Coated film piece combustion inhibition type peeling agent and coated film peeling method
A paint film stripping agent using alcohols, paraffins, and thixotropic agents forms a moisture-rich layer to prevent ignition of peeled paint film pieces, addressing the fire risk of water-based strippers while maintaining peelability.
Patent Information
- Application Number
- JP2024129737
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-04-15
- Filing Date
- 2024-08-06
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-04-13
AI Technical Summary
Existing water-based paint film strippers pose a risk of igniting peeled paint film pieces due to the presence of organic components, which can catch fire, and increasing water content to mitigate this risk compromises peelability and workability.
A paint film stripping agent composed of alcohols, including aromatic alcohols, paraffins with a melting point of 65°C or less, a thixotropic agent, and a low polarity solvent, forming a water-containing emulsion film that is maintained for a specified time to suppress ignition.
The agent effectively prevents the ignition and combustion of peeled paint film pieces by maintaining a moisture-rich layer that inhibits evaporation, ensuring safe paint film removal.
Smart Images

Figure 2024144729000001 
Figure 2024144729000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a novel paint stripper capable of suppressing combustion of peeled paint pieces, and a paint stripping method using the paint stripper. [Background technology]
[0002] For example, structures such as bridges, storage tanks, exterior staircases, and water gates (especially metal structures) are painted to enhance their corrosion resistance (rust prevention) and weather resistance, but when they are repaired, some or all of the paint is repainted.
[0003] When repainting a metal structure, it is necessary to remove the old paint film (which should be peeled off) from the surface of the structure before applying a new coat of paint. There are two methods for removing this paint film: physical and chemical.
[0004] Physical methods include, for example, a blasting method, a grinding method using a disk sander, etc. Although these methods are excellent in terms of removal speed, they generate a large amount of dust, which has a negative impact on workers and the surrounding environment.
[0005] A method of chemically removing the coating film includes a method of using a coating film stripper. Coating film strippers are broadly divided into solvent-based coating film strippers and water-based coating film strippers. Since the solvent-based coating film stripper is a stripper containing an organic solvent as the main component, there is a problem of pollution of the working environment due to the evaporation of the organic solvent, and there is also a risk of the evaporated organic solvent catching fire. Since the water-based coating film stripper contains water, it is a relatively safe coating film stripper.
[0006] For this reason, water-based paint stripping agents have come into widespread use in recent years, and various types of stripping agents have actually been developed.
[0007] For example, a coating remover is known which contains (A) a monohydric or dihydric alcohol solvent or a derivative thereof having a boiling point of 100°C or higher, (B) water, and (C) a rheology control agent, wherein component (C) is a metal soap which is a non-alkali metal salt and has a viscosity adjusted to 25 Pa s or less (25°C) (Patent Document 1).
[0008] Further, for example, a coating stripping composition is known that has a pH in the range of 5 to 9 and contains water, benzyl alcohol, and at least one type of cellulose derivative (Patent Document 2). [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Patent Publication 2019-131651 [Patent Document 2] International Publication WO2018 / 179925 Summary of the Invention [Problem to be solved by the invention]
[0010] However, even if a water-based paint stripper is used, there is a risk of the paint pieces catching fire after removal. The reason is unclear, but when a water-based paint stripper is applied to an old paint film and the stripping work is performed, the paint pieces are in a flammable state because the organic components contained in the water-based paint stripper are attached to them in addition to the organic components contained in the original paint film, and it is assumed that the paint pieces are ignited by some ignition source in that state, causing the paint pieces to burn. In this case, it is possible to increase the water content in the water-based paint stripper, but increasing the water content not only reduces the stripping ability, but also may cause a decrease in workability.
[0011] For this reason, there is a strong demand for a stripping agent that can suppress the ignition of peeled off pieces of paint film, but at present, such a stripping agent has not yet been developed.
[0012] Therefore, a primary object of the present invention is to provide a paint stripper that can effectively suppress ignition of peeled paint pieces. [Means for solving the problem]
[0013] As a result of extensive research conducted in light of the problems in the prior art, the present inventors discovered that the above-mentioned object can be achieved by using a composition containing specific components as a coating film remover, and thus completed the present invention.
[0014] That is, the present invention relates to the following paint piece combustion suppressing stripping agent and paint film stripping method. 1. An aqueous emulsion-based paint film stripper for stripping paint films, comprising: (1) The release agent is (1a) Alcohols, including aromatic alcohols; (1b) Paraffins having a melting point of 65°C or less; (1c) at least one of a thixotropic agent and a low-polarity solvent having a solubility parameter of 20 or less, and (1d) Water and (2) The water-containing emulsion film formed by the release agent is maintained at a temperature of 15°C for at least 6 hours from immediately after application of the release agent. A paint film combustion suppressing stripping agent characterized by the above. 2. The paint piece burn-retardant stripping agent according to item 1, wherein the paraffin content is 0.1 to 5% by weight. 3. The paint piece combustion retardant stripper according to item 1 or 2, further comprising at least one of a surfactant and a thickener. 4. A method for removing a coating film, comprising: (1) A step of forming a water-containing emulsion film by applying the paint film piece combustion-suppressing stripping agent described in any one of items 1 to 3 to a surface of a paint film to be stripped; (2) Aging the coated film for a certain period of time while maintaining the water-containing emulsion film; and (3) A process of peeling off the coating film having the water-containing emulsion film. A coating film peeling method comprising the steps of: 5. The amount of paint film combustion retardant stripper applied (before drying) is 0.3 to 2 kg / m 2 5. The method according to claim 4, Effect of the Invention
[0015] According to the present invention, a coating film stripper that can effectively suppress ignition of peeled coating film pieces can be provided. In particular, the stripper of the present invention employs a combination of paraffins having a melting point of 65°C or less, a thixotropic agent, and at least one low-polarity solvent having a solubility parameter of 20 or less, so that it is possible to maintain a water-containing emulsion film on the surface of the peeled coating film pieces for a relatively long period of time. As a result, it is possible to suppress ignition or combustion of the coating film pieces, so that the coating film can be peeled off more safely. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] 1. Paint film combustion retardant stripper The paint film piece combustion suppressing stripping agent of the present invention (the stripping agent of the present invention) is an aqueous emulsion-based paint film stripping agent for stripping paint films, (1) The release agent is (1a) Alcohols, including aromatic alcohols; (1b) Paraffins having a melting point of 65°C or less; (1c) at least one of a thixotropic agent and a low-polarity solvent having a solubility parameter of 20 or less, and (1d) Water and (2) The water-containing emulsion film formed by the release agent is maintained at a temperature of 15°C for at least 6 hours from immediately after application of the release agent. It is characterized by:
[0017] The stripping agent of the present invention is basically in the form of an aqueous emulsion composed of water (aqueous phase) and an oil phase containing an organic component, but a part of the organic component may be dissolved in water within a range that does not impair the effects of the present invention. By taking the form of an emulsion composed of two phases, an aqueous phase and an oil phase, when the stripping agent of the present invention is applied to the surface of the old coating film to be stripped (hereinafter also referred to as the "coating film to be stripped"), it becomes possible to more reliably form a water-containing emulsion film by the stripping agent of the present invention on the surface of the coating film to be stripped. As a result, it becomes possible to effectively suppress ignition and combustion of the stripped coating pieces. The reason for this is not clear, but it is thought to be due to the following mechanism of action. After the release agent of the present invention in the form of an emulsion is applied onto the coating film to be peeled off, the coating film formed by the release agent of the present invention forms a layer structure of "coating film to be peeled off / water-rich layer / organic component (especially paraffin)-rich layer" by aging, and the water in the water-rich layer is prevented from evaporating due to the organic component-rich layer. This state is maintained for a long period of time, and as a result, the water-rich layer suppresses ignition of the coating film pieces, or even if it does ignite temporarily, the combustion (spread of fire) is suppressed. In other words, the water-containing emulsion film is still maintained for a certain period of time in the coating film pieces after peeling, so that ignition and combustion of the coating film pieces are effectively suppressed. In the following, each component constituting the release agent of the present invention will be described.
[0018] (1a) Alcohols, including aromatic alcohols The aromatic alcohol functions primarily as a stripping component for stripping the coating film to be stripped.
[0019] The aromatic alcohol itself is not particularly limited, and examples thereof include benzyl alcohol, phenethyl alcohol, hydroxybenzyl alcohol, hydroxyphenethyl alcohol, 4-methylbenzyl alcohol, 2-ethylbenzyl alcohol, etc. Among these, benzyl alcohol is preferred. These can be used alone or in combination of two or more. These can also be used as the same release components used in known or commercially available release agents.
[0020] The content of aromatic alcohol in the release agent of the present invention can be appropriately set depending on the type and thickness of the coating film to be removed, but is usually about 30 to 80% by weight, and preferably 35 to 70% by weight.
[0021] In the present invention, alcohols other than aromatic alcohols may be contained, for example, monohydric alcohols such as methanol, ethanol, propanol, isopropyl alcohol, and butanol, and polyhydric alcohols such as ethylene glycol, propylene glycol, butylene glycol, diethylene glycol, dipropylene glycol, triethylene glycol, and glycerin.
[0022] The content of alcohols other than aromatic alcohols in the release agent of the present invention can be appropriately set depending on the type and thickness of the coating film to be removed, but it is usually about 1 to 20% by weight, and preferably 3 to 10% by weight. (1b) Paraffins having a melting point of 65°C or less (hereinafter simply referred to as "paraffins") Paraffins mainly contribute to the formation of the organic component-rich layer in the water-containing emulsion membrane.
[0023] The melting point of the paraffins is 65° C. or less, and particularly preferably 60° C. or less. If the melting point exceeds 65° C., it may be difficult to form a water-containing emulsion film. The lower limit of the melting point may be, for example, about 40° C., but is not limited thereto.
[0024] As such paraffins, for example, paraffin wax can be suitably used, but is not limited thereto. Paraffin wax is a wax that is solid at room temperature and is separated and refined from reduced pressure distillate oil, and is also called "solid wax". Paraffin wax is classified into four types, 120P, 125P, 130P, and 135P, depending on the difference in melting point (Japanese Industrial Standard JIS K2235-1991), and any type can be used in the present invention, and among them, 135P can be suitably used. These paraffins can also be commercially available products. When using commercially available products, emulsion type paraffin containing a surfactant may be used. For example, commercially available products include "Paraffin Wax-115" (manufactured by Nippon Seiro Co., Ltd.) and "AQUACER497" (manufactured by BYK-Chemie Japan Co., Ltd.).
[0025] The content of paraffins in the release agent of the present invention can be appropriately set depending on the type and thickness of the coating film to be removed, but is usually about 0.1 to 5% by weight, preferably 0.3 to 4% by weight, more preferably 0.5 to 3.5% by weight, and most preferably 0.5 to 2% by weight. Therefore, it can be set to, for example, 1 to 2% by weight.
[0026] (1c) At least one of a thixotropic agent and a low-polarity solvent having a solubility parameter of 20 or less. The thixotropic agent and at least one low polarity solvent having a solubility parameter of 20 or less are components that can mainly contribute to an excellent combustion suppressing effect in combination with the paraffins.
[0027] The thixotropic agent is also known as a thixotropic agent, and various types such as amide-based, castor oil-based, polyethylene oxide-based, and vegetable oil polymerized oil-based agents can be used. Among these, amide-based thixotropic agents can be preferably used in the present invention. In terms of properties, either powder type or paste type can be used. These thixotropic agents can also be used as commercially available products. For example, commercially available products include "Disparlon F-9030", "Disparlon 6900-20X", "Disparlon A670-20M", "Disparlon A650-20X" (all manufactured by Kusumoto Chemical Co., Ltd.), "Tallen BA-600", "Tallen M-1020XFS", "Tallen M-1021B", and "Tallen VA750B" (all manufactured by Kyoeisha Chemical Co., Ltd.).
[0028] The low polarity solvent (hereinafter, simply referred to as "low polarity solvent") having a solubility parameter (SP value) of 20 or less is not particularly limited, but various organic solvents such as ester solvents such as ethyl acetate (8.6) and butyl acetate (8.5); ketone solvents such as acetone (9.4) and cyclohexanone (9.8); ether solvents such as anisole (19.6), diethyl ether (7.4), tetrahydrofuran (9.1), and propylene glycol monomethyl ether acetate (9.1), aromatic solvents such as toluene (8.9) and xylene (8.8), and petroleum solvents such as naphtha (7.6) and mineral spirits (6.9) can be used. Among these, at least one of anisole and naphtha can be preferably used. The values in parentheses are literature values of the SP value.
[0029] The solubility parameter (SP value) in the present invention may be either a literature value or an actual measurement value, but if the two are significantly different, it is desirable to adopt the actual measurement value. The actual measurement value can be performed according to a known method. For example, a solubility test is performed to determine whether a sample (usually a polymer) is dissolved in 20 types of solvents (acetone, methylcyclohexane, methyl ethyl ketone, tetrahydrofuran, metaxylene hexafluoride, HFE-7100 (hydrofluoroether), dimethyl sulfoxide, diethylene glycol, N-methylpyrrolidone, acetonitrile, 2-propanol, 2-(2-ethoxyethoxy)ethanol, toluene, diiodomethane, acetophenone, benzaldehyde, acetic acid, 2-ethylhexanol, propylene carbonate, and ethanol), and an SP sphere (Hansen's dissolution sphere) is constructed from the SP values of the solvents that were able to dissolve the sample, and the Hansen's SP value can be calculated based on the SP sphere (by converting the units as necessary). The SP value of the monomer that constitutes the polymer can be determined using commercially available calculation software.
[0030] In the release agent of the present invention, the total amount of the thixotropic agent and at least one low-polarity solvent having a solubility parameter of 20 or less can be appropriately changed depending on, for example, the type of thixotropic agent or low-polarity solvent used, but is usually about 0.5 to 20% by weight, and preferably 0.5 to 15% by weight.
[0031] (1d) Water Water is a component that is mainly used to form a water-containing emulsion film by the stripping agent of the present invention. From this viewpoint, the water content in the stripping agent of the present invention is preferably about 20 to 80% by weight, and more preferably 30 to 70% by weight.
[0032] In particular, in relation to the aromatic alcohol, the weight ratio of aromatic alcohol:water is preferably 1:1 to 1:2, and more preferably 1:1.3 to 1:1.7. By setting such a ratio, better flame retardancy can be obtained.
[0033] (1e) Other ingredients In the stripping agent of the present invention, as long as it does not interfere with the effect of the present invention, other components than the above-mentioned components can be appropriately blended as necessary. For example, thickeners, surfactants, pH adjusters, preservatives, rust inhibitors, etc. can be mentioned. In addition, when an optional component used also functions as an essential component in the stripping agent of the present invention, the content of such optional component is included in the content of essential components. For example, in the case of a surfactant, depending on the surfactant used, it may also function as a thixotropic agent, and the content of such surfactant is included in the content of the thixotropic agent.
[0034] The thickener may be either inorganic or organic. Examples of inorganic thickeners include inorganic powders such as silica, kaolin, serpentine, talc, mica, vermiculite, smectite, bentonite, and sepiolite. Examples of organic thickeners include cellulose derivatives such as sodium alginate, propylene glycol alginate, sodium carboxymethylcellulose, calcium carboxymethylcellulose, sodium starch glycolate, sodium starch phosphate, sodium polyacrylate, and methylcellulose, and synthetic products such as hydroxypropylmethylcellulose. Examples of natural polysaccharides include guar gum, tara gum, gum arabic, tragacanth gum, alginic acid, carrageenan, xanthan gum, dielan gum, perithin, chitin, chitosan, and chitosamine.
[0035] The surfactant may be, for example, an anionic surfactant, a cationic surfactant, an amphoteric surfactant, a nonionic surfactant, etc. Examples of the anionic surfactant include fatty acid salts, alkyl sulfate ester salts, alkylbenzene sulfonates, polyoxyethylene alkyl ether sulfates, dialkyl sulfosuccinic acids, etc. Examples of the cationic surfactant include alkylamine acetates, quaternary ammonium salts, etc. Examples of the amphoteric surfactant include alkyldimethylaminoacetate betaine, alkyldimethylamine oxide, etc. Examples of the nonionic surfactant include glycerin fatty acid esters, propylene glycol fatty acid esters, sorbitan fatty acid esters, polyoxyethylene alkyl ethers, polyoxyethylene polyoxypropylene ethers, etc.
[0036] Examples of the pH adjuster include acid components such as inorganic acids, such as hydrochloric acid and phosphoric acid, and organic acids, such as acetic acid, oxalic acid, and citric acid. Examples of the base components include inorganic alkalis, such as sodium hydroxide and potassium hydroxide, and organic alkalis, such as monoethanolamine, monoisopropanolamine, diethanolamine, and triethanolamine.
[0037] (2) Water-containing emulsion film produced by the stripping agent of the present invention In the case of the release agent of the present invention, the water-containing emulsion film formed by the release agent of the present invention is maintained at a temperature of 15° C. for at least 6 hours from immediately after the application of the release agent.
[0038] The release agent of the present invention is in the form of an aqueous emulsion, and when it is applied, a water-containing emulsion film is formed. After peeling off the coating film to be peeled off, which has such a water-containing emulsion film on its surface, the water-containing emulsion film is also retained on the surface of the peeled coating film piece for a certain period of time, so that the combustion of the coating film piece after peeling can be effectively suppressed. The reason why such an effect is achieved is not clear, but it is thought to be due to the following mechanism. In general, the water-containing emulsion film formed by the aqueous emulsion type release agent starts to evaporate water. With existing release agents, water is easily evaporated, and a dry coating film with a low water content is formed in a relatively short time. In contrast, the water-containing emulsion film by the release agent of the present invention forms a layer structure of "coating film to be peeled off / water-rich layer / organic component-rich layer" as described above in the water-containing emulsion film, and the water-rich layer is in a state where the evaporation of water is hindered by the organic component-rich layer, and this state is maintained for a longer period of time, so that the water-rich layer suppresses the ignition of the coating film piece, or even if it temporarily ignites, the combustion (spread of fire) is suppressed.
[0039] The environment in which the water-containing emulsion film is maintained is one in which the release agent of the present invention is usually used outdoors, and therefore the environment is maintained at normal temperature and normal humidity for a specified period of time, and as a standard in the present invention, the temperature is 15° C. (preferably 25° C.) for 6 hours or more, preferably 6 hours or more, more preferably 8 hours or more, even more preferably 12 hours or more, more preferably 18 hours or more, and most preferably 24 hours or more. The humidity may be normal humidity, for example, about 10 to 85%, but is not limited thereto.
[0040] (3) Production of the release agent of the present invention The release agent of the present invention can be prepared by uniformly mixing and emulsifying each of these components. In this case, mixing can be performed using a known or commercially available mixer, kneader, etc. The order of mixing each of these components is not particularly limited as long as a homogeneous aqueous emulsion is obtained, and each component may be mixed simultaneously or sequentially. In this way, the release agent of the present invention in the form of an aqueous emulsion can be obtained.
[0041] (4) Use of the stripping agent of the present invention The stripping agent of the present invention can be preferably used in accordance with the method described below in "2. Method for stripping coating film."
[0042] 2. How to remove the coating The present invention includes a method for stripping a coating film using the stripping agent of the present invention. In particular, the present invention is a method for stripping a coating film, comprising the steps of: (1) A step of forming a water-containing emulsion film by applying the release agent of the present invention to the surface of the coating film to be peeled (the coating film to be peeled) (coating step); (2) Aging the emulsion film for a certain period of time after application while maintaining the emulsion film (aging step); and (3) A step of peeling off the coating film having the water-containing emulsion film (peeling step) The present invention relates to a coating peeling method comprising the steps of:
[0043] (1) Coating process In the coating step, the release agent of the present invention is applied to the surface of the coating film to be stripped to form a water-containing emulsion film.
[0044] The coating film to be peeled off (the coating film to be removed) is not particularly limited as long as it is a coating film formed on the surface of a structure (particularly a metal structure). The coating film to be peeled off is not particularly limited as long as it is coated with a general paint, and the type of paint and the thickness of the coating film to be peeled off are not particularly limited. For example, the coating film to be peeled off can be applied to a coating film containing at least one of melamine-based resin, acrylic-based resin, phthalic acid-based resin, urethane-based resin, epoxy-based resin, etc.
[0045] The material of the base of the coating film to be peeled off is not limited, and may be, for example, any of metal, concrete, wood, etc. In particular, the stripping agent of the present invention is suitable for use in coating films to be peeled off whose base is metal (preferably steel). The type of the base structure is not particularly limited, and it can be applied to any structure that requires corrosion resistance and rust prevention, such as bridges, building exterior walls, storage tanks, water gates, garages, etc.
[0046] The method for applying the release agent of the present invention is not particularly limited, and can be carried out according to known methods such as spraying, roller, brush, etc. The amount of application (before drying) is not limited, but is usually 0.3 to 2 kg / m 2 Approximately 0.5 to 1 kg / m 2 It is preferable to set the above.
[0047] (2) Aging process In the aging step, after the application of the release agent of the present invention, the aqueous emulsion film is maintained and aged for a certain period of time.
[0048] In the aging step, the coating film to be peeled is left for a sufficient time for the release agent of the present invention to penetrate into the coating film to be peeled and for the coating film to be peeled to swell. At this time, the time is set to a time during which the water-containing emulsion film is maintained on the surface of the coating film to be peeled. This time depends on the working environment and season (temperature, humidity, presence or absence of sunlight), etc., but is generally about 6 to 48 hours after application of the release agent of the present invention, and preferably about 10 to 26 hours.
[0049] The aqueous emulsion film produced by the release agent of the present invention is opaque or semi-transparent due to the fact that the release agent of the present invention is opaque or semi-transparent due to the emulsification, and is formed on the surface of the coating film to be peeled off in an opaque or semi-transparent state. When most of the water in the aqueous emulsion film has evaporated, its appearance changes from opaque or semi-transparent to transparent. Therefore, the aging time can be appropriately adjusted within a range in which such a change in appearance is not substantially visible to the naked eye.
[0050] (3) Peeling process In the peeling step, the coating film to be peeled off having the aqueous emulsion film is peeled off. That is, the coating film to be peeled off is peeled off and removed from the base at a stage where the aqueous emulsion film has not yet dried and its appearance has not yet changed to transparent.
[0051] The peeling method can be carried out using a known or commercially available peeling tool such as a scraper. The peeled coating pieces still contain the water-containing emulsion film on their surface, making them less likely to ignite or burn. By collecting the coating pieces while they are in this state, it is possible to more reliably prevent fires caused by the coating pieces. EXAMPLES
[0052] The features of the present invention will be described in more detail below with reference to examples and comparative examples, although the scope of the present invention is not limited to the examples.
[0053] Examples 1 to 7 and Comparative Examples 1 to 4 A release agent (aqueous emulsion) was prepared by uniformly mixing each component shown in Table 1. The content of each component is expressed in "wt %."
[0054] [Table 1]
[0055] Details of each product name in Table 1 are as follows: "T-SOL150" - Naphtha manufactured by Ando Parachemie Co., Ltd. "Metolose SM4000" - Cellulose-based thickener manufactured by Shin-Etsu Chemical Co., Ltd. "Metolose 60SH4000" - Cellulose-based thickener manufactured by Shin-Etsu Chemical Co., Ltd. "Metolose 90SH4000" - Cellulose-based thickener manufactured by Shin-Etsu Chemical Co., Ltd. "Disparlon F-9030" - Manufactured by Kusumoto Chemicals Co., Ltd., fatty acid amide thixotropic agent "Paraffin Wax-115" Paraffin with a melting point of 47°C, manufactured by Nippon Seiro Co., Ltd. "AQUACER497" - Manufactured by BYK Japan Co., Ltd. A mixture of 40-50% paraffin, 1-10% stearate, 1-10% fatty acid carboxylate, and water with a melting point of 60°C "No.70-S" Liquid paraffin, manufactured by Sanko Chemical Industry Co., Ltd. Docosanol: Higher alcohol, melting point 70°C "Rheodor TW-O320V" - Kao Corporation, sorbitan fatty acid ester nonionic surfactant
[0056] Test Example 1 (Confirmation of water-containing emulsion membrane) In Examples 1 to 7 and Comparative Examples 1 to 4, the change over time in the appearance of the water-containing emulsion film produced by each release agent was examined. The formation of the aqueous emulsion film was carried out by applying 1 kg / m2 of the coating (before drying) to the surface of the coating film (film thickness 200 μm) of the steel bridge used in the following "Test Example 2 (flammability test)". 2 The release agents of Examples 1 to 7 and Comparative Examples 1 to 4 were applied with a brush so that the above-mentioned Each release agent was in a cloudy state, and a cloudy water-containing emulsion film was formed immediately after application. Thereafter, as drying proceeded, the appearance of the water-containing emulsion film changed to transparent. In such a series of appearance changes, it was measured whether the time from immediately after application at a temperature of 15°C until the water-containing emulsion film became transparent at a visual level was 6 hours or more. As a result, in Examples 1 to 7, the water-containing emulsion film maintained a cloudy state even after 6 hours, and maintained a cloudy state even after 24 hours. On the other hand, in Comparative Examples 1 to 4, the water-containing emulsion film became transparent within 30 minutes.
[0057] Test Example 2 (Flammability Test) The coating amount (before drying) on the surface of the coating film of a steel bridge (film thickness approx. 200 μm) is 1 kg / m 2 The release agents of Examples 1 to 7 and Comparative Examples 1 to 4 were applied with a brush so that the coating film was coated with the release agent. 24 hours after the completion of application, the coating film coated with the release agent was scraped with a scraper to remove the coating film. After removal, a piece of the coating film (approximately 3 cm x 3 cm in size) was placed on a brick block, and a lighter flame was brought close to the coating film piece. It was held close for 15 seconds, and visually confirmed whether the coating film piece had burned. The results are shown in Table 1. Cases where there was no ignition or combustion were marked with "○", and cases where there was ignition were marked with "×".
[0058] Examples 8 to 11 and Comparative Examples 5 to 11 A release agent (aqueous emulsion) was prepared by uniformly mixing each component shown in Table 2. Each component in Table 2 is the same as that described above for Table 1. The content of each component is expressed in "wt %".
[0059] Test Example 3 (Confirmation of Water-containing Emulsion Film) In Examples 8 to 11 and Comparative Examples 5 to 11, the change over time in the appearance of the water-containing emulsion film produced by each release agent was examined. The formation of the aqueous emulsion film was carried out by applying 1 kg / m2 of the coating amount (before drying) to the coating surface of the test piece prepared in "(1) (Preparation of coating film test piece)" of "Test Example 4 (Removability test)" below. 2 The release agents of Examples 8 to 11 and Comparative Examples 5 to 11 were applied with a brush so that the above-mentioned Each release agent was in a cloudy state, and a cloudy water-containing emulsion film was formed immediately after application. Thereafter, as drying proceeded, the appearance of the water-containing emulsion film changed to transparent. In such a series of appearance changes, it was measured whether the time from immediately after application until the water-containing emulsion film became transparent at a visual level was 8 hours or more at a temperature of 25°C. As a result, in Examples 8 to 11, the water-containing emulsion film maintained a cloudy state even after 8 hours, and maintained a cloudy state even after 24 hours. On the other hand, in Comparative Examples 5 to 11, the water-containing emulsion film became transparent within 8 hours.
[0060] Test Example 4 (Peeling Test) (1) Preparation of coating test specimens A long-form etching primer (Vinylex 120 Active Primer Eco (color: dark green), manufactured by Nippon Paint Co., Ltd.) was applied to a steel plate of SS400 (Japanese Industrial Standard) that had been blast-treated in accordance with ISO Sa 2 1 / 2. On top of that, two layers of a lead- and chromium-free rust-preventive paint (Lasgon Safety (color: red rust, gray), manufactured by Kansai Paint Co., Ltd.) were applied, and on top of that, a long-oil-based phthalic acid resin paint undercoat (SD Marine Safety undercoat (color: white), manufactured by Kansai Paint Co., Ltd.) and a long-oil-based phthalic acid resin paint topcoat (SD Marine Safety topcoat (color: yellow), manufactured by Kansai Paint Co., Ltd.) were applied. The painted steel plate was baked at 60°C for one week to prepare a coating film test piece with a coating thickness of approximately 200 μm. (2) Peel test The coating amount on the coating surface of the coating test piece prepared above is 1 kg / m 2 Each of the release agents of Examples 8 to 11 and Comparative Examples 5 to 11 was applied with a brush so that the coating film was peeled off after 24 hours had passed in an environment of a temperature of 25°C and a humidity of 50%. The case where the entire coating film could be peeled off was marked with "◯", and the case where a part or the entire coating film could not be peeled off was marked with "X". The results are shown in Table 2.
[0061] Test Example 5 (Flame Retardancy Test) The coating film peeled off in Test Example 4 (peelability test) was placed on a brick block, and a fire was brought close to it with a lighter, and it was visually confirmed whether the coating film burned or not. If the coating film did not ignite even after being held close to the fire for 5 seconds, it was marked as "○", if the coating film ignited within 5 seconds of being held close to the brick block but immediately went out, it was marked as "△", and if the coating film ignited within 5 seconds of being held close to the brick block and did not go out until the coating film burned out, it was marked as "×". The results are shown in Table 2.
[0062] [Table 2]
[0063] As is clear from the results in Table 2, Examples 8 to 10, in which 0.5 wt% or more of solid paraffin was added as an evaporation inhibitor, had good flame retardancy, whereas Comparative Examples 5 to 6, in which no evaporation inhibitor was added, had poor flame retardancy. Comparative Examples 7 to 8, in which liquid paraffin and higher alcohol were added as evaporation inhibitors, also had poor flame retardancy.
[0064] From the above, it can be said that it is desirable for the evaporation inhibitor to be solid at room temperature and to have no hydrophilic groups such as hydroxyl groups, and that the blending amount thereof is desirably 0.5% by weight or more.
[0065] Furthermore, in Examples 8 and 9, in which the benzyl alcohol content was 40% by weight and the same solid paraffin was used but the blending amounts were different, Example 9 had improved flame retardancy, and when the benzyl alcohol content was 40% by weight, it is particularly desirable that the blending amount of solid paraffin be 1% by weight or more.
[0066] In Examples 8 and 11 and Comparative Examples 9 and 10, 0.5% by weight of solid paraffin was added, and the ratio of the amount of benzyl alcohol to the amount of water was changed. The blending amounts were adjusted so that the viscosities were similar. Examples 8 to 11, which contain 0.5% by weight or more of solid paraffin and have a ratio of the weight of water to the weight of benzyl alcohol (i.e., [(water content) / (benzyl alcohol content)]) of 1 or more, have good flame retardancy, whereas Comparative Examples 9 to 11, which contain 0.5% by weight or more of solid paraffin but have a ratio of the weight of water to the weight of benzyl alcohol of less than 1, have poor flame retardancy. It is believed that by making the ratio of the weight of water to the weight of benzyl alcohol 1 or more, more water is retained in the release agent, and the cooling effect of the contained water improves the flame retardancy. [Industrial Applicability]
[0067] The stripping agent of the present invention is effective in safely removing coating films applied to structures such as bridges, storage tanks, exterior staircases, and water gates.
Claims
1. An aqueous emulsion-based paint film stripper for stripping a paint film, comprising: (1) The release agent is (1a) 30 to 80% by weight of an aromatic alcohol; (1b) 0.4 to 5% by weight of paraffins having a melting point of 65° C. or less, (1c) 0.5 to 20% by weight of a low-polarity solvent having a solubility parameter of 20 or less; (1d) 20 to 80% by weight of water; (1e) 0.7 to 1.9% by weight of a cellulose derivative and (2) The water-containing emulsion film formed by the release agent is maintained at a temperature of 15° C. for at least 6 hours from immediately after application of the release agent. A paint film combustion suppressing stripping agent characterized by the above.
2. The paint piece burn-retardant stripping agent according to claim 1, further comprising a surfactant.
3. 2. The paint piece combustion suppressing stripping agent according to claim 1, which is used to suppress ignition and combustion of peeled paint piece pieces.
4. A method for stripping a coating, comprising the steps of: (1) a step of forming a water-containing emulsion film by applying the paint piece combustion suppressing stripping agent according to claim 1 or 2 to the surface of the paint film to be stripped; (2) Aging the coated film for a certain period of time while maintaining the water-containing emulsion film; and (3) Step of peeling off the coating film having the water-containing emulsion film A coating film peeling method comprising the steps of:
5. The coating amount (before drying) in the process of applying the paint film piece combustion retardant stripping agent is 0.3 to 2 kg / m 2 The method according to claim 4, wherein
Citation Information
Patent Citations
Paint remover comprising benzyl alcohol activated by ammonium bicarbonate / ammonium carbamate
JP1996253713A
improved paint remover
JP1997503812A
Water drop-in-oil type emulsion containing anisole
JP1998330660A
Water-in-oil emulsion containing terpene
JP1998338825A
paint remover composition
JP2003505528A