Method for producing nickel powder
By controlling atmospheric exposure time and water temperature during nickel powder production, the method suppresses the formation of nickel hydroxide coarse particles, enhancing the quality of nickel powder for multilayer ceramic capacitors.
Patent Information
- Application Number
- JP2023058856
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-31
AI Technical Summary
The production of nickel powder using wet methods results in the formation of coarse particles composed of nickel hydroxide due to oxidation during washing and filtration processes, especially in high-temperature environments, which can lead to malfunctions in multilayer ceramic capacitors.
Control the atmospheric exposure time of the nickel powder cake during washing and filtration to within a specified range (10 minutes or less) and maintain the temperature of pure water between 25°C to 45°C to suppress the generation of coarse particles, primarily composed of nickel hydroxide, by minimizing oxidation.
The method effectively reduces the content of coarse particles in nickel powder, ensuring high flatness and suitability for use as internal electrodes in multilayer ceramic capacitors, even in high-temperature environments.
Smart Images

Figure 2024146129000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing high-performance nickel powder used as an electrode material for multilayer ceramic parts, and more particularly to a method for producing inexpensive, high-performance nickel powder obtained by a wet method. [Background technology]
[0002] Nickel powder is used as a material for capacitors in electronic circuits, in particular as a material for thick-film conductors that form internal electrodes of multilayer ceramic components such as multilayer ceramic capacitors (MLCCs) and multilayer ceramic substrates.
[0003] In recent years, the capacity of multilayer ceramic capacitors has increased, and the amount of internal electrode paste used to form the internal electrodes of multilayer ceramic capacitors has also increased significantly. For this reason, inexpensive base metals such as nickel are mainly used as metal powders for the internal electrode paste that constitutes the thick-film conductor, instead of expensive precious metals.
[0004] In the process of manufacturing a multilayer ceramic capacitor, an internal electrode paste made by kneading nickel powder, a binder resin such as ethyl cellulose, and an organic solvent such as terpineol is screen-printed on a dielectric green sheet. The dielectric green sheet on which the internal electrode paste has been printed and dried is then laminated so that the internal electrode paste printed layers and the dielectric green sheet are alternately overlapped, and further compressed to obtain a laminate.
[0005] This laminate is cut to a specified size, then the binder resin is removed by heat treatment (binder removal treatment), and the laminate after binder removal treatment is fired at a high temperature of about 1300°C to obtain a ceramic molded body.
[0006] Then, external electrodes are attached to the obtained ceramic compact to obtain a multilayer ceramic capacitor. Since base metals such as nickel are used as the metal powder in the internal electrode paste that becomes the internal electrodes, the binder removal process of the laminate is carried out in an atmosphere with an extremely low oxygen concentration, such as an inert atmosphere, so as to prevent the oxidation of these base metals.
[0007] As multilayer ceramic capacitors become smaller and their capacitance increases, the internal electrodes and dielectrics are both becoming thinner. Accordingly, the particle size of the nickel powder used in the internal electrode paste is also becoming finer, and nickel powder with an average particle size of 0.3 μm or less is required, with the use of nickel powder with an average particle size of 0.2 μm or less becoming mainstream.
[0008] Nickel powder manufacturing methods are roughly divided into gas phase methods and wet methods. Gas phase methods include, for example, a method described in Patent Document 1 in which nickel chloride vapor is reduced with hydrogen to produce nickel powder, and a method described in Patent Document 2 in which nickel metal is vaporized in plasma to produce nickel powder. In addition, wet methods include, for example, a method described in Patent Document 3 in which a reducing agent is added to a nickel salt solution to produce nickel powder.
[0009] The gas phase method is an effective means of obtaining nickel powder with excellent crystallinity and high properties because it is a high-temperature process of about 1000°C or more, but the particle size distribution of the obtained nickel powder is broad. As mentioned above, nickel powder with a relatively narrow particle size distribution and an average particle size of 0.3 μm or less that does not contain coarse particles is required for thinning of internal electrodes. Therefore, in order to obtain such nickel powder by the gas phase method, it is necessary to classify the nickel powder by introducing expensive classification equipment.
[0010] In the classification process, it is possible to remove coarse particles larger than the classification point, which has a particle size of about 0.6 μm to 2 μm, but since some of the particles smaller than the classification point are also removed at the same time, there is a problem that the actual product yield is significantly reduced. Therefore, in the gas phase method, an increase in product costs is unavoidable, including the introduction of the above-mentioned expensive equipment.
[0011] Furthermore, with the gas phase method, when nickel powder with an average particle size of 0.2 μm or less is used, especially when nickel powder with an average particle size of 0.1 μm or less is used, it becomes difficult to remove coarse particles by classification processing, making it impossible to accommodate future efforts to make internal electrodes even thinner.
[0012] On the other hand, the wet method has an advantage over the gas phase method in that the particle size distribution of the resulting nickel powder is narrow. In particular, in the method described in Patent Document 3, in which a solution containing hydrazine as a reducing agent is added to a solution containing a copper salt as a nickel salt, a reduction reaction is carried out in the resulting reaction solution, and the nickel salt (more precisely, nickel ions (Ni 2+ ), or nickel complex ions) are reduced with hydrazine, so that the number of nuclei generated is controlled (i.e., the particle size is controlled), and nuclei generation and particle growth become uniform, resulting in the production of fine nickel powder with a narrower particle size distribution (hereinafter, the "nickel powder generated in the reaction solution" may be referred to as "nickel crystallized powder").
[0013] Incidentally, when the nickel powder obtained by the above-mentioned wet method is applied to a multilayer ceramic capacitor, in order to prevent short circuits between electrodes in the laminate consisting of the internal electrode layer and the dielectric layer, a high flatness is required for the nickel paste dry film (dried film obtained by printing and drying the nickel paste) mainly composed of nickel powder and resin. In particular, in order to respond to the thinning of the internal electrode layer (film thickness of about 0.5 μm to 1.0 μm) accompanying the high capacity of the multilayer ceramic capacitor in recent years, fine nickel powder with an average particle size of 0.3 μm or less, preferably an average particle size of 0.2 μm or less is used, and it is required to reduce coarse particles of the same size as the film thickness of the internal electrode layer contained in the nickel powder (for example, 0.4 μm to 0.8 μm) to the utmost limit.
[0014] Therefore, Patent Document 4 discloses a method for producing nickel powder using a wet method, in which a crystallization process is carried out in a strongly alkaline reaction solution to increase the reducing power of hydrazine, and in this process, a very small amount of a specific amine compound or sulfide compound is added to the reaction solution to significantly suppress the self-decomposition reaction of hydrazine and make it difficult for nickel particles to bond together to form coarse particles, thereby inexpensively obtaining high-performance nickel powder with an extremely low content of coarse particles. [Prior art documents] [Patent documents]
[0015] [Patent Document 1] Japanese Patent Application Publication No. 4-365806 [Patent Document 2] Special Publication No. 2002-530521 [Patent Document 3] JP 2002-53904 A [Patent Document 4] WO2017 / 069067 issue Summary of the Invention [Problem to be solved by the invention]
[0016] In the above-mentioned wet method for producing nickel powder, hydrazine is often used as a reducing agent, and therefore the reaction solution generally becomes strongly alkaline, as is clear from Patent Document 4 and the like. In the crystallization step shown in Fig. 1 (a schematic diagram showing a typical manufacturing process in a wet method for producing nickel powder), a nickel powder slurry is obtained in which nickel crystallized powder is generated in the strongly alkaline reaction solution by the reduction reaction of hydrazine, and the nickel crystallized powder is filtered and recovered from the nickel powder slurry while being washed with pure water to obtain a nickel powder cake, and a drying step is performed after the crystallization step, in which the nickel powder cake is dried (vacuum drying, etc.) to obtain a dried nickel crystallized powder (nickel powder).
[0017] The above washing and filtering process is usually carried out in the air, so the nickel powder cake obtained is exposed to the air to some extent during the washing and filtering process and before drying in the drying process, and it is inevitable that the nickel crystallized powder will be oxidized. In particular, when producing nickel powder by performing a crystallization reaction on a mass production scale, unlike handling a small amount at the laboratory level, it takes time to handle the nickel powder cake, so the nickel crystallized powder is likely to be oxidized due to exposure to the air in the state of the nickel powder cake. In addition, the higher the temperature, the more likely the nickel crystallized powder is to be oxidized, and oxidation tends to progress further in the hot summer months than in the cold winter months, and temperature changes in the manufacturing environment due to seasonal fluctuations are also one of the reasons for the oxidation of nickel crystallized powder.
[0018] In the nickel powder cake obtained from the strongly alkaline nickel powder slurry through the washing and filtration processes, when oxidation of the nickel crystallized powder occurs, coarse particles 10 (see FIG. 2) mainly composed of nickel hydroxide, which is formed by strongly binding nickel crystallized powder 1 (particle size 0.2 μm or less) with nickel hydroxide 2 generated by oxidation, may be generated. In many cases, these coarse particles 10 have a particle size of 0.4 μm or more and can cause defects in multilayer ceramic capacitors, etc., so effective measures to suppress this have been required.
[0019] Therefore, the present invention aims to provide a method for producing nickel powder that has a low content of coarse particles mainly composed of nickel hydroxide even in the summer when the temperature of the production environment is high, and in particular, to provide a method for producing nickel powder by a wet method that can produce the nickel powder more simply and easily. [Means for solving the problem]
[0020] The present inventors have found that in a wet method for producing nickel powder used in multilayer ceramic capacitors, etc., the generation of coarse particles mainly composed of nickel hydroxide can be effectively suppressed by controlling within a predetermined range the temperature of the pure water used to wash the nickel powder cake in the washing and filtration process in which the nickel crystallized powder (nickel powder) is washed and filtered from the strongly alkaline nickel powder slurry, which is the end solution of the reaction after crystallization, and recovered as a nickel powder cake, and the time during which the nickel powder cake is exposed to the air from the time of filtration until the drying of the nickel powder cake is started in the drying process (air exposure time).The present invention was completed based on such findings.
[0021] In order to solve the above problems, the method for producing nickel powder of the present invention includes a washing and filtration step of washing and filtering the nickel crystallized powder in a nickel powder slurry containing nickel crystallized powder obtained by crystallizing the water-soluble nickel salt through a reduction reaction with the reducing agent in a reaction liquid containing a water-soluble nickel salt, a metal salt of a metal nobler than nickel, a reducing agent, an alkali hydroxide, and water, using pure water at 25°C to 45°C to obtain a nickel powder cake, and a drying step of drying the nickel powder cake to obtain nickel powder, wherein the exposure time of the nickel powder cake to the atmosphere between the time of filtration in the washing and filtration step and the start of drying in the drying step is kept to 10 minutes or less.
[0022] In the method for producing nickel powder of the present invention, the moisture content of the nickel powder cake may be 5% by mass or more and 70% by mass or less.
[0023] The method for producing nickel powder of the present invention may include a crystallization step of crystallizing the nickel crystallized powder from the water-soluble nickel salt by a reduction reaction with the reducing agent in a reaction liquid containing a water-soluble nickel salt, a metal salt of a metal more noble than nickel, a reducing agent, an alkali hydroxide, and water. Effect of the Invention
[0024] The present invention can provide a method for producing nickel powder that has a low content of coarse particles mainly composed of nickel hydroxide, even in the summer when the temperature of the production environment is high, and in particular, a method for producing nickel powder by a wet method that can produce the nickel powder more simply and easily. [Brief description of the drawings]
[0025] [Figure 1] FIG. 1 is a schematic diagram showing typical manufacturing steps in a method for manufacturing nickel powder by a wet method. [Diagram 2] FIG. 2 is a schematic diagram showing coarse particles mainly composed of nickel hydroxide found in nickel powder produced by a wet method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] Hereinafter, a method for producing nickel powder according to the present embodiment will be described. The present embodiment is not limited to the above, and can be arbitrarily modified without departing from the gist of the present embodiment.
[0027] 1. Nickel powder 2. Nickel powder manufacturing method using wet method 2-1.Crystallization process 2-1-1. Chemicals used in the crystallization process 2-1-2. Crystallization procedure 2-1-3. Reduction reaction 2-1-4.Reaction start temperature 2-2. Washing and filtration process 2-2-1. Methods and procedures for cleaning and filtering 2-3.Drying process 2-4. Crushing process (post-processing process)
[0028] <1. Nickel powder> The nickel powder obtained by the manufacturing method of the present invention has an extremely low content of coarse particles mainly composed of nickel hydroxide having a particle size exceeding 0.4 μm, and can achieve high flatness in a dried nickel paste film. This makes it possible to effectively prevent short circuits between electrodes in a laminate consisting of an internal electrode layer and a dielectric layer, and is suitable for use as an internal electrode in a multilayer ceramic capacitor.
[0029] The nickel powder has a roughly spherical particle shape, and its average particle size is 0.03 μm to 0.15 μm from the viewpoint of responding to the recent trend of thinning of the internal electrodes of multilayer ceramic capacitors. The roughly spherical shape includes not only a true sphere, but also an ellipsoid whose cross section has an elliptical shape with a ratio of the minor axis to the major axis (minor axis / major axis) of 0.8 to less than 1.0.
[0030] The average particle size in this embodiment is the number-average particle size determined from a scanning electron microscope (SEM) image of the nickel powder. Nickel powder produced by the wet method of this embodiment described later has a sufficiently narrow particle size distribution without classification. In other words, in this case, the CV value (number), which is the standard deviation of the particle size divided by the number-average particle size, is 0.2 or less, resulting in nickel powder with a uniform particle size.
[0031] Here, the coarse particles mainly composed of nickel hydroxide are solids that are tightly bound to the nickel crystallized powder by nickel hydroxide generated on the surface of the nickel crystallized powder during the process from the washing and filtering process to the drying process described later. These are not easily disintegrated even if the crushing process described later is performed. The coarse particles mainly composed of nickel hydroxide can be identified by separating the coarse particles from the crushed nickel powder using a filter such as a membrane filter, and analyzing the coarse particles using EDS (energy dispersive X-ray analysis) or XPS (X-ray photoelectron spectroscopy) and observing the shape using a scanning electron microscope (SEM).
[0032] According to the method for producing nickel powder of the present invention, the content of coarse particles mainly composed of nickel hydroxide and having a particle size exceeding 0.4 μm in the nickel powder can be reduced to 4000 ppm by mass or less.
[0033] Of course, the effect of coarse particles depends on the film thickness of the internal electrode layer of the multilayer ceramic capacitor in which nickel powder is used, but in recent thin internal electrode layers, if the content of coarse particles mainly composed of nickel hydroxide with a particle size exceeding 0.4 μm exceeds 4000 mass ppm, the occurrence of short circuits between electrodes may become significant. It goes without saying that the lower the content of coarse particles mainly composed of nickel hydroxide, the better, and if the content of coarse particles mainly composed of nickel hydroxide with a particle size exceeding 0.4 μm is 4000 mass ppm or less, the occurrence rate of short circuits between electrodes can be sufficiently reduced. The particle size of the coarse particles mainly composed of nickel hydroxide may be the minor axis diameter determined from the SEM image.
[0034] Usually, nickel powder may contain a small amount of impurities. For example, nickel powder obtained by a wet method may contain a small amount of oxygen caused by the surface oxidation of nickel particles, chlorine thought to be caused by nickel chloride, which is a nickel raw material, and alkali metals such as sodium caused by sodium hydroxide. Nickel powder obtained by a gas phase method may also contain oxygen caused by the surface oxidation of nickel particles, and a small amount of chlorine in the case of nickel powder obtained by a method of reducing nickel chloride vapor with hydrogen. These impurities may cause defects in the internal electrodes during the manufacture of a multilayer ceramic capacitor, so it is preferable to reduce them as much as possible. For example, it is preferable that the content of chlorine and alkali metals in the nickel powder is 0.01 mass% or less.
[0035] Nickel powder applicable to the internal electrodes of multilayer ceramic capacitors, such as the nickel powder of this embodiment, may usually contain a small amount of sulfur to suppress its catalytic activity. This is because the surface of nickel particles has high catalytic activity, and if it is used as is without sulfur, for example, it will promote thermal decomposition of binder resin such as ethyl cellulose resin contained in the internal electrode paste during binder removal treatment during the manufacture of multilayer ceramic capacitors, causing the binder resin to decompose at low temperatures, significantly reducing the strength of the laminate, and at the same time, a large amount of decomposition gas will be generated, making the laminate more likely to crack.
[0036] In order to make the nickel powder contain sulfur as described above, it is most preferable to carry out a surface treatment to attach sulfur to the surface of the nickel particles, and to thinly and uniformly modify (coat) the entire surface of the nickel particles with sulfur, from the viewpoint of manifesting the effect of inhibiting the decomposition of the binder resin and reducing the influence of sulfur as an impurity on the characteristics of the multilayer ceramic capacitor. However, as long as the effect of inhibiting the decomposition of the binder resin can be exhibited, it is also possible to modify (coat) the entire surface of the nickel particles, and to modify (coat) only a part of the surface. In this embodiment, the term "surface treatment" is used as a concept that includes such modification (coating) of the entire nickel particles and modification (coating) of a part of the nickel particles. In addition, in the manufacturing method of nickel powder using the wet method of this embodiment, since the final reaction solution after the crystallization reaction in the crystallization step contains an excess amount of alkali hydroxide and exhibits strong alkalinity, even if the pH of the final reaction solution may be slightly lowered by the surface treatment with sulfur as described above, the pH of the final reaction solution, that is, the nickel powder slurry or its dilution solution, will not be 7.0 to pH 9.0, and this surface treatment does not correspond to neutralization as defined in this embodiment.
[0037] If the sulfur content of the nickel powder exceeds 0.5% by mass, internal electrode defects due to sulfur may occur, and therefore the sulfur content is preferably 0.3% by mass or less, and more preferably 0.2% by mass or less. The lower limit of the sulfur content is not particularly limited, and may be an extremely small content that is below the detection limit of an analytical instrument used for content analysis, such as a sulfur analyzer using a combustion method or an ICP analyzer.
[0038] The moisture content derived from nickel hydroxide in the nickel powder is considered to be in a positive correlation with the amount of nickel hydroxide in the nickel powder, and therefore it is considered to be a guideline for measuring the amount of coarse particles mainly composed of nickel hydroxide. That is, from the viewpoint of reducing the amount of nickel hydroxide in the nickel powder, it is ideal that the moisture content derived from nickel hydroxide in the nickel powder is as low as possible, and specifically, as a guideline for suppressing the generation of coarse particles, the moisture content derived from nickel hydroxide in the nickel powder is preferably 0.5% or less, more preferably 0.4% or less. The lower limit of the moisture content derived from nickel hydroxide in the nickel powder is ideally 0%, but in reality, the measurement limit value is the lower limit. The moisture content derived from nickel hydroxide in the nickel powder can be obtained, for example, using a Karl Fischer moisture meter.
[0039] <2. Manufacturing method of nickel powder using wet method> Next, a method for producing nickel powder using a wet method according to one embodiment of the present invention will be described. The method for producing nickel powder using a wet method according to one embodiment of the present invention includes a crystallization step in which nickel is crystallized by a reduction reaction using hydrazine or the like in a strongly alkaline reaction solution obtained by mixing at least a water-soluble nickel salt, a salt of a metal nobler than nickel, a reducing agent (e.g., hydrazine), an alkali hydroxide as a pH adjuster, and water to obtain a strongly alkaline nickel powder slurry, which is a reaction end solution containing nickel crystallized powder, a washing and filtering step in which the nickel powder slurry is washed while separating the nickel crystallized powder to obtain a nickel powder cake, and a drying step in which the nickel powder cake is dried to obtain nickel crystallized powder (nickel powder). In addition, an amine compound or a sulfur-containing compound may be blended into the reaction solution as necessary to act as a hydrazine self-decomposition inhibitor (amine compound, sulfur-containing compound) and a reduction reaction accelerator (complexing agent) (amine compound). In addition, a crushing step may be added as a post-treatment step as necessary.
[0040] If desired, a very small amount of sulfur compound may be added to the strongly alkaline nickel powder slurry, which is the reaction end solution containing the nickel crystallized powder, or to the dilution or washing solution thereof, so that the content in the nickel powder is 0.5 mass% or less, and a surface treatment (sulfur coating treatment) may be performed to modify the surface of the nickel particles with the sulfur component. Nickel powder can also be obtained by subjecting the obtained nickel powder to a heat treatment at about 200°C to 300°C in an inert atmosphere or reducing atmosphere. This sulfur coating treatment or heat treatment is very effective if used within an appropriate range, because it can control the binder removal behavior and sintering behavior of the nickel powder in the internal electrodes during the above-mentioned production of the multilayer ceramic capacitor.
[0041] Furthermore, if necessary, it is preferable to add a crushing process (post-processing process) in which the nickel crystallized powder is subjected to a crushing treatment, thereby obtaining nickel powder in which the coarse particles caused by the joining of nickel particles during the nickel particle production process in the crystallization process has been reduced.
[0042] By carrying out such a crystallization step, washing / filtration step, drying step, and optionally a crushing step, nickel powder having a substantially spherical particle shape and an average particle size of 0.03 μm to 0.15 μm can be obtained.
[0043] (2-1.Crystallization process) In the crystallization step, nickel salt (more precisely, nickel ion or nickel complex ion) can be reduced by a reduction reaction using a reducing agent such as hydrazine in a reaction solution containing at least a water-soluble nickel salt, a salt of a metal nobler than nickel, a reducing agent, an alkali hydroxide, and water. In this embodiment, when hydrazine is used, an amine compound or a sulfur-containing compound can be mixed into this reaction solution as necessary, and the nickel salt can be reduced in the presence of the amine compound or the sulfur-containing compound while suppressing the decomposition of hydrazine as a reducing agent. The crystallization step is not an essential step, and the crystallization step may be performed as one step of the method for producing nickel powder of the present invention. In addition, a nickel powder slurry containing nickel crystallized powder obtained by the crystallization step (e.g., a reaction end liquid) may be obtained by purchase or the like, and the nickel crystallized powder in the nickel powder slurry containing nickel crystallized powder may be subjected to a washing and filtration step described later.
[0044] (2-1-1. Chemicals used in the crystallization process) In the crystallization step of this embodiment, a reaction liquid containing various chemicals such as nickel salt, salt of a metal nobler than nickel, a reducing agent, an alkali hydroxide, and, as necessary, an amine compound or a sulfur-containing compound, and water is used. From the viewpoint of reducing the amount of impurities in the obtained nickel powder, the water used as the solvent is preferably high-purity water such as ultrapure water (electrical conductivity: ≦0.06 μS / cm (microsiemens per centimeter)) or pure water (electrical conductivity: ≦1 μS / cm), and among these, it is preferable to use pure water, which is inexpensive and easily available. Each of the above-mentioned various chemicals will be described in detail below.
[0045] (a) Nickel salts The nickel salt used in this embodiment is not particularly limited as long as it is a nickel salt that is easily soluble in water, and for example, one or more selected from nickel chloride, nickel sulfate, and nickel nitrate can be used. Among these nickel salts, it is more preferable to use nickel chloride, nickel sulfate, or a mixture thereof.
[0046] (b) Salts of metals more noble than nickel Salts of metals more noble than nickel have a lower ionization tendency than nickel, and are therefore reduced before nickel when nickel is reduced and precipitated. Therefore, when a salt of a metal more noble than nickel is contained in a nickel salt solution, the salt acts as a nucleating agent that reduces the metal more noble than nickel first and becomes an initial nucleus when nickel is reduced and precipitated. Therefore, in the nickel crystallized powder (nickel powder) obtained by particle growth of the initial nuclei, it becomes easy to control the particle size of the nickel powder and make it finer.
[0047] The salt of a metal more noble than nickel may be any metal salt that is water-soluble and has a lower ionization tendency than nickel, and examples of the salt include water-soluble copper salts, gold salts, silver salts, platinum salts, palladium salts, rhodium salts, iridium salts, etc. For example, the water-soluble copper salt may be copper sulfate, the water-soluble silver salt may be silver nitrate, and the water-soluble palladium salt may be sodium palladium(II) chloride, ammonium palladium(II) chloride, palladium(II) nitrate, palladium(II) sulfate, etc., but are not limited thereto.
[0048] As the salt of a metal more noble than nickel, it is preferable to use the above-mentioned palladium salt, since although the particle size distribution becomes somewhat broad, it is possible to more finely control the particle size of the resulting nickel powder. When a palladium salt is used, the ratio of palladium salt to nickel [mol ppm] (moles of palladium salt / moles of nickel × 10 6) can be appropriately selected depending on the desired number average particle size of the nickel powder. For example, if the average particle size of the nickel powder is set to 0.15 μm or less, the ratio of palladium salt to nickel is set within the range of 3 mol ppm to 250 mol ppm, preferably within the range of 5 mol ppm to 200 mol ppm. If the ratio is less than 3 mol ppm, the average particle size of the resulting nickel powder may exceed 0.15 μm. On the other hand, if the ratio exceeds 250 mol ppm, a large amount of expensive palladium salt will be used, which may lead to an increase in the cost of the nickel powder.
[0049] (c) Reducing agent The reducing agent used in the crystallization step of this embodiment is not particularly limited, but may be, for example, hydrazine (N2H4, molecular weight: 32.05). In addition to anhydrous hydrazine, hydrazine hydrate (N2H4·H2O, molecular weight: 50.06) may be used as hydrazine. Either may be used. The reduction reaction of hydrazine is as shown in the formula (2) described later, and has the following characteristics: it is particularly alkaline and has high reducing power; the by-products of the reduction reaction are nitrogen gas and water, so that impurity components due to the reduction reaction are not generated in the reaction solution; the amount of impurities in hydrazine is small to begin with; and it is easily available. Therefore, hydrazine is suitable as a reducing agent, and for example, commercially available industrial grade 60% by mass hydrazine hydrate can be used.
[0050] (d) Alkali hydroxide As shown in formula (2) described later, the reducing power of hydrazine increases as the alkalinity of the reaction solution increases. Therefore, in this embodiment, an alkali hydroxide can be used as a pH adjuster to increase the alkalinity in the crystallization step. The alkali hydroxide is not particularly limited, but it is preferable to use an alkali metal hydroxide in terms of availability and cost. Specifically, it is more preferable to use one or more selected from sodium hydroxide (NaOH) and potassium hydroxide (KOH).
[0051] The amount of alkali hydroxide to be added should be determined so that the pH of the reaction solution at the reaction temperature is 9.5 or more, preferably 10 or more, and more preferably 10.5 or more, so that the reducing power of hydrazine as a reducing agent is sufficiently increased. For example, when comparing the pH of the reaction solution at 25°C and around 70°C, the pH at the higher temperature of 70°C is somewhat lower.
[0052] (e) Amine compounds As described above, the amine compound acts as an inhibitor of self-decomposition of hydrazine, an accelerator of reduction reaction, and an inhibitor of bonding between nickel particles, and may be added to the reaction solution as necessary. The amine compound is a compound containing a total of two or more functional groups selected from primary amino groups (-NH2) or secondary amino groups (-NH-) in the molecule, and at least one of alkyleneamines or alkyleneamine derivatives can be used. As an example, it is preferable to use an amine compound having at least the structure of the following formula A in which the nitrogen atom of the amino group in the molecule is bonded via a carbon chain having two carbon atoms.
[0053] [ka]
[0054] More specifically, the alkyleneamine may be one or more selected from ethylenediamine (H2NC2H4NH2), diethylenetriamine (H2NC2H4NHC2H4NH2), triethylenetetramine (H2N(C2H4NH)2C2H4NH2), tetraethylenepentamine (H2N(C2H4NH)3C2H4NH2), pentaethylenehexamine (H2N(C2H4NH)4C2H4NH2), and propylenediamine (CH3CH(NH2)CH2NH2). In addition, alkyleneamine derivatives include tris(2-aminoethyl)amine (N(C2H4NH2)3), N-(2-aminoethyl)ethanolamine (H2NC2H4NHC2H4OH), N-(2-aminoethyl)propanolamine (H2NC2H4NHC3H6OH), 2,3-diaminopropionic acid (H2NCH2CH(NH)COOH), 1,2-cyclohexanediamine (H2NC6H 10 NH2), ethylenediamine-N,N'-diacetic acid (also known as ethylene-N,N'-diglycine, HOOCCH2NHC2H4NHCH2COOH), N,N'-diacetylethylenediamine (CH3CONHC2H4NHCOCH3), N,N'-dimethylethylenediamine (CH3NHC2H4NHCH3), N,N'-diethylethylenediamine (C2H5NHC2H4NHC2H5), N,N'-diisopropylethylenediamine (CH3(CH3)CHNHC2H4NHCH(CH3)CH3), 1,2-cyclohexanediamine (H2NC6H 10 These alkyleneamines and alkyleneamine derivatives are water-soluble, and among them, ethylenediamine and diethylenetriamine are preferred because they are easily available and inexpensive.
[0055] The above amine compound acts as a reduction reaction accelerator by absorbing nickel ions (Ni 2+It is believed that this is due to its function as a complexing agent that complexes hydrazine with amine compound ions to form nickel complex ions. As for its function as an inhibitor of the self-decomposition of hydrazine and an inhibitor of the bonding between nickel particles, it is presumed that this is due to the interaction between the primary amino group (-NH2) and secondary amino group (-NH-) in the amine compound molecule and the surface of the nickel crystallized powder in the reaction solution.
[0056] In addition, it is preferable that the alkyleneamine or alkyleneamine derivative, which is an amine compound, has the structure of the above formula A in which the nitrogen atom of the amino group in the molecule is bonded via a carbon chain with two carbon atoms. This is because the effect of suppressing the decomposition of hydrazine molecules is increased. For example, if the nitrogen atom of the amino group that strongly adsorbs to nickel crystallized powder is bonded via a carbon chain with three or more carbon atoms, it is considered that the carbon chain becomes longer and the degree of freedom of movement (molecular flexibility) of the carbon chain part of the amine compound molecule increases. As a result, it is considered that the contact of hydrazine molecules with nickel crystallized powder cannot be effectively hindered, and the number of hydrazine molecules that self-decompose due to the catalytic activity of nickel increases, thereby reducing the effect of suppressing the self-decomposition of hydrazine.
[0057] In fact, it has been confirmed that trimethylenediamine (also known as 1,3-diaminopropane, 1,3-propanediamine) (H2NC3H6NH2), in which the nitrogen atoms of the amino groups in the molecule are bonded via a carbon chain with three carbon atoms, is inferior in its ability to inhibit the self-decomposition of hydrazine, compared to ethynediamine (H2NC2H4NH2) and propylenediamine (also known as 1,2-diaminopropane, 1,2-propanediamine) (CH3CH(NH2)CH2NH2).
[0058] Here, the ratio of the amine compound to nickel in the reaction solution [mol %] ((moles of amine compound / moles of nickel) × 100) is in the range of 0.01 mol % to 5 mol %, preferably in the range of 0.03 mol % to 2 mol %. If the ratio is less than 0.01 mol %, the amount of the amine compound is too small, and the functions of the amine compound as an inhibitor of self-decomposition of hydrazine, an accelerator of reduction reaction, or an inhibitor of linkage between nickel particles may not be obtained. On the other hand, if the ratio exceeds 5 mol %, the amine compound may act too strongly as a complexing agent for forming nickel complex ions, which may cause abnormal particle growth of the nickel crystallized powder, and the granularity or sphericity of the nickel powder may be lost, resulting in an irregular shape, or many coarse particles formed by linking nickel particles to each other, which may cause deterioration of the properties of the nickel powder.
[0059] (f) Sulfur-containing compounds (hydrazine self-decomposition inhibitors) The sulfur-containing compound is a compound that is applied as a brightener for nickel plating or a stabilizer for plating baths, and unlike the above-mentioned amine compound, when used alone, the effect of inhibiting the self-decomposition of hydrazine is not so great. However, it has an interaction such as adsorption with the surface of nickel particles, and when used in combination with the above-mentioned amine compound, it has the effect of an auto-decomposition inhibitor of hydrazine that can significantly strengthen the self-decomposition inhibitor of hydrazine. Therefore, it is recommended to add it to the reaction solution as necessary. The above-mentioned sulfur-containing compound is a compound that contains at least one of the following groups in the molecule: sulfide group (-S-), sulfonyl group (-S(=O)2-), sulfonic acid group (-S(=O)2-O-), and thioketone group (-C(=S)-). Furthermore, the above-mentioned sulfur-containing compound, in addition to the effect of an auto-decomposition inhibitor of hydrazine, also has the effect of an inhibitor of linking nickel particles together, and when used in combination with the above-mentioned amine compound, it can more effectively reduce the amount of coarse particles formed by linking nickel particles together.
[0060] As the sulfur-containing compound, for example, in the case of a sulfide compound having a sulfide group (-S-) in the molecule, it is desirable that the compound has high water solubility, and therefore, it is preferable that the compound is any of a carboxyl group-containing sulfide compound, a hydroxyl group-containing sulfide compound, and an amino group-containing sulfide compound, which further contain at least one of a carboxyl group (-COOH), a hydroxyl group (-OH), and an amino group (primary: -NH2, secondary: -NH-, tertiary: -N<) in the molecule. In addition, a thiazole ring-containing sulfide compound, which contains at least one thiazole ring (C3H3NS), is also applicable, although it is not highly water soluble. More specifically, L (or D, or DL)-methionine (CH3SC2H4CH(NH2)COOH), L (or D, or DL)-ethionine (C2H5SC2H4CH(NH2)COOH), N-acetyl-L (or D, or DL)-methionine (CH3SC2H4CH(NH(COCH3))COOH), lanthionine (also known as 3,3'-thiodialanine) (HOOCCH(NH2)CH2SCH2CH(NH2)COOH), thiodipropionic acid (also known as 3,3'-thiodipropionic acid) (HOOCC2H At least one selected from the group consisting of 4SC2H4COOH), thiodiglycolic acid (other names: 2,2'-thiodiglycolic acid, 2,2'-thiodiacetic acid, 2,2'-thiobisacetic acid, mercaptodiacetic acid) (HOOCCH2SCH2COOH), methionol (other names: 3-methylthio-1-propanol) (CH3SC3H6OH), thiodiglycol (other names: 2,2'-thiodiethanol) (HOC2H5SC2H5OH), thiomorpholine (C4H9NS), thiazole (C3H3NS), and benzothiazole (C7H5NS) are suitable. Among these, methionine and thiodiglycolic acid are preferred because they are excellent in assisting in suppressing the self-decomposition of hydrazine, and are easily available and inexpensive.
[0061] More specifically, sulfur-containing compounds other than sulfide compounds include saccharin (also known as o-benzoic acid sulfimide, o-sulfobenzimid) (C7H5NO3S), sodium dodecyl sulfate (C 12 H 25 OS(O)2ONa), dodecylbenzenesulfonic acid (C12 H 25 C6H4S(O)2OH), sodium dodecylbenzenesulfonate (C 12 H 25 Suitable sulfur-containing compounds include saccharin, saccharin, and thiourea. These sulfur-containing compounds are water-soluble, and among them, saccharin and thiourea are preferred because they are excellent at helping to inhibit the self-decomposition of hydrazine, and are easily available and inexpensive.
[0062] The action of the sulfur-containing compound as an auxiliary agent for inhibiting the self-decomposition of hydrazine and as an inhibitor of the connection between nickel particles can be speculated as follows. That is, the sulfide group (-S-), sulfonyl group (-S(=O)2-), sulfonic acid group (-S(=O)2-O-), and thioketone group (-C(=S)-) in the molecule of the sulfur-containing compound are adsorbed to the nickel surface of the nickel particles by intermolecular forces, but the action of covering and protecting the nickel crystallized powder is not as great as that of the amine compound molecule described above when the amine compound molecule is used in combination with the sulfur-containing compound. On the other hand, when the amine compound molecule is strongly adsorbed to the surface of the nickel crystallized powder to cover and protect it, there is a high possibility that a minute area that cannot be completely covered by the amine compound molecules is generated, but the sulfur-containing compound molecule covers this part by auxiliary adsorption, which more effectively prevents the contact between the hydrazine molecule in the reaction solution and the nickel crystallized powder, and furthermore, the nickel crystallized powder can be more strongly prevented from coalescing, thereby manifesting the above action.
[0063] Here, the ratio [mol %] of the sulfur-containing compound to nickel in the reaction solution ((moles of sulfur-containing compound / moles of nickel) x 100) is in the range of 0.01 mol % to 5 mol %, preferably 0.03 mol % to 2 mol %, and more preferably 0.05 mol % to 1 mol %. If the ratio is less than 0.01 mol %, the amount of the sulfur-containing compound is too small, and the effects of the hydrazine self-decomposition inhibitor and the nickel particle bond inhibitor may not be obtained. On the other hand, even if the ratio exceeds 5 mol %, the above effects are not improved, and the amount of the sulfur-containing compound used simply increases, increasing the chemical cost and the amount of organic components blended in the reaction solution, increasing the chemical oxygen demand (COD) of the reaction wastewater in the crystallization process, resulting in an increase in wastewater treatment costs.
[0064] (g) Other Ingredients In addition to the nickel salt, salt of a metal nobler than nickel, reducing agent (e.g., hydrazine), alkali hydroxide, and amine compound, the reaction solution in the crystallization step may contain small amounts of various additives such as dispersants, complexing agents, and antifoaming agents. For example, if an appropriate dispersant or complexing agent is used in an appropriate amount, it may be possible to improve the granularity (sphericity) and surface smoothness of the nickel crystallized powder, or to reduce coarse particles. In addition, if an appropriate antifoaming agent is used in an appropriate amount, it is possible to prevent, for example, the aqueous solution from overflowing from the container by suppressing foaming in the crystallization step caused by nitrogen gas (see formulas (2) to (4) below) generated in the crystallization reaction. As the dispersant, known substances can be used, such as alanine (CH3CH(COOH)NH2), glycine (H2NCH2COOH), triethanolamine (N(C2H4OH)3), diethanolamine (also known as iminodiethanol) (NH(C2H4OH)2), etc. As the complexing agent, known substances can be used, and examples thereof include hydroxycarboxylic acid, carboxylic acid (organic acid containing at least one carboxyl group), hydroxycarboxylic acid salts and hydroxycarboxylic acid derivatives, carboxylates and carboxylate derivatives, specifically, tartaric acid, citric acid, malic acid, ascorbic acid, formic acid, acetic acid, pyruvic acid, and salts and derivatives thereof. Furthermore, as the defoaming agent, there is no particular limitation so long as it has excellent foam breaking properties under alkaline conditions, and oil-type or solvent-type silicone-based or non-silicone-based defoaming agents can be used.
[0065] (2-1-2. Crystallization Procedure) In the crystallization step, a nickel salt solution in which at least a water-soluble nickel salt and a salt of a metal nobler than nickel are dissolved in water, a reducing agent solution in which a reducing agent (e.g., hydrazine) is dissolved in water, and an alkali hydroxide solution in which an alkali hydroxide is dissolved in water are prepared, and these are added and mixed to prepare a reaction liquid. Then, a crystallization reaction is performed in which nickel particles are crystallized in this reaction liquid by a reduction reaction to obtain nickel crystallized powder. Note that an amine compound or a sulfur-containing compound, which is added as necessary, can be added and mixed to any of the above solutions or a mixture of them before preparing the reaction liquid, or can be added and mixed to the reaction liquid after preparing the reaction liquid. Note that, in a room temperature environment, the reduction reaction starts at the time when the reaction liquid is prepared.
[0066] Here, there are two specific crystallization procedures: a procedure in which a reducing agent (e.g., hydrazine) and a reducing agent-alkali hydroxide solution containing an alkali hydroxide are added to a nickel salt solution containing nickel salt as a reduction target and a salt of a metal nobler than nickel to prepare a reaction solution, and a procedure in which an alkali hydroxide solution is added to the nickel salt-reducing agent solution obtained by adding a reducing agent solution (e.g., hydrazine solution) to the nickel salt solution to prepare a reaction solution. The former procedure involves adding a reducing agent (e.g., hydrazine) that has been made highly alkaline and has increased reducing power due to the alkali hydroxide to a nickel salt solution containing a reduction target, whereas the latter procedure involves mixing a reducing agent (e.g., hydrazine) with a nickel salt solution containing a reduction target in advance, and then adjusting (raising) the pH with an alkali hydroxide to increase the reducing power.
[0067] In the former case (when nickel salt solution and reducing agent / alkali hydroxide solution are added and mixed), depending on the temperature at the time when the reaction solution is prepared, that is, at the time when the reduction reaction starts (hereinafter, sometimes referred to as the reaction start temperature), if the time required for adding and mixing the nickel salt solution (a solution containing nickel salt and a salt of a metal nobler than nickel) and the reducing agent / alkali hydroxide solution, which has been made more alkaline by using an alkali hydroxide to increase the reducing power, becomes long, the alkalinity increases locally in the nickel salt solution and reducing agent / alkali hydroxide solution addition and mixing area from the middle of the addition and mixing stage, and the reducing power of hydrazine increases, causing nucleation due to the salt of a metal nobler than nickel, which is the nucleating agent. Therefore, the closer to the end of the raw material mixing time, the greater the dependency of nucleation on the raw material mixing time becomes, which means that the nucleation effect of the added nucleating agent weakens, and there is a tendency that it becomes difficult to refine the nickel crystallized powder or obtain a narrow particle size distribution. This tendency is more noticeable when an alkaline reducing agent / alkali hydroxide solution is added and mixed with a weakly acidic nickel salt solution. The above tendency can be suppressed more easily by mixing the raw materials for a shorter time, so mixing for a short time is desirable. However, taking into consideration constraints on mass production equipment, the mixing time of the raw materials is preferably 10 to 180 seconds, more preferably 20 to 120 seconds, and even more preferably 30 to 80 seconds.
[0068] On the other hand, in the latter case (when an alkali hydroxide solution is added and mixed into a nickel salt-reducing agent solution obtained by adding and mixing a nickel salt solution and a reducing agent solution), the reducing agent hydrazine is added and mixed in advance in the nickel salt-reducing agent solution containing nickel salt, a salt of a metal nobler than nickel, and a reducing agent, to obtain a uniform concentration. Therefore, the dependency of nucleation that occurs when adding and mixing an alkali hydroxide solution on the mixing time of the raw materials of the alkali hydroxide is not as large as in the former case, and it is easy to refine the nickel crystallized powder and obtain a narrow particle size distribution. However, for the same reason as in the former case, it is desirable to mix the alkali hydroxide solution for a short time, and considering the constraints of mass production equipment, the mixing time is preferably 10 seconds to 180 seconds, more preferably 20 seconds to 120 seconds, and even more preferably 30 seconds to 80 seconds.
[0069] As described above, there are two types of procedures for adding and mixing the amine compound and the sulfur-containing compound in this embodiment: a procedure in which the amine compound and the sulfur-containing compound are mixed in advance with the reaction liquid before the reaction liquid is prepared, and a procedure in which the amine compound and the sulfur-containing compound are added and mixed after the reaction liquid is prepared and the reduction reaction is started.
[0070] In the former case (when an amine compound or sulfur-containing compound is added to the reaction solution before the reaction solution is prepared), since the amine compound or sulfur-containing compound is added to the reaction solution beforehand, there is an advantage that the various actions of the amine compound or sulfur-containing compound are manifested from the start of nucleation caused by the salt (nucleating agent) of a metal more noble than nickel. On the other hand, the interaction of the amine compound or sulfur-containing compound with the nickel particle surface, such as adsorption, is involved in nucleation, and may affect the particle size and particle size distribution of the resulting nickel crystallized powder.
[0071] On the contrary, in the latter case (when the reaction solution is prepared and the amine compound or sulfur-containing compound is added and mixed after the start of the reduction reaction), the amine compound or sulfur-containing compound is added and mixed into the reaction solution after the very early stage of the crystallization process in which nucleation due to the nucleating agent occurs. Therefore, although the action of the amine compound or sulfur-containing compound described above is somewhat delayed, the amine compound or sulfur-containing compound is no longer involved in nucleation, so that the particle size and particle size distribution of the obtained nickel crystallized powder are less likely to be affected by the amine compound or sulfur-containing compound, and there is an advantage that they can be easily controlled. Here, the mixing time for adding and mixing the amine compound or sulfur-containing compound into the reaction solution in this procedure may be added all at once within a few seconds, or may be added in portions or dropwise over a period of several minutes to about 30 minutes. As mentioned above, the amine compound acts as a reduction reaction accelerator (complexing agent). Therefore, slow addition will cause the crystal growth to proceed slowly and the nickel crystallized powder to have high crystallinity, but the inhibition of the self-decomposition of hydrazine will also gradually work, and the effect of reducing the amount of hydrazine consumed will decrease, so the mixing time can be appropriately determined while taking into account the balance between these two. Note that the timing of adding and mixing the amine compound and the sulfur-containing compound in the former procedure can be appropriately selected by comprehensively judging according to the purpose.
[0072] When adding and mixing the nickel salt solution and the reducing agent / alkali hydroxide solution, when adding and mixing the nickel salt solution and the reducing agent solution, and when adding and mixing the alkali hydroxide solution to the nickel salt / reducing agent solution, it is preferable to use stirring and mixing in which the solutions are stirred while mixing. If the stirring and mixing properties are good, the frequency of uneven nuclei generation decreases, depending on the location of nuclei generation, and the dependency of nuclei generation on the raw material mixing time and the alkali hydroxide mixing time as described above decreases, making it easier to refine the nickel crystallized powder and obtain a narrow particle size distribution. Any known method may be used for the stirring and mixing method, and it is preferable to use a stirring blade in terms of controlling the stirring and mixing properties and equipment costs.
[0073] (2-1-3. Reduction reaction) In the crystallization step, nickel salt is reduced with hydrazine in the presence of an alkali hydroxide and a salt of a metal nobler than nickel in the reaction solution to obtain nickel crystallized powder. If necessary, the reduction reaction can be carried out while significantly suppressing the self-decomposition of hydrazine by the action of a trace amount of a specific amine compound or sulfur-containing compound.
[0074] First, the reduction reaction in the crystallization process will be explained. 2+ The reaction in which nickel (Ni) crystallizes is a two-electron reaction as shown in the following formula (1). The reaction with hydrazine (N2H4) is a four-electron reaction as shown in the following formula (2). For example, as mentioned above, when nickel chloride (NiCl2) is used as the nickel salt and sodium hydroxide (NaOH) is used as the alkali hydroxide, the overall reduction reaction is expressed as shown in the following formula (3), in which nickel hydroxide (Ni(OH)2), which is produced by the neutralization reaction of nickel chloride and sodium hydroxide, is reduced by hydrazine. Stoichiometrically (theoretical value), 0.5 moles of hydrazine (N2H4) are required for 1 mole of nickel (Ni).
[0075] Here, from the reduction reaction of hydrazine in formula (2), we can see that the stronger the alkalinity of hydrazine, the greater its reducing power. The alkali hydroxide is used as a pH adjuster to increase the alkalinity of the reaction solution, and it plays a role in promoting the reduction reaction of hydrazine.
[0076] [Case 2] Ni 2+ +2e - →Ni↓ (two-electron reaction) ···(1) N2H4→N2↑+4H + +4e - (4-electron reaction) (2) 2NiCl2+N2H4+4NaOH →2Ni(OH)2+N2H4+4NaCl →2Ni↓+N2↑+4NaCl+4H2O ···(3)
[0077] As described above, in the conventional crystallization process, the active surface of the nickel crystallization powder acts as a catalyst to promote the self-decomposition reaction of hydrazine shown in the following formula (4), and hydrazine as a reducing agent may be consumed in large quantities other than for reduction. For this reason, although it depends on the crystallization conditions such as the reaction start temperature, for example, about 2 moles of hydrazine per mole of nickel, which is about four times the theoretical value required for the reduction described above, was generally used. Furthermore, as shown in formula (4), a large amount of ammonia is by-produced in the self-decomposition of hydrazine, and ammonia is contained in the reaction liquid at a high concentration, resulting in the generation of nitrogen-containing waste liquid. Thus, the use of an excessive amount of hydrazine, which is an expensive chemical, and the generation of the cost of treating the nitrogen-containing waste liquid are factors that increase the production cost of nickel powder by the wet method (wet nickel powder).
[0078] [C3] 3N2H4→N2↑+4NH3...(4)
[0079] Therefore, in the method for producing nickel powder of this embodiment, it is preferable to add a trace amount of a specific amine compound or sulfur-containing compound to the reaction solution to significantly suppress the self-decomposition reaction of hydrazine, and to significantly reduce the amount of hydrazine used, which is expensive as a drug. The specific amine compound can suppress the self-decomposition of hydrazine because (I) the molecules of the specific amine compound or sulfur-containing compound are adsorbed on the surface of the nickel crystallized powder in the reaction solution, physically preventing the contact between the active surface of the nickel crystallized powder and the hydrazine molecules, and (II) the molecules of the specific amine compound or sulfur-containing compound act on the surface of the nickel crystallized powder, deactivating the catalytic activity of the surface, etc.
[0080] In the conventional wet crystallization process, nickel ions (Ni 2+In general, a complexing agent that forms a complex ion with hydrazine and increases the concentration of ionic nickel is used as a reduction reaction accelerator. However, these complexing agents such as tartaric acid and citric acid do not have the effect of inhibiting the self-decomposition of hydrazine, such as the above-mentioned specific amine compounds and sulfur-containing compounds, or the effect of inhibiting linkage that makes it difficult for nickel particles to link together during crystallization to form coarse particles.
[0081] On the other hand, the specific amine compound also functions as a complexing agent like tartaric acid, citric acid, etc., and has the advantage of acting as a hydrazine self-decomposition inhibitor, a linkage inhibitor, and a reduction reaction accelerator.
[0082] (2-1-4. Reaction start temperature) The crystallization reaction in the crystallization step is initiated in a reaction solution obtained by adding and mixing a solution containing a reducing agent (e.g., hydrazine) and an alkali hydroxide (reducing agent-alkali hydroxide solution) to a solution (nickel salt solution) containing at least a water-soluble nickel salt and a salt of a metal nobler than nickel. In this case, the reaction initiation temperature of the crystallization reaction is preferably 40°C to 95°C, more preferably 50°C to 80°C, and even more preferably 60°C to 70°C. The temperatures of the nickel salt solution and the reducing agent-alkali hydroxide solution are not particularly limited and can be freely set as long as the temperature of the mixed solution obtained by premixing them, i.e., the reaction initiation temperature, is within the above temperature range.
[0083] The higher the reaction initiation temperature, the more the reduction reaction is promoted and the nickel crystallized powder tends to be highly crystallized, but on the other hand, the self-decomposition reaction of hydrazine is promoted even more, so the consumption of hydrazine increases and the reaction solution tends to foam violently. Therefore, if the reaction initiation temperature is too high, the consumption of hydrazine may increase significantly or the crystallization reaction may not be able to continue due to a large amount of foaming. On the other hand, if the reaction initiation temperature is too low, the crystallinity of the nickel crystallized powder may decrease significantly, the reduction reaction may slow down, the time of the crystallization process may be significantly extended, and the productivity of the nickel powder may decrease. For the above reasons, by setting the temperature within the above range, it is possible to produce high-performance nickel powder at a low cost while suppressing the consumption of hydrazine and maintaining high productivity.
[0084] (2-2. Washing and filtration process) In the above-mentioned wet method for producing nickel powder, hydrazine is often used as a reducing agent, and therefore the reaction solution generally becomes strongly alkaline (for example, about pH 14), as is clear from Patent Document 4 and the like. As shown in Fig. 1, in the crystallization step, a nickel powder slurry is obtained in which nickel crystallized powder is generated in the strongly alkaline reaction solution by the reduction reaction of hydrazine, and the crystallization step is followed by a washing and filtration step in which the nickel crystallized powder is washed with pure water and filtered and recovered from the nickel powder slurry to obtain a nickel powder cake, and a drying step in which the nickel powder cake is dried (vacuum drying, etc.) to obtain nickel crystallized powder (nickel powder).
[0085] Since the above washing and filtering steps are usually carried out in the air, the obtained nickel powder cake is exposed to the air to a greater or lesser extent during the washing and filtering steps or until drying in the drying step, and oxidation of the nickel crystallized powder is unavoidable. In particular, when the crystallization reaction is carried out on a mass production scale, unlike handling of small amounts at the laboratory level, handling of the nickel powder cake takes time, and therefore the oxidation of the nickel crystallized powder due to the above exposure to the air is likely to progress.
[0086] In the nickel powder cake obtained through the washing and filtration process in which the strongly alkaline nickel powder slurry (e.g., pH 14) is washed with pure water and filtered, the strongly alkaline alkali hydroxide is removed by washing, but a small amount of the alkali hydroxide may remain on the nickel powder cake as a weakly alkaline adhesion liquid (e.g., pH 11). Therefore, if oxidation of the nickel crystallized powder occurs in this state, the nickel ions (Ni 2+ ) is more likely to form nickel hydroxide (Ni(OH)2) according to formula (5). In particular, the higher the temperature, the more likely the oxidation of nickel crystallized powder will progress, and the oxidation of nickel crystallized powder tends to progress even more in the hot summer months than in the cold winter months. In locations where a large amount of nickel hydroxide is formed, it is likely that nickel crystallized powder 1 (particle size 0.1 μm or less) will end up being firmly bound together by nickel hydroxide 2 to form coarse particles 10 (coarse particles whose main component is nickel hydroxide) (often with a particle size of 0.8 μm or more, see Figure 2).
[0087] [C4] Ni 2+ +2OH - →Ni(OH)2···(5)
[0088] Therefore, in this embodiment, the air exposure time of the nickel powder cake is kept at 10 minutes or less from the time of filtration in the washing and filtration process until the drying of the nickel powder is started in the drying process described below. More specifically, when the temperature of the pure water used to wash the nickel powder cake is in the range of 25°C to 45°C, the air exposure time is kept at 10 minutes or less. Since the temperature in the environment in which the nickel powder is produced is high, the temperature of the pure water used for washing is also high, so that even if the temperature of the nickel powder cake is high and in the range of 25°C to 45°C, the oxidation of the nickel powder is less likely to proceed by shortening the air exposure time, and as a result, nickel hydroxide (Ni(OH)2) is less likely to grow.
[0089] Here, the lower limit of the air exposure time is ideally 0 minutes. However, since time is required to move the nickel powder cake from the equipment used for the washing and filtration process to the equipment used for the drying process, it is preferable from the viewpoint of suppressing the generation of nickel hydroxide that the air exposure time is in the range of 1 to 5 minutes.
[0090] If the temperature of the pure water used to wash the nickel powder cake exceeds 45°C and the exposure time to the atmosphere exceeds 10 minutes, the oxidation of the nickel powder will progress and the number of coarse particles in the nickel powder will increase.
[0091] Furthermore, it is desirable that the moisture content of the nickel powder cake is 70% by mass or less from the time of filtration to the start of drying. In particular, from the viewpoint that moisture can prevent direct contact between the nickel crystallized powder and substances that cause oxidation, such as oxygen in the air, and thus suppress oxidation of the nickel crystallized powder, it is more desirable that the moisture content is 5% by mass or more and 70% by mass or less. Here, by having the moisture content of the nickel powder cake be 70% by mass or less, the drying time in the subsequent drying step can be shortened. And, in order to make the moisture content of the nickel powder cake less than 5% by mass, the filtration time becomes long, and even if it is less than 5% by mass, the drying time is not significantly shortened, so the lower limit of the moisture content is preferably 5% by mass. Also, by making the moisture content of the nickel powder cake 70% by mass or less, the moisture content derived from the nickel hydroxide of the nickel powder can be 0.5% or less, and further, the drying time in the drying step can be further shortened, so that the moisture content of the nickel powder cake is preferably 60% by mass or less, and more preferably 50% by mass or less.
[0092] In addition, when the temperature of the pure water used to wash the nickel crystallized powder in the washing and filtering process is 25°C to 45°C, this pure water is used to wash the nickel crystallized powder with pure water so that the conductivity of the liquid containing the nickel crystallized powder is 30μS / cm to 1000μS / cm, preferably 30μS / cm to 500μS / cm, and more preferably 30μS / cm to 100μS / cm (washing step), and then the nickel crystallized powder is filtered from the liquid to obtain a nickel powder cake containing the adhering liquid (filtration step). By going through these steps, the amount of remaining impurities (Na, Cl, etc.) due to the chemicals used in the crystallization process is significantly reduced, and at the same time, the alkalinity of the adhering liquid of the nickel powder cake is weakened to make it difficult to form nickel hydroxide (Ni(OH)2), and the generation of coarse particles mainly composed of nickel hydroxide as described above can be significantly suppressed.
[0093] For example, after obtaining a liquid containing nickel crystallized powder by setting the reaction start temperature of the crystallization reaction at 40°C to 95°C, the liquid containing the nickel crystallized powder is washed with pure water at 25°C to 45°C until the conductivity of the liquid containing the nickel crystallized powder becomes 30 μS / cm to 1000 μS / cm. Even when the temperature of the nickel powder cake becomes 25°C to 45°C, by keeping the exposure time of the nickel powder cake to the atmosphere for 10 minutes or less, the oxidation of the nickel powder is unlikely to proceed and nickel hydroxide (Ni(OH)2) is unlikely to be formed.
[0094] In this embodiment, before the washing step in the washing and filtering process, a neutralization step (neutralization step) can be performed in which the strongly alkaline nickel powder slurry or its diluted solution is neutralized with an inorganic acid or an organic acid to a pH of 7.0 to 9.0. After the neutralization step, the solution containing the nickel crystallized powder can be washed with pure water at 25°C to 45°C until the electrical conductivity of the solution is 30 μS / cm to 1000 μS / cm.
[0095] In the neutralization step, the pH of the nickel powder slurry or its dilution is preferably 7.0 to 9.0 when neutralized with inorganic acid or organic acid. If the pH is less than 7.0 in the neutralization treatment, that is, if an excessive amount of inorganic acid or organic acid is added, the generation of coarse particles mainly composed of nickel hydroxide may increase. As the pH of the nickel powder slurry or its dilution, which is in a strongly alkaline state, is lowered by neutralizing it, the generation of coarse particles mainly composed of nickel hydroxide is suppressed, but if the pH is set to 7.0 to 9.0 by the neutralization treatment, the content of coarse particles mainly composed of nickel hydroxide in the nickel powder can be sufficiently reduced.
[0096] The agent used for neutralizing the nickel powder slurry or its dilution may be one or more selected from inorganic acids or organic acids, and is not particularly limited as long as it is easily soluble in water. Specifically, hydrochloric acid (HCl), nitric acid (HNO3), sulfuric acid (H2SO4), carbonic acid (H2CO3), etc. can be used as inorganic acids, and acetic acid (CH3COOH), citric acid (C(OH)(CH2COOH)2COOH), ascorbic acid (C6H8O6), etc. can be used as organic acids. These inorganic acids and organic acids may be used as they are for neutralization, but it is more preferable to use them in the form of an aqueous solution in consideration of ease of handling. For example, when carbonic acid is used, carbon dioxide gas (CO2) may be blown into the liquid (nickel powder slurry or its dilution) to perform the neutralization action as carbonic acid in the liquid. In addition, if an organic acid that forms a complex ion with nickel, such as citric acid, is used, the effect of preventing oxidation of the nickel crystallized powder can be expected.
[0097] If the nickel powder slurry is strongly alkaline, for example with a pH of about 14, even if the cleaning solution is washed directly with pure water and the conductivity of the cleaning solution is reduced to about 100 μS / cm, the pH of the cleaning solution can remain strongly alkaline at about 11. However, in the method of neutralization using an inorganic acid or organic acid of this embodiment, when the conductivity of the cleaning solution is similarly reduced to about 100 μS / cm, the pH of the cleaning solution can be reduced to a maximum of about 9 or less.
[0098] In addition, inorganic acids or organic acids can be added directly to a strongly alkaline nickel powder slurry (e.g., pH 14), but in that case, a large amount of inorganic acid or organic acid is required for neutralization, which may be disadvantageous in terms of cost and workability. Therefore, it is preferable to first remove the supernatant liquid of the nickel powder slurry by a method such as decantation, reduce the amount of alkaline components in the nickel powder slurry, and then mix and add inorganic acids or organic acids and their aqueous solutions to neutralize it.
[0099] (2-2-1. Methods and procedures for cleaning and filtering) In this embodiment, in the process of washing the strongly alkaline nickel powder slurry (e.g., about pH 14) obtained in the crystallization process using a general-purpose washing method to obtain nickel crystallized powder, the strongly alkaline nickel powder slurry or its diluted solution is washed using pure water at, for example, 25°C to 45°C, and finally, the nickel crystallized powder is filtered and recovered using a general-purpose solid-liquid separation device as a nickel powder cake containing the adhering liquid at a temperature of 25°C to 45°C.
[0100] Specific examples of the general-purpose washing method include, but are not limited to, repeated decantation and dilution with pure water, repeated concentration of nickel crystallized powder (high concentration slurry or cake formation) and pure water repulping (re-slurrying by adding pure water) using a solid-liquid separation device, and washing by passing pure water through the concentrate (cake) of nickel crystallized powder in the solid-liquid separation device, etc. Specific examples of the general-purpose solid-liquid separation device include, but are not limited to, a Denver filter, a filter press, a centrifuge, a decanter, etc.
[0101] The pure water used for the above cleaning should generally be of high purity with a conductivity of 1 μS / cm or less. Although distilled water or ultrapure water (conductivity: ≦0.06 μS / cm) can be used instead of pure water, it is preferable to use pure water, which is inexpensive and easily available.
[0102] As a washing procedure for the nickel powder slurry, pure water can be directly mixed and added to the strongly alkaline nickel powder slurry (for example, about pH 14), but in that case, a large amount of pure water is required, which may be disadvantageous in terms of workability. Therefore, it is preferable to once remove the supernatant liquid of the nickel powder slurry by a method such as decantation, reduce the amount of alkaline components in the nickel powder slurry, and then add pure water.
[0103] (2-3. Drying process) The nickel powder cake containing the neutralized adhesion liquid obtained in the washing and filtration process is exposed to the atmosphere for 10 minutes or less from the time of filtration until the start of drying in the drying process, and is dried at 50 to 300 ° C, preferably 80 to 150 ° C, using a general-purpose drying device such as an inert gas atmosphere dryer or a vacuum dryer so that the nickel crystallized powder is not exposed to the atmosphere in the drying process, to obtain nickel crystallized powder (nickel powder). If necessary, the adhesion water in the nickel powder cake can be replaced with a low-temperature volatile organic solvent such as ethanol, and then dried with the inert gas atmosphere dryer or vacuum dryer to weaken the drying aggregation between nickel particles that occurs during drying due to the large surface tension of water.
[0104] In addition, when the nickel powder cake is dried at about 200°C to 300°C in an inert atmosphere, reducing atmosphere, or vacuum atmosphere using a drying device such as an inert gas atmosphere dryer or a vacuum dryer, it is possible to obtain nickel powder that has been heat-treated in addition to being simply dried.
[0105] (2-4. Crushing process (post-processing process)) As described above, when an amine compound or a sulfur-containing compound is added as necessary to the nickel crystallized powder (nickel powder) obtained through the crystallization process, the washing / filtration process, and the drying process, the compound acts as an inhibitor of nickel particle linkage during nickel crystallization. Therefore, the content of coarse particles formed by nickel particles linking to each other during the reduction precipitation process (hereinafter, to distinguish from "coarse particles mainly composed of nickel hydroxide") is not so large in the first place. However, depending on the crystallization procedure and crystallization conditions, the content of linked coarse particles may become somewhat large and become a problem. In this case, a crushing process is provided following the crystallization process, and the linked coarse particles formed by nickel particles are cut at the linkages to reduce the linked coarse particles. In the crushing process, it is possible to apply dry crushing methods such as spiral jet crushing and counter jet mill crushing, wet crushing methods such as high-pressure fluid collision crushing, and other general-purpose crushing methods.
[0106] In addition, since the coarse particles mainly composed of nickel hydroxide, which are the nickel crystallized powder (average particle size 0.03 μm to 0.15 μm) firmly bound together by nickel hydroxide, cannot be easily disintegrated using the various general-purpose disintegration methods described above, effective measures to suppress the formation of coarse particles mainly composed of nickel hydroxide are very important, and this embodiment is extremely useful from that perspective as well. EXAMPLES
[0107] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples. The properties of the nickel powder, including the average particle size, oxygen value, moisture content derived from nickel hydroxide, and content of coarse particles, are evaluated as follows.
[0108] (Average particle size) The nickel powder obtained in the present invention has an approximately spherical particle shape, and its average particle size is a number-average particle size based on the particle size obtained from the results of image analysis of observation images (SEM images) of the nickel powder using a scanning electron microscope (SEM, JSM-7100F, manufactured by JEOL Ltd.).
[0109] (Oxygen value measurement) The oxygen value was determined by the inert gas fusion method. Specifically, nickel powder was placed in a graphite crucible in a helium stream and heated and melted by impulse heating, and the nitrogen in the sample was extracted as N2 and the oxygen as CO. The CO was oxidized to CO2 with heated copper oxide and measured with an infrared absorption detector.
[0110] (Measurement of moisture content derived from nickel hydroxide) Using a Karl Fischer moisture meter, the moisture content of nickel powder was measured at a vaporization temperature of 110°C (KF110°C) and at a vaporization temperature of 300°C (KF300°C). Here, the moisture content at KF110°C can be regarded as the moisture content (%) attached to the nickel powder, and the moisture content at KF300°C can be regarded as the sum (%) of the moisture content derived from nickel hydroxide and the above-mentioned moisture content. Therefore, the moisture content (%) derived from nickel hydroxide was obtained by subtracting the moisture content at KF110°C from the moisture content at KF300°C and excluding the attached moisture content.
[0111] (Content of coarse particles) The nickel powder dispersion obtained by ultrasonically dispersing 0.05 g of nickel powder of Example 1, Comparative Examples 1 and 2, and Reference Examples 1 to 3 obtained by the method described below in 100 mL of 0.1 mass % sodium hexametaphosphate aqueous solution was filtered through a membrane filter (pore size 0.4 μm) to capture coarse particles (0.4 μm) larger than the pore size of the membrane filter on the filter, and the amount of the coarse particles was calculated by ICP atomic emission spectrometry (inductively coupled plasma atomic emission spectrometry) of a solution in which all the coarse particles were dissolved in acid, and the content of coarse particles exceeding 0.4 μm in particle size contained in the nickel powder was determined.
[0112] In principle, the content of the coarse particles includes all of the following cases ((1) to (3)): (1) coarse nickel particles each having a particle size exceeding 0.4 μm; (2) nickel particles (nickel crystallized powder) having an average particle size of 0.03 μm to 0.15 μm are connected to each other on the surface of the nickel particle during the crystallization process (reduction precipitation process) to form connected coarse particles having a size exceeding 0.8 μm; and (3) coarse particles mainly composed of nickel hydroxide having a size exceeding 0.4 μm (see FIG. 2) that are formed by nickel particles (nickel crystallized powder) having an average particle size of 0.03 μm to 0.15 μm being firmly solidified with nickel hydroxide produced by oxidation.
[0113] However, in the present invention, as described above, since the wet nickel powder characterized by a narrow particle size distribution is used, coarse nickel particles having a particle size exceeding 0.4 μm are not generated alone, and the above case (1) does not need to be considered. Furthermore, the content of the connected coarse particles generated by nickel particles (nickel crystallized powder) having an average particle size of 0.03 μm to 0.15 μm connecting on the surface of the nickel particles during the crystallization process (reduction precipitation process) is not so high if appropriate crystallization conditions are adopted, and the connection strength between the nickel particles is not so strong. Therefore, as described above, if a crushing process is performed after crystallization, even if the content ratio of the connected coarse particles becomes somewhat large, the connected coarse particles can be divided at the connecting parts to make the connected coarse particles 0.4 μm or less in size, so the above case (2) does not need to be considered. Therefore, the coarse particles captured by the membrane filter are only in the case of (3), and the content of coarse particles exceeding 0.4 μm in the present invention may be considered to be the content of coarse particles mainly composed of nickel hydroxide having a particle size exceeding 0.4 μm. Coarse particles mainly composed of nickel hydroxide having a particle size exceeding 0.4 μm are coarse particles that are tightly bound together by nickel hydroxide formed on the surface of the nickel crystallized powder, entangling multiple nickel particles (nickel crystallized powder), and therefore will not be disintegrated even if the above-mentioned crushing treatment is performed, and will remain in the nickel powder as coarse particles of the same size.
[0114] (Coarse particles mainly composed of nickel hydroxide) The coarse particles with a size exceeding 0.4 μm captured on the membrane filter as described above have a structure in which multiple nickel particles (nickel crystallized powder) are entrapped in a matrix made of nickel hydroxide and are firmly bound via the nickel hydroxide matrix, as shown in Figure 2. The fact that the matrix (reference number 2 in Figure 2) is mainly composed of nickel hydroxide (Ni(OH)2) has been confirmed by the following: (a) In the measurement of the matrix part of the coarse particles with a size exceeding 0.4 μm captured on the membrane filter, many parts are observed in which the molar ratio of nickel to oxygen is about Ni:O=1:2 in the measurement by energy dispersive X-ray spectroscopy (SEM-EDX) using a scanning electron microscope, and (b) In the measurement result of X-ray photoelectron spectroscopy (XPS) of the coarse particles with a size exceeding 0.4 μm recovered from the membrane filter, nickel hydroxide (Ni(OH)2) is detected as the main component.
[0115] Example 1 [Preparation of solutions of nickel salts and salts of metals more noble than nickel] A nickel salt solution was prepared by dissolving 6,717 g of nickel sulfate hexahydrate (NiSO4·6H2O, molecular weight: 262.85) as a nickel salt, 19.067 g of L-methionine (CH3SC2H4CH(NH2)COOH, molecular weight: 149.21) containing one sulfide group (-S-) in the molecule as a sulfur-containing compound acting as an auxiliary agent for inhibiting the self-decomposition of hydrazine, and 0.134 mg of ammonium palladium (II) chloride (also known as ammonium tetrachloropalladate (II)) ((NH4)2PdCl4, molecular weight: 284.31) as a salt of a metal more noble than nickel in 1,880 mL of pure water. The nickel salt solution was prepared by dissolving 6,717 g of nickel sulfate hexahydrate (NiSO4·6H2O, molecular weight: 262.85) as a nickel salt, 19.067 g of L-methionine containing one sulfide group (-S-) in the molecule as a sulfur-containing compound acting as an auxiliary agent for inhibiting the self-decomposition of hydrazine in the molecule, and 0.134 mg of ammonium palladium (II) chloride (also known as ammonium tetrachloropalladate (II)) ((NH4)2PdCl4, molecular weight: 284.31) as a salt of a metal more noble than nickel in 1,880 mL of pure water. Here, in the nickel salt solution, the sulfide compound L-methionine was present in a trace amount of 0.5 mol % (molar ratio of 0.005) relative to nickel, and palladium was present in an amount of 200 mol ppm relative to nickel.
[0116] [Preparation of reducing agent solution] As a reducing agent, hydrazine hydrate (N2H4·H2O, molecular weight: 50.06) was diluted 1.67 times with pure water to prepare 60% industrial grade hydrazine hydrate (manufactured by Otsuka MGC Chemical Co., Ltd.) weighing out 517.5 g for addition mixing and 2587.5 g for dropwise mixing, to prepare a reducing agent solution that does not contain alkali hydroxide and contains hydrazine as the main component. The hydrazine contained in the reducing agent solution was adjusted so that the molar ratio to nickel in the nickel salt solution was 0.87.
[0117] [Alkaline hydroxide solution] As an alkali hydroxide, 5637 mL of sodium hydroxide (NaOH, molecular weight: 40.0) was dissolved in 5637 mL of pure water to prepare an alkali hydroxide solution containing sodium hydroxide as the main component. The sodium hydroxide contained in the alkali hydroxide solution was adjusted so that the molar ratio to nickel in the nickel salt solution was 5.75.
[0118] [Amine compound solution] As an amine compound serving as a hydrazine self-decomposition inhibitor and reduction reaction accelerator (complexing agent), 15.359 g of ethylenediamine (abbreviation: EDA) (H2NC2H4NH2, molecular weight: 60.1), an alkyleneamine containing two primary amino groups (-NH2) in the molecule, was dissolved in 300 mL of pure water to prepare an amine compound solution, which is an aqueous solution containing ethylenediamine as the main component. The amount of ethylenediamine contained in the amine compound solution was a trace amount of 1.0 mol % (0.01 in molar ratio) relative to the nickel in the nickel salt solution. The materials used in the nickel salt solution, reducing agent solution, alkali hydroxide solution, and amine compound solution, except for 60% hydrazine hydrate by mass, were all reagents manufactured by Wako Pure Chemical Industries, Ltd.
[0119] [Crystallization process] A nickel salt solution in which nickel chloride and palladium salt were dissolved in pure water was placed in a Teflon (registered trademark) coated stainless steel container with a stirring blade and stirred. Next, 517.5 g of the above-mentioned reducing agent solution containing hydrazine and water at a liquid temperature of 25°C was added and mixed in the container for a mixing time of 30 seconds to prepare a nickel salt-reducing agent-containing solution. The above-mentioned alkali hydroxide solution containing an alkali hydroxide and water at a liquid temperature of 25°C was added and mixed in a mixing time of 30 seconds to this nickel salt-reducing agent-containing solution to prepare a reaction solution (nickel chloride + palladium salt + hydrazine + sodium hydroxide), and the temperature of the water bath for heating the container was set to 95°C to start heating the reaction solution, thereby starting the reduction reaction (crystallization reaction). The reaction start temperature was 26.2°C. Over a period of 20 minutes from 54 minutes to 74 minutes after the start of the reaction, the above-mentioned amine compound solution was added dropwise to the above-mentioned reaction solution, and the reduction reaction was promoted while suppressing the self-decomposition of hydrazine, causing nickel crystallization powder to crystallize in the reaction solution. In addition, over a period of 36 minutes from 54 minutes to 90 minutes after the start of the reaction, 2587.5 g of the reducing agent solution containing hydrazine and water at a liquid temperature of 25° C. was added dropwise to the reaction solution. Within 80 minutes after the start of the reaction, the reduction reaction of the above-mentioned formula (3) was completed, the supernatant liquid of the reaction solution was transparent, and it was confirmed that all of the nickel components in the reaction solution had been reduced to metallic nickel, and a slurry containing nickel crystallized powder was obtained as the end-of-reaction liquid.
[0120] The amount of 60% hydrazine hydrate consumed in the crystallization reaction was 1858.4 g, relative to 3105 g of 60% hydrazine hydrate (517.5 g for addition and mixing + 2587.5 g for dropwise mixing) blended in the reducing agent solution, and the molar ratio to nickel was 0.87.
[0121] [Washing and filtration process] The slurry containing nickel crystallized powder was subjected to suction filtration and washing using a Buchner funnel (filter paper: 5C) with pure water adjusted to 40°C until the conductivity of the filtrate filtered from the slurry containing nickel crystallized powder became 30μS / cm or less, to obtain a nickel powder cake. In order to set the air exposure time from after filtration in the washing and filtration process to the start of drying in the drying process described below to 5 minutes, the nickel powder cake obtained after suction filtration and washing was exposed to the air for 5 minutes in an air dryer preheated and maintained at 40°C to simulate the air exposure of the nickel powder cake in summer.
[0122] [Drying process] The nickel powder cake after exposure to the atmosphere was dried in a vacuum dryer set at a temperature of 150° C. to obtain nickel crystallized powder (nickel powder).
[0123] [Crushing process (post-processing process)] The crystallization process, washing / filtration process, and drying process were followed by a crushing process to reduce the coarse particles formed by the connection of nickel particles in the nickel powder. Specifically, the nickel crystallized powder (nickel powder) obtained in the crystallization process was mixed with pure water to prepare a nickel slurry having a slurry concentration of 300 g / L, and the nickel slurry was subjected to a wet crushing process. For the wet crushing, a high-pressure fluid collision crushing process was adopted, and specifically, the nickel slurry delivered by a roller pump was hit against high-pressure air (1.4 MPa) and dropped, and the dropped nickel slurry was collided with a collision plate to crush the coarse particles formed by the connection. The obtained nickel slurry was subjected to suction filtration using a Buchner funnel (filter paper: 5C) to perform solid-liquid separation. Thereafter, the adhering water in the nickel powder cake after the solid-liquid separation was replaced with ethanol, and then the cake was dried in a vacuum dryer to obtain nickel powder. The nickel powder according to Example 1, which was produced using a wet method, was obtained by the above process.
[0124] (Physical properties of nickel powder) Table 1 shows the nickel powder production conditions, such as the temperature of the pure water used for washing and the time of exposure to air, as well as the average particle size, oxygen value, moisture content derived from nickel hydroxide, and content of coarse particles exceeding 0.4 μm mainly composed of nickel hydroxide of the produced nickel powder. Similarly, Table 1 shows the results of Reference Examples 1 to 3 and Comparative Examples 1 and 2 described later.
[0125] (Comparative Examples 1 and 2) In the washing and filtration process, the nickel powder cake was exposed to the atmosphere for 15 minutes (Comparative Example 1) and 25 minutes (Comparative Example 2) during the period from the time of filtration in the filtration process to the start of drying in the drying process, and nickel crystallized powder (nickel powder) was obtained in the same manner as in Example 1. The nickel crystallized powder (nickel powder) was then subjected to the same wet crushing treatment as in Example 1. Through the above steps, nickel powders according to Comparative Examples 1 and 2, which were produced using a wet method, were obtained.
[0126] (Reference examples 1~3) Reference Examples 1 to 3 are examples of nickel powders produced by simulating the manufacturing environment of nickel powders in seasons other than summer. In the washing and filtration process, pure water adjusted to 16.9°C was used, and the time of exposure to the atmosphere of the nickel powder cake obtained after suction filtration and washing from the time of filtration in the filtration process to the start of drying in the drying process was 5 minutes (Reference Example 1), 15 minutes (Reference Example 2), and 25 minutes (Reference Example 3), and the temperature of exposure to the atmosphere was 23°C. The nickel crystallized powder (nickel powder) was obtained in the same manner as in Example 1. The nickel crystallized powder (nickel powder) was subjected to the same wet crushing treatment as in Example 1. The nickel powders according to Reference Examples 1 to 3 produced using a wet method were obtained by the above steps.
[0127] [Table 1]
[0128] In all the examples, the procedure for crystallizing the nickel powder was the same, and the number average particle size was the same.
[0129] In addition, since it is believed that the amount of nickel hydroxide increases due to the oxidation of nickel powder, the oxygen value is used as an index of the amount of nickel hydroxide, and an oxygen value of 3% or less is set as the acceptance criterion for nickel powder. Since the moisture content derived from nickel hydroxide is thought to be positively correlated with the amount of nickel hydroxide, it is thought to be a guideline for measuring the amount of coarse particles mainly composed of nickel hydroxide, and a moisture content derived from nickel hydroxide of 0.5% or less is set as the acceptance criterion for nickel powder. Therefore, the nickel powder of Comparative Example 2, which had an oxygen value exceeding 3% and a moisture content derived from nickel hydroxide exceeding 0.5%, was judged to be unsuccessful, and the content of coarse particles was not measured.
[0130] Reference Examples 1 to 3 are examples in which nickel powder was produced by simulating the nickel powder production environment in seasons other than summer, and are examples in which the conditions were known in advance to be capable of producing nickel powder with no abnormalities in physical properties. Because the temperature of the pure water used for washing was low and the temperature of exposure to the atmosphere was also low, it was possible to reproduce the ability to produce nickel powder with no abnormalities in physical properties under conditions in which the exposure time to the atmosphere was 5 to 25 minutes (Reference Examples 1 to 3).
[0131] Furthermore, when the temperature of the pure water used for cleaning was as high as 40°C and the temperature of exposure to the atmosphere was also as high as 40°C, the time of exposure to the atmosphere was 15 minutes or longer, and the amount of oxidized nickel powder increased, and the amount of nickel hydroxide produced also increased. As a result, the content of coarse particles with a particle size exceeding 0.4 μm exceeded 4000 ppm by mass, resulting in the production of a large amount of coarse particles (Comparative Examples 1 and 2).
[0132] However, even when the temperature of the pure water used for washing was as high as 40°C and the temperature of exposure to the atmosphere was also as high as 40°C, the nickel powder obtained by the method of Example 1 had a number average particle size, oxygen value, moisture content derived from nickel hydroxide, and content of coarse particles equivalent to those of Reference Examples 1 to 3 by shortening the exposure time to the atmosphere to 5 minutes. From these results, it was revealed that even in the summer when the temperature is high, by shortening the exposure time of the nickel powder cake to the atmosphere from after filtration to the start of drying, the oxidation of the nickel powder is unlikely to progress and nickel hydroxide (Ni(OH)2) is unlikely to grow, thereby suppressing the generation of coarse particles. [Explanation of symbols]
[0133] 1. Nickel particles (nickel crystallized powder) 2 Nickel hydroxide produced by oxidation of nickel crystal powder 10 Coarse particles mainly composed of nickel hydroxide
Claims
1. a washing and filtering step of washing and filtering the nickel crystallized powder in a nickel powder slurry containing nickel crystallized powder obtained by crystallizing the water-soluble nickel salt by a reduction reaction with the reducing agent in a reaction solution containing a water-soluble nickel salt, a metal salt of a metal nobler than nickel, a reducing agent, an alkali hydroxide, and water, using pure water at 25°C to 45°C to obtain a nickel powder cake; A drying step of drying the nickel powder cake to obtain nickel powder, A method for producing nickel powder, wherein the nickel powder cake is exposed to the atmosphere for a period of time from after filtration in the washing / filtration step until drying is started in the drying step, the period of time being kept to 10 minutes or less.
2. The method for producing nickel powder according to claim 1, wherein the moisture content of the nickel powder cake is 5% by mass or more and 70% by mass or less.
3. 3. The method for producing nickel powder according to claim 1, further comprising a crystallization step of crystallizing the nickel crystallized powder from the water-soluble nickel salt by a reduction reaction caused by the reducing agent in a reaction solution containing a water-soluble nickel salt, a metal salt of a metal more noble than nickel, a reducing agent, an alkali hydroxide, and water.
Citation Information
Patent Citations
Manufacture of hyperfine metallic powder
JP1985238406A
Nickel powder and method for manufacturing the same
JP2014189835A
Nickel powder and method for producing the same
JP2020100858A
Method of producing nickel powder
JP2020147802A
Production of globular-nickel superfine powder
JP1992365806A