Method for producing fine fibrous cellulose
By utilizing heat from the ionic group introduction step in the production of fine fibrous cellulose and recycling it through heat exchangers, the method addresses the high energy demands of existing cellulose defibration processes, achieving energy-efficient cellulose production.
Patent Information
- Application Number
- JP2023057434
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-31
AI Technical Summary
The production of fine fibrous cellulose requires significant energy due to the mechanical treatment involved in defibrating cellulose fibers, and existing methods do not efficiently utilize the energy used in introducing ionic groups into the pulp.
A method that incorporates the use of heat generated during the introduction of ionic groups into the pulp by heating the pulp with an aqueous solution containing a reaction agent, followed by refining, and utilizes this heat in subsequent steps through heat removal using water or gas in a heat exchanger to reduce overall energy consumption.
This approach enables the production of fine fibrous cellulose while significantly reducing energy usage by effectively recycling the heat from the ionic group introduction step across various manufacturing processes.
Smart Images

Figure 2024145178000001 
Figure 2024145178000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing fine fibrous cellulose. [Background technology]
[0002] Fine fibrous cellulose obtained by defibrating cellulose fibers to a fiber width of 1000 nm or less has excellent strength, elasticity, thermal stability, etc., and is used industrially as a filler for compounding resins and rubbers. In addition, aqueous dispersions of fine fibrous cellulose are used as viscosity adjusters, stabilizers, etc. Fine fibrous cellulose can be obtained by defibrating pulp fibers through a mechanical treatment. In this case, it is said that the energy required for the mechanical treatment can be efficiently reduced by defibrating the pulp fibers after introducing ionic groups into them (see Patent Documents 1 and 2). However, the production of fine fibrous cellulose requires a lot of energy. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2008-1728 A [Patent Document 2] JP 2010-235679 A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide a method for producing fine fibrous cellulose, which is capable of producing fine fibrous cellulose in an energy-saving manner. [Means for solving the problem]
[0005] The present inventors have found that the above problems can be solved by using, in any one of the steps, the heat used in the step of introducing ionic groups into the fine fibrous cellulose. The present invention relates to the following <1> ~ <8> Regarding. <1> contacting the raw pulp with an aqueous solution containing a reactant; A step of introducing ionic groups into the raw pulp by heating at a temperature of 120°C or higher; and The method includes, in this order, a step of micronizing the raw pulp into which the ionic group has been introduced, the reacting agent is an esterifying agent which introduces an anionic group into the raw pulp via an ester bond, an etherifying agent which introduces an anionic group into the raw pulp via an ether bond, or a cationizing agent; The heat used in the step of introducing ionic groups into the raw pulp is used in any one of the production steps. A method for producing fine fibrous cellulose. <2> The heat used in the step of introducing ionic groups into the raw pulp is removed by using water, or by using a gas in a heat exchanger. <1> A method for producing fine fibrous cellulose according to claim 1. <3> Using the water or gas heated in the heat removal step, water to be used in a water washing step following the step of introducing ionic groups into the raw pulp is heated. <2> A method for producing fine fibrous cellulose according to claim 1. <4> The water or gas heated in the heat removal step is used to heat the gas used in the step of introducing ionic groups into the raw pulp. <2> A method for producing fine fibrous cellulose according to claim 1. <5> The reactant is an esterifying agent that introduces anionic groups into the raw pulp via ester bonds; <1> ~ <4> 13. The method for producing fine fibrous cellulose according to claim 12, wherein the cellulose is <6> The reactant is an esterifying agent that introduces phosphorus oxo acid groups into the raw pulp via ester groups; <1> ~ <5> 13. The method for producing fine fibrous cellulose according to claim 12, wherein the cellulose is <7> The method includes a step of removing the heat used in the step of introducing ionic groups into the raw pulp by using water, or a heat removal step of removing the heat by using a gas in a heat exchanger, and heating an aqueous solution containing an esterifying agent by using the water or gas heated in the heat removal step. <5> or <6> A method for producing fine fibrous cellulose according to claim 1. <8> The aqueous solution containing the esterifying agent further contains urea or a derivative thereof. <5> ~ <7> 13. The method for producing fine fibrous cellulose according to claim 12, wherein the cellulose is Effect of the Invention
[0006] According to the present invention, there is provided a method for producing fine fibrous cellulose, which is capable of producing fine fibrous cellulose in an energy-saving manner. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] [Method of producing fine fibrous cellulose] The method for producing fine fibrous cellulose in this embodiment includes, in this order, a step of contacting raw material pulp with an aqueous solution containing a reactive agent (hereinafter also referred to as "step 1"), a step of heating at a temperature of 120°C or higher to introduce ionic groups into the raw material pulp (hereinafter also referred to as "step 2"), and a step of finely dividing the raw material pulp into which the ionic groups have been introduced (hereinafter also referred to as "step 3"), wherein the reactive agent is an esterifying agent that introduces anionic groups into the raw material pulp via an ester bond, an etherifying agent that introduces anionic groups into the raw material pulp via an ether bond, or a cationizing agent, and the heat used in the step of introducing ionic groups into the raw material pulp (step 2) is used in any of the production steps. In the present invention, the heat used in step 2 is used in any one of the steps in the production process of fine fibrous cellulose, thereby making it possible to effectively utilize the heat generated in the process and produce fine fibrous cellulose with less energy. The present invention will be described in detail below.
[0008] [Process 1] Step 1 is a step of contacting a raw pulp with an aqueous solution containing a reactant. The raw pulp and the reactant used in step 1 will be described in detail. <Raw pulp> The raw material pulp is a fiber raw material containing cellulose, and examples of the raw material pulp include, but are not limited to, wood pulp, non-wood pulp, and deinked pulp. Examples of wood pulp include, but are not limited to, chemical pulp such as hardwood kraft pulp (LBKP), softwood kraft pulp (NBKP), sulfite pulp (SP), dissolving pulp (DP), soda pulp (AP), unbleached kraft pulp (UKP), and oxygen bleached kraft pulp (OKP), semi-chemical pulp such as semi-chemical pulp (SCP) and chemi-ground wood pulp (CGP), and mechanical pulp such as groundwood pulp (GP) and thermomechanical pulp (TMP, BCTMP). Examples of non-wood pulp include, but are not limited to, cotton-based pulp such as cotton linters and cotton lint, and non-wood-based pulp such as hemp, straw, bamboo, and bagasse. Examples of deinked pulp include, but are not limited to, deinked pulp made from waste paper. The pulp raw material of this embodiment may be one of the above-mentioned materials, or a mixture of two or more of them. Among the above pulps, for example, wood pulp and deinked pulp are preferred from the viewpoint of availability. Furthermore, among wood pulps, for example, chemical pulp is more preferred, and kraft pulp and sulfite pulp are even more preferred, from the viewpoint of high cellulose ratio and high yield of fine fibrous cellulose during defibration treatment, and small decomposition of cellulose in the pulp to obtain long-fiber fine fibrous cellulose with a large axial ratio. Note that the viscosity tends to increase when long-fiber fine fibrous cellulose with a large axial ratio is used.
[0009] <Reactant> In this embodiment, the reactant is an esterifying agent that introduces anionic groups into the raw pulp via ester bonds, an etherifying agent that introduces anionic groups into the raw pulp via ether bonds, or a cationizing agent. Examples of anionic groups introduced into the raw pulp via an ester bond include phosphorus oxoacid groups or substituents derived from phosphorus oxoacid groups (sometimes simply referred to as phosphorus oxoacid groups), and sulfur oxoacid groups or substituents derived from sulfur oxoacid groups (sometimes simply referred to as sulfur oxoacid groups). Examples of the anionic group introduced into the raw pulp via an ether bond include a phosphonic group or a substituent derived from a phosphonic group, a phosphine group or a substituent derived from a phosphine group, a sulfonic group or a substituent derived from a sulfonic group, and a carboxyalkyl group (e.g., a carboxymethyl group, a carboxyethyl group). Examples of the cationic group to be introduced into the raw pulp include an ammonium group, a phosphonium group, a sulfonium group, etc. Among these, the cationic group is preferably an ammonium group. The ionic group introduced into the raw pulp by the reacting agent is preferably at least one selected from the group consisting of phosphorus oxoacid groups, substituents derived from phosphorus oxoacid groups, sulfur oxoacid groups, substituents derived from sulfur oxoacid groups, carboxyalkyl groups, and sulfone groups, more preferably at least one selected from the group consisting of phosphorus oxoacid groups, substituents derived from phosphorus oxoacid groups, sulfur oxoacid groups, substituents derived from sulfur oxoacid groups, carboxymethyl groups, and carboxyethyl groups, still more preferably phosphorus oxoacid groups and sulfur oxoacid groups, and even more preferably phosphorus oxoacid groups. Introducing phosphorus oxoacid groups as anionic groups is preferred in that fine fibrous cellulose that is more energy-efficient and has excellent transparency is produced.
[0010] The phosphorus oxoacid group or the substituent derived from the phosphorus oxoacid group is, for example, a substituent represented by the following formula (1). A plurality of substituents represented by the following formula (1) may be introduced into each fibrous cellulose. In this case, the plurality of introduced substituents represented by the following formula (1) may be the same or different.
[0011] [ka]
[0012] In formula (1), a, b, and n are natural numbers, and m is an arbitrary number (where a=b×m). At least one of the n α and α' is O. - and the rest are R or OR. Note that each α and α' is O. - The n α's may all be the same or may be different. b+ is a cation of one or more valences consisting of organic or inorganic substances.
[0013] Each R is a hydrogen atom, a saturated linear hydrocarbon group, a saturated branched hydrocarbon group, a saturated cyclic hydrocarbon group, an unsaturated linear hydrocarbon group, an unsaturated branched hydrocarbon group, an unsaturated cyclic hydrocarbon group, an aromatic group, or a group derived therefrom. In formula (1), n is preferably 1.
[0014] Examples of saturated linear hydrocarbon groups include, but are not limited to, methyl, ethyl, n-propyl, or n-butyl groups. Examples of saturated branched hydrocarbon groups include, but are not limited to, i-propyl or t-butyl groups. Examples of saturated cyclic hydrocarbon groups include, but are not limited to, cyclopentyl or cyclohexyl groups. Examples of unsaturated linear hydrocarbon groups include, but are not limited to, vinyl or allyl groups. Examples of unsaturated branched hydrocarbon groups include, but are not limited to, i-propenyl or 3-butenyl groups. Examples of unsaturated cyclic hydrocarbon groups include, but are not limited to, cyclopentenyl or cyclohexenyl groups. Examples of aromatic groups include, but are not limited to, phenyl or naphthyl groups.
[0015] In addition, the derivative group in R is a carboxy group, a carboxylate group (-COO -), functional groups in which at least one selected from functional groups such as hydroxyl, amino and ammonium groups is added or substituted, but are not particularly limited. The number of carbon atoms constituting the main chain of R is not particularly limited, but is preferably 20 or less, more preferably 10 or less. By setting the number of carbon atoms constituting the main chain of R within the above range, the molecular weight of the phosphorus oxoacid group can be set to an appropriate range, which facilitates penetration into the fiber raw material and increases the yield of fibrous cellulose. When multiple Rs exist in formula (1) or multiple types of substituents represented by the above formula (1) are introduced into the fibrous cellulose, the multiple Rs may be the same or different.
[0016] β b+ is a monovalent or higher cation made of an organic or inorganic substance. An example of the monovalent or higher cation made of an organic substance is an organic onium ion. An example of the organic onium ion is an organic ammonium ion or an organic phosphonium ion. An example of the organic ammonium ion is an aliphatic ammonium ion or an aromatic ammonium ion, and an example of the organic phosphonium ion is an aliphatic phosphonium ion or an aromatic phosphonium ion. An example of the monovalent or higher cation made of an inorganic substance is an ion of an alkali metal such as sodium, potassium, or lithium, an ion of a divalent metal such as calcium or magnesium, a hydrogen ion, an ammonium ion, or the like. In addition, in formula (1), β b+ When a plurality of substituents represented by the above formula (1) are present or when a plurality of substituents represented by the above formula (1) are introduced into the fibrous cellulose, the plurality of β b+ may be the same or different. The organic or inorganic cations of monovalent or higher include β b+ Sodium or potassium ions are preferred because they are less likely to yellow when the fiber raw material containing the cation is heated and are easy to use industrially, but there is no particular limitation.
[0017] More specifically, examples of the phosphorus oxoacid group or the substituent derived from the phosphorus oxoacid group include a phosphoric acid group (-PO3H2), a salt of a phosphoric acid group, a phosphorous acid group (phosphonic acid group) (-PO2H2), and a salt of a phosphorous acid group (phosphonic acid group). In addition, the phosphorus oxoacid group or the substituent derived from the phosphorus oxoacid group may be a group in which a phosphoric acid group is condensed (e.g., a pyrophosphate group), a group in which a phosphonic acid is condensed (e.g., a polyphosphonic acid group), a phosphoric ester group (e.g., a monomethyl phosphate group, a polyoxyethylene alkyl phosphate group), an alkyl phosphonic acid group (e.g., a methyl phosphonic acid group), and the like.
[0018] The sulfur oxoacid group (sulfur oxoacid group or a substituent derived from a sulfur oxoacid group) is, for example, a substituent represented by the following formula (2). A plurality of substituents represented by the following formula (2) may be introduced into each fibrous cellulose. In this case, the plurality of introduced substituents represented by the following formula (2) may be the same or different.
[0019] [ka]
[0020] In the above structural formula, b and n are natural numbers, p is 0 or 1, and m is an arbitrary number (where 1=b×m). When n is 2 or more, the multiple p's may be the same or different. In the above structural formula, β b+is a monovalent or higher cation made of an organic or inorganic substance. Examples of the monovalent or higher cation made of an organic substance include organic onium ions. Examples of the organic onium ions include organic ammonium ions and organic phosphonium ions. Examples of the organic ammonium ions include aliphatic ammonium ions and aromatic ammonium ions, and examples of the organic phosphonium ions include aliphatic phosphonium ions and aromatic phosphonium ions. Examples of the monovalent or higher cation made of an inorganic substance include ions of alkali metals such as sodium, potassium, or lithium, ions of divalent metals such as calcium or magnesium, hydrogen ions, and ammonium ions. When multiple types of substituents represented by the above formula (2) are introduced into the fibrous cellulose, the multiple β b+ may be the same or different. The organic or inorganic cations of monovalent or higher include β b+ Sodium or potassium ions are preferred because they are less likely to yellow when the fiber raw material containing the cation is heated and are easy to use industrially, but there is no particular limitation.
[0021] (Esterification agent) The esterification agent is a reactant that introduces anionic groups into the raw pulp via ester bonds. As described above, examples of the anionic groups introduced by the esterification agent include phosphorus oxoacid groups, sulfur oxoacid groups, and xanthate groups. -Phosphorus oxo acid group- The esterification agent (hereinafter also referred to as compound A) for introducing a phosphorus oxo acid group may be any compound that has a phosphorus atom and can form an ester bond with cellulose, and examples thereof include phosphoric acid or a salt thereof, phosphorous acid or a salt thereof, dehydrated condensed phosphoric acid or a salt thereof, and anhydrous phosphoric acid (diphosphorus pentoxide), but is not particularly limited thereto. Phosphoric acid of various purities can be used, for example, 100% phosphoric acid (orthophosphoric acid) or 85% phosphoric acid can be used. Phosphorous acid can be 99% phosphorous acid (phosphonic acid). Dehydrated condensed phosphoric acid is phosphoric acid in which two or more molecules are condensed by a dehydration reaction, and examples thereof include pyrophosphoric acid and polyphosphoric acid. Phosphates, phosphites, and dehydrated condensed phosphates can include lithium salts, sodium salts, potassium salts, and ammonium salts of phosphoric acid, phosphorous acid, or dehydrated condensed phosphoric acid, and these can be neutralized to various degrees. Among these, from the viewpoints of high efficiency of introduction of phosphate groups, easier improvement of defibration efficiency in the defibration step described below, low cost, and ease of industrial application, phosphoric acid, sodium salt of phosphoric acid, potassium salt of phosphoric acid, ammonium salt of phosphoric acid, or phosphorous acid, sodium salt of phosphorous acid, potassium salt of phosphorous acid, or ammonium salt of phosphorous acid are preferred, and phosphoric acid, sodium dihydrogen phosphate, disodium hydrogen phosphate, ammonium dihydrogen phosphate, or phosphorous acid and sodium phosphite are more preferred.
[0022] The amount of compound A added to the raw pulp is not particularly limited, but for example, when the amount of compound A added is converted into the amount of phosphorus atoms, the amount of phosphorus atoms added to the raw pulp (bone dry mass) is preferably 0.5% by mass or more and 100% by mass or less, more preferably 1% by mass or more and 50% by mass or less, and even more preferably 2% by mass or more and 30% by mass or less. By setting the amount of phosphorus atoms added to the raw pulp within the above range, the yield of fine fibrous cellulose can be further improved. On the other hand, by setting the amount of phosphorus atoms added to the raw pulp to the above upper limit or less, a balance between the effect of improving the yield and the cost can be achieved.
[0023] The step of contacting the raw pulp with the aqueous solution containing compound A may be carried out in the presence of at least one selected from urea and its derivatives (hereinafter also referred to as "compound B"), or the reaction between the raw pulp and compound A may be carried out in the absence of compound B. Among these, it is preferable to contact the raw pulp with the aqueous solution containing compound A in the presence of compound B. Examples of compound B include urea, biuret, 1-phenylurea, 1-benzylurea, 1-methylurea, and 1-ethylurea. From the viewpoint of improving the uniformity of the reaction, it is preferable to use compound B as an aqueous solution. In addition, from the viewpoint of further improving the uniformity of the reaction, it is preferable to use an aqueous solution in which both compound A and compound B are dissolved. That is, when an esterifying agent is used as the reactant, it is preferable that the aqueous solution containing the esterifying agent further contains urea or a derivative thereof.
[0024] The amount of compound B added relative to the raw material pulp (bone dry mass) is not particularly limited, but is preferably, for example, 1 mass% or more and 500 mass% or less, more preferably 10 mass% or more and 400 mass% or less, and even more preferably 100 mass% or more and 350 mass% or less.
[0025] In the reaction of the raw pulp containing cellulose with compound A, in addition to compound B, for example, amides or amines may be included in the reaction system. Examples of amides include formamide, dimethylformamide, acetamide, and dimethylacetamide. Examples of amines include methylamine, ethylamine, trimethylamine, triethylamine, monoethanolamine, diethanolamine, triethanolamine, pyridine, ethylenediamine, and hexamethylenediamine. Among these, triethylamine in particular is known to act as a good reaction catalyst.
[0026] -Sulfur oxo acid group- The esterification agent (hereinafter also referred to as compound C) for introducing sulfur oxo acid groups may be any compound that has a sulfur atom and can form an ester bond with cellulose, and examples thereof include, but are not limited to, sulfuric acid or its salts, sulfurous acid or its salts, and sulfuric acid amides. Sulfuric acid of various purities can be used, for example, 96% sulfuric acid (concentrated sulfuric acid). Sulfurous acid can be 5% aqueous sulfurous acid. Sulfate or sulfite can be lithium salt, sodium salt, potassium salt, ammonium salt, etc. of sulfate or sulfite, which can be neutralized to various degrees. Sulfamic acid or the like can be used as sulfuric acid amide. In the sulfone group introduction step, it is preferable to use compound B in the above-mentioned <phosphorus oxo acid group introduction step> in the same manner.
[0027] (Etherification Agent) The etherifying agent is a reacting agent that introduces anionic groups into the raw pulp via ether bonds. As described above, examples of the anionic groups introduced by the etherifying agent include a phosphonic group or a substituent derived from a phosphonic group, a phosphine group or a substituent derived from a phosphine group, a sulfonic group or a substituent derived from a sulfonic group, and a carboxyalkyl group (e.g., a carboxymethyl group, a carboxyethyl group).
[0028] -Phosphonic or phosphine group- As an etherification agent for introducing a phosphonic or phosphine group, a compound having a reactive group and a phosphonic or phosphine group (compound E A ) and, as an optional component, an alkali compound and a compound B selected from the above-mentioned urea and its derivatives are added to the raw pulp and reacted. This introduces a phosphoalkyl group.
[0029] Examples of the reactive group include a halogenated alkyl group, a vinyl group, and an epoxy group (glycidyl group). Compound E, an etherifying agent AExamples of the compound E include vinyl phosphonic acid, phenyl vinyl phosphonic acid, and phenyl vinyl phosphinic acid. From the viewpoints of the efficiency of introducing the substituent, the defibration efficiency, the cost, and the ease of handling, the compound E A is preferably vinylphosphonic acid. Furthermore, it is also preferable to use the above-mentioned compound B as an optional component, and the amount added is also preferably as described above. It is preferable that the raw pulp is converted into alkali cellulose in advance or simultaneously with the reaction. The method for converting the raw pulp into alkali cellulose is as described above. Compound E A The amount of additive per 100 parts by mass of raw material pulp is preferably 1 part by mass or more and 100,000 parts by mass or less, more preferably 2 parts by mass or more and 10,000 parts by mass or less, and even more preferably 5 parts by mass or more and 1,000 parts by mass or less.
[0030] -Sulfonic acid group- An etherification agent may be used to introduce a sulfoalkyl group. A compound having a reactive group and a sulfone group (compound E) is used as an etherification agent for introducing a sulfoalkyl group. B ) and, as an optional component, an alkali compound and a compound B selected from the above-mentioned urea and its derivatives are added to the raw pulp and reacted. This introduces sulfoalkyl groups into the raw pulp.
[0031] Examples of the reactive group include a halogenated alkyl group, a vinyl group, and an epoxy group (glycidyl group). Compound E, an etherifying agent B Examples of the sulfonate include sodium 2-chloroethanesulfonate, sodium vinylsulfonate, sodium p-styrenesulfonate, and 2-acrylamido-2-methylpropanesulfonic acid. Among them, compound E is preferred in terms of the efficiency of introducing substituents, and therefore the defibration efficiency, cost, and ease of handling. B is preferably sodium vinyl sulfonate. Furthermore, it is also preferable to use the above-mentioned compound B as an optional component, and the amount added is also preferably as described above.
[0032] It is preferable that the raw pulp is converted into alkali cellulose in advance or simultaneously with the reaction. The method for converting the raw pulp into alkali cellulose is as described above. Compound E B The amount of additive per 100 parts by mass of raw material pulp (dry mass) is preferably 1 part by mass or more and 100,000 parts by mass or less, more preferably 2 parts by mass or more and 10,000 parts by mass or less, and even more preferably 5 parts by mass or more and 1,000 parts by mass or less.
[0033] -Carboxyalkyl group- Etherification agents may be used to introduce carboxyalkyl groups. As an etherification agent for introducing a carboxyalkyl group, a compound having a reactive group and a carboxy group (compound E C ) is used, and an optional component is an alkali compound and a compound B selected from the above-mentioned urea and its derivatives, which are then added to the raw pulp and reacted. This introduces carboxyalkyl groups into the pulp raw material.
[0034] Examples of the reactive group include a halogenated alkyl group, a vinyl group, and an epoxy group (glycidyl group). Compound E, an etherifying agent C As the chloropropionic acid, monochloroacetic acid, sodium monochloroacetate, 2-chloropropionic acid, 3-chloropropionic acid, sodium 2-chloropropionate, and sodium 3-chloropropionate are preferred from the standpoint of efficiency of introducing substituents, and therefore defibration efficiency, cost, and ease of handling. Furthermore, it is also preferable to use the above-mentioned compound B as an optional component, and the amount added is also preferably as described above.
[0035] It is preferable that the raw pulp is converted into alkali cellulose in advance or simultaneously with the reaction. The method for converting the raw pulp into alkali cellulose is as described above. Compound E C The amount of additive per 100 parts by mass of raw material pulp (dry mass) is preferably 1 part by mass or more and 100,000 parts by mass or less, more preferably 2 parts by mass or more and 10,000 parts by mass or less, and even more preferably 5 parts by mass or more and 1,000 parts by mass or less.
[0036] (Cationizing agent) A cationic group may be introduced into the raw pulp using a cationic agent. As a cationic agent for introducing a cationic group, a compound having a reactive group and a cationic group (compound E D ) and, as an optional component, an alkali compound and a compound B selected from the above-mentioned urea and its derivatives are added to the raw pulp to carry out the reaction. This introduces cationic groups into the raw pulp.
[0037] Examples of the reactive group include a halogenated alkyl group, a vinyl group, and an epoxy group (glycidyl group). Examples of the cationic group include an ammonium group, a phosphonium group, a sulfonium group, etc. Among these, the cationic group is preferably an ammonium group. Compound E D As the alkyl group, glycidyl trimethyl ammonium chloride, 3-chloro-2-hydroxypropyl trimethyl ammonium chloride, etc. are preferred from the viewpoints of the efficiency of introducing a substituent, and therefore the defibration efficiency, cost, and ease of handling. Furthermore, it is also preferable to use the above-mentioned compound B as an optional component. The amount of addition is also preferably as described above.
[0038] It is preferable that the raw pulp is converted into alkali cellulose in advance or simultaneously with the reaction. The method for converting the raw pulp into alkali cellulose is as described above. Compound E DThe amount of additive per 100 parts by mass of raw material pulp (dry mass) is preferably 1 part by mass or more and 100,000 parts by mass or less, more preferably 2 parts by mass or more and 10,000 parts by mass or less, and even more preferably 5 parts by mass or more and 1,000 parts by mass or less.
[0039] <Process 1> In step 1, the raw pulp is contacted with an aqueous solution containing a reactant. The raw material pulp is preferably in the form of a sheet or a cut form of a sheet-like raw material pulp. The raw material pulp may be in a dry state, a wet state, or a slurry state, but it is preferable to use raw material pulp in a dry state or a wet state, and it is more preferable to use raw material pulp in a dry state, because this provides excellent uniformity of the reaction. The raw pulp may be contacted with the aqueous solution containing the reactant by immersing it in the aqueous solution containing the reactant, or may be contacted with the raw pulp by spraying or dropping the aqueous solution containing the reactant onto the raw pulp, and is not particularly limited. Prior to step 2, it is preferable to remove excess aqueous solution, and it is preferable to remove it by squeezing or filtration. When compound B is used, the reactant and compound B may be contacted with the raw pulp in the form of an aqueous solution, or an aqueous solution containing the reactant and an aqueous solution containing compound B may be contacted with the raw pulp simultaneously or separately. From the viewpoint of ease of production, however, it is preferable to contact the raw pulp with an aqueous solution containing the reactant and compound B. In addition, since compound B absorbs heat when it is dissolved in an aqueous solution, it is preferable to heat compound B when it is dissolved.
[0040] [Process 2] Step 2 is a step in which the raw pulp that has been contacted with an aqueous solution containing a reactant is heated at a temperature of 120° C. or higher to introduce ionic groups into the raw pulp. The heat treatment temperature is preferably selected so that ionic groups can be efficiently introduced while suppressing thermal decomposition and hydrolysis of the fiber, and is preferably 120°C or higher, more preferably 130°C or higher, more preferably 140°C or higher, and even more preferably 150°C or higher, and is preferably 300°C or lower, more preferably 250°C or lower. In addition, for the heat treatment, equipment having various heat media can be used, such as an agitation dryer, a rotary dryer, a disk dryer, a roll-type heating device, a drum-type heating device, a plate-type heating device, a fluidized bed dryer, a band-type dryer, a filtration dryer, a vibration fluidized dryer, an air flow dryer, a reduced pressure dryer, an infrared heating device, a far-infrared heating device, a microwave heating device, a high frequency drying device, or a dryer that uses heated steam. From the viewpoint of suppressing unevenness in the concentration of the reactant in the raw pulp and introducing ionic groups more uniformly onto the surface of cellulose fibers contained in the raw pulp, it is preferable to heat while stirring, etc. This is believed to be because it is possible to suppress the fact that when water molecules move to the surface of the raw pulp as the pulp is dried, the dissolved compound A is attracted to the water molecules by surface tension and similarly moves to the surface of the raw pulp (i.e., causing unevenness in the concentration of the reactant).
[0041] In addition, the heating device used in the heat treatment is preferably a device that can constantly discharge, to the outside of the device system, for example, moisture held by the slurry and moisture generated by the dehydration condensation reaction between the reactant and the hydroxyl groups contained in the cellulose in the raw pulp. Examples of such heating devices include ovens that use a blowing system, specifically, hot air dryers. By constantly discharging moisture from within the device system, the phosphorylation reaction can be promoted, and the hydrolysis reaction of ionic groups, particularly ionic groups introduced by ester bonds, which is the reverse reaction of phosphorylation, can be suppressed, and acid hydrolysis of the sugar chains in the raw pulp can also be suppressed. This makes it possible to obtain fine fibrous cellulose with a high axial ratio.
[0042] The heat treatment time is, for example, preferably 1 second or more and 300 minutes or less after the moisture is substantially removed from the raw pulp, more preferably 150 minutes or less, even more preferably 60 minutes or less, still more preferably 1000 seconds or less, particularly preferably 800 seconds or less, and more preferably 2 seconds or more, even more preferably 3 seconds or more, still more preferably 5 seconds or more, particularly preferably 10 seconds or more. In this embodiment, the amount of ionic groups introduced can be kept within a preferred range by setting the heating temperature and heating time within appropriate ranges.
[0043] The amount of ionic groups introduced into the raw pulp is, for example, preferably 0.10 mmol / g or more, more preferably 0.20 mmol / g or more, even more preferably 0.40 mmol / g or more, and particularly preferably 0.60 mmol / g or more per gram (mass) of cellulose fiber. The amount of ionic substituents introduced into the cellulose fiber is, for example, preferably 5.20 mmol / g or less, more preferably 3.65 mmol / g or less, and even more preferably 3.00 mmol / g or less per gram (mass) of cellulose fiber. Here, the denominator in the unit mmol / g is the counter ion of the ionic substituent, which is a hydrogen ion (H + By setting the amount of the ionic substituent introduced within the above range, it is possible to easily refine the fiber raw material and to increase the stability of the cellulose fiber.
[0044] The amount of ionic substituents introduced into cellulose fibers can be measured, for example, by neutralization titration after subjecting the cellulose fibers to microfine processing. In the measurement by neutralization titration, a slurry containing the obtained cellulose fibers is treated with a strongly acidic ion exchange resin, and then an alkali such as an aqueous sodium hydroxide solution is added to determine the change in pH, thereby measuring the amount introduced.
[0045] After completion of step 2 and before step 3, excess reaction reagents, by-products, etc. may be removed by washing with water and filtration. After completion of step 2 and before step 3, it is preferable to have at least one step selected from the group consisting of a washing step, an alkali treatment step, and an acid treatment step, and it is more preferable to have at least a washing step. <Cleaning process> A washing step can be carried out on the raw material pulp into which ionic groups have been introduced (hereinafter also referred to as "ionic group-introduced pulp"). The washing step is carried out, for example, by washing the ionic group-introduced pulp with water or an organic solvent. The washing step may be carried out after each step described below, and the number of washing steps carried out in each washing step is not particularly limited. In addition, the water and the organic solvent used in the washing step are preferably heated from the viewpoint of improving the washing efficiency.
[0046] <Alkaline treatment process> An alkali treatment step may be performed between step 2 and step 3. The method of the alkali treatment is not particularly limited, but may be, for example, a method in which the ionic group-introduced pulp is immersed in an alkali solution.
[0047] The alkaline compound contained in the alkaline solution is not particularly limited, and may be an inorganic alkaline compound or an organic alkaline compound. In this embodiment, it is preferable to use, for example, sodium hydroxide or potassium hydroxide as the alkaline compound because of its high versatility. The solvent contained in the alkaline solution may be either water or an organic solvent. Among them, the solvent contained in the alkaline solution is preferably a polar solvent including water or a polar organic solvent exemplified by alcohol, and more preferably an aqueous solvent including at least water. As the alkaline solution, for example, an aqueous sodium hydroxide solution or an aqueous potassium hydroxide solution is preferable because of its high versatility.
[0048] The temperature of the alkaline solution in the alkaline treatment step is not particularly limited, but is preferably, for example, from 5° C. to 80° C., and more preferably from 10° C. to 60° C. The immersion time of the ionic group-introduced pulp in the alkaline solution in the alkaline treatment step is not particularly limited, but is, for example, preferably from 5 minutes to 30 minutes, and more preferably from 10 minutes to 20 minutes. The amount of the alkaline solution used in the alkaline treatment is not particularly limited, but is, for example, preferably from 100 mass% to 100,000 mass%, and more preferably from 1,000 mass% to 10,000 mass%, based on the absolute dry mass of the ionic group-introduced pulp.
[0049] In order to reduce the amount of alkaline solution used in the alkaline treatment step, the ionic group-introduced pulp may be washed with water or an organic solvent after step 2 and before the alkaline treatment step. From the viewpoint of improving handleability, it is preferable to wash the alkaline-treated ionic group-introduced pulp with water or an organic solvent after the alkaline treatment step and before step 3.
[0050] <Acid treatment process> An acid treatment step may be provided between step 2 and step 3. For example, step 2, acid treatment step, alkali treatment step, and step 3 may be performed in this order. The method of acid treatment is not particularly limited, but may be, for example, a method of immersing the fiber raw material in an acidic solution containing an acid. The concentration of the acidic solution used is not particularly limited, but is preferably, for example, 10% by mass or less, and more preferably, 5% by mass or less. The pH of the acidic solution used is not particularly limited, but is preferably, for example, 0 to 4, and more preferably, 1 to 3. The acid contained in the acidic solution may be, for example, an inorganic acid, a sulfonic acid, a carboxylic acid, or the like. Examples of inorganic acids include sulfuric acid, nitric acid, hydrobromic acid, hydroiodic acid, hypochlorous acid, chlorous acid, chloric acid, perchloric acid, phosphoric acid, and boric acid. Examples of sulfonic acids include, for example, methanesulfonic acid, ethanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, and trifluoromethanesulfonic acid. Examples of carboxylic acids include, for example, formic acid, acetic acid, citric acid, gluconic acid, lactic acid, oxalic acid, and tartaric acid. Among these, it is particularly preferable to use hydrochloric acid or sulfuric acid.
[0051] The temperature of the acid solution in the acid treatment is not particularly limited, but is preferably, for example, 5° C. to 100° C., and more preferably, 20° C. to 90° C. The immersion time in the acid solution in the acid treatment is not particularly limited, but is preferably, for example, 5 minutes to 120 minutes, and more preferably, 10 minutes to 60 minutes. The amount of the acid solution used in the acid treatment is not particularly limited, but is preferably, for example, 100 mass% to 100,000 mass%, and more preferably, 1000 mass% to 10,000 mass%, based on the absolute dry mass of the fiber raw material.
[0052] [Step 3] Step 3 is a step of micronizing the raw pulp into which ionic groups have been introduced (ionic group-introduced pulp). In step 3, for example, a defibration treatment device can be used. The defibration treatment device is not particularly limited, but for example, a high-speed defibrator, a grinder (stone mill type grinder), a high-pressure homogenizer, an ultra-high-pressure homogenizer, a high-pressure collision type grinder, a ball mill, a bead mill, a disk type refiner, a conical refiner, a twin-shaft kneader, a vibration mill, a homomixer under high-speed rotation, an ultrasonic disperser, or a beater can be used. Among the above defibration treatment devices, it is more preferable to use a high-speed defibrator, a high-pressure homogenizer, or an ultra-high-pressure homogenizer, which are less affected by the grinding media and have less risk of contamination.
[0053] Step 3 may be performed in one stage using the above-mentioned defibration processing device, or may be performed in two stages consisting of a rough defibration step and a fine defibration step. When step 3 is carried out in two stages, it is preferable to carry out defibration using a refiner in the rough defibration step, and the refiner performs preliminary defibration of the ionic group-introduced pulp. The refiner is a device that beats the ionic group-introduced pulp, and by beating while applying a load, a shear force is imparted to the ionic group-introduced pulp, causing fluffing in the raw pulp and softening the fibers, thereby performing preliminary defibration.
[0054] The refiner is not particularly limited as long as it can beat the ionic group-introduced pulp, and any known refiner can be used. As the refiner, a conical type, double disc refiner (DDR), or single disc refiner (SDR) is preferable because it can efficiently apply shear force to the pulp fibers and advance preliminary defibration.
[0055] In the fine defibration step, it is preferable to use a high-pressure homogenizer. The high-pressure homogenizer is used to finely pulp fibers in a slurry, and is used as a dispersing machine that discharges the slurry or the like from fine holes at high pressure. The high-pressure homogenizer is a homogenizer that has the ability to discharge the slurry at a pressure of, for example, 10 MPa or more, preferably 100 MPa or more. By treating the ionic group-introduced pulp with a high-pressure homogenizer, collisions between pulp fibers, pressure differences, microcavitation, etc., occur, and defibration occurs effectively. This allows the number of treatments in the fine defibration step to be reduced (shortened), and the production efficiency of fine fibrous cellulose to be further improved.
[0056] In the defibration process, for example, the ionic group-introduced pulp is preferably diluted with a dispersion medium to form a slurry. As the dispersion medium, one or more selected from water and organic solvents such as polar organic solvents can be used. The polar organic solvent is not particularly limited, but for example, alcohols, polyhydric alcohols, ketones, ethers, esters, aprotic polar solvents, etc. are preferable. Examples of alcohols include methanol, ethanol, isopropanol, n-butanol, isobutyl alcohol, etc. Examples of polyhydric alcohols include ethylene glycol, propylene glycol, glycerin, etc. Examples of ketones include acetone, methyl ethyl ketone (MEK), etc. Examples of ethers include diethyl ether, tetrahydrofuran, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono n-butyl ether, propylene glycol monomethyl ether, etc. Examples of esters include ethyl acetate, butyl acetate, etc. Aprotic polar solvents include dimethylsulfoxide (DMSO), dimethylformamide (DMF), dimethylacetamide (DMAc), and N-methyl-2-pyrrolidinone (NMP).
[0057] The solids concentration of the fine fibrous cellulose during the defibration treatment can be appropriately set. Furthermore, the slurry obtained by dispersing the ionic group-introduced pulp may contain solid matter other than the ionic group-introduced pulp, such as urea having hydrogen bonding properties.
[0058] <Fine fibrous cellulose> The fine fibrous cellulose obtained by the production method of this embodiment is a fibrous cellulose having a fiber width of 1,000 nm or less. The fiber width of the fibrous cellulose can be measured, for example, by observation under an electron microscope. The fiber width of the fine fibrous cellulose is 1,000 nm or less. The fiber width of the fine fibrous cellulose is, for example, preferably 2 nm or more and 1,000 nm or less, more preferably 2 nm or more and 100 nm or less, even more preferably 2 nm or more and 50 nm or less, and particularly preferably 2 nm or more and 10 nm or less. By making the fiber width of the fine fibrous cellulose 2 nm or more, it is possible to suppress dissolution of the cellulose molecules in water, and to more easily realize the effect of improving the strength, rigidity, and dimensional stability of the fine fibrous cellulose.
[0059] The average fiber width of the fine fibrous cellulose is, for example, 1,000 nm or less. The average fiber width of the fine fibrous cellulose is preferably 2 nm or more and 1,000 nm or less, more preferably 2 nm or more and 100 nm or less, even more preferably 2 nm or more and 50 nm or less, and particularly preferably 2 nm or more and 10 nm or less. By making the average fiber width of the fine fibrous cellulose 2 nm or more, it is possible to suppress dissolution of the cellulose molecules in water, and to more easily realize the effect of improving the strength, rigidity, and dimensional stability of the fine fibrous cellulose. The fine fibrous cellulose is, for example, a single-fiber cellulose.
[0060] The average fiber width of fine fibrous cellulose is measured, for example, using an electron microscope as follows. First, an aqueous suspension of fibrous cellulose with a concentration of 0.05% by mass or more and 0.1% by mass or less is prepared, and this suspension is cast on a hydrophilically treated carbon film-coated grid to prepare a sample for TEM observation. When wide fibers are included, an SEM image of the surface cast on glass may be observed. Next, observation is performed using an electron microscope image at a magnification of 1,000x, 5,000x, 10,000x, or 50,000x depending on the width of the fiber to be observed. However, the sample, observation conditions, and magnification are adjusted to satisfy the following conditions. (1) A straight line X is drawn at any point within the observed image, and 20 or more fibers intersect with the straight line X. (2) Within the same image, draw a line Y that intersects the line perpendicularly, and 20 or more fibers intersect the line Y.
[0061] For observation images that satisfy the above conditions, the width of the fibers that intersect with lines X and Y is visually read. In this manner, three or more sets of observation images of at least the surface portions that do not overlap each other are obtained. Next, for each image, the width of the fibers that intersect with lines X and Y is read. In this manner, the width of at least 20 fibers x 2 x 3 = 120 fibers is read. The average value of the read fiber widths is then determined as the average fiber width of the fibrous cellulose.
[0062] The fiber length of the fine fibrous cellulose is not particularly limited, but is preferably 0.1 μm or more and 1,000 μm or less, more preferably 0.1 μm or more and 800 μm or less, and even more preferably 0.1 μm or more and 600 μm or less. By setting the fiber length within the above range, destruction of the crystalline region of the fine fibrous cellulose can be suppressed. In addition, it is also possible to set the slurry viscosity of the fine fibrous cellulose to an appropriate range. The fiber length of the fine fibrous cellulose can be determined by image analysis using, for example, TEM, SEM, or AFM.
[0063] The fine fibrous cellulose preferably has a type I crystal structure. The fact that the fine fibrous cellulose has a type I crystal structure can be identified from a diffraction profile obtained from a wide-angle X-ray diffraction photograph using CuKα (λ=1.5418 Å) monochromated with graphite. Specifically, it can be identified from the presence of typical peaks at two positions, around 2θ=14° to 17° and around 2θ=22° to 23°. The proportion of I-type crystal structure in the fine fibrous cellulose is, for example, preferably 30% or more, more preferably 40% or more, and even more preferably 50% or more. This is expected to provide even better performance in terms of heat resistance and low linear thermal expansion coefficient. The degree of crystallinity is determined by measuring an X-ray diffraction profile and using the pattern in a conventional manner (Seagal et al., Textile Research Journal, Vol. 29, p. 786, 1959).
[0064] The axial ratio (fiber length / fiber width) of the fine fibrous cellulose is not particularly limited, but is preferably, for example, 20 to 10,000, and more preferably 50 to 1,000. By setting the axial ratio to the above lower limit or more, a sheet containing the fine fibrous cellulose can be easily formed. In addition, sufficient viscosity can be easily obtained when a solvent dispersion is prepared. By setting the axial ratio to the above upper limit or less, it is preferable in that, for example, when the fine fibrous cellulose is treated as an aqueous dispersion, handling such as dilution is facilitated.
[0065] In the method for producing fine fibrous cellulose of this embodiment, the heat used in the step of introducing ionic groups into the raw material pulp (step 2) is used in any one of the production steps. The heat used in step 2 may be used as it is in any of the production steps, or the heat may be removed by water or gas, and the water or gas warmed by the heat removal may be used. The production method of this embodiment preferably includes a step of removing the heat used in step 2 by using water or a step of removing the heat by using a gas. More specifically, in this embodiment, the heated gas used in step 2 and water or gas are supplied to a heat exchanger (heat removal means). The heated gas supplied to the heat exchanger is cooled by heat exchange with the water or gas, while the water or gas supplied to the heat exchanger is heated by heat exchange with the heated gas used in step 2. The heated gas used in step 2 may be used as it is. However, since ammonia and the like derived from compound B are contained in the heated gas in step 2, it is preferable to heat water or gas using a heat exchanger and use the heated water or gas, rather than using the heated gas used in step 2 as it is. As the heat exchanger, a conventionally known one can be appropriately used, and various types such as a double-pipe heat exchanger, a multi-pipe heat exchanger, and a spiral heat exchanger can be used.
[0066] In the present embodiment, the water or gas heated by heat removal may be used in any step of the production of fine fibrous cellulose, but is preferably used in any of the steps below. 1. Heat the water used in the washing process after the process of introducing ionic groups into the raw pulp. By heating the water used in the water-washing step, impurities and the like can be removed more efficiently. Note that the water heated by the heat exchanger may itself be used in the water-washing step. 2. Heat the gas used in the process of introducing ionic groups into the raw pulp By using the heat used in step 2 again in step 2 via a heat exchanger, it is possible to produce fine fibrous cellulose using less energy. 3. In the preparation of the aqueous solution containing the reactant, the aqueous solution containing the reactant is heated. When the reactant is an esterifying agent and the above-mentioned compound B is used together with the esterifying agent, it is effective to heat the aqueous solution containing compound B. As described above, the reaction of dissolving compound B in water is an endothermic reaction, so that when dissolving compound B, it is preferable to heat the aqueous solution, and by utilizing the heat used in step 2 for preparing the aqueous solution containing compound B, fine fibrous cellulose can be produced with less energy. 4. Heating the obtained fine fibrous cellulose The obtained fine fibrous cellulose can be heated in the following ways (1) to (5), for example. (1) When the reactant is an esterifying agent, the ester groups can be eliminated by heating the fine fibrous cellulose, and the number of ionic groups introduced into the fine fibrous cellulose can be reduced, thereby producing fine fibrous cellulose with a reduced amount of ionic groups. (2) As described in WO 2020 / 080393, the resulting fine fibrous cellulose can be heated during enzyme treatment or subsequently heated to inactivate the enzyme in order to reduce the thixotropy and degree of polymerization of the resulting fine fibrous cellulose. (3) The fine fibrous cellulose is obtained in the form of a slurry, and can be used for heating to remove moisture in order to increase the concentration of the slurry. (4) When forming a sheet made of fine fibrous cellulose or a sheet containing the fine fibrous cellulose and a resin component, it can be used for heating in the process of drying a slurry containing the fine fibrous cellulose and optionally a resin component. (5) When various additives are mixed into the slurry of fine fibrous cellulose as required, heating can be used for the purpose of reducing the viscosity of the slurry of fine fibrous cellulose, improving the solubility of the additives, etc. Examples of additives include preservatives, ultraviolet protection agents, plasticizers, flame retardants, antistatic agents, and resins (e.g., hydrophilic resins such as polyvinyl alcohol and resin emulsions). [Industrial Applicability]
[0067] According to the method for producing fine fibrous cellulose of the present embodiment, fine fibrous cellulose can be produced with greater energy savings.
Claims
1. contacting the raw pulp with an aqueous solution containing a reactant; A step of heating at a temperature of 120° C. or higher to introduce ionic groups into the raw pulp; and The method includes, in this order, a step of micronizing the raw pulp into which the ionic group has been introduced, the reacting agent is an esterifying agent which introduces an anionic group into the raw pulp via an ester bond, an etherifying agent which introduces an anionic group into the raw pulp via an ether bond, or a cationizing agent; The heat used in the step of introducing ionic groups into the raw pulp is used in any one of the production steps. A method for producing fine fibrous cellulose.
2. 2. The method for producing fine fibrous cellulose according to claim 1, further comprising a heat removal step of removing heat used in the step of introducing ionic groups into the raw material pulp by using water or a heat removal step of removing heat by using a gas.
3. 3. The method for producing fine fibrous cellulose according to claim 2, wherein the water or gas heated in the heat removal step is used to heat water to be used in the water washing step following the step of introducing ionic groups into the raw pulp.
4. 3. The method for producing fine fibrous cellulose according to claim 2, wherein the water or gas heated in the heat removal step is used to heat the gas used in the step of introducing ionic groups into the raw material pulp.
5. 2. The method for producing fine fibrous cellulose according to claim 1, wherein the reacting agent is an esterifying agent which introduces anionic groups into the raw material pulp via ester bonds.
6. 2. The method for producing fine fibrous cellulose according to claim 1, wherein the reacting agent is an esterifying agent which introduces phosphorus oxoacid groups into the raw pulp via ester groups.
7. 6. The method for producing fine fibrous cellulose according to claim 5, further comprising a step of removing heat used in the step of introducing ionic groups into the raw material pulp by using water or a heat removal step of removing heat by using a gas in a heat exchanger, and heating an aqueous solution containing an esterifying agent by using the water or gas heated in the heat removal step.
8. The method for producing fine fibrous cellulose according to claim 5, wherein the aqueous solution containing the esterifying agent further contains urea or a derivative thereof.
Citation Information
Patent Citations
Cellulose nanofiber production device and method for producing cellulose nanofiber
JP2018048237A
Manufacturing method of phosphorus-oxo acid-oxidized pulp
JP2020165064A
Fine cellulose fiber
JP2008001728A
Method for manufacturing cellulose nano-fiber
JP2010235679A