Laminate and method for producing laminate

The laminate design addresses the issues of insufficient contrast and gloss in colloidal crystal laminates by employing regular and irregular resin particle arrangements with coating layers, enhancing both visual properties and durability.

JP2024144968AActive Publication Date: 2024-10-15TOYO INK MFG CO LTD +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023057167
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

Existing laminates using colloidal crystals for structural colors suffer from insufficient contrast and gloss due to cracks and scattering, and lack abrasion resistance.

Method used

A laminate design with pattern parts A and B, where part A features regularly arranged resin fine particles for structural color and part B has irregularly present resin particles, accompanied by coating layers to enhance contrast and gloss, and includes specific thickness and optical properties to improve abrasion resistance.

Benefits of technology

The laminate achieves excellent contrast and gloss with improved abrasion resistance by utilizing regular and irregular arrangements of resin particles and coating layers, reducing scattering and maintaining structural color integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144968000001
    Figure 2024144968000001
  • Figure 2024144968000002
    Figure 2024144968000002
  • Figure 2024144968000003
    Figure 2024144968000003
Patent Text Reader

Abstract

To provide a laminate with excellent contrast between a part showing structural colors and a part showing no structural colors, along with excellent glossiness and abrasion resistance.SOLUTION: This laminate has, on a base material, a pattern part A showing structural colors and a pattern part B showing no structural colors. In the pattern part A, fine resin particles are regularly arranged, and in the pattern part B, fine resin particles are irregularly present. The pattern part A has a thickness of 5-30 μm.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate and a method for producing the laminate. [Background technology]

[0002] The colors of creatures such as Morpho butterflies and jewel beetles are called structural colors, and are produced by the diffraction and interference of light caused by regular structures with spacing similar to the wavelength of light. Structural colors are characterized by vivid coloring and angle dependency, where the color changes depending on the angle from which it is observed, and can produce a sense of luxury and splendor that has never been seen before. In recent years, artificial structural colors have been widely used, for example, to decorate the back of smartphones and for sticker labels. For these applications, there is a demand for pattern formation technology using structural colors, which allows arbitrary characters or pictures to be expressed in structural colors.

[0003] Colloidal crystals are a type of structural color material, with particles that are regularly packed together, and the difference in refractive index between the particles and the gaps between them causes Bragg reflection, resulting in structural color. Among structural color materials, colloidal crystals are characterized by their narrow half-width and high-intensity reflection peaks due to the regularity of the particles, which results in a bright, monochromatic structural color. Another feature is that they can be easily produced, and they can be formed by applying a particle suspension to a substrate and then drying. However, it is known that when colloidal crystals are formed at practical production speeds, a number of cracks occur during drying. A known technique for forming patterns on structural color materials using colloidal crystals is to partially apply heat to the material to fill the gaps between the particles and fade the structural color.

[0004] Patent Documents 1 and 2 disclose a colloidal crystal laminate having a heat-sensitive function, and state that the structural color can be faded by heat treatment with a laser or the like to form an image. The colloidal crystal laminate develops color due to the difference in refractive index between the fine particles and their voids, and the structural color fades when the voids are filled by heat treatment. However, as described in Patent Documents 1 and 2, by simply performing heat treatment, the structural color does not disappear completely, and there is a concern that the contrast will be insufficient because the voids are filled while maintaining the regular arrangement of the fine particles, and that the contrast will be reduced due to cracks generated in the treated area. In addition, the presence of the cracks causes unnecessary scattering, reducing the gloss of the heat-treated area. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2022-80205 [Patent Document 2] WO2006 / 129506 Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a laminate that is excellent in contrast between a portion exhibiting a structural color and a portion not exhibiting a structural color, in gloss, and in abrasion resistance. [Means for solving the problem]

[0007] As a result of extensive research into the above problems, the inventors have found that the above problems can be solved by using the laminate and the method for producing the laminate described below, thereby completing the present invention.

[0008] That is, the present invention relates to the following [1] to

[12] .

[0009] [1] A laminate having a pattern portion A exhibiting a structural color and a pattern portion B exhibiting no structural color on a substrate, wherein resin fine particles are regularly arranged in the pattern portion A, A laminate in which resin fine particles are present irregularly in the pattern portion B.

[0010] [2] The laminate according to [1], wherein the film thickness of the pattern portion A is 5 to 30 μm.

[0011] [3] The laminate according to [1] or [2], wherein, when the diffuse reflectance spectrum of pattern portion A is measured at an incident angle of 5°, the pattern portion A exhibits a reflection peak having a half-width of less than 100 nm and a reflected light intensity of 5% or more in the wavelength range of 380 nm to 2000 nm.

[0012] [4] A laminate according to any one of [1] to [3], wherein, when the diffuse reflectance spectrum of pattern portion B is measured at an incident angle of 5°, the pattern portion B does not exhibit a reflection peak having a half-width of less than 100 nm and a reflected light intensity of 5% or more in the wavelength range of 380 nm to 2000 nm.

[0013] [5] The laminate according to any one of [1] to [4], further comprising a coating layer on the pattern portion A and / or the pattern portion B.

[0014] [6] The laminate according to [5], wherein the coating layer has a thickness of 0.1 to 10 μm.

[0015] [7] The laminate according to [5], wherein the coating layer contains a colorant.

[0016] [8] A laminate according to [5], having a coating layer C containing a resin on the pattern portion B.

[0017] [9] A laminate according to [5], having a coating layer D containing a resin on the pattern portion A.

[0018]

[10] The laminate according to [8], wherein the coating layer C contains a non-aqueous resin.

[0019]

[11] The laminate according to [9], wherein the coating layer D contains an aqueous resin.

[0020]

[12] A method for producing a laminate having a pattern portion A exhibiting a structural color and a pattern portion B exhibiting no structural color on a substrate, comprising the steps of: A step 1 of applying a coating agent containing resin fine particles onto a substrate to form a pattern portion A exhibiting a structural color due to the regular arrangement of the resin fine particles; A process 2 of applying a coating agent not containing resin fine particles to a part of the pattern portion A to change the pattern portion A into a pattern portion B not exhibiting a structural color; A method for producing a laminate, comprising: Effect of the Invention

[0021] According to the present invention, it is possible to provide a laminate that is excellent in contrast between a portion exhibiting a structural color and a portion not exhibiting a structural color, in gloss, and in abrasion resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The following describes in detail the embodiments of the present invention. However, the following description of the components is merely an example of an embodiment of the present invention, and the present invention is not limited to these contents as long as it does not deviate from the gist of the present invention.

[0023] <Laminate> The laminate of the present invention is a laminate having, on a substrate, a pattern portion A exhibiting structural color and a pattern portion B exhibiting no structural color, in which resin microparticles are regularly arranged in the pattern portion A and resin microparticles are irregularly arranged in the pattern portion B.

[0024] In pattern part A, the resin particles are regularly arranged, so that the structural color exhibits excellent color development, while in pattern part B, the resin particles are irregularly arranged, so that the coating film has few cracks and is smooth, so that unnecessary scattering is reduced. Due to the above effects, it is believed that the laminate of the present invention can achieve high levels of contrast and gloss. Note that this explanation is based only on technical considerations and does not limit the invention in any way.

[0025] The laminate of the present invention preferably has a coating layer on the pattern portion A and / or the pattern portion B. In the present invention, the coating layer located on the pattern portion A is referred to as coating layer D, and the coating layer located on the pattern portion B is referred to as coating layer C.

[0026] <Layer structure> Specific examples of the configuration of the laminate of the present invention include, but are not limited to, the following configurations. In the configuration descriptions (1) to (8) below, " / " means the boundary between layers. Although pattern A and pattern B may coexist on one substrate, for the sake of clarity, the layers are described separately as pattern portion A and pattern portion B. (1) Substrate / Pattern part A, Pattern part B (2) Substrate / patterned portion A, patterned portion B / coating layer C (on patterned portion B) (3) Substrate / patterned portion A, patterned portion B / coating layer D (on patterned portion A) (4) Substrate / pattern portion A, pattern portion B / coating layer C (on pattern portion B), coating layer D (on pattern portion A) (5) Substrate / primer layer / pattern part A, pattern part B (6) Substrate / primer layer / pattern portion A, pattern portion B / coating layer C (on pattern portion B) (7) Substrate / primer layer / pattern portion B / coating layer D (on pattern portion A) (8) Substrate / primer layer / pattern portion A, pattern portion B / coating layer C (on pattern portion B), coating layer D (on pattern portion A)

[0027] <Pattern section A> In the present invention, the pattern portion A has a structure in which resin particles are regularly arranged, and the difference in refractive index between the densely packed particles and the gaps between the particles causes Bragg reflection, resulting in a vivid structural color. The resin particles present in the pattern portion A are preferably spherical.

[0028] The film thickness of the pattern portion A is preferably 5 to 30 μm, more preferably 7 to 20 μm, and even more preferably 8 to 15 μm. When the film thickness of the pattern portion A is 5 μm or more, excellent structural color is expressed, resulting in good contrast with the non-structural color portion. Furthermore, when the film thickness is 30 μm or less, the strength of the pattern portion A is maintained, resulting in good abrasion resistance of the laminate.

[0029] When the diffuse reflectance spectrum of the pattern portion A is measured at an incident angle of 5°, it is preferable that the pattern portion A has a reflection peak in the wavelength range of 380 nm to 2000 nm, with a half-width of less than 100 nm and a reflected light intensity of 5% or more. The wavelength range of the reflection peak is more preferably 380 nm to 700 nm, the half-width is more preferably less than 60 nm, and the reflected light intensity is more preferably 10% or more. When the pattern portion A exhibits the above optical properties, excellent structural color appears and the contrast of the laminate becomes good.

[0030] <Resin fine particles> Resin fine particles refer to particulate resin. Some of the resin fine particles exhibit structural color due to regular arrangement. As the resin fine particles, resin fine particles made of a polymer of an ethylenically unsaturated monomer are preferred because it is easy to prepare monodisperse fine particles with a narrow particle size distribution that exhibits excellent structural coloring, and resin fine particles made of an acrylic resin or a styrene acrylic resin are more preferred because it is easy to introduce reactive groups that can form crosslinks between adjacent particles in the pattern portion A and / or crosslinks between the pattern portion A and the adjacent coating layer and / or substrate.

[0031] Moreover, the resin microparticles preferably have a core-shell structure including a core (inner layer) and a shell (outer layer) structure in which the core and shell are water-insoluble polymers and are incompatible with each other. The core functions to maintain the spherical shape, and the shell has fluidity and functions as a binding site. A composition containing core-shell type resin microparticles (hereinafter also referred to as a composition for pattern section A) is applied to a substrate, and the core-shell type resin microparticles are advected and accumulated to be regularly arranged to form a resin layer, whereby the shells of adjacent core-shell type resin microparticles and the shells of the core-shell type resin microparticles and the substrate layer or the primer layer described below are easily bound to each other, and the laminate exhibits excellent abrasion resistance. When the resin fine particles constituting the resin layer are made of a polymer of an ethylenically unsaturated monomer, the desired resin fine particles can be obtained by emulsion polymerization of the ethylenically unsaturated monomer.

[0032] <Core-shell type resin particles> The method for producing core-shell type resin microparticles is not particularly limited, and includes a method of polymerizing ethylenically unsaturated monomer in an aqueous medium such as emulsion polymerization, and a phase inversion emulsification method in which polymerization is performed in a non-aqueous system and then the phase is inverted to an aqueous phase while removing the solvent, but it is preferable to use emulsion polymerization because it can achieve high molecular weight, low viscosity, and high solid content concentration.In addition, in emulsion polymerization, either two-stage polymerization in which the monomer composition is changed between the first stage and the second stage and dropped, or multi-stage polymerization in which the monomer composition is changed in three or more stages and dropped, may be used. The core-shell type resin fine particles can be prepared by the above-mentioned two-stage polymerization, specifically, by the procedure shown below. (1) First, an aqueous medium and a surfactant are charged into a reaction tank and the temperature is raised. Then, under a nitrogen atmosphere, a radical polymerization initiator is added while an emulsion of an ethylenically unsaturated monomer in the first step of forming the core is dropped. After the reaction starts, the particles gradually grow according to the amount of the drop to form the core particle. (2) Next, when the first stage of dropping is completed and the heat generation has subsided, the second stage of dropping the emulsion of the ethylenically unsaturated monomer that forms the shell is started. At this time, additional initiator may be added. The dropped second stage ethylenically unsaturated monomer is once distributed to the core particles, but as the polymerization proceeds, it precipitates as a polymer on the outer layer of the core particles to form a shell layer.

[0033] <Ethylenically unsaturated monomer> Examples of the ethylenically unsaturated monomer include styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, m-methylstyrene, vinylnaphthalene, benzyl(meth)acrylate, phenoxyethyl(meth)acrylate, phenoxydiethylene glycol(meth)acrylate, phenoxytetraethylene glycol(meth)acrylate, phenoxyhexaethylene glycol(meth)acrylate, phenoxyhexaethylene glycol(meth)acrylate, phenyl(meth)acrylate, aromatic ethylenically unsaturated compounds such as acrylate; methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, heptyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, lauryl (meth)acrylate, thiazolinone, tetrahydrofuran ... linear or branched alkyl group-containing ethylenically unsaturated monomers such as tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, and behenyl (meth)acrylate; cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentanyl (meth)acrylate; Alicyclic alkyl group-containing ethylenically unsaturated monomers such as adamantyl (meth)acrylate; fluorinated alkyl group-containing ethylenically unsaturated monomers such as trifluoroethyl (meth)acrylate, heptadecafluorodecyl (meth)acrylate; carboxy group-containing ethylenically unsaturated monomers such as (anhydrous) maleic acid, fumaric acid, itaconic acid, citraconic acid, or alkyl or alkenyl monoesters thereof, succinic acid β-(meth)acryloxyethyl monoester, acrylic acid, methacrylic acid, crotonic acid, cinnamic acid, etc.Sulfo group-containing ethylenically unsaturated monomers such as 2-acrylamido 2-methylpropanesulfonate sodium, methallylsulfonic acid, methallylsulfonic acid, sodium methallylsulfonate, allylsulfonic acid, sodium allylsulfonate, ammonium allylsulfonate, and vinylsulfonic acid; (meth)acrylamide, N-methoxymethyl-(meth)acrylamide, N-ethoxymethyl-(meth)acrylamide, N-propoxymethyl-(meth)acrylamide, N-butoxymethyl-(meth)acrylamide, N-pentoxymethyl-(meth)acrylamide, N,N-di(methoxymethyl)acrylamide, N-ethoxymethyl-N-methoxymethylmethacrylamide, N,N-di(ethoxymethyl)acrylamide, N-ethoxymethyl-N-propoxymethylmethacrylamide, N,N-di(propoxymethyl)acrylamide, N-butoxymethyl-N-(propoxymethyl)methacrylamide, N,N-di(butoxymethyl)acrylamide, ethylenically unsaturated monomers containing an amide group, such as N-butyl-N-(methoxymethyl)acrylamide, N,N-di(pentoxymethyl)acrylamide, N-methoxymethyl-N-(pentoxymethyl)methacrylamide, N,N-dimethylaminopropylacrylamide, N,N-diethylaminopropylacrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide, and diacetone acrylamide; ethylenically unsaturated monomers containing a hydroxyl group, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, glycerol mono(meth)acrylate, 4-hydroxyvinylbenzene, 1-ethynyl-1-cyclohexanol, and allyl alcohol; ethylenically unsaturated monomers containing a polyoxyethylene group, such as methoxypolyethylene glycol (meth)acrylate and polyethylene glycol (meth)acrylate; Amino group-containing ethylenically unsaturated monomers such as dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, methylethylaminoethyl (meth)acrylate, dimethylaminostyrene, and diethylaminostyrene; epoxy group-containing ethylenically unsaturated monomers such as glycidyl (meth)acrylate and 3,4-epoxycyclohexyl (meth)acrylate; diacetone (meth)acrylamide, acetoacetoxy (meth)acrylate, and 2-acetoacetoxyethyl (meth)acrylate. ethylenically unsaturated monomers containing a ketone group, such as allyl (meth)acrylate, 1-methylallyl (meth)acrylate, 2-methylallyl (meth)acrylate, 1-butenyl (meth)acrylate, 2-butenyl (meth)acrylate, 3-butenyl (meth)acrylate, 1,3-methyl-3-butenyl (meth)acrylate, 2-chloroallyl (meth)acrylate, 3-chloroallyl (meth)acrylate, o-allylphenyl (meth)acrylate, 2-(allyloxy)ethyl (meth)acrylate, acrylate, allyl lactyl (meth)acrylate, citronellyl (meth)acrylate, geranyl (meth)acrylate, rosinyl (meth)acrylate, cinnamyl (meth)acrylate, diallyl maleate, diaryl itaconic acid, vinyl (meth)acrylate, vinyl crotonate, vinyl oleate, vinyl linoleate, 2-(2'-vinyloxyethoxy)ethyl (meth)acrylate, ethylene glycol di(meth)acrylate, triethylene glycol (meth)acrylate, tetraethylene glycol Ethylenically unsaturated monomers having two or more ethylenically unsaturated groups, such as cholesteryl (meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, 1,1,1-trishydroxymethylethane diacrylate, 1,1,1-trishydroxymethylethane triacrylate, 1,1,1-trishydroxymethylpropane triacrylate, divinylbenzene, divinyl adipate, diallyl isophthalate, diallyl phthalate, and diallyl maleate;Examples of the ethylenically unsaturated monomers include alkoxysilyl groups, such as γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-methacryloxypropyltributoxysilane, γ-methacryloxypropylmethyldimethoxysilane, γ-methacryloxypropylmethyldiethoxysilane, γ-acryloxypropyltrimethoxysilane, γ-acryloxypropyltriethoxysilane, γ-acryloxypropylmethyldimethoxysilane, γ-methacryloxymethyltrimethoxysilane, γ-acryloxymethyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltributoxysilane, and vinylmethyldimethoxysilane; and ethylenically unsaturated monomers containing methylol groups, such as N-methylol(meth)acrylamide, N,N-dimethylol(meth)acrylamide, and alkyl etherified N-methylol(meth)acrylamide. These monomers may be used alone or in combination of two or more.

[0034] <Average particle size> The average particle size of the resin fine particles is preferably 160 to 350 nm, more preferably 190 to 320 nm, and further preferably 220 to 280 nm. The average particle size in the present invention can be measured by a dynamic light scattering method, and the peak of the obtained volume particle size distribution data (histogram) is taken as the average particle size. The coefficient of variation (Cv value) of the average particle size of the resin fine particles is preferably 30% or less, more preferably 20% or less. When the coefficient of variation is 30% or less, the colored portion exhibits a vivid structural color, and the contrast of the laminate is improved. The coefficient of variation is a value that indicates the uniformity of the particle size, and can be calculated by the following formula. Formula: Coefficient of variation Cv value (%) = standard deviation of particle size / average particle size x 100 [In the formula, the units of standard deviation and average particle size are the same]

[0035] <Glass transition temperature> When the resin microparticles are core-shell type resin microparticles, the glass transition point of the core is preferably 80°C or higher, more preferably 80 to 250°C. The glass transition point of the shell is preferably -20°C or higher, more preferably -20 to 100°C, and even more preferably -20 to 50°C. When the glass transition point of the core is 80°C or higher, the shape of the core is prevented from being deformed by the influence of heat or force from the outside. This allows the pattern part A to maintain excellent color development during the formation of the pattern part B or during winding, and the contrast of the laminate is good. When the glass transition point of the shell is -20°C or higher, the shell has appropriate fluidity and functions as a binding site between particles, so that the abrasion resistance of the laminate is good. The glass transition point can be measured by DSC (differential scanning calorimetry).

[0036] <Particle gap> It is preferable that the pattern part A has particle gaps, and air is present in the particle gaps. The presence of air in the particle gaps increases the difference in refractive index between the particles and the particle gaps, resulting in excellent color development in the colored part and good contrast in the laminate. In the present invention, when voids with a mode pore size of 10 to 200 nm are detected by the nitrogen adsorption method, it can be determined that the particle gaps in the resin layer are air. The mode pore size can be determined by the peak top in the nitrogen adsorption isotherm on the adsorption side, which is obtained by analysis based on the Barrett-Joyner-Halenda method (BJH method). In the BJH method, a standard t curve is calculated using the Harkins-Jura type equation and analyzed based on the volume frequency distribution. In the present invention, the measurement was performed using an apparatus named BELSORP-maxII manufactured by Microtrack Bell Co., Ltd.

[0037] <Additives> The pattern portion A may contain additives such as antifoaming agents, thickeners, surfactants, antiblocking agents, crosslinking agents, leveling agents, waxes, UV absorbers, light stabilizers, and organic solvents such as alcohols, as necessary.

[0038] <Formation of Pattern Part A> The pattern portion A can be formed by applying a coating agent containing resin particles onto a substrate and then drying the coating agent. The coating agent containing resin particles preferably contains resin particles and water. It is known that a dispersion of fine resin particles is regularly arranged as it dries, and at the same time, cracks are generated to no small extent.

[0039] <Method of manufacturing a coating agent containing resin fine particles> A method for producing a coating agent containing resin particles for forming the pattern portion A will be described. The coating agent containing resin particles can be obtained, for example, by feeding an aqueous dispersion of resin particles and any additives into a mixer equipped with a stirring blade, rotor, etc., and mixing and stirring them. There is no particular restriction on the stirring speed, and stirring can be performed at 50 to 2000 rpm. In order to improve the handling and application properties of the coating agent containing resin particles, water and additives can also be appropriately added.

[0040] <Pattern section B> Pattern part B has a structure in which resin particles are irregularly arranged, and does not show structural color. In the present invention, "irregularly arranged resin particles" refers to the resin particles being not regularly arranged, and it is sufficient that the shape of the resin particles remains partially, including the case where the resin particles are partially dissolved and have an irregular shape, and the case where the shells of the resin particles are fused together. The irregularly arranged resin particles result in a smooth coating film with fewer cracks that occur with regular arrangement, thereby reducing unnecessary scattering. Therefore, the laminate of the present invention is excellent in contrast, gloss, and abrasion resistance. The resin particles can be the same as the embodiment of <resin particles> described in the above <pattern part A>. It is preferable that pattern portion B contains amorphous resin particles. Pattern portion B can be formed by applying a coating agent not containing resin particles, which will be described later, to a part of pattern portion A. In this case, it is preferable that the resin particles contained in pattern portion A are partially dissolved and partly changed into amorphous resin particles.

[0041] When the diffuse reflectance spectrum of pattern portion B is measured at an incident angle of 5°, it is preferable that the pattern portion B does not exhibit a reflection peak having a half-width of less than 100 nm and a reflected light intensity of 5% or more in the wavelength range of 380 nm to 2000 nm. When pattern portion B does not exhibit the above optical characteristics, the contrast of the laminate becomes good.

[0042] <Other resins> The pattern part B of the present invention may contain resins other than the above-mentioned resin fine particles, such as acrylic resins, urethane resins, polyolefin resins, polyester resins, and composite resins obtained by combining these resins, and may contain one or more of these.

[0043] <Additives> The pattern portion B of the present invention may contain a colorant, an ultraviolet absorber, or a light stabilizer for adjusting the color tone of the structural color or for protecting the structural color. When the pattern portion B contains an ethylenically unsaturated monomer, it may contain a photopolymerization initiator for the purpose of curing the coating film.

[0044] <Formation of Pattern Part B> Pattern portion B can be formed by applying a coating agent that does not contain resin particles onto a portion of pattern portion A.

[0045] <Coating agent that does not contain resin particles> The coating agent that does not contain resin particles preferably contains a non-aqueous low molecular weight component. The coating agent that does not contain resin particles preferably further contains a non-aqueous resin described below. When the coating agent that does not contain resin particles contains a non-aqueous resin, the coating agent is applied onto the pattern portion A, whereby the formation of the pattern portion B and the formation of the coating layer C described below can be performed simultaneously.

[0046] <Non-aqueous low molecular weight component> The non-aqueous low molecular weight component contained in the coating agent that does not contain resin fine particles is not particularly limited as long as it can destroy the shape and regular array structure of the resin fine particles. Examples of such non-aqueous low molecular weight components include organic solvents such as toluene, xylene, methylcyclohexane, ethyl acetate, normal propyl acetate, butyl acetate, isopropanol, butanol, methyl ethyl ketone, and methyl isobutyl ketone, and the ethylenically unsaturated monomers described in the above section of <ethylenically unsaturated monomers>.

[0047] <Coating layer> The laminate of the present invention preferably further has a coating layer on the pattern portion A and / or the pattern portion B. By having the coating layer, scattering due to resin fine particles and cracks in the pattern portion A and / or the pattern portion B is suppressed, and the contrast and gloss of the laminate are further improved.

[0048] In the present invention, the coating layer located on the pattern portion A is referred to as coating layer D, and the coating layer located on the pattern portion B is referred to as coating layer C. The laminate of the present invention preferably has coating layer C and / or coating layer D, more preferably has coating layer C, and particularly preferably has coating layer C and coating layer D.

[0049] The coating layer preferably has a thickness of 0.1 to 10 μm. When the coating layer has a thickness of 0.1 μm or more, scattering due to resin fine particles and cracks in pattern portion A and / or pattern portion B is suppressed, thereby further improving the contrast and gloss of the laminate. Furthermore, by making the thickness of the coating layer 10 μm or less, the maximum thickness difference within the plane of the laminate is kept small, and the winding properties of the laminate are improved.

[0050] <Coloring agent> The coating layer preferably contains a colorant. By containing a colorant in the coating layer, scattered light unrelated to the structural color can be reduced when the laminate is observed from the non-coated surface side in a reverse printing configuration, and the contrast of the laminate is improved. The type of colorant is not particularly limited, but examples thereof include pigments and dyes, and among them, pigments are preferred. The pigments that can be used in the present invention are not particularly limited, and various inorganic pigments and organic pigments that can be generally used in printing inks and paints can be suitably used. Examples of inorganic pigments include colored pigments such as titanium oxide, red ocher, Prussian blue, ultramarine blue, carbon black, and graphite, and extender pigments such as calcium carbonate, kaolin, clay, barium sulfate, aluminum hydroxide, and talc. In addition, examples of organic pigments include soluble azo pigments, insoluble azo pigments, azo lake pigments, condensed azo pigments, copper phthalocyanine pigments, condensed polycyclic pigments, and the like. However, the pigments are not limited to these, and those listed by generic name in the Color Index can be used as appropriate.

[0051] <Additives> The coating layer may contain additives such as antifoaming agents, thickeners, surfactants, antiblocking agents, crosslinking agents, leveling agents, waxes, ultraviolet absorbing agents, and light stabilizers, as necessary.

[0052] <Coating layer C> By positioning the covering layer C on the pattern portion B, fading of the structural color of the pattern portion B is further promoted and scattering is reduced, improving the contrast and gloss of the laminate. The film thickness of the covering layer C is preferably 0.3 to 25 μm, more preferably 0.8 to 20 μm, and further preferably 1 to 18 μm.

[0053] The coating layer C preferably contains a resin, and more preferably contains a non-aqueous resin. As described above, the coating layer C preferably further contains a colorant. When the coating layer C contains a colorant, the content of the colorant in the coating layer C is preferably 0.1 to 50 mass %.

[0054] <Non-aqueous resin> The non-aqueous resin that can be contained in the coating part C refers to a resin that can be dispersed or dissolved in an organic solvent, and does not include a hydrophilic resin. The non-aqueous resin may contain at least one resin selected from the group consisting of, for example, acrylic resin, styrene-acrylic resin, urethane resin, vinyl chloride resin, vinyl chloride-vinyl acetate resin, vinyl chloride-acrylic resin, polyolefin resin, polyester resin, soluble nitrocellulose, polyamide resin, and composite resins obtained by combining these resins. The non-aqueous resin preferably contains an acrylic resin, a styrene-acrylic resin, or a urethane resin, and more preferably is a styrene-acrylic resin or a urethane resin, since it has a high affinity with the resin fine particles and improves the abrasion resistance of the laminate.

[0055] <Formation of Covering Layer C> The covering layer C can be formed by applying a coating agent containing a resin onto the pattern portion A or the pattern portion B, followed by drying. The coating agent is preferably a coating agent containing a non-aqueous resin. Alternatively, the covering layer C can be formed by applying a coating agent containing a UV monomer onto the pattern portion A or the pattern portion B, followed by UV irradiation. In addition, by applying a coating agent that contains resin but does not contain resin microparticles onto pattern portion A and then drying it, it is possible to simultaneously form pattern portion B and form coating layer C on pattern portion B.

[0056] <Coating agent containing non-aqueous resin> The coating agent containing a non-aqueous resin preferably contains a non-aqueous resin and a non-aqueous low molecular weight component, and more preferably further contains a colorant. In addition, it may contain additives that may be contained in the coating layer as appropriate. As the non-aqueous low molecular weight component, the embodiment of the <non-aqueous low molecular weight component> described in the above <Pattern part B> may be used.

[0057] <Method of manufacturing a coating agent containing a non-aqueous resin> A coating agent containing a non-aqueous resin can be produced, for example, by dispersing a pigment in a non-aqueous low molecular weight component using a disperser with a non-aqueous resin, and then mixing the resulting pigment dispersion with a non-aqueous resin, various additives, a non-aqueous low molecular weight component, and the like. As the disperser, a commonly used one, for example, a roller mill, a ball mill, a pebble mill, an attritor, or a sand mill, can be used. The particle size distribution of the pigment in the pigment dispersion can be adjusted by appropriately adjusting the size of the grinding media of the disperser, the filling rate of the grinding media, the dispersion treatment time, the discharge speed of the pigment dispersion, the viscosity of the pigment dispersion, and the like. The viscosity of the coating agent containing a non-aqueous resin at 25°C is preferably in the range of 10 mPa·s or more from the viewpoint of preventing the pigment from settling and dispersing appropriately, and 300 mPa·s or less from the viewpoint of workability and efficiency during ink production and printing.

[0058] <Coating layer D> By positioning the covering layer D on the pattern portion A, the excellent structural color of the pattern A is maintained, and the contrast and gloss of the laminate are improved. The film thickness of the covering layer D is preferably 0.2 to 12 μm, more preferably 0.5 to 9 μm, and further preferably 1 to 5 μm. The coating layer D preferably contains a resin, and more preferably contains an aqueous resin. As described above, the coating layer D also preferably contains a colorant.

[0059] <Formation of Covering Layer D> The covering layer D can be formed by applying a coating agent containing a resin onto the pattern portion A and then drying the coating agent. The coating agent is preferably a coating agent containing a water-based resin.

[0060] <Coating agent containing water-based resin> The coating agent containing the aqueous resin preferably contains an aqueous resin and an aqueous medium, and more preferably contains a colorant. In addition, the coating layer may contain additives as appropriate. The aqueous resin contained in the coating agent containing the aqueous resin represents a resin that can be dispersed or dissolved in an aqueous medium. The aqueous resin preferably contains at least one resin selected from the group consisting of, for example, acrylic resin, urethane resin, polyolefin resin, polyester resin, and composite resins obtained by combining these resins. In addition, the aqueous resin preferably contains an acrylic resin, a styrene acrylic resin, or a urethane resin, since it has a high affinity with resin fine particles and improves the abrasion resistance of the laminate.

[0061] <Aqueous medium> The main component of the aqueous medium is preferably water, but in addition to water, a hydrophilic organic solvent can be used. Specifically, depending on the printing conditions (speed, plate depth, design, drying temperature), an alcohol-based organic solvent, a glycol-based organic solvent, etc. can be contained. In the present invention, the term "mainly water" means that the content of water is the largest in the aqueous medium, and the term "hydrophilic organic solvent" means that the solvent is liquid at 25° C. and has a solubility of 1% by mass or more in water at 25° C.

[0062] <Method of manufacturing a coating agent containing a water-based resin> A coating agent containing an aqueous resin can be produced, for example, by dispersing a pigment in an aqueous medium with an aqueous resin or the like using a dispersing machine, and mixing the obtained pigment dispersion with an aqueous resin, various additives, an aqueous medium, and the like. As the dispersing machine, a commonly used machine, for example, a roller mill, a ball mill, a pebble mill, an attritor, or a sand mill, can be used. The particle size distribution of the pigment in the pigment dispersion can be adjusted by appropriately adjusting the size of the grinding media of the dispersing machine, the filling rate of the grinding media, the dispersion processing time, the discharge speed of the pigment dispersion, the viscosity of the pigment dispersion, and the like. The viscosity of the coating agent containing an aqueous resin at 25°C is preferably in the range of 10 mPa·s or more from the viewpoint of preventing the pigment from settling and dispersing appropriately, and 300 mPa·s or less from the viewpoint of workability and efficiency during ink production and printing.

[0063] <Base material> The substrate is not particularly limited and can be appropriately selected depending on the application. Examples of the substrate include thermoplastic resin substrates such as polyvinyl chloride sheet, polyethylene terephthalate (PET) film, polypropylene film, polyethylene film, nylon film, polystyrene film, and polyvinyl alcohol film; metal substrates such as aluminum foil; glass substrates, paper substrates such as coated paper; and cloth substrates. The substrate may have a smooth or uneven coating surface. The substrate may be transparent, semi-transparent, or opaque, and may be a substrate that has been colored in advance, such as black, to make the color of the pattern portion A clearer. These substrates may be used alone or as a laminate consisting of two or more layers. The thickness of the substrate is not particularly limited and can usually be appropriately selected within the range of 5 to 500 μm.

[0064] <Primer layer> The laminate of the present invention preferably has a primer layer in order to further improve the fixation of the pattern portion A and the pattern portion B on the substrate. The primer layer is located between the substrate and the pattern portion A and the pattern portion B, and can be formed by applying a primer coating agent onto the substrate before the formation of the pattern portion A. The thickness of the primer layer is preferably from 0.5 to 30 μm, more preferably from 0.8 to 15 μm, and particularly preferably from 1 to 5 μm.

[0065] From the viewpoint of suppressing the influence on the pattern portion A and the pattern portion B, the primer layer preferably has a low content of unreacted components and residual solvent, and is preferably formed from an aqueous resin.

[0066] The aqueous resin forming the primer layer is not particularly limited and can be appropriately selected according to the type of the substrate and the pattern part A. Preferably, it contains at least one selected from the group consisting of acrylic resin, urethane resin, polyolefin resin, polyester resin, and composite resin obtained by combining these resins. Among them, it preferably contains acrylic resin and / or urethane resin, more preferably contains acrylic resin, and further preferably contains acrylic resin containing styrene as a constituent unit (hereinafter, styrene acrylic resin) from the viewpoint of excellent adhesion to the substrate and the pattern part A, excellent substrate followability and water resistance of the primer layer, and good substrate followability, abrasion resistance, and water resistance of the laminate, so it is preferable to use styrene acrylic resin. These resins may be used alone or in combination of two or more.

[0067] <Primer coating agent> The method for forming the primer layer is not particularly limited. For example, the primer layer can be formed by applying a primer coating agent containing an aqueous resin and an aqueous medium that form the primer layer onto a substrate, and drying the same as necessary. The primer coating agent may contain various additives such as hydrophilic solvents, achromatic black fine particles, photothermal conversion agents, crosslinking agents, etc., for the purpose of improving the coatability, contrast, gloss, and winding properties of the laminate, as long as they do not adversely affect the various physical properties of the laminate.

[0068] <Level difference on the coated surface of the laminate> The laminate of the present invention has a step (maximum film thickness difference) of the coated surface of preferably 10 μm or less, more preferably 5 μm or less, and more preferably 0 to 3 μm. By having a step of 10 μm or less, no wrinkles are generated in the film due to the unevenness of the coating film when the laminate is wound up, and the contrast and gloss are good.

[0069] <Method of manufacturing laminate> The method for producing the laminate of the present invention includes a step 1 of applying a coating agent containing resin fine particles onto a substrate or a primer layer to form a pattern portion A exhibiting a structural color due to a regular arrangement of the resin fine particles; The method includes step 2 of applying a coating agent that does not contain resin fine particles to a part of the pattern portion A to change the pattern portion A into a pattern portion B that does not exhibit a structural color.

[0070] In step 2, it is preferable that the regular arrangement of the resin particles in pattern portion A formed in step 1 is disrupted by application of a coating agent that does not contain resin particles, and pattern portion B in which the resin particles are irregularly distributed is formed. In step 2, it is preferable that the resin particles in the pattern portion A formed in step 1 are partially dissolved by application of the coating agent not containing resin particles, and some of them are changed into amorphous resin particles. In step 2, it is preferable to use a coating agent containing a non-aqueous resin as the coating agent not containing resin fine particles, so that the formation of the pattern portion B and the formation of the coating layer C are carried out simultaneously.

[0071] Moreover, the method for producing a laminate of the present invention preferably further comprises a step of forming a covering layer D by applying a coating agent containing an aqueous resin onto the pattern portion A.

[0072] <Coating method> The coating method of the various coating agents is not particularly limited, and can be formed by using a known printing method. Examples of the printing method include non-plate printing methods such as inkjet method, spray method, dipping method, slot die method, and spin coating method; and plate printing methods such as offset gravure coater, gravure coater, doctor coater, kiss coater, bar coater, blade coater, flexo coater, and roll coater.

[0073] The coating agent containing resin fine particles is preferably applied by a spray method, a dipping method, a slot die method, a spin coating method, a gravure coater, a doctor coater, a kiss coater, a bar coater, a blade coater, or a roll coater. By applying the coating agent containing resin fine particles by any of the above methods, the color development of the pattern portion A is excellent and the contrast of the laminate is improved.

[0074] The coating speed of the coating agent containing the resin particles is preferably 0.1 to 100 m / min. By setting the coating speed to 100 m / min or less, the particles form a precise regular arrangement, and the color development of the pattern portion A is excellent.

[0075] The coating method for coating agents that do not contain resin particles is preferably an inkjet method, a spray method, an offset gravure coater, a gravure coater, or a flexo coater, because pattern formation is easy.

[0076] In addition, the coating speed of the coating agent that does not contain resin particles is preferably 20 m / min or more. By using a coating speed of 20 m / min or more, it is possible to form a clear pattern portion B, and the productivity of the laminate is also improved. EXAMPLES

[0077] The present invention will be described below with reference to examples, but the present invention is not limited thereto. In the examples and comparative examples, "parts" and "%" mean "parts by mass" and "% by mass" unless otherwise specified.

[0078] <Average particle size, Cv value> The average particle size was measured by diluting the microparticle dispersion 500 times with water, measuring about 5 ml of the diluted solution by dynamic light scattering measurement (measuring device manufactured by Nanotrack UPA Co., Ltd., Microtrack Bell Co., Ltd.), and the peak of the obtained volumetric particle size distribution data (histogram) was taken as the average particle size. The coefficient of variation Cv value, which indicates the uniformity of the particle size, was calculated by the following formula. Formula: Cv value (%) = standard deviation of particle size / average particle size x 100 [In the formula, the units of standard deviation and average particle size are the same]

[0079] <Glass transition temperature> The glass transition point was measured by DSC (differential scanning calorimeter manufactured by TA Instruments Co., Ltd.). Specifically, about 2 mg of a sample obtained by drying the resin fine particle dispersion was weighed on an aluminum pan, the aluminum pan was set in a DSC measurement holder, and the endothermic peak of the baseline shift (inflection point) chart to the endothermic side of the DSC curve obtained under the temperature increase condition of 5° C. / min was read to obtain the glass transition point.

[0080] <Acid value> The acid value is the number of milligrams of potassium hydroxide required to neutralize the free fatty acids, resin acids, etc. contained in 1 g of a sample, and was measured by the method described in JIS K 0070.

[0081] <Amine value> The amine value is the amount of potassium hydroxide in mg equivalent to the amount of hydrochloric acid required to neutralize the amino groups contained in 1 g of sample, and was measured in accordance with JIS K 0070. 0.5 to 2 g of sample was precisely weighed out (sample solid content: Sg), and 50 mL of a mixed solution of methanol / methyl ethyl ketone = 60 / 40 (mass ratio) was added to the precisely weighed sample to dissolve it. Bromophenol blue was added as an indicator to the resulting solution, and the resulting solution was titrated with a 0.2 mol / L ethanolic hydrochloric acid solution (titer: f). The point at which the color of the solution changed from green to yellow was set as the end point, and the titration amount (AmL) at this point was used to calculate the amine value according to the following formula. (Formula) Amine value = (A x f x 0.2 x 56.108) / S [mgKOH / g]

[0082] <Weight average molecular weight> The weight average molecular weight was determined by measuring the molecular weight distribution using a gel permeation chromatography (GPC) device (HLC-8220 manufactured by Tosoh Corporation) and calculating the molecular weight converted using polystyrene as a standard substance. The measurement conditions are shown below. Columns: The following columns were used in series connection: Tosoh Corporation TSKgel Super AW2500 Tosoh Corporation TSKgel Super AW3000 Tosoh Corporation TSKgel Super AW4000 Tosoh Corporation's TSK gelguard column Super AWH Detector: RI (differential refractometer) Measurement conditions: Column temperature 40℃ Eluent: Tetrahydrofuran Flow rate: 1.0mL / min

[0083] <Measurement of the shape and arrangement of resin particles, and the film thickness of each layer> The shape and arrangement of the resin particles and the thickness of each layer were measured by observing the cross section of the laminate with a scanning electron microscope (JSM-7800F manufactured by JEOL Ltd.).

[0084] <Measurement of half-width, reflected wavelength, and reflected light intensity> The diffuse reflectance spectrum of the laminate was measured in the wavelength range of 350 to 2000 nm using a UV-Vis-NIR spectrophotometer (JASCO Corporation V-770D, integrating sphere unit ISN-923). The reflectance at each wavelength is the relative reflectance measured using a standard white plate with a known reflectance (Labosphere Corporation SRS-99-010) as a reference. The half-width, reflection wavelength, and reflection light intensity were read for the reflection peak with the highest reflection intensity in the obtained reflection spectrum.

[0085] <Production of resin particles> [Production Example 1] Production of core-shell type resin particles 99.0 parts of styrene, 1.0 parts of acrylic acid, 4.0 parts of 25% aqueous solution of Aqualon AR-10 (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., anionic reactive surfactant (polyoxyethylene styrenated phenyl ether sulfate salts) (solid content 1.0 part), and 39.0 parts of ion-exchanged water were mixed and stirred to prepare an emulsion of ethylenically unsaturated monomers in the first stage. 95.0 parts of ion-exchanged water and 1.5% of the emulsion in the first stage were added to a reaction vessel equipped with a stirrer, thermometer, dropping funnel, and reflux condenser. After the internal temperature of the reaction vessel was raised to 70°C and sufficiently substituted with nitrogen, 6.0 parts of a 2.5% aqueous solution of potassium persulfate (solid content 0.15 parts) was added as an initiator to start polymerization. The internal temperature was raised to 80°C and maintained at the same temperature, and the remaining emulsion and 4.2 parts of a 2.5% aqueous solution of potassium persulfate (solid content 0.11 parts) were added dropwise over 2 hours to react, synthesizing core particles. Next, 27.6 parts of styrene, 13.2 parts of n-butyl acrylate, 2.2 parts of methacrylic acid, 1.7 parts of 25% aqueous solution of Aqualon AR-10 (0.4 parts solids), and 16.7 parts of ion-exchanged water were mixed and stirred to prepare the second stage emulsion of ethylenically unsaturated monomer. 20 minutes after the completion of the first stage dripping, the second stage emulsion was started to be dripped. While maintaining the internal temperature at 80°C, the second stage emulsion and 1.6 parts of a 2.5% aqueous solution of potassium persulfate (0.04 parts solids) were dripped over 2 hours to proceed with the reaction, and a water dispersion of core-shell type resin particles was obtained. After the reaction, water was added to adjust the solid content to 45.0%. 1.7 parts of 25% aqueous ammonia (NH3(aq)) was added to neutralize the core-shell type resin microparticles. The amount of aqueous ammonia blended was equivalent to the amount required to neutralize all carboxy groups contained in the shell (hereinafter, 1 equivalent). The average particle size of the obtained microparticles was 258 nm, the Cv value was 12.9%, the Tg of the core was 100.1°C, and the Tg of the shell was 51.8°C.

[0086] [Production Examples 2 to 5] Production of core-shell type resin microparticles In Production Examples 2 to 5, the amount of the first-stage emulsion charged into the reaction vessel was changed from 1.5% in Production Example 1 to 0.9%, 1.0%, 3.0%, and 3.3%, respectively. Otherwise, the same procedure as in Production Example 1 was followed to obtain an aqueous dispersion of core-shell type resin microparticles as shown in Table 1. The amount of water in the reaction vessel was charged to 67% of the total amount of ethylenically unsaturated monomers. The emulsion of ethylenically unsaturated monomers was prepared by adding water so that the concentration of the ethylenically unsaturated monomers in the emulsion was 69% and the concentration of the surfactant was 0.69%. In the 2.5% aqueous solution of potassium persulfate, the ratios at the start of the reaction / when the first-stage emulsion was dropped / when the second-stage emulsion was dropped were the same as in Production Example 1. In addition, 1 equivalent of ammonia water was added to the carboxyl group contained in the shell to neutralize the core-shell type resin microparticles.

[0087] [Table 1]

[0088] [Production Example 6] Production of single-structure resin particles 99.0 parts of styrene, 1.0 part of methacrylic acid, 3.6 parts of a 25% aqueous solution of Aqualon AR-10 (solid content 0.9 parts), and 40.4 parts of ion-exchanged water were mixed and stirred in advance to prepare an emulsion of an ethylenically unsaturated monomer. In a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, and a reflux condenser, 68.9 parts of ion-exchanged water and 3% of the emulsion were added, the internal temperature was raised to 80°C, and the atmosphere was fully replaced with nitrogen. Then, 6.0 parts of a 2.5% aqueous solution of potassium persulfate (0.15 parts solids) was added as an initiator to start emulsion polymerization. While maintaining the internal temperature at 80°C, the remainder of the emulsion and 6.0 parts of a 2.5% aqueous solution of potassium persulfate (0.15 parts solids) were dropped over 3 hours, and the reaction was continued for another 4 hours to obtain an aqueous dispersion of styrene-acrylic resin. After the reaction was completed, 1 equivalent of ammonia water was added to the carboxyl group contained in the resin fine particles to neutralize them, and the solid content of the aqueous dispersion was adjusted to 45.0% with ion-exchanged water. The average particle size of the obtained fine particles was 251 nm, the Cv value was 13.4%, and the Tg was 116.1°C.

[0089] [Production Example 7] Production of resin microparticles An emulsion of an ethylenically unsaturated monomer was prepared by mixing and stirring 40.2 parts of styrene, 57.8 parts of n-butyl acrylate, 2.0 parts of methacrylic acid, 4.0 parts of a 25% aqueous solution of Aqualon AR-10 (solid content 1.0 part), and 40.4 parts of ion-exchanged water. In a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, and a reflux condenser, 68.9 parts of ion-exchanged water and 3% of the emulsion were added, the internal temperature was raised to 80°C, and the atmosphere was fully replaced with nitrogen. Then, 6.0 parts of a 2.5% aqueous solution of potassium persulfate (0.15 parts solids) was added as an initiator to start emulsion polymerization. While maintaining the internal temperature at 80°C, the remainder of the emulsion and 6.0 parts of a 2.5% aqueous solution of potassium persulfate (0.15 parts solids) were dropped over 3 hours, and the reaction was continued for another 4 hours to obtain an aqueous dispersion of styrene-acrylic resin. After the reaction was completed, 1 equivalent of ammonia water was added to the carboxyl group contained in the resin fine particles to neutralize them, and the solid content of the aqueous dispersion was adjusted to 45.0% with ion-exchanged water. The average particle size of the obtained fine particles was 225 nm, the Cv value was 13.9%, and the Tg was 7.4°C.

[0090] [Production Example 8] Production of urethane resin 1 100 parts of polyester polyol having a number average molecular weight of 2,000, which is a condensation product of 3-methyl-1,5-pentanediol and sebacic acid, 1 part of 1,4-butanediol, 28.5 parts of isophorone diisocyanate, and 32.1 parts of ethyl acetate were mixed and reacted at 90°C for 5 hours in a nitrogen atmosphere to obtain a urethane prepolymer with a terminal isocyanate. Next, 11.0 parts of isophoronediamine, 1.0 parts of N-(2-aminoethyl)ethanolamine, 1.0 parts of dibutylamine and 298.1 parts of mixed solvent 1 (ethyl acetate / isopropanol=70 / 30 (mass ratio)) were stirred and mixed, and the obtained urethane prepolymer with terminal isocyanate was gradually added at 40° C. The mixture was reacted at 80° C. for 1 hour to obtain a solution of urethane resin 1 with a solid content of 30 mass%, an amine value of 6.5 mg KOH / g, a hydroxyl value of 3.8 mg KOH / g and a weight average molecular weight of 50,000. The chlorine content of urethane resin 1 was 0 mass%.

[0091] <Coating agent containing resin particles> [Production Example 9] To 100.0 parts of the aqueous dispersion of the core-shell type resin particles of Production Example 1, 1.0 part of Surfynol 420 (an acetylene-based nonionic surfactant manufactured by Nisshin Chemical Industry Co., Ltd.) was added as a surfactant and stirred to prepare a coating agent containing resin particles.

[0092] [Examples 10-15] A coating composition containing resin fine particles was prepared in the same manner as in Production Example 9, except that the blending composition was changed to that shown in Table 2.

[0093] [Table 2]

[0094] <Primer coating agent> [Production Example 16] To 100.0 parts of the aqueous dispersion of resin particles of Production Example 7, 1.0 part of Surfynol 420 (an acetylene-based nonionic surfactant manufactured by Nisshin Chemical Industry Co., Ltd.) was added as a surfactant and stirred to prepare a primer coating agent.

[0095] <Coating agent containing non-aqueous resin> [Production Example 17] A coating agent containing a non-aqueous resin was prepared by adding 190.0 parts of methyl ethyl ketone as a water-insoluble low molecular weight component to 210.0 parts of Taisei Fine Chemical's 7550MA (solid content 47.5%, ethyl acetate / IPA solution, oil-based styrene acrylic resin) and stirring.

[0096] [Examples 18-27] A coating agent containing a non-aqueous resin was prepared in the same manner as in Production Example 17, except that the blending composition was changed to that shown in Table 3.

[0097] [Table 3]

[0098] <Coating agent containing water-based resin> [Production Example 28] To 260.0 parts of BASF JONCRYL PDX7326, 1.0 part of Surfynol 420 as a surfactant, 5.0 parts of Mitsubishi Carbon Black #40 as a colorant, and 240.0 parts of water were added to adjust the solid content to 20%, and then the mixture was stirred to prepare a coating agent containing an aqueous resin.

[0099] [Examples 29-32] A coating agent containing an aqueous resin was prepared in the same manner as in Production Example 28, except that the blending composition was changed to that shown in Table 4.

[0100] [Table 4]

[0101] The abbreviations in Tables 2 to 4 are as follows. Styrene acrylic 1: Taisei Fine Chemical 7550MA (solid content 47.5%, ethyl acetate / IPA solution, oil-based styrene acrylic resin) Urethane 1: Urethane resin 1 produced in Production Example 8 PVC acrylic: Tomoe Engineering's Binnol E15 / 40A (oil-based PVC-acrylic resin) Polyamide: Vegichem Green 725 (25% solids, ethyl acetate / IPA=1 / 1 solution, oil-based polyamide resin) manufactured by Tsuno Foods Industries Nitrocellulose: TNC INDUSTRIAL NC TR2 (25% solids, ethyl acetate / IPA=1 / 1 solution, oil-based nitrocellulose resin) Polyester 1: Toyobo Vylon 200 (oil-based polyester resin) Styrene acrylic 2: BASF JONCRYL PDX7326 (solid content 38.5%, water-based styrene acrylic resin) Urethane 2: Superflex 210 (35% solids, water-based polyurethane resin) manufactured by Daiichi Kogyo Seiyaku Co., Ltd. Polyolefin: Auroren AE-301 (30% solids, water-based polyolefin resin) manufactured by Nippon Paper Industries Co., Ltd. Polyester 2: Pluscoat Z-221 (20% solids, water-based polyester resin) manufactured by GOO Chemical Co., Ltd. MEK: Methyl ethyl ketone EA: Ethyl acetate MCH: Methylcyclohexane IPA: Isopropanol Surfynol 420: An acetylene-based nonionic surfactant manufactured by Nisshin Chemical Industry Co., Ltd. SN Thickener 617: Acrylic thickener manufactured by San Nopco Ltd. Mitsubishi Carbon Black #40: Carbon black manufactured by Mitsubishi Chemical Corporation TMP-A: Light Acrylate TMP-A (trimethylolpropane triacrylate) manufactured by Kyoeisha Chemical Co., Ltd. Omnirad1173: IGM Resins Omnirad1173 (2-hydroxy-2-methyl-1-phenylpropanone)

[0102] <Manufacture of Laminate> [Example 1] The primer coating agent shown in Table 5 was applied to the corona-treated surface of Toyobo Ester Film E5100 with a bar coater selected so that the thickness after drying would be 3.0 μm, and the primer layer was formed by drying at 70 ° C for 1 minute. Next, the coating agent containing the resin fine particles shown in Table 5 was applied to the primer layer with a bar coater selected so that the thickness after drying would be 10.0 μm, and the primer layer was dried at 50 ° C for 1 minute to form a pattern part A. Furthermore, a coating agent containing a non-aqueous resin was applied to a part of the pattern part A by gravure printing with a plate selected so that the thickness after drying would be 1.5 μm, forming a pattern part B and a coating layer C. Next, a coating agent containing an aqueous resin was applied to the pattern part A and the coating layer C with a bar coater selected so that the thickness after drying would be 1.5 μm, forming a primer layer on the PET substrate, and further obtaining a laminate having a pattern part A exhibiting a structural color on the primer layer and a pattern part B not exhibiting a structural color, a coating layer C on the pattern part B, and a coating layer D on the pattern part A.

[0103] [Examples 2 to 6, 8, 11 to 25, 27 to 31] Except for changing the combination shown in Table 5, laminates were produced in the same manner as in Example 1. In Examples 14 to 17, the thicknesses of pattern portion A were adjusted to 3.0, 6.0, 25.8, and 33.1 μm, respectively. In Examples 18 to 20, the coating agent containing a non-aqueous resin and the coating agent containing an aqueous resin were adjusted so that the thickness of the coating layer after drying would be as shown in Table 5.

[0104] [Example 7] A coating agent containing resin particles shown in Table 5 was applied to the corona-treated surface of Toyobo Ester Film E5100 using a bar coater selected so that the thickness after drying would be 10.0 μm, and the coating was dried at 50° C. for 1 minute to form pattern portion A. Furthermore, a coating agent containing a non-aqueous resin was applied to a part of the pattern portion A using a plate selected so that the thickness after drying would be 1.5 μm by gravure printing to form pattern portion B and coating layer C. Next, a coating agent containing an aqueous resin was applied to the pattern portion A and coating layer C using a bar coater selected so that the thickness after drying would be 1.5 μm, to obtain a laminate having a pattern portion A exhibiting structural color on a PET substrate and a pattern portion B not exhibiting structural color, a coating layer C on the pattern portion B, and a coating layer D on the pattern portion A.

[0105] [Example 9] The primer coating agent shown in Table 5 was applied to the corona-treated surface of Toyobo Ester Film E5100 with a bar coater selected so that the thickness after drying would be 3.0 μm, and the primer layer was formed by drying at 70 ° C for 1 minute. Next, a coating agent containing resin fine particles shown in Table 5 was applied to a part of the primer layer with a plate selected so that the thickness after drying would be 10.0 μm, and gravure printing was performed to form pattern part A. Furthermore, on the primer layer where pattern part A was not formed, a coating agent containing single-structure resin fine particles of Production Example 15 was applied with a plate selected so that the thickness after drying would be 10.0 μm by gravure printing to form pattern part B. Next, a coating agent containing an aqueous resin was applied to pattern part A and pattern part B with a bar coater selected so that the thickness after drying would be 1.5 μm, forming a primer layer on the PET substrate, and further, a laminate having pattern part A showing structural color and pattern part B not showing structural color on the primer layer, and having a coating layer D on pattern part A was obtained.

[0106] [Example 10] The primer coating agent shown in Table 5 was applied to the corona-treated surface of Toyobo Ester Film E5100 using a bar coater selected so that the thickness after drying would be 3.0 μm, and then dried at 70 ° C for 1 minute to form a primer layer. Next, the coating agent containing resin fine particles shown in Table 5 was applied to the primer layer using a bar coater selected so that the thickness after drying would be 10.0 μm, and then dried at 50 ° C for 1 minute to form pattern part A. Furthermore, MEK (methyl ethyl ketone) was applied as a coating agent not containing resin fine particles to a part of the pattern part A by gravure printing and dried to form pattern part B, and a primer layer was formed on the PET substrate, and a laminate was obtained having pattern part A exhibiting structural color and pattern part B not exhibiting structural color on the primer layer.

[0107] [Example 26] A primer coating agent shown in Table 5 was applied to the corona-treated surface of Toyobo Ester Film E5100 using a bar coater selected so that the thickness after drying would be 3.0 μm, and then dried at 70° C. for 1 minute to form a primer layer. Next, a coating agent containing resin fine particles shown in Table 5 was applied to the primer layer using a bar coater selected so that the thickness after drying would be 10.0 μm, and then dried at 50° C. for 1 minute to form pattern portion A. Furthermore, a coating agent containing a UV monomer and an initiator was applied to a part of the pattern portion A by flexographic printing using a selected plate so that the thickness after drying would be 1.5 μm, and then 500 mJ / cm was applied using a high-pressure mercury lamp. 2 The pattern portion A was irradiated with ultraviolet light of 1000 W at 1000 W to form a pattern portion B and a coating layer C. Next, a coating agent containing an aqueous resin was applied onto the pattern portion A and the coating layer C using a bar coater so that the thickness after drying would be 1.5 μm, forming a primer layer on the PET substrate, and further obtaining a laminate having a pattern portion A exhibiting a structural color on the primer layer and a pattern portion B not exhibiting a structural color, a coating layer C on the pattern portion B, and a coating layer D on the pattern portion A.

[0108] [Comparative Example 1] The primer coating agent shown in Table 6 was applied to the corona-treated surface of Toyobo Ester Film E5100 using a bar coater selected so that the thickness after drying would be 3.0 μm, and the coating was dried at 70° C. for 1 minute to form a primer layer. Next, the coating agent containing the resin fine particles shown in Table 6 was applied to the primer layer using a bar coater selected so that the thickness after drying would be 10.0 μm, and the coating was dried at 50° C. for 1 minute to form pattern part A. Furthermore, MEK (methyl ethyl ketone) was applied to the entire surface of pattern part A using a bar coater and dried at 70° C. for 1 minute to obtain a laminate having a primer layer and pattern part B on a PET substrate.

[0109] [Comparative Example 2] A primer coating agent shown in Table 6 was applied to the corona-treated surface of Toyobo Ester Film E5100 with a bar coater selected so that the thickness after drying was 3.0 μm, and the primer layer was formed by drying at 70 ° C for 1 minute. Next, a coating agent containing resin fine particles shown in Table 6 was applied to the primer layer with a bar coater selected so that the thickness after drying was 10.0 μm, and the primer layer was dried at 50 ° C for 1 minute to form a pattern part A, and a primer layer was formed on the PET substrate, and a laminate having a pattern part A exhibiting a structural color on the primer layer was obtained. Next, a coating agent containing a non-aqueous resin was applied to the pattern part A with a bar coater selected so that the thickness after drying was 1.5 μm, and a primer layer was formed on the PET substrate, and a laminate having a pattern part B exhibiting no structural color on the primer layer and a coating layer C on the pattern part B was obtained.

[0110] [Comparative Example 3] A primer coating agent shown in Table 6 was applied to the corona-treated surface of Toyobo Ester Film E5100 using a bar coater selected so that the thickness after drying would be 3.0 μm, and the coating was dried for 1 minute at 70° C. to form a primer layer. Next, a coating agent containing resin fine particles shown in Table 6 was applied to the primer layer using a bar coater selected so that the thickness after drying would be 10.0 μm, and the coating was dried for 1 minute at 50° C. to form pattern part A, forming a primer layer on the PET substrate, and a laminate having pattern part A exhibiting structural color on the primer layer was obtained. Next, pattern part B was formed using a thermal printer equipped with a thermal head (PocketJet PJ-673 manufactured by Brother Industries, Ltd.), a primer layer was formed on the PET substrate, and a laminate was obtained having pattern part A exhibiting structural color and pattern part B not exhibiting structural color on the primer layer.

[0111] <Evaluation of the laminate> The obtained laminate was evaluated as follows, and the results are shown in Tables 5 and 6.

[0112] [contrast] The laminate was measured for diffuse reflectance spectrum in the wavelength range of 350 to 2000 nm using an ultraviolet-visible near-infrared spectrophotometer (V-770D manufactured by JASCO Corporation, integrating sphere unit ISN-923). The reflectance at each wavelength is the relative reflectance measured using a standard white board with a known reflectance (SRS-99-010 manufactured by Labsphere) as a reference. For all laminates, the diffuse reflectance spectrum was measured for pattern part A and pattern part B from the coated side (assuming a front printing configuration) and from the uncoated side (assuming a back printing configuration). For the obtained reflectance spectrum, the difference (ΔR) between the maximum reflectance due to the structural color and the baseline reflectance not due to the structural color was calculated, and the difference between ΔR in pattern part A and ΔR in pattern part B was evaluated as the contrast on the coated side and the uncoated side, respectively, and the excellent result was adopted. In Examples 10 and 11, the contrast evaluation results of the coated side were used, while in Examples 1 to 9 and 12 to 31, the evaluation results of the uncoated side were used. (Evaluation Criteria) S: Contrast is 70% or more (very good) A: Contrast is 60% or more but less than 70% (good) B: Contrast is 5% or more and less than 60% (usable) C: Contrast is less than 5% or pattern A showing structural color does not exist (unusable)

[0113] [Glossiness] For pattern portion A and pattern portion B of the laminate, the gloss values ​​were measured from the coated surface side using a Micro-TRI-glossmeter manufactured by BYK-Gardner at an incident angle of 60° and a receiving angle of 60°. (Evaluation Criteria) S: The sum of the gloss values ​​of pattern part A and pattern part B is 50 or more (very good) A: The sum of the gloss values ​​of pattern part A and pattern part B is 40 or more and less than 50 (good) B: The sum of the gloss values ​​of pattern part A and pattern part B is 30 or more and less than 40 (usable) C: The sum of the gloss values ​​of pattern part A and pattern part B is less than 30 (unusable)

[0114] [Abrasion resistance] The abrasion resistance of the coated surface of the patterned portion A and patterned portion B of the laminate was measured using a Gakushin-type abrasion fastness tester manufactured by Tester Sangyo Co., Ltd. The measurement conditions were as follows: test piece 20 mm wide, load 200 g, 10 reciprocations, against Kanakin No. 3. (Evaluation Criteria) A: No change in appearance in either pattern A or pattern B (good) B: Either pattern part A or pattern part B is whitened (usable) C: The entire surface of the laminate turns white (unusable).

[0115] [Table 5]

[0116] [Table 5]

[0117] [Table 5]

[0118] [Table 6]

[0119] From the above results, Comparative Example 1 had poor contrast because it did not have pattern portion A, Comparative Example 2 had poor contrast and abrasion resistance because it did not have pattern portion B, and Comparative Example 3 had poor gloss because the resin microparticles in pattern portion B were regularly arranged. On the other hand, the Example had good contrast, gloss and abrasion resistance since it had pattern portion A in which the resin particles were regularly arranged and pattern portion B in which the resin particles were irregularly arranged.

Claims

1. A laminate having a pattern portion A exhibiting a structural color and a pattern portion B exhibiting no structural color on a substrate, wherein resin fine particles are regularly arranged in the pattern portion A, A laminate, in which resin fine particles are irregularly present in the pattern portion B.

2. 2. The laminate according to claim 1, wherein the film thickness of the pattern portion A is 5 to 30 μm.

3. The laminate according to claim 1 or 2, wherein the pattern portion A exhibits a reflection peak having a half-width of less than 100 nm and a reflected light intensity of 5% or more in a wavelength range of 380 nm to 2000 nm when the diffuse reflectance spectrum is measured at an incident angle of 5°.

4. The laminate according to claim 1 or 2, wherein the pattern portion B does not exhibit a reflection peak having a half-width of less than 100 nm and a reflected light intensity of 5% or more in a wavelength range of 380 nm to 2000 nm when the diffuse reflectance spectrum is measured at an incident angle of 5°.

5. The laminate according to claim 1 or 2, further comprising a coating layer on the pattern portion A and / or the pattern portion B.

6. The laminate according to claim 5, wherein the coating layer has a thickness of 0.1 to 10 μm.

7. The laminate of claim 5 , wherein the coating layer comprises a colorant.

8. The laminate according to claim 5 , further comprising a coating layer C containing a resin on the pattern portion B.

9. The laminate according to claim 5 , further comprising a coating layer D containing a resin on the pattern portion A.

10. The laminate according to claim 8 , wherein the coating layer C comprises a non-aqueous resin.

11. The laminate according to claim 9 , wherein the coating layer D comprises a water-based resin.

12. A method for producing a laminate having a pattern portion A exhibiting a structural color and a pattern portion B exhibiting no structural color on a substrate, comprising the steps of: A step 1 of applying a coating agent containing resin fine particles onto a substrate to form a pattern portion A exhibiting a structural color due to the regular arrangement of the resin fine particles; a step 2 of applying a coating agent not containing resin fine particles to a part of the pattern portion A to change the pattern portion A into a pattern portion B not exhibiting a structural color; A method for producing a laminate, comprising:

Citation Information

Patent Citations

  • Colloid material, and determination method of existence of low dielectric-constant solvent using it

    JP2007051944A

  • Colloid crystal structure and method for producing the same

    JP2010271528A

  • Method for manufacturing patterned colloidal crystal film

    JP2011167663A

  • Elastic body material having periodic structure which varies structural color with modulus

    JP2012000994A

  • Laminated body, thermal recording body, and image forming method

    JP2022080205A