Laminate

The laminate structure with a urethane resin surface layer, ultraviolet absorber, and polyester resin base layer addresses the issues of weather resistance and flexibility in metal-like decorative sheets, providing a durable mirror-like appearance.

JP2024145722APending Publication Date: 2024-10-15NIPPON CARBIDE KOGYO KK
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023058201
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing metal-like decorative sheets and metal vapor-deposited laminates for materials lack sufficient weather resistance and flexibility, and the addition of ultraviolet absorbers to improve weather resistance can compromise the mirror-like appearance.

Method used

A laminate structure comprising a surface layer with a urethane resin and ultraviolet absorber, a resin layer with an ultraviolet absorber, and a base layer with a polyester resin, with specific elastic modulus and ultraviolet transmittance values, ensuring both weather resistance and mirror-like appearance.

Benefits of technology

The laminate achieves a mirror-like appearance with excellent weather resistance and flexibility, maintaining a luxurious feel and preventing deterioration over time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145722000001_ABST
    Figure 2024145722000001_ABST
Patent Text Reader

Abstract

To provide a laminate that has a mirror-like appearance and exhibits superior weather resistance and adaptability to various materials.SOLUTION: A laminate includes a surface layer, a resin layer, a substrate layer, and a metal layer in that order, the surface layer containing an urethane resin, the substrate layer containing a polyester resin, the surface layer and the resin layer each containing an ultraviolet absorber, an elastic modulus being less than 155 N / 25 mm, the surface layer having ultraviolet transmittance of less than 0.60%, and the surface layer having absorbance of 0.45 or less at 400 nm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a laminate. [Background technology]

[0002] When making the surface of various materials into a mirror finish to give them a design or a luxurious feel, it is possible to polish the surface of metal materials or to paint the surface of various materials with paint containing metal powder or glittering pigments. However, when using these methods, although a metallic appearance can be obtained, the surface of the material tends to have a dull color, and it is difficult to obtain a luxurious mirror finish.

[0003] One simple method for making the surfaces of various materials look like a mirror is to attach a metallic decorative film to the surface of the material. For example, Patent Document 1 discloses a metallic decorative sheet as a composite material having a metallic mirror-like luster, in which a metal layer, a pattern layer, and a fluorine-based resin film are laminated in this order on one side of a base film. Patent Document 2 discloses a metal vapor deposition laminate in which a metal vapor deposition layer is laminated on the surface of a substrate made of a polymer resin, and a resin layer is laminated on the opposite surface of the substrate. In Patent Document 2, the resin used is any one or more of an acrylic resin, a urethane resin, and a polyester resin. Since these metallic decorative sheets or metal vapor deposition laminates have a metal layer or a metal vapor deposition layer, by attaching them to the surface of a material, a luxurious mirror-like appearance can be obtained. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-58660 [Patent Document 2] JP 2007-216608 A Summary of the Invention [Problem to be solved by the invention]

[0005] Here, when various materials are used in, for example, buildings and vehicles, the buildings and vehicles are placed in various environments, and therefore high weather resistance is required. The metallic decorative sheet described in Patent Document 1 has high weather resistance because it uses a fluororesin film on the surface layer, but it is difficult to attach it to the surface shape of various materials because the fluororesin film is hard. On the other hand, the metal vapor deposition laminate described in Patent Document 2 has a resin layer containing a urethane resin or the like, and therefore has superior conformability compared to the metallic decorative sheet described in Patent Document 1, which uses a fluorine-based resin film as the surface layer. However, the metal vapor deposition laminate described in Patent Document 2 has insufficient weather resistance. Therefore, the present inventors added additives such as an ultraviolet absorber and a light stabilizer to the resin layer in order to improve the weather resistance of the resin layer in the metal vapor deposition laminate described in Patent Document 2. In this case, the presence of these additives reduced the transparency of the resin layer, and it was sometimes impossible to obtain a luxurious mirror-like appearance. The present disclosure has been made in consideration of the above-mentioned conventional circumstances, and has an object to provide a laminate having a mirror-like appearance and excellent weather resistance and conformability. [Means for solving the problem]

[0006] Specific means for achieving the above object are as follows. <1> The laminate includes a surface layer, a resin layer, a base layer, and a metal layer in this order, The surface layer contains a urethane resin, The base layer contains a polyester resin, The surface layer and the resin layer contain an ultraviolet absorber, The elastic modulus is less than 155N / 25mm; The ultraviolet transmittance of the surface layer is less than 0.60%, The surface layer has an absorbance at 400 nm of 0.45 or less. <2> The content of the ultraviolet absorbing agent in the surface layer is 2 parts by mass or more per 100 parts by mass of the total of the resins contained in the surface layer. <1> The laminate according to claim 1. <3> The content of the ultraviolet absorber in the resin layer is 0.3 parts by mass or more per 100 parts by mass of the total of the resins contained in the resin layer. <1> or <2> The laminate according to claim 1. <4> The resin layer contains a colorant. <1> ~ <3> 13. The laminate according to claim 12 . <5> The resin layer has a total light transmittance of 15.0% to 100%. <1> ~ <4> 13. The laminate according to claim 12 . <6> The average thickness of the base layer is 40 μm or less. <1> ~ <5> 13. The laminate according to claim 12 . <7> The metal layer comprises a metal, a metal oxide, or an alloy. <1> ~ <6> 13. The laminate according to claim 12 . <8> The average thickness of the surface layer is 50 μm or less. <1> ~ <7> 13. The laminate according to claim 12 . <9> The average thickness of the metal layer is 1 μm or less. <1> ~ <8> 13. The laminate according to claim 12 . Effect of the Invention

[0007] According to the present disclosure, it is possible to provide a laminate having a mirror-like appearance and excellent weather resistance and conformability. [Brief description of the drawings]

[0008] [Figure 1] 1 is a cross-sectional view of a laminate 1 according to a first embodiment. [Diagram 2] FIG. 4 is a cross-sectional view of a laminate 2 according to a second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, the embodiments of the present disclosure will be described in detail. However, the present disclosure is not limited to the following embodiments. In the following embodiments, the components (including element steps, etc.) are not essential unless specifically stated. The same applies to the numerical values ​​and their ranges, and do not limit the present disclosure.

[0010] In the present disclosure, the term "step" includes not only a step that is independent of other steps, but also a step that cannot be clearly distinguished from other steps as long as the purpose of the step is achieved. In the present disclosure, a numerical range indicated using "~" includes the numerical values ​​before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in the present disclosure in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value of the numerical range may be replaced with a value shown in the examples. In the present disclosure, each component may contain multiple types of corresponding substances. When multiple types of substances corresponding to each component are present in the composition, the content or amount of each component means the total content or amount of the multiple substances present in the composition, unless otherwise specified. In the present disclosure, the terms "layer" and "film" include cases where the layer or film is formed over the entire area when the area in which the layer or film is present is observed, as well as cases where the layer or film is formed over only a portion of the area. In this disclosure, the term "lamination" refers to stacking layers, where two or more layers may be bonded together or two or more layers may be removable. In the present disclosure, "(meth)acrylic" means at least one of acrylic and methacrylic. In this disclosure, the thickness of a layer or film refers to a value measured using a micrometer. In the present disclosure, the average thickness of a layer or film is a value obtained by measuring the thicknesses of any five points of the layer or film in question and calculating the arithmetic mean value of the measured thicknesses. In the present disclosure, the solid content concentration (mass %) refers to the mass ratio of components other than the solvent contained in the solution.

[0011] <Laminate> The laminate of the present disclosure comprises a surface layer, a resin layer, a base layer, and a metal layer, in this order; the surface layer contains a urethane-based resin, the base layer contains a polyester-based resin, the surface layer and the resin layer contain an ultraviolet absorber, and the elastic modulus is less than 155 N / 25 mm, the ultraviolet transmittance of the surface layer is less than 0.60%, and the absorbance at 400 nm of the surface layer is 0.45 or less. The laminate of the present disclosure has a mirror-like appearance and is excellent in weather resistance and conformability. The reason for this is not clear, but is presumed to be as follows. It is believed that the conformability of the laminate is influenced not only by the type of resin components constituting the surface layer and the base layer, but also by the elastic modulus of the entire laminate. In the laminate of the present disclosure, the surface layer contains a urethane resin, the base layer contains a polyester resin, and the elastic modulus of the entire laminate is less than 155 N / 25 mm. This is believed to have improved the conformability of the laminate. On the other hand, by including an ultraviolet absorber in the surface layer, the weather resistance of the surface layer can be improved. Furthermore, by including an ultraviolet absorber in the resin layer, the ultraviolet absorber contained in the resin layer prevents light that enters from the surface layer side and is reflected by the metal layer from reaching the surface layer again, so that it is believed that the weather resistance of the surface layer is further improved. It is also believed that the improved weather resistance of the surface layer suppresses the deterioration of the mirror-like appearance over time. Furthermore, by making the ultraviolet ray transmittance of the surface layer less than 0.60%, the weather resistance of the surface layer is further improved, and it is presumed that deterioration of the mirror-like appearance over time is suppressed. Furthermore, it is presumed that by making the absorbance of the surface layer at 400 nm 0.45 or less, the colorless transparency of the surface layer is ensured, and a mirror-like appearance is obtained.

[0012] The elastic modulus of the laminate of the present disclosure is less than 155N / 25mm, preferably 154N / 25mm or less, more preferably 153N / 25mm or less, and even more preferably 152N / 25mm or less. From the viewpoint of the handleability of the laminate, the elastic modulus of the laminate of the present disclosure is preferably 130N / 25mm or more, more preferably 133N / 25mm or more, and even more preferably 135N / 25mm or more. The elastic modulus of the laminate of the present disclosure is preferably 130N / 25mm or more and less than 155N / 25mm. The elastic modulus of the laminate is the value obtained by carrying out a tensile test on a test piece having a width of 25 mm and a length of 100 mm in an environment of 25° C. The test condition is a tensile speed of 200 mm / min. The elastic modulus of the laminate can be adjusted to fall within the desired range by adjusting the thicknesses of the surface layer, base layer, resin layer and other layers provided as necessary, as well as the components of each layer.

[0013] From the viewpoint of setting the elastic modulus of the laminate within the above desired range, the thickness of the laminate of the present disclosure is preferably 100 μm to 200 μm, more preferably 120 μm to 190 μm, and even more preferably 140 μm to 180 μm.

[0014] The laminate of the present disclosure includes a surface layer, a resin layer, a substrate layer, and a metal layer in this order, and may include other layers as necessary. Hereinafter, the laminate of the present disclosure will be described with reference to the drawings. Note that the size of the members in each drawing is conceptual, and the relative relationship of the size between the members is not limited thereto. In addition, the same reference numerals are given to members or parts having similar functions throughout all the drawings, and the description thereof may be omitted.

[0015] [First embodiment] 1 is a cross-sectional view of a laminate 1 according to a first embodiment. The laminate 1 includes a surface layer 10, an adhesive layer 40, a resin layer 50, a substrate layer 20, and a metal layer 30, in this order. Each layer will be described below.

[0016] (Surface layer 10) The surface layer 10 contains a urethane resin. The surface layer 10 also contains an ultraviolet absorbing agent from the viewpoint of weather resistance. The surface layer 10 constitutes the surface of the laminate 1 and protects the surface of the laminate 1. It is more preferable that the surface layer 10 has optical transparency from the viewpoint of fully expressing the design provided by the metal layer 30. It is also preferable that the surface layer 10 has weather resistance, particularly in the application of decorating the adherend. Furthermore, it is preferable that the surface layer 10 has sufficiently high mechanical strength from the viewpoint of increasing the tensile strength and surface hardness of the laminate 1.

[0017] The surface layer may contain a resin other than the urethane resin, such as (meth)acrylic resin, polyester resin, polycarbonate resin, polyolefin resin, vinyl chloride resin, and acrylonitrile-butadiene-styrene (ABS) resin. When the surface layer contains a resin other than a urethane-based resin, the proportion of the urethane-based resin in the resin components constituting the surface layer is preferably 50 mass% or more, more preferably 70 mass% or more, even more preferably 90 mass% or more, and particularly preferably 99 mass% or more.

[0018] The type of the ultraviolet absorbing agent contained in the surface layer is not particularly limited. Examples of the ultraviolet absorbing agent include a benzotriazole-based ultraviolet absorbing agent, a benzophenone-based ultraviolet absorbing agent, a benzoate-based ultraviolet absorbing agent, and a hydroxyphenyltriazine-based ultraviolet absorbing agent. Among these, the ultraviolet absorber is preferably a hydroxyphenyltriazine ultraviolet absorber from the viewpoint of the colorless transparency and weather resistance of the surface layer.

[0019] The surface layer may contain only one type of ultraviolet absorbing agent, or two or more types of ultraviolet absorbing agents may be used in combination. The content of the ultraviolet absorbing agent contained in the surface layer is not particularly limited. The content of the ultraviolet absorbing agent in the surface layer is preferably 2 parts by mass or more, more preferably 2.5 parts by mass or more, and even more preferably 3 parts by mass or more, based on 100 parts by mass of the resin contained in the surface layer in total, from the viewpoint of weather resistance. The content of the ultraviolet absorbing agent may be 10 parts by mass or less, based on 100 parts by mass of the resin contained in the surface layer in total, from the viewpoint of colorless transparency. The content of the ultraviolet absorbing agent is preferably 2 parts by mass to 10 parts by mass, based on 100 parts by mass of the resin contained in the surface layer in total.

[0020] From the viewpoint of improving the weather resistance of the laminate, the surface layer may contain stabilizers other than the ultraviolet absorber, such as a light stabilizer, a heat stabilizer, and a stabilization assistant. Examples of the light stabilizer include hindered amine compounds. Examples of the heat stabilizer include phosphite compounds and metal perchlorates. As the stabilizing aid, epoxy compounds such as epoxidized soybean oil, epoxidized linseed oil, bisphenol A diglycidyl ether, and hydrogenated bisphenol A diglycidyl ether, and β-diketone compounds such as benzoylacetone, dibenzoylmethane, and stearoylbenzoylmethane may be used. The content of other stabilizers in the surface layer is not particularly limited, and is preferably 1 to 7 parts by mass, more preferably 2 to 6 parts by mass, and even more preferably 3 to 5 parts by mass, relative to a total of 100 parts by mass of the resins contained in the surface layer.

[0021] The average thickness of the surface layer is set based on various conditions such as mechanical strength, optical function, and moldability. From the viewpoint of setting the elastic modulus of the laminate in a desirable range, the average thickness of the surface layer is preferably 50 μm or less, more preferably 45 μm or less, and even more preferably 40 μm or less. From the viewpoint of handling of the laminate, the average thickness of the surface layer is preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 20 μm or more. The average thickness of the surface layer is preferably 10 μm to 50 μm.

[0022] From the viewpoint of weather resistance, the ultraviolet transmittance of the surface layer is less than 0.60%, preferably 0.59% or less, and more preferably 0.58% or less. The ultraviolet transmittance of the surface layer may be 0.01% or more. The ultraviolet transmittance of the surface layer is preferably 0.01% or more and less than 0.60%. In this disclosure, ultraviolet transmittance refers to the value obtained by measuring the transmittance at wavelengths from 240 nm to 600 nm using a spectrophotometer and calculating the ultraviolet transmittance at wavelengths from 300 nm to 380 nm in accordance with JIS A5759 (2016).

[0023] From the viewpoint of colorless transparency, the absorbance of the surface layer at 400 nm is set to 0.45 or less, preferably 0.40 or less, and more preferably 0.20 or less. The absorbance of the surface layer at 400 nm may be 0.01 or more. The absorbance of the surface layer at 400 nm is preferably 0.01 to 0.45.

[0024] The surface layer may contain a matting agent in the resin so as to make the surface of the laminate matte, or the surface of the surface layer may be coated with a matting agent.

[0025] Other additives that can be added to the surface layer include a leveling agent, an antifoaming agent, an additive for preventing soiling such as a silicone resin, a slip agent, a filler, and the like.

[0026] (Base material layer 20) The base layer 20 contains a polyester resin. The base layer 20 can function as a support layer for supporting the metal layer 30. The base layer 20 is preferably substantially transparent. The term "substantially transparent" means that the laminate 1 has sufficient transparency to exhibit a metallic appearance due to the metal layer 30.

[0027] Examples of polyester-based resins constituting the base layer include polyesters such as polyethylene terephthalate (PET) and modified polyesters such as glycol-modified polyethylene terephthalate (PETG). Glycol-modified polyethylene terephthalate has a molecular structure in which a part of the structural units derived from ethylene glycol in the PET monomer is replaced with structural units derived from cyclohexanedimethanol. As the polyester-based resin, polyethylene terephthalate (PET) is preferred. The substrate layer may contain other resins besides polyester-based resins, such as (meth)acrylic resins, polyurethane resins, polycarbonate resins, polyolefin resins, vinyl chloride resins, and acrylonitrile-butadiene-styrene (ABS) resins. When the base layer contains a resin other than the polyester-based resin, the proportion of the polyester-based resin in the resin components constituting the base layer is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 90% by mass or more, and particularly preferably 99% by mass or more. The substrate layer may be made of a polyester resin, and in this case, it is more preferable that the substrate layer is made of polyethylene terephthalate (PET).

[0028] The average thickness of the base layer is set based on various conditions such as mechanical strength, optical function, and moldability. From the viewpoint of setting the elastic modulus of the laminate in a desirable range, the average thickness of the base layer is preferably 40 μm or less, more preferably 39 μm or less, and even more preferably 38 μm or less. From the viewpoint of handling of the laminate, the average thickness of the base layer is preferably 20 μm or more, more preferably 22 μm or more, and even more preferably 25 μm or more. The average thickness of the base layer is preferably 20 μm to 40 μm.

[0029] (metal layer 30) The metal layer 30 is a layer that imparts an appearance of metallic luster to the laminate 1. The metal layer 30 may usually be a thin layer of metal, and the metal can be appropriately selected within a range that exhibits metallic luster and exhibits sufficient malleability when the thin film adheres the laminate 1 to an adherend. The metal layer may comprise a metal, a metal oxide or an alloy. Specific examples of the metal contained in the metal layer include aluminum, indium, chromium, zinc, gallium, nickel, tin, silver, gold, silicon, titanium, platinum, palladium, stainless steel, and Hastelloy. Among these, the metal is preferably aluminum from the viewpoint of processability.

[0030] The metal layer 30 may be composed of a metal foil, or may be a vapor-deposited film formed on the surface of the base layer 20. The metal layer 30 is preferably a layer formed directly on the surface of the base layer 20, such as a vapor-deposited film, from the viewpoints of being able to omit a step relating to the preparation of an adhesive layer that bonds the metal layer 30 and the base layer 20 and thus reducing costs, and of suppressing an increase in the rigidity of the laminate 1 due to the adhesive layer. The metal layer can be formed on the surface of the substrate layer using known techniques such as vacuum deposition, sputtering, and chemical vapor deposition (CVD).

[0031] The average thickness of the metal layer is determined based on various conditions such as the optical effect and the expected conformability of the laminate. The average thickness of the metal layer is preferably 1 μm or less, more preferably 0.5 μm or less, and even more preferably 0.1 μm or less. The average thickness of the metal layer may be 0.01 μm or more. The average thickness of the metal layer is preferably 0.01 μm to 1 μm.

[0032] (adhesive layer 40) The adhesive layer 40 bonds the surface layer 10 and the base layer 20, which are separately prepared, via the resin layer 50 provided on the surface of the base layer 20. In this case, the adhesive layer 40 may be provided on the surface of the surface layer 10, or on the surface of the resin layer 50 in the base layer 20. In the first embodiment, when the surface layer 10 is provided directly on the surface of the resin layer 50, the adhesive layer 40 does not necessarily have to be provided.

[0033] The adhesive layer 40 is made of a resin composition. Examples of the resin composition used for the adhesive layer include a (meth)acrylic adhesive, a silicone adhesive, and a synthetic rubber adhesive. From the viewpoint of increasing the adhesion between the resin layer and the adhesive layer, a (meth)acrylic adhesive is more preferable.

[0034] The average thickness of the adhesive layer is not particularly limited, but is preferably in the range of 5 μm to 100 μm. When the average thickness of the adhesive layer is in the above range, the workability (e.g., handleability) when bonding the surface layer and the base layer, which are separately prepared, is improved.

[0035] (Resin layer 50) In the laminate 1, a resin layer 50 is provided between the surface layer 10 and the base layer 20 from the viewpoint of design. The resin layer 50 contains an ultraviolet absorbing agent from the viewpoint of weather resistance. When the resin layer 50 contains an ultraviolet absorbing agent, light that enters from the surface layer 10 side of the laminate 1 and is reflected by the metal layer 30 is attenuated by the action of the ultraviolet absorbing agent when passing through the resin layer 50. As a result, the amount of reflected light that reaches the surface layer 10 is reduced, and the weather resistance of the surface layer 10 is further improved.

[0036] The content of the ultraviolet absorbing agent in the resin layer is preferably 0.3 parts by mass or more, more preferably 0.4 parts by mass or more, and even more preferably 0.5 parts by mass or more, based on the total 100 parts by mass of the resin contained in the resin layer, from the viewpoint of transparency. The content of the ultraviolet absorbing agent is preferably 4 parts by mass or less, more preferably 3 parts by mass or less, and even more preferably 2.5 parts by mass or less, based on the total 100 parts by mass of the resin contained in the resin layer, from the viewpoint of weather resistance. The content of the ultraviolet absorbing agent is preferably 0.3 parts by mass to 4 parts by mass, based on the total 100 parts by mass of the resin contained in the resin layer. Specific examples of the ultraviolet absorbing agent contained in the resin layer are the same as those in the surface layer. Specific examples and preferred contents of other stabilizers used as necessary in the resin layer are the same as those in the surface layer.

[0037] The resin layer contains a resin. The resin contained in the resin layer is not particularly limited. Examples of the resin contained in the resin layer include polyester resin, (meth)acrylic resin, polyurethane resin, polycarbonate resin, polyolefin resin, vinyl chloride resin, acrylonitrile-butadiene-styrene (ABS) resin, etc. Among these, (meth)acrylic resin is preferred from the viewpoint of transparency. The (meth)acrylic resin may be a homopolymer consisting of structural units derived from a single (meth)acrylic monomer, or a copolymer consisting of structural units derived from two or more types of (meth)acrylic monomers. Here, the (meth)acrylic monomer means at least one of acrylic acid, derivatives of acrylic acid such as acrylic acid alkyl esters, and derivatives of methacrylic acid such as methacrylic acid alkyl esters. The derivatives of acrylic acid and the derivatives of methacrylic acid may have a substituent such as a hydroxyl group, an amino group, a carboxyl group, or a glycidyl group. In addition, the (meth)acrylic resin may contain other monomers than the (meth)acrylic monomer. The total proportion of structural units derived from monomers containing a carboxy group in the molecule, such as acrylic acid, methacrylic acid, and other monomers containing a carboxy group, in the total structural units of the (meth)acrylic resin is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less. The total proportion of structural units derived from monomers containing a carboxy group in the molecule in the total structural units of the (meth)acrylic resin may be 0.5% by mass or more. The total proportion of structural units derived from monomers containing a carboxy group in the molecule in the total structural units of the (meth)acrylic resin is preferably 0.5% by mass to 20% by mass.

[0038] The weight average molecular weight (Mw) of the (meth)acrylic resin is preferably within the range of 5,000 to 1,000,000, more preferably within the range of 10,000 to 800,000, and even more preferably within the range of 100,000 to 750,000. If the weight average molecular weight (Mw) of the (meth)acrylic resin is 5,000 or more, the resin layer tends not to become brittle. Also, if the weight average molecular weight (Mw) of the (meth)acrylic resin is 1,000,000 or less, the film-forming property tends to be excellent. When two or more types of (meth)acrylic resins are used in combination as the (meth)acrylic resin, the weight average molecular weight (Mw) of the mixture of two or more types of (meth)acrylic resins is preferably within the above range.

[0039] The weight average molecular weight (Mw) of the (meth)acrylic resin is a value measured by the following method, specifically, according to the following (1) to (3). (1) A solution of a (meth)acrylic resin is applied to a release paper and dried at 100° C. for 1 minute to obtain a film of the (meth)acrylic resin. (2) Using the (meth)acrylic resin film obtained in (1) above and tetrahydrofuran, a sample solution with a solid concentration of 0.2% by mass is obtained. (3) The weight average molecular weight of the (meth)acrylic resin is measured in terms of standard polystyrene using gel permeation chromatography (GPC) under the following conditions.

[0040] ~Conditions~ Measurement equipment: High-speed GPC [Model: HLC-8220 GPC, manufactured by Tosoh Corporation] Detector: Differential refractometer (RI) [installed in HLC-8220, manufactured by Tosoh Corporation] Column: 4 TSKgel GMHXL (Tosoh Corporation) columns Column temperature: 40°C Eluent: tetrahydrofuran Sample solution injection volume: 100μL Flow rate: 0.8mL / min

[0041] From the viewpoint of mechanical strength, the glass transition temperature Tg of the (meth)acrylic resin is preferably -20°C or higher, more preferably 0°C or higher, and even more preferably 10°C or higher. From the viewpoint of good workability of the resin film and resistance to brittleness, the glass transition temperature Tg of the (meth)acrylic resin may be 100°C or lower. The glass transition temperature Tg of the (meth)acrylic resin is preferably -20°C to 100°C. The glass transition temperature Tg of the (meth)acrylic resin refers to the value determined as the inflection point of the DSC curve obtained by measuring 10 mg of a measurement sample in a nitrogen gas flow at a heating rate of 10° C. / min using a differential scanning calorimeter (DSC) (e.g., EXSTAR6000 manufactured by Seiko Instruments Inc.). When two or more inflection points are observed in the DSC curve using the differential scanning calorimeter (DSC), the temperature at the highest inflection point is regarded as the glass transition temperature Tg of the (meth)acrylic resin.

[0042] In addition, when the structural units constituting the (meth)acrylic resin are known, the Tg of the (meth)acrylic resin may be a value obtained by converting the absolute temperature (K) calculated by the following formula into Celsius temperature (°C).

[0043]

number

[0044] In the formula, Tg1, Tg2, . . . and Tg nare the glass transition temperatures of the homopolymers of monomer 1, monomer 2, ..., and monomer n, expressed in absolute temperature (K). m1, m2, ..., and m n are the mole fractions of each monomer.

[0045] The "glass transition temperature of a homopolymer expressed in absolute temperature (K)" refers to the glass transition temperature of a homopolymer produced by polymerizing the monomer alone, expressed in absolute temperature (K). The glass transition temperature of a homopolymer can be measured by the above-mentioned method using a differential scanning calorimeter (DSC).

[0046] The "glass transition temperatures expressed as Celsius temperatures (°C) of homopolymers" of representative monomers are as follows: 10°C for methyl acrylate, -22°C for ethyl acrylate, -54°C for n-butyl acrylate, -70°C for 2-ethylhexyl acrylate, -15°C for 4-hydroxybutyl acrylate, -80°C for t-butyl acrylate, 43°C for vinyl acetate, 32°C for acrylic acid, 106°C for methyl methacrylate, and 85°C for 2-hydroxyethyl methacrylate. For example, by using these representative monomers, it is possible to appropriately adjust the above-mentioned glass transition temperatures. Regarding the "glass transition temperature when made into a homopolymer" of a monomer other than the above-mentioned monomers, the value described in Polymer Handbook (4th edition, Wiley-Interscience; the same applies hereinafter) is adopted. When there is no description in the Polymer Handbook, the glass transition temperature of the homopolymer obtained by the above-mentioned measurement method is adopted. In addition, absolute temperature (K) can be converted to Celsius temperature (℃) by subtracting 273 from absolute temperature (K), and Celsius temperature (℃) can be converted to absolute temperature (K) by adding 273 to Celsius temperature (℃).

[0047] When two or more (meth)acrylic resins are used in combination, the glass transition temperature Tg of the (meth)acrylic resin exhibiting the highest glass transition temperature Tg is preferably within the above range.

[0048] The method for producing the (meth)acrylic resin is not particularly limited, and the resin can be produced by polymerizing monomers by a method such as solution polymerization, emulsion polymerization, suspension polymerization, etc. In addition, when preparing a resin composition after the production of the (meth)acrylic resin, solution polymerization is preferred because the treatment process is relatively simple and can be carried out in a short time.

[0049] The (meth)acrylic resin may be a commercially available product. Examples of commercially available (meth)acrylic resins include KP-1876E (product name: Nissetsu (registered trademark), manufactured by Nippon Carbide Industries Co., Ltd.) and H-4002 (manufactured by Negami Chemical Industries Co., Ltd.).

[0050] The resin layer may contain a colorant in order to adjust the color of the laminate. Examples of colorants contained in the resin layer include organic pigments, inorganic pigments, and organic dyes. Among these, weather-resistant colorants are preferred, and specifically, they can be selected from colorants listed in COLOUR INDEX 3RD EDITION (Second Revision) (1982) and SUPPLEMENT (1982) published by THE SOCIETY OF DYERS AND COLOURISTS. The colorant may be any color tone, such as yellow, orange, red, purple, blue, green, brown, black, and white. In addition to the above pigments, mica and aluminum powder may be contained within a range that does not affect the light transmittance and weather resistance of the resin layer.

[0051] As the colorant, it is preferable to use a color base that is commercially available in the form of a pigment dispersed in a resin. Polyester plasticizer-based color bases, (meth)acrylic resin-based color bases, vinyl acetate resin-based color bases, cellulose resin-based color bases, etc. can be used.

[0052] When the resin layer contains a colorant, the content of the colorant in the resin layer is, from the viewpoint of adjusting the total light transmittance of the resin layer within a predetermined range, preferably 10 parts by mass or less, more preferably 7.5 parts by mass or less, and even more preferably 5 parts by mass or less, per 100 parts by mass of the total resin contained in the resin layer.

[0053] From the viewpoint of transparency, the total light transmittance of the resin layer is preferably from 15.0% to 100%, more preferably from 50.0% to 100%, and even more preferably from 75.0% to 100%. In the present disclosure, the total light transmittance refers to a value measured based on JIS K7361-1 (1997).

[0054] The resin layer may contain additives for the purpose of preventing stains, such as a leveling agent, an antifoaming agent, a silicone resin, a slip agent, etc., as required.

[0055] The average thickness of the resin layer is set based on various conditions such as mechanical strength, optical function, and moldability. From the viewpoint of setting the elastic modulus of the laminate in a desirable range, the average thickness of the resin layer is preferably 50 μm or less, more preferably 45 μm or less, and even more preferably 40 μm or less. From the viewpoint of handling of the laminate, the average thickness of the resin layer is preferably 15 μm or more, more preferably 20 μm or more, and even more preferably 25 μm or more. The average thickness of the resin layer is preferably 15 μm to 50 μm.

[0056] [Second embodiment] 2 is a cross-sectional view of a laminate 2 according to a second embodiment. The laminate 2 includes a surface layer 10, a first adhesive layer 42, a resin layer 50, a base layer 20, a metal layer 30, a primer layer 60, and a second adhesive layer 44, in this order. In the laminate 2, the details of the surface layer 10, the base layer 20, the metal layer 30, and the resin layer 50 are similar to those in the laminate 1, and therefore will not be described again. In the laminate 2, the details of the first adhesive layer 42 are similar to those of the adhesive layer 40, and therefore a description thereof will be omitted.

[0057] (Primer layer 60) The primer layer 60 is provided to improve adhesion between the metal layer 30 and the second adhesive layer 44 . The primer layer may be formed from a primer layer composition containing, for example, a urethane resin and a (meth)acrylic resin. In particular, the urethane resin contained in the primer layer is preferably an aqueous urethane resin from the viewpoint of not corroding the second adhesive layer. Examples of the aqueous urethane resin include self-emulsifying urethane resin, forced emulsifying urethane resin, and water-soluble urethane resin. The self-emulsifying urethane resin is an aqueous urethane resin in which the molecular structure of the urethane resin has hydrophilic groups such as anionic and nonionic groups, and the urethane resin is emulsified and dispersed in an aqueous system by these hydrophilic groups. The forced emulsifying urethane resin is an aqueous urethane resin in which the urethane resin or urethane prepolymer is emulsified and dispersed in an aqueous system by surfactants such as anionic surfactants and nonionic surfactants. Examples of such urethane resins include Takelac (registered trademark) WS series (manufactured by Mitsui Chemicals).

[0058] The primer layer may further contain a crosslinking agent, silica powder, a coloring agent, and the like.

[0059] The average thickness of the primer layer is preferably 0.1 μm or more, more preferably 0.5 μm or more, from the viewpoint of increasing the adhesion between the metal layer and the second adhesive layer. Also, the average thickness of the primer layer is preferably 6 μm or less, more preferably 4 μm or less, from the viewpoint of transparency. The average thickness of the primer layer is preferably 0.1 μm to 6 μm.

[0060] (Second adhesive layer 44) The second adhesive layer 44 is provided for attaching the laminate 2 to an adherend. The components constituting the second adhesive layer are the same as those of the adhesive layer. The average thickness of the second adhesive layer is not particularly limited, but is preferably in the range of 5 μm to 100 μm. If the average thickness of the second adhesive layer is in the above range, the workability (e.g., handleability) when attaching the laminate to an adherend is improved.

[0061] [Method of manufacturing laminate] The laminate of the present disclosure can be manufactured by a method capable of realizing the above-mentioned layer structure, and such a method can be realized by utilizing a known method for manufacturing a laminate. The manufacturing method of the laminate will be described below by taking the laminate 1 shown in Fig. 1 and the laminate 2 shown in Fig. 2 as examples. For example, the laminate 1 can be manufactured by laminating two laminates. That is, a metal layer 30 is formed on one surface of a base layer 20, for example, by vacuum deposition, and a resin composition constituting a resin layer 50 is applied to the other surface of the base layer 20, dried, and if necessary, subjected to a treatment such as heating, to prepare a first laminate. Next, an adhesive layer 40 is formed on one surface of a surface layer 10 to prepare a second laminate. The surface of the first laminate facing the resin layer 50 and the surface of the second laminate facing the adhesive layer 40 may be brought into contact with each other and pressure-bonded to integrate the two, thereby obtaining the laminate 1. When forming the adhesive layer 40, a resin composition for forming the adhesive layer may be applied onto a temporary support, dried, and heated, if necessary, to form the adhesive layer 40 on the temporary support, and then the obtained adhesive layer 40 may be brought into contact with one surface of the surface layer 10 and pressed to integrate the two, and then the temporary support may be removed to form the adhesive layer 40 on one surface of the surface layer 10. The laminate 2 can be produced by applying a primer layer composition to the surface of the metal layer 30 in the laminate 1, drying it, and, if necessary, heating it to form a primer layer 60 on the metal layer 30, and then forming the second adhesive layer 44 on the primer layer 60. When forming the second adhesive layer 44, the method using the temporary support described above can also be applied. It should be noted that the method for producing the laminate of the present disclosure is not limited to the above method.

[0062] [Applications of laminates] The laminate of the present disclosure is preferably used as a building material for improving the design of the surface of an adherend. Examples of the adherend include surface materials such as sliding doors, doors, kitchen doors, and washroom storage doors, bottom plates of kitchen storage interiors and washroom storage interiors, and sashes. In addition to building materials, the laminate of the present disclosure can be applied to emblems, badges, badges, stickers, seals, labels, nameplates, ribbons, etc. that are attached to the exterior parts of vehicles such as automobiles and the surface of objects installed outdoors. The method of attaching the laminate to the surface of the adherend is not particularly limited. When an adhesive layer is provided on the surface of the laminate opposite to the surface layer, the surface of the adhesive layer may be brought into contact with the surface of the adherend. When an adhesive layer is not provided on the surface of the laminate opposite to the surface layer, an adhesive may be applied to the portion of the surface of the adherend where the laminate is to be attached, and then the surface of the laminate opposite to the surface layer may be brought into contact with the surface of the adherend. EXAMPLES

[0063] The present disclosure will be described in more detail below based on examples, but the present disclosure is not limited to these examples.

[0064] (Synthesis of acrylic copolymer A) In a reaction vessel of a reaction apparatus equipped with a stirrer, a reflux condenser, a successive dropping device, and a thermometer, 70 parts by mass of ethyl acetate was charged. In addition, 100.0 parts by mass of a monomer mixture consisting of 62.5 parts by mass of methyl methacrylate, 29.5 parts by mass of ethyl acrylate, 7.0 parts by mass of 2-hydroxyethyl methacrylate, and 1.0 part by mass of acrylic acid was prepared in a separate vessel. 20.0 parts by mass of this prepared monomer mixture was charged into the reaction vessel, and then heated and refluxed at the reflux temperature for 10 minutes. Next, under reflux temperature conditions, the remaining 80.0 parts by mass of the monomer mixture, 50.0 parts by mass of ethyl acetate, and 0.026 parts by mass of 2,2'-azobisisobutyronitrile [AIBN; polymerization initiator] were successively dropped into the reaction vessel over 120 minutes, and after the dropwise addition was completed, the reaction was continued for another 150 minutes to complete the reaction. The solution after the reaction was completed was diluted with ethyl acetate to a solid content concentration of 26.5% by mass, and an acrylic copolymer A solution having a weight average molecular weight of 200,000 to 250,000 and a glass transition temperature of 49°C was obtained.

[0065] (Synthesis of Acrylic Copolymer B) An acrylic copolymer B solution having a solid content of 40.0% by mass, a weight average molecular weight of 200,000 to 250,000, and a glass transition temperature of 1°C was obtained in the same manner as in the synthesis of acrylic copolymer A, except that a monomer mixture consisting of 65.0 parts by mass of ethyl acrylate, 20.0 parts by mass of methyl methacrylate, 14.0 parts by mass of 2-hydroxyethyl methacrylate, and 1.0 part by mass of acrylic acid was used.

[0066] (Synthesis of acrylic copolymer C) An acrylic copolymer C solution having a solid content of 33.5% by mass, a weight average molecular weight of 600,000 to 700,000, and a glass transition temperature of -37°C was obtained in the same manner as in the synthesis of acrylic copolymer A, except that a monomer mixture consisting of 90 parts by mass of butyl acrylate and 10 parts by mass of acrylic acid was used.

[0067] <Example 1> An aluminum metal layer (average thickness 0.05 μm) was provided by vacuum deposition on one surface of a substrate layer made of a polyethylene terephthalate film (manufactured by Toyobo STC Co., Ltd., product name "A4360", average thickness 38 μm). Next, on the other surface of the base layer, a resin composition for forming a resin layer was prepared by adding 0.6 parts by mass of a hexamethylene diisocyanate (HMDI)-based crosslinking agent (manufactured by Asahi Kasei Corporation, product name "Duranate E405-70B", solid content 70 mass%) and 0.5 parts by mass of a hydroxyphenyltriazine (HPT)-based ultraviolet absorber (manufactured by BASF Japan Ltd., product name "Tinuvin 477", solid content 100 mass%) to a mixture of 71.5 parts by mass of an acrylic copolymer A solution and 28.5 parts by mass of an acrylic copolymer B solution, so that the thickness after solvent drying was 30 μm, and the mixture was heated and dried in a 120° C. atmosphere for 3 minutes to obtain a resin layer. To 100 parts by mass of the acrylic copolymer C solution, 2.5 parts by mass of a toluene diisocyanate crosslinking agent (manufactured by Nippon Polyurethane Industry Co., Ltd., product name "Coronate L45E", solid content 45% by mass) was added to prepare a resin composition for forming an adhesive layer. This resin composition for forming an adhesive layer was applied to one surface of another polyethylene terephthalate film that had been subjected to a peeling treatment so that the average thickness after solvent drying was 38 μm, and the film was heated and dried for 1 minute in a 100°C atmosphere to obtain an adhesive layer (second adhesive layer). Next, the metal layer and the adhesive layer were bonded together to obtain a laminate A having a laminate structure of resin layer / base layer / metal layer / adhesive layer / polyethylene terephthalate film.

[0068] Next, 1.0 part by mass of a hydroxyphenyltriazine (HPT)-based ultraviolet absorber (manufactured by BASF Japan Ltd., trade name "Tinuvin 477", solid content 100% by mass) and 1.0 part by mass of a hindered amine-based light stabilizer (manufactured by BASF Japan Ltd., trade name "Tinuvin 292", solid content 100% by mass) were added to 100 parts by mass of a polyurethane resin A solution (Urethane A, manufactured by Dainichi Seika Chemicals Co., Ltd., trade name "NE-8836", solid content 25.0% by mass) to prepare a surface layer forming resin composition. This surface layer forming resin composition was applied to one surface of a polyethylene terephthalate film that had been subjected to a release treatment so that the average thickness after solvent drying was 30 μm, and the surface layer was obtained by heating and drying in a 140 ° C. atmosphere for 3 minutes. To 100 parts by mass of the acrylic copolymer C solution, 0.13 parts by mass of an aluminum chelate crosslinking agent (manufactured by Kawaken Fine Chemical Co., Ltd., product name "Aluminum Chelate A", solid content 100% by mass) and 13 parts by mass of ethyl acetate as a dilution solvent were added to prepare a resin composition for forming an adhesive layer. This resin composition for forming an adhesive layer was applied to one surface of another polyethylene terephthalate film that had been subjected to a peeling treatment so that the average thickness after drying the solvent was 25 μm, and the adhesive layer was heated and dried for 1 minute in a 100 ° C. atmosphere to obtain an adhesive layer. Next, the surface layer and the adhesive layer were bonded together to obtain a laminate B having a laminate structure of polyethylene terephthalate film / adhesive layer / surface layer / polyethylene terephthalate film.

[0069] The polyethylene terephthalate film on the side in contact with the adhesive layer in laminate B was peeled off, and the adhesive layer was brought into contact with the surface on the resin layer side of laminate A to laminate the adhesive layer and surface layer on the resin layer, and the polyethylene terephthalate film on the side in contact with the surface layer was peeled off to obtain laminate 1 having a laminate structure of polyethylene terephthalate film / adhesive layer / metal layer / substrate layer / resin layer / adhesive layer / surface layer.

[0070] <Example 2> Laminate 2 was obtained under the same conditions as in Example 1, except that polyurethane resin B (Urethane B, manufactured by Dainichi Seikagaku Chemicals Co., Ltd., product name "NE-8811", solid content 25.0 mass%) was used instead of polyurethane resin A, and a surface layer was obtained so that the average thickness after solvent drying was 30 μm.

[0071] <Example 3> Laminate 3 was obtained in the same manner as in Example 1, except that the base layer was changed to a polyethylene terephthalate film (manufactured by Toyobo Co., Ltd., product name "E5100", average thickness 25 μm).

[0072] <Example 4> Laminate 4 was obtained in the same manner as in Example 1, except that the average thickness of the surface layer after drying of the solvent was set to 40 μm.

[0073] <Example 5> Laminate 5 was obtained in the same manner as in Example 1, except that the average thickness of the surface layer after drying of the solvent was set to 20 μm.

[0074] <Example 6> Laminate 6 was obtained in the same manner as in Example 1, except that the amount of the ultraviolet absorber added to the surface layer was changed to 0.75 parts by mass, and the amount of the ultraviolet absorber added to the resin layer was changed to 0.70 parts by mass.

[0075] <Example 7> Laminate 7 was obtained in the same manner as in Example 1, except that the amount of UV absorber added to the surface layer was changed to 1.50 parts by mass, and the UV absorber in the resin layer was changed to 0.38 parts by mass of a benzophenone-based UV absorber (manufactured by Shipro Chemical Co., Ltd., product name "SEESORB103", solid content 100% by mass).

[0076] <Example 8> Laminate 8 was obtained in the same manner as in Example 1, except that the amount of the ultraviolet absorber added to the surface layer was changed to 2.00 parts by mass, and the amount of the ultraviolet absorber added to the resin layer was changed to 0.30 parts by mass.

[0077] <Example 9> Laminate 9 was obtained in the same manner as in Example 1, except that the amount of UV absorber added to the surface layer was changed to 1.50 parts by mass, and 0.50 parts by mass of a benzotriazole-based UV absorber (manufactured by BASF Japan Ltd., product name "Tinuvin 326", solid content 100% by mass) was further added to the surface layer.

[0078] <Example 10> A laminate 10 was obtained in the same manner as in Example 1, except that the amount of the ultraviolet absorbing agent added to the resin layer was changed to 0.70 parts by mass.

[0079] <Example 11> A laminate 11 was obtained in the same manner as in Example 1, except that the amount of the ultraviolet absorbing agent added to the resin layer was changed to 0.30 parts by mass.

[0080] <Example 12> A laminate 12 was obtained in the same manner as in Example 1, except that the amount of the ultraviolet absorbing agent added to the surface layer was changed to 0.75 parts by mass.

[0081] <Comparative Example 1> A laminate 13 was obtained in the same manner as in Example 1, except that the base layer was changed to a polyethylene terephthalate film (manufactured by Toyobo Co., Ltd., product name "Cosmoshine (registered trademark) A4160", average thickness 50 μm).

[0082] <Comparative Example 2> A laminate 14 was obtained in the same manner as in Example 1, except that the amount of the ultraviolet absorbing agent added to the surface layer was changed to 0.50 parts by mass.

[0083] <Comparative Example 3> A laminate 15 was obtained in the same manner as in Example 1, except that the surface layer (average thickness: 36 μm) of the laminate B was formed in the same process as in Example 1 to form the resin layer.

[0084] <Comparative Example 4> A laminate 16 was obtained in the same manner as in Example 1, except that a fluorine-based resin film (manufactured by Denka Company Ltd., product name "Denka DX Film", average thickness 50 μm) was used as the surface layer.

[0085] <Comparative Example 5> A laminate 17 was obtained in the same manner as in Example 1, except that the amount of the ultraviolet absorbing agent added to the resin layer was changed to 0.00 part by mass.

[0086] <Comparative Example 6> A laminate 18 was obtained in the same manner as in Example 1, except that the amount of the ultraviolet absorbing agent added to the surface layer was changed to 0.00 part by mass.

[0087] <Comparative Example 7> A laminate 19 was obtained in the same manner as in Example 1, except that the amount of the ultraviolet absorber added to the surface layer was changed to 0.00 part by mass, and the amount of the ultraviolet absorber added to the resin layer was changed to 0.00 part by mass.

[0088] <Comparative Example 8> A laminate 20 was obtained in the same manner as in Example 1, except that the amount of UV absorber added to the surface layer was changed to 1.50 parts by mass, and 1.00 part by mass of a benzotriazole-based UV absorber (manufactured by BASF Japan Ltd., product name "Tinuvin 326", solid content 100% by mass) was further added to the surface layer.

[0089] The laminates obtained as described above were subjected to the following evaluations.

[0090] <Elasticity measurement> The elastic modulus was measured using Tensilon (manufactured by A&D Co., Ltd.) at a tension speed of 200 mm / min in an environment of 25° C. Each laminate was cut into a test piece measuring 25 mm in width and 100 mm in length, and evaluation was performed. The results are shown in Table 1 or Table 2.

[0091] <Follow-up evaluation> Each laminate obtained as described above was attached to an aluminum molded material of 50 mm x 30 mm x 100 mm, and the presence or absence of lifting of each laminate was visually observed at the right angle of the aluminum molded material, and the conformability was evaluated according to the following criteria. The obtained results are shown in Table 1 or Table 2. -Judgment criteria- A: There was no lifting of the laminate at any of the right-angled parts of the aluminum profile. B: There was no lifting of the laminate at any of the right-angled parts of the aluminum profile, but wrinkles occurred in the laminate when it was attached. C: The laminate had lifted at some or all of the right-angled parts of the aluminum profile.

[0092] <Appearance (colorless and transparent)> The surface layer was held up to transmitted light in a single film state, and the colorless transparency of the surface layer was judged visually. In addition, the absorbance at 400 nm was measured using a spectrophotometer (Hitachi High-Tech Science Corporation, model number "UH4150") in a single film state of the surface layer. Based on the results obtained, the appearance (colorless transparency) was evaluated according to the following criteria. The results obtained are shown in Table 1. If the appearance is rated A, it can be determined that a laminate having a mirror-like appearance is obtained. -Judgment criteria- A: It is colorless and transparent to the naked eye, and the absorbance at 400 nm is less than 0.5. B: Coloration is confirmed with the naked eye, or the absorbance at 400 nm is 0.5 or more.

[0093] <UV transmittance> The transmittance of the surface layer in a single film state was measured using a spectrophotometer (Hitachi High-Tech Science Corporation, model number "UH4150") at wavelengths of 240 nm to 600 nm, and the ultraviolet transmittance at wavelengths of 300 nm to 380 nm was calculated in accordance with JIS A5759 (2016). The results are shown in Table 1 or Table 2.

[0094] <Weather resistance evaluation> Accelerated weather resistance tests were conducted using a Sunshine Weather Meter (Model "S80B" manufactured by Suga Test Instruments Co., Ltd.) under conditions of a black panel temperature of 63±3°C, 30% RH±5% RH, and showering with pure water for 18 minutes out of 120 minutes. Each laminate before and after 5000 hours of exposure was visually inspected for significant fading, discoloration, and cracking, and its appearance was evaluated according to the following criteria. The results are shown in Table 1 or Table 2. -Judgment criteria- A: No significant fading, discoloration or cracks. B: Significant fading, discoloration or cracks have occurred.

[0095] [Table 1]

[0096] [Table 2]

[0097] The thickness (average thickness) of each layer was measured by the method described above.

[0098] The evaluation results shown in Table 1 or Table 2 reveal the following. Because polyester film and fluororesin film are both highly rigid materials, it was necessary to adjust the rigidity of the laminate, which uses a polyester film as a base layer and a fluororesin film as a surface layer, in order to attach the laminate to the right corners of the timber. In order to adjust the rigidity, the fluororesin film used in the surface layer was changed to a more flexible film, which resulted in a laminate with excellent conformability. However, the weather resistance was poor, so it was necessary to adjust the weather resistance by using an ultraviolet absorber, etc. The laminates of Examples 1 to 12, in which the surface layer contains a urethane-based resin, the base layer contains a polyester-based resin, and both the surface layer and the resin layer contain an ultraviolet absorber, the elastic modulus of the entire laminate is less than 155 N / 25 mm, the ultraviolet transmittance of the surface layer is less than 0.60%, and the absorbance at 400 nm of the surface layer is 0.45 or less, had a mirror-like appearance and were excellent in weather resistance and tracking properties, as is clear from the evaluation results shown in Table 1 or Table 2. On the other hand, a comparison between Example 1 and Comparative Example 1 revealed that when a polyester film having an average thickness of 50 μm or more was used as the base layer, the adhesive strength was defeated by the restoring force of the polyester film trying to return to its original state, causing the laminate to float from the aluminum molded material. However, when a polyester film having an average thickness of 40 μm or less was used as the base layer, the laminate could be bonded without sagging, and the laminate could be bonded while following the right angle without floating. Furthermore, by comparing Example 5 with Comparative Example 3 or Comparative Example 4, it was found that changing the surface layer from a highly rigid and brittle layer such as an acrylic resin layer or a fluorine-based resin film to a layer with excellent flexibility such as urethane also leads to the prevention of lifting from the aluminum mold material. In addition, it was found that Comparative Example 5, in which the UV transmittance of the surface layer was 0.60% or more (Comparative Examples 2-3, 6-7) or the resin layer did not contain a UV absorber, had poor weather resistance. In Comparative Example 4, the deterioration of weather resistance was suppressed even though the UV transmittance of the surface layer was 0.60% or more (4.73%). This is thought to be due to the use of a fluorine-based resin film in the surface layer. Moreover, in Comparative Example 8, in which the absorbance at 400 nm of the surface layer exceeded 0.45, the appearance was poor. [Explanation of symbols]

[0099] 1, 2 Laminate 10 Surface layer 20 Base material layer 30 metal layer 40, 42, 44 Adhesive layer 50 Resin layer 60 primer layer

Claims

1. The laminate includes a surface layer, a resin layer, a base layer, and a metal layer in this order, The surface layer contains a urethane resin, The base layer contains a polyester resin, The surface layer and the resin layer contain an ultraviolet absorber, The elastic modulus is less than 155 N / 25 mm; The ultraviolet transmittance of the surface layer is less than 0.60%, The surface layer has an absorbance at 400 nm of 0.45 or less.

2. 2. The laminate according to claim 1, wherein the content of the ultraviolet absorbing agent in the surface layer is 2 parts by mass or more per 100 parts by mass of the total of the resins contained in the surface layer.

3. The laminate according to claim 1 , wherein the content of the ultraviolet absorbing agent in the resin layer is 0.3 parts by mass or more per 100 parts by mass of the total of the resins contained in the resin layer.

4. The laminate according to claim 1 , wherein the resin layer contains a colorant.

5. 2. The laminate according to claim 1, wherein the resin layer has a total light transmittance of 15.0% to 100%.

6. The laminate according to claim 1 , wherein the average thickness of the base layer is 40 μm or less.

7. The laminate of claim 1 , wherein the metal layer comprises a metal, a metal oxide, or an alloy.

8. 2. The laminate according to claim 1, wherein the surface layer has an average thickness of 50 μm or less.

9. 2. The laminate according to claim 1, wherein the average thickness of the metal layer is 1 μm or less.

Citation Information

Patent Citations

  • Decorative sheet having metallic appearance

    JP1999058660A

  • Metal vapor deposition laminate

    JP2007216608A