Silver coated resin particle and manufacturing method of silver coated resin particle
Optimized silver-coated resin particles with controlled protrusions on a core particle coating layer enhance conductivity and durability, addressing stability and cost issues in conductive materials.
Patent Information
- Application Number
- JP2023057813
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Silver-coated resin particles with a true spherical outer shape and smooth surface have limited contact points, leading to unstable electrical contacts and variations in conductivity, while particles with excessive protrusions face availability issues.
Silver-coated resin particles with a core particle covered by a coating layer containing fine silver particles and protruding silver particles, where the protruding particles have a specific diameter and number relative to the core particle, and are produced through controlled precipitation.
The solution achieves high conductivity and cost-effectiveness by optimizing the contact area and adhesion of the protruding particles, resulting in durable and conductive materials.
Smart Images

Figure 2024145454000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to silver-coated resin particles and a method for producing silver-coated resin particles. [Background technology]
[0002] For example, conductive adhesives such as conductive pastes and conductive films made by mixing resin with silver-coated resin particles, in which resin particles are coated with silver, are known as conductive materials that can replace lead solder or lead-free solder. The conductive adhesives are used as materials for forming electrodes and electrical wiring that constitute electronic devices such as solar cell panels, liquid crystal displays, and touch panels.
[0003] As examples of silver-coated resin particles used in such conductive materials, Patent Document 1 discloses silver-coated resin particles in which the resin particles are pretreated with tin to form a catalyst, and the pretreated resin particles are then electrolessly plated with silver to enhance adhesion between the resin particles and the silver coating layer.
[0004] Furthermore, Patent Document 2 discloses silver-coated resin particles in which a silver coating layer is formed on the surface of a resin particle serving as a core particle, the surface of the core particle having a base layer made of fine silver particles and a plurality of hard protrusions made of silver particles protruding from this base layer. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2015-199970 A [Patent Document 2] JP 2020-056088 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, the silver-coated resin particles disclosed in Patent Document 1 have a spherical outer shape and a smooth particle surface, so there are few contact points between the particles and they tend to roll easily. Therefore, when used as a conductive material, there is a problem that the electrical contacts are not stable and the conductivity tends to vary widely.
[0007] In addition, the silver-coated resin particles disclosed in Patent Document 2 had the problem that, within the disclosed size range, the protrusion amount of the hard protrusions relative to the base layer was too large, and therefore, when used as a conductive material, the effect of improving conductivity was limited.
[0008] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide silver-coated resin particles that realize high conductivity when used as a conductive material and can be easily formed at low cost, and a method for producing silver-coated resin particles. [Means for solving the problem]
[0009] In order to solve the above problems, the silver-coated resin particles of aspect 1 of the present invention have a core particle made of resin, a coating layer containing silver covering the surface of the core particle, and a plurality of protruding particles made of silver particles, at least a portion of which protrude from the surface of the coating layer and are formed so as to be scattered in the coating layer, wherein the maximum diameter of the protruding particles is in the range of 1 / 20 to 1 / 8 of the maximum diameter of the core particle, and 20 or more of the protruding particles are formed on one core particle.
[0010] A second aspect of the present invention is characterized in that, in the silver-coated resin particles of the first aspect, the average protrusion height between the outermost part of the protruding particle and the surface of the coating layer is in the range of 1 / 20 or more and 1 / 10 or less of the maximum diameter of the core particle.
[0011] A third aspect of the present invention is characterized in that, in the silver-coated resin particles of the first or second aspect, the average particle size of the core particles is in the range of 1.0 μm or more and 30 μm or less.
[0012] A fourth aspect of the present invention is the silver-coated resin particle according to any one of the first to third aspects, wherein the core particle contains at least one of a silicone resin, an acrylic resin, a styrene resin, and a urethane resin.
[0013] The method for producing silver-coated resin particles of aspect 5 of the present invention is a method for producing silver-coated resin particles of any one of aspects 1 to 4, characterized in that it includes a step of adjusting the temperature of a core particle slurry obtained by dispersing the core particles in water in a range of 5% by mass or more and 10% by mass or less to a range of 10°C or more and 30°C or less, and simultaneously dripping a mixed solution of a silver salt and a silver complexing agent, a pH adjusting solution, and an aqueous reducing agent solution into the core particle slurry to form the coating layer and the protruding particles on the core particles, and the time for dripping the mixed solution, the pH adjusting solution, and the aqueous reducing agent solution into the core particle slurry is in a range of 10 minutes or more and 40 minutes or less from the start of dripping. Effect of the Invention
[0014] According to the present invention, it is possible to provide silver-coated resin particles which realize high conductivity when used as a conductive material and can be easily formed at low cost, and a method for producing silver-coated resin particles. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a silver-coated resin particle according to one embodiment of the present invention. [Diagram 2] FIG. 2 is an enlarged cross-sectional view of a main portion of the silver-coated resin particle of FIG. [Diagram 3] 1 is a SEM photograph of silver-coated resin particles of Example 1 of the present invention in the Examples. [Figure 4] 2 is a SEM photograph of silver-coated resin particles of Comparative Example 1 in the Examples. [Diagram 5] 2 is a SEM photograph of silver-coated resin particles of Comparative Example 2 in the Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, the silver-coated resin particles and the method for producing the silver-coated resin particles according to one embodiment of the present invention will be described with reference to the drawings. Note that each embodiment shown below is specifically described to better understand the gist of the invention, and does not limit the present invention unless otherwise specified. In addition, the drawings used in the following description may show the main parts enlarged for convenience in order to easily understand the features of the present invention, and the dimensional ratios of each component may not necessarily be the same as the actual ones.
[0017] [Silver-coated resin particles] The silver-coated resin particles according to one embodiment of the present invention will now be described. Fig. 1 is a schematic cross-sectional view showing a silver-coated resin particle of the present embodiment, and Fig. 2 is an enlarged cross-sectional view of a main part of the silver-coated resin particle of Fig. 1. Each silver-coated resin particle 10 is composed of a core particle 11, a coating layer 12 formed on the surface of this core particle 11, and a plurality of protruding particles 13 formed so that at least a portion of the protruding particles protrude from the surface of this coating layer 12 and are scattered throughout the coating layer 12.
[0018] The core particle 11 may be a solid particle entirely made of resin. The outer shape of the core particle 11 is preferably as close to spherical as possible, but elliptical particles and particles with larger irregularities than the roughened surface are also acceptable. However, such irregularities are preferably free of sharp corners. If the surface of the core particle 11 has irregularities with sharp corners, there is a concern that the adhesion of the coating film may decrease when forming the coating layer 12 described below, or that the conductivity may decrease when the silver-coated resin particles are used in a conductive paste or the like due to a decrease in dispersibility in the binder.
[0019] The aspect ratio, which is the ratio of the major axis to the minor axis of the core particle 11, is preferably in the range of 1 to 1.5, more preferably in the range of 1 to 1.3, and even more preferably in the range of 1 to 1.1. This aspect ratio is determined by measuring the ratio of the major axis to the minor axis (major axis / minor axis) of each particle by observing 10 particles with a scanning electron microscope (manufactured by Hitachi High-Technologies Corporation: model name: SU-1500) and averaging these values.
[0020] Moreover, the core particles 11 preferably have an average particle diameter of 1.0 μm or more and 30 μm or less, preferably 1.0 μm or more and 10 μm or less. If the average particle diameter is less than 1.0 μm, the ratio of the surface area of the core particles 11 becomes too large, and the amount of silver required to obtain the necessary conductivity as a conductive particle becomes too large, which may increase the manufacturing cost. If the average particle diameter is greater than 30 μm, it becomes difficult to apply the silver-coated resin particles to a fine pattern. The average particle diameter referred to here indicates the volume-based median diameter measured by a laser diffraction particle size distribution meter (manufactured by Shimadzu Corporation: model name: SDLD200VER).
[0021] Examples of materials constituting the core particle 11 include silicone resin particles, aramid resin particles, fluororesin particles, polysulfone resin particles, polyether resin particles, polyimide resin particles, polyamideimide resin particles, epoxy resin particles, phenolic resin particles, acrylic resin particles, acrylic-styrene copolymer particles, polyurethane particles, rubber particles, styrene resin particles, and resin particles having a core-shell structure.
[0022] Specific examples of silicone resin particles include polysilsesquioxane (PSQ) resin particles and polymethylsilsesquioxane (PMSQ) resin particles.Specific examples of aramid resin particles include polymetaphenylene isophthalamide (MPIA) resin particles and polyparaphenylene terephthalamide (PPTA) resin particles.
[0023] Specific examples of fluorine-based particles include polytetrafluoroethylene (PTFE) resin particles, tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride (THV) resin particles, polyvinylidene fluoride (PVDF)-based resin particles, polychlorotrifluoroethylene (PCTFE)-based resin particles, chlorotrifluoroethylene-ethylene (ECTFE)-based resin particles, tetrafluoroethylene-ethylene (ETFE)-based resin particles, tetrafluoroethylene-hexafluoropropylene (FEP)-based resin particles, and tetrafluoroethylene-perfluoroalkyl vinyl ether (PFA)-based resin particles.
[0024] Specific examples of polysulfone resin particles include polyphenylene sulfide (PPS) resin, polyether sulfone (PES) resin, etc. Specific examples of polyether resin particles include polyether ether ketone (PEEK) resin particles, polyphenylene ether (PPE) resin particles, etc. Specific examples of phenol resin particles include novolac type phenol resin, resol type phenol resin, or phenol resins partially modified from these.
[0025] Specific examples of polyurethane particles include polyester-based polyurethane particles and polyol-based polyurethane particles. Specific examples of rubber particles include silicone rubber particles and fluororubber particles. Specific examples of resin particles having a core-shell structure include acrylic resin core-silicone resin shell resin particles. The acrylic resin core-silicone resin shell resin particles can be produced by coating acrylic resin particles with a silicone resin film.
[0026] The coating layer 12 is a layer formed on the surface of the core particle 11 and made of fine silver particles having an average crystallite size smaller than that of the protruding particles 13. Such a coating layer 12 covers the entire surface of the core particle 11 except for the portion where the protruding particles 13 are in direct contact with the surface of the core particle 11. The fine silver particles constituting the coating layer 12 may have a silver content of, for example, 95% by mass or more.
[0027] The average thickness of the coating layer 12 may be, for example, 30 nm or more and 300 nm or less, and more preferably 40 nm or more and 200 nm or less. If the average thickness is less than 30 nm, there may be areas where the surface of the core particle 11 is exposed without being covered with the coating layer 12, which may reduce the conductivity of the silver-coated resin particle 10. If the average thickness exceeds 200 nm, the coating layer 12 may easily peel off, which may cause poor electrical continuity. The average thickness of the coating layer 12 can be calculated by observing the cross-sectional shape of the silver-coated resin particle 10 with a transmission electron microscope.
[0028] The average crystallite size of the fine silver particles constituting the coating layer 12 may be 10 nm or more and 400 nm or less. The average crystallite size of the fine silver particles constituting the coating layer 12 can be obtained as follows. First, silver-coated resin particles 10 sprinkled on a carbon sample stage were cross-sectionally exposed to a thickness of about 100 nm using a FIB (focused ion beam device) to prepare a sample. Next, the cross-sectional shape of the silver / resin particle interface in the cross-sectionally exposed sample was observed using a transmission electron microscope (TEM) for 10 silver-coated resin particles 10 in a range of 5000 nm from the surface of the core particle 11 in the thickness direction, divided into multiple sections so that the entire coating layer 12 could be observed without overlap, and the crystal orientation distribution of the coating layer 12 was obtained.
[0029] The crystal orientation distribution was obtained as follows. Using a crystal orientation analyzer attached to a transmission electron microscope (TEM), an electron beam tilted at 0.5 to 1.0 degrees with respect to the normal direction of the polished surface was irradiated in precession while scanning with the electron beam, continuously capturing electron diffraction patterns, and obtaining electron diffraction patterns for each measurement point. The conditions for obtaining the electron diffraction pattern used in this measurement were an acceleration voltage of 200 kV, a camera length of 20 cm, a beam size of 2.2 nm, and a measurement step of 5.0 nm.
[0030] The obtained electron diffraction pattern for each measurement point was compared with a pre-calculated electron diffraction pattern for an arbitrary orientation of a cubic crystal, and the crystal orientation that best matched was determined as the crystal orientation for that measurement point. Among the obtained crystal orientations, those with a minimum grain boundary angle of 5 degrees and a crystallite size of 5 nm or less were removed as noise, and an image with the identified crystal orientation distribution was obtained by outputting the image.
[0031] The crystallite size was measured for the obtained image using the image processing software "imageJ:NIH". Specifically, the measurement was performed as follows. First, the measurement scale in the software was set according to the scale of the observed image. Next, the crystallites were determined based on the grain boundaries determined from the image in which the crystal orientation distribution was identified, obtained by the above-mentioned method, and for all crystallites in the observed image, the length of the line segment connecting any two points of the grain boundaries of each crystallite was measured by the software when the length was the longest, and this was taken as the crystallite size of the crystallite. This corresponds to the Feret size. Furthermore, the average value of all the measured crystallite sizes was calculated, and this value was taken as the average crystallite size of the fine silver particles constituting the coating layer 12.
[0032] The protruding particles 13 are formed so that at least a portion of each protruding particle 13 protrudes from the surface of the coating layer 12 and are scattered throughout the coating layer 12 . Each protruding particle 13 is a large-diameter silver particle having a polygonal outer shape and an average crystallite size larger than that of the fine silver particles constituting the coating layer 12. The large-diameter silver particles constituting such protruding particles 13 may have a silver content of, for example, 95% by mass or more.
[0033] As shown in FIG. 2, the protruding particles 13 may be formed so that a portion of them is in contact with the surface of the core particle 11, or they may be formed so that a portion of them is embedded in the coating layer 12 without contacting the surface of the core particle 11.
[0034] The maximum diameter of the protruding particles 13 is in the range of 1 / 20 or more and 1 / 8 or less of the diameter of the core particle 11. If the maximum diameter of the protruding particles 13 is less than 1 / 20 of the diameter of the core particle 11, the size of the protruding particles 13 is too small compared to the size of the core particle 11, and the amount of protruding particles 13 protruding from the surface of the coating layer 12 becomes small, so that there is a concern that when the silver-coated resin particles 10 are used in a conductive paste or the like, the adhesive effect to an electrode layer or the like will be too low.
[0035] On the other hand, if the maximum diameter of the protruding particles 13 exceeds 1 / 8 of the diameter of the core particle 11, the size of the protruding particles 13 will be too large compared to the size of the core particle 11, and there is a risk that the protruding particles 13 will be easily detached from the core particle 11 or the coating layer 12.
[0036] Furthermore, 20 or more protruding particles 13 are formed per core particle 11. If the number of protruding particles 13 formed per core particle 11 is less than 20, there is a concern that when the silver-coated resin particles 10 are used in a conductive paste or the like, the adhesive effect to an electrode layer or the like will be reduced, resulting in reduced conductivity.
[0037] There is no upper limit to the number of protruding particles 13 as long as there are 20 or more per core particle 11, but if the protruding particles 13 are formed so densely that adjacent protruding particles 13 come into contact with each other, there is a risk that the protruding particles 13 may easily fall off from the core particle 11 or the coating layer 12. For this reason, it is preferable that the protruding particles 13 are formed so that a certain distance is maintained between them and part of the surface of the coating layer 12 is exposed between them.
[0038] The average protruding height between the outermost portion of the protruding particles 13 and the surface of the coating layer 12 may be in the range of 1 / 20 or more and 1 / 10 or less of the maximum diameter of the core particles 11. If the average protruding height of the protruding particles 13 is less than 1 / 20 of the maximum diameter of the core particles 11, the protruding height of the protruding particles 13 from the surface of the coating layer 12 is low, and there is a concern that when the silver-coated resin particles 10 are used in a conductive paste or the like, the adhesive effect to an electrode layer or the like will be too low.
[0039] On the other hand, if the average protruding height of the protruding particles 13 exceeds 1 / 10 of the maximum diameter of the core particle 11, the protruding height of the protruding particles 13 from the surface of the coating layer 12 will be too high, and there is a risk that the protruding particles 13 will be easily detached from the core particle 11 or the coating layer 12.
[0040] The average crystallite diameter of the protruding particles 13 may be, for example, 200 nm or more and 1000 nm or less, preferably 200 nm or more and 500 nm or less. If the average crystallite diameter is less than 200 nm, when the silver-coated resin particles 10 are used in a conductive paste, etc., the adhesive effect to the electrode layer, etc. may be reduced, and the conductivity may be reduced. If the average crystallite diameter exceeds 1000 nm, the protruding particles 13 may easily fall off from the core particles 11 and the coating layer 12.
[0041] The average protruding height and average crystallite diameter of the above-mentioned protruding particles 13 can be calculated, for example, by using a transmission electron microscope and a crystal orientation analyzer to capture an image and measure the image in which the crystal orientation distribution is identified using image processing software.
[0042] For example, the protruding particles 13 are a group of crystallites located outside the coating layer 12, and the average crystallite diameter is their average Feret diameter. The average protruding height refers to the vertical distance from the surface of the coating layer 12 to the tip of the protruding particles 13, and even when the protruding particles 13 protrude from the surface of the core particle 11, it refers to the vertical distance from the surface of the coating layer 12 to the tip of the protruding particles 13.
[0043] These protruding particles 13 have an average crystallite diameter larger than that of the fine silver particles constituting the coating layer 12 and have high crystallinity, so that when used in a conductive paste or the like, the protruding particles 13 can be embedded into an electrode layer or the like. The protruding particles 13 may be formed so that all of them protrude from the surface of the coating layer 12 or from inside the coating layer 12, or all of them protrude from the surface of the core particle 11, or a mixture of these. The form of these protruding particles 13 can be controlled by the manufacturing conditions in the method for manufacturing silver-coated resin particles described below.
[0044] The silver-coated resin particles 10 having the above-mentioned configuration have a volume resistivity of 1×10 -2 It is sufficient if it is less than Ω cm, and it is 3×10 -3 It is more preferable that the volume resistivity is 1×10 -2 If the resistivity is higher than Ω·cm, the loss due to the voltage drop becomes large, which is not preferable as a conductive material. Note that the volume resistivity can be calculated, for example, by placing the silver-coated resin particles 10 in a powder state in a pressure vessel and compressing them at 9.8 MPa to obtain a green compact, and measuring the resistance value of the green compact with a resistivity meter.
[0045] The amount of silver coating (silver content) of the silver-coated resin particles 10 configured as above, which is the total amount of the fine silver particles in the coating layer 12 and the silver particles in the protruding particles 13, depends on the average particle diameter of the core particles 11 and is determined by the required level of conductivity, and may be, for example, 2 to 80 parts by mass, more preferably 28 to 70 parts by mass, and even more preferably 28 to 60 parts by mass, per 100 parts by mass of the silver-coated resin particles.
[0046] If the silver content is less than 2 parts by mass per 100 parts by mass of silver-coated resin particles, for example, when the silver-coated resin particles are dispersed as a conductive paste, the number of contact points between silver particles will be reduced, and it may be difficult to impart conductivity. On the other hand, if the silver content exceeds 80 parts by mass, the specific gravity will increase, the cost will be high, and the conductivity will not improve as much as the silver content due to saturation of the conductivity.
[0047] According to the silver-coated resin particle 10 of the present embodiment having the above-mentioned configuration, the maximum diameter of the protruding particles 13 is set to be in the range of 1 / 20 to 1 / 8 of the maximum diameter of the core particle 11, and 20 or more of these protruding particles 13 are formed for one core particle 11, so that when the silver-coated resin particle 10 is used as a conductive material, the contact area of the protruding particles 13 with the electrode or the like to be connected is increased, and as a result, high conductivity can be realized. In addition, by preventing the maximum diameter of the protruding particles 13 from becoming too large relative to the core particle 11, it is possible to prevent the protruding particles 13 from falling off the core particle 11 or the coating layer 12, and thus realize a silver-coated resin particle 10 with excellent durability.
[0048] [Application examples of silver-coated resin particles] The silver-coated resin particles 10 of this embodiment are excellent as conductive fillers, and can be particularly suitably used as conductive fillers for conductive materials such as conductive adhesives, conductive films (sheets), conductive rubbers (elastomers), conductive pressure sensitive adhesives, TIM (Thermal Interface Material) materials such as heat dissipation sheets and heat dissipation greases, or conductive materials such as conductive spacers.
[0049] (Conductive adhesive) Conductive adhesives are classified into isotropic conductive adhesives (ICA) and anisotropic conductive adhesives (ACA). They are also available in paste, film, and ink forms depending on the binder type. In isotropic conductive adhesives, the binder shrinks when hardening, causing the fillers to come into contact with each other in all directions, vertically, horizontally, and diagonally, which brings the fillers into contact with the conductive objects to be connected, providing conductivity. It is also possible to form sheets using isotropic conductive adhesives.
[0050] The anisotropic conductive adhesive has silver-coated resin particles 10 dispersed in a binder as a filler, and the anisotropic conductive adhesive is sandwiched between the conductive objects to be connected. By applying pressure vertically, the filler between the conductive objects to be connected comes into contact with the conductive objects to be connected vertically, providing conductivity. On the other hand, in the non-pressurized portion, the fillers are arranged horizontally via the binder, which is an insulator, and do not come into contact with each other, so no conductivity is obtained.
[0051] Examples of the conductive adhesive include anisotropic or isotropic conductive paste, and anisotropic or isotropic conductive ink. The conductive adhesive is prepared by uniformly mixing the silver-coated resin particles 10 and the insulating binder resin using a kneader such as a planetary mixer or a three-roll mill. In such a conductive adhesive, the silver-coated resin particles 10 are uniformly dispersed in the insulating binder resin. The content of the silver-coated resin particles 10 is not particularly limited and is appropriately determined depending on the application, but may be within the range of 0.5 parts by mass to 90 parts by mass with respect to 100 parts by mass of the binder resin.
[0052] The insulating binder resin in the conductive adhesive is not particularly limited, and examples thereof include thermoplastic resins and compositions that are cured by heat or light, such as curable resin compositions. Examples of the thermoplastic resin include styrene-butadiene block copolymer, acrylic resin, ethylene-vinyl acetate resin, phenoxy resin, etc. Examples of the thermosetting resin composition include a resin composition containing a resin such as a silicone resin or an epoxy resin, or a mixture thereof, as a main component.
[0053] (Conductive film (sheet)) The conductive film may be an anisotropic or isotropic conductive film formed into a film shape. The conductive film is produced by first preparing a resin composition in which silver-coated resin particles 10 are dispersed in an insulating binder resin, and then applying the resin composition to the surface of a support film such as PET. The resin composition can be prepared by uniformly mixing the silver-coated resin particles 10 and the insulating binder resin using a kneader such as a planetary mixer or a three-roll mill.
[0054] In the conductive film, the silver-coated resin particles 10 are uniformly dispersed in the insulating binder resin on the support film. Examples of the insulating binder resin in the conductive film include resin compositions containing, as a main component, resins such as acrylic resins, silicone resins, epoxy resins, and phenoxy resins, or mixtures thereof. The content of the silver-coated resin particles 10 in the resin composition in the conductive film is not particularly limited and is appropriately determined depending on the application, but is preferably within the range of 0.5 to 90 parts by mass with respect to 100 parts by mass of the binder resin.
[0055] (Conductive rubber (elastomer)) Conductive rubber includes conductive rubber formed into a sheet or a rectangular parallelepiped shape, and can be used as a heat dissipation sheet or a conductive connector. Conductive rubber is produced by first kneading a binder rubber, a vulcanizing agent, and silver-coated resin particles 10 using a biaxial roll or the like, and then vulcanizing and molding the mixture by applying heat and pressure using a heating press or dryer. Examples of the binder rubber in the conductive rubber include nitrile rubber, acrylic rubber, styrene butadiene rubber, silicone rubber, and fluororubber. The content of the silver-coated resin particles 10 in the composition of the conductive rubber is not particularly limited and is appropriately determined depending on the application, but is preferably within the range of 0.5 parts by mass to 90 parts by mass with respect to 100 parts by mass of the binder rubber.
[0056] (Conductive adhesive) The conductive adhesive includes a conductive adhesive or a conductive gel formed into a sheet or a rectangular parallelepiped shape, and can be used as an electrical contact material, a heat dissipation sheet, and an electrode. The conductive adhesive can be produced by first preparing an adhesive composition in which the silver-coated resin particles 10 are dispersed in an adhesive that serves as an insulating binder, and then applying the adhesive composition to the surface of a support film such as PET.
[0057] Examples of the binder adhesive in the conductive adhesive include acrylic adhesives, urethane adhesives, silicone adhesives, etc. The content of the silver-coated resin particles 10 in the composition of the conductive adhesive is not particularly limited and is appropriately determined depending on the application, etc., but is preferably within the range of 0.5 parts by mass to 90 parts by mass with respect to 100 parts by mass of the adhesive.
[0058] (Thermal grease) The thermal grease may be a mixture of a non-volatile base oil and silver-coated resin particles 10, and may be used as a thermal material. The thermal grease is prepared by uniformly mixing the base oil and the silver-coated resin particles 10 using a kneader such as a planetary mixer or a three-roll mill. Examples of the base oil used in the thermal grease include silicone oil-based base oils, mineral oil-based base oils, synthetic hydrocarbon-based base oils, ester-based base oils, ether-based base oils, and glycol-based base oils, or combinations thereof. The content of the silver-coated resin particles 10 in the composition of the thermal grease is not particularly limited and is appropriately determined depending on the application, but is preferably within the range of 0.5 parts by mass to 90 parts by mass with respect to 100 parts by mass of the base oil.
[0059] (Conductive spacer) Conductive spacers are used in liquid crystal display devices to form the wiring between the two upper and lower substrates that sandwich the liquid crystal material. The conductive spacer is used by electrically connecting the upper and lower substrates and maintaining the gap between the substrates at a specified dimension. The conductive spacer is prepared by first adding the silver-coated resin particles 10 to an insulating binder resin such as a thermosetting resin or an ultraviolet light curing adhesive, and then uniformly mixing the silver-coated resin particles 10 and the binder resin using a kneader such as a planetary mixer or a three-roll mill to prepare a resin composition.
[0060] Next, the above-mentioned resin composition is applied to one or both of the wiring portions of the upper and lower two substrates, and the two substrates are laminated together to produce the substrate. The content of the silver-coated resin particles 10 is not particularly limited and is appropriately determined depending on the application, but is preferably within the range of 2 parts by mass to 10 parts by mass per 100 parts by mass of the binder resin.
[0061] [Method of manufacturing silver-coated resin particles] Next, a method for producing silver-coated resin particles according to one embodiment of the present invention will be described. The method for producing silver-coated resin particles 10 of this embodiment is a method for precipitating and forming coating layer 12 and protruding particles 13 on the surface of core particle 11 using a silver liquid containing silver salt and silver complexing agent, a pH adjusting liquid, and an aqueous reducing agent solution.
[0062] First, core particles 11 having an average particle size in the range of 1.0 μm or more and 30 μm or less are prepared. In this embodiment, silicone resin particles having an average particle size of 20 μm are used as the core particles 11.
[0063] Next, a dropping liquid for precipitating silver is prepared. As the silver salt constituting the silver liquid in the dropping liquid, silver nitrate or silver dissolved in nitric acid can be used. As the silver complexing agent constituting the silver liquid, for example, salts such as ammonia, ethylenediaminetetraacetic acid, tetrasodium ethylenediaminetetraacetate, nitrotriacetic acid, triethylenetetraaminehexaacetic acid, sodium thiosulfate, succinate, succinimide, citrate, etc. can be used. It is preferable that such a silver complexing agent is completely dissolved in the silver liquid.
[0064] Of the liquids to be dropped, examples of the pH adjusting liquid include an aqueous solution of sodium hydroxide and an aqueous solution of potassium hydroxide.
[0065] The reducing agent may be, for example, formalin, glucose, Rochelle salt (potassium sodium tartrate), hydrazine and its derivatives, hydroquinone, L-ascorbic acid, or formic acid. In particular, formalin, which is an aqueous solution of formaldehyde, is preferred, a mixture of two or more reducing agents containing at least formaldehyde is more preferred, and a mixture of reducing agents containing formaldehyde and glucose is most preferred. The reducing agent aqueous solution is formed by dissolving these reducing agents in pure water.
[0066] Next, water is added to the core particles 11 to form a core particle slurry in which the core particles 11 are dispersed in water. The ratio of the core particles 11 contained in the core particle slurry may be, for example, in the range of 5% by mass or more and 10% by mass or less. The temperature of this core particle slurry is adjusted to a range of 10°C or more and 30°C or less, preferably 15°C or more and 25°C or less. If the core particle slurry is at a temperature below 10°C, the crystal particles of the coating layer 12 become coarse, and if it exceeds 30°C, the coating layer 12 becomes easily peeled off from the core particles 11 due to rapid precipitation of silver. If it is within the normal room temperature range (20°C to 25°C), there is no need to perform heating or cooling.
[0067] Then, the core particle slurry is stirred using a stirring device or the like to uniformly disperse the core particles 11, while the above-mentioned three liquids, i.e., the silver liquid (silver salt and silver complexing agent), pH adjusting liquid, and aqueous reducing agent solution, are simultaneously dripped into the core particle slurry. Note that the pH adjusting liquid and the aqueous reducing agent solution may be mixed in advance, and the two liquids may be simultaneously dripped together with the silver liquid.
[0068] The dripping time of each dripping liquid is set to be in the range of 10 minutes or more and 40 minutes or less from the start of dripping. If the dripping time is less than 10 minutes, all the particles will be fine silver particles that compose the coating layer 12, and protruding particles 13 with a larger average particle size will not be formed. If the dripping time exceeds 40 minutes, the protruding particles 13 will be formed too densely, and there is a concern that they will be easily peeled off from the core particles 11.
[0069] In addition, within the above-mentioned dropping time, the dropping speed of each of the silver solution, the pH adjusting solution, and the aqueous reducing agent solution is preferably set to be in the range of 30 mL / min to 200 mL / min.
[0070] By simultaneously dripping three liquids, namely, silver liquid (silver salt and silver complexing agent), pH adjusting liquid, and reducing agent aqueous solution, into the core particle slurry within the dripping time range described above, a large number of fine silver particles that constitute the coating layer 12 are formed in the early stages of dripping, and then, as the dripping proceeds, protruding silver particles 13 with an average particle size larger than the fine silver particles grow.
[0071] By the method for producing silver-coated resin particles of this embodiment as described above, it is possible to produce silver-coated resin particles 10 each having a coating layer 12 made of fine silver particles that covers the surface of a core particle 11, and 20 or more protruding particles 13 each having a maximum diameter in the range of 1 / 20 or more and 1 / 8 or less of the maximum diameter of the core particle 11.
[0072] Although the embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope of the invention and its equivalents described in the claims, as well as in the scope and spirit of the invention. EXAMPLES
[0073] The effects of the present invention were verified below. Silicone resin core particles (product number: KMP-701, manufactured by Shin-Etsu Chemical Co., Ltd.) having an average particle size of 4 μm were dispersed in pure water to a concentration of 5 mass % to form a core particle slurry. While stirring this core particle slurry using a magnetic stirrer, three liquids (dropping liquids), namely, a silver liquid (silver salt and silver complexing agent), a pH adjusting liquid, and an aqueous reducing agent solution, were simultaneously dropped into the core particle slurry (except for Comparative Example 1), thereby producing silver-coated resin particles (samples).
[0074] Silver nitrate was used as the silver salt (silver nitrate concentration in the dropped silver solution: 30% by mass). Tetrasodium ethylenediaminetetraacetate was used as the silver complexing agent (concentration in the dropped solution: 9.8% by mass). A sodium hydroxide aqueous solution with a concentration of 12.5% by mass was used as the pH adjusting solution. Formalin was used as the reducing agent for the aqueous reducing agent solution (concentration: 5% by mass).
[0075] (Example 1 of the present invention) The core particle concentration in the silicone core particle slurry was 5% by mass, the liquid temperature of the core particle slurry was kept at 20° C., and the dropping time of the dropping liquid was 20 minutes. (Invention Example 2) The core particle concentration in the silicone core particle slurry was 5 mass %, the liquid temperature of the core particle slurry was kept at 15°C, and the dropping time of the dropping liquid was 10 minutes. (Example 3 of the present invention) The core particle concentration in the acrylic core particle slurry was kept at 8 mass %, the liquid temperature of the core particle slurry was kept at 20° C., and the dropping time of the dropping liquid was set to 30 minutes. (Example 4 of the present invention) The core particle concentration in the styrene core particle slurry was kept at 5 mass %, the liquid temperature of the core particle slurry was kept at 20° C., and the dropping time of the dropping liquid was set to 10 minutes. (Invention Example 5) The core particle concentration in the silicone core particle slurry was kept at 10 mass %, the liquid temperature of the core particle slurry was kept at 20° C., and the dropping time of the dropping liquid was 30 minutes. (Example 6 of the present invention) The core particle concentration in the acrylic core particle slurry was kept at 10% by mass, the liquid temperature of the core particle slurry was kept at 20° C., and the dropping time of the dropping liquid was set to 30 minutes. (Invention Example 7) The core particle concentration in the silicone core particle slurry was 5 mass %, the liquid temperature of the core particle slurry was kept at 30° C., and the dropping time of the dropping liquid was 20 minutes. (Example 8 of the present invention) The core particle concentration in the urethane core particle slurry was kept at 5 mass %, the liquid temperature of the core particle slurry was kept at 20° C., and the dropping time of the dropping liquid was set to 15 minutes.
[0076] Comparative Example 1 Three liquids, namely, a silver liquid (silver salt and silver complexing agent), a pH adjusting liquid, and an aqueous solution of a reducing agent, were dissolved in advance in a silicone core particle slurry, and the solution was kept at 20° C. and allowed to stand for 20 minutes. Comparative Example 2 The core particle concentration in the silicone core particle slurry was 5 mass %, the liquid temperature of the core particle slurry was kept at 20° C., and the dropping time of the dropping liquid was 7 minutes. Comparative Example 3 The core particle concentration in the silicone core particle slurry was 12 mass %, the liquid temperature of the core particle slurry was kept at 20° C., and the dropping time of the dropping liquid was 20 minutes. Comparative Example 4 The core particle concentration in the silicone core particle slurry was 5 mass %, the liquid temperature of the core particle slurry was kept at 20° C., and the dropping time of the dropping liquid was 50 minutes. Comparative Example 5 The core particle concentration in the silicone core particle slurry was kept at 5 mass %, the liquid temperature of the core particle slurry was kept at 5° C., and the dropping time of the dropping liquid was set to 10 minutes. Comparative Example 6 The core particle concentration in the silicone core particle slurry was kept at 3 mass %, the liquid temperature of the core particle slurry was kept at 20° C., and the dropping time of the dropping liquid was set to 15 minutes.
[0077] For each of the above samples of Examples 1 to 8 of the present invention and Comparative Examples 1 to 6, the number of protruding particles per silver-coated resin particle, the average particle diameter of the protruding particles, the ratio of the maximum diameter of the protruding particles to the maximum diameter of the core particle, and the average particle diameter of the fine silver particles that make up the coating layer were each measured. The number and average particle size of the protruding particles, the diameter ratio, and the average particle size of the fine silver particles were each measured by photographing them with a scanning microscope and then processing the images using the image processing software "imageJ:NIH."
[0078] The shapes of the silver-coated resin particles formed were observed based on SEM photographs. The shapes of each particle are as follows: Chestnut-shaped: 20 or more protruding particles with an average particle diameter of 1 / 20 to 1 / 8 the diameter of the core particle are formed from one core particle. No protruding particles: No protruding particles were found protruding from the surface of the coating layer. Coarse protruding particles: The average particle diameter of the protruding particles is 1 / 8 or more of the diameter of the core particle. Almost no protruding particles: There are 5 or fewer protruding particles protruding from the surface of the coating layer. Silver particle precipitation in places other than core particles: Silver particles are present that are isolated and not in contact with the core particle or coating layer.
[0079] Furthermore, the silver-coated resin particles of each sample were used as a conductive filler and uniformly dispersed in epoxy resin (before curing) to a concentration of 50% by volume to create a conductive paste. The conductive paste of each sample was then applied to a substrate and cured to form a coating film with a thickness of 50 μm. The surface resistance of each coating film was then measured. The surface resistance was measured using a resistance meter (Loresta, manufactured by Mitsubishi Chemical Corporation) by measuring the surface resistance of the center of a measurement sample measuring 10 cm x 10 cm square. The surface resistance was evaluated using a ratio of 1.0 x 10 -3 (Ω / □) or less is marked as "〇", 1.0×10 -3 Beyond 1.0×10 -2 (Ω / □) or less is marked as "△", 1.0×10 -2 (Ω / □) or more was marked as "×". The conditions for each sample are shown in Table 1, and the measurement results are shown in Table 2.
[0080] [Table 1]
[0081] [Table 2]
[0082] According to the results shown in Table 1, it was confirmed that the silver-coated resin particles of Examples 1 to 7 of the present invention, which were obtained by setting the core particle concentration in the core particle slurry in the range of 5% by mass or more and 10% by mass or less, the liquid temperature of the core particle slurry during dripping of the dripping liquid in the range of 10° C. or more and 30° C. or less, and the dripping time of the dripping liquid in the range of 10 minutes or more and 40 minutes or less, all had a maximum diameter of the protruding particles in the range of 1 / 20 to 1 / 8 of the maximum diameter of the core particle, and each silver-coated resin particle had 20 or more protruding particles formed thereon. Furthermore, it was confirmed that the coating films formed with the conductive pastes using the silver-coated resin particles of Examples 1 to 8 of this embodiment all had a surface resistivity of 1.0×10 -3 (Ω / □) or less, showing excellent conductivity.
[0083] On the other hand, the number of protruding particles in the silver-coated resin particles obtained in Comparative Examples 1 to 6 was less than 20, and the coating films formed from the conductive pastes using these particles all had a surface resistivity of 1.0 × 10 -3 It was confirmed that the electrical conductivity was low.
[0084] FIG. 3 shows an SEM photograph of the silver-coated resin particles of Inventive Example 1, FIG. 4 shows an SEM photograph of the silver-coated resin particles of Comparative Example 1, and FIG. 5 shows an SEM photograph of the silver-coated resin particles of Comparative Example 2. FIG. 3 shows that the silver-coated resin particles of Example 1 of the present invention are formed so that a core particle is covered with a coating layer made of fine silver particles, and a plurality of protruding particles protrude from the surface of the coating layer. On the other hand, it is seen that no protruding particles are formed on the surface of the coating layer covering the core particles in the silver-coated resin particles of Comparative Example 1. Also, it is seen that the silver-coated resin particles of Comparative Example 2 have silver particles precipitated in areas other than the core particles. [Explanation of symbols]
[0085] 10...Silver-coated resin particles 11…Core particle 12…Covering layer 13...Protruding particles
Claims
1. A core particle made of a resin; a coating layer containing silver that covers the surface of the core particle; a plurality of protruding particles, at least a portion of which protrudes from the surface of the coating layer and is formed so as to be scattered in the coating layer, and the protruding particles are made of silver particles, Silver-coated resin particles, characterized in that the maximum diameter of the protruding particles is in the range of 1 / 20 to 1 / 8 of the maximum diameter of the core particle, and 20 or more of the protruding particles are formed on one core particle.
2. 2. The silver-coated resin particle according to claim 1, wherein the average protruding height between the outermost part of the protruding particle and the surface of the coating layer is in the range of 1 / 20 or more and 1 / 10 or less of the maximum diameter of the core particle.
3. 3. The silver-coated resin particle according to claim 1, wherein the average particle diameter of the core particle is in the range of 1.0 μm or more and 30 μm or less.
4. 3. The silver-coated resin particle according to claim 1, wherein the core particle contains at least one of a silicone resin, an acrylic resin, a styrene resin, and a urethane resin.
5. A method for producing silver-coated resin particles according to claim 1 or 2, comprising the steps of: the core particles are dispersed in water in an amount of 5% by mass or more and 10% by mass or less to obtain a core particle slurry, the temperature of which is adjusted to a range of 10° C. or more and 30° C. or less, and a mixed solution of a silver salt and a silver complexing agent, a pH adjusting solution, and an aqueous reducing agent solution are simultaneously dropped into the core particle slurry to form the coating layer and the protruding particles on the core particles, A method for producing silver-coated resin particles, characterized in that the time for dropping the mixed solution, the pH adjusting solution, and the reducing agent aqueous solution to the core particle slurry is in the range of 10 minutes or more and 40 minutes or less from the start of dropping.
Citation Information
Patent Citations
Silver coated spherical resin particle, method for manufacturing the same, and conductive composition using silver coated spherical resin particle
JP2015199970A
Silver coated resin particle and method for manufacturing the same
JP2020056088A