Inkjet ink composition and production method thereof

The inkjet ink composition addresses filter clogging by using ethylenically unsaturated monomers with controlled SP value differences and stirring/filtration, ensuring stable ejection in inkjet printers and material jet stereolithography.

JP2024145914APending Publication Date: 2024-10-15MAXELL LTD

Patent Information

Application Number
JP2023058508
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Inkjet printer filters can become clogged due to the generation of foreign matter, such as homopolymers, from certain components in active energy ray-curable inkjet ink compositions, leading to poor ejection and stability issues.

Method used

An inkjet ink composition comprising ethylenically unsaturated monomers with specific SP value differences and controlled stirring and filtration conditions to prevent homopolymer aggregation, ensuring stable and continuous discharge.

Benefits of technology

The ink composition effectively prevents filter clogging, allowing stable and continuous ejection over time, suitable for use in inkjet printers and material jet stereolithography.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145914000001
    Figure 2024145914000001
  • Figure 2024145914000002
    Figure 2024145914000002
  • Figure 2024145914000003
    Figure 2024145914000003
Patent Text Reader

Abstract

To provide an active energy ray-curable inkjet ink composition which does not easily cause clogging of a filter in the inkjet printer and can be stably discharged continuously.SOLUTION: An active energy ray-curable inkjet ink composition comprises at least two kinds of ethylenically unsaturated monomers and at least one kind of photoinitiator. The ethylenically unsaturated monomers comprise an ethylenically unsaturated monomer (A) having an SP value of 10 or more and an ethylenically unsaturated monomer (B) having an SP value of less than 10. Among the ethylenically unsaturated monomers contained in the composition, the difference between the SP value of the ethylenically unsaturated monomer (A) having the highest SP value and the SP value of the ethylenically unsaturated monomer (B) having the lowest SP value is 1 or more. The content of the ethylenically unsaturated monomcomposition er (A) is less than the content of the ethylenically unsaturated monomer (B). When 100 ml of the ink-jet ink is stirred at 1,500 rpm for 12 hours using a stirrer having a major axis of 30 mm or more and thereafter filtered using a hydrophilic PTFE membrane filter having a pore size of 1 μm at a filtration pressure of 0.8 MPa, the ratio of the time T1 for the first 20 ml of the 100 ml to pass the filter to the time T2 for the last 20 ml of the 100 ml to pass the filter is 0.5 or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an actinic radiation-curable ink-jet ink composition and a method for producing the same. [Background technology]

[0002] An image forming method by an inkjet system using an active energy ray curable inkjet ink is used in various printing fields as a method capable of easily and inexpensively forming images on various recording media at high speed. In recent years, the inkjet system has been utilized not only for forming two-dimensional images but also for producing three-dimensional objects, and a three-dimensional object can be freely produced by discharging an active energy ray curable inkjet ink from an inkjet nozzle and laminating a cured layer having a predetermined shape.

[0003] An active energy ray-curable inkjet ink typically contains a polymerizable compound that is cured by active energy rays and a photopolymerization initiator, and the components are determined depending on the application of the ink, the desired performance, etc. For example, Patent Documents 1 to 3 disclose active energy ray-curable inkjet ink compositions that contain several types of ethylenically unsaturated monomers and polymerization initiators depending on the respective purposes. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2021 / 182509 [Patent Document 2] JP 2013-79383 A [Patent Document 3] JP 2016-14144 A Summary of the Invention [Problem to be solved by the invention]

[0005] In forming images or three-dimensional objects by the inkjet method, it is important that the ink composition used can be stably discharged by the inkjet printer. However, depending on the components constituting the ink composition, foreign matter originating from the components may be generated during storage of the ink composition, and the generated foreign matter may clog a filter provided in an ink supply path in an inkjet head or inkjet printer, causing discharge failure.

[0006] An object of the present invention is to provide an actinic ray-curable ink-jet ink composition that is unlikely to clog the filter of an ink-jet printer and can be stably and continuously ejected. [Means for solving the problem]

[0007] The present inventors have conducted intensive research to solve the above problems and have completed the present invention. That is, the present invention provides the following preferred embodiments. [1] An active energy ray-curable inkjet ink composition comprising at least two ethylenically unsaturated monomers and at least one photopolymerization initiator, the ethylenically unsaturated monomer comprises an ethylenically unsaturated monomer (A) having an SP value of 10 or more and an ethylenically unsaturated monomer (B) having an SP value of less than 10; Among the ethylenically unsaturated monomers contained in the composition, the difference between the SP value of the ethylenically unsaturated monomer (A) having the highest SP value and the SP value of the ethylenically unsaturated monomer (B) having the lowest SP value is 1 or more; The content of the ethylenically unsaturated monomer (A) is less than the content of the ethylenically unsaturated monomer (B), The ink-jet ink composition, wherein when 100 ml of the ink-jet ink composition is stirred at 1,500 rpm for 12 hours using a stirrer having a major axis of 30 mm or more, and then filtered using a hydrophilic PTFE membrane filter having a pore size of 1 μm at a filtration pressure of 0.8 MPa, the ratio of the time T1 required for the first 20 ml of the 100 ml to the time T2 required for the last 20 ml of the 100 ml to pass is 0.5 or more. [2] The ink-jet ink composition according to [1] above, wherein the ethylenically unsaturated monomer (A) includes a nitrogen atom-containing ethylenically unsaturated monomer. [3] The ethylenically unsaturated monomer (A) is (meth) The ink-jet ink composition according to [1] or [2] above, further comprising an acrylamide. [4] The ink-jet ink composition according to any one of [1] to [3] above, wherein a mass ratio of the content of the ethylenically unsaturated monomer (A) to the content of the ethylenically unsaturated monomer (B) (ethylenically unsaturated monomer (A) / ethylenically unsaturated monomer (B)) is 0.03 to 0.9. [5] The ink-jet ink composition according to any one of [1] to [4] above, wherein the total content of ethylenically unsaturated monomers having an SP value that is less than 1 different from the SP value of the ethylenically unsaturated monomer (A) having the highest SP value is less than the content of the ethylenically unsaturated monomer (A) having the highest SP value. [6] based on the total weight of the inkjet ink composition, 1 to 49% by mass of an ethylenically unsaturated monomer (A), 5 to 90% by mass of an ethylenically unsaturated monomer (B), and 0.1 to 15% by mass of photopolymerization initiator The ink-jet ink composition according to any one of the above [1] to [5], [7] The ink-jet ink composition according to any one of [1] to [6] above, which is a clear ink composition having a colorant content of 0.1 mass % or less based on the total mass of the ink composition. [8] The ink-jet ink composition according to any one of [1] to [7] above, which is a model material composition used in a material jet stereolithography method. [9] A method for producing an active energy ray-curable ink-jet ink composition comprising a photopolymerization initiator, and an ethylenically unsaturated monomer (A) having an SP value of 10 or more and an ethylenically unsaturated monomer (B) having an SP value less than 10, the SP values ​​of which differ by 1 or more, wherein the content of the ethylenically unsaturated monomer (A) is less than the content of the ethylenically unsaturated monomer (B), A step of agglomerating the homopolymer of the ethylenically unsaturated monomer (A); and A step of removing the homopolymer aggregates obtained in the previous step. A method comprising:

[10] The method according to [9] above, wherein the step of agglomerating the homopolymer is carried out by stirring the ethylenically unsaturated monomer (A) and the ethylenically unsaturated monomer (B) for 3 hours or more.

[11] The method according to [9] above, wherein the step of aggregating the homopolymer is carried out by stirring all of the components constituting the inkjet ink composition for 3 hours or more.

[12] The method according to any one of the above [9] to

[11] , wherein the step of aggregating the homopolymer is carried out at 5 to 45°C.

[13] The method according to any one of [9] to

[12] above, wherein the step of removing the aggregates is carried out by filtration.

[14] The method according to

[13] , wherein a glass fiber filter is used in the filtration.

[15] The method according to

[13] or

[14] , wherein the filtration accuracy of the filter is 0.8 μm or less. Effect of the Invention

[0008] According to the present invention, it is possible to provide an actinic ray-curable ink-jet ink composition which is unlikely to clog the filter of an ink-jet printer even when stored for a long period of time and can be stably and continuously discharged. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, the embodiments of the present invention will be described in detail. Note that the scope of the present invention is not limited to the embodiments described here, and various modifications can be made without departing from the spirit of the present invention.

[0010] <Inkjet ink composition> The ink-jet ink composition of the present invention contains at least two kinds of ethylenically unsaturated monomers and at least one kind of photopolymerization initiator. In the present invention, the at least two kinds of ethylenically unsaturated monomers include an ethylenically unsaturated monomer (A) having an SP value of 10 or more (hereinafter also referred to as "monomer (A)") and an ethylenically unsaturated monomer (B) having an SP value of less than 10 (hereinafter also referred to as "monomer (B)"), and among the ethylenically unsaturated monomers contained in the ink-jet ink composition of the present invention, the difference between the SP value of the monomer (A) having the highest SP value and the SP value of the monomer (B) having the lowest SP value is 1 or more. In addition, in the ink-jet ink composition of the present invention, the content of the monomer (A) is less than the content of the monomer (B).

[0011] The present inventors have found that when an ink composition containing a monomer (A) and a monomer (B) whose SP values ​​differ from each other by 1 or more is stored for a certain period of time or more (for example, a long period of time such as one month to one year) and then used in an inkjet printer, filter clogging may occur in the ink supply path in the printer, and that the cause is aggregates derived from the monomers constituting the ink composition. Although the reason for this phenomenon is not necessarily clear, it is presumed that it may occur as follows. Many of the ethylenically unsaturated monomers that are generally used as components that can constitute an inkjet ink composition are liquid. In the manufacturing process of an ethylenically unsaturated monomer that is a liquid monomer, or in some cases during the distribution process or storage as a product, a homopolymer of the monomer may be spontaneously generated, and often the homopolymer of the monomer is dissolved in the monomer and exists in a small amount. When such a monomer is used as a part of the components that constitute the inkjet ink composition, if a component that can be a poor solvent for the monomer is also included, the homopolymer of the monomer that exists in a small amount together with the monomer gradually precipitates. It is further believed that the particles aggregate over time and cause the aggregates to clog filters in the printer.

[0012] For example, a monomer (B) having an SP value different from that of a monomer (A) by 1 or more can be a poor solvent for a homopolymer of the monomer (A) that exists in a small amount together with the monomer (A). When the content of the monomer (B) that acts as a poor solvent is large, the homopolymer of the monomer (A) tends to gradually precipitate in the ink composition. When the homopolymer of the monomer (A) precipitates in the ink composition, the precipitated homopolymers may aggregate with each other over time. For this reason, an ink composition having such a composition tends to clog the filter in an inkjet printer.

[0013] The present invention provides an ink-jet ink composition that is composed of components that are prone to filter clogging due to aggregates derived from the homopolymer of the monomer (A) as described above, and that is less likely to cause filter clogging by controlling the filtration rate within a specific range when the ink composition is stirred under specific conditions and then filtered through a filter. Specifically, when 100 ml of the ink-jet ink composition of the present invention is stirred at 1,500 rpm for 12 hours using a stirrer with a major axis of 30 mm or more and then filtered through a hydrophilic PTFE membrane filter with a pore size of 1 μm at a filtration pressure of 0.8 MPa, the ratio (T1 / T2) of the time T1 for the first 20 ml of 100 ml to the time T2 for the last 20 ml of 100 ml to pass is 0.5 or more.

[0014] In measuring the T1 / T2 value, the container in which the ink-jet ink composition is stirred may be any container with a flat bottom and made of a material that does not interfere with the stirring bar. Examples include a beaker and a glass bottle. From the viewpoint of appropriate stirring treatment of the ink composition to be measured, the capacity of the container is usually 250 to 600 ml, and it is preferable to use a 300 ml beaker.

[0015] The stirrer used for stirring is one that has a major axis of 30 mm or more and can sufficiently stir the ink composition under the above conditions. The shape of the stirrer may be tapered, oval, cylindrical, rugby ball, or the like. If the stirrer has a major axis of 30 mm or more, the presence of a homopolymer of a monomer that can cause aggregates over time can be confirmed in 100 ml of the ink composition under the above stirring conditions. From the viewpoint of sufficient stirring and ease of stirring the ink composition, a stirrer having a major axis of 30 to 70 mm is preferred, and a stirrer having a major axis of 30 to 50 mm and a diameter of Φ5 to 20 mm is more preferred. In the present disclosure, the major axis of the stirrer means the length in the longest direction of the stirrer. In addition, the diameter of the stirrer means the length in the direction perpendicular to the major axis, and in the case of a tapered type or the like where the length in the direction perpendicular to the major axis is not fixed, it is preferable that the longest diameter is within the above range.

[0016] In the present invention, the ink-jet ink composition is stirred, for example, by using a magnetic stirrer and stirring with the stirring bar at 1500 rpm for 12 hours. The temperature during stirring is preferably in the range of 25° C.±5° C. In detail, the stirring operation in measuring the T1 / T2 value can be performed according to the method described in the Examples below.

[0017] After stirring under the above conditions, the mixture is filtered at a filtration pressure of 0.8 MPa using a hydrophilic PTFE (polytetrafluoroethylene) membrane filter with a pore size of 1 μm, and the time T1 for the first 20 ml of 100 ml to pass through and the time T2 for the last 20 ml of 100 ml to pass through are measured. As the hydrophilic PTFE (polytetrafluoroethylene) membrane filter with a pore size of 1 μm, for example, a hydrophilic PTFE membrane filter (pore size: 1.00 μm) manufactured by ADVANTEC, an Omnipore membrane filter (pore size: 1.00 μm) manufactured by Merck Millipore, etc. can be used. The filtration method is not particularly limited as long as the filtration pressure can be adjusted to 0.8 MPa, but reduced pressure filtration is preferred from the viewpoint of control of the filtration pressure and ease of operation.

[0018] The time T1 for 20 ml of the ink-jet ink composition to flow after the start of the passage of 100 ml of the ink-jet ink composition to be measured, and the time T2 for 20 ml to flow before the end of the passage, can be measured, for example, as follows. A filter holder for vacuum filtration is attached to a vacuum filtration chuck, and the filter is set. While measuring 20 ml of the ink composition to be measured for T1 and T2, filtration is started under a reduced pressure of 0.8 MPa. The time measurement is started with a stopwatch from the moment the ink composition passes through the filter, and the time from the top of the filter to the moment when 20 ml of the ink composition has passed through the filter is defined as T1. Next, 60 ml of the ink composition is passed through the filter as it is, and then T2 is measured in the same manner as T1 while measuring the remaining 20 ml. T2 is the time from the moment when the remaining 20 ml of the ink composition starts passing through the filter to the moment when all 20 ml of the ink composition has passed through the filter.

[0019] The liquid temperature of the ink-jet ink composition during the measurement of T1 and T2 is preferably adjusted to within the range of 25°C ± 1.0°C.

[0020] The clogging of the filter in the inkjet printer to be solved by the present invention is caused by a homopolymer of the monomer (A) present in a small amount dissolved in the monomer (A) constituting the inkjet ink composition. This homopolymer of the monomer (A) is considered to be present dissolved in the monomer (A) with an extremely small size (molecular weight), and therefore, for example, it is difficult to remove it by filtering the monomer (A) before using it as one component of the ink composition. For this reason, when the monomer (A) is used as a component of the ink composition together with the monomer (B) which can be a poor solvent for the monomer (A), it is difficult to suppress the generation of aggregates derived from the homopolymer of the monomer (A). In the present invention, by stirring the ink composition containing the monomer (A) and the monomer (B) under the above-mentioned specific conditions, it is possible to accelerate the aggregation of the homopolymer of the monomer (A), which may occur gradually over time under natural conditions. That is, when the ink composition is stirred under the above-mentioned specific conditions and then subjected to the above-mentioned specific filtration operation, the ink composition having a small T1 / T2 value (less than 0.5) is considered to have a large amount of homopolymer aggregates of the monomer (A) that hinder filtration. In other words, it is presumed that in such an ink composition, a homopolymer of the monomer (A) that may cause filter clogging when stored under natural conditions is present in a state dissolved in the monomer (A). On the other hand, in an ink composition having a T1 / T2 value of 0.5 or more, it is considered that there is no or almost no homopolymer of the monomer (A) that may cause filter clogging by causing aggregation over time. In other words, it is considered that such an ink composition is unlikely to cause filter clogging in an inkjet printer even when stored for a long period of time. Therefore, it is possible to obtain an inkjet ink composition that is unlikely to cause filter clogging by using the above-mentioned T1 / T2 value as an index.

[0021] When the value of T1 / T2 is 0.5 or more, it is possible to obtain an ink composition that is difficult to cause filter clogging due to aggregates derived from the homopolymer of the monomer (A) and can be continuously discharged. In addition, it is considered that the homopolymer of the monomer (A), which is a cause of the generation of aggregates over time, is not dissolved in the ink-jet ink composition having a value of T1 / T2 within the above range, and the generation of aggregates over time is suppressed and the ink-jet ink composition can be stably stored for a long period of time. From the viewpoint of further enhancing the effect of suppressing the generation of aggregates and preventing filter clogging, the value of T1 / T2 in the ink-jet ink composition of the present invention is preferably 0.6 or more, more preferably 0.65 or more, even more preferably more than 0.7, particularly preferably 0.75 or more, and particularly preferably 0.8 or more. In the above-mentioned method for measuring T1 / T2, it is desirable that the speed at which 100 ml of the ink composition passes through does not change from the beginning to the end, so the value of T1 / T2 is preferably as close to 1.0 as possible. Taking into consideration measurement errors, the value of T1 / T2 is usually 0.5 to 1.1, and preferably in the range of 0.5 to 1.0.

[0022] The time T1 required for 20 ml of 100 ml of the ink-jet ink composition to flow after the start of the flow can vary depending on the composition, viscosity, wettability, and use of the ink-jet ink composition. From the viewpoint of the speed of image formation and three-dimensional modeling by the ink-jet printer, the accuracy and characteristics of the resulting image and model, etc., T1 is usually 1800 seconds or less, preferably 1500 seconds or less, and more preferably 1200 seconds or less. The lower limit of T1 is not particularly limited, but is usually 60 seconds or more in consideration of the viscosity suitable for ejection from the ink-jet printer. The above value of T1 is the time assumed when a filter with a diameter of 2.5 cm is used. The filter diameter and the flow time are usually inversely proportional to each other, and if a filter with a diameter larger than the filter diameter is used, the preferred range of T1 becomes shorter inversely proportional to the diameter. This is also true for T2 described later.

[0023] The time T2 for 20 ml of the ink-jet ink composition to flow before the end of the passage of 100 ml of the ink-jet ink composition may vary depending on the composition, viscosity, wettability, and use of the ink-jet ink composition. From the viewpoints of the effect of suppressing filter clogging in an ink-jet printer, the speed of image formation and three-dimensional modeling, and the accuracy and characteristics of the resulting images and models, for example, when a filter with a diameter of 2.5 cm is used, T2 is usually 3600 seconds or less, preferably 3000 seconds or less, and more preferably 1200 seconds or less. The lower limit of T2 is not particularly limited, but is usually 60 seconds or more in consideration of the effect of suppressing filter clogging and the viscosity suitable for ejection from an ink-jet printer.

[0024] The value of T1 / T2 can be controlled to a desired range by appropriately determining the types, combinations and amounts of the monomers (A) and (B) constituting the inkjet ink composition, and then forcibly precipitating and coagulating the homopolymer of the monomer (A) present in a small amount dissolved in the monomer (A) constituting the inkjet ink composition, and removing it. Specifically, for example, the types, combinations and amounts of each component in the inkjet ink composition can be appropriately adjusted based on the preferred embodiments of the monomer (A), monomer (B) and other polymerizable compounds in the inkjet ink composition of the present invention described later. In particular, T1 / T2 can be controlled to a desired range by efficiently removing the homopolymer of the monomer (A) present in a small amount dissolved in the monomer (A) according to the method and conditions for precipitating and coagulating the homopolymer of the monomer (A) in the manufacturing method of the inkjet ink composition of the present invention described later.

[0025] The inkjet ink composition of the present invention contains at least two kinds of ethylenically unsaturated monomers. The ethylenically unsaturated monomer is a polymerizable monomer having at least one ethylenic double bond in the molecule, which has the property of being cured by energy rays. The ethylenically unsaturated monomer may be a monofunctional ethylenically unsaturated monomer having one ethylenic double bond in the molecule, or a polyfunctional ethylenically unsaturated monomer having two or more ethylenic double bonds in the molecule.

[0026] The ink-jet ink composition of the present invention contains, as the ethylenically unsaturated monomer, an ethylenically unsaturated monomer (A) having an SP value of 10 or more and an ethylenically unsaturated monomer (B) having an SP value of less than 10. The SP value of the monomer (A) having the highest SP value among the ethylenically unsaturated monomers constituting the ink-jet ink composition of the present invention differs by 1 or more from the SP value of the monomer (B) having the lowest SP value. That is, the ink-jet ink composition of the present invention contains at least one combination of monomer (A) and monomer (B) whose SP value difference is 1 or more. For example, when one monomer is contained as each of monomer (A) and monomer (B), if the SP values ​​of these monomers differ from each other by 1 or more, monomer (B) functions as a poor solvent for a homopolymer of monomer (A), and thus the homopolymer of monomer (A) dissolved in monomer (A) can be precipitated.

[0027] Here, the SP value means the solubility parameter, which is a value inherent to a substance. The SP value can be measured experimentally, or calculated based on the molecular structure. In this specification, the SP value of each monomer means the value at 25°C obtained according to the Fedors method (Harasaki Yuji, "Basic Science of Coatings", Chapter 3, page 35, 1977, Maki Shoten Publishing), which is one of the methods for estimating based on the molecular structure. The unit of SP value is the conventionally used unit (cal / cm 3 ) 1 / 2 To convert to SI units, multiply by approximately 2.0455 to get (J / cm 3 ) 1 / 2 It becomes.

[0028] In the inkjet ink composition of the present invention, the difference in SP value between the monomer (A) having the highest SP value and the monomer (B) having the lowest SP value is preferably 1.1 or more, more preferably 1.2 or more, and even more preferably 1.3 or more. When the difference in SP value between the monomer (A) having the largest difference in SP value and the monomer (B) is equal to or more than the above lower limit, the homopolymer of the monomer (A) is easily removed, so that the value of T1 / T2 can be controlled within a desired range, and an inkjet ink composition that can more effectively suppress filter clogging in an inkjet printer can be obtained. The upper limit of the difference in SP value in the combination of the monomer (A) and the monomer (B) having the largest difference in SP value is usually 7 or less, preferably 6 or less, more preferably 5 or less, and even more preferably 4.5 or less, from the viewpoint of compatibility between the monomers. In one embodiment of the present invention, the difference in SP value in the combination of monomer (A) and monomer (B) having the largest difference in SP value is preferably 1 or more and 7 or less, more preferably 1.1 or more and 6 or less, even more preferably 1.2 or more and 5 or less, and particularly preferably 1.3 or more and 4.5 or less.

[0029] In the inkjet ink composition of the present invention, it is preferable that, based on the total mass of all monomers (A), preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, particularly preferably 90% by mass or more, and particularly preferably 95% by mass or more of monomers (A) have a monomer (B) having an SP value different by 1 or more. When the monomer (B) is present in an amount equal to or greater than the above lower limit relative to the monomer (A) constituting the inkjet ink composition, it is possible to obtain an inkjet ink composition that is easy to control the T1 / T2 value within a desired range, is less likely to cause filter clogging in an inkjet printer, and can be stably discharged. From the viewpoint of obtaining the above-mentioned effect, in a preferred embodiment of the present invention, it is preferable that, based on the total mass of all monomers (A), a monomer (B) having at least one SP value different by 1 or more is present. When the inkjet ink composition contains two or more monomers (A), the monomer (B) may be one or more. For example, one monomer (B) having an SP value different by 1 or more from all of two or more monomers (A) may be included, or separate monomers (B) having an SP value different by 1 or more from two or more monomers (A) may be included. The difference in SP value in such a combination of monomer (A) and monomer (B) having an SP value difference of 1 or more is preferably 1 or more and 7 or less, more preferably 1.1 or more and 6 or less, even more preferably 1.2 or more and 5 or less, and particularly preferably 1.2 or more and 4.5 or less. In one embodiment of the present invention, it is preferable that the difference in SP value is within the above range in all combinations of monomer (A) and monomer (B) having an SP value difference of 1 or more.

[0030] In the inkjet ink composition of the present invention, the content of monomer (A) is less than the content of monomer (B). By having a large amount of monomer (B) that can function as a poor solvent for monomer (A), it is possible to control the value of T1 / T2 within a desired range, thereby obtaining an inkjet ink composition that is unlikely to clog the filter of an inkjet printer and can be stably discharged.

[0031] In one embodiment of the present invention, the mass ratio of the content of the monomer (A) to the content of the monomer (B) (monomer (A) / monomer (B)) is preferably 0.03 to 0.9. When the content ratio of the monomer (A) to the monomer (B) is within the above range, the value of T1 / T2 can be easily controlled to a desired range, and the filter clogging in the inkjet printer is unlikely to occur, and an inkjet ink composition that can be stably discharged can be obtained. Since the homopolymer of the monomer (A) is easily removed, the content ratio of the monomer (A) to the monomer (B) may be, for example, 0.03 to 0.8, 0.03 to 0.7, or 0.03 to 0.65 depending on the case, and in a particularly preferred embodiment, it is 0.03 or more and less than 0.6. When a plurality of monomers (A) and / or monomers (B) are contained, the content ratio means the content ratio of the total monomers (A) to the total monomers (B) constituting the inkjet ink composition. However, in particular, when the content ratio of monomer (A) and monomer (B) having an SP value difference of 1 or more (when multiple monomers (B) having SP values ​​differing by 1 or more are present for one monomer (A), all corresponding monomers (B)) is within the above range, the above-mentioned effects of the present invention can be expected to be improved.

[0032] In one embodiment of the present invention, the total content of ethylenically unsaturated monomers having an SP value that is less than 1 different from the SP value of the monomer (A) having the highest SP value (hereinafter also referred to as "monomers having an SP value less than 1") is preferably less than the content of the monomer (A) having the highest SP value. When the content of ethylenically unsaturated monomers having a small difference in SP value with respect to the monomer (A) having the highest SP value is small, it becomes easier to control the value of T1 / T2 within a desired range. In particular, the higher the mass ratio of the content of the monomer (A) to the content of the monomer (B) is (the closer to 1), the lower the content of the monomers having an SP value less than 1, and the more likely it is that the effect of suppressing filter clogging can be improved compared to the case where the content of the monomers having an SP value less than 1 is high. The content of the monomers having an SP value less than 1 relative to 100 parts by mass of the monomer (A) having the highest SP value is preferably 60 parts by mass or less, more preferably 50 parts by mass or less, and may be, for example, 20 parts by mass or less or 10 parts by mass or less. In one embodiment of the present invention, the inkjet ink composition of the present invention is substantially free of an ethylenically unsaturated monomer having an SP value less than 1 different from that of the monomer (A) having the highest SP value, and may be 0 part by mass. The term "substantially free" means that the content of a monomer having an SP value less than 1 is 1 part by mass or less per 100 parts by mass of the monomer (A) having the highest SP value. Hereinafter, the term "substantially free" in this specification means that the content is 1 part by mass or less relative to the standard, as described above. The "monomer having an SP value less than 1" may include both the monomer (A) and the monomer (B).

[0033] When the ink-jet ink composition contains two or more monomers (A), it is preferable that the total content of ethylenically unsaturated monomers having an SP value less than 1 different from that of the monomer (A) other than the monomer (A) having the highest SP value is less than the content of the monomer (A) other than the monomer (A) having the highest SP value. This makes it easier to control the T1 / T2 value to a desired range. In one embodiment of the present invention, the content is the same as the preferred range of the content of monomers having an SP value less than 1 relative to the monomer (A) having the highest SP value described in the previous paragraph.

[0034] In one embodiment of the present invention, the total mass of the ethylenically unsaturated monomers whose SP value difference with respect to the total amount of the monomers (A) is less than 1 is preferably less than the content of the monomer (A) whose content is the highest. As one embodiment, it may be preferable that the content of the monomer (A) having the highest SP value is the highest with respect to the total amount of the monomers (A). When the inkjet ink composition contains two or more monomers (A), the content of the monomer (A) having the highest SP value with respect to the total amount (100% by mass) of the monomers (A) is preferably 50% by mass or more, more preferably 55% by mass or more, even more preferably 60% by mass or more, particularly preferably 65% ​​by mass or more, and may be, for example, 70% by mass or more, 80% by mass or more, or 90% by mass or more. When the content of the monomer (A) having the highest SP value with respect to the total amount of the monomers (A) is the above-mentioned lower limit or more, it is easier to control the value of T1 / T2 to a desired range.

[0035] In the present invention, the monomer (A) and the monomer (B) are not particularly limited, and can be appropriately selected from ethylenically unsaturated monomers known in the art according to the application and desired physical properties and characteristics of the ink-jet ink composition. Examples of such ethylenically unsaturated monomers include: Methyl (meth)acrylate, ethyl (meth)acrylate, isobutyl (meth)acrylate, amyl (meth)acrylate, isoamyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, isomyristyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, 2-ethylhexyl-diglycol (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, t-butyl (meth)acrylate, β-carboxyethyl (meth)acrylate alkyl (meth)acrylates having a linear or branched alkyl group, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2-(2-ethoxyethoxy)ethyl (meth)acrylate, butoxyethyl (meth)acrylate, ethoxy-diethylene glycol (meth)acrylate, methoxy-triethylene glycol (meth)acrylate, methoxy-polyethylene glycol (meth)acrylate, methoxydipropylene glycol (meth)acrylate, caprolactone (meth)acrylate, and 2-(meth)acryloyloxyethyl-succinic acid; (meth)acrylates having an alicyclic structure, such as cyclohexyl (meth)acrylate, 4-t-butylcyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, adamantyl (meth)acrylate, 3,3,5-trimethylcyclohexanol (meth)acrylate, and 2-(meth)acryloyloxyethyl hexahydrophthalic acid; (Meth)acrylates having an aromatic ring structure, such as phenoxyethyl (meth)acrylate, phenoxy-polyethylene glycol (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, nonylphenol ethylene oxide adduct (meth)acrylate, 2-(meth)acryloyloxyethyl-phthalic acid, and neopentyl glycol-acrylic acid-benzoic acid ester; (meth)acrylates having a heterocyclic structure, such as tetrahydrofurfuryl (meth)acrylate, cyclic trimethylolpropane formal (meth)acrylate, 4-(meth)acryloyloxymethyl-2-methyl-2-ethyl-1,3-dioxolane, and 4-(meth)acryloyloxymethyl-2-cyclohexyl-1,3-dioxolane; Monofunctional ethylenically unsaturated monomers containing a nitrogen atom, which are different from the (meth)acrylates, such as (meth)acrylamides, N-vinyllactams, and N-vinylformamide; 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 2-n-butyl-2-ethyl-1,3-propanediol di(meth)acrylate, 3-methyl-1,5-pentanediol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, Alkylene glycol di- or tri-(meth)acrylates such as dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, and glycerin propoxy tri(meth)acrylate; Di- or tri-(meth)acrylates containing a cyclic structure, such as cyclohexanedimethanol di(meth)acrylate, dimethyloltricyclodecane di(meth)acrylate, bisphenol A ethylene oxide adduct di(meth)acrylate, and bisphenol A propylene oxide adduct di(meth)acrylate; Polyfunctional ethylenically unsaturated monomers such as bifunctional or higher aminoacrylates The monomer (A) and the monomer (B) can be selected from a wide range of combinations, and can be used in combination, so long as the combination satisfies the above-mentioned relationship in SP value. In this specification, "(meth)acrylate" refers to either or both of acrylate and methacrylate, and "(meth)acrylamide" refers to either or both of acrylamide and methacrylamide.

[0036] The monomer (A) can be selected from a wide range of monofunctional or polyfunctional ethylenically unsaturated monomers as described above, so long as the monomer (A) has an SP value of 10 or more. (Meth)acrylic monomers such as benzyl methacrylate, phenoxyethyl acrylate (SP value: 10.12), tricyclodecane dimethanol diacrylate, pentaerythritol triacrylate, and pentaerythritol tetraacrylate; (Meth)acrylamides such as N,N-dimethylacrylamide, N,N-diethylacrylamide, hydroxyethylacrylamide (SP value: 13.33), and N,N-acryloylmorpholine (SP value: 11.21); N-vinyllactams such as N-vinylcaprolactam (SP value: 10.80); The monomer (A) may be used alone or in combination of two or more kinds.

[0037] In one embodiment of the present invention, the monomer (A) preferably contains an ethylenically unsaturated monomer containing a nitrogen atom. Hereinafter, an ethylenically unsaturated monomer having an SP value of 10 or more and containing a nitrogen atom is also referred to as "monomer (A1)". Examples of the monomer (A1) include (meth)acrylamides such as N,N-dimethylacrylamide, N,N-diethylacrylamide, N-isopropylacrylamide, hydroxyethylacrylamide, hydroxypropylacrylamide, and N,N-acryloylmorpholine, N-vinyl lactams such as N-vinylpyrrolidone and N-vinylcaprolactam, and N-vinylformamide. Among them, it is preferable to contain (meth)acrylamides, and more preferable to contain acryloylmorpholine. When the ethylenically unsaturated monomer (A1) containing a nitrogen atom, particularly a (meth)acrylamide, is contained, it is easy to obtain a printed coating film or a shaped object having high hardness and strength while maintaining the viscosity of the ink composition at an appropriate level.

[0038] The content of the monomer (A) in the inkjet ink composition of the present invention is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, based on the total mass of the inkjet ink composition, and is preferably 49% by mass or less, and more preferably 45% by mass or less. When the content of the monomer (A) is within the above range, it is possible to obtain an inkjet ink composition that has an excellent effect of suppressing filter clogging caused by the homopolymer of the monomer (A) while the monomer (A) is in an amount that allows the monomer (A) to function as one component of the inkjet ink composition. Since the value of T1 / T2 is easily controlled within a desired range, the content of the monomer (A) may be, for example, 40% by mass or less, 35% by mass or less, or 30% by mass or less, based on the total mass of the inkjet ink composition. In one embodiment of the present invention, the content of the monomer (A) is preferably 1 to 49% by mass, more preferably 2 to 45% by mass, based on the total mass of the inkjet ink composition, and may be, for example, 2 to 40% by mass, 2 to 35% by mass, or 3 to 30% by mass.

[0039] Monomer (B) can be broadly selected from the above monofunctional or polyfunctional ethylenically unsaturated monomers as long as the SP value is less than 10. Specific examples include alkyl (meth)acrylates having a linear or branched alkyl group such as hexanediol dimethacrylate (SP value: 9.56), tripropylene glycol diacrylate (SP value: 9.21), 2-ethylhexyl acrylate, dipropylene glycol diacrylate, and lauryl acrylate; and (meth)acrylates having an alicyclic structure such as isobornyl acrylate (SP value: 9.28), dicyclopentenyloxyethyl acrylate (SP value: 9.97), 3,3,5-trimethylcyclohexanol acrylate (SP value: 8.73), cyclic trimethylolpropane formal acrylate, tetrahydrofurfuryl acrylate, dicyclopentenyl acrylate, and dicyclopentanyl acrylate. The monomer (B) may be used alone or in combination of two or more kinds.

[0040] In the present invention, the monomer (B) may be appropriately selected depending on the monomer (A) used. In one embodiment of the present invention, the monomer (B) preferably contains an ethylenically unsaturated monomer having an alicyclic structure. Hereinafter, an ethylenically unsaturated monomer having an SP value of less than 10 and an alicyclic structure is also referred to as "monomer (B1)". Examples of the monomer (B1) include the (meth)acrylate having an alicyclic structure described above, cyclohexyl (meth)acrylate, 4-t-butylcyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, adamantyl (meth)acrylate, 3,3,5-trimethylcyclohexanol (meth)acrylate, and the like. Among them, it is preferable to contain isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, adamantyl (meth)acrylate, 3,3,5-trimethylcyclohexanol (meth)acrylate, and more preferable to contain isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, 3,3,5-trimethylcyclohexanol (meth)acrylate. When it contains a monomer (B1) having an alicyclic structure, it is possible to increase the hardness and strength of the printed coating film and the shaped object.

[0041] The content of the monomer (B) in the inkjet ink composition of the present invention is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, particularly preferably 30% by mass or more, particularly preferably 40% by mass or more, and preferably 90% by mass or less, more preferably 85% by mass or less, based on the total mass of the inkjet ink composition. When the content of the monomer (B) is within the above range, it is easy to control the value of T1 / T2, and it is possible to obtain an inkjet ink composition that is excellent in the effect of suppressing filter clogging caused by the homopolymer of the monomer (A). Since it is easy to control the value of T1 / T2 within the desired range, the content of the monomer (B) may be, for example, 50% by mass or more or 55% by mass or more, based on the total mass of the inkjet ink composition, as the case may be. In one embodiment of the present invention, the content of monomer (B) is preferably 5 to 90 mass%, more preferably 10 to 90 mass%, even more preferably 20 to 90 mass%, particularly preferably 30 to 90 mass%, and especially preferably 40 to 90 mass%, based on the total mass of the ink-jet ink composition, and may be, for example, 50 to 85 mass%, or 55 to 85 mass%.

[0042] The contents of monomer (A) and monomer (B) in the inkjet ink composition of the present invention are preferably 65 to 99 mass%, more preferably 70 to 99 mass%, and even more preferably 75 to 99 mass%, based on the total mass of the polymerizable compounds contained in the inkjet ink composition, and may be, for example, 65 to 95 mass%, 70 to 90 mass%, or 70 to 85 mass%. When the contents of monomer (A) and monomer (B) are within the above ranges, the value of T1 / T2 can be easily controlled to a desired range, and the effects of the present invention can be sufficiently obtained.

[0043] The inkjet ink composition of the present invention may contain a polymerizable compound other than the monomer (A) and the monomer (B). Examples of the polymerizable compound other than the monomer (A) and the monomer (B) include oligomers. The oligomer is a component that has the property of being polymerized and cured by irradiation with active energy rays. By blending an oligomer, it is possible to improve the strength and hardness while reducing the brittleness of the printed coating film or the shaped object. This makes it possible to obtain a printed coating film or a shaped object that is not easily broken even when bent. In this specification, the term "oligomer" refers to a polymer having a weight average molecular weight (M w The preferred weight average molecular weight (M) of the oligomer is 500 to 10,000. w ) is 800 or more, and more preferably exceeds 1,000. w ) means the weight average molecular weight in terms of polystyrene measured by GPC (gel permeation chromatography). The oligomers may be used alone or in combination of two or more kinds.

[0044] Examples of the oligomer include an epoxy (meth)acrylate oligomer, a polyester (meth)acrylate oligomer, a urethane (meth)acrylate oligomer, a polyether (meth)acrylate oligomer, etc. As the oligomer, a polyfunctional oligomer having two or more functionalities is preferable, and a bifunctional oligomer is more preferable.

[0045] From the viewpoint of being able to select materials with a wide range of properties, the oligomer constituting the inkjet ink composition of the present invention is preferably an oligomer having a urethane group, more preferably a urethane (meth)acrylate oligomer. Specific examples of the urethane (meth)acrylate oligomer include a urethane (meth)acrylate oligomer having a dicyclohexylmethane structure, a urethane (meth)acrylate oligomer having an isophorone structure, and a urethane (meth)acrylate oligomer having a cyclohexylmethane structure.

[0046] When the inkjet ink composition of the present invention contains an oligomer, the content thereof is preferably 1 to 30 mass %, more preferably 3 to 25 mass %, and even more preferably 5 to 23 mass %, based on the total mass of the polymerizable compounds contained in the inkjet ink composition. When the content of the oligomer is within the above upper and lower limits, it is easy to adjust the strength and hardness of the ink composition without affecting the control of T1 / T2 by the monomer (A) and the monomer (B).

[0047] The content of the polymerizable compound in the inkjet ink composition of the present invention is preferably 80 to 99.9 mass %, and can be, for example, 85 to 99 mass %, or 90 to 98 mass %, based on the total mass of the inkjet ink composition.

[0048] The inkjet ink composition of the present invention contains a photopolymerization initiator. The photopolymerization initiator is not particularly limited as long as it is a compound that promotes a radical reaction when irradiated with light having a wavelength in the ultraviolet, near ultraviolet, or visible light region. Examples of the photopolymerization initiator include benzoin compounds (e.g., benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isobutyl ether, etc.), acetophenone compounds (e.g., acetophenone, 2,2-diethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 2-hydroxy-2-methyl-phenylpropan-1-one, diethoxyacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, etc.), anthraquinone compounds (e.g., 2-ethylanthraquinone, 2-t-butylanthraquinone, 2-chloroanthraquinone, 2-amyl anthraquinone, etc.), and the like. raquinone, etc.), thioxanthone compounds (e.g., 2,4-diethylthioxanthone, 2-isopropylthioxanthone, 2-chlorothioxanthone, etc.), ketal compounds (e.g., acetophenone dimethyl ketal, benzyl dimethyl ketal, etc.), benzophenone compounds (e.g., benzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 4,4'-bismethylaminobenzophenone, etc.), acylphosphine oxide compounds (e.g., 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide), and mixtures of these compounds. These may be used alone or in combination of two or more. In addition, commercially available products may be used as the photopolymerization initiator. Examples of such commercially available products include DAROCURE TPO, IRGACURE184, and IRGACURE907 manufactured by BASF.

[0049] The content of the photopolymerization initiator in the inkjet ink composition may be appropriately determined depending on the type of polymerizable compound used, the content thereof, etc. In one embodiment of the present invention, the content of the photopolymerization initiator is preferably 0.1 to 15 mass %, more preferably 0.5 to 10 mass %, and even more preferably 1 to 8 mass %, based on the total mass of the inkjet ink composition. When the content of the photopolymerization initiator is within the above range, it is possible to reduce unreacted polymerization components, sufficiently increase the curability of the inkjet ink composition, and also to suppress the influence of the remaining unreacted photopolymerization initiator on the shaped object over time (for example, discoloration such as yellowing).

[0050] The inkjet ink composition may contain other additives as necessary within the range that does not impair the effects of the present invention. Examples of other additives include storage stabilizers, surface conditioners, antioxidants, UV absorbers, light stabilizers, polymerization inhibitors, chain transfer agents, fillers, diluents, thickeners, colorants, etc.

[0051] The surface conditioner is a component that adjusts the surface tension of the ink-jet ink composition to an appropriate range, and the type of the surface conditioner is not particularly limited. By adjusting the surface tension of the ink-jet ink composition to an appropriate range, it is possible to stabilize the ejection properties and suppress interfacial mixing during image formation or three-dimensional modeling.

[0052] Examples of the surface conditioner include silicone compounds. Examples of the silicone compounds include silicone compounds having a polydimethylsiloxane structure. Specific examples of the silicone compounds include polyether-modified polydimethylsiloxane, polyester-modified polydimethylsiloxane, and polyaralkyl-modified polydimethylsiloxane. These include the trade names BYK-300, BYK-302, BYK-306, BYK-307, BYK-310, BYK-315, BYK-320, BYK-322, BYK-323, BYK-325, BYK-330, BYK-331, BYK-333, BYK-337, BYK-344, BYK-370, BYK-375, BYK-377, BYK-UV3500, BYK-UV3510, BYK-UV3570 (all manufactured by BYK-Chemie), TEGO-Rad210 0, TEGO-Rad2200N, TEGO-Rad2250, TEGO-Rad2300, TEGO-Rad2500, TEGO-Rad2600, TEGO-Rad2700 (all manufactured by Degussa), Granol 100, Granol 115, Granol 400, Granol 410, Granol 435, Granol 440, Granol 450, B-1484, Polyflow ATF-2, KL-600, UCR-L72, UCR-L93 (manufactured by Kyoeisha Chemical Co., Ltd.), etc. may be used. Surface conditioners other than silicone-based compounds (for example, fluorine-based surface conditioners, etc.) may also be used. These may be used alone or in combination of two or more.

[0053] When the ink-jet ink composition contains a surface conditioner, the content thereof is preferably 0.005% by mass or more, more preferably 0.01% by mass or more, and even more preferably 0.05% by mass or more, based on the total mass of the ink-jet ink composition, and is preferably 3% by mass or less, more preferably 2% by mass or less, and even more preferably 1.5% by mass or less. When the content of the surface conditioner is within the above range, it is easy to adjust the surface tension of the ink-jet ink composition to an appropriate range.

[0054] The storage stabilizer is a component that can enhance the storage stability of the inkjet ink composition. In addition, it can prevent head clogging caused by polymerization of the polymerizable compound due to thermal energy. Examples of the storage stabilizer include hindered amine compounds (HALS), phenolic antioxidants, and phosphorus antioxidants. Specific examples include hydroquinone, methoquinone, benzoquinone, p-methoxyphenol, hydroquinone monomethyl ether, hydroquinone monobutyl ether, TEMPO, 4-hydroxy-TEMPO, TEMPOL, cupferron Al, IRGASTAB UV-10, IRGASTAB UV-22, FIRSTCURE ST-1 (manufactured by ALBEMARLE), t-butylcatechol, pyrogallol, and TINUVIN 111 FDL, TINUVIN 144, TINUVIN 292, TINUVIN XP40, TINUVIN XP60, and TINUVIN 400 (manufactured by BASF). These may be used alone or in combination of two or more.

[0055] When the inkjet ink composition contains a storage stabilizer, the content thereof is preferably 0.01 to 5% by mass based on the total mass of the inkjet ink composition, from the viewpoint of easily achieving the above-mentioned effects.

[0056] The inkjet ink composition of the present invention may be a clear ink composition that does not contain a colorant or that contains only a small amount of a pigment and / or dye such as a bluing agent, or may be a color ink composition that contains a colorant. When the inkjet ink composition of the present invention is a clear ink composition, the content of the colorant is usually 0.1% by mass or less, more preferably 0.05% by mass or less, based on the total mass of the inkjet ink composition, and the lower limit is 0% by mass or more.

[0057] When the ink-jet ink composition contains a colorant, the composition is not particularly limited, but preferably contains cyan, magenta, and yellow, and more preferably further contains white and / or black. The colorant may be a pigment or a dye.

[0058] Examples of cyan include CI Pigment Blue 15:3 and CI Pigment Blue 15:4. Examples of magenta include CI Pigment Red 122, CI Pigment Red 202, and CI Pigment Violet 19. Examples of yellow include CI Pigment Yellow 150 and CI Pigment Yellow 155. Examples of white include titanium oxide. Examples of black include carbon black.

[0059] When the inkjet ink composition contains a colorant, the content thereof may be appropriately set depending on the desired color of the inkjet ink composition and the type of colorant used, but is usually 0.1 to 5 mass %, more preferably 0.2 to 3 mass %, based on the total mass of the inkjet ink composition.

[0060] The inkjet ink composition of the present invention preferably has a viscosity of 1 mPa·s or more and 500 mPa·s or less at 25° C., since it is used in an inkjet printer. From the viewpoint of improving the ejection properties from the nozzle of the inkjet printer, the viscosity at 25° C. is preferably 10 to 400 mPa·s, and more preferably 20 to 300 mPa·s. The viscosity can be measured using an R100 type viscometer in accordance with JIS Z 8803. The viscosity of the inkjet ink composition can be controlled by adjusting the type and blending ratio of the polymerizable compound, the type and addition amount of the dilution solvent and thickener, etc.

[0061] The surface tension of the inkjet ink composition of the present invention is preferably 24 to 36 mN / m, and more preferably 26 to 32 mN / m. When the surface tension is within the above range, droplets can be normally formed from the nozzle even during high-speed ejection from the inkjet printer, making it easier to ensure an appropriate droplet volume and improving modeling accuracy. In the present invention, the surface tension of the inkjet ink composition can be controlled by adjusting the type and amount of the surface conditioner.

[0062] In the present invention, the composition of the inkjet ink composition can be determined by appropriately selecting the types, combinations and amounts of the monomer (A), the monomer (B) and the photopolymerization initiator, as well as other components as necessary, depending on the desired ink physical properties and characteristics, the use of the ink, the physical properties and characteristics of the printed matter, the physical properties and characteristics of the shaped object, etc. In one embodiment of the present invention, the inkjet ink composition of the present invention preferably contains 1 to 40% by mass of a monomer (A), 5 to 90% by mass of a monomer (B), and 0.1 to 15% by mass of photopolymerization initiator Includes.

[0063] The inkjet ink composition of the present invention is excellent in suppressing filter clogging in an inkjet printer, and is therefore suitable as a model material composition for use in material jet stereolithography (also referred to as inkjet stereolithography), which is desired to be continuously discharged stably and at high speed. In particular, the monomer (A1) containing a nitrogen atom, such as (meth)acrylamides and N-vinyllactams, is effective in improving the hardness and strength of a three-dimensional object, for example. On the other hand, according to the present inventors, the monomer (A1) often contains a homopolymer that causes aggregates over time and is dissolved in the monomer, which can be a cause of preventing stable continuous discharge in an inkjet printer. In the present invention, by controlling T1 / T2 to a specific range, filter clogging caused by the homopolymer of the monomer (A) can be effectively suppressed, and stable continuous discharge is possible. Therefore, it is possible to contain a relatively large amount of the monomer (A), which is prone to cause aggregates over time, particularly the monomer (A1), and to obtain a three-dimensional object with excellent hardness and strength under high production efficiency due to high-speed discharge.

[0064] When the inkjet ink composition of the present invention is used as a model material composition, the monomer (A) and the monomer (B) can be, for example, the polymerizable compounds constituting the model material composition described in International Publication No. 2021 / 182509, and the combination and blending amounts of the monomer (A) and the monomer (B) can be determined based on the SP value of each compound in accordance with the description above in this specification.

[0065] <Method of manufacturing inkjet ink composition> The inkjet ink composition of the present invention may, for example, A step of agglomerating a homopolymer of monomer (A), and A step of removing the homopolymer aggregates obtained in the previous step. The ink-jet ink composition of the present invention includes a monomer (A) having an SP value of 10 or more and a monomer (B) having an SP value of less than 10, the SP values ​​of which differ by 1 or more. As described above, in an ink composition having such a composition, the monomer (B) having an SP value different by 1 or more from the monomer (A) serves as a poor solvent for the homopolymer of the monomer (A) present in a small amount together with the monomer (A), and the homopolymer of the monomer (A) is likely to gradually precipitate in the ink composition. In the production method of the present invention, aggregates derived from the homopolymer of the monomer (A), which do not usually exist immediately after the production of the ink composition but may precipitate over time, are forcibly generated and removed during the preparation of the ink-jet ink composition. This makes it possible to remove the homopolymer of the monomer (A) present in a small amount dissolved in the monomer (A). If the homopolymer in the monomer (A) is forcibly aggregated and removed, no aggregates will be generated again in the inkjet ink composition thereafter. When such an ink composition is used in an inkjet printer, it is unlikely to clog the filter and can be ejected stably and continuously.

[0066] Accordingly, the present invention provides a method for producing an active energy ray-curable ink-jet ink composition comprising a photopolymerization initiator, and an ethylenically unsaturated monomer (A) having an SP value of 10 or more and an ethylenically unsaturated monomer (B) having an SP value of less than 10, the SP values ​​of which differ from each other by 1 or more, the content of the ethylenically unsaturated monomer (A) being lower than the content of the ethylenically unsaturated monomer (B), the method comprising the steps of: A step of agglomerating the homopolymer of the ethylenically unsaturated monomer (A); and A step of removing the homopolymer aggregates obtained in the previous step. The present invention also covers a method, including:

[0067] In the production method of the present invention, the step of aggregating the homopolymer of monomer (A) (hereinafter also referred to as the "aggregation step") is preferably carried out by stirring monomer (A) and monomer (B) for 3 hours or more. By stirring monomer (A) and monomer (B) for 3 hours or more, monomer (B) functions as a poor solvent for the homopolymer of monomer (A) present in small amounts together with monomer (A), and the homopolymer of monomer (A) can be precipitated and aggregated. The types, combinations, and blending amounts of monomer (A) and monomer (B) constituting the inkjet ink composition in the production method of the present invention are the same as those described above as being suitable for the inkjet ink composition of the present invention. By appropriately selecting these within the ranges suitable for the inkjet ink composition of the present invention, the homopolymer of monomer (A) can be more effectively removed.

[0068] In one embodiment of the present invention, the stirring of the monomer (A) and the monomer (B) can be performed in a mixture consisting of only the monomer (A) and the monomer (B) constituting the inkjet ink composition. When the inkjet ink composition contains two or more monomers (A) and / or monomers (B), the monomer (A) and / or monomer (B) contained in the mixture consisting of only the monomer (A) and the monomer (B) may each be one or two or more. From the viewpoint of effectively precipitating and aggregating the homopolymer of the monomer (A), it is preferable to include a combination of the monomer (A) and the monomer (B) having the largest difference in SP value. By performing the aggregation step in a mixture consisting of only the monomer (A) and the monomer (B), the monomer (B) can easily act as a poor solvent for the homopolymer of the monomer (A), and the precipitation and aggregating of the homopolymer of the monomer (A) can be efficiently performed.

[0069] In another embodiment of the present invention, the stirring of the monomer (A) and the monomer (B) can be performed with a mixture containing other components in addition to the monomer (A) and the monomer (B) constituting the inkjet ink composition. The mixture containing other components may be a part or all of the components other than the monomer (A) and the monomer (B) constituting the inkjet ink composition. When a part of other components is contained in addition to the monomer (A) and the monomer (B), a mixture in which the monomer (A) and the monomer (B) are the main components is preferred. The term "main components" means that the monomer (A) and the monomer (B) account for 50% by mass or more of the total mass of the mixture, preferably 60% by mass or more, more preferably 70% by mass or more, and particularly preferably 80% by mass or more. By performing the aggregation process with such a mixture, the precipitation and aggregation of the homopolymer of the monomer (A) can be efficiently performed. On the other hand, when the aggregation step is carried out on a mixture containing other components in addition to the monomer (A) and the monomer (B), particularly all of the other components, the number of steps for preparing the ink-jet ink composition can be reduced, which is advantageous in terms of production efficiency.

[0070] The mixture used in the aggregation step can be prepared by mixing necessary components such as monomer (A) and monomer (B) using, for example, a mixer or stirrer.

[0071] The stirring time in the aggregation step can be appropriately determined depending on the composition, temperature, stirring conditions, mixability and solubility of each component of the mixture used in the aggregation step. In one embodiment of the present invention, the stirring time is preferably 3 hours or more. When the stirring time is 3 hours or more, the homopolymer of the monomer (A) can be sufficiently precipitated and aggregated, and the homopolymer of the monomer (A) that may cause aggregates over time can be sufficiently removed. The upper limit of the stirring time is not particularly limited, but is usually 24 hours or less, preferably 12 hours or less, from the viewpoint of production efficiency. The stirring in the aggregation step may be the same as or different from the stirring conditions for preparing the mixture to be subjected to the aggregation step, but the stirring time in the production method of the present invention refers to the stirring time after the components constituting the mixture are uniformly mixed.

[0072] The stirring temperature in the aggregation step is preferably 5 to 45°C. When the stirring temperature is within the above range, the homopolymer of the monomer (A) is easily precipitated and aggregated. From the viewpoint of more efficiently precipitating and aggregating the homopolymer of the monomer (A), the stirring temperature is preferably 10°C or higher, more preferably 15°C or higher, and even more preferably 20°C or higher, and is preferably 40°C or lower, more preferably 35°C or lower, and even more preferably 30°C or lower. In a particularly preferred embodiment of the present invention, the stirring temperature is 25°C.

[0073] The stirring conditions in the aggregation step can be appropriately determined depending on the composition of the mixture to be stirred and the equipment and devices to be used. In order to increase the opportunity for the homopolymer precipitates of the monomer (A) to come into contact with each other and aggregate, it is preferable that the flow is turbulent. Turbulent stirring can be performed using a stirrer such as a disperser, a magnetic stirrer, a homogenizer, or a planetary mixer. In terms of ease and efficiency of stirring, a disperser or a magnetic stirrer is preferred. The stirring speed, etc. can be appropriately determined depending on the stirrer to be used, the viscosity of the solution to be stirred, the liquid amount, the container size, etc., so that turbulent stirring occurs.

[0074] The production method of the present invention includes a step of removing the aggregates of the homopolymer of monomer (A) after the aggregation step (hereinafter, also referred to as a "removal step"). By removing the aggregates of the homopolymer of monomer (A) obtained in the aggregation step, it is possible to control T1 / T2 within a desired range, and it is possible to obtain the inkjet ink composition of the present invention which is less likely to generate aggregates of the homopolymer of monomer (A) over time.

[0075] The removal of the aggregates is preferably carried out by filtration using a filter, since this is an easy operation and has excellent ability to remove aggregates.

[0076] The filter used for the filter filtration can be appropriately selected according to the size and properties of the aggregates to be removed, the properties, viscosity, pressure, flow rate, and liquid amount of the liquid (monomer mixture or ink composition) to be passed through. Examples of the filter include a depth filter and a screen filter. Examples of the depth filter include a porous filter, a nonwoven fabric / fiber laminate filter, a sintered metal filter, and a sintered wire mesh filter. Examples of the screen filter include a membrane filter, a filter paper / filter cloth filter, a hollow fiber filter, and a mesh wire mesh filter. Examples of the material of the filter include polypropylene, polyethylene, polyethylene terephthalate, polybutylene terephthalate, polytetrafluoroethylene, polystyrene, polyvinyl alcohol, polyvinylidene fluoride, polyethersulfone, urethane, acrylic, rayon, nylon, cellulose, glass, SUS, copper, and nickel. For the filter filtration, the above materials can be accumulated in a disk, cartridge, or capsule shape. In one embodiment of the present invention, from the viewpoint of productivity and filterability, it is preferable to use a cartridge or capsule-shaped glass fiber filter for the filter filtration.

[0077] The filtration accuracy of the filter used in the removal step can be appropriately selected depending on the size, amount, properties, etc. of the aggregates to be removed. In one embodiment of the present invention, the filtration accuracy of the filter is preferably 0.8 μm or less, more preferably 0.5 μm or less, and even more preferably 0.3 μm or less. If the filtration accuracy is equal to or less than the above upper limit, it is possible to sufficiently remove even fine aggregates of the homopolymer of the monomer (A). From the viewpoint of liquid permeability, the filtration accuracy is usually 0.1 μm or more.

[0078] Examples of the filtration method include vacuum filtration, reduced pressure filtration, and pressure filtration. The filtration conditions can be appropriately determined depending on the size and properties of the aggregates to be removed, and the properties, viscosity, pressure, flow rate, and liquid amount of the liquid (monomer mixture or ink composition) to be passed. For example, liquid transfer by a pump can be used.

[0079] When only a part of the components constituting the inkjet ink composition is subjected to the aggregation process, only the mixture that has been subjected to the aggregation process may be subjected to the removal process to remove aggregates in the mixture. In addition, after the aggregation process, the mixture that has been subjected to the aggregation process may be added with a part or all of the remaining components constituting the inkjet ink composition and then subjected to the removal process. When only a part of the components constituting the inkjet ink composition is subjected to the aggregation process and / or the removal process, the inkjet ink composition of the present invention is obtained by mixing the remaining components after the removal process. After mixing the remaining components, filtration may be performed again to remove foreign matter such as dust and impurities. In this case, the filtration conditions are not particularly limited and may be the same as or different from the filtration conditions in the removal process.

[0080] The inkjet ink composition of the present invention has T1 / T2 controlled within a specific range, and is excellent in the effect of suppressing the generation of aggregates over time originating from the homopolymer of the monomer (A). Therefore, the ink supply path in the inkjet printer is less likely to clog the filter, and stable continuous ejection is possible. The inkjet ink composition of the present invention is suitable as an ink for forming an image or an ink for forming a three-dimensional object to be used in an inkjet printer. The formation of an image or the formation of a three-dimensional object using the inkjet ink composition of the present invention can be carried out by a conventionally known method. EXAMPLES

[0081] The present invention will be described in more detail below with reference to examples. In the examples, "%" and "parts" are by mass % and parts by mass unless otherwise specified.

[0082] 1. Preparation of Inkjet Ink Composition Table 1 shows details of the components constituting the ink-jet ink compositions used in the examples and comparative examples.

[0083] [Table 1]

[0084] (1) Example 1 The components constituting the inkjet ink compositions were mixed and stirred according to the following preparation procedures 1 to 8, respectively, in accordance with the formulations shown in Table 2. The resulting mixtures were filtered through a glass fiber filter with a filtration accuracy of 0.3 μm to obtain the inkjet ink compositions of Examples 1-1 to 1-8.

[0085] <Preparation Procedure> (i) Preparation Procedure 1 A total of 350 g of all monomers (A) and (B) whose SP values ​​differ by 1 or more were weighed into a 1000 ml beaker and turbulently stirred at 25° C. for 3 hours at 1500 rpm using a disperser equipped with a disperser blade having a diameter of 1.4 inches. After stirring, the resulting mixture was filtered according to the above-mentioned filtration conditions. The remaining components constituting the inkjet ink composition were added to the filtrate after filtration, and the mixture was stirred and mixed until homogenous. Finally, the mixture was filtered again to remove foreign matter such as dust and impurities, thereby obtaining inkjet ink composition 1-1. (ii) Preparation Procedure 2 A total of 350 g of all components constituting the inkjet ink composition was weighed into a 1000 ml beaker and turbulently stirred at 1500 rpm using a disper equipped with a disper blade having a diameter of 1.4 inches at 25° C. for 3 hours. After stirring, the resulting mixture was filtered according to the filtration conditions described above to obtain inkjet ink composition 1-2. (iii) Preparation Procedure 3 A total of 350 g of all monomers (A) and (B) whose SP values ​​differ by 1 or more were weighed into a 1000 ml beaker and turbulently stirred at 25° C. for 6 hours at 1500 rpm using a disperser equipped with a 1.4 inch diameter disperser blade. After stirring, the resulting mixture was filtered according to the above-mentioned filtration conditions. The remaining components constituting the inkjet ink composition were added to the filtrate after filtration, and the mixture was stirred and mixed until homogenous. Finally, the mixture was filtered again to remove foreign matter such as dust and impurities, thereby obtaining inkjet ink composition 1-3. (iv) Preparation Procedure 4 A total of 350 g of all components constituting the inkjet ink composition was weighed into a 1000 ml beaker and turbulently stirred at 1500 rpm using a disperser equipped with a disperser blade having a diameter of 1.4 inches for 6 hours at 25° C. After stirring, the resulting mixture was filtered according to the filtration conditions described above to obtain inkjet ink composition 1-4. (v) Preparation Step 5 A total of 350 g of all monomers (A) and (B) whose SP values ​​differ by 1 or more were weighed into a 1000 ml beaker and turbulently stirred at 1500 rpm and 40° C. for 3 hours using a disperser equipped with a 1.4 inch diameter disperser blade. After stirring, the resulting mixture was filtered according to the above-mentioned filtration conditions. The remaining components constituting the inkjet ink composition were added to the filtrate after filtration, and the mixture was stirred and mixed until homogenous. Finally, the mixture was filtered again to remove foreign matter such as dust and impurities, thereby obtaining inkjet ink composition 1-5. (vi) Preparation Step 6 A total of 350 g of all components constituting the inkjet ink composition was weighed into a 1000 ml beaker and turbulently stirred at 1500 rpm using a disperser equipped with a disperser blade having a diameter of 1.4 inches at 40° C. for 3 hours. After stirring, the resulting mixture was filtered according to the filtration conditions described above to obtain inkjet ink composition 1-6. (vii) Preparation Procedure 7 A total of 350 g of all monomers (A) and (B) whose SP values ​​differ by 1 or more were weighed into a 1000 ml beaker and turbulently stirred at 1500 rpm and 10° C. for 3 hours using a disperser equipped with a 1.4 inch diameter disperser blade. After stirring, the resulting mixture was filtered according to the above-mentioned filtration conditions. The remaining components constituting the inkjet ink composition were added to the filtrate after filtration, and the mixture was stirred and mixed until homogenous. Finally, the mixture was filtered again to remove foreign matter such as dust and impurities, thereby obtaining inkjet ink composition 1-7. (viii) Preparation Procedure 8 A total of 350 g of all components constituting the inkjet ink composition, which have an SP value differing by 1 or more, were weighed out into a 1000 ml beaker and stirred at 1500 rpm using a disperser equipped with a disperser blade having a diameter of 1.4 inches at 10° C. for 3 hours. After stirring, the resulting mixture was filtered according to the filtration conditions described above to obtain inkjet ink composition 1-8.

[0086] (2) Examples 2 to 8 Inkjet ink compositions 2-1 to 8-8 were prepared according to the same preparation procedures 1 to 8 as in Example 1, except that the components and / or contents constituting the inkjet ink compositions were changed according to the compositions shown in Table 2. In addition, in preparation procedures 1, 3, 5, and 7, in Examples 7 and 8 including two types of monomers (A), the two types of monomers (A) each have a relationship in which the SP value differs by 1 or more in combination with at least one type of monomer (B), so all of the monomers (A) and (B) were mixed. In addition, in Example 6 including a monomer (B) (TPGDA) that does not have a relationship in which the SP value differs by 1 or more from the monomer (A), TPGDA was added together with the remaining components.

[0087] [Table 2]

[0088] (3) Comparative Example 1 The components constituting the inkjet ink compositions were mixed and stirred according to the formulations shown in Table 3, respectively, in the following preparation procedures 9 to 14. The resulting mixtures were filtered through a glass fiber filter with a filtration accuracy of 0.3 μm to obtain the inkjet ink compositions of Comparative Examples 1-9 to 1-14.

[0089] <Preparation Procedure> (i) Preparation procedure 9 A total of 350 g of monomer (A) and monomer (B) having an SP value that differs by 1 or more were weighed into a 1000 ml beaker, and turbulent stirring was performed for 1 hour at 25° C. at a rotation speed of 1500 rpm using a disperser equipped with a disperser blade having a diameter of 1.4 inches. After stirring, the resulting mixture was filtered according to the above-mentioned filtration conditions. The remaining components constituting the inkjet ink composition were added to the filtrate after filtration, and the mixture was stirred and mixed until homogenous. Finally, the mixture was filtered again to remove foreign matter such as dust and impurities, thereby obtaining inkjet ink composition 1-9. (ii) Preparation Procedure 10 A total of 350 g of all components constituting the inkjet ink composition was weighed into a 1000 ml beaker and turbulently stirred at 1500 rpm using a disperser equipped with a disperser blade having a diameter of 1.4 inches for 1 hour at 25° C. After stirring, the resulting mixture was filtered according to the filtration conditions described above to obtain inkjet ink composition 1-10. (iii) Preparation Procedure 11 A total of 350 g of monomer (A) and monomer (B) having an SP value that differs by 1 or more were weighed into a 1000 ml beaker, and turbulent stirring was performed for 3 hours at 50°C at a rotation speed of 1500 rpm using a disperser equipped with a disperser blade having a diameter of 1.4 inches. After stirring, the resulting mixture was filtered according to the above-mentioned filtration conditions. The remaining components constituting the inkjet ink composition were added to the filtrate after filtration, and the mixture was stirred and mixed until homogenous. Finally, the mixture was filtered again to remove foreign matter such as dust and impurities, thereby obtaining inkjet ink composition 1-11. (iv) Preparation Procedure 12 A total of 350 g of all components constituting the inkjet ink composition was weighed into a 1000 ml beaker and turbulently stirred at 1500 rpm using a disper equipped with a disper blade having a diameter of 1.4 inches at 50° C. for 3 hours. After stirring, the resulting mixture was filtered according to the filtration conditions described above to obtain inkjet ink composition 1-12. (v) Preparation Procedure 13 A total of 350 g of monomer (A) and monomer (B) having an SP value that differs by 1 or more were weighed into a 1000 ml beaker, and turbulent stirring was performed for 3 hours at 3° C. at a rotation speed of 1500 rpm using a disperser equipped with a disperser blade having a diameter of 1.4 inches. After stirring, the resulting mixture was filtered according to the above-mentioned filtration conditions. The remaining components constituting the inkjet ink composition were added to the filtrate after filtration, and the mixture was stirred and mixed until homogenous. Finally, the mixture was filtered again to remove foreign matter such as dust and impurities, thereby obtaining inkjet ink composition 1-13. (vi) Preparation Procedure 14 A total of 350 g of all components constituting the inkjet ink composition was weighed into a 1000 ml beaker and turbulently stirred at 1500 rpm using a disper equipped with a disper blade having a diameter of 1.4 inches at 3° C. for 3 hours. After stirring, the resulting mixture was filtered according to the filtration conditions described above to obtain inkjet ink composition 1-14.

[0090] (4) Comparative Examples 2 to 8 Inkjet ink compositions 2-9 to 8-14 were prepared according to preparation procedures 9 to 14 similar to those of Comparative Example 1, except that the components and / or contents constituting the inkjet ink compositions were changed according to the compositions shown in Table 3. Note that in preparation procedures 9, 11, and 13, in Comparative Examples 7 and 8 containing two types of monomers (A), the two types of monomers (A) each have a relationship in which the SP value differs by 1 or more in combination with at least one type of monomer (B), so all of the monomers (A) and (B) were mixed. In Comparative Example 6 containing a monomer (B) (TPGDA) that does not have a relationship in which the SP value differs by 1 or more from the monomer (A), TPGDA was added together with the remaining components.

[0091] [Table 3]

[0092] (5) Reference example 1 In accordance with each composition shown in Table 4, the components constituting the inkjet ink composition and / or their contents were changed, and Reference Inkjet Ink Compositions 1-1 to 1-8 were prepared according to Preparation Procedures 1 to 8 similar to those of Example 1. Note that in Preparation Procedures 1, 3, 5, and 7, stirring and filtration of the mixture of monomer (A) and monomer (B) were performed using only monomer (B).

[0093] (6) Reference example 2 Reference inkjet ink compositions 2-1 to 2-8 were prepared according to the same preparation procedures 1 to 8 as in Example 1, except that the components and / or contents constituting the inkjet ink composition were changed according to the compositions shown in Table 4.

[0094] [Table 4]

[0095] 2. Physical properties of ink-jet ink composition Measurement of T1 / T2 of Inkjet Ink Compositions The T1 / T2 values ​​of the ink-jet ink compositions prepared in the above Examples and Comparative Examples were measured according to the following method. 100 ml of the inkjet ink composition was placed in a glass bottle and stirred for 12 hours at 1500 rpm using a magnetic stirrer with a tapered stirrer (long diameter 50 mm, Φ7.5 mm). The inkjet ink composition after stirring was filtered at a filtration pressure of 0.8 MPa using a hydrophilic PTFE membrane filter (pore size 1 μm) manufactured by ADVANTEC Co., Ltd., and the time T1 for the first 20 ml of 100 ml to pass and the time T2 for the last 20 ml of 100 ml to pass were measured. The value of T1 / T2 was calculated from the measured T1 and T2. The value of T1 / T2 exceeding 0.7 was evaluated as A, the value of T1 / T2 between 0.5 and 0.7 was evaluated as B, and the value of T1 / T2 less than 0.5 was evaluated as C. The results are shown in Tables 2 to 4.

[0096] 3. Evaluation of Inkjet Ink Compositions (1) Discharge test (i) Immediately after preparation The inkjet ink compositions of Examples 1 to 8 prepared according to Preparation Procedures 1 to 8, the inkjet ink compositions of Comparative Examples 1 to 8 prepared according to Preparation Procedures 9 to 14, and the inkjet ink compositions of Reference Examples 1 and 2 prepared according to Preparation Procedures 1 and 2 were evaluated for IJ dischargeability of the ink compositions immediately after preparation using an inkjet recording device equipped with a piezoelectric inkjet nozzle. This inkjet recording device is equipped with an ink supply system including an ink tank, a supply pipe, an anterior ink tank immediately before the head, and a piezoelectric head. In addition, a filter (PP capsule, pore size 8 μm) for removing dust from the ink is provided between the ink tank and the anterior ink tank immediately before the head. Furthermore, when discharging the ink, the ink was heated by a temperature control system in the inkjet recording device so that the ink viscosity at the head was 8 to 25 mPa·s, which is an appropriate discharge viscosity. In addition, the inkjet recording device was driven at a drive frequency of 10 kHz so that the ink could be discharged with a droplet size of about 7 pl and a resolution of 600×600 dpi. At that time, the IJ dischargeability of the ink was evaluated according to the following criteria. All the inkjet ink compositions had a viscosity suitable for ejection from the inkjet nozzle of the inkjet recording device used in the ejection test. [Ejection performance evaluation criteria] A: 30L discharge was possible. B: Unable to excrete within 30L

[0097] (ii) After 180 days of storage The inkjet ink compositions of Examples 1 to 8 prepared according to Preparation Procedures 1 to 8, the inkjet ink compositions of Comparative Examples 1 to 8 prepared according to Preparation Procedures 9 to 14, and the inkjet ink compositions of Reference Examples 1 and 2 prepared according to Preparation Procedures 1 and 2 were each stored at 25°C for 180 days, and then the IJ ejection properties of the ink compositions were evaluated in the same manner as in procedure (i) above.

[0098] For all of the inkjet ink compositions of Examples 1 to 8 prepared according to Preparation Procedures 1 to 8, the ejection properties immediately after preparation and after 180 days of storage were both rated as "A". In contrast, for the inkjet ink compositions of Comparative Examples 1 to 8 prepared according to Preparation Procedures 9 to 14, the ejection properties immediately after preparation and after 180 days of storage were both rated as "B". Note that in Reference Example 1, which does not contain monomer (A), and Reference Example 2, in which the amount of monomer (A) is greater than the amount of monomer (B), it is believed that homopolymers of monomer (A) are not generated at a level that would cause filter clogging, and the ejection properties were all rated as "A".

Claims

1. An active energy ray-curable inkjet ink composition comprising at least two ethylenically unsaturated monomers and at least one photopolymerization initiator, the ethylenically unsaturated monomer comprises an ethylenically unsaturated monomer (A) having an SP value of 10 or more and an ethylenically unsaturated monomer (B) having an SP value of less than 10; Among the ethylenically unsaturated monomers contained in the composition, the difference between the SP value of the ethylenically unsaturated monomer (A) having the highest SP value and the SP value of the ethylenically unsaturated monomer (B) having the lowest SP value is 1 or more; The content of the ethylenically unsaturated monomer (A) is less than the content of the ethylenically unsaturated monomer (B), The ink-jet ink composition, wherein when 100 ml of the ink-jet ink composition is stirred at 1,500 rpm for 12 hours using a stirrer having a major axis of 30 mm or more, and then filtered using a hydrophilic PTFE membrane filter having a pore size of 1 μm at a filtration pressure of 0.8 MPa, the ratio of the time T1 for the first 20 ml of the 100 ml to the time T2 for the last 20 ml of the 100 ml to pass is 0.5 or more.

2. The ink-jet ink composition of claim 1 , wherein the ethylenically unsaturated monomer (A) comprises a nitrogen atom-containing ethylenically unsaturated monomer.

3. The ink-jet ink composition of claim 1 , wherein the ethylenically unsaturated monomer (A) comprises a (meth)acrylamide.

4. 2. The ink-jet ink composition according to claim 1, wherein a mass ratio of a content of the ethylenically unsaturated monomer (A) to a content of the ethylenically unsaturated monomer (B) (ethylenically unsaturated monomer (A) / ethylenically unsaturated monomer (B)) is 0.03 to 0.

9.

5. 2. The ink-jet ink composition according to claim 1, wherein a total content of ethylenically unsaturated monomers having an SP value that is less than 1 different from the SP value of the ethylenically unsaturated monomer (A) having the highest SP value is less than the content of the ethylenically unsaturated monomer (A) having the highest SP value.

6. Based on the total weight of the inkjet ink composition, 1 to 49% by weight of an ethylenically unsaturated monomer (A), 5 to 90% by weight of an ethylenically unsaturated monomer (B), and 0.1 to 15% by mass of a photopolymerization initiator The ink-jet ink composition of claim 1 , comprising:

7. The ink-jet ink composition according to claim 1 , which is a clear ink composition having a colorant content of 0.1% by mass or less based on the total mass of the ink composition.

8. The ink-jet ink composition of claim 1 , which is a modeling material composition for use in material jet stereolithography.

9. A method for producing an active energy ray-curable ink-jet ink composition comprising a photopolymerization initiator, and an ethylenically unsaturated monomer (A) having an SP value of 10 or more and an ethylenically unsaturated monomer (B) having an SP value less than 10, the SP values ​​of which differ from each other by 1 or more, the content of the ethylenically unsaturated monomer (A) being lower than the content of the ethylenically unsaturated monomer (B), A step of agglomerating the homopolymer of the ethylenically unsaturated monomer (A); and A step of removing the homopolymer aggregates obtained in the previous step. A method comprising:

10. The method according to claim 9, wherein the step of agglomerating the homopolymer is carried out by stirring the ethylenically unsaturated monomer (A) and the ethylenically unsaturated monomer (B) for 3 hours or more.

11. The method according to claim 9 , wherein the step of aggregating the homopolymer is carried out by stirring all of the components constituting the ink-jet ink composition for 3 hours or more.

12. 10. The method of claim 9, wherein the step of agglomerating the homopolymer is carried out at 5 to 45°C.

13. The method of claim 9 , wherein the step of removing the aggregates is carried out by filtration.

14. 14. The method of claim 13, wherein the filtration uses a glass fiber filter.

15. The method according to claim 13, wherein the filter has a filtering accuracy of 0.8 μm or less.

Citation Information

Patent Citations

  • Activated energy beam-curable ink-jetting ink

    JP2002241647A

  • Active energy ray-curable ink composition and method for creating printed matter

    JP2012001587A

  • Active energy ray-curable inkjet ink composition

    JP2013245240A

  • Radiation-curable red color gel ink compound

    JP2014091829A

  • Active energy ray-curable inkjet ink composition

    JP2014210918A

Cited By