. The ratio of the amount of crosslinking agent or reactant derived therefrom to the amount of cellulose can be calculated as W1 / W2=C1 / C2 from the count number (C1) derived from the crosslinking agent or reactant derived therefrom (for example, in the case of blocked polyisocyanate, the count number of m / z=26 (fragment ion: CN)) and the count number (C2) derived from cellulose of m / z=59 (fragment ion: C2H3O2). For example, CNO (m / z=42) may be used as another fragment ion derived from blocked polyisocyanate or its crosslinked product. Also, for example, C3H3O2 (m / z=71) may be used as another fragment ion derived from cellulose. The observed fragment ions may differ depending on the composition of the crosslinking agent, the raw material of the cellulose, etc., and are not limited to the above fragment ions. The measurement conditions of the TOF-SIMS used are, for example, as follows.
[0117] (Measurement conditions) Equipment used: nanoTOF (ULVAC-PHI) Primary ion: Bi3 ++ Accelerating voltage: 30 kV Ion current: Approx. 0.1nA (as DC) Analysis area: 200μm×200μm Analysis time: approx. 6sec / cycle Detected ions: negative ions Neutralization: Using an electron gun (Sputtering conditions) Sputter ion: Ar2500 + Accelerating voltage: 20kV Ion current: approx. 5nA Sputtering area: 500μm×500μm Sputtering time: 60sec / cycle Neutralization: Using an electron gun
[0118] <Additional Ingredients> The composite molded body may contain, in addition to the above-mentioned cellulose fine fibers, organic filler, and any reactive crosslinking agent or its reactant, additional components such as a dispersant, inorganic filler particles, additional fibers (fibers other than the cellulose fine fibers and cut fibers of the present disclosure), and a functionalizing agent.
[0119] (Dispersant) The dispersant can improve the mechanical properties and thermal stability of the composite molded body by improving and controlling the dispersion state of the cellulose fine fibers and the organic filler in the composite molded body. The mass ratio of the dispersant to the total mass of the composite molded body may be preferably 0.01 mass% or more, or 0.05 mass% or more, or 0.1 mass% or more, or 0.5 mass% or more, or 1 mass% or more from the viewpoint of obtaining a good effect of improving the mechanical properties and thermal stability of the composite molded body, and may be preferably 20 mass% or less, or 10 mass% or less, or 5 mass% or less, or 3 mass% or less from the viewpoint of good exertion of the desired properties of the cellulose fine fibers and the organic filler in the composite molded body.
[0120] As the dispersant, a surfactant is suitable. The surfactant may have a chemical structure in which a portion having a hydrophilic substituent and a portion having a hydrophobic substituent are covalently bonded, and examples of the surfactant include anionic surfactants such as alkyl sulfate ester salts, polyoxyethylene alkyl sulfate ester salts, alkylbenzene sulfonate salts, and α-olefin sulfonate salts; cationic surfactants such as alkyltrimethylammonium chloride, dialkyldimethylammonium chloride, and benzalkonium chloride; amphoteric surfactants such as alkyldimethylaminoacetate betaine and alkylamidedimethylaminoacetate betaine; and nonionic surfactants such as alkylpolyoxyethylene ether and fatty acid glycerol ester. Nonionic surfactants are preferred because they are advantageous for more uniform mixing of cellulose fine fibers and organic fillers.
[0121] In particular, when the organic filler is a hydrophobic resin such as polyolefin, the dispersant acts effectively during the production of the composite molded article.
[0122] Examples of the inorganic filler particles include silica particles, alumina particles, titanium oxide particles, calcium carbonate particles, etc. In the composite molded body, the mass ratio of the inorganic filler particles may be, for example, 1 to 30 mass %, or 3 to 20 mass %.
[0123] Examples of the additional fibers that can be used include inorganic fibers such as glass fibers, carbon fibers, carbon nanofibers, and fibers containing carbon nanomaterials (e.g., graphene), and organic fibers such as regenerated cellulose fibers and fibrillated cellulose fibers. The amount of the additional fibers may be, for example, 1 to 30% by mass, 3 to 20% by mass, or 5 to 15% by mass relative to 100% by mass of the total mass of the cellulose fine fibers, cut fibers, and additional fibers.
[0124] The functionalizing agent may be, for example, one or more selected from the group consisting of a water repellent, a water- and oil-repellent, an antibacterial polymer, an oily compound, a thermoplastic resin, a thermosetting resin, a photocurable resin, and a flame retardant. In the composite molded product, the mass ratio of the functionalizing agent based on the solid content may be, for example, 0.1 to 20 mass%, or 0.2 to 15 mass%, or 0.3 to 10 mass%.
[0125] Examples of the water repellent or water- and oil-repellent agent include various organic resins containing fluorine. In particular, a polymer of an unsaturated monomer containing a perfluoroalkyl group, such as an acrylic acid ester, a methacrylic acid ester, an alkylacrylamide, an alkylvinyl ether, or a vinyl alkyl ketone, or a copolymer of the above-mentioned perfluoroalkyl group-containing unsaturated monomer and an unsaturated monomer not containing a perfluoroalkyl group, such as acrylic acid, an acrylic acid ester, a methacrylic acid ester, vinyl chloride, acrylonitrile, a maleic acid ester, or a polyoxyethylene group-containing unsaturated monomer, is preferred. Examples of the water repellent or water- and oil-repellent agent not containing a fluorine-based compound include silicone compounds, such as methylhydrogenpolysiloxane, dimethylsiloxane, reactive (OH group terminal) dimethylpolysiloxane, wax compounds, waxes such as ordinary waxes, synthetic paraffin wax, and paraffin wax. A mixture of paraffin and an acrylic acid ester-based polymer can also be used to achieve the desired effect. Other examples include wax-zirconium compounds, i.e., reaction products of the above-mentioned wax compounds with zirconium compounds (specifically, basic zirconium compounds such as zirconium acetate, zirconium hydrochloride, zirconium nitrate, and potassium hydroxide), alkylene urea compounds (e.g., octadecylethylene urea or modified products thereof), and higher fatty acid amide derivatives such as aliphatic amide compounds (e.g., N-methylolstearyl amide or modified products thereof). These may be used alone or in combination of two or more.
[0126] Examples of antibacterial polymers include polyhexamethylene biguanide hydrochloride, chlorhexidine, 2-acrylamido-2-methylpropanesulfonic acid copolymers, polymethacrylic acid, blends of polyacrylates and zinc sulfate, quaternary ammonium salt compounds of copolymers of phosphate monomers, dicyanamide-diethylenetriamine-ammonium chloride condensates, dicyandiamide-polyalkylene-polyamine ammonium polycondensates, reaction products of partially deacetylated (polyβ-1,4)-N-acetyl-D-glucosamine compounds and hexamethylenebis(3-chloro-2-hydroxypropyldimethylammonium chloride), acrylonitrile-acrylic acid copolymer copper crosslinked products, acrylic Examples of the antibacterial polymer include amide-diallylamine hydrochloride copolymer, methacrylate copolymer, hydroxypropyl chitosan, crosslinked chitosan, chitosan organic acid salt, chitosan fine powder (polyglucosamine), chitin fiber, chitin, and N-acetyl-D-glucosamine. For example, it is also preferable that these antibacterial polymers are fixed in the composite molded body by blocked polyisocyanate. Examples of the method of processing with the antibacterial polymer include a method of coating the above-mentioned composite molded body with the antibacterial polymer, and specifically, a method of coating or spraying the antibacterial polymer on the surface of the composite molded body, a method of immersing the composite molded body in a solution of the antibacterial polymer, and a method of impregnating the composite molded body with a resin containing the antibacterial polymer.
[0127] Antibacterial evaluation can be performed, for example, by the antibacterial test method for textile products (unified method) established in JIS-1902-1998. Specifically, 2 g of sample is placed in the bottom of a sealed container, 0.2 ml of a solution of Staphylococcus aureus (test species: AATCC-6538P) diluted with 1 / 50 broth that has been previously cultured is spread on the sample, and the sample is left to stand in an incubator at 37°C for 18 hours, after which 20 mL of SCDLP medium is added and the sample is thoroughly shaken to wash off the bacteria. The sample is placed on a normal agar medium, and the number of bacteria is counted 24 hours later, and the antibacterial properties are judged by comparing it with the number of bacteria counted with the untreated sample fabric that was measured at the same time. D = (Ma-Mb)-(Mc-Md) During the ceremony, Ma: logarithm of viable cell count after 18 hours of incubation of unprocessed sample (average of three samples) Mb: logarithm of viable cell count immediately after inoculation of unprocessed sample (average of three samples) Mc: logarithm of viable bacteria count after 18 hours of incubation on treated fabric Md: logarithm of viable cell count immediately after inoculation of treated fabric culture D: Bacteriostatic activity value It is. When the bacteriostatic activity value D is 2.2 or more, it is judged to have antibacterial properties. Therefore, it is preferable that the composite molding also has a bacteriostatic activity value D of 2.2 or more.
[0128] The oily compound is preferably an oily compound having a boiling point range of 50°C or more and 200°C or less under atmospheric pressure. The oily compound is preferably dispersed in the slurry in the form of an emulsion at a concentration of 0.15% by mass to 10% by mass. The concentration of the oily compound in the slurry is preferably 0.15% by mass to 10% by mass, more preferably 0.3% by mass to 5% by mass, and even more preferably 0.5% by mass to 3% by mass. Even if the concentration of the oily compound exceeds 10% by mass, a composite molded body can be obtained, but the amount of the oily compound used in the manufacturing process increases, which is undesirable because it requires safety measures and generates cost constraints. In addition, when the concentration of the oily compound is 0.15% by mass or more, it is preferable because the air resistance can be reduced.
[0129] In addition, since the oily compound is removed during drying (i.e., during the production of a composite molded body), it is desirable that the oily compound can be easily removed by drying. Therefore, the boiling point of the oily compound is preferably 50°C or more and 200°C or less under atmospheric pressure, more preferably 60°C or more and 190°C or less. When the boiling point is within the above range, the papermaking slurry can be easily operated as an industrial production process, and it is possible to heat and remove the oily compound relatively efficiently. If the boiling point of the oily compound under atmospheric pressure is less than 50°C, it is necessary to handle the papermaking slurry under low temperature control in order to handle it stably, which is not preferable in terms of efficiency. Furthermore, if the boiling point of the oily compound under atmospheric pressure exceeds 200°C, a large amount of energy is required to heat and remove the oily compound in the drying process, which is also not preferable. Furthermore, it is desirable that the solubility of the above oily compound in water at 25°C is 5% by mass or less, preferably 2% by mass or less, and more preferably 1% by mass or less, from the viewpoint of efficient contribution of the oily compound to the formation of the required structure.
[0130] Examples of oily compounds include hydrocarbons having 6 to 14 carbon atoms, linear saturated hydrocarbons, cyclic hydrocarbons, linear or cyclic unsaturated hydrocarbons, aromatic hydrocarbons, and monovalent and primary alcohols having 5 to 9 carbon atoms. In particular, the composite molded body of this embodiment can be produced particularly preferably by using at least one compound selected from 1-pentanol, 1-hexanol, and 1-heptanol. This is because the oil droplet size of the emulsion is extremely small (1 μm or less under normal emulsification conditions), and is therefore considered to be suitable for producing a composite molded body having a high porosity and a fine porous structure. These oily compounds may be blended alone or in combination. Furthermore, in order to control the emulsion properties to an appropriate state, a water-soluble compound may be dissolved in the papermaking slurry.
[0131] Examples of thermoplastic resins include styrene-based resins, acrylic-based resins, aromatic polycarbonate-based resins, aliphatic polycarbonate resins, aromatic polyester-based resins, aliphatic polyester-based resins, aliphatic polyolefin-based resins, cyclic olefin-based resins, polyamide-based resins, polyphenylene ether-based resins, thermoplastic polyimide-based resins, polyacetal-based resins, polysulfone-based resins, and amorphous fluorine-based resins. The number-average molecular weight of these thermoplastic resins is generally 1000 or more, preferably 5000 or more and 5 million or less, and more preferably 10,000 or more and 1 million or less. These thermoplastic resins may be used alone or in combination of two or more. When two or more types of thermoplastic resins are used, it is preferable to use a resin having a refractive index of about 1.53, since it is possible to adjust the refractive index of the resin by adjusting the content ratio. For example, when polymethyl methacrylate (refractive index of about 1.49) and acrylonitrile styrene (acrylonitrile content of about 21%, refractive index of about 1.57) are used in a ratio of 50:50, a resin having a refractive index of about 1.53 is obtained.
[0132] Examples of thermosetting resins include, but are not limited to, epoxy resins, thermosetting modified polyphenylene ether resins, thermosetting polyimide resins, urea resins, allyl resins, silicon resins, benzoxazine resins, phenolic resins, unsaturated polyester resins, bismaleimide triazine resins, alkyd resins, furan resins, melamine resins, polyurethane resins, aniline resins, and other industrially available resins, as well as resins obtained by mixing two or more of these resins. Among these, epoxy resins, allyl resins, unsaturated polyester resins, vinyl ester resins, thermosetting polyimide resins, and the like are transparent and therefore suitable for use as optical materials. Examples of the photocurable resin include epoxy resins containing a latent photocationic polymerization initiator. These thermosetting resins or photocurable resins may be contained alone or in combination of two or more.
[0133] The thermosetting resin and photocurable resin refer to relatively low molecular weight substances that are liquid, semi-solid, or solid at room temperature and exhibit fluidity at room temperature or under heating. These can become insoluble and infusible resins that undergo a curing reaction or crosslinking reaction due to the action of a curing agent, catalyst, heat, or light to increase the molecular weight and form a three-dimensional mesh-like structure. The cured resin refers to a resin that is formed by curing the thermosetting resin or photocurable resin.
[0134] The curing agent and curing catalyst are not particularly limited as long as they are used for curing a thermosetting resin or a photocurable resin. Specific examples of the curing agent include polyfunctional amines, polyamides, acid anhydrides, and phenolic resins, and specific examples of the curing catalyst include imidazole, etc., which may be contained in the present invention alone or as a mixture of two or more kinds.
[0135] Examples of the flame retardant include inorganic flame retardants, inorganic phosphorus compounds, nitrogen-containing compounds, chlorine compounds, bromine compounds, etc., and examples of the flame retardant include aqueous solutions or water-dispersible flame retardants such as a mixture of borax and boric acid, aluminum hydroxide, antimony trioxide, ammonium phosphate, ammonium polyphosphate, ammonium sulfamate, guanidine sulfamate, guanidine phosphate, amide phosphoric acid, chlorinated polyolefin, ammonium bromide, and non-ether polybromo cyclic compounds. Examples of the method of processing with a flame retardant include a method of coating the flame retardant on the composite molded body, and specifically, a method of coating or spraying the flame retardant on the surface of the composite molded body, a method of immersing the composite molded body in a solution of the flame retardant, and a method of impregnating the composite molded body with a resin containing the flame retardant.
[0136] The functionalizing agent is preferably bonded to the reactive crosslinking agent (e.g., blocked polyisocyanate) of the present disclosure. In one embodiment, such a bond is formed by subjecting the reactive crosslinking agent to a heat treatment for forming a chemical bond (covalent bond). The reactive crosslinking agent (e.g., blocked polyisocyanate) chemically bonds to the cellulose fine fibers and / or organic filler and also bonds to the functionalizing agent, so that the functionalizing agent can be fixed inside and / or on the surface of the composite molded body of the present embodiment, and thus the function derived from the functionalizing agent is well maintained even after long-term use in water, for example.
[0137] <Manufacturing method of composite molded body> One aspect of the present invention provides a method for producing a composite molded body, the method comprising the steps of: A slurry preparation step of preparing a slurry containing cellulose fine fibers, an organic filler, and a liquid medium containing water; A concentrating step of dehydrating the slurry by a papermaking method to obtain a wet molded body; and a solidification step of at least drying the wetted molded body to obtain a composite molded body; Includes.
[0138] <Slurry preparation process> In this step, a slurry containing cellulose fine fibers, an organic filler, and a liquid medium is prepared. The liquid medium contains water and may contain an organic solvent (e.g., one or more selected from 1-hexanol, 1-heptanol, isobutanol, t-butanol, 1-butanol, isopropanol, 1-propanol, ethanol, methyl cellosolve, ethyl cellosolve, methyl ethyl ketone, and acetone). In one embodiment, the liquid medium is water. The slurry can be prepared by mixing the components of the slurry. An apparatus for uniformly mixing and dispersing the components is appropriately selected depending on the viscosity and state of the slurry, but it is important that the cellulose fine fibers and the organic filler are uniformly dispersed in the dispersion in which the cellulose fine fibers and the organic filler are dispersed in the liquid medium. From this viewpoint, suitable devices include, for example, agitators, homomixers, pipeline mixers, dispersers with cutting functions such as blenders, disc refiners, high-pressure homogenizers, etc., when the slurry has low viscosity (fluidity), and devices and dispersion conditions effective for uniform dispersion according to the composition are selected. Even when the slurry has high viscosity to the extent that it has no fluidity, it is preferable to first disperse the slurry in a high shear field (for example, high shear dispersion using a homomixer, blender, disc refiner, or high-pressure homogenizer, etc.) and then perform a uniform dispersion process, add a component whose structure is destroyed by a high shear field, and use various kneaders that are driven at low speed. For example, when an emulsion of water-dispersible blocked polyisocyanate or the like is used, from the viewpoint of preventing the emulsion from collapsing due to excessive shear stress, it is preferable not to use devices that provide a high shear field, such as high-pressure homogenizers, grinder-type micronizers, and stone mill-type grinding devices, after adding the emulsion. For example, it is preferable to carry out a dispersion treatment in a high shear field as described above in advance (that is, before the addition of the emulsion), and then carry out a dispersion treatment in a relatively low shear field using an agitator or the like after the addition of the emulsion.
[0139] From the viewpoint of obtaining good paper-forming properties, the solid content ratio of the slurry may be preferably 0.2 mass % to 1.5 mass %, or 0.3 mass % to 1.2 mass %, or 0.4 mass % to 1.0 mass %.
[0140] The mass fraction of the cellulose fine fibers in the slurry may be 0.04% by mass or more, or 0.08% by mass or more, or 0.1% by mass or more, in order to avoid excessively long drainage time during production of the composite molded body, improve productivity, and improve the uniformity of the structure within the composite molded body, and may be 1.0% by mass or less, or 0.9% by mass or less, or 0.8% by mass or less, in order to avoid excessively high viscosity, enable the cellulose fine fibers to be uniformly dispersed in the slurry, and result in a composite molded body with a uniform structure.
[0141] The mass fraction of the organic filler in the slurry may be 0.1 mass% or more, or 0.12 mass% or more, or 0.16 mass% or more, in order to avoid excessively long drainage time during production of the composite molded body, improve productivity, and improve the uniformity of the structure within the composite molded body; and the mass fraction may be 0.8 mass% or less, or 0.75 mass% or less, or 0.7 mass% or less, in order to avoid excessively high viscosity, enable the organic filler to be uniformly dispersed in the slurry, and result in a composite molded body with a uniform structure.
[0142] The mass ratio of the liquid medium in the slurry may be preferably 45% by mass or more and 99.9% by mass or less. The mass ratio of the liquid medium is preferably 55% by mass or more, more preferably 70% by mass or more, in order to prevent the viscosity from becoming excessively high, to enable the cellulose fine fibers and the organic filler to be uniformly dispersed in the slurry, and to obtain a composite molded body with a uniform structure, and is preferably 99.9% by mass or less, more preferably 99.4% by mass or less, and even more preferably 99.2% by mass or less, in order to prevent the drainage time during the production of the composite molded body from becoming excessively long, to improve productivity, and to improve the uniformity of the structure within the composite molded body.
[0143] For example, when a composite molded body crosslinked with a reactive crosslinking agent (e.g., blocked polyisocyanate) is produced, the reactive crosslinking agent may be contained in the slurry. In the slurry, the amount of the reactive crosslinking agent relative to the total of 100 parts by mass of the cellulose fine fibers and the organic filler is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, even more preferably 0.5 parts by mass or more, even more preferably 1 part by mass or more, and even more preferably 3 parts by mass or more from the viewpoint of obtaining the advantages of using the reactive crosslinking agent well, and is preferably 100 parts by mass or less, more preferably 90 parts by mass or less, and even more preferably 80 parts by mass or less from the viewpoint of reducing the remaining unreacted reactive crosslinking agent in the composite molded body and preventing inconveniences such as crack generation in the member well.
[0144] The amount of the reactive crosslinking agent (preferably a blocked polyisocyanate) relative to the entire slurry is preferably 0.0001 mass% or more, more preferably 0.001 mass% or more, and even more preferably 0.005 mass% or more, from the viewpoint of obtaining the advantages of using the reactive crosslinking agent well, and is preferably 10 mass% or less, more preferably 6 mass% or less, and even more preferably 4 mass% or less, from the viewpoint of reducing the amount of unreacted reactive crosslinking agent remaining in the composite molded body.
[0145] The reactive crosslinking agent is preferably present in the slurry in the form of a water-dispersed form (e.g., emulsion), and in this case, the dispersibility of the reactive crosslinking agent in the slurry is better. Examples of the emulsion include a self-emulsifying emulsion and a forced emulsifying emulsion. In both the self-emulsifying emulsion and the forced emulsifying emulsion, an anionic, nonionic, or cationic hydrophilic group is exposed on the surface.
[0146] The self-emulsifying emulsion is an emulsion obtained by directly bonding a hydrophilic compound (e.g., an active hydrogen group-containing compound having an anionic group, a nonionic group, or a cationic group) to a reactive crosslinking agent and emulsifying the compound. The active hydrogen group-containing compound having an anionic group is not particularly limited, but may be, for example, a compound having one anionic group and two or more active hydrogen groups.
[0147] Examples of the anionic group include a carboxyl group, a sulfonic acid group, a phosphoric acid group, a betaine structure-containing group, etc. More specifically, examples of the active hydrogen group-containing compound having a carboxyl group include dihydroxyl carboxylic acids such as 2,2-dimethylol acetic acid and 2,2-dimethylol lactic acid, diamino carboxylic acids such as 1-carboxy-1,5-pentylenediamine and dihydroxybenzoic acid, and half ester compounds of polyoxypropylene triol with maleic anhydride and / or phthalic anhydride.
[0148] Examples of the active hydrogen group-containing compound having a sulfonic acid group include N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid, 1,3-phenylenediamine-4,6-disulfonic acid, and the like. Furthermore, examples of active hydrogen group-containing compounds having a phosphoric acid group include 2,3-dihydroxypropylphenyl phosphate. Furthermore, examples of active hydrogen group-containing compounds having a betaine structure-containing group include sulfobetaine group-containing compounds obtained by reacting a tertiary amine such as N-methyldiethanolamine with 1,3-propane sultone.
[0149] The active hydrogen group-containing compound having an anionic group may be modified with an alkylene oxide by adding an alkylene oxide such as ethylene oxide or propylene oxide. The active hydrogen group-containing compound having an anionic group may be used alone or in combination of two or more kinds.
[0150] The active hydrogen group-containing compound having a nonionic group is not particularly limited, but for example, polyalkylene ether polyols containing a normal alkoxy group as a nonionic group are used.Normal nonionic group-containing polyester polyols and polycarbonate polyols are also used. As the polymer polyol, one having a number average molecular weight of 500 to 10,000, particularly 500 to 5,000 is preferably used.
[0151] The active hydrogen group-containing compound having a cationic group is not particularly limited, and examples thereof include aliphatic compounds having an active hydrogen-containing group such as a hydroxyl group or a primary amino group and a tertiary amino group, such as N,N-dimethylethanolamine, N-methyldiethanolamine, and N,N-dimethylethylenediamine. In addition, N,N,N-trimethylolamine and N,N,N-triethanolamine having a tertiary amine can also be used. Among them, polyhydroxy compounds having a tertiary amino group and containing two or more active hydrogens reactive with an isocyanate group are preferred.
[0152] The cationic group-containing active hydrogen group-containing compound may be modified with an alkylene oxide such as ethylene oxide or propylene oxide by addition of the cationic group-containing active hydrogen group-containing compound. The cationic group-containing active hydrogen group-containing compound may be used alone or in combination of two or more kinds.
[0153] The cationic group can be easily dispersed in water in the form of a salt by neutralizing it with a compound having an anionic group. Examples of the anionic group include a carboxyl group, a sulfonic acid group, and a phosphoric acid group. Examples of the compound having a carboxyl group include formic acid, acetic acid, propionic acid, butyric acid, and lactic acid, examples of the compound having a sulfonic group include ethanesulfonic acid, and examples of the compound having a phosphoric acid group include phosphoric acid and acidic phosphoric acid esters. Compounds having a carboxyl group are preferred, and more preferred are acetic acid, propionic acid, and butyric acid. The equivalent ratio of the cationic group:anionic group introduced into the reactive crosslinking agent when neutralizing is preferably 1:0.5 to 1:3, and more preferably 1:1 to 1:1.5. In addition, when a tertiary amino group is introduced, the tertiary amino group can be quaternized with dimethyl sulfate, diethyl sulfate, and the like.
[0154] For example, when a blocked polyisocyanate is used as a reactive crosslinking agent, the ratio of the blocked polyisocyanate to the active hydrogen group-containing compound is preferably an equivalent ratio of isocyanate group / active hydrogen group in the range of 1.05 to 1000, more preferably 2 to 200, and even more preferably 4 to 100. When the equivalent ratio is 1.05 or more, the isocyanate group content in the hydrophilic polyisocyanate does not become too low, and a decrease in the curing speed of the blocked polyisocyanate and weakening of the cured product can be avoided, and the number of crosslinking points between the cellulose fine fibers and the isocyanate groups is increased, so that the blocked polyisocyanate acts well as a water-resistant agent and a fixing agent for the cellulose fine fibers. When the equivalent ratio is 1000 or less, the effect of lowering the interfacial tension is good, and hydrophilicity is well expressed. As a method for reacting a polyisocyanate compound (i.e., a compound having two or more isocyanate groups in one molecule) with an active hydrogen group-containing compound, a method can be used in which the two are mixed and a normal urethane reaction is carried out.
[0155] The forced emulsification type emulsion is an emulsion obtained by forcibly emulsifying a reactive crosslinking agent with a surfactant or the like. The forced emulsification type emulsion may be a compound emulsified and dispersed with a well-known general emulsifier (e.g., anionic surfactant, nonionic surfactant, cationic surfactant, amphoteric surfactant, polymeric surfactant, reactive surfactant, etc.). Among the emulsifiers, anionic surfactants, nonionic surfactants, and cationic surfactants are preferred because they are low in cost and can provide good emulsification.
[0156] Examples of the anionic surfactant include alkyl carboxylate compounds, alkyl sulfate compounds, and alkyl phosphate compounds. Examples of nonionic surfactants include ethylene oxide and / or propylene oxide adducts of alcohols having 1 to 18 carbon atoms, ethylene oxide and / or propylene oxide adducts of alkylphenols, and ethylene oxide and / or propylene oxide adducts of alkylene glycols and / or alkylenediamines. Examples of the cationic surfactant include primary to tertiary amine salts, pyridinium salts, alkylpyridinium salts, and quaternary ammonium salts such as alkyl halide quaternary ammonium salts.
[0157] The amount of these emulsifiers used is not particularly limited, but a mass ratio of 0.01 parts by mass or more to 1 part by mass of the reactive crosslinking agent is preferable since good dispersibility can be obtained, and a mass ratio of 0.3 parts by mass or less is preferable since water resistance and the action as a functionalizing agent or fixing agent can be well exhibited. The above amount is more preferably 0.05 to 0.2 parts by mass.
[0158] The water-dispersible reactive crosslinking agent may contain, for example, 20% by mass or less of a solvent other than water, whether it is a self-emulsifying type or a forced emulsifying type. The solvent is not particularly limited, but examples thereof include ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol dimethyl ether, ethylene glycol, diethylene glycol, and triethylene glycol. These solvents may be used alone or in combination of two or more. From the viewpoint of the dispersibility of the solvent in water, the solvent preferably has a solubility in water of 5% by mass or more, and specifically, dipropylene glycol monomethyl ether and dipropylene glycol dimethyl ether are preferred.
[0159] The average dispersed particle diameter of the water-dispersed reactive crosslinking agent is preferably 1 to 1000 nm, more preferably 10 to 500 nm, and further preferably 10 to 200 nm. The average dispersed particle diameter is a value measured by a static light scattering laser particle size measurement method.
[0160] When the slurry contains cellulose fine fibers, an organic filler, a reactive crosslinking agent, and a liquid medium, e.g. (1) Mixing cellulose fine fibers, a reactive crosslinking agent, and a liquid medium to prepare a premixture, and then mixing the premixture with an organic filler (which may be the organic filler alone or in the form of an organic filler aqueous dispersion, etc.); or (2) mixing cellulose fine fibers, an organic filler, and a liquid medium to prepare a premix, and then mixing the premix with a reactive crosslinker; The slurry can be prepared by the above steps.
[0161] Of the above methods (1) and (2), method (1) is preferred because the reactive crosslinking agent is mixed with the cellulose fine fibers prior to the organic filler, and therefore the reactive crosslinking agent can be adsorbed in greater amounts (i.e. selectively) to the cellulose fine fibers, improving the dispersibility of the cellulose fine fibers and improving the crosslinking effect of the reactive crosslinking agent. In particular, when the reactive crosslinking agent is a cationic reactive crosslinking agent and has electrostatic interaction with the cellulose fine fibers, or when the affinity between the blocked polyisocyanate and the cellulose fine fibers is high, it is extremely advantageous to pre-adsorb the reactive crosslinking agent to the cellulose fine fibers by method (1) in terms of localizing the reactive crosslinking agent around the cellulose fine fibers. On the other hand, even in the above method (2), since the cellulose fine fibers have a larger surface area per unit mass than, for example, the organic filler due to their fine structure, it is possible to adsorb a considerable proportion of the total amount of the reactive crosslinking agent to the cellulose fine fibers, and the above method (2) may be advantageous, for example, when the reactive crosslinking agent is adsorbed to both the cellulose fine fibers and the organic filler. Therefore, the order and manner of addition of each component in the production of the slurry may be appropriately designed depending on the types and amounts of the components in the slurry, as well as the use of the slurry.
[0162] For example, in a system in which a plurality of additives are added and the additives aggregate with each other (for example, a system in which a cationic polymer and an anionic polymer are present in the slurry and form an ion complex), the dispersion state, zeta potential, etc. of the slurry may change depending on the order of addition of the additives. The amount and order of addition of the additives are appropriately selected according to the desired dispersion state of the slurry.
[0163] The mixing temperature when preparing a slurry containing a reactive crosslinking agent is preferably 5°C or more, or 7°C or more, or 9°C or more from the viewpoint of mixing efficiency, and is preferably 60°C or less, or 55°C or less, or 50°C or less from the viewpoint of preventing the reaction of the reactive crosslinking agent. For example, when the reactive crosslinking agent is a blocked polyisocyanate, the above conditions are suitable. In one embodiment, the reactive crosslinking agent may be reacted in the slurry preparation step. In this case, the mixing temperature may be set to a reaction temperature of the reactive crosslinking agent or higher (for example, in the case of a blocked polyisocyanate, a temperature higher than the desorption temperature of the blocking group), and examples thereof include 130°C to 220°C, or 140°C to 210°C.
[0164] <Concentration process> In this step, the slurry is dehydrated by a papermaking method to obtain a wet molded body. The papermaking method is advantageous in that it reduces drying shrinkage between the cellulose fine fibers. In one embodiment, the slurry is dehydrated by filtering it on a porous substrate. In the papermaking method, any papermaking machine equipped with wires of a mesh size that dehydrates the slurry and retains the cellulose fine fibers and organic filler can be used. As a papermaking device, when a composite molded body having a flat sheet shape is obtained, a wet molded body having a flat sheet shape with few defects can be suitably obtained by using a papermaking machine such as an inclined wire papermaking machine, a fourdrinier papermaking machine, or a cylinder papermaking machine. In addition, when a composite molded body having various shapes other than a flat sheet shape is obtained, a wet molded body having a desired shape can be obtained by using a metal mold for pulp molding molded into a predetermined shape. Papermaking can be performed by either a continuous method or a batch method (for example, papermaking by a batch papermaking machine and a pulp molding method) depending on the purpose.
[0165] When obtaining a flat sheet, from an industrial point of view, it is preferable in terms of cost to prepare a long sheet by continuous papermaking using a papermaking machine and make it into a roll-shaped product form. In particular, in the case of continuous papermaking using a papermaking machine, in normal papermaking (for example, papermaking using beaten pulp fibers or cut yarn), the fibers in the aqueous dispersion are oriented in the running direction of the wire belt due to the generation of shear stress between the aqueous dispersion of fibers fed onto the papermaking wire and the running wire belt, and as a result, in the obtained flat sheet, anisotropy of physical properties (strength, elastic modulus, etc.) occurs between the running direction (Machine direction, MD) and the perpendicular direction (Transverse direction, TD) due to the orientation of the fibers. On the other hand, the composite molded body obtained in this embodiment has the characteristic that the difference in physical properties between the MD direction and the TD direction is unlikely to appear even in continuous papermaking. This feature is considered to be due to the fact that, when the flat sheet, which is the composite molded body of this embodiment, is produced by a papermaking machine, in an aqueous dispersion containing cellulose fine fibers and an organic filler, the cellulose fine fibers form an isotropic soft aggregate based on fiber-to-fiber association, the organic filler is incorporated into the soft aggregate to form a composite soft aggregate in which the cellulose fine fibers and the organic filler are integrated, and even if the organic filler has an anisotropic shape, it is incorporated in the composite soft aggregate in a non-oriented state (in a disordered and non-anisotropic state). The composite soft aggregate has a strength sufficient to not collapse due to the shear stress applied to the aqueous dispersion during the belt running in the above-mentioned normal papermaking, so that the composite soft aggregate in which the organic filler is fixed in a non-oriented state is deposited and dehydrated on the belt, and a sheet without anisotropy is formed by subsequent drying treatment or the like. Typically, in continuous papermaking, the MD / TD ratio of physical properties such as tensile strength, tensile modulus, bending strength, bending modulus, and coefficient of linear thermal expansion increases according to the running speed during papermaking (usually 5 m / min or more) (see, for example, Comparative Example 8 in the [Examples] section of this disclosure).On the other hand, when the composite molded body of this embodiment is produced by a continuous papermaking method, the tensile strength, tensile modulus, bending strength, bending modulus, and / or MD / TD ratio of the linear thermal expansion coefficient may be 1.6 or less in one aspect, preferably 1.4 or less, or 1.2 or less (see, for example, the tensile strength in Example 27 in the [Example] section of this disclosure). In addition, even when produced by three-dimensional molding such as the pulp molding method, the composite molded body of this embodiment is characterized in that anisotropy is unlikely to appear not only in highly flat parts but also in parts with high curvature.
[0166] In one embodiment, when a composite member is formed by a composite molded body and an additional member (e.g., an organic polymer sheet) in order to manufacture the composite member, the additional member may be used as a support for papermaking. In this case, a material that satisfies the requirements related to the yield rate and water permeability in combination with the support can be selected, for example, as a wire or filter cloth for a papermaking machine.
[0167] In the dehydration by the concentration process, high solid fractionation progresses, and a wet molded body is obtained. The solid fraction of the wet molded body is adjusted to a level of dehydration controlled by the suction pressure (wet suction or dry suction) in papermaking or the pressing process, and the solid fraction is preferably adjusted to a range of 6% by mass or more and 50% by mass or less, more preferably 8% by mass or more and 45% by mass or less. When the solid fraction of the wet molded body is 6% by mass or more, the wet molded body has good self-supporting properties and process problems can be avoided. In addition, when the solid fraction of the wet molded body is 50% by mass or less, cracks are less likely to occur in the wet molded body, which is preferable.
[0168] In addition, if a method is used in which a paper is made on a wire or a mesh in a mold, the water in the wet molded body is replaced with an organic solvent in a process of replacing the water with an organic solvent, and then the molded body is dried, a porous composite molded body is obtained after drying, so that the air resistance of the composite molded body can be controlled and, for example, heat insulation can be imparted. For details of this method, please refer to the pamphlet of International Publication WO 2006 / 004012 by the present inventors.
[0169] The drainage time during filtration in batch-type papermaking may be, for example, 180 seconds or less, preferably 120 seconds or less, and more preferably 60 seconds or less, from the viewpoint of the production efficiency of the composite molded body. From the viewpoint of obtaining a high-quality composite molded body, the drainage time may be, for example, 1 second or more, 3 seconds or more, or 5 seconds or more. The drainage time is evaluated as follows. A batch-type papermaking machine (Kumagaya Riki Kogyo Co., Ltd., automatic square sheet machine, 25 cm x 25 cm, 80 mesh) equipped with a metal mesh equivalent to 80 mesh is used to filter a 50 g / m2 sheet. 2 A slurry prepared based on the composite molded body of is poured in, and then the pressure is reduced to 4 KPa relative to atmospheric pressure to perform papermaking (dewatering). The time it takes to dewater at this stage is measured as the drainage time. The drainage time of the slurry can also be adjusted by increasing or decreasing the degree of vacuum.
[0170] In order to satisfactorily form a composite molded body having a large thickness according to this embodiment, it is advantageous to prepare the papermaking slurry at a solid content concentration of 0.4 mass % or more.
[0171] In the case of producing a composite of a composite molded body and an additional member, when the additional member is used as a support, for example, the support is placed on a papermaking machine equipped with a wire, a part of the water in the papermaking slurry is dehydrated (papermaking) on the support, and the wet molded body is laminated on the support and integrated to produce a multi-layered molded body having at least two or more multi-layered composite molded bodies. Also, two or more composite molded bodies may be multi-stage-paper-made on the support to produce a multi-layered molded body having three or more layers.
[0172] <Solidification process> In this step, the wet molded body is at least dried to obtain a composite molded body. Drying can be performed using a fixed-length drying type dryer that can dry the liquid medium while keeping the width of the wet molded body at a fixed length, such as a drum dryer or a pin tenter. This drying method is suitable for forming a composite molded body with a relatively high air resistance. The drying temperature may be appropriately selected depending on the conditions, but if it is preferably set to a range of 45°C to 180°C, more preferably 60°C to 150°C, and even more preferably 80°C to 120°C, a composite molded body with suitable air permeability can be produced. The air resistance of the composite molded body can be controlled by the composition ratio of the cellulose fine fibers and organic filler that constitute the slurry, the overall basis weight, the dispersion method of the raw liquid, the blending conditions of various additives, the average fiber diameter of the fine fibers, etc. The drying temperature is preferably 80°C or higher, 85°C or higher, or 90°C or higher from the viewpoint of drying efficiency (particularly, from the viewpoint of increasing the evaporation rate of the liquid medium to obtain good productivity), and is preferably 120°C or lower, 115°C or lower, or 110°C or lower from the viewpoint of preventing thermal denaturation of the hydrophilic polymer (specifically, cellulose fine fibers and other components) constituting the composite molded body, preventing a decrease in energy efficiency that affects costs, and further, preventing the reaction of the reactive crosslinking agent when a reactive crosslinking agent is used. For example, multi-stage drying in which low-temperature drying at a temperature of 100°C or lower is first performed and then drying at a temperature above 100°C is also effective in obtaining a composite molded body with high uniformity. For example, when a blocked polyisocyanate is used as a reactive crosslinking agent, the above conditions are suitable.
[0173] In one embodiment, when a reactive crosslinking agent is used (for example, a slurry containing a reactive crosslinking agent is used), the reactive crosslinking agent is reacted in the slurry preparation step, or simultaneously with or after drying, to crosslink between the cellulose fine fibers, between the organic fillers, and / or between the cellulose fine fibers and the organic filler. The reaction temperature may be selected according to the type of reactive crosslinking agent. For example, when a blocked polyisocyanate is used, the reaction temperature is set to be equal to or higher than the desorption temperature of the blocking group. When the blocked polyisocyanate is heated at a temperature equal to or higher than a predetermined desorption temperature according to the blocking group, the blocked group is desorbed to generate a free isocyanate group, and the isocyanate group reacts with a functional group having active hydrogen (such as a hydroxyl group, an amide group, an amino group, a thiol group, or a carboxyl group) in the system to form a covalent bond. This covalent bond can be formed three-dimensionally at least with respect to the hydroxyl group of the cellulose fine fiber. Furthermore, when the organic filler has a functional group having active hydrogen, a three-dimensional covalent bond is also formed with respect to the organic filler. The formation of such a covalent bond imparts good mechanical strength, water resistance, and solvent resistance to the composite molded article, and also suppresses leaching of the blocked polyisocyanate and the polyisocyanate derived therefrom (e.g., leaching into water or solvents).
[0174] When using a blocked polyisocyanate, the reaction temperature is set to the desorption temperature of the blocking group of the blocked polyisocyanate or higher, and in one embodiment, may be 130°C to 220°C or 140°C to 210°C. Below the desorption temperature, the isocyanate group is not regenerated, so the crosslinking reaction does not proceed. On the other hand, at temperatures above 220°C, the cellulose fine fibers and the blocked polyisocyanate, and depending on the type, the organic filler may be thermally deteriorated and colored, so 220°C or lower is preferable. The reaction time is preferably 5 seconds to 10 minutes, more preferably 7 seconds to 3 minutes. When the reaction temperature is sufficiently higher than the desorption temperature of the blocking group, the reaction time can be shortened. In one embodiment, in the solidification step, drying is performed at 80°C to 120°C, and then the reaction is performed at 130°C to 220°C.
[0175] In a typical embodiment, the structure derived from the blocked polyisocyanate (specifically, a crosslinked body) exists as an aggregate in the composite molded body. Such an aggregate is significantly formed when the composite molded body is produced using a slurry containing, for example, the above-mentioned water-dispersible blocked polyisocyanate as the blocked polyisocyanate. In one embodiment, the aggregate is formed on the cellulose fine fiber and / or the organic filler in the form of a coating film.
[0176] In one embodiment, reactants derived from the crosslinking agent are distributed uniformly in the planar direction of the composite molded body between the cellulose fine fibers, between the organic filler, and / or between the cellulose fine fibers and the organic filler in the composite molded body.
[0177] In the composite molded body, the hydrophilicity and hydrophobicity may be appropriately controlled. The hydrophilicity and hydrophobicity of the composite molded body affect the coating or impregnation amount of the hydrophilic or hydrophobic compound and the operability of coating or impregnation, for example, when the hydrophilic or hydrophobic compound is coated on the composite molded body or impregnated with the composite molded body for a specific purpose depending on the application. For example, since the degree of crosslinking (and therefore hydrophobization) in the composite molded body can vary greatly depending on the type and addition amount of the reactive crosslinking agent, it is possible to control the hydrophilicity and hydrophobicity of the composite molded body by selecting or designing the reactive crosslinking agent.
[0178] Furthermore, producing a composite molded body using a slurry containing a compound having hydrophobic or water-repellent properties with which a reactive crosslinking agent can react is also effective as a means for improving the dry / wet strength ratio or controlling hydrophilicity / hydrophobicity. Examples of the compound having hydrophobic or water-repellent properties include the compounds described above as water-repellent or water- and oil-repellent finishing agents.
[0179] Hydrophilicity and hydrophobicity are relative indices, so they can be evaluated by comparing them with a reference substance. For example, a composite molded body consisting of only cellulose fine fibers and organic fillers is used as a reference substance to judge the hydrophilicity and hydrophobicity of a molded body to which a reactive crosslinking agent and various functionalizing agents have been added. One evaluation method is, for example, measuring the static contact angle of a water droplet. Specifically, 4 μL of distilled water (20°C) is dropped onto the sample, and the static contact angle 1 second after the drop is placed is measured using an automatic contact angle meter (for example, product name: "DM-301", manufactured by Kyowa Interface Science Co., Ltd.). At this time, the smaller the static contact angle, the more hydrophilic it is, and the larger it is, the more hydrophobic it is. Another method is to measure the time it takes for a water droplet to absorb water. 4 μL of distilled water (20°C) is dropped onto the sample, and the time it takes for the droplet to absorb water is measured. The longer it takes for the water to be absorbed, the more hydrophobic it is judged to be.
[0180] By treating the composite molded body with a hot press at a temperature equal to or higher than the glass transition point of the organic filler, the composite surface can be smoothed and the strength of the composite molded body can be increased. When the organic filler is a cut fiber having a sheath-core structure, a high-strength composite molded body can also be obtained by melting the sheath part, which has a low melting point, to fuse the cut fibers together.
[0181] <Characteristics of composite molding> The thickness of the composite molded body may be 100 μm or more, preferably 150 μm or more, or 200 μm or more, and may be 10,000 μm or less, preferably 5,000 μm or less, or 3,000 μm or less in one embodiment. The thickness of the composite molded body refers to the minimum dimension of a representative portion of the composite molded body. The thickness means (1) a number average value of thicknesses measured at nine different points on the composite molded body using a thickness meter (e.g., Mitutoyo Model ID-C112XB) (more specifically, dividing the composite molded body into nine equal areas and measuring the center of each area, a total of nine points), and (2) however, if it is not possible to measure with the thickness meter, the value is obtained by the alternative method described below. In the alternative method, one point on the surface of the composite molded body is defined as the measurement point, and the minimum diameter of the composite molded body at the measurement point is measured using a vernier caliper, and the maximum of the minimum diameter lengths obtained by determining measurement points over the entire surface of the composite molded body is the thickness of the composite molded body.
[0182] The weight of the composite molded body is 50 g / m in one embodiment, which allows it to be used in a wide range of applications. 2 More preferably, 70 g / m 2 or more than 80g / m 2 or more than 90g / m 2 From the viewpoint of ease of manufacturing the composite molded body, 2 Preferably, 700 g / m 2 or less than 500g / m 2 or less than 400g / m 2 The basis weight of the composite molded body means the value obtained by dividing the mass of the composite molded body by the number average value of the total area of one side (more specifically, the front side when the composite molded body is projected in the thickness direction) of the composite molded body and the total area of the opposite side (more specifically, the back side in the projected view). Therefore, when the composite molded body has a complex shape (various parts shapes, etc.), the basis weight value is a value for convenience, but the basis weight is an index that represents the properties of the entire composite molded body.
[0183] The average air permeability resistance of the composite molded body is, in one embodiment, 0.5 seconds / 100 mL or more, preferably 1.0 seconds / 100 mL or more, or 1.5 seconds / 100 mL or more, from the viewpoint of increasing the voids within the composite molded body, for example, to facilitate impregnation of the resin into the composite molded body and / or to impregnate the resin in a larger amount, and in one embodiment, from the viewpoint of improving the uniformity of the structure within the composite molded body and uniformly impregnating the resin into the composite molded body, is 100,000 seconds / 100 mL or less, or 60,000 seconds / 100 mL or less, or 30,000 seconds / 100 mL or less, or 10,000 seconds / 100 mL or less, or 8,000 seconds / 100 mL or less, or 3,000 seconds / 100 mL or less. The average air resistance can be controlled by selecting the average minor axis diameter of the cellulose fine fibers and organic filler used, selecting the mixing ratio of multiple types of organic fillers with different average minor axis diameters, the composition of the liquid medium in the slurry prepared in the slurry preparation step (type and amount of organic solvent), the type and amount of surfactant in the slurry, etc. The smaller the average minor axis diameter, the denser the composite molded body tends to be. When a reactive crosslinking agent is used, the air resistance can also be controlled by the type and amount of the reactive crosslinking agent added.
[0184] The air permeability resistance in the present disclosure means the result of measuring the time for air to pass through 100 mL using a Gurley densometer (e.g., model G-B2C, manufactured by Toyo Seiki Co., Ltd.). The average air permeability resistance is the number average value of the air permeability resistance in the thickness direction obtained by any of the above methods for nine different points on the composite molded body selected in the same manner as in the thickness measurement described above. However, for samples with an average air permeability resistance exceeding 1,000 seconds / 100 mL, the measurement is performed at room temperature (23°C) using an Oken air permeability resistance tester (e.g., model EG01, manufactured by Asahi Seiko Co., Ltd.) instead of the Gurley densometer. The air permeability resistance means (1) a value obtained by performing the above measurement using a sample of the size (200 mm x 200 mm) specified by the measuring device, and (2) for composite molded bodies for which a sample of the above size cannot be obtained, a sample size of 50 mm x 50 mm is used, and the value obtained by any of the above methods for five different points on the composite molded body. In the case of a composite molding having a complex shape, the air permeation resistance may be measured by cutting a flat portion constituting the molding with scissors or the like.
[0185] The coefficient of variation of air resistance, which is the standard deviation of the air resistance of the composite molded body divided by the average air resistance, is 0.5 or less in one embodiment, preferably 0.42 or less, or 0.35 or less, or 0.2 or less, in terms of good uniformity of the structure within the composite molded body. The smaller the coefficient of variation of air resistance, the more preferable it is, but from the viewpoint of ease of production of the composite molded body, it may be, for example, 0.01 or more, or 0.015 or more, or 0.02 or more. The coefficient of variation of air resistance is the standard deviation of the air resistance of 9 points obtained by the above method divided by the average air resistance.
[0186] The tensile strength of the composite molded body is preferably 0.1 kg / 15 mm or more, or 0.2 kg / 15 mm or more, or 0.3 kg / 15 mm or more from the viewpoint of obtaining physical properties that allow the composite molded body to be easily handled as an independent molded body, and is preferably 40 kg / 15 mm or less, or 30 kg / 15 mm or less, or 25 kg / 15 mm or less from the viewpoint of ease of production of the composite molded body. The tensile strength is a value (i.e., dry tensile strength) measured in accordance with JIS P 8113 for a composite molded body cut into a size of 20 cm in length and 15 mm in width after storage for 24 hours in an environment controlled at a room temperature of 20° C. and a humidity of 50% RH.
[0187] The wet tensile strength of the composite molded body is affected by its basis weight, but is preferably 0.07 kg / 15 mm or more, or 0.21 kg / 15 mm or more, or 0.35 kg / 15 mm or more so that the composite molded body is less likely to break when used in applications where it is used in liquid, and is preferably 30 kg / 15 mm or less, or 25 kg / 15 mm or less, or 20 kg / 15 mm or less from the viewpoint of ease of production. The wet tensile strength is the value of the tensile strength measured in the same manner as the dry tensile strength after immersing the composite molded body for 5 minutes in a container filled with water sufficient to immerse the composite molded body.
[0188] The wet / dry strength ratio of the tensile strength of the composite molded body is preferably 0.4 to 1.2. From the viewpoint of obtaining a composite molded body having good durability even in applications where the composite molded body is used in liquids such as water, the wet / dry strength ratio is preferably 0.4 or more, or 0.5 or more, or 0.6 or more, and from the viewpoint of easily maintaining other properties of the composite molded body, the wet / dry strength ratio is preferably 1.2 or less, or 1.1 or less, or 1.0 or less. The wet / dry strength ratio is a value calculated by the following formula. Wet / dry strength ratio (%) = (wet tensile strength) / (dry tensile strength) x 100
[0189] The composite molded body is typically a single layer, but may be a multi-layer body having the same or different configurations. For example, two or more composite molded bodies may be integrated together by pressing or the like.
[0190] The composite molded body contains cellulose fine fibers having a high elastic modulus. Therefore, the composite molded body can have a high elastic modulus depending on the content of cellulose fine fibers and due to the network structure formed by the cellulose fine fibers inside the composite molded body. The tensile elastic modulus of the composite molded body is preferably 0.05 GPa or more, or 0.07 GPa or more, or 0.1 GPa or more, and from the viewpoint of maintaining the handleability of the composite molded body, 4 GPa or less, or 3 GPa or less, or 2.5 GPa or less. The tensile elastic modulus of the composite molded body is measured using a vertical Tensilon measuring device by fixing a sample cut into a rectangular strip with a width of 15 mm and a length of 125 mm and a total thickness at a chuck distance of 100 mm. The tensile elastic modulus is a value measured after storing for 24 hours in an environment controlled at room temperature of 20°C and humidity of 50% RH (i.e., dry tensile elastic modulus).
[0191] The composite molded body can have a small linear thermal expansion coefficient. The linear thermal expansion coefficient of the composite molded body is preferably 0.1 ppm / °C or more, or 0.5 ppm / °C or more, and preferably 100 ppm / °C or less, or 70 ppm / °C or less, or 40 ppm / °C or less. The linear thermal expansion coefficient is measured using a thermomechanical analysis (TMA) device in a measurement temperature range of -40°C to 100°C in accordance with ISO11359-2, and is a value obtained as an average linear thermal expansion coefficient between 0°C to 60°C. When the composite molded body is not a uniform planar shape having irregularities (such as in the case of molding by the pulp molding method), it is possible to measure it even in a size smaller than the planar shape sample, and the tensile strength, tensile modulus, and linear thermal expansion coefficient can be measured in any size.
[0192] In addition, when a composite molded product has MD and TD directions resulting from its manufacturing process (e.g., when it has undergone continuous papermaking), the above-mentioned numerical ranges of tensile strength, tensile modulus, and linear thermal expansion coefficient may be satisfied in at least one of the MD and TD directions regardless of its shape. In a composite molded product having MD and TD directions, a sample with the MD direction as its length direction is used for measurement in the MD direction, and a sample with the TD direction as its length direction is used for measurement in the TD direction. On the other hand, in a composite molded product not having MD and TD directions, a sample cut in any direction is used for measurement.
[0193] <Applications of composite moldings> The composite molded body of the present embodiment can be suitably used for a wide range of applications, such as automobile parts (for example, bonnets, doors, roofs, trunk lids, front fenders, rear fenders, FRP core materials for frames, roof headlining materials for interior materials, sunshade materials, engine silencer materials, indoor silencer materials, sound absorbing materials, heat insulating materials, heat dissipation materials, etc.) other than automobiles, mobility parts other than automobiles, housings for communication devices (mobile phones, tablet terminals, PCs), housings for home appliances, speaker cones for audio products, sound absorbing materials, heat insulating materials, heat dissipation materials, various filters, medical materials, etc. One aspect of the present invention provides a sound absorbing material, air filter, or automobile part material composed of the composite molded body of the present disclosure. The composite molded body of the present disclosure can also be further combined with a resin, for example as described below, to form a resin molded body suitable as an automobile part, etc.
[0194] For example, when the composite molded body of the present embodiment is used as a sound absorbing material, it has a frequency-dependent sound absorption coefficient and shows a relatively sharp sound absorption peak at a specific frequency, so it can be suitably used as a sound absorbing material in a specific frequency range. In addition, when multiple composite molded bodies are used in layers, the sound absorption peak shifts to the lower frequency side as the thickness increases, but in this case, even if the thickness is increased, the sound absorption coefficient tends not to decrease. Therefore, the composite molded body of the present embodiment is preferably used in layers, because it is possible to control the desired sound absorption frequency range while maintaining a high sound absorption coefficient.
[0195] One aspect of the present invention provides a fiber composition which is a shredded product (specifically, a dry-ground product) of the composite molded body of the present embodiment. The fiber composition can be produced by cutting the composite molded body into, for example, granules, pellets, strips, sheet fragments, etc., using a slitter or shredder. In one aspect, the shredded product may be granules or pellets. The fiber composition may be in the form of, for example, a strip or sheet fragment with a width of about 1 mm to 300 mm. Such a fiber composition can be mixed (for example, melt-kneaded) with other materials to form various members.
[0196] <Resin molded body> One aspect of the present invention provides a method for producing a resin molded body containing cellulose fine fibers and a resin, the method including a mixing step of mixing the fiber composition of the present disclosure with a resin to obtain a mixture, and a molding step of molding the mixture. In one aspect, the organic filler in the fiber composition and the resin may each contain a thermoplastic resin, and the fiber composition and the resin may be melt-mixed in the mixing step. The molding may be, for example, extrusion molding or injection molding, and the molding conditions may be appropriately designed depending on the types of organic filler and resin used, the desired properties of the resin molded body, and the like.
[0197] Another aspect of the present invention provides a method for producing a resin molded body containing cellulose fine fibers and a resin, the method comprising a composite molded body formation step of forming a composite molded body containing cellulose fine fibers and an organic filler, and a molding step of impregnating the composite molded body with resin and then solidifying it.
[0198] The resin used in the manufacture of the resin molded body may be a thermoplastic resin (e.g., polyamide, polyolefin, polyester, etc.), a thermosetting resin (e.g., epoxy resin, allyl resin, unsaturated polyester resin, vinyl ester resin, thermosetting polyimide resin, etc.), etc. The resin may contain a curing agent component as necessary. By mixing the cellulose fine fiber and the organic filler with the resin and then molding, the resin molded body can be easily molded into a flat plate or other desired shape, and such a resin molded body can be suitably applied to a wide range of applications, such as automobile parts. The characteristics of the resin molded body may be controlled by appropriately designing the combination of the type of resin and the type of polymer constituting the organic filler. For example, a composite molded body having a high elastic modulus can be formed by using aramid fiber as the organic filler and polypropylene as the resin.
[0199] In the resin molded body, the amount of resin per 100 parts by mass of the composite molded body can be selected appropriately depending on the desired characteristics, and may be, for example, 10 parts by mass or more, or 15 parts by mass or more, or 20 parts by mass or more, and may be, for example, 90 parts by mass or less, or 85 parts by mass or less, or 80 parts by mass or less.
[0200] When the composite molded body is impregnated with resin and then solidified, a method for forming a member of a desired shape can be, for example, molding, which is a manufacturing method for fiber reinforced plastics (FRP). For example, a method in which the composite molded body is arranged along a mold of a desired shape and the resin is impregnated while being degassed (hand lay-up method and spray-up method), a method in which a sheet of the resin to be impregnated is prepared in advance and the sheet and the composite molded body are stacked in a mold and compression molded (SMC press method), a method in which a resin is injected into a mating mold in which composite molded bodies are laid out (injection molding such as the RTM method), a method in which a thermosetting resin is cured in an autoclave and molded, and a de-autoclave molding method that does not use an autoclave, which has become widespread in recent years, can be applied. Below, as an example embodiment, an example of a molding method using a mold according to the desired shape of the member will be described.
[0201] Prior to molding, the resin for impregnation (which may be kneaded with optional additive components using a single-screw kneader, a twin-screw kneader, or the like) is supplied to the mold in a fluid state (for example, in the form of a melt, solution, or dispersion in the case of a thermoplastic resin, or in the form of an uncured product in the case of a thermosetting resin or a photocurable resin). The resin is then solidified by removing the solvent (in the case of a solution or dispersion), cooling (in the case of a melt of a thermoplastic resin), or curing (in the case of a thermosetting or photocurable resin). The solidification conditions may be appropriately designed depending on the type of resin used, etc. For example, solidification under reduced pressure (for example, vacuum heat pressing, etc.) may be preferable in terms of good impregnation of the resin into the inside of the composite molded body.
[0202] When a thermoplastic resin is used as the resin for impregnation, a heated melt of the resin may be impregnated and then cooled and solidified. In one embodiment, the organic filler contains a thermoplastic resin, and the resin to be impregnated is a heated melt of a thermoplastic resin having a melting point lower than that of the thermoplastic resin in the organic filler.
[0203] In addition, when a thermosetting or photosetting resin is used as the resin for impregnation, an uncured or semi-cured product of the resin may be impregnated. For example, the uncured product may be cured once to a semi-cured product before solidification after impregnation or before impregnation. Semi-curing means a state in which the resin is cured to an extent that it has no fluidity but still maintains flexibility to the extent that it can follow the mold shape. In particular, a prepreg formed by impregnating a composite molded body with an uncured resin and then semi-curing it is advantageous in terms of handleability during the manufacture of a resin-impregnated molded body. After impregnation, the resin may be cured and solidified using, for example, a mold press. In one embodiment, the prepreg is preferably laminated in a range of 20 sheets or less, 15 sheets or less, or 12 sheets or less, and press-molded, and then a curing reaction is performed, thereby obtaining a resin molded body with a large thickness, for example, a maximum thickness of 30 mm. The number of layers of the prepreg is advantageous in terms of suppressing the occurrence of defects.
[0204] Another aspect of the present invention provides a method for producing a resin molded body containing cellulose fine fibers and a resin, comprising a composite molded body forming step of forming a composite molded body containing cellulose fine fibers and an organic filler containing a thermoplastic resin, and a molding step of molding the composite molded body at a temperature equal to or higher than the melting point of the thermoplastic resin in the organic filler. According to this method, a molten organic filler is impregnated between the cellulose fine fibers, and then the molten organic filler is solidified, thereby obtaining a resin molded body in which the cellulose fine fibers are well dispersed in the resin derived from the organic filler. In the resin molded body, the organic filler may or may not still retain its filler shape. When producing a resin molded body by this method, the composite molded body is preferably laminated and molded in a range of 20 sheets or less, 15 sheets or less, or 12 sheets or less, to obtain a resin molded body having a large thickness, for example, a maximum thickness of 15 mm. The number of laminated sheets of the composite molded body in the above range is advantageous in terms of suppressing the occurrence of defects. The molding method is not limited, but for example, melt pressing using a mold of a desired shape is preferable because it is easy to manufacture a resin molded body of a desired shape by the above method. The melt pressing may be performed in a batch or continuous manner using a manual hydraulic vacuum heating press device, a heating calendar device, or the like. The molding step is preferably performed at a molding temperature that is 10°C to 40°C, or 15°C to 30°C, or about 20°C higher than the melting point of the thermoplastic resin in the organic filler. Thereafter, the thermoplastic resin is cooled and solidified to obtain a resin molded body of a desired shape. As a cooling condition, it is preferable to sandwich the resin molded body after melt pressing between metal plates and air-cool it.
[0205] In one aspect, the resin molded product of the present embodiment has the composite molded product of the present embodiment as a skeleton structure and is impregnated with a resin, whereby the resin molded product can have higher strength, higher elastic modulus, and lower coefficient of linear thermal expansion than the impregnated resin itself.
[0206] In one embodiment, the ratio of the tensile strength of the resin molded body to the tensile strength of the resin itself is preferably 1.1 or more, or 1.2 or more, or 1.4 or more, and preferably 5 or less, or 4 or less, or 3 or less.
[0207] In one embodiment, the ratio of the tensile modulus of the resin molded body to the tensile modulus of the resin itself is preferably 1.1 or more, or 1.2 or more, or 1.4 or more, and preferably 8 or less, or 6 or less, or 5 or less.
[0208] In one aspect, the ratio of the linear thermal expansion coefficient of the resin molded body to the linear thermal expansion coefficient of the resin itself is preferably 70% or less, or 65% or less, or 60% or less, and preferably 2% or more, or 4% or more, or 6% or more. The methods for measuring the tensile strength, tensile modulus, and linear thermal expansion coefficient of the resin molded body of this embodiment are similar to the methods for measuring the tensile strength, tensile modulus, and linear thermal expansion coefficient of the composite molded body of this embodiment described above. When the resin molded body is not of a uniform planar shape having irregularities, a planar resin molded body of the same composition is molded to measure the tensile strength, tensile modulus, and linear thermal expansion coefficient.
[0209] One aspect of the present invention also provides a composite of a composite molded body or a resin molded body and an additional member. For example, the composite may be a laminate of a composite molded body or a resin molded body and an organic polymer sheet (hereinafter, simply referred to as an organic polymer sheet) as an additional member. In such a laminate, mechanical strength such as tensile strength may be further strengthened by the organic polymer sheet. The material of the organic polymer sheet is not particularly specified, but is appropriately selected according to the required performance such as the shape, hardness, mechanical properties, thermal properties (e.g., dimensional stability against temperature change), durability, water resistance, and air resistance of the intended laminate, or the use of the laminate. In one aspect, the composite molded body or the resin molded body and the additional member may be chemically crosslinked by a blocked polyisocyanate. From this viewpoint, preferred materials for the additional member include materials having a functional group having active hydrogen, specifically, cellulose, polyamide, polyvinyl alcohol, polycarboxylic acid, etc. In addition, in the case of a material that does not have a functional group having active hydrogen (for example, polyolefins such as polyethylene and polypropylene, polyesters such as polyethylene terephthalate, etc.), the functional group can be introduced by surface activation treatment such as corona discharge treatment, plasma treatment, etc. The composite may be, for example, a composite molded body containing a blocked polyisocyanate and an additional member are laminated together, and then the blocked polyisocyanate is crosslinked under the above-mentioned conditions, so that the composite molded body and the additional member are crosslinked by the crosslinked body of the blocked polyisocyanate. EXAMPLES
[0210] The present invention will now be described in detail with reference to examples. The main physical properties were measured by the following methods.
[0211] <Material> [Cellulose microfibers] (Slurry Production Example 1: Cellulose Fine Fiber Slurry 1) As a raw material, natural cellulose linter pulp obtained from Japan Pulp and Paper Co., Ltd. was used, and the linter pulp was immersed in water so that the linter pulp was 4% by mass. Then, heat treatment was performed in an autoclave at 130°C for 4 hours, and the resulting swollen pulp was washed with water multiple times to obtain purified linter pulp impregnated with water. Then, the purified linter pulp obtained was dispersed in water so that the solid content was 1.5% by mass to obtain a 400L dispersion. Using an SDR14 type lab refiner (pressure type DISK type) manufactured by Aikawa Iron Works Co., Ltd. as a disc refiner device, the 400L aqueous dispersion was beaten for 20 minutes with a clearance between discs of 1 mm. Subsequently, the beating treatment was continued under conditions in which the clearance was gradually reduced to a level close to zero. Sampling was performed over time, and the CSF value of the sampled slurry was evaluated according to the Canadian Standard Freeness Test for Pulp defined in JIS P 8121 (hereinafter referred to as the CSF method). The CSF value decreased over time and once reached near zero. When the beating process was continued, the CSF value tended to increase. After the clearance reached near zero, the beating process was continued under the above conditions for 10 minutes, and a beating slurry with a CSF value of 100 ml or more was obtained. The obtained beating water slurry was directly subjected to a high-pressure homogenizer (NS015H manufactured by Niro Soavi Co., Ltd. (Italy)) at an operating pressure of 100 MPa five times to obtain cellulose fine fiber slurry 1 (solid content concentration: 1.5 mass%). The average fiber diameter of the cellulose fine fibers contained in the cellulose fine fiber slurry 1 was 98 nm.
[0212] (Slurry Production Example 2: Cellulose Fine Fiber Slurry 2) Tencel cut yarn (3 mm long), which is a regenerated cellulose fiber obtained from Sojitz Corporation, was placed in a cleaning net, a surfactant was added, and the fiber surface was washed repeatedly with water in a washing machine to remove the oil. Then, a slurry of cellulose fine fibers (solid content concentration: 1.5 mass%) was obtained in the same manner as in Slurry Production Example 1. The average fiber diameter of the cellulose fine fibers contained in the cellulose fine fiber slurry 2 was 390 nm.
[0213] (Slurry Production Example 3: Cellulose Fine Fiber Slurry 3) Except for not carrying out the micronization treatment using the high-pressure homogenizer, a slurry of cellulose fine fibers was obtained in the same manner as in the cellulose fine fiber slurry 1. The average fiber diameter of the cellulose fine fibers contained in the cellulose fine fiber slurry 3 was 118 nm.
[0214] (Comparative slurry manufacturing example) In a manufacturing example of cellulose fine fiber slurry 1, an SDR14 lab refiner (pressurized disk type) manufactured by Aikawa Iron Works Co., Ltd. was used as the disk refiner device, and in the beating process with a clearance between disks of 1 mm, the CSF value decreased and the beating process was terminated when it reached about 600, and other than that no refining process using a high-pressure homogenizer was performed, a cellulose fiber slurry was obtained in the same manner as for cellulose fine fiber slurry 1. The average fiber diameter of the cellulose fibers contained in the cellulose fiber slurry was 15,000 nm.
[0215] [Cut fiber] (Cut Fiber 1) Cut fibers (3.0 mm long) made of polyethylene terephthalate were weighed, water was added, and the mixture was stirred for 4 minutes in a household mixer to obtain a slurry (solid content concentration: 1.5% by mass) of cut fibers 1. The average fiber diameter of the cut fibers in the slurry was 3.0 μm.
[0216] (Cut Fiber 2) Cut fibers (3.0 mm long) made of polyethylene terephthalate were weighed, water was added, and the mixture was stirred for 4 minutes in a household mixer to obtain a slurry (solid content concentration: 1.5% by mass) of cut fibers 2. The average fiber diameter of the cut fibers in the slurry was 10.0 μm.
[0217] (Cut Fiber 3) PA6 cut fibers (5.0 mm long) were weighed, water was added, and the mixture was stirred for 4 minutes in a household mixer to obtain a slurry (solid content concentration: 1.5% by mass) of cut fibers 3. The average fiber diameter of the cut fibers in the slurry was 11.0 μm.
[0218] (Cut Fiber 4) Cut fibers (3.0 mm long) made of PA66 were weighed, water was added, and the mixture was stirred for 4 minutes in a household mixer to obtain a slurry (solid content concentration: 1.5% by mass) of cut fibers 4. The average fiber diameter of the cut fibers in the slurry was 11.0 μm.
[0219] (Cut Fiber 5) Cut polypropylene fibers (5.0 mm long) were weighed, water was added, and the mixture was stirred for 4 minutes in a household mixer to obtain a slurry (solid content concentration: 1.5% by mass) of cut fibers 5. The average fiber diameter of the cut fibers in the slurry was 5.9 μm.
[0220] (Cut Fiber 6) Cut fibers (5.0 mm long) made of polyphenylene sulfide were weighed, water was added, and the mixture was stirred for 4 minutes in a household mixer to obtain a slurry (solid content concentration: 1.5% by mass) of cut fibers 6. The average fiber diameter of the cut fibers in the slurry was 9.3 μm.
[0221] (Cut Fiber 7) Fibrillated cut polyethylene fibers (0.9 mm long) were weighed, water was added, and the mixture was stirred for 4 minutes in a household mixer to obtain a slurry (solid content: 1.5% by mass) of cut fibers 7. The average fiber diameter of the cut fibers in the slurry was 8.0 μm.
[0222] [Irregular particles] (irregular particles 1) Irregular particles 1 obtained by pulverizing a phenolic resin foam were weighed, water was added, and the mixture was stirred for 4 minutes in a household mixer to obtain a slurry (solid content concentration: 1.5% by mass) of irregular particles 1. The average minor axis diameter of the irregular particles 1 in the slurry was 10.0 μm.
[0223] (irregular particles 2) Irregular particles 2 obtained by pulverizing a phenolic resin foam were weighed, water was added, and the mixture was stirred for 4 minutes in a household mixer to obtain a slurry (solid content concentration: 1.5% by mass) of irregular particles 2. The average minor axis diameter of the irregular particles 2 in the slurry was 50.0 μm.
[0224] <Production of composite molded body> [Example 1] Using the cellulose fine fibers 1 and the cut fibers 1, a composite molded body 1 was produced according to the following procedure. The slurry of Slurry Production Example 1 and the slurry of Cut Fiber 1 were mixed to a solid content mass ratio of 10:90, diluted with water to a solid content concentration of 0.8 mass%, and stirred for 4 minutes with a household mixer to prepare 800 g of papermaking slurry. While stirring 781.25 g of the papermaking slurry with a Three-One Motor, 3.75 g of cationic blocked polyisocyanate (product name "Meikanate CX", manufactured by Meisei Chemical Industry Co., Ltd., diluted with water to a solid content concentration of 1.0 mass%) was dropped, and then stirred for 3 minutes to obtain a papermaking slurry (total 785 g). The mass ratio of the cationic blocked polyisocyanate added was 3 mass% relative to the solid content mass of the cellulose fine fibers. Plain weave fabric made of PET / nylon blend {NT20 manufactured by Shikishima Canvas Co., Ltd., water permeation amount at 25°C under air: 0.03 ml / (cm 2 The paper was placed on a batch-type papermaking machine (Kumagaya Riki Kogyo Co., Ltd., automatic square sheet machine, 25 cm x 25 cm, 80 mesh) with a basis weight of 115 g / m2. 2 The papermaking slurry prepared above was poured into the mold, with the composite molding of the above as a guide, and then papermaking (dehydration) was carried out at a reduced pressure of 50 KPa relative to atmospheric pressure.
[0225] The wet paper made of the concentrated composition in a wet state placed on the filter cloth was peeled off from the wire and subjected to a pressure of 1 kg / cm 2The wet paper was pressed for 1 minute at a pressure of 1000 g / m. The wet paper surface was placed in contact with the drum surface, and the wet paper / filter cloth two-layer state was dried for about 120 seconds in a drum dryer with a surface temperature set to 130°C. Of the resulting dried two-layer body, the filter cloth was peeled off from the composite molded body and heat-treated for 5 minutes in an oven heated to 180°C to obtain a white composite molded body S1 (25 cm x 25 cm, basis weight 115 g / m). 2 ) was obtained.
[0226] [Example 2] A composite molded body S2 (25 cm × 25 cm, basis weight 115 g / m) was produced in the same manner as in Example 1, except that the slurry of Slurry Production Example 1 and the slurry of Cut Fiber 1 were mixed in a solid content mass ratio of 20:80. 2 ) was prepared.
[0227] [Example 3] A composite molded body S3 (25 cm × 25 cm, basis weight 115 g / m) was produced in the same manner as in Example 1, except that the slurry of Slurry Production Example 1 and the slurry of Cut Fiber 1 were mixed in a solid content mass ratio of 40:60. 2 ) was prepared.
[0228] [Example 4] A composite molded body S4 (25 cm × 25 cm, basis weight 115 g / m) was produced in the same manner as in Example 1, except that the slurry of Slurry Production Example 1 and the slurry of Cut Fiber 1 were mixed in a solid content mass ratio of 60:40. 2 ) was prepared.
[0229] The sound absorption coefficient of the composite molded body S4 was measured using one sheet or when the composite molded body S4 was stacked with three, six or ten sheets. The results are shown in Figure 3. As shown in Figure 3, the sound absorption coefficient peak had a sharp shape, and the peak sound absorption coefficient value was extremely high. In addition, as the number of stacked sheets of the sheet-like composite molded body increased, the sound absorption coefficient peak shifted to the lower frequency side, but almost no decrease in the sound absorption coefficient was observed. The above results showed that the composite molded body S4 can be applied to absorbing sound in a specific frequency range.
[0230] [Example 5] A composite molded body S5 (25 cm × 25 cm, basis weight 115 g / m) was produced in the same manner as in Example 1, except that the slurry of Slurry Production Example 1 and the slurry of Cut Fiber 1 were mixed in a solid content mass ratio of 80:20. 2 ) was prepared. [Example 6] The slurry of Slurry Production Example 2 and the slurry of Cut Fiber 1 were mixed in a solid content mass ratio of 20:80 to prepare 1,520 g of a slurry with a solid content concentration of 1.25 mass %. The same procedure as in Example 1 was repeated to prepare a composite molded body S6 (25 cm × 25 cm, basis weight 310 g / m 2 ) was prepared.
[0231] [Example 7] A composite molded body S7 (25 cm × 25 cm, basis weight 110 g / m) was produced in the same manner as in Example 1, except that the slurry of Slurry Production Example 2 and the slurry of Cut Fiber 1 were mixed in a solid content mass ratio of 40:60. 2 ) was prepared.
[0232] [Example 8] A composite molded body S8 (25 cm × 25 cm, basis weight 110 g / m) was produced in the same manner as in Example 1, except that the slurry of Slurry Production Example 2 and the slurry of Cut Fiber 1 were mixed in a solid content mass ratio of 60:40. 2 ) was prepared.
[0233] [Example 9] A composite molded body S9 (25 cm × 25 cm, basis weight 120 g / m) was produced in the same manner as in Example 1, except that the slurry of Slurry Production Example 3 and the slurry of Cut Fiber 1 were mixed in a solid content mass ratio of 20:80. 2 ) was prepared.
[0234] The sound absorption coefficient of the composite molding S9 was measured with one sheet or with three, six or ten sheets stacked. The results are shown in FIG. 4. As shown in FIG. 4, the sound absorption coefficient peak had a sharp shape, similar to the composite molding S4 (Example 4), and the peak sound absorption coefficient was high, but slightly lower than that of S4. Also, similar to the composite molding S4, the sound absorption coefficient peak shifted to the lower frequency side as the number of stacked sheets of the sheet-like composite molding increased, but almost no decrease in the sound absorption coefficient was observed. The above results showed that the composite molding S9 can be applied to absorbing sound in a specific frequency range.
[0235] [Example 10] A composite molded body S10 (25 cm × 25 cm, basis weight 115 g / m) was produced in the same manner as in Example 1, except that the slurry of Slurry Production Example 1 and the slurry of Cut Fiber 2 were mixed in a solid content mass ratio of 20:80. 2 ) was prepared.
[0236] [Example 11] A composite molded body S11 (25 cm × 25 cm, basis weight 110 g / m) was produced in the same manner as in Example 1, except that the slurry of Slurry Production Example 2 and the slurry of Cut Fiber 2 were mixed in a solid content mass ratio of 20:80. 2 ) was prepared.
[0237] [Example 12] The composite molded body S6 was treated at 130°C and 40 kN for 1 minute using a manual hydraulic vacuum heating press to obtain a composite molded body S12 (25 cm x 25 cm, basis weight 110 g / m 2 ) was prepared.
[0238] [Example 13] A composite molded body S13 (25 cm × 25 cm, basis weight 110 g / m) was prepared in the same manner as in Example 12, except that the composite molded body S8 was used. 2 ) was prepared.
[0239] [Example 14] The slurry of Slurry Production Example 1 and the slurry of Cut Fiber 3 were mixed in a solid content mass ratio of 20:80, and a composite molded body S14 (25 cm × 25 cm, basis weight 100 g / m) was produced in the same manner as in Example 1, except that the addition of blocked polyisocyanate and heat treatment were not performed. 2 ) was prepared.
[0240] [Example 15] A composite molded body S15 (25 cm × 25 cm, basis weight 100 g / m) was produced in the same manner as in Example 1, except that the slurry of Slurry Production Example 2 and the slurry of Cut Fiber 3 were mixed in a solid content mass ratio of 20:80. 2 ) was prepared.
[0241] [Example 16] A composite molded body S16 (25 cm × 25 cm, basis weight 100 g / m) was produced in the same manner as in Example 1, except that the slurry of Slurry Production Example 2 and the slurry of Cut Fiber 3 were mixed in a solid content mass ratio of 40:60. 2 ) was prepared.
[0242] [Example 17] A composite molded body S17 (25 cm × 25 cm, basis weight 100 g / m) was produced in the same manner as in Example 1, except that the slurry of Slurry Production Example 2 and the slurry of Cut Fiber 3 were mixed in a solid content mass ratio of 60:40. 2 ) was prepared.
[0243] [Example 18] A composite molded body S18 (25 cm × 25 cm, basis weight 100 g / m) was produced in the same manner as in Example 1, except that the slurry of Slurry Production Example 2 and the slurry of Cut Fiber 4 were mixed in a solid content mass ratio of 40:60. 2 ) was prepared.
[0244] [Example 19] The slurry of Slurry Production Example 1 and the slurry of Cut Fibers 5 were mixed to a solid content mass ratio of 20:80, and a papermaking dispersant (product name "Meikasurf MK-37", manufactured by Meisei Chemical Industry Co., Ltd., diluted with water to a solid content concentration of 1.0 mass %) was added instead of the blocked isocyanate (the mass ratio of the papermaking dispersant added was 3 mass % based on the total solid content mass of the cellulose fine fibers and the cut fibers). A composite molded body S19 (25 cm × 25 cm, basis weight 100 g / m) was produced in the same manner as in Example 1, except that 2 ) was prepared.
[0245] [Example 20] The slurry of Slurry Production Example 2 and the slurry of Cut Fiber 5 were mixed in a solid content mass ratio of 20:80, and the mixture was diluted with water to a solid content concentration of 0.4 mass%. The same procedure as in Example 19 was repeated to produce a composite molded body S20 (25 cm × 25 cm, basis weight 50 g / m 2 ) was prepared.
[0246] [Example 21] A composite molded body S21 (25 cm × 25 cm, basis weight 100 g / m) was produced in the same manner as in Example 19, except that the slurry of Slurry Production Example 2 and the slurry of Cut Fiber 6 were mixed in a solid content mass ratio of 40:60. 2 ) was prepared.
[0247] [Example 22] A composite molded body S22 (25 cm × 25 cm, basis weight 115 g / m) was produced in the same manner as in Example 19, except that the slurry of Slurry Production Example 2 and the slurry of Cut Fiber 7 were mixed in a solid content mass ratio of 20:80. 2 ) was prepared.
[0248] [Example 23] A composite molded body S23 (25 cm × 25 cm, basis weight 115 g / m) was produced in the same manner as in Example 19, except that the slurry of Slurry Production Example 2 and the slurry of Cut Fiber 7 were mixed in a solid content mass ratio of 60:40. 2 ) was prepared.
[0249] [Example 24] The slurry of Slurry Production Example 2 and the slurry of Cut Fiber 7 were mixed in a solid content mass ratio of 20:80, and the mixture was diluted with water to a solid content concentration of 0.4 mass%. The same procedure as in Example 19 was repeated to produce a composite molded body S24 (25 cm × 25 cm, basis weight 50 g / m 2 ) was prepared.
[0250] [Example 25] The slurry of Slurry Production Example 2 and the slurry of Irregular Particles 1 were mixed in a solid content mass ratio of 40:60, and a composite molded body S25 (25 cm × 25 cm, basis weight 100 g / m) was produced in the same manner as in Example 1, except that the addition of blocked polyisocyanate and heat treatment were not performed. 2 ) was prepared.
[0251] [Example 26] The slurry of Slurry Production Example 2 and the slurry of Irregular Particles 2 were mixed in a solid content mass ratio of 40:60, and a composite molded body S26 (25 cm × 25 cm, basis weight 100 g / m) was produced in the same manner as in Example 1, except that the addition of blocked polyisocyanate and heat treatment were not performed. 2 ) was prepared.
[0252] [Example 27] The slurry of Slurry Production Example 1 and the slurry of Cut Fiber 1 were mixed to a solid content mass ratio of 20:80, diluted with water to a solid content rate of 0.8 mass%, and stirred in a tank with an agitator. After that, a lab refiner (pressurized disk type) was used for uniform mixing treatment, and the clearance between the disks was set to 1.5 mm, and 1200 L of the aqueous dispersion was dispersed for 15 minutes. While stirring the papermaking slurry after the treatment with an agitator in a tank, cationic blocked polyisocyanate (trade name "Meikanate CX", as described above, diluted with water to a solid content concentration of 1.0 mass%) was added to the cellulose fine fibers to a solid content of 3 mass%, and stirring with the agitator was continued for 10 minutes, and a long sheet was produced by a papermaking and drying process consisting of independent parts of a papermaking part, a dehydration press part, and a drying part. Using a 0.65m wide inclined wire type continuous papermaking device (manufactured by Saito Iron Works Co., Ltd.) set at an inclination angle of 2°, a roll of polyethylene terephthalate cut fiber / cellulose fiber mixed paper (width 0.7m) (binder processed) was placed on a polymer wire (Nihon Filcon Co., Ltd. LTT-9FE) in front of the papermaking dispersion liquid input section as a support, and the papermaking slurry obtained above was supplied on it at a supply rate of 65.4L / min, the papermaking speed was set to 7m / min in the running direction, and wet suction (inclined section) and dry suction were operated to perform continuous papermaking. After papermaking, functional paper (width 0.7m) (thermally melted) made of polyethylene terephthalate cut fiber was continuously placed on top of the composite molded wet paper / support as an interleaf paper, and the three-layer structure of interleaf paper / composite molded wet paper / support was dehydrated by a metal roll, and the three-layer structure was transported to the drying part. In the drying section, the composite was dried using a drum dryer with a surface temperature set to 100°C, and immediately after drying, the composite was peeled off from the upper and lower interleaving papers and support to produce a long composite product S27 (approximately 15 m long).
[0253] [Comparative Example 1] A comparative composite molded body RS1 (25 cm × 25 cm, basis weight 100 g / m) was prepared in the same manner as in Example 20, except that the solid content was diluted with water to 0.4 mass%. 2 ) was obtained.
[0254] [Comparative Example 2] A comparative composite molded body RS2 (25 cm × 25 cm, basis weight 115 g / m) was produced in the same manner as in Example 1, except that the slurry of Slurry Production Example 1 and the slurry of Cut Fiber 1 were mixed in a solid content mass ratio of 2:98. 2 ) was obtained.
[0255] [Comparative Example 3] The slurry of Slurry Production Example 1 and the slurry of Cut Fiber 1 were mixed in a solid content mass ratio of 20:80, and the mixture was diluted with water to a solid content concentration of 0.36 mass%. The same procedure as in Example 1 was repeated to produce a comparative composite molded body RS3 (25 cm × 25 cm, basis weight 45 g / m 2 ) was obtained.
[0256] [Comparative Example 4] A comparative composite molding RS4 (25 cm × 25 cm, basis weight 115 g / m) was produced in the same manner as in Example 1, except that the slurry of Comparative Slurry Production Example and the slurry of Cut Fiber 1 were mixed in a solid content mass ratio of 20:80. 2 ) was obtained.
[0257] [Comparative Example 5] Papermaking was carried out in the same manner as in Example 1, except that the slurry of Slurry Production Example 1 and the slurry of Cut Fiber 1 were mixed in a solid mass ratio of 95:5. However, since drainage did not progress, a comparative composite molding RS5 could not be obtained.
[0258] [Comparative Example 6] A comparative composite molded body RS6 (25 cm x 25 cm, basis weight 50 g / m) was prepared in the same manner as in Example 24, except that no papermaking dispersant was added. 2 ) was prepared.
[0259] [Comparative Example 7] A composite molding RS7 (25 cm × 25 cm, basis weight 50 g / m) was produced in the same manner as in Comparative Example 6, except that the slurry of Slurry Production Example 2 and the slurry of Cut Fiber 7 were mixed in a solid content mass ratio of 10:90. 2 ) was prepared.
[0260] [Comparative Example 8] The cut fibers 1 were diluted with water to a solid content of 0.8% by mass, and the mixture was stirred with an agitator in a tank for 20 minutes. Using an inclined wire type continuous papermaking machine (manufactured by Saito Iron Works Co., Ltd.) with a width of 0.65 m set at an inclination angle of 2°, the papermaking slurry obtained above was fed onto a polymer wire (Nihon Filcon Co., Ltd. LTT-9FE) at a feed rate of 65.4 L / min, the papermaking speed was set to 7 m / min in the running direction, and wet suction (inclined part) and dry suction were operated to carry out continuous papermaking. After papermaking, dehydration was performed using a metal roll, and the obtained sheet was transported to the drying part. In the drying part, the sheet was dried using a drum dryer with a surface temperature set to 100°C, and a long product RS8 (approximately 15 m long) was produced.
[0261] The composition ratio of cellulose fine fibers and cut fibers in the composite molded body was determined by strongly dispersing the composite molded body in water using a mixer, leaving it to stand to separate them based on the difference in specific gravity, and weighing the weight of each fiber after drying. The amount of crosslinking agent can be estimated by subtracting the weight of the fiber component from the total weight of the composite molded body, assuming that the yield rate of the fiber component is 100%.
[0262] <Preparation of resin molded body> [Example 28] The composite molded body S22 was cut into a 10 cm square, and sandwiched between a polyethylene terephthalate film, a mirror-finished SUS plate, thick paper, and an iron plate from both sides of the composite molded body S22 in that order from the side closest to the composite molded body S22, and pressed for 30 minutes at 180°C and 80 kN in a manual hydraulic vacuum heating press. After the heat pressing, the sample was removed from the press and cooled to room temperature over 20 minutes while being pressurized to 10 kN by another press. The cooled sample was peeled off from the polyethylene terephthalate film to obtain a highly transparent resin molded body S28 (thickness 100 μm). The linear thermal expansion coefficient of the resin molded body S28 at 0 to 60°C was measured to be 86 ppm / °C, which was reduced to 53% of the linear thermal expansion coefficient of the polyethylene film alone (Comparative Example 9 described later).
[0263] [Example 29] The composite molded body S27 was cut into a 10 cm square, sandwiched between four polypropylene films each having a thickness of 50 μm on both sides, and then sandwiched between a polyethylene terephthalate film, a mirror-finished SUS plate, thick paper, and an iron plate from both sides in that order from the side closest to the composite molded body S27, and pressed at 180°C and 80 kN for 30 minutes in a manual hydraulic vacuum heating press. After the heat pressing, the sample was removed from the press and cooled to room temperature over 20 minutes while being pressurized to 10 kN by another press. The cooled sample was peeled off from the polyethylene terephthalate film to obtain a resin molded body S29 (thickness 400 μm). The linear thermal expansion coefficient of the resin molded body S29 at 0 to 60°C was measured to be 49 ppm / °C, which was reduced to 58% of the linear thermal expansion coefficient of the polypropylene film alone (Comparative Example 10 described later).
[0264] [Example 30] The composite molded body S27 was cut into 10 cm squares, and a bisphenol A type epoxy resin varnish containing an imidazole-based curing agent was applied to a polyethylene terephthalate film using a bar coater, impregnated into the composite molded body S27, and treated in an oven heated to 120 ° C for 15 minutes. The obtained slightly cured film (thickness 450 μm) was peeled off from the polyethylene terephthalate film, and the slightly cured epoxy resin composite film was sandwiched between a new polyethylene terephthalate film and a metal plate on both sides, and pressed under vacuum at 120 ° C and 30 kN for 10 minutes using a manual hydraulic vacuum heating press. After this, the temperature was raised to 190 ° C over 10 minutes while applying pressure at 50 kN. After reaching 190 ° C, pressure was continued at 50 kN for 60 minutes. After this, the sample was removed from the above press device, cooled to room temperature, and then peeled off from the polyethylene terephthalate film to obtain a resin molded body S30 (thickness 400 μm). The linear thermal expansion coefficient of the resin molding S30 at 0 to 60° C. was measured and found to be 25 ppm / ° C., which was reduced to 19% of the linear thermal expansion coefficient of the epoxy resin film alone (Comparative Example 11 described later).
[0265] [Comparative Example 9] A molded body was produced in the same manner as in Example 22, except that only the slurry of Cut Fibers 7 was used instead of the mixture of the slurry of Slurry Production Example 2 and the slurry of Cut Fibers 7, and a polyethylene film was produced from the molded body in the same manner as in Example 28. The linear thermal expansion coefficient of the obtained polyethylene film (thickness 100 μm) at 0 to 60° C. was measured and found to be 161 ppm / ° C.
[0266] [Comparative Example 10] The linear thermal expansion coefficient of the same polypropylene film (thickness: 400 μm) as used in Example 29 at 0 to 60° C. was measured and found to be 84 ppm / ° C.
[0267] [Comparative Example 11] On a polyethylene terephthalate film, the same epoxy resin varnish as that used in Example 30 was applied by a bar coater, and the film was treated in an oven heated to 120°C for 15 minutes. The resulting slightly cured film (thickness 450μm) was peeled off from the polyethylene terephthalate film, and the slightly cured epoxy resin film was sandwiched between a new polyethylene terephthalate film and a metal plate on both sides, and pressed at 120°C and 30kN for 10 minutes under vacuum using a manual hydraulic vacuum heating press. After this, the temperature was raised to 190°C over 10 minutes while applying pressure at 50kN. After reaching 190°C, pressure was continued at 50kN for 60 minutes. After this, the sample was removed from the press and cooled to room temperature, and the linear thermal expansion coefficient at 0 to 60°C of the film (thickness 400μm) obtained by peeling it off from the polyethylene terephthalate film was measured, and it was 130ppm / °C.
[0268] <Performance evaluation> <Cellulose microfibers> [Average fiber diameter] Water in the cellulose fine fiber slurry was gradually replaced with tert-butanol to obtain a dispersion liquid, from which a wet paper sheet was prepared by a filtration method and dried to obtain a sample for fiber diameter evaluation. The surface of the sample for fiber diameter evaluation was observed with a scanning electron microscope (SEM) at a magnification of 10,000 to 100,000 times according to the average fiber diameter of the fine fibers. The fiber diameter of each fiber was measured from the obtained SEM image, and the number average value was taken as the average fiber diameter.
[0269] <Cut fiber> [Average fiber diameter and average fiber length] A wet paper sheet was prepared from the aqueous dispersion of the cut fibers by a filtration method, and dried to obtain a sample for fiber diameter evaluation. The surface of the sample for fiber diameter evaluation was observed with a scanning electron microscope (SEM) at a magnification of 250 to 2000 times depending on the average fiber diameter and average fiber length of the fibers. From the obtained SEM image, the fiber diameter and fiber length of each fiber were measured, and the number average value of 20 fibers was taken as the average fiber diameter and average fiber length.
[0270] <Irregular particles> [Average minor axis diameter and average major axis diameter] A wet paper sheet was prepared from an aqueous dispersion of irregular particles by filtration, and dried to obtain a sample for particle size evaluation. The surface of the sample for particle size evaluation was observed with a scanning electron microscope (SEM) at a magnification of 250 to 2000 times depending on the average minor axis diameter and average major axis diameter of the particles. From the obtained SEM image, the minor axis diameter and major axis diameter of each particle were measured, and the number average value of 20 particles was taken as the average minor axis diameter and average major axis diameter.
[0271] <Composite molded body> Thickness The thickness of the sample, which had been conditioned at room temperature of 20° C. and humidity of 50% RH, was measured at nine points using an automatic micrometer manufactured by Hybridge Seisakusho, and the number average value was regarded as the thickness of the sample.
[0272] [Metaku] The basis weight of the sheet was calculated in accordance with JIS P 8124.
[0273] [Tensile strength] Two samples of 200 mm in length and 15 mm in width were cut from the composite molded body. For each of Example 27 and Comparative Example 8 (i.e., continuous papermaking examples), two samples were cut out whose length direction was the MD direction and two samples were cut out whose length direction was the TD direction. For each of the other examples (i.e., batch-type papermaking examples), two samples were cut out whose length direction was an arbitrarily selected direction. First, the dry tensile strength was measured using a tabletop horizontal tensile tester (No. 2000) manufactured by Kumagai Riki Kogyo Co., Ltd. according to the method defined in JIS P 8113, and the number average value of the two samples was taken as the dry strength (kg / 15 mm).
[0274] [Air resistance and its coefficient of variation] A composite molded body of 20 cm x 20 cm was conditioned under an atmosphere of room temperature 23°C and humidity 50%RH. The conditioned sample was measured for air resistance at nine points using a Gurley densometer (manufactured by Toyo Seiki Co., Ltd., model G-B2C) or an Oken air resistance tester (manufactured by Asahi Seiko Co., Ltd., model EG01) with a circle of 2.5 cm in diameter as the measurement area, and the number average value was taken as the air resistance (average air resistance) of the sample. In addition, the standard deviation of the air resistance was divided by the average air resistance to calculate the coefficient of variation of the air resistance.
[0275] [Porosity] The porosity of a composite molding containing cellulose fine fibers and an organic filler in a mass ratio of X (%):Y (%) is calculated by setting the density of the cellulose fine fibers at 1.5 g / cm 3 It was calculated using the following formula. Porosity (%) = 100 - ([Weight (g / m 2 ) / {Thickness of composite molded body (μm) × (1.5 (g / cm 3 )×X / 100+specific gravity of organic filler (g / cm 3 )×Y / 100)}]×100)
[0276] [Peelability] The peelability of the dried composite molded product from the filter cloth was visually judged, with good peelability being rated ".largecircle.", moderate peelability being rated ".DELTA.", and poor peelability being rated "x."
[0277] [Market conditions] The texture of the obtained composite molded body was visually judged, with a good texture being rated ".largecircle.", a fair texture being rated ".DELTA.", and a poor texture being rated "x." The results are shown in Tables 1 to 3.
[0278] [Sound absorption coefficient] A circular disk with a diameter of 16.5 mm was cut out from the composite molded sample, and measurements were performed using a normal incidence sound absorption coefficient measurement system Winzac-MTX manufactured by Nihon Onkyo Engineering Co., Ltd., under the condition of a 15 mm pipe (effective frequency: 400 to 12,000 Hz). A loose support holder was used, and measurements were performed with one composite molded piece or multiple composite molded pieces stacked together with no (zero) air space behind them.
[0279] [Linear thermal expansion coefficient] The obtained resin molded body was heat-treated at 80°C for 24 hours, and then cut into a width of 3 mm and a length of 25 mm in an arbitrarily selected direction to prepare a measurement sample. Using a thermomechanical analysis (TMA) device (Q400-EM manufactured by TA Instruments), the average linear thermal expansion coefficient was determined between 0 and 60°C when the temperature was raised from -40°C to 100°C at 5°C / min. in a nitrogen atmosphere with a chuck distance of 8 mm and a load of 0.05 N in tension mode.
[0280] [Table 1]
[0281] [Table 2]
[0282] [Table 3] [Industrial Applicability]
[0283] The composite molded product according to the present invention can be suitably used as a core material for fiber reinforced resins, a sound absorbing material, and the like.
Claims
1. A composite molded body containing cellulose fine fibers and an organic filler, The average fiber diameter of the cellulose fine fibers is 5 nm or more and 2 μm or less, The content of the cellulose fine fibers in the composite molded body is 3% by mass or more and 90% by mass or less, The composite molding has a basis weight of 50 g / m 2 More than 1000g / m 2 is as follows: The average air resistance of the composite molded body is 0.5 sec / 100 mL or more and 100,000 sec / 100 mL or less, The coefficient of variation of air resistance, which is the standard deviation of the air resistance of the composite molded body divided by the average air resistance, is 0.5 or less; The average minor axis diameter of the organic filler is 0.1 μm or more and 100 μm or less, The thickness of the composite molded body is 100 μm or more and 10,000 μm or less. Composite molded body.
2. 2. The composite molded product according to claim 1, having a tensile strength of 0.1 kg / 15 mm or more and 40 kg / 15 mm or less.
3. The composite molding according to claim 1 or 2, wherein the organic filler is a fibrillated cut fiber.
4. a reactant derived from a crosslinking agent is uniformly distributed between the cellulose fine fibers, between the organic filler, and / or between the cellulose fine fibers and the organic filler in the composite molded body in a planar direction of the composite molded body, The composite molded body according to any one of claims 1 to 3, wherein the mass ratio of the reactant to the total mass (100 mass%) of the cellulose fine fibers and the organic filler is 0.1 to 100 mass%.
5. The composite molded body of claim 4 , wherein the reactants include urethane linkages.
6. The composite molded body according to any one of claims 1 to 5, wherein the organic filler is made of a thermoplastic resin.
7. The composite molded body according to claim 6, wherein the thermoplastic resin comprises at least one selected from the group consisting of polyolefins, polyesters, polyamides, acrylic polymers, polyvinyl alcohols, polylactic acids, polyphenylene ethers, polyoxymethylenes, and polyphenylene sulfides.
8. 8. The composite molded body according to claim 6, wherein the melting point of the thermoplastic resin is 50°C or higher and 500°C or lower.
9. The composite molded product according to any one of claims 1 to 8, which is a sheet.
10. The composite molded body according to any one of claims 1 to 9, which is a curved molded body, a box-shaped molded body, or a cone-shaped molded body.
11. A method for producing a composite molded body according to any one of claims 1 to 10, A slurry preparation step of preparing a slurry containing cellulose fine fibers, an organic filler, and a liquid medium containing water; A concentrating step of dehydrating the slurry by a papermaking method to obtain a wet molded body; and a solidification step of at least drying the wetted molded body to obtain a composite molded body; A method comprising:
12. The method according to claim 11, wherein the solids content of the slurry is 0.2% by mass to 1.5% by mass.
13. the slurry further comprises a reactive cross-linking agent; The method according to claim 11 or 12, wherein in the slurry preparation step, or simultaneously with or after the drying, the reactive crosslinking agent is reacted to crosslink between the cellulose fine fibers, between the organic fillers, and / or between the cellulose fine fibers and the organic filler.
14. the reactive crosslinking agent is a blocked polyisocyanate; The method of claim 13, wherein the reaction is carried out at or above the deblocking temperature of the blocked polyisocyanate.
15. The method of claim 14, wherein the blocked polyisocyanate is a cationic blocked polyisocyanate.
16. The method according to any one of claims 13 to 15, wherein the drying is carried out at 80°C or more and 120°C or less, and then the reaction is carried out at 130°C or more and 220°C or less.
17. The method according to any one of claims 13 to 16, wherein in the slurry preparation step, a premix is prepared by mixing cellulose fine fibers, a reactive crosslinking agent, and a liquid medium, and then the premix is mixed with an organic filler to obtain the slurry.
18. The method according to any one of claims 13 to 16, wherein in the slurry preparation step, a premix is prepared by mixing cellulose fine fibers, an organic filler, and a liquid medium, and then the premix is mixed with a reactive crosslinking agent to obtain the slurry.
19. A fiber composition which is a shredded product of the composite molding according to any one of claims 1 to 10.
20. 20. The fiber composition of claim 19, wherein the shredded material is granular.
21. 20. The fiber composition of claim 19, wherein the shreds are pellets.
22. A method for producing a resin molded product containing cellulose fine fibers and a resin, comprising: A mixing step of mixing the fiber composition according to any one of claims 19 to 21 with a resin to obtain a mixture; and a molding step of molding the mixture; A method comprising:
23. The organic filler in the fiber composition comprises a thermoplastic resin; the resin comprises a thermoplastic resin, 23. The method of claim 22, wherein the fiber composition and the resin are melt mixed in the mixing step.
24. 24. The method of claim 22 or 23, wherein the molding is selected from the group consisting of extrusion and injection molding.
25. A method for producing a resin molded product containing cellulose fine fibers and a resin, comprising: A composite molded body forming step of forming a composite molded body containing cellulose fine fibers and an organic filler containing a thermoplastic resin by the method according to any one of claims 11 to 18; a molding step of molding the composite molded body at a temperature equal to or higher than the melting point of the thermoplastic resin in the organic filler; A method comprising:
26. A method for producing a resin molded product containing cellulose fine fibers and a resin, comprising: A composite molded body forming step of forming a composite molded body containing cellulose fine fibers and an organic filler by the method according to any one of claims 11 to 18; a molding step of impregnating the composite molded body with a resin and then solidifying the resin; A method comprising:
27. 27. The method according to claim 26, wherein the resin to be impregnated is a heated melt of a thermoplastic resin, and the solidification is a cooling solidification.
28. the organic filler comprises a thermoplastic resin; 28. The method of claim 27, wherein the impregnated resin is a hot melt of a thermoplastic resin having a lower melting point than the thermoplastic resin in the organic filler.
29. The method according to claim 26, wherein the resin to be impregnated is an uncured or semi-cured thermosetting resin or photocurable resin, and the solidification is curing.
30. The method according to any one of claims 25 to 29, wherein the molding step is carried out by mold pressing.
31. The method according to any one of claims 25 to 30, wherein the resin molded article is an automobile part.
32. A sound-absorbing material comprising the composite molded body according to any one of claims 1 to 10.
33. An air filter comprising the composite molded body according to any one of claims 1 to 10.
34. An automobile part material comprising the composite molded body according to any one of claims 1 to 10.
Citation Information
Patent Citations
Low density body
JP1998245792A
Cellulosic nonwoven fabric and method for manufacturing the same, and separator
JP2013104142A
Composite sheet material and production method thereof
JP2015014078A
Sheet and molded body
JP2017082071A
Fine cellulose fiber sheet
WO2015008868A1
Cited By
Hydrophobized modified-cellulose-containing material and method for producing same
WO2026110849A1