Method for manufacturing carbon nanotube for spinning

By controlling the formation and cooling of a metal oxide catalyst layer under low-pressure conditions, the method enhances the uniformity of particle size and distribution, resulting in CNTs with superior spinnability for spinning applications.

JP2024145785AInactive Publication Date: 2024-10-15NIPPON SANSO CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023058282
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for producing carbon nanotubes (CNTs) for spinning face challenges in achieving uniform particle size and distribution of metal catalysts, leading to poor spinnability.

Method used

A method involving low-pressure chemical vapor phase synthesis is employed, where a metal oxide catalyst layer is formed on a base material, heated and cooled under controlled conditions to create uniform particles, followed by CNT synthesis using specific gas ratios and pressures to enhance spinnability.

Benefits of technology

The method results in CNTs with improved spinnability, characterized by good drawability and reproducibility, as demonstrated through SEM imaging and spinnability tests.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145785000006
    Figure 2024145785000006
  • Figure 2024145785000007
    Figure 2024145785000007
  • Figure 2024145785000008
    Figure 2024145785000008
Patent Text Reader

Abstract

To provide a method for manufacturing CNTs for spinning, capable of synthesizing the CNTs with excellent spinnability.SOLUTION: A method for manufacturing carbon nanotubes for spinning by the reduced pressure chemical vapor phase synthesis process comprises: forming a catalyst layer composed of metal oxide on at least a part of the surface of a base material; granulating the metal oxide in the catalyst layer by heating and cooling the base material at a pressure that is equal to or higher than 101 Pa and equal to or lower than the atmospheric pressure and in an inert gas atmosphere; and synthesizing carbon nanotubes on the surface of the catalyst layer after granulating the metal oxide.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing carbon nanotubes for spinning. [Background technology]

[0002] Carbon nanotubes (CNTs) are generally in powder form, but research has been reported on spinning spinnable CNTs in a dry process. This "spinnability" refers to the property that when a large number of CNTs are synthesized on a substrate, oriented upward and adjacent to one another, and one CNT is pulled out with tweezers or the like, it is possible to pull out a succession of CNTs like a vine. By twisting the pulled CNTs together, it is possible to make yarn made of CNTs. This yarn is conductive, light, and flexible, and research is currently underway into its use in wearable devices, etc.

[0003] When spinnable CNTs are synthesized on a substrate, a catalyst layer made of a metal catalyst such as iron is formed on the substrate. For example, in Patent Document 1, a catalyst layer is formed by sputtering iron on a substrate, and then the iron in the catalyst layer is granulated under an inert atmosphere and atmospheric pressure, and CNTs for spinning are synthesized by atmospheric pressure CVD. In Patent Document 2, a catalyst layer is formed by sputtering iron on a substrate, and then the iron in the catalyst layer is granulated under an inert atmosphere and reduced pressure, and CNTs for spinning are synthesized by reduced pressure CVD. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 4512750 [Patent Document 2] Patent No. 5636337 Summary of the Invention [Problem to be solved by the invention]

[0005] When the present inventors performed CVD according to the methods of Patent Documents 1 and 2, it was difficult to obtain CNTs with good spinnability. When the cause of this was investigated, it was found that the shape of the iron particles in the catalyst layer was non-uniform. The present inventors believed that the properties of the CNTs to be spun on the substrate depended on the properties of the catalyst layer, and from the viewpoint of improving spinnability, they thought that it was desirable for the particle size and distribution of the metal particles in the catalyst layer to be as uniform as possible.

[0006] The present invention provides a method for producing CNTs for spinning, which enables the synthesis of CNTs with excellent spinnability. [Means for solving the problem]

[0007] [1] A method for producing spinnable carbon nanotubes by reduced pressure chemical vapor synthesis, comprising the steps of: forming a catalyst layer made of a metal oxide on at least a portion of a surface of a substrate; placing the substrate under an inert gas atmosphere at a pressure of 101 Pa or more and equal to or less than atmospheric pressure, and heating and cooling the substrate to granulate the metal oxide in the catalyst layer; and synthesizing carbon nanotubes on the surface of the catalyst layer that has been subjected to the metal oxide particulation. The method of heating and cooling the substrate comprises: First, the mixture is heated at a rate of 25° C. / min to 75° C. / min from room temperature to a predetermined temperature of 650° C. or higher at which the metal oxide is turned into particles, and then allowed to stand at the predetermined temperature. Next, in the first stage of temperature reduction, the temperature is reduced from the predetermined temperature to 650°C at a rate of 35°C / min to 85°C / min. Then, in the second stage, the temperature is rapidly decreased from 650°C to 100°C or less at a rate of 145°C / min to 305°C / min. The substrate having the catalyst layer having the metal oxide particles is placed in a reactor; When heating from a predetermined temperature of 500° C. or less to a predetermined temperature of 600° C. or more at which the carbon nanotubes can be synthesized, The method for producing CNTs for spinning comprises reducing the pressure in the reactor from atmospheric pressure to a predetermined reaction pressure at a pressure reduction rate of 25 to 305 Pa / sec. [2] The method for producing CNTs for spinning described in [1], wherein the substrate on which the catalyst layer is formed is placed in an inert gas atmosphere at a pressure of 10,000 Pa or more and less than atmospheric pressure, and heated and cooled to granulate the metal oxide in the catalyst layer. [3] The method for producing CNTs for spinning according to [1] or [2], wherein the substrate having the catalyst layer that has been subjected to granulation of the metal oxide is placed in a reactor, a supply gas containing a mixture of a raw material gas and a carrier gas is supplied into the reactor, and when synthesizing the carbon nanotubes, the linear velocity of the supply gas at the position of the substrate placed in the reactor is 2.50 to 6.50 cm / sec, and the C / N ratio, which is expressed as the partial pressure of the raw material gas in the supply gas divided by the partial pressure of the carrier gas, is 0.40 to 0.65. Effect of the Invention

[0008] According to the manufacturing method of the present invention, the particle size and distribution of the metal oxide particles in the catalyst layer for synthesizing CNTs can be made more uniform than before, so that CNTs for spinning with good spinnability can be manufactured by the low-pressure CVD method. Here, "spinnability" can be said to be good when both drawability and reproducibility are achieved, as shown in the examples described later. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a cross-sectional view showing an example of the configuration of a carbon nanotube manufacturing apparatus. [Diagram 2] 2 is an enlarged cross-sectional view showing an area A shown in FIG. 1 in an enlarged manner. [Diagram 3] 1 is a SEM image of the granulated catalyst layer in Example 1-1. [Figure 4] 1 is an SEM image of a granulated catalyst layer in Comparative Example 1-1. [Diagram 5] 1 is an SEM image of a granulated catalyst layer in Comparative Example 1-2. [Figure 6] 1 is an SEM image of a granulated catalyst layer in Comparative Example 1-3. [Figure 7] FIG. 4 is a diagram showing preferred ranges of the linear velocity of the supply gas and the C / N ratio. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. In the drawings used in the following description, the dimensions of the components may be shown at different scales to make each component easier to see, and the dimensional ratios of each component may not necessarily be the same as in reality. Furthermore, the materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not necessarily limited to them, and may be appropriately modified and implemented within the scope of the present invention. Furthermore, a numerical range expressed by "~" indicates a numerical range in which the numerical values ​​before and after "~" are the lower and upper limits.

[0011] <Carbon nanotube manufacturing equipment> First, as an example of a production apparatus (synthesis apparatus) applicable to the carbon nanotube production method of the present invention, a carbon nanotube production apparatus shown in FIG. 1 and FIG. 2 will be described. 1 is a cross-sectional view showing the configuration of a carbon nanotube production apparatus, and FIG 2 is an enlarged cross-sectional view showing an area A shown in FIG 1.

[0012] In FIG. 1, reference numeral 1 denotes a carbon nanotube production apparatus (hereinafter simply referred to as the "production apparatus"), reference numeral 2 denotes a cylindrical heater whose upper end is closed, reference numeral 3 denotes a cylindrical outer reaction tube whose upper end is closed and which is disposed coaxially with heater 2, and reference numeral 4 denotes a cylindrical inner reaction tube whose upper end is open and which is disposed coaxially inside outer reaction tube 3.

[0013] Between the outer reaction tube 3 and the inner reaction tube 4, a cylindrical space 5 having a closed lower end is located. That is, the production apparatus 1 includes a reactor having a double-tube structure consisting of an outer reaction tube 3 and an inner reaction tube 4. The inside of the reactor may mean the inside of the outer reaction tube 3 including the space 5 or the inside of the inner reaction tube 4.

[0014] An exhaust pipe 6 is located at the lower end of the space 5, and the space 5 and the exhaust pipe 6 are in communication with each other. A vacuum gauge 7 and a vacuum pump 8 are positioned in the exhaust pipe 6 . The vacuum gauge 7 is located on the primary side of the vacuum pump 8, and measures the pressure inside the outer reaction tube 3 and the inner reaction tube 4. The vacuum gauge 7 is not particularly limited, but for example, a Baratron type vacuum gauge can be applied. The vacuum pump 8 is located on the secondary side of the vacuum gauge 7, and exhausts the atmosphere in the outer reaction tube 3 and the inner reaction tube 4 to reduce the pressure. A supply gas introduction pipe 9 is located at the lower end of the inner reaction tube 3, and the inside of the inner reaction tube 3 and the supply gas introduction pipe 9 are in communication with each other.

[0015] The heater 2 is vertically divided into four heating areas 2A to 2D, and the temperatures of the outer reaction tube 3 and the inner reaction tube 4 can be adjusted individually in the height direction. Thermometers 10A-10D are provided at the center of the height direction of the four heating areas 2A-2D, respectively. The tip of each of the thermometers 10A-10D is located in the space between the outer reaction tube 3 and each of the heating areas 2A-2D. Each of the thermometers 10A-10D can measure the temperature in the height direction of the outer reaction tube 3 and the inner reaction tube 4. A heat insulating material 11 is positioned outside the heater 2 so as to cover the periphery of the heater 2 .

[0016] A vertical wafer boat 12 can be inserted into the inner reaction tube 4 . The vertical wafer boat 12 is erected on a lift flange 13. A furnace port cover 14 is provided on the lift flange 13, and the lower end of the outer reaction tube 4 is air-tightly closed by the furnace port cover 14.

[0017] 2, the vertical wafer boat 12 has a plurality of support columns 15. Furthermore, grooves 16 are provided at a predetermined interval (pitch) in the vertical direction on each of the support columns 15. The vertical wafer boat 12 can hold a plurality of substrates 17 horizontally by inserting the substrates 17 into two or more grooves 16 located at the same height. The vertical wafer boat 12 loaded with a plurality of substrates 17 is inserted into the inner reaction tube 4 to process the substrates.

[0018] The manufacturing apparatus applicable to the present invention is not limited to the above-mentioned configuration of the manufacturing apparatus 1, as long as it can manufacture carbon nanotubes using the low pressure chemical vapor deposition (LPCVD) method. A commercially available manufacturing apparatus may be applied to the present invention. Examples of such manufacturing apparatus include the TELINDY series manufactured by Tokyo Electron Ltd., the VERTEX series manufactured by KOKUSAI ELECTRIC Co., Ltd., and the ADVANCE VERTICAL FURNACE series manufactured by ASM Co., Ltd. These apparatuses include a resistance heating type heater equipped with a thermocouple for control, a quartz reactor serving as a reaction field, a quartz nozzle for introducing gas, a quartz boat for storing wafers, an elevator mechanism for transferring the quartz boat to the quartz reactor, a robot mechanism for transferring substrates to the quartz boat, an exhaust pump, a gas pipe for supplying a supply gas, and an exhaust gas pipe for exhausting exhaust gas.

[0019] <Manufacturing method for CNT for spinning> A first aspect of the present invention is a method for producing spinnable carbon nanotubes by low pressure chemical vapor deposition (LPCVD). This embodiment preferably includes a catalyst layer forming step, a granulation step, and a synthesis step. A preferred embodiment of each step will be described below with reference to the reference symbols in FIGS.

[0020] [Catalyst layer formation process] The catalyst layer forming step is a step of forming a catalyst layer made of a metal oxide on at least a part of the surface of the substrate.

[0021] (base material) The substrate 17 has a catalyst layer on at least a portion of its surface. The substrate 17 is not particularly limited, but is preferably a flat substrate capable of supporting a catalyst layer composed of a plurality of catalyst particles and having a smoothness that does not impede the movement of the catalyst when it is fluidized and granulated, and more preferably a substrate having a pair of parallel and flat surfaces. Furthermore, it is preferable that a catalyst layer is formed on one of the pair of surfaces of the flat substrate.

[0022] The material of the base material 17 is not particularly limited, but is preferably a material that has low reactivity with the catalytic metal. An example of such a base material 17 is a single crystal silicon substrate, which is excellent in terms of smoothness, cost, and heat resistance. Specific examples include those with the following specifications.

[0023] [Table 1]

[0024] When a single crystal silicon substrate is used as the base material 17, it is preferable to oxidize or nitride the surface of the substrate in order to prevent unintended compounds from being formed on the surface of the substrate. As a result, a silicon oxide film (SiO2 film) or a silicon nitride film (Si3N4 film) is formed on the surface of the single crystal silicon substrate. In addition, a coating made of a metal oxide or metal nitride, such as alumina, which has low reactivity, may be formed on the surface of the single crystal silicon substrate, and then a catalyst layer may be formed on the coating. The thickness of the coating is preferably 10 nm to 1000 nm.

[0025] (catalyst layer) Examples of materials that make up the catalyst layer include metals such as nickel, cobalt, and iron. As the catalyst, it is preferable to use a single catalyst (metal catalyst) made of one type of metal, and it is more preferable to use an iron-based catalyst. This makes it easy to form CNTs using the catalyst as a nucleus. From the viewpoint of forming catalyst particles having uniform particle size and distribution in the catalyst layer in the subsequent granulation step, the material constituting the catalyst is preferably a metal oxide, more preferably an oxide of nickel, cobalt or iron, and even more preferably an oxide of iron.

[0026] The thickness of the catalyst layer is not particularly limited, but is preferably in the range of 0.5 to 100 nm, and more preferably in the range of 1.5 to 15 nm. If the thickness of the catalyst layer is 0.5 nm or more, a catalyst layer of uniform thickness can be easily formed on the surface of the substrate. If the thickness of the catalyst layer is 15 nm or less, it can be easily granulated by preheating at 800°C or less before the CVD reaction. Here, the thickness of the catalyst layer is the average value measured for any 10 cross sections. The catalyst layer in this step is preferably a film that uniformly covers the entire surface of the substrate, from the viewpoint of forming uniform catalyst particles in the subsequent particulate forming step.

[0027] The method for forming the catalyst layer is not particularly limited, but specifically includes a method of depositing a catalyst material on the surface of a substrate by a sputtering method, a vacuum deposition method, etc., and a method of applying a solution containing a catalyst material (catalyst solution) on the surface of a substrate to form a coating film, and then heating and drying the coating film. A coating method of applying a catalyst solution is preferred because it can easily form a catalyst layer made of a metal oxide.

[0028] (Catalyst solution) The solute of the catalyst solution may be, for example, a catalyst solution containing one of metals such as nickel, cobalt, iron, etc., or one of metal complex compounds such as nickel, cobalt, iron, etc. For example, iron nitrate nonahydrate or the like may be used as the catalyst solution.

[0029] Examples of the solvent for the catalyst solution include a special solvent that is compatible with water and has a boiling point higher than that of water, or a mixed solvent containing a special solvent and ethanol. The characteristic solvents consist of one or more of alcohols, glycol ethers, esters, ketones, and aprotic polar solvents. The concentration of the solute relative to the total mass of the catalyst solution can be adjusted, for example, in the range of 0.2 to 8.0 mass %, and the blending concentration of the special solvent can be adjusted, for example, in the range of 5.0 to 99.8 mass %. The solute and the solvent are mixed to obtain a catalyst solution.

[0030] The alcohol preferably comprises one or more of 1-butanol, 2-butanol, and diacetone alcohol. The glycol ether is preferably one or more of ethylene glycol monomethyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether, ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether, and propylene glycol monoethyl ether. The glycol ether is preferably one or more of ethylene glycol monomethyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether, ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether, and propylene glycol monoethyl ether. Preferably, the ketone comprises acetylacetone. The aprotic polar solvent preferably comprises one or more of dimethylsulfoxide, N-methyl-2-pyrrolidone, and N,N-dimethylformamide.

[0031] (Catalyst Coating Method) The method for applying the catalyst solution onto the surface of the substrate is not particularly limited, but examples thereof include spin coating, spray coating, bar coater, inkjet, and slit coater methods.

[0032] It is desirable to perform spin coating in a clean work environment created using a clean bench or the like. The rotation speed of the spin coater can be set arbitrarily from 1 rpm to 5000 rpm, and the rotation speed can be set in one or more stages. The rotation time can be set arbitrarily from 1 sec to 600 sec at each rotation speed.

[0033] The procedure for the spin coating method is to place the substrate at the center of the spin stage of a spin coater, then drip 0.1 ml to 10 ml of catalyst solution onto the surface of the substrate, and rotate the spin stage at a preset rotation speed. Here, the catalyst solution can be dripped after the spin stage starts rotating. After the preset rotation time has elapsed, the spin stage rotation is stopped and the substrate is collected.

[0034] The substrate after the spin coating process may be placed on a hot plate or heated in a furnace to remove the solvent and oxidize the metal contained in the catalyst layer with oxygen in the air to form a metal oxide. This heat treatment is preferably carried out in air at atmospheric pressure, under reduced pressure, or in a non-oxidizing atmosphere at a temperature range of 100 to 300°C, more preferably at a temperature range of 120 to 300°C. This allows even solvents with relatively high boiling points to be removed reliably. Note that if the heating is performed at 300°C or less, the metal oxide in the catalyst layer will not be granulated.

[0035] The spin-coating procedure can be performed in a commercially available single-wafer spin-coating or spin-cleaning apparatus, which includes any or all of the following: a stage for mounting a substrate carrier that holds multiple substrates, a transfer robot for transporting the substrates, a centering mechanism, a spin stage, a coating arm with a syringe, and a baking mechanism consisting of a hot plate or furnace.

[0036] [Particle formation process] The granulation step is a step of granulating the metal oxide in the catalyst layer by placing the base material on the surface of which the catalyst layer is formed under an inert gas atmosphere at a pressure of 101 Pa or more and less than atmospheric pressure, and heating and cooling the base material. Hereinafter, granulating the metal oxide in the catalyst layer may be simply referred to as "granulating the catalyst layer."

[0037] The heating and cooling of the substrate is preferably performed by placing the substrate in a heating furnace capable of controlling the temperature and atmosphere. The heating furnace is preferably capable of controlling the reduced pressure. As an apparatus equipped with such a heating furnace, the above-mentioned carbon nanotube production apparatus, which can also be used in the subsequent synthesis step, is preferable. For example, this step can be performed in the reaction furnace (inner reaction tube 4) of the carbon nanotube production apparatus 1.

[0038] The pressure when the catalyst layer is granulated in this step is 101 Pa or more, preferably 1500 Pa or more, more preferably 10000 Pa or more, and even more preferably atmospheric pressure (0.10 MPa). The closer the pressure is to atmospheric pressure, the better the spinnability of the CNTs obtained in the subsequent synthesis step.

[0039] The heating temperature for granulating the catalyst layer in this process may be equal to or higher than the temperature at which the metal oxide is granulated under an inert gas atmosphere. The detailed mechanism by which the metal oxide in the catalyst layer is granulated by heating has not been elucidated, but it is believed that the cohesive force and surface tension between the metal oxides affect each other in a complex manner to granulate the metal oxide. It is not necessary to heat the metal oxide to its melting point in order to granulate the metal oxide. If the metal oxide is a general metal oxide, it can be granulated by heating at 500 to 1000°C. Also, if the catalyst layer is made of iron oxide, it can be granulated sufficiently by heating to about 700 to 750°C.

[0040] The method of heating and cooling the catalyst layer to form particles in this step is preferably the following method because it is easy to form uniform particles: First, the catalyst layer is heated from room temperature (15 to 35°C) to a predetermined temperature (any temperature) of 650°C or more at which the metal oxide is to be particulated, at a temperature increase rate of 25°C / min to 75°C / min, and then allowed to stand at the predetermined temperature, and then the catalyst layer is cooled from the predetermined temperature to 650°C at a temperature decrease rate of 35°C / min to 85°C / min in the first stage, and then rapidly cooled from 650°C to 100°C or less at a temperature decrease rate of 145°C / min to 305°C / min in the second stage. The predetermined temperature is preferably 700 to 800° C. The time for leaving the mixture at the predetermined temperature is preferably 1 to 5 minutes. The temperature increase rate and the temperature decrease rate can be controlled by PID control.

[0041] According to this step, a catalyst layer made up of a plurality of catalyst particles having a diameter of about 0.5 nm to 50 nm can be formed. When the surface of such a catalyst layer is observed with a scanning electron microscope (SEM), and, for example, 80% or more of the catalyst particles observed in a field of view of 1 μm x 1 μm have part or all of four or more other catalyst particles within a circle of radius 50 nm from the center of each particle, it can be determined that the catalyst particles in the catalyst layer are adjacent to each other at a high density and the particle distribution is uniform.

[0042] The average particle size of the catalyst particles in the catalyst layer is determined as the average particle size (longest diameter) of 40 or more particles randomly selected from catalyst particles present within a 1 μm × 1 μm SEM observation field of a representative portion of the catalyst layer (e.g., near the center of the substrate). The average particle size of the catalyst particles in the catalyst layer is preferably 0.5 nm to 50 nm, from the viewpoint of synthesizing CNTs with excellent spinnability.

[0043] [Synthesis process] The synthesis step is a step of synthesizing carbon nanotubes on the surface of the catalyst layer (particulated catalyst layer) that has been subjected to particulation of the metal oxide.

[0044] For example, as shown in Figures 1 and 2, a vertical wafer boat 12 loaded with one or more substrates 17 having a granulated catalyst layer is inserted into a reaction furnace (inside the inner reaction tube 4), the pressure inside the reaction furnace is evacuated to a predetermined pressure using a vacuum pump 8, the temperature inside the reaction furnace (inside the outer reaction tube 3) is heated to a predetermined reaction temperature using a heater 2, and then a supply gas is supplied into the reaction furnace from a supply gas inlet tube 9 to synthesize carbon nanotubes on the surface of the granulated catalyst layer of each substrate 17 by reduced pressure chemical vapor synthesis, and the exhaust gas is discharged from an exhaust tube 6. This will be explained in more detail below.

[0045] A substrate 17 on which a catalyst layer is formed is placed in a reactor with a high-temperature atmosphere, and a supply gas containing a raw material gas and a carrier gas is supplied to the substrate 17 in the reactor, and carbon nanotubes are grown using the catalyst particles as nuclei. During this process, the metal oxide of the catalyst particles is reduced by the raw material gas to become metal, and multiple carbon nanotubes are formed so as to be oriented perpendicular to the surface of the substrate 17.

[0046] The length of each vertically aligned carbon nanotube can be adjusted by adjusting the amount of raw material gas supplied, the reaction pressure (pressure inside the reactor), and the reaction time inside the reactor. By extending the reaction time inside the reactor, the length of the carbon nanotube can be extended to several mm.

[0047] (raw gas) The raw material gas used for the synthesis and growth of carbon nanotubes may be, for example, an aliphatic hydrocarbon gas such as acetylene, methane, ethylene, etc. Among these, the acetylene gas may be general industrial acetylene applied to welding processing, or may be ultra-high purity acetylene gas with an acetylene concentration of 99.9999% or more.

[0048] When acetylene gas is used as the raw material gas, multiple carbon nanotubes with a multi-layer structure and a diameter of 0.5 to 50 nm, which reflects the particle size of the catalyst particles that serve as the nuclei, grow perpendicular to the substrate and aligned in a certain direction. In addition, by using ultra-high purity acetylene gas as the raw material gas, it is possible to grow high-quality carbon nanotubes.

[0049] (Carrier gas) Examples of carrier gases for transporting the raw material gas include He, Ne, Ar, N2, H2, etc. Among these, He, N2, and Ar are preferable, and N2 is more preferable.

[0050] (Insertion temperature) The temperature inside the reactor when the vertical wafer boat 12 loaded with the substrates 17 is inserted into the reactor (insertion temperature) is preferably at least room temperature (20°C) and not more than a temperature 100°C lower than the reaction temperature (reaction temperature -100°C), and more preferably not more than a temperature 300°C lower than the reaction temperature. For example, as described below, when the reaction temperature is 730°C, it is preferable to insert the substrates into the reactor when the temperature inside the reactor is between room temperature and 650°C, and more preferably to insert the substrates into the reactor when the temperature inside the reactor is between room temperature and 450°C. By inserting the granulated catalyst layer into the reactor at the above-mentioned suitable temperature, it is possible to prevent the particle size and distribution of the particles in the catalyst layer from being changed due to rapid heating during insertion.

[0051] In the example shown in FIGS. 1 and 2, a vertical wafer boat 12 has a structure in which a plurality of substrates 17 are inserted into the vertical wafer boat 12 to perform reaction processing simultaneously. In this embodiment, the number of substrates 17 inserted into the reactor is not particularly limited, and may be one, or may be multiple as in the illustrated example.

[0052] (Reaction pressure) The pressure inside the reactor (reaction pressure) is preferably 4000 to 10000 Pa, and more preferably 5000 to 8000 Pa. For example, it can be set to 8000 Pa. When the reaction pressure is 4000 Pa or higher, the reaction rate of the raw material gas with the catalyst increases, and the amount of CNTs synthesized for spinning increases. When the reaction pressure is 10,000 Pa or less, the diffusibility of the raw material gas is good, and CNTs for spinning having excellent spinnability can be easily obtained.

[0053] When the substrate having the particulate catalyst layer is placed in a reactor and heated from a predetermined temperature of, for example, 500°C or less to a predetermined reaction temperature of, for example, 600°C or more at which the carbon nanotubes can be synthesized, it is preferable to reduce the pressure in the reactor from atmospheric pressure to the predetermined reaction pressure at a reduction speed of 25 to 305 Pa / sec. When the reduction speed is within this range, CNTs with excellent spinnability can be easily obtained. For example, the reduction speed can be 100 Pa / sec.

[0054] (Reaction temperature) The temperature (reaction temperature) in the reactor when synthesizing carbon nanotubes on the surface of the granulated catalyst layer is not particularly limited, and can be, for example, in the range of 500° C. to 1000° C., and preferably in the range of 700° C. to 800° C. For example, it can be set to 730° C. At reaction temperatures of 700°C or higher, the reaction of the raw material gas with the catalyst is enhanced, making it easy to synthesize CNTs for spinning. At a reaction temperature of 800° C. or lower, synthesis tends to proceed in the direction of increasing CNT density rather than in the length direction of the CNTs, making it easier to obtain CNTs for spinning with excellent spinnability.

[0055] (Gas flow rate) The flow rates of the source gas and the carrier gas can be set independently to, for example, 1.0 L / min to 20 L / min. The total amount of the gas to be supplied, which is a mixture of the raw material gas and the carrier gas, is preferably 1.0 L / min to 20 L / min, and more preferably 3.0 L / min to 10 L / min. For example, it can be set to 7.0 L / min. The content of the raw material gas is preferably 5 to 90% by volume, more preferably 10 to 60% by volume, based on the total volume of the feed gas obtained by mixing the raw material gas and the carrier gas. When the content of the raw material gas is equal to or more than the lower limit of the above preferred range, the bulk density of the synthesized carbon nanotubes can be increased.

[0056] Regarding the supply gas, the mixture ratio of the raw material gas:carrier gas can be set in the range of, for example, 20:80 to 60:40 by volume ratio. Specifically, it can be set to, for example, 40:60.

[0057] The partial pressures of the raw material gas and the carrier gas in the reactor preferably have a relationship of raw material gas partial pressure < carrier gas partial pressure. For example, it is preferable that the partial pressure of the raw material gas is 20-40% of the total pressure, and the partial pressure of the carrier gas is 80-60%. Specifically, for example, when the total pressure is 8000 Pa, it is preferable that the partial pressure of the raw material gas is 2000-3900 Pa, and the partial pressure of the carrier gas is 6000-4100 Pa. More specifically, for example, when the total pressure is 8000 Pa, the partial pressure of the raw material gas: partial pressure of the carrier gas can be set to 3000 Pa: 5000 Pa.

[0058] The C / N ratio, expressed as (partial pressure of raw material gas / partial pressure of carrier gas) in the reaction furnace, is preferably from 0.35 to 0.70, and more preferably from 0.40 to 0.65. When the content is within the above range, CNTs for spinning having excellent spinnability can be easily obtained.

[0059] The linear velocity (unit: cm / sec) of the gas supplied into the reactor is calculated by the following formula. Linear velocity of the supply gas = Flow rate of the supply gas × (atmospheric pressure / reaction pressure) / cross-sectional area of ​​the reactor Here, the cross-sectional area of ​​the reactor is the cross-sectional area in the direction perpendicular to the direction in which the supply gas flows. 1 and 2, the supply gas rises upward from the lower end of the internal reaction tube 4 and is exhausted from the open upper end into the space 5 continuing to the exhaust pipe 6. Therefore, the supply gas flows in the length direction of the reaction furnace, and the perpendicular direction to this is parallel to the planar direction of the flat substrate 17. The cross-sectional area of ​​the reaction furnace applied to the calculation of the linear velocity is the cross-sectional area of ​​the reaction space obtained by cutting the internal reaction tube 4 in a cross-section at the position where the substrate 17 is installed.

[0060] The linear velocity of the gas supplied during the synthesis of CNTs for spinning is preferably 2.50 to 6.50 cm / sec, and can be set to, for example, 4.20 cm / sec.

[0061] In this step, it is preferable that the linear velocity of the supply gas at the position of the substrate placed in the reactor is 2.50 to 6.50 cm / sec, and the C / N ratio, which is expressed by dividing the partial pressure of the raw material gas in the supply gas by the partial pressure of the carrier gas, is 0.40 to 0.65. When synthesized under these conditions, CNTs for spinning with excellent spinnability can be easily obtained.

[0062] After the synthesis of the CNTs for spinning is completed, the introduction of the supply gas is stopped, and an inert gas is introduced into the reactor to purge the reactor, after which the vertical wafer boat 12 is pulled out from the reactor and each substrate 17 is taken out. The CNTs for spinning can be pulled out one after the other in a conventional manner from one end of the CNT group formed on the catalyst layer surface of the substrate 17, and continuously collected.

[0063] The technical scope of the present invention is not limited to the above-described embodiment, and various modifications can be made without departing from the spirit of the present invention. EXAMPLES

[0064] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.

[0065] (Example 1-1) Carbon nanotubes were synthesized using a production apparatus 1 shown in FIG. A silicon substrate with an oxide film (φ150 mm, thickness: 625 μm) was used as the substrate. The catalyst solution was prepared in the following manner. Iron nitrate nonahydrate was used as the solute, and N,N-dimethylformamide and 1-ethoxy-2-propanol were used as the solvents, and they were mixed to prepare the catalyst solution. The respective contents were 5.0 wt% iron nitrate nonahydrate, 19.0 wt% N,N-dimethylformamide, and 76.0 wt% 1-ethoxy-2-propanol. 2 ml of the catalyst solution was dropped onto the substrate and applied by spin coating (rotation speed: two stages of 750 rpm and 3500 rpm).Then, the substrate was heated on a hot plate at 300°C for 10 minutes to dry the coating, resulting in a substrate with a catalyst layer made of iron oxide (Fe2O3) with a thickness of 5 nm. Next, the substrate was heated and cooled in a temperature-controllable reactor according to the following procedure, thereby granulating the iron oxide in the catalyst layer on the substrate.

[0066] (Particleization procedure) The catalyst layer was granulated under atmospheric pressure in a nitrogen atmosphere. First, the temperature was increased from room temperature (approximately 30°C) at a rate of 70°C / min, and when it reached 730°C, it was left to stand for 2 minutes. During this period, the iron oxide in the catalyst layer was granulated. Then, in the first stage, the temperature was decreased from 730°C to 650°C at a rate of 80°C / min, and then in the second stage, the temperature was rapidly decreased from 650°C to below 100°C at a rate of 150°C / min. By the above procedure, a large number of particles made of iron oxide were formed in the catalyst layer on the substrate.

[0067] (CNT synthesis) The substrate with the catalyst layer was inserted into a reactor preheated to 450° C., and the temperature was increased at 10° C. / min to 730° C. in a nitrogen atmosphere. During this, the pressure was reduced from atmospheric pressure to reaction pressure (8000 Pa) at 100 Pa / sec. The feed gas was a mixture of general industrial acetylene gas as the raw material gas and nitrogen gas as the carrier gas in a volume ratio of 37.5:62.5 using a mass flow controller, and the mixture was supplied to the reactor, synthesizing CNTs for spinning that were oriented upward from the surface of the catalyst layer. The partial pressures of the supplied gases were acetylene gas:nitrogen gas=3000 Pa:5000 Pa, and the C / N ratio expressed as (partial pressure of acetylene gas / partial pressure of nitrogen gas) was 0.60. The cross-sectional area of ​​the space in which the reactor substrate is installed, perpendicular to the direction of the supply gas flow, is 346.2 cm 2 The total flow rate of the supplied gas under atmospheric pressure (101 kPa) was set to 7.0 L / min, so the volumetric flow rate in the furnace under 8000 Pa was 1466 cm 3 / sec {=7.0 L / min × (101 kPa / 8 kPa)} and the linear velocity of the supplied gas was 4.2 cm / sec. The linear velocity is the gas flow rate divided by the cross-sectional area of ​​the pipe through which the gas flows.

[0068] The spinnability of the spinning CNTs of Example 1-1 produced by the above method was evaluated according to the following evaluation method and criteria. The results are shown in the table below.

[0069] (Method of evaluating spinnability) The CNTs for spinning formed on the surface of the catalyst layer are highly dense, and when observed visually, it appears that a layer of CNTs is formed on the surface of the catalyst layer. If the end of this CNT layer is pinched with tweezers and pulled up, it is possible to continuously pull out the CNTs like a vine. The tips of the pinched out CNTs for spinning were attached to the surface (side of a cylinder), and the roll was rotated to judge the spinnability according to the criteria described below. At this time, the surface of the substrate on which the CNTs for spinning were synthesized and the top of the roll were positioned at the same height, so that the CNTs for spinning on the substrate were pulled out horizontally toward the roll. In other words, the pull angle of the CNTs for spinning was 0 degrees. The diameter of the roll was 165 mm, and the roll rotation speed was 200 rpm. The number of samples for evaluating the spinnability was two.

[0070] (Evaluation Criteria for Spinnability) The spinning properties were evaluated based on the drawing property and reproducibility according to the criteria in the table below. The pull-out ability was evaluated as better the longer the length that could be continuously pulled out in one pull-out test. Specifically, the evaluation was made on a four-point scale: "good" if the sample could be pulled out 140mm or more, "fair" if the sample could be pulled out 20mm or more but less than 140mm, "unacceptable" if the sample could be pulled out 10mm or more but less than 20mm, and "poor" if the sample could only be pulled out less than 10mm. Of the two evaluation samples, the result of the sample with the longer pull-out length was used. To evaluate reproducibility, a pull-out test was conducted once for each evaluation sample. With the difference in the length pulled out between the first evaluation sample and the second evaluation sample being the longer of the two (100%), a reproducibility of within ±20% was rated as "good," a reproducibility of within ±50% was rated as "passable," and a reproducibility of more than ±50% was rated as "poor."

[0071] In the following test example, the manufacturing method of Example 1-1 was used as a base, but some modifications were made to obtain CNTs for spinning. The evaluation results of the spinnability are shown in the table below. (Example 1-2) The iron oxide in the catalyst layer was granulated under reduced pressure of 10,000 Pa. (Examples 1-3) The iron oxide in the catalyst layer was granulated under reduced pressure of 1000 Pa. (Comparative Example 1-1) The iron oxide in the catalyst layer was granulated under reduced pressure of 100 Pa. (Comparative Example 1-1) The iron oxide in the catalyst layer was granulated in an air atmosphere. (Comparative Example 1-2) A catalyst layer made of iron was formed using a sputtering apparatus CFS-4ES (manufactured by Shibaura Mechatronics Corporation) with sputtering gas: Ar and gas pressure: 0.75 Pa, and the iron in the catalyst layer was granulated under atmospheric pressure conditions. (Comparative Example 1-3) A catalyst layer made of iron was formed using a sputtering apparatus CFS-4ES (manufactured by Shibaura Mechatronics Corporation) with sputtering gas: Ar and gas pressure: 0.75 Pa, and the iron in the catalyst layer was granulated under reduced pressure conditions of 100 Pa.

[0072] [Table 2]

[0073] Among Examples 1-1 to 1-3, the spinnability of the spinnable CNTs obtained in Example 1-1 was the best. These results show that atmospheric pressure is the most preferable pressure condition for particle-forming the catalyst layer. An SEM image of the surface of the granulated catalyst layer of Example 1-1 is shown in Figure 3. Individual particles could be clearly identified, and the particle size (longest diameter of the particle) was uniform, about 10 to 50 nm. In addition, in 80% or more of the particles observed in a 1 μm x 1 μm visual field, four or more other particles were partially or entirely contained within a circle of a radius of 50 nm from the center of each particle, and it was found that the particles were closely adjacent to each other and the particle distribution was uniform.

[0074] An SEM image of the surface of the granulated catalyst layer of Comparative Example 1-1 is shown in Figure 4. Overall, it was difficult to distinguish the individual particles. The particles were fused together to form a membrane-like shape. An SEM image of the surface of the granulated catalyst layer of Comparative Example 1-2 is shown in Fig. 5. Individual particles could be clearly identified, and the particle size was uniform, about 5 to 20 nm. However, in an observation field of 1 µm x 1 µm, many areas were confirmed within a circle of radius 50 nm from the center of each particle where not even one particle was contained in part or in whole, indicating that the density of the particles was low and the particle distribution was low compared to Example 1-1. The SEM image of the surface of the granulated catalyst layer of Comparative Example 1-3 is shown in Figure 6. There were many places where it was difficult to clearly distinguish individual particles, and in some places the particles were fused together to form a membrane-like shape. The distribution of the particles was partially non-uniform. The SEM image of the surface of the granulated catalyst layer of Comparative Example 1-4 was similar to that of Comparative Example 1-3, and the distribution of the particles was partially non-uniform.

[0075] (Example 2-1) The same conditions as in Example 1-1 were used to obtain CNTs for spinning. The evaluation results of the spinnability are shown in the table below. In the following test example, the manufacturing method of Example 1-1 was used as a base, but a part of the particle formation procedure was changed to obtain CNTs for spinning. The evaluation results of the spinnability are shown in the table below. (Example 2-2) The temperature rise rate was 30° C. / min. (Example 2-3) The temperature drop rate in the first stage was 40° C. / min. (Examples 2-4) The cooling rate in the second stage was 300° C. / min. (Examples 2-5) The temperature drop rate in the first stage was 40° C. / min, and the temperature drop rate in the second stage was 300° C. / min. (Comparative Example 2-1) The heating rate was 100° C. / min. (Comparative Example 2-2) The temperature rise rate was 20° C. / min. (Comparative Example 2-3) The temperature drop rate in the second stage was 100° C. / min. (Comparative Example 2-4) The temperature drop rate in the first stage was 20° C. / min. (Comparative Example 2-5) The temperature drop rate in the first stage was 150° C. / min. (Comparative Example 2-6) The temperature drop rate in the first stage was 300° C. / min, and the temperature drop rate in the second stage was 300° C. / min.

[0076] [Table 3]

[0077] From the above results, it was found that the procedure for granulating the metal oxide that constitutes the catalyst layer involves heating the material to a temperature above the temperature at which the metal oxide granulates (at least above 650°C) at a heating rate of 25°C / min to 75°C / min, leaving it to stand, and then cooling it to 650°C at a first temperature reduction rate of 35°C / min to 85°C / min, and then rapidly cooling it to below 100°C at a second temperature reduction rate of 145°C / min to 305°C / min to granulate the catalyst layer, resulting in CNTs with excellent spinnability.

[0078] (Example 3-1) The same conditions as in Example 1-1 were used to obtain CNTs for spinning. The evaluation results of the spinnability are shown in the table below. In the following test example, the manufacturing method of Example 1-1 was used as a base, but some of the conditions for CNT synthesis were changed to obtain CNTs for spinning. The evaluation results of the spinnability are shown in the table below. (Example 3-2) The pressure reduction rate during heating of the reactor was set to 300 Pa / sec. (Example 3-3) The pressure reduction rate during heating of the reactor was set to 30 Pa / sec. (Comparative Example 3-1) The pressure reduction rate during heating of the reactor was set to 400 Pa / sec. (Comparative Example 3-2) The pressure reduction rate during heating of the reactor was set to 10 Pa / sec.

[0079] [Table 4]

[0080] From the above results, it was found that when the reactor is heated to the CNT synthesis temperature after the substrate is inserted into the reactor, the pressure is reduced from atmospheric pressure to the reaction pressure at a reduction rate of 25 to 305 Pa / s, resulting in CNTs with excellent spinnability.

[0081] (Example 4-1) The same conditions as in Example 1-1 were used to obtain CNTs for spinning. The evaluation results of the spinnability are shown in the table below. In the following test example, the manufacturing method of Example 1-1 was used as a base, but some of the conditions for CNT synthesis were changed to obtain CNTs for spinning. The evaluation results of the spinnability are shown in the table below. (Example 4-2) The mixture ratio of acetylene gas and nitrogen gas was changed, and the C / N ratio in the reactor was set to 0.65. (Example 4-3) The mixture ratio of acetylene gas and nitrogen gas was changed, and the C / N ratio in the reactor was set to 0.40. (Example 4-4) The total flow rate of the supplied gas was changed to set the linear velocity of the supplied gas to 6.50 cm / sec, and the mixture ratio of acetylene gas and nitrogen gas was changed to set the C / N ratio in the reactor to 0.65. (Examples 4-5) The total flow rate of the supplied gas was changed to set the linear velocity of the supplied gas to 2.50 cm / sec, and the mixture ratio of acetylene gas and nitrogen gas was changed to set the C / N ratio in the reactor to 0.40. (Examples 4-6) The mixture ratio of acetylene gas and nitrogen gas was changed, and the C / N ratio in the reactor was set to 0.75. (Examples 4-7) The mixture ratio of acetylene gas and nitrogen gas was changed, and the C / N ratio in the reactor was set to 0.30. (Examples 4-8) The total flow rate of the supplied gas was changed to set the linear velocity of the supplied gas to 6.50 cm / sec, and the mixture ratio of acetylene gas and nitrogen gas was changed to set the C / N ratio in the reactor to 0.75. (Examples 4-9) The total flow rate of the supplied gas was changed to set the linear velocity of the supplied gas to 2.50 cm / sec, and the mixture ratio of acetylene gas and nitrogen gas was changed to set the C / N ratio in the reactor to 0.30.

[0082] [Table 5]

[0083] From the above results, as shown in Figure 7, it was found that CNTs with excellent spinnability can be obtained when the linear velocity of the supply gas during CNT synthesis is 2.50 to 6.50 cm / sec and the value obtained by dividing the partial pressure of the raw material gas in the supply gas by the partial pressure of the carrier gas (C / N ratio) is 0.40 to 0.65. In Figure 7, the circle, triangle, and diamond plots correspond to Examples 4-1 to 4-9. The dotted line indicates a particularly preferable region.

[0084] <Overall considerations regarding the test example> The present inventors have investigated the material constituting the catalyst layer and the gas supply conditions during CNT synthesis. As exemplified in Comparative Examples 1-3 and 1-4, it was discovered that when iron is used as the metal material constituting the catalyst layer, the catalyst layer is formed non-uniformly. The cause of this is thought to be that oxygen and moisture contained in the catalyst layer react with iron to partially form iron oxide with a low degree of oxidation. Therefore, the present inventors have investigated a method of using iron oxide instead of iron as the material for the catalyst layer and growing it into uniform particles. As a result of the investigation, it was found that uniform iron oxide particles can be formed by growing the iron oxide layer in an inert atmosphere at atmospheric pressure and then performing low-pressure CVD, and it became possible to synthesize continuous and spinnable CNTs with good reproducibility by using these uniform particles (Examples 1-1 to 1-3). As a result of further investigations, the present inventors have found that in the process of particle-forming the catalyst layer, by adjusting the temperature increase and decrease rates when heating and cooling the catalyst layer, it is possible to synthesize CNTs with excellent spinnability (Examples 2-1 to 2-5). The inventors further conducted extensive research and discovered that the pressure reduction rate of the reactor, the linear velocity of the supply gas supplied to the reactor, and the component ratio of the supply gas affect the synthesis of CNTs, making it possible to reproducibly synthesize CNTs that can be continuously spun by low-pressure CVD (Examples 3-1 to 3-3, Examples 4-1 to 4-5, etc.). [Industrial Applicability]

[0085] INDUSTRIAL APPLICABILITY The present invention makes it possible to produce CNTs for spinning with excellent spinnability by the LPCVD method, and is therefore industrially useful. [Explanation of symbols]

[0086] 1. Carbon nanotube manufacturing equipment (manufacturing equipment) 2. Heater 2A~2D Heating area 3. External reaction tube 4. Inner reaction tube 5...space 6...Exhaust pipe 7...Vacuum gauge 8. Vacuum pump 9. Supply gas introduction pipe 10A~10D...Thermometer 11. Insulation material 12 Vertical wafer boat 13. Lifting flange 14 Furnace cover 15...post 16...Groove 17...Base material

Claims

1. A method for producing carbon nanotubes for spinning by reduced pressure chemical vapor synthesis, comprising the steps of: forming a catalyst layer made of a metal oxide on at least a portion of a surface of a substrate; placing the substrate under an inert gas atmosphere at a pressure of 101 Pa or more and equal to or less than atmospheric pressure, and heating and cooling the substrate to granulate the metal oxide in the catalyst layer; and synthesizing carbon nanotubes on the surface of the catalyst layer that has been subjected to the metal oxide particulation. The method of heating and cooling the substrate comprises: First, the mixture is heated at a rate of 25° C. / min to 75° C. / min from room temperature to a predetermined temperature of 650° C. or higher at which the metal oxide is turned into particles, and then allowed to stand at the predetermined temperature. Next, in the first stage of temperature reduction, the temperature is reduced from the predetermined temperature to 650° C. at a temperature reduction rate of 35° C. / min to 85° C. / min. Then, in the second stage, the temperature is rapidly decreased from 650°C to 100°C or less at a rate of 145°C / min to 305°C / min. The substrate having the catalyst layer having the metal oxide particles is placed in a reactor; When the temperature is increased from a predetermined temperature of 500° C. or less to a predetermined temperature of 600° C. or more at which the carbon nanotubes can be synthesized, The method for producing CNT for spinning comprises reducing the pressure in the reactor from atmospheric pressure to a predetermined reaction pressure at a pressure reduction rate of 25 to 305 Pa / sec.

2. 2. The method for producing CNT for spinning according to claim 1, wherein the substrate on which the catalyst layer is formed is placed in an inert gas atmosphere at a pressure of 10,000 Pa or more and less than atmospheric pressure, and heated and cooled to granulate the metal oxide in the catalyst layer.

3. The substrate having the catalyst layer having the metal oxide particles is placed in a reactor; When a feed gas containing a raw material gas and a carrier gas is fed into the reactor to synthesize the carbon nanotubes, The linear velocity of the feed gas at the position of the substrate placed in the reactor is 2.50 to 6.50 cm / sec; and 3. The method for producing CNT for spinning according to claim 1, wherein the C / N ratio, which is expressed by the partial pressure of the raw material gas in the supply gas divided by the partial pressure of the carrier gas, is 0.40 to 0.65.

Citation Information

Patent Citations

  • Different diameter hole punching apparatus

    JP1981036337A

  • Carbon-based microstructures, aggregates of carbon-based microstructures, their uses, and methods for manufacturing them.

    JP4512750B2