Resin composition for damping material, damping material, and damping laminate
A resin composition using a chlorine-containing thermoplastic resin and specific additives addresses toxicity issues in damping materials, achieving high damping performance and low toxicity through a balanced blend of components.
Patent Information
- Application Number
- JP2023057431
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
The use of chlorinated paraffins in damping materials is regulated due to toxicity concerns, and existing high damping resin compositions containing short- or medium-chain chlorinated paraffins are harmful, necessitating a low-toxicity alternative with excellent damping properties.
A resin composition comprising a chlorine-containing thermoplastic resin with specific chlorine content, blended with a compound B having defined molecular weight and melting point, along with optional resin additives, plasticizers, and inorganic fillers, to achieve a damping material with improved damping performance and reduced toxicity.
The proposed resin composition results in a damping material with low toxicity and excellent damping properties, as evidenced by a primary loss coefficient exceeding 0.4, effectively suppressing vibrations and noise.
Smart Images

Figure 2024145177000003 
Figure 2024145177000001 
Figure 2024145177000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition for a vibration-damping material, a vibration-damping material, and a vibration-damping laminate. [Background technology]
[0002] Conventionally, vibration-damping materials and sound-insulating members have been used to block and absorb vibrations and noises generated in various fields, such as houses, automobiles, airplanes, ships, and other vehicles, OA product housings, home appliance housings, and transportation facilities such as piping. Vibration-damping materials that utilize viscoelasticity and use polymeric materials that efficiently convert vibrations into heat and absorb them are used. Examples of vibration-damping materials that utilize the viscoelasticity of polymeric materials include constrained vibration-damping materials in which a viscoelastic layer is laminated on the vibration source, and a constraining layer with a high elastic modulus, such as metal, is further laminated on the surface that is not in contact with the vibration source.
[0003] Conventionally, the loss factor (η) has generally been used as an index of vibration-damping properties, with the larger the loss factor, the better the vibration-damping properties. A loss factor (η) value of over 0.1 is an excellent vibration-damping material, and a value of 0.3 or more is preferable.
[0004] In addition, the loss tangent (tan δ=E″ / E′) obtained by dividing the loss modulus (E″) by the storage modulus (E′) of the material is used as an index of vibration-damping properties, and the larger the loss tangent, the better the vibration-damping properties of the material. A material with a tan δ value of more than 1 is said to be excellent, but further improvement in vibration-damping properties is desired. As an excellent vibration-damping material, a high-damping resin composition containing a chlorine-containing thermoplastic resin and a chlorinated paraffin having an average carbon number of 12 to 16 and having a loss tangent of more than 3 has been disclosed (see, for example, Patent Document 1). A vibration-damping material in which such a high-damping resin composition is laminated with a constraining layer such as a metal has a loss factor (η) of more than 0.4, which shows excellent vibration-damping properties. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 3306415 Summary of the Invention [Problem to be solved by the invention]
[0006] In recent years, chlorinated paraffins have become a regulated substance due to their harmfulness. Chlorinated paraffins are classified into short chain (10-13 carbon atoms), medium chain (14-17 carbon atoms), and long chain (18 or more carbon atoms) according to the number of carbon atoms. However, short chain chlorinated paraffins are difficult to decompose, highly accumulative, and toxic to humans and living organisms, so their manufacture and import are prohibited in principle in Japan. In addition, medium chain chlorinated paraffins have also been selected as substances of very high concern (SVHC) in recent years under the REACH regulation. The high damping resin composition described in Patent Document 1 contains short or medium chain chlorinated paraffins with 12 or 14 carbon atoms, and can be said to be highly harmful.
[0007] In view of the above, an object of the present invention is to provide a resin composition for a vibration-damping material, a vibration-damping material, and a vibration-damping laminate, which are capable of obtaining a vibration-damping material that is less harmful and exhibits excellent vibration-damping properties. [Means for solving the problem]
[0008] The present inventors have conducted extensive research to solve the above problems. As a result, they have found that the above problems can be solved by using a chlorine-containing thermoplastic resin having specific conditions and a specific compound, and by blending the chlorine-containing thermoplastic resin and the specific compound in a specific ratio, and have arrived at the present invention. That is, the present invention provides the following [1] to [6]. [1] A resin composition for vibration-damping materials, comprising a chlorine-containing thermoplastic resin having a chlorine content of 20 to 65% by weight and a compound B, wherein the compound B has a molecular weight of 200 to 400 and a melting point of 50 to 70°C, and the content of the compound B is 150 to 800 parts by mass relative to 100 parts by mass of the chlorine-containing thermoplastic resin. [2] The resin composition for vibration-damping materials according to [1], wherein the compound B is a phthalate ester compound. [3] The resin composition for vibration-damping materials according to [1] or [2], further comprising a resin additive having a molecular weight of 400 to 1,500 and a melting point of 50 to 140°C, the content of the resin additive being 0.5 to 300 parts by mass per 100 parts by mass of the chlorine-containing thermoplastic resin. [4] A vibration-damping material comprising the resin composition for vibration-damping materials according to any one of [1] to [3]. [5] The vibration-damping material according to [4], which is a vibration-damping sheet. [6] A vibration-damping laminate comprising a substrate and a vibration-damping resin layer disposed on at least one surface of the substrate and made of the vibration-damping material according to [4]. Effect of the Invention
[0009] According to the present invention, it is possible to provide a resin composition for a vibration-damping material, a vibration-damping material, and a vibration-damping laminate, which are capable of obtaining a vibration-damping material that is low harmful and exhibits excellent vibration-damping properties. [Brief description of the drawings]
[0010] [Figure 1] 1 is a cross-sectional view showing a vibration-damping laminate according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, the resin composition for vibration-damping material, the vibration-damping material, and the vibration-damping laminate of the present invention will be described in detail, but the following description is an example of the embodiment of the present invention, and the present invention is not limited to these. In addition, in this specification, "~" indicating a numerical range means a range including the numerical values before and after it.
[0012] [Resin composition for vibration-damping materials] The vibration-damping material resin composition of the present invention contains a chlorine-containing thermoplastic resin having a chlorine content of 20 to 65 mass % and compound B.
[0013] (Chlorine-containing thermoplastic resin) The chlorine-containing thermoplastic resin used in the present invention is not particularly limited as long as it is a chlorine-containing thermoplastic resin having a chlorine content of 20 to 65% by mass. If the chlorine content of the chlorine-containing thermoplastic resin is less than 20% by mass, the crystals of the chlorine-containing thermoplastic resin tend to grow easily, so that the storage modulus increases, the loss tangent value decreases, and the vibration damping performance decreases. If the chlorine content exceeds 65% by mass, the intermolecular force becomes too strong, so that the storage modulus increases, the loss tangent value decreases, and the vibration damping performance decreases. The chlorine content of the chlorine-containing thermoplastic resin is preferably 25 to 60% by mass, more preferably 30 to 55% by mass, and even more preferably 35 to 50% by mass.
[0014] The chlorine-containing thermoplastic resin may contain a substituent other than chlorine, such as a cyano group, a hydroxyl group, an acetyl group, a methyl group, an ethyl group, bromine, or fluorine. The ratio of such a substituent other than chlorine is preferably 5% by mass or less. When the ratio of the substituent other than chlorine is 5% by mass or less, the possibility of causing a decrease in vibration damping performance can be suppressed.
[0015] The chlorine-containing thermoplastic resin may have a low storage modulus, and examples of such a resin include chlorinated polyethylene, polyvinyl chloride, vinyl chloride-vinyl acetate copolymer, etc. From the viewpoint that the chlorine-containing thermoplastic resin is preferably one having a low storage modulus, it is preferable that the chlorine-containing thermoplastic resin is an amorphous resin having a large loss tangent value, and chlorinated polyethylene is preferable.
[0016] (Compound B) The compound B used in the present invention has a molecular weight of 200 to 400 and a melting point of 50 to 70° C. Each condition will be explained below.
[0017] The molecular weight of the compound B of the present invention is 200 to 900. If the molecular weight is too low, less than 200, there is a concern that the material will volatilize or bleed out. If the molecular weight is too high, more than 900, the compound B cannot penetrate into the molecular chain of the chlorine-containing thermoplastic resin, so that the compatibility with the chlorine-containing thermoplastic resin is poor, the free rotational motion of the chlorine-containing thermoplastic resin is hindered, the loss tangent value is small, and the vibration damping performance is reduced. From the above viewpoint, the molecular weight of the compound B used in the present invention is preferably 220 to 800, more preferably 240 to 700, even more preferably 260 to 600, and particularly preferably 280 to 500.
[0018] The melting point of the compound B of the present invention is 50 to 70° C. If the melting point of the compound B is too low, less than 50° C., the peak of the loss tangent shifts to the low temperature side, and if the melting point is too high, more than 70° C., the peak of the loss tangent shifts to the high temperature side, and the vibration damping performance at room temperature (20° C.) decreases. From the above viewpoint, the melting point is preferably 52 to 68° C., more preferably 54 to 67° C., and further preferably 56 to 66° C. The melting point is measured by the method described in the Examples.
[0019] Compound B used in the present invention includes, for example, phthalate compounds, phosphoric acid ester compounds, etc., among which, phthalate compounds are preferred. Phthalate compounds include dicyclohexyl phthalate and bis(trans-3,3,5-trimethylcyclohexyl) phthalate. Phosphate compounds include triphenyl phosphate.
[0020] (Compound ratio of chlorine-containing thermoplastic resin and compound B) The content of the compound B of the present invention is 150 to 800 parts by mass relative to 100 parts by mass of the chlorine-containing thermoplastic resin. If the content of the compound B is less than 150 parts by mass, the crystals of the chlorine-containing thermoplastic resin tend to grow, the storage modulus increases, the loss tangent value decreases, and the vibration-damping performance decreases. On the other hand, if the content of the compound B is more than 800 parts by mass, the mechanical strength of the obtained vibration-damping material tends to decrease, and shape retention may become difficult. From the above viewpoint, the content of the compound B is preferably 175 to 700 parts by mass, more preferably 200 to 600 parts by mass, even more preferably 225 to 500 parts by mass, and more particularly preferably 250 to 400 parts by mass relative to 100 parts by mass of the chlorine-containing thermoplastic resin.
[0021] (Resin additives) The resin composition for vibration-damping material according to the present invention may further contain a resin additive. The resin additive used in the present invention adjusts the storage modulus of the resin composition for vibration-damping material and shifts the peak temperature of the loss tangent to a higher temperature. The resin additive used in the present invention has a molecular weight of 400 to 1,500 and a melting point of 50 to 140°C. Each condition will be described below.
[0022] The molecular weight of the resin additive of the present invention is preferably 500 to 1,400, more preferably 600 to 1,300, and even more preferably 700 to 1,200. When the molecular weight of the resin additive is equal to or greater than the lower limit, the occurrence of volatilization and bleed-out of the material can be suppressed. When the molecular weight of the resin additive is equal to or less than the upper limit, the compatibility with the chlorine-containing thermoplastic resin is improved, and the loss tangent value is increased without inhibiting the free rotational motion of the chlorine-containing thermoplastic resin, improving the vibration damping performance.
[0023] The melting point of the resin additive of the present invention is preferably 53 to 135° C., more preferably 56 to 130° C., and even more preferably 60 to 125° C. When the melting point of the resin additive is equal to or higher than the lower limit, the peak temperature of the loss tangent can be prevented from shifting to a lower temperature side. When the melting point of the resin additive is equal to or lower than the upper limit, the resin additive melts at the kneading temperature (150° C.), and the expected effect is easily exhibited. The melting point is measured by the method described in the Examples.
[0024] The resin additive used in the present invention is not particularly limited as long as it has good compatibility with the element-containing thermoplastic resin and compound B, and examples thereof include hindered phenol compounds, solid chlorinated paraffins, phosphite compounds, rosin ester compounds, etc. Among these, hindered phenol compounds and solid chlorinated paraffins are preferred.
[0025] The carbon number of the solid chlorinated paraffin used as the resin additive in the present invention is preferably 15 to 40, and more preferably 18 to 30. When the carbon number of the solid chlorinated paraffin is within the above range, it is less harmful and can impart sufficient viscosity.
[0026] The content of the resin additive of the present invention is preferably 0.5 to 300 parts by mass, more preferably 5 to 250 parts by mass, further preferably 15 to 200 parts by mass, and particularly preferably 25 to 150 parts by mass, relative to 100 parts by mass of the chlorine-containing thermoplastic resin. When the content of the resin additive is within the above range, the heat resistance and creep slippage of the obtained vibration-damping material can be improved.
[0027] (Plasticizer) The resin composition for vibration-damping materials of the present invention may further contain a plasticizer. The plasticizer used in the present invention adjusts the storage modulus of the resin composition for vibration-damping materials and shifts the peak temperature of the loss tangent to a lower temperature side. The plasticizer used in the present invention has a molecular weight of 200 to 2,500, a glass transition point (Tg) of -100 to 15°C, and a viscosity at 20°C of 10 to 600,000 mPa·s. Each condition will be described below.
[0028] The molecular weight of the plasticizer of the present invention is preferably 300 to 2,000, more preferably 400 to 1,500, and even more preferably 500 to 1,000. When the molecular weight of the plasticizer is equal to or greater than the lower limit, the occurrence of volatilization and bleed-out of the material can be suppressed. When the molecular weight of the plasticizer is equal to or less than the upper limit, the compatibility with the chlorine-containing thermoplastic resin is improved, and the loss tangent value is increased without inhibiting the free rotational motion of the chlorine-containing thermoplastic resin, improving the vibration damping performance.
[0029] The glass transition point (Tg) of the plasticizer of the present invention is preferably −95 to 5° C., more preferably −90 to −5° C., further preferably −85 to −15° C., and particularly preferably −80 to −20° C. When the glass transition point (Tg) of the plasticizer is equal to or higher than the lower limit, the peak temperature of the loss tangent can be prevented from shifting too far to the low temperature side. When the glass transition point (Tg) of the plasticizer is equal to or lower than the upper limit, the peak temperature of the loss tangent can be prevented from shifting to the high temperature side, and vibration damping performance at room temperature (20° C.) can be improved. The glass transition point (Tg) is measured by the method described in the Examples.
[0030] The viscosity of the plasticizer of the present invention at 20°C is preferably 30 to 100,000 mPa·s, more preferably 50 to 10,000 mPa·s, even more preferably 70 to 5,000 mPa·s, and particularly preferably 100 to 3000 mPa·s. When the viscosity of the plasticizer at 20°C is equal to or higher than the lower limit, the peak temperature of the loss tangent can be prevented from shifting too far to the low temperature side. When the viscosity of the plasticizer at 20°C is equal to or lower than the upper limit, the peak temperature of the loss tangent can be prevented from shifting to the high temperature side, and vibration damping performance at room temperature (20°C) can be improved. The viscosity is measured by the method described in the examples.
[0031] The plasticizer used in the present invention is not particularly limited as long as it has good compatibility with the chlorine-containing thermoplastic resin and compound B, and examples thereof include trimellitic acid-based plasticizers, epoxy-based plasticizers, adipic acid-based plasticizers, ester-based plasticizers, and phosphate-based plasticizers. Among these, trimellitic acid-based plasticizers and epoxy-based plasticizers are preferred.
[0032] The content of the plasticizer of the present invention is preferably 0.5 to 200 parts by mass, more preferably 5 to 200 parts by mass, further preferably 15 to 175 parts by mass, and particularly preferably 25 to 150 parts by mass, relative to 100 parts by mass of the chlorine-containing thermoplastic resin. When the content of the plasticizer is within the above range, the heat resistance and creep slippage of the obtained vibration-damping material can be improved.
[0033] (Inorganic filler) The resin composition for vibration-damping materials of the present invention may contain an inorganic filler. The inorganic filler contributes to improving vibration-damping performance.
[0034] The inorganic filler used in the present invention has a flaky shape. By making the inorganic filler flaky, when vibration is applied, the energy loss at the interface between the flaky inorganic filler and the resin increases, and high vibration damping performance can be achieved. Here, the term "scale-like" refers to a thin plate-like shape in which the thickness is extremely small compared to the maximum dimension, and the aspect ratio, which is the maximum dimension (long diameter) divided by the thickness (long diameter / thickness), is 10 or more. The aspect ratio of the scaly filler is more preferably equal to or greater than 20, and desirably equal to or greater than 50. The aspect ratio of the inorganic filler is preferably an average aspect ratio of a plurality of inorganic fillers, and can be determined by observing 50 arbitrarily selected inorganic fillers with an electron microscope or optical microscope and calculating the average value of the major axis / thickness of each inorganic filler.
[0035] Examples of the inorganic filler used in the present invention include mica, graphite, talc, wollastonite, titanium oxide, sepiolite, calcium carbonate, silica, glass beads, alumina, barium sulfate, glass fiber, cellulose fiber, carbon fiber, carbon nanotube, and carbon nanocoil. Of these, it is preferable to use calcium carbonate.
[0036] The content of the inorganic filler of the present invention is preferably 100 to 1,000 parts by mass, more preferably 200 to 900 parts by mass, and even more preferably 300 to 800 parts by mass, relative to 100 parts by mass of the chlorine-containing thermoplastic resin. By having the content of the inorganic filler within the above range, the storage modulus can be improved, thereby improving vibration damping properties, and the handling property is improved by having fluidity.
[0037] (Other added ingredients) The resin composition for vibration-damping materials of the present invention may contain other additive components as required within the scope of the invention not impairing the object of the present invention. As other additives, when the vibration-damping material needs to be transparent, a rosin-based compound can be added. The rosin-based compound may be, for example, a rosin metal salt or a rosin ester.
[0038] In addition, a tin-based stabilizer can be contained as a heat stabilizer when molding the resin composition for vibration-damping material. The tin-based stabilizer is not particularly limited, and examples thereof include dialkyltin maleate, dialkyltin bis(monoalkyl maleate), dibutyltin maleate polymer, dialkyltin laurate, dialkyltin mercapto, dialkyltin bis(mercapto fatty acid ester), dialkyltin sulfide, dioctyltin maleate polymer, etc. These may be used alone or in combination of two or more kinds.
[0039] Furthermore, other additives such as fillers, lubricants, shrinkage prevention agents, crystal nucleating agents, colorants (pigments, dyes, etc.), UV absorbers, antioxidants, antiaging agents, reinforcing agents, flame retardant assistants, antistatic agents, surfactants, vulcanizing agents, and surface treatment agents may be added as necessary.
[0040] [Vibration-damping materials] The vibration-damping material of the present invention is obtained by shaping the resin composition for vibration-damping material of the present invention. The shape of the vibration-damping material is not particularly limited, and may be sheet-like, plate-like, rod-like, or block-like, but a sheet-like vibration-damping sheet is preferred. The term "sheet" does not strictly refer to a thickness, but includes thin ones usually called "films" and thick ones usually called "plates". The thickness of the vibration-damping sheet is not particularly limited, but if it is too thin, the vibration-damping effect may be small, and if it is too thick, handling may be inconvenient when applied to a source of vibration, etc., so a thickness of 0.05 to 50 mm is preferred.
[0041] [Vibration-damping laminate] Next, a vibration-damping laminate according to an embodiment of the present invention will be described. As shown in Fig. 1, the vibration-damping laminate 1 according to an embodiment of the present invention comprises a substrate 10 and a vibration-damping resin layer 20 made of the above-described vibration-damping material and disposed on at least one surface of the substrate 10. The vibration-damping laminate 1 according to an embodiment of the present invention further comprises a constraining layer 30 on the vibration-damping resin layer 20.
[0042] The thickness of the vibration-damping laminate 1 may be any thickness, but if it is too thin, sufficient vibration-damping properties cannot be obtained, and if it is too thick, the mass becomes heavy and workability becomes poor, so the thickness is preferably 1 mm to 50 mm, more preferably 2 mm to 40 mm, and even more preferably 3 mm to 30 mm.
[0043] (base material) The substrate 10 is not particularly limited as long as it is a material having a high elastic modulus. Examples of the substrate 10 include metal materials such as lead, steel (including stainless steel), copper, and aluminum; and inorganic materials such as concrete, gypsum board, marble, slate, sand, and glass. These may be used alone or in combination of two or more kinds.
[0044] The thickness of the substrate 10 may be any thickness; however, if it is too thin, sufficient vibration damping properties cannot be obtained, and if it is too thick, the mass becomes heavy and workability becomes poor, so the thickness is preferably 50 μm to 50 mm, more preferably 100 μm to 40 mm, and even more preferably 200 μm to 30 mm.
[0045] (Vibration-damping resin layer) The vibration-damping resin layer 20 is formed from the resin composition for vibration-damping materials described above. The vibration-damping resin layer 20 may be formed by any conventionally known method, such as extrusion molding, press molding, roll molding, injection molding, etc.
[0046] The thickness of the vibration-damping resin layer 20 may be arbitrary, but if it is too thin, sufficient vibration-damping properties cannot be obtained, whereas if it is too thick, the mass becomes heavy and workability deteriorates, so that the thickness is preferably 100 μm to 5.0 mm.
[0047] (restriction layer) The constraining layer 30 preferably has a modulus of longitudinal elasticity of 1 GPa or more. In addition, a material having a modulus of longitudinal elasticity greater than that of the chlorine-containing thermoplastic resin constituting the vibration-damping resin layer 20 is preferable, and in order to achieve a sufficient vibration-damping effect, a modulus of longitudinal elasticity of 10 GPa or more is more preferable.
[0048] Examples of the constraint layer 30 include metal materials such as lead, iron, steel (including stainless steel), and aluminum (including aluminum alloys); inorganic materials such as concrete, gypsum board, marble, slate board, sand board, and glass; bisphenol A modified resins such as polycarbonate and polysulfone; acrylic resins such as poly(meth)acrylate; chlorine-based resins such as vinyl chloride resins and chlorinated vinyl chloride resins; rubber-based materials such as acrylonitrile-butadiene-styrene rubber; saturated polyesters such as polyethylene terephthalate and polyethylene naphthalate; styrene-based resins; olefin-based resins such as polyethylene and polypropylene; polyamide-based resins such as nylon 6, nylon 66, and aramid (aromatic polyamide); melamine-based resins; polyimide-based resins; urethane-based resins; thermosetting resins such as dicyclopentadiene and bakelite; cellulose-based materials such as wood and paper; and plates or sheets made of chitin, chitosan, etc.
[0049] The constraining layer 30 may be used alone or in combination of two or more. The constraining layer 30 may be reinforced with glass fiber, carbon fiber, liquid crystal, etc., may be a composite plate made of different materials, or may be a foam made of these materials.
[0050] The thickness of the constraining layer 30 may be arbitrary, but if it is too thin, sufficient vibration damping properties cannot be obtained, and if it is too thick, the mass becomes heavy and workability deteriorates, so that the thickness is preferably 50 μm to 5.0 mm.
[0051] The vibration-damping laminate 1 according to the embodiment of the present invention has a primary loss factor of 0.4 or more at 20° C. When the vibration-damping laminate 1 has a primary loss factor of 0.4 or more at 20° C., the vibration-damping material has excellent vibration-damping performance in a normal usage environment.
[0052] (action) The resin composition for vibration-damping material of the present invention is composed of a chlorine-containing thermoplastic resin having specific conditions and a compound B having specific conditions, and is obtained by blending this compound B with the chlorine-containing thermoplastic resin in a specific ratio. The vibration-damping material obtained from this resin composition for vibration-damping material shows excellent vibration-damping absorption properties, such as a primary loss coefficient value of more than 0.4. EXAMPLES
[0053] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the examples and comparative examples, the following materials and measurement methods were used.
[0054] [Chlorine-containing thermoplastic resin] As the chlorine-containing thermoplastic resin, chlorinated polyethylene (manufactured by Showa Denko KK, product number "ELASLENE 401A", chlorine content 40% by mass) was used. [Compound B] As compound B, those shown in Table 1 were used. [Resin additives] The resin additives used were those listed in Table 1. [Other low molecular weight compounds] In the Reference Examples and Comparative Examples, the other low molecular weight compounds used were those shown in Table 1. [Tackifier] As the tackifier, rosin ester (manufactured by Arakawa Chemical Industries, Ltd., product number "KE-359") was used. [Inorganic filler] As the inorganic filler, calcium carbonate (manufactured by Shiraishi Calcium Co., Ltd., product number "Whiten 305-S") was used.
[0055] [Resin composition for vibration-damping materials] Each material was weighed out in a PE cup according to the compounding ratio shown in Table 2, heated to 150° C., and kneaded with a roller to obtain resin compositions for vibration damping materials of the Examples, Reference Examples, and Comparative Examples.
[0056] [Vibration-damping laminate] The vibration-damping resin composition for vibration-damping materials of the Examples, Reference Examples and Comparative Examples was sandwiched between polyethylene terephthalate with a release treatment on the surface, and molded into a sheet-like resin composition with a thickness of 1.0 mm by a heat press. This sheet-like resin composition was cut into a piece with a width of 20 mm and a length of 250 mm, and a steel plate of the same shape with a thickness of 1.6 mm, the sheet-like resin composition and a steel plate of the same shape with a thickness of 0.3 mm were laminated in this order, and lightly pressed by hand to prepare a vibration-damping laminate for loss factor evaluation.
[0057] [Measurement method] The methods for measuring the various physical properties in this specification are as follows. <Loss factor measurement> The primary loss factor in the present invention refers to a loss factor calculated by a half-width method at a primary resonance frequency obtained by a central excitation method at 20°C for the vibration-damping laminate for loss factor evaluation based on JIS K7391:2008. <Glass transition point (Tg) and melting point measurements> The glass transition point (Tg) in the present invention refers to the midpoint glass transition temperature obtained for the obtained resin composition for vibration-damping material using a differential scanning calorimeter under measurement conditions of a heating rate of 10°C / min based on JIS K 7121: 2012. The melting point refers to the melting peak temperature obtained using a differential scanning calorimeter under measurement conditions of a heating rate of 10°C / min based on JIS K 7121: 2012. As the differential scanning calorimeter, DSC7020 (manufactured by Seiko Electric Industries Co., Ltd.) was used. <Viscosity measurement> The viscosity in the present invention refers to the complex viscosity measured by a rotational rheometer at 20° C., an angular frequency of 10 rad / s, and a strain of 100%. The rotational rheometer used was MCR102 (manufactured by Anton Paar).
[0058] [Table 1]
[0059] [Table 2]
[0060] Example 1 had a primary loss factor of 0.4 or more and exhibited excellent vibration-damping properties, whereas Comparative Examples 1 to 3 had primary loss factors of less than 0.4 and did not exhibit excellent vibration-damping properties. [Explanation of symbols]
[0061] 1: Vibration-damping laminate 10: Base material 20: Vibration-damping resin layer 30:Restriction layer
Claims
1. A resin composition for vibration-damping materials, comprising a chlorine-containing thermoplastic resin having a chlorine content of 20 to 65% by weight and a compound B, The compound B has a molecular weight of 200 to 400 and a melting point of 50 to 70° C. The resin composition for vibration-damping materials, wherein the content of the compound B is 150 to 800 parts by mass based on 100 parts by mass of the chlorine-containing thermoplastic resin.
2. 2. The resin composition for vibration-damping materials according to claim 1, wherein the compound B is a phthalate ester compound.
3. Further containing a resin additive having a molecular weight of 400 to 1,500 and a melting point of 50 to 140°C, 2. The resin composition for vibration-damping materials according to claim 1, wherein the content of the resin additive is 0.5 to 300 parts by mass based on 100 parts by mass of the chlorine-containing thermoplastic resin.
4. A vibration-damping material comprising the resin composition for vibration-damping materials according to any one of claims 1 to 3.
5. The vibration-damping material according to claim 4, which is a vibration-damping sheet.
6. A substrate; A vibration-damping laminate comprising: a vibration-damping resin layer made of the vibration-damping material according to claim 4, the vibration-damping resin layer being disposed on at least one surface of the substrate.
Citation Information
Patent Citations
Polyvinyl chloride resin composition
JP1993078537A
Polyvinyl chloride resin composition
JP1994057076A
Vibration-damping resin composition
JP1997227745A
Undercoat agent, undercoat film and undercoating method for preventing noise
JP1998287825A
High damping material composition
JP2000086900A