Diffusion film, light diffusion device, and method of manufacturing diffusion film
The multi-layer diffusion film with a polymer matrix and dispersed particles addresses the non-uniformity of PDLC films, enhancing brightness uniformity and durability.
Patent Information
- Application Number
- JP2023057697
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing PDLC films used as light diffusing devices in combination with light sources often suffer from insufficient uniformity of in-plane luminance.
A diffusion film comprising multiple layers with a polymer matrix and dispersed particles, including liquid crystal compounds and polymers, with alternating layers and optional thickening layers, to enhance scattering properties and uniformity.
The multi-layer structure improves in-plane brightness uniformity and prevents issues like scratching and pattern degradation, achieving enhanced light diffusion.
Smart Images

Figure 2024145374000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a diffusion film, a light diffusion device, and a method for manufacturing a diffusion film. [Background technology]
[0002] A PDLC film having a polymer dispersed liquid crystal (hereinafter sometimes referred to as "PDLC") layer between a pair of transparent electrode layers is a type of light control film, and can switch between a light scattering state (scattering state) and a light transmitting state (non-scattering state or transparent state) by switching between a voltage application state and a non-voltage application state. Specifically, the PDLC layer includes a polymer matrix and droplets of a liquid crystal compound (hereinafter sometimes referred to as "liquid crystal droplets") dispersed in the polymer matrix, and the liquid crystal droplets become scattering particles and can cause light scattering due to the difference in refractive index between the liquid crystal compound in the liquid crystal droplets and the polymer matrix, etc.
[0003] Moreover, in recent years, display devices and lighting devices that use light-emitting diodes (hereinafter referred to as LEDs) as light sources have become widespread due to their low power consumption and ability to be made smaller and thinner, and a diffusion film is placed over the light source to obtain uniform surface light emission.
[0004] The above-mentioned diffusion film includes a surface-type diffusion film in which a diffusion pattern is formed on the surface by uneven processing, dot printing, etc. When a surface-type diffusion film is laminated to an adjacent member without an adhesive layer, the adjacent member may be scratched by rubbing, the diffusion pattern may change over time, etc., and when the surface-type diffusion film is laminated to an adjacent member via an adhesive layer, the diffusion pattern may change or disappear due to the adhesive, and air bubbles may be generated in the uneven parts, etc.
[0005] Another type of diffusion film is an internal diffusion film that contains scattering particles inside. A PDLC film having the above-mentioned PDLC layer can be used as an internal diffusion film by utilizing the scattering effect of the liquid crystal droplets (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent Publication No. 2021-077534 Summary of the Invention [Problem to be solved by the invention]
[0007] When a PDLC film is combined with a light source and used as a light diffusion device, the uniformity of the in-plane luminance may be insufficient. Therefore, the main object of the present invention is to provide a diffusion film that can realize more uniform surface emission when used as a light diffusion device in combination with a light source. [Means for solving the problem]
[0008] [1] According to one aspect of the present invention, there is provided a diffusion film having two or more diffusion layers including a polymer matrix and dispersed particles, the dispersed particles including at least one type selected from a liquid crystal compound and a liquid crystal polymer, dispersed in the polymer matrix. [2] In the diffusion film of [1] above, the diffusion layer may have a total thickness of 50 μm or more. [3] The diffusion film of [1] or [2] above may have two or more structural units each including a pair of supporting substrates and the diffusion layer disposed therebetween. [4] The diffusion film of [1] or [2] above may have a laminated structure in which supporting substrates and the diffusion layers are arranged alternately. [5] The diffusion film according to any one of the above [1] to [4] may further have a thickening layer. [6] In the diffusion film according to any one of [1] to [5] above, at least one of the diffusion layers may have regions with different hazes when viewed in a plan view. [7] In the diffusion film according to [6] above, the regions having different haze may be arranged in a predetermined pattern. [8] In the diffusion film according to the above [6] or [7], the difference between the maximum and minimum haze values may be 10% or more. [9] According to another aspect of the present invention, there is provided a light diffusion device comprising the diffusion film according to any one of [1] to [8] above and a light source unit.
[10] In the light diffusing device described in [9] above, the light source section may include a plurality of point light sources.
[11] According to another aspect of the present invention, there is provided a method for producing a diffusion film, comprising: step I of applying a coating liquid containing a polymer matrix-forming resin, a liquid crystal compound, and a solvent to a supporting substrate to obtain a coating layer; step II of drying the coating layer to obtain a polymer-dispersed liquid crystal layer containing a polymer matrix and dispersed particles containing the liquid crystal compound dispersed in the polymer matrix; and step III of laminating another supporting substrate on the polymer-dispersed liquid crystal layer, wherein steps I to III are repeated two or more times to produce a laminate in which two or more of the supporting substrates and two or more of the polymer-dispersed liquid crystal layers are arranged alternately.
[12] In the manufacturing method described in
[11] above, the liquid crystal compound may include a polymerizable liquid crystal compound and a non-polymerizable liquid crystal compound, and the manufacturing method may include irradiating a predetermined region with active energy rays while applying a voltage to the polymer dispersed liquid crystal layer contained in the laminate, thereby polymerizing the polymerizable liquid crystal compound. Effect of the Invention
[0009] While it is difficult to make the PDLC layer thicker due to film-forming properties, the diffusion film according to the embodiment of the present invention has two or more diffusion layers, and the total thickness of the diffusion layers can be sufficiently thick, resulting in improved scattering properties and more uniform in-plane luminance. [Brief description of the drawings]
[0010] [Figure 1] 1(a) to 1(c) are each a schematic cross-sectional view showing the configuration of a diffusion film according to an embodiment of the present invention. [Diagram 2] 3(a) to 3(d) are schematic cross-sectional views illustrating an example of the configuration of a diffusion layer. [Diagram 3] 5A to 5C are schematic diagrams illustrating an example of a method for manufacturing a diffusion layer. [Figure 4] 5A to 5C are schematic diagrams illustrating an example of a method for manufacturing a diffusion layer. [Diagram 5] 1 is a schematic cross-sectional view showing a configuration of a light diffusing device according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, preferred embodiments of the present invention will be described, but the present invention is not limited to these embodiments. In addition, each embodiment can be appropriately combined. In this specification, the term "to" indicating a numerical range includes the upper and lower numerical limits.
[0012] A. Diffusion film The diffusion film according to the embodiment of the present invention has two or more diffusion layers including a polymer matrix and dispersed particles including at least one selected from a liquid crystal compound and a liquid crystal polymer dispersed in the polymer matrix. With such a configuration, the diffusion film according to the embodiment of the present invention can realize more uniform surface emission when used as a light diffusion device in combination with a light source unit. In addition, since two or more diffusion layers are integrated, problems such as deterioration due to rubbing between films, film waviness, water marks, etc. that may occur when the diffusion films are stacked without being integrated can be avoided.
[0013] The haze of the diffusion film can be appropriately set depending on the application. The haze of the diffusion film can be, for example, 50% to 80%, or, for example, 70% to 100%. When the diffusion film includes a diffusion layer having regions with different hazes as described below, the maximum haze value of the diffusion film can be, for example, 30% to 100%, and the minimum haze value can be, for example, 0% to 70%. The difference between the maximum and minimum haze values typically exceeds 0%, and can be, for example, 5% or more, preferably 10% or more, more preferably 20% to 100%, and even more preferably 30% to 100%.
[0014] 1(a) to 1(c) are schematic cross-sectional views showing the structure of a diffusion film according to one embodiment of the present invention. The diffusion film shown in FIG. 1(a) has two structural units including a pair of support substrates and a diffusion layer disposed therebetween. Specifically, the diffusion film 100A has a first structural unit 30a including a pair of support substrates 20a, 20a' and a diffusion layer 10a disposed therebetween, and a second structural unit 30b including a pair of support substrates 20b, 20b' and a diffusion layer 10b disposed therebetween. The first structural unit 30a and the second structural unit 30b are typically laminated via an adhesive layer (not shown). The diffusion layer and the support substrate may be laminated via an adhesive layer, or may be laminated in close contact without an adhesive layer. In one embodiment, the diffusion layer and the support substrate are laminated in close contact without an adhesive layer. The adhesive layer can be preferably exemplified by an adhesive layer or a pressure-sensitive adhesive layer. The thickness of the adhesive layer is, for example, 0.1 μm to 50 μm, and preferably 0.3 μm to 30 μm.
[0015] The diffusion film shown in FIG. 1(b) has a laminated structure in which the support substrate and the diffusion layer are alternately arranged. Specifically, the diffusion film 100B has a first support substrate 20a, a first diffusion layer 10a, a second support substrate 20b, a second diffusion layer 10b, and a third support substrate 20c, in this order. These diffusion layers and support substrates are typically laminated without an adhesive layer. In a diffusion film having a laminated structure in which the support substrate and the diffusion layer are alternately arranged, the support substrates can be preferably arranged on both sides of the diffusion layer from the viewpoints of handling, durability, etc.
[0016] The diffusion film shown in FIG. 1(c) further has a thickening layer in addition to the support substrate and the diffusion layer. Specifically, the diffusion film 100C has a thickening layer 40 arranged on the first support substrate 20a side of the diffusion film 100B. The thickening layer is typically laminated to the first support substrate 20a via an adhesive layer. When the diffusion film having the thickening layer is arranged on the light source unit, the distance from the light source unit to the diffusion layer can be sufficiently secured, and as a result, the in-plane luminance can be more suitably uniformed. The thickening layer may be arranged on one side (light source side) of two or more diffusion layers as in the illustrated example, or may be arranged between two or more diffusion layers, unlike the illustrated example.
[0017] The number of diffusion layers in the diffusion film is not limited to the illustrated example. The number of diffusion layers in the diffusion film may be, for example, 2 to 4, preferably 2 to 3. Therefore, for example, a configuration in which one or more of the above-mentioned structural units are laminated on the second structural unit 30b of the diffusion film 100A via an adhesive layer, a configuration in which one or more of the above-mentioned structural units are laminated on the third support base material 20c of the diffusion film 100B via an adhesive layer, and the like are also included in the embodiments of the present invention.
[0018] The total thickness of the diffusion layers included in the diffusion film is, for example, 50 μm or more, preferably 60 μm or more, more preferably 70 μm or more, and even more preferably 80 μm or more. The diffusion layers used in the embodiments of the present invention are difficult to increase in thickness per layer due to their structure, but by laminating two or more diffusion layers, the total thickness of the diffusion layers can be increased to obtain a diffusion film with excellent diffusion properties. The upper limit of the total thickness of the diffusion layers is, for example, 300 μm or less, or, for example, 200 μm or less, from the viewpoint of the complexity of the manufacturing process and the thinning of the diffusion film.
[0019] In the above diffusion film, at least one of the thicknesses from one surface to the diffusion layer disposed farthest from the surface (thicknesses indicated as T1 or T2 in FIG. 1(c)) is, for example, 100 μm or more, preferably 100 μm to 400 μm, and more preferably 100 μm to 300 μm. If the distance from one surface to the diffusion layer is within the above range, when the film is disposed above the light source unit, the distance from the light source unit to the diffusion layer can be ensured, and as a result, the in-plane luminance can be more suitably uniformed.
[0020] The total thickness of the diffusion film is, for example, 100 μm to 450 μm, preferably 125 μm to 425 μm, and more preferably 150 μm to 400 μm.
[0021] A-1. Diffusion layer The diffusion layer includes a polymer matrix and dispersed particles that are dispersed in the polymer matrix and include at least one selected from a liquid crystal compound and a liquid crystal polymer. Two or more diffusion layers included in the diffusion film may have the same configuration (type or composition of the polymer matrix, the liquid crystal compound, and the liquid crystal polymer, dispersed particle size, thickness, etc.) or different configurations.
[0022] The diffusion layer may have a substantially uniform haze in plan view, or may have regions with different hazes. The regions with different hazes may be formed in any suitable pattern depending on the purpose. For example, for a light source unit having point light sources arranged in a predetermined pattern, a diffusion film having a high haze region in a pattern corresponding to the arrangement of the point light sources and a diffusion layer having other regions as low haze regions may be used to suitably uniformize the in-plane luminance. The diffusion film may include both a diffusion layer having a substantially uniform haze in plan view and a diffusion layer having regions with different hazes. In addition, when the diffusion film includes two or more diffusion layers having regions with different hazes, the formation patterns of the regions with different hazes in these diffusion layers may be the same or different.
[0023] The haze of the diffusion layer can be appropriately set depending on the use of the diffusion film, the number of diffusion layers in the diffusion film, etc. The haze of a diffusion layer having a substantially uniform haze can be, for example, 50% to 80%, or, for example, 70% to 100%. The maximum haze of a diffusion layer having regions with different hazes can be, for example, 30% to 100%, and the minimum haze can be, for example, 0% to 70%. The difference between the maximum and minimum haze values typically exceeds 0%, and can be, for example, 5% or more, preferably 10% or more, more preferably 20% to 100%, and even more preferably 30% to 100%.
[0024] 2(a) to (d) are each a schematic cross-sectional view illustrating an example of the configuration of a diffusion layer. 2(a) includes a polymer matrix 12 and dispersed particles 16a containing a liquid crystal compound 13 dispersed in the polymer matrix 12. The liquid crystal compound 13 in the dispersed particles 16a is in a non-oriented state, and the liquid crystal compound 13 exhibits diffusibility due to the difference in refractive index between the polymer matrix 12 and the dispersed particles 16a. The liquid crystal compound 13 used in this embodiment may be a polymerizable liquid crystal compound or a non-polymerizable liquid crystal compound.
[0025] The diffusion layer 10 shown in FIG. 2(b) includes a polymer matrix 12 and dispersed particles 16b containing a liquid crystal polymer 14 dispersed in the polymer matrix 12. In the dispersed particles 16b, the liquid crystal polymer 14 is fixed in a non-oriented state, and the diffusivity is exhibited due to the refractive index difference between the polymer matrix 12 and the dispersed particles 16b. Here, the liquid crystal polymer is a polymer of a polymerizable liquid crystal compound and is non-liquid crystal. That is, in the liquid crystal polymer, for example, the transition to a liquid crystal phase, a glass phase, or a crystalline phase due to a temperature change specific to a liquid crystal compound does not occur. In this embodiment, dispersed particles containing a liquid crystal polymer and a liquid crystal compound may be used instead of the dispersed particles 16b. In this case, a non-polymerizable liquid crystal compound is preferably used as the liquid crystal compound.
[0026] The diffusion layer 10 shown in FIG. 2(c) includes a polymer matrix 12 and dispersion particles 16c that are dispersed in the polymer matrix 12 and contain a non-polymerizable liquid crystal compound 13a and a liquid crystal polymer 14. In the region A, the liquid crystal polymer 14 in the dispersion particles 16c is fixed in a non-oriented state, and the non-polymerizable liquid crystal compound 13a is also non-oriented following the liquid crystal polymer 14. On the other hand, in the region B, the liquid crystal polymer 14 in the dispersion particles 16c is fixed in a state oriented substantially perpendicular to the thickness direction, and the non-polymerizable liquid crystal compound 13a is also oriented following the liquid crystal polymer 14. According to the diffusion layer having such a configuration, in a plan view, the region A shows a higher haze than the region B. In this embodiment, dispersion particles that contain a liquid crystal polymer and do not contain a non-polymerizable liquid crystal compound may be used instead of the dispersion particles 16c as long as the above-mentioned oriented state of the liquid crystal polymer can be formed.
[0027] The diffusion layer 10 shown in FIG. 2(d) includes a polymer matrix 12, dispersed particles 16c containing a non-polymerizable liquid crystal compound 13a and a liquid crystal polymer 14, and dispersed particles 16d containing a non-polymerizable liquid crystal compound 13a and a polymerizable liquid crystal compound 13b, which are dispersed in the polymer matrix 12. In the region A, the non-polymerizable liquid crystal compound 13a and the polymerizable liquid crystal compound 13b in the dispersed particles 16d are both in a non-oriented state. On the other hand, in the region B, the liquid crystal polymer 14 in the dispersed particles 16c is fixed in a state oriented substantially perpendicular to the thickness direction, and the non-polymerizable liquid crystal compound 13a is also oriented following the liquid crystal polymer 14. According to the diffusion layer having such a configuration, in a plan view, the region A shows a higher haze than the region B. In this embodiment, as long as the above-mentioned orientation state of the liquid crystal polymer can be formed, the dispersed particles 16c and the dispersed particles 16d may be replaced with dispersed particles containing a liquid crystal polymer and not containing a non-polymerizable liquid crystal compound, and dispersed particles containing a polymerizable liquid crystal compound and not containing a non-polymerizable liquid crystal compound.
[0028] The polymer matrix may be composed of any suitable resin. The resin for forming the polymer matrix may be appropriately selected depending on the light transmittance, the refractive index of the liquid crystal polymer or liquid crystal compound, the adhesion to the support substrate, and the like. For example, water-soluble or water-dispersible resins such as urethane-based resins, polyvinyl alcohol-based resins, polyethylene-based resins, polypropylene-based resins, and acrylic-based resins may be preferably used. The resin for forming the polymer matrix may be used alone or in combination.
[0029] The content of the polymer matrix in the diffusion layer is, for example, 30% by weight to 70% by weight, preferably 35% by weight to 65% by weight, and more preferably 40% by weight to 60% by weight. If the content of the polymer matrix is within this range, it is possible to obtain effects such as good mechanical strength and prevention of liquid crystal leakage from the edges.
[0030] As the non-polymerizable liquid crystal compound, any suitable non-polymerizable liquid crystal compound can be used alone or in combination of two or more kinds. The dielectric anisotropy of the non-polymerizable liquid crystal compound may be positive or negative. The non-polymerizable liquid crystal compound may be, for example, a nematic type, a smectic type, or a cholesteric type liquid crystal compound. It is preferable to use a nematic type liquid crystal compound because it can achieve high transparency in the aligned state.
[0031] Examples of nematic liquid crystal compounds include biphenyl-based compounds, phenylbenzoate-based compounds, cyclohexylbenzene-based compounds, azoxybenzene-based compounds, azobenzene-based compounds, azomethine-based compounds, terphenyl-based compounds, biphenylbenzoate-based compounds, cyclohexylbiphenyl-based compounds, phenylpyridine-based compounds, cyclohexylpyrimidine-based compounds, cholesterol-based compounds, fluorine-based compounds, etc. These low molecular weight liquid crystal compounds may be used alone or in combination.
[0032] The birefringence Δn (=ne-no; ne is the refractive index of the liquid crystal compound molecule in the major axis direction, and no is the refractive index of the liquid crystal compound molecule in the minor axis direction) of the non-polymerizable liquid crystal compound at a wavelength of 589 nm is preferably 0.05 to 0.50, and more preferably 0.10 to 0.45.
[0033] As the polymerizable liquid crystal compound, a polymerizable liquid crystal compound appropriately selected according to light transmittance, compatibility with non-polymerizable liquid crystal compound, etc. can be used alone or in combination of two or more kinds. The polymerizable liquid crystal compound may be a crosslinked type having two or more functionalities. As the polymerizable liquid crystal compound, for example, polymerizable mesogen compounds described in JP-A-2002-533742 (WO00 / 37585), EP358208 (US5211877), EP66137 (US4388453), WO93 / 22397, EP0261712, DE19504224, DE4408171, GB2280445, etc. can be used. As the polymerizable liquid crystal compound, for example, a nematic type liquid crystal monomer is preferable. The birefringence Δn of the polymerizable liquid crystal compound at a wavelength of 589 nm is preferably 0.05 to 0.50, more preferably 0.10 to 0.45.
[0034] The liquid crystal polymer is a polymer of the above-mentioned polymerizable liquid crystal compound, and is non-liquid crystal, as described above.
[0035] The total content of the liquid crystal polymer and the liquid crystal compound (non-polymerizable liquid crystal compound and polymerizable liquid crystal compound) in the diffusion layer is, for example, 30% by weight to 70% by weight, preferably 35% by weight to 65% by weight, more preferably 40% by weight to 60% by weight. When the dispersed particles contain a liquid crystal polymer, the content of the liquid crystal polymer relative to the total content of the liquid crystal polymer and the liquid crystal compound in the diffusion layer may be, for example, 5% by weight or more, preferably 7% by weight or more, more preferably 10% by weight or more, and may be, for example, 100% by weight or less, preferably 80% by weight or less, more preferably 50% by weight or less. The total content of the polymer matrix, the liquid crystal polymer, and the liquid crystal compound in the diffusion layer may be, for example, 90% by weight to 99.9% by weight, preferably 95% by weight to 99.9% by weight.
[0036] The diffusion layer may further contain any appropriate component as necessary. Such optional components include a polymerization initiator, a surfactant, a leveling agent, a crosslinking agent, a dispersion stabilizer, etc. The total content of the optional components in the diffusion layer may be, for example, 0.1% by weight to 10% by weight, preferably 0.1% by weight to 5% by weight.
[0037] The average particle diameter of the dispersed particles may be, for example, 0.2 μm to 9 μm, preferably 0.3 μm to 8 μm. If the average particle diameter of the dispersed particles is too small, the dispersed particle size is smaller than the wavelength of light, so that the light passes through the dispersed particles without being scattered, and as a result, a problem may occur in which sufficient haze cannot be obtained. If the average particle diameter is too large, the dispersed particle size is too large than the wavelength of light, so that a problem may occur in which sufficient haze cannot be obtained. The average particle diameter of the dispersed particles in the diffusion layer is the volume average particle diameter of the dispersed particles when viewed from a direction perpendicular to the main surface of the diffusion layer.
[0038] The thickness of the diffusion layer is, for example, 10 μm to 60 μm, preferably 15 μm to 55 μm, and more preferably 20 μm to 50 μm.
[0039] A-2. Supporting base material The supporting substrate includes a substrate body. The supporting substrate may have a hard coat (HC) layer on one or both sides of the substrate body, if necessary.
[0040] The substrate body may be formed using any suitable material. Specific examples include glass films and polymer films. Polymer films are preferred because they have excellent smoothness and can be continuously produced by rolls to greatly improve productivity.
[0041] The substrate body is typically a polymer film mainly composed of a thermoplastic resin. Examples of thermoplastic resins include polyester resins; cycloolefin resins such as polynorbornene; acrylic resins; polycarbonate resins; and cellulose resins. Among them, polyester resins, cycloolefin resins, and acrylic resins are preferred. These resins are excellent in transparency, mechanical strength, thermal stability, and moisture shielding properties. The above-mentioned thermoplastic resins may be used alone or in combination of two or more. In addition, optical films such as those used in polarizing plates, such as low retardation substrates, high retardation substrates, retardation plates, absorptive polarizing films, and polarized selective reflection films, can also be used as the substrate body.
[0042] The haze of the supporting substrate is preferably 20% or less, more preferably 10% or less, and further preferably 0.1% to 10%.
[0043] The total light transmittance of the supporting substrate is preferably 30% or more, more preferably 60% or more, and further preferably 80% or more. The total light transmittance can be measured according to JIS K 7361.
[0044] The thickness of the supporting substrate is, for example, 200 μm or less, preferably 3 μm to 150 μm, and more preferably 5 μm to 100 μm. When the diffusion layer is formed while applying a voltage as described in section B, the thickness of the supporting substrate is preferably 50 μm or less, more preferably 3 μm to 40 μm, and even more preferably 5 μm to 30 μm.
[0045] A-3.Thickened layer The thickening layer may be made of any suitable material as long as the effect of the present invention can be obtained. The thickening layer may be, for example, a glass film or a polymer film, and is preferably a polymer film. The polymer film constituting the thickening layer may be the same film as the polymer film constituting the substrate body of the supporting substrate.
[0046] The haze of the thickened layer is preferably 20% or less, more preferably 10% or less, and further preferably 0.1% to 10%.
[0047] The total light transmittance of the thickened layer is preferably 30% or more, more preferably 60% or more, and further preferably 80% or more.
[0048] The thickness of the thickened layer may be, for example, 30 μm or more, preferably 40 μm or more, more preferably 50 μm or more, and may be, for example, 300 μm or less, preferably 250 μm or less.
[0049] B. How to make the diffusion film The diffusion films described in section A can be manufactured by any suitable method. In one embodiment, a method for producing a diffusion film includes the steps of: Coating a coating liquid containing a polymer matrix-forming resin, a liquid crystal compound, and a solvent onto one of the supporting substrates to obtain a coating layer; drying the coating layer to obtain a PDLC layer including a polymer matrix and dispersed particles including a liquid crystal compound dispersed in the polymer matrix; and forming a structural unit including a pair of support substrates and a PDLC layer disposed therebetween by a manufacturing method including laminating another support substrate on the PDLC layer; and laminating two or more of the above structural units via an adhesive layer; According to the above manufacturing method (also referred to as "manufacturing method A"), it is possible to obtain a diffusion film having two or more structural units, each of which includes a pair of supporting substrates and a diffusion layer (PDLC layer) disposed between them.
[0050] In another embodiment, a method for manufacturing a diffusion film includes the steps of: A step I of applying a coating liquid containing a polymer matrix-forming resin, a liquid crystal compound, and a solvent to a supporting substrate to obtain a coating layer; Step II of drying the coating layer to obtain a PDLC layer including a polymer matrix and dispersed particles including a liquid crystal compound dispersed in the polymer matrix; and Step III of laminating another supporting substrate on the PDLC layer; The method includes repeating the above steps I to III two or more times to prepare a laminate in which two or more of the above supporting substrates and two or more of the above PDLC layers are alternately arranged. According to the above manufacturing method (also referred to as "manufacturing method B"), it is possible to obtain a diffusion film having a laminated structure in which supporting substrates and diffusion layers (PDLC layers) are alternately arranged.
[0051] In the above-mentioned diffusion film manufacturing methods A and B, the coating liquid is preferably an emulsion coating liquid in which liquid crystal particles containing a liquid crystal compound are dispersed in a solvent. As the solvent, water or a mixed solvent of water and a water-miscible organic solvent can be preferably used. Examples of the water-miscible organic solvent include C1-3 alcohol, acetone, DMSO, etc. The coating liquid may further contain optional components such as a polymerization initiator, a surfactant, a leveling agent, a crosslinking agent, and a dispersion stabilizer depending on the purpose.
[0052] In the manufacturing methods A and B of the above-mentioned diffusion film, the diffusion layer is a PDLC layer (for example, the diffusion layer shown in FIG. 2(a)) containing a polymer matrix and dispersed particles containing a liquid crystal compound dispersed in the polymer matrix. However, a PDLC layer is prepared using a coating liquid containing a polymerizable liquid crystal compound as a liquid crystal compound, and then the polymerizable liquid crystal compound is polymerized to form a diffusion layer (for example, the diffusion layer shown in FIG. 2(b)) containing a polymer matrix and dispersed particles containing a liquid crystal polymer dispersed in the polymer matrix. In the manufacturing method A, the structural units may be laminated after polymerization is performed for each structural unit, or the structural units may be laminated and then polymerized together. In the manufacturing method B, polymerization may be performed for each cycle of steps I to III, or polymerization may be performed on a laminate in which two or more supporting substrates and PDLC layers are alternately arranged.
[0053] Furthermore, in the above-mentioned diffusion film manufacturing methods A and B, a PDLC layer is produced using a coating liquid containing a polymerizable liquid crystal compound as the liquid crystal compound, and then the polymerizable liquid crystal compound is polymerized while applying a voltage from the first main surface side and the second main surface side of the PDLC layer so as to generate regions with different electric field strengths, thereby forming a diffusion layer (for example, the diffusion layer shown in Figure 2(c)) that contains a polymer matrix and dispersed particles containing a liquid crystal polymer dispersed in the polymer matrix, and has regions with different hazes when viewed in a plane.
[0054] To explain this in detail with reference to FIG. 3(a), a first electrode 310 having a recess on its surface is disposed on the outside of one of the supporting substrates 20 of a structural unit including a pair of supporting substrates 20, 20' and a PDLC layer 10 disposed therebetween, and a second electrode 320 having a flat surface (e.g., a glass substrate with ITO) is disposed on the outside of the other supporting substrate 20', and a voltage is applied to these electrodes, thereby generating regions with different electric field strengths in the PDLC layer 10. More specifically, the electric field strength is high in the region B where the distance between the electrodes is small, and the non-polymerizable liquid crystal compound 13a and the polymerizable liquid crystal compound 13b in this region can be aligned in the electric field direction. On the other hand, the electric field strength is low in the region A where the distance between the electrodes is large, and the non-polymerizable liquid crystal compound 13a and the polymerizable liquid crystal compound 13b in this region are in a non-aligned state. By irradiating light in this state to polymerize the polymerizable liquid crystal compound 13b, a liquid crystal polymer with a fixed non-aligned state is generated in the region A, and a liquid crystal polymer 14 with a fixed substantially vertical alignment state is generated in the region B (FIG. 3(b)). The region A can exhibit a higher haze than the region B. In the illustrated example, the polymerization treatment is performed on one structural unit 30, but the polymerization treatment may be performed on a laminate of two or more structural units or a laminate in which a support substrate and a PDLC layer are alternately arranged. As illustrated in the illustrated example, the dispersed particles 16d contain the non-polymerizable liquid crystal compound 13a in addition to the polymerizable liquid crystal compound 13b, thereby widening the temperature range of the liquid crystal phase (for example, a nematic phase) and enabling more suitable alignment control, but the dispersed particles may not contain the non-polymerizable liquid crystal compound depending on the purpose.
[0055] In the above manufacturing method, a desired inter-electrode distance can be realized in a desired pattern by providing the surface of the electrode with unevenness, steps, inclinations, etc. in a desired pattern. For example, the inter-electrode distance can be continuously changed by providing a tapered protrusion on the surface of the electrode. Specifically, the amount and rate of change in the inter-electrode distance can be arbitrarily controlled by changing the height and inclination angle of the tapered protrusion, and as a result, the resulting diffusion layer can have a haze change with an arbitrary gradient.
[0056] In addition, in the above-mentioned diffusion film manufacturing methods A and B, a PDLC layer is prepared using a coating liquid containing a polymerizable liquid crystal compound and a non-polymerizable liquid crystal compound as liquid crystal compounds, and then, while a voltage is applied to the PDLC layer, active energy rays are irradiated to a specified region to polymerize the polymerizable liquid crystal compound, thereby forming a diffusion layer (for example, the diffusion layer shown in FIG. 2(d)) that contains a polymer matrix, dispersed particles that are dispersed in the polymer matrix and contain a non-polymerizable liquid crystal compound and a liquid crystal polymer, and dispersed particles that contain a non-polymerizable liquid crystal compound and a polymerizable liquid crystal compound, and has regions with different hazes when viewed in a plane.
[0057] Explaining with reference to FIG. 4(a), a first electrode 310 is arranged on the outside of the first support substrate 20a, a second electrode (e.g., a glass substrate with ITO) 320 is arranged on the outside of the third support substrate 20c, and a voltage is applied to these electrodes, thereby aligning the non-polymerizable liquid crystal compound 13a and the polymerizable liquid crystal compound 13b in the PDLC layer 10 in the direction of the electric field. In this state, light is irradiated through a photomask 330 to polymerize the polymerizable liquid crystal compound 13b, whereby a liquid crystal polymer 14 with a substantially vertical alignment state is generated in the region B (irradiated region), and the non-polymerizable liquid crystal compound 13a and the polymerizable liquid crystal compound 13b can exist in a non-aligned state in the region A (non-irradiated region) (FIG. 4(b)). The region A can exhibit a higher haze than the region B. In the illustrated example, the polymerization treatment is performed on a laminate in which the support substrate and the PDLC layer are alternately arranged, but the polymerization treatment may be performed on a laminate of two or more structural units, or one structural unit may be polymerized and then laminated with another structural unit. As in the illustrated example, the dispersed particles 16d contain the non-polymerizable liquid crystal compound 13a in addition to the polymerizable liquid crystal compound 13b, thereby widening the temperature range of the liquid crystal phase (e.g., nematic phase) and enabling more suitable alignment control, but the dispersed particles may not contain the non-polymerizable liquid crystal compound depending on the purpose.
[0058] In the above-mentioned diffusion film manufacturing methods A and B, a diffusion film further having a thickened layer can be obtained by attaching a thickened layer to a desired portion.
[0059] C. Light Diffuser A light diffusion device according to an embodiment of the present invention has the diffusion film described in Section A and a light source unit. FIG. 5 is a schematic cross-sectional view showing the configuration of a light diffusion device according to one embodiment of the present invention. The light diffusion device 200 has a light source layer 110 and a diffusion film 100C arranged thereon. The diffusion film 100C is arranged so that the thickened layer 40 faces the light source layer 110, which allows the distance between the diffusion layers 10a and 10b and the light source unit to be increased. The diffusion film 100C may be laminated on the light source layer 110 via an adhesive layer, or may be placed without an adhesive layer.
[0060] The light source layer 110 includes a light source section 112 and a sealing resin layer 114 that seals the light source section 112 .
[0061] The light source unit 112 is typically composed of a plurality of point light sources 112a. The plurality of point light sources are, for example, arranged two-dimensionally in a predetermined pattern. As the point light source, a light source that emits light with high directivity is preferable, and for example, an LED element can be used.
[0062] Examples of resins that form the sealing resin layer 114 include thermosetting resins such as silicone resin, epoxy resin, polyester resin, urethane resin, and ethylene vinyl acetate, ultraviolet-curing resins such as acrylic resin, urethane resin, vinyl ester resin, and alkyd resin, and thermoplastic resins such as polyolefin, polystyrene, polyisobutylene, and isobutylene-based elastomer. Among these, silicone resin and epoxy resin are preferred, and silicone resin is more preferred, because they have high adhesion to resin films in general and the effects of the present invention can be suitably obtained. The sealing resin layer may be formed using a single resin, or may be formed using two or more types of resins in combination. EXAMPLES
[0063] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring the various properties are as follows. In addition, unless otherwise specified, "parts" and "%" in the examples and comparative examples are based on weight.
[0064] (1) Thickness The measurement was performed using a digital micrometer (manufactured by Anritsu Corporation, product name "KC-351C"). (2) Volume average particle size of liquid crystal particles in liquid crystal emulsion The volume average particle diameter was calculated using a particle size distribution measuring device (Microtrac, "MT3300EXII"). (3) Average particle size of resin particles A few drops of the resin dispersion were added to 100 mL of water to prepare a measurement sample. Using a dynamic light scattering particle size distribution analyzer (Microtrac, device name "Nanotrac150"), the measurement sample was placed in the measurement holder of the device, and the device monitor was used to confirm that the concentration was measurable, after which the measurement was performed. (4) Hayes Measurements were carried out in accordance with JIS K 7136 using a Nippon Denshoku product called "NDH4000."
[0065] [Example 1] 1. Preparation of emulsion coating fluid A liquid crystal emulsion was prepared by mixing 34.1 parts of a non-polymerizable liquid crystal compound (JNC, product name "JC-5240XX", birefringence Δn = 0.252 (ne = 1.766, no = 1.514), viscosity = 75 mPa·s), 3.8 parts of a polymerizable liquid crystal compound (BASF, product name "PALIOCOLOR LC-242"), 0.1 parts of a photopolymerization initiator (IGM, product name "OMNIRAD651"), 60.0 parts of pure water, and 2.0 parts of a dispersant (Dai-ichi Kogyo Seiyaku, "Noigen ET159"), and irradiating the mixture with ultrasonic waves at a frequency of 24 kHz for 1 minute using an ultrasonic homogenizer (Hielscher ultrasonics, UP-200S). The average particle size of the liquid crystal particles in the obtained liquid crystal emulsion was 0.8 μm. An emulsion coating liquid was obtained by mixing 19.03 parts of the above liquid crystal emulsion, 9.16 parts of a polyether-based polyurethane resin aqueous dispersion (manufactured by DSM, product name "NeoRez R967", average polymer particle size: 80 nm, solid content: 40 wt%), 8.12 parts of a polyester-based polyurethane resin aqueous dispersion (manufactured by Sanyo Chemical Industries, product name "Eucoat C-102", average polymer particle size: 168 nm, solid content: 45 wt%), 0.38 parts of a leveling agent (manufactured by DIC, product name "F-444"), 1.23 parts of a crosslinking agent (tris[3-(2-methylaziridin-1-yl)propionic acid]=propylidinetrimethyl), and 62.0 parts of pure water.
[0066] 2. Formation of the First PDLC Layer The emulsion coating liquid was applied to one side of a PET film (thickness: 25 μm) as a first supporting substrate to form a coating layer with a thickness of 150 μm using a wire bar. The coating layer was then dried at 25° C. for 90 minutes to form a first PDLC layer with a thickness of 45 μm. The obtained first PDLC layer showed a uniform haze (haze: 99%) over the entire main surface.
[0067] 3. Lamination of the second supporting substrate A PET film (thickness: 25 μm) was laminated as a second supporting substrate on the first PDLC layer while applying a lamination pressure of 0.4 MPa / m using a laminator.
[0068] 4. Formation of the Second PDLC Layer The same emulsion coating liquid as in 1 above was applied to the surface of the second support substrate to form a coating layer with a thickness of 150 μm using a wire bar. The coating layer was then dried at 25° C. for 90 minutes to form a second PDLC layer with a thickness of 45 μm. The resulting second PDLC layer showed a uniform haze over the entire main surface.
[0069] 5. Lamination of the third supporting substrate A PET film (thickness 25 μm) was laminated as a third support substrate on the second PDLC layer while applying a lamination pressure of 0.4 MPa / m using a laminator, thereby obtaining a laminate having a structure of [first support substrate / first PDLC layer / second support substrate / second PDLC layer / third support substrate].
[0070] 6.UV irradiation A flat metal electrode was placed on the first supporting substrate side of the laminate, and an ITO-attached glass electrode was placed on the third supporting substrate side. While applying a voltage of 7 kV to 8 kV to these electrodes, UV irradiation was performed from the third supporting substrate side through a photomask (φ1.5) having a predetermined pattern. Specifically, the laminate was exposed to 20 mW / cm under a UV-LED lamp (manufactured by Hamamatsu Photonics, product name "C11924-101", peak wavelength 365 nm). 2 The film was exposed to light at 25°C for 3 minutes. This caused the polymerizable liquid crystal compound in the irradiated area to polymerize, resulting in a diffusion film 1 having a structure of [first supporting substrate / first patterned diffusion layer / second supporting substrate / second patterned diffusion layer / third supporting substrate]. In the resulting diffusion film 1, the non-irradiated area exhibited a higher haze than the irradiated area. The non-irradiated area (high haze area) was arranged in a pattern corresponding to the arrangement pattern of point light sources in the light source layer A described below.
[0071] [Example 2] In the same manner as in 1. to 5. of Example 1, a laminate having a structure of [first supporting substrate / first PDLC layer / second supporting substrate / second PDLC layer / third supporting substrate] was obtained. The same emulsion coating liquid as in 1. of Example 1 was applied to the surface of the third supporting substrate to form a coating layer with a thickness of 150 μm using a wire bar. The coating layer was then dried at 25° C. for 90 minutes to form a third PDLC layer with a thickness of 45 μm. The obtained third PDLC layer showed a uniform haze over the entire main surface. A PET film (thickness 25 μm) was laminated as a fourth support substrate on the third PDLC layer while applying a lamination pressure of 0.4 MPa / m using a laminator, thereby obtaining a laminate having a structure of [first support substrate / first PDLC layer / second support substrate / second PDLC layer / third support substrate / third PDLC layer / fourth support substrate]. The laminate was irradiated with UV light through a photomask in the same manner as in 6. of Example 1. This caused the polymerizable liquid crystal compound in the irradiated area to polymerize, resulting in a diffusion film 2 having a structure of [first supporting substrate / first patterned diffusion layer / second supporting substrate / second patterned diffusion layer / third supporting substrate / third patterned diffusion layer / fourth supporting substrate]. In the resulting diffusion film 2, the non-irradiated area showed a higher haze than the irradiated area.
[0072] [Example 3] A PET film (thickness 100 μm) was attached as a thickening layer to the first supporting substrate side of the diffusion film 1 produced in Example 1 via a transparent adhesive layer (thickness 25 μm), to obtain a diffusion film 3 having a structure of [thickening layer / first supporting substrate / first patterned diffusion layer / second supporting substrate / second patterned diffusion layer / third supporting substrate].
[0073] [Example 4] In the same manner as in 1. to 3. of Example 1, two laminates (structural units) each having a configuration of [first supporting substrate / first PDLC layer / second supporting substrate] were produced. The two laminates were separately irradiated with UV light through a photomask in the same manner as in 6. of Example 1, whereby the polymerizable liquid crystal compound in the irradiated area was polymerized. The above laminate was bonded to both sides of a PET film (thickness 50 μm) as a thickening layer, via a transparent adhesive layer (thickness 25 μm), with the patterns aligned so that the irradiated areas and the non-irradiated areas overlapped, to obtain diffusion film 4 having a structure of [first supporting substrate / first patterned diffusion layer / second supporting substrate / thickening layer / third supporting substrate / second patterned diffusion layer / fourth supporting substrate].
[0074] [Comparative Example 1] In the same manner as in 1. to 3. of Example 1, a laminate having a structure of [first supporting substrate / first PDLC layer / second supporting substrate] was produced. The laminate was irradiated with UV light through a photomask in the same manner as in step 6 of Example 1. This caused the polymerizable liquid crystal compound in the irradiated area to polymerize, thereby obtaining a diffusion film 1c having a structure of [first supporting substrate / first patterned diffusion layer / second supporting substrate].
[0075] A light source layer including a light source unit and a silicone resin layer (thickness 150 μm) sealing the light source unit was taken out from a liquid crystal display device (Apple, "iPad Pro (registered trademark) 12.9 inch (5th generation)") and used as light source layer A. The light source unit was composed of mini-LEDs arranged two-dimensionally in 119 rows and 88 columns. The diffusion films obtained in the Examples and Comparative Examples were laminated on the light source layer A without an adhesive layer, thereby obtaining a light diffusion device. In the obtained light diffusion device, the non-irradiated areas (high haze areas) of the diffusion film corresponded to the arrangement positions of the LEDs in a plan view. The light diffusion device was turned on, and the uniformity of in-plane luminance was evaluated as follows. The results are shown in Table 1 together with the configuration of the light diffusion device. In the table, "total thickness" refers to the total thickness of the diffusion film. <In-plane luminance uniformity> The luminance of the surface on the diffusion film side of the light diffusion device was measured with a 2D spectroradiometer (Topcon Technohouse, "SR-5000HS") at a resolution of 0.2 mm x 0.2 mm, and the maximum luminance (Lmax) and minimum luminance (Lmin) were substituted into the following formula to calculate the in-plane luminance uniformity. The in-plane luminance uniformity of the light source layer alone was 30.6%. In-plane luminance uniformity (%) = [1-(Lmax-Lmin) / (Lmax+Lmin)] x 100
[0076] [Table 1]
[0077] The diffusion film of the embodiment having two or more diffusion layers was able to improve the uniformity of the in-plane luminance more than the diffusion film of the comparative example having only one diffusion layer. Moreover, such an effect was obtained more favorably when the number of diffusion layers was large and when a thickening layer was provided. [Industrial Applicability]
[0078] The light diffusing device of the present invention is suitably used in display devices such as liquid crystal display devices. [Explanation of symbols]
[0079] 10 Diffusion layer (PDLC layer) 12 Polymer matrix 16 Dispersed particles 20 Supporting base material 30 Structural Units 40 Thickening layer 100 Diffusion Film 110 Light source layer 112 Light source section 200 Light Diffuser
Claims
1. A diffusion film having two or more diffusion layers each including a polymer matrix and dispersed particles, the dispersed particles including at least one type selected from a liquid crystal compound and a liquid crystal polymer, dispersed in the polymer matrix.
2. The diffusion film according to claim 1 , wherein the total thickness of the diffusion layer is 50 μm or more.
3. The diffusion film according to claim 1 , comprising two or more structural units each including a pair of supporting substrates and the diffusion layer disposed therebetween.
4. The diffusion film according to claim 1 , which has a laminated structure in which supporting substrates and the diffusion layers are alternately arranged.
5. The diffusion film of claim 1 further comprising a thickening layer.
6. The diffusion film according to claim 1 , wherein at least one of the diffusion layers has regions with different hazes when viewed in a plan view.
7. The diffusion film according to claim 6 , wherein the regions of different haze are arranged in a predetermined pattern.
8. 7. The diffusion film according to claim 6, wherein the difference between the maximum and minimum haze values is 10% or more.
9. A light diffusing device comprising: the diffusion film according to claim 1 ; and a light source unit.
10. The light diffusing device according to claim 9 , wherein the light source section includes a plurality of point light sources.
11. A step I of applying a coating liquid containing a polymer matrix-forming resin, a liquid crystal compound, and a solvent to a supporting substrate to obtain a coating layer; A step II of drying the coating layer to obtain a polymer dispersed liquid crystal layer including a polymer matrix and dispersed particles including the liquid crystal compound dispersed in the polymer matrix; and Step III of laminating another supporting substrate on the polymer dispersed liquid crystal layer; repeating steps I to III two or more times to prepare a laminate in which two or more of the supporting substrates and two or more of the polymer dispersed liquid crystal layers are alternately arranged.
12. the liquid crystal compound includes a polymerizable liquid crystal compound and a non-polymerizable liquid crystal compound, The method for producing a diffusion film according to claim 11, comprising irradiating a predetermined region with active energy rays while applying a voltage to the polymer dispersed liquid crystal layer included in the laminate, thereby polymerizing the polymerizable liquid crystal compound.
Citation Information
Patent Citations
Lighting system
JP2021077534A