Conductive ink, and method for producing conductive film
A two-step heat treatment process for a conductive ink with fine silver particles and blocked isocyanate addresses heat damage issues, achieving good adhesion and conductivity in forming electrical wiring on base materials.
Patent Information
- Application Number
- JP2023057616
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conductive inks used for forming electrical wiring on base materials, such as resin films, require multiple applications and heat treatments to sinter silver particles, which can cause heat damage to the base material.
A conductive ink containing fine silver particles, an amine with a hydroxyl group, and a blocked isocyanate, where the ink undergoes a two-step heat treatment: a first heat treatment at a temperature below the dissociation temperature of the blocked isocyanate, followed by a second heat treatment at a higher temperature to ensure adhesion and conductivity without excessive heat damage.
The method forms a conductive film with excellent adhesion and conductivity while minimizing heat damage to the base material, suitable for applications like film devices and printed electronics.
Smart Images

Figure 2024145324000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a conductive ink and a method for producing a conductive film. [Background technology]
[0002] By reducing the particle size to nanometer size, silver particles can be sintered at low temperatures due to a drop in the melting point. By utilizing this property, conductive inks containing silver particles can be used as materials for drawing electrical wiring on substrates.
[0003] Regarding conductive inks used in such fields, Patent Document 1 describes a method for producing silver nanoparticles by reacting a thermally decomposable silver compound (a) with an amine compound (b) that forms a complex, in which an amino alcohol that (i) has a linear structure, (ii) has one amino group and one hydroxyl group at each end of the linear molecule, and (iii) has one or more ether bonds within the linear structure is used as the amine compound. Patent Document 1 describes that by using such a specific amino alcohol, silver nanoparticles having a wide distribution and relatively large particle size can be easily obtained, and that silver nanoparticles in the large particle size range of 200 to 500 nm can be particularly easily synthesized.
[0004] Furthermore, Patent Document 1 describes a method for producing a silver coating composition, in which the obtained silver nanoparticles are dispersed in an organic solvent and an organic binder is further added. Cited document 1 also describes that a silver coating composition containing silver particles with controlled particle size can be sintered even at low temperatures below 150° C., and that the resulting sintered body exhibits a low resistance value close to that of bulk silver. Cited document 1 also describes that this silver coating composition is a material that can be used to form thick silver wiring of several to several tens of μm on a plastic substrate with relatively low heat resistance, such as PET or polypropylene, by a printing method such as screen printing. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2021-105218 A Summary of the Invention [Problem to be solved by the invention]
[0006] A conductive ink containing silver fine particles can be used as a material for forming electrical wiring on a substrate made of a resin film, etc. Therefore, it is used for forming electrical wiring that constitutes a film device. When forming electrical wiring on a base material, the electrical wiring is formed through at least a step of printing a conductive ink on a substrate and a step of heating at a predetermined temperature to sinter the silver particles. In the manufacturing method of the film device, the step of applying the conductive ink may be performed multiple times depending on the design of the film device. For example, when manufacturing a film device having electrical wiring on both sides of a substrate, a step of applying the conductive ink to one side of the substrate and a step of applying the conductive ink to the other side of the substrate may be performed separately.
[0007] In this way, when the step of applying the conductive ink is performed multiple times, a heat treatment for sintering the silver particles may be performed each time the conductive ink is applied to complete the electrical wiring. However, if the heat treatment for sintering the silver particles is performed each time the conductive ink is applied, the substrate is susceptible to damage by heat. Therefore, in the manufacturing method of the film device, it is desirable to perform the heat treatment at a low temperature and for a short time as possible.
[0008] In addition, for example, a roll-to-roll method may be adopted as a method for manufacturing a film device. In a manufacturing method using the roll-to-roll method, a conductive ink may be applied to an unwound substrate, the substrate may be wound into a roll, and then, in a separate process, a conductive ink may be applied again to the unwound substrate. In this case, the conductive ink applied to the substrate needs to be in close contact with the substrate. If the conductive ink is not in close contact with the substrate, the applied conductive ink may migrate to the surface of the substrate opposite to the ink-applied surface when the substrate is wound into a roll. Therefore, in order to make the applied conductive ink adhere to the substrate, a heat treatment may be performed to sinter the silver fine particles. However, if a heat treatment is performed to sinter the silver particles every time the conductive ink is applied, the base material becomes susceptible to damage from heat, as described above.
[0009] In light of this situation, in order to reduce heat damage to the substrate in a manufacturing method for film devices that involves applying conductive ink multiple times, we considered a method in which, after each application of conductive ink, a heating treatment is performed at a temperature lower than the temperature at which the silver microparticles are sufficiently sintered, so that the conductive ink adheres to the substrate to the extent that it does not peel off, and after completing the process of applying conductive ink multiple times, the silver microparticles are sufficiently sintered in a single heating treatment.
[0010] Therefore, we investigated a conductive ink that can exhibit good conductivity and also has excellent adhesion to the substrate by adhering it to the substrate through heat treatment at a temperature lower than the temperature at which the silver microparticles are sintered, and then baking it at a specified temperature. As a result, the present inventors discovered a novel conductive ink that satisfies these requirements, and completed the present invention. It was thought that it would be difficult to ensure sufficient adhesion to the substrate with the silver coating composition described in Patent Document 1. [Means for solving the problem]
[0011] (1) The conductive ink of the present invention contains silver fine particles, an amine having a hydroxyl group, and a blocked isocyanate, A method for producing a conductive film, comprising a first heating treatment for heating a conductive ink at a first heating temperature, and a second heating treatment for heating the conductive ink that has been subjected to the first heating treatment at a second heating temperature, The dissociation temperature of the blocked isocyanate is higher than the first heating temperature and is equal to or lower than the second heating temperature +10°C.
[0012] The conductive ink contains an amine having a hydroxyl group and a blocked isocyanate, and the blocked isocyanate has a predetermined dissociation temperature. Therefore, when the above-mentioned conductive ink is subjected to a first heating treatment, it becomes a coating film that is in close contact with the substrate, and when the above-mentioned conductive ink is subjected to a second heating treatment, it becomes a conductive film that has good conductivity and maintains its adhesion to the substrate.
[0013] (2) In the conductive ink of (1) above, it is preferable that the dissociation temperature of the blocked isocyanate is equal to or higher than the second heating temperature −20° C. and equal to or lower than the second heating temperature. (3) In the conductive ink of (1) or (2) above, it is preferable that the boiling point of the amine having a hydroxyl group is equal to or higher than the first heating temperature + 100°C and equal to or higher than the second heating temperature + 50°C and equal to or higher than the second heating temperature + 100°C. (4) In the conductive ink of any one of (1) to (3) above, the temperature difference between the first heating temperature and the second heating temperature is preferably 30° C. or more and 60° C. or less. In these cases, it is even more suitable to perform a first heating treatment to increase adhesion to the substrate, or to perform a second heating treatment to sufficiently sinter the silver microparticles while ensuring adhesion to the substrate.
[0014] (5) The method for producing a conductive film of the present invention comprises the steps of: (1) applying a conductive ink to a substrate; (2) heating the substrate coated with the conductive ink at a first heating temperature; and Step (3) of further heating the substrate after step (2) at a second heating temperature. Including, The conductive ink contains silver fine particles, an amine having a hydroxyl group, and a blocked isocyanate, the first heating temperature is lower than the dissociation temperature of the blocked isocyanate, The second heating temperature is equal to or higher than the dissociation temperature of the blocked isocyanate −10° C.
[0015] The above-mentioned method for producing a conductive film can form a conductive film having excellent electrical conductivity and adhesion to a substrate, while preventing the substrate from being damaged by heat. In the method for producing a conductive film according to (5) above, the conductive ink may be any one of the conductive inks according to (2) to (4) above. Effect of the Invention
[0016] The above conductive ink is adhered to a substrate by heat treatment at a temperature lower than the temperature at which the silver particles are sintered, and then baked at a predetermined temperature to form a conductive film that has good adhesion to the substrate and excellent conductivity. According to the method for producing a conductive film, a conductive film having good adhesion to a substrate and excellent conductivity can be formed. The method for producing a conductive film is less likely to damage the substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of the present invention will be described. (Conductive ink) The conductive ink according to the embodiment of the present invention contains silver fine particles, an amine having a hydroxyl group, and a blocked isocyanate. The silver particles are sintered by heating to form a conductive film. The amine having a hydroxyl group adheres to the surface of the silver particles and functions as a dispersant for the silver particles, and also binds to the blocked isocyanate from which the protective group has been removed and to the surface of the substrate through intermolecular forces or chemical bonds (collectively referred to as intermolecular forces, etc.), improving the adhesion of the applied conductive ink to the substrate.
[0018] The blocked isocyanate contributes to improving the adhesion between the substrate and the conductive film. When the protective group (blocking agent) of the blocked isocyanate is dissociated, the isocyanate group is activated and the isocyanate group is bonded to the substrate by intermolecular forces or the like, thereby improving the adhesion between the conductive film and the substrate. On the other hand, if the protective group of the blocked isocyanate dissociates before the silver particles are sintered, the sintering of the silver particles is inhibited, and the formed conductive film may have poor conductivity. Therefore, the conductive ink according to the embodiment of the present invention contains, as the blocked isocyanate, a blocked isocyanate having a predetermined dissociation temperature. The dissociation temperature of the blocked isocyanate is measured by differential scanning calorimetry (DSC). Specifically, the temperature of the endothermic peak associated with the deprotection reaction of the blocked isocyanate measured by differential scanning calorimetry corresponds to the dissociation temperature of the blocked isocyanate. In this case, for example, a differential scanning calorimeter (DSC 3500 Sirius) manufactured by NETZSCH can be used as the differential scanning calorimeter.
[0019] First, an example of a method for using the conductive ink will be described. The conductive ink may be, for example, (a) applying a conductive ink to a substrate (first step); (b) a first heating treatment (first time) for heating the conductive ink at a first heating temperature; (c) applying a conductive ink to the substrate (for the second time); (d) a first heating treatment (second time) for heating the conductive ink at a first heating temperature; and (e) a second heating treatment in which the conductive ink that has been subjected to the first heating treatment is heated at a second heating temperature; is carried out and used in a method for forming electrical wiring of a film device. By using the conductive ink in this manner, a conductive film can be produced.
[0020] The method of carrying out the above steps (a) to (e) is preferably used in a method for producing a film device in which the step of applying a conductive ink is carried out multiple times, such as when forming electrical wiring on both sides of a substrate or when a roll-to-roll method is employed.
[0021] Furthermore, in the method of using the conductive ink, for example, a step of applying the conductive ink to a substrate and a first heating treatment of heating the conductive ink at a first heating temperature may be defined as one set, and this step may be performed three or more sets.
[0022] In the above-mentioned method of using a conductive ink, the first heating temperature is set, for example, to 60° C. or higher and 120° C. or lower. In this case, it is suitable for adhering the applied conductive ink to the substrate. The second heating temperature is set, for example, to 120° C. or higher and 170° C. or lower. This is suitable for forming a conductive film in which the silver particles are sintered while suppressing damage caused by heat to the base material. The second heating temperature is higher than the first heating temperature, and the temperature difference between the first heating temperature and the second heating temperature is, for example, 30° C. or more and 60° C. or less. When the first heat treatment is carried out, the silver fine particles may not be sintered at all or may be sintered to a certain extent.
[0023] Next, the configuration of the conductive ink will be described. <Silver particles> The smaller the particle size of the silver particles, the more they tend to sinter at a lower temperature. The average primary particle size of the fine silver particles may be any size that allows sufficient sintering at the second heating temperature. For example, fine silver particles having an average primary particle size of 10 nm or more and 30 nm or less can be sufficiently sintered at 150°C. If the silver fine particles can be sintered at about 120° C. to 170° C., it is possible to form a conductive film (electrical wiring) while sufficiently suppressing damage caused by heat to the base material.
[0024] However, if the average primary particle diameter of the silver microparticles is too small, a large amount of dispersant is required to disperse the silver microparticles and maintain the ink properties, which may result in insufficient conductivity of the formed conductive film or make the formed conductive film more susceptible to cracks. Considering these points, the average primary particle size of the fine silver particles is preferably 10 nm or more and 30 nm or less.
[0025] The average primary particle size of the silver particles is determined by number average. Specifically, the silver particles are observed at a magnification of 200,000 times using a scanning electron microscope (S-4800 manufactured by Hitachi Ltd.), the primary particle size of the particles contained in the captured image is measured using image analysis software (WinROOF manufactured by MITANI CORPORATION), and the number average is calculated.
[0026] The content (concentration) of the silver particles in the conductive ink is, for example, 20% by mass or more and 65% by mass or less. If the content of the silver particles is 20% by mass or more, it is suitable for forming a conductive film with high conductivity.If the content of the silver particles is 65% by mass or less, the viscosity does not become too high and handling is easy. The content of the fine silver particles is preferably 25% by mass or more and 40% by mass or less.
[0027] The conductive ink may contain at least one type of metal particles other than silver in addition to the silver fine particles. By blending the metal particles other than silver, migration is less likely to occur in the conductive film formed by the conductive ink. As the metal other than silver, a metal whose ionization series is more noble than hydrogen is preferable. As the metal whose ionization series is more noble than hydrogen, gold, copper, platinum, palladium, rhodium, iridium, osmium, ruthenium, and rhenium are preferable, and gold, copper, platinum, and palladium are more preferable. These metals may be used alone or in combination of two or more kinds. The average primary particle size of the particles of a metal other than silver is preferably 10 nm or more and 30 nm or less.
[0028] <Amine having a hydroxyl group> The conductive ink contains an amine having a hydroxyl group.
[0029] A hydroxyl-containing amine has at least two polar groups (an amino group and a hydroxyl group) in one molecule, and therefore can act as a dispersant to disperse silver particles and also as a catalyst to generate chemical bonds and intermolecular forces between the blocked isocyanate and the substrate from which the protective groups have been removed. In addition, amines having hydroxyl groups have higher boiling points than alcohols having comparable molecular weights or amines having no hydroxyl groups, and therefore are less likely to disappear completely when the first heating treatment is performed, and tend to remain in an appropriate amount.
[0030] The boiling point of the amine containing a hydroxyl group is preferably equal to or higher than the first heating temperature + 100°C. If the boiling point is within this range, the amine containing a hydroxyl group remains in the coating film of the conductive ink to a suitable extent even after the first heating treatment. Therefore, chemical bonds or intermolecular forces can be formed between the substrate or the blocked isocyanate from which the protective group has been removed, which can contribute to improving the adhesion between the coating film of the conductive ink and the substrate after the first heating treatment. In addition, the boiling point of the amine containing a hydroxyl group is preferably the second heating temperature + 50°C or more and the second heating temperature + 100°C or less. In this case, the amine containing a free hydroxyl group is easily removed when the second heating process is performed. Therefore, the sintering of the silver particles is not inhibited, and a conductive film with good conductivity can be formed. In the present invention, the boiling point refers to the boiling point at 1 atmospheric pressure.
[0031] As the amine having a hydroxyl group, 2-(2-aminoethoxy)ethanol, 2-(2-aminoethylamino)ethanol, 2-[2-(2-aminoethoxy)ethoxy]ethanol, and monoethanolamine are preferred. The amine having a hydroxyl group may be used alone or in combination of two or more kinds.
[0032] The content (concentration) of the amine having a hydroxyl group is preferably 0.01% by mass or more and 2% by mass or less, which is suitable for achieving both the role of a dispersant for dispersing silver particles and the role of generating intermolecular forces between the substrate and the blocked isocyanate from which the protective group has been removed. On the other hand, if the content of amine having a hydroxyl group is less than 0.01% by mass, the silver particles cannot be stably dispersed and may aggregate. If the content exceeds 2% by mass, the amount of amine having a hydroxyl group remaining after baking the conductive ink (after performing the second heat treatment) becomes large, and the conductivity of the formed conductive film may become insufficient.
[0033] <Dispersants other than amines having a hydroxyl group> The conductive ink may contain a dispersant other than the amine having a hydroxyl group. Examples of the other dispersants include polymers having an acidic group and alkoxyamines.
[0034] The above-mentioned polymer having an acidic group can also play a role as a dispersant for dispersing the silver particles, and a role of generating intermolecular forces between the substrate and the blocked isocyanate from which the protective group has been removed. The polymer having an acidic group may be a homopolymer or a copolymer.
[0035] The content (concentration) of the polymer having the acidic group is preferably 0.01% by mass or more and 2% by mass or less, which is suitable for achieving both the role of a dispersant for dispersing silver particles and the role of generating intermolecular forces between the substrate and the blocked isocyanate from which the protective group has been removed. On the other hand, if the content of the polymer having an acidic group is less than 0.01% by mass, the silver particles cannot be stably dispersed and may aggregate, and if the content exceeds 2% by mass, a large amount of the polymer having an acidic group remains after the silver particles are sintered (after the second heat treatment), which may cause a loss of conductivity of the formed conductive film.
[0036] The above-mentioned polymer having an acidic group preferably has an acid value of 5 or more and 200 or less. When the acid value of the polymer having an acidic group is 5 or more, the polymer starts to adsorb to the fine silver particles, which are coordinated with amines and have a basic particle surface, through acid-base interaction.When the acid value is 200 or less, the polymer does not have an excessive number of adsorption sites, and is adsorbed to the fine silver particles in a suitable form.
[0037] The polymer having the acidic group is preferably one having a functional group derived from phosphoric acid as the acidic group. In this case, phosphorus (P) interacts with and attracts silver via oxygen (O), so the polymer having a functional group derived from phosphoric acid is suitable for adsorbing silver or a silver compound, and can ensure suitable dispersibility of silver particles with the minimum necessary amount of adsorption.
[0038] As the above-mentioned polymer having an acidic group, a commercially available product can be used. Commercially available products of the polymer having the above acidic group include, for example, DISPERBYK-102, DISPERBYK-106, DISPERBYK-110, DISPERBYK-111, DISPERBYK-118, DISPERBYK-140, DISPERBYK-142, DISPERBYK-145, DISPERBYK-180 (all manufactured by BYK Japan), SOLSPERSE 36000, SOLSPERSE 36600, SOLSPERSE 41000, SOLSPERSE 41090, SOLSPERSE 43000, SOLSPERSE 44000, SOLSPERSE 46000, SOLSPERSE Examples of such compounds include Disparlon 55000 (all manufactured by Lubrizol Japan), Disparlon 1831, Disparlon 1850, Disparlon 1860, Disparlon 2150, Disparlon PW-36, Disparlon DA-1200 (all manufactured by Kusumoto Chemical Industry), Floren AF-1000, Floren AF-1005, Floren G-700, and Floren GW-1500 (all manufactured by Kyoeisha Chemical Industry). These may be used alone or in combination of two or more.
[0039] As described above, the conductive ink may further contain an alkoxyamine as a dispersant. When an alkoxyamine is contained, the conductive ink containing silver particles has good low-temperature sintering properties. In addition, the size (primary particle diameter) of the silver particles is easily adjusted during the production of the conductive ink. For example, when silver particles are produced in the presence of an alkoxyamine, it is easy to narrow the particle size distribution of the silver particles or to reduce the size of the silver particles. The alkoxyamine is preferably an alkoxyamine having a carbon number of 6 or less. Here, the carbon number of the alkoxyamine is the carbon number not including the alkoxy group, which is a functional group.
[0040] Examples of the alkoxyamine include 2-methoxyethylamine, 3-methoxypropylamine, 3-ethoxypropylamine, 3-propoxypropylamine, 3-butoxypropylamine, 2-ethoxypropylamine, 3-isopropoxypropylamine, 2-methoxy-2-methylpropylamine, and N-(3-methoxypropyl)propane-1,3-diamine.
[0041] The conductive ink may contain, as the other dispersant, an amine other than the amine having a hydroxyl group and the alkoxyamine.
[0042] <Blocked isocyanate> A blocked isocyanate is an isocyanate compound (isocyanate component) in which the isocyanate group is protected with a blocking agent. The blocked isocyanate remains stable under normal conditions (when it is blended into a conductive ink and the conductive ink is not heated), and when it is heat-treated, the blocking agent dissociates and active isocyanate groups are regenerated.
[0043] The amine having a hydroxyl group has an amino group and a hydroxyl group in the molecule. The amino group and / or the hydroxyl group can form a chemical bond with the isocyanate group of the blocked isocyanate from which the protecting group has been removed. In addition, the blocked isocyanate from which the protecting group has been removed forms intermolecular forces between the block and the substrate, and is therefore more likely to exhibit adhesion to the substrate. Therefore, the conductive ink containing the blocked isocyanate sinters the fine silver particles to form a conductive film, and the formed conductive film exhibits good adhesion to the substrate.
[0044] The blocked isocyanate is a reaction product between an isocyanate compound and a blocking agent. The isocyanate compound may be any compound having an isocyanate group, and is preferably one having two or more isocyanate groups. The above isocyanate compound more preferably has two isocyanate groups. As the blocked isocyanate, a known blocked isocyanate can be used.
[0045] The blocked isocyanate is preferably a reaction product of an isocyanate compound having a hydrocarbon group and a plurality of isocyanate groups, such as an aliphatic polyisocyanate, an alicyclic polyisocyanate, or an aromatic polyisocyanate (hereinafter also referred to as a hydrocarbon polyisocyanate), with a blocking agent.
[0046] Examples of the aliphatic polyisocyanate include 1,4-tetramethylene diisocyanate, 1,5-pentamethylene diisocyanate, 1,6-hexamethylene diisocyanate (HDI), 2,2,4-trimethylhexamethylene diisocyanate, and their isocyanurate modified products, prepolymer modified products, biuret modified products, and allophanate modified products.
[0047] Examples of the alicyclic polyisocyanate include isophorone diisocyanate (IPDI), 1,3-bis(isocyanatemethyl)-cyclohexane, 4,4'-dicyclohexylmethane diisocyanate, 1,4-cyclohexane diisocyanate, norbornane diisocyanate (NBDI), and their isocyanurate modified products, prepolymer modified products, biuret modified products, and allophanate modified products.
[0048] Examples of the aromatic isocyanate include tolylene diisocyanate (TDI), phenylene diisocyanate, 4,4'-diphenylmethane diisocyanate (MDI), 1,5-naphthalene diisocyanate, xylylene diisocyanate (XDI), 4,4'-diisocyanate-3,3'-dimethylbiphenyl, 1,3-bis(2-isocyanate-2-propyl)benzene, and isocyanurate-modified, prepolymer-modified, biuret-modified, and allophanate-modified versions of these.
[0049] As the blocking agent, known blocking agents such as alkyl ketone oximes, phenols, alcohols, β-diketones, and lactams can be used. Specific examples of the blocking agent include methyl ethyl ketone oxime, ε-caprolactam, phenol, cresol, acetylacetone, diethyl malonate, isopropyl alcohol, tert-butyl alcohol, and maleic acid imide. As the blocking agent, dialkyl ketone oximes such as methyl ethyl ketone oxime, lactams such as ε-caprolactam, etc. are preferred, because they are suitable for producing blocked isocyanates having a dissociation temperature of 80° C. or higher and 150° C. or lower.
[0050] When the blocked isocyanate is a reaction product of a hydrocarbon polyisocyanate and a blocking agent, the hydrocarbon polyisocyanate is preferably an aliphatic polyisocyanate or an alicyclic polyisocyanate rather than an aromatic polyisocyanate. Aliphatic polyisocyanates and alicyclic polyisocyanates are not as reactive as aromatic isocyanates, and form an appropriate three-dimensional structure in the second heating treatment to sinter the silver particles, so that the conductivity of the conductive film is less likely to be impaired.
[0051] Furthermore, the hydrocarbon polyisocyanate is preferably an aliphatic polyisocyanate rather than an alicyclic polyisocyanate, since aliphatic polyisocyanates are more likely to achieve both electrical conductivity and bending resistance. In the aliphatic polyisocyanate, the hydrocarbon group may be linear or may have a branched chain, but is preferably linear. When an aliphatic polyisocyanate having a linear hydrocarbon group is used as the aliphatic polyisocyanate, it is easy to ensure the flexibility of the conductive film formed by using the conductive ink. Hexamethylene diisocyanate is particularly preferred as the aliphatic polyisocyanate, as it is particularly suitable for ensuring good electrical conductivity and good bending resistance in the formed conductive film.
[0052] The dissociation temperature of the blocked isocyanate is higher than the first heating temperature and is equal to or lower than the second heating temperature +10°C. In this case, the protective group is not dissociated much in the first heating treatment, and most of the protective group is dissociated in the second heating treatment. Therefore, the reaction easily proceeds in parallel with the sintering of the silver particles, and the formed conductive film has good adhesion to the substrate. The dissociation temperature of the blocked isocyanate is preferably the second heating temperature −20° C. or more and the second heating temperature or less. In this case, the protecting group is less likely to dissociate in the first heating treatment and more likely to dissociate in the second heating treatment.
[0053] As the blocked isocyanate, commercially available products can also be used. Commercially available examples of the blocked isocyanate include Takenate B-882N, Takenate B-890, Takenate B-7005 (all manufactured by Mitsui Chemicals, Inc.), Duranate MF-K60B, Duranate SBB-70P, Duranate SBN-70D, Duranate 17B-60P, Duranate E402-B80B, Duranate TPA-B80E, Duranate WM44-L70G (all manufactured by Asahi Kasei Corporation), and Coronate BI-301 (manufactured by Tosoh Corporation).
[0054] The content (concentration) of the blocked isocyanate is preferably 0.5% by mass or more and 4% by mass or less, which is suitable for ensuring the adhesion of the formed conductive film to the substrate by generating an intermolecular force between the substrate and the like. If the content of the blocked isocyanate is less than 0.5% by mass, the adhesion between the formed conductive film and the substrate is not significantly improved, whereas if the content of the blocked isocyanate is more than 4% by mass, the amount of the isocyanate compound contained in the formed conductive film becomes too large, which may result in a decrease in conductivity.
[0055] <Dispersion medium> The conductive ink may further contain a dispersion medium. As the solvent, for example, various highly polar solvents can be used. Examples of the highly polar solvent include methanol, ethanol, 1-propanol, isopropanol, 1-butanol, isobutanol, 2-butanol, tert-butanol, isoamyl alcohol, furfuryl alcohol, nitromethane, acetonitrile, pyridine, acetone cresol, dimethylformamide, dioxane, ethylene glycol, glycerin, phenol, p-cresol, propyl acetate, isopropyl acetate, 1-methoxy-2-propanol, 1- Examples of the alcohol include pentanol, 2-pentanol, 4-methyl-2-pentanol, 3-methyl-1-pentanol, 2-methyl-2,4-pentanediol, 3-methyl-2-pentanol, 1-hexanol, 2-hexanol, 2-pentanone, 2-heptanone, dipropylene glycol, 2-(2-ethoxyethoxy)ethyl acetate, 2-butoxyethyl acetate, 2-(2-butoxyethoxy)ethyl acetate, 2-methoxyethyl acetate, and 2-hexyloxyethanol. Among these, alcohols having 1 to 6 carbon atoms are preferred because it is easy to avoid attacking the substrate when the conductive ink is applied to the substrate. The above dispersion medium may be used alone or in combination of two or more kinds.
[0056] The boiling point of the dispersion medium is preferably at least the first heating temperature + 30° C. If the boiling point of the dispersion medium is in this range, it is possible to prevent the conductive ink from drying excessively after application and before the first heating treatment.
[0057] The content (concentration) of the dispersion medium relative to the entire conductive ink is preferably 27% by mass or more and 79% by mass or less. If the concentration of the dispersion medium is 27% by mass or more, the conductive ink will not become too viscous and will be easy to handle.If the content of the dispersion medium is 79% by mass or less, the conductive film formed will tend to have sufficient conductivity.
[0058] The conductive ink may contain other components besides the silver particles, the amine having a hydroxyl group, other dispersants, the blocked isocyanate, and the dispersion medium, as long as the effects of the present invention are not impaired. Examples of the other components include a surfactant, an antifoaming agent, etc. Addition of a surfactant or an antifoaming agent makes it easier to form a uniform conductive film. The surfactant is not particularly limited, and anionic surfactants, cationic surfactants, and nonionic surfactants can be used.
[0059] In the conductive ink, the total amount of the silver particles, the amine having a hydroxyl group, the blocked isocyanate, and the dispersion medium is preferably 98% by mass or more, and more preferably 99% by mass, based on the entire conductive ink. The conductive ink may be composed of only silver particles, an amine having a hydroxyl group, a blocked isocyanate, and a dispersion medium.
[0060] In the conductive ink, the content of each of the constituent components can be measured, for example, by carrying out thermogravimetric analysis in which the temperature is raised from room temperature to 550° C. in the atmosphere.
[0061] Next, a method for producing the conductive ink will be described. The method for producing the conductive ink is not particularly limited, and examples thereof include the following methods. First, silver particles having at least a hydroxyl group-containing amine attached to the surface are prepared. The obtained silver particles are then dispersed in a dispersion medium together with a blocked isocyanate. Through these steps, the conductive ink is obtained. In the step of dispersing the silver particles in the dispersion medium, a dispersant may be added to the dispersion medium as necessary.
[0062] An example of a method for producing silver microparticles having an amine having a hydroxyl group attached to their surface includes a method including a first step of preparing a mixed solution of an amine and a silver compound that can be decomposed by reduction to produce silver, and a second step of reducing the silver compound in the mixed solution to produce silver microparticles having an amine attached to at least a portion of their surface. In addition, if an amine having a hydroxyl group is not mixed as the amine in the first step, an amine having a hydroxyl group is added after the second step and adhered to the surface of the silver particles.
[0063] In the first step, the total amount of amine added is preferably 2 mol or more per mol of silver atom. By adding 2 mol or more of amine per mol of silver atom, an appropriate amount of the amine can be attached to the surface of the silver fine particles generated by reduction, and the silver fine particles can be provided with excellent dispersibility in various dispersion media and low-temperature sinterability.
[0064] When the conductive ink to be produced contains a polymer having an acidic group, the polymer having an acidic group may be added together with the amine in the first step. In this case, the amount of the polymer having an acidic group added in the first step is preferably 0.03 parts by mass or more and 0.2 parts by mass or less per part by mass of the silver compound. If the amount of the polymer having an acidic group added per part by mass of the silver compound is more than 0.2 parts by mass, the conductivity of the formed conductive film may deteriorate, and if it is less than 0.03 parts by mass, the effect of dispersing silver fine particles may not be obtained.
[0065] The composition of the mixed solution in the first step and the reduction conditions in the second step (e.g., heating temperature and heating time) are adjusted so that the particle size of the resulting silver particles is nanometer-sized. This causes a drop in the melting point of the silver particles, making low-temperature firing possible. In producing the conductive ink, it is preferable to adjust the average primary particle size of the silver particles to 10 nm or more and 30 nm or less.
[0066] A colloidal solution containing silver particles is obtained by carrying out the reduction reaction in the second step. After the reduction reaction, an amine may be added to adjust the composition of the colloidal solution. In addition to the silver particles, the colloidal solution contains a dispersant (e.g., an amine having a hydroxyl group) and the like, and the electrolyte concentration of the entire solution tends to be high. In a colloidal solution in such a state, the silver particles tend to coagulate and precipitate due to high electrical conductivity, etc. Therefore, it is preferable to carry out the next step of washing the colloidal solution to remove excess electrolyte.
[0067] As a method for washing the colloidal liquid, for example, the colloidal liquid may be left to stand for a certain period of time, the supernatant liquid may be removed, pure water or a lower alcohol (e.g., methanol) may be added and stirred, and the colloidal liquid may be further left to stand for a certain period of time, after which the process of removing the supernatant liquid may be repeated several times. Other washing methods include, for example, a method of performing centrifugation instead of the above-mentioned standing, and a method of desalting using an ultrafiltration device, an ion exchange device, etc. Among them, the desalting method is preferable. The desalted liquid may be appropriately concentrated.
[0068] As the silver compound, various known silver compounds can be used, for example, silver salts or hydrates of silver salts can be used.Specific examples include silver salts such as silver nitrate, silver sulfate, silver chloride, silver oxide, silver acetate, silver oxalate, silver formate, silver nitrite, silver chlorate, and silver sulfide.These are not particularly limited as long as they are reducible, and may be dissolved in a suitable solvent or used as dispersed in the solvent.In addition, these may be used alone or in combination of two or more.
[0069] The silver compound is preferably silver oxalate. Silver oxalate is the simplest silver dicarboxylate, and the silver oxalate amine complex synthesized using silver oxalate is suitable for the synthesis of nanometer-sized silver particles because it undergoes reduction at low temperature and in a short time. Furthermore, when silver oxalate is used, no by-products are generated during synthesis, and only carbon dioxide derived from oxalate ions is generated outside the system, so there is little effort required for purification after synthesis.
[0070] The method of reducing the silver compound is preferably a heating method. The heating method is not particularly limited. The method of reducing the silver compound by heating includes, for example, a method of heating a complex compound generated from a silver compound such as silver oxalate and an amine, and decomposing a metal compound such as oxalate ion contained in the complex compound to generate atomic silver, which is aggregated. By the above method, silver fine particles having amine attached to the surface can be produced.
[0071] The particle size of the resulting silver microparticles can be controlled, for example, by adjusting the compounding ratio of the materials. In addition, when the silver compound is reduced by heating, the particle size can also be controlled by adjusting the heating conditions. Specifically, for example, when synthesizing fine silver particles having an average primary particle size of 10 nm or more and 30 nm or less, the temperature rise rate during heating is preferably 5° C. / min or more and 30° C. / min or less. In this case, examples of the heating method include a method using a thermostatic bath, an oil bath, various heaters, a microwave, a hot plate, etc. The heating method is preferably a method that can control the heating conditions while actually measuring the temperature of the reaction solution. In addition, in order to stably produce silver fine particles having a predetermined particle size, the heating method is preferably a method that can set a temperature program.
[0072] Thus, in the metal amine complex decomposition method in which a complex compound of a silver compound is thermally decomposed in the presence of an amine to produce silver fine particles with an amine attached to the surface, atomic silver is generated by the decomposition reaction of a silver amine complex, which is a single type of molecule. Therefore, it is possible to generate atomic silver uniformly in the reaction system, and compared to the case in which silver atoms are generated by the reaction between multiple components, the non-uniformity of the reaction caused by composition fluctuations of the components that make up the reaction is suppressed, which is particularly advantageous when producing large amounts of silver powder on an industrial scale.
[0073] In addition, in the metal amine complex decomposition method, amine molecules are coordinated to the silver atoms produced, and it is presumed that the movement of the silver atoms during aggregation is controlled by the action of the amine molecules coordinated to the silver atoms. As a result, the metal amine complex decomposition method makes it possible to produce very fine metal particles (silver fine particles) with a narrow particle size distribution.
[0074] Furthermore, amine molecules are coordinately bonded to the surface of the produced silver particles, and these form a protective coating on the surface of the silver particles, making it possible to produce silver particles with excellent storage stability. Furthermore, since the amine molecules that form the protective coating can be easily eliminated by heating or the like, it is possible to produce fine silver particles that can be sintered at extremely low temperatures.
[0075] Next, the obtained silver particles are dispersed in a dispersion medium together with a blocked isocyanate to obtain the conductive ink. At this time, a dispersant may be added to the dispersion medium as necessary. Specifically, for example, a silver slurry obtained by washing the colloidal liquid containing the fine silver particles obtained in the second step is dispersed in a dispersion medium such as an alcohol having 1 to 6 carbon atoms together with a blocked isocyanate.
[0076] The method for dispersing the silver slurry or the blocked isocyanate in the dispersion medium is not particularly limited, and can be carried out by a conventionally known method using, for example, a mixer, a stirrer, etc. Alternatively, the mixture may be stirred with a spatula or the like, and an ultrasonic homogenizer with an appropriate output may be applied.
[0077] (Method of manufacturing conductive film) The method for producing a conductive film according to an embodiment of the present invention includes the steps of: (1) applying a conductive ink to a substrate; (2) heating the substrate coated with the conductive ink at a first heating temperature; and Step (3) of further heating the substrate after step (2) at a second heating temperature. Including, The conductive ink contains silver fine particles, an amine having a hydroxyl group, and a blocked isocyanate, the first heating temperature is lower than the dissociation temperature of the blocked isocyanate, The second heating temperature is equal to or higher than the dissociation temperature of the blocked isocyanate −10° C.
[0078] The conductive film manufacturing method can be carried out by using the conductive ink according to an embodiment of the present invention. The above-mentioned method for producing a conductive film can be suitably used in the fields of film devices, printed electronics, and the like. The conductive film produced by the above-mentioned method for producing a conductive film can be used as wiring, electrodes, and the like for electronic circuit boards (for example, semiconductor integrated circuits), printed wiring boards, and thin film transistor substrates.
[0079] In the method for producing the conductive film, the steps (2) and (3) are carried out separately. Here, being carried out separately means that (i) after heating at the first heating temperature is terminated, the temperature of the substrate is reduced to below the first heating temperature, and then heated at the second heating temperature; or (ii) being held at the first heating temperature for a period of time and then being heated at a second heating temperature; means... On the other hand, when a heat treatment is performed in which the substrate coated with the conductive ink is continuously heated from a temperature lower than the first heating temperature to the second heating temperature, this does not correspond to step (2) and step (3) being performed separately.
[0080] Specific examples of performing step (2) and step (3) separately include, for example, performing step (2) and step (3) in different firing furnaces, performing step (3) a predetermined time after performing step (2), and the like.
[0081] Examples of materials for the substrate include resin materials such as polycarbonate (PC), acrylonitrile-butadiene-styrene copolymer (ABS), acrylonitrile-styrene copolymer (AS), polypropylene (PP), polyethylene (PE), cycloolefin polymer (COP), polyamide (PA), polyacetal (POM), polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polyphenylene sulfide (PPS), polyether ether ketone (PEEK), polystyrene (PS), polymethyl methacrylate (PMMA), polyphenylene ether (PPE), polysulfone (PSF), polyethersulfone (PES), polyamideimide (PAI), polyetherimide (PEI), polyimide (PI), and polyvinyl chloride (PVC). The material of the substrate may be, for example, an ink-absorbent material such as paper, fabric, porous ceramics, etc. Here, the ink-absorbent material means a material having a structure with an ink-receiving function. The above resin material is classified as an ink non-absorbent material.
[0082] The surface of the substrate may be provided with a surface layer (primer layer) for the purpose of enhancing adhesion to the conductive film, or may be subjected to a surface treatment such as hydrophilization treatment. Examples of the surface treatment method include dry treatments such as corona treatment, plasma treatment, UV treatment, and electron beam treatment.
[0083] The above-mentioned coating is a concept that includes both the case where the conductive ink is applied in a planar shape and the case where the conductive ink is applied (drawn) in a linear shape. The shape of the coating film (including the conductive film) may be planar, linear, or a combination of these. In addition, the coating film (conductive film) may be a continuous pattern, a discontinuous pattern, or a combination of these.
[0084] The method for applying the conductive ink is not particularly limited, and examples thereof include inkjet printing, screen printing, letterpress printing, intaglio printing, reverse printing, microcontact printing, dipping, spraying, bar coating, spin coating, dispenser method, casting, flexography, gravure, syringe method, and brush coating.
[0085] The heating time in the above step (2) is not particularly limited, and is, for example, 15 to 60 minutes. The heating conditions in the above step (2) can be selected, for example, from conditions in which the sample is placed in an oven preset to a first heating temperature, conditions in which the sample is heated from room temperature to the first heating temperature at a heating rate of 5°C / min and then maintained at the first heating temperature, and the like.
[0086] The heating time in the above step (3) is not particularly limited, and is, for example, 15 to 60 minutes. The heating conditions in the above step (3) can be selected, for example, from a condition in which the sample is placed in an oven preset to the second heating temperature, or a condition in which the sample is heated from a temperature below the first heating temperature to the second heating temperature at a heating rate of 5°C / min and then maintained at the second heating temperature. The heat treatment in the above steps (2) and (3) can be carried out, for example, by a method using a conventionally known constant temperature dryer, reflow furnace, or the like.
[0087] The conductive film has a thickness of, for example, 0.1 μm to 5 μm, and preferably 0.2 μm to 3 μm.The conductive film has a volume resistivity of, for example, 40 μΩ·cm or less. EXAMPLES
[0088] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0089] The blocked isocyanates used in the examples and comparative examples are as follows. (Blocked isocyanate) (1) Duranate E402-B80B (manufactured by Asahi Kasei Corporation): Contains about 80% by mass of blocked hexamethylene diisocyanate, which is a blocked isocyanate. The blocking agent is methyl ethyl ketone oxime. The dissociation temperature of the protecting group is 130°C. (2) Takenate B-890 (manufactured by Mitsui Chemicals): Contains about 60% by mass of blocked xylylene diisocyanate, which is a blocked isocyanate. The dissociation temperature of the protecting group is 150°C.
[0090] Example 1 1g of DISPERBYK-118 (Big Chemie Japan) and 100g of 2-(2-aminoethoxy)ethanol (Fujifilm Wako Pure Chemical Industries) were weighed into a 10L glass container and thoroughly mixed. 30g of silver oxalate (Toyo Kagaku Kogyo) was added and further mixed to obtain a viscous substance. The obtained viscous substance was heated to 100°C for 5 minutes to allow the reduction reaction to proceed. After the reduction reaction, 100 ml of methanol (manufactured by Fujifilm Wako Pure Chemical Industries) was added to the reaction solution, which was then stirred and centrifuged twice to remove excess organic components. This was then dried for 20 minutes, after which 30 g of dispersion medium was added. As the dispersion medium, 15 g of dipropylene glycol (manufactured by Fujifilm Wako Pure Chemical Industries) and 15 g of 4-methyl-2-pentanol (manufactured by Fujifilm Wako Pure Chemical Industries) were used. After stirring to disperse the silver particles, the mixture was centrifuged to remove coarse particles, and the supernatant was collected. 0.7 g of Duranate E402-B80B was added to the supernatant and stirred to obtain conductive ink 1.
[0091] Example 2 1 g of DISPERBYK-102 (Big Chemie Japan), 80 g of 3-methoxypropylamine (Tokyo Chemical Industry Co., Ltd.), and 100 g of 2-(2-butoxyethoxy)ethyl acetate (Fujifilm Wako Pure Chemical Industries, Ltd.) were weighed into a 10 L glass container and mixed thoroughly. 30g of silver oxalate was added and further stirred to obtain a viscous substance. The obtained viscous substance was heated to 100°C for 5 minutes to allow the reduction reaction to proceed. Then, 85g of 2-(2-aminoethoxy)ethanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added and stirred for 10 minutes. 100ml of methanol was further added to the reaction solution to which 2-(2-aminoethoxy)ethanol had been added, stirred, and centrifuged twice to remove excess organic components. After drying for 20 minutes, 30g of dispersion medium was added. As the dispersion medium, 15g of 2-methyl-2,4-pentanediol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 15g of 4-methyl-2-pentanol were used. After stirring and dispersing the silver fine particles, the mixture was centrifuged to remove coarse particles, and the supernatant was collected. 0.7g of Duranate E402-B80B was added to the supernatant and stirred to obtain conductive ink 2.
[0092] Example 3 Conductive ink 3 was obtained in the same manner as in Example 2, except that the amount of DISPERBYK-102 was changed to 2 g, and 80 g of 3-methoxypropylamine was changed to 68 g of 3-ethoxypropylamine (manufactured by Tokyo Chemical Industry Co., Ltd.).
[0093] Example 4 Conductive ink 4 was obtained in the same manner as in Example 2, except that 0.7 g of Duranate E402-B80B was changed to 1.0 g of Takenate B-890, and 4-methyl-2-pentanol was changed to 2-butoxyethanol.
[0094] Example 5 Conductive ink 5 was obtained in the same manner as in Example 2, except that 2-(2-aminoethoxy)ethanol was changed to 2-(2-aminoethylamino)ethanol (manufactured by Tokyo Chemical Industry Co., Ltd.).
[0095] Example 6 Conductive ink 6 was obtained in the same manner as in Example 1, except that the amount of each dispersion medium (dipropylene glycol and 4-methyl-2-pentanol) was changed from 15 g to 5 g.
[0096] Comparative Example 1 Conductive ink 7 was obtained in the same manner as in Example 2, except that 2-(2-aminoethoxy)ethanol was not added.
[0097] Comparative Example 2 Conductive ink 8 was obtained in the same manner as in Example 2, except that no blocked isocyanate was added.
[0098] Comparative Example 3 Conductive ink 9 was obtained in the same manner as in Example 1, except that 0.7 g of Duranate E402-B80B was changed to 0.5 g of EPICLON 850 (bisphenol A type epoxy resin, manufactured by DIC Corporation).
[0099] <Evaluation> The average primary particle size and the concentration of the silver particles contained in the conductive ink were measured. Furthermore, evaluation samples were prepared and then subjected to various evaluations. The results are shown in Table 1.
[0100] (Particle size measurement) The conductive inks prepared in the examples and comparative examples were observed for silver microparticles at a magnification of 200,000 times using a scanning electron microscope (Hitachi S-4800 model), and the particle diameters of the microparticles contained in the captured images were measured using image analysis software WinROOF (MITANI CORPORATION), and the number average particle diameter was calculated as the average primary particle diameter.
[0101] (Measurement of silver particle concentration) The concentration of silver particles contained in the conductive inks prepared in the examples and comparative examples was measured by the following method. Using a differential thermobalance TG-DTA8122 (Rigaku), thermogravimetric analysis was performed by increasing the temperature from room temperature to 550°C at a rate of 10°C / min in air. The residue at 550°C was taken as the silver particle concentration.
[0102] (Preparation of evaluation samples) The conductive inks prepared in the examples and comparative examples were applied to a 30 mm x 30 mm PET film (thickness 50 μm) as a substrate using a spin coater at 500 rpm x 20 sec. Then, the film was heated for 30 minutes in a constant temperature dryer set at 100°C (first heat treatment). Then, the film was transferred to another constant temperature dryer set at 150°C and heated for 30 minutes (second heat treatment). The thickness of the obtained conductive film after the second heat treatment was approximately 1.0 μm. The evaluation of (1) electrical conductivity and (2) adhesion described below were carried out on the coating film after the first heat treatment and the coating film after the second heat treatment.
[0103] (1) Conductivity evaluation The surface resistance of the evaluation sample was measured using a Loresta (MCP-T610, manufactured by Nitto Seiko Analytech). The film thickness was also measured using a laser microscope (VK-X150, manufactured by KEYENCE). The volume resistance was calculated from the measurement results. The conductivity of the coating film (conductive film) formed after the second heat treatment was also evaluated according to the following criteria. A: Less than 25μΩ·cm B: 25μΩ·cm or more and 40μΩ·cm or less C: More than 40 μΩ cm
[0104] (2) Evaluation of adhesion Adhesion evaluation was performed using cross-cuts according to ASTM D3359-09. That is, 25 grids of 1 mm width were created on the evaluation sample with a cutter, cellophane tape (CT-24, manufactured by Nichiban, 24 mm wide) was adhered to the grids with finger pressure, and the tape was peeled off in one go at an angle of approximately 60° from one end. The results were evaluated according to the following criteria. A: Peeling rate is less than 5% B: Peeling rate is 5% or more and 15% or less C: Peeling rate is over 15%
[0105] (3) Overall evaluation Based on the results of the three items of adhesion after the first heat treatment, volume resistivity after the second heat treatment, and adhesion after the second heat treatment, an overall judgment was made according to the following criteria. A: All three items are evaluated B: At least one B out of three items and no C C: Any of the three items is rated C
[0106] [Table 1]
Claims
1. The ink contains silver particles, an amine having a hydroxyl group, and a blocked isocyanate, A method for producing a conductive film, the method comprising: a first heating treatment for heating a conductive ink at a first heating temperature; and a second heating treatment for heating the conductive ink that has been subjected to the first heating treatment at a second heating temperature, The conductive ink, wherein a dissociation temperature of the blocked isocyanate is higher than the first heating temperature and is equal to or lower than the second heating temperature + 10°C.
2. 2. The conductive ink according to claim 1, wherein the dissociation temperature of the blocked isocyanate is equal to or higher than the second heating temperature −20° C. and equal to or lower than the second heating temperature.
3. The boiling point of the amine having a hydroxyl group is the first heating temperature + 100° C. or more, and The conductive ink according to claim 1 , wherein the temperature is not lower than the second heating temperature + 50° C. and not higher than the second heating temperature + 100° C.
4. The conductive ink according to claim 1 , wherein a temperature difference between the first heating temperature and the second heating temperature is 30° C. or more and 60° C. or less.
5. (1) applying a conductive ink to a substrate; (2) heating the substrate coated with the conductive ink at a first heating temperature; and Step (3) of further heating the substrate after step (2) at a second heating temperature. Including, the conductive ink contains silver fine particles, an amine having a hydroxyl group, and a blocked isocyanate; the first heating temperature is lower than the dissociation temperature of the blocked isocyanate, The second heating temperature is equal to or higher than the dissociation temperature of the blocked isocyanate minus 10°C. A method for manufacturing a conductive film.
Citation Information
Patent Citations
Method for producing silver nanoparticles having wide particle size distribution, and silver nanoparticles
JP2021105218A