Method for manufacturing electrostatic charge image development toner
The aggregation and fusion of amorphous and crystalline polyester resins in an aqueous medium address the issues of low-temperature fixability and fogging in toners, enhancing thermal responsiveness and image stability.
Patent Information
- Application Number
- JP2023057032
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Conventional toners for electrophotography face issues with low-temperature fixability at high speeds and are prone to fogging due to wide charge distribution and surface exposure of crystalline polyester, which affects image quality.
A method involving the aggregation and fusion of resin particles containing an amorphous polyester resin and a crystalline polyester resin in an aqueous medium, where the amorphous resin with higher hydrophilicity is on the surface, enhancing thermal responsiveness and reducing fogging.
The method achieves excellent low-temperature fixability at high speeds while suppressing fogging, ensuring stable image quality by optimizing resin composition and distribution.
Smart Images

Figure 2024144873000001 
Figure 2024144873000002 
Figure 2024144873000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a toner for developing electrostatic images used in developing latent images formed in electrophotography, electrostatic recording, electrostatic printing and the like. [Background technology]
[0002] In the field of electrophotography, with the development of electrophotographic systems, there is a demand for the development of electrophotographic toners that can handle higher speeds and higher image quality. To handle higher speeds, toners need to have rapid thermal response, and it has been found that conventional toners have insufficient low-temperature fixing properties. Furthermore, as speeds increase, the time it takes for toner to be transferred to paper also becomes shorter, so toners with excellent charging properties are needed.
[0003] Patent Document 1 describes a pulverized toner produced by a melt kneading method, which contains an amorphous polyester A, which is a polycondensate of an alcohol component containing an aliphatic diol having a hydroxyl group bonded to a secondary carbon atom having 3 to 5 carbon atoms, and a carboxylic acid component containing an aromatic dicarboxylic acid compound, and a crystalline polyester C, which is a polycondensate of an alcohol component containing an aliphatic diol, and a carboxylic acid component containing an aliphatic dicarboxylic acid compound, in which the glass transition temperature of the amorphous polyester A is in a specific range, and the solubility parameter of the amorphous polyester A and the solubility parameter and crystallization temperature of the crystalline polyester C satisfy a specific relationship, and the toner is described as having excellent low-temperature fixing properties, heat-resistant storage stability, and suppression of blurring. Patent Document 2 describes an electrophotographic toner having toner particles containing a crystalline polyester (a), an amorphous polyester (b), and a release agent, in which the crystalline polyester (a) is obtained by polycondensation of an alcohol component containing an α,ω-alkanediol having 10 to 12 carbon atoms and an average carbon number of 10 to 12 and an acid component containing succinic acid, and has a weight average molecular weight of 2.5×10 4 Above 9.0×10 4The document describes an electrophotographic toner which is a crystalline polyester as described below, and describes that the toner for developing electrostatic images has both good low-temperature fixing properties and heat-resistant storage stability, and is also excellent in suppressing toner scattering and in dot reproducibility. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-59964 A [Patent Document 2] JP 2014-130291 A Summary of the Invention [Problem to be solved by the invention]
[0005] Although the toner described in Patent Document 1 has the above-mentioned effects, since it is a pulverized toner produced by a melt-kneading method, the crystalline polyester is exposed on the surface, and therefore the charge distribution is wide and fogging is likely to occur. Also, the toner described in Patent Document 2 has room for improvement in low-temperature fixability at high speeds. The present invention relates to a method for producing a toner for developing electrostatic images, which has excellent low-temperature fixing property even at high speed and suppresses the occurrence of fogging. [Means for solving the problem]
[0006] The present inventors have found that a toner for developing electrostatic images produced by a method including a step of aggregating and fusing, in an aqueous medium, resin particles containing, in the same or different particles, an amorphous resin containing an amorphous polyester resin (A) which is a polycondensate of an alcohol component (a) containing a specific diol and a carboxylic acid component (b), and a crystalline resin containing a crystalline polyester resin (C) which is a polycondensate of an alcohol component (c) containing a specific diol and a carboxylic acid component (d) containing a specific dicarboxylic acid, has excellent low-temperature fixing ability even at high speeds and suppresses the occurrence of fogging. The present invention relates to the following [1]. [1] A method for producing a toner for developing an electrostatic image, comprising a step of aggregating and fusing resin particles, the resin particles including an amorphous resin and a crystalline resin in the same or different particles, in an aqueous medium, the method comprising the steps of: the amorphous resin contains an amorphous polyester resin (A) which is a polycondensate of an alcohol component (a) containing an aliphatic diol having from 2 to 5 carbon atoms and a carboxylic acid component (b); The crystalline resin contains a crystalline polyester resin (C) which is a polycondensate of an alcohol component (c) containing a diol having 8 to 14 carbon atoms and a carboxylic acid component (d) containing a dicarboxylic acid having 4 carbon atoms. A method for producing a toner for developing electrostatic images. Effect of the Invention
[0007] According to the present invention, there is provided a method for producing a toner for developing electrostatic images, which has excellent low-temperature fixing properties even at high speeds and suppresses the occurrence of fogging. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] [Method of manufacturing toner for developing electrostatic images] The method for producing the toner for developing electrostatic images (hereinafter also simply referred to as "toner") of the present invention includes a step of aggregating and a step of fusing resin particles, the resin particles containing an amorphous resin and a crystalline resin in the same or different particles, in an aqueous medium. The amorphous resin contains an amorphous polyester resin (A) (hereinafter also simply referred to as "resin (A)") which is a polycondensate of an alcohol component (a) containing an aliphatic diol having from 2 to 5 carbon atoms and a carboxylic acid component (b). The crystalline resin contains a crystalline polyester resin (C) (hereinafter also simply referred to as "resin (C)") which is a polycondensate of an alcohol component (c) containing a diol having from 8 to 14 carbon atoms and a carboxylic acid component (d) containing a dicarboxylic acid having 4 carbon atoms. According to the above-mentioned manufacturing method, a toner having excellent low-temperature fixability even at high speed and suppressing the occurrence of fog can be obtained.
[0009] Although the detailed mechanism by which the production method of the present invention provides a toner that is excellent in low-temperature fixability at high speed and suppresses the occurrence of fog is not clear, it is believed to be as follows. In chemical toners produced by conventional emulsion aggregation methods, the hydrophobic crystalline polyester resin among the binder resins is present in large amounts inside the toner by avoiding the interface with water during production, so conventional chemical toners are disadvantageous in terms of rapid thermal response during fixing. On the other hand, when the crystalline polyester resin is exposed on the toner surface, there is a problem that fogging is likely to occur during printing. In contrast, in the production method of the present invention, by using a crystalline resin containing a crystalline polyester (C) which is a polycondensate of an alcohol component (c) containing a diol having 8 to 14 carbon atoms and a carboxylic acid component (d) containing a dicarboxylic acid having 4 carbon atoms, the hydrophilicity of the crystalline resin is relatively improved, and the resin (C) can be present closer to the toner surface. Furthermore, by using an amorphous polyester resin (A) which is a polycondensate of an alcohol component (a) containing an aliphatic diol having 2 to 5 carbon atoms and a carboxylic acid component (b), in the step of aggregating the resin particles, an amorphous resin containing a resin (A) having a higher hydrophilicity than the resin (C) is present on the outermost surface of the aggregated particles, and aggregated particles in which the resin particles (C) are finely dispersed inside, including near the surface, can be obtained. Therefore, in the fused particles obtained in the step of fusing the resin particles constituting the aggregated particles, the resin (C) is present closer to the toner surface, but the surface exposure of the resin (C) is suppressed, and in printing using a toner for developing electrostatic images containing fused particles, the thermal responsiveness of the toner is improved, the toner can be melted by instantaneous heating during fixing, and the toner has excellent low-temperature fixing ability at high speeds and stable image quality with suppressed fogging can be obtained. This effect is not limited to the case where an amorphous resin containing resin (A) and a crystalline resin containing resin (C) are contained in different resin particles, but is thought to be similarly obtained even when an amorphous resin containing resin (A) and a crystalline resin containing resin (C) are contained in the same resin particles. The above-mentioned mechanism regarding the effect of the present invention is merely a presumption, and the present invention is not limited thereto.
[0010] The definitions of various terms used in this specification are given below. In the specification, the carboxylic acid component of the polyester resin includes not only the compound itself, but also anhydrides that decompose during the reaction to produce a carboxylic acid, and alkyl esters of each carboxylic acid (alkyl groups having 1 to 3 carbon atoms). Whether a resin is crystalline or amorphous is determined by the crystallinity index. The crystallinity index is defined as the ratio of the softening point of the resin to the maximum endothermic peak temperature (softening point (°C) / maximum endothermic peak temperature (°C)) in the measurement method described in the examples below. A crystalline resin is one with a crystallinity index of 0.6 or more and 1.4 or less. An amorphous resin is one in which no endothermic peak is observed, or, if observed, has a crystallinity index of less than 0.6 or more than 1.4. The crystallinity index can be appropriately adjusted by the types and ratios of raw material monomers, as well as production conditions such as reaction temperature, reaction time, and cooling rate. With respect to hydrocarbon groups, the references "(iso or tertiary)" and "(iso)" in parentheses refer to both the cases with and without the prefixes present; the absence of the prefixes indicates normal. "(Meth)acrylic acid" means at least one selected from acrylic acid and methacrylic acid. By "styrenic compound" is meant unsubstituted or substituted styrene.
[0011] A method for producing a toner according to an embodiment of the present invention includes a step of aggregating and fusing resin particles, the resin particles including an amorphous resin and a crystalline resin in the same or different particles, in an aqueous medium. The resin particles can be obtained, for example, by a phase inversion emulsification method using an amorphous resin and / or a crystalline resin, as described below. The present invention will be described below by taking this embodiment as an example.
[0012] <Step of aggregating resin particles> In the step of aggregating the resin particles, resin particles containing an amorphous resin and a crystalline resin in the same or different particles are aggregated in an aqueous medium to obtain aggregated particles 1. Here, in addition to the resin particles, it is preferable to further aggregate at least one of a colorant and a release agent, and it is more preferable to mix a resin particle dispersion containing resin particles with a colorant particle dispersion containing colorant particles containing a colorant and / or a release agent particle dispersion containing release agent particles containing a release agent to aggregate these particles. It is more preferable that the resin particle dispersion, the colorant particle dispersion, and the release agent particle dispersion are an aqueous dispersion of resin particles, an aqueous dispersion of colorant particles, and an aqueous dispersion of release agent particles, respectively.
[0013] In the present invention, the aqueous medium is a medium containing water as a main component, and the water content in the aqueous medium is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, and 100% by mass or less. As the water, deionized water, ion-exchanged water, or distilled water is preferable. Examples of components other than water that can form an aqueous medium together with water include organic solvents that dissolve in water, such as alkyl alcohols having 1 to 5 carbon atoms, dialkyl ketones having 3 to 5 carbon atoms, such as acetone and methyl ethyl ketone, and cyclic ethers, such as tetrahydrofuran. Among these, alkyl alcohols having 1 to 5 carbon atoms are preferred, and ethanol is more preferred.
[0014] <Amorphous resin> The amorphous resin is used as a binder resin for the toner, and contains an amorphous polyester resin (A) which is a polycondensation product of an alcohol component (a) containing an aliphatic diol having 2 to 5 carbon atoms and a carboxylic acid component (b).
[0015] [Amorphous polyester resin (A)] The polyester resin (A) is a polycondensation product of an alcohol component (a) and a carboxylic acid component (b), and the alcohol component contains an aliphatic diol having 2 to 5 carbon atoms. Examples of the aliphatic diol having 2 to 5 carbon atoms include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 2-methyl-1,3-propanediol, 1,2-pentanediol, 1,3-pentanediol, 1,4-pentanediol, 1,5-pentanediol, 2,3-pentanediol, 2,4-pentanediol, and neopentyl glycol. The aliphatic diol having 2 to 5 carbon atoms is preferably ethylene glycol, 1,2-propanediol, 1,2-butanediol, 1,3-butanediol, 2,3-butanediol, 2-methyl-1,3-propanediol, and neopentyl glycol, more preferably ethylene glycol, 1,2-propanediol, 2,3-butanediol, and neopentyl glycol, and even more preferably 1,2-propanediol and neopentyl glycol. In the alcohol component (a), the content of the aliphatic diol having 2 to 5 carbon atoms is preferably 85 mol % or more, more preferably 90 mol % or more, even more preferably 95 mol % or more, from the viewpoint of obtaining a toner that is excellent in low-temperature fixing property at high speed and suppresses the occurrence of fog, and is preferably 100 mol % or less, more preferably 100 mol %.
[0016] Examples of the alcohol component (a) other than the aliphatic diol having 2 to 5 carbon atoms include alkylene oxide adducts of aromatic diols, aliphatic diols having 6 or more carbon atoms, alicyclic diols, and trihydric or higher polyhydric alcohols. The alkylene oxide adduct of an aromatic diol is preferably represented by the formula (I):
[0017] [ka] (wherein OR and RO are oxyalkylene groups, R each independently represents an ethylene or propylene group, x and y represent the average number of moles of alkylene oxide added and are each positive numbers, and the sum of x and y is 1 or more, preferably 1.5 or more, and 16 or less, preferably 8 or less, and more preferably 4 or less). Examples of the alkylene oxide adduct of bisphenol A represented by formula (I) include a propylene oxide adduct of 2,2-bis(4-hydroxyphenyl)propane, an ethylene oxide adduct of 2,2-bis(4-hydroxyphenyl)propane, etc. One or more of these may be used.
[0018] Examples of the aliphatic diols having 6 or more carbon atoms include 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,12-dodecanediol, and 1,4-butenediol. Examples of alicyclic diols include hydrogenated bisphenol A [2,2-bis(4-hydroxycyclohexyl)propane] and alkylene oxide adducts of hydrogenated bisphenol A having 2 to 4 carbon atoms (average number of moles added: 2 to 12). Examples of trihydric or higher polyhydric alcohols include glycerin, pentaerythritol, trimethylolpropane, and sorbitol. These alcohol components may be used alone or in combination of two or more.
[0019] Examples of the carboxylic acid component (b) include aromatic dicarboxylic acid compounds, aliphatic dicarboxylic acid compounds, and trivalent or higher carboxylic acid compounds. Among these, the carboxylic acid component (b) preferably contains an aromatic dicarboxylic acid compound, from the viewpoint of obtaining a toner that is excellent in low-temperature fixability under high speed conditions and suppresses the occurrence of fogging. Examples of the aromatic dicarboxylic acid compound include phthalic acid, isophthalic acid, and terephthalic acid. Among these, at least one selected from terephthalic acid and isophthalic acid is more preferable from the above viewpoint. The content of the aromatic dicarboxylic acid compound in the carboxylic acid component (b) is preferably 60 mol % or more, more preferably 70 mol % or more, even more preferably 80 mol % or more, and preferably 100 mol % or less, from the viewpoint of obtaining a toner that has excellent low-temperature fixing properties at high speed and suppresses the occurrence of fog.
[0020] Examples of the aliphatic dicarboxylic acid compound include aliphatic dicarboxylic acids such as oxalic acid, malonic acid, maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, succinic acid which may be substituted with an aliphatic hydrocarbon group having 1 to 20 carbon atoms, and adipic acid. Examples of succinic acid substituted with an aliphatic hydrocarbon group having 1 to 20 carbon atoms include octyl succinic acid and dodecenyl succinic acid (tetrapropenyl succinic acid). Of these, fumaric acid is preferred. The content of the aliphatic dicarboxylic acid compound in the carboxylic acid component (b) is preferably 40 mol % or less, more preferably 30 mol % or less, even more preferably 20 mol % or less, and preferably 0 mol % or more, from the viewpoint of obtaining a toner having excellent low-temperature fixing properties at high speed.
[0021] Examples of trivalent or higher carboxylic acid compounds include 1,2,4-benzenetricarboxylic acid (trimellitic acid), 2,5,7-naphthalenetricarboxylic acid, and pyromellitic acid. The alcohol component (a) may appropriately contain a monohydric alcohol, and the carboxylic acid component (b) may appropriately contain a monocarboxylic acid compound.
[0022] The equivalent ratio of the carboxyl groups of the carboxylic acid component (b) to the hydroxyl groups of the alcohol component (a) [COOH groups / OH groups] is preferably 0.7 or more, more preferably 0.8 or more, and is preferably 1.3 or less, more preferably 1.2 or less.
[0023] (Production method of polyester resin (A)) The resin (A) may be produced, for example, by polycondensing raw material monomers containing an alcohol component (a) and a carboxylic acid component (b).
[0024] The polycondensation of the alcohol component (a) and the carboxylic acid component (b) can be carried out, for example, in an inert gas atmosphere, in the presence of an esterification catalyst, an esterification promoter, a polymerization inhibitor, etc., as necessary, at a temperature of about 120°C or higher and 250°C or lower. Examples of the esterification catalyst include tin compounds such as dibutyltin oxide and tin(II) di(2-ethylhexanoate), and titanium compounds such as titanium diisopropoxybis(triethanolaminate). Examples of the esterification promoter that can be used together with the esterification catalyst include gallic acid. The amount of the esterification catalyst used is preferably 0.01 parts by mass or more and 10 parts by mass or less based on 100 parts by mass in total of the alcohol component (a) and the carboxylic acid component (b), which are raw material monomers for the resin (A). The amount of the esterification promoter used is preferably 0.001 part by mass or more and 1 part by mass or less based on 100 parts by mass in total of the alcohol component (a) and the carboxylic acid component (b). Furthermore, examples of the polymerization inhibitor include radical polymerization inhibitors such as 4-tert-butylcatechol. When a polymerization inhibitor is used, the amount of the polymerization inhibitor used is preferably 0.001 part by mass or more and 1 part by mass or less based on 100 parts by mass in total of the alcohol component (a) and the carboxylic acid component (b).
[0025] (Physical properties of polyester resin (A)) The softening point of the resin (A) is preferably 70°C or higher, more preferably 80°C or higher, and even more preferably 90°C or higher from the viewpoint of heat-resistant storage stability, and is preferably 130°C or lower, more preferably 120°C or lower, and even more preferably 110°C or lower from the viewpoint of low-temperature fixability at high speed. The glass transition temperature of the resin (A) is preferably 30° C. or higher, more preferably 40° C. or higher, and even more preferably 45° C. or higher, from the viewpoint of heat-resistant storage stability, and is preferably 80° C. or lower, more preferably 70° C. or lower, and even more preferably 60° C. or lower, from the viewpoint of low-temperature fixability at high speed.
[0026] The acid value of the resin (A) is preferably 5 mgKOH / g or more, more preferably 10 mgKOH / g or more, even more preferably 15 mgKOH / g or more, and is preferably 40 mgKOH / g or less, more preferably 30 mgKOH / g or less, even more preferably 25 mgKOH / g or less. The softening point, glass transition temperature, and acid value of the resin (A) can be appropriately adjusted by the types and amounts of raw material monomers used, as well as production conditions such as reaction temperature, reaction time, and cooling rate, and these values can be determined by the methods described in the examples. When two or more resins (A) are used in combination, the softening point, glass transition temperature and acid value of the mixture thereof preferably fall within the above-mentioned ranges.
[0027] The amorphous resin contains preferably 90% by mass or more of the amorphous polyester resin (A). From the viewpoint of obtaining a toner having excellent low-temperature fixing ability under high speed and suppressing the occurrence of fog, the content of the resin (A) in the amorphous resin is more preferably 92% by mass or more, even more preferably 95% by mass or more, even more preferably 97% by mass or more, and is preferably 100% by mass or less, more preferably 100% by mass.
[0028] [Amorphous polyester resin (B)] The amorphous resin may contain a resin other than the resin (A) within a range that does not impair the effects of the present application. Examples of such resins include an amorphous polyester resin (B) (hereinafter, simply referred to as "resin (B)") whose alcohol component does not contain an aliphatic diol having 2 to 5 carbon atoms, and other polyester resins. Examples of the resin (B) include polyester resins and modified polyester resins. Examples of the modified polyester resins include urethane modified polyester resins, epoxy modified polyester resins, and composite resins containing polyester resin segments and addition polymerization resin segments.
[0029] <Crystalline resin> The crystalline resin is used as a binder resin for the toner and contains a crystalline polyester resin (C) which is a polycondensate of an alcohol component (c) containing a diol having 8 to 14 carbon atoms and a carboxylic acid component (d) containing a dicarboxylic acid having 4 carbon atoms.
[0030] [Crystalline polyester resin (resin (C))] The resin (C) is a polycondensate of an alcohol component (c) and a carboxylic acid component (d). The alcohol component (c) contains a diol having 8 to 14 carbon atoms, from the viewpoint of obtaining a toner that is excellent in low-temperature fixability even at high speed and that suppresses the occurrence of fog. The diol having 8 to 14 carbon atoms is preferably an aliphatic diol having 8 to 14 carbon atoms, and more preferably an α,ω-aliphatic diol having 8 to 14 carbon atoms. The aliphatic diol having 8 to 14 carbon atoms is preferably an α,ω-aliphatic diol having 8 to 14 carbon atoms, such as 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, or 1,14-tetradecanediol, more preferably one selected from 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, and 1,12-dodecanediol, and even more preferably one selected from 1,9-nonanediol and 1,12-dodecanediol.
[0031] In the alcohol component (c), the content of the diol having 8 to 14 carbon atoms is preferably 80 mol % or more, more preferably 85 mol % or more, even more preferably 90 mol % or more, still more preferably 95 mol % or more, and is preferably 100 mol % or less, more preferably 100 mol %, from the viewpoint of obtaining a toner that is excellent in low-temperature fixing property at high speed and suppresses the occurrence of fog.
[0032] The alcohol component (c) may contain another alcohol component different from the diol having 8 to 14 carbon atoms. Examples of the other alcohol component include a diol having 2 to 7 carbon atoms, a diol having 15 or more carbon atoms, and a trihydric or higher alcohol. These alcohol components may be used alone or in combination.
[0033] The carboxylic acid component (d) contains a dicarboxylic acid having 4 carbon atoms from the viewpoint of obtaining a toner that is excellent in low-temperature fixing ability under high speed conditions and suppresses the occurrence of fogging. Examples of the dicarboxylic acid having 4 carbon atoms include fumaric acid, succinic acid, and methylmalonic acid, and preferably fumaric acid.
[0034] In terms of obtaining a toner that is excellent in low-temperature fixing property under high speed conditions and suppresses the occurrence of fogging, the content of the dicarboxylic acid having 4 carbon atoms in the carboxylic acid component (d) is preferably 80 mol % or more, more preferably 85 mol % or more, even more preferably 90 mol % or more, and is preferably 100 mol % or less, more preferably 100 mol %.
[0035] The carboxylic acid component (d) may contain another carboxylic acid component different from the dicarboxylic acid having 4 carbon atoms. Examples of the other carboxylic acid component include aliphatic dicarboxylic acids having 5 or more carbon atoms, such as adipic acid, sebacic acid, dodecanedioic acid, and tetradecanedioic acid; monovalent carboxylic acids, such as stearic acid; aromatic dicarboxylic acids, such as terephthalic acid and isophthalic acid; and polyvalent carboxylic acids having three or more carboxylic acids. These carboxylic acid components may be used alone or in combination. Among them, the carboxylic acid component (d) preferably contains a monovalent carboxylic acid. Examples of the monovalent carboxylic acid include monovalent carboxylic acids having 6 to 24 carbon atoms, such as caprylic acid, pelargonic acid, lauric acid, myristic acid, palmitic acid, stearic acid, arachidic acid, behenic acid, and lignoceric acid. From the viewpoint of obtaining a toner that is excellent in low-temperature fixing property under high speed conditions and suppresses the occurrence of fogging, preferred are caprylic acid, lauric acid, stearic acid, and behenic acid, more preferred are stearic acid and behenic acid, and even more preferred is stearic acid.
[0036] From the viewpoint of obtaining a toner that has excellent low-temperature fixing properties at high speeds and suppresses the occurrence of fogging, the content of the monovalent carboxylic acid in the carboxylic acid component (d) is preferably 1 mol % or more, more preferably 5 mol % or more, even more preferably 7 mol % or more, and is preferably 20 mol % or less, more preferably 15 mol % or less.
[0037] The equivalent ratio of the carboxyl groups of the carboxylic acid component to the hydroxyl groups of the alcohol component [COOH groups / OH groups] is preferably 0.7 or more, more preferably 0.8 or more, and is preferably 1.3 or less, more preferably 1.2 or less.
[0038] (Physical properties of resin (C)) From the viewpoint of heat-resistant storage stability, the softening point of resin (C) is preferably 55°C or higher, more preferably 60°C or higher, even more preferably 65°C or higher, and preferably 120°C or lower, more preferably 110°C or lower, even more preferably 100°C or lower. From the viewpoint of heat-resistant storage stability, the melting point of resin (C) is preferably 50°C or higher, more preferably 60°C or higher, even more preferably 65°C or higher, and preferably 120°C or lower, more preferably 110°C or lower, even more preferably 100°C or lower.
[0039] The acid value of the resin (C) is preferably 1 mgKOH / g or more, more preferably 3 mgKOH / g or more, and preferably 20 mgKOH / g or less, more preferably 15 mgKOH / g or less, and even more preferably 10 mgKOH / g or less.
[0040] The softening point, melting point, and acid value of the resin (C) can be appropriately adjusted by the types and ratios of the raw material monomers, as well as production conditions such as reaction temperature, reaction time, and cooling rate. These values are determined by the method described in the Examples below. When two or more types of resin (C) are used in combination, it is preferable that the softening point, melting point, and acid value obtained as a mixture of them are each within the above-mentioned ranges.
[0041] Resin (C) can be obtained, for example, by polycondensation of alcohol component (c) and carboxylic acid component (d). The polycondensation conditions can be the same as those described above for polycondensation of resin (A).
[0042] The crystalline resin preferably contains 90% by mass or more of the crystalline polyester resin (C). From the viewpoint of obtaining a toner having excellent low-temperature fixing property under high speed, the content of the resin (C) in the crystalline resin is more preferably 92% by mass or more, even more preferably 95% by mass or more, even more preferably 97% by mass or more, and is preferably 100% by mass or less, more preferably 100% by mass.
[0043] The total content of resin (A) and resin (C) in the amorphous resin and crystalline resin in the resin particles is preferably 80% by mass or more, more preferably 90% by mass or more, and is preferably 100% by mass or less, more preferably 100% by mass, from the viewpoint of obtaining a toner that is excellent in low-temperature fixing property at high speed and suppresses the occurrence of fog.
[0044] The mass ratio of resin (C) to resin (A) [resin (C) / resin (A)] is preferably 5 / 95 or more, more preferably 8 / 92 or more, and even more preferably 12 / 88 or more, from the viewpoint of obtaining a toner that suppresses the occurrence of fog, and is preferably 40 / 60 or less, more preferably 35 / 65 or less, and even more preferably 25 / 75 or less, from the viewpoint of low-temperature fixability at high speed.
[0045] From the viewpoint of obtaining a toner that suppresses the occurrence of fog, the content of resin (A) in the toner particles is preferably 50% by mass or more, more preferably 55% by mass or more, even more preferably 60% by mass or more, and is preferably 80% by mass or less, more preferably 78% by mass or less, even more preferably 75% by mass or less. The content of the resin (C) in the toner particles is preferably 5% by mass or more, more preferably 7% by mass or more, and even more preferably 8% by mass or more from the viewpoint of low-temperature fixability at high speed, and is preferably 30% by mass or less, more preferably 25% by mass or less, and even more preferably 20% by mass or less from the viewpoint of obtaining a toner that suppresses the occurrence of fog. The total content of resin (A) and resin (C) in the toner particles is preferably 60% by mass or more, more preferably 65% by mass or more, even more preferably 70% by mass or more, from the viewpoint of low-temperature fixability at high speed and from the viewpoint of obtaining a toner that suppresses the occurrence of fog, and is preferably 99% by mass or less, more preferably 95% by mass or less, even more preferably 93% by mass or less.
[0046] [Method for producing resin particles] The resin particles of the amorphous resin and the resin particles of the crystalline resin may be produced as an aqueous dispersion of resin particles containing the amorphous resin and the crystalline resin in the same or different particles. The aqueous medium used for the aqueous dispersion is preferably one containing water as a main component.
[0047] Dispersion can be performed using a known method, but it is preferable to disperse by a phase inversion emulsification method. For example, the phase inversion emulsification method includes a method of adding an aqueous medium to an organic solvent solution of a non-crystalline resin and / or a crystalline resin or a molten non-crystalline resin and / or a crystalline resin to perform phase inversion emulsification. A method of adding an aqueous medium to an organic solvent solution of a resin to perform phase inversion emulsification is preferable. The organic solvent used for phase inversion emulsification is not particularly limited as long as it dissolves the amorphous resin and the crystalline resin and is water-soluble, and examples thereof include methyl ethyl ketone. A neutralizing agent may be added to the organic solvent solution. Examples of the neutralizing agent include basic substances. Examples of the basic substance include alkali metal hydroxides such as sodium hydroxide and potassium hydroxide; and nitrogen-containing basic substances such as ammonia, trimethylamine, and diethanolamine. Among these, alkali metal hydroxides such as sodium hydroxide and potassium hydroxide are preferred. The degree of neutralization of the amorphous resin and / or crystalline resin contained in the resin particles is preferably 10 mol % or more, more preferably 20 mol % or more, even more preferably 30 mol % or more, even more preferably 40 mol % or more, and is preferably 100 mol % or less, more preferably 80 mol % or less, even more preferably 70 mol % or less. The degree of neutralization of the amorphous resin and / or the crystalline resin contained in the resin particles can be calculated by the following formula. Degree of neutralization (mol%)=[{weight of neutralizing agent added (g) / equivalent weight of neutralizing agent} / [{weighted average acid value of resin constituting resin particle (mgKOH / g)×weight of resin constituting resin particle (g)} / (56×1000)]]×100
[0048] While stirring the organic solvent solution or the molten resin, the aqueous medium is gradually added to cause phase inversion. From the viewpoint of improving the dispersion stability of the resin particles, the temperature of the organic solvent solution when the aqueous medium is added is preferably not less than the glass transition temperature of the resin (A), more preferably not less than 60°C, even more preferably not less than 65°C, even more preferably not less than 70°C, and is preferably not more than 100°C, more preferably not more than 90°C, even more preferably not more than 80°C.
[0049] After the phase inversion emulsification, the organic solvent may be removed from the obtained dispersion by distillation or the like, if necessary. Also, the resin particles may be isolated by filtration or the like. In this case, the remaining amount of the organic solvent in the dispersion is preferably 1% by mass or less, more preferably 0.5% by mass or less, and even more preferably substantially 0% by mass.
[0050] Volume median diameter D of resin particles in dispersion 50 From the viewpoint of obtaining a toner that is excellent in low-temperature fixing property under high speed conditions and suppresses the occurrence of fog, the average particle diameter is preferably 0.05 μm or more, more preferably 0.10 μm or more, even more preferably 0.15 μm, and is preferably 1 μm or less, more preferably 0.6 μm or less, even more preferably 0.4 μm or less. From the viewpoint of obtaining a toner that has excellent low-temperature fixing property at high speed and suppresses the occurrence of fog, the CV value of the resin particles in the dispersion is preferably 20% or more, more preferably 25% or more, and is preferably 40% or less, more preferably 35% or less.
[0051] From the viewpoint of improving the productivity of the toner and the dispersion stability of the aqueous dispersion of the resin particles, the solids concentration of the aqueous dispersion of the resin particles is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, and is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less. The solid content is the total amount of non-volatile components.
[0052] [Coloring Agent] The colorant is preferably incorporated into the aggregated particles 1 by mixing the colorant in the form of a dispersion of colorant particles with the resin particles and aggregating the colorant. As the colorant, any of the dyes, pigments, etc. used as toner colorants can be used. Examples of colorants include carbon black, phthalocyanine blue, permanent brown FG, brilliant fast scarlet, pigment green B, rhodamine B base, solvent red 49, solvent red 146, solvent blue 35, quinacridone, carmine 6B, disazo yellow, and pigment red 269. The toner may be either a black toner or a color toner other than black.
[0053] (Colorant particle dispersion) The colorant particles are preferably mixed with resin particles as a dispersion of colorant particles, and aggregated to be contained in aggregated particles 1, and are preferably obtained by dispersing the colorant and an aqueous medium using a dispersing machine such as a homogenizer or an ultrasonic dispersing machine. From the viewpoint of improving the dispersion stability of the colorant, the dispersion is preferably carried out in the presence of an addition polymer (hereinafter, the addition polymer used to disperse the colorant is also referred to as "addition polymer E") or a surfactant. Examples of the surfactant include a nonionic surfactant, an anionic surfactant, and a cationic surfactant. The addition polymer E preferably has a constituent unit derived from an addition polymerizable monomer a having an aromatic group, and further preferably contains at least one selected from the group consisting of an addition polymerizable monomer b having an ionic group, an addition polymerizable monomer c having a polyalkylene oxide group, and a macromonomer d. For the colorant particle dispersion and the addition polymer E, reference is made to the addition polymer E described in JP 2021-026129 A.
[0054] From the viewpoint of image density of the printed matter, the content of the colorant in the colorant particle dispersion liquid is preferably 2% by mass or more, more preferably 5% by mass or more, even more preferably 10% by mass or more, and is preferably 45% by mass or less, more preferably 30% by mass or less, even more preferably 20% by mass or less. The solids concentration of the colorant particle dispersion is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, and is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less.
[0055] Volume median particle size D of colorant particles 50 From the viewpoint of improving the dispersibility of the colorant particles in the toner particles, the average particle diameter is preferably 0.05 μm or more, more preferably 0.1 μm or more, even more preferably 0.15 μm or more, and is preferably 0.4 μm or less, more preferably 0.3 μm or less, even more preferably 0.25 μm or less. From the viewpoint of improving the dispersibility of the colorant particles in the toner particles, the CV value of the colorant particles is preferably 10% or more, more preferably 20% or more, and is preferably 45% or less, more preferably 40% or less, and even more preferably 35% or less. Volume median particle size D of colorant particles 50 and CV values are measured by the methods in the Examples.
[0056] From the viewpoint of image density of the printed matter, the content of the colorant in the toner particles is preferably 1% by mass or more, more preferably 2% by mass or more, even more preferably 5% by mass, and is preferably 15% by mass or less, more preferably 10% by mass or less, even more preferably 8% by mass or less.
[0057] [Release Agent] The release agent is preferably contained in the aggregated particles 1 by mixing the resin particles with a dispersion of release agent particles containing the release agent and aggregating the mixture. Examples of the release agent include polypropylene wax, polyethylene wax, polypropylene-polyethylene copolymer wax, hydrocarbon waxes such as microcrystalline wax, paraffin wax, Fischer-Tropsch wax, and oxides thereof, ester waxes such as carnauba wax, montan wax, and deacidified waxes thereof, and fatty acid ester wax, fatty acid amides, fatty acids, higher alcohols, and fatty acid metal salts. These may be used alone or in combination of two or more.
[0058] The melting point of the release agent is preferably 60° C. or higher, more preferably 70° C. or higher, and preferably 160° C. or lower, more preferably 140° C. or lower, even more preferably 120° C. or lower, and even more preferably 100° C. or lower. The content of the release agent in the toner particles is preferably 0.1% by mass or more, more preferably 1% by mass or more, and even more preferably 2% by mass or more, and is preferably 10% by mass or less, and more preferably 5% by mass or less.
[0059] (Release agent particle dispersion) The release agent particle dispersion can be obtained using a surfactant, but is preferably obtained by mixing the release agent with resin particles S, which will be described later. By preparing the release agent particles using the release agent and resin particles S, the release agent particles are stabilized by the resin particles S, and it becomes possible to disperse the release agent in an aqueous medium without using a surfactant. It is considered that the release agent particle dispersion has a structure in which a large number of resin particles S are attached to the surfaces of the release agent particles. The resin constituting the resin particles (S) in which the release agent is dispersed is preferably a polyester resin, and it is more preferable to use a composite resin D having a polyester resin segment and an addition polymerization resin segment. For information on the release agent particle dispersion and composite resin D, see JP 2021-182045 A.
[0060] Volume median particle size D of release agent particles 50 From the viewpoint of obtaining uniform aggregated particles 1 by aggregation, the average particle size is preferably 0.05 μm or more, more preferably 0.1 μm or more, even more preferably 0.2 μm or more, and is preferably 1 μm or less, more preferably 0.8 μm or less, even more preferably 0.6 μm or less. The CV value of the release agent particles is preferably 10% or more, more preferably 15% or more, and is preferably 40% or less, more preferably 35% or less, and further preferably 30% or less. Volume median particle size D of release agent particles 50 The CV value is measured by the method described in the Examples.
[0061] Aggregated particles 1 may also contain additives such as charge control agents, magnetic powders, flowability improvers, conductivity adjusters, reinforcing fillers such as fibrous substances, antioxidants, antiaging agents, and cleaning improvers.
[0062] [Surfactant] In the step of aggregating the resin particles, when the dispersions of the respective particles are mixed to prepare a mixed dispersion, the process may be carried out in the presence of a surfactant from the viewpoint of improving the dispersion stability of the resin particles, the release agent particles, the colorant particles, etc. Examples of the surfactant include anionic surfactants such as alkylbenzene sulfonates and alkyl ether sulfates; and nonionic surfactants such as polyoxyethylene alkyl ethers and polyoxyethylene alkenyl ethers. When a surfactant is used, the total amount used is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, and preferably 10 parts by mass or less, more preferably 5 parts by mass or less, and even more preferably 3 parts by mass or less, per 100 parts by mass of the total amount of resin particles.
[0063] [Flocculant] In the step of aggregating the resin particles, it is preferable to add an aggregating agent from the viewpoint of efficient aggregation. Examples of the flocculant include cationic surfactants such as quaternary salts, organic flocculants such as polyethyleneimine, and inorganic flocculants. Examples of the inorganic flocculant include inorganic metal salts such as sodium sulfate, sodium nitrate, sodium chloride, calcium chloride, and calcium nitrate; inorganic ammonium salts such as ammonium sulfate, ammonium chloride, and ammonium nitrate; and divalent or higher metal complexes. From the viewpoint of improving the coagulation properties and obtaining uniformly coagulated particles 1, inorganic coagulants having a valence of 1 to 5 are preferred, inorganic metal salts having a valence of 1 to 2 and inorganic ammonium salts are more preferred, inorganic ammonium salts are even more preferred, and ammonium sulfate is even more preferred.
[0064] For example, 5 parts by mass or more and 50 parts by mass or less of the aggregating agent is added to a mixed dispersion liquid containing resin particles, release agent particles, and colorant particles at 0° C. or more and 40° C. or less, relative to 100 parts by mass of the resin in the resin particles, and the resin particles, release agent particles, and colorant particles are aggregated in an aqueous medium to obtain aggregated particles 1. Furthermore, from the viewpoint of promoting aggregation, it is preferable to increase the temperature of the dispersion liquid after adding the aggregating agent.
[0065] Examples of a method for stopping the aggregation include a method of cooling the dispersion, a method of adding an aggregation terminator, a method of diluting the dispersion, etc. From the viewpoint of reliably preventing unnecessary aggregation, a method of stopping the aggregation by adding an aggregation terminator is preferred.
[0066] [Aggregation Stopper] The aggregation terminator is preferably a surfactant, more preferably an anionic surfactant. Examples of the anionic surfactant include alkylbenzenesulfonate, alkyl sulfate, alkyl ether sulfate, polyoxyalkylene alkyl ether sulfate, etc. These may be used alone or in combination. The aggregation terminator may be added in the form of an aqueous solution. The amount of the aggregation terminator added is preferably 1 part by mass or more, more preferably 3 parts by mass or more, per 100 parts by mass of the resin in the resin particles, from the viewpoint of reliably preventing unnecessary aggregation, and is preferably 15 parts by mass or less, more preferably 12 parts by mass or less, and even more preferably 10 parts by mass or less, from the viewpoint of reducing residue in the toner.
[0067] Volume median particle size D of aggregate 1 50 is preferably 2 μm or more, more preferably 3 μm or more, even more preferably 4 μm or more, and is preferably 10 μm or less, more preferably 8 μm or less, even more preferably 7 μm or less.
[0068] In the present invention, after the step of aggregating the resin particles and before the step of fusing, a step of aggregating the shell resin particles may be included in which shell resin particles containing an amorphous resin (preferably an amorphous polyester resin) are attached to the obtained aggregated particles 1 to obtain aggregated particles 2. By including the step of aggregating the shell resin particles, toner particles having a core-shell structure can be obtained. Here, the amorphous resin used in the shell resin particles is preferably an amorphous polyester resin, and may be the above-mentioned amorphous polyester resin (A). The shell resin particles are obtained by the same method as the resin particles containing the above-mentioned amorphous resin and / or crystalline resin. Furthermore, when the toner manufacturing method includes a step of aggregating shell resin particles, it is preferable to stop the aggregation in the step when the aggregated particles 2 have grown to an appropriate particle size for toner particles, and a method of stopping the aggregation by adding the above-mentioned aggregation terminator is preferable.
[0069] <Fusing process> In the fusion step, for example, the aggregated particles are fused in an aqueous medium. By fusion, the particles contained in the aggregated particles are fused together to obtain fused particles. In the fusion step, from the viewpoint of improving the fusion properties of the aggregated particles, the aggregated particles are maintained at a temperature equal to or higher than the glass transition temperature of the resin having the highest glass transition temperature among the resins contained in the aggregated particles. The holding temperature when fusing the aggregated particles is, from the viewpoint of improving the fusing property of the aggregated particles and improving the productivity of the toner, preferably at least 5° C. higher than the glass transition temperature of the resin, more preferably at least 10° C. higher, even more preferably at least 15° C. higher, and is preferably not higher than 40° C. higher, more preferably not higher than 35° C. higher, even more preferably not higher than 30° C. higher than the glass transition temperature of the resin. In this case, the time for which the resin is maintained at a temperature equal to or higher than the glass transition temperature is preferably 1 minute or more, more preferably 10 minutes or more, even more preferably 30 minutes or more, and is preferably 240 minutes or less, more preferably 180 minutes or less, even more preferably 120 minutes or less, even more preferably 90 minutes or less. It is preferable to maintain the temperature at the above temperature until the desired circularity is achieved.
[0070] The volume median particle size D of the fused particles obtained by fusion 50 is preferably 2 μm or more, more preferably 3 μm or more, even more preferably 4 μm or more, and is preferably 10 μm or less, more preferably 8 μm or less, even more preferably 7 μm or less.
[0071] The circularity of the fused particles obtained by fusion is preferably 0.955 or more, more preferably 0.960 or more, and is preferably 0.990 or less, more preferably 0.985 or less, and further preferably 0.980 or less. The fusion is preferably terminated after the above-mentioned preferred circularity is reached. The circularity is measured by the method described in the Examples.
[0072] <Post-processing process> After the fusion step, a post-treatment step may be performed, and the fused particles are isolated to obtain toner particles. Since the fused particles obtained in the fusion step are present in an aqueous medium, it is preferable to first perform solid-liquid separation. For the solid-liquid separation, a suction filtration method or the like is preferably used. It is preferable to wash the solid-liquid separation product. In this case, it is preferable to remove the surfactant added, and therefore it is preferable to wash the product with an aqueous medium at a temperature below the cloud point of the surfactant. It is preferable to wash the product several times. Next, drying is preferably performed. Examples of the drying method include vacuum low-temperature drying, vibration-type fluidized bed drying, spray drying, freeze drying, and flash jet drying.
[0073] [Toner Particles] Volume median particle size of toner particles D 50 From the viewpoint of obtaining a toner that is excellent in low-temperature fixing property under high speed and suppresses the occurrence of fogging, and from the viewpoint of further improving the cleaning property of the toner, the average particle size is preferably 2 μm or more, more preferably 3 μm or more, even more preferably 4 μm or more, and is preferably 10 μm or less, more preferably 8 μm or less, even more preferably 7 μm or less.
[0074] The circularity of the toner particles is preferably 0.955 or more, more preferably 0.960 or more, from the viewpoint of obtaining high quality images, and is preferably 0.990 or less, more preferably 0.985 or less, and even more preferably 0.980 or less, from the viewpoint of cleaning properties.
[0075] The CV value of the toner particles is preferably 10% or more, more preferably 15% or more, and even more preferably 20% or more from the viewpoint of improving the productivity of the toner, and is preferably 40% or less, more preferably 35% or less, and even more preferably 30% or less from the viewpoint of obtaining high-quality images. Volume median particle size of toner particles D 50 The CV value can be measured by the method described in the Examples.
[0076] <Toner for developing electrostatic images> The toner for developing electrostatic images of the present invention comprises toner particles. The toner particles can be used as they are, but it is preferable to use the toner after adding a fluidizing agent or the like as an external additive to the surface of the toner particles.
[0077] [External additives] Examples of the external additive include inorganic fine particles such as hydrophobic silica, titanium oxide, alumina, cerium oxide, and carbon black, and polymer fine particles such as polycarbonate, polymethyl methacrylate, and silicone resin. Among these, hydrophobic silica is preferred. The external additive may be used alone or in combination with two or more kinds. In addition, two or more kinds of hydrophobic silica having different particle sizes may be used. When the toner particles are surface-treated using an external additive, the amount of the external additive added is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and preferably 5 parts by mass or less, more preferably 4.5 parts by mass or less, and even more preferably 4 parts by mass or less, relative to 100 parts by mass of the toner particles.
[0078] Toners are used for developing electrostatic images in electrophotographic printing. The toners can be used, for example, as one-component developers or mixed with a carrier to form two-component developers. EXAMPLES
[0079] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. Each property value was measured and evaluated by the following methods. In the notation "alkylene oxide (X)" and the like, the number X in parentheses means the average number of moles of alkylene oxide added.
[0080] <Measurement method> The properties of the polyester resin, the resin particles, the toner, etc. were measured and evaluated by the following methods. [Softening point, crystallinity index, melting point, and glass transition temperature of resin] (1) Softening point Using a flow tester "CFT-500D" (Shimadzu Corporation), 1 g of sample was heated at a temperature increase rate of 6°C / min, while applying a load of 1.96 MPa with the plunger, and extruding the sample from a nozzle with a diameter of 1 mm and a length of 1 mm. The plunger descent amount of the flow tester was plotted against the temperature, and the temperature at which half of the sample flowed out was taken as the softening point. (2) Crystallinity index Using a differential scanning calorimeter "Q100" (manufactured by TA Instruments Japan Co., Ltd.), 0.02 g of sample was weighed into an aluminum pan and cooled to 0°C at a rate of 10°C / min. The sample was then left to stand for 1 minute, and then heated to 180°C at a rate of 10°C / min to measure the amount of heat. The temperature of the peak with the largest peak area among the observed endothermic peaks was taken as the endothermic maximum peak temperature (1), and the crystallinity index was calculated by (softening point (°C)) / (endothermic maximum peak temperature (1) (°C)). (3) Melting point and glass transition temperature Using a differential scanning calorimeter "Q100" (manufactured by TA Instruments Japan Co., Ltd.), 0.02 g of the sample was weighed into an aluminum pan, heated to 200°C, and cooled from that temperature to 0°C at a rate of 10°C / min. The sample was then heated at a rate of 10°C / min, and the amount of heat was measured. Among the endothermic peaks observed, the temperature of the peak with the largest peak area was taken as the maximum endothermic peak temperature (2). In the case of a crystalline resin, this peak temperature was taken as the melting point. In the case of an amorphous resin, when a peak was observed, the temperature of the peak was taken as the glass transition temperature. When no peak was observed but a step was observed, the temperature at the intersection of the tangent showing the maximum slope of the curve at the step and an extension of the baseline on the low temperature side of the step was taken as the glass transition temperature.
[0081] [Acid value of resin] The acid value of the resin was measured according to the neutralization titration method described in JIS K 0070:1992, except that the measurement solvent was chloroform.
[0082] [Melting point of release agent] Using a differential scanning calorimeter "Q100" (manufactured by TA Instruments Japan Co., Ltd.), 0.02 g of the sample was weighed into an aluminum pan, heated to 200°C, and then cooled from 200°C to 0°C at a rate of 10°C / min. The sample was then heated at a rate of 10°C / min, the amount of heat was measured, and the maximum endothermic peak temperature was taken as the melting point.
[0083] [Volume median particle diameter D of resin particles, colorant particles, and release agent particles 50 and CV value] (1) Measuring device: Laser diffraction type particle size measuring device "LA-920" (manufactured by Horiba Ltd.) (2) Measurement conditions: Put the sample dispersion in a measurement cell, add distilled water, and measure the volume median particle size D at a concentration where the absorbance is in the appropriate range. 50 and the volume average particle diameter Dv were measured. The CV value (coefficient of variation (particle size distribution)) was calculated according to the following formula. CV value (%) = (Standard deviation of particle size distribution / Volume average particle size Dv) x 100
[0084] [Solid Content Concentration of Resin Particle Dispersion, Colorant Particle Dispersion, and Release Agent Particle Dispersion] Using an infrared moisture meter "FD-230" (Kett Electric Laboratory Co., Ltd.), the moisture content (mass%) of 5 g of the measurement sample was measured at a drying temperature of 150°C and measurement mode 96 (monitoring time 2.5 minutes, moisture content fluctuation range 0.05%). The solid content concentration was calculated according to the following formula. Solid concentration (mass%) = 100-moisture (mass%)
[0085] [Volume median particle diameter of agglomerated particles D 50 〕 Volume median particle size of agglomerated particles D 50 was measured as follows: Measuring instrument: "Coulter Multisizer (registered trademark) III" (manufactured by Beckman Coulter, Inc.) Aperture diameter: 50μm Analysis software: "Multisizer (registered trademark) III version 3.51" (Beckman Coulter, Inc.) Electrolyte: "Isoton (registered trademark) II" (manufactured by Beckman Coulter, Inc.) Measurement conditions: The sample dispersion is added to 100 mL of the electrolyte to adjust the concentration so that the particle size of 30,000 particles can be measured in 20 seconds. Then, 30,000 particles are measured again, and the volume median particle size D is calculated from the particle size distribution. 50 asked for.
[0086] [Circularity of fused particles] The circularity of the fused particles was measured under the following conditions. Measurement equipment: Flow-type particle image analyzer "FPIA-3000" (Sysmex Corporation) Preparation of dispersion: A dispersion of fused particles was prepared by diluting with deionized water to a solids concentration of 0.001 to 0.05% by mass. Measurement mode: HPF measurement mode
[0087] [Volume median particle size of toner particles D 50 and CV value] Volume median particle size of toner particles D 50 was measured as follows: The measurement device, aperture diameter, analysis software, and electrolyte were determined based on the volume median particle diameter D 50 The same one used in the measurement was used. Dispersion: Polyoxyethylene lauryl ether "EMULGEN (registered trademark) 109P" (manufactured by Kao Corporation, HLB (hydrophile-lipophile balance) = 13.6) was dissolved in the electrolyte to obtain a dispersion with a concentration of 5 mass %. Dispersion conditions: 10 mg of a measurement sample of dried toner particles was added to 5 mL of the dispersion liquid, and dispersed for 1 minute using an ultrasonic disperser. Thereafter, 25 mL of the electrolyte was added, and the mixture was further dispersed for 1 minute using an ultrasonic disperser to prepare a sample dispersion liquid. Measurement conditions: The sample dispersion is added to 100 mL of the electrolyte to adjust the concentration so that the particle size of 30,000 particles can be measured in 20 seconds. Then, 30,000 particles are measured again, and the volume median particle size D is calculated from the particle size distribution. 50 and volume average particle size D V asked for. The CV value (%) was calculated according to the following formula. CV value (%) = (Standard deviation of particle size distribution / Volume average particle size D V ) x 100
[0088] <Resin manufacturing> [Production of amorphous polyester resin (A)] Production Example A1 (Production of Resin A-1) The raw material monomers of polyester resin other than fumaric acid shown in Table 1, and the esterification catalyst were placed in a 10L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube equipped with a fractionating tube through which hot water of 98 ° C was passed, a stirrer, and a thermocouple. Under a nitrogen atmosphere, the reaction system was held at 180 ° C for 1 hour, then heated from 180 ° C to 230 ° C at 10 ° C / h, and then held at 230 ° C for 5 hours to perform polycondensation. After that, after cooling to 180 ° C, 5 g of fumaric acid and a radical polymerization inhibitor (4-tert-butylcatechol) were added to the reaction system, heated from 180 ° C to 210 ° C at 10 ° C / h, and reacted at 210 ° C for 1 hour, and reacted at 210 ° C and 10 kPa until the softening point shown in Table 1 was obtained. The physical properties are shown in Table 1.
[0089] Production Example A2 (Production of Resin A-2) The raw material monomers of polyester resin other than isophthalic acid shown in Table 1, and the esterification catalyst were placed in a 10L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube equipped with a fractionating tube through which hot water of 98 ° C. was passed, a stirrer, and a thermocouple. Under a nitrogen atmosphere, the reaction system was held at 180 ° C. for 1 hour, then heated from 180 ° C. to 230 ° C. at 10 ° C. / h, and then held at 230 ° C. for 5 hours to perform polycondensation. After that, after cooling to 180 ° C., isophthalic acid was added to the reaction system, heated from 180 ° C. to 230 ° C. at 10 ° C. / h, reacted at 230 ° C. for 1 hour, and reacted at 230 ° C. and 10 kPa until the softening point shown in Table 1 was obtained. The physical properties are shown in Table 1.
[0090] Comparative Production Example A1 (Production of Resin A-51) The raw material monomers of polyester resin other than fumaric acid shown in Table 1, and the esterification catalyst were placed in a 10L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple. The temperature was raised to 235°C under a nitrogen atmosphere, and then held at 235°C for 5 hours to perform polycondensation. After that, after cooling to 180°C, 5g of fumaric acid and a radical polymerization inhibitor (4-tert-butylcatechol) were added to the reaction system, the temperature was raised from 180°C to 210°C at 10°C / h, and the reaction was carried out at 210°C for 1 hour, and the reaction was carried out at 210°C and 10kPa until the softening point shown in Table 1 was reached, and resin A-51 was obtained. The physical properties are shown in Table 1.
[0091] [Table 1]
[0092] [Production of crystalline polyester resin (C)] Production Examples C1 to C3 and Comparative Production Example C1 (Production of Resins C-1 to C-3 and C51) The raw material monomers and polymerization inhibitor shown in Table 2 were placed in a 10 L four-neck flask equipped with a thermometer, a stainless steel stirring rod, a downflow condenser, and a nitrogen inlet tube, and the temperature was raised to 200°C over 9 hours in a nitrogen atmosphere in a mantle heater. Then, an esterification catalyst was added, and the reaction was carried out at 8 kPa until the softening point shown in the table was reached, obtaining crystalline polyester resins C1 to C3 and C51. The physical properties are shown in Table 2.
[0093] [Table 2]
[0094] [Production of Resin Particle Dispersion] Production Example X1 (Production of Resin Particle Dispersion X-1) In a 3 L vessel equipped with a stirrer, a reflux condenser, a dropping funnel, a thermometer, and a nitrogen inlet tube, 160 g of resin A-1, 40 g of resin C-1, and 200 g of methyl ethyl ketone were placed and dissolved for 2 hours at 73° C. A 5% by mass aqueous solution of sodium hydroxide was added to the resulting solution so that the degree of neutralization with respect to the acid value of the resin was 60 mol%, and the mixture was stirred for 30 minutes. Next, while maintaining the temperature at 73°C, 700 g of deionized water was added over 50 minutes while stirring at 200 r / min to cause phase inversion emulsification. While maintaining the temperature of the obtained solution at 73°C, methyl ethyl ketone was distilled off under reduced pressure to obtain a dispersion. Thereafter, while continuing to stir, the dispersion was cooled to 30°C, and deionized water was added so that the solid concentration was 20 mass%, thereby obtaining a resin particle dispersion X-1. The volume median particle diameter D of the resin particles in the obtained resin particle dispersion X-1 was 50 and CV values are shown in Table 3.
[0095] Production Examples X2 to X4 and Comparative Production Examples X1 and X2 (Production of Resin Particle Dispersions X-2 to X-4, X-51, and X-52) Resin particle dispersions X-2 to X-4, X-51, and X-52 were obtained in the same manner as in Production Example X1, except that the resin was changed as shown in Table 3. The volume median particle diameter D 50 and CV values are shown in Table 3.
[0096] Production Examples X5 to X7 (Production of Resin Particle Dispersions X-5 to X-7) Resin particle dispersions X-5 to X-7 were obtained in the same manner as in Production Example X1, except that the amounts of Resin A-1 and Resin C-1 were changed as shown in Table 3. The volume median particle diameter D of the resin particles in the obtained resin particle dispersions was 50 and CV values are shown in Table 3.
[0097] [Table 3] [Production of composite resin (D)] Manufacturing Example D1 (Manufacturing of Resin D-1) The inside of a 10L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple was replaced with nitrogen, and 4,313g of a propylene oxide (2.2) adduct of bisphenol A, 818g of terephthalic acid, 727g of succinic acid, 30g of tin (II) di(2-ethylhexanoate), and 3.0g of gallic acid were added, and the reaction system was heated to 235°C under a nitrogen atmosphere while stirring, and then maintained at 235°C for 5 hours, after which the pressure in the flask was reduced and maintained at 8kPa for 1 hour. After that, the pressure was returned to atmospheric pressure, and the temperature was cooled to 160°C, and while maintaining the temperature at 160°C, a mixture of 2,756g of styrene, 689g of stearyl methacrylate, 142g of acrylic acid, and 413g of dibutyl peroxide was added dropwise to the reaction system over 1 hour. The reaction system was then kept at 160°C for 30 minutes, then heated to 200°C, and the pressure in the flask was further reduced to 8 kPa, and the reaction was continued until the desired softening point was reached, yielding Resin D-1. The resulting resin had a softening point of 91°C, a glass transition temperature of 42°C, a crystallinity index of 1.8, and an acid value of 24 mgKOH / g.
[0098] Production Example S1 (Production of Resin Particle Dispersion S-1) 200 g of Resin D-1 and 200 g of methyl ethyl ketone were placed in a 3 L vessel equipped with a stirrer, a reflux condenser, a dropping funnel, a thermometer, and a nitrogen inlet tube, and the resin was dissolved for 2 hours at 73° C. A 5% by mass aqueous solution of sodium hydroxide was added to the resulting solution so that the degree of neutralization with respect to the acid value of Resin D-1 was 60 mol%, and the mixture was stirred for 30 minutes. Next, while maintaining the temperature at 73°C, 700 g of deionized water was added over 50 minutes while stirring at 280 r / min to cause phase inversion emulsification. While maintaining the temperature at 73°C, the methyl ethyl ketone was distilled off under reduced pressure to obtain an aqueous dispersion. Thereafter, while stirring at 280 r / min, the aqueous dispersion was cooled to 30°C, and deionized water was added so that the solid content concentration was 20 mass%, to obtain a resin particle dispersion S-1. The volume median particle diameter D of the resin particles in the obtained resin particle dispersion S-1 was 50 The thickness was 0.09 μm and the CV value was 23%.
[0099] [Preparation of Release Agent Particle Dispersion] Production Example W1 (Production of Release Agent Particle Dispersion W-1) Into a 1 L beaker were added 120 g of deionized water, 86 g of resin particle dispersion S-1, and 40 g of paraffin wax "HNP-9" (manufactured by Nippon Seiro Co., Ltd., melting point 75°C), and the mixture was melted and stirred while maintaining the temperature at 90-95°C to obtain a molten mixture. The obtained molten mixture was dispersed for 20 minutes using an ultrasonic homogenizer "US-600T" (manufactured by Nippon Seiki Seisakusho Co., Ltd.) while maintaining the temperature at 90 to 95°C, and then cooled to room temperature (20°C). Deionized water was added to the obtained dispersion to adjust the solid concentration to 20 mass%, thereby obtaining a release agent particle dispersion W-1. The volume median particle diameter D of the release agent particles in the obtained release agent particle dispersion W-1 was 50 The diameter was 0.47 μm and the CV value was 27%.
[0100] [Preparation of Colorant Particle Dispersion] Production Example Z1 (Production of Colorant Particle Dispersion Z-1) In a beaker with an internal volume of 1 L, 100 g of magenta pigment "Permanent Carmine 3810" (manufactured by Sanyo Pigment Co., Ltd., CI Pigment Red 269), 35 g of polyoxyethylene (13) distyrenated phenyl ether "Emulgen A-60" (manufactured by Kao Corporation, nonionic surfactant), and 300 g of deionized water were mixed and dispersed at room temperature for 1 hour at a rotation speed of the stirring blade of 8000 rpm using a homomixer "TKAGI HOMOMIXER 2M-03" (manufactured by Tokushu Kika Kogyo Co., Ltd.), and then subjected to 15 PASS treatment at a pressure of 150 MPa using a "Microfluidizer M-110EH" (manufactured by Microfluidics Co., Ltd.), and then passed through a 200 mesh filter, and deionized water was added so that the solid concentration was 20 mass%, thereby obtaining a colorant particle dispersion liquid Z-1. The volume median particle diameter D of the colorant particles in the obtained colorant particle dispersion liquid Z-1 was 50 The average particle size was 0.19 μm and the CV value was 28%.
[0101] [Toner manufacturing] Example 1 (Production of Toner 1) In a 3 L four-neck flask equipped with a dehydration tube, a stirrer, and a thermocouple, 500 g of resin particle dispersion X-1, 35 g of release agent particle dispersion W-1, 54 g of colorant particle dispersion Z-1, and 3.3 g of 15 mass % sodium dodecylbenzenesulfonate aqueous solution "Neopelex G-15" (Kao Corporation, anionic surfactant) were placed and mixed at a temperature of 25° C. Next, while stirring the mixture, a solution obtained by dissolving 43 g of ammonium sulfate in 980 g of deionized water and adding a 4.8 mass % potassium hydroxide aqueous solution to adjust the pH to 8.2 was added dropwise over 10 minutes at 25° C., and the temperature was then raised to 58° C. over 2 hours, and the volume median particle diameter D of the aggregated particles was measured. 50 The temperature was maintained at 58° C. until the particle size reached 6.2 μm, thereby obtaining a dispersion of aggregated particles 1. To the obtained dispersion liquid of aggregated particles 1, 22 g of sodium polyoxyethylene lauryl ether sulfate "EMAL E-27C" (manufactured by Kao Corporation, anionic surfactant, effective concentration 27% by mass) and 1100 g of deionized water were added. Thereafter, the temperature was raised to 75°C over one hour, and the temperature was maintained at 75°C until the circularity reached 0.970, thereby obtaining a dispersion liquid of fused particles in which aggregated particles 1 were fused. The obtained dispersion of fused particles was cooled to 30°C, and the dispersion was filtered by suction to separate the solid content, washed with deionized water at 25°C, and filtered by suction at 25°C for 2 hours. Thereafter, the solid content was vacuum dried at 33°C for 24 hours using a vacuum constant temperature dryer "DRV622DA" (manufactured by ADVANTEC Co., Ltd.) to obtain toner particles. 100 parts by mass of toner particles, 2.5 parts by mass of hydrophobic silica "RY50" (manufactured by Nippon Aerosil Co., Ltd., number average particle size; 0.04 μm), and 1.0 part by mass of hydrophobic silica "Cabosil (registered trademark) TS720" (manufactured by Cabot Japan Co., Ltd., number average particle size; 0.012 μm) were put into a Henschel mixer and stirred, and passed through a 150 mesh sieve to obtain toner 1. The physical properties of the toner particles are shown in Table 4.
[0102] <Toner Evaluation> The toner thus obtained was evaluated for its low-temperature fixability under high speed conditions and for fogging of printed matter as follows. [Low temperature fixability at high speed] Using a commercially available printer "Microline (registered trademark) 5400" (manufactured by Oki Electric Industry Co., Ltd.) on high-quality paper "J paper A4 size" (manufactured by Fujifilm Business Innovation Co., Ltd.), the amount of toner attached to the paper was 0.60 ± 0.01 mg / cm 2 The solid image was printed without fixing, leaving a margin of 5 mm from the top edge of A4 paper, and a length of 50 mm. Next, the same printer was prepared with a modified temperature-variable fixing unit, the temperature of the fixing unit was set to 100° C., and the toner was fixed on A4 sheets in portrait orientation at a speed of 0.8 seconds per sheet to obtain a printout. In the same manner, the temperature of the fixing unit was increased by 5° C. each time, and the toner was fixed to obtain a printed matter. A piece of mending tape, Scotch (registered trademark) Mending Tape 810 (manufactured by Sumitomo 3M Limited, width 18 mm), was cut to a length of 50 mm and lightly applied to the top margin of the printed image over the solid image, and then a 500 g weight (contact area 1963 mm2) was applied. 2 ) was placed on the print and pressed against it once at a speed of 10 mm / s. The applied tape was then peeled off from the bottom end at a peeling angle of 180° and a speed of 10 mm / s to obtain a print after the tape had been peeled off. 30 sheets of high-quality paper "Excellent White Paper A4 Size" (manufactured by Oki Electric Industry Co., Ltd.) were placed under the print before and after the tape had been applied and peeled off, and the reflected image density of the fixed image portion of each print before and after the tape had been applied and peeled off was measured using a colorimeter "SpectroEye" (manufactured by GretagMacbeth, light irradiation conditions: standard light source D50, observation field of view 2°, density standard DINNB, absolute white standard), and the fixing rate was calculated from each reflected image density according to the following formula. Fixation rate (%) = (reflection image density after tape peeling / reflection image density before tape application) x 100 The lowest temperature at which the fixing rate was 90% or more was defined as the minimum fixing temperature T1. The lower the minimum fixing temperature, the better the low-temperature fixing ability at high speed.
[0103] [Fog on printed matter] The toner was loaded into a commercially available printer "Microline (registered trademark) 5400" (manufactured by Oki Electric Industry Co., Ltd.), and blank printing was performed on high-quality paper "Excellent White Paper A4 Size" (manufactured by Oki Electric Industry Co., Ltd.) in an environment with a temperature of 23°C and humidity of 50% (NN environment), during which the printer was stopped midway through blank printing. The developing unit was removed from the printer, and "Scotch (registered trademark) Mending Tape 810" (manufactured by 3M Japan Ltd., width: 18 mm) was attached onto the photoconductor, and the toner on the photoconductor was peeled off with the tape. The tape peeled off from the photoreceptor and unused tape were attached to high-quality paper "Excellent White Paper A4 Size" (manufactured by Oki Electric Industry Co., Ltd.), and the tape peeled off from the photoreceptor and unused tape were each measured using a colorimeter "SpectroEye" (manufactured by GretagMacbeth, light irradiation conditions: standard light source D50, observation field of view 2°, density standard DINNB, absolute white standard). The color difference (ΔE) between the tape peeled off from the photoreceptor and unused tape was taken as fog. The smaller the fog value, the better the image without fog that can be obtained.
[0104] Examples 2 to 7 and Comparative Examples 1 and 2 (Production of Toners 2 to 7, 81, and 82) Toners 2 to 7, 81, and 82 were produced in the same manner as in Example 1, except that the type of resin particle dispersion used was changed as shown in Table 4. The physical properties of the obtained toner particles and the evaluation results of the toners are shown in Table 4.
[0105] Comparative Example 3 (Production of Toner 83) 80 parts by mass of amorphous polyester resin A-1, 20 parts by mass of crystalline polyester resin C-1, 8 parts by mass of magenta pigment "Permanent Carmine 3810" (manufactured by Sanyo Pigment Co., Ltd., CI Pigment Red 269), and 6 parts by mass of paraffin wax "HNP-9" (manufactured by Nippon Seiro Co., Ltd., melting point 75°C) as a release agent were mixed in a Henschel mixer. The obtained mixture was melt-kneaded at a screw rotation speed of 200 r / min and a barrel set temperature of 100°C using a co-rotating twin-screw extruder with a kneading section total length of 1560 mm, a screw diameter of 42 mm, and a barrel inner diameter of 43 mm, to obtain a melt-kneaded product. The feed rate of the mixture in the melt-kneading was 20 kg / hour, and the average residence time was about 18 seconds. The obtained melt-kneaded product was cooled and coarsely crushed, then crushed in a jet mill, and classified using an airflow classifier (manufactured by Nippon Pneumatic Mfg. Co., Ltd.) to obtain a volume median particle size (D 50 ) was 6.0 μm in powder (toner particles). 100 parts by mass of toner particles, 2.5 parts by mass of hydrophobic silica "RY50" (manufactured by Nippon Aerosil Co., Ltd., number average particle size: 0.04 μm), and 1.0 part by mass of hydrophobic silica "Cabosil (registered trademark) TS720" (manufactured by Cabot Japan Co., Ltd., number average particle size: 0.012 μm) were placed in a Henschel mixer, stirred, and passed through a 150 mesh sieve to obtain toner 83. The physical properties of the obtained toner particles and the evaluation results of the toner are shown in Table 4.
[0106] [Table 4]
[0107] As shown in Table 4, toners 1 to 7, which have excellent low-temperature fixing properties even at high speeds and suppress the occurrence of fogging, were obtained by the production method of the present invention, which includes a process for aggregating and a process for fusing, in an aqueous medium, resin particles containing, in the same particle, an amorphous resin containing an amorphous polyester resin (A) which is a polycondensate of an alcohol component (a) containing an aliphatic diol having 2 to 5 carbon atoms and a carboxylic acid component (b), and a crystalline resin containing a crystalline polyester resin (C) which is a polycondensate of an alcohol component (c) containing a diol having 8 to 14 carbon atoms and a carboxylic acid component (d) containing a dicarboxylic acid having 4 carbon atoms. On the other hand, in the toner 81 of Comparative Example 1, the hydrophilicity of the amorphous polyester resin (A) in which the alcohol component (a) is an alkylene oxide (2.2) adduct of bisphenol A was insufficient, so that the crystalline polyester resin (C) could not exist near the surface of the toner in the agglomeration and fusion processes, and therefore the fixing temperature at high speed was relatively high. In addition, in the toner 82 of Comparative Example 2, the alcohol component (c) contains 1,4-butanediol and 1,6-hexanediol, so that the exposure of the crystalline polyester resin (C) to the surface of the fused particles could not be suppressed, and the occurrence of fogging could not be suppressed. Furthermore, in the toner 83 of Comparative Example 3 in which the toner particles were produced by the crushing method, the composition of the toner particle surface was non-uniform, so that the fixing temperature at high speed was relatively high, and the occurrence of fogging could not be suppressed.
Claims
1. A method for producing a toner for developing an electrostatic image, comprising the steps of aggregating and fusing resin particles, the resin particles including an amorphous resin and a crystalline resin in the same or different particles, in an aqueous medium, the method comprising the steps of: the amorphous resin contains an amorphous polyester resin (A) which is a polycondensate of an alcohol component (a) containing an aliphatic diol having from 2 to 5 carbon atoms and a carboxylic acid component (b); the crystalline resin contains a crystalline polyester resin (C) which is a polycondensate of an alcohol component (c) containing a diol having 8 to 14 carbon atoms and a carboxylic acid component (d) containing a dicarboxylic acid having 4 carbon atoms; A method for producing a toner for developing electrostatic images.
2. 2. The method for producing a toner for developing an electrostatic image according to claim 1, wherein a mass ratio of the crystalline polyester resin (C) to the amorphous polyester resin (A) [crystalline polyester resin (C) / amorphous polyester resin (A)] is 5 / 95 or more and 40 / 60 or less.
3. 3. The method for producing a toner for developing electrostatic images according to claim 1, wherein the content of the aliphatic diol having 2 to 5 carbon atoms in the alcohol component (a) is 85 mol % or more and 100 mol % or less.
4. 4. The method for producing a toner for developing electrostatic images according to claim 1, wherein the aliphatic diol having from 2 to 5 carbon atoms contains at least one selected from the group consisting of ethylene glycol, 1,2-propanediol, 2,3-butanediol, and neopentyl glycol.
5. 5. The method for producing a toner for developing electrostatic images according to claim 1, wherein the carboxylic acid component (b) contains at least one selected from the group consisting of terephthalic acid, isophthalic acid, and fumaric acid.
6. 6. The method for producing a toner for developing electrostatic images according to claim 1, wherein the content of the diol having 8 to 14 carbon atoms in the alcohol component (c) is 80 mol % or more and 100 mol % or less.
7. 7. The method for producing a toner for developing electrostatic images according to claim 1, wherein the amount of the dicarboxylic acid having 4 carbon atoms in the carboxylic acid component (d) is 80 mol % or more and 100 mol % or less.
8. The method for producing a toner for developing an electrostatic image according to any one of claims 1 to 7, wherein the carboxylic acid component (d) contains a monovalent carboxylic acid.
Citation Information
Patent Citations
Toner for electrophotography
JP2014130291A
toner
JP2018059964A
Cited By
Toner for developing electrostatic images
JP2026154483A
Toner for developing electrostatic images
JP7863245B1
Toner for developing electrostatic latent images
WO2026110856A1