Polarizing film, polarizing plate, and method of manufacturing polarizing film
A polyvinyl alcohol resin-based polarizing film with enhanced puncture strength and optical properties addresses the tearing issue in conventional films, enabling flexible and foldable display applications.
Patent Information
- Application Number
- JP2024131751
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-02-08
- Filing Date
- 2024-08-08
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional polarizing films for liquid crystal displays are prone to tearing along the absorption axis direction, compromising their durability and flexibility.
A polarizing film composed of a polyvinyl alcohol resin containing a dichroic substance, with an orientation function of 0.30 or less, a thickness of 8 μm or less, and a puncture strength of 30 gf/μm or more, manufactured through a process involving auxiliary stretching, dyeing, and drying shrinkage to enhance flexibility and optical properties.
The film achieves high puncture strength and acceptable optical properties, preventing tearing along the absorption axis and enabling applications in flexible and foldable display devices.
Smart Images

Figure 2024144775000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a polarizing film, a polarizing plate, and a method for producing the polarizing film. [Background technology]
[0002] In a liquid crystal display device, which is a representative image display device, a polarizing film is arranged on both sides of a liquid crystal cell due to its image formation method. As a method for manufacturing a polarizing film, for example, a method has been proposed in which a laminate having a resin substrate and a polyvinyl alcohol (PVA)-based resin layer is stretched and then dyed to obtain a polarizing film on the resin substrate (for example, Patent Document 1). Since such a method can obtain a thin polarizing film, it has attracted attention as a possible contribution to the thinning of image display devices in recent years. However, such a thin polarizing film has a problem in that it is easily torn (torn) along the absorption axis direction. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2001-343521 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention has been made to solve the above-mentioned problems in the conventional art, and a main object of the present invention is to provide a polarizing film in which breakage along the absorption axis direction is suppressed. [Means for solving the problem]
[0005] The polarizing film according to an embodiment of the present invention is made of a polyvinyl alcohol-based resin film containing a dichroic material, and has an orientation function of 0.30 or less. In one embodiment, the polarizing film has a thickness of 8 μm or less. In one embodiment, the polarizing film has a single transmittance of 40.0% or more and a polarization degree of 99.0% or more. In one embodiment, the polarizing film has a piercing strength of 30 gf / μm or more. A polarizing film according to another embodiment of the present invention is made of a polyvinyl alcohol-based resin film containing a dichroic material, and has a puncture strength of 30 gf / μm or more. According to another aspect of the present invention, there is provided a polarizing plate having the above polarizing film and a protective layer disposed on at least one side of the polarizing film. According to another aspect of the present invention, there is provided a method for producing the polarizing film. The method includes forming a polyvinyl alcohol-based resin layer containing iodide or sodium chloride and a polyvinyl alcohol-based resin on one side of a long thermoplastic resin substrate to form a laminate; and subjecting the laminate to an auxiliary air-stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment in this order, in which the laminate is heated while being transported in the longitudinal direction, thereby shrinking the laminate by 2% or more in the width direction. The total stretching ratio in the auxiliary air-stretching treatment and the underwater stretching treatment is 3.0 to 4.5 times the original length of the laminate; and the stretching ratio in the auxiliary air-stretching treatment is greater than the stretching ratio in the underwater stretching treatment. Effect of the Invention
[0006] According to the present invention, by setting the orientation function to 0.30 or less, or by setting the piercing strength to 30 gf / μm or more, it is possible to realize a polarizing film in which breakage along the absorption axis direction is suppressed. Conventionally, it has been difficult to obtain acceptable optical properties (typically, single transmittance and degree of polarization) with a polarizing film having such a small orientation function, but according to the present invention, it is possible to achieve both such a small orientation function and acceptable optical properties. Furthermore, according to the present invention, it is possible to achieve both such a large piercing strength and acceptable optical properties. [Brief description of the drawings]
[0007] [Figure 1]1 is a schematic cross-sectional view of a polarizing plate according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing an example of a drying shrinkage treatment using a heating roll. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.
[0009] A. Polarizing film The polarizing film according to the embodiment of the present invention is composed of a polyvinyl alcohol (PVA) resin film containing a dichroic material (typically, iodine, a dichroic dye), and has an orientation function of 0.30 or less. With such a configuration, it is possible to significantly prevent the polarizing film from tearing (breaking) along the absorption axis direction. As a result, a polarizing film (and, as a result, a polarizing plate) with very excellent flexibility can be obtained. Such a polarizing film (and, as a result, a polarizing plate) can be preferably applied to a curved image display device, more preferably a bendable image display device, and even more preferably a foldable image display device. The orientation function is, for example, 0.25 or less, preferably 0.22 or less, more preferably 0.20 or less, even more preferably 0.18 or less, and particularly preferably 0.15 or less. The lower limit of the orientation function can be, for example, 0.05. If the orientation function is too small, an acceptable single-unit transmittance and / or polarization degree may not be obtained.
[0010] The orientation function (f) can be determined, for example, by attenuated total reflection (ATR) measurement using a Fourier transform infrared spectrophotometer (FT-IR) with polarized light as the measurement light. Specifically, the measurement is performed with the stretching direction of the polarizing film parallel and perpendicular to the polarization direction of the measurement light. -1 The intensity I is calculated according to the following formula using the intensity of 3330 cm -1 is used as the reference peak, and 2941 cm -1 / 3330cm -1The value is 2941 cm. Note that f=1 is perfect alignment, and f=0 is random. -1 The peak is due to the main chain (-CH) of PVA in the polarizing film. 2 It is believed that this absorption is due to vibrations of the -. f=(3 <cos 2 θ>-1) / 2 =(1-D) / [c(2D+1)] =-2×(1-D) / (2D+1) however, c = (3cos 2 β-1) / 2, 2941cm -1 For vibration, β=90°. θ: Angle of molecular chain to stretching direction β: Angle of the transition dipole moment with respect to the chain axis D=(I ⊥ ) / (I / / ) (In this case, the more the PVA molecules are oriented, the larger D becomes.) I ⊥ : Absorption intensity when the polarization direction of the measurement light and the stretching direction of the polarizing film are perpendicular I / / : Absorption intensity when the polarization direction of the measurement light is parallel to the stretching direction of the polarizing film
[0011] The thickness of the polarizing film is preferably 8 μm or less, more preferably 7 μm or less, even more preferably 5 μm or less, particularly preferably 3 μm or less, and particularly preferably 2 μm or less. The lower limit of the thickness of the polarizing film may be, for example, 1 μm. The thickness of the polarizing film may be 2 μm to 6 μm in one embodiment, 2 μm to 4 μm in another embodiment, 2 μm to 3 μm in yet another embodiment, 5.5 μm to 7.5 μm in yet another embodiment, and 6 μm to 7.2 μm in yet another embodiment. By making the thickness of the polarizing film very thin in this way, it is possible to make the thermal shrinkage very small. It is presumed that such a configuration may also contribute to suppressing breakage in the absorption axis direction.
[0012] The polarizing film preferably exhibits absorption dichroism at any wavelength of 380 nm to 780 nm. The single transmittance of the polarizing film is preferably 40.0% or more, more preferably 41.0% or more. The upper limit of the single transmittance may be, for example, 49.0%. In one embodiment, the single transmittance of the polarizing film is 40.0% to 45.0%. The degree of polarization of the polarizing film is preferably 99.0% or more, more preferably 99.4% or more. The upper limit of the degree of polarization may be, for example, 99.999%. In one embodiment, the degree of polarization of the polarizing film is 99.0% to 99.99%. According to the present invention, despite the very small orientation function as described above, such a practically acceptable single transmittance and degree of polarization can be realized. This is presumably due to the manufacturing method described later. The single transmittance is typically a Y value measured using an ultraviolet-visible spectrophotometer and corrected for luminosity. The degree of polarization is typically calculated by the following formula based on the parallel transmittance Tp and the crossed transmittance Tc that have been measured using an ultraviolet-visible spectrophotometer and subjected to luminosity correction. Degree of polarization (%)={(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100
[0013] The piercing strength of the polarizing film is 30 gf / μm or more, preferably 35 gf / μm or more, more preferably 40 gf / μm or more, even more preferably 45 gf / μm or more, and particularly preferably 50 gf / μm or more. The upper limit of the piercing strength can be, for example, 80 gf / μm. By setting the piercing strength of the polarizing film in such a range, it is possible to significantly suppress the polarizing film from tearing along the absorption axis direction. As a result, a polarizing film (and, as a result, a polarizing plate) with very excellent flexibility can be obtained. The piercing strength indicates the crack resistance of the polarizing film when the polarizing film is pierced with a predetermined strength. The piercing strength can be expressed, for example, as the strength (breaking strength) at which the polarizing film breaks when a predetermined needle is attached to a compression tester and the needle is pierced into the polarizing film at a predetermined speed. As is clear from the unit, the piercing strength means the piercing strength per unit thickness (1 μm) of the polarizing film.
[0014] As described above, the polarizing film is composed of a PVA-based resin film containing iodine. Preferably, the PVA-based resin constituting the PVA-based resin film (substantially the polarizing film) contains an acetoacetyl-modified PVA-based resin. With such a configuration, a polarizing film having a desired puncture strength can be obtained. The blending amount of the acetoacetyl-modified PVA-based resin is preferably 5% by weight to 20% by weight, and more preferably 8% by weight to 12% by weight, when the entire PVA-based resin is taken as 100% by weight. If the blending amount is within such a range, the puncture strength can be set to a more suitable range.
[0015] A polarizing film can be typically produced using a laminate of two or more layers. A specific example of a polarizing film obtained using a laminate is a polarizing film obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate. A polarizing film obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate can be produced, for example, by applying a PVA-based resin solution to the resin substrate, drying the resin substrate to form a PVA-based resin layer on the resin substrate, thereby obtaining a laminate of the resin substrate and the PVA-based resin layer, and stretching and dyeing the laminate to make the PVA-based resin layer into a polarizing film. In this embodiment, a polyvinyl alcohol-based resin layer containing a halide and a polyvinyl alcohol-based resin is preferably formed on one side of the resin substrate. The stretching typically includes immersing the laminate in an aqueous boric acid solution to stretch the laminate. Furthermore, the stretching preferably further includes stretching the laminate in air at a high temperature (e.g., 95°C or higher) before stretching in the aqueous boric acid solution. In an embodiment of the present invention, the total stretching ratio is, for example, 3.0 to 4.5 times, which is significantly smaller than usual. Even at such a total stretching ratio, a polarizing film having acceptable optical properties can be obtained by combining the addition of a halide and a drying shrinkage treatment. Furthermore, in an embodiment of the present invention, the stretching ratio of the auxiliary air stretching is greater than the stretching ratio of the boric acid water stretching. With this configuration, a polarizing film having acceptable optical properties can be obtained even at a small total stretching ratio. In addition, the laminate is preferably subjected to a drying shrinkage treatment in which the laminate is heated while being transported in the longitudinal direction, thereby shrinking the laminate by 2% or more in the width direction. In one embodiment, the method for producing a polarizing film includes subjecting the laminate to an auxiliary air stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment in this order. By introducing the auxiliary stretching, even when PVA is applied onto a thermoplastic resin, it is possible to increase the crystallinity of PVA and achieve high optical properties. At the same time, by increasing the orientation of the PVA in advance, it is possible to prevent problems such as a decrease in the orientation of the PVA or dissolution when the film is immersed in water in the subsequent dyeing and stretching processes, making it possible to achieve high optical properties.Furthermore, when the PVA-based resin layer is immersed in a liquid, the orientation of polyvinyl alcohol molecules is disturbed and the orientation is reduced, compared to when the PVA-based resin layer does not contain a halide. This can improve the optical properties of the polarizing film obtained by immersing the laminate in a liquid through a treatment process such as a dyeing process and an underwater stretching process. Furthermore, the optical properties can be improved by shrinking the laminate in the width direction through a drying shrinkage process. The obtained resin substrate / polarizing film laminate may be used as it is (i.e., the resin substrate may be used as a protective layer for the polarizing film), or the resin substrate may be peeled off from the resin substrate / polarizing film laminate and any suitable protective layer may be laminated on the peeled surface according to the purpose. Details of the method for producing the polarizing film will be described later in Section C.
[0016] B. Polarizing plate 1 is a schematic cross-sectional view of a polarizing plate according to one embodiment of the present invention. The polarizing plate 100 has a polarizing film 10, a first protective layer 20 arranged on one side of the polarizing film 10, and a second protective layer 30 arranged on the other side of the polarizing film 10. The polarizing film 10 is the polarizing film of the present invention described in the above section A. One of the first protective layer 20 and the second protective layer 30 may be omitted. As described above, one of the first protective layer and the second protective layer may be a resin substrate used in the manufacture of the above polarizing film.
[0017] The first and second protective layers are formed of any suitable film that can be used as a protective layer for a polarizing film. Specific examples of materials that are the main components of the films include cellulose-based resins such as triacetyl cellulose (TAC), and transparent resins such as polyesters, polyvinyl alcohols, polycarbonates, polyamides, polyimides, polyethersulfones, polysulfones, polystyrenes, polynorbornenes, polyolefins, (meth)acrylics, and acetates. Other examples include thermosetting resins or ultraviolet-curing resins such as (meth)acrylics, urethanes, (meth)acrylic urethanes, epoxys, and silicones. Other examples include glassy polymers such as siloxane polymers. Polymer films described in JP 2001-343529 A (WO01 / 37007) can also be used. The material for this film may be, for example, a resin composition containing a thermoplastic resin having a substituted or unsubstituted imide group in the side chain, and a thermoplastic resin having a substituted or unsubstituted phenyl group and a nitrile group in the side chain, such as a resin composition containing an alternating copolymer of isobutene and N-methylmaleimide, and an acrylonitrile-styrene copolymer. The polymer film may be, for example, an extrusion molded product of the above resin composition.
[0018] When the polarizing plate 100 is applied to an image display device, the thickness of the protective layer (outer protective layer) disposed on the opposite side to the display panel is typically 300 μm or less, preferably 100 μm or less, more preferably 5 μm to 80 μm, and further preferably 10 μm to 60 μm. When a surface treatment is applied, the thickness of the outer protective layer includes the thickness of the surface treatment layer.
[0019] When the polarizing plate 100 is applied to an image display device, the thickness of the protective layer (inner protective layer) disposed on the display panel side is preferably 5 μm to 200 μm, more preferably 10 μm to 100 μm, and even more preferably 10 μm to 60 μm. In one embodiment, the inner protective layer is a retardation layer having any appropriate retardation value. In this case, the in-plane retardation Re(550) of the retardation layer is, for example, 110 nm to 150 nm. "Re(550)" is the in-plane retardation measured with light having a wavelength of 550 nm at 23°C, and is calculated by the formula: Re=(nx-ny)×d. Here, "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the direction perpendicular to the slow axis in the plane (i.e., the fast axis direction), "nz" is the refractive index in the thickness direction, and "d" is the thickness (nm) of the layer (film).
[0020] C. Manufacturing method of polarizing film A method for producing a polarizing film according to one embodiment of the present invention includes forming a polyvinyl alcohol-based resin layer (PVA-based resin layer) containing a halide and a polyvinyl alcohol-based resin (PVA-based resin) on one side of a long thermoplastic resin substrate to form a laminate, and subjecting the laminate to an auxiliary air-stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment in this order, in which the laminate is heated while being transported in the longitudinal direction to shrink the laminate by 2% or more in the width direction. The content of the halide in the PVA-based resin layer is preferably 5 parts by weight to 20 parts by weight with respect to 100 parts by weight of the PVA-based resin. The drying shrinkage treatment is preferably performed using a heating roll, and the temperature of the heating roll is preferably 60° C. to 120° C. The shrinkage rate of the laminate in the width direction due to the drying shrinkage treatment is preferably 2% or more. According to such a production method, the polarizing film described in the above item A can be obtained. In particular, a laminate containing a PVA-based resin layer containing a halide is prepared, the laminate is stretched in multiple stages including auxiliary air stretching and underwater stretching, and the laminate after stretching is heated with a heating roll, whereby a polarizing film having excellent optical properties (typically, single transmittance and unit absorbance) can be obtained.
[0021] C-1. Preparation of laminate Any suitable method can be adopted as a method for producing a laminate of a thermoplastic resin substrate and a PVA-based resin layer. Preferably, a coating liquid containing a halide and a PVA-based resin is applied to the surface of the thermoplastic resin substrate, and then dried to form a PVA-based resin layer on the thermoplastic resin substrate. As described above, the content of the halide in the PVA-based resin layer is preferably 5 to 20 parts by weight relative to 100 parts by weight of the PVA-based resin.
[0022] Any appropriate method can be used as the coating method of the coating liquid. For example, roll coating, spin coating, wire bar coating, dip coating, die coating, curtain coating, spray coating, knife coating (comma coating, etc.), etc. are listed. The coating and drying temperature of the coating liquid is preferably 50° C. or higher.
[0023] The thickness of the PVA-based resin layer is preferably 2 μm to 30 μm, and more preferably 2 μm to 20 μm. By making the thickness of the PVA-based resin layer before stretching very thin in this manner and reducing the total stretching ratio as described below, it is possible to obtain a polarizing film having an acceptable single-unit transmittance and polarization degree despite a very small orientation function.
[0024] Before forming the PVA-based resin layer, the thermoplastic resin substrate may be subjected to a surface treatment (e.g., corona treatment, etc.), or an easy-adhesion layer may be formed on the thermoplastic resin substrate. By carrying out such treatment, the adhesion between the thermoplastic resin substrate and the PVA-based resin layer can be improved.
[0025] C-1-1. Thermoplastic resin base material Any suitable thermoplastic resin film may be used as the thermoplastic resin substrate. Details of the thermoplastic resin substrate are described in, for example, JP 2012-73580 A. The entire disclosure of this publication is incorporated herein by reference.
[0026] C-1-2. Coating solution The coating liquid contains a halide and a PVA resin as described above. The coating liquid is typically a solution in which the halide and the PVA resin are dissolved in a solvent. Examples of the solvent include water, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, various glycols, polyhydric alcohols such as trimethylolpropane, and amines such as ethylenediamine and diethylenetriamine. These can be used alone or in combination of two or more. Among these, water is preferred. The concentration of the PVA resin in the solution is preferably 3 to 20 parts by weight relative to 100 parts by weight of the solvent. With such a resin concentration, a uniform coating film that is in close contact with the thermoplastic resin substrate can be formed. The content of the halide in the coating liquid is preferably 5 to 20 parts by weight relative to 100 parts by weight of the PVA resin.
[0027] Additives may be added to the coating liquid. Examples of additives include plasticizers and surfactants. Examples of plasticizers include polyhydric alcohols such as ethylene glycol and glycerin. Examples of surfactants include nonionic surfactants. These can be used to further improve the uniformity, dyeability, and stretchability of the resulting PVA-based resin layer.
[0028] Any suitable resin may be used as the PVA resin. Examples include polyvinyl alcohol and ethylene-vinyl alcohol copolymer. Polyvinyl alcohol is obtained by saponifying polyvinyl acetate. Ethylene-vinyl alcohol copolymer is obtained by saponifying ethylene-vinyl acetate copolymer. The saponification degree of the PVA resin is usually 85 mol% to 100 mol%, preferably 95.0 mol% to 99.95 mol%, and more preferably 99.0 mol% to 99.93 mol%. The saponification degree can be determined in accordance with JIS K 6726-1994. By using a PVA resin having such a saponification degree, a polarizing film having excellent durability can be obtained. If the saponification degree is too high, gelation may occur. As described above, the PVA resin preferably contains an acetoacetyl-modified PVA resin.
[0029] The average degree of polymerization of the PVA resin can be appropriately selected depending on the purpose. The average degree of polymerization is usually 1000 to 10000, preferably 1200 to 4500, and more preferably 1500 to 4300. The average degree of polymerization can be determined in accordance with JIS K 6726-1994.
[0030] Any suitable halide may be used as the halide. For example, iodide and sodium chloride may be used. For example, iodide may be potassium iodide, sodium iodide, and lithium iodide. Among these, potassium iodide is preferred.
[0031] The amount of the halide in the coating solution is preferably 5 to 20 parts by weight per 100 parts by weight of the PVA-based resin, and more preferably 10 to 15 parts by weight per 100 parts by weight of the PVA-based resin. If the amount of the halide exceeds 20 parts by weight per 100 parts by weight of the PVA-based resin, the halide may bleed out, causing the final polarizing film to become cloudy.
[0032] Generally, the orientation of polyvinyl alcohol molecules in the PVA-based resin increases when the PVA-based resin layer is stretched, but when the stretched PVA-based resin layer is immersed in a liquid containing water, the orientation of the polyvinyl alcohol molecules may become disordered, and the orientation may decrease. In particular, when a laminate of a thermoplastic resin and a PVA-based resin layer is stretched in boric acid water, the tendency of the orientation degree to decrease is remarkable when the laminate is stretched in boric acid water at a relatively high temperature to stabilize the stretching of the thermoplastic resin. For example, the stretching of a PVA film alone in boric acid water is generally performed at 60°C, whereas the stretching of a laminate of A-PET (thermoplastic resin substrate) and a PVA-based resin layer is performed at a high temperature of about 70°C, and in this case, the orientation of PVA at the initial stage of stretching may decrease before it increases due to underwater stretching. In response to this, a laminate of a PVA-based resin layer containing a halide and a thermoplastic resin substrate is prepared, and the laminate is stretched at high temperature (auxiliary stretching) in air before being stretched in boric acid water, so that the crystallization of the PVA-based resin in the PVA-based resin layer of the laminate after the auxiliary stretching can be promoted. As a result, when the PVA-based resin layer is immersed in a liquid, the orientation of the polyvinyl alcohol molecules is disturbed and the orientation is reduced, compared to when the PVA-based resin layer does not contain a halide. This can improve the optical properties of the polarizing film obtained through a process in which the laminate is immersed in a liquid, such as a dyeing process and an underwater stretching process.
[0033] C-2. Aerial supplementary stretching process In particular, in order to obtain high optical properties, a two-stage stretching method is selected, which combines dry stretching (auxiliary stretching) and stretching in boric acid water. By introducing auxiliary stretching like two-stage stretching, it is possible to stretch while suppressing the crystallization of the thermoplastic resin substrate. Furthermore, when applying a PVA-based resin on a thermoplastic resin substrate, it is necessary to lower the application temperature compared to when applying a PVA-based resin on a normal metal drum in order to suppress the influence of the glass transition temperature of the thermoplastic resin substrate, and as a result, the crystallization of the PVA-based resin becomes relatively low, and a problem that sufficient optical properties cannot be obtained may occur. On the other hand, by introducing auxiliary stretching, it is possible to increase the crystallinity of the PVA-based resin even when applying a PVA-based resin on a thermoplastic resin, and it is possible to achieve high optical properties. At the same time, by increasing the orientation of the PVA-based resin in advance, problems such as a decrease in the orientation of the PVA-based resin or dissolution can be prevented when immersed in water in the subsequent dyeing process or stretching process, and it is possible to achieve high optical properties.
[0034] The stretching method of the auxiliary air stretching may be fixed end stretching (for example, a method of stretching using a tenter stretching machine) or free end stretching (for example, a method of uniaxially stretching a laminate between rolls with different peripheral speeds), but in order to obtain high optical properties, free end stretching may be actively adopted. In one embodiment, the air stretching process includes a heated roll stretching process in which the laminate is stretched by the difference in peripheral speed between heated rolls while being transported in its longitudinal direction. The air stretching process typically includes a zone stretching process and a heated roll stretching process. The order of the zone stretching process and the heated roll stretching process is not limited, and the zone stretching process may be performed first, or the heated roll stretching process may be performed first. The zone stretching process may be omitted. In one embodiment, the zone stretching process and the heated roll stretching process are performed in this order. In another embodiment, the film is stretched by gripping the film end in a tenter stretching machine and widening the distance between the tenters in the flow direction (the widening of the distance between the tenters is the stretching ratio). At this time, the distance of the tenter in the width direction (perpendicular to the machine direction) is set to be as close as possible. Preferably, it can be set to be as close as possible to the free end stretching ratio in the machine direction. In the case of free end stretching, the shrinkage ratio in the width direction = (1 / stretching ratio) 1 / 2 It is calculated as follows.
[0035] The auxiliary air-drawing may be performed in one step or in multiple steps. When the auxiliary air-drawing is performed in multiple steps, the draw ratio is the product of the draw ratios in each step. The draw direction in the auxiliary air-drawing is preferably approximately the same as the draw direction in the underwater drawing.
[0036] The stretching ratio in the auxiliary air stretching is preferably 1.0 to 4.0 times, more preferably 1.5 to 3.5 times, and further preferably 2.0 to 3.0 times. If the stretching ratio in the auxiliary air stretching is in this range, the total stretching ratio can be set in a desired range when combined with underwater stretching, and a desired orientation function can be achieved. As a result, a polarizing film in which breakage along the absorption axis direction is suppressed can be obtained. Furthermore, as described above, the stretching ratio in the auxiliary air stretching is higher than the stretching ratio in the boric acid water. With this configuration, a polarizing film having acceptable optical properties can be obtained even if the total stretching ratio is small.
[0037] The stretching temperature of the auxiliary in-air stretching can be set to any appropriate value depending on the material of the thermoplastic resin substrate, the stretching method, etc. The stretching temperature is preferably equal to or higher than the glass transition temperature (Tg) of the thermoplastic resin substrate, more preferably equal to or higher than the glass transition temperature (Tg) of the thermoplastic resin substrate + 10°C, and particularly preferably equal to or higher than Tg + 15°C. On the other hand, the upper limit of the stretching temperature is preferably 170°C. By stretching at such a temperature, rapid crystallization of the PVA resin can be suppressed, and defects due to the crystallization (for example, the orientation of the PVA resin layer due to stretching is hindered) can be suppressed.
[0038] C-3. Insolubilization, dyeing and crosslinking treatments If necessary, after the auxiliary air stretching treatment, an insolubilization treatment is performed before the underwater stretching treatment or the dyeing treatment. The insolubilization treatment is typically performed by immersing the PVA-based resin layer in an aqueous boric acid solution. The dyeing treatment is typically performed by dyeing the PVA-based resin layer with a dichroic substance (typically iodine). If necessary, after the dyeing treatment, a crosslinking treatment is performed before the underwater stretching treatment. The crosslinking treatment is typically performed by immersing the PVA-based resin layer in an aqueous boric acid solution. Details of the insolubilization treatment, the dyeing treatment, and the crosslinking treatment are described, for example, in JP 2012-73580 A (above).
[0039] C-4. Underwater stretching process The underwater stretching treatment is performed by immersing the laminate in a stretching bath. The underwater stretching treatment allows stretching at a temperature lower than the glass transition temperature (typically about 80° C.) of the thermoplastic resin substrate or the PVA-based resin layer, and allows the PVA-based resin layer to be stretched while suppressing crystallization. As a result, a polarizing film having excellent optical properties can be produced.
[0040] The stretching method of the laminate can be any appropriate method. Specifically, it may be fixed end stretching or free end stretching (for example, a method of uniaxially stretching the laminate by passing it between rolls having different peripheral speeds). Preferably, free end stretching is selected. The stretching of the laminate may be performed in one stage or multiple stages. When performing multiple stages, the total stretching ratio is the product of the stretching ratios in each stage.
[0041] The underwater stretching is preferably performed by immersing the laminate in an aqueous solution of boric acid (stretching in boric acid water). By using an aqueous solution of boric acid as a stretching bath, it is possible to impart to the PVA-based resin layer rigidity that can withstand the tension applied during stretching and water resistance that does not dissolve in water. Specifically, boric acid can generate tetrahydroxyborate anions in the aqueous solution and crosslink with the PVA-based resin through hydrogen bonds. As a result, it is possible to impart rigidity and water resistance to the PVA-based resin layer and stretch it well, and a polarizing film having excellent optical properties can be produced.
[0042] The boric acid aqueous solution is preferably obtained by dissolving boric acid and / or a borate in water as a solvent. The boric acid concentration is preferably 1 to 10 parts by weight, more preferably 2.5 to 6 parts by weight, and particularly preferably 3 to 5 parts by weight, relative to 100 parts by weight of water. By setting the boric acid concentration to 1 part by weight or more, dissolution of the PVA-based resin layer can be effectively suppressed, and a polarizing film with higher characteristics can be produced. In addition to boric acid or a borate, an aqueous solution obtained by dissolving a boron compound such as borax, glyoxal, glutaraldehyde, or the like in a solvent can also be used.
[0043] Preferably, an iodide is added to the stretching bath (boric acid aqueous solution). By adding an iodide, it is possible to suppress the elution of iodine adsorbed in the PVA resin layer. Specific examples of the iodide are as described above. The concentration of the iodide is preferably 0.05 to 15 parts by weight, more preferably 0.5 to 8 parts by weight, relative to 100 parts by weight of water.
[0044] The stretching temperature (liquid temperature of the stretching bath) is preferably 40°C to 85°C, more preferably 60°C to 75°C. At such a temperature, the laminate can be stretched at a high ratio while suppressing dissolution of the PVA-based resin layer. Specifically, as described above, the glass transition temperature (Tg) of the thermoplastic resin substrate is preferably 60°C or higher in relation to the formation of the PVA-based resin layer. In this case, if the stretching temperature is lower than 40°C, there is a risk that the substrate cannot be stretched well even when the plasticization of the thermoplastic resin substrate by water is taken into consideration. On the other hand, the higher the temperature of the stretching bath, the higher the solubility of the PVA-based resin layer, and there is a risk that excellent optical properties cannot be obtained. The immersion time of the laminate in the stretching bath is preferably 15 seconds to 5 minutes.
[0045] The stretching ratio in underwater stretching is preferably 1.0 to 3.0 times, more preferably 1.0 to 2.0 times, and further preferably 1.0 to 1.5 times. When the stretching ratio in underwater stretching is in this range, the total stretching ratio can be set in a desired range, and a desired orientation function can be realized. As a result, a polarizing film in which breakage along the absorption axis direction is suppressed can be obtained. As described above, the total stretching ratio (the total stretching ratio when the auxiliary air stretching and the underwater stretching are combined) is, for example, 3.0 to 4.5 times, preferably 3.0 to 4.0 times, and more preferably 3.0 to 3.5 times, relative to the original length of the laminate. By appropriately combining the addition of a halide to the coating solution, the adjustment of the stretching ratios of the auxiliary air stretching and the underwater stretching, and the drying shrinkage treatment, a polarizing film having acceptable optical properties can be obtained even at such a total stretching ratio.
[0046] C-5. Drying shrinkage treatment The drying shrinkage treatment may be performed by zone heating, which heats the entire zone, or by heating the transport roll (using a so-called heating roll) (heat roll drying method). Preferably, both are used. By drying using a heating roll, it is possible to efficiently suppress the heat curl of the laminate and produce a polarizing film with excellent appearance. Specifically, by drying the laminate in a state where it is aligned with the heating roll, it is possible to efficiently promote the crystallization of the thermoplastic resin substrate and increase the crystallinity, and even at a relatively low drying temperature, it is possible to satisfactorily increase the crystallinity of the thermoplastic resin substrate. As a result, the rigidity of the thermoplastic resin substrate increases and it becomes in a state where it can withstand the shrinkage of the PVA-based resin layer due to drying, and curling is suppressed. In addition, by using a heating roll, it is possible to dry the laminate while maintaining it in a flat state, so that it is possible to suppress not only curling but also wrinkles. At this time, the optical properties of the laminate can be improved by shrinking it in the width direction by the drying shrinkage treatment. This is because the orientation of the PVA and the PVA / iodine complex can be effectively increased. The shrinkage rate in the width direction of the laminate due to the drying shrinkage treatment is preferably 1% to 10%, more preferably 2% to 8%, and particularly preferably 4% to 6%.
[0047] 2 is a schematic diagram showing an example of the drying shrinkage treatment. In the drying shrinkage treatment, the laminate 200 is dried while being transported by transport rolls R1 to R6 heated to a predetermined temperature and guide rolls G1 to G4. In the illustrated example, the transport rolls R1 to R6 are arranged so as to alternately and continuously heat the surface of the PVA resin layer and the surface of the thermoplastic resin substrate, but, for example, the transport rolls R1 to R6 may be arranged so as to continuously heat only one surface of the laminate 200 (for example, the thermoplastic resin substrate surface).
[0048] Drying conditions can be controlled by adjusting the heating temperature of the transport rolls (temperature of the heating rolls), the number of heating rolls, the contact time with the heating rolls, etc. The temperature of the heating rolls is preferably 60°C to 120°C, more preferably 65°C to 100°C, and particularly preferably 70°C to 80°C. The crystallinity of the thermoplastic resin can be favorably increased, curling can be favorably suppressed, and an optical laminate with extremely excellent durability can be produced. The temperature of the heating rolls can be measured by a contact thermometer. In the illustrated example, six transport rolls are provided, but there is no particular restriction as long as there are multiple transport rolls. The number of transport rolls is usually 2 to 40, preferably 4 to 30. The contact time (total contact time) between the laminate and the heating rolls is preferably 1 to 300 seconds, more preferably 1 to 20 seconds, and even more preferably 1 to 10 seconds.
[0049] The heating roll may be provided in a heating furnace (for example, an oven) or in a normal production line (under room temperature environment). It is preferably provided in a heating furnace equipped with a blowing means. By using drying with a heating roll in combination with hot air drying, it is possible to suppress abrupt temperature changes between the heating rolls, and it is possible to easily control shrinkage in the width direction. The hot air drying temperature is preferably 30°C to 100°C. The hot air drying time is preferably 1 second to 300 seconds. The hot air speed is preferably about 10 m / s to 30 m / s. The wind speed is the wind speed in the heating furnace, and can be measured by a mini-vane type digital anemometer.
[0050] C-6. Other processing Preferably, after the underwater stretching treatment and before the drying shrinkage treatment, a washing treatment is carried out. The washing treatment is typically carried out by immersing the PVA-based resin layer in an aqueous potassium iodide solution. EXAMPLES
[0051] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring each property are as follows. In the examples and comparative examples, "parts" and "%" are by weight unless otherwise specified. (1) Thickness The thickness was measured using an interference film thickness meter (Otsuka Electronics Co., Ltd., product name "MCPD-3000") The calculation wavelength range used for thickness calculation was 400 nm to 500 nm, and the refractive index was 1.53. (2) Orientation function For the polarizing films obtained in the examples and comparative examples, a Fourier transform infrared spectrophotometer (FT-IR) (manufactured by Perkin Elmer, product name: "Frontier") was used to measure attenuated total reflection (ATR) spectroscopy of the polarizing film surface using polarized infrared light as the measurement light. Germanium was used as the crystallite to which the polarizing film was adhered, and the angle of incidence of the measurement light was 45°. The orientation function was calculated using the following procedure. The polarized infrared light (measurement light) to be incident was polarized light (s-polarized light) that vibrated parallel to the surface to which the germanium crystal sample was adhered, and the absorbance spectrum of each was measured with the stretching direction of the polarizing film arranged perpendicular (⊥) and parallel ( / / ) to the polarization direction of the measurement light. From the obtained absorbance spectrum, the (3330 cm -1 Intensity) was used as a reference (2941 cm -1 The intensity I was calculated. ⊥ is obtained from the absorbance spectrum obtained when the stretching direction of the polarizing film is arranged perpendicular (⊥) to the polarization direction of the measurement light (2941 cm -1 strength) / (3330cm -1 In addition, I / / is obtained from the absorbance spectrum obtained when the stretching direction of the polarizing film is arranged parallel ( / / ) to the polarization direction of the measurement light (2941 cm -1 strength) / (3330cm -1 Intensity), where (2941 cm -1 Intensity) is the bottom of the absorbance spectrum, 2770 cm -1 and 2990cm -1 2941cm when using this as the baseline-1 is the absorbance of (3330cm -1 Strength) is 2990cm -1 and 3650cm -1 3330cm when the baseline is -1 The absorbance of the obtained I ⊥ and I / / The orientation function f was calculated according to formula 1. Note that f = 1 is perfect orientation, and f = 0 is random. -1 The peak is due to the main chain (-CH) of PVA in the polarizing film. 2 -) vibration-induced absorption. -1 The peak is said to be due to the vibration of the hydroxyl group of PVA. (Formula 1)f=(3<cos2θ> -1) / 2 =(1-D) / [c(2D+1)] however c = (3cos 2 β-1) / 2 So, as mentioned above, 2941cm -1 When using, β=90°⇒f=-2×(1-D) / (2D+1). θ: Angle of molecular chain to stretching direction β: Angle of the transition dipole moment with respect to the chain axis D=(I ⊥ ) / (I / / ) I ⊥ : Absorption intensity when the polarization direction of the measurement light and the stretching direction of the polarizing film are perpendicular I / / : Absorption intensity when the polarization direction of the measurement light is parallel to the stretching direction of the polarizing film (3) Single unit transmittance and polarization degree The polarizing film was peeled off from the laminate of polarizing film / thermoplastic resin substrate used in the examples and comparative examples, and the single transmittance Ts, parallel transmittance Tp, and crossed transmittance Tc of the polarizing film were measured using an ultraviolet-visible spectrophotometer ("V-7100" manufactured by JASCO Corporation), which were designated as Ts, Tp, and Tc of the polarizing film, respectively. These Ts, Tp, and Tc are Y values measured using a 2-degree visual field (C light source) according to JIS Z8701 and corrected for luminosity. From the obtained Tp and Tc, the degree of polarization P was calculated according to the following formula. Polarization degree P(%)={(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100 It should be noted that equivalent measurements can also be made using a spectrophotometer such as the Otsuka Electronics LPF-200, and it has been confirmed that equivalent measurement results can be obtained regardless of which spectrophotometer is used. (4) Breaking strength The polarizing film was peeled off from the laminate of polarizing film / thermoplastic resin substrate used in the examples and comparative examples, and placed on a compression tester (manufactured by Kato Tech, product name "NDG5" needle penetration force measurement specifications) equipped with a needle, and pierced at a piercing speed of 0.33 cm / sec under a room temperature (23°C ± 3°C) environment. The strength at which the polarizing film broke was taken as the breaking strength (piercing strength). The evaluation value was the average value of the breaking strengths of 10 sample pieces. The needle used had a tip diameter of 1 mmφ and a radius of 0.5 R. The polarizing film to be measured was fixed by clamping both sides of the polarizing film with a jig having a circular opening with a diameter of about 11 mm, and the needle was pierced into the center of the opening to perform the test. The breaking strength per unit thickness was used as an index of resistance to breaking, and was evaluated according to the following criteria. ○: Breaking strength exceeds 30gf / μm ×: Breaking strength is 30gf / μm or less
[0052] [Example 1] The thermoplastic resin substrate was a long, amorphous, isophthalic copolymerized polyethylene terephthalate film (thickness: 100 μm) with a water absorption rate of 0.75% and a Tg of approximately 75°C. One side of the resin substrate was subjected to corona treatment (treatment conditions: 55 W min / m 2 ) was applied. A PVA aqueous solution (coating solution) was prepared by adding 13 parts by weight of potassium iodide to 100 parts by weight of a PVA-based resin prepared by mixing polyvinyl alcohol (polymerization degree 4200, saponification degree 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., product name "GOHSEFFIMER Z410") in a ratio of 9:1. The above PVA aqueous solution was applied to the corona-treated surface of a resin substrate and dried at 60° C. to form a PVA-based resin layer with a thickness of 13 μm, thereby producing a laminate. The obtained laminate was uniaxially stretched at its free end to 2.4 times its original size in the machine direction (longitudinal direction) between rolls with different peripheral speeds in an oven at 130° C. (auxiliary air stretching treatment). Next, the laminate was immersed in an insolubilizing bath (a boric acid aqueous solution obtained by mixing 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (insolubilizing treatment). Next, the film was immersed in a dye bath (an aqueous iodine solution obtained by mixing iodine and potassium iodide in a weight ratio of 1:7 with 100 parts by weight of water) at a liquid temperature of 30°C for 60 seconds while adjusting the concentration so that the single transmittance (Ts) of the final polarizing film would be 41.6% (dyeing process). Next, the piece was immersed in a crosslinking bath (a boric acid aqueous solution obtained by mixing 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with respect to 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (crosslinking treatment). Thereafter, the laminate was immersed in an aqueous boric acid solution (boric acid concentration 4.0 wt %, potassium iodide 5.0 wt %) at a liquid temperature of 62°C and uniaxially stretched in the longitudinal direction (longitudinal direction) between rolls with different peripheral speeds so that the total stretch ratio was 3.0 times (underwater stretching treatment: the stretch ratio in the underwater stretching treatment was 1.25 times). Thereafter, the laminate was immersed in a cleaning bath (an aqueous solution obtained by mixing 4 parts by weight of potassium iodide with 100 parts by weight of water) at a liquid temperature of 20° C. (cleaning treatment). Thereafter, while drying in an oven maintained at 90°C, it was brought into contact with a SUS heated roll whose surface temperature was maintained at 75°C for about 2 seconds (drying shrinkage treatment). The shrinkage rate of the laminate in the width direction due to the drying shrinkage treatment was 2%. In this manner, a polarizing film having a thickness of 7.1 μm was formed on the resin substrate.
[0053] The orientation function, single transmittance, polarization degree and breaking strength of the obtained polarizing film are shown in Table 1.
[0054] [Example 2] A polarizing film having a thickness of 6.6 μm was produced in the same manner as in Example 1, except that the stretching ratio in the underwater stretching treatment was 1.45 times and the total stretching ratio was 3.5 times. The obtained polarizing film was subjected to the same evaluation as in Example 1. The results are shown in Table 1.
[0055] [Example 3] A polarizing film having a thickness of 6.1 μm was produced in the same manner as in Example 1, except that the stretching ratio in the underwater stretching treatment was 1.67 times and the total stretching ratio was 4.0 times. The obtained polarizing film was subjected to the same evaluation as in Example 1. The results are shown in Table 1.
[0056] [Example 4] A polarizing film having a thickness of 5.6 μm was produced in the same manner as in Example 1, except that the stretching ratio in the underwater stretching treatment was 1.87 times and the total stretching ratio was 4.5 times. The obtained polarizing film was subjected to the same evaluation as in Example 1. The results are shown in Table 1.
[0057] [Comparative Example 1] A polarizing film having a thickness of 5.0 μm was produced in the same manner as in Example 1, except that the stretching ratio in the underwater stretching treatment was 2.4 times, the total stretching ratio was 5.5 times, and the liquid temperature of the stretching bath was 70° C. The remaining width ratio of the obtained polarizing film was 48% (shrinkage ratio in the width direction was 52%). The obtained polarizing film was subjected to the same evaluation as in Example 1. The results are shown in Table 1.
[0058] [Comparative Example 2] A polarizing film having a thickness of 5.5 μm was produced in the same manner as in Comparative Example 1, except that the width residual rate was 43% (the shrinkage rate in the width direction was 57%). The obtained polarizing film was subjected to the same evaluation as in Example 1. The results are shown in Table 1.
[0059] [Comparative Example 3] A long roll of a 30 μm-thick PVA-based resin film (manufactured by Kuraray, product name "PE3000") was uniaxially stretched in the long direction by a roll stretching machine so that the total stretch ratio was 6.0 times, while simultaneously subjecting the film to swelling, dyeing, crosslinking and washing treatments, and finally subjecting the film to a drying treatment, thereby producing a polarizer with a thickness of 12 μm. The obtained polarizer was subjected to the same evaluation as in Example 1. The results are shown in Table 1.
[0060] [Table 1]
[0061] As is clear from Table 1, the polarizing films of the examples of the present invention have practically acceptable single transmittance and polarization degree, and also have very high breaking strength along the absorption axis direction. Such breaking strength means that the polarizing film is unlikely to tear along the absorption axis direction. [Industrial Applicability]
[0062] The polarizing film and polarizing plate of the present invention are suitably used in liquid crystal displays. [Explanation of symbols]
[0063] 10 Polarizing film 20 First protective layer 30 Second layer of protection 100 Polarizing Plate
Claims
1. A polarizing film comprising a polyvinyl alcohol-based resin film containing a dichroic material, and having an orientation function of 0.30 or less.
2. A polarizing film comprising a polyvinyl alcohol-based resin film containing a dichroic material, and having a puncture strength of 30 gf / μm or more.
3. A method for producing the polarizing film according to claim 1 or 2, comprising the steps of: forming a polyvinyl alcohol-based resin layer containing iodide or sodium chloride and a polyvinyl alcohol-based resin on one side of a long thermoplastic resin substrate to form a laminate; The laminate is subjected to an air-assisted stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment in which the laminate is heated while being transported in the longitudinal direction to shrink the laminate by 2% or more in the width direction, in this order; a total stretching ratio in the auxiliary air-stretching treatment and the underwater stretching treatment is 3.0 to 4.5 times the original length of the laminate; The stretching ratio in the auxiliary air-stretching process is greater than the stretching ratio in the underwater stretching process. Manufacturing method.
Citation Information
Patent Citations
Polarizing plate and method for manufacturing the same