Acid generator
The use of cellulose nanofibers with sulfate ester groups as a thermal acid generator addresses the limitations of photosensitive and non-biodegradable photoacid generators, offering a sustainable and controlled acid release for aqueous polymerization and crosslinking processes.
Patent Information
- Application Number
- JP2023056949
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Existing photoacid generators are photosensitive, require expensive equipment for handling, have poor dispersibility in aqueous media, and are not biodegradable, posing environmental risks.
Development of an acid generator using cellulose nanofibers with sulfate ester groups that generate acid through thermal energy, allowing for use in aqueous systems and being non-photosensitive and biodegradable.
The cellulose nanofiber-based acid generator provides a sustainable and environmentally friendly solution for polymerization and crosslinking processes, ensuring controlled acid release and reducing environmental impact.
Smart Images

Figure 2024144814000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an acid generator, and more particularly to an acid generator containing cellulose nanofibers having sulfate ester groups as an active ingredient. [Background technology]
[0002] Acid generators are used in the fields of photocurable resins, such as coating materials, adhesive materials, and molding materials, and photolithography materials.
[0003] A typical use of an acid generator is as a photopolymerization initiator. For example, Patent Document 1 discloses a photopolymerization initiator that reacts to high-energy rays such as ultraviolet rays, far ultraviolet rays, electron beams, X-rays, excimer lasers, gamma rays, or synchrotron radiation and reacts with a compound represented by the general formula: HOCH2CH2CF2CF2SO3 - M + (In the formula, M + represents a lithium ion, a sodium ion, a potassium ion, an ammonium ion, or a tetramethylammonium ion. A photoacid generator for a chemically amplified resist material is disclosed, which generates a sulfonic acid represented by the following formula:
[0004] Many cationic photopolymerization initiators have an onium salt structure of an organic cation and an anion. Compounds in which the organic cation structure is a trivalent sulfonium ion are called sulfonium salts, and since the anion functions as an active species for polymerization, a counter anion of a Brønsted acid is used. Among these, aromatic sulfonium salts are used industrially as highly stable cationic photopolymerization initiators. When excited by light, aromatic sulfonium salts decompose radically to generate cationic radicals. The cationic radicals abstract hydrogen from molecules such as monomers present in the system. Ultimately, aromatic sulfides and acids (H + X - The photodecomposition of aromatic sulfonium salts is completed by the production of the following compound:
[0005] [ka]
[0006] For example, Patent Document 2 discloses a composition containing 80% by mass or more of water and 0.1% by mass or more of an onium salt dissolved in the water, the onium salt being represented by the following general formula (I): [ka] The present invention discloses a photoacid generator composition comprising a sulfonium salt represented by the following formula: [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2008-7409 A [Patent Document 2] JP 2013-234320 A [Non-patent literature]
[0008] [Non-Patent Document 1] Toshihiko Murai, "Development of Network Polymers by Photocationic Polymerization with Sulfonium Salts as the Main Source," Journal of Network Polymers, Vol. 40, No. 1, 2019, p. 37 Summary of the Invention [Problem to be solved by the invention]
[0009] From the perspective of reducing VOCs and moving away from petroleum, demand for water-based polymerizable polymers using acids as initiators and water-based crosslinked polymers using acids as initiators will continue to increase in the future.
[0010] However, for example, the photoacid generator of Patent Document 1 has a hydrophilic group, but also has a skeleton containing fluorine atoms and methylene, so that it has poor dispersibility in aqueous media and is difficult to apply to coating agents and adhesives with aqueous compositions. In addition, since the photoacid generator is photosensitive, it requires oblique light management and expensive equipment for handling. Furthermore, the photoacid generator is not biodegradable, and there is a risk when it is leaked into the environment.
[0011] In addition, the photoacid generator composition of Patent Document 2 is also photosensitive, so that handling requires oblique light management and expensive equipment. Furthermore, the photoacid generator is also not biodegradable, and there is a risk if it is leaked into the environment.
[0012] Therefore, an object of the present invention is to provide an acid generator made of a biomass-derived material that is non-photosensitive, biodegradable, and usable in aqueous systems. [Means for solving the problem]
[0013] Due to growing environmental awareness, research is being conducted around the world to put biomass-derived materials to practical use. For example, cellulose is a component of plant cell walls and is the largest biomass resource on earth. When using lignocellulosic biomass such as wood (wood chips, etc.), herbs, coconut shells, and nut shells as raw materials, if the components cellulose, lignin, and hemicellulose can be used in industry without waste, it will contribute greatly to both circular resource utilization and CO2 fixation.
[0014] When cellulose is processed into nano-sized cellulose (also known as "nanocellulose") such as cellulose nanofibers (also known as "CNF") and cellulose nanocrystals (also known as "CNC"), it leads to improved physical properties such as strength, flexibility, and elongation when combined with resin, rubber, and even concrete, and is therefore attracting attention as a new, environmentally friendly material.
[0015] As a result of intensive research into providing new uses for such nanocellulose, the inventors discovered that cellulose nanofibers having sulfate ester groups have the effect of gradually eliminating the sulfate ester groups when thermal energy is applied, thereby generating sulfuric acid (H2SO4), in particular the effect of generating acid during the production of aqueous polymerizable polymers and / or aqueous crosslinked polymers, and thus completed the present invention.
[0016] That is, the gist of the present invention is as follows. (1) An acid generator comprising, as an active ingredient, a cellulose nanofiber having a sulfate ester group, The cellulose nanofiber has an average fiber width of 1 nm to 1000 nm, The sulfate ester group is represented by the following general formula (I): [ka] In the general formula (I), n is an integer of 1 to 3, and M n+ is an n-valent cation, and the wavy lines are the sites of attachment to other atoms.) Represented by The acid generator. (2) The acid generator according to (1), wherein the amount of sulfur introduced into the cellulose nanofiber resulting from the sulfate ester group is 0.3 mmol / g to 3.0 mmol / g relative to the mass of the cellulose nanofiber. (3) The acid generator according to (1) or (2), further comprising one or more salts selected from metal salts and ammonium salts, the content of the salt being 0.002 parts by mass to 10 parts by mass per 100 parts by mass of the cellulose nanofiber. (4) The acid generator according to any one of (1) to (3), further comprising water, the content of the water being 50 mass % or less based on the total mass of the acid generator. (5) The acid generator according to any one of (1) to (4), further comprising water, the content of the water being 1,000 parts by mass or more per 100 parts by mass of the cellulose nanofiber. (6) The acid generator according to any one of (1) to (5), wherein when the acid generator and water are mixed to prepare an aqueous dispersion in which the concentration of the cellulose nanofibers is 0.3 mass% relative to the total mass of the aqueous dispersion, and the aqueous dispersion is heat-treated at 80°C for 24 hours, the pH of the aqueous dispersion after the heat treatment is reduced by 0.5 to 6.0 from the pH before the heat treatment. (7) The acid generator according to any one of (1) to (6), wherein when the acid generator is mixed with water to prepare an aqueous dispersion in which the concentration of the cellulose nanofibers is 0.3 mass% relative to the total mass of the aqueous dispersion, the viscosity of the aqueous dispersion measured at 2.6 rpm at 25°C is 500 mPa s or more. (8) The acid generator according to any one of (1) to (7) for producing an aqueous polymerizable polymer and / or an aqueous crosslinked polymer. Effect of the Invention
[0017] The present invention provides an acid generator made of a biomass-derived material that is non-photosensitive, biodegradable, and can be used in aqueous systems. [Brief description of the drawings]
[0018] [Figure 1] 2 is a graph showing the relationship between the amount of sulfur introduced and viscosity in the examples. [Diagram 2] 1 is a graph showing the relationship between salt concentration and viscosity in an example. [Diagram 3] 3 is a graph showing the salt concentration in FIG. 2 in logarithmic scale. [Figure 4] 1 is a graph showing the relationship between the amount of sulfur introduced and the pH change (pH before heat treatment−pH after heat treatment) in the examples. [Diagram 5] 2 is a graph showing the relationship between salt concentration and pH change (pH before heat treatment−pH after heat treatment) in an example. [Figure 6] FIG. 6 is a graph showing the salt concentration in FIG. 5 in logarithmic scale. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Preferred embodiments of the present invention will now be described in detail. In this specification, the features of the present invention will be described with reference to the drawings as appropriate. The acid generator of the present invention is not limited to the following embodiments, and can be embodied in various forms including modifications and improvements that can be made by those skilled in the art without departing from the gist of the present invention.
[0020] In this specification, a range expressed by "numeric value to numerical value" means a range including the numerical value. For example, the above-mentioned "1 nm to 1000 nm" means "1 nm or more and 1000 nm or less", that is, the range from 1 nm to 1000 nm, including 1 nm and 1000 nm.
[0021] The present invention relates to an acid generator that contains cellulose nanofibers having sulfate ester groups as an active ingredient.
[0022] Here, the acid generator means a composition containing a compound having the property of generating an acid under specific conditions. The acid generator of the present invention is particularly a thermal acid generator that generates an acid upon input of thermal energy.
[0023] Cellulose is a polysaccharide formed by the β-1,4-glycosidic bond of glucose (C6H 10 O5) n As shown in the figure.
[0024] Cellulose nanofibers are fibers made from cellulose.
[0025] The average fiber width (fiber diameter (equivalent circle diameter)) of the cellulose nanofiber is not limited, but is usually 1 nm to 1000 nm, preferably 2 nm to 200 nm. The average fiber length of the cellulose nanofiber is not limited, but is usually 0.05 μm to 6 μm, preferably 0.1 μm to 1 μm.
[0026] The average fiber width and the average fiber length are not limited, but can be measured, for example, by using an atomic force microscope (SPM-9700HT, manufactured by Shimadzu Corporation) to measure the fiber width and fiber length of 50 arbitrarily selected fibers and calculating the arithmetic average value for each.
[0027] Cellulose nanofibers having sulfate ester groups are also called sulfated cellulose nanofibers, and are cellulose nanofibers in which at least one of the OH groups in the cellulose constituting the cellulose nanofibers has been substituted with a sulfate ester group. The sulfate ester groups of cellulose nanofibers having sulfate ester groups are sulfate ester groups represented by the following formula (I).
[0028] [ka] In the general formula (I), n is an integer of 1 to 3, and M n+ is an n-valent cation, and the wavy lines are the sites of attachment to other atoms.)
[0029] M in formula (I) n+ Examples of the monovalent to trivalent cations represented by the formula (I) include hydrogen ions, metal ions, and ammonium ions. n+ When -OSO3- is a divalent or trivalent cation, the cation forms an ionic bond with two or three -OSO3-.
[0030] Examples of the metal ion include an alkali metal ion, an alkaline earth metal ion, a transition metal ion, and other metal ions.
[0031] Here, examples of the alkali metal ions include lithium ions, sodium ions, potassium ions, rubidium ions, and cesium ions. Examples of the alkaline earth metal ions include calcium ions and strontium ions. Examples of the transition metal ions include iron ions, nickel ions, palladium ions, copper ions, and silver ions. Examples of other metals include beryllium ions, magnesium ions, zinc ions, and aluminum ions.
[0032] The ammonium ion is NH4 + Not only NH4 + Examples of ammonium ions include those derived from various amines in which one or more hydrogen atoms are replaced by organic groups. For example, NH + , quaternary ammonium cations, alkanolamine ions, pyridinium ions, etc.
[0033] M n+ In view of high processability, the cation represented by the formula (I) is preferably a hydrogen ion, a sodium ion, a potassium ion, a calcium ion, or a quaternary ammonium cation. The above-listed cations may be used alone or in combination of two or more.
[0034] In the cellulose nanofiber having sulfate ester groups of the present invention, the amount of sulfur introduced due to sulfate ester groups is not limited, but is usually 0.3 mmol / g to 3.0 mmol / g, preferably 1.0 mmol / g to 2.9 mmol / g or less, and more preferably 1.3 mmol / g to 2.7 mmol / g or less. The amount of sulfur introduced due to sulfate ester groups in the cellulose nanofiber having sulfate ester groups is expressed as the sulfur content (mmol) due to sulfate ester groups per 1 g of cellulose nanofiber having sulfate ester groups. The amount of sulfur introduced due to sulfate ester groups can be set to any appropriate value within the above range depending on the amount of acid generated required by the acid generator. The amount of sulfur introduced due to sulfate ester groups can be set to a desired range by adjusting the concentration of reagents such as sulfuric acid and sulfamic acid, the amount of pulp relative to the reaction solution, and the reaction time.
[0035] The amount of sulfur introduced due to sulfate ester groups in cellulose nanofibers can be determined, for example, by combustion absorption-ion chromatography (IC). Alternatively, the amount of sulfur introduced due to sulfate ester groups in cellulose nanofibers can also be confirmed by infrared spectroscopy (IR). The amount of sulfur introduced due to sulfate ester groups in cellulose nanofibers having sulfate ester groups can be measured, for example, by the following method.
[0036] Measurement method: Combustion absorption - IC Measurement equipment: ICS-1500 manufactured by Nippon Dionex Co., Ltd. Measurement conditions: 0.01 g of the sample (cellulose nanofiber having sulfate ester groups) is weighed onto a magnetic board, burned in an oxygen atmosphere (flow rate: 1.5 L / min) in a ring furnace (1350°C), and the generated gas components are absorbed in 3% hydrogen peroxide solution (20 ml) to obtain an absorbed solution. The absorbed solution obtained is made up to 100 ml with pure water, and the diluted solution is subjected to ion chromatography. From the measurement results, the substance amount (mmol) of sulfate ions per 1 g of the cellulose nanofiber is calculated. The detection limit of sulfate ion concentration based on cellulose using this method is 0.009 mmol / g. Therefore, the quantification lower limit of the sulfur content converted from the sulfate ion concentration is 0.003 mmol / g. Therefore, cellulose nanofibers having sulfate ester groups with a sulfur content of less than 0.003 mmol / g may be unmodified (i.e., not modified by sulfate esterification) cellulose nanofibers.
[0037] The cellulose nanofibers having sulfate ester groups of the present invention may have other substituents in addition to the sulfate ester groups. Here, when the cellulose nanofibers having sulfate ester groups have other substituents, the other substituents are substituted with at least one of the OH groups in the cellulose constituting the cellulose nanofibers. Examples of the other substituents include, but are not limited to, anionic substituents and their salts, ester groups, ether groups, acyl groups, aldehyde groups, alkyl groups, alkylene groups, aryl groups, and combinations of two or more of these. When the other substituents are a combination of two or more types, the content ratio of each of the substituents is not limited. Among them, the other substituents are preferably anionic substituents and their salts, or acyl groups from the viewpoint of nano-dispersibility. As the anionic substituents and their salts, particularly preferred are carboxy groups, phosphate groups, phosphite groups, and xanthate groups. When the anionic substituent is in the form of a salt, sodium salts, potassium salts, and calcium salts are particularly preferred from the viewpoint of nano-dispersibility. In addition, as a particularly preferred acyl group, an acetyl group is preferred from the viewpoint of nano-dispersibility.
[0038] The average fiber diameter of the cellulose nanofiber having sulfate ester groups of the present invention is equivalent to the fiber diameter of the cellulose nanofiber defined above, and is usually in the range of 1 nm to 1000 nm. The average fiber diameter of the cellulose nanofiber is preferably 2 nm to 200 nm, more preferably 3 nm to 50 nm. If the average fiber diameter is less than 1 nm, the performance aspects such as the strength of the nanofiber may be reduced. If the average fiber diameter exceeds 1000 nm, the performance of the nanofiber tends to be difficult to exhibit due to the large fiber diameter. The average fiber diameter is the value obtained by averaging 50 fibers randomly selected from an atomic force microscope image, as in the case of the cellulose nanofiber described above. The average fiber width and average fiber length can be set to a desired range by adjusting the concentration of the reagent such as sulfuric acid, the amount of pulp relative to the reaction solution, and the reaction time.
[0039] The degree of crystallinity of the cellulose nanofibers having sulfate ester groups of the present invention may depend on the raw cellulose used. For example, the inherent crystallinity of cotton cellulose may be higher than that of wood cellulose. In other words, the degree of crystallinity of the cellulose nanofibers varies depending on the raw cellulose used. However, the degree of crystallinity of the cellulose nanofibers affects the performance of the cellulose nanofibers, such as homogenization with lignin-derived substances, processability, heat resistance, and reinforcing effect, and is therefore usually 20% to 99%, preferably 25% to 90%, more preferably 30% to 85%, and even more preferably 35% to 80%. If the degree of crystallinity is lower than 20%, the heat resistance and rigidity of the cellulose nanofibers may decrease.
[0040] An example of the cellulose nanofiber having sulfate ester groups of the present invention is as follows. [ka]
[0041] As a method for producing cellulose nanofibers having sulfate ester groups according to the present invention, a method can be applied in which cellulose fibers such as pulp are treated with a defibrating solution consisting of dimethyl sulfoxide (DMSO), acetic anhydride, and sulfuric acid. In addition, a method can be applied in which cellulose fibers such as pulp are treated with a defibrating solution in which sulfamic acid, urea, or a urea derivative is dissolved in a solvent such as water.
[0042] Adjustment of the sulfuric acid or sulfamic acid concentration is particularly effective as a factor for changing the amount of sulfur introduced. When the concentration of sulfuric acid or sulfamic acid in the defibration liquid is less than 1 mass%, the amount of sulfur introduced is easily adjusted to less than 1.0 mmol / g. When the concentration of sulfuric acid or sulfamic acid in the defibration liquid is 1 mass% to 3 mass%, the amount of sulfur introduced is easily adjusted to 1.0 mmol / g to 3.0 mmol / g. In addition, if the concentration of sulfuric acid or sulfamic acid in the defibration liquid is too high, the fiber length of the sulfated CNF tends to be short. Therefore, in order to obtain CNF with a long fiber length, it is effective to take measures such as not increasing the concentration of sulfuric acid or sulfamic acid in the defibration liquid too much and extending the reaction time.
[0043] The cellulose nanofiber having sulfate ester groups in the present invention can be a cellulose nanofiber having sulfate ester groups known in the art, and its manufacturing method is also known. As the cellulose nanofiber having sulfate ester groups, for example, the cellulose nanofiber having sulfate ester groups described in JP 2020-41255 A can be used.
[0044] The acid generator of the present invention may further contain one or more salts selected from metal salts and ammonium salts.
[0045] In the metal salt, the metal ion may be an alkali metal ion, an alkaline earth metal ion, a transition metal ion, or another metal ion.
[0046] Here, examples of the alkali metal ion include lithium ion, sodium ion, potassium ion, rubidium ion, and cesium ion. Examples of the alkaline earth metal ion include calcium ion and strontium ion. Examples of the transition metal ion include iron ion, nickel ion, palladium ion, copper ion, and silver ion. Examples of other metal ions include beryllium ion, magnesium ion, zinc ion, and aluminum ion. Examples of the counter anion of the metal ion include an anion of an organic acid, for example, a carboxylate ion, such as an acetate ion, an anion of an inorganic acid, for example, a sulfate ion, and a halide ion, for example, a fluoride ion (F - ), chloride ion (Cl - ), bromide ion (Br - ) and iodide ion (I - , I 3- ) etc.
[0047] In ammonium salts, the ammonium ion is NH4 + Not only NH4 + Examples of ammonium ions include those derived from various amines in which one or more hydrogen atoms are replaced by organic groups. For example, NH + , quaternary ammonium cation, alkanolamine ion, pyridinium ion, etc. Counter anions of the ammonium ion include anions of organic acids, such as carboxylate ions, for example acetate ions, anions of inorganic acids, for example sulfate ions, halide ions, for example fluoride ions, chloride ions, bromide ions, and iodide ions, etc.
[0048] The content of the salt is not limited, but is usually 0.002 parts by mass to 10 parts by mass, and preferably 0.01 parts by mass to 0.1 parts by mass, per 100 parts by mass of the cellulose nanofibers having sulfate ester groups.
[0049] By containing the salt in the above amount in the acid generator of the present invention, the viscosity of the acid generator and the amount of acid generated can be appropriately adjusted.
[0050] The acid generator of the present invention may further contain water.
[0051] The water content is usually 50% by mass or less, and preferably 20% by mass or less, based on the total mass of the acid generator, and is usually 1,000 parts by mass or more, and preferably 5,000 parts by mass or more, based on 100 parts by mass of the cellulose nanofiber having sulfate ester groups.
[0052] When the water content is within the above range, the viscosity can be adjusted by the thickening effect of the cellulose nanofiber during production of the aqueous polymerizable polymer and / or aqueous crosslinked polymer, and the degree of diffusion of the generated acid can be controlled, making it possible to provide an appropriate amount of acid generator during the production.
[0053] The acid generator of the present invention may further contain one or more additives.
[0054] The additives include various bases.
[0055] The content of the additive varies depending on the required use of the additive, so is not limited, but is usually 0.001 to 5.0 parts by mass, and preferably 0.01 to 1.0 part by mass, per 100 parts by mass of cellulose nanofiber having sulfate ester groups.
[0056] The form of the acid generator of the present invention is not limited. The acid generator of the present invention may be in any shape, such as a solid or semi-solid form, such as a powder, a spherical form, an elliptical form, or a polygonal form, or in the form of a dispersion dispersed in a solvent, such as water, alcohol, ethylene glycol monobutyl ether, formamide, or a mixture thereof. When alcohol, ethylene glycol monobutyl ether, or formamide is used as the solvent, it is preferable that the solvent contains 50% by mass or more of water from the viewpoint of uniform dispersion.
[0057] When the acid generator of the present invention is mixed with water to prepare an aqueous dispersion having a cellulose nanofiber concentration of 0.3 mass% relative to the total mass of the aqueous dispersion, and the aqueous dispersion is heat-treated at 80°C for 24 hours, the pH of the aqueous dispersion after heat treatment is usually 0.5 to 6.0, and preferably 1.0 to 4.0, lower than the pH before heat treatment.
[0058] Since the acid generator of the present invention has the above-mentioned pH lowering effect, it can be used as an acid generator during the production of an aqueous polymerizable polymer and / or an aqueous crosslinked polymer.
[0059] When the acid generator of the present invention is mixed with water to prepare an aqueous dispersion in which the concentration of the cellulose nanofibers is 0.3 mass% relative to the total mass of the aqueous dispersion, the viscosity of the aqueous dispersion measured at 2.6 rpm at 25° C. is usually 500 mPa s or more, preferably 2,000 mPa s or more. There are no limitations on the upper limit of the viscosity, but it is usually 100,000 mPa s, preferably 50,000 mPa s.
[0060] In the production of aqueous polymerizable polymers and aqueous crosslinked polymers, it takes time for the water medium to dry. Therefore, if polymerization or crosslinking by acid is started and the reaction is completed in an insufficient drying state, the cured film may become non-uniformly porous. This is because even after the reaction is completed, the water remaining in the coating film gradually evaporates as time passes, and as a result, holes originating from the remaining water are formed in the coating film. Therefore, when the polymer is produced in a particularly thick film, an acid generator is required that has an acid generating mechanism that disperses in the water medium during polymerization and crosslinking, and gradually releases acid during the drying of the coating film, i.e., the process in which the water gradually dries from the coating film, to promote polymerization and crosslinking.
[0061] For example, the photoacid generator composition of Patent Document 2 is a photoacid generator having an onium salt skeleton. Therefore, although the photoacid generator composition can generate acid rapidly by light energy, it is difficult to gradually release acid over a long period of time. In addition, when the photocuring of a coating film is performed all at once using the photoacid generator composition in a state where the water in the medium is not sufficiently dried, the curing is completed with water remaining in the coating film. If moisture remains in the coating film, as described above, holes derived from the remaining water are formed in the coating film obtained thereafter, and the final coating film becomes porous. Therefore, this phenomenon is particularly noticeable when forming a thick coating film, and there was a problem that it may be difficult to form the desired dense film.
[0062] The acid generator of the present invention has the above-mentioned viscosity, so that the diffusion rate of the acid can be controlled during the production of the aqueous polymerizable polymer and / or the aqueous crosslinked polymer, and the polymerization rate of the aqueous polymerizable polymer and / or the aqueous crosslinked polymer can be adjusted. For example, when the viscosity is increased by the acid generator of the present invention, the polymerization rate can be adjusted to be slow. If the polymerization rate can be adjusted to be slow, it is possible to suppress the porosity of the coating film caused by the polymerization or crosslinking being completed during the drying of the coating film when the aqueous polymerizable polymer and / or the aqueous crosslinked polymer is coated in a thick film.
[0063] The acid generator of the present invention can be used as a curing agent for coating materials, adhesives, and molding materials of aqueous polymerizable polymers and / or aqueous crosslinked polymers. EXAMPLES
[0064] The present invention will be described in more detail below using examples, but the technical scope of the present invention is not limited to these examples.
[0065] <Method for producing cellulose nanofibers having sulfate ester groups (sulfate-esterified CNF)> (Sample 1) 150 g of dimethyl sulfoxide (DMSO), 16.5 g of acetic anhydride, and 3.35 g of sulfuric acid (concentration in defibration solution: 1.97% by mass) were placed in a 300 ml sample bottle and stirred for approximately 30 seconds using a magnetic stirrer at room temperature of 23°C to prepare a defibration solution.
[0066] Next, 5.0 g of softwood kraft pulp NBKP (manufactured by Nippon Paper Industries Co., Ltd.) was added to the defibrated solution and stirred for an additional 30 minutes at room temperature of 23°C to carry out a sulfuric acid esterification reaction. After stirring, 250 ml of distilled water was added to the cellulose-containing defibrated solution to stop the reaction, and then a 5% by mass aqueous solution of sodium hydroxide was added until the pH reached 7 to neutralize the sulfuric acid in the reaction solution. After that, the supernatant was removed by centrifugation (speed: 12,000 rpm, centrifugation time: 50 minutes).
[0067] Further, 1350 ml of distilled water and 1350 ml of ethanol were added and stirred until uniformly dispersed, and then the supernatant was removed by centrifugation under the same conditions as above. The same procedure was repeated for a total of three washings. After washing by centrifugation, distilled water was added and the total weight was diluted to 1000 g.
[0068] Next, the mixture was stirred for 3 minutes using a mixer (G5200, manufactured by Biolomix) to obtain a uniform aqueous dispersion of sulfated CNF with a concentration of 0.5% by mass and an incorporated sulfur amount of 0.4 mmol / g.
[0069] Next, the obtained aqueous dispersion of sulfated CNF was frozen in a freezer at -18°C for 24 hours, and then dried for 72 hours using a freeze dryer (FDU-2110, Tokyo Rikakikai Co., Ltd.) to obtain a dried sulfated CNF with a moisture content of 8%.
[0070] (Sample 2) 150 g of dimethyl sulfoxide (DMSO), 16.5 g of acetic anhydride, and 3.35 g of sulfuric acid (concentration in defibration solution: 1.97% by mass) were placed in a 300 ml sample bottle and stirred for approximately 30 seconds using a magnetic stirrer at room temperature of 23°C to prepare a defibration solution.
[0071] Next, 5.0 g of softwood kraft pulp NBKP (manufactured by Nippon Paper Industries Co., Ltd.) was added to the defibrated solution and stirred for an additional 2 hours at room temperature of 23°C to carry out a sulfuric acid esterification reaction. After stirring, 250 ml of distilled water was added to the cellulose-containing defibrated solution to stop the reaction, and then a 5% by mass aqueous solution of sodium hydroxide was added until the pH reached 7 to neutralize the sulfuric acid in the reaction solution. After that, the supernatant was removed by centrifugation (speed: 12,000 rpm, centrifugation time: 50 minutes).
[0072] Further, 1350 ml of distilled water and 1350 ml of ethanol were added and stirred until uniformly dispersed, and then the supernatant was removed by centrifugation under the same conditions as above. The same procedure was repeated for a total of three washings. After washing by centrifugation, distilled water was added and the total weight was diluted to 1000 g.
[0073] Next, the mixture was stirred for 3 minutes using a mixer (G5200, manufactured by Biolomix) to obtain a uniform aqueous dispersion of sulfated CNF with a concentration of 0.5% by mass and an incorporated sulfur amount of 1.5 mmol / g.
[0074] Next, the obtained aqueous dispersion of sulfated CNF was frozen in a freezer at -18°C for 24 hours, and then dried for 72 hours using a freeze dryer (FDU-2110, Tokyo Rikakikai Co., Ltd.) to obtain a dried sulfated CNF with a moisture content of 5%.
[0075] (Sample 3) 150 g of dimethyl sulfoxide (DMSO), 16.5 g of acetic anhydride, and 3.35 g of sulfuric acid (concentration in defibration solution: 1.97% by mass) were placed in a 300 ml sample bottle and stirred for approximately 30 seconds using a magnetic stirrer at room temperature of 23°C to prepare a defibration solution.
[0076] Next, 5.0 g of softwood kraft pulp NBKP (manufactured by Nippon Paper Industries Co., Ltd.) was added to the defibrated solution and stirred for an additional 2 hours at room temperature of 23°C to carry out a sulfuric acid esterification reaction. After stirring, 250 ml of distilled water was added to the cellulose-containing defibrated solution to stop the reaction, and then a 5% by mass aqueous solution of sodium hydroxide was added until the pH reached 7 to neutralize the sulfuric acid in the reaction solution. After that, the supernatant was removed by centrifugation (speed: 12,000 rpm, centrifugation time: 50 minutes).
[0077] Further, 1350 ml of distilled water and 1350 ml of ethanol were added and stirred until uniformly dispersed, and then the supernatant was removed by centrifugation under the same conditions as above. The same procedure was repeated for a total of three washings. After washing by centrifugation, distilled water was added and the total weight was diluted to 1000 g.
[0078] Next, the mixture was stirred for 3 minutes using a mixer (G5200, manufactured by Biolomix) to obtain a uniform aqueous dispersion of sulfated CNF with a concentration of 0.5% by mass and an incorporated sulfur amount of 1.5 mmol / g.
[0079] Next, the obtained aqueous dispersion of sulfated CNF was frozen in a freezer at -18°C for 24 hours, and then dried for 24 hours using a freeze dryer (FDU-2110, Tokyo Rikakikai Co., Ltd.) to obtain a dried sulfated CNF with a moisture content of 48%.
[0080] (Sample 4) 150 g of dimethyl sulfoxide (DMSO), 16.5 g of acetic anhydride, and 5 g of sulfuric acid (concentration in defibration solution: 2.92 mass%) were placed in a 300 ml sample bottle and stirred for approximately 30 seconds using a magnetic stirrer at room temperature of 23°C to prepare a defibration solution.
[0081] Next, 5.0 g of softwood kraft pulp NBKP (manufactured by Nippon Paper Industries Co., Ltd.) was added to the defibrated solution and stirred for an additional 2 hours at room temperature of 23°C to carry out a sulfuric acid esterification reaction. After stirring, 250 ml of distilled water was added to the cellulose-containing defibrated solution to stop the reaction, and then a 5% by mass aqueous solution of sodium hydroxide was added until the pH reached 7 to neutralize the sulfuric acid in the reaction solution. After that, the supernatant was removed by centrifugation (speed: 12,000 rpm, centrifugation time: 50 minutes).
[0082] Further, 1350 ml of distilled water and 1350 ml of ethanol were added and stirred until uniformly dispersed, and then the supernatant was removed by centrifugation under the same conditions as above. The same procedure was repeated for a total of three washings. After washing by centrifugation, distilled water was added and the total weight was diluted to 1000 g.
[0083] Next, the mixture was stirred for 3 minutes using a mixer (G5200, manufactured by Biolomix) to obtain a uniform aqueous dispersion of sulfated CNF with a concentration of 0.5% by mass and an incorporated sulfur amount of 2.8 mmol / g.
[0084] Next, the obtained aqueous dispersion of sulfated CNF was frozen in a freezer at -18°C for 24 hours, and then dried for 72 hours using a freeze dryer (FDU-2110, Tokyo Rikakikai Co., Ltd.) to obtain a dried sulfated CNF with a moisture content of 6%.
[0085] (Sample 5) 150 g of dimethyl sulfoxide (DMSO), 16.5 g of acetic anhydride, and 3.35 g of sulfuric acid (concentration in defibration solution: 1.97% by mass) were placed in a 300 ml sample bottle and stirred for approximately 30 seconds using a magnetic stirrer at room temperature of 23°C to prepare a defibration solution.
[0086] Next, 5.0 g of softwood kraft pulp NBKP (manufactured by Nippon Paper Industries Co., Ltd.) was added to the defibrated solution and stirred for an additional 2 hours at room temperature of 23°C to carry out a sulfuric acid esterification reaction. After stirring, 250 ml of distilled water was added to the cellulose-containing defibrated solution to stop the reaction, and then a 5% by mass aqueous solution of sodium hydroxide was added until the pH reached 7 to neutralize the sulfuric acid in the reaction solution. After that, the supernatant was removed by centrifugation (speed: 12,000 rpm, centrifugation time: 50 minutes).
[0087] Further, 1350 ml of distilled water and 1350 ml of ethanol were added and stirred until uniformly dispersed, and then the supernatant was removed by centrifugation under the same conditions as above. The same procedure was repeated for washing three times in total.
[0088] Next, 100 ml of distilled water was added to the washed solid matter and stirred with a stirrer for 5 minutes to prepare an aqueous dispersion, which was then frozen in a freezer at -18°C for 24 hours and then dried for 72 hours using a freeze dryer (FDU-2110, manufactured by Tokyo Rikakikai Co., Ltd.).
[0089] Next, 5 g of the freeze-dried solid, 1 g of an aqueous sodium acetate solution, and 994 g of distilled water were mixed together. Here, the aqueous sodium acetate solution was prepared by mixing 10 mg of sodium acetate and 100 g of distilled water.
[0090] Next, the mixture was stirred for 3 minutes using a mixer (G5200, manufactured by Biolomix) to obtain a uniform aqueous dispersion of sulfated CNF with a concentration of 0.5% by mass and an incorporated sulfur amount of 1.5 mmol / g.
[0091] Next, the obtained aqueous dispersion of sulfated CNF was dried for 72 hours using a freeze dryer (FDU-2110, Tokyo Rikakikai Co., Ltd.) to obtain a dried sulfated CNF with a moisture content of 3% and containing 0.002 mass% sodium acetate relative to the sulfated CNF.
[0092] (Sample 6) 150 g of dimethyl sulfoxide (DMSO), 16.5 g of acetic anhydride, and 3.35 g of sulfuric acid (concentration in defibration solution: 1.97% by mass) were placed in a 300 ml sample bottle and stirred for approximately 30 seconds using a magnetic stirrer at room temperature of 23°C to prepare a defibration solution.
[0093] Next, 5.0 g of softwood kraft pulp NBKP (manufactured by Nippon Paper Industries Co., Ltd.) was added to the defibrated solution and stirred for an additional 2 hours at room temperature of 23°C to carry out a sulfuric acid esterification reaction. After stirring, 250 ml of distilled water was added to the cellulose-containing defibrated solution to stop the reaction, and then a 5% by mass aqueous solution of sodium hydroxide was added until the pH reached 7 to neutralize the sulfuric acid in the reaction solution. After that, the supernatant was removed by centrifugation (speed: 12,000 rpm, centrifugation time: 50 minutes).
[0094] Further, 1350 ml of distilled water and 1350 ml of ethanol were added and stirred until uniformly dispersed, and then the supernatant was removed by centrifugation under the same conditions as above. The same procedure was repeated for washing three times in total.
[0095] Next, 100 ml of distilled water was added to the washed solid matter and stirred with a stirrer for 5 minutes to prepare an aqueous dispersion, which was then frozen in a freezer at -18°C for 24 hours and then dried for 72 hours using a freeze dryer (FDU-2110, manufactured by Tokyo Rikakikai Co., Ltd.).
[0096] Next, 5 g of the freeze-dried solid, 1 g of an aqueous sodium acetate solution, and 994 g of distilled water were mixed together. Here, the aqueous sodium acetate solution was prepared by mixing 0.5 g of sodium acetate and 99.5 g of distilled water.
[0097] Next, the mixture was stirred for 3 minutes using a mixer (G5200, manufactured by Biolomix) to obtain a uniform aqueous dispersion of sulfated CNF with a concentration of 0.5% by mass and an incorporated sulfur amount of 1.5 mmol / g.
[0098] Next, the obtained aqueous dispersion of sulfated CNF was dried for 72 hours using a freeze dryer (FDU-2110, Tokyo Rikakikai Co., Ltd.) to obtain a dried sulfated CNF with a moisture content of 4% and containing 0.1 mass% sodium acetate relative to the sulfated CNF.
[0099] (Sample 7) 150 g of dimethyl sulfoxide (DMSO), 16.5 g of acetic anhydride, and 3.35 g of sulfuric acid (concentration in defibration solution: 1.97% by mass) were placed in a 300 ml sample bottle and stirred for approximately 30 seconds using a magnetic stirrer at room temperature of 23°C to prepare a defibration solution.
[0100] Next, 5.0 g of softwood kraft pulp NBKP (manufactured by Nippon Paper Industries Co., Ltd.) was added to the defibrated solution and stirred for an additional 2 hours at room temperature of 23°C to carry out a sulfuric acid esterification reaction. After stirring, 250 ml of distilled water was added to the cellulose-containing defibrated solution to stop the reaction, and then a 5% by mass aqueous solution of sodium hydroxide was added until the pH reached 7 to neutralize the sulfuric acid in the reaction solution. After that, the supernatant was removed by centrifugation (speed: 12,000 rpm, centrifugation time: 50 minutes).
[0101] Further, 1350 ml of distilled water and 1350 ml of ethanol were added and stirred until uniformly dispersed, and then the supernatant was removed by centrifugation under the same conditions as above. The same procedure was repeated for washing three times in total.
[0102] Next, 100 ml of distilled water was added to the washed solid matter and stirred with a stirrer for 5 minutes to prepare an aqueous dispersion, which was then frozen in a freezer at -18°C for 24 hours and then dried for 72 hours using a freeze dryer (FDU-2110, manufactured by Tokyo Rikakikai Co., Ltd.).
[0103] Next, 5 g of the freeze-dried solid was mixed with 0.4 g of sodium acetate and 994.6 g of distilled water.
[0104] Next, the mixture was stirred for 3 minutes using a mixer (G5200, manufactured by Biolomix) to obtain a uniform aqueous dispersion of sulfated CNF with a concentration of 0.5% by mass and an incorporated sulfur amount of 1.5 mmol / g.
[0105] Next, the obtained aqueous dispersion of sulfated CNF was dried for 72 hours using a freeze dryer (FDU-2110, Tokyo Rikakikai Co., Ltd.) to obtain a dried sulfated CNF with a moisture content of 6% and containing 8% by mass of sodium acetate relative to the sulfated CNF.
[0106] (Sample 8) 150 g of dimethyl sulfoxide (DMSO), 16.5 g of acetic anhydride, and 3.35 g of sulfuric acid (concentration in defibration solution: 1.97% by mass) were placed in a 300 ml sample bottle and stirred for approximately 30 seconds using a magnetic stirrer at room temperature of 23°C to prepare a defibration solution.
[0107] Next, 5.0 g of softwood kraft pulp NBKP (manufactured by Nippon Paper Industries Co., Ltd.) was added to the defibrated solution and stirred for an additional 2 hours at room temperature of 23°C to carry out a sulfuric acid esterification reaction. After stirring, 250 ml of distilled water was added to the cellulose-containing defibrated solution to stop the reaction, and then a 5% by mass aqueous solution of sodium hydroxide was added until the pH reached 7 to neutralize the sulfuric acid in the reaction solution. After that, the supernatant was removed by centrifugation (speed: 12,000 rpm, centrifugation time: 50 minutes).
[0108] Further, 1350 ml of distilled water and 1350 ml of ethanol were added and stirred until uniformly dispersed, and then the supernatant was removed by centrifugation under the same conditions as above. The same procedure was repeated for washing three times in total.
[0109] Next, 100 ml of distilled water was added to the washed solid matter and stirred with a stirrer for 5 minutes to prepare an aqueous dispersion, which was then frozen in a freezer at -18°C for 24 hours and then dried for 72 hours using a freeze dryer (FDU-2110, manufactured by Tokyo Rikakikai Co., Ltd.).
[0110] Next, 5 g of the freeze-dried solid, 1 g of an aqueous sodium sulfate solution, and 994 g of distilled water were mixed together. Here, the aqueous sodium sulfate solution was prepared by mixing 0.5 g of sodium sulfate and 99.5 g of distilled water.
[0111] Next, the mixture was stirred for 3 minutes using a mixer (G5200, manufactured by Biolomix) to obtain a uniform aqueous dispersion of sulfated CNF with a concentration of 0.5% by mass and an incorporated sulfur amount of 1.5 mmol / g.
[0112] Next, the obtained aqueous dispersion of sulfated CNF was dried for 72 hours using a freeze dryer (FDU-2110, Tokyo Rikakikai Co., Ltd.) to obtain a dried sulfated CNF with a moisture content of 8% and containing 0.1 mass% sodium sulfate relative to the sulfated CNF.
[0113] (Sample 9) 150 g of dimethyl sulfoxide (DMSO), 16.5 g of acetic anhydride, and 3.35 g of sulfuric acid (concentration in defibration solution: 1.97% by mass) were placed in a 300 ml sample bottle and stirred for approximately 30 seconds using a magnetic stirrer at room temperature of 23°C to prepare a defibration solution.
[0114] Next, 5.0 g of softwood kraft pulp NBKP (manufactured by Nippon Paper Industries Co., Ltd.) was added to the defibrated solution and stirred for an additional 2 hours at room temperature of 23°C to carry out a sulfuric acid esterification reaction. After stirring, 250 ml of distilled water was added to the cellulose-containing defibrated solution to stop the reaction, and then a 5% by mass aqueous solution of sodium hydroxide was added until the pH reached 7 to neutralize the sulfuric acid in the reaction solution. After that, the supernatant was removed by centrifugation (speed: 12,000 rpm, centrifugation time: 50 minutes).
[0115] Further, 1350 ml of distilled water and 1350 ml of ethanol were added and stirred until uniformly dispersed, and then the supernatant was removed by centrifugation under the same conditions as above. The same procedure was repeated for washing three times in total.
[0116] Next, 100 ml of distilled water was added to the washed solid matter and stirred with a stirrer for 5 minutes to prepare an aqueous dispersion, which was then frozen in a freezer at -18°C for 24 hours and then dried for 72 hours using a freeze dryer (FDU-2110, manufactured by Tokyo Rikakikai Co., Ltd.).
[0117] Next, 5 g of the freeze-dried solid, 1 g of an aqueous ammonium sulfate solution, and 994 g of distilled water were mixed together. Here, the aqueous ammonium sulfate solution was prepared by mixing 0.5 g of ammonium sulfate and 99.5 g of distilled water.
[0118] Next, the mixture was stirred for 3 minutes using a mixer (G5200, manufactured by Biolomix) to obtain a uniform aqueous dispersion of sulfated CNF with a concentration of 0.5% by mass and an incorporated sulfur amount of 1.5 mmol / g.
[0119] Next, the obtained aqueous dispersion of sulfated CNF was dried for 72 hours using a freeze dryer (FDU-2110, manufactured by Tokyo Rikakikai Co., Ltd.) to obtain a dried sulfated CNF with a moisture content of 4% and 0.1% by mass of ammonium sulfate relative to the sulfated CNF.
[0120] (Sample 10) 150 g of dimethyl sulfoxide (DMSO), 16.5 g of acetic anhydride, and 3.35 g of sulfuric acid (concentration in defibration solution: 1.97% by mass) were placed in a 300 ml sample bottle and stirred for approximately 30 seconds using a magnetic stirrer at room temperature of 23°C to prepare a defibration solution.
[0121] Next, 5.0 g of softwood kraft pulp NBKP (manufactured by Nippon Paper Industries Co., Ltd.) was added to the defibrated solution and stirred for an additional 2 hours at room temperature of 23°C to carry out a sulfuric acid esterification reaction. After stirring, 250 ml of distilled water was added to the cellulose-containing defibrated solution to stop the reaction, and then a 5% by mass aqueous solution of sodium hydroxide was added until the pH reached 7 to neutralize the sulfuric acid in the reaction solution. After that, the supernatant was removed by centrifugation (speed: 12,000 rpm, centrifugation time: 50 minutes).
[0122] Further, 1350 ml of distilled water and 1350 ml of ethanol were added and stirred until uniformly dispersed, and then the supernatant was removed by centrifugation under the same conditions as above. The same procedure was repeated for washing three times in total.
[0123] Next, 100 ml of distilled water was added to the washed solid matter and stirred with a stirrer for 5 minutes to prepare an aqueous dispersion, which was then frozen in a freezer at -18°C for 24 hours and then dried for 72 hours using a freeze dryer (FDU-2110, manufactured by Tokyo Rikakikai Co., Ltd.).
[0124] Next, 5 g of the freeze-dried solid, 1 g of an aqueous calcium acetate solution, and 994 g of distilled water were mixed together. Here, the aqueous calcium acetate solution was prepared by mixing 0.5 g of calcium acetate and 99.5 g of distilled water.
[0125] Next, the mixture was stirred for 3 minutes using a mixer (G5200, manufactured by Biolomix) to obtain a uniform aqueous dispersion of sulfated CNF with a concentration of 0.5% by mass and an incorporated sulfur amount of 1.5 mmol / g.
[0126] Next, the obtained aqueous dispersion of sulfated CNF was dried for 72 hours using a freeze dryer (FDU-2110, manufactured by Tokyo Rikakikai Co., Ltd.) to obtain a dried sulfated CNF with a moisture content of 2% and containing 0.1 mass% calcium acetate relative to the sulfated CNF.
[0127] (Sample 11) 0.13 mmol of 2,2,6,6-tetramethylpiperidine-N-oxyl (TEMPO) and 10 mmol of sodium bromide were dissolved in water to obtain a 250 mL aqueous solution. 5 g of absolute dry softwood kraft pulp NBKP (manufactured by Nippon Paper Industries Co., Ltd.) was added to this aqueous solution and stirred until the pulp was uniformly dispersed. After the temperature of the mixture was brought to 20°C, 32 mmol of an aqueous sodium hypochlorite solution (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to start the oxidation reaction. During the reaction, the temperature of the reaction system was kept at 20°C, and the pH was maintained at 10 by successively adding a 3N aqueous sodium hydroxide solution. After the reaction for 3 hours, the resultant product was filtered through a glass filter, and the filter cake was thoroughly washed with water. As a result, an oxidation-treated pulp was obtained.
[0128] Ion-exchanged water was added to the oxidized pulp to adjust the solid content of the slurry to 0.5% by mass, and the slurry was treated three times at 140 MPa using an ultra-high pressure homogenizer to obtain an aqueous dispersion of TEMPO-oxidized CNF. The aqueous dispersion of CNF obtained was then frozen in a freezer at -18°C for 24 hours. It was then placed in a freeze dryer (FDU-2110, Tokyo Rikakikai Co., Ltd.) and dried for 72 hours to obtain a TEMPO-oxidized CNF dried body with a moisture content of 5%.
[0129] (Sample 12) A phosphorylating reagent was prepared by dissolving 5 g of urea, 2.8 g of sodium dihydrogen phosphate dihydrate, and 2.1 g of disodium hydrogen phosphate in 5.5 g of water.
[0130] A dry softwood kraft pulp NBKP (manufactured by Nippon Paper Industries Co., Ltd.) was processed in a cutter mill and a pin mill to obtain cotton-like fibers. A phosphorylation reagent was sprayed evenly onto 5 g of cotton-like fibers on an absolute dry basis, and the fibers were kneaded by hand to obtain impregnated pulp. The impregnated pulp was heat-treated for 80 minutes in a damper-equipped air dryer heated to 140°C. The above treatments yielded phosphorylated pulp.
[0131] 500mL of ion-exchanged water was added to 5g of phosphorylated pulp, and the mixture was stirred until uniformly dispersed, and the dispersion was filtered and dehydrated. The obtained sheet was stirred with 500mL of ion-exchanged water until uniformly dispersed, and the dispersion was filtered and dehydrated. The obtained sheet was treated once more in the same manner. Next, while stirring the obtained sheet and 500mL of ion-exchanged water, 1N aqueous sodium hydroxide solution was added little by little to obtain a pulp slurry with a pH of 12 to 13. This pulp slurry was dehydrated to obtain a sheet. The sheet was stirred with 500mL of ion-exchanged water until uniformly dispersed, and the dispersion was filtered and dehydrated. The obtained sheet was treated twice more in the same manner. The obtained sheet was mixed with ion-exchanged water to obtain a slurry containing 0.5% by mass of phosphorylated pulp.
[0132] A slurry containing 0.5% by mass of phosphorylated pulp was defibrated for 180 minutes at 6,900 rpm using a defibration treatment device (Clearmix-11S, manufactured by M-Technique Co., Ltd.). Ion-exchanged water was then added to adjust the solid content of the slurry to 0.5% by mass, and an aqueous dispersion of phosphorylated CNF was obtained.
[0133] The resulting aqueous dispersion of CNF was then frozen in a freezer at -18°C for 24 hours, and then placed in a freeze dryer (FDU-2110, Tokyo Rikakikai Co., Ltd.) and dried for 72 hours to obtain a phosphate-esterified CNF dry body.
[0134] (Sample 13: Photoacid generator described in JP 2013-234320 A) As a photoacid generator, exemplified compound 1 described in JP2013-234320A [ka] Sample 13 was prepared by the method described in Synthesis Example 1 of JP2013-234320A.
[0135] The amounts of sulfur introduced into Samples 1 to 10 were quantified using an infrared spectrometer (Nicolet iS 5N FT-IR, manufactured by Thermo Fisher Science) and an organic elemental analyzer (EA-3100, manufactured by JASCO).
[0136] Moreover, the moisture content (%) of Samples 1 to 12 was measured in accordance with JIS P 8203. That is, the moisture content (%) was calculated based on the following formula. Moisture content (%) = ((mass of sample - mass of solids of sample) / mass of sample) x 100 (In the formula, the mass of the sample means the mass (g) of the sample used for the measurement, i.e., the mass of the dried CNF, and the mass of the solid content of the sample means the mass (g) of the solid matter remaining after drying an equal amount of the sample used for the measurement in an atmosphere at 105°C for 2 hours until it reaches a constant mass, i.e., the mass (g) of the dried CNF after drying the dried CNF at 105°C for 2 hours until it reaches a constant mass.)
[0137] The average fiber width of the CNFs of samples 1 to 12 was measured by measuring the fiber width of 50 randomly selected fibers using an atomic force microscope (SPM-9700HT, manufactured by Shimadzu Corporation) and taking the arithmetic average value. The evaluation samples were prepared as follows.
[0138] 149.0g of distilled water was added to 1.0g of 0.5% by mass of uniform CNF aqueous dispersion, and the mixture was stirred for 3 minutes using a mixer (G5200, manufactured by Biolomix) to obtain a 0.003% by mass of uniform CNF aqueous dispersion. Next, 30μL of 0.003% by mass of uniform aqueous dispersion of exemplary compound 1 was dropped onto a natural mica (natural muscovite) substrate (15mm×15mm×thickness 0.15mm) using a micropipette, and the substrate was naturally dried for 0.5 hours to obtain a sample for fiber width evaluation.
[0139] <Method for preparing aqueous dispersion containing cellulose fibers and evaluation test method> [Example 1] The sulfated CNF of sample 1 (sulfur introduction amount: 0.4 mmol / g) was mixed with water to prepare an aqueous dispersion in which the concentration of the sulfated CNF of sample 1 was 0.3 mass% relative to the total mass of the aqueous dispersion. The viscosity of the aqueous dispersion was then measured at 2.6 rpm at 25°C. Furthermore, the aqueous dispersion was heat-treated at 80°C for 1 hour, 5 hours, and 24 hours, and the pH change from before to after the heat treatment (pH before heat treatment - pH after heat treatment) of the aqueous dispersion was measured.
[0140] [Example 2] The sulfated CNF of sample 2 (sulfur introduction amount: 1.5 mmol / g) was mixed with water to prepare an aqueous dispersion in which the concentration of the sulfated CNF of sample 2 was 0.3 mass% relative to the total mass of the aqueous dispersion. Then, the viscosity of the aqueous dispersion was measured at 2.6 rpm at 25°C. Furthermore, when the aqueous dispersion was heat-treated at 80°C for 1 hour, 5 hours, and 24 hours, the pH change of the aqueous dispersion from before to after the heat treatment (pH before heat treatment - pH after heat treatment) was measured.
[0141] [Example 3] The sulfated CNF of sample 3 (sulfur introduction amount: 1.5 mmol / g) was mixed with water to prepare an aqueous dispersion in which the concentration of the sulfated CNF of sample 3 was 0.3 mass% relative to the total mass of the aqueous dispersion. The viscosity of the aqueous dispersion was then measured at 25°C and 2.6 rpm. Furthermore, when the aqueous dispersion was heat-treated at 80°C for 24 hours, the pH change of the aqueous dispersion from before to after the heat treatment (pH before heat treatment - pH after heat treatment) was measured.
[0142] [Example 4] The sulfated CNF of sample 4 (sulfur introduction amount: 2.8 mmol / g) was mixed with water to prepare an aqueous dispersion in which the concentration of the sulfated CNF of sample 4 was 0.3 mass% relative to the total mass of the aqueous dispersion. The viscosity of the aqueous dispersion was then measured at 2.6 rpm at 25°C. Furthermore, the aqueous dispersion was heat-treated at 80°C for 1 hour, 5 hours, and 24 hours, and the pH change from before to after the heat treatment (pH before heat treatment - pH after heat treatment) of the aqueous dispersion was measured.
[0143] [Example 5] The sulfated CNF of sample 5 (sulfur introduction amount: 1.5 mmol / g), water, and sodium acetate were mixed to prepare an aqueous dispersion in which the concentration of the sulfated CNF of sample 5 was 0.3 mass% relative to the total mass of the aqueous dispersion, and the concentration of sodium acetate was 0.002 mass% relative to the total mass of the aqueous dispersion. Then, the viscosity of the aqueous dispersion measured at 2.6 rpm at 25°C was measured. Furthermore, when the aqueous dispersion was heat-treated at 80°C for 1 hour, 5 hours, and 24 hours, the pH change of the aqueous dispersion from before to after the heat treatment (pH before heat treatment - pH after heat treatment) was measured.
[0144] [Example 6] The sulfated CNF of sample 6 (sulfur introduction amount: 1.5 mmol / g), water, and sodium acetate were mixed to prepare an aqueous dispersion in which the concentration of the sulfated CNF of sample 6 was 0.3 mass% relative to the total mass of the aqueous dispersion, and the concentration of sodium acetate was 0.1 mass% relative to the total mass of the aqueous dispersion. Then, the viscosity of the aqueous dispersion measured at 2.6 rpm at 25°C was measured. Furthermore, when the aqueous dispersion was heat-treated at 80°C for 1 hour, 5 hours, and 24 hours, the pH change of the aqueous dispersion from before to after the heat treatment (pH before heat treatment - pH after heat treatment) was measured.
[0145] [Example 7] The sulfated CNF of sample 7 (sulfur introduction amount: 1.5 mmol / g), water, and sodium acetate were mixed to prepare an aqueous dispersion in which the concentration of the sulfated CNF of sample 7 was 0.3 mass% relative to the total mass of the aqueous dispersion, and the concentration of sodium acetate was 8 mass% relative to the total mass of the aqueous dispersion. Then, the viscosity of the aqueous dispersion measured at 2.6 rpm at 25°C was measured. Furthermore, when the aqueous dispersion was heat-treated at 80°C for 1 hour, 5 hours, and 24 hours, the pH change of the aqueous dispersion from before to after the heat treatment (pH before heat treatment - pH after heat treatment) was measured.
[0146] [Example 8] The sulfated CNF of sample 8 (sulfur introduction amount: 1.5 mmol / g), water, and sodium sulfate were mixed to prepare an aqueous dispersion in which the concentration of the sulfated CNF of sample 8 was 0.3 mass% relative to the total mass of the aqueous dispersion, and the concentration of sodium sulfate was 0.1 mass% relative to the total mass of the aqueous dispersion. Then, the viscosity of the aqueous dispersion measured at 2.6 rpm at 25°C was measured. Furthermore, when the aqueous dispersion was heat-treated at 80°C for 1 hour, 5 hours, and 24 hours, the pH change of the aqueous dispersion from before to after the heat treatment (pH before heat treatment - pH after heat treatment) was measured.
[0147] [Example 9] The sulfated CNF of sample 9 (sulfur introduction amount: 1.5 mmol / g), water, and ammonium sulfate were mixed to prepare an aqueous dispersion in which the concentration of the sulfated CNF of sample 9 was 0.3 mass% relative to the total mass of the aqueous dispersion, and the concentration of ammonium sulfate was 0.1 mass% relative to the total mass of the aqueous dispersion. Then, the viscosity of the aqueous dispersion measured at 2.6 rpm at 25°C was measured. Furthermore, when the aqueous dispersion was heat-treated at 80°C for 1 hour, 5 hours, and 24 hours, the pH change of the aqueous dispersion from before to after the heat treatment (pH before heat treatment - pH after heat treatment) was measured.
[0148] [Example 10] The sulfated CNF of sample 10 (sulfur introduction amount: 1.5 mmol / g), water, and calcium acetate were mixed to prepare an aqueous dispersion in which the concentration of the sulfated CNF of sample 10 was 0.3 mass% relative to the total mass of the aqueous dispersion, and the concentration of calcium acetate was 0.1 mass% relative to the total mass of the aqueous dispersion. Then, the viscosity of the aqueous dispersion measured at 2.6 rpm at 25°C was measured. Furthermore, when the aqueous dispersion was heat-treated at 80°C for 1 hour, 5 hours, and 24 hours, the pH change of the aqueous dispersion from before to after the heat treatment (pH before heat treatment - pH after heat treatment) was measured.
[0149] [Comparative Example 1] TEMPO-oxidized CNF of Sample 11 and water were mixed to prepare an aqueous dispersion in which the concentration of TEMPO-oxidized CNF of Sample 11 was 0.3% by mass based on the total mass of the aqueous dispersion. Subsequently, the viscosity of the aqueous dispersion measured at 2.6 rpm at 25°C was measured. Further, when the aqueous dispersion was heat-treated at 80°C for 1 hour, 5 hours, and 24 hours, the pH change (pH before heat treatment - pH after heat treatment) of the aqueous dispersion from before to after the heat treatment was measured.
[0150] [Comparative Example 2] Phosphorylated CNF of Sample 12 and water were mixed to prepare an aqueous dispersion in which the concentration of phosphorylated CNF of Sample 12 was 0.3% by mass based on the total mass of the aqueous dispersion. Subsequently, the viscosity of the aqueous dispersion measured at 2.6 rpm at 25°C was measured. Further, when the aqueous dispersion was heat-treated at 80°C for 1 hour, 5 hours, and 24 hours, the pH change (pH before heat treatment - pH after heat treatment) of the aqueous dispersion from before to after the heat treatment was measured.
[0151] <Evaluation Results of Aqueous Dispersion Containing CNF> Table 1 shows the results of Examples 1 to 10 and Comparative Examples 1 to 2. Figure 1 shows the relationship between the sulfur introduction amount and the viscosity. Figure 2 shows the relationship between the salt concentration and the viscosity. Note that Figure 3 is a graph in which the salt concentration in Figure 2 is shown in logarithmic scale. Figure 4 shows the relationship between the sulfur introduction amount and the pH change (pH before heat treatment - pH 24 hours after heat treatment). Figure 5 shows the relationship between the salt concentration and the pH change (pH before heat treatment - pH 24 hours after heat treatment). Note that Figure 6 is a graph in which the salt concentration in Figure 5 is shown in logarithmic scale.
[0152]
Table 1
[0153] From Table 1 and Figure 1, it was found that the viscosity of the aqueous dispersion can be adjusted by the sulfur introduction amount, that is, the introduction amount of the sulfate ester group. The viscosity of the aqueous dispersion leads to the adjustment of the diffusion rate, and as a result, leads to the adjustment of the acid release effect.
[0154] From Table 1, Figures 2 and 3, it was found that the viscosity of the aqueous dispersion can be adjusted to decrease by adding salt. The viscosity of the aqueous dispersion leads to the adjustment of the diffusion rate, and as a result, it leads to the adjustment of the acid release effect.
[0155] From Table 1 and Figure 4, it was found that when the sulfur introduction amount, that is, the introduction amount of the sulfate group, is large, the pH change (pH before heat treatment - pH after heat treatment) becomes large. In addition, since there is a proportional relationship between the introduction amount of the sulfate group and the pH change, it was found that the target pH can be achieved by adjusting the introduction amount of the sulfate group.
[0156] From Table 1, Figures 5 and 6, it was found that the pH change (pH before heat treatment - pH after heat treatment) can be adjusted by adding salt. In addition, it was found that a buffering effect can be obtained by using a weak acid salt as the salt.
[0157] <Preparation of a crosslinked film of a water-soluble polymer using a thermal acid generator composed of CNF> [Examples 11 to 20 and Comparative Examples 3 to 4] 5.0 g of polyvinyl alcohol (special grade reagent, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 95.0 g of pure water were stirred at 80 °C for 5 hours with a three-one motor stirrer (BL300, manufactured by AS ONE Corporation) to obtain a polyvinyl alcohol aqueous dispersion having a solid content concentration of 5% by mass.
[0158] Using each of Samples 1 to 12, 0.6 g of the CNF dry solid and 99.4 g of pure water were stirred with a three-one motor stirrer (BL300, manufactured by AS ONE Corporation) for 1 hour to obtain 12 kinds of CNF aqueous dispersions having a solid content concentration of 0.6% by mass.
[0159] 100 g of a polyvinyl alcohol aqueous dispersion having a solid content concentration of 5% by mass, 100 g of a CNF aqueous dispersion having a solid content concentration of 0.6% by mass, and 2.0 g of a 25% aqueous glutaraldehyde solution (Wako first grade, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as a crosslinking agent were added and stirred with a three-one motor stirrer (BL300, manufactured by AS ONE Corporation) for 1 hour to obtain a uniform reaction solution.
[0160] Next, 23.7 g (wet film thickness 1 cm) of the reaction liquid was poured into a polystyrene petri dish with an inner diameter of 55 mm and dried in an oven (OFW-600SB, AS ONE Corporation) at 80°C for 24 hours to obtain a crosslinked water-soluble polymer film (Examples 11 to 20: Preparation of crosslinked water-soluble polymer films using Samples 1 to 10 as acid generators, respectively; Comparative Examples 3 and 4: Preparation of crosslinked water-soluble polymer films using Samples 11 and 12, respectively).
[0161] <Preparation of crosslinked film of water-soluble polymer using photoacid generator> [Comparative Example 5] 5.0 g of polyvinyl alcohol (special reagent grade, Fujifilm Wako Pure Chemical Industries, Ltd.) and 95.0 g of pure water were stirred at 80° C. for 5 hours using a three-one motor stirrer (BL300, AS ONE Corporation) to obtain a polyvinyl alcohol aqueous dispersion with a solids concentration of 5% by mass.
[0162] 0.6 g of the photoacid generator Sample 13 and 99.4 g of pure water were stirred with a stirrer for 1 hour to obtain an aqueous dispersion of the photoacid generator with a solid content concentration of 0.6 mass %.
[0163] 100 g of a polyvinyl alcohol aqueous dispersion with a solid content concentration of 5% by mass, 100 g of a photoacid generator aqueous dispersion with a solid content concentration of 0.6% by mass, and 2.0 g of a 25% aqueous glutaraldehyde solution (Wako Grade 1, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as a crosslinker were added and stirred for 1 hour with a three-one motor stirrer (BL300, manufactured by AS ONE Corporation) to obtain a homogeneous reaction solution.
[0164] Next, 23.7 g (wet film thickness 1 cm) of the reaction solution was poured into a polystyrene petri dish with an inner diameter of 55 mm, and the reaction solution was incubated in air with an illuminance of 50 mW / cm at 365 nm. 2 The film was irradiated with ultraviolet light for 5 seconds in an 80°C environment using a UV curing oven (UV PITARI LED, manufactured by Hisol Co., Ltd.), and then dried at 80°C for 24 hours to obtain a crosslinked film of the water-soluble polymer.
[0165] <Evaluation of crosslinking properties of crosslinked membranes of water-soluble polymers> 0.5 g of pure water was dropped with a dropper onto the surface of the crosslinked water-soluble polymer film prepared in Examples 11 to 20 and Comparative Examples 3 to 5, and the film was left at room temperature for 24 hours. The surface of the crosslinked water-soluble polymer film after the film was left was observed with a loupe (10x magnification, MG7173, AS ONE CORPORATION) and evaluated according to the following criteria. ○: The area where the water was dropped is smooth, there are no dents or distortions on the film surface, and it can be said that the cross-linking is sufficient. ×: The part where water was dropped dissolved, and dents or distortions occurred on the film surface, indicating that crosslinking was not performed or was insufficient.
[0166] <Evaluation of the prevention of porosity in crosslinked membranes of water-soluble polymers> As an index of porosity of the crosslinked water-soluble polymer films prepared in Examples 11 to 20 and Comparative Examples 3 to 5, the haze value was measured using a haze meter (HZ-V3, manufactured by Suga Test Instruments Co., Ltd.) and evaluated according to the following indexes. ○: The haze value of the crosslinked film of the water-soluble polymer is less than 6%. △: The haze value of the crosslinked film of the water-soluble polymer is 6% or more and less than 8%. ×: The haze value of the crosslinked film of the water-soluble polymer is 8% or more.
[0167] <Evaluation results of crosslinked membrane of water-soluble polymer> Table 2 shows the evaluation results of the crosslinked water-soluble polymer films prepared in Examples 11 to 20 and Comparative Examples 3 to 5.
[0168] [Table 2]
[0169] As shown in Table 2, by using sulfated CNF as an acid generator in the crosslinking reaction of the water-based polymer, it is possible to ensure the amount of acid required to form a crosslinked water-based polymer film, i.e., crosslinkability, while also ensuring the sustained release of acid required to prevent the crosslinked water-based polymer film from becoming porous, i.e., to achieve both the crosslinking reaction and the evaporation of water.
Claims
1. An acid generator comprising, as an active ingredient, cellulose nanofiber having a sulfate ester group, The cellulose nanofiber has an average fiber width of 1 nm to 1000 nm; The sulfate ester group is represented by the following general formula (I): [Formula 1] (In general formula (I), n is an integer of 1 to 3, M n+ is an n-valent cation, and the wavy lines are the bonding sites to other atoms.) Represented by The acid generator.
2. 2. The acid generator according to claim 1, wherein an amount of sulfur introduced into the cellulose nanofiber resulting from the sulfate ester group is 0.3 mmol / g to 3.0 mmol / g relative to the mass of the cellulose nanofiber.
3. The acid generator according to claim 1, further comprising one or more salts selected from metal salts and ammonium salts, the content of the salt being 0.002 parts by mass to 10 parts by mass per 100 parts by mass of the cellulose nanofiber.
4. The acid generator according to claim 1 , further comprising water, the content of the water being 50% by mass or less based on the total mass of the acid generator.
5. The acid generator according to claim 1 , further comprising water, the content of the water being 1,000 parts by mass or more per 100 parts by mass of the cellulose nanofiber.
6. The acid generator according to claim 1, wherein when an aqueous dispersion is prepared by mixing the acid generator with water so that the concentration of the cellulose nanofibers is 0.3 mass% relative to the total mass of the aqueous dispersion, and the aqueous dispersion is heat-treated at 80°C for 24 hours, the pH of the aqueous dispersion after the heat treatment is reduced by 0.5 to 6.0 from the pH before the heat treatment.
7. 2. The acid generator according to claim 1, wherein when the acid generator and water are mixed to prepare an aqueous dispersion in which the concentration of the cellulose nanofibers is 0.3 mass% relative to the total mass of the aqueous dispersion, the viscosity of the aqueous dispersion measured at 2.6 rpm at 25°C is 500 mPa s or more.
8. The acid generator according to any one of claims 1 to 7 for producing an aqueous polymerizable polymer and / or an aqueous crosslinked polymer.
Citation Information
Patent Citations
Method for producing composition containing cellulose nanofiber and polyvinyl alcohol-based polymer
JP2019156915A
Cellulose composition and method for producing cellulose composition
JP2021152123A
Fibrous cellulose-containing substance, and application thereof
JP2022020607A
Microcrystalline cellulose fiber solid and method for producing microcrystalline cellulose fiber solid
JP7215553B1
Microcrystalline cellulose fiber powder and method for producing microcrystalline cellulose fiber powder
JP7215554B1