Method for fixing carbon dioxide and method for producing cement admixture
A two-step carbonation process involving high-temperature and moisture-controlled carbon dioxide exposure effectively addresses inefficiencies in existing methods, achieving enhanced carbon dioxide fixation in cementitious materials.
Patent Information
- Application Number
- JP2023058356
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing methods for fixing carbon dioxide in cementitious materials suffer from inefficiencies such as low carbonation rates due to moisture evaporation and inefficient recovery processes, particularly at varying processing temperatures.
A two-step carbonation process is employed, where a cementitious hardened body is first contacted with carbon dioxide at high temperatures (300°C or higher) followed by adding water at a specific ratio and then mixing with carbon dioxide at lower temperatures (20-100°C) to enhance carbon dioxide fixation.
This method allows for efficient immobilization of carbon dioxide in cementitious materials, achieving higher carbonation rates and improved recovery by optimizing conditions for each step, thereby enhancing the fixation process.
Smart Images

Figure 2024145833000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for sequestration of carbon dioxide and a method for producing a cement mix. [Background technology]
[0002] In order to achieve carbon neutrality in 2050, the reduction of CO2 emitted from factories, including cement factories, is an issue. Therefore, a method for fixing CO2 as CaCO3 in materials containing a lot of calcium, such as cement hardened bodies, has been developed. For example, Patent Document 1 proposes a method of fixing carbon dioxide by contacting a cementitious hardened body with a carbon dioxide-containing gas having a moisture content of 1.5% or more and a temperature of 75 to 175°C. Patent Document 2 proposes a method of fixing CO2 in exhaust gas to solid particles by contacting a gas containing CO2 with an aggregate of solid particles containing CaO and / or Ca(OH)2. Patent Document 3 also proposes a method of obtaining cement paste by grinding waste concrete and separating aggregate and cement paste. Patent Document 4 describes a method of fixing CO2 by collecting materials obtained by crushing waste concrete, supplying water, stirring, and repeating alternating processes of wetting and drying. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-15659 A [Patent Document 2] JP 2000-197810 A [Patent Document 3] Patent Publication No. 2022-126254 [Patent Document 4] JP 2009-90198 A Summary of the Invention [Problem to be solved by the invention]
[0004] Patent Documents 1 and 2 describe supplying moisture to the cementitious hardened body to carbonate it, but even if moisture is supplied, the moisture evaporates depending on the treatment temperature, resulting in a low final carbonation rate. Patent Document 3 does not describe how to efficiently recover (in a short time and at a high carbonation rate) the cement paste in which CO2 has been fixed. The method of Patent Document 4 is inefficient because the material is repeatedly dried and wetted intermittently.
[0005] The present disclosure has been made in consideration of the above circumstances, and aims to provide a method for efficiently fixing CO2 in a cementitious hardened body, and a method for producing a cement mixture. [Means for solving the problem]
[0006] [1] A method for fixing carbon dioxide in a hardened cementitious material, comprising the steps of: a first carbonation step of contacting the cementitious hardened body with a gas containing carbon dioxide at 300°C or higher; the first carbonation step being followed by a second carbonation step including adding water to the cementitious hardened body in a solid-liquid ratio of 0.1 to 0.5, and contacting the cementitious hardened body to which water has been added with a gas containing carbon dioxide at 20 to 100°C. [2] The method according to [1], wherein the first step is carried out in a heating device. [3] The method according to [1] or [2], wherein the grain size of the cementitious hardened body is 40 mm or less. [4] The method according to any one of [1] to [3], wherein in the second carbonation step, the gas containing carbon dioxide is an exhaust gas, and the exhaust gas is cooled before being brought into contact with the cementitious hardened body. [5] A method for producing a cement mixture obtained by fixing carbon dioxide in a cementitious hardened body, comprising the steps of: a first carbonation step of contacting the cementitious hardened body with a gas containing carbon dioxide at 300°C or higher; the production method comprising: after the first carbonation step, adding water to the cementitious hardened body in a solid-liquid ratio of 0.1 to 0.5; and a second carbonation step including contacting the hardened cement body to which water has been added with a gas containing carbon dioxide at 20 to 100°C. Effect of the Invention
[0007] According to the present disclosure, it is possible to provide a method for efficiently fixing CO2 in a cementitious hardened body and a method for producing a cement mixture. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a diagram showing the relationship between the amount of CO2 absorbed and the reaction time for the first carbonation step in Example 1 and Comparative Example 1. [Diagram 2] FIG. 2 shows the results of a test in which carbonation was carried out by adding water at 20° C. [Diagram 3] FIG. 3 is a schematic diagram of the reaction apparatus used in the examples. [Figure 4] FIG. 4 is a diagram showing the relationship between reaction time and carbonation degree for each of the Reference Examples and Reference Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The method for fixing carbon dioxide in a cementitious hardened body of the present embodiment (hereinafter also referred to as a carbon dioxide fixation method) includes a first carbonation step of contacting the cementitious hardened body with a gas containing carbon dioxide at 300°C or higher, and a second carbonation step including, after the first carbonation step, adding water to the cementitious hardened body in a solid-liquid ratio of 0.1 to 0.5, and contacting the cementitious hardened body to which water has been added with gas at 20 to 100°C.
[0010] According to the present inventors, when carbon dioxide is fixed in the cementitious hardened body (carbonation of the cementitious hardened body), it has been found that the cementitious hardened body contains components that have different optimal conditions. Therefore, by selecting the optimal conditions for each component and carbonating the cementitious hardened body, the reaction can be carried out more efficiently.
[0011] (First carbonation process) In the first carbonation step, the temperature (treatment temperature) of the cementitious hardened body in contact with the gas containing carbon dioxide may be 350° C. or higher, or 400° C. or higher. The treatment temperature in the first carbonation step may be 800° C. or lower, or 700° C. or lower.
[0012] In the first carbonation step, water may be added to the cementitious hardened body, but water may not be added. When water is added from the viewpoint of workability, etc., the amount of water added may be 0.03 or less, 0.01, 0.005 or less, or 0.001 or less in terms of solid-liquid ratio.
[0013] The cementitious hardened body is a hardened body obtained by hardening a composition containing cement and water. The cementitious hardened body may be any of a hardened body of cement paste, a hardened body of mortar, and a hardened body of concrete. Examples of cement include various cements such as Portland cement, mixed cement, and ecocement. The cementitious hardened body may be waste materials such as waste building materials made of concrete or mortar, waste materials of hardened cement paste, and sludge generated in ready-mixed concrete. The cementitious hardened body may be a pulverized concrete mass. By using such waste materials, it is possible to effectively utilize resources. The shape and size of the cementitious hardened body are not particularly limited.
[0014] The age of the cementitious hardened body is not particularly limited, and may be, for example, 1 day or more, 7 days or more, 14 days or more, or 1 year or more.
[0015] The cementitious hardened body may contain water. The water content in the cementitious hardened body may be, for example, 15% by mass or more, or 20% by mass or more. The water content W in the cementitious hardened body may be, for example, 70% by mass or less, or 60% by mass or less.
[0016] The gas containing carbon dioxide is not particularly limited, and may be exhaust gas, exhaust gas from a factory, or exhaust gas discharged from equipment such as an incinerator or an electric dust collector. The inflow rate of the gas may be, for example, 0.5 to 5 L / min, or 1 to 3 L / min. The temperature of the gas may be 300° C. or higher, 350° C. or higher, or 400° C. or higher. When the reaction is carried out in a vessel, the temperature of the gas may be the temperature at the inlet of the vessel.
[0017] The carbon dioxide content in the gas may be 1% by volume or more, 5 to 50% by volume, or 10 to 30% by volume relative to the total volume of the gas. The gas may contain nitrogen, oxygen, volatile organic compounds, water (water vapor), etc. in addition to carbon dioxide.
[0018] The first carbonation step may be carried out in a container containing the cementitious hardened body. The container may be easily introduced with gas and may be included in a device capable of heating the cementitious hardened body in the container, such as a heating device such as a filling type heating device. For example, such a device may be a reactor equipped with a heater or having a function as a heater. The heater is not particularly limited, and may be an external heating device such as a rubber heater, or an internal heating device such as an infrared irradiation device.
[0019] The cementitious hardened body may be a pulverized product. The cementitious hardened body may be classified using a test sieve as specified in JIS Z8801-1:2019, or the average particle size (d50 on a volume basis or a number basis, etc.) may be measured using a laser particle size distribution measuring device. The particle size may be 40 mm or less, 10 mm or less, or 1 mm or less.
[0020] (Second carbonation process) In the second carbonation step, the cementitious hardened material carbonated in the first carbonation step is further carbonated under conditions different from those in the first carbonation step.
[0021] The second carbonation step is carried out in a state where water is added to the cementitious hardened body (i.e., to a mixture containing the cementitious hardened body and water). The amount of water added may be 0.15 to 0.40, or 0.15 to 0.35, in terms of solid-liquid ratio. In order to compensate for the water that evaporates during the second carbonation step, the second carbonation step may be carried out while adding water to the cementitious hardened body.
[0022] The gas containing carbon dioxide is not particularly limited, and may be exhaust gas, exhaust gas from a factory, or exhaust gas discharged from equipment such as an incinerator or an electric dust collector. The inflow rate of the gas may be, for example, 0.5 to 5 L / min, or 1 to 3 L / min. The temperature of the gas may be 20 to 120° C. When the reaction is carried out in a vessel, the temperature of the gas may be the temperature at the inlet of the vessel. The gas may be cooled before contacting with the mixture.
[0023] In the second carbonation step, the carbonation reaction may be carried out at a temperature (treatment temperature) of the mixture within the range of 20° C. to the boiling point of water (100° C. at normal pressure). The temperature of the mixture can be measured by a temperature measuring means such as a thermocouple arranged in the reactor.
[0024] The carbon dioxide content in the gas may be 1% by volume or more, 5 to 50% by volume, or 10 to 30% by volume relative to the total volume of the gas. The gas may contain nitrogen, oxygen, volatile organic compounds, water (water vapor), etc. in addition to carbon dioxide.
[0025] The method for adding water to the mixture is not particularly limited, and may be, for example, by supplying water (liquid water) to the mixture with a pump.
[0026] The second carbonation step may be performed in the above-mentioned reactor, but may also be performed in a grinding device. In the grinding device, the carbon dioxide fixation step may be performed while grinding the cementitious hardened body. In addition, after the carbon dioxide fixation step is performed in a heating device such as a filling type heating device, the cementitious hardened body in which carbon dioxide is fixed may be further ground by a grinding device. The grinding may be performed by a plurality of grinding devices. Note that both the first carbonation step and the second carbonation step may be performed in a grinding device. When the second carbonation step is performed in a grinding device, the grinding device may be provided with a moisture supplying means so that moisture can be supplied to the cementitious hardened body in the grinding device. In addition, when the second carbonation step is performed in a grinding device, the cementitious hardened body in which carbon dioxide is fixed may be collected by a dust collector as fine powder contained in the gas from the grinding device.
[0027] The method for producing a cement mixture obtained by fixing carbon dioxide in a cementitious hardened body of the present embodiment includes a first carbonation step of contacting the cementitious hardened body with a gas containing carbon dioxide at 300° C. or higher, and a second carbonation step including adding water to the cementitious hardened body in a solid-liquid ratio of 0.1 to 0.5 after the first carbonation step, and contacting the hardened cement body to which water has been added with a gas containing carbon dioxide at 20 to 100° C. That is, the cement mixture of the present embodiment may be one produced by the carbon dioxide fixation method of the present embodiment.
[0028] There are no particular limitations on the use of the cement admixture as long as it is used by mixing with cement, but it can also be used as a solidification material such as a soil improvement material. EXAMPLES
[0029] The present disclosure will be described in more detail below with reference to examples and comparative examples, but the present disclosure is not limited to the following examples.
[0030] <Preparation of hardened cementitious material> Ordinary Portland cement was mixed with water to achieve a water-cement ratio (W / C) of 0.4, and then cured for 28 days. After curing, the cementitious hardened body was pulverized in a ball mill until the particle size was 0.3 mm or less, obtaining a cement paste powder. The particle size (average particle diameter) of the cementitious hardened body was measured using a laser particle size distribution analyzer. Table 1 shows the chemical composition of the cement paste powder.
[0031] [Table 1]
[0032] Example 1 <First carbonation process> Cement paste powder (25μg) was placed in a sample container and placed in a TG-DTA (thermogravimetric differential thermal analyzer). N2 gas was passed through the TG-DTA at a flow rate of 200mL / min, and the sample was heated to 500℃ at a heating rate of 50℃ / min. When the temperature reached 500℃, the gas passed through was switched to gas with a CO2 concentration adjusted to 25% using a N2 cylinder and a CO2 cylinder. The time when the gas was switched was set as the reaction start time, and the amount of CO2 absorbed by the cement paste powder was measured from the weight change. The results are shown in Figure 1. Carbonation at high temperatures proceeds at an extremely fast rate, but the maximum amount of CO2 absorbed was about 6% of the weight of the cement paste.
[0033] <Second carbonation step> The cement paste powder that had been carbonated at 500°C was mixed well with water so that the solid-liquid ratio was 0.25, then placed in a sample container and placed in the TG-DTA. Gas with a CO2 concentration adjusted to 25% was passed through the TG-DTA at a flow rate of 200mL / min using a N2 cylinder and a CO2 cylinder, and the amount of CO2 absorbed was calculated by measuring the weight change while maintaining the temperature inside the TG-DTA at 20°C. The results are shown in Figure 2. 2.2% of CO2 was absorbed after a reaction time of 8 minutes.
[0034] Comparative Example 1 Water was thoroughly mixed into the cement paste powder so that the solid-liquid ratio was 0.25, and 31 mg of the sample was placed in a sample container and placed in the TG-DTA. Gas with a CO2 concentration adjusted to 25% was passed through the TG-DTA at a flow rate of 200 mL / min using a N2 cylinder and a CO2 cylinder, and the amount of CO2 absorbed was calculated by measuring the weight change while maintaining the temperature inside the TG-DTA at 20°C. The results are shown in Figure 1. When carbonation is performed by adding water at room temperature, the rate at which carbonation progresses is slow, but the amount of CO2 absorbed after a reaction time of 10 minutes is about 7% of the weight of the cement paste.
[0035] The relationship between the amount of CO2 absorbed and the reaction time is shown in FIG. 1 for the first carbonation step of Example 1 ("500°C" in the figure) and Comparative Example 1 (W / P=0.25_20°C in the figure). If a large amount of CO2 is to be fixed in the cementitious hardened body, it is desirable to add water and perform carbonation at room temperature. However, as shown in the result of Comparative Example 1 in FIG. 1, the amount of CO2 fixed in 10 minutes is about 7%. Therefore, carbonation can be performed efficiently by adding water to the cementitious hardened body and performing carbonation at room temperature after carbonation at high temperature. As shown in FIG. 1, 6% of CO2 is absorbed in about 2 minutes in carbonation at 500°C. Then, 2.2% of CO2 is fixed by performing carbonation at room temperature for about 8 minutes as shown in FIG. The amount of CO2 absorbed in the total reaction time of 10 minutes is about 8.2%, and CO2 can be absorbed in a short time compared to the carbonation reaction at room temperature.
[0036] <Reaction Apparatus> Carbon dioxide was fixed in a reactor. A schematic diagram of the reactor is shown in Figure 3. The reactor has the following configuration: First, the reaction device 10 has a reactor 1 for performing a CO2 fixation reaction on a sample (a mixture of cement paste powder and water). A Hobart mixer 2 is attached to the reactor 1, and it is possible to stir the sample in the reactor. A CO2 cylinder 3 and an N2 cylinder 4 are connected to the inlet of the reactor 1, and it is possible to flow gas into the reactor 1. The reaction device 10 has a pump 5. The pump 5 is connected to the reactor 1 and a tank 6 containing water, and it is possible to share water with the reactor 1. A rubber heater 7 is attached to the reactor 1, and it is possible to heat the reactor 1. A temperature controller 8 is further connected to the rubber heater, and a thermocouple 9 attached inside the reactor is connected to the temperature controller 8. This makes it possible to manage the temperature of the sample in the reactor by controlling the temperature of the rubber heater with the temperature controller 8 while measuring the temperature inside the reactor 1 with the thermocouple 9.
[0037] <Carbon dioxide fixation (carbonation) reaction> The prepared cement paste powder (200 g) was put into the reactor of the above-mentioned reactor and stirred with a Hobart mixer. The temperature inside the reactor was adjusted to 20°C with a rubber heater installed at the bottom of the reactor. Gas with a CO2 concentration adjusted to 20% by volume using N2 and CO2 cylinders was passed into the reactor at a flow rate of 2.0 L / min, and water was added so as to obtain the W / P value in Table 2, and a CO2 fixation reaction was performed. During the fixation reaction, samples were collected at regular intervals and the carbonation degree was measured using the following formula (1) with a thermogravimetric differential thermal analyzer (TG-DTA). W / P is the mass ratio of water (W) to cement paste powder (P).
[0038] <How to calculate carbonation> The carbonation degree was calculated using the following formula (1).
number
[0039] (Reference Examples 1 to 5, Reference Comparative Examples 1 and 2) Table 2 shows the W / P and carbonation degree 4 hours after the start of the reaction for each of the reference and reference comparative examples. Figure 4 also shows the relationship between time and carbonation degree for each of the reference and reference comparative examples. As shown in Figure 2, it was confirmed that when the W / P was 0.1 to 0.5, treatment with a high carbonation degree could be achieved in a short time. On the other hand, it was found that when the solid-liquid ratio was increased, the initial carbonation was slow.
[0040] [Table 2] [Explanation of symbols]
[0041] 10...Reactor, 1...Reactor, 2...Hobart mixer, 3...CO2 cylinder, 4...N2 cylinder, 5...Pump, 6...Tank, 7...Rubber heater, 8...Temperature controller, 9...Thermocouple.
Claims
1. A method for fixing carbon dioxide in a hardened cementitious material, comprising the steps of: a first carbonation step of contacting the cementitious hardened body with a gas containing carbon dioxide at 300°C or higher; The method comprises: after the first carbonation step, adding water to the cementitious hardened body in a solid-liquid ratio of 0.1 to 0.5; and a second carbonation step including contacting the cementitious hardened body to which water has been added with a gas containing carbon dioxide at 20 to 100°C.
2. The method of claim 1 , wherein the first step is carried out in a heating device.
3. The method according to claim 1 or 2, wherein the particle size of the cementitious hardened body is 40 mm or less.
4. The method according to claim 1 or 2, wherein in the second carbonation step, the gas containing carbon dioxide is exhaust gas, and the exhaust gas is cooled before being contacted with the cementitious hardened body.
5. A method for producing a cement mixture obtained by fixing carbon dioxide in a cementitious hardened body, comprising the steps of: a first carbonation step of contacting the cementitious hardened body with a gas containing carbon dioxide at 300°C or higher; The method includes, after the first carbonation step, adding water to the cementitious hardened body in a solid-liquid ratio of 0.1 to 0.5, and a second carbonation step including contacting the hardened cement body to which water has been added with a gas containing carbon dioxide at 20 to 100°C.
Citation Information
Patent Citations
Method for lessening carbon dioxide gas emission
JP2000197810A
Method for fixing carbon dioxide
JP2009090198A
Stabilization method of carbon dioxide
JP2020015659A
Method for recovering cement paste from waste concrete
JP2022126254A