Tin-containing lithium oxysulfide and production method thereof
A tin-containing lithium oxysulfide with a crystalline structure is synthesized in the atmosphere, addressing moisture reactivity issues in sulfide electrolytes, providing high ionic conductivity and improved safety for lithium-ion batteries.
Patent Information
- Application Number
- JP2023057014
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing lithium-ion secondary batteries face challenges in synthesizing sulfide solid electrolytes in the atmosphere due to moisture reactivity, leading to hydrogen sulfide generation and poor moisture resistance, which affects safety and performance.
A tin-containing lithium oxysulfide with a specific composition (Li x SnO y S z ) is synthesized using mechanical milling and can be produced in the atmosphere, featuring a crystalline structure with high ionic conductivity and moisture resistance, including rock salt type Li 2 SnO 3 and lithium sulfide crystal phases.
The tin-containing lithium oxysulfide exhibits excellent ionic conductivity and moisture resistance, enabling its use as a solid electrolyte in lithium-ion batteries, reducing hydrogen sulfide generation and enhancing safety.
Smart Images

Figure 2024144864000004 
Figure 2024144864000005 
Figure 2024144864000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a tin-containing lithium oxysulfide and a method for producing the same. [Background technology]
[0002] Lithium-ion secondary batteries have been attracting attention as high-energy density batteries, and their applications are expanding not only to portable devices (small consumer applications) but also to stationary applications such as in-vehicle and social infrastructure. One of the demands for these large-scale lithium-ion secondary batteries is the improvement of safety. Ordinary lithium-ion secondary batteries (hereafter abbreviated as liquid-based) use organic electrolytes, which contain large amounts of flammable low-boiling-point solvents (dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, etc.) that fall under the second petroleum of Class 4 of the Fire Service Act as viscosity reducers, raising concerns about battery ignition and smoke. Although companies are making efforts to improve safety, if the components are changed, that is, the electrolyte is changed to a less flammable solid electrolyte, and a dramatic improvement in safety and energy density can be achieved in the material composition, it will be possible to reduce costs for safety considerations, which will be extremely useful from an industrial perspective.
[0003] There are two types of solid electrolytes: polymer electrolytes and inorganic electrolytes. Currently, polymer electrolytes have low ionic conductivity below room temperature, and sufficient battery operation similar to that of liquid electrolytes cannot be expected unless the temperature is above 60°C.
[0004] On the other hand, inorganic electrolytes include oxides and sulfides, and although oxides have high ionic conductivity, they have low moldability and are brittle, making it difficult to build batteries using press alone. On the other hand, sulfide solid electrolytes have higher ionic conductivity than current organic electrolytes, and some of them are considered promising as solid electrolytes to replace electrolytes.
[0005] However, although sulfide solid electrolytes have high ionic conductivity and excellent moldability, they react with moisture in the air when exposed to the atmosphere to generate hydrogen sulfide. In contrast, when Sn is used as an electrolyte constituent element, it is less likely to react with moisture in the air (see, for example, Non-Patent Document 1). For example, Non-Patent Document 2 describes the synthesis of orthorhombic Li4SnS4 by heat treating Li2S, Sn, and S in a quartz ampoule. [Prior art documents] [Non-patent literature]
[0006] [Non-Patent Document 1] Energy Environ.Sci.,7(2014)1053. [Non-Patent Document 2] Chem.Mater.,24(2012)2211-2219. Summary of the Invention [Problem to be solved by the invention]
[0007] However, Li4SnS4 as described in Non-Patent Document 2 is difficult to synthesize in air, so it must be synthesized in an inert gas atmosphere. In addition, the amount of hydrogen sulfide generated cannot be sufficiently suppressed, and it has problems with moisture resistance.
[0008] The present invention has been made in consideration of the current state of the prior art described above, and a main object of the present invention is to provide a solid electrolyte that can be synthesized even in the air and has excellent ionic conductivity and moisture resistance. [Means for solving the problem]
[0009] The inventors of the present invention have conducted intensive research to achieve the above object. As a result, it has been found that a specific tin-containing lithium thiophosphate can be synthesized even in the atmosphere and is a solid electrolyte excellent in ionic conductivity and moisture resistance. The present invention has been completed through further research based on such findings. That is, the present invention includes the following configurations.
[0010] Item 1. General formula (1): Li x SnO y S z (1) [In the formula, x, y, and z satisfy 2.0 ≤ x ≤ 10.0; 1.0 < y ≤ 5.0; 0 < z ≤ 3.0.] A tin-containing lithium thiophosphate having a composition represented by
[0011] Item 2. The tin-containing lithium thiophosphate according to Item 1, having crystals.
[0012] Item 3. The tin-containing lithium thiophosphate according to Item 1 or 2, having a rock-salt type Li2SnO3 type crystal phase and a lithium sulfide (Li2S) crystal phase and / or an orthorhombic Li4SnS4 crystal phase.
[0013] Item 4. The tin-containing lithium thiophosphate according to any one of Items 1 to 3, having the strongest peak at a position of 42.0° within a range of diffraction angle 2θ = 10° to 70° in an X-ray diffraction pattern by CuKα rays with an allowable range of ±0.4°.
[0014] Item 5. The tin-containing lithium thiophosphate according to Item 4, having peaks at positions of at least one of 27.0°, 36.0°, and 61.0° within a range of diffraction angle 2θ = 10° to 70° in an X-ray diffraction pattern by CuKα rays with an allowable range of ±0.4°.
[0015] Item 6. The tin-containing lithium oxysulfide according to Item 4 or 5, which has a peak at a position of 36.0° within a diffraction angle 2θ range of 10° to 70° in an X-ray diffraction pattern using CuKα rays, within a tolerance of ±0.4°, and has a ratio of the peak intensity at 42.0° to the peak intensity at 36.0° (peak intensity at 42.0° / peak intensity at 36.0°) of 1.0 to 2.0.
[0016] Item 7. In Raman spectra, at least ±8 cm -1 With a wave number of 360 cm -1 Item 7. The tin-containing lithium oxysulfide according to any one of items 1 to 6, having a peak at the position:
[0017] Item 8. A method for producing a tin-containing lithium oxysulfide according to any one of items 1 to 7, A process of using a raw material containing lithium oxide and tin sulfide as a raw material and subjecting it to a mechanical milling process. A manufacturing method comprising:
[0018] Item 9. The method according to item 8, wherein the amount of the lithium oxide used is 1.5 to 5.0 moles per mole of the tin sulfide.
[0019] Item 10. The manufacturing method according to item 8 or 9, wherein the mechanical milling treatment is carried out in an inert gas atmosphere, at atmospheric pressure, or in a dry room.
[0020] Item 11. The method according to any one of Items 8 to 10, wherein after the mechanical milling treatment, a heat treatment or a pressure treatment is performed.
[0021] Item 12. A solid electrolyte for a lithium ion secondary battery, comprising the tin-containing lithium oxysulfide according to any one of items 1 to 7.
[0022] Item 13. A lithium ion secondary battery using the solid electrolyte for lithium ion secondary batteries according to item 12. Effect of the Invention
[0023] The tin-containing lithium oxysulfide of the present invention can be synthesized even in the air, and is a solid electrolyte having excellent ionic conductivity and moisture resistance. [Brief description of the drawings]
[0024] [Figure 1] 1 shows X-ray diffraction patterns of the powders obtained in Examples 1 to 3 and Comparative Example 1. [Diagram 2] 1 shows Raman spectra of the powders obtained in Example 3 and Comparative Example 1. [Diagram 3] 1 shows X-ray diffraction patterns of the powders obtained in Examples 3 to 5 and Comparative Examples 2 to 3. [Figure 4] 1 is a graph showing the measurement results of the amount of hydrogen sulfide gas generated in Test Example 6, using the powders obtained in Examples 4 and 5 and Comparative Example 2. For reference, the results for SnS2 are also shown. [Diagram 5] 1 is a graph showing the results of differential scanning calorimetry of the powder obtained in Example 3. [Figure 6] 1 shows X-ray diffraction patterns of the powders obtained in Examples 3 and 6 to 8. [Figure 7] 1 shows X-ray diffraction patterns of the powders obtained in Examples 8 to 10. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] In this specification, the term "containing" is a concept that encompasses all of "comprise," "consist essentially of," and "consist only of."
[0026] In this specification, when a numerical range is indicated as "A to B," it means A or more and B or less.
[0027] 1. Tin-containing lithium oxysulfide The tin-containing lithium oxysulfide of the present invention is General formula (1): Li x SnO y S z(1) [Wherein, x, y and z satisfy 2.0 ≦ x ≦ 10.0; 1.0 < y ≦ 5.0; 0 < z ≦ 3.0.] It has a composition represented by
[0028] The tin-containing lithium thiophosphate of the present invention is not particularly limited, but preferably has crystals from the viewpoints of being easily synthesized even in the atmosphere and being easily improved in ionic conductivity and moisture resistance.
[0029] When the tin-containing lithium thiophosphate of the present invention contains crystals, the crystallinity of the tin-containing lithium thiophosphate is evaluated by an X-ray diffraction pattern. In the present invention, the X-ray diffraction pattern is obtained by the powder X-ray diffraction measurement method, and the following measurement conditions: X-ray source: CuKα 40 kV - 40 mA Measurement conditions: 2θ = 10° to 70°, 0.1° step, scanning speed 5 seconds / step It is measured under
[0030] When the tin-containing lithium thiophosphate of the present invention contains crystals, it preferably has the strongest peak at the position of 42.0° within the range of diffraction angle 2θ = 10° to 70° in the X-ray diffraction pattern by CuKα line within an allowable range of ±0.4° (particularly ±0.3°). That is, the tin-containing lithium thiophosphate of the present invention preferably has the strongest peak in the range of 41.6° to 42.4° (particularly 41.7° to 42.3°) within the range of diffraction angle 2θ = 10° to 70° in the X-ray diffraction pattern by CuKα line. In the present invention, the strongest peak means the peak having the largest diffraction intensity among the peaks detected in the X-ray diffraction pattern by CuKα line. In the case of lithium tin sulfide not containing oxygen, it often has the strongest peak at the position of 25.5°, and does not have the strongest peak at the position of 42.0°. This also suggests that the tin-containing lithium thiophosphate of the present invention is different from lithium tin sulfide not containing oxygen.
[0031] When the tin-containing lithium oxysulfide of the present invention contains crystals, depending on the crystallinity, it can have a peak at least at one point (preferably all points) of 27.0°, 36.0°, and 61.0° within the range of diffraction angle 2θ=10° to 70° in the X-ray diffraction diagram by CuKα radiation, within the allowable range of ±0.4° (particularly ±0.3°). That is, the tin-containing lithium oxysulfide of the present invention can have a peak at least at one point (preferably all points) of 26.6° to 27.4° (particularly 26.7 to 27.3°), 35.6 to 36.4° (particularly 35.7 to 36.3°), and 60.6° to 61.4° (particularly 60.7 to 61.3°) within the range of diffraction angle 2θ=10° to 70° in the X-ray diffraction diagram by CuKα radiation. In addition, in the case of lithium tin sulfide that does not contain oxygen, there are often no peaks at the positions of 27.0°, 36.0°, and 61.0°. This also suggests that the tin-containing lithium oxysulfide of the present invention is different from lithium tin sulfide that does not contain oxygen.
[0032] When the tin-containing lithium oxysulfide of the present invention contains crystals, within the range of diffraction angles 2θ=10° to 70° in an X-ray diffraction diagram using CuKα rays, the ratio of the peak intensity at 42.0° to the peak intensity at 36.0° (peak intensity at 42.0° / peak intensity at 36.0°) is preferably 1.0 to 2.0, and more preferably 1.1 to 1.8.
[0033] The crystal structure of the tin-containing lithium oxysulfide of the present invention, when it contains crystals, can have a rock salt Li2SnO3 type crystal phase, a lithium sulfide (Li2S) crystal phase and / or a cubic Li4SnS4 crystal phase. The rock salt Li2SnO3 type crystal phase is not limited to rock salt Li2SnO3, but may also include a crystal structure similar to that of rock salt Li2SnO3 while also containing sulfur (S). In addition, in conventional electrolytes, when lithium sulfide is contained, hydrogen sulfide is easily generated and moisture resistance is easily reduced. However, even if the tin-containing lithium oxysulfide of the present invention contains a lithium sulfide (Li2S) crystal phase, hydrogen sulfide is unlikely to be generated and moisture resistance can be improved, which is an unexpected result, probably because it is coated with other materials such as oxides.
[0034] In addition, when the tin-containing lithium oxysulfide of the present invention has a rock salt type Li2SnO3 type crystal phase and a lithium sulfide (Li2S) crystal phase and / or a rhombic Li4SnS4 crystal phase, the content of the rock salt type Li2SnO3 type crystal phase is preferably 50 to 83 mol % (particularly 55 to 80 mol %), and the content of the lithium sulfide (Li2S) crystal phase and / or the rhombic Li4SnS4 crystal phase is preferably 0 to 50 mol % (particularly 0 to 33 mol %), with the total amount of the crystal phases being 100 mol %.
[0035] However, the tin-containing lithium oxysulfide of the present invention does not necessarily have to be composed of crystals alone, and may be a mixture of crystals and amorphous materials. When the tin-containing lithium oxysulfide of the present invention contains an amorphous material, the amorphous material that can be contained may be, for example, SnS2, SnS, Li2SnS3, Li4SnS4, S, Li2S, Li2SnOS2, Li2SnO2S2, Li2O, etc.
[0036] When the tin-containing lithium oxysulfide of the present invention is a mixture of crystalline and amorphous materials, the content of the crystalline phase is preferably 40 to 60 mol % (particularly 45 to 55 mol %) and the content of the amorphous material is preferably 40 to 60 mol % (particularly 45 to 55 mol %), with the total amount of the tin-containing lithium oxysulfide of the present invention being 100 mol %.
[0037] The tin-containing lithium thiophosphate of the present invention has, in the Raman spectrum, at least a tolerance range of ±8 cm -1 (particularly ±5 cm -1 ) and preferably has a peak at a wavenumber of 360 cm -1 . That is, the tin-containing lithium thiophosphate of the present invention preferably has a peak in the range of 352 to 368 cm -1 (particularly 355 to 365 cm -1 ) in the Raman spectrum. In the case of lithium tin sulfide without oxygen, it often has a peak at a wavenumber of 350 cm -1 and does not have a peak at a wavenumber of 360 cm -1 . This also suggests that the tin-containing lithium thiophosphate of the present invention is different from lithium tin sulfide without oxygen.
[0038] The tin-containing lithium thiophosphate of the present invention has the general formula (1): Li x SnO y S z (1) [wherein x, y and z satisfy 2.0 ≦ x ≦ 10.0; 1.0 < y ≦ 5.0; 0 < z ≦ 3.0.] It has a composition represented by
[0039] In the general formula (1), x means the amount of lithium in the tin-containing lithium thiophosphate of the present invention, and 3.0 ≦ x ≦ 10.0, preferably 3.2 ≦ x ≦ 7.0, more preferably 3.6 ≦ x ≦ 5.0. By setting x within this range, the tin-containing lithium thiophosphate of the present invention becomes stable, is easy to synthesize even at room temperature, and can improve ionic conductivity and moisture resistance. If x is less than 2.0, it has a crystal structure different from that of the tin-containing lithium thiophosphate of the present invention, and the ionic conductivity also decreases. Also, materials with x greater than 10.0 are difficult to synthesize.
[0040] In general formula (1), y represents the amount of oxygen in the tin-containing lithium oxysulfide of the present invention, where 1.0 < y ≤ 5.0, preferably 1.6 ≤ y ≤ 3.5, more preferably 1.8 ≤ y ≤ 2.5. By setting y within this range, the tin-containing lithium oxysulfide of the present invention becomes stable, is easy to synthesize even at room temperature, and can improve ionic conductivity and moisture resistance. When y is 1.0 or less, it has a crystal structure different from that of the tin-containing lithium oxysulfide of the present invention, and the ionic conductivity also decreases. Also, materials with y greater than 5.0 are difficult to synthesize.
[0041] In general formula (1), z represents the amount of sulfur in the tin-containing lithium oxysulfide of the present invention, where 0 < z ≤ 3.0, preferably 1.5 ≤ z ≤ 2.5, more preferably 1.8 ≤ z ≤ 2.2. By setting z within this range, the tin-containing lithium oxysulfide of the present invention becomes stable, is easy to synthesize even at room temperature, and can improve ionic conductivity and moisture resistance. When z is 0, since it does not contain sulfur, the ionic conductivity decreases. Also, materials with z greater than 3.0 are difficult to synthesize.
[0042] In general formula (1), the relationship between x, y, and z is not particularly limited. However, in the manufacturing method of the present invention described later, considering the use of lithium oxide (preferably Li2O) and tin sulfide (preferably SnS2), x is preferably about twice y. Therefore, 1.5y ≤ x ≤ 2.5y is preferred, 1.7y ≤ x ≤ 2.3y is more preferred, and 1.8y ≤ x ≤ 2.2y is even more preferred.
[0043] Also, the tin-containing lithium oxysulfide of the present invention has an ionic conductivity at room temperature of 1.0×10 -6 ~5.0×10 -4 Scm -1 (particularly 5.0×10 -6 ~5.0×10 -4 Scm -1 ) is preferably achieved, and the ionic conductivity at 60°C is 5.0×10 -6 ~2.0×10 -3 Scm -1 (particularly 2.0×10-5 ~2.0×10 -3 Scm -1 The ionic conductivity of the tin-containing lithium oxysulfide of the present invention is measured by an AC impedance method using a blocking electrode.
[0044] The tin-containing lithium oxysulfide of the present invention satisfies the above-mentioned conditions, but may contain other impurities as long as the performance of the tin-containing lithium oxysulfide is not impaired. Examples of such impurities include metals such as transition metals and typical metals that may be mixed into the raw materials; and carbon that may be mixed into the raw materials and during production. Furthermore, impurities may include residual materials from the raw materials (lithium oxide (Li2O), tin sulfide (SnS2), etc.) and products other than the target product of the present invention. The amount of these impurities may be within a range that does not impair the performance of the tin-containing lithium oxysulfide described above, and is usually preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 2% by mass or less, based on the total amount of the tin-containing lithium oxysulfide that satisfies the above-mentioned conditions as 100% by mass.
[0045] When these impurities are present, in addition to the peaks in the X-ray diffraction diagram described above, diffraction peaks may be present depending on the impurities.
[0046] 2. Manufacturing method of tin-containing lithium oxysulfide The tin-containing lithium oxysulfide of the present invention can be obtained by subjecting suitable raw materials to a mechanical milling treatment.
[0047] for example, A process of using a raw material containing lithium oxide and tin sulfide as a raw material and subjecting it to a mechanical milling process. The manufacturing method can be obtained by the method.
[0048] Mechanical milling, also known as mechanochemical processing, is a method of grinding and mixing raw materials while applying mechanical energy. According to this method, the raw materials are ground and mixed by applying mechanical impact and friction, so that lithium oxide and tin sulfide come into vigorous contact with each other and are finely divided, causing a reaction of the raw materials. In other words, mixing, grinding, and reaction occur simultaneously. Therefore, it is possible to more reliably react the raw materials without heating them to high temperatures. By using mechanical milling, a metastable crystal structure that cannot be obtained by normal heat treatment can be obtained.
[0049] Specifically, the mechanical milling treatment can involve mixed pulverization using a mechanical pulverizing device such as a ball mill, a bead mill, a rod mill, a vibration mill, a disk mill, a hammer mill, or a jet mill.
[0050] There is no particular limitation on the lithium oxide (preferably Li2O, etc.) used as a raw material, and commercially available lithium oxide can be used. In particular, it is preferable to use lithium oxide with high purity. In addition, since the lithium oxide is mixed and pulverized by mechanical milling, there is no limitation on the particle size of the lithium oxide used, and commercially available powdered lithium oxide can usually be used.
[0051] There is no particular limitation on the tin sulfide (preferably SnS, SnS2, etc.) used as a raw material, and any commercially available tin sulfide can be used. In particular, it is preferable to use a high-purity tin sulfide. In addition, since the tin sulfide is mixed and pulverized by mechanical milling, there is no particular limitation on the particle size of the tin sulfide used, and commercially available powdered tin sulfide can usually be used.
[0052] The mixing ratio of these raw materials can be adjusted so as to be the same as the desired composition of the tin-containing lithium oxysulfide.
[0053] Specifically, the amount of lithium sulfide used is preferably 1.5 to 5.0 mol, more preferably 1.6 to 3.5 mol, and even more preferably 1.8 to 2.5 mol, per mol of tin sulfide.
[0054] The atmosphere in which the mechanical milling process is carried out is not particularly limited, and may be in air, in an inert gas atmosphere (nitrogen gas atmosphere, argon gas atmosphere, etc.), or in a dry room.
[0055] In the present invention, the dry room means a system in which the dew point is −100 to −30° C., preferably −80 to −50° C. In the present invention, the atmospheric gas constituting the dry room is composed of dry air containing nitrogen, oxygen, argon, carbon dioxide, etc.
[0056] Among them, from the viewpoint of ion conductivity, an inert gas atmosphere or a dry room is preferable, and an inert gas atmosphere is more preferable. Also, from the viewpoint of reducing the amount of hydrogen sulfide generated and improving the hygroscopicity, an inert gas atmosphere or a dry room is preferable, and a dry room is more preferable. Note that while oxygen-free lithium tin sulfide cannot be synthesized in the air, the tin-containing lithium oxysulfide of the present invention can be synthesized in the air, and therefore, when synthesized in the air, it can be easily synthesized.
[0057] There are no particular limitations on the temperature at which mechanical milling is performed. However, from the viewpoint of preventing sulfur from volatilizing and preventing the previously reported crystal phase from being generated, it is preferable to perform mechanical milling at 100°C or less, preferably at 20 to 40°C.
[0058] The time for the mechanical milling treatment is not particularly limited, and the mechanical milling treatment can be performed for any time until the desired tin-containing lithium oxysulfide is precipitated.
[0059] For example, the mechanical milling process can be carried out at a rotation speed of about 200 to 600 rpm, for a processing time of about 0.1 to 200 hours, with an energy amount of about 0.1 to 100 kWh / 1 kg of raw material mixture. This mechanical milling process can also be carried out in multiple steps with breaks in between as necessary.
[0060] By the above-mentioned mechanical milling treatment, the target tin-containing lithium oxysulfide of the present invention can be obtained as a fine powder.
[0061] The thus obtained tin-containing lithium oxysulfide of the present invention may be further subjected to heat treatment or pressure treatment. When heat treatment is performed, it may be performed at, for example, 100 to 700 ° C. In addition, the tin-containing lithium oxysulfide of the present invention often has a rock salt type Li2SnO3 type crystal phase and a lithium sulfide (Li2S) crystal phase after the above mechanical milling treatment, but when heated at 280 ° C or higher, which is the crystallization peak temperature observed in the differential scanning calorimetry of the tin-containing lithium oxysulfide of the present invention, a rhombic Li4SnS4 crystal phase may also be generated, probably because the lithium sulfide (Li2S) crystal phase reacts with amorphous SnS2. When the heating temperature is further increased to 500 ° C or higher, the lithium sulfide (Li2S) crystal phase reacts, and the structure may include a crystal phase different from that before the heat treatment, such as a rock salt type Li2SnO3 type crystal phase, and a rhombic Li4SnS4 crystal phase. By such a heat treatment, it is possible to further improve the ionic conductivity of the tin-containing lithium oxysulfide of the present invention. In this regard, Li7La3Zr2O having a garnet structure, which is a conventionally known oxide solid electrolyte, 12 (LLZ) and Ta-doped Li 6.6 La3Zr 1.6 Ta 0.4 O 12 (LLZ-Ta), a rhombohedral Li crystal with a Nasicon structure 1.5 Al 0.5 Ge 1.5 This is an unexpected effect, considering that (PO4)3(LAGP) and amorphous LAGP have low ionic conductivity even after heat treatment.
[0062] On the other hand, when pressure treatment is performed, pressure can be applied at, for example, 100 to 600 MPa, preferably 300 to 550 MPa. When such pressure treatment is performed, even if heat treatment is not performed, it is also possible to further improve the ionic conductivity of the tin-containing lithium oxysulfide of the present invention. In this respect, it is an unexpected effect compared to the fact that the ionic conductivity is low even when pressure treatment is performed in the conventionally known electrolytes LLZ-Ta, rhombohedral crystal, and amorphous LAGP.
[0063] 3. Applications of tin-containing lithium oxysulfide The above-mentioned tin-containing lithium oxysulfide of the present invention can improve ionic conductivity, reduce the amount of hydrogen sulfide generated, and improve moisture resistance as described above. Therefore, the tin-containing lithium oxysulfide of the present invention is useful as an ion conductor (particularly, a solid electrolyte), and is particularly preferably used as a solid electrolyte for lithium ion secondary batteries.
[0064] When the tin-containing lithium oxysulfide of the present invention is used as a solid electrolyte for a lithium ion secondary battery, the structure of the lithium ion secondary battery of the present invention (particularly, an all-solid-state lithium ion secondary battery) can be the same as that of a known lithium ion secondary battery, except that the tin-containing lithium oxysulfide of the present invention is used as a solid electrolyte.
[0065] For example, known positive electrode active materials such as lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMn2O4), lithium iron phosphate (LiFePO4), vanadium oxide-based materials, and sulfur-based materials can be used as the positive electrode, and a positive electrode mixture containing this positive electrode active material, the tin-containing lithium oxysulfide of the present invention, and a conductive agent and a binder as necessary can be supported on a positive electrode current collector such as Al, Ni, stainless steel, or carbon cloth. As the conductive agent, for example, carbon materials such as graphite, coke, carbon black, and acicular carbon can be used. In addition, as the binder, for example, materials such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyimide (PI), polyamide, polyamideimide, polyacrylic, styrene butadiene rubber (SBR), styrene-ethylene-butylene-styrene copolymer (SEBS), and carboxymethyl cellulose (CMC) can be used alone or in combination of two or more. Incidentally, as the electrolyte, a conventionally used electrolyte may also be used in combination.
[0066] As the negative electrode, known negative electrode active materials such as metallic lithium, carbon-based materials (activated carbon, graphite, etc.), silicon, silicon oxide, Si-SiO-based materials, and lithium titanium oxide are used, and a positive electrode mixture containing this negative electrode active material, the tin-containing lithium oxysulfide of the present invention, and a conductive agent and a binder as necessary can be supported on a negative electrode current collector such as Al, Ni, stainless steel, or carbon cloth. As the conductive agent, for example, carbon materials such as graphite, coke, carbon black, and acicular carbon can be used. As the binder, for example, materials such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyimide (PI), polyamide, polyamideimide, polyacrylic, styrene butadiene rubber (SBR), styrene-ethylene-butylene-styrene copolymer (SEBS), and carboxymethylcellulose (CMC) can be used alone or in combination of two or more. As the electrolyte, a conventionally used electrolyte can also be used in combination.
[0067] In addition, the tin-containing lithium oxysulfide of the present invention can be formed into a layer by a conventional method using a known binder as necessary, and used as the electrolyte layer. As the binder, for example, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyimide (PI), polyamide, polyamideimide, polyacrylic, styrene butadiene rubber (SBR), styrene-ethylene-butylene-styrene copolymer (SEBS), carboxymethyl cellulose (CMC), and other materials can be used alone or in combination of two or more. In addition, as the electrolyte layer, it is also possible to use a combination of electrolyte layers that have been used conventionally.
[0068] The separator may be made of a material such as a polyolefin resin, such as polyethylene or polypropylene, a fluororesin, nylon, aromatic aramid, or inorganic glass, and may be in the form of a porous film, a nonwoven fabric, or a woven fabric.
[0069] Furthermore, a lithium ion secondary battery can be assembled in a conventional manner using other known battery components. In the present invention, the term "lithium ion secondary battery" is a concept that also includes a "lithium secondary battery" that uses metallic lithium as the negative electrode material.
[0070] The shape of the lithium ion secondary battery is not particularly limited, and may be any of cylindrical, rectangular, and the like. EXAMPLES
[0071] The present invention will be described in more detail below with reference to examples. However, it goes without saying that the present invention is not limited to the following examples.
[0072] In addition, although the mechanical milling time may differ between the examples and comparative examples, this is because the mechanical milling was performed until all of the raw material powder reacted, and the difference in the mechanical milling time is not a substantial difference.
[0073] [Example 1: Synthesis of Li8SnO4S2 powder in argon atmosphere] In a glove box with an argon atmosphere (not exposed to air), commercially available lithium oxide (Li2O) powder and tin sulfide (SnS2) powder were weighed and mixed in a molar ratio of 80:20, respectively, and then mechanical milling was performed for 40 hours at 370 rpm in a ball mill (Fritsch P-7, Classic Line) using a 45 mL zirconia container containing 65 g (about 160 pieces) of zirconia balls with a diameter of 5 mm to obtain Li8SnO4S2 powder. The mechanical milling was performed in an overpot for controlling the atmosphere. For convenience, the obtained powder of Li8SnO4S2 composition is referred to as Li8SnO4S2 powder (before heat treatment).
[0074] [Example 2: Synthesis of Li6SnO3S2 powder in argon atmosphere] In a glove box with an argon atmosphere (not exposed to air), commercially available lithium oxide (Li2O) powder and tin sulfide (SnS2) powder were weighed and mixed in a molar ratio of 75:25, respectively, and then mechanical milling was performed for 60 hours at 370 rpm in a ball mill (Fritsch P-7, Classic Line) using a 45 mL zirconia container containing 65 g (about 160 pieces) of zirconia balls with a diameter of 5 mm to obtain Li6SnO3S2 powder. The mechanical milling was performed in an overpot for controlling the atmosphere. For convenience, the obtained powder of Li6SnO3S2 composition is referred to as Li6SnO3S2 powder (before heat treatment).
[0075] [Example 3: Synthesis of Li4SnO2S2 powder in argon atmosphere] In a glove box with an argon atmosphere (not exposed to air), commercially available lithium oxide (Li2O) powder and tin sulfide (SnS2) powder were weighed and mixed in a molar ratio of 67:33, respectively, and then mechanical milling was performed for 80 hours at 510 rpm in a ball mill (Fritsch P-7, Classic Line) using a 45 mL zirconia container containing 90 g (about 500 pieces) of zirconia balls with a diameter of 4 mm to obtain Li4SnO2S2 powder. The mechanical milling was performed in an overpot for controlling the atmosphere. For convenience, the obtained powder of Li4SnO2S2 composition is referred to as Li4SnO2S2 powder (before heat treatment).
[0076] [Example 4: Synthesis of Li4SnO2S2 powder in air] In a glove box with an argon atmosphere (not exposed to air), commercially available lithium oxide (Li2O) powder and tin sulfide (SnS2) powder were weighed and mixed in a molar ratio of 67:33, respectively. Then, the powder was placed in a 45 mL zirconia container containing 90 g (about 500 pieces) of zirconia balls with a diameter of 4 mm, the lid was closed, and the container was removed from the glove box. After leaving the container in the air with the lid open for 15 minutes, the lid was closed in the air atmosphere, and mechanical milling treatment was performed at 510 rpm for 40 hours in a ball mill device (Fritsch P-7, Classic Line) to obtain Li4SnO2S2 powder. The mechanical milling treatment was performed in an overpot for controlling the atmosphere. For convenience, the obtained powder of Li4SnO2S2 composition is referred to as Li4SnO2S2 powder (synthesized in the air atmosphere, before heat treatment).
[0077] [Example 5: Synthesis of Li4SnO2S2 powder in a dry room atmosphere] In a glove box with an argon atmosphere (not exposed to air), commercially available lithium oxide (Li2O) powder and tin sulfide (SnS2) powder were weighed and mixed in a molar ratio of 67:33, respectively. Then, the powder was placed in a 45 mL zirconia container containing 90 g (about 500 pieces) of zirconia balls with a diameter of 4 mm, the lid was closed, and the container was removed from the glove box. After leaving the container for 15 minutes with the lid open in a dry room with a dew point of about -70°C, the lid was closed in a dry room atmosphere, and mechanical milling was performed at 510 rpm for 40 hours in a ball mill device (Fritsch P-7, Classic Line) to obtain Li4SnO2S2 powder. The mechanical milling was performed in an overpot for controlling the atmosphere. For convenience, the obtained powder of Li4SnO2S2 composition is referred to as Li4SnO2S2 powder (synthesized in a dry room atmosphere, before heat treatment). The constituent gas of the dry room is dry air containing nitrogen, oxygen, argon and carbon dioxide.
[0078] [Example 6: Synthesis of Li4SnO2S2 powder (argon atmosphere) after heat treatment at 250 °C] The Li4SnO2S2 powder obtained in Example 3 was heated from room temperature to 250°C at 2°C / min, heat-treated at 250°C for 2 hours, and then allowed to cool, yielding Li4SnO2S2 powder after heat treatment at 250°C.
[0079] [Example 7: Synthesis of Li4SnO2S2 powder (argon atmosphere) after 320°C heat treatment] The Li4SnO2S2 powder obtained in Example 3 was heated from room temperature to 320°C at 2°C / min, heat-treated at 320°C for 2 hours, and then allowed to cool, yielding Li4SnO2S2 powder after heat treatment at 320°C.
[0080] [Example 8: Synthesis of Li4SnO2S2 powder (argon atmosphere) after heat treatment at 500 °C] The Li4SnO2S2 powder obtained in Example 3 was heated from room temperature to 500°C at 2°C / min, heat-treated at 500°C for 2 hours, and then allowed to cool, yielding Li4SnO2S2 powder after heat treatment at 500°C.
[0081] [Example 9: Synthesis of Li4SnO2S2 powder (air atmosphere) after heat treatment at 500 °C] The Li4SnO2S2 powder obtained in Example 4 was heated from room temperature to 500°C at 2°C / min, heat-treated at 500°C for 2 hours, and then allowed to cool, yielding Li4SnO2S2 powder after heat treatment at 500°C.
[0082] [Example 10: Synthesis of Li4SnO2S2 powder (dry room atmosphere) after heat treatment at 500 °C] The Li4SnO2S2 powder obtained in Example 5 was heated from room temperature to 500°C at 2°C / min, heat-treated at 500°C for 2 hours, and then allowed to cool, yielding Li4SnO2S2 powder after heat treatment at 500°C.
[0083] [Comparative Example 1: Synthesis of Li2SnOS2 powder] In a glove box with an argon atmosphere (not exposed to air), commercially available lithium oxide (Li2O) powder and tin sulfide (SnS2) powder were weighed and mixed in a molar ratio of 50:50, and then mechanical milling was performed for 40 hours at 510 rpm in a ball mill (Fritsch P-7, Classic Line) using a 45 mL zirconia container containing 90 g (about 500 balls) of 4 mm diameter zirconia balls to obtain Li2SnOS2 powder. The mechanical milling was performed in an overpot for controlling the atmosphere. For convenience, the obtained powder of Li2SnOS2 composition is referred to as Li2SnOS2 powder (before heat treatment).
[0084] [Comparative Example 2: Synthesis of Li4SnS4 powder in an argon atmosphere] In a glove box with an argon atmosphere (not exposed to air), commercially available lithium sulfide (Li2S) powder and tin sulfide (SnS2) powder were weighed and mixed in a molar ratio of 67:33, respectively, and then mechanical milling was performed for 10 hours at 510 rpm in a ball mill (Fritsch P-7, Classic Line) using a 45 mL zirconia container containing 90 g (about 500 balls) of 4 mm diameter zirconia balls to obtain Li4SnS4 powder. The mechanical milling was performed in an overpot for controlling the atmosphere. For convenience, the obtained powder of Li4SnS4 composition is referred to as Li4SnS4 powder (before heat treatment).
[0085] [Comparative Example 3: Synthesis of Li4SnS4 powder in air] In a glove box in an argon atmosphere (not exposed to air), commercially available lithium sulfide (Li2S) powder and tin sulfide (SnS2) powder were weighed and mixed in a molar ratio of 67:33, respectively, and then the powder was placed in a 45 mL zirconia container containing 90 g (about 500 pieces) of zirconia balls with a diameter of 4 mm, the lid was closed, and the container was removed from the glove box. After leaving the container in the air with the lid open for 15 minutes, the lid was closed in the air atmosphere, and mechanical milling treatment was performed at 510 rpm for 10 hours in a ball mill device (Fritsch P-7, Classic Line) to obtain the powder of Comparative Example 3. The mechanical milling treatment was performed in an atmosphere-controlling overpot.
[0086] [Comparative Example 4: LLZ-Ta (cold-pressed body)] Commercially available Li 6.6 La3Zr 1.6 Ta 0.4 O 12 150 mg of (LLZ-Ta) was homogeneously packed into a molding machine with a diameter of 10 mm and uniaxially molded at 540 MPa for 5 minutes to produce pellets with a thickness of 0.5 to 0.8 mm and a diameter of 10 mm.
[0087] [Comparative Example 5: LLZ-Ta (500°C sintered body)] Commercially available Li 6.6 La3Zr 1.6 Ta0.4 O 12 200 mg of (LLZ-Ta) was homogeneously packed into a 10 mm diameter molding machine and uniaxially molded at 540 MPa for 5 minutes to produce pellets with a thickness of 0.8 to 0.9 mm and a diameter of 10 mm. The pellets obtained were heated from room temperature to 500°C at 2°C / min, heat-treated at 500°C for 2 hours, and then allowed to cool to obtain sintered pellets.
[0088] [Comparative Example 6: Amorphous LAGP (cold-pressed body)] Commercially available Li 1.5 Al 0.5 Ge 1.5 120 mg of (PO4)3 (amorphous LAGP) was homogeneously packed into a 10 mm diameter molding machine and uniaxially molded at 540 MPa for 5 minutes to produce pellets with a thickness of 0.5 to 0.8 mm and a diameter of 10 mm.
[0089] [Comparative Example 7: Amorphous LAGP (sintered at 500°C)] Commercially available Li 1.5 Al 0.5 Ge 1.5 120 mg of (PO4)3 (amorphous LAGP) was homogeneously filled into a 10 mm diameter molding machine and uniaxially molded at 540 MPa for 5 minutes to produce pellets with a thickness of 0.8-0.9 mm and a diameter of 10 mm. The pellets obtained were heated from room temperature to 500°C at 2°C / min, heat-treated at 500°C for 2 hours, and then allowed to cool to obtain sintered pellets. It was also confirmed by X-ray diffraction that amorphous LAGP did not crystallize even when heat-treated at 500°C.
[0090] [Comparative Example 8: Rhombohedral LAGP (cold-pressed body)] Commercially available Li 1.5 Al 0.5 Ge 1.5 200 mg of (PO4)3 (rhombohedral LAGP) was homogeneously packed in a 10 mm diameter molding machine and uniaxially molded at 540 MPa for 5 minutes to produce pellets with a thickness of 0.8 to 1.0 mm and a diameter of 10 mm. It was difficult to produce a sintered body from this pellet even when it was heat-treated at 500°C.
[0091] [Test Example 1: X-ray diffraction (part 1)] X-ray diffraction (XRD) using CuKα radiation was measured for the powders obtained in Examples 1 to 3 and Comparative Example 1. The results are shown in Figure 1. In the XRD measurement, a polymeric air-protected folder was used to prevent the prepared samples from being exposed to the air.
[0092] In the X-ray diffraction diagram shown in FIG. 1, all of Examples 1 to 3 have the strongest peak at 2θ=42.0°, and also have peaks at 27.0°, 36.0°, and 61.0°. In addition, the ratio of the peak intensity at 2θ=42.0° to the peak intensity at 36.0° (peak intensity at 42.0° / peak intensity at 36.0°) was 1.2 in Example 1, 1.4 in Example 2, and 1.4 in Example 3. On the other hand, in Comparative Example 1, the strongest peak was at 2θ=34.2°, and also had peaks at 30.2°, 36.0°, 42.0°, 49.2°, and 61.0°, and no peak was at 27.0°. In addition, the ratio of the peak intensity at 2θ=42.0° to the peak intensity at 36.0° (peak intensity at 42.0° / peak intensity at 36.0°) was as small as 1.1 in Comparative Example 1.
[0093] From the above, it can be seen that in Examples 1 to 3, a new crystal phase similar to rock-salt Li2SnO3 having the strongest peak at 2θ=42.0° was obtained, whereas in Comparative Example 1, a crystal phase derived from a cubic crystal was also mixed in. In addition, from the X-ray diffraction patterns, it is assumed that the powders of Examples 1 to 3 have a lithium sulfide (Li2S) crystal phase and a rock-salt Li2SnO3 type crystal phase, but from the composition, it is assumed that the rock-salt Li2SnO3 type crystal phase contains sulfur, and that it also contains an amorphous phase containing sulfur (S, SnS2, etc.) in addition to the rock-salt Li2SnO3 type crystal phase.
[0094] In addition, for the powder of Example 3, the Rietveld analysis revealed that the content of the Li2S phase in the crystal phase was about 33 mol %, and the content of the Li2SnO3 phase was 67 mol %.
[0095] As a result of X-ray diffraction measurement (Rietveld analysis), the powder of Comparative Example 3 was found to contain Li4SnS4·4H2O.
[0096] [Test Example 2: Measurement of ionic conductivity of solid electrolyte pellets (part 1)] 100 mg of the powders obtained in Examples 1 to 3 and Comparative Example 1 were uniformly filled into a molding machine with a diameter of 10 mm, and uniaxially molded at 540 MPa for 5 minutes to produce pellets with a thickness of 0.5 to 0.8 mm and a diameter of 10 mm. The resistance of these pellets at 25°C (room temperature) and 60°C was measured by an AC impedance method, and the ionic conductivity σ at 25°C (room temperature) and 60°C was calculated from the resistance. The results are shown in Table 1.
[0097] [Table 1]
[0098] As a result, it is assumed that in Examples 1 to 3, the ionic conductivity is high due to the presence of a lithium sulfide (Li2S) crystal phase and a rock salt Li2SnO3 type crystal phase. It is assumed that in Examples 1 to 3, the smaller the amount of Li2O added, that is, the smaller the amount of oxygen, the higher the ionic conductivity. On the other hand, in Comparative Example 1, although the amount of oxygen is the smallest, that is, the ionic conductivity should be the highest, the ionic conductivity was lower than that of Example 3, probably because of the presence of a cubic crystal.
[0099] [Test Example 3: Raman Spectroscopic Analysis] The powders obtained in Example 3 and Comparative Example 2 were subjected to Raman spectroscopy analysis. The Raman spectroscopy analysis was performed under the following measurement conditions: Laser wavelength: 532nm Exposure time: 10 seconds Number of times: 4 The results are shown in FIG. 2. As a result, in the powders of Examples 1 to 3, like Li4SnS4, SnS4 4- A Raman band that can be attributed to the unit was observed. Therefore, it is presumed that the powders of Examples 1 to 3 contain SnS4 tetrahedrons.
[0100] [Test Example 4: X-ray diffraction (part 2)] X-ray diffraction (XRD) using CuKα radiation was measured for the powders obtained in Examples 3 to 5 and Comparative Examples 2 to 3. The results are shown in Figure 3. In the XRD measurement, a polymeric air-protected folder was used to prevent the prepared samples from being exposed to the air.
[0101] In the X-ray diffraction diagram shown in Fig. 3, in all of Examples 4 and 5, the strongest peak was at 2θ = 42.0°, and peaks were also present at 27.0°, 36.0°, and 61.0°. The ratio of the peak intensity at 2θ = 42.0° to the peak intensity at 36.0° (peak intensity at 42.0° / peak intensity at 36.0°) was 1.4 in Example 4 and 1.5 in Example 5. On the other hand, in Comparative Example 2, the strongest peak was at 2θ = 25.5°, and peaks were also present at 27.8°, 38.2°, 45.0°, 50.0°, and 54.0°, and no peaks were present at 27.0°, 36.0°, 42.0°, and 61.0°. In addition, in Comparative Example 3, the strongest peak was at 2θ=26.0°, and also had peaks at 15.0°, 24.0°, 28.2°, 30.0°, 31.8°, 34.0°, 37.0°, 39.4°, 39.8°, 45.8°, and 50.8°, but no peaks were present at 27.0°, 36.0°, 42.0°, or 61.0°.
[0102] From the above, it can be seen that in Examples 4 to 5, as in Examples 1 to 3, a new crystal phase similar to that of rock salt type Li2SnO3 having the strongest peak at 2θ=42.0° is obtained, and that a similar crystal phase can be obtained not only in an inert gas atmosphere but also in the air and in a dry room. In addition, from the X-ray diffraction diagram, it is assumed that the powders of Examples 4 to 5 have a lithium sulfide (Li2S) crystal phase and a rock salt type Li2SnO3 type crystal phase, but from the composition, it is assumed that the rock salt type Li2SnO3 type crystal phase contains sulfur, and that it also contains an amorphous phase containing sulfur (S, SnS2, etc.) in addition to the rock salt type Li2SnO3 type crystal phase. In addition, for the powders of Examples 4 to 5, the Rietveld analysis showed that the content of the Li2S phase in the crystal phase was about 33 mol % and the content of the Li2SnO3 phase was 67 mol %. In contrast, in Comparative Examples 2 and 3, especially Comparative Example 3, hydrates such as Li4SnS4·4H2O were formed, suggesting that synthesis in the atmosphere is not possible.
[0103] [Test Example 5: Measurement of ionic conductivity of solid electrolyte pellets (part 2)] 100 mg of the powders obtained in Examples 3 to 5 and Comparative Example 3 were uniformly packed into a molding machine with a diameter of 10 mm, and uniaxially molded at 540 MPa for 5 minutes to produce pellets with a thickness of 0.5 to 0.8 mm and a diameter of 10 mm. The resistance of these pellets at 25°C (room temperature) and 60°C was measured by an AC impedance method, and the ionic conductivity σ at 25°C (room temperature) and 60°C was calculated from the resistance. The results are shown in Table 2. It can be seen that the powder of Comparative Example 3 has a lower ionic conductivity than Examples 3 to 5 because it contains Li4SnS4·4H2O, which has low ionic conductivity.
[0104] [Table 2]
[0105] [Test Example 6: Measurement of hydrogen sulfide gas generation amount] Approximately 2000cm at 50% RH and 25°C (room temperature) 3 50 mg of electrolyte powder was sealed in a container and the amount of hydrogen sulfide (H2S) generated was measured.
[0106] As the electrolyte powder, the powders obtained in Examples 3 and 5 and Comparative Example 2, and SnS2 used as the raw material were used.
[0107] The electrolyte powder was placed in a screw tube No. 4 and double-sealed in a laminated zipper bag to prevent reaction before the start of the measurement.
[0108] Next, a small electric fan, a temperature and humidity logger, a hydrogen sulfide detector, and the electrolyte powder sealed in a laminated zip-lock bag were placed in the glove box, and the box was left to stand until the humidity reached 50% RH.
[0109] Next, the electrolyte powder was removed from the laminated zipper bag and placed in a sealed container (volume approximately 2000 cm 3 ) was closed.
[0110] The temperature, humidity and hydrogen sulfide concentration were measured (automatically) every minute. The measurement was completed after one hour. The results are shown in FIG. 4. As a result, it can be understood that the SnS2 used as the raw material does not generate hydrogen sulfide, but the Li4SnS4 powder of Comparative Example 2 generates hydrogen sulfide. In contrast, it can be understood that the Li4SnO2S2 powder of Examples 3 and 5 can reduce the amount of hydrogen sulfide generated, and Example 5 hardly generates any hydrogen sulfide. In the present invention, although it has a lithium sulfide crystal phase, it is unexpected that the amount of hydrogen sulfide generated can be reduced, possibly because it is coated with other materials such as oxides.
[0111] [Test Example 7: Differential Scanning Calorimetry] Differential scanning calorimetry was performed on the powder obtained in Example 3. The differential scanning calorimetry was performed under the following measurement conditions: Measurement temperature range: Room temperature to 500℃ Heating rate: 10℃ / min The results are shown in Figure 5. As a result, a crystallization peak was detected at about 280°C.
[0112] [Test Example 8: X-ray diffraction (part 3)] X-ray diffraction (XRD) using CuKα radiation was measured for the powders obtained in Examples 3 and 6 to 10. The results are shown in Figures 6 to 7. In the XRD measurement, a polymeric air-protected folder was used to prevent the prepared samples from being exposed to the air.
[0113] In the X-ray diffraction patterns shown in Figures 6 to 7, all of Examples 6 to 8 have the strongest peak at 2θ = 42.0 °, and also have peaks at 27.0 °, 36.0 °, and 61.0 °. In addition, the ratio of the peak intensity at 2θ = 42.0 ° to the peak intensity at 36.0 ° (peak intensity at 42.0 ° / peak intensity at 36.0 °) was 1.4 in Example 6, 1.4 in Example 7, 1.5 in Example 8, 1.7 in Example 9, and 1.7 in Example 10. In addition, in Examples 7 to 10, which were heated at a temperature higher than 280 ° C, which is the crystallization peak temperature, a peak derived from the orthorhombic Li4SnS4 was also detected, probably due to the reaction between lithium sulfide (Li2S) and the amorphous phase (SnS2).
[0114] [Test Example 9: Measurement of ionic conductivity of solid electrolyte pellets (part 3)] 100 mg of the powder obtained in Examples 3 and 6 to 10 was uniformly filled in a molding machine with a diameter of 10 mm, and uniaxially molded at 540 MPa for 5 minutes to prepare pellets with a thickness of 0.5 to 0.8 mm and a diameter of 10 mm. These were heat-treated at each temperature to obtain the sintered pellets of Examples 6 to 10. The pellets in Example 3 were not heat-treated, and were cold-pressed. The resistance of the pellets at 25°C (room temperature) and 60°C was measured by an AC impedance method, and the ionic conductivity σ at 25°C (room temperature) and 60°C was calculated from the resistance. The results are shown in Table 3. As a result, it can be understood that the cold-pressed or sintered compacts of the tin-containing lithium oxysulfide in the Examples can remarkably improve the ionic conductivity, even when compared with the cold-pressed or sintered compacts of commercially available products.
[0115] [Table 3] [Industrial Applicability]
[0116] The tin-containing lithium oxysulfide of the present invention can be synthesized even in the air, and is a solid electrolyte having excellent ionic conductivity and moisture resistance.
[0117] Therefore, the tin-containing lithium oxysulfide of the present invention is suitable for use in solid electrolyte layers, which must have high conductivity and in which a relatively large amount of electrolyte is used, and can be suitably used as a solid electrolyte in batteries for electric vehicles or plug-in hybrid vehicles, stationary storage batteries, and the like.
Claims
1. General formula (1): Li x Snッ y S z (1) [In the formula, x, y, and z satisfy the following: 2.0≦x≦10.0; 1.0<y≦5.0; 0<z≦3.0.] Tin-containing lithium oxysulfide having a composition represented by the formula:
2. The tin-containing lithium oxysulfide according to claim 1 , which has crystallinity.
3. Rock salt Li 2 SnO 3 The crystalline phase and lithium sulfide (Li 2 S) crystalline phase and / or cuboidal Li 4 SnS 4 The tin-containing lithium oxysulfide according to claim 2, having a crystalline phase.
4. The tin-containing lithium oxysulfide according to claim 2, having the strongest peak at 42.0° within a range of diffraction angles 2θ = 10 ° to 70 ° in an X-ray diffraction diagram using CuKα rays, with a tolerance of ± 0.4 °.
5. The tin-containing lithium oxysulfide according to claim 4, wherein the X-ray diffraction pattern by CuKα ray has a diffraction angle 2θ of 10° to 70° within a tolerance of ±0.4°, and further has a peak at at least one position of 27.0°, 36.0°, and 61.0°.
6. The tin-containing lithium oxysulfide according to claim 5, which has a peak at 36.0° within a diffraction angle 2θ=10° to 70° in an X-ray diffraction diagram using CuKα rays, with a tolerance of ±0.4°, and has a ratio of the peak intensity at 42.0° to the peak intensity at 36.0° (peak intensity at 42.0° / peak intensity at 36.0°) of 1.0 to 2.
0.
7. In the Raman spectrum, at least ±8 cm -1 Within the allowable range, the wave number is 360 cm -1 The tin-containing lithium oxysulfide according to claim 1, having a peak at the position
8. A method for producing the tin-containing lithium oxysulfide according to any one of claims 1 to 7, A process of using a raw material containing lithium oxide and tin sulfide as a raw material and subjecting it to a mechanical milling process. A manufacturing method comprising:
9. The method according to claim 8, wherein the amount of the lithium oxide used is 1.5 to 5.0 moles per mole of the tin sulfide.
10. The method according to claim 8 , wherein the mechanical milling is carried out in an inert gas atmosphere, at atmospheric pressure, or in a dry room.
11. The method according to claim 8 , further comprising the step of subjecting the material to a heat treatment or a pressure treatment after the mechanical milling treatment.
12. A solid electrolyte for a lithium ion secondary battery, comprising the tin-containing lithium oxysulfide according to any one of claims 1 to 7.
13. A lithium ion secondary battery using the solid electrolyte for lithium ion secondary batteries according to claim 12.
Citation Information
Patent Citations
Electrode protection using an electrolyte-inhibiting ion conductor
JP2017506419A
Electrode protection using electrolyte-suppressed ionic conductors
JP2017506420A
Solid electrolyte for all-solid lithium ion battery and all-solid lithium ion battery
JP2020061260A
Method for producing modified sulfide solid electrolyte
JP2020087794A
Cited By
Materials
GB2702353A
Solid-state battery
WO2026070206A1