Polyurethane resin composition and coating composition
A polyurethane resin composition with a specific formulation of polycarbonate polyol and hydroxyl group-containing acrylic resin addresses the issue of weather resistance, achieving high gloss retention and low color difference in coating films.
Patent Information
- Application Number
- JP2023057891
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
The existing polyurethane resin compositions, as described in Patent Document 1, lack well-balanced weather resistance, leading to issues with gloss retention and color difference after weathering tests.
A polyurethane resin composition is formulated using a polycarbonate polyol with an average number of hydroxyl functional groups exceeding 2, combined with a hydroxyl group-containing acrylic resin and a polyisocyanate, where the polycarbonate polyol is composed of a transesterification product of polycarbonate and polyester polyols, with specific ratios and concentrations to enhance gloss retention and reduce color difference.
The composition results in a coating film with high gloss retention and low color difference after weathering tests, demonstrating improved weather resistance and appearance.
Smart Images

Figure 2024145507000001 
Figure 2024145507000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a polyurethane resin composition and a coating composition. [Background technology]
[0002] Acrylic resin-containing polycarbonate-based polyurethane resin compositions are advantageous in terms of hydrolysis resistance, heat resistance, abrasion resistance, chemical resistance, and the like, and are therefore used in a variety of exterior and interior applications.
[0003] Here, Patent Document 1 discloses a polyurethane resin obtained by reacting a hydroxyl group-containing acrylic resin (a), a polymer polyol having a carbonate skeleton (b), and a curing agent (c). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-59072 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the polyurethane resin disclosed in Patent Document 1 does not provide well-balanced weather resistance, and there is a demand for improvement in the degree of yellowing and gloss retention after weather resistance testing.
[0006] Therefore, one aspect of the present disclosure is directed to providing a polyurethane resin composition and a coating composition that contribute to the production of a coating film having a high gloss retention rate and a low color difference after a weathering test. Another aspect of the present disclosure is directed to providing a coating film having a high gloss retention rate and a low color difference after a weathering test. [Means for solving the problem]
[0007] Each aspect of the present disclosure includes the following embodiments. (1) A polyol (A) containing a polycarbonate polyol (B); A hydroxyl-containing acrylic resin (C); and a polyisocyanate (D), The polyurethane resin composition, wherein the polycarbonate polyol (B) has an ester bond and has an average number of hydroxyl functional groups exceeding 2. (2) The polyurethane resin composition according to (1), wherein the content of the polycarbonate polyol (B) is 5 to 90 mass % based on the total content of the polyol (A) and the solid content of the hydroxyl group-containing acrylic resin (C). (3) The polycarbonate polyol (B) is or comprising an ester exchange reaction product of a polycarbonate polyol (b-1) and a polyester polyol (b-2) having an average hydroxyl functional group number of 3 or more; The polyurethane resin composition according to (1) or (2), comprising an ester exchange reaction product of a polycarbonate polyol (b-1), a polyester polyol (b-2) having an average hydroxyl group functionality of 3 or more, and a polyester polyol (b-3) having an average hydroxyl group functionality of 2 or more and less than 3. (4) The polycarbonate polyol (B) has a deemed average hydroxyl functional number of 2.1 to 3.5, The hydroxyl value of the polycarbonate polyol (B) is 40 to 500 mgKOH / g, The number average molecular weight of the polycarbonate polyol (B) is 400 to 4,000 g / mol; 4. The polyurethane resin composition according to claim 3, wherein a mass ratio of the polycarbonate polyol (b-1) to the polyester polyol (b-2) ([mass of (b-1)] / [mass of (b-2)]) is 90 / 10 to 10 / 90, or a mass ratio of the polycarbonate polyol (b-1) to the sum of the polyester polyol (b-2) and the polyester polyol (b-3) ([mass of (b-1)] / ([mass of (b-2)]+[mass of (b-3)])) is 95 / 5 to 5 / 95. (5) The polyurethane resin composition according to any one of (1) to (4), wherein the polycarbonate polyol (B) has an ester group concentration of 10 to 90 mass %. (6) The polyurethane resin composition according to any one of (1) to (5), wherein the polycarbonate polyol (B) is liquid at room temperature. (7) A coating composition comprising the polyurethane resin composition according to any one of (1) to (6). (8) A coating film comprising a cured product of the coating composition according to (7).
[0008] According to one aspect of the present disclosure, it is possible to provide a polyurethane resin composition and a coating composition that contribute to the production of a coating film having a high gloss retention rate and a low color difference after a weathering test. Also, according to another aspect of the present disclosure, it is possible to provide a coating film having a high gloss retention rate and a low color difference after a weathering test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Exemplary embodiments for carrying out each aspect of the present disclosure will be described in further detail below, although the present disclosure is not limited to the following embodiments. In this specification, a numerical range indicated using "~" indicates a range including the numerical values before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in this specification, the upper limit or lower limit of the numerical range may be replaced with a value shown in the examples. Furthermore, the upper limit and lower limit values described individually can be combined in any combination.
[0010] The polyurethane resin composition according to one embodiment of the present disclosure comprises: A polyol (A) including a polycarbonate polyol (B); A hydroxyl-containing acrylic resin (C); Polyisocyanate (D) and the reaction product of The polycarbonate polyol (B) has an ester bond and an average number of hydroxyl functional groups exceeding two.
[0011] The components (A), (B), (C), and (D) of the polyurethane resin composition, as well as other components that may be contained therein, will be described below.
[0012] <Polyol (A)> The polyol (A) contains a polycarbonate polyol (B) having an ester bond and an average number of hydroxyl functional groups exceeding 2. Examples of polyols other than the polycarbonate polyol (B) contained in the polyol (A) include polyester polyols, polyether polyols, polycarbonate polyols (excluding the polycarbonate polyol (B)), polyolefin polyols, and polyols (A-1) consisting of any combination of two or more of these.
[0013] Preferred polyester polyols include polyester polyols (polyester diols) obtained from a diol and a dicarboxylic acid and / or anhydride thereof, polyester polyols (polyester diols) obtained by ring-opening addition polymerization of cyclic ester compounds such as lactones using a diol as an initiator, polyester polyols obtained from a trifunctional or higher polyhydric alcohol, a diol, and a dicarboxylic acid and / or anhydride thereof, and polyester polyols obtained by ring-opening addition polymerization of cyclic ester compounds such as lactones using a trifunctional or higher polyhydric alcohol and, if necessary, a diol as an initiator, and combinations of any two or more of these.
[0014] Examples of diols include low molecular weight polyols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 3-methyl-1,5-pentanediol, 3,3-dimethylolheptane, diethylene glycol, dipropylene glycol, neopentyl glycol, cyclohexane-1,4-diol, cyclohexane-1,4-dimethanol, diol dimer acid, ethylene oxide or propylene oxide adducts of bisphenol A, bis(β-hydroxyethyl)benzene, and xylylene glycol, and combinations of any two or more of these.
[0015] Examples of trifunctional or higher polyhydric alcohols include trimethylolpropane, trimethylolethane, glycerin, pentaerythritol, dipentaerythritol, sorbitol, and combinations of any two of these. Among these, trimethylolpropane, trimethylolethane, and pentaerythritol are preferred.
[0016] Examples of dicarboxylic acids and / or anhydrides thereof include phthalic acid, isophthalic acid, terephthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, cyclohexanedicarboxylic acid, maleic acid, fumaric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, sebacic acid, dodecanedioic acid, hydrogenated dimer fatty acid, tartaric acid, and the like, and anhydrides thereof, as well as combinations of any two or more thereof.
[0017] Examples of cyclic ester compounds include β-propiolactone, β-butyrolactone, γ-butyrolactone, β-valerolactone, γ-valerolactone, δ-valerolactone, α-caprolactone, β-caprolactone, γ-caprolactone, δ-caprolactone, ε-caprolactone, α-methyl-ε-caprolactone, β-methyl-ε-caprolactone, 4-methylcaprolactone, γ-caprylolactone, ε-caprylolactone, ε-palmitolactone, and the like, as well as combinations of any two or more of these. Among these, ring-opening addition polymers of ε-caprolactone using ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, 3-methyl-1,5-pentanediol, 2-methyl-1,8-octanediol, or the like as an initiator are preferred from the viewpoints of stability during polymerization and economy.
[0018] Examples of polyether polyols include polyethylene glycol, polypropylene ether polyol, polytetramethylene ether polyol, and the like, as well as combinations of any two or more of these.
[0019] Examples of the polycarbonate polyol include the following polycarbonate polyols (α), (β), and (γ), the following polycarbonate polyols (α') and (β'), and any combination of two or more of these. Note that the polycarbonate polyol contained in the polyol (A-1) is different from the polycarbonate polyol (B). (α) Polycarbonate polyol obtained from diol (a-1) and carbonate ester (a-2) (hereinafter also referred to as "polycarbonate polyol (α)") (β) A polycarbonate polyol obtained from a diol (a-1), a carbonate ester (a-2), and a cyclic ester compound (a-3) such as a lactone (hereinafter also referred to as "polycarbonate polyol (β)"). (γ) Polycarbonate polyol obtained from polycarbonate polyol (a-4) and polyester polyol (a-5) (hereinafter also referred to as "polycarbonate polyol (γ)") (α') A polycarbonate polyol which is an ester exchange reaction product between a diol (a-1), a polyhydric alcohol (a-6) having three or more functional groups, and a carbonate ester (a-2) (hereinafter also referred to as "polycarbonate polyol (α')"). (β') A polycarbonate polyol which contains a polyhydric alcohol (a-6) having three or more functional groups and a diol (a-1) used as needed, and is an ester exchange reaction product with a polycarbonate polyol (a-7) (hereinafter also referred to as "polycarbonate polyol (β')").
[0020] Examples of the diol (a-1) include the same diols as those mentioned in the description of the polyester polyol. Among them, ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, 3-methyl-1,5-pentanediol, and 2-methyl-1,8-octanediol are preferred.
[0021] Examples of the carbonate ester (a-2) include dialkyl carbonates such as dimethyl carbonate and diethyl carbonate; alkylene carbonates such as ethylene carbonate and propylene carbonate; diaryl carbonates such as diphenyl carbonate, dinaphthyl carbonate, dianthryl carbonate, diphenanthryl carbonate, diindanyl carbonate, and tetrahydronaphthyl carbonate; and the like, and combinations of any two or more of these.
[0022] Examples of the cyclic ester compound (a-3) include the same cyclic ester compounds as those mentioned in the description of the polyester polyol.
[0023] Examples of the polycarbonate polyol (a-4) include the same ones as those mentioned in the description of the polycarbonate polyol (α).
[0024] Examples of the polyester polyol (a-5) include the same polyester polyols (polyester diols) as those mentioned in the description of the polyester polyol.
[0025] Examples of the polyhydric alcohol (a-6) include the same polyhydric alcohols as those mentioned in the description of the polyester polyols. Among these, trimethylolpropane, trimethylolethane, and pentaerythritol are preferred.
[0026] The polycarbonate polyol (a-7) is a polycarbonate polyol having two or more functional groups, and may be a polycarbonate polyol (a-7-1) having two functional groups, a polycarbonate polyol (a-7-2) having more than two functional groups, or a combination of two or more selected from the polycarbonate polyol (a-7-1) and the polycarbonate polyol (a-7-2).
[0027] Examples of the polycarbonate polyol (a-7-1) include the same ones as those mentioned in the description of the polycarbonate polyol (α).
[0028] Examples of the polycarbonate polyol (a-7-2) include the same ones as those mentioned in the description of the polycarbonate polyol (α').
[0029] Examples of polyolefin polyols include hydroxyl-terminated polybutadiene and hydrogenated products thereof, hydroxyl-containing chlorinated polyolefins, and combinations of any two or more of these.
[0030] In consideration of various durability and adhesion of the coating obtained from the polyurethane resin composition, the polyol (A-1) preferably contains a polycarbonate polyol, and more preferably contains a polycarbonate diol.
[0031] From the viewpoints of handling properties and coating film appearance when used in a urethane resin, the polycarbonate polyol of the polyol (A-1) is preferably liquid at room temperature.
[0032] The number average molecular weight of the polyol (A-1) is preferably 300 to 10,000, and may be 500 to 7,000, 800 to 5,000, or 1000 to 3,000. The details of the method for measuring the number average molecular weight may be as described in the examples below.
[0033] The average hydroxyl value of the polyol (A-1) is preferably 30 to 500 mgKOH / g, more preferably 40 to 400 mgKOH / g, and even more preferably 50 to 300 mgKOH / g. When the average hydroxyl value is within the above range, a polyurethane resin having a good coating appearance, a high gloss retention at 20° after a weathering test, and a low color difference ΔE is easily obtained.
[0034] The polyol (A) may contain, as a polyol other than the polycarbonate polyol (B), in addition to the polyol (A-1) or instead of the polyol (A-1), a diol (A-2) and / or a tri- or higher functional polyhydric alcohol (A-3).
[0035] Examples of the diol (A-2) include the same diols as those mentioned in the description of the polyester polyol. Among them, ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, and 2-methyl-1,8-octanediol are preferred.
[0036] Examples of the polyhydric alcohol (A-3) include the same polyhydric alcohols as those mentioned in the description of the polyester polyols. Among them, trimethylolpropane, trimethylolethane, and pentaerythritol are preferred from an economical point of view.
[0037] The molar ratio of the polyol (A-1) to the diol (A-2) and / or polyhydric alcohol (A-3) in the polyol (A) [polyol (A-1) / (diol (A-2) and / or polyhydric alcohol (A-3)] is preferably 10 / 0 to 1 / 20, more preferably 10 / 0 to 1 / 10, and even more preferably 7 / 1 to 1 / 5. By setting it within this range, a polyurethane resin having a good appearance, a high gloss retention at 20° after a weathering test, and a low color difference ΔE is easily obtained.
[0038] <Polycarbonate polyol (B)> In one embodiment of the present disclosure, the polycarbonate polyol (B) is a polycarbonate polyol having an ester bond and an average number of hydroxyl functional groups exceeding 2. The polycarbonate polyol (B) is included in the polyol (A).
[0039] Examples of the polycarbonate polyol (B) include the following copolymer polyols (α”) and (β”), and any combination of two or more of these. (α") A copolymer polyol which is an ester exchange reaction product between a polycarbonate polyol (b-1) and a polyester polyol (b-2) having an average hydroxyl functional group number of 3 or more (hereinafter also referred to as "polycarbonate polyol (α")"). (β") A copolymer polyol which is an ester exchange reaction product of a polycarbonate polyol (b-1), a polyester polyol (b-2) having an average hydroxyl functional group number of 3 or more, and a polyester polyol (b-3) having an average hydroxyl functional group number of 2 or more and less than 3 (hereinafter also referred to as "polycarbonate polyol (β")"). Copolymer polyols not only provide excellent mechanical properties and weather resistance, but also have improved solubility in solvents and handleability due to their liquid state at room temperature.
[0040] Examples of the polycarbonate polyol (b-1) include the same ones as those mentioned in the description of the polycarbonate polyol (a-7).
[0041] Examples of the polyester polyol (b-2) include the following polyester polyols (δ) to (ε) and any combination of two or more of these. (δ) A polyester polyol obtained from a diol (b-2-1), a dicarboxylic acid and / or its anhydride (b-2-2), and a polyhydric alcohol (b-2-3) having an average hydroxyl functional group number of 3 or more (hereinafter also referred to as "polyester polyol (δ)"). (ε) A polyester polyol obtained by ring-opening addition polymerization of a cyclic ester compound (b-2-4) such as a lactone using a polyhydric alcohol (b-2-3) having an average hydroxyl functional group number of 3 or more and a difunctional alcohol (b-2-5) used as needed as an initiator (hereinafter also referred to as "polyester polyol (ε)").
[0042] Examples of the diol (b-2-1), dicarboxylic acid and / or its anhydride, and cyclic ester compound (b-2-4) include the same diol, dicarboxylic acid and / or its anhydride, and cyclic ester compound as those mentioned in the description of the polyester polyol.
[0043] Examples of the polyhydric alcohol (b-2-3) include the same trifunctional or higher polyhydric alcohols as those mentioned in the description of the polyester polyol. In addition, as long as the desired effect is achieved, a bifunctional alcohol (b-2-5) such as ethylene glycol, diethylene glycol, propylene glycol, butanediol, neopentyl glycol, hexamethylene glycol, dipropylene glycol, trimethylene glycol, etc. may be used as an initiator in combination with the polyhydric alcohol (b-2-3). In other words, the polyester polyol (ε) may be a polyester polyol having a moiety derived from the polyhydric alcohol (b-2-3) and a moiety derived from the cyclic ester compound (b-2-4), and may further include a polyester polyol having a moiety derived from the bifunctional alcohol (b-2-5) and a moiety derived from the cyclic ester compound (b-2-4).
[0044] Considering ease of synthesis and ease of handling, the number average molecular weight of the polycarbonate polyol (b-1) is preferably 400 to 5,000 g / mol, and more preferably 500 to 3,000 g / mol.
[0045] (catalyst) It is preferable to use a catalyst when preparing the polycarbonate polyol (B). Examples of the catalyst include known transesterification catalysts, such as metal alkoxides such as lithium methoxide, sodium methoxide, sodium ethoxide, potassium methoxide, and potassium ethoxide; metal enolates such as lithium acetylacetonate, aluminum acetylacetonate, and zirconium acetylacetonate; metal carbonates such as lithium carbonate, sodium carbonate, and potassium carbonate; metal hydroxides such as lithium hydroxide, sodium hydroxide, and potassium hydroxide; metal carboxylates such as lithium acetate, sodium acetate, and potassium acetate; trimethylamine, triethylamine, diisopropylethylamine, tributylamine, and ethylamine. tertiary alkylamines such as pyridine, pyrazine, and quinoline; cyclic azines such as pyridine, pyrazine, and quinoline; tertiary cyclic amines such as N-methylpyrrolidine, N-methylpiperidine, N,N'-dimethylpiperazine, N-methylmorpholine, diazabicycloundecene, 1,4-diazabicyclo[2.2.2]octane, and 1,8-diazabicyclo[5.4.0]undecene; t-butyliminotris(dimethylamino)phosphorane (P1-t-Bu), t-butyliminotri(pyrrolidino)phosphorane, t-octyliminotris(dimethylamino)phosphorane (P1-t-Oct), and 1-t-butyl-2,2,4,4,4-pentakis(dimethylamino)-2λ 5 ,4λ 5 -Catenazi(phosphazene)(P2-t-Bu), 1-ethyl-2,2,4,4,4-pentakis(dimethylamino)-2λ 5 , 4λ 5 -Catenazi(phosphazene), 1-t-butyl-4,4,4-tris(dimethylamino)-2,2-bis[tris(dimethylamino)phosphoranylideneamino]-2λ 5 ,4λ 5 -Catenazi(phosphazene)(P4-t-Bu), 1-tert-octyl-4,4,4-tris(dimethylamino)-2,2-bis[tris(dimethylamino)phosphoranylideneamino]-2λ 5 ,4λ 5-catenadi(phosphazene) (P4-t-Oct), and any combination of two or more of these. Among these, potassium hydrogen carbonate, sodium hydrogen carbonate, lithium acetate, lithium acetylacetonate, diazabicycloundecene, and P4-t-Bu are preferred in terms of high yield.
[0046] In the case of a two-component system of (b-1) and (b-2) (polycarbonate polyol (α”)) The mass ratio of the polycarbonate polyol (b-1) to the polyester polyol (b-2) having an average number of hydroxyl functional groups of 3 or more ([mass of (b-1)] / [mass of (b-2)]) is preferably 90 / 10 to 10 / 90, more preferably (b-1) / (b-2)=80 / 20 to 20 / 80, even more preferably 70 / 30 to 30 / 70, and particularly preferably 60 / 40 to 40 / 60. In the case of a three-component system of (b-1), (b-2), and (b-3) (polycarbonate polyol (β")) The mass ratio of the polycarbonate polyol (b-1) to the polyester polyol (b-2) having an average hydroxyl group functionality of 3 or more and the polyester polyol (b-3) having an average hydroxyl group functionality of 2 or more and less than 3 ([mass of (b-1)] / ([mass of (b-2)]+[mass of (b-3)])) is preferably 95 / 5 to 5 / 95, more preferably 90 / 10 to 10 / 90, still more preferably 80 / 20 to 20 / 80, even more preferably 70 / 30 to 30 / 70, and particularly preferably 60 / 40 to 40 / 60. When the mass ratio is within these ranges, a polyurethane resin having good weather resistance and coating appearance is easily obtained due to the balance between the cohesive force of the polycarbonate polyol (b-1), the urethane group concentration, and the content of the polyester polyol (b-2) or the content of the polyester polyol (b-2) and the polyester polyol (b-3).
[0047] The deemed average hydroxyl functionality of the polycarbonate polyol (B) is preferably 2.1 to 3.5, more preferably 2.2 to 3.0, even more preferably 2.3 to 2.9, and particularly preferably 2.4 to 2.8. When the deemed average hydroxyl functionality is 3.5 or less, a polyurethane resin having good coating appearance is easily obtained. When the deemed average hydroxyl functionality is 2.1 or more, a polyurethane resin having high gloss retention at 20° after weathering test and low color difference ΔE is easily obtained.
[0048] The average hydroxyl value of the polycarbonate polyol (B) is preferably 40 to 500 mgKOH / g, more preferably 50 to 300 mgKOH / g. When the average hydroxyl value is 40 mgKOH / g or more, the urethane group concentration in the polyurethane resin does not become too low, and weather resistance is further improved. When the average hydroxyl value is 500 mgKOH / g or less, the urethane group concentration does not become too high, and the coating film appearance tends to be good.
[0049] The number average molecular weight of the polycarbonate polyol (B) is preferably 400 to 4,000 g / mol, and more preferably 500 to 3000 g / mol. When the number average molecular weight is 400 g / mol or more, the urethane group concentration in the polyurethane does not become too high, and the coating film appearance tends to be good. When the number average molecular weight is 4000 g / mol or less, the urethane group concentration in the polyurethane resin does not become too low, and the weather resistance is further improved.
[0050] The ester group concentration of the polycarbonate polyol (B) is preferably 10 to 90% by mass, more preferably 15 to 80% by mass, further preferably 20 to 70% by mass, and particularly preferably 25 to 60% by mass. When the ester group concentration is 10% by mass or more, a polyurethane resin having excellent low-temperature properties and adhesion to substrates tends to be easily obtained. When the ester group concentration is 90% by mass or less, a polyurethane resin having excellent weather resistance tends to be easily obtained.
[0051] The polycarbonate polyol (B) is preferably in a liquid state at room temperature from the viewpoints of handling properties and paint appearance when used as a urethane resin composition.
[0052] (Production method of polycarbonate polyol (B)) The polycarbonate polyol (B) can be produced by transesterification of polycarbonate polyol (b-1), polyester polyol (b-2) having an average hydroxyl functionality of 3 or more, and, if necessary, polyester polyol (b-3) having an average hydroxyl functionality of 2 or more and less than 3. At this time, it is preferable to use a catalyst, and the amount of the catalyst used is 0.0001 to 1 mass%, preferably 0.001 to 0.1 mass%, of the total mass of polycarbonate polyol (b-1) and polyester polyol (b-2) having an average hydroxyl functionality of 3 or more, or, in the case of including polyester polyol (b-3), of the total mass of polycarbonate polyol (b-1), polyester polyol (b-2) having an average hydroxyl functionality of 3 or more, and polyester polyol (b-3). When the amount of catalyst is equal to or more than the lower limit, the reaction time can be further prevented from being elongated, so that the obtained polycarbonate polyol is further less likely to be colored. When the amount of the catalyst is equal to or less than the upper limit, the turbidity is further suppressed. The reaction temperature for the transesterification reaction is preferably from 70 to 250°C, and more preferably from 80 to 220°C.
[0053] <Hydroxyl-containing acrylic resin (C)> The hydroxyl-containing acrylic resin (C) used in this embodiment is a component that imparts surface hardness, water resistance, weather resistance, heat resistance, etc. The hydroxyl-containing acrylic resin of this embodiment is not particularly limited as long as it is a polymer essentially containing a structural unit derived from an acrylic monomer having a hydroxyl group, and may be a copolymer further containing a structural unit derived from a monomer such as an acrylic monomer having a carboxyl group, another acrylic monomer, an acrylic monomer having a copolymerizable ester group, or another vinyl monomer, and the type of structural unit constituting the polymer is not particularly limited.
[0054] Examples of acrylic monomers having a hydroxyl group include 1-hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, and ε-caprolactone adducts thereof, as well as any combination of two or more of these.
[0055] Examples of the acrylic monomer having a carboxyl group include unsaturated carboxylic acids such as acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, and anhydrides of these acids, and combinations of any two or more of these acids.
[0056] Examples of acrylic monomers having an ester group include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, n-amyl (meth)acrylate, isoamyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, octadecyl (meth)acrylate, cyclohexyl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, and the like, as well as combinations of any two or more of these.
[0057] Examples of other vinyl monomers include acrylamide monomers such as acrylamide, methacrylamide, N-methylolacrylamide, N,N-dimethylacrylamide, and diacetoneacrylamide; styrene, and combinations of any two or more of these. The hydroxyl group-containing acrylic resin can be obtained by appropriately selecting a monomer from the above acrylic monomers and vinyl monomers and polymerizing the monomer with a radical polymerization initiator and a chain transfer agent.
[0058] The hydroxyl value of the hydroxyl-containing acrylic resin (C) is not particularly limited, but is preferably 30 to 500 mgKOH / g, more preferably 50 to 300 mgKOH / g, and even more preferably 70 to 200 mgKOH / g. By having a hydroxyl value of 50 mgKOH / g or more, the coating film obtained from the coating composition tends to have improved coating film hardness and coating film strength, and the initial scratch resistance tends to be better. In addition, by having a hydroxyl value of 500 mgKOH / g or less, the crosslink density of the coating film obtained from the coating composition is adjusted to an appropriate range, and the weather resistance tends to be better.
[0059] The number average molecular weight of the hydroxyl-containing acrylic resin (C) is not particularly limited, but is preferably 500 to 10,000 g / mol, more preferably 1,500 to 8,000 g / mol, and even more preferably 2,000 to 6,000 g / mol. When the number average molecular weight of the hydroxyl-containing acrylic resin (C) is 500 g / mol or more, the scratch recovery of the coating film obtained from the coating composition tends to be better. In addition, when the number average molecular weight of the hydroxyl-containing acrylic resin (C) is 10,000 g / mol or less, the viscosity of the coating composition is adjusted to an appropriate range, the coating appearance is good, and the initial scratch resistance tends to be good.
[0060] The glass transition temperature of the hydroxyl-containing acrylic resin (C) is not particularly limited, but is preferably -20 to 70°C, more preferably 0°C to 60°C. When the glass transition temperature of the hydroxyl-containing acrylic resin (C) is -20°C or higher, the surface hardness of the coating film obtained from the coating composition tends to be high and the initial scratch resistance tends to be good. In addition, when the glass transition temperature of the hydroxyl-containing acrylic resin (C) is 70°C or lower, the hardness of the coating film obtained from the coating composition is adjusted to an appropriate range, and the scratch recovery tends to be better.
[0061] As the hydroxyl group-containing acrylic resin (C), for example, commercially available products can be used. Specifically, ACRYDIC A-801, ACRYDIC 54-768, ACRYDIC HU-596, ACRYDIC A-49-394-IM, ACRYDIC A-859, ACRYDIC A-858, Setalux 1152, Setalux 1184, Setalux 1767 manufactured by Nuplex Corporation, LR-7606 manufactured by Mitsubishi Rayon Co., Ltd., Superlac O-150 Clear manufactured by Nippon Paint Co., Ltd., and the like can be suitably used.
[0062] (Polycarbonate polyol (B) content) Since it is possible to form a polyurethane resin having a high gloss retention at 20° after a weather resistance test and a low color difference ΔE, the content of the polycarbonate polyol (B) may be 5.0 mass% or more, 7.0 mass% or more, 10.0 mass% or more, 15.0 mass% or more, or 20.0 mass% or more, and may be 90 mass% or less, 80 mass% or less, 70 mass% or less, 60 mass% or less, or 50 mass% or less, based on the sum of the content of the polyol (A) and the content of the solids of the hydroxyl group-containing acrylic resin (C) in the polyurethane resin composition. The content of the polycarbonate polyol (B) may be, for example, 5.0 to 90 mass% based on the total content of the polyol (A) in the polyurethane resin composition and the solid content of the hydroxyl group-containing acrylic resin (C), and is preferably 8.0 to 80 mass%, more preferably 10 to 70 mass%, further preferably 15 to 60 mass%, and particularly preferably 20 to 50 mass%. When the content of the polycarbonate polyol (B) is within the above range, a polyurethane resin having a good coating appearance, a high gloss retention at 20° after a weathering test, and a low color difference ΔE is easily obtained.
[0063] <Polyisocyanate (D)> The polyisocyanate (D) is a compound having two or more isocyanate groups (-N=C=O). The number of isocyanate groups in the polyisocyanate (D) may be, for example, 6 or less, 4 or less, or 3 or less. The number of isocyanate groups in the polyisocyanate (D) may be, for example, 2 to 3, or may be 2. The polyisocyanate (D) may be, for example, a compound having a plurality of isocyanate groups and a hydrocarbon group connecting the plurality of isocyanate groups.
[0064] The polyisocyanate (D) is not particularly limited, and may be any of various conventionally known polyisocyanates. For example, aliphatic isocyanates such as hexamethylene diisocyanate, 1,5-pentamethylene diisocyanate, 1,4-tetramethylene diisocyanate, 2-methylpentane-1,5-diisocyanate, and lysine diisocyanate; alicyclic diisocyanates such as isophorone diisocyanate, norbornane diisocyanate, hydrogenated tolylene diisocyanate, hydrogenated xylene diisocyanate, hydrogenated diphenylmethane diisocyanate, and hydrogenated tetramethylxylene diisocyanate; 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, 4,4'-diphenylether diisocyanate, and 2- Examples of the isocyanate include aromatic isocyanates such as nitrodiphenyl-4,4'-diisocyanate, 2,2'-diphenylpropane-4,4'-diisocyanate, 3,3'-dimethyldiphenylmethane-4,4'-diisocyanate, 4,4'-diphenylpropane diisocyanate, m-phenylene diisocyanate, p-phenylene diisocyanate, naphthylene-1,4-diisocyanate, naphthylene-1,5-diisocyanate, and 3,3'-dimethoxydiphenyl-4,4'-diisocyanate; aromatic aliphatic diisocyanates such as xylylene-1,4-diisocyanate and xylylene-1,3-diisocyanate; and allophanate-modified polyisocyanates obtained by reacting these organic polyisocyanates with alcohols; and combinations of any two or more of these.
[0065] From the viewpoint of improving the acid resistance, alkali resistance, alcohol resistance, oil resistance, abrasion resistance and scratch resistance of the cured coating film, the polyisocyanate (D) is preferably an aliphatic and / or alicyclic organic isocyanate compound having 2.5 or more isocyanate groups and / or blocked isocyanate groups in one molecule, and specifically, diisocyanate derivatives such as biuret, allophanate, uretdione and isocyanurate, and polyhydric alcohol adduct types are more preferred.
[0066] The ratio of the total number of moles of hydroxyl groups contained in the polyol (A) and the hydroxyl group-containing acrylic resin (C) to the total number of moles of isocyanate groups contained in the polyisocyanate (D) (hydroxyl groups / isocyanate groups) may be, for example, 0.500 or more, 0.600 or more, or 0.700 or more, and may be 1.20 or less, 1.10 or less, or 1.00 or less.
[0067] <Method of producing polyurethane resin composition> The polyurethane resin composition can be produced, for example, by a method including a step of reacting a polyol (A) containing a polycarbonate polyol (B), a hydroxyl group-containing acrylic resin (C), and a polyisocyanate (D) to obtain a polyurethane resin composition.
[0068] When mixing the polyol (A) including the polycarbonate polyol (B), the hydroxyl-containing acrylic resin (C), and the polyisocyanate (D), a catalyst can be used to shorten the curing process and improve the reaction rate. Examples of the catalyst include urethane-forming reaction catalysts such as tertiary amine catalysts such as triethylamine, tetramethylpropylenediamine, tetramethylhexamethylenediamine, and tolylenediamine, and metals such as tin-based catalysts such as stannous octoate, stannous oleate, and dibutyltin dilaurate, as well as combinations of any two or more of these.
[0069] <Inert organic solvent> In order to adjust the workability during coating, the coating composition of this embodiment may contain an inert organic solvent in an amount of 10 to 90% by mass based on the total amount of the coating composition, if necessary. The content of the inert organic solvent is more preferably 20 to 80% by mass, even more preferably 30 to 70% by mass, and even more preferably 40 to 60% by mass.
[0070] The inert organic solvent is not particularly limited, but is preferably an organic solvent that is substantially inert to polyisocyanate compounds and does not have active hydrogen. Examples of the inert organic solvent include, but are not particularly limited to, pentane, hexane, heptane, octane, decane, petroleum ether, petroleum benzine, ligroin, petroleum spirit, cyclohexane, methylcyclohexane, and other hydrocarbons, trichlorofluoroethane, tetrachlorodifluoroethane, perfluoroether, and other fluorinated oils, fluorine-based inert liquids, perfluorocyclohexane, perfluorobutyltetrahydrofuran, perfluorodecalin, perfluoro-n-butylamine, perfluoropolyether, dimethylpolysiloxane, and other solvents, either alone or in combination. In addition, methyl ethyl ketone, acetone, ethyl acetate, butyl acetate, toluene, xylene, and other solvents, and combinations of any two or more of these solvents can be mentioned.
[0071] <Other additives> To the coating composition of the present embodiment, curing accelerators (catalysts), fillers, flame retardants, dyes, organic or inorganic pigments, release agents, flow control agents, plasticizers, antioxidants, UV absorbers, light stabilizers, defoamers, leveling agents, colorants, solvents, and the like can be added depending on various applications.
[0072] The curing accelerator is not particularly limited, but examples thereof include monoamines such as triethylamine and N,N-dimethylcyclohexylamine, diamines such as tetramethylethylenediamine, other triamines, cyclic amines, alcohol amines such as dimethylethanolamine, and ether amines. The metal catalyst is not particularly limited, but examples thereof include commonly used ones such as potassium acetate, potassium 2-ethylhexanoate, calcium acetate, lead octoate, dibutyltin dilaurate, tin octoate, bismuth neodecanoate, bismuth oxycarbonate, bismuth-2-ethylhexanoate, zinc octoate, zinc neodecanoate, phosphine, and phospholine.
[0073] The filler and pigment are not particularly limited, but for example, commonly used fillers and pigments such as woven fabric, glass fiber, carbon fiber, polyamide fiber, mica, kaolin, bentonite, metal powder, azo pigments, carbon black, clay, silica, talc, gypsum, alumina white, and barium carbonate can be used.
[0074] The release agent, flow control agent, and leveling agent are not particularly limited, but examples thereof include silicone, aerosil, wax, stearates, and polysiloxanes such as BYK-331 and BYK-Silcrean-370 (manufactured by BYK Chemical Co.).
[0075] The additives used in this embodiment are preferably at least an antioxidant, a light stabilizer and a heat stabilizer.These antioxidants are not particularly limited, but include, for example, phosphoric acid, phosphorous acid, aliphatic, aromatic or alkyl group-substituted aromatic esters, hypophosphorous acid derivatives, phosphorus compounds such as phenylphosphonic acid, phenylphosphinic acid, diphenylphosphonic acid, polyphosphonates, dialkyl pentaerythritol diphosphite, dialkyl bisphenol A diphosphite, etc.; phenol derivatives, especially hindered phenol compounds, thioethers, dithioacid salts, mercaptobenzimidazoles, thiocarbanilides, thiodipropionates, etc., sulfur-containing compounds; tin compounds such as tin maleates and dibutyltin monoxide, etc., and combinations of any two or more of these.
[0076] <Painting method> The method for applying the coating composition of this embodiment is not particularly limited, but for example, the components are mixed immediately before application and then applied to the substrate by spray, roll, brush, etc. It is also possible to mix the components other than the curing agent in advance, add the components immediately before application, mix uniformly, and then apply.
[0077] <Application> The coating composition of the present embodiment has excellent weather resistance and is therefore suitable for use as a clear coating material for automobile exteriors and automobile interiors. It can also be used for surface treatment of home appliances, office automation products, leather, synthetic leather, etc.
[0078] The substrate may be stainless steel, phosphate-treated steel, galvanized steel, iron, copper, aluminum, brass, glass, acrylic resin, polycarbonate resin, polyethylene terephthalate resin, polyethylene naphthalate resin, polybutylene phthalate resin, polystyrene resin, AS resin, ABS resin, polycarbonate-ABS resin, 6-nylon resin, 6,6-nylon resin, MXD6 nylon resin, polyvinyl chloride resin, polyvinyl alcohol resin, polyurethane resin, phenol resin, melamine resin, polyacetal resin, chlorinated polyolefin resin, polyolefin resin, polyamide resin, polyether ether ketone, etc. Examples of the material include substrates molded from materials such as olefin resins, such as polyethylene resin, polyphenylene sulfide resin, NBR resin, chloroprene resin, SBR resin, SEBS resin, polyethylene, and polypropylene; organic fibers containing at least one type of main component selected from polyethylene terephthalate resin, polytrimethylene terephthalate resin, polybutylene terephthalate resin, polyethylene resin, polypropylene resin, polystyrene resin, 6-nylon resin, 6,6-nylon resin, acrylic resin, polyvinyl alcohol resin, cellulose, polylactic acid, cotton, and wool; inorganic fibers, such as glass wool; and carbon fibers.
[0079] In order to improve the adhesiveness of these substrates, the surfaces of the substrates may be previously subjected to treatments such as corona discharge treatment, frame treatment, ultraviolet irradiation treatment, and ozone treatment.
[0080] According to one aspect of the present disclosure, it is possible to provide a polyurethane resin composition and a coating composition that contribute to the preparation of a coating film having a high gloss retention rate and a low color difference after a weathering test. According to another aspect of the present disclosure, it is possible to provide a coating film having excellent weather resistance. Furthermore, the coating film according to each aspect has a good appearance. EXAMPLES
[0081] Examples of the present invention will be described below, but the present invention is not limited to these Examples. In the Examples, % and parts are by weight unless otherwise specified.
[0082] <Calculation method for each composition> (Deemed average number of hydroxyl functional groups) The deemed average hydroxyl functionality of polyol (A-1) or polycarbonate polyol (B) with an average hydroxyl functionality exceeding 2 was calculated from the number average molecular weight and hydroxyl value obtained by GPC (Gel Permeation Chromatography) measurement. Normally, the deemed average hydroxyl functionality is calculated from the true number average molecular weight and average hydroxyl value, but since it is difficult to calculate the true number average molecular weight of polyol (A-1) or polycarbonate polyol (B) with an average hydroxyl functionality exceeding 2, the number average molecular weight converted from the PPG calibration curve in GPC measurement is used to define the deemed average hydroxyl functionality. The deemed average hydroxyl functionality is defined by the following formula. Deemed average number of hydroxyl functional groups = (average hydroxyl value (mg KOH / g) of polycarbonate polyol (B) x number average molecular weight (g / mol) calculated from the PPG calibration curve obtained by GPC measurement of polycarbonate polyol (B)) / (56.11 (KOHg / mol) x 1000) When calculating the deemed average hydroxyl functionality of polyol (A-1) having an average hydroxyl functionality exceeding 2, "polycarbonate polyol (B)" is to be read as "polyol (A-1)."
[0083] [Ester group concentration] The ester group concentration of the polycarbonate polyol (B) was calculated from the charged amounts of the raw materials polycarbonate compound (polycarbonate polyol (b-1), etc.) and polyester compound (polyester polyol (b-2), polyester polyol (b-3), etc.). The ester group concentration is defined by the following formula. Ester group concentration (mass%) = polyester compound charge (g) / (polycarbonate compound charge (g) + polyester compound charge (g)) x 100
[0084] (Polycarbonate polyol (B) content) The content of the polycarbonate polyol (B) in the polyurethane resin composition was calculated from the mass ratio of the solid content when the polyol (A) and the hydroxyl group-containing acrylic resin (C) were mixed. Therefore, the content of the polycarbonate polyol (B) is defined by the following formula.
[0085] Content of polycarbonate polyol (B) (% by mass) = Charge amount of polycarbonate polyol (B) (g) / (Charge amount of polyol (A) (g) + Charge amount of solid content of hydroxyl group-containing acrylic resin (C) (g)) × 100
[0086] (Urethane group concentration) The urethane group concentration in the polyurethane resin composition was calculated from the mass ratio of the solid content when polyol (A), hydroxyl group-containing acrylic resin (C), and polyisocyanate (D) were mixed. Therefore, the urethane group concentration is defined by the following formula.
[0087] Urethane group concentration (mmol / g) = (hydroxyl value of polyol (A) (KOHmg / g) / 56.11 (KOHg / mol) × charge amount of polyol (A) + hydroxyl value of hydroxyl-containing acrylic resin (C) (KOHmg / g) / 56.11 (KOHg / mol) × charge amount of hydroxyl-containing acrylic resin (C) (g)) / (charge amount of polyol (A) (g) + charge amount of solids of hydroxyl-containing acrylic resin (C) (g) + charge amount of polyisocyanate (D) (g)) (Analysis and Evaluation) [Measurement of number average molecular weight] The composition thus obtained was subjected to GPC analysis under the following conditions to measure the number average molecular weight of the composition. The results are shown in Table 1.
[0088] -conditions- (1) Measuring instrument: HLC-8420 (manufactured by Tosoh Corporation) (2) Column: TSKgel (Tosoh Corporation) G3000H-XL G3000H-XL G2000H-XL G2000H-XL (3) Mobile phase: THF (tetrahydrofuran) (4) Detector: RI (refractive index) detector (accessory for HLC-8420) (5) Temperature: 40℃ (6)Flow rate: 1.000ml / min (7) Calibration curve: A calibration curve was obtained using the following products (all bifunctional polyoxypropylene polyols manufactured by Sanyo Chemical Industries, Ltd.). "Sannix PP-200" (number average molecular weight = 200, average number of functional groups: 2) "Sannix PP-400" (number average molecular weight = 400, average number of functional groups: 2) "Sannix PP-1000" (number average molecular weight = 1000, average number of functional groups: 2) "Sannix PP-2000" (number average molecular weight = 2000, average number of functional groups: 2) "Sannix PP-3000" (number average molecular weight = 3200, average number of functional groups: 2) "Sannix PP-4000" (number average molecular weight = 4160, average number of functional groups: 2) (8) Approximation of calibration curve: Cubic equation (9) Sample solution concentration: 0.5% by mass in THF solution
[0089] [Measurement of hydroxyl value (OHv)] The hydroxyl value of the resulting composition was measured by a method using an acetylating agent in accordance with JIS K1557-1, and the results are shown in Table 1.
[0090] [Characteristics evaluation] The obtained composition was used as a sample, which was heated at 80°C for 1 hour and then left at 25°C for 3 days. The state of the sample after leaving it was visually confirmed, and if it had even a slight fluidity at the above temperature, it was classified as liquid, and if it had no fluidity, it was classified as solid. The results are shown in Table 1.
[0091] [Production of polyol 1] 826g of 1,6-hexanediol, 787g of diethyl carbonate, and 0.05g of tetrabutyl titanate were mixed in a 2L two-necked glass reactor equipped with a stirrer, a thermometer, a heating device, a fractionator filled with structured packing, and a cooler, and reacted at 100-190°C for 8 hours under normal pressure while removing low boiling point components. The reaction temperature was then increased to 190°C, the pressure in the flask was reduced to 1kPa, and the reaction was continued for another 8 hours to obtain a polycarbonate polyol (PCD-1).
[0092] [Production of polyol 2] 830g of 1,6-hexanediol, 771g of diethyl carbonate, and 0.05g of tetrabutyl titanate were mixed in a 2L two-necked glass reactor equipped with a stirrer, a thermometer, a heating device, a fractionator filled with structured packing, and a cooler, and reacted at 100-190°C for 8 hours under normal pressure while removing low boiling point components. The reaction temperature was then increased to 190°C, the pressure in the flask was reduced to 1kPa, and the reaction was continued for another 8 hours to obtain a polycarbonate polyol (PCD-2).
[0093] [Production of polyol 3] 1,6-hexanediol 107.6g, 1,5-pentanediol 94.8g, diethyl carbonate 197.6g, and tetrabutyl titanate 0.02g were mixed in a 1L two-neck glass reactor equipped with a stirrer, thermometer, heater, and a rectification column filled with structured packing and a cooler, and reacted at 100-190°C for 8 hours under normal pressure while removing low boiling point components. The reaction temperature was then increased to 190°C, the pressure in the flask was reduced to 1kPa, and the reaction was continued for another 8 hours to obtain a polycarbonate polyol (PCD-3).
[0094] [Production of polyol 4] In a 1 L four-neck glass reactor equipped with an agitator, a thermometer, a heating device, and a cooler, 575 g of the polyol (PCD-1) obtained in Polyol Production 1, 400 g of polycaprolactone triol (PLACCEL 305), 25 g of polycaprolactone diol (PLACCEL 210), and 0.03 g of potassium hydrogen carbonate were charged, and an ester exchange reaction was carried out at 190°C for 5 hours to obtain a polyol (PCP-1).
[0095] [Production of polyol 5] In a 1 L four-neck glass reactor equipped with an agitator, a thermometer, a heating device, and a cooler, 674 g of the polyol (PCD-2) obtained in Polyol Production 2, 326 g of polycaprolactone triol (Placcel 305), and 0.03 g of potassium hydrogen carbonate were charged, and an ester exchange reaction was carried out at 190°C for 5 hours to obtain a polyol (PCP-2).
[0096] [Production of polyol 6] 322.3g of 1,6-hexanediol, 61.4g of 1,4-butanediol, 73.2g of trimethylolpropane, 443.0g of diethyl carbonate, and 0.045g of lithium acetylacetonate were mixed in a 1L two-neck glass reactor equipped with a stirrer, a thermometer, a heating device, a fractionator filled with structured packing, and a cooler, and reacted at 100-150°C for 8 hours under normal pressure while removing low boiling point components. The reaction temperature was then increased to 150°C, the pressure in the flask was reduced to 1kPa, and the reaction was continued for another 8 hours to obtain a polycarbonate polyol (PCP-3).
[0097] [Table 1]
[0098] Polyol (A) including polycarbonate polyol (B), hydroxyl-containing acrylic resin (C), polyisocyanate (D), curing catalyst, phosphorus compound, and leveling agent were mixed as shown in Table 2, and the liquid immediately after mixing was poured onto Color Aluminum EP White (manufactured by Paltec), cast with an applicator to a thickness of 100 μm, and dried at 25° C. for 30 minutes and at 80° C. for 12 hours to form a coating film. This coating film was used as a sample and evaluated for the following items. The results are shown in Table 2. The unit of charge in the table is grams.
[0099] [Evaluation test] <Appearance of coating film> The appearance of the coating film was judged by visual inspection of the condition of the coating film after drying, and if the coating film condition was smooth, it was rated as good.
[0100] <Weather resistance test> Coating films (approximately 20 μm thick after drying) made from the paints obtained according to the formulations shown in Table 2 were subjected to accelerated weather resistance tests under the following conditions. Test equipment: QUV (Q-LAB) Lamp: EL-313 ·Illuminance: 0.59w / m2 λmax:313nm 1 cycle: 12 hours (UV irradiation: 8 hours (temperature 70°C), condensation: 4 hours (temperature 50°C)) Test time: 504 hours
[0101] [Coating film characteristics] <20° gloss retention> In accordance with JIS Z8741, the gloss at 20° was measured using a gloss meter (product name: micro-TRI-gloss, manufactured by BYK) and the gloss retention was calculated using the following formula (Formula-1). Gloss retention (%) = gloss after weathering test ÷ initial gloss × 100 (Formula 1)
[0102] <Color difference ΔE> In accordance with JIS Z28722, the L*, a*, and b* values were measured using a handy colorimeter (spectro 2 guide 45°:C:0°, manufactured by BYK) and the color difference ΔE was calculated using the following formula (Formula-2). Color difference ΔE=[(ΔL*) 2 +(Δa*) 2 +(Δb*) 2 ] 1 / 2 (Formula-2) ΔL* = L* (after weather resistance test) - L* (before weather resistance test) Δa*=a*(after weather resistance test)-a*(before weather resistance test) Δb*=b*(after weather resistance test)-b*(before weather resistance test)
[0103] [Evaluation Criteria] A coating was rated as "good" when it had a 20° gloss retention of 60% or more and a color difference ΔE of 4.5 or less. A coating was rated as "very good" when it had good appearance, a gloss retention of 60% or more, and a color difference ΔE of 4.5 or less.
[0104] [Table 2]
[0105] 1,4-Butanediol: Fujifilm Wako Pure Chemical Industries, Ltd. 1,5-Pentanediol: Fujifilm Wako Pure Chemical Industries, Ltd. 1,6-Hexanediol: BASF JAPAN Trimethylolpropane: Sigma-Aldrich Diethyl carbonate: Sigma-Aldrich Plaxel 305 Polycaprolactone triol (molecular weight = 550, hydroxyl value = 305, number of functional groups = 3) manufactured by Daicel Corporation Plaxel 210 Polycaprolactone diol (molecular weight = 1000, hydroxyl value = 112, functionality = 2) manufactured by Daicel Corporation Tetrabutyl titanate: Tokyo Chemical Industry Co., Ltd. Potassium bicarbonate: Fujifilm Wako Pure Chemical Industries, Ltd. Lithium acetylacetonate: Sigma-Aldrich Acrydic A-801: DIC (solid content 50%, OHv: 50mgKOH / g, hydroxyl group-containing acrylic resin) C-HXLV: (HDI-based isocyanurate, NCO content: 23.2%, solid content: 50%, manufactured by Tosoh Corporation) -Butyl acetate: manufactured by Tokyo Chemical Industry Co., Ltd. BYK-Silcrean-370: BYK DOTDL: Dioctyltin dilaurate, manufactured by Kishida Chemical Industry Co., Ltd. JP-508: Product name, 2-ethylhexyl acid phosphate, Johoku Chemical Industry Co., Ltd.
Claims
1. A polyol (A) including a polycarbonate polyol (B); A hydroxyl group-containing acrylic resin (C), and a polyisocyanate (D), The polyurethane resin composition, wherein the polycarbonate polyol (B) has an ester bond and has an average hydroxyl functional group number of more than 2.
2. The polyurethane resin composition according to claim 1, wherein the content of the polycarbonate polyol (B) is 5 to 90 mass% based on the total content of the polyol (A) and the solid content of the hydroxyl group-containing acrylic resin (C).
3. The polycarbonate polyol (B) is or comprising an ester exchange reaction product of a polycarbonate polyol (b-1) and a polyester polyol (b-2) having an average hydroxyl functional group number of 3 or more; 2. The polyurethane resin composition according to claim 1, comprising an ester exchange reaction product of a polycarbonate polyol (b-1), a polyester polyol (b-2) having an average hydroxyl functional number of 3 or more, and a polyester polyol (b-3) having an average hydroxyl functional number of 2 or more and less than 3.
4. the deemed average hydroxyl functional number of the polycarbonate polyol (B) is 2.1 to 3.5, The hydroxyl value of the polycarbonate polyol (B) is 40 to 500 mgKOH / g, The number average molecular weight of the polycarbonate polyol (B) is 400 to 4,000 g / mol; The polyurethane resin composition according to claim 3, wherein the mass ratio of the polycarbonate polyol (b-1) to the polyester polyol (b-2) ([mass of (b-1)] / [mass of (b-2)]) is 90 / 10 to 10 / 90, or the mass ratio of the polycarbonate polyol (b-1) to the sum of the polyester polyol (b-2) and the polyester polyol (b-3) ([mass of (b-1)] / ([mass of (b-2)]+[mass of (b-3)])) is 95 / 5 to 5 / 95.
5. The polyurethane resin composition according to claim 1, wherein the polycarbonate polyol (B) has an ester group concentration of 10 to 90 mass%.
6. The polyurethane resin composition according to any one of claims 1 to 5, wherein the polycarbonate polyol (B) is liquid at room temperature.
7. A coating composition comprising the polyurethane resin composition according to any one of claims 1 to 5.
8. A coating film comprising a cured product of the coating composition according to claim 7.
Citation Information
Patent Citations
Coating composition
JP2018059072A