Bent article, bending method and metal mold for bending
The described bending method and mold configuration for high-strength metal plates address dimensional accuracy, springback, and strength issues by managing residual stress through a punch with a protrusion and die recess, ensuring high-quality, aesthetically pleasing results for building materials.
Patent Information
- Application Number
- JP2023058123
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing methods for bending high-strength metal plates used in building materials face challenges such as reduced dimensional accuracy, springback, insufficient strength, and aesthetic defects, particularly when forming long lengths, which are exacerbated by high yield strength and strict processing conditions.
A bending method and mold configuration using a punch with a protrusion and a die with a V-shaped recess, where the protrusion's tip forms a convex curved surface with a specific radius and length, and the die recess has a concave surface, applying compressive stress to the bent portion, and incorporating a recess with a concave surface to manage residual stress distribution.
The method and mold enable high-dimensional accuracy, suppress springback, ensure sufficient strength, and maintain aesthetic quality, particularly suitable for long lengths, with improved buckling resistance and reduced risk of cracking.
Smart Images

Figure 2024145672000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a bent product, a bending method, and a die for bending. [Background technology]
[0002] Exterior and interior building materials include components used in easily visible locations such as window frames and curtain walls. These components require precise dimensions without distortion, small diameters at bent parts, and sharp bend ridges, and are required to have design and aesthetic appeal. In recent years, there has been a trend to use metal materials with high yield strength of 300 MPa or more for these components in order to ensure their strength as structural members.
[0003] When bending a high-strength metal plate material, the dimensional accuracy after bending may decrease. If the processing conditions are made strict in order to improve the dimensional accuracy, cracks may occur in the bent portion. In addition, if the processing conditions are made strict, it may cause scratches or scoring scratches, which may impair the design. This is particularly problematic when applied to building materials where aesthetics are important. In addition, when manufacturing a bent product with a total length of, for example, 1 m or more, the forming load becomes very large, and the capacity of the press molding machine may be insufficient, making it impossible to perform the bending process.
[0004] Patent Document 1 describes a grooved austenitic stainless steel sheet that makes it possible to provide a grooved steel sheet material that can form sharp ridgelines with excellent design by bending. However, Patent Document 1 requires the provision of a V-groove on the steel sheet surface, which is disadvantageous in terms of cost. In addition, the provision of a V-groove on the steel sheet surface reduces the thickness of the steel sheet, which reduces the wall thickness at the bent part of the bent product after bending, which may result in insufficient strength.
[0005] Patent Document 2 describes a press processing method in which, when bending a metal plate using a bending device consisting of a punch and a die, a recess having a depth of 20% or less of the metal plate thickness is formed on at least a part of the convex side of the bent metal plate in the final step of the forming stroke. However, the processed product manufactured by the press processing method described in Patent Document 2 may be unsightly because a recess is formed on the convex side, making it difficult to use it as a material for exterior or interior building materials. In addition, Patent Document 2 assumes that the material is a soft aluminum alloy plate, so there is a risk that it cannot be applied to bending metal plate materials having high strength.
[0006] Patent Document 3 describes a method of bending a workpiece having a thickness of t at a desired angle using a bending die that is made of a die and a punch, with the vicinity of the portion of the die and punch where the workpiece is to be bent being higher than the other die surfaces by a height of at most 10% of the thickness t, and with the apex corner of the die being rounded with a radius of approximately t. However, with the bending method described in Patent Document 3, it is difficult to suppress springback after bending. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2008-169423 A [Patent Document 2] Patent No. 3633012 [Patent Document 3] Special Publication No. 47-25266 Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made in consideration of the above circumstances, and aims to provide a bent product that can suppress springback, has no risk of insufficient strength at the bent portion, and has excellent resistance to buckling deformation. Another aim of the present invention is to provide a bending method and a bending die that can stably obtain bent products with high dimensional accuracy without increasing the forming load and can suppress springback. [Means for solving the problem]
[0009] In order to solve the above problems, the present invention employs the following configuration. [1] A plate part made of a metal plate material having a 0.2% proof stress of 300 MPa or more, a yield ratio of 0.90 or less, and a plate thickness of 6.0 mm or less; and a bending part provided on the plate part; The radius of curvature of the convex curved surface on the outer side of the bent portion is a radius of a length equivalent to the plate thickness of the plate portion, The minimum thickness of the bent portion is 0.75 times or more the plate thickness t of the plate portion, A recess is provided on the inner side of the bent portion along the longitudinal direction of the bent portion, The recess has a depth equivalent to a length of 10% or more and less than 30% of the plate thickness of the plate portion, and a concave curved surface having a curvature radius equivalent to a length of more than 50% and less than 100% of the plate thickness of the plate portion is provided at the bottom, On both sides of a first imaginary line L1 connecting the apex of the convex curved surface on the outer side of the bend and the apex of the concave curved surface of the concave portion, L1 Average Vickers hardness HV greater than L2 There is a high hardness region showing A bent product that satisfies the following formula (1) and the following formula (2). 1.10≦(HV L2 / HV L1 )≦1.30…(1) 1.20≦(HV L2 / HV m )<1.50 …(2) However, HV in formula (1) L1is the average Vickers hardness on the first virtual line L1, and HV L2 is the average Vickers hardness on a second imaginary line L2 that connects the outer surface of the bent portion and the inner surface of the recess and passes through the high hardness region, and HV m is the Vickers hardness of the plate portion. [2] The bent product described in [1], wherein the total length of the plate material portion is 1 m or more, and the bent portion extends along the total length of the plate material portion. [3] The metal plate material has a 0.2% yield strength of 450 MPa or more and a yield ratio of 0.50 to 0.90, Its chemical composition is in mass percent, C: 0.050% or less, Si: 2.00% or less, Mn: 1.00-8.00%, P: 0.050% or less, S: 0.0500% or less, Ni: 0.10-6.00%, Cr: 17.00~25.00%, Mo: 0.10-2.50%, Cu: 0.10-3.00%, N: Contains 0.080 to 0.300% The bent product according to [1] or [2], wherein the remainder is a ferritic-austenitic duplex stainless steel plate consisting of Fe and impurities. [4] The bent product according to [3], wherein the metal plate further contains, in mass %, one or more of the following group A, group B or group C in place of a portion of Fe: (Group A) One or more of the following: Sn: 0.01 to 1.00% or less, W: 0.01 to 1.00%, V: 0.01 to 1.00%. (Group B) One or more of the following: Ca: 0.0050% or less, Mg: 0.0050% or less, Al: 0.50% or less, rare earth elements: 0.50% or less. (Group C) Nb: 0.100% or less [5] A placement step of placing a blank made of a metal plate between the punch and the die; a forming step of bending the blank by bringing the punch and the die closer to each other, The material is a metal plate material having a 0.2% proof stress of 300 MPa or more, a yield ratio of 0.90 or less, and a plate thickness of 6.0 mm or less, the punch comprises a pair of punch type surfaces approaching each other toward the punch tip, and a protrusion provided at the punch tip, the tip surface of the protrusion is a convex curved surface with a radius of curvature corresponding to a length of more than 50% and not more than 100% of the plate thickness of the material, and the length of the protrusion is a length corresponding to 10% or more and less than 30% of the plate thickness of the material; the die is provided with a V-groove-shaped die recess facing the pair of punch type surfaces, and a concave curved surface with a radius of curvature corresponding to a length of 20% or more and 60% of the plate thickness of the material is provided at the bottom of the die recess; The forming step is a step of bringing the punch and the die close to each other so that the punch and the die are in close contact with the material, and pressing at least a portion of the protrusion of the punch into the material. [6] The total length of the material made of the metal plate is 1 m or more; The bending method according to [5], wherein in the positioning step, the metal plate is positioned so that the overall length direction of the metal plate is aligned with the longitudinal direction of the V-groove-shaped die recess. [7] A die for bending a material made of a metal plate having a 0.2% proof stress of 300 MPa or more, a yield ratio of 0.90 or less, and a plate thickness of 6.0 mm or less, A punch including a pair of punch die faces approaching each other toward a tip of the punch and a protrusion provided at the tip of the punch; A die block having a V-groove-shaped die recess corresponding to the pair of punch faces, The tip surface of the protrusion is a convex curved surface having a radius of curvature corresponding to a length of more than 50% and not more than 100% of the plate thickness of the material, and the length of the protrusion is a length corresponding to 10% or more and less than 30% of the plate thickness of the material, A bending die, wherein a bottom of the V-groove-shaped recess is provided with a concave curved surface having a radius of curvature corresponding to a length of 20% to 60% of the plate thickness of the material. Effect of the Invention
[0010] According to the bent product of the present invention, the radius of curvature of the convex curved surface on the outer side of the bent portion is a radius of a length equivalent to or less than the thickness of the plate portion, so that the radius of curvature of the convex curved surface on the outer side of the bent portion is small and a sharp shape can be obtained. Also, since the minimum thickness of the bent portion is 0.75 times or more the thickness of the plate portion, the strength of the bent portion can be made sufficient. In addition, the bent product of the present invention has a recess along the longitudinal direction of the bent portion, and a concave curved surface is provided inside the recess. This recess is an indentation formed by the protruding portion of the punch during die bending. By providing such an indentation, the bent portion of the bent product is in a state in which compressive residual stress is imparted in the thickness direction of the bent portion. Therefore, according to the present invention, springback caused by the relationship between the conventional compressive residual stress and the tensile residual stress is reduced, and the springback can be reduced. In addition, since the inner surface of the recess is a concave curved surface, the occurrence of cracks originating from the recess can also be prevented. Furthermore, according to the bent product of the present invention, on both sides of a first imaginary line L1 connecting the apex of the convex curved surface on the outside of the bend and the apex of the concave curved surface of the concave portion, the average Vickers hardness HV L1 Average Vickers hardness HV greater than L2 and satisfies the above formulas (1) and (2). In this way, the bent portion of the bent product of the present invention has two high hardness regions with a relatively high Vickers hardness HV, and therefore has excellent buckling resistance. Furthermore, by satisfying formula (2), it is possible to impart sufficient strength to the bent portion, even though the thickness of the bent portion is smaller than the plate thickness of the plate portion due to the provision of a recess in the bent portion.
[0011] Furthermore, according to the bent product of the present invention, the total length of the plate portion is 1 m or more, and the bent portion extends along the entire length of the plate portion, so that the product can be suitably used as an exterior or interior building material for buildings, particularly as a component for use in areas that are easily visible, such as window frames and curtain walls.
[0012] According to the bending method of the present invention, when bending a material using a punch and a die, a punch having a protrusion at the tip of the punch and a die having a V-shaped groove with a concave bottom are used, and at least a part of the protrusion of the punch is pressed into the material, so that the material is pressed into the bottom of the die recess, and material flows into the bottom of the die recess. In addition, since the radius of curvature of the concave bottom of the die recess is set to a length equivalent to 60% or less of the plate thickness of the material, the radius of curvature of the convex curved surface on the outside of the bend of the bent portion is reduced. Furthermore, by pressing the protrusion into the material, the distribution state of the residual stress in the bent portion is made different from the distribution state of the residual stress in the bent portion when the punch without the protrusion is used for the bent portion. In conventional bending, it is believed that springback occurs due to the tensile residual stress on the outside of the bend and the compressive residual stress on the inside of the bend, but in the present invention, the residual stress distribution in the bent portion changes compared to the conventional method, so that the springback after the bending process is reduced.
[0013] Furthermore, according to the bending method of the present invention, by forming the tip surface of the protrusion of the punch into a convex curved surface with a predetermined radius of curvature and setting the length of the protrusion to a predetermined length, it is possible to manufacture a bent product in which, on both sides of an imaginary line connecting the tip of the convex curved surface on the outside of the bend and the tip of the concave curved surface of the recess, there are high hardness regions exhibiting a Vickers hardness HV higher than the Vickers hardness HV on this imaginary line. Such a bent product has excellent buckling resistance.
[0014] Therefore, according to the present invention, by using a metal plate material satisfying the requirements of 0.2% proof stress of 300 MPa or more, a yield ratio of 0.90 or less, and a plate thickness of 6.0 mm or less, springback can be suppressed, there is no risk of insufficient strength at the bent portion, and a bent product with excellent resistance to buckling deformation can be manufactured. Also, according to the bending method of the present invention, the radius of curvature of the convex curved surface on the outside of the bent portion can be made small and the shape can be made sharp.
[0015] The bending die of the present invention includes a punch having a protrusion at its tip, and a die having a V-groove-shaped die recess with a concave curved bottom. By using this die when bending a material made of a metal plate satisfying the following requirements: 0.2% proof stress of 300 MPa or more, a yield ratio of 0.90 or less, and a plate thickness of 6.0 mm or less, it is possible to stably produce bent products with high dimensional accuracy and excellent buckling resistance. [Brief description of the drawings]
[0016] [Figure 1A] FIG. 1A is a schematic diagram showing a die for bending a metal plate according to an embodiment of the present invention. [Figure 1B] FIG. 1B is a schematic diagram illustrating the length of a protrusion in a mold according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram illustrating a method for bending a metal plate material according to an embodiment of the present invention. [Diagram 3] FIG. 3 is a schematic diagram illustrating a method for bending a metal plate material according to an embodiment of the present invention. [Figure 4] FIG. 4 is a schematic diagram illustrating a method for bending a metal plate material according to an embodiment of the present invention. [Diagram 5] FIG. 5 is a schematic cross-sectional view of a bent product made of a metal plate according to an embodiment of the present invention. [Figure 6] FIG. 6 is a schematic cross-sectional view showing a main part of a bent product made of a metal plate according to an embodiment of the present invention. [Figure 7] FIG. 7 is a schematic diagram illustrating a conventional method for bending a metal plate material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, a bending method, a bending die (hereinafter sometimes referred to as a die), and a bent product according to embodiments of the present invention will be described.
[0018] The outline of this embodiment is as follows. The bending method of this embodiment includes a placement step of placing a material 3 made of a metal plate between a punch 1 and a die 2 as shown in Fig. 2, and a forming step of bending the material 3 by bringing the punch 1 and the die 2 close to each other as shown in Fig. 3 and Fig. 4. The material 3 is a metal plate satisfying the following requirements: a 0.2% proof stress of 300 MPa or more, a yield ratio of 0.90 or less, and a plate thickness t of 6.0 mm or less.
[0019] As shown in Fig. 1A, the punch 1 has a pair of punch die faces 1b and a protrusion 1c provided at the punch tip 1a. The tip surface 1e of the protrusion 1c is a convex curved surface, and the length H of the protrusion 1c is a predetermined length. The die 2 is provided with a V-groove-shaped die recess 2a facing the pair of punch die faces 1b. The bottom 2d of the die recess 2a is provided with a concave curved surface 2b with a predetermined radius of curvature.
[0020] In the forming process, the punch 1 and the die 2 are brought close to each other so that the punch 1 and the die 2 are brought into close contact with the material 3, and at least a part of the protrusion 1c of the punch 1 is pressed into the material 3. As a result, as shown in Fig. 5, the radius of curvature Rout of the convex curved surface 4c on the outer side of the bent portion becomes small, and a bent product 4 having a sharply shaped bent portion 4b is obtained.
[0021] 5, the manufactured bent product 4 includes a plate portion 4a made of a metal plate and a bent portion 4b provided on the plate portion 4a. A recess 4d is provided on the inner side of the bent portion 4b along the longitudinal direction of the bent portion. The recess 4d is provided by pressing the protrusion 1c of the punch 1 into the blank 3. The bent product 4 has an average Vickers hardness HV on both sides of an imaginary line L1 connecting the apex of the convex curved surface 4c on the outside of the bend and the groove bottom of the concave portion 4d corresponding to the tip (apex of the convex curved surface) of the protrusion 1c of the punch 1, i.e., the apex of the concave curved surface 4e. L1 Average Vickers hardness HV greater than L2 and satisfies the following formula (1) and formula (2). This improves the buckling resistance.
[0022] 1.10≦(HV L2 / HV L1 )≦1.30…(1) 1.20≦(HV L2 / HV m )<1.50 …(2)
[0023] However, HV in formula (1) L1 is the average Vickers hardness on the first virtual line L1, and HV in formulas (1) and (2) L2 is the average Vickers hardness on the second imaginary line L2 that connects the outer surface of the bent portion and the inner surface of the recess and passes through the high hardness region R, and is expressed by HV in formula (2). m is the Vickers hardness of the plate portion 4a.
[0024] The present embodiment will be described below in order.
[0025] (material) The raw material 3 according to this embodiment is a metal plate material that satisfies the following requirements: 0.2% proof stress of 300 MPa or more, a yield ratio of 0.90 or less, and a plate thickness t of 6.0 mm or less. The reasons for limiting the metal plate material suitable for the raw material 3 will be described below.
[0026] <0.2% yield strength> The 0.2% yield strength of the metal plate material according to this embodiment is 300 MPa or more. This ensures sufficient strength when the metal plate material according to this embodiment is used as a material for exterior building materials or interior building materials. If the 0.2% yield strength is less than 300 MPa, the strength is insufficient. The 0.2% yield strength may be 450 MPa or more.
[0027] <Yield ratio> The yield ratio of the metal plate material according to this embodiment is set to 0.90 or less. This makes it possible to suppress cracks in the bent portion, particularly on the outer surface of the bent portion, during bending. If the yield ratio exceeds 0.90, cracks will occur on the outer surface of the bent portion during bending, making it impossible to provide a bent product with excellent appearance. The ratio of yield strength (YS) to tensile strength (TS) is called the yield ratio (YS / TS), and here, the 0.2% proof stress is defined as the yield strength (YS). The yield ratio may be 0.50 or more.
[0028] <Thickness> The sheet thickness t of the metal sheet material according to this embodiment is 6.0 mm or less, preferably 4.0 mm or less. The lower limit of the sheet thickness t may be 0.5 mm or more, or may be 1 mm or more. By setting the sheet thickness t to 6.0 mm or less, the springback of the bent product after bending can be reduced.
[0029] The metal plate material according to the present embodiment is preferably a ferritic-austenitic duplex stainless steel plate (hereinafter, referred to as a duplex stainless steel plate). The duplex stainless steel plate has sufficient strength, is less expensive than an austenitic stainless steel plate, and has better corrosion resistance than a ferritic stainless steel plate.
[0030] However, because stainless steel has a higher yield strength than austenitic stainless steel and ferritic stainless steel, bending the material may result in poor dimensional accuracy. If the processing conditions are made strict in order to improve dimensional accuracy, cracks may occur in the bent portion. In addition, if the processing conditions are made strict, scratches or scoring may occur, which may impair the design and aesthetics of the material.
[0031] Furthermore, because the material itself is hard, a large forming load must be applied, and large stress concentration occurs in the punch and die, which may damage the die. For this reason, it has been difficult to apply duplex stainless steel sheets to exterior and interior building materials that require bending in places that are easily visible. In addition, when manufacturing bent products with a total length of, for example, 1 m or more, the forming load becomes so large that the capacity of the press molding machine is insufficient, making it impossible to perform the bending process.
[0032] However, by applying the present invention, bending can be performed without causing such problems and without damaging the mold, and it is also possible to provide a bent product with excellent design and aesthetic appeal.
[0033] When the metal plate material is a duplex stainless steel plate, the metal plate may be a steel plate having a 0.2% proof stress of 450 MPa or more, a yield ratio of 0.50 to 0.90, and a plate thickness t of 6.0 mm or less.
[0034] (Mold) Next, a metal plate bending die used in manufacturing the bent product of this embodiment will be described with reference to FIG. 1A. The die K according to this embodiment is a die for so-called die bending. That is, the die K according to this embodiment is used as a die for a processing method in which the die K (punch 1 and die 2) is pressed against the top and bottom of the material 3 with both ends 3a of the material 3 as free ends to bend the material 3. The die K according to this embodiment will be described below.
[0035] The mold K according to this embodiment is composed of a punch 1 and a die 2.
[0036] As shown in Fig. 1A, the punch 1 has a pair of punch die faces 1b that are inclined so as to approach each other toward the punch tip 1a, and a protrusion 1c provided on the punch tip 1a. The pair of punch die faces 1b have a relative angle θp in the range of, for example, 80 to 100°, preferably 85 to 95°, more preferably 88 to 92°, and even more preferably 90°. The pair of punch die faces 1b form the outer shape of the punch 1, and are inclined so as to approach each other toward the punch tip 1a. The punch tip 1a has a protrusion 1c.
[0037] The protrusion 1c protrudes from the punch tip 1a toward the die 2. As shown in Fig. 1A, the protrusion 1c has a side wall surface 1d in contact with the punch die surface 1b and a tip surface 1e in contact with the side wall surface 1d. The side wall surface 1d is flat, and the tip surface 1e is a convex curved surface.
[0038] The tip surface 1e of the protrusion 1c is a convex curved surface with a radius of curvature Rp. The radius of curvature Rp of the tip surface 1e is a radius corresponding to a length that is more than 50% and not more than 100% of the thickness t of the material 3, that is, a length that is more than 0.50t and not more than 1.00t. By setting the radius of curvature Rp to a radius corresponding to a length that is more than 50% (0.50t) of the thickness t of the material 3, as described below, it is possible to impart sufficient compressive stress to the bent portion 4b, thereby reducing the springback of the bent product 4. Furthermore, it is possible to reduce the forming load applied to the punch 1 during forming. The radius of curvature Rp of the tip surface 1e is preferably a radius corresponding to a length that is more than 55% (0.55t) of the thickness t of the material 3. Moreover, by setting the radius of curvature Rp to a radius equivalent to a length equal to or less than 100% (1.00t) of the plate thickness t of the raw material 3, it is possible to reduce the radius of curvature Rout of the convex curved surface 4c on the outer side of the bent portion 4b after bending. Furthermore, by making the tip surface 1e a convex curved surface, it is possible to prevent cracking of the bent portion 4b of the bent product 4.
[0039] The length H of the protrusion 1c is set to a length equivalent to 10% or more and less than 30% of the sheet thickness t of the material 3, that is, a length equivalent to 0.10t or more and less than 0.30t. As shown in FIG. 1A, the length H of the protrusion 1c is the length in the protruding direction of the protrusion 1c, and is the length from the boundary position between the side wall surface 1d and the punch die surface 1b to the tip surface 1e. By setting the length H of the protrusion 1c to a length equivalent to 10% (0.10t) or more of the sheet thickness t of the material 3, the material flow to the bottom of the die recess 2a is promoted, and the curvature radius Rout of the convex curved surface 4c on the outer side of the bent portion 4b after bending can be reduced. In addition, sufficient compressive stress can be applied to the bent portion 4b, and springback of the bent product can be suppressed. Furthermore, by setting the length H of the protrusion 1c to a length equivalent to less than 30% (0.30t) of the sheet thickness t of the blank 3, when the punch 1 reaches the bottom dead center, the blank 3 can be tightly attached to the punch die surface 1b and the die recess 2a of the punch 1, and can be constrained between the punch 1 and the die 2, thereby ensuring reliable bending. Furthermore, the protrusion 1c does not penetrate excessively into the blank 3, ensuring a sufficient thickness at the bent portion 4b of the bent product, and suppressing spring go. The length H of the protrusion 1c is preferably set to a radius equivalent to a length equal to or less than 28% (0.28t) of the sheet thickness t of the blank 3.
[0040] Furthermore, by setting the radius of curvature Rp of the tip surface 1e of the protrusion 1c and the length H of the protrusion 1c within the above range, two separated high hardness regions R with large Vickers hardness HV can be formed in the bent portion of the bent product, thereby making it possible to improve the buckling resistance of the bent product.
[0041] The length H of the protrusion 1c is defined as the length from the boundary between the side wall surface 1d and the punch die surface 1b to the tip surface 1e, but if the position of the boundary between the side wall surface 1d and the punch die surface 1b is unclear, the length H of the protrusion 1c may be determined as follows. That is, as shown in Fig. 1B, the position of the intersection X between the extension of the contour of the punch die surface 1b and the extension of the contour of the side wall surface 1d is identified, and an imaginary horizontal line M is drawn from the intersection X in the direction of the width W of the protrusion 1c. The distance between the horizontal line M and the tip of the protrusion 1c (the apex of the convex curved surface) is defined as the length H of the protrusion 1c.
[0042] In addition, it is preferable that the distance between the side wall surfaces 1d of the protrusions 1c, i.e., the width W of the protrusions 1c, is a length equivalent to 50% to 150% (0.50t to 1.50t) of the plate thickness t of the material 3. This can prevent damage to the protrusions 1c.
[0043] A concave curved surface 1g may be provided at the boundary between the pair of punch die surfaces 1b and the protrusion 1c. The radius of curvature Rj of the concave curved surface 1g is preferably set to a radius of curvature equivalent to a length equal to or less than 150% (1.50t) of the plate thickness t of the material 3. The provision of the concave curved surface 1g can prevent damage to the protrusion 1c.
[0044] Next, the die 2 will be described. As shown in FIG. 1A, the die 2 is made of a die block 2A provided with a die recess 2a. The die recess 2a is provided on the upper surface 2m of the die block 2A. The cross-sectional shape of the die recess 2a is a V-shaped groove with respect to the punch die surface 1b of the punch 1. That is, the die recess 2a is defined by a pair of die die surfaces 2c corresponding to the pair of punch die surfaces 1b and a concave curved surface 2b provided on the bottom 2d of the die recess 2a. The pair of die die surfaces 2c are inclined so as to approach each other toward the bottom 2d of the die recess 2a. The concave curved surface 2b is located between the pair of die die surfaces 2c. The pair of die die surfaces 2c and the concave curved surface 2b are in contact with each other.
[0045] The radius of curvature Rd of the concave surface 2b of the die recess 2a is set to a radius equivalent to a length of 20% to 60% of the thickness t of the material 3, i.e., a length of 0.20t to 0.60t. When bending is performed with a punch 1 having a protrusion, stress is concentrated on the concave surface 2b of the die recess 2a. This stress concentration increases as the radius of curvature Rd of the concave surface 2b becomes smaller. When the radius of curvature Rd is less than 20% of the thickness t of the material 3, the concentrated stress exceeds the fracture limit of the die 2, which may cause plastic deformation or cracking of the die 2. For this reason, the radius of curvature Rd of the concave surface 2b of the die recess 2a is set to 20% (0.20t) or more of the thickness t of the material 3. Furthermore, by setting the radius of curvature Rd to a radius of 60% (0.60t) or less of the plate thickness t of the raw material 3, a space in which the material can flow is secured at the bottom 2d of the die recess 2a, and the radius of curvature Rout of the convex curved surface 4c on the outer side of the bent portion 4b after bending can be reduced. Also, a compressive stress of an appropriate magnitude that does not cause spring-back can be applied to the bent portion 4b, thereby suppressing springback.
[0046] Next, the bending method of this embodiment will be described with reference to Fig. 2 to Fig. 4. In the bending method of this embodiment, a bent portion 4b is formed in the blank 3 by performing die bending on the blank 3 using a punch 1 and a die 2. The punch 1 and die 2 used in the bending are as shown in Fig. 1. The bending method of this embodiment includes a placement step and a forming step.
[0047] (Placement process) In the placement step, as shown in Fig. 2, the material 3 is placed on the upper surface 2m of the die block 2A of the die 2, and the punch 1 is placed above it. The material 3 is placed on the die 2 so that the upper surface 3b faces the punch 1 and the lower surface 3c contacts the upper surface 2m of the die block 2A. In this manner, the material 3 is placed between the punch 1 and the die 2. Both ends 3a of the material 3 are not constrained and are free ends. The punch 1 and the die 2 are attached to a press molding machine (not shown).
[0048] The total length of the blank 3 may be 1 m or more. In this case, the blank 3 (metal plate) is arranged so that the total length direction of the blank 3 (metal plate) is aligned with the longitudinal direction (depth direction in FIG. 2) of the V-groove-shaped die recess 2a.
[0049] (molding process) Next, in the forming step, the press molding machine is operated to bring the punch 1 and the die 2 closer to each other, and the blank 3 is subjected to a bending process.
[0050] In the forming process, as shown in Fig. 3, the punch 1 and the die 2 are brought relatively close to each other, and the protrusion 1c of the punch 1 is pressed against the upper surface 3b of the material 3. The material 3 against which the protrusion 1c is pressed is further pressed into the die recess 2a by the punch 1. As a result, bending deformation (plastic deformation) of the material 3 begins at the point where the protrusion 1c is in contact.
[0051] When the punch 1 and the die 2 are brought closer to each other, the material 3 undergoes bending deformation (plastic deformation) and the lower surface 3c of the material comes into close contact with the die surface 2c of the die 2. Meanwhile, the lower surface 3c of the material 3 separates from the upper surface 2m of the die 2. At this stage, the lower surface 3c of the material does not come into contact with the concave curved surface 2b of the bottom 2d of the die 2, leaving a gap S1. Meanwhile, the upper surface 3b of the material 3 is in contact only with the protrusion 1c, and the upper surface 3b of the material 3 is not in contact with the punch surface 1b. As a result, a space S2 is generated between the upper surface 3b of the material 3 and the punch surface 1b. There is still room to press the punch 1 further down until this space S2 is eliminated.
[0052] When the punch 1 and the die 2 are moved relatively close to each other until the punch surface 1b of the punch 1 comes into close contact with the upper surface of the blank 3, the punch surface 1b and the die surface 2c come into close contact with the upper surface 3b and the lower surface 3c of the blank 3, respectively, as shown in FIG. 4, and the protrusion 1c is pressed into the bent inner side of the bent portion 4b. The bent portion 4b is subjected to a process similar to forging as a result of compressive stress being applied in the thickness direction by the protrusion 1c. This causes material flow in the bent portion 4b, and the gap S1 that existed between the lower surface 3c of the blank 3 and the concave curved surface 2b of the die 2 is partially or entirely filled by the material flow. This reduces the radius of curvature Rout of the convex curved surface 4c on the outer side of the bent portion 4b. As a result of the above, a bent product 4 having a bent portion 4b as shown in FIG. 5 is manufactured.
[0053] FIG. 7 shows a schematic cross-sectional view of a case where a punch 111 without a protrusion is used for comparison. When the blank 3 is bent using the punch 111 without a protrusion, the punch 111 and the die 2 are moved relatively close to each other until the punch surface 111b and the die surface 2c are in close contact with the upper surface 3b and the lower surface 3c of the blank 3, respectively, as shown in FIG. 7. However, since the punch 111 does not have a protrusion, no material flow occurs in the bent portion 14b, and the bending process ends with a gap S1 remaining between the lower surface 3c of the blank 3 and the concave curved surface 2b of the die 2. For this reason, the bent product manufactured using the punch 111 without a protrusion cannot reduce the radius of curvature Rout of the convex curved surface 4c on the outer side of the bent portion 14b. In addition, since no compressive residual stress is imparted in the thickness direction of the bent portion 14b, it is difficult to suppress springback.
[0054] Next, the bent product 4 according to this embodiment will be described. Fig. 5 shows a schematic cross-sectional view of the bent product of this embodiment.
[0055] The bent product 4 according to this embodiment includes a plate part 4a made of a metal plate having a 0.2% proof stress of 300 MPa or more, a yield ratio of 0.90 or less, and a plate thickness t of 6.0 mm or less, and a bent part 4b provided on the plate part 4a. A convex curved surface 4c is provided on the bent outer side of the bent part 4b, and a concave part 4d is provided on the bent inner side. The total length of the plate part 4a (the length in the depth direction of the cross section shown in FIG. 5) is set to 1 m or more.
[0056] The bending angle θ of the bent portion 4b is in the range of 85° to 95°, more preferably in the range of 88 to 92°, and further preferably 90°. This means that when the target bending angle θ is 90°, the bending angle θ of the bent portion 4b is within the range of ±5° or ±2°. By setting the bending angle θ within the above range, the variation in the bending angle θ is reduced, and a sharp ridgeline is formed over the entire length of the outer side of the bend of the bent portion 4b.
[0057] Furthermore, the radius of curvature Rout of the convex curved surface 4c on the outside of the bend is set to a radius of a length equivalent to or less than the plate thickness t of the plate portion 4a. By setting the radius of curvature Rout of the convex curved surface 4c on the outside of the bend to be or less than the plate thickness t of the plate portion 4a, the appearance of the outside of the bend of the bent portion 4b becomes angular and sharp, making it suitable for use as an exterior building material and an interior building material.
[0058] A recess 4d is provided on the inner side of the bent portion 4b. This recess 4d is an indentation formed by pressing in the protrusion 1c of the punch 1 in the final stage of the forming process. A concave curved surface 4e is provided at the bottom of the recess 4d, which is formed by the tip surface 1e of the protrusion 1c. Since the inside of the recess 4d is the concave curved surface 4e, the occurrence of cracks starting from the recess 4d is prevented.
[0059] The depth D of the recess 4d provided on the inner side of the bend of the bent portion 4b is set to a depth equivalent to a length of 10% or more and less than 30% of the plate thickness t of the plate material portion 4a. The depth D of the recess 4d is preferably set to a depth equivalent to a length of 10% or more and 28% or less of the plate thickness t. Furthermore, the bottom of the recess 4d is provided with a concave curved surface 4e having a curvature radius Rq equivalent to a length of more than 50% and 100% or less of the plate thickness t of the plate material portion 4a. The curvature radius Rq of the concave curved surface 4e is preferably set to a curvature radius equivalent to a length of 55% or more and 100% or less of the plate thickness t. This makes it possible to reduce the curvature radius Rout of the convex curved surface 4c on the outer side of the bend. 6, the depth D of the recess 4d is the length in the depth direction of the recess 4d, and is the length from the position corresponding to the boundary between the side wall surface 1d and the punch die surface 1b of the punch 1 to the groove bottom (the apex of the concave curved surface 4e) of the recess 4d corresponding to the tip (the apex of the convex curved surface) of the protrusion 1c of the punch. The depth D of the recess 4d can be determined in the same manner as the method for measuring the length H of the protrusion 1c of the punch.
[0060] In addition, by providing a recess 4d on the inner side of the bend of the bent portion 4b, the thickness of the bent portion 4b becomes smaller than the plate thickness t of the plate portion 4a, but the minimum thickness of the bent portion 4b needs to be 0.75 times (0.75t) or more the plate thickness t of the plate portion 4a, thereby making it possible to ensure sufficient strength of the bent portion 4b.
[0061] Furthermore, in the bent product 4 of this embodiment, as shown in FIG. 6, when a first imaginary line L1 is provided connecting the apex of the convex curved surface 4c on the outside of the bend and the apex of the concave curved surface 4e at the groove bottom of the concave portion 4d, the average Vickers hardness HV on the first imaginary line L1 is L1 Average Vickers hardness HV greater than L2 In FIG. 6, the range in which the high hardness region R may exist is indicated by a dotted line. Note that the position and range of the high hardness region R are not limited to the position and range enclosed by the dotted line. In addition, the Vickers hardness HV in the high hardness region R is L2 does not need to be constant throughout the entire region, and there may be a distribution in the Vickers hardness HV. Therefore, the Vickers hardness HV in the high hardness region RL2 is the average value as described below.
[0062] In the bent portion 4b according to this embodiment, in addition to the work hardening caused by the plastic deformation of the material 3 by performing the molding process using the above-mentioned mold, the work hardening is also caused by the residual stress applied in the thickness direction by the protrusion 1c during the molding process, so that two high hardness regions R exist in the bent portion 4b. The average Vickers hardness HV L2 is the average Vickers hardness HV on the first virtual line L1 L1 and the Vickers hardness HV m The presence of such two high hardness regions R improves the buckling resistance of the bent portion 4b. This is because the two high hardness regions R are spaced apart from each other, and therefore the stress that the bent portion 4b receives when compressed in the longitudinal direction of the plate portion 4a is distributed to the high hardness regions, suppressing buckling deformation and improving buckling resistance. In addition, the presence of two high hardness regions R on both sides of the first virtual line L1 significantly improves the strength of the bent portion 4b.
[0063] In order to improve the buckling resistance and the strength of the bent portion 4b, it is necessary to satisfy the above formulas (1) and (2).
[0064] As shown in the above formula (1), (HV L2 / HV L1 ) is 1.10 or more, it is possible to reliably improve the buckling resistance. L2 / HV L1 The higher the average Vickers hardness HV, the better the buckling resistance. L2 is the average Vickers hardness HV L1 If it becomes too large compared to HV, it is not desirable because it may cause cracks. L2 / HV L1 ) shall be 1.30 or less.
[0065] In addition, as shown in the above formula (2), (HV L2 / HV mBy making the HV ) equal to or greater than 1.20, it is possible to increase the strength of the bent portion 4b and reliably improve the buckling resistance. L2 / HV m The higher the average Vickers hardness HV, the higher the buckling resistance and the strength of the bent portion 4b. L2 is HV m If it becomes too large compared to HV, it is not desirable because it may cause cracks. L2 / HV m ) must be less than 1.50. (HV L2 / HV m ) is preferably 1.45 or less.
[0066] The presence of the two high hardness regions R can be confirmed, for example, as follows. As shown in FIG. 6, the bent product 4 is cut to expose the cross section of the bent portion 4b. Next, a first imaginary line L1 is set connecting the apex of the convex curved surface 4c on the outside of the bend and the apex of the concave curved surface 4e at the groove bottom of the concave portion 4d. The Vickers hardness HV is measured at at least three points on the set first imaginary line L1. The interval between the measurement positions on the first imaginary line L1 is, for example, 100 μm. The average of the measured values is referred to as the average Vickers hardness HV on the first imaginary line L1. L1 Let us assume that.
[0067] Next, a second virtual line L2 is set that connects the shortest distance between the outer surface 4h on the outside of the bend of the bent portion 4b and the inner surface 4k of the recess 4d. The outer surface 4h on the outside of the bend of the bent portion 4b corresponds to the lower surface 3c of the material 3 and is a surface that includes the convex curved surface 4c. The inner surface 4k of the recess 4d is a surface that defines the recess 4d and is a surface that includes the concave curved surface 4e. The second virtual line L2 is set by gradually approaching a parallel line L3 parallel to the outer surface 4h from the outer surface 4h side toward the recess 4d side, specifying the point where the parallel line L3 first contacts the inner surface 4k of the recess as a contact point S, and setting a straight line L2 perpendicular to the outer surface 4h from the contact point S toward the outer surface 4h. This straight line is the second virtual line L2. The second virtual line L2 is set on both sides of the first virtual line L1. That is, two second virtual lines L2 are set.
[0068] Next, the Vickers hardness HV is measured at at least three points on each of the second imaginary lines L2. The interval between the measurement points on the second imaginary lines L2 is, for example, 100 μm. The average of the measurement values is called the average Vickers hardness HV on the second imaginary lines L2. L2 Let us assume that.
[0069] And the average Vickers hardness HV on the first virtual line L1 L1 Average Vickers hardness HV on the second imaginary line L2 L2 Ratio (HV L2 / HV L1 ) is 1.10 or more, it is determined that two high hardness regions R exist on both sides of the first virtual line L1.
[0070] It is advisable to use a micro Vickers hardness tester to measure the Vickers hardness HV. The Vickers hardness HV is measured in accordance with the micro Vickers hardness test in JIS Z 2244:2009. The test force (F) is 0.098N (HV0.01).
[0071] In addition, the Vickers hardness HV m As shown in Fig. 5, a virtual line Lm connecting the inner surface and the outer surface of the bent portion is set along the thickness direction of the plate portion 4a at a position t mm from the plate end of the bent product 4, and the Vickers hardness HV is measured at least at three points on the virtual line Lm. The average of the measured values is taken as the Vickers hardness HV of the plate portion 4a. m Here, t is the plate thickness of the plate portion 4a. The interval between the measurement positions on the imaginary line Lm is, for example, 100 μm.
[0072] The material for the bent product 4 is preferably a ferritic-austenitic duplex stainless steel sheet having a 0.2% proof stress of 300 MPa or more, preferably 450 MPa or more, a yield ratio of 0.90 or less, preferably 0.50 to 0.90, and a sheet thickness t of 6.0 mm or less.
[0073] An example of such a stainless steel sheet is a ferritic-austenitic duplex stainless steel sheet having a chemical composition, in mass%, of C: 0.050% or less, Si: 2.00% or less, Mn: 1.00 to 8.00%, P: 0.050% or less, S: 0.0500% or less, Ni: 0.10 to 6.00%, Cr: 17.00 to 25.00%, Mo: 0.10 to 2.50%, Cu: 0.10 to 3.00%, N: 0.080 to 0.300%, with the balance being Fe and impurities.
[0074] Moreover, the above stainless steel sheet may further contain, in mass %, one or more of Sn: 0.01 to 1.00%, W: 0.01 to 1.00%, and V: 0.01 to 1.00%, instead of a portion of Fe. Furthermore, the above stainless steel sheet may contain, in place of a portion of Fe, one or more of the following, by mass%, Ca: 0.0050% or less, Mg: 0.0050% or less, Al: 0.50% or less, and rare earth elements: 0.50% or less. Furthermore, the above stainless steel sheet may further contain, in mass %, Nb: 0.100% or less in place of a portion of Fe.
[0075] In order to ensure the corrosion resistance of the steel sheet, the C content may be 0.050% or less, preferably 0.040% or less. On the other hand, since C is an element that forms austenite that constitutes a dual-phase structure, the C content may be preferably 0.005% or more, more preferably 0.010% or more.
[0076] For deoxidation, the Si content is preferably 0.01% or more, more preferably 0.10% or more, and even more preferably 0.30% or more. Since the Si content exceeding 2.00% promotes the precipitation of the σ phase, the Si content is preferably 2.00% or less, and more preferably 0.60% or less.
[0077] Mn is a deoxidizing agent and an austenite stabilizing element for forming a dual-phase structure, and should be contained in an amount of 1.00% or more, preferably 1.30% or more, and more preferably 2.00% or more. On the other hand, if the Mn content exceeds 8.00%, the corrosion resistance deteriorates, so the Mn content should be 8.00% or less, preferably 5.00% or less, and more preferably 4.00% or less.
[0078] Since P deteriorates hot workability and toughness, the P content is limited to 0.050% or less, and preferably 0.035% or less. On the other hand, since an excessive reduction in the P content increases refining costs, it may be set to 0.005% or more.
[0079] Since S deteriorates hot workability, toughness, and corrosion resistance, the S content is limited to 0.0500% or less, preferably 0.0100% or less, and more preferably 0.0040% or less. On the other hand, if the S content is excessively reduced, the raw material cost and refining cost will increase, so it may be set to 0.0003% or more.
[0080] When Ni is contained in the coating of the steel sheet, it has the effect of suppressing the occurrence of pitting corrosion when the Fe concentration of the coating is high, and the effect of suppressing the progression of corrosion when corrosion occurs. On the other hand, if the Ni content is excessive, the Cr content of the coating is too low, and sufficient corrosion resistance cannot be obtained. Therefore, it is preferable to set the Ni content in the range of 0.10 to 6.00%. The lower limit of the Ni content is preferably 0.30% or more, 0.50% or more, or may be 1.00% or more. The upper limit of the Ni content is preferably 5.50% or less, 4.00% or less, or 3.00% or less.
[0081] In order to impart sufficient corrosion resistance to the steel, the Cr content is preferably in the range of 17.00 to 25.00%. The lower limit of the Cr content is preferably 17.50% or more, more preferably 20.00% or more, and further preferably 21.00% or more. The upper limit of the Cr content is preferably 24.00% or less, and more preferably 22.00% or less.
[0082] Mo is an element that improves corrosion resistance, and is effective when contained at 0.10% or more. Mo may be contained up to 2.50%, but if the Mo content exceeds 2.50%, σ phase is likely to precipitate during hot working. Therefore, the lower limit of the Mo content is 0.10% or more, preferably 0.20% or more, and more preferably 0.30% or more. The upper limit of the Mo content is 2.50% or less, preferably 2.00% or less, and more preferably 1.50% or less.
[0083] When 0.10% or more of Cu is contained, the effect of suppressing the progress of corrosion when corrosion occurs is obtained. Cu may be contained in an amount of 3.00% or less. Furthermore, when the Cu amount exceeds 3.00%, cracks may easily occur during casting. Therefore, the lower limit of the Cu amount is 0.10% or more, preferably 0.30% or more, and more preferably 0.50% or more. The upper limit of the Cu amount is 3.00% or less, preferably 2.50% or less, and more preferably 2.00% or less.
[0084] N is an element that significantly improves corrosion resistance and increases the amount of austenite phase, and is preferably contained at 0.080% or more as an austenite stabilizing element. The lower limit of the N content is preferably 0.120% or more, and more preferably 0.150% or more. On the other hand, if the N content is excessive, nitrides are formed in the steel, which reduces the corrosion resistance and toughness, so the upper limit of the N content should be 0.300% or less. The upper limit of the N content is preferably 0.250% or less.
[0085] Furthermore, when a small amount of Sn is contained, the corrosion resistance is improved. Therefore, Sn is an element useful for improving the corrosion resistance, and may be contained within a range that does not impair the low cost. If the Sn content is less than 0.001%, the effect of improving the corrosion resistance is not realized, and if the Sn content exceeds 1.00%, the cost increase becomes apparent and the workability is also reduced, so the appropriate range of the Sn content is 0.001 to 1.00%. The lower limit of the Sn content is preferably 0.01% or more, and the upper limit of the Sn content is preferably 0.50% or less. Note that Sn is an optional element and may not be contained. In other words, the Sn content may be 0%.
[0086] V and W may be contained as necessary to improve corrosion resistance, particularly crevice corrosion resistance. However, excessive inclusion of V or W reduces workability and saturates the effect of improving corrosion resistance, so the lower limit of each of the amounts of V and W is set to 0.01% or more, and the upper limit of each of the amounts of V and W is set to 1.00% or less. The lower limit of each of the amounts of V and W is preferably 0.04% or more, and the upper limit of each of the amounts of V and W is preferably 0.50% or less. Note that V and W are optional elements and may not be contained. In other words, the V amount and the W amount may each be 0%.
[0087] Ca, Mg, and REM are elements that improve hot workability, and for that purpose, one or more of Ca, Mg, and REM may be contained. Since the effects of Ca and Mg are manifested at an amount of 0.0002% or more, the lower limit of each of the amounts of Ca and Mg is set to 0.0002% or more. In the case of REM, the lower limit is set to 0.001% or more. Note that Ca, Mg, and REM are optional elements and do not need to be contained. In other words, the amount of Ca, the amount of Mg, and the amount of REM may each be 0%.
[0088] However, since excessive content of either element adversely reduces hot workability, it is preferable to set the upper and lower limits of their contents as follows: the amounts of Ca and Mg are each 0.0002-0.0050%, and the amount of REM is 0.001-0.50%.
[0089] The lower limit of each of the Ca and Mg contents is preferably 0.0005% or more. The upper limit of each of the Ca and Mg contents is preferably 0.0025% or less. The lower limit of the REM content is preferably 0.005% or more, and the upper limit of the REM content is preferably 0.30% or less.
[0090] Here, rare earth elements (REM) refer to the two elements scandium (Sc) and yttrium (Y) and the 15 elements (lanthanoids) from lanthanum (La) to lutetium (Lu) according to the general definition. They may be contained alone or as a mixture. The amount of REM is the total amount of these elements.
[0091] Al is useful as a deoxidizing element, but should not be contained in large amounts because it deteriorates workability. It is preferable to limit the upper limit of the Al content to 0.50% or less. The preferred range of the Al content is 0.30% or less. The lower limit of the Al content is 0.01% or more. Note that Al is an optional element and does not need to be contained. In other words, the Al content may be 0%.
[0092] Nb has a strong affinity with N and forms nitrides preferentially over chromium, thereby suppressing the decrease in the amount of chromium in the material and improving corrosion resistance. For this reason, it may be contained as necessary. However, if Nb is contained in excess, toughness will decrease, so the Nb content is set to 0.100% or less, and may be 0.060% or less. On the other hand, in order to obtain the above effect, the Nb content is preferably 0.005% or more, more preferably 0.010% or more, and more preferably 0.020% or more. Note that Nb is an optional element and may not be contained. In other words, the Nb content may be 0%.
[0093] The balance other than the above-mentioned elements is Fe and impurities. In addition to the above-mentioned elements, other elements may be contained within a range that does not impair the effects of this embodiment.
[0094] As described above, according to the bent product 4 of the present invention, the radius of curvature Rout of the convex curved surface 4c on the outer side of the bent portion 4b is a radius of a length equivalent to or less than the plate thickness t of the plate portion 4a, so that the radius of curvature Rout of the convex curved surface 4c on the outer side of the bent portion can be made small and sharp. In addition, since the minimum thickness of the bent portion 4b is 0.75 times or more the plate thickness t of the plate portion, the strength of the bent portion 4b can be made sufficient.
[0095] In addition, the bent product 4 of this embodiment has a recess 4d along the longitudinal direction of the bent portion 4b, and a concave curved surface 4e is provided inside the recess 4d. The recess 4d is an indentation formed by the protrusion 1c of the punch 1 during die bending. By providing such an indentation, the bent portion 4b of the bent product 4 is in a state in which compressive residual stress is imparted in the thickness direction of the bent portion 4b. Therefore, according to this embodiment, the springback caused by the relationship between the conventional compressive residual stress and the tensile residual stress is reduced, and the springback can be reduced. In addition, since a part of the inner surface of the recess 4d is the concave curved surface 4e, the occurrence of cracks originating from the recess 4d can also be prevented.
[0096] Furthermore, according to the bent product 4b of this embodiment, on both sides of a first imaginary line L1 connecting the apex of the convex curved surface 4c on the outside of the bend and the apex of the concave curved surface 4e of the concave portion 4d, the average Vickers hardness HV L1 Average Vickers hardness HV greater than L2 and satisfies the above formulas (1) and (2). In this way, the bent portion 4b of the bent product 4 has two high hardness regions with a relatively large Vickers hardness HV, and therefore has excellent buckling resistance. Furthermore, by satisfying formula (2), it is possible to impart sufficient strength to the bent portion 4b, even though the thickness of the bent portion 4b is smaller than the plate thickness of the plate portion due to the provision of the recess 4d in the bent portion 4b.
[0097] Furthermore, according to the bent product 4 of this embodiment, the overall length of the plate portion 4a is 1 mm or more, and the bent portion 4 extends along the overall length of the plate portion, so that the product can be suitably used as an exterior or interior building material for construction, particularly as a component for use in areas that are easily visible, such as window frames and curtain walls.
[0098] Furthermore, by using stainless steel having the above-mentioned chemical composition as the material for the bent product 4, the bent product 4 of this embodiment has excellent strength and corrosion resistance and can be suitably used as an exterior building material and an interior building material.
[0099] According to the bending method of the present embodiment, when the blank 3 is bent using the punch 1 and the die 2, the punch 1 having the protrusion 1c at the tip and the die 2 having the V-shaped groove-shaped die recess 2a with the bottom having the concave curved surface 2b are used, and by pressing at least a part of the protrusion 1c of the punch 1 into the blank 3, the blank 3 is pressed into the bottom of the die recess 2a, so that the material flows into the bottom of the die recess 2a. In addition, since the curvature radius Rd of the concave curved surface 2b at the bottom of the die recess 2a is a length equivalent to 60% or less of the sheet thickness t of the blank 3, the curvature radius Rout of the convex curved surface 4c on the outer side of the bent portion 4b is reduced. Furthermore, by pressing the protrusion 1c into the blank 3, the distribution state of the residual stress in the bent portion 2b is made different from the distribution state of the residual stress in the bent portion when the blank 3 is bent using a punch without a protrusion. In conventional die bending processing, springback is thought to occur due to tensile residual stress on the outside of the bend and compressive residual stress on the inside of the bend. However, in this embodiment, the residual stress distribution in the bent portion 4b is changed compared to the conventional method, thereby reducing springback after die bending processing.
[0100] Furthermore, according to the bending method of this embodiment, by forming the tip surface of the protrusion 1c of the punch 1 into a convex curved surface 1e with a predetermined radius of curvature and setting the length H of the protrusion 1c to a predetermined length, it is possible to manufacture a bent product 4 having two high hardness regions R on both sides of a first imaginary line L1 connecting the tip of the convex curved surface 4c on the outside of the bend and the tip of the concave curved surface 4e of the concave portion 4d. Such a bent product 4 has excellent buckling resistance.
[0101] Therefore, according to this embodiment, by using a metal plate material satisfying the requirements of 0.2% proof stress of 300 MPa or more, a yield ratio of 0.90 or less, and a plate thickness of 6.0 mm or less, springback can be suppressed, and a bent product having excellent resistance to buckling deformation can be manufactured without fear of insufficient strength in the bent portion. Also, according to the bending method of the present invention, the radius of curvature of the convex curved surface on the outer side of the bent portion can be made small to form a sharp shape.
[0102] The bending die K of this embodiment includes a punch 1 having a protrusion 1c at the tip of the punch, and a die 2 having a V-groove-shaped die recess 2a with a concave curved surface 2e at the bottom. By using this die K when bending a material 3 made of a metal plate material that satisfies the following requirements: 0.2% proof stress of 300 MPa or more, a yield ratio of 0.90 or less, and a plate thickness of 6.0 mm or less, it is possible to stably produce a bent product 4 with high dimensional accuracy and excellent buckling resistance. EXAMPLES
[0103] A ferritic-austenitic duplex stainless steel sheet was prepared having the chemical composition shown in Table 1 and the sheet thickness t shown in Table 2A. The mechanical properties of the ferritic-austenitic duplex stainless steel sheet were as shown in Table 1. The metal sheet material consisting of the ferritic-austenitic duplex stainless steel sheet was cut into a size of 100 mm in length and 30 mm in width to prepare the material. In Table 1, YS means yield strength, TS means tensile strength, and T.El means total elongation, and 0.2 proof stress is shown as yield strength (YS).
[0104] Also, a die having a punch and a die as shown in FIG. 1A was prepared. The punch used had a protrusion having a convex curved surface and a side wall surface connected to the convex curved surface. The relative angle θp of the punch type surface of the punch was 90°. The width of the punch was 80 mm, and the length (length in the depth direction of FIG. 1A) was 1000 mm. The width of the die recess was 80 mm, and the length (length in the depth direction of FIG. 1A) was 1000 mm.
[0105] The punch and die were then attached to a press molding machine, and the material was placed between the punch and die as shown in FIG. 2. At this time, the material was placed so that the length direction of the material coincided with the depth direction of FIG. 2. The center of the material in the width direction was also aligned with the center of the die. The press molding machine was then operated to move the punch and die closer to each other until they were in close contact with the material, thereby V-bending the material to form a bent portion. In this manner, a bent product having a bent portion was manufactured.
[0106] The bending angle θ at the bent part was measured for the obtained bent product. The bending angle θ was measured by setting four measurement points at 1 cm intervals along the longitudinal direction of the bent part, and the bending angle θ at each measurement point was measured on the inside of the bent part. The average value of the bending angle θ at the four measurement points was then calculated. Δθ (= θ-θp) was calculated from the average value of the obtained bending angle θ and the relative angle θp (= 90 °) of the punch mold surface. Δθ is the angle change amount of the bent product with respect to the bending punch, and it indicates that springback has occurred when Δθ > 0, and spring-go has occurred when Δθ < 0. Since it is desirable that the absolute value of Δθ is small from the viewpoint of shape freezing, the range in which Δθ is -1.5 / t or more and 1.5 / t or less was passed. More specifically, when Δθ is 0 or more and 1.5 / t or less, the springback was evaluated as good, and when Δθ is less than 0 and -1.5 / t or more, the spring-go was evaluated as good. In addition, since the likelihood of springback or spring-go occurring and the absolute value of the angle change Δθ of the bent product relative to the bending punch vary depending on the plate thickness t, the plate thickness t is taken into consideration and a pass range of Δθ is set to be between -1.5 / t and 1.5 / t. The results are shown in Table 2B.
[0107] The obtained bent product was checked for the presence or absence of high hardness regions by the method described in the embodiment. When the difference between the average hardness on the second virtual line L2 and the average hardness on the first virtual line L1 was 50 or more in Vickers hardness HV0.01, it was determined that there were two high hardness regions R on both sides of the first virtual line L1. When two high hardness regions R were confirmed on both sides of the first virtual line L1, it was marked as "○", and otherwise it was marked as "×". "○" was determined to be acceptable.
[0108] Furthermore, the moldability was judged. If the molding load of the press molding machine was 250 tons or less, which is the equipment specification, it was marked as "Good", and if it exceeded 250 tons and the machine stopped midway through molding, it was marked as "Poor". A "Good" was considered a pass.
[0109] In addition, the bent portion of the bent product was observed to check for the presence or absence of cracks.
[0110] The maximum stress was evaluated by carrying out a compression test on the bent product. Specifically, the bent product was cut to a total length of 150 mm and a plate width of 40 mm to prepare a test specimen. The test specimen was placed between the upper and lower plates so that the ridgeline of the bent part of the test specimen was parallel to the compression axis. A compressive load was then applied to the test specimen by moving the upper and lower plates closer to each other at a test speed of 1 mm / min. Compression was continued up to a strain range exceeding the maximum load point, and the compressive stress (N / mm 2 The change in compressive stress (N / mm 2 ) was set as the maximum stress. The maximum stress was 660N / mm 2 If the result was more than this, it was considered a pass.
[0111] As shown in Tables 2A to 2C, inventive examples A1 to A12, die bending was performed under conditions that satisfied the range of the present invention. As a result, the obtained bent product had a radius of curvature Rout of the convex curved surface on the outside of the bent portion that was less than the thickness t of the plate portion, a minimum thickness tm of the bent portion that was 0.75 times or more the thickness t of the plate portion, and an angle change Δθ of the bent product relative to the bending punch that satisfied the range of -1.5 / t to 1.5 / t. Furthermore, two high hardness regions R were confirmed on both sides of the first virtual line L1, and furthermore, HV L2 / HV L1 and HV L2 / HV m Therefore, in the bent products of the invention examples A1 to A12, spring back and spring go were suppressed, there was no risk of insufficient strength in the bent portion, the shape of the outside of the bent portion was sharp, and the buckling resistance was also good.
[0112] On the other hand, as shown in Tables 2A to 2C, in Comparative Example B1, the radius of curvature Rp of the tip surface of the protrusion of the punch was more than 100% of the sheet thickness t of the material, so the forming load was large and forming was insufficient. As a result, the radius of curvature Rout of the convex curved surface on the outside of the bent part exceeded the sheet thickness t, and a sharp shape was not obtained.
[0113] In comparative example B2, the radius of curvature Rp of the tip surface of the protrusion of the punch was less than 50% of the thickness of the material, so the radius of curvature Rq of the concave curved surface of the recess of the bent portion was less than 50%, resulting in a small compressive stress in the bent portion and large springback.
[0114] In Comparative Example B3, the length of the protruding portion of the punch was 30% or more of the plate thickness of the material, so that the forming load became large and forming became difficult.
[0115] In Comparative Example B4, the length of the punch protrusion was less than 10% of the plate thickness of the material, so the material flow during processing was insufficient, and as a result, the outer curvature radius Rout of the bent part exceeded the plate thickness, making it impossible to obtain a sharp shape. In addition, the springback was large.
[0116] In Comparative Example B5, the length H of the protrusion of the punch was 30% or more of the plate thickness t of the material, so the depth D of the recess was excessively large. L2 / HV L1 The maximum stress was small and the formation of high hardness regions R was not observed, resulting in a decrease in the maximum stress and a decrease in buckling resistance.
[0117] In Comparative Example B6, the 0.2% yield strength of the material is less than 300 MPa, and HV L2 / HV L1 and HV L2 / HV m Since this was outside the scope of the invention, the maximum stress was small and the buckling resistance was reduced.
[0118] In Comparative Example B7, a stainless steel plate was prepared by forming a V-shaped groove half the plate thickness along the ridge line that was to become the bent portion, and this plate was then formed using a punch without a protrusion. In Comparative Example B7, the accumulation of strain in the bent portion was insufficient, resulting in the HV L2 / HV L1 The hardness was small and no high hardness region R was formed. L2 / HV m Since this was outside the scope of the invention, the buckling resistance was reduced and cracks occurred during the compression test.
[0119] [Table 1]
[0120] [Table 2A]
[0121] [Table 2B]
[0122] [Table 2C] [Explanation of symbols]
[0123] 1... punch, 1a... punch tip, 1b... punch die surface, 1c... protrusion, 1e... tip surface of protrusion, 2... die, 2A... die block, 2a... die recess, 2c... die concave surface, 2d... bottom, 3... material, 4... bent product (bent product made of metal plate), 4a... plate material portion, 4b... bent portion, 4c... bent outer convex surface of bent portion, 4d... bent portion, 4e... concave surface of recess, D: depth of the recess; H: length of the protrusion; Rd: radius of curvature of the concave surface of the die; Rp: radius of curvature of the convex surface of the protrusion; Rq: radius of curvature of the concave surface of the recess; t: plate thickness; L1: first virtual line; L2: second virtual line; R: high hardness region.
Claims
1. A plate portion made of a metal plate material satisfying the following requirements: 0.2% proof stress is 300 MPa or more, a yield ratio is 0.90 or less, and a plate thickness is 6.0 mm or less; and a bending portion provided on the plate portion, The radius of curvature of the convex curved surface on the outer side of the bent portion is a radius of a length equivalent to the plate thickness of the plate portion, The minimum thickness of the bent portion is 0.75 times or more the plate thickness t of the plate portion, A recess is provided on the inner side of the bent portion along the longitudinal direction of the bent portion, The recess has a depth equivalent to a length of 10% or more and less than 30% of the plate thickness of the plate portion, and a concave curved surface having a curvature radius equivalent to a length of more than 50% and less than 100% of the plate thickness of the plate portion is provided at the bottom, On both sides of a first imaginary line L1 connecting the apex of the convex curved surface on the outer side of the bend and the apex of the concave curved surface of the concave portion, L1 Average Vickers hardness HV greater than L2 There is a high hardness region showing A bent product that satisfies the following formula (1) and the following formula (2): 1.10≦(HV L2 / HV L1 ) ≦1.30…(1) 1.20≦(HV L2 / HV m ) < 1.50 ... (2) However, HV in formula (1) L1 is the average Vickers hardness on the first virtual line L1, and HV in formulas (1) and (2) L2 is the average Vickers hardness on a second imaginary line L2 that connects the outer surface of the bent portion and the inner surface of the recess and passes through the high hardness region, and HV in formula (2) m is the Vickers hardness of the plate portion.
2. 2. The bent product according to claim 1, wherein the plate portion has a total length of 1 m or more, and the bent portion extends along the total length of the plate portion.
3. The metal plate material has a 0.2% proof stress of 450 MPa or more and a yield ratio of 0.50 to 0.90, Its chemical composition is in mass percent: C: 0.050% or less, Si: 2.00% or less, Mn: 1.00-8.00%, P: 0.050% or less, S: 0.0500% or less, Ni: 0.10-6.00%, Cr: 17.00-25.00%, Mo: 0.10-2.50%, Cu: 0.10-3.00%, N: 0.080 to 0.300%; 3. The bent product according to claim 1, wherein the balance is a ferritic-austenitic duplex stainless steel plate consisting of Fe and impurities.
4. The bent product according to claim 3, wherein the metal plate further contains, in mass %, one or more of the following group A, group B or group C in place of a portion of Fe: (Group A) One or more of Sn: 0.01 to 1.00% or less, W: 0.01 to 1.00%, V: 0.01 to 1.00%. (Group B) One or more of the following: Ca: 0.0050% or less, Mg: 0.0050% or less, Al: 0.50% or less, rare earth elements: 0.50% or less. (Group C) Nb: 0.100% or less
5. a placement step of placing a blank made of a metal plate between the punch and the die; a forming step of bending the blank by bringing the punch and the die closer to each other, The material is a metal plate material satisfying the following requirements: 0.2% proof stress is 300 MPa or more, a yield ratio is 0.90 or less, and a plate thickness is 6.0 mm or less; the punch comprises a pair of punch type surfaces approaching each other toward the punch tip, and a protrusion provided at the punch tip, the tip surface of the protrusion is a convex curved surface with a radius of curvature corresponding to a length of more than 50% and not more than 100% of the plate thickness of the material, and the length of the protrusion is a length corresponding to 10% or more and less than 30% of the plate thickness of the material, the die is provided with a V-groove-shaped die recess corresponding to the pair of punch type surfaces, and a bottom of the die recess is provided with a concave curved surface with a radius of curvature corresponding to a length of 20% or more and not more than 60% of the plate thickness of the material, The forming step is a step of bringing the punch and the die close to each other so that the punch and the die are in close contact with the material, and pressing at least a portion of the protrusion of the punch into the material.
6. The total length of the material made of the metal plate material is 1 m or more, The bending method according to claim 5 , wherein in the arranging step, the metal plate is arranged so that a full length direction of the metal plate is aligned with a longitudinal direction of the V-groove-shaped die recess.
7. A die for bending a material made of a metal plate material having a 0.2% proof stress of 300 MPa or more, a yield ratio of 0.90 or less, and a plate thickness of 6.0 mm or less, A punch including a pair of punch die faces approaching each other toward a tip of the punch and a protrusion provided at the tip of the punch; A die including a die block having a V-groove-shaped die recess corresponding to the pair of punch faces, The tip surface of the protrusion is a convex curved surface having a radius of curvature corresponding to a length of more than 50% and not more than 100% of the plate thickness of the material, and the length of the protrusion is a length corresponding to 10% or more and less than 30% of the plate thickness of the material, A bending die, wherein a bottom of the V-groove-shaped recess is provided with a concave curved surface having a radius of curvature corresponding to a length of 20% to 60% of the plate thickness of the material.
Citation Information
Patent Citations
Manufacture of angle material
JP1991161127A
Metal plate bending method, metal mold for metal plate bending and bent article comprised of metal plate
JP2022182994A
JP1972025266U
Austenitic stainless steel sheet for bending