Photosensitive resin composition, cured film made by curing photosensitive resin composition, substrate with cured film, and method for producing substrate with cured film
The photosensitive resin composition, utilizing a cyclic siloxane compound and alkali-soluble resin, addresses the challenges of high definition and adhesion in display technologies by forming a cured film with low reflectance and improved heat and light resistance.
Patent Information
- Application Number
- JP2023058458
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Existing display technologies face challenges in achieving high definition with low reflectance and improved adhesion to substrates, particularly in ultra-high definition displays, due to the use of conventional black matrices that do not meet the requirements for thinner lines and adequate adhesion, and epoxy compounds that lack sufficient hydrophobicity and resistance to developing solutions.
A photosensitive resin composition incorporating a cyclic siloxane compound with multiple epoxy groups, an alkali-soluble resin with unsaturated groups, and inorganic fine particles, along with a photopolymerization initiator, to form a cured film pattern that achieves low reflectance, high definition, and improved heat and light resistance.
The composition enables the formation of a cured film pattern with low reflectance and high definition, exhibiting excellent adhesion and resistance to heat and light, suitable for ultra-high definition displays.
Smart Images

Figure 2024145891000001 
Figure 2024145891000002 
Figure 2024145891000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a photosensitive resin composition, a cured film obtained by curing the photosensitive resin composition, a substrate with a cured film, and a method for producing a substrate with a cured film. [Background technology]
[0002] In recent years, with the development of mobile terminals, there has been an increase in display devices having touch panels or liquid crystal panels, etc., for use outdoors or in vehicles. In such display devices, a light-shielding film is provided on the outer frame of the touch panel to block light leakage from the periphery of the liquid crystal panel on the back, and a light-shielding film (black matrix) is provided on the liquid crystal panel to suppress light leakage from the screen when displaying black and to suppress color mixing between adjacent color resists.
[0003] In display devices and the like, in order to suppress light leakage and the like and improve the visibility of the screen of the display device and the like, the concentration of the black pigment in the light-shielding film may be increased to increase the light-shielding property of the light-shielding film (reduce the light transmittance of the light-shielding film). Since the refractive index of the black pigment is higher than that of the transparent substrate and the curable resin, increasing the concentration of the black pigment in the light-shielding film increases the reflectance when viewed from the surface of the transparent substrate on which the light-shielding film is formed. For this reason, a light-shielding film having not only high light-shielding property but also low reflectance is desired. In addition, it is useful to provide low reflectance not only for the application of photoresists (black resists) that form black matrices, but also for clear resists and RGB resists, because reflection inside the display can be suppressed.
[0004] In order to reduce the reflectance in applications such as black matrices, a technique of blending transparent particles such as silica, which has a smaller refractive index than black pigments and curable resins, has been proposed (for example, Patent Document 1). However, although blending silica into a photosensitive resin composition is useful for reducing the reflectance, there is a concern that it may affect adhesion to the substrate to some extent.
[0005] In recent years, ultra-high definition (400 pixels per inch or more) technology is required to obtain full high definition resolution for small and medium-sized panels such as smartphones, and high definition has become an essential technological trend. To achieve high definition, it is necessary to make the size of each red, green, and blue pixel finer, but it is necessary to maintain the aperture ratio of the color filter (the area ratio of RGB pixels through which backlight light passes) in order to increase brightness, and at the same time, thinning of the black matrix is also required. That is, while the line width of the black matrix was previously mainstream at 6 to 8 μm, recently, 7 μm or less or 4 to 5 μm sizes are required. Furthermore, for example, high definition of 1000 ppi or more is required for displays for new devices such as augmented reality (AR) and virtual reality (VR), so the line width of the black matrix is required to be 3 μm or less. Previous black matrices aimed at reducing reflectance have not necessarily satisfied the recent demand for higher definition (thinner lines), and there is a demand for further improvement in adhesion (thin-line adhesion) to glass substrates and the like.
[0006] In this regard, in the past, when forming a resin film pattern by photolithography using a substrate with a heat-resistant temperature of 140° C. or less, in order to form a resin film pattern that is excellent in development adhesion and linearity, and is excellent in solvent resistance and alkali resistance, even when heat-treated (thermal curing) at a relatively low temperature, a technique has been proposed in which a predetermined amount of an epoxy compound, a curing agent for the epoxy compound, and / or a curing accelerator are used together with components such as an alkali-soluble resin and a photopolymerization initiator in order to form a resin film pattern that is excellent in development adhesion and linearity, and is excellent in solvent resistance and alkali resistance, etc. (for example, Patent Document 2). However, when such an epoxy compound or a curing agent is used, the hydrophobicity is not sufficient, and there is a demand for improvement in resistance to the developer, and there is room for further improvement in high definition and fine line adhesion. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2016-161926 A [Patent Document 2] JP 2019-070720 A [Patent Document 3] JP 2018-004920 A Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made in consideration of the above-mentioned problems, and in particular, it has been newly discovered that as a photosensitive resin composition capable of forming a cured film pattern which achieves both low reflectance and high definition on the film surface and which also has heat resistance and light resistance, the composition can be blended with inorganic fine particles to reduce the reflectance of the coating film surface, and a cyclic siloxane compound having two or more epoxy groups in the molecule can be blended in place of epoxy compounds that have been conventionally used.
[0009] It has already been known that a cyclic siloxane compound having two or more epoxy groups in a molecule is blended into a photosensitive resin composition (Patent Document 3), but it has only been disclosed as an example of a multifunctional crosslinkable compound (D) having multiple epoxy groups or oxetanyl groups for the purpose of forming a cured film that generates a small amount of gas as a bank for dividing an emitting layer in an organic EL element. In other words, there has been no disclosure or suggestion that blending the siloxane compound contributes to high definition and fine line adhesion in the formation of a cured film pattern by photolithography. [Means for solving the problem]
[0010] That is, the gist of the present invention is as follows. [1] (A) an unsaturated group-containing alkali-soluble resin; (B) a photopolymerizable compound having at least two unsaturated bonds; (C) a cyclic siloxane compound having two or more epoxy groups in the molecule; (D) a photopolymerization initiator; (G) inorganic fine particles; (H) a solvent; A photosensitive resin composition comprising: [2] The photosensitive resin composition according to [1], wherein the component (C) is a cyclic siloxane compound represented by general formula (1). [ka] [R in general formula (1)] a and R b represents a monovalent group containing an epoxy group or a monovalent hydrocarbon group having 1 to 20 carbon atoms. a and R b At least two of R are monovalent groups containing an epoxy group. a and R b may be the same or different, and n represents an integer of 3 or more and 10 or less. [3] The photosensitive resin composition according to [1], wherein the component (A) comprises a polymer containing a unit represented by the following general formula (2) and a unit represented by the general formula (3), the polymer containing 5 to 90 mol % of the unit represented by the general formula (2) and 10 to 95 mol % of the unit represented by the general formula (3), and having a weight average molecular weight of 3,000 to 50,000 and an acid value of 30 to 200 mg / KOH: [ka] [ka] (However, R c , R f and R h R independently represents a hydrogen atom or a methyl group. d represents a monovalent hydrocarbon group having 1 to 20 carbon atoms, and the hydrocarbon group may contain an ether bond, an ester bond, or a urethane bond therein. d R is a dicyclopentanyl group or a dicyclopentenyl group that accounts for 40 mol % or more of all the units represented by the general formula (2). e represents a divalent hydrocarbon group having 2 to 10 carbon atoms. p represents the number 0 or 1. X represents a hydrogen atom or -OC-L-(COOH) kgroup (wherein L represents a divalent or trivalent carboxylic acid residue, and k is 1 to 2). [4] (F) The photosensitive resin composition according to [1], which contains one or more light-shielding materials selected from the group consisting of black organic pigments, mixed-color organic pigments, and black inorganic pigments. [5] (E) The photosensitive resin composition according to [1], further comprising a curing agent and / or a curing accelerator. [6] The photosensitive resin composition according to [1], wherein the component (G) has a refractive index of 1.20 to 1.50 and an average particle size of 1 to 150 nm. [7] A cured film obtained by curing the photosensitive resin composition according to any one of [1] to [6]. [8] A substrate having the cured film according to [7] on the substrate. [9] A method for producing a substrate with a cured film by forming a cured film pattern on a substrate, comprising the steps of: A method for producing a substrate with a cured film, comprising applying the photosensitive resin composition according to any one of [1] to [6] onto a substrate, exposing the composition through a photomask, removing unexposed areas by development, and heating the composition to form a cured film pattern. Effect of the Invention
[0011] According to the photosensitive resin composition of the present invention, it is possible to form a cured film pattern that achieves both low reflectance and high definition of the film surface. In addition, it is possible to form a cured film pattern that is also excellent in heat resistance and light resistance. In addition, it is possible to provide a method for producing a substrate with a cured film by forming such a cured film pattern. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] As described above, the photosensitive resin composition of the present invention contains, as essential components, at least (A) an unsaturated group-containing alkali-soluble resin, (B) a photopolymerizable compound having at least two unsaturated bonds, (C) a cyclic siloxane compound having two or more epoxy groups in the molecule, (D) a photopolymerization initiator, (G) inorganic fine particles, and (H) a solvent. In addition, the photosensitive resin composition of the present invention may contain, as necessary, (F) one or more light-shielding materials selected from the group consisting of black organic pigments, mixed-color organic pigments, and black inorganic pigments, and (E) a curing agent and / or a curing accelerator. Each of the components used will be described in detail below.
[0013] <(A) Unsaturated group-containing alkali-soluble resin>
[0014] The unsaturated group-containing alkali-soluble resin (A) contained in the photosensitive resin composition of the present invention will now be described.
[0015] The unsaturated group-containing alkali-soluble resin (A) can be used without any particular limitation so long as it has an acid value sufficient to impart alkali developability and can be combined with the photopolymerizable compound, component (B), to provide appropriate photocurability.
[0016] Examples of component (A) include an alkali-soluble resin having a carboxy group and a polymerizable unsaturated group in one molecule, represented by general formula (4), which is obtained by reacting a reaction product of an epoxy compound (a-1) having two epoxy groups in one molecule and an unsaturated group-containing monocarboxylic acid, represented by general formula (9), with a dicarboxylic acid or tricarboxylic acid or an acid monoanhydride thereof (b), and a tetracarboxylic acid or an acid dianhydride thereof (c). The alkali-soluble resin represented by general formula (4) has excellent heat resistance due to the presence of many aromatic rings. In addition, a highly precise pattern can be obtained. Another example of the component (A) may be a (meth)acrylate resin, which is a polymer containing a unit represented by general formula (2) and a unit represented by general formula (3), as described below. Note that "(meth)acrylate" is a general term for acrylate and methacrylate, and means one or both of them. The same applies to (meth)acrylic acid, etc., described below.
[0017] First, the unsaturated group-containing alkali-soluble resin represented by the following general formula (4) will be described. [ka]
[0018] In formula (4), R1, R2, R3, and R4 are each independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, a halogen atom, or a phenyl group, R5 is a hydrogen atom or a methyl group, A is -CO-, -SO2-, -C(CF3)2-, -Si(CH3)2-, -CH2-, -C(CH3)2-, -O-, a fluorene-9,9-diyl group, or a direct bond, Y is a tetravalent carboxylic acid residue, and Z is each independently a hydrogen atom or a substituent represented by general formula (5), with the proviso that at least one of Z is a substituent represented by general formula (5), and q is an integer of 1 to 20.
[0019] [ka]
[0020] In formula (5), W is a divalent or trivalent carboxylic acid residue, and m is 1 or 2.
[0021] A method for producing an alkali-soluble resin having a carboxy group and a polymerizable unsaturated group in one molecule, represented by general formula (4) (hereinafter, simply referred to as "alkali-soluble resin represented by general formula (4)") will be described in detail.
[0022] First, an epoxy compound (a-1) having two epoxy groups in one molecule and represented by general formula (9) (hereinafter also simply referred to as "epoxy compound (a-1)") is reacted with an unsaturated group-containing monocarboxylic acid (e.g., (meth)acrylic acid) to obtain a diol compound containing a polymerizable unsaturated group.
[0023] [ka]
[0024] In formula (9), R1, R2, R3 and R4 each independently represent a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, a halogen atom or a phenyl group, and A represents -CO-, -SO2-, -C(CF3)2-, -Si(CH3)2-, -CH2-, -C(CH3)2-, -O-, a fluorene-9,9-diyl group or a direct bond.
[0025] The epoxy compound (a-1) is an epoxy compound having two glycidyl ether groups obtained by reacting a bisphenol with epichlorohydrin.
[0026] Examples of bisphenols used as raw materials for the epoxy compound (a-1) include bis(4-hydroxyphenyl) ketone, bis(4-hydroxy-3,5-dimethylphenyl) ketone, bis(4-hydroxy-3,5-dichlorophenyl) ketone, bis(4-hydroxyphenyl) sulfone, bis(4-hydroxy-3,5-dimethylphenyl) sulfone, bis(4-hydroxy-3,5-dichlorophenyl) sulfone, bis(4-hydroxyphenyl) hexafluoropropane, and bis(4-hydroxy-3,5-dimethylphenyl) hexafluoropropane. propane, bis(4-hydroxy-3,5-dichlorophenyl)hexafluoropropane, bis(4-hydroxyphenyl)dimethylsilane, bis(4-hydroxy-3,5-dimethylphenyl)dimethylsilane, bis(4-hydroxy-3,5-dichlorophenyl)dimethylsilane, bis(4-hydroxyphenyl)methane, bis(4-hydroxy-3,5-dichlorophenyl)methane, bis(4-hydroxy-3,5-dibromophenyl)methane, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl) 2,2-bis(4-hydroxy-3,5-dichlorophenyl)propane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 2,2-bis(4-hydroxy-3-chlorophenyl)propane, bis(4-hydroxyphenyl)ether, bis(4-hydroxy-3,5-dimethylphenyl)ether, bis(4-hydroxy-3,5-dichlorophenyl)ether, 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxy-3-chlorophenyl)fluorene, 9,9-bis(4-hydroxy-3-bromophenyl)fluorene, 9,9-bis(4-hydroxy-3-fluorophenyl)fluorene, 9,9-bis(4-hydroxy-3-methoxyphenyl)fluorene, 9,9-bis(4-hydroxy-3,5-dimethylphenyl)fluorene, 9,9-bis(4-hydroxy-3,5-dichlorophenyl)fluorene, 9,9-bis(4-hydroxy-3,5-dibromophenyl)fluorene, 4,4'-biphenol, 3,3'-biphenol, and the like.These may be used alone or in combination of two or more.
[0027] Examples of the unsaturated group-containing monocarboxylic acid compound include, in addition to acrylic acid and methacrylic acid, compounds obtained by reacting acrylic acid or methacrylic acid with an acid monoanhydride such as succinic anhydride, maleic anhydride, or phthalic anhydride.
[0028] The reaction between the epoxy compound (a-1) and the unsaturated group-containing monocarboxylic acid compound can be carried out by a known method. For example, JP-A-4-355450 describes that a diol compound containing a polymerizable unsaturated group can be obtained by using about 2 moles of (meth)acrylic acid per mole of an epoxy compound having two epoxy groups. In the present invention, the compound obtained by the above reaction is a diol compound containing a polymerizable unsaturated group, and is a diol (d) containing a polymerizable unsaturated group represented by general formula (10) (hereinafter, also simply referred to as "diol (d) represented by general formula (10)").
[0029] [ka]
[0030] In formula (10), R1, R2, R3 and R4 are each independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, a halogen atom or a phenyl group; R5 is a hydrogen atom or a methyl group; and A is -CO-, -SO2-, -C(CF3)2-, -Si(CH3)2-, -CH2-, -C(CH3)2-, -O-, a fluorene-9,9-diyl group or a direct bond.
[0031] In the production of the alkali-soluble resin represented by the general formula (4) by synthesis of the diol (d) represented by the general formula (10), the subsequent addition reaction of a polyvalent carboxylic acid or anhydride thereof, and further reaction with a monofunctional epoxy compound having a polymerizable unsaturated group reactive with a carboxy group, the reaction is usually carried out in a solvent using a catalyst as necessary.
[0032] Examples of the solvent include cellosolve-based solvents such as ethyl cellosolve acetate and butyl cellosolve acetate, high-boiling ether or ester-based solvents such as diglyme, ethyl carbitol acetate, butyl carbitol acetate, and propylene glycol monomethyl ether acetate, and ketone-based solvents such as cyclohexanone and diisobutyl ketone. There are no particular limitations on the reaction conditions such as the solvent and catalyst used, but it is preferable to use, for example, a solvent that does not have a hydroxyl group and has a boiling point higher than the reaction temperature as the reaction solvent.
[0033] In addition, it is preferable to use a catalyst in the reaction between a carboxy group and an epoxy group. JP-A-9-325494 describes ammonium salts such as tetraethylammonium bromide and triethylbenzylammonium chloride, and phosphines such as triphenylphosphine and tris(2,6-dimethoxyphenyl)phosphine.
[0034] Next, the diol (d) represented by the general formula (10) is reacted with a tetracarboxylic acid or its dianhydride (b), and a dicarboxylic acid or tricarboxylic acid or its anhydride (c) to obtain an alkali-soluble resin having a carboxy group and a polymerizable unsaturated group in one molecule represented by the general formula (4).
[0035] The acid component used to synthesize the alkali-soluble resin represented by the general formula (4) is a polyvalent acid component capable of reacting with the hydroxyl group in the diol (d) molecule represented by the general formula (10), and it is necessary to use a dicarboxylic acid or tricarboxylic acid or an acid monoanhydride thereof (b) in combination with a tetracarboxylic acid or an acid dianhydride thereof (c). The carboxylic acid residue of the acid component may be either a saturated or unsaturated hydrocarbon group. In addition, these carboxylic acid residues may contain bonds containing heteroatoms such as -O-, -S-, and carbonyl groups.
[0036] As the dicarboxylic acid or tricarboxylic acid or their monoanhydrides (b), chain hydrocarbon dicarboxylic acids or tricarboxylic acids, alicyclic hydrocarbon dicarboxylic acids or tricarboxylic acids, aromatic hydrocarbon dicarboxylic acids or tricarboxylic acids, or their monoanhydrides, etc. can be used.
[0037] Examples of monoanhydrides of chain hydrocarbon dicarboxylic acids or tricarboxylic acids include monoanhydrides of succinic acid, acetylsuccinic acid, maleic acid, adipic acid, itaconic acid, azelaic acid, citramalic acid, malonic acid, glutaric acid, citric acid, tartaric acid, oxoglutaric acid, pimelic acid, sebacic acid, suberic acid, diglycolic acid, and the like, and monoanhydrides of dicarboxylic acids or tricarboxylic acids having any substituent introduced therein. Examples of monoanhydrides of alicyclic dicarboxylic acids or tricarboxylic acids include monoanhydrides of cyclobutanedicarboxylic acid, cyclopentanedicarboxylic acid, hexahydrophthalic acid, tetrahydrophthalic acid, norbornanedicarboxylic acid, and the like, and monoanhydrides of dicarboxylic acids or tricarboxylic acids having any substituent introduced therein. Examples of monoanhydrides of aromatic dicarboxylic acids or tricarboxylic acids include monoanhydrides of phthalic acid, isophthalic acid, trimellitic acid, and the like, and monoanhydrides of dicarboxylic acids or tricarboxylic acids having any substituent introduced therein.
[0038] Among the dicarboxylic acid or tricarboxylic acid monoanhydrides, succinic acid, itaconic acid, tetrahydrophthalic acid, hexahydrotrimellitic acid, phthalic acid, and trimellitic acid are preferred, and succinic acid, itaconic acid, and tetrahydrophthalic acid are more preferred.In addition, it is preferred to use the dicarboxylic acid or tricarboxylic acid monoanhydrides thereof.The above-mentioned dicarboxylic acid or tricarboxylic acid monoanhydrides may be used alone or in combination of two or more kinds.
[0039] As the tetracarboxylic acid or its dianhydride (c), a chain hydrocarbon tetracarboxylic acid, an alicyclic hydrocarbon tetracarboxylic acid, an aromatic hydrocarbon tetracarboxylic acid, or their dianhydrides can be used.
[0040] Examples of the chain hydrocarbon tetracarboxylic acid include butane tetracarboxylic acid, pentane tetracarboxylic acid, hexane tetracarboxylic acid, and chain hydrocarbon tetracarboxylic acid having a substituent such as an alicyclic hydrocarbon group or an unsaturated hydrocarbon group introduced therein. Examples of the alicyclic tetracarboxylic acid include cyclobutane tetracarboxylic acid, cyclopentane tetracarboxylic acid, cyclohexane tetracarboxylic acid, cycloheptane tetracarboxylic acid, norbornane tetracarboxylic acid, and alicyclic tetracarboxylic acid having a substituent such as an chain hydrocarbon group or an unsaturated hydrocarbon group introduced therein. Examples of the aromatic tetracarboxylic acid include pyromellitic acid, benzophenone tetracarboxylic acid, biphenyl tetracarboxylic acid, diphenyl ether tetracarboxylic acid, diphenyl sulfone tetracarboxylic acid, and the like.
[0041] Among the tetracarboxylic acids or their dianhydrides, biphenyltetracarboxylic acid, benzophenonetetracarboxylic acid, and diphenylethertetracarboxylic acid are preferred, and biphenyltetracarboxylic acid and diphenylethertetracarboxylic acid are more preferred. In addition, among the tetracarboxylic acids or their dianhydrides, it is preferred to use the dianhydrides. The above-mentioned tetracarboxylic acids or their dianhydrides may be used alone or in combination of two or more.
[0042] The reaction of the diol (d) represented by the general formula (10) with the acid components (b) and (c) is not particularly limited, and any known method can be used. For example, JP-A-9-325494 describes a method in which an epoxy (meth)acrylate is reacted with a tetracarboxylic dianhydride at a reaction temperature of 90 to 140° C.
[0043] Here, it is preferable to react the compound so that the terminals of the compound become carboxy groups, in such a manner that the molar ratio of the diol (d) represented by the general formula (10), the dicarboxylic acid or tricarboxylic acid or an acid monoanhydride thereof (b), and the tetracarboxylic acid dianhydride (c) is (d):(b):(c)=1:0.01-1.0:0.2-1.0.
[0044] For example, when (b) acid monoanhydride and (c) acid dianhydride are used, it is preferable to react them so that the molar ratio [[(b) / 2+(c)] / (d)] of the amount of the acid component [(b) / 2+(c)] to the diol (d) represented by the general formula (5) is 0.5 to 1.0. Here, when the molar ratio exceeds 0.5, the content of the diol compound containing unreacted polymerizable unsaturated groups is not increased, so the stability over time of the photosensitive resin composition can be improved. On the other hand, when the molar ratio is 1.0 or less, the terminal of the alkali-soluble resin represented by the general formula (4) does not become an acid anhydride, so that the content of the unreacted acid dianhydride can be suppressed from increasing, so the stability over time of the photosensitive resin composition can be improved. In addition, in order to adjust the acid value and molecular weight of the alkali-soluble resin represented by the general formula (4), the molar ratio of each component (d), (b) and (c) can be arbitrarily changed within the above-mentioned range.
[0045] The acid value of the alkali-soluble resin represented by the general formula (4) is preferably in the range of 20 to 180 mgKOH / g, and more preferably 80 mgKOH / g or more and 120 mgKOH / g or less. When the acid value is 20 mgKOH / g or more, residues are less likely to remain during alkaline development, and when the acid value is 180 mgKOH / g or less, the penetration of the alkaline developer is not too fast, so peeling development can be suppressed. The acid value can be determined by titration with a 1 / 10N-KOH aqueous solution using a potentiometric titrator "COM-1600" (manufactured by Hiranuma Sangyo Co., Ltd.).
[0046] The weight average molecular weight (Mw) of the alkali-soluble resin represented by the general formula (4) in terms of polystyrene, as measured by gel permeation chromatography (GPC) (HLC-8220GPC, manufactured by Tosoh Corporation), is usually 1000 to 100000, preferably 2000 to 20000, and more preferably 2000 to 6000. When the weight average molecular weight is 1000 or more, it is possible to suppress a decrease in the adhesion of the pattern during alkali development. In addition, when the weight average molecular weight is 100000 or less, it is easy to adjust the solution viscosity of the photosensitive resin composition to a suitable level for application, and alkali development does not take too long.
[0047] The alkali-soluble resin represented by the general formula (4) may be used alone in the component (A), or a (meth)acrylate resin described later may be used instead, or these may be used in combination. The type of alkali-soluble resin used can be appropriately selected depending on the desired application, characteristics, etc., but when the content of the alkali-soluble resin represented by the general formula (4) is high, the heat resistance is particularly excellent and a high-definition pattern can be formed. From the viewpoint of imparting these characteristics, it is preferable that the content of the alkali-soluble resin represented by the general formula (4) is high, and the content of the alkali-soluble resin represented by the general formula (4) is preferably 50 to 100 mass%, more preferably 75 to 100 mass%, and particularly preferably 85 to 100 mass%, based on the mass of the total of the component (A) (for example, the total of the alkali-soluble resin represented by the general formula (4) and the (meth)acrylate resin described later).
[0048] [(Meth)acrylate resin] Next, a (meth)acrylate resin will be described as another example of the component (A).
[0049] By containing a (meth)acrylate resin instead of the alkali-soluble resin represented by the general formula (4) or together with the alkali-soluble resin represented by the general formula (4), the number of aromatic rings can be reduced and deterioration due to light can be relatively suppressed, so that light resistance can be improved. In addition, since the refractive index is lower than that of the alkali-soluble resin represented by the general formula (4), it is advantageous for reducing reflectance. When these resins are used in combination, it is also possible to improve light resistance and reduce reflectance while maintaining heat resistance and high-definition pattern formation to a certain extent.
[0050] Such a (meth)acrylate resin is a polymer containing a unit represented by the following general formula (2) and a unit represented by the general formula (3), and has a carboxyl group and a polymerizable unsaturated group in the side chain. That is, the (meth)acrylate resin is a random copolymer in which r units and s units of the units represented by the general formula (2) and the units represented by the general formula (3) are linked together (where r and s are any integers). It is also possible to contain a third component unit other than these, and for example, it is possible to further contain a unit derived from an unsaturated group-containing carboxylic acid represented by the general formula (8) described later, a styrene or a monomaleimide which may have a substituent on the phenyl group, as a copolymerization component. Examples of the substituent that may be present on the phenyl group of the styrene include an alkyl group having 1 to 10 carbon atoms. Examples of the monomaleimide include N-phenylmaleimide, N-cyclohexylmaleimide, N-laurylmaleimide, and N-(4-hydroxyphenyl)maleimide. Of these third component units, it is preferable to use styrene and N-phenylmaleimide. The ratio of the unit represented by the general formula (2) and the unit represented by the general formula (3) is preferably 5 to 90 mol %, more preferably 20 to 70 mol %, when the total of the whole polymer consisting of the unit represented by the general formula (2), the unit represented by the general formula (3), and the unit of the third component is taken as 100 mol %. The ratio of the unit represented by the general formula (3) is preferably 10 to 95 mol %, more preferably 30 to 80 mol %. The ratio of the unit of the third component other than these can be 0 to 50 mol %, when the whole polymer is taken as 100 mol %.
[0051] [ka] [ka]
[0052] Here, in formulas (2) and (3), R c , R f and R h R independently represents a hydrogen atom or a methyl group. d represents a monovalent hydrocarbon group having 1 to 20 carbon atoms, and the hydrocarbon group may contain an ether bond, an ester bond, or a urethane bond therein. d R is a dicyclopentanyl group or a dicyclopentenyl group that accounts for 40 mol % or more of all the units represented by the general formula (2). e represents a divalent hydrocarbon group having 2 to 10 carbon atoms. p represents the number 0 or 1. X represents a hydrogen atom or -OC-L-(COOH) k group (wherein L is a divalent or trivalent carboxylic acid residue, and k is 1 to 2). In addition, two or more kinds of X may be contained in one polymer molecule. That is, the OX group is -OC-L-(COOH) k The OH groups may include OH groups if unreacted.
[0053] A method for producing such a (meth)acrylate resin will be described below. Although not limited thereto, for example, in the first step, a copolymer is obtained by copolymerizing a compound of the following formula (6) for forming a unit represented by general formula (2) with glycidyl (meth)acrylate in a solvent. The blending ratio of the compound of formula (6) is preferably 5 to 90 mol% relative to 100 mol% of the total of the compound of formula (6), glycidyl (meth)acrylate, and the other third component. More preferably, the compound of formula (6) is 20 to 70 mol%. That is, the unit represented by the following general formula (2) is preferably 5 to 90 mol%, more preferably 20 to 70 mol%, relative to 100 mol% of the total of the unit represented by general formula (3) and the other third component units. The copolymer may contain the above-mentioned styrenes or other components. [ka]
[0054] R in the above formulas (2) and (6) dExamples of the monovalent hydrocarbon group having 1 to 20 carbon atoms include, but are not limited to, saturated linear hydrocarbon groups such as a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a sec-butyl group, an isobutyl group, a tert-butyl group, a pentyl group, an isopentyl group, a neopentyl group, a tert-pentyl group, a hexyl group, a heptyl group, an octyl group, an isooctyl group, a 2-ethylhexyl group, a decyl group, a dodecyl group, a tetradecyl group, a hexadecyl group, an octadecyl group, and an eicosyl group; unsaturated linear hydrocarbon groups such as a vinyl group, an allyl group, and an ethynyl group; a cyclopropyl group, a cyclopentyl group, a cyclohexyl group, a 2-methylcyclohexyl group, a 4-methylcyclohexyl group; Examples of the unit represented by the general formula (2) include cyclic aliphatic hydrocarbon groups such as dicyclopentanyl, dicyclopentenyl, dicyclohexyl, norbornyl, isobornyl, adamantyl, tricyclodecylmethyl, and the substituent represented by the following general formula (7) (* indicates the bond to the ester moiety in general formula (2)), hydrocarbon groups having an aromatic ring such as phenyl, tolyl, mesityl, naphthyl, anthryl, phenanthryl, benzyl, 2-phenylethyl, 2-phenylvinyl, and decahydronaphthyl, aliphatic ethers such as methoxyethyl, 2-(methoxyethoxy)ethyl, and isoamyl, and aliphatic urethanes such as 2-(ethoxycarbonylamino)ethyl. The unit represented by the general formula (2) is represented by R d may include multiple units with different [ka] Of these, R d From the viewpoint of imparting heat resistance and light resistance, it is preferred that 40 mol % or more of all units formed as general formula (2) are dicyclopentanyl groups or dicyclopentenyl groups.
[0055] Next, in the second step, the epoxy groups in the copolymer obtained above are reacted with unsaturated group-containing carboxylic acids such as (meth)acrylic acid to open the epoxy groups. In this case, the amount of unsaturated group-containing carboxylic acids to be reacted is preferably 80 mol% or more, more preferably 90 mol% or more, and even more preferably 100 mol% relative to the epoxy groups. By increasing the amount of unsaturated group-containing carboxylic acids reacted with epoxy groups, it is possible to increase the amount of unsaturated groups and groups corresponding to X shown below introduced into the obtained (meth)acrylate resin, which is preferable.
[0056] As the unsaturated group-containing carboxylic acid, a compound represented by the following formula (8) can be used. e , R f and p is as defined above. [ka]
[0057] R e The divalent hydrocarbon group having 2 to 10 carbon atoms is preferably a divalent alkylene group or alkylarylene group having 2 to 10 carbon atoms, and may be linear, branched, or cyclic. e The hydrocarbon group represented by the formula (3) is preferably an ethylene group, a 1,2-propylene group, or a 1,4-butylene group. e A preferred unsaturated group-containing carboxylic acid is (meth)acrylic acid, where p=0.
[0058] In the third step, the OH group formed by the ring-opening in the second step is reacted with an anhydride of a dicarboxylic acid or tricarboxylic acid to form a unit represented by general formula (3). The (meth)acrylate resin obtained in this way is an alkali-soluble resin containing a polymerizable unsaturated group. The dicarboxylic acid or tricarboxylic acid anhydride to be reacted is not limited, but is preferably a dicarboxylic acid or tricarboxylic acid or an acid monoanhydride thereof used in the formation of the alkali-soluble resin represented by the general formula (4) above. These may be used alone or in combination of two or more. Among these, maleic acid, succinic acid, itaconic acid, tetrahydrophthalic acid, hexahydrophthalic acid, hexahydrotrimellitic acid, chlorendic acid, phthalic acid, and trimellitic acid are preferred, and succinic acid, itaconic acid, and tetrahydrophthalic acid monoanhydrides are more preferred, and tetrahydrophthalic acid, succinic acid, and trimellitic acid monoanhydrides are even more preferred.
[0059] In the third step, the amount of the dicarboxylic acid or tricarboxylic acid anhydride used can be appropriately adjusted relative to the OH group formed by the ring-opening in the second step, thereby adjusting the acid value to within the range described below. However, the synthesis method of such a (meth)acrylate resin is not limited to this. For example, the above-mentioned (meth)acrylic acid esters and (meth)acrylic acid are radically copolymerized in a solvent, then a (meth)acrylic acid ester compound having a glycidyl group such as glycidyl (meth)acrylate is reacted with a carboxyl group in the copolymer, and then the above-mentioned dicarboxylic acid compound, tricarboxylic acid compound, or their acid monoanhydride is reacted with the generated hydroxyl group.
[0060] The weight average molecular weight (Mw) of the (meth)acrylate resin obtained is preferably 3000 to 50000, more preferably 4000 to 20000. When the weight average molecular weight is 3000 or more, it is possible to suppress the decrease in adhesion of the pattern during alkaline development. When the weight average molecular weight is 50000 or less, it is easy to adjust the solution viscosity of the photosensitive resin composition to a suitable level for application, and alkaline development does not require too much time.
[0061] The acid value of the (meth)acrylate resin is preferably 30 mgKOH / g or more and 200 mgKOH / g or less, more preferably 40 mgKOH / g or more and 140 mgKOH / g or less, and even more preferably 50 to 150 mgKOH / g. When the acid value is 30 mgKOH / g or more, residues are less likely to remain during alkaline development. When the acid value is 200 mgKOH / g or less, the penetration of the alkaline developer is not too fast, so peeling development can be suppressed. The acid value can be adjusted by the amount of carboxyl groups present in X in the unit represented by general formula (3).
[0062] The weight average molecular weight (Mw) and acid value of the (meth)acrylate resin can be measured by the same method as that used for the alkali-soluble resin represented by general formula (4).
[0063] The (meth)acrylate resin may be used alone in the (A) component, or may be used in combination with the alkali-soluble resin represented by general formula (4) according to the desired application, properties, etc., as described above, and can be appropriately selected. The (meth)acrylate resin can be used in an amount of usually 10 to 100% by mass relative to the total mass of the (A) component (for example, the total mass of the alkali-soluble resin represented by general formula (4) and the (meth)acrylate resin). When the (meth)acrylate resin is present in a large amount, the light resistance and low reflectance are particularly excellent, so from the viewpoint of imparting these properties, the amount is preferably 50 to 100% by mass, more preferably 75 to 100% by mass, and particularly preferably 90 to 100% by mass relative to the total mass of the (A) component (for example, the total mass of the alkali-soluble resin represented by general formula (4) and the (meth)acrylate resin).
[0064] The content of component (A) in the photosensitive resin composition of the present invention is preferably 30 to 80 mass % based on the total mass of the solid contents when no colorant or light-shielding material is contained, and is preferably 2 mass % or more and 70 mass % or less when no colorant or light-shielding material is contained.
[0065] <(B) Photopolymerizable monomer having at least two ethylenically unsaturated bonds> The component (B) can play a role in crosslinking the molecules of the alkali-soluble resin, which is the component (A). Examples of the component (B) include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, tetramethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, glycerol (meth)acrylate, and the like. Examples of the (meth)acrylic acid esters include glycerol di(meth)acrylate, glycerol tri(meth)acrylate, sorbitol penta(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, sorbitol hexa(meth)acrylate, alkylene oxide-modified hexa(meth)acrylate of phosphazene, and caprolactone-modified dipentaerythritol hexa(meth)acrylate, and dendritic polymers having a (meth)acryloyl group, and one or more of these can be used. Examples of the dendritic polymer having a (meth)acryloyl group include known dendritic polymers obtained by adding a thiol group in a polyvalent mercapto compound to a part of the carbon-carbon double bond in the (meth)acryloyl group of a polyfunctional (meth)acrylate compound.
[0066] Since the component (B) plays the role described above, it is more preferable to use one having two or more ethylenically unsaturated bonds in order to exert its function. In addition, the acrylic equivalent, which is the molecular weight of the monomer divided by the number of (meth)acryloyl groups in one molecule, may be 50 to 300.
[0067] The amount of the (B) component is preferably 30 / 70 to 90 / 10 in terms of the mass ratio (A) / (B) with the (A) component, more preferably 35 / 65 to 60 / 40. If the (A) component is less than 30 / 70, the cured product after photocuring becomes brittle, and the acid value of the coating film is low in the unexposed area, so that the solubility in an alkaline developer decreases, and the pattern edge may become jagged and not sharp. If the (A) component is more than 90 / 10, the proportion of photoreactive functional groups in the resin is low, so that the crosslinked structure is not sufficiently formed, and furthermore, the acid value of the resin component is too high, so that the solubility in an alkaline developer in the exposed area may increase, and problems such as the formed pattern being narrower than the target line width or the pattern being easily missing may occur.
[0068] <(C) Cyclic siloxane compound having two or more epoxy groups in the molecule> The photosensitive resin composition of the present invention contains (C) a cyclic siloxane compound having two or more epoxy groups in the molecule. More preferably, it is a cyclic siloxane compound having three or more epoxy groups in the molecule. Since such a (C) component has a cyclic siloxane structure, it is presumed that the rigid cyclic structure has higher resistance to a developer than a chain structure, and it is considered that it is possible to improve adhesion to a glass substrate and fine line adhesion. In addition, since it has two or more epoxy groups in the molecule, the crosslink density is improved during curing, and it is excellent in curability. As for the (C) component, only one type of compound may be used, or two or more types may be used in combination. The (C) component is represented by the following general formula (1).
[0069] [ka]
[0070] R in general formula (1) a and R b represents a monovalent group containing an epoxy group or a monovalent hydrocarbon group having 1 to 20 carbon atoms. a and R bAt least two of R are monovalent groups containing an epoxy group. a and R b may be the same or different. n represents an integer of 3 or more and 10 or less. Preferably, n is 4 or more and 6 or less.
[0071] Here, the monovalent group containing an epoxy group is not limited, but may be -R g It is preferable that R is a group represented by -Ep. g represents an alkylene group which may be linked to an ether bond, an ester bond, an amino group, or the like, and Ep represents a group containing an epoxy group.
[0072] R g Examples of the alkylene group include linear or branched alkylene groups having 1 to 18 carbon atoms, such as a methylene group, a methylmethylene group, a dimethylmethylene group, a dimethylene group, and a trimethylene group.
[0073] On the other hand, Ep (a group containing an epoxy group) may be a glycidyl group, a 3,4-epoxycyclohexyl group, etc. As for the group containing an epoxy group, it is more preferable that the group is a 3,4-epoxycyclohexyl group because of its high reactivity with cations. By having a 3,4-epoxycyclohexyl group, which has high reactivity with cations, in the molecule, the solvent resistance of the cured film (coating film) can be improved at an addition amount that allows the development speed to fall within an appropriate range.
[0074] Examples of the monovalent hydrocarbon group having 1 to 20 carbon atoms include an alkyl group, an aryl group, an aralkyl group, and an alkenyl group having 1 to 20 carbon atoms.
[0075] When the hydrocarbon group having 1 to 20 carbon atoms is an alkyl group, the number of carbon atoms is preferably 1 to 16, more preferably 1 to 12. A part or all of the hydrogen atoms on the carbon of the alkyl group may be substituted with other groups that are not involved in the reaction. The alkyl group may be linear, branched, or cyclic. Specific examples of the groups that are not involved in the reaction include alkoxy groups having 1 to 6 carbon atoms, alkoxycarbonyl groups having 1 to 6 carbon atoms, and halogen atoms. Specific examples of the alkyl group that may be substituted with groups that are not involved in the reaction include a methyl group, an ethyl group, a propyl group, a butyl group, a sec-butyl group, a pentyl group, a hexyl group, a cyclohexyl group, an octyl group, a decyl group, a 2-methoxyethyl group, a 3-ethoxypropyl group, a 2-methoxycarbonylethyl group, a trifluoromethyl group, and a 3-chloropropyl group.
[0076] In addition, when the hydrocarbon group having 1 to 20 carbon atoms is an aryl group, a monovalent aromatic organic group of a hydrocarbon ring system or a heterocyclic ring system can be used. When the aryl group is a hydrocarbon ring system, the number of carbon atoms is preferably 6 to 18, more preferably 6 to 14. Specific examples of the aryl group include a phenyl group, a naphthyl group, an anthryl group, a phenanthryl group, and a pyrenyl group. In addition, when the aryl group is a heterocyclic ring system, the heteroatom in the heterocyclic ring is a sulfur or oxygen atom, and the number of carbon atoms is preferably 4 to 12, more preferably 4 to 8, and specific examples of the aryl group include a thienyl group, a benzothienyl group, a dibenzothienyl group, a furyl group, a benzofuryl group, and a dibenzofuryl group. A part or all of the hydrogen atoms of the aryl group may be substituted with a group that does not participate in the reaction. Specific examples of the group that does not participate in the reaction include those shown in the case of the alkyl group. In addition, other groups that do not participate in the reaction include an oxyethylene group, an oxyethyleneoxy group, and the like, which are divalent groups that bond two carbon atoms on a ring. Specific examples of the aryl group which may be substituted by a group which does not participate in the reaction include a methylphenyl group, an ethylphenyl group, a hexylphenyl group, a methoxyphenyl group, an ethoxyphenyl group, a butoxyphenyl group, an octoxyphenyl group, a methyl(methoxy)phenyl group, a fluoro(methyl)phenyl group, a chloro(methoxy)phenyl group, a bromo(methoxy)phenyl group, a 2,3-dihydrobenzofuranyl group, and a 1,4-benzodioxanyl group.
[0077] When the hydrocarbon group having 1 to 20 carbon atoms is an aralkyl group, the number of carbon atoms is preferably 7 to 19, more preferably 7 to 15. A part or all of the hydrogen atoms on the carbon of the aralkyl group may be substituted with a group that does not participate in the reaction. Specific examples of the group that does not participate in the reaction include those shown above for the alkyl group. Specific examples of the aralkyl group that may be substituted with a group that does not participate in the reaction include a benzyl group, a phenethyl group, a 2-naphthylmethyl group, a 9-anthrylmethyl group, a (4-chlorophenyl)methyl group, and a 1-(4-methoxyphenyl)ethyl group.
[0078] Furthermore, when the hydrocarbon group having 1 to 20 carbon atoms is an alkenyl group, the number of carbon atoms is preferably 2 to 18, more preferably 2 to 14. A part or all of the hydrogen atoms on the carbon of the alkenyl group may be substituted with a group that does not participate in the reaction. Specific examples of the group that does not participate in the reaction include those shown above in the case of the alkyl group, as well as the aryl group shown above. Specific examples of the alkenyl group that may be substituted with a group that does not participate in the reaction include a vinyl group, a 2-propenyl group, a 3-butenyl group, a 5-hexenyl group, a 9-decenyl group, a 2-phenylethenyl group, a 2-(methoxyphenyl)ethenyl group, a 2-naphthylethenyl group, and a 2-anthrylethenyl group.
[0079] Specific examples of the component (C) that satisfy the above conditions include, but are not limited to, silsesquioxanes having two or more epoxy groups in the molecule. More specifically, examples include 2,4-di[2-(3-{oxabicyclo[4.1.0]heptyl})ethyl]-2,4,6,6,8,8-hexamethyl-cyclotetrasiloxane, 4,8-di[2-(3-{oxabicyclo[4.1.0]heptyl})ethyl]-2,2,4,6,6,8-hexamethyl-cyclotetrasiloxane, 2,4-di[2-(3-{oxabicyclo[4.1.0]heptyl})ethyl]-6,8-dipropyl-2,4,6,8-tetramethyl-cyclotetrasiloxane, 4,8-di[2-(3-{oxabicyclo[4.1.0]heptyl})ethyl]- 2,4,8-tri[2-(3-{oxabicyclo[4.1.0]heptyl})ethyl]-2,4,6,6,8-pentamethyl-cyclotetrasiloxane, 2,4,8-tri[2-(3-{oxabicyclo[4.1.0]heptyl})ethyl]-6-propyl-2,4,6,8-tetramethyl-cyclotetrasiloxane, 2,4,6,8-tetra[2-(3-{oxabicyclo[4.1.0]heptyl})ethyl]-2,4,6,8-tetramethyl-cyclotetrasiloxane. For example, commercially available products such as X-40-2678 and KR-470 (both manufactured by Shin-Etsu Chemical Co., Ltd.) can be obtained and used. Among them, in order to express the function, it is preferable that the number of monovalent groups containing an epoxy group is 3 or more. There is no upper limit on the number of monovalent groups containing an epoxy group.
[0080] The content of the component (C) is preferably 0.1 to 1.5, more preferably 0.28 to 1.0, and even more preferably 0.62 to 0.8, when the content of the component (A) is taken as 1 in terms of mass ratio.
[0081] The number average molecular weight (Mn) of component (C) is preferably 100 to 5000. The epoxy group equivalent is preferably 50 to 300 g / eq. When the number average molecular weight (Mn) is 100 to 5000, it is possible to obtain a cured film with good solvent resistance while ensuring the development adhesion during development. When the epoxy equivalent is 50 to 300 g / eq, it is possible to design a photosensitive resin composition with an appropriate range of development speed, and also ensure the solvent resistance of the cured film.
[0082] <(D) Photopolymerization initiator> Examples of the component (D) in the photosensitive resin composition of the present invention include acetophenones such as acetophenone, 2,2-diethoxyacetophenone, p-dimethylacetophenone, p-dimethylaminopropiophenone, dichloroacetophenone, trichloroacetophenone, p-tert-butylacetophenone, and benzyl dimethyl ketal; benzophenone, 2-chlorobenzophenone, p,p'-bisdimethylaminobenzophenone, 4,4'-bisdimethylaminobenzophenone (Michler's ketone), 4-phenylbenzophenone, 4,4'-dichloroacetophenone, and the like. benzophenones such as benzophenone, hydroxybenzophenone, and 4,4'-diethylaminobenzophenone; benzoin ethers such as benzil, benzoin, benzoin methyl ether, benzoin isopropyl ether, and benzoin isobutyl ether; 2-(o-chlorophenyl)-4,5-phenylbiimidazole, 2-(o-chlorophenyl)-4,5-di(m-methoxyphenyl)biimidazole, 2-(o-fluorophenyl)-4,5-diphenylbiimidazole, and 2-(o-methoxyphenyl)-4,5-diphenylbiimidazole. biimidazole compounds such as 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2-biimidazole; halomethyldiazole compounds such as 2-trichloromethyl-5-styryl-1,3,4-oxadiazole, 2-trichloromethyl-5-(p-cyanostyryl)-1,3,4-oxadiazole, and 2-trichloromethyl-5-(p-methoxystyryl)-1,3,4-oxadiazole; 2,4,6-tris(trichloromethyl)-1,3,5-triazine, 2-methyl- 2-phenyl-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(4-chlorophenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(4-methoxynaphthyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(4-methoxystyryl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(3,4,Halomethyl-s-triazine compounds such as 5-trimethoxystyryl)-4,6-bis(trichloromethyl)-1,3,5-triazine and 2-(4-methylthiostyryl)-4,6-bis(trichloromethyl)-1,3,5-triazine; 1,2-octanedione, 1-[4-(phenylthio)phenyl]-, 2-(O-benzoyloxime), 1-(4-phenylsulfanylphenyl)butane-1,2-dione-2-oxime-O-benzoate, 1-(4-methylsulfanylphenyl)butane-1,2-dione-2-oxime-O-acetate, 1-(4-methylsulfanylphenyl)butan-1-one oxime-O-acetate, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-bicycloheptyl-1-one oxime-O-acetate, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-adamantylmethan-1-one oxime-O-benzoate, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol- 3-yl]-adamantylmethan-1-one oxime-O-acetate, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-tetrahydrofuranylmethan-1-one oxime-O-benzoate, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-tetrahydrofuranylmethan-1-one oxime-O-acetate, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-thiophenylmethan-1-one Oxime-O-benzoate, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-thiophenylmethane-1-one oxime-O-acetate, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-morphonylmethane-1-one oxime-O-benzoate, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-morphonylmethane-1-one oxime-O-acetate, 1-[9-ethyl-6-(2 -methylbenzoyl)-9H-carbazol-3-yl]-ethan-1-one oxime-O-bicycloheptane carboxylate, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-ethan-1-one oxime-O-tricyclodecane carboxylate, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-ethan-1-one oxime-O-adamantane carboxylate, 1-[4-(phenylsulfanyl)phenyl]octane-1,2-Dione = 2-O-benzoyloxime, 1-[9-ethyl-6-(2-methylbenzoyl)carbazol-3-yl]ethanone-O-acetyloxime, (2-methylphenyl)(7-nitro-9,9-dipropyl-9H-fluoren-2-yl)-acetyloxime, ethanone, 1-[7-(2-methylbenzoyl)-9,9-dipropyl-9H-fluoren-2-yl]-1-(o-acetyloxime), ethanone, 1-(-9,9-dibutyl-7-nitro-9H-fluoren-2-yl)-1-O-acetyloxime O-Acyloxime compounds such as ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime); sulfur compounds such as thioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-methylthioxanthone, 2-isopropylthioxanthone, 4-isopropylthioxanthone, 2,4-dichlorothioxanthone, 1-chloro-4-propoxythioxanthone; 2-ethylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-methylthioxanthone, 2-isopropylthioxanthone, 4-isopropylthioxanthone, 2,4-dichlorothioxanthone, 1-chloro-4-propoxythioxanthone; anthraquinones such as 1,2-benzanthraquinone, octamethylanthraquinone, 1,2-benzanthraquinone, 2,3-diphenylanthraquinone; organic peroxides such as azobisisobutylnitrile, benzoyl peroxide, cumene peroxide; 2-mercaptobenzimidazole, 2-mercaptobenzoxazole, 2-mercaptobenzothiazole, β-mercaptopropionic acid, 2-ethylhexyl-3-mercaptopropionate, n-octyl-3-mercaptopropionate, methoxybutyl-3- Mercaptopropionate, stearyl-3-mercaptopropionate, trimethylolpropane tris(3-mercaptopropionate), tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate, pentaerythritol tetrakis(3-mercaptobutyrate), pentaerythritol tetrakis(3-mercaptopropionate), tetraethylene glycol bis(3-mercaptopropionate), dipentaerythritol hexakis(3-mercaptopropionate), 3,Examples of the photopolymerization initiator include thiol compounds such as 3'-thiodipropionic acid, dithiodipropionic acid, and laurylthiopropionic acid. Among these, it is preferable to use O-acyloxime compounds, from the viewpoint of easily obtaining high sensitivity. Two or more kinds of these photopolymerization initiators can also be used. In the present invention, the photopolymerization initiator is used to include a sensitizer.
[0083] In addition, a compound that does not act as a photopolymerization initiator or sensitizer by itself but can increase the ability of the photopolymerization initiator or sensitizer by using it in combination with the above-mentioned compound may be added. Examples of such compounds include amine-based compounds that are effective when used in combination with benzophenone. Examples of the amine-based compounds include triethylamine, triethanolamine, methyldiethanolamine, triisopropanolamine, methyl 4-dimethylaminobenzoate, ethyl 4-dimethylaminobenzoate, isoamyl 4-dimethylaminobenzoate, 2-dimethylaminoethyl benzoate, 2-ethylhexyl 4-dimethylaminobenzoate, N,N-dimethyl-p-toluidine, 4,4'-bis(dimethylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone, and 4,4'-bis(ethylmethylamino)benzophenone.
[0084] The amount of component (D) is preferably 2 to 30 parts by mass, and more preferably 3 to 20 parts by mass, per 100 parts by mass of the total of components (A) and (B), and is preferably 0.1 to 1% by mass in the photosensitive resin composition.
[0085] <(G) Inorganic fine particles> The photosensitive resin composition of the present invention can contain inorganic fine particles (G). The inorganic fine particles preferably have a refractive index of 1.20 to 1.50, and examples of such inorganic fine particles include silicon oxide. The inorganic fine particles of component (G) can be any known particles that satisfy the above refractive index range without any restrictions, and the manufacturing method, such as gas phase reaction or liquid phase reaction, and the shape (spherical, non-spherical) are not particularly limited. Inorganic fine particles that have been surface-treated with a silane coupling agent treatment or the like can also be used without any restrictions.
[0086] The refractive index of the inorganic fine particles is more preferably 1.33 to 1.48. By using inorganic fine particles having the above refractive index, the refractive index of the cured film (coating film) surface can be reduced, and reflection can be suppressed without providing a separate anti-reflection film or the like.
[0087] The refractive index of the inorganic fine particles can be determined from a transparent mixed liquid obtained by mixing the inorganic fine particles processed into a powder form with a standard refractive index liquid having a known refractive index. In this case, the refractive index of the standard refractive index liquid of the mixed liquid is taken as the refractive index of the inorganic fine particles. The refractive index of the inorganic fine particles can be measured using an Abbe refractometer.
[0088] By using the inorganic fine particles, the reflectance of the light-shielding film containing the inorganic fine particles can be reduced. In the present invention, when such a (G) component is contained, a light-shielding film with a relatively low reflectance can be obtained even if the light-shielding film has a high light-shielding property, which is preferable. As a suitable example, a light-shielding material as the (F) component described later is used, and in a cured film (or a light-shielding film) of a photosensitive resin composition using the (F) component, the reflectance is preferably less than 10% when the OD is 1 / μm or more, more preferably less than 5%, and even more preferably less than 4%.
[0089] The average particle size of the inorganic fine particles is preferably 1 to 150 nm, more preferably 1 to 100 nm, even more preferably 1 to 50 nm, particularly preferably 1 to 30 nm, and most preferably 1 to 10 nm. By using inorganic fine particles with an average particle size in this range, the inorganic fine particles can be effectively present on the film surface, which is advantageous for reducing the reflectance. In addition, the wobbling of the side surface of the fine line pattern can be suppressed. In addition, there is an effect of reducing the unevenness of the cured film (coating film) surface, and the variation in reflectance within the cured film (coating film) surface can be suppressed.
[0090] The content of the inorganic fine particles is preferably 0.1 to 5 parts by mass, more preferably 0.1 to 2 parts by mass, based on the total mass of the photosensitive resin composition. Also, it is preferably 1 to 20% by mass, based on the total solid content in the photosensitive resin composition. When the content of the inorganic fine particles is within the above range, it is possible to achieve low reflectance and ensure good patterning properties.
[0091] The average particle size of the inorganic fine particles can be measured, for example, by an electron microscope as in the method described later in the Examples, but is not limited thereto.
[0092] The inorganic fine particles can be mixed with other formulation components as an inorganic fine particle dispersion dispersed in a solvent. The dispersant can be any known compound used for pigment dispersion (compounds commercially available under the names of dispersant, dispersion wetting agent, dispersion promoter, etc.) without any particular limitation. <(H) Solvent> Examples of the solvent (H) in the photosensitive resin composition of the present invention include alcohols such as methanol, ethanol, n-propanol, isopropanol, ethylene glycol, propylene glycol, 3-methoxy-1-butanol, ethylene glycol monobutyl ether, 3-hydroxy-2-butanone, and diacetone alcohol; terpenes such as α- or β-terpineol; ketones such as acetone, methyl ethyl ketone, cyclohexanone, and N-methyl-2-pyrrolidone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; methyl cellosolve, ethyl cellosolve, methyl carbitol, ethyl carbitol, butyl carbitol, diethylene glycol ethyl methyl ether, propylene glycol monomethyl ether, and propylene glycol monoethyl ether. Examples of suitable esters include glycol ethers such as dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, triethylene glycol monomethyl ether, and triethylene glycol monoethyl ether; and esters such as ethyl acetate, butyl acetate, ethyl lactate, 3-methoxybutyl acetate, 3-methoxy-3-butyl acetate, 3-methoxy-3-methyl-1-butyl acetate, cellosolve acetate, ethyl cellosolve acetate, butyl cellosolve acetate, carbitol acetate, ethyl carbitol acetate, butyl carbitol acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate. By using these and dissolving and mixing, a uniform solution-like composition can be obtained.
[0093] <(E) Curing agent and / or curing accelerator> In the photosensitive resin composition of the present invention, in addition to other components, (E) a curing agent and / or a curing accelerator for the component (C) may be used in combination. Examples of the curing agent of the component (E) include amine compounds, polycarboxylic acid compounds, phenolic resins, amino resins, dicyandiamide, Lewis acid complex compounds, etc. In the present invention, polycarboxylic acid compounds can be preferably used.
[0094] Examples of polycarboxylic acid compounds include polycarboxylic acids, polycarboxylic anhydrides, and polycarboxylic heat decomposable esters. Polycarboxylic acids refer to compounds having two or more carboxy groups in one molecule, such as succinic acid, maleic acid, cyclohexane-1,2-dicarboxylic acid, cyclohexene-1,2-dicarboxylic acid, cyclohexene-4,5-dicarboxylic acid, norbornane-2,3-dicarboxylic acid, phthalic acid, 3,6-dihydrophthalic acid, 1,2,3,6-tetrahydrophthalic acid, methyltetrahydrophthalic acid, benzene-1,2,4-tricarboxylic acid, cyclohexane-1,2,4-tricarboxylic acid, benzene-1,2,4,5-tetracarboxylic acid, cyclohexane-1,2,4,5-tetracarboxylic acid, butane-1,2,3,4-tetracarboxylic acid, etc. Examples of polycarboxylic acid anhydrides include the acid anhydrides of the above compounds. These may be intermolecular acid anhydrides, but generally, acid anhydrides that are ring-closed within a molecule are used. Examples of the thermally decomposable ester of polycarboxylic acid include t-butyl ester, 1-(alkyloxy)ethyl ester, and 1-(alkylsulfanyl)ethyl ester of the above-mentioned compound (wherein alkyl is a saturated or unsaturated hydrocarbon group having 1 to 20 carbon atoms, and the hydrocarbon group may have a branched or cyclic structure, and may be substituted with any substituent). In addition, a polymer or copolymer having two or more carboxy groups may be used as the polycarboxylic acid compound, and the carboxy groups may be anhydrides or thermally decomposable esters. The acid components used to synthesize the alkali-soluble resins described above may also be used.
[0095] As the curing accelerator, known compounds known as curing accelerators for epoxy compounds, curing catalysts, latent curing agents, etc. can be used. Examples of curing accelerators for epoxy compounds include tertiary amines, quaternary ammonium salts, tertiary phosphines, quaternary phosphonium salts, boric acid esters, Lewis acids, organometallic compounds, imidazoles, etc. Among the above curing accelerators, 1,8-diazabicyclo[5.4.0]undec-7-ene or 1,5-diazabicyclo[4.3.0]non-5-ene or salts thereof are preferred.
[0096] The mass ratio of the component (C) to the component (E) is preferably component (C):component (E)=90:10 to 40:60. By including the component (C) and the component (E) that satisfy the above, the solvent resistance of the formed cured film can be sufficiently increased.
[0097] The ratio (Eb / Ea) of the total number of moles of epoxy groups in the (C) component Ea to the number of moles of reactive functional groups in the (E) component curing agent Eb that react with epoxy groups is preferably Eb / Ea=0.5 to 1.0. When Eb / Ea is 0.5 or more, the epoxy compound can be sufficiently cured, so that the unreacted epoxy compound can be prevented from remaining in the photosensitive resin composition. When Eb / Ea is 1.0 or less, the adhesion and linearity reproducibility of the cured film can be sufficiently improved.
[0098] <(F) Light shielding material> In the photosensitive resin composition of the present invention, in addition to other components, a light-shielding material, which is the component (F), can be used. The light-shielding material is more preferably one or more light-shielding materials selected from the group consisting of black organic pigments, mixed-color organic pigments, and black inorganic pigments. Here, examples of the black organic pigment include perylene black, aniline black, cyanine black, lactam black, and the like. Examples of the mixed-color organic pigment include those obtained by mixing two or more pigments selected from red, blue, green, purple, yellow, cyanine, magenta, and the like to give a pseudo-black color. Examples of the black inorganic pigment include carbon black, chromium oxide, iron oxide, titanium black, and the like. These coloring components may be used alone or in combination of two or more. They may be appropriately selected and used depending on the purpose of the photosensitive resin composition of the present invention.
[0099] Among these light-shielding materials, carbon black is more preferable from the viewpoints of light-shielding properties, surface smoothness, dispersion stability, and affinity with resin. In addition, when low dielectric constant properties of the coating film are required, the light-shielding material is preferably a black organic pigment and / or a mixed-color organic pigment. On the other hand, in applications where it is important to achieve both visible light shielding properties and infrared transmittance, a combination of carbon black and a black organic pigment, such as a combination of carbon black and lactam black, is preferably used.
[0100] The carbon black is preferably untreated or oxidized carbon black. Here, "untreated" means that no special surface treatment such as oxidation or resin coating is performed, and "oxidization" means that the surface of the carbon black is treated with some kind of oxidizing agent before the dispersion process. Since such untreated or oxidized carbon black has many acidic functional groups on the surface, it is preferable to use untreated or oxidized carbon black when utilizing them. Furthermore, when it is desired to further increase the resistance value of the cured film using carbon black, surface-coated carbon black in which the carbon black surface is coated with a dye, pigment, resin, or the like may be used.
[0101] When such a component (F) is used, the amount can be appropriately set depending on the purpose and application of the present invention. For example, it can be determined arbitrarily so as to obtain a desired light-shielding degree, but it is preferably 20 to 80 mass % based on the solid content in the photosensitive resin composition.
[0102] The component (F) is usually dispersed in a solvent and mixed with other components, and a dispersant may be added in this case. The dispersant may be any known compound (compounds commercially available under the names of dispersant, dispersion wetting agent, dispersion promoter, etc.) used for dispersing light-shielding materials, without any particular restrictions.
[0103] Examples of the dispersant include cationic polymer dispersants, anionic polymer dispersants, nonionic polymer dispersants, and pigment derivative dispersants (dispersion aids). In particular, the dispersant is preferably a cationic polymer dispersant having a cationic functional group such as an imidazolyl group, a pyrrolyl group, a pyridyl group, a primary, secondary or tertiary amino group as an adsorption point to the colorant, an amine value of 1 to 100 mgKOH / g, and a number average molecular weight (Mn) in the range of 1000 to 100000. The blending amount of this dispersant is preferably 1 to 35 parts by mass, more preferably 2 to 25 parts by mass, per 100 parts by mass of the light-shielding material component. Note that, although high-viscosity substances such as resins generally have the effect of stabilizing dispersion, those that do not have the ability to promote dispersion are not treated as dispersants. However, there is no restriction on using them for the purpose of stabilizing dispersion.
[0104] <Other components other than components (E) to (F)> In addition to the components (E) to (F), the photosensitive resin composition of the present invention may contain additives such as epoxy resins other than the component (C), colorants other than the component (F), thermal polymerization inhibitors, antioxidants, plasticizers, leveling agents, defoamers, surfactants, coupling agents, and viscosity modifiers, as necessary. As the epoxy resins other than the component (C), known epoxy resins can be used without restrictions. As the colorants other than the component (F), known organic pigments, inorganic pigments, dyes, and the like can be used without restrictions. Examples of the thermal polymerization inhibitors and antioxidants include hydroquinone, hydroquinone monomethyl ether, pyrogallol, tert-butylcatechol, phenothiazine, and hindered phenol-based compounds, and examples of the plasticizers include dibutyl phthalate, dioctyl phthalate, and tricresyl phosphate. Examples of the defoamers and leveling agents include silicone-based, fluorine-based, and acrylic-based compounds. Examples of the surfactants include fluorine-based surfactants and silicone-based surfactants. Examples of the coupling agent include silane coupling agents such as 3-(glycidyloxy)propyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, and 3-ureidopropyltriethoxysilane.
[0105] <Solid content> The photosensitive resin composition of the present invention contains the above components (A) to (D) and (G) as main components. When the solid content excluding the solvent (including the monomer that becomes a solid content after curing) does not contain the light-shielding material of the component (F) or the curing agent and / or curing accelerator of the component (E), the total amount of the components (A) to (D) and (G) is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more. When the light-shielding material of the component (F) or the curing agent and / or curing accelerator of the component (E) is contained, the total amount of the components including the components (A) to (D) and (G) as well as the components (F) and (E) is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more. The amount of the solvent, which is the component (H), varies depending on the target viscosity, but it is preferable that the amount of the solvent in the photosensitive resin composition of the present invention is in the range of 60 to 90% by mass.
[0106] <Method of forming a cured product (cured film, matrix pattern)> The photosensitive resin composition of the present invention is excellent as a composition for forming, for example, a cured film (protective film, light-shielding film) of a color filter, and the method for forming the cured film includes the following photolithography method: First, the photosensitive resin composition is applied onto a transparent substrate, and then the solvent is dried (prebaked), and then a photomask is placed on the coating thus obtained, and the exposed portion is cured by irradiating with ultraviolet light, and further development is performed using an alkaline aqueous solution to dissolve the unexposed portion to form a pattern, and further post-baking (thermal firing) is performed as post-drying.
[0107] Examples of the transparent substrate to which the composition is applied include glass substrates and transparent films (e.g., polycarbonate, polyethylene terephthalate, polyethersulfone, etc.) on which transparent electrodes such as ITO and gold are deposited or patterned. Examples of other substrates used in the method for producing a cured film of the present invention include glass substrates, silicon wafers, polyimide films, etc., which have high heat resistance but low heat resistance thin films formed on the substrate. Specific examples include substrates with organic devices on which OLEDs or organic thin film transistors (TFTs) are formed, and also include substrates on which protective films, protective films, etc. are formed after the formation of an organic device. The heat resistance temperature of such substrates with low heat resistance varies depending on the type of resin and the device, but is preferably 100°C or less, more preferably 80 to 100°C. The substrates with organic devices also include those on which protective films, protective films, etc. are formed after the formation of an organic device. Even if the heat resistance of these protective films and protective films themselves is 100°C or more, if the heat resistance is substantially only 100°C or less to ensure the function of the organic device, they are considered to be substrates with organic devices. The present invention is an effective technique for substrates with low heat resistance, but it also enables post-baking at low temperatures, which has traditionally been done at temperatures of 200°C or higher, and reduces process costs, making it an effective technique for such purposes as well.
[0108] As a method for applying a solution of the composition onto a transparent substrate, any method can be adopted, such as a known solution immersion method, a spray method, or a method using a roller coater, a land coater, a slit coater, or a spinner. After applying the composition to a desired thickness by these methods, the solvent is removed (prebaked) to form a coating. Prebaking is performed by heating in an oven, a hot plate, or the like. The heating temperature and heating time in prebaking are appropriately selected depending on the solvent used, and are performed, for example, at a temperature of 60 to 100°C for 1 to 3 minutes.
[0109] The exposure after pre-baking is performed by an ultraviolet exposure device, and only the resist in the portion corresponding to the pattern is exposed by exposing through a photomask. The exposure device and its exposure irradiation conditions are appropriately selected, and the exposure is performed using a light source such as an ultra-high pressure mercury lamp, a high pressure mercury lamp, a metal halide lamp, or a far ultraviolet lamp, to photocure the composition in the coating film.
[0110] The alkaline development after exposure is carried out for the purpose of removing the resist in the unexposed portion, and the desired pattern is formed by this development. Examples of the developer suitable for this alkaline development include an aqueous solution of carbonate of an alkali metal or an alkaline earth metal, an aqueous solution of hydroxide of an alkali metal, etc., but it is particularly preferable to use a weakly alkaline aqueous solution containing 0.05 to 3 mass % of carbonate such as sodium carbonate, potassium carbonate, or lithium carbonate at a temperature of 23 to 28°C, and fine images can be precisely formed using a commercially available developing machine, ultrasonic cleaner, etc.
[0111] After development, in the case of a substrate having high heat resistance, post-baking is usually preferably performed at about 120 to 250° C., more preferably 140 to 240° C., and further preferably 150 to 230° C. There are no limitations on the heating time, but the heating is usually performed under conditions of 20 to 60 minutes per 1 μm of film thickness. On the other hand, in the case of a substrate with low heat resistance, post-baking is preferably performed at a temperature of 100°C or less, more preferably 80 to 100°C, for 20 to 60 minutes. This post-baking is performed for the purpose of increasing the adhesion between the patterned cured film and the substrate. This is performed by heating in an oven, a hot plate, or the like, similarly to pre-baking. The patterned cured film of the present invention is formed through each step of the photolithography method described above. The desired matrix pattern can then be obtained using the obtained cured film.
[0112] As described above, the resist composition of the present invention is suitable for forming a fine pattern by exposure, alkaline development, etc. In addition, the cured film (light-shielding film) of the present invention can be used for a black matrix used in a color filter or a touch panel, or for a partition material or pixel definition layer for each color separation or light shielding in various multicolor display devices such as an electroluminescent device represented by an organic EL element, a color liquid crystal display device, or an image sensor, and further for a display component such as a bezel surrounding the display part of a display. EXAMPLES
[0113] Hereinafter, the embodiments of the present invention will be described in detail based on examples and comparative examples, but the present invention is not limited to these.
[0114] First, synthesis examples of the polymerizable unsaturated group-containing alkali-soluble resin, which is the component (A), will be described. Unless otherwise specified, the resins in these synthesis examples were evaluated as follows.
[0115] [Solid content concentration] The resin content was calculated from the weight [W1(g)] of 1 g of the resin solution obtained in Synthesis Example impregnated into a glass filter [weight: W0(g)] and the weight [W2(g)] after heating at 160°C for 2 hours, using the following formula: Solid content concentration (weight%) = 100 × (W2-W0) / (W1-W0)
[0116] [Acid value] The resin solution was dissolved in tetrahydrofuran and titrated with a 1 / 10N KOH aqueous solution using a potentiometric titrator "COM-A19" (manufactured by Hiranuma Sangyo Co., Ltd.) to determine the acid value per 1 g of the sample (synthetic resin solution).
[0117] [Molecular weight] Measurement was performed using gel permeation chromatography (GPC) "HLC-8320GPC" (manufactured by Tosoh Corporation, developing solvent: tetrahydrofuran, columns: PL1110-6540 (1 tube) + PL1110-6530 (1 tube) + PL1110-6525 (1 tube) + PL1110-6520 (1 tube), column temperature: 40°C, flow rate: 1.0 mL / min), and the weight average molecular weight (Mw) was calculated as a value converted into standard polystyrene (manufactured by SAS Corporation, polystyrene kit).
[0118] [Average primary particle size] The inorganic fine particle-containing solution was diluted with a solvent to a particle concentration of about 0.1 wt%, and the resulting dispersion was dropped onto a metal mesh with a carbon support film to create a measurement sample, which was then observed with a transmission electron microscope "JEM-2100Plus" (manufactured by JEOL Ltd.) to determine the amount of measurements. The number of measurements was n=3 for each.
[0119] The abbreviations used in the synthesis examples are as follows. AA: Acrylic acid BPFE: A reaction product of 9,9-bis(4-hydroxyphenyl)fluorene and chloromethyloxirane. In the compound of general formula (9), A is a fluorene-9,9-diyl group, and R1 to R4 are hydrogen atoms. BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride THPA: 1,2,3,6-Tetrahydrophthalic anhydride TPP: Triphenylphosphine PGMEA: Propylene glycol monomethyl ether acetate TEAB: Tetraethylammonium bromide DCPMA: dicyclopentanyl methacrylate GMA: glycidyl methacrylate St: styrene SA: Succinic anhydride AIBN: Azobisisobutyronitrile TDMAMP: Trisdimethylaminomethylphenol TEA: Triethylamine PTMA: Pentaerythritol tetra(mercaptoacetate) DPHA: A mixture of dipentaerythritol pentaacrylate and hexaacrylate HQ: Hydroquinone BzDMA: benzyldimethylamine
[0120] [Synthesis Example 1] BPFE (114.4g, 0.23mol), AA (33.2g, 0.46mol), PGMEA (157g) and TEAB (0.48g) were charged into a 500ml four-neck flask equipped with a reflux condenser, and the mixture was stirred at 100-105°C for 20 hours to react. Next, BPDA (35.3g, 0.12mol) and THPA (18.3g, 0.12mol) were charged into the flask, and the mixture was stirred at 120-125°C for 6 hours to obtain a polymerizable unsaturated group-containing alkali-soluble resin solution (A)-1. The solid content concentration of the obtained resin solution was 56.1% by mass, the acid value (solid content equivalent) was 103mgKOH / g, and the Mw by GPC analysis was 3600.
[0121] [Synthesis Example 2] In a 1 L four-neck flask equipped with a reflux condenser, 300.0 g of PGMEA was placed, and the inside of the flask was replaced with nitrogen, and then the temperature was raised to 120° C. A monomer mixture (a mixture of 66.1 g (0.3 mol) of DCPMA, 85.3 g (0.6 mol) of GMA, and 10.4 g (0.10 mol) of St dissolved in 10 g of AIBN) was added dropwise from a dropping funnel to the flask over 2 hours, and the mixture was further stirred at 120° C. for 2 hours to obtain a copolymer solution. Next, the atmosphere in the flask was replaced with air, and then 43.2 g (0.6 mol) of AA, 0.8 g of TDMAMP, and 0.15 g of HQ were added to the obtained copolymer solution, and the mixture was stirred for 6 hours under heating at 120°C to obtain a copolymer solution containing a polymerizable unsaturated group. Further, 59.3 g (0.39 mol) of THPA and 0.5 g of TEA were added to the obtained polymerizable unsaturated group-containing copolymer solution and reacted at 120° C. for 4 hours to obtain a polymerizable unsaturated group-containing alkali-soluble copolymer resin solution (A)-2. The solid content concentration of the resin solution was 48 mass%, the acid value (solid content equivalent) was 79 mgKOH / g, and the Mw by GPC analysis was 8500.
[0122] In addition, a synthesis example of the component (B)-2 described below will be shown (Synthesis Example 3). [Synthesis Example 3] PTMA (20 g, 0.19 mol of mercapto groups), DPHA (212 g (2.12 mol of acrylic groups)), PGMEA (58 g), HQ (0.1 g), and BzDMA (0.01 g) were added to a 1 L four-neck flask and reacted at 60° C. for 12 hours to obtain a dendritic polymer solution (H)-3. The solid content of the dendritic polymer solution was 80 mass %, and Mw was 10,000 by GPC analysis. The disappearance of mercapto groups from the obtained dendritic polymer was confirmed by iodometry.
[0123] [Preparation example F] 1000g of carbon black (TPX-1099: manufactured by Cabot) was mixed with water to prepare 10L of slurry, which was stirred at 95°C for 1 hour and then cooled and washed with water. This was mixed again with water to prepare 10L of slurry, to which 42.9g of 70% nitric acid was added and stirred at 40°C for 4 hours. This was cooled, washed with water, and then mixed with water again to prepare 10L of slurry, to which 769.2g of 13% aqueous sodium hypochlorite solution was added and stirred at 40°C for 6 hours. This was cooled, washed with water, and then mixed with water again to prepare 10L of slurry, to which 38.1g of a 38.4% pure dye (Direct Deep BLACK) was added and stirred at 40°C for 1 hour, after which 10.1g of aluminum sulfate was added and stirred at 40°C for 1 hour. This was cooled, washed with water, filtered, and dried to obtain dye-coated carbon black.
[0124] The dye-coated carbon black, a polymer dispersant, the alkali-soluble resin obtained in Synthesis Example 1 (below, (A)-1), and PGMEA were mixed and dispersed using a bead mill to obtain a carbon black dispersion (F) having a dye-coated carbon black concentration of 25.0 mass%, a polymer dispersant concentration of 2.0 mass%, and a resin concentration of (A)-1 of 8.0 mass%.
[0125] Photosensitive resin compositions of Examples 1 to 24 and Comparative Examples 1 to 4 were prepared in the amounts (unit: parts by mass) shown in Tables 1 and 2. The components used in Tables 1 and 2 are as follows.
[0126] (Alkali-soluble resin containing unsaturated groups) (A)-1: Alkali-soluble resin solution obtained in Synthesis Example 1 above (A)-2: Alkali-soluble resin solution obtained in Synthesis Example 2 above
[0127] (Photopolymerizable compound) (B)-1: 50% PGMEA solution of a mixture of dipentaerythritol hexaacrylate and dipentaerythritol pentaacrylate (Aronix M-405, manufactured by Toa Gosei Co., Ltd., "Aronix" is a registered trademark of the company) (B)-2: Resinous polymer solution obtained in Synthesis Example 3 above
[0128] (Epoxy group-containing cyclic siloxane) (C)-1: KR-470, manufactured by Shin-Etsu Chemical Co., Ltd. (C)-2: X-40-2678, manufactured by Shin-Etsu Chemical Co., Ltd.
[0129] (Epoxy group-containing linear siloxane) (C)-3: X-40-2669, manufactured by Shin-Etsu Chemical Co., Ltd.
[0130] (Other epoxy compounds) (C')-4: 1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol (EHPE-3150, epoxy + oxetanyl equivalent: 180, manufactured by Daicel Corporation) (C')-5: 3',4'-epoxycyclohexylmethyl 3',4'-epoxycyclohexanecarboxylate (Celloxide 2021P, epoxy + oxetanyl equivalent: 126, manufactured by Daicel Corporation)
[0131] (Photopolymerization initiator) (D): ADEKA Arcles NCI-831E, manufactured by ADEKA Corporation, "ADEKA Arcles" is a registered trademark of the company.
[0132] (hardening agent) (E)-1: Trimellitic anhydride (TMA, manufactured by Mitsubishi Gas Chemical Company, Inc.) (Curing agent) (E)-2: U-CAT SA102, manufactured by San-Apro Ltd.
[0133] (Carbon black dispersion) (F)-1: Pigment dispersion (solid content 35.0% by mass) in PGMEA solvent containing the dye-coated carbon black obtained in Preparation Example F at a concentration of 25.0% by mass, the polymer dispersant at a concentration of 2.0% by mass, and the resin concentration of (A)-1 at 8.0% by mass. (F)-2: PGMEA dispersion with carbon black concentration of 20.0% by mass and polymer dispersant concentration of 5.0% by mass (solid content 25.0% by mass)
[0134] (Inorganic fine particle dispersion) (G)-1: Silica PGMEA dispersion "YA010C" (manufactured by Admatechs Co., Ltd., silica concentration 20% by mass, PGMEA concentration 80% by mass, refractive index: 1.46, average primary particle size 10 nm) (G)-2: Silica PGMEA dispersion (silica concentration 30% by mass, PGMEA concentration 70% by mass, refractive index: 1.46, average primary particle diameter 70 nm)
[0135] (solvent) (H)-1: Propylene glycol monomethyl ether acetate (PGMEA) (H)-2: Diethylene glycol dimethyl ether (DMDG) (H)-3: Diethylene glycol methyl ethyl ether (EDM)
[0136] (Other ingredients): DOWSIL SH3775M, manufactured by Dow Chemical Japan Co., Ltd. "DOWSIL" is a trademark of the company.
[0137] [Table 1]
[0138] [Table 2]
[0139] [evaluation] The following evaluations were carried out using the photosensitive resin compositions of Examples 1 to 24 and Comparative Examples 1 to 4. The evaluation results are shown in Tables 3 and 4.
[0140] <Evaluation of patterning ability> Each of the compositions obtained above was applied to a 125 mm × 125 mm glass substrate (Corning 1737) using a spin coater so that the film thickness after post-baking would be 1.0 μm, and the substrate was pre-baked at 85° C. for 1 minute. Thereafter, a negative photomask having a line pattern with an opening width of 1 to 20 μm was placed in close contact with the dried coating film, and the substrate was exposed to an i-line illuminance of 30 mW / cm. 2 40mJ / cm2 ultra-high pressure mercury lamp 2 The exposed portion was exposed to ultraviolet light for a photo-curing reaction.
[0141] Next, the exposed coated plate was soaked in a 0.04% aqueous potassium hydroxide solution at 23°C for 1 kgf / cm 2 After 20 seconds of development from the development time (break time = BT) when the pattern begins to appear, the shower development pressure is 5kgf / cm 2 The non-exposed areas of the coating were removed by spraying water at high pressure to form a line pattern on the glass substrate, and then the substrate was post-baked at 85°C for 60 minutes using a hot air dryer. The minimum opening line that did not peel off in the line pattern obtained was defined as the minimum resolution line width. A grade of ◯ or higher was considered to be the pass grade. (Evaluation criteria for fine line adhesion) ◎: Less than 3μm ○: 3μm or more and less than 10μm ×: 10μm or more
[0142] In addition, the 10 μm mask pattern after main curing (post-baking) was observed using an optical microscope. A grade of ◯ or higher was considered to be the pass mark. (Evaluation criteria for pattern linearity) ⊚: When the length of the pattern is taken as 100%, the jaggedness of the pattern edge is less than 1% with a 0.5 μm protrusion for a line width of 10 μm. ◯: When the length of the pattern is taken as 100%, the jaggedness of the pattern edge is such that a protrusion of 0.5 μm is observed in only 1% or more and less than 25% of a line width of 10 μm. ×: When the length of the pattern is taken as 100%, the edge of the pattern is roughened to such an extent that protrusions of 0.5 μm are observed in 25% or more of a line width of 10 μm.
[0143] <Reflectance evaluation> Each of the compositions obtained above was applied onto a 125 mm × 125 mm glass substrate (Corning 1737) using a spin coater so that the film thickness after post-baking would be 1.0 μm, and the substrate was pre-baked at 85° C. for 1 minute. Thereafter, the substrate was pre-baked under an i-line irradiance of 30 mW / cm 2 50mJ / cm with ultra-high pressure mercury lamp 2 The resin was irradiated with ultraviolet light to carry out a photocuring reaction.
[0144] Next, the exposed plate was soaked in a 0.04% aqueous potassium hydroxide solution at 23°C for 1 kgf / cm 2 After 20 seconds of development from the development time (break time = BT) when the pattern begins to appear, the shower pressure is 5kgf / cm 2 The plate was then sprayed with water and post-baked at 85°C for 60 minutes using a hot air dryer. The reflectance of the film side of the plate was measured at an incidence angle of 2° using a UV-Vis-Near-Infrared Spectrophotometer UH4150 (manufactured by Hitachi High-Tech Science Corporation). A grade of △ or higher was considered to be acceptable. (Reflectance evaluation criteria) ◎: Reflectance is less than 4% ○: Reflectance is 4% or more but less than 5% △: 5% to less than 10% ×: Reflectance is 10% or more
[0145] <Heat resistance evaluation> The post-baked coated plate obtained above was further heat-treated at 230°C for 3 hours, and the b * The pass mark was △ or higher. (Evaluation criteria for heat resistance) ◎:Δb * is less than 0.2 ○:Δb * is 0.2 or more and less than 0.5 △: Δb * is 0.5 or more and less than 1 ×:Δb * is 1 or more
[0146] <Light resistance evaluation> The post-baked coated plate obtained above was then exposed to a low-pressure mercury lamp with a wavelength of 254 nm and an illumination intensity of 130 W / cm 2 The sample was exposed to ultraviolet light for 2 hours and measured by a spectrophotometer. * The pass mark was △ or higher. (Evaluation criteria for light resistance) ◎:Δb * is less than 0.5 ○:Δb * is 0.5 or more and less than 1 △: Δb * is 1 or more and less than 1.5 ×:Δb * is 1.5 or more
[0147] [Table 3]
[0148] [Table 4]
[0149] From the results of Examples 1 to 24 and Comparative Examples 1 to 4, it was confirmed that by adding epoxy group-containing cyclic siloxane as component (C) and silica dispersion as inorganic fine particles (G) to the photosensitive resin composition, it is possible to achieve both high-definition pattern formation and reduction in reflectance on the coating surface side. Furthermore, it was confirmed that by using the alkali-soluble resin (A)-1 of Synthesis Example 1 and using the (C) component and the above component, heat resistance was achieved, and also that by using the alkali-soluble resin (A)-2 of Synthesis Example 2 and using the (C) component and the above component, light resistance was achieved.
Claims
1. (A) an unsaturated group-containing alkali-soluble resin; (B) a photopolymerizable compound having at least two unsaturated bonds; (C) a cyclic siloxane compound having two or more epoxy groups in the molecule; (D) a photopolymerization initiator; and (G) inorganic fine particles; (H) a solvent; A photosensitive resin composition comprising:
2. 2. The photosensitive resin composition according to claim 1, wherein the component (C) is a cyclic siloxane compound represented by general formula (1). 【Chemistry 1】 [R in formula (1)] a and R b represents a monovalent group containing an epoxy group or a monovalent hydrocarbon group having 1 to 20 carbon atoms. a and R b At least two of R are monovalent groups containing an epoxy group. a and R b may be the same or different, and n represents an integer of 3 or more and 10 or less.
3. The photosensitive resin composition according to claim 1, wherein the component (A) comprises a polymer including a unit represented by the following general formula (2) and a unit represented by the following general formula (3), the polymer including 5 to 90 mol % of the unit represented by the general formula (2) and 10 to 95 mol % of the unit represented by the general formula (3), and having a weight average molecular weight of 3,000 to 50,000 and an acid value of 30 to 200 mg / KOH: 【Chemistry 2】 【Chemistry 3】 (However, R c , R f and R h R independently represents a hydrogen atom or a methyl group. d represents a monovalent hydrocarbon group having 1 to 20 carbon atoms, and the hydrocarbon group may contain an ether bond, an ester bond, or a urethane bond therein. d R represents that 40 mol % or more of all the units represented by the general formula (2) are dicyclopentanyl groups or dicyclopentenyl groups. e represents a divalent hydrocarbon group having 2 to 10 carbon atoms. p represents the number 0 or 1. X represents a hydrogen atom or -OC-L-(COOH) k group (wherein L represents a divalent or trivalent carboxylic acid residue, and k is 1 to 2).
4. The photosensitive resin composition according to claim 1, further comprising (F) one or more light-shielding materials selected from the group consisting of black organic pigments, mixed-color organic pigments, and black inorganic pigments.
5. The photosensitive resin composition according to claim 1 , further comprising (E) a curing agent and / or a curing accelerator.
6. 2. The photosensitive resin composition according to claim 1, wherein the component (G) has a refractive index of 1.20 to 1.50 and an average particle size of 1 to 150 nm.
7. A cured film obtained by curing the photosensitive resin composition according to any one of claims 1 to 6.
8. A substrate having the cured film according to claim 7 on the substrate.
9. A method for producing a substrate with a cured film by forming a cured film pattern on a substrate, comprising the steps of: A method for producing a substrate with a cured film, comprising applying the photosensitive resin composition according to any one of claims 1 to 6 onto a substrate, exposing the composition through a photomask, removing unexposed areas by development, and heating the composition to form a cured film pattern.
Citation Information
Patent Citations
Polyacetal resin composition and method for producing polyacetal resin composition
JP2020105252A
Photosensitive composition, colored pattern, and method for producing the same
JP2021071661A
Curable composition and cured product of the same, and wafer-level lens
JP2024025155A
Negative photosensitive composition, optical semiconductor device, solid-state imaging device and electronic device
WO2022210797A1
Black resin composition for light blocking films, substrate with light blocking film obtained by curing composition, color filter having substrate with light blocking film, and touch panel
JP2016161926A
Cited By
Resin, resin composition and application thereof
CN121045472A