Gas barrier coating material, laminate, packaging material, and method for producing laminate
The gas barrier coating material with a specific formulation of polyurethane resin and silane coupling agent enhances laminate barrier properties, ensuring high oxygen and water vapor resistance even after bending, suitable for packaging applications.
Patent Information
- Application Number
- JP2023057293
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Conventional laminates require improved oxygen and water vapor barrier properties, especially when bent, with specific permeation rates that need to be maintained after folding.
A gas barrier coating material containing a gas barrier polyurethane resin, layered inorganic compounds, and a silane coupling agent, with a predetermined ratio of silane coupling agent to layered inorganic compound, is applied to form a laminate with enhanced barrier properties.
The laminate achieves both oxygen and water vapor barrier properties exceeding predetermined levels even after bending, suitable for use in packaging materials.
Smart Images

Figure 2024145057000003 
Figure 2024145057000001 
Figure 2024145057000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a gas barrier coating material, a laminate, a packaging material, and a method for producing the laminate. [Background technology]
[0002] Conventionally, a laminate including a substrate and a gas barrier layer has been widely known. The gas barrier layer has, for example, excellent oxygen barrier properties. Therefore, the laminate is suitably used, for example, in the field of packaging materials.
[0003] The laminate is formed, for example, by applying a gas barrier coating material to the surface of a substrate and drying the material to form a gas barrier layer.
[0004] For example, a laminate obtained by the following method has been proposed. In this method, first, a polyvinyl alcohol-based polymer aqueous solution (PVA-based polymer solution) with an ethylene content of 8 mol% is prepared. In this method, 3 g of natural montmorillonite is mixed with 0.9 g of a silane coupling agent (γ-glycidyloxypropyltrimethoxysilane) to obtain a dispersant of a silane-modified inorganic layered compound. Next, in this method, the PVA-based polymer solution is mixed with the dispersant of a silane-modified inorganic layered compound to obtain a coating liquid. Thereafter, the coating liquid is applied to the primer-treated surface of cellophane paper, dried at 70°C for 5 minutes, and heat-treated at 130°C for 2 minutes. In this way, a coated film (laminate) is obtained (see, for example, Patent Document 1 (Example 1)). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2003-268184 A Summary of the Invention [Problem to be solved by the invention]
[0006] On the other hand, the laminate is required to have excellent water vapor barrier properties in addition to excellent oxygen barrier properties. In particular, when the substrate is paper, the laminate may be folded. Therefore, even when the laminate is folded, the laminate is required to have excellent oxygen barrier properties and excellent water vapor barrier properties.
[0007] More specifically, even after the laminate is folded, the oxygen permeability (20°C, 80% RH) of the laminate is 50 (cc / m 2 ·day·atm) and the water vapor permeability (40°C, 90% RH) of the laminate is less than 50 (g / m 2 The required period is less than 10 days.
[0008] The present invention relates to a gas barrier coating material that can give a laminate that, after folding, has both a predetermined level of oxygen barrier property and a predetermined level of water vapor barrier property; a laminate obtained by using the gas barrier coating material; a packaging material containing the laminate; and a method for producing the laminate. [Means for solving the problem]
[0009] The present invention [1] is a gas barrier coating material containing a gas barrier resin and an additive, wherein the gas barrier resin contains a gas barrier polyurethane resin, the additive contains a layered inorganic compound and a silane coupling agent, and the content of the silane coupling agent per part by mass of the layered inorganic compound is 0.03 parts by mass or more and 2.7 parts by mass or less.
[0010] The present invention [2] comprises the gas barrier coating material according to the above [1], wherein the gas barrier polyurethane resin contains a reaction product of an isocyanate-terminated prepolymer and a chain extender, the isocyanate-terminated prepolymer contains a reaction product of a polyisocyanate component and an active hydrogen group-containing component, the polyisocyanate component contains xylylene diisocyanate and / or hydrogenated xylylene diisocyanate, and the active hydrogen group-containing component contains a short-chain diol having 2 to 6 carbon atoms and an active hydrogen compound containing an anionic group.
[0011] The present invention [3] includes the gas barrier coating material described in [2] above, in which the active hydrogen compound containing an anionic group contains an active hydrogen group-containing compound containing a carboxy group, and the silane coupling agent contains an epoxy group capable of reacting with the carboxy group and an alkoxysilyl group capable of reacting with the layered inorganic compound.
[0012] The present invention [4] includes the gas barrier coating material according to the above [3], in which the content of the silane coupling agent per part by mass of the layered inorganic compound is 0.3 parts by mass or more and 1.1 parts by mass or less.
[0013] The present invention [5] includes a laminate comprising a substrate and a gas barrier layer disposed on at least one side of the substrate, the gas barrier layer including a cured film of the gas barrier coating material according to any one of the above [1] to [4].
[0014] The present invention [6] includes the laminate according to the above [5], in which the substrate is a paper substrate.
[0015] The present invention [7] includes the laminate according to the above [5] or [6], in which a filling layer is interposed between the substrate and the gas barrier layer.
[0016] The present invention [8] further comprises the step of: 2The laminate according to any one of the above items [5] to [7] is included.
[0017] The present invention [9] includes a packaging material containing the laminate according to any one of the above [5] to [8].
[0018] The present invention
[10] includes a method for producing a laminate, comprising: a coating step of coating the gas barrier coating material described in any one of the above [1] to [4] on at least one side of a substrate; and a curing step of heating the coating film of the gas barrier coating material at 100°C or higher for 1 hour or more to form a cured film of the gas barrier coating material.
[0019] The present invention
[11] includes the method for producing a laminate described in the above
[10] , wherein the substrate is a paper substrate, and the method for producing the laminate includes a filling layer forming step of forming a filling layer on at least one surface of the substrate before the coating step, and in the coating step, the gas barrier coating material is applied to at least one surface of the filling layer. Effect of the Invention
[0020] The gas barrier coating material of the present invention contains a gas barrier resin and an additive. The gas barrier resin contains a gas barrier polyurethane resin. The additive contains a layered inorganic compound and a silane coupling agent in a predetermined ratio. Therefore, according to the gas barrier coating material, a laminate having both a predetermined level of oxygen barrier property and a predetermined level of water vapor barrier property can be obtained after bending.
[0021] The laminate of the present invention is obtained by using the gas barrier coating material described above, and therefore the laminate has at least a predetermined level of oxygen barrier property and at least a predetermined level of water vapor barrier property after folding.
[0022] The laminate of the present invention contains the above-mentioned laminate, and therefore has at least a predetermined level of oxygen barrier property and at least a predetermined level of water vapor barrier property after folding.
[0023] The method for producing a laminate of the present invention uses the gas barrier coating material described above, and therefore, the method for producing a laminate of the present invention can provide a laminate that, after folding, has at least a predetermined level of oxygen barrier property and at least a predetermined level of water vapor barrier property. [Brief description of the drawings]
[0024] [Figure 1] FIG. 1 is a schematic diagram showing one embodiment of a laminate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] 1. Gas barrier coating material The gas barrier coating material contains a gas barrier resin and an additive, more specifically, the gas barrier coating material is an aqueous dispersion in which the gas barrier resin and the additive are dispersed in water.
[0026] (1) Gas barrier resin A gas barrier resin is a resin having an oxygen permeability of a predetermined value or less. More specifically, the oxygen permeability of a 10 μm-thick film made of a gas barrier resin is, for example, 1 (cc / m) at room temperature. 2 ·day·atm). The oxygen permeability is measured in accordance with JIS K7126 (2006) Method B using an oxygen permeability measuring device (MOCON, OX-TRAN2 / 22H). The measurement conditions are 20°C and 80% RH (relative humidity).
[0027] The gas barrier resin contains a gas barrier polyurethane resin as an essential component. The gas barrier resin can further contain other gas barrier resins as optional components. The other gas barrier resins are gas barrier resins other than gas barrier polyurethane resins. Examples of the other gas barrier resins include gas barrier acrylic resins and gas barrier polyvinyl alcohol resins. The content ratio of the other gas barrier resins is, for example, 30% by mass or less, preferably 10% by mass or less, and more preferably 0% by mass, relative to the total amount of the gas barrier resins. In other words, the gas barrier resin preferably does not contain other gas barrier resins and is made of a gas barrier polyurethane resin.
[0028] The gas barrier resin is produced, for example, as an aqueous dispersion of the gas barrier resin. For example, the gas barrier polyurethane resin is produced as a polyurethane dispersion (PUD).
[0029] The gas barrier polyurethane resin is a resin having an oxygen permeability equal to or less than the above-mentioned predetermined value. More specifically, the gas barrier polyurethane resin contains, for example, a reaction product of an isocyanate-terminated prepolymer and a chain extender, and is preferably made of a reaction product of an isocyanate-terminated prepolymer and a chain extender. The isocyanate-terminated prepolymer contains, for example, a reaction product of a polyisocyanate component and an active hydrogen group-containing component, and is preferably made of a reaction product of a polyisocyanate component and an active hydrogen group-containing component.
[0030] That is, the primary reaction product of the polyisocyanate component and the active hydrogen group-containing component is an isocyanate-terminated prepolymer, and the secondary reaction product of the isocyanate-terminated prepolymer and a chain extender is a gas barrier polyurethane resin.
[0031] [Polyisocyanate component] The polyisocyanate component contains, for example, xylylene diisocyanate and / or hydrogenated xylylene diisocyanate from the viewpoint of improving the oxygen barrier property and water vapor barrier property.
[0032] Examples of xylylene diisocyanate (XDI) include 1,2-xylylene diisocyanate (o-XDI), 1,3-xylylene diisocyanate (m-XDI), and 1,4-xylylene diisocyanate (p-XDI). These can be used alone or in combination of two or more. Examples of xylylene diisocyanate (XDI) include preferably 1,3-xylylene diisocyanate (m-XDI) and 1,4-xylylene diisocyanate (p-XDI), and more preferably 1,3-xylylene diisocyanate (m-XDI).
[0033] Examples of hydrogenated xylylene diisocyanate (also known as bis(isocyanatomethyl)cyclohexane) (H6XDI) include 1,2-hydrogenated xylylene diisocyanate (1,2-H6XDI), 1,3-hydrogenated xylylene diisocyanate (1,3-H6XDI), and 1,4-hydrogenated xylylene diisocyanate (1,4-H6XDI). These can be used alone or in combination of two or more. Preferred examples of hydrogenated xylylene diisocyanate (H6XDI) include 1,3-hydrogenated xylylene diisocyanate (1,3-H6XDI) and 1,4-hydrogenated xylylene diisocyanate (1,4-H6XDI), and more preferably, 1,3-hydrogenated xylylene diisocyanate (1,3-H6XDI).
[0034] The xylylene diisocyanate and / or hydrogenated xylylene diisocyanate includes xylylene diisocyanate derivatives and / or hydrogenated xylylene diisocyanate derivatives. Examples of the derivatives include multimers, isocyanurate modified products, allophanate modified products, polyol adducts, biuret modified products, urea modified products, oxadiazinetrione modified products, and carbodiimide modified products. These can be used alone or in combination of two or more types.
[0035] As the xylylene diisocyanate and / or hydrogenated xylylene diisocyanate, preferably, a monomer is used, more preferably, a monomer of xylylene diisocyanate is used, and further preferably, a monomer of 1,3-xylylene diisocyanate (m-XDI) is used.
[0036] The polyisocyanate component can contain other polyisocyanates (polyisocyanates other than xylylene diisocyanate and hydrogenated xylylene diisocyanate) as necessary.
[0037] Examples of other polyisocyanates include linear aliphatic polyisocyanates, alicyclic polyisocyanates (excluding hydrogenated xylylene diisocyanate), aromatic polyisocyanates, and araliphatic polyisocyanates (excluding xylylene diisocyanate).
[0038] Examples of the chain aliphatic polyisocyanate include chain aliphatic diisocyanate. Examples of the chain aliphatic diisocyanate include ethylene diisocyanate, trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate (PDI) and hexamethylene diisocyanate (HDI). Examples of the chain aliphatic polyisocyanate include the above-mentioned derivatives of the chain aliphatic diisocyanate. These can be used alone or in combination of two or more kinds.
[0039] Examples of alicyclic polyisocyanates (excluding hydrogenated xylylene diisocyanate) include alicyclic diisocyanates (excluding hydrogenated xylylene diisocyanate). Examples of alicyclic diisocyanates include cyclohexane diisocyanate, isophorone diisocyanate (IPDI), norbornene diisocyanate (NBDI), and methylene bis(cyclohexyl isocyanate) (H 12 The alicyclic polyisocyanate includes, for example, the above-mentioned derivatives of the alicyclic diisocyanate. These can be used alone or in combination of two or more kinds.
[0040] Examples of aromatic polyisocyanates include aromatic diisocyanates. Examples of aromatic diisocyanates include diphenylmethane diisocyanate (MDI), tolylene diisocyanate (TDI), toluidine diisocyanate (TODI), paraphenylene diisocyanate, and naphthalene diisocyanate (NDI). Examples of aromatic polyisocyanates include the above-mentioned derivatives of aromatic diisocyanates. These can be used alone or in combination of two or more.
[0041] Examples of the araliphatic polyisocyanate (excluding xylylene diisocyanate) include araliphatic diisocyanate (excluding xylylene diisocyanate). Examples of the araliphatic diisocyanate include tetramethyl xylylene diisocyanate (TMXDI). Examples of the araliphatic polyisocyanate include the above-mentioned derivatives of araliphatic diisocyanate. These can be used alone or in combination of two or more kinds.
[0042] The other polyisocyanates can be used alone or in combination of two or more kinds. As the other polyisocyanates, preferably, alicyclic polyisocyanates, more preferably, methylene bis(cyclohexyl isocyanate) (H 12 MDI) are examples.
[0043] As the polyisocyanate component, from the viewpoint of improving the oxygen barrier property and the water vapor barrier property, a mixture of xylylene diisocyanate (XDI) and methylene bis(cyclohexyl isocyanate) (H 12 Use in combination with MDI is also recommended.
[0044] The content ratio of xylylene diisocyanate and hydrogenated xylylene diisocyanate relative to the total amount of polyisocyanate components is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 80% by mass or more. The content ratio of xylylene diisocyanate and hydrogenated xylylene diisocyanate relative to the total amount of polyisocyanate components is, for example, 100% by mass or less, preferably 99% by mass or less, more preferably 95% by mass or less, and even more preferably 90% by mass or less.
[0045] The content of other polyisocyanates (polyisocyanates other than xylylene diisocyanate and hydrogenated xylylene diisocyanate) is, for example, 0% by mass or more, preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, based on the total amount of polyisocyanate components. The content of other polyisocyanates (polyisocyanates other than xylylene diisocyanate and hydrogenated xylylene diisocyanate) is, for example, 50% by mass or less, preferably 40% by mass or less, and more preferably 20% by mass or less, based on the total amount of polyisocyanate components.
[0046] [Active hydrogen group-containing components] The active hydrogen group-containing component is an organic compound containing an active hydrogen group. Examples of the active hydrogen group include a hydroxyl group and an amino group, and a hydroxyl group is preferable.
[0047] The active hydrogen group-containing component contains, for example, a short-chain diol having 2 to 6 carbon atoms, from the viewpoint of reducing oxygen permeability and water vapor permeability. Also, the active hydrogen group-containing component contains, for example, an active hydrogen group-containing compound containing an anionic group and / or an active hydrogen group-containing compound containing a nonionic group, from the viewpoint of improving water dispersibility. Preferably, the active hydrogen group-containing component contains an active hydrogen group-containing compound containing an anionic group, from the viewpoint of improving water dispersibility. That is, the active hydrogen group-containing component preferably contains a short-chain diol having 2 to 6 carbon atoms and an active hydrogen group-containing compound containing an anionic group.
[0048] The short-chain diol having 2 to 6 carbon atoms is an organic compound having 2 to 6 carbon atoms and having two hydroxyl groups in one molecule. Examples of the short-chain diol include an alkane diol having 2 to 6 carbon atoms, an ether diol having 2 to 6 carbon atoms, and an alkene diol having 2 to 6 carbon atoms. Examples of the alkane diol having 2 to 6 carbon atoms include ethylene glycol, propylene glycol, 1,3-propane diol, 1,4-butylene glycol, 1,3-butylene glycol, 1,2-butylene glycol, 1,5-pentane diol, 1,6-hexane diol, neopentyl glycol, 3-methyl-1,5-pentane diol, 1,3-cyclohexane diol, and 1,4-cyclohexane diol. Examples of the ether diol having 2 to 6 carbon atoms include diethylene glycol, triethylene glycol, and dipropylene glycol. Examples of alkene diols having 2 to 6 carbon atoms include 1,4-dihydroxy-2-butene. These can be used alone or in combination of two or more. From the viewpoint of gas barrier properties, preferred are alkane diols having 2 to 6 carbon atoms, and more preferred are ethylene glycol.
[0049] The content ratio of the short-chain diol having 2 to 6 carbon atoms is, for example, 10 parts by mass or more, preferably 30 parts by mass or more, and more preferably 50 parts by mass or more, relative to 100 parts by mass of the total amount of the active hydrogen group-containing components. The content ratio of the short-chain diol having 2 to 6 carbon atoms is, for example, 90 parts by mass or less, preferably 80 parts by mass or less, and more preferably 70 parts by mass or less, relative to 100 parts by mass of the total amount of the active hydrogen group-containing components.
[0050] The active hydrogen group-containing compound containing anionic group is an organic compound that has one or more anionic group and two or more active hydrogen groups in one molecule.The anionic group can be, for example, a carboxy group (carboxylic acid group) and a sulfo group (sulfonic acid group), and preferably, a carboxy group.The active hydrogen group can be, for example, a hydroxyl group and an amino group, and preferably, a hydroxyl group.
[0051] As the active hydrogen group-containing compound containing an anionic group, preferably, an active hydrogen group-containing compound containing a carboxy group can be mentioned. That is, the active hydrogen compound containing an anionic group preferably contains an active hydrogen group-containing compound containing a carboxy group, and preferably consists of an active hydrogen group-containing compound containing a carboxy group.
[0052] Examples of the active hydrogen group-containing compound containing a carboxy group include organic compounds having one carboxy group and two or more hydroxyl groups in one molecule, and preferably organic compounds having one carboxy group and two hydroxyl groups in one molecule. Examples of organic compounds having one carboxy group and two hydroxyl groups in one molecule include carboxy group-containing diols. Examples of the carboxy group-containing diols include dihydroxyalkanoic acids. Examples of the dihydroxyalkanoic acids include 2,2-dimethylol acetic acid, 2,2-dimethylol lactic acid, 2,2-dimethylol propionic acid (also known as dimethylol propionic acid), 2,2-dimethylol butanoic acid, 2,2-dimethylol butyric acid, and 2,2-dimethylol valeric acid. These can be used alone or in combination of two or more. From the viewpoint of water dispersibility, 2,2-dimethylol propionic acid is preferable.
[0053] The content of the active hydrogen group-containing compound containing an anionic group is, for example, 10 parts by mass or more, preferably 20 parts by mass or more, based on 100 parts by mass of the total amount of the active hydrogen group-containing components. The content of the active hydrogen group-containing compound containing an anionic group is, for example, 50 parts by mass or less, preferably 40 parts by mass or less, based on 100 parts by mass of the total amount of the active hydrogen group-containing components.
[0054] The active hydrogen group-containing compound containing a nonionic group is an organic compound having one or more nonionic groups and two or more active hydrogen groups in one molecule. Examples of the nonionic group include a polyoxyethylene group having one end blocked. That is, the nonionic group is defined as a polyoxyethylene group having one end blocked with an alkoxy group (e.g., an alkoxy group having 1 to 4 carbon atoms). A polyoxyethylene group having no end blocked and having hydroxyl groups at both ends (i.e., polyoxyethylene glycol) is the above polyol compound, and is not included in the active hydrogen group-containing compound containing a nonionic group. Examples of the active hydrogen group include a hydroxyl group and an amino group, and preferably a hydroxyl group.
[0055] More specifically, the active hydrogen group-containing compound containing a nonionic group includes one-end-capped (one-end alkoxy-capped) polyoxyethylene glycol and nonionic side chain-containing polyol, preferably nonionic side chain-containing polyol. The nonionic side chain-containing polyol includes, for example, a nonionic side chain-containing diol. The nonionic side chain-containing diol includes, for example, a one-end alkoxy-capped polyoxyethylene side chain-containing polyol. These active hydrogen group-containing compounds containing a nonionic group are prepared by a known method. The active hydrogen group-containing compounds containing a nonionic group can be used alone or in combination of two or more kinds. The content ratio of the active hydrogen group-containing compound containing a nonionic group is appropriately set according to the purpose and use.
[0056] The active hydrogen group-containing component may further contain other low molecular weight polyols. The other low molecular weight polyols are low molecular weight polyols excluding short chain diols having 2 to 6 carbon atoms and anionic active hydrogen group-containing compounds. Examples of the other low molecular weight polyols include diols having 7 or more carbon atoms and low molecular weight polyols having 3 or more valences.
[0057] The diol having 7 or more carbon atoms is an organic compound having 7 or more carbon atoms and having two hydroxyl groups in one molecule. Examples of the diol having 7 or more carbon atoms include alkanediols having 7 to 20 carbon atoms, 2,6-dimethyl-1-octene-3,8-diol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, hydrogenated bisphenol A, and bisphenol A. These can be used alone or in combination of two or more kinds.
[0058] The trihydric or higher low molecular weight polyol has three or more hydroxyl groups in the molecule and is a relatively low molecular weight organic compound. The relatively low molecular weight indicates a molecular weight of 50 or more and 650 or less. When the low molecular weight polyol has a molecular weight distribution, the molecular weight indicates a number average molecular weight in terms of polystyrene measured by GPC measurement. Examples of the trihydric or higher low molecular weight polyol include trihydric alcohol, tetrahydric alcohol, pentahydric alcohol, hexahydric alcohol, heptahydric alcohol, and octahydric alcohol. Examples of the trihydric or higher low molecular weight polyol include trihydric alcohol and tetrahydric alcohol. Examples of the trihydric alcohol include glycerin, 2-methyl-2-hydroxymethyl-1,3-propanediol, 2,4-dihydroxy-3-hydroxymethylpentane, 1,2,6-hexanetriol, trimethylolpropane, and 2,2-bis(hydroxymethyl)-3-butanol. Examples of the tetrahydric alcohol include tetramethylolmethane (pentaerythritol) and diglycerin. These can be used alone or in combination of two or more types.
[0059] As the other low molecular weight polyol, preferably, a low molecular weight polyol having a valence of three or more is used, more preferably, a trihydric alcohol is used, and further preferably, trimethylolpropane is used.
[0060] The content ratio of the other low molecular weight polyol is, for example, 0 parts by mass or more, preferably 1 part by mass or more, more preferably 2 parts by mass or more, relative to 100 parts by mass of the total amount of the active hydrogen group-containing components. The content ratio of the other low molecular weight polyol is, for example, 20 parts by mass or less, preferably 10 parts by mass or less, more preferably 8 parts by mass or less, relative to 100 parts by mass of the total amount of the active hydrogen group-containing components.
[0061] In addition, the content ratio of the short chain diol having 2 to 6 carbon atoms relative to 100 parts by mass of the total amount of the short chain diol having 2 to 6 carbon atoms and the other low molecular weight polyol is, for example, 80 parts by mass or more, preferably 85 parts by mass or more, more preferably 90 parts by mass or more. In addition, the content ratio of the short chain diol having 2 to 6 carbon atoms relative to 100 parts by mass of the total amount of the short chain diol having 2 to 6 carbon atoms and the other low molecular weight polyol is, for example, 98 parts by mass or less, preferably 95 parts by mass or less. In addition, the content ratio of the other low molecular weight polyol relative to 100 parts by mass of the short chain diol having 2 to 6 carbon atoms and the other low molecular weight polyol is, for example, 2 parts by mass or more, preferably 5 parts by mass or more. In addition, the content ratio of the other low molecular weight polyol relative to 100 parts by mass of the total amount of the short chain diol having 2 to 6 carbon atoms and the other low molecular weight polyol is, for example, 20 parts by mass or less, preferably 15 parts by mass or less, more preferably 10 parts by mass or less.
[0062] Furthermore, the active hydrogen group-containing component can further contain a high molecular weight polyol. The high molecular weight polyol has two or more hydroxyl groups in the molecule and is a relatively high molecular weight organic compound (polymer). The number average molecular weight of the high molecular weight polyol is, for example, more than 650 and, for example, 20,000 or less. The number average molecular weight indicates the number average molecular weight in terms of polystyrene measured by GPC. Examples of the high molecular weight polyol include polyether polyol, polyester polyol, polycarbonate polyol, polyurethane polyol, epoxy polyol, vegetable oil polyol, polyolefin polyol, acrylic polyol, and vinyl monomer modified polyol. These are used alone or in combination of two or more kinds. From the viewpoint of gas barrier properties, preferably, the active hydrogen group-containing component does not contain a high molecular weight polyol.
[0063] The active hydrogen group-containing component preferably comprises a short-chain diol having 2 to 6 carbon atoms and an active hydrogen group-containing compound containing an anionic group, or comprises a short-chain diol having 2 to 6 carbon atoms, an active hydrogen group-containing compound containing an anionic group, and a low-molecular-weight polyol having a valence of 3 or more.The active hydrogen group-containing component more preferably comprises a short-chain diol having 2 to 6 carbon atoms, an active hydrogen group-containing compound containing an anionic group, and a low-molecular-weight polyol having a valence of 3 or more.
[0064] The method for synthesizing the isocyanate-terminated prepolymer is not particularly limited. For example, the above-mentioned components are mixed in a predetermined equivalent ratio and reacted.
[0065] More specifically, the equivalent ratio (isocyanate group / active hydrogen group) of the isocyanate group in the polyisocyanate component to the active hydrogen groups (hydroxyl group and amino group) in the active hydrogen group-containing component is, for example, more than 1, and preferably 1.1 or more. In addition, the equivalent ratio (isocyanate group / active hydrogen group) of the isocyanate group in the polyisocyanate component to the active hydrogen groups (hydroxyl group and amino group) in the active hydrogen group-containing component is, for example, 20 or less, and preferably 10 or less.
[0066] [Isocyanate-terminated prepolymer] In the synthesis of the isocyanate group-terminated prepolymer, a known polymerization method is adopted. Examples of the polymerization method include bulk polymerization and solution polymerization. From the viewpoint of adjusting the reactivity, the polymerization method is preferably solution polymerization. In the bulk polymerization, for example, the above components are mixed and reacted under a nitrogen atmosphere. The reaction temperature is, for example, 75 to 85°C. The reaction time is, for example, 1 to 20 hours. In the solution polymerization, for example, the above components are mixed and reacted in an organic solvent under a nitrogen atmosphere. The reaction temperature is, for example, 20 to 80°C. The reaction time is, for example, 1 to 20 hours. Examples of the organic solvent include solvents that are inactive to isocyanate groups. Examples of the organic solvent include acetone, methyl ethyl ketone, ethyl acetate, tetrahydrofuran, and acetonitrile. These can be used alone or in combination of two or more. In addition, in the above polymerization, a catalyst can be added as necessary. Examples of the catalyst include amine catalysts and organometallic catalysts. These can be used alone or in combination of two or more. The amount of catalyst added is appropriately determined depending on the purpose and application.
[0067] In the synthesis of the isocyanate-terminated prepolymer, the polymerization is continued until the isocyanate group concentration of the reaction product liquid reaches a predetermined isocyanate group concentration of the isocyanate group-terminated prepolymer. Thereafter, if necessary, the unreacted polyisocyanate component is removed from the reaction product liquid by a known removal method. Examples of the removal method include distillation and extraction. As a result, the isocyanate-terminated prepolymer is obtained.
[0068] The isocyanate group concentration of the isocyanate group-terminated prepolymer is, for example, 4 mass% or more, preferably 5 mass% or more, more preferably 6 mass% or more.The isocyanate group concentration of the isocyanate group-terminated prepolymer is, for example, 25 mass% or less, preferably 20 mass% or less, more preferably 17 mass% or less, and even more preferably 15 mass% or less.
[0069] The average number of isocyanate groups in the isocyanate-terminated prepolymer is, for example, 1.5 or more, preferably 1.9 or more, more preferably 2.0 or more. The average number of isocyanate groups in the isocyanate-terminated prepolymer is, for example, 3.0 or less, preferably 2.5 or less.
[0070] When the above-mentioned isocyanate-terminated prepolymer has an anionic group derived from an active hydrogen compound containing an anionic group, the isocyanate-terminated prepolymer is neutralized with a neutralizing agent to form a salt of the anionic group.
[0071] The neutralizing agent may be a conventional base. Specific examples of the base include organic bases and inorganic bases. The base refers to a Lewis base. The organic base is a Lewis base containing an organic component. Examples of the organic base include tertiary amines and secondary amines. Examples of the tertiary amine include trialkylamines and alkanolamines. Examples of the trialkylamine include trialkylamines having 1 to 4 carbon atoms. Examples of such trialkylamines include trimethylamine and triethylamine. Examples of the alkanolamine include dimethylethanolamine, methyldiethanolamine, triethanolamine, and triisopropanolamine. Examples of the secondary amine include heterocyclic amines. Examples of the heterocyclic amine include morpholine. These organic bases may be used alone or in combination of two or more. The inorganic base is a Lewis base consisting of an inorganic component. Examples of the inorganic base include ammonia, alkali metal hydroxides, alkaline earth metal hydroxides, alkali metal carbonates, alkali metal hydrogencarbonates, and alkaline earth metal carbonates. Examples of alkali metal hydroxides include lithium hydroxide, sodium hydroxide, and potassium hydroxide. Examples of alkaline earth metal hydroxides include magnesium hydroxide and calcium hydroxide. Examples of alkali metal carbonates include sodium carbonate and potassium carbonate. Examples of alkali metal hydrogen carbonates include sodium hydrogen carbonate and potassium hydrogen carbonate. Examples of alkaline earth metal carbonates include magnesium carbonate and calcium carbonate. These inorganic bases can be used alone or in combination of two or more. These neutralizing agents can be used alone or in combination of two or more. As the neutralizing agent, preferably, an organic base can be used, more preferably, a tertiary amine can be used, even more preferably, a trialkylamine can be used, and particularly preferably, triethylamine (TEA) can be used.
[0072] The amount of the neutralizing agent added is, for example, 0.4 equivalents or more, preferably 0.6 equivalents or more, relative to 1 equivalent of the anionic group. The amount of the neutralizing agent added is, for example, 1.2 equivalents or less, preferably 1.0 equivalents or less, relative to 1 equivalent of the anionic group.
[0073] Next, in this method, the isocyanate-terminated prepolymer (primary reaction product) is reacted with a chain extender to obtain a gas-barrier polyurethane resin (secondary reaction product). For example, the isocyanate-terminated prepolymer is reacted with a chain extender in water to produce a gas-barrier polyurethane resin that is dispersed in water.
[0074] [Chain extender] The chain extender is an organic compound that causes a chain extension reaction of the isocyanate-terminated prepolymer and has a plurality of active hydrogen groups.
[0075] Examples of chain extenders include polyamines and amino alcohols. Examples of polyamines include aromatic polyamines, araliphatic polyamines, alicyclic polyamines, aliphatic polyamines, and polyoxyethylene group-containing polyamines. Examples of aromatic polyamines include 4,4'-diphenylmethanediamine and tolylenediamine. Examples of araliphatic polyamines include 1,3-xylylenediamine and 1,4-xylylenediamine. Examples of alicyclic polyamines include 3-aminomethyl-3,5,5-trimethylcyclohexylamine (also known as isophoronediamine), 4,4'-dicyclohexylmethanediamine, 2,5-bis(aminomethyl)bicyclo[2.2.1]heptane, 2,6-bis(aminomethyl)bicyclo[2.2.1]heptane, 1,4-cyclohexanediamine, 1-amino-3-aminomethyl-3,5,5-trimethylcyclohexane, bis-(4-aminocyclohexyl)methane, diaminocyclohexane, 3,9-bis(3-aminopropyl)-2,4,8,10-tetraoxaspiro[5,5]undecane, 1,3-bis(aminomethyl)cyclohexane, and 1,4-bis(aminomethyl)cyclohexane. Examples of aliphatic polyamines include ethylenediamine, propylenediamine, 1,3-propanediamine, 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexamethylenediamine, hydrazine, hydrazine hydrate, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, 1,2-diaminoethane, 1,2-diaminopropane, and 1,3-diaminopentane. Examples of polyoxyethylene group-containing polyamines include polyoxyalkylene ether diamines. Examples of polyoxyalkylene ether diamines include polyoxyethylene ether diamines. Examples of amino alcohols include 2-((2-aminoethyl)amino)ethanol and 2-((2-aminoethyl)amino)-1-methylpropanol.
[0076] In addition, the chain extender may be, for example, an alkoxysilyl compound having a primary amino group. In addition, the chain extender may be, for example, an alkoxysilyl compound having a primary amino group, such as γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, and N-phenyl-γ-aminopropyltrimethoxysilane. In addition, the chain extender may be, for example, an alkoxysilyl compound having a primary amino group and a secondary amino group. In addition, the chain extender may be, for example, an alkoxysilyl compound having a primary amino group and a secondary amino group, such as N-β(aminoethyl)γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropyltriethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane, and N-β(aminoethyl)γ-aminopropylmethyldiethoxysilane.
[0077] The chain extender may be used alone or in combination of two or more kinds. As the chain extender, preferred is amino alcohol, more preferred is 2-((2-aminoethyl)amino)ethanol.
[0078] The method of reacting the isocyanate-terminated prepolymer with the chain extender in water is not particularly limited. For example, first, the isocyanate-terminated prepolymer is dispersed in water. Next, the chain extender is added to the water in which the isocyanate-terminated prepolymer is dispersed, and the isocyanate-terminated prepolymer is chain-extended in water. The method of dispersing the isocyanate-terminated prepolymer in water is not particularly limited. For example, the isocyanate-terminated prepolymer is added to water while stirring the water. In this case, the amount of water is 100 to 1000 parts by mass per 100 parts by mass of the isocyanate-terminated prepolymer. Then, the chain extender is dropped into the water in which the isocyanate-terminated prepolymer is dispersed while stirring the water. In this case, the equivalent ratio of the active hydrogen group of the chain extender to the isocyanate group of the isocyanate-terminated prepolymer (active hydrogen group / isocyanate group) is, for example, 0.8 to 1.2. The chain extension reaction is completed, for example, at room temperature. The time required for the reaction to be completed is, for example, 0.1 to 10 hours. In this method, the organic solvent and / or water can be removed after the reaction is completed in order to adjust the solid content concentration. In this method, water can be added after the reaction is completed in order to adjust the solid content concentration.
[0079] [Primary aqueous dispersion] A gas-barrier polyurethane resin is obtained by the reaction of the isocyanate-terminated prepolymer with a chain extender. More specifically, a primary aqueous dispersion of the gas-barrier polyurethane resin (hereinafter referred to as a primary polyurethane dispersion, or primary PUD) is obtained by the above-mentioned chain extension reaction in water.
[0080] The primary polyurethane dispersion (primary PUD) is an aqueous dispersion containing a gas barrier polyurethane resin without the additives described below. Even when the gas barrier resin contains other gas barrier resins, the gas barrier resin is preferably prepared as a primary aqueous dispersion.
[0081] The urethane group / urea group concentration of the gas barrier polyurethane resin is, for example, 30% by mass or more, preferably 34% by mass or more, and more preferably 38% by mass or more. The urethane group / urea group concentration of the gas barrier polyurethane resin is, for example, 50% by mass or less, preferably 46% by mass or less, and more preferably 42% by mass or less. The urethane group / urea group concentration of the gas barrier polyurethane resin can be calculated from the charging ratio of the raw material components.
[0082] The solid content concentration of the primary aqueous dispersion is, for example, 10% by mass or more, preferably 15% by mass or more, more preferably 20% by mass or more, and, for example, 60% by mass or less, preferably 50% by mass or less, more preferably 40% by mass or less.
[0083] The pH of the primary aqueous dispersion is, for example, 5 or more, preferably 6 or more. The pH of the primary aqueous dispersion is, for example, 11 or less, preferably 10 or less.
[0084] The average particle size of the primary aqueous dispersion is, for example, 10 nm or more, preferably 20 nm or more, more preferably 50 nm or more, and, for example, 500 nm or less, preferably 300 nm or less, more preferably 200 nm or less.
[0085] (2) Additives [Essential additives] The additive contains, as essential components, a layered inorganic compound and a silane coupling agent. Hereinafter, the layered inorganic compound and the silane coupling agent are collectively referred to as essential additives.
[0086] [Layered inorganic compounds] The layered inorganic compound is a filler that improves the oxygen barrier property of the gas barrier layer (described later).The layered inorganic compound may be, for example, a swellable layered inorganic compound or a non-swellable layered inorganic compound.From the viewpoint of gas barrier property, the layered inorganic compound may preferably be a swellable layered inorganic compound.
[0087] The swellable layered inorganic compound is a clay mineral consisting of extremely thin unit crystals. The swellable layered inorganic compound has the property of swelling by coordinating and / or absorbing a solvent between the unit crystal layers. The swellable layered inorganic compound may be a natural clay mineral, or may be a synthetic clay mineral. Examples of the swellable layered inorganic compound include hydrated silicates, kaolinite clay minerals, antigorite clay minerals, smectite clay minerals, vermiculite clay minerals, and mica clay minerals. Examples of the hydrated silicates include phyllosilicate minerals. Examples of the kaolinite clay minerals include halloysite, kaolinite, endelite, dickite, and nacrite. Examples of the antigorite clay minerals include antigorite and chrysotile. Examples of the smectite clay minerals include montmorillonite, beidellite, nontronite, saponite, hectorite, sauconite, and stevensite. Examples of vermiculite clay minerals include vermiculite. Examples of mica clay minerals include mica, margarite, tetrasilylic mica, taeniolite, and synthetic mica. These can be used alone or in combination of two or more. Examples of swellable layered inorganic compounds include preferably smectite clay minerals, mica clay minerals, and synthetic mica, and more preferably synthetic mica.
[0088] The average particle size of the layered inorganic compound is, for example, 50 nm or more, preferably 100 nm or more.The average particle size of the layered inorganic compound is, for example, 10 μm or less, preferably 5 μm or less, more preferably 3 μm or less.
[0089] The aspect ratio of the layered inorganic compound is, for example, 50 or more, preferably 100 or more, more preferably 200 or more. The aspect ratio of the layered inorganic compound is, for example, 5000 or less, preferably 3000 or less, more preferably 2000 or less.
[0090] The layered inorganic compound may be used as 100% solid content, or may be used as a dispersion liquid in which the layered inorganic compound is dispersed in a solvent. Preferably, the layered inorganic compound is used as a dispersion liquid in which the layered inorganic compound is dispersed in a solvent. The type of the solvent is not particularly limited, and is appropriately set according to the purpose and use. The solid content concentration of the dispersion is not particularly limited, and is appropriately set according to the purpose and use.
[0091] [Silane coupling agents] The silane coupling agent is a crosslinking agent that crosslinks the gas barrier resin and the layered inorganic compound. As the silane coupling agent, for example, a silane coupling agent that can react with the gas barrier resin and the layered inorganic compound is selected.
[0092] More specifically, the silane coupling agent preferably contains a reactive group capable of reacting with a substituent carried by the gas-barrier polyurethane resin.
[0093] For example, the gas barrier polyurethane resin contains an anionic group derived from an active hydrogen compound containing an anionic group. Preferably, the gas barrier polyurethane resin contains a carboxy group derived from an active hydrogen group-containing compound containing a carboxy group.
[0094] Therefore, the silane coupling agent preferably contains a reactive group capable of reacting with an anionic group, more preferably contains a reactive group capable of reacting with a carboxy group. More specifically, the reactive group may be an epoxy group.
[0095] In the gas-barrier polyurethane resin, the anionic group is neutralized by the neutralizing agent. However, the neutralizing agent is eliminated by heating as described below. Therefore, the gas-barrier polyurethane resin contains free anionic groups by heating as described below. Therefore, the silane coupling agent preferably contains a reactive group. More specifically, the silane coupling agent preferably contains an epoxy group that can react with the carboxy group of the gas-barrier polyurethane resin.
[0096] Moreover, the silane coupling agent usually contains an alkoxysilyl group. The alkoxysilyl group is hydrolyzed to generate a silanol group. On the other hand, the layered inorganic compound contains, for example, a hydroxyl group on the surface. The silanol group of the silane coupling agent and the hydroxyl group of the layered inorganic compound can be condensed (silanol condensation). In other words, the silane coupling agent contains an alkoxysilyl group that can react with the layered inorganic compound.
[0097] More specifically, such a silane coupling agent includes an epoxy group-containing silane coupling agent. An example of the epoxy group-containing silane coupling agent is a trialkoxysilane compound containing an epoxy group. An example of the trialkoxysilane compound containing an epoxy group is 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane. In addition, the epoxy group-containing silane coupling agent is available as a commercial product. Examples of commercially available products include trade names KBM-403 (glycidoxypropyltrimethoxysilane), KBE-403 (3-glycidoxypropyltriethoxysilane), KBM-402 (3-glycidoxypropylmethyldimethoxysilane), KBE-402 (3-glycidoxypropylmethyldiethoxysilane), and KBM-303 (2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane) (all manufactured by Shin-Etsu Chemical Co., Ltd.). These can be used alone or in combination of two or more kinds.
[0098] The epoxy equivalent of the epoxy group-containing silane coupling agent is, for example, 100 g / eq or more, preferably 200 g / eq or more. The epoxy equivalent of the epoxy group-containing silane coupling agent is, for example, 1000 g / eq or less, preferably 500 g / eq or less.
[0099] [Optional Additives] In addition to the above essential additives (layered inorganic compound and silane coupling agent), the additives may contain other additives (hereinafter, optional additives). Examples of optional additives include heat stabilizers, antioxidants, light stabilizers, ultraviolet absorbers, thickening inhibitors, curing agents, plasticizers, antistatic agents, lubricants, antiblocking agents, pigments, dyes, and crystal nucleating agents. These may be used alone or in combination of two or more kinds. The amount and timing of addition of the optional additives are appropriately set according to the type of optional additive.
[0100] (3) Secondary aqueous dispersion In the secondary aqueous dispersion, the content ratio of the gas barrier resin and the additive is appropriately set depending on the oxygen permeability, water vapor permeability and flex resistance of the laminate.
[0101] For example, the content of the gas barrier resin based on the solid content (dry mass basis) is, for example, 40 mass% or more, preferably 50 mass% or more, more preferably 60 mass% or more, and even more preferably 65 mass% or more, based on the total amount of the gas barrier resin, the layered inorganic compound, and the silane coupling agent. The content of the gas barrier resin is, for example, 90 mass% or less, preferably 85 mass% or less, more preferably 80 mass% or less, and even more preferably 75 mass% or less, based on the total amount of the gas barrier resin, the layered inorganic compound, and the silane coupling agent.
[0102] In addition, the content ratio of the layered inorganic compound based on solid content (dry mass basis) is, for example, 1 mass% or more, preferably 5 mass% or more, more preferably 10 mass% or more, and even more preferably 15 mass% or more, based on the total amount of the gas barrier resin, the layered inorganic compound, and the silane coupling agent. In addition, the content ratio of the layered inorganic compound is, for example, 40 mass% or less, preferably 30 mass% or less, more preferably 25 mass% or less, and even more preferably 20 mass% or less, based on the total amount of the gas barrier resin, the layered inorganic compound, and the silane coupling agent.
[0103] In addition, the content ratio of the silane coupling agent is, for example, 0.1% by mass or more, preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, based on the solid content (based on dry mass), based on the total amount of the gas barrier resin, the layered inorganic compound, and the silane coupling agent. In addition, the content ratio of the silane coupling agent is, for example, 40% by mass or less, preferably 30% by mass or less, more preferably 25% by mass or less, and even more preferably 20% by mass or less, based on the total amount of the gas barrier resin, the layered inorganic compound, and the silane coupling agent.
[0104] In the gas barrier coating material, the ratio of the silane coupling agent to the layered inorganic compound is adjusted to a predetermined range from the viewpoint of improving the oxygen barrier property and water vapor barrier property of the laminate.
[0105] More specifically, the content of silane coupling agent is 0.03 parts by mass or more, preferably 0.3 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 0.7 parts by mass or more, and particularly preferably 0.8 parts by mass or more, relative to 1 part by mass of the content of layered inorganic compound.Furthermore, the content of silane coupling agent is 2.7 parts by mass or less, preferably 2.5 parts by mass or less, more preferably 2.0 parts by mass or less, even more preferably 1.5 parts by mass or less, and particularly preferably 1.1 parts by mass or less, relative to 1 part by mass of the content of layered inorganic compound.
[0106] The content of the gas barrier resin is, for example, 1 part by mass or more, preferably 2 parts by mass or more, more preferably 3 parts by mass or more, even more preferably 4 parts by mass or more, and particularly preferably 4.5 parts by mass or more, relative to 1 part by mass of the layered inorganic compound. The content of the gas barrier resin is, for example, 20 parts by mass or less, preferably 15 parts by mass or less, more preferably 10 parts by mass or less, even more preferably 8 parts by mass or less, and particularly preferably 5 parts by mass or less, relative to 1 part by mass of the layered inorganic compound.
[0107] Furthermore, when the gas barrier polyurethane resin contains a carboxy group and the silane coupling agent contains an epoxy group, the equivalent ratio of the epoxy group to the carboxy group (epoxy group / carboxy group) is preferably adjusted from the viewpoint of improving the oxygen barrier property and water vapor barrier property of the laminate.
[0108] For example, the equivalent ratio of the epoxy group of the silane coupling agent to the carboxy group of the gas-barrier polyurethane resin (epoxy group / carboxy group) is, for example, 0.5 or more, preferably 0.8 or more. Also, the equivalent ratio of the epoxy group of the silane coupling agent to the carboxy group of the gas-barrier polyurethane resin (epoxy group / carboxy group) is, for example, 2.0 or less, preferably 1.5 or less.
[0109] The method of mixing the gas barrier resin and the additive is not particularly limited. For example, first, a dispersion of the additive (layered inorganic compound and silane coupling agent) is prepared. The dispersion of the additive (layered inorganic compound and silane coupling agent) is not particularly limited and is prepared by a known method. For example, the additive (layered inorganic compound and silane coupling agent) is added to water, and mixed and stirred. This results in a dispersion of the additive (layered inorganic compound and silane coupling agent). The solid content concentration of the dispersion of the additive is appropriately set.
[0110] Next, the dispersion of the additives and the above-mentioned primary aqueous dispersion are mixed to obtain an aqueous dispersion (secondary aqueous dispersion) containing the gas barrier resin and the essential additives.
[0111] For example, when the gas barrier resin is a gas barrier polyurethane resin, the above method produces a polyurethane dispersion containing the gas barrier polyurethane resin and essential additives (secondary polyurethane dispersion, secondary PUD).
[0112] The secondary aqueous dispersion is preferably used as a gas barrier coating material. In other words, the gas barrier coating material is preferably composed of the secondary aqueous dispersion.
[0113] In order to adjust the solids concentration of the gas barrier coating material, water can be removed from the secondary aqueous dispersion by a known method. In addition, in this method, water can be added to the secondary aqueous dispersion in order to adjust the solids concentration of the gas barrier coating material.
[0114] The solid content concentration of the gas barrier coating material is, for example, 10% by mass or more, preferably 15% by mass or more, more preferably 20% by mass or more, and, for example, 60% by mass or less, preferably 50% by mass or less, more preferably 40% by mass or less.
[0115] The gas barrier coating material contains a gas barrier resin. Therefore, the gas barrier coating material can form a coating layer (gas barrier layer) having excellent gas barrier properties. Therefore, the gas barrier coating material is preferably used as a gas barrier coating material for paper substrates.
[0116] 2. Laminate and manufacturing method thereof (1) Laminate In FIG. 1, the laminate 1 includes a substrate 2 and a gas barrier layer 4 disposed on at least one side of the substrate 2 in the thickness direction (the upper side of the paper).
[0117] Moreover, the laminate 1 may further include, as an optional layer, a filling layer 3 interposed between the substrate 2 and the gas barrier layer 4. In FIG.
[0118] The laminate 1 may further include, as an optional layer, a heat seal layer 5 disposed on at least one side in the thickness direction (the upper side of the paper surface) of the gas barrier layer 4. In FIG.
[0119] 1, the laminate 1 includes a base material 2, a sealing layer 3, a gas barrier layer 4, and a heat seal layer 5, which are arranged in this order from the other side (lower side of the paper) to one side (upper side of the paper) in the thickness direction. A method for producing the laminate 1 will be described in detail below.
[0120] (2) Manufacturing method of laminate [Base material preparation process] In this method, first, a substrate 2 is prepared (substrate preparation step). The substrate 2 is not particularly limited, and examples thereof include a plastic substrate, a fiber substrate, a metal substrate, and a ceramic substrate. These may be used alone or in combination of two or more types. As the substrate 2, a plastic substrate and a fiber substrate are preferably used.
[0121] The plastic substrate is, for example, a film made of plastic. Examples of plastic include thermoplastic resins and thermosetting resins, and preferably include thermoplastic resins. Examples of thermoplastic resins include polyolefin resins, polyester resins, polyamide resins, polyvinyl resins, acrylic resins, polycarbonate resins, and cellulose resins. These can be used alone or in combination of two or more. Examples of thermoplastic resins include polyolefin resins and polyester resins. Examples of plastic substrates include non-stretched substrates, uniaxially stretched substrates, and biaxially stretched substrates, and preferably include biaxially stretched substrates. Examples of fiber substrates include paper substrates, cloth substrates, and wood substrates. These can be used alone or in combination of two or more.
[0122] The substrate 2 may be a single layer or a multi-layer. The substrate 2 may be surface-treated. Examples of the surface treatment include deposition treatment, corona discharge treatment, and anchor coat treatment. The shape of the substrate 2 may be, for example, a sheet shape, a bottle shape, or a cup shape.
[0123] The substrate 2 is preferably a fiber substrate, more preferably a paper substrate. The paper substrate is a substrate formed from paper. The paper substrate is, for example, paper made from pulp. The pulp is, for example, natural pulp and synthetic pulp. More specifically, the paper substrate is, for example, glassine paper, coated paper, one-sided gloss kraft paper, roll paper, and cup base paper. The substrate 2 may be a single-layer paper or may be a multi-layer paper. The paper substrate is appropriately selected depending on the application of the laminate 1.
[0124] The thickness of the substrate 2 is, for example, 1 μm or more, or preferably 3 μm or more. The thickness of the substrate 2 is, for example, 500 μm or less, or preferably 200 μm or less.
[0125] In addition, when the base material 2 is a paper base material, the basis weight of the paper base material is, for example, 20 g / m 2 More than 30 g / m 2 The basis weight of the paper base material is, for example, 400 g / m 2 Preferably, 300 g / m or less 2 The following is the result.
[0126] [Sealing layer formation process] Next, in this method, the filling layer 3 is formed on at least one surface of the base material 2 (filling layer forming step). More specifically, the filling layer 3 is formed before the coating step described later.
[0127] The filling layer 3 is laminated on the substrate 2 (preferably a paper substrate) in order to suppress impregnation of the gas barrier coating material into the substrate 2. The filling layer 3 is also laminated on the substrate 2 in order to absorb irregularities on the surface of the substrate 2 and smooth the surface. The filling layer 3 is disposed on at least one surface of the substrate 2. The filling layer 3 may be disposed on both surfaces of the substrate 2. The filling layer 3 is preferably disposed only on one surface of the substrate 2.
[0128] The filling layer 3 contains, for example, a filling resin. More specifically, the filling layer 3 is formed, for example, by applying a coating material containing a filling resin (hereinafter, a filling coating material) to the surface of the base material 2 and drying it.
[0129] The filler coating material is not particularly limited, and examples thereof include coating materials containing known filler resins. More specifically, examples of the filler coating material include a solution obtained by dissolving a filler resin in a solvent, and a dispersion obtained by dispersing a filler resin in a solvent.
[0130] The filler resin is a resin that inhibits the impregnation of the gas barrier coating material into the substrate 2. Examples of the filler resin include polyolefin resin, polyester resin, polyamide resin, polyvinyl resin, (meth)acrylic resin, polycarbonate resin, and cellulose resin. These can be used alone or in combination of two or more. Preferred examples of the filler resin include polyolefin resin and (meth)acrylic resin.
[0131] The solvent is not particularly limited, but examples thereof include water, methanol, ethanol, propanol, isopropanol, acetone, methyl ethyl ketone, ethyl acetate, tetrahydrofuran, and acetonitrile. These solvents can be used alone or in combination of two or more kinds.
[0132] More specifically, examples of the filler coating material include a resin dispersion and a resin emulsion containing a filler resin and a solvent.
[0133] The solid content concentration of the filling coating material is, for example, 10 mass% or more, preferably 15 mass% or more, more preferably 20 mass% or more. The solid content concentration of the filling coating material is, for example, 60 mass% or less, preferably 50 mass% or less, more preferably 40 mass% or less.
[0134] The application method of the filler coating material is not particularly limited. Examples of application methods include dip coating, gravure coating, reverse coating, roll coating, bar coating, spray coating, and air knife coating. The drying conditions of the filler coating material are not particularly limited. For example, the drying temperature is, for example, 40° C. or higher, preferably 50° C. or higher. The drying temperature is, for example, 200° C. or lower, preferably 180° C. or lower. The drying time is, for example, 1 second or higher, preferably 30 seconds or higher. The drying time is, for example, 10 minutes or less, preferably 5 minutes or less.
[0135] This forms the filling layer 3. The amount (dry mass) of the filling layer 3 is, for example, 1 g / m 2 More than 3 g / m 2 The amount (dry mass) of the filling layer 3 is, for example, 30 g / m 2 Preferably, 15 g / m or less 2 The following is the result.
[0136] [Gas barrier layer formation process] Next, in this method, the gas barrier layer 4 is formed on at least one surface of the filling layer 3 (gas barrier layer forming step).
[0137] The gas barrier layer 4 is a layer having gas barrier properties. Gas barrier properties are the property of reducing oxygen permeability. More specifically, the gas barrier layer 4 is made of a gas barrier resin having an oxygen permeability of a predetermined value or less. For example, the oxygen permeability of a gas barrier layer 4 having a thickness of 10 μm is, for example, 1 (cc / m) at room temperature. 2 ·day·atm). The oxygen permeability is measured in accordance with JIS K7126 (2006) Method B using an oxygen permeability measuring device (MOCON, OX-TRAN2 / 22H). The measurement conditions are 20°C and 80% RH (relative humidity).
[0138] The gas barrier layer 4 is disposed, for example, on the surface of the filling layer 3 on one side of the substrate 2. That is, the gas barrier layer 4 is disposed on the surface of the filling layer 3 on the side of the substrate 2 on which the filling layer 3 is disposed. The gas barrier layer 4 may be disposed on both sides of the substrate 2 together with the filling layer 3. The gas barrier layer 4 is preferably disposed only on one surface of the substrate 2 together with the filling layer 3.
[0139] The gas barrier layer 4 contains, for example, a cured film of the above-mentioned gas barrier coating material, and is preferably made of a cured film of the gas barrier coating material. More specifically, the gas barrier layer 4 is formed by heating and curing the coating film of the above-mentioned gas barrier coating material.
[0140] To form the gas barrier layer 4, first, a gas barrier coating material is applied to at least one side of the base material 2 (at least one side of the filling layer 3) (application step).
[0141] More specifically, in the coating step, a gas barrier coating material is applied to at least one surface of the filling layer 3 .
[0142] The method for applying the gas barrier coating material is not particularly limited, and examples of the application method include dip coating, gravure coating, reverse coating, roll coating, bar coating, spray coating, and air knife coating.
[0143] In this method, the gas barrier coating material is dried as necessary. The drying conditions are not particularly limited. For example, the drying temperature is, for example, 40° C. or higher, preferably 50° C. or higher. The drying temperature is, for example, 200° C. or lower, preferably 180° C. or lower. The drying time is, for example, 1 second or longer, preferably 30 seconds or longer. The drying time is, for example, 10 minutes or shorter, preferably 5 minutes or shorter.
[0144] This results in a coating film (uncured coating film) of the gas barrier coating material. Next, in this method, the coating film (uncured coating film) of the gas barrier coating material is heated to form a cured film of the gas barrier coating material (curing step).
[0145] More specifically, in the curing step, the coating film of the gas barrier coating material is heated to cause the gas barrier resin and the layered inorganic compound to react with the silane coupling agent.
[0146] The heating conditions are not particularly limited as long as they allow the gas barrier resin and layered inorganic compound to react with the silane coupling agent.
[0147] For example, when the heating temperature is relatively high (e.g., 150°C or higher), the heating time may be relatively short (e.g., less than 10 minutes). In such a case, the heating temperature is, for example, 150°C or higher, preferably 180°C or higher, and more preferably 200°C or higher. The heating temperature is, for example, 300°C or lower, preferably 200°C or lower. The heating time is, for example, 1 second or longer, preferably 10 seconds or longer. The heating time is, for example, less than 10 minutes, preferably 5 minutes or shorter, and more preferably 1 minute or shorter.
[0148] Furthermore, when the heating time is relatively long (e.g., 10 minutes or more), the heating temperature may be relatively low (e.g., less than 150°C). In such a case, the heating temperature is, for example, 60°C or more, preferably 80°C or more, more preferably 100°C or more. The heating temperature is, for example, less than 150°C, preferably 130°C or less. The heating time is, for example, 10 minutes or more, preferably 30 minutes or more, more preferably 1 hour or more. The heating time is, for example, 10 hours or less, preferably 5 hours or less, more preferably 3 hours or less.
[0149] The heating causes the silane coupling agent to react with the gas barrier polyurethane resin and the layered inorganic compound. More specifically, when the gas barrier polyurethane resin contains a carboxy group and the silane coupling agent contains an epoxy group, the heating causes the carboxy group to react with the epoxy group (ester condensation). The heating also causes the hydroxyl group of the layered inorganic compound to react with the alkoxysilyl group of the silane coupling agent (silanol condensation). This causes the silane coupling agent to react with the gas barrier polyurethane resin and the layered inorganic compound, crosslinking them.
[0150] From the viewpoint of gas barrier property and flex resistance, the reaction rate of the silane coupling agent is, for example, 40% by mass or more, preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 80% by mass or more. From the viewpoint of workability, the reaction rate of the silane coupling agent is, for example, 99% by mass or less, preferably 90% by mass or less. The reaction rate of the silane coupling agent is, for example, the disappearance rate of the reactive group (e.g., epoxy group) according to the examples described later.
[0151] Through the above reaction, the coating film of the gas barrier coating material is thermally cured, and a cured film serving as the gas barrier layer 4 is obtained.
[0152] The gas barrier layer 4 is aged as necessary. The aging temperature (curing temperature) is, for example, 20° C. or more, preferably 40° C. or more. The aging temperature (curing temperature) is, for example, 80° C. or less, preferably 60° C. or less. The aging time (curing time) is, for example, 1 hour or more, preferably 10 hours or more. The aging time (curing time) is, for example, 7 days or less, preferably 3 days or less.
[0153] The amount (dry mass) of the gas barrier layer 4 is, for example, 1.0 g / m 2 More than 2.0 g / m 2 More preferably, 2.5 g / m 2The amount (dry mass) of the gas barrier layer 4 is, for example, 10 g / m 2 Preferably, 7 g / m or less 2 The following is the result.
[0154] [Heat seal layer formation process] Next, in this method, if necessary, a heat seal layer 5 can be formed on at least one surface of the gas barrier layer 4 (heat seal layer forming step).
[0155] The heat seal layer 5 is a resin layer having heat sealability. The heat seal layer 5 is disposed on the surface of the gas barrier layer 4. That is, the heat seal layer 5 is disposed on the surface of the gas barrier layer 4 on the side of the base material 2 on which the gas barrier layer 4 is disposed. The heat seal layer 5 may be disposed on both sides of the base material 2 together with the gas barrier layer 4. The heat seal layer 5 is preferably disposed on only one surface of the base material 2 together with the gas barrier layer 4.
[0156] The heat seal layer 5 contains, for example, a heat sealable resin. More specifically, the heat seal layer 5 is formed, for example, by applying a coating material containing a heat sealable resin (hereinafter, referred to as a heat sealable coating material) to the gas barrier layer 4 and drying it.
[0157] The heat-sealable resin is a resin that can be heat-sealed (thermally fused) to each other. The heat-sealable resin is not particularly limited, and a known heat-sealable resin is used. More specifically, the heat-sealable resin may be, for example, a polyolefin resin, an acrylic resin, or a polyurethane resin. These may be used alone or in combination of two or more kinds.
[0158] The heat-sealable resin is prepared, for example, as a solution and / or dispersion in which it is dissolved and / or dispersed in a solvent. For example, the heat-sealable resin is synthesized in a solvent. This results in a solution and / or dispersion of the heat-sealable resin.
[0159] The solvent is not particularly limited, but may be, for example, water, methanol, ethanol, propanol, isopropanol, acetone, methyl ethyl ketone, ethyl acetate, tetrahydrofuran, and acetonitrile. These solvents may be used alone or in combination of two or more. The solid content concentration of the sealing coating material is not particularly limited, and may be appropriately set according to the purpose and application.
[0160] More specifically, the heat-sealable coating material may be a polyolefin dispersion containing a polyolefin resin, an acrylic emulsion containing an acrylic resin, or a polyurethane dispersion containing a polyurethane resin. A preferable example of the heat-sealable coating material is a polyolefin dispersion.
[0161] The heat-sealable coating material may contain additives. That is, the heat-sealable coating material may contain the above-mentioned heat-sealable resin and additives. Examples of additives include heat stabilizers, antioxidants, light stabilizers, ultraviolet absorbers, plasticizers, antistatic agents, lubricants, antiblocking agents, pigments, dyes, crystal nucleating agents, and curing agents. These may be used alone or in combination of two or more.
[0162] The solid content of the heat-sealable coating material is, for example, 10% by mass or more, preferably 15% by mass or more, more preferably 20% by mass or more, and, for example, 60% by mass or less, preferably 50% by mass or less, more preferably 40% by mass or less.
[0163] The application method of the heat-sealable coating material is not particularly limited. Examples of application methods include dip coating, gravure coating, reverse coating, roll coating, bar coating, spray coating, and air knife coating. The drying conditions of the gas barrier coating material are not particularly limited. For example, the drying temperature is, for example, 40° C. or higher, preferably 50° C. or higher. The drying temperature is, for example, 200° C. or lower, preferably 180° C. or lower. The drying time is, for example, 1 second or higher, preferably 30 seconds or higher. The drying time is, for example, 10 minutes or less, preferably 5 minutes or less.
[0164] This forms the heat seal layer 5. The amount (dry mass) of the heat seal layer 5 is set from the viewpoint of achieving both gas barrier properties and heat sealability.
[0165] More specifically, from the viewpoint of heat sealability, the amount (dry mass) of the heat seal layer 5 is, for example, 1.0 g / m 2 More than 1.0 g / m 2 More preferably, 1.1 g / m 2 More preferably, 1.5 g / m 2 More preferably, 1.8 g / m 2 From the viewpoint of gas barrier properties, the amount (dry mass) of the heat seal layer 5 is, for example, 7.0 g / m 2 Less than 5.0 g / m 2 More preferably, less than 4.9 g / m 2 More preferably, 4.0 g / m or less 2 Below, particularly preferably 3.5 g / m 2 The following is the result.
[0166] In this manner, the laminate 1 is manufactured. The laminate 1 has a total thickness of, for example, 5 μm or more, or preferably 10 μm or more. The laminate 1 has a total thickness of, for example, 1 mm or less, or preferably 0.5 mm or less.
[0167] 3. Effects The gas barrier coating material contains a gas barrier resin and an additive. The gas barrier resin contains a gas barrier polyurethane resin. The additive contains a layered inorganic compound and a silane coupling agent in a predetermined ratio. Therefore, the gas barrier coating material can provide a laminate 1 having both a predetermined level of oxygen barrier property and a predetermined level of water vapor barrier property after bending.
[0168] Moreover, the laminate 1 is obtained using the gas barrier coating material, and therefore the laminate has at least a predetermined level of oxygen barrier property and at least a predetermined level of water vapor barrier property after folding.
[0169] Moreover, in the manufacturing method of the laminate 1, the gas barrier coating material is used. Therefore, according to the manufacturing method of the laminate 1, it is possible to obtain a laminate 1 having both a predetermined level of oxygen barrier property and a predetermined level of water vapor barrier property after folding. In particular, according to the manufacturing method of the laminate 1, even if the substrate is a paper substrate, it is possible to obtain a laminate 1 (paper substrate-based laminate) having both a predetermined level of oxygen barrier property and a predetermined level of water vapor barrier property after folding. Therefore, the manufacturing method of the laminate 1 is preferably used in the manufacture of a paper substrate-based laminate.
[0170] 4.Applications The gas barrier coating material, the laminate 1, and the method for producing the laminate 1 are suitable for use in various industrial fields that require oxygen barrier properties, water vapor barrier properties, and flex resistance. More specifically, the laminate 1 is suitable for use as a packaging material. That is, the packaging material preferably contains the laminate 1, and more preferably consists of the laminate 1.
[0171] Such a packaging material contains the laminate 1 described above, and therefore has at least a predetermined level of oxygen barrier property and at least a predetermined level of water vapor barrier property after folding.
[0172] 5. Variations In the laminate 1 described above, the filling layer 3 is interposed between the substrate 2 and the gas barrier layer 4, but the filling layer 3 does not have to be interposed between the substrate 2 and the gas barrier layer 4. For example, depending on the type of the substrate 2 and the type of the gas barrier layer 4, the filling layer 3 may be omitted.
[0173] Furthermore, the laminate 1 may not include the heat seal layer 5 depending on the purpose and use. When the laminate 1 includes the heat seal layer 5, the heat seal layer 5 may be directly laminated on the gas barrier layer 4 as described above. The heat seal layer 5 may be bonded to the gas barrier layer 4 with a known adhesive. That is, an adhesive layer (not shown) may be interposed between the gas barrier layer 4 and the heat seal layer 5. Instead of the heat seal layer 5 or together with the heat seal layer 5, an arbitrary functional layer may be laminated on the gas barrier layer 4. EXAMPLES
[0174] Next, the present invention will be described based on examples and comparative examples, but the present invention is not limited to the following examples. Note that "parts" and "%" are based on mass unless otherwise specified. In addition, the specific numerical values of the blending ratio (content ratio), physical property values, parameters, etc. used in the following description can be replaced with the upper limit value (numerical value defined as "less than or equal to" or "less than") or lower limit value (numerical value defined as "more than or equal to" or "exceeding") of the corresponding blending ratio (content ratio), physical property values, parameters, etc. described in the above "Form for carrying out the invention".
[0175] 1.Paper base material Preparation example 1 The base material was a semi-glossy (bleached) kraft paper (product name: Gintake, made by Nippon Paper Industries, basis weight 67 g / m 2 ) was prepared.
[0176] 2.Sealing coating material Preparation Example 2 (Acrylic Emulsion) A reaction vessel equipped with a stirrer, a reflux condenser, a dropping device, and a thermometer was charged with 2193 parts by mass of ion-exchanged water (solvent) and 2.5 parts by mass of sodium dodecyl sulfate (surfactant). The contents of the reaction vessel were heated to 75° C. while stirring and replacing with nitrogen.
[0177] While maintaining the internal temperature of the reaction vessel at 75° C., 7.5 parts by mass of potassium persulfate (polymerization initiator) was added to the reaction vessel and dissolved in the contents of the reaction vessel. Then, a monomer emulsion prepared in advance was continuously added dropwise to the reaction vessel over a period of 5 hours.
[0178] The monomer emulsion is a raw material composition containing the following components: Ion-exchanged water (solvent) 900 parts by weight Sodium dodecyl sulfate (surfactant) 5 parts by weight Acrylamide (raw material monomer) 25 parts by weight Methyl methacrylate (raw monomer) 175 parts by weight 2-Ethylhexyl acrylate (raw material monomer) 1088 parts by mass Methacrylic acid (raw material monomer) 80 parts by weight Styrene (raw monomer) 1133 parts by mass
[0179] After the dropping of the monomer emulsion was completed, the contents of the reaction vessel were aged for 3 hours. This allowed the raw material monomers to polymerize, yielding a (meth)acrylic resin. Also, an acrylic emulsion in which the (meth)acrylic resin was dispersed in water was obtained.
[0180] The acrylic emulsion was cooled to room temperature, and then ion-exchanged water and ammonia water (neutralizing agent) were added to the acrylic emulsion to adjust the solid content to 41% by mass and the pH to 8.0.
[0181] This resulted in an acrylic emulsion in which the (meth)acrylic resin was dispersed in water. The average particle size of the acrylic emulsion was 140 nm. The average particle size was measured by dynamic light scattering (measurement device FPAR-1000, manufactured by Otsuka Electronics Co., Ltd.) (hereinafter the same).
[0182] Thereafter, water was further added to the above acrylic emulsion (solid content concentration: 41% by mass), and the mixture was mixed for 5 minutes in a mixer to prepare a sealing coating material (solid content concentration: 40% by mass).
[0183] 3. Gas barrier coating material Example 1 (1) Primary PUD The following components were mixed and reacted in a nitrogen atmosphere at 65 to 70° C. until the isocyanate group concentration (NCO%) reached 6.11 mass % or less, thereby obtaining a transparent isocyanate-terminated prepolymer reaction product liquid.
[0184] 1,3-Xylylene Diisocyanate (Takenate 500, 1,3-XDI, manufactured by Mitsui Chemicals) 143.2 parts by mass Methylenebis(cyclohexyl isocyanate) (VestanatH 12 MDI, H 12 MDI, manufactured by Evonik) 25.0 parts by weight Ethylene glycol 29.2 parts by weight Trimethylolpropane 2.7 parts by mass Dimethylolpropionic acid 14.8 parts by mass Methyl ethyl ketone (solvent) 121.6 parts by mass
[0185] Next, the reaction product liquid was cooled to 40° C. Next, 11.0 parts by mass of triethylamine (TEA) was added to the reaction product liquid, thereby neutralizing the isocyanate group-terminated prepolymer.
[0186] Next, the reaction product liquid was dispersed in 838.0 parts by mass of ion-exchanged water using a homodisper. Next, an amine aqueous solution was added to the obtained dispersion liquid to carry out a chain extension reaction. The reaction product liquid of the chain extension reaction was aged for 1 hour. This resulted in a gas barrier polyurethane resin. The amine aqueous solution was a mixed solution of 48.4 parts by mass of ion-exchanged water and 24.2 parts by mass of 2-((2-aminoethyl)amino)ethanol. Then, an evaporator was used to distill off methyl ethyl ketone and ion-exchanged water from the reaction product liquid. This resulted in adjusting the solid content concentration to 30% by mass.
[0187] As a result of the above, a primary polyurethane dispersion (primary PUD) in which the gas barrier polyurethane resin was dispersed in water was obtained.
[0188] The pH of the primary polyurethane dispersion (primary PUD) was 8.6, and the average particle size of the primary polyurethane dispersion (primary PUD) was 58 nm.
[0189] (2) Secondary PUD 57.86 parts by mass of water, 14.02 parts by mass (1.5 parts by mass of solid content) of a dispersion of a swellable layered inorganic compound (product name: NTS-10NC, synthetic mica, manufactured by Topy Industries, solid content concentration 10.7%), and 1.2 parts by mass (1.2 parts by mass of solid content) of an epoxy group-containing silane coupling agent (product name: KBM-403, 3-glycidoxypropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd., epoxy equivalent 236g / eq, solid content concentration 100%) were mixed and mixed in a mixer for 5 minutes. This produced a dispersion of an additive.
[0190] The content of the silane coupling agent per 1 part by mass of the layered inorganic compound was 0.8 parts by mass.
[0191] Next, the additive dispersion was mixed with 24.33 parts by weight (7.3 parts by weight solids) of the primary PUD (30% by weight solids) in a mixer for 5 minutes.
[0192] This resulted in a secondary polyurethane dispersion (secondary PUD) in which the gas barrier polyurethane resin and the additives were dispersed in water. The solid content of the secondary PUD was 10% by mass. The secondary PUD was used as a gas barrier coating material.
[0193] Examples 2 to 9 and Comparative Examples 1 to 2 The compounding recipe was changed so that the mass of the solid content of the layered inorganic compound, the mass of the solid content of the silane coupling agent, and the mass of the solid content of the gas barrier polyurethane resin were in the ratio shown in Table 1. A gas barrier coating material was obtained in the same manner as in Example 1 except for this.
[0194] Comparative Examples 3 to 4 Polyvinyl alcohol resin (product name PVA-217, manufactured by Kuraray, solid content concentration 100%) and water at room temperature were mixed for 30 minutes to obtain a mixed liquid. The mixed liquid was gradually heated and mixed at 90°C for 1 hour to obtain a transparent solution. The transparent solution was allowed to cool to room temperature. As a result, an aqueous polyvinyl alcohol resin solution with a solid content concentration of 10% by mass was obtained.
[0195] Instead of the gas barrier polyurethane resin (primary PUD), a polyvinyl alcohol resin aqueous solution (solid content concentration 10 mass%) was used. In addition, the blending recipe was changed so that the mass of the solid content of the layered inorganic compound, the mass of the solid content of the silane coupling agent, and the mass of the solid content of the gas barrier polyurethane resin were in the ratio shown in Table 1. Other than this, a gas barrier coating material was obtained in the same manner as in Example 1. The solid content concentration of the gas barrier coating material was 7 mass%.
[0196] Comparative Example 5 Instead of the gas barrier polyurethane resin (primary PUD), the above polyvinyl alcohol resin aqueous solution (Comparative Examples 3-4, solid content concentration 10% by mass) was used. Also, instead of the epoxy group-containing silane coupling agent, an amino group-containing silane coupling agent (product name: KBE-903, 3-aminopropyltriethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd., solid content concentration 100%) was used. Also, the compounding recipe was changed so that the mass of the solid content of the layered inorganic compound, the mass of the solid content of the silane coupling agent, and the mass of the solid content of the gas barrier polyurethane resin were in the ratio shown in Table 1. Other than this, a gas barrier coating material was obtained in the same manner as in Example 1. The solid content concentration of the gas barrier coating material was 7% by mass.
[0197] 4.Laminate Example 10 The filling coating material (Preparation Example 1) was applied to the glossy side of a paper substrate (one-sided glossy kraft paper) using a bar coater. 2 The coating amount was adjusted so that the coating film of the filler coating material was then dried at 120° C. for 60 seconds, thereby forming a filler layer.
[0198] Next, the gas barrier coating material of Example 1 was applied to the surface of the filling layer with a bar coater. 2 The coating amount was adjusted so that the coating film of the gas barrier coating material was 120°C. The coating film of the gas barrier coating material was then dried at 120°C for 60 seconds. The coating film of the gas barrier coating material was then heated at 110°C for 1 hour. This caused the layered inorganic compound, the silane coupling agent, and the gas barrier polyurethane resin to react with each other, and the coating film of the gas barrier coating material was thermally cured. As a result, a cured film was formed as a gas barrier layer on the surface of the filling layer. In addition, the cured film was aged at 40°C for 2 days. This resulted in a laminate. The layer structure of the laminate was as follows.
[0199] Paper base material / Sealing layer / Gas barrier layer
[0200] The dry mass of the filling layer was calculated by subtracting the mass of the paper substrate from the total mass of the laminate (two layers) including the paper substrate and the filling layer.
[0201] In addition, the dry mass of the gas barrier layer was calculated by subtracting the total mass of the laminate (2 layers) comprising the paper substrate and the filling layer from the total mass of the laminate (3 layers) comprising the paper substrate, the filling layer and the gas barrier layer.
[0202] Examples 11 to 18 and Comparative Examples 6 to 10 Gas barrier coating materials were used in the combinations shown in Table 1. Except for this, a laminate was obtained in the same manner as in Example 10.
[0203] Example 19 As shown in Table 2, the coating film of the gas barrier coating material was heated at 200° C. for 30 seconds instead of at 110° C. for 1 hour. Except for this, a laminate was obtained in the same manner as in Example 11.
[0204] Example 20 As shown in Table 2, the coating film of the gas barrier coating material was heated at 200° C. for 1 minute instead of at 110° C. for 1 hour. Except for this, a laminate was obtained in the same manner as in Example 11.
[0205] 5. Evaluation (1) Oxygen transmission rate (OTR) of laminate Oxygen permeability of laminate before folding (cc / m 2 The oxygen permeability (°C) was measured using an oxygen permeability measuring device (MOCON, OX-TRAN 2 / 22H). The measurement temperature was 20°C. The relative humidity was 80%.
[0206] At 25°C, the laminate was heated at 2 kg / cm with the coated surface (sealing layer and gas barrier layer) facing inwards. 2 The laminate was folded again at a pressure of 2 kg / cm for 10 seconds. The folding direction was changed by 90° so that a cross crease was formed, and the laminate was folded again at a pressure of 2 kg / cm. 2 The sheet was folded at a pressure of 0.01 mm for 10 seconds.
[0207] The oxygen permeability (cc / m 2 The results are shown in Tables 1 and 2.
[0208] (2) Water vapor transmission rate (WVTR) of laminate Water vapor permeability of the laminate before folding (g / m 2 ·day) was measured using a water vapor transmission rate measuring device (MOCON, PARMATRAN-W 3 / 34 G). The measurement temperature was 40°C. The relative humidity was 90% RH.
[0209] At 25°C, the laminate was laminated with a pressure of 2 kg / cm2 so that the coated surface (the sealing layer and the gas barrier layer) was on the inside. 2 The laminate was folded again at a pressure of 2 kg / cm for 10 seconds. The folding direction was changed by 90° so that a cross crease was formed, and the laminate was folded again at a pressure of 2 kg / cm. 2 The sheet was folded at a pressure of 0.01 mm for 10 seconds.
[0210] The water vapor permeability (g / m 2 ·day) was measured under the above conditions. The results are shown in Tables 1 and 2.
[0211] (3) Reaction rate of silane coupling agent A laminate was obtained in the same manner as in Example 11, except that the coating film of the gas barrier coating material was not heated at 110° C. for 1 hour. The obtained laminate was used as a sample (control) of a laminate in which the silane coupling agent was not reacted.
[0212] The infrared spectrum of the gas barrier layer of the above sample was measured using a Fourier transform infrared spectrophotometer (FT / IR-4700). -1 The height (A1) of the peak (corresponding to the disubstituted aromatic ring) at 910 cm -1 The IR peak ratio (A2 / A1) of the height (A2) of the peak (peak corresponding to the epoxy group) was calculated.
[0213] The infrared spectrum of the gas barrier layer of the laminate of Example 11, Example 19 and Example 20 was measured in the same manner as above. -1 The height of the peak (A1) at 910 cm -1 The IR peak ratio (A2 / A1) of the peak height (A2) was calculated.
[0214] The IR peak ratio (A2 / A1) of the control was determined to indicate a state in which the reaction rate of the silane coupling agent was 0% and the remaining rate of the epoxy groups was 100%.
[0215] Moreover, when the reaction rate of the silane coupling agent is 100% and the residual rate of the epoxy groups is 0%, it was determined that the IR peak ratio (A2 / A1) was 0.
[0216] The reduction rate of the IR peak ratio (A2 / A1) of each example relative to the IR peak ratio (A2 / A1) of the control was calculated as the reaction rate of the silane coupling agent. The results are shown in Table 2.
[0217] [Table 1]
[0218] [Table 2] [Explanation of symbols]
[0219] 1. Laminate 2 Base material 3. Filling layer 4 Gas barrier layer 5 Heat seal layer
Claims
1. A gas barrier coating material containing a gas barrier resin and an additive, The gas barrier resin contains a gas barrier polyurethane resin, The additive contains a layered inorganic compound and a silane coupling agent, The gas barrier coating material has a content of the silane coupling agent of 0.03 parts by mass or more and 2.7 parts by mass or less relative to 1 part by mass of the layered inorganic compound.
2. The gas barrier polyurethane resin is Contains a reaction product of an isocyanate-terminated prepolymer and a chain extender, The isocyanate-terminated prepolymer contains a reaction product of a polyisocyanate component and an active hydrogen group-containing component, The polyisocyanate component contains xylylene diisocyanate and / or hydrogenated xylylene diisocyanate, 2. The gas barrier coating material according to claim 1, wherein the active hydrogen group-containing component comprises a short-chain diol having 2 to 6 carbon atoms and an active hydrogen compound containing an anionic group.
3. The active hydrogen compound containing an anionic group contains an active hydrogen group-containing compound containing a carboxy group, The silane coupling agent is an epoxy group capable of reacting with the carboxy group; An alkoxysilyl group capable of reacting with the layered inorganic compound; The gas barrier coating material according to claim 2 , comprising:
4. 4. The gas barrier coating material according to claim 3, wherein the content of the silane coupling agent relative to 1 part by mass of the layered inorganic compound is 0.3 parts by mass or more and 1.1 parts by mass or less.
5. A substrate and a gas barrier layer disposed on at least one side of the substrate, The gas barrier layer contains a cured film of the gas barrier coating material according to claim 1. Laminate.
6. The laminate of claim 5 , wherein the substrate is a paper substrate.
7. The laminate according to claim 5 , further comprising a sealing layer interposed between the substrate and the gas barrier layer.
8. The dry mass of the gas barrier layer is 2.5 g / m 2 The laminate according to claim 5 .
9. A packaging material comprising the laminate according to claim 5 .
10. A coating step of coating at least one side of a substrate with the gas barrier coating material according to claim 1; a curing step of heating the coating film of the gas barrier coating material at 100° C. or higher for 1 hour or more to form a cured film of the gas barrier coating material; A method for manufacturing a laminate comprising the steps of:
11. The substrate is a paper substrate, The method for producing the laminate includes the steps of: A filling layer forming step of forming a filling layer on at least one surface of the base material before the coating step, In the coating step, the gas barrier coating material is coated on at least one surface of the filling layer. The method for producing the laminate according to claim 10 .
Citation Information
Patent Citations
Gas barrier polyurethane resin and gas barrier film containing the same
JP2001098047A
Coating agent and gas barrier film
JP2017071693A
Gas barrier film
JP2017222151A
Gas barrier film
JP2019195936A
Reinforcement barrier coatings
US20190352530A1