Fire-resistant multilayer pipe
The fire-resistant multilayer pipe with a specific composition of vinyl chloride resin, thermally expandable graphite, and impact modifier addresses the issue of maintaining strength and impact resistance, ensuring effective fire containment by sealing gaps during a fire.
Patent Information
- Application Number
- JP2023057876
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Conventional fire-resistant multilayer pipes face challenges in maintaining impact resistance while preventing a decrease in mechanical strength, particularly when the diameter is large, and thermally expandable resin pipes may suffer from low strength after expansion, leading to potential dripping of combustion materials and reduced fire resistance.
A fire-resistant multilayer pipe design comprising a fire-resistant layer with a vinyl chloride resin, thermally expandable graphite, and an impact modifier, where the impact modifier content is between 0.5 to 3.5 parts by weight, enhancing impact resistance and preventing a decrease in mechanical strength, even at larger diameters.
The proposed design improves impact resistance and maintains mechanical strength, effectively preventing fire spread by expanding to seal compartment penetration spaces during a fire.
Smart Images

Figure 2024145499000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a fire-resistant multi-layer pipe. [Background technology]
[0002] In the walls, floors, and other partitions of a building, holes are sometimes provided to form partition penetrations through which pipes and the like can pass. In addition, buildings are usually provided with fire compartments to prevent the rapid spread of flames and smoke in the event of a fire. In fire compartments, as a general rule, pipes other than those with a specified fire resistance cannot be installed by passing them through the partition penetrations.
[0003] Plastic pipes with thermal expansion (fire-resistant pipes) are sometimes used as piping to pass through compartment penetrations. By using plastic pipes with thermal expansion, the plastic pipes expand due to the heat of a fire, blocking the gap between the plastic pipes and the wall of the compartment penetration, preventing the spread of fire.
[0004] The following Patent Document 1 discloses a building piping material that contains polyvinyl chloride resin and thermally expandable graphite, and the content of the thermally expandable graphite is 1 to 10 parts by weight per 100 parts by weight of the polyvinyl chloride resin. The building piping material is a single-layered resin pipe.
[0005] The following Patent Document 2 discloses a multi-layer fireproof piping material including a fireproof expansion layer and a coating layer that covers at least one of the outside and inside of the fireproof expansion layer. In this multi-layer fireproof piping material, the fireproof expansion layer contains 100 parts by weight of polyvinyl chloride resin and 1 to 15 parts by weight of thermally expandable graphite, and the coating layer contains polyvinyl chloride resin. In the examples of Patent Document 2, the coating layer contains an inorganic filler in an amount of 3 parts by weight relative to 100 parts by weight of polyvinyl chloride resin. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2008-180068 A [Patent Document 2] JP 2008-180367 A Summary of the Invention [Problem to be solved by the invention]
[0007] In a single-layered resin pipe containing thermally expandable graphite as described in Patent Document 1, the strength of the resin pipe after thermal expansion may be low. If the strength of the resin pipe after thermal expansion is low, dripping of combustion products may occur, and fire resistance may decrease.
[0008] In addition, in conventional multi-layer fire-resistant pipes, an impact modifier may be added to improve impact resistance. However, when an impact modifier is added to a conventional multi-layer fire-resistant piping material as described in Patent Document 2, there is a problem that mechanical strength such as tensile strength and flattening strength is reduced. The present inventors found that this problem is particularly significant when the diameter of the multi-layer fire-resistant pipe is relatively large.
[0009] In conventional fire-resistant multi-layer pipes, it is difficult to improve impact resistance and prevent a decrease in mechanical strength.
[0010] An object of the present invention is to provide a multi-layer fire-resistant pipe which has improved impact resistance and is capable of preventing a decrease in mechanical strength. [Means for solving the problem]
[0011] The following fire-resistant multi-layer pipe is disclosed herein:
[0012] Item 1. A fire-resistant multi-layer pipe comprising a fire-resistant layer and at least one of an inner layer disposed inside the fire-resistant layer and an outer layer disposed outside the fire-resistant layer, the outer diameter of the fire-resistant multi-layer pipe being 180 mm or more, the fire-resistant layer containing a polyvinyl chloride resin, thermally expandable graphite, and an impact modifier, the content of the impact modifier contained in the fire-resistant layer being 0.5 parts by weight or more and 3.5 parts by weight or less per 100 parts by weight of the polyvinyl chloride resin contained in the fire-resistant layer.
[0013] Item 2. The fire-resistant multi-layer pipe according to item 1, wherein the impact modifier comprises chlorinated polyethylene.
[0014] Item 3. The fire-resistant multi-layer pipe according to item 1 or 2, wherein the content of the impact modifier contained in the fire-resistant layer is 1.0 part by weight or more and 3.0 parts by weight or less relative to 100 parts by weight of the vinyl chloride resin contained in the fire-resistant layer.
[0015] Item 4. The fire-resistant multi-layer pipe according to any one of Items 1 to 3, wherein the content of the thermally expandable graphite contained in the fire-resistant layer is 1.0 part by weight or more and 15.0 parts by weight or less relative to 100 parts by weight of the vinyl chloride resin contained in the fire-resistant layer.
[0016] Item 5. The fire-resistant multi-layer pipe according to any one of items 1 to 4, comprising the fire-resistant layer, an inner layer disposed inside the fire-resistant layer, and an outer layer disposed outside the fire-resistant layer. Effect of the Invention
[0017] The multi-layer fire-resistant pipe according to the present invention is a multi-layer fire-resistant pipe comprising a fire-resistant layer and at least one of an inner layer disposed inside the fire-resistant layer and an outer layer disposed outside the fire-resistant layer. In the multi-layer fire-resistant pipe according to the present invention, the outer diameter of the multi-layer fire-resistant pipe is 180 mm or more. In the multi-layer fire-resistant pipe according to the present invention, the fire-resistant layer contains a vinyl chloride resin, thermally expandable graphite, and an impact modifier, and the content of the impact modifier contained in the fire-resistant layer is 0.5 parts by weight or more and 3.5 parts by weight or less per 100 parts by weight of the vinyl chloride resin contained in the fire-resistant layer. Since the multi-layer fire-resistant pipe according to the present invention has the above configuration, it is possible to increase impact resistance and prevent a decrease in mechanical strength. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a cross-sectional view showing a schematic diagram of a multi-layer fire-resistant pipe according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a plan view showing a schematic diagram of a manufacturing apparatus used for manufacturing a multi-layer fire-resistant pipe according to one embodiment of the present invention. [Diagram 3] FIG. 3 is a front view showing a schematic diagram of a manufacturing apparatus used for manufacturing a multi-layer fire-resistant pipe according to one embodiment of the present invention. [Figure 4] FIG. 4 is an enlarged cross-sectional view showing a mold portion and a tube portion for forming an outer surface of a pipe in a manufacturing apparatus. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The present invention will be described in detail below.
[0020] The multi-layer fire-resistant pipe of the present invention comprises a fire-resistant layer and at least one of an inner layer disposed inside the fire-resistant layer and an outer layer disposed outside the fire-resistant layer. In the multi-layer fire-resistant pipe of the present invention, the outer diameter of the multi-layer fire-resistant pipe is 180 mm or more. In the multi-layer fire-resistant pipe of the present invention, the fire-resistant layer contains a polyvinyl chloride resin, thermally expandable graphite, and an impact modifier, and the content of the impact modifier in the fire-resistant layer is 0.5 parts by weight or more and 3.5 parts by weight or less per 100 parts by weight of the polyvinyl chloride resin contained in the fire-resistant layer.
[0021] In conventional multi-layer fire-resistant pipes, when an impact modifier is added, there is a problem that mechanical strength such as tensile strength and flattening strength is reduced. The present inventors have found that this problem is particularly significant when the diameter of the multi-layer fire-resistant pipe is relatively large (for example, the outer diameter is 180 mm or more).
[0022] Since the fire-resistant multi-layer pipe according to the present invention has the above-mentioned configuration, it is possible to improve impact resistance and prevent a decrease in mechanical strength such as tensile strength and flattening strength, even though the outer diameter of the fire-resistant multi-layer pipe is relatively large. In addition, since the fire-resistant multi-layer pipe according to the present invention has a fire-resistant layer, the heat-expandable graphite causes the fire-resistant multi-layer pipe (particularly the fire-resistant layer) to expand well in the event of a fire, and the pressure generated between the wall surface of the compartment penetration part and the fire-resistant multi-layer pipe blocks the entire compartment penetration part, thereby preventing the spread of fire.
[0023] The multi-layer fire-resistant pipe includes a fire-resistant layer and at least one of an inner layer disposed inside the fire-resistant layer and an outer layer disposed outside the fire-resistant layer. The multi-layer fire-resistant pipe may include the fire-resistant layer and an inner layer disposed inside the fire-resistant layer. The multi-layer fire-resistant pipe may include the fire-resistant layer and an outer layer disposed outside the fire-resistant layer. The multi-layer fire-resistant pipe may include the fire-resistant layer, an inner layer disposed inside the fire-resistant layer, and an outer layer disposed outside the fire-resistant layer. From the viewpoint of more effectively preventing a decrease in mechanical strength, it is preferable that the multi-layer fire-resistant pipe includes the fire-resistant layer, an inner layer disposed inside the fire-resistant layer, and an outer layer disposed outside the fire-resistant layer. When the multi-layer fire-resistant pipe includes the fire-resistant layer, the inner layer, and the outer layer, the fire-resistant layer is an intermediate layer.
[0024] The inner layer is a layer located inside the fire-resistant layer. The outer layer is a layer located outside the fire-resistant layer. The fire-resistant layer may be a single layer or may be a multi-layer. The fire-resistant layer may be a single layer, may be two layers, may be two or more layers, or may be three or more layers. The inner layer may be a single layer or may be a multi-layer. The inner layer may be a single layer, may be two layers, may be two or more layers, or may be three or more layers. The outer layer may be a single layer or may be a multi-layer. The outer layer may be a single layer, may be two layers, may be two or more layers, or may be three or more layers.
[0025] The inner layer does not have to be a fire-resistant layer. The inner layer is preferably formed of a composition for obtaining the inner layer (a composition other than the material for the fire-resistant layer). The outer layer does not have to be a fire-resistant layer. The outer layer is preferably formed of a composition for obtaining the outer layer (a composition other than the material for the fire-resistant layer).
[0026] Hereinafter, specific embodiments of the present invention will be described with reference to the drawings. Note that in the following drawings, the size, thickness, shape, etc. may differ from the actual size, thickness, shape, etc. for convenience of illustration.
[0027] Fig. 1 is a cross-sectional view showing a multi-layer fire-resistant pipe according to an embodiment of the present invention, taken along a radial direction of the multi-layer fire-resistant pipe.
[0028] The multi-layer fire-resistant pipe 10 shown in FIG. 1 includes an inner layer 1, a fire-resistant layer 2, and an outer layer 3. The multi-layer fire-resistant pipe 10 has a three-layer structure. The fire-resistant layer 2 is disposed on the outside of the inner layer 1. The outer layer 3 is disposed on the outside of the fire-resistant layer 2. The fire-resistant layer 2 is disposed on the outer surface of the inner layer 1 and is laminated therewith. The outer layer 3 is disposed on the outer surface of the fire-resistant layer 2 and is laminated therewith. The inner layer 1 is a single layer and is a surface layer. The outer layer 3 is a single layer and is a surface layer. The inner layer 1, the fire-resistant layer 2, and the outer layer 3 are each tubular.
[0029] The fire-resistant layer 2 contains a polyvinyl chloride resin, thermally expandable graphite, and an impact modifier.
[0030] The outer diameter of the fire-resistant multi-layer pipe is 180 mm or more. The outer diameter of the fire-resistant multi-layer pipe is preferably 200 mm or more, more preferably 205 mm or more, even more preferably 210 mm or more, and is preferably 230 mm or less, more preferably 225 mm or less, even more preferably 220 mm or less.
[0031] The inner diameter of the above-mentioned fire-resistant multi-layer pipe is preferably 175 mm or more, more preferably 185 mm or more, even more preferably 190 mm or more, and is preferably 210 mm or less, more preferably 205 mm or less, even more preferably 200 mm or less.
[0032] The thickness of the inner layer is preferably 1.0 mm or more, more preferably 1.2 mm or more, and even more preferably 1.4 mm or more, and is preferably 3.0 mm or less, more preferably 2.8 mm or less, and even more preferably 2.6 mm or less. When the thickness of the inner layer is equal to or greater than the lower limit, the impact resistance can be further improved. When the thickness of the inner layer is equal to or less than the upper limit, the inner layer can be uniformly formed during the production of the fire-resistant multi-layer pipe.
[0033] The thickness of the fire-resistant layer is preferably 6.0 mm or more, more preferably 6.2 mm or more, and even more preferably 6.4 mm or more, and is preferably 8.2 mm or less, more preferably 8.0 mm or less, and even more preferably 7.8 mm or less. When the thickness of the fire-resistant layer is equal to or greater than the lower limit, the fire resistance can be further improved. When the thickness of the fire-resistant layer is equal to or less than the upper limit, the fire-resistant layer can be formed uniformly during the production of the fire-resistant multi-layer pipe.
[0034] The thickness of the outer layer is preferably 1.0 mm or more, more preferably 1.2 mm or more, even more preferably 1.4 mm or more, and is preferably 3.0 mm or less, more preferably 2.8 mm or less, even more preferably 2.6 mm or less. When the thickness of the outer layer is equal to or more than the lower limit, the impact resistance can be further improved. When the thickness of the outer layer is equal to or less than the upper limit, the outer layer can be uniformly formed during the production of the fire-resistant multi-layer pipe.
[0035] The ratio of the thickness of the fireproof layer to the sum of the thickness of the inner layer and the thickness of the outer layer (thickness of the fireproof layer / total thickness of the inner layer and the outer layer) is preferably 1.0 or more, more preferably 1.5 or more, even more preferably 2.0 or more, and is preferably 7.0 or less, more preferably 5.0 or less, even more preferably 4.0 or less. When the ratio (thickness of the fireproof layer / total thickness of the inner layer and the outer layer) is equal to or more than the lower limit, the fire resistance can be further improved. When the ratio (thickness of the fireproof layer / total thickness of the inner layer and the outer layer) is equal to or less than the upper limit, the decrease in mechanical strength can be more effectively prevented.
[0036] (Vinyl chloride resin) The fire-resistant layer contains a vinyl chloride resin. The inner layer and the outer layer may contain a vinyl chloride resin. From the viewpoint of more effectively exerting the effects of the present invention, in the fire-resistant multi-layer pipe, it is preferable that the inner layer contains a vinyl chloride resin, it is preferable that the outer layer contains a vinyl chloride resin, and it is more preferable that the inner layer and the outer layer contain a vinyl chloride resin. When the outer layer or the inner layer contains a vinyl chloride resin, the vinyl chloride resin contained in the inner layer or the vinyl chloride resin contained in the outer layer may be the same as or different from the vinyl chloride resin contained in the fire-resistant layer.
[0037] As the vinyl chloride resin, a conventionally known vinyl chloride resin can be used. Examples of the vinyl chloride resin include (1) a homopolymer of vinyl chloride, (2) a copolymer of vinyl chloride and another monomer copolymerizable with vinyl chloride, and (3) a graft copolymer in which vinyl chloride is graft-copolymerized onto a polymer or copolymer other than vinyl chloride. The vinyl chloride resin may be used alone or in combination of two or more kinds.
[0038] Examples of other monomers copolymerizable with vinyl chloride include α-olefin compounds having 2 to 16 carbon atoms, such as ethylene, propylene, and butylene; vinyl ester compounds having 2 to 16 carbon atoms, such as vinyl acetate and vinyl propionate; vinyl ether compounds having 2 to 16 carbon atoms, such as butyl vinyl ether and cetyl vinyl ether; alkyl (meth)acrylate compounds having an alkyl group having 1 to 16 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate; aryl (meth)acrylate compounds such as phenyl (meth)acrylate; aromatic vinyl compounds such as styrene and α-methylstyrene; dicarboxylic acid compounds such as maleic anhydride; halogenated vinyl compounds such as vinylidene chloride and vinylidene fluoride; and N-substituted maleimide compounds such as N-phenylmaleimide and N-cyclohexylmaleimide. The other monomers copolymerizable with vinyl chloride may be used alone or in combination of two or more.
[0039] The copolymer may be a random copolymer, a block copolymer, or a graft copolymer.
[0040] Examples of the polymers and copolymers other than vinyl chloride that are graft-copolymerized with vinyl chloride include copolymers of α-olefin compounds and vinyl ester compounds such as ethylene-vinyl acetate copolymers; copolymers of α-olefin compounds, vinyl ester compounds, and carbon monoxide such as ethylene-vinyl acetate-carbon monoxide copolymers; copolymers of α-olefin compounds and alkyl (meth)acrylate compounds such as ethylene-methyl methacrylate copolymers and ethylene-ethyl acrylate copolymers; and copolymers of α-olefin compounds, alkyl (meth)acrylate compounds, and carbon monoxide such as ethylene-butyl acrylate-carbon monoxide copolymers; copolymers of two or more different α-olefin compounds such as ethylene-propylene copolymers; copolymers of unsaturated nitrile compounds and diene compounds such as acrylonitrile-butadiene copolymers; polyurethanes; chlorinated polyolefin compounds such as chlorinated polyethylene and chlorinated polypropylene. The polymers and copolymers other than vinyl chloride that are graft-copolymerized with vinyl chloride may be used alone or in combination of two or more.
[0041] In 100% by weight of the vinyl chloride resin contained in the fire-resistant layer, the content of structural units derived from vinyl chloride is preferably 50% by weight or more, more preferably 60% by weight or more, even more preferably 70% by weight or more, and is preferably 99% by weight or less, more preferably 98% by weight or less, even more preferably 97% by weight or less.
[0042] When the inner layer or the outer layer contains a vinyl chloride resin, the content of structural units derived from vinyl chloride in 100% by weight of the vinyl chloride resin contained in the inner layer or the outer layer is preferably 50% by weight or more, more preferably 60% by weight or more, and is preferably 99% by weight or less, more preferably 98% by weight or less.
[0043] The polymerization method for producing the vinyl chloride resin is not particularly limited, and any conventionally known polymerization method can be used. Examples of the polymerization method include bulk polymerization, solution polymerization, emulsion polymerization, and suspension polymerization.
[0044] The average degree of polymerization of the vinyl chloride resin contained in the fire-resistant layer is preferably 400 or more, more preferably 600 or more, and preferably 1600 or less, more preferably 1400 or less. When the average degree of polymerization of the vinyl chloride resin contained in the fire-resistant layer is equal to or more than the lower limit, the physical properties of the multi-layer fire-resistant pipe can be prevented from deteriorating. When the average degree of polymerization of the vinyl chloride resin contained in the fire-resistant layer is equal to or less than the upper limit, the melt viscosity of the material of the fire-resistant layer can be prevented from becoming too high during molding of the multi-layer fire-resistant pipe, and the processability can be further improved.
[0045] The average degree of polymerization of the vinyl chloride resin contained in the inner layer and the outer layer is preferably 400 or more, more preferably 600 or more, and preferably 1600 or less, more preferably 1400 or less. When the average degree of polymerization of the vinyl chloride resin contained in the inner layer and the outer layer is equal to or more than the lower limit, the physical properties of the fire-resistant multi-layer pipe can be prevented from deteriorating. When the average degree of polymerization of the vinyl chloride resin contained in the inner layer and the outer layer is equal to or less than the upper limit, the melt viscosity of the material of the inner layer and the outer layer can be prevented from becoming too high during molding of the fire-resistant multi-layer pipe, and the processability can be further improved.
[0046] The average degree of polymerization of the vinyl chloride resin can be measured as follows. The vinyl chloride resin is dissolved in tetrahydrofuran (THF), and insoluble components are removed by filtration. The THF in the filtrate is dried and removed to obtain a measurement sample. The average degree of polymerization of the measurement sample measured in accordance with JIS K6721 "Testing Method for Vinyl Chloride Resins" is regarded as the average degree of polymerization of the vinyl chloride resin.
[0047] The vinyl chloride resin may be a chlorinated vinyl chloride resin.
[0048] In 100% by weight of the fire-resistant layer, the content of the vinyl chloride resin is preferably 80% by weight or more, more preferably 85% by weight or more, and preferably 99% by weight or less, more preferably 95% by weight or less. When the content of the vinyl chloride resin is equal to or more than the lower limit and equal to or less than the upper limit, the effects of the present invention can be more effectively exhibited.
[0049] When the inner layer contains a vinyl chloride resin, the content of the vinyl chloride resin in 100% by weight of the inner layer is preferably 80% by weight or more, more preferably 85% by weight or more, and preferably 99% by weight or less, more preferably 98% by weight or less. When the content of the vinyl chloride resin is equal to or more than the lower limit and equal to or less than the upper limit, the effects of the present invention can be more effectively exhibited.
[0050] When the outer layer contains a vinyl chloride resin, the content of the vinyl chloride resin in 100% by weight of the outer layer is preferably 80% by weight or more, more preferably 85% by weight or more, and preferably 99% by weight or less, more preferably 98% by weight or less. When the content of the vinyl chloride resin is equal to or more than the lower limit and equal to or less than the upper limit, the effects of the present invention can be more effectively exhibited.
[0051] (Thermal Expandable Graphite) The fire-resistant layer contains thermally expandable graphite. The inner layer and the outer layer may contain thermally expandable graphite. As the thermally expandable graphite, a conventionally known thermally expandable graphite may be used. Only one type of the thermally expandable graphite may be used, or two or more types may be used in combination.
[0052] The thermally expandable graphite can be obtained by reacting graphite powder such as natural scaly graphite, pyrolytic graphite, and kish graphite with an inorganic acid and a strong oxidizing agent to generate a compound between the graphite layers. The thermally expandable graphite is a crystalline compound in which the layered structure of graphite is maintained. Examples of the inorganic acid include concentrated sulfuric acid, nitric acid, and selenic acid. Examples of the strong oxidizing agent include concentrated nitric acid, perchloric acid, perchlorates, permanganates, dichromates, and hydrogen peroxide. The thermally expandable graphite is preferably a crystalline compound having a layered structure of graphite obtained by performing an acid treatment to insert an inorganic acid between the graphite layers of graphite, and then adjusting the pH to 1.5 to 4.0. If the pH is less than 1.5, corrosion of the molding device is more likely to occur than when the pH is 1.5 or more. If the pH is more than 4.0, the carbonization promotion effect of the vinyl chloride resin is weakened and the fire resistance may be reduced compared to when the pH is 4.0 or less.
[0053] From the viewpoint of further improving fire resistance, the above-mentioned thermally expandable graphite is preferably thermally expandable graphite having a 1.3-fold expansion temperature (the temperature at which the volume expands to 1.3 times that before expansion) of 180°C or higher and 240°C or lower.
[0054] The average particle size of the thermally expandable graphite is preferably 100 μm or more, more preferably 120 μm or more, and is preferably 400 μm or less, more preferably 350 μm or less. When the average particle size of the thermally expandable graphite is equal to or more than the lower limit, the expansion coefficient can be further increased, and the fire resistance can be further increased. When the average particle size of the thermally expandable graphite is equal to or less than the upper limit, the decrease in mechanical strength can be more effectively prevented.
[0055] The average particle size of the thermally expandable graphite can be measured by a laser diffraction method or by analyzing SEM images. The average particle size of the thermally expandable graphite is preferably a number average particle size.
[0056] The content of the thermally expandable graphite in the fire-resistant layer is preferably 4.0% by weight or more, more preferably 6.0% by weight or more, and preferably 11.0% by weight or less, more preferably 9.0% by weight or less, based on 100% by weight of the fire-resistant layer. When the content of the thermally expandable graphite in the fire-resistant layer is equal to or more than the lower limit, the thermal expansion performance during combustion can be further improved, and the fire resistance can be further improved. When the content of the thermally expandable graphite in the fire-resistant layer is equal to or less than the upper limit, the decrease in mechanical strength can be more effectively prevented.
[0057] The content of the thermally expandable graphite contained in the fire-resistant layer is preferably 1.0 parts by weight or more, more preferably 5.0 parts by weight or more, even more preferably 7.0 parts by weight or more, and preferably 15.0 parts by weight or less, more preferably 12.0 parts by weight or less, and even more preferably 10.0 parts by weight or less, relative to 100 parts by weight of the vinyl chloride resin contained in the fire-resistant layer. When the content of the thermally expandable graphite contained in the fire-resistant layer is equal to or more than the lower limit, the thermal expansion performance during combustion can be further improved, and the fire resistance can be further improved. When the content of the thermally expandable graphite contained in the fire-resistant layer is equal to or less than the upper limit, the excessive expansion of the fire-resistant layer can be suppressed, and the fire resistance can be further improved.
[0058] (Impact Modifier) The fire-resistant layer contains an impact modifier. The inner layer and the outer layer may contain an impact modifier. From the viewpoint of further improving impact resistance, it is preferable that the inner layer contains an impact modifier, it is preferable that the outer layer contains an impact modifier, and it is more preferable that the inner layer and the outer layer contain an impact modifier. When the outer layer or the inner layer contains an impact modifier, the impact modifier contained in the inner layer or the impact modifier contained in the outer layer and the impact modifier contained in the fire-resistant layer may be the same or different.
[0059] Examples of the impact modifier include polybutadiene, polyisoprene, polychloroprene, chlorinated polyethylene, fluororubber, styrene-butadiene copolymer rubber, methyl methacrylate-butadiene-styrene copolymer, methyl methacrylate-butadiene-styrene graft copolymer, acrylonitrile-styrene-butadiene copolymer rubber, acrylonitrile-styrene-butadiene graft copolymer, styrene-butadiene-styrene block copolymer rubber, styrene-isoprene-styrene copolymer rubber, styrene-ethylene-butylene-styrene copolymer rubber, ethylene-propylene copolymer rubber, ethylene-propylene-diene copolymer rubber (EPDM), acrylic rubber, silicone / acrylic composite rubber graft copolymer, and silicone rubber. The acrylic rubber may be a silicone-containing acrylic rubber. The impact modifier may be used alone or in combination of two or more.
[0060] From the viewpoint of more effectively preventing a decrease in mechanical strength and enhancing chemical resistance, it is preferable that the impact modifier contains chlorinated polyethylene.
[0061] The content of the impact modifier contained in the fire-resistant layer is preferably 0.5% by weight or more, more preferably 1.0% by weight or more, and preferably 3.5% by weight or less, more preferably 3.0% by weight or less, based on 100% by weight of the fire-resistant layer. When the content of the impact modifier contained in the fire-resistant layer is equal to or more than the lower limit, the impact resistance can be further improved. When the content of the impact modifier contained in the fire-resistant layer is equal to or less than the upper limit, the decrease in mechanical strength can be more effectively prevented.
[0062] The content of the chlorinated polyethylene in the fire-resistant layer is preferably 0.5% by weight or more, more preferably 1.0% by weight or more, and preferably 3.5% by weight or less, more preferably 3.0% by weight or less, based on 100% by weight of the fire-resistant layer. When the content of the chlorinated polyethylene in the fire-resistant layer is equal to or more than the lower limit, the impact resistance can be further improved. When the content of the chlorinated polyethylene in the fire-resistant layer is equal to or less than the upper limit, the decrease in mechanical strength can be more effectively prevented.
[0063] The content of the impact modifier contained in the fire-resistant layer is 0.5 parts by weight or more and 3.5 parts by weight or less, based on 100 parts by weight of the vinyl chloride resin contained in the fire-resistant layer. The content of the impact modifier contained in the fire-resistant layer is preferably 0.7 parts by weight or more, more preferably 1.0 parts by weight or more, and preferably 3.3 parts by weight or less, more preferably 3.0 parts by weight or less, based on 100 parts by weight of the vinyl chloride resin contained in the fire-resistant layer. When the content of the impact modifier contained in the fire-resistant layer is equal to or more than the lower limit, the impact resistance can be further improved. When the content of the impact modifier contained in the fire-resistant layer is equal to or less than the upper limit, the decrease in mechanical strength can be more effectively prevented.
[0064] (Inner layer, fireproof layer and other details of outer layer) The inner layer, the fire-resistant layer, and the outer layer may each contain various additives as necessary. Examples of the additives include stabilizers, stabilization aids, lubricants, processing aids, heat resistance improvers, antioxidants, ultraviolet absorbers, antistatic agents, light stabilizers, inorganic fillers, organic fillers, pigments, flame retardants, and plasticizers. The additives may be used alone or in combination of two or more.
[0065] Examples of the stabilizer include a heat stabilizer and a heat stabilization assistant. Examples of the heat stabilizer include an organic tin stabilizer, a lead stabilizer, a calcium-zinc stabilizer, a barium-zinc stabilizer, and a barium-cadmium stabilizer. Examples of the organic tin stabilizer include dibutyltin mercapto, dioctyltin mercapto, dimethyltin mercapto, dibutyltin mercapto, dibutyltin maleate, dibutyltin maleate polymer, dioctyltin maleate, dioctyltin maleate polymer, dibutyltin laurate, and dibutyltin laurate polymer. The heat stabilizer may be used alone or in combination of two or more.
[0066] Examples of the heat stabilization assistant include epoxidized soybean oil, phosphoric acid ester, polyol, hydrotalcite, zeolite, etc. The heat stabilization assistant may be used alone or in combination of two or more kinds.
[0067] The lubricant includes an internal lubricant and an external lubricant. The internal lubricant is used to reduce the flow viscosity of the molten resin during molding and to prevent frictional heat generation. The internal lubricant includes butyl stearate, lauryl alcohol, stearyl alcohol, epoxy soybean oil, glycerin monostearate, stearic acid, and bisamide. The external lubricant is used to increase the sliding effect between the molten resin and the metal surface during molding. The external lubricant includes paraffin wax, polyolefin wax, ester wax, and montanic acid wax. The lubricant may be used alone or in combination of two or more.
[0068] Examples of the processing aid include acrylic processing aids. Examples of the acrylic processing aid include homopolymers or copolymers of alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, and butyl methacrylate; copolymers of alkyl methacrylates and alkyl acrylates such as methyl acrylate, ethyl acrylate, and butyl acrylate; copolymers of alkyl methacrylates and aromatic vinyl compounds such as styrene, α-methylstyrene, and vinyltoluene; copolymers of alkyl methacrylates and vinyl cyan compounds such as acrylonitrile and methacrylonitrile. Examples of the acrylic processing aid include alkyl acrylate-alkyl methacrylate copolymers having a weight average molecular weight of 100,000 to 2,000,000. Examples of the alkyl acrylate-alkyl methacrylate copolymers having a weight average molecular weight of 100,000 to 2,000,000 include n-butyl acrylate-methyl methacrylate copolymers and 2-ethylhexyl acrylate-methyl methacrylate-butyl methacrylate copolymers. The processing aids may be used alone or in combination of two or more.
[0069] Examples of the heat resistance improver include α-methylstyrene-based resins, N-phenylmaleimide-based resins, etc. The heat resistance improver may be used alone or in combination of two or more kinds.
[0070] Examples of the antioxidant include phenol-based antioxidants such as 4,4'-butylidenebis-(6-t-butyl-3-methylphenol); phosphite-based antioxidants such as tris(mixed mono- and di-nonylphenyl)phosphite; and thioether-based antioxidants such as distearyl thiodipropionate. The antioxidant is preferably a phenol-based antioxidant, more preferably 4,4'-butylidenebis-(6-t-butyl-3-methylphenol), because of its low decomposition inhibition function at high temperatures. The antioxidant may be used alone or in combination of two or more kinds.
[0071] Examples of the ultraviolet absorbent include salicylic acid ester ultraviolet absorbents, benzophenone ultraviolet absorbents, benzotriazole ultraviolet absorbents, and cyanoacrylate ultraviolet absorbents. The ultraviolet absorbents may be used alone or in combination of two or more.
[0072] As the antistatic agent, a conventionally known antistatic agent can be used. Examples of the antistatic agent include anionic surfactants, cationic surfactants, nonionic surfactants, and amphoteric surfactants. Examples of the anionic surfactant include fatty acid salts, higher alcohol sulfate salts, liquid fatty oil sulfate salts, fatty amines, sulfate salts of amides, sulfonic acid salts of dibasic fatty acid esters, fatty acid amide sulfonates, alkylaryl sulfonates, formalin condensed naphthalene sulfonates, and mixtures thereof. Examples of the cationic surfactant include fatty amine salts, quaternary ammonium salts, alkylpyridinium salts, and mixtures thereof. Examples of the nonionic surfactant include polyoxyethylene alkyl ethers, polyoxyethylene alkylphenol esters, polyoxyethylene alkyl esters, sorbitan alkyl esters, polyoxyethylene sorbitan alkyl esters, and mixtures thereof. The antistatic agent may be a mixture of a nonionic surfactant and an anionic surfactant or a cationic surfactant. Examples of the amphoteric surfactant include amphoteric surfactants of imidazoline type, higher alkylamino type (betaine type), sulfate ester, phosphate ester type, sulfonic acid type, etc. The antistatic agent may be used alone or in combination of two or more types.
[0073] The light stabilizer may be a hindered amine light stabilizer, etc. The light stabilizer may be used alone or in combination of two or more kinds.
[0074] Examples of the inorganic filler include carbonates such as talc, heavy calcium carbonate, precipitated calcium carbonate, and colloidal calcium carbonate, aluminum hydroxide, magnesium hydroxide, titanium oxide, clay, mica, wollastonite, zeolite, silica (SiO2), calcium oxide (CaO), aluminum oxide (Al2O3), zinc oxide, magnesium oxide, carbon black, graphite, glass beads, glass fibers, carbon fibers, and metal fibers. Only one type of the inorganic filler may be used, or two or more types may be used in combination.
[0075] The organic filler may be polyamide, etc. The organic filler may be used alone or in combination of two or more kinds.
[0076] Examples of the pigment include organic pigments and inorganic pigments. Examples of the organic pigment include azo-based organic pigments, phthalocyanine-based organic pigments, threne-based organic pigments, and dye lake-based organic pigments. Examples of the inorganic pigment include oxide-based inorganic pigments, molybdenum chromate-based inorganic pigments, sulfide-selenide-based inorganic pigments, and ferrocyanide-based inorganic pigments. Only one type of the pigment may be used, or two or more types may be used in combination.
[0077] Examples of the flame retardant include metal hydroxides, bromine compounds, triazine ring-containing compounds, zinc compounds, phosphorus compounds, halogen flame retardants, silicone flame retardants, intumescent flame retardants, antimony oxide, etc. The flame retardants may be used alone or in combination of two or more.
[0078] The plasticizer may be added for the purpose of improving the processability during molding. Since the addition of a plasticizer may reduce the heat resistance of the molded body, it is preferable to add a small amount of plasticizer. Examples of the plasticizer include phthalate ester plasticizers and non-phthalate plasticizers. Examples of the phthalate ester plasticizer include dioctyl phthalate (DOP). Examples of the non-phthalate plasticizer include trimellitic acid compounds, phosphoric acid compounds, adipic acid compounds, citric acid compounds, ether compounds, polyester compounds, soybean oil compounds, cyclohexane dicarboxylate compounds, and terephthalic acid compounds. The plasticizer may be used alone or in combination of two or more.
[0079] (Manufacturing method of fire-resistant multi-layer pipe) Fig. 2 is a plan view showing a manufacturing apparatus used to manufacture a multi-layer fire-resistant pipe according to one embodiment of the present invention. Fig. 3 is a front view showing a manufacturing apparatus used to manufacture a multi-layer fire-resistant pipe according to one embodiment of the present invention. Figs. 2 and 3 are views showing a manufacturing apparatus for manufacturing a multi-layer fire-resistant pipe 10.
[0080] The manufacturing apparatus 20 includes an inner / outer layer extruder 11, a fireproof layer extruder 12, a die 13, a cooling water tank 15, a take-up machine 16, and a cutting machine 17. The die 13 is connected to the inner / outer layer extruder 11 and the fireproof layer extruder 12. The cooling water tank 15 is connected to the die 13. The take-up machine 16 is connected to the cooling water tank 15. The cutter 17 is connected to the take-up machine 16.
[0081] The materials for the inner layer and the outer layer are fed from a hopper, melted and kneaded in the inner and outer layer extruder 11 , and extruded into a die 13 .
[0082] The material for the fire-resistant layer is fed from a hopper, melted and kneaded in the fire-resistant layer extruder 12, and extruded into a die 13.
[0083] From the outlet of the die 13, an uncured fire-resistant multi-layer pipe having a three-layer structure is extruded.
[0084] A tube 14 for forming the outer surface of a pipe is attached to the cooling water tank 15 in order to form the uncured multi-layer fire-resistant pipe to a predetermined size, and the outer surface of the uncured multi-layer fire-resistant pipe is cooled while being in contact with the tube 14 for forming the outer surface of the pipe.
[0085] FIG. 4 is an enlarged cross-sectional view showing a mold portion and a tube portion for forming an outer surface of a pipe in a manufacturing apparatus.
[0086] 4, the inner layer material 21 and the outer layer material 23 melt-kneaded by the inner and outer layer extruder 11, and the fire-resistant layer material 22 melt-kneaded by the fire-resistant layer extruder 12 are injected into a mold 13 to form an uncured multi-layer fire-resistant pipe 10X. The uncured multi-layer fire-resistant pipe 10X includes an uncured inner layer 31, an uncured outer layer 33, and an uncured fire-resistant layer 32.
[0087] The uncured multi-layer fire-resistant pipe 10X is inserted into a tube for forming an outer surface of the pipe 14. The uncured multi-layer fire-resistant pipe 10X is cooled in a cooling water tank 15 while being molded into a predetermined size.
[0088] 2 and 3, a take-off machine 16 takes up the fire-resistant multi-layer pipe 10 cooled in the cooling water tank 15, and a cutter 17 cuts the fire-resistant multi-layer pipe 10 sent from the take-off machine 16 to a predetermined length. In this way, a fire-resistant multi-layer pipe 10 having a predetermined length is obtained.
[0089] The heating temperature in the mold 13 is preferably 140° C. or more, more preferably 160° C. or more, and preferably 200° C. or less, more preferably 190° C. or less. The heating time in the mold 13 is preferably 10 minutes or more, preferably 30 minutes or less, more preferably 20 minutes or less.
[0090] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0091] The following materials were prepared:
[0092] Material of fireproof layer: Polyvinyl chloride resin (Tokuyama Sekisui Kogyo Co., Ltd. "TS1000R") Thermally expandable graphite (Air Water "CA-60N") Impact modifier (chlorinated polyethylene, Resonac's "Elaslen 351A") Lead-based stabilizer (SAN ACE "SAK-NS-GBN")
[0093] Inner and outer layer materials: Polyvinyl chloride resin (Tokuyama Sekisui Kogyo Co., Ltd. "TS1000R") Lead-based stabilizer (SAN ACE "SAK-NS-GBN")
[0094] Example 1 100 parts by weight of vinyl chloride resin, 9 parts by weight of thermally expandable graphite, 1 part by weight of impact modifier, and 2 parts by weight of lead-based stabilizer were mixed and stirred in a 200-liter Super Mixer (manufactured by Kawata Co., Ltd.) to obtain a material for the fire-resistant layer. 100 parts by weight of vinyl chloride resin and 1 part by weight of the lead-based stabilizer were mixed and stirred in a 200-liter Super Mixer (manufactured by Kawata Co., Ltd.) to obtain materials for the inner layer and outer layer.
[0095] Fabrication of fire-resistant multi-layer pipe: The obtained material for the fireproof layer, the material for the inner layer, and the material for the outer layer were co-extruded by an extruder to produce a fireproof multi-layer pipe including a fireproof layer, an inner layer disposed inside the fireproof layer, and an outer layer disposed outside the fireproof layer. The resin temperature during molding of the fireproof multi-layer pipe was 190°C. The size of the fireproof multi-layer pipe was 4000 mm in length, 216 mm in outer diameter, 11.0 mm in thickness, and 200 A in nominal diameter. The thickness of the fireproof layer of the fireproof multi-layer pipe was 7.1 mm, the thickness of the inner layer was 2.4 mm, and the thickness of the outer layer was 1.5 mm.
[0096] (Example 2 and Comparative Example 1) A multi-layer fire-resistant pipe was obtained in the same manner as in Example 1, except that the blending amounts of the materials contained in the fire-resistant layer were changed as shown in Table 1.
[0097] (evaluation) (1) Impact resistance From the obtained fire-resistant multi-layer pipe, 20 cylindrical test pieces with a length of 15 cm were cut out at random positions, and the obtained test pieces were left to stand at 0°C ± 3°C for 60 minutes to condition. The obtained test pieces were subjected to an impact resistance test in accordance with "7.5 Puncture Impact Test Procedure" in JIS K7211-1:2006. Specifically, the test pieces were placed on a support stand, and a weight (9 kg) with a flat bottom was dropped from above. If the test piece was broken, it was dropped from a height of 10 cm below, and if it was not broken, it was dropped again from a height of 10 cm above. This test was repeated 20 times, and the 50% breaking height was measured. The impact resistance of the fire-resistant multi-layer pipe was judged according to the following criteria.
[0098] [Impact resistance evaluation criteria] ○○: 50% destruction height is 300cm or more ○: 50% destruction height is 200cm or more and less than 300cm ×: 50% destruction height is less than 200cm
[0099] (2) Mechanical strength (2-1) Tensile strength A dumbbell test piece was cut out at an arbitrary position from the obtained fire-resistant multi-layer pipe, and the obtained dumbbell test piece was left to stand at 23°C ± 2°C for 60 minutes to condition it. A tensile test was performed on the obtained dumbbell test piece at 23°C and a tensile speed of 5mm ± 0.5mm / min in accordance with JIS K6815-1:2002 and JIS K6815-2:2002. The tensile strength of the fire-resistant multi-layer pipe was judged according to the following criteria.
[0100] [Tensile strength criteria] ○○: Tensile strength exceeds 45.0MPa ○: Tensile strength is more than 43.0 MPa and less than or equal to 45.0 MPa ×: Tensile strength is 43.0 MPa or less
[0101] (2-2) Flattening strength Two cylindrical test pieces with a length of 5 cm were cut out from the obtained fire-resistant multi-layer pipe at arbitrary positions, and the obtained test pieces were left to stand at 23°C ± 2°C for 60 minutes to condition them. The obtained test pieces were subjected to a flattening test in accordance with "9.1.4 Flattening Test" in JIS K6741:2016. Specifically, the test pieces were sandwiched between two flat plates of a constant crosshead moving speed material testing machine, and compressed in a direction perpendicular to the pipe axis at a speed of 10 mm ± 2 mm / min until the outer diameter of the pipe was reduced to half, and the flattening strength was measured.
[0102] [Criteria for flattening strength] ○: Flattening strength is 50% or more ×: Flattening strength is less than 50%
[0103] The composition and results of the fire-resistant multi-layer pipe are shown in Table 1.
[0104] [Table 1] [Explanation of symbols]
[0105] 1…Inner layer 2…Fireproof layer 3…Outer layer 10…Fireproof multilayer pipe 10X: Uncured fire-resistant multi-layer pipe 11…Inner and outer layer extruder 12…Fireproof layer extrusion machine 13...Mold 14...Tube for forming outer surface 15…Cooling water tank 16...Removal machine 17…cutting machine 20…Manufacturing equipment 21…Inner layer material 22...Fireproof layer material 23…Outer layer material 31…Uncured inner layer 32...Uncured fireproof layer 33…Uncured outer layer
Claims
1. A fire-resistant multi-layer pipe comprising a fire-resistant layer, and at least one of an inner layer disposed inside the fire-resistant layer and an outer layer disposed outside the fire-resistant layer, The outer diameter of the fire-resistant multi-layer pipe is 180 mm or more, The fire-resistant layer contains a polyvinyl chloride resin, thermally expandable graphite, and an impact modifier, A fire-resistant multi-layer pipe, wherein the content of the impact modifier contained in the fire-resistant layer is 0.5 parts by weight or more and 3.5 parts by weight or less per 100 parts by weight of the vinyl chloride resin contained in the fire-resistant layer.
2. 10. The fire resistant multi-layer pipe of claim 1, wherein the impact modifier comprises chlorinated polyethylene.
3. 3. The fire-resistant multi-layer pipe according to claim 1, wherein the content of the impact modifier contained in the fire-resistant layer is 1.0 part by weight or more and 3.0 parts by weight or less relative to 100 parts by weight of the vinyl chloride-based resin contained in the fire-resistant layer.
4. 3. The fire-resistant multi-layer pipe according to claim 1, wherein the content of the thermally expandable graphite contained in the fire-resistant layer is 1.0 part by weight or more and 15.0 parts by weight or less relative to 100 parts by weight of the vinyl chloride-based resin contained in the fire-resistant layer.
5. 3. The fire-resistant multi-layer pipe according to claim 1, comprising: the fire-resistant layer; an inner layer disposed inside the fire-resistant layer; and an outer layer disposed outside the fire-resistant layer.
Citation Information
Patent Citations
Multilayered fireproof pipe material
JP2008180367A
Three layer pipe of vinyl chloride resin
JP2010274577A
Piping material, piping structure, and manufacturing method for piping material
JP2021167659A
Pipe having resistance to both fire and cold
US20150323105A1
Piping materials for building, and its molding method
JP2008180068A