Anomalous nernst effect material, thermoelectric conversion module, and heat flow sensor

The Fe3AlxGa1-x material with a specific composition range addresses the scalability and cost issues of thermoelectric conversion modules by providing efficient power generation in a cost-effective manner, suitable for large-area applications and film integration.

JP2024146186APending Publication Date: 2024-10-15THE UNIV OF TOKYO +1

Patent Information

Application Number
JP2023058935
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing thermoelectric conversion modules using the Seebeck effect face challenges in scalability, material rarity, and high manufacturing costs, while those utilizing the anomalous Nernst effect require expensive materials like Co, limiting their widespread adoption.

Method used

Development of an Fe3AlxGa1-x material with a composition formula where 0.25≦x≦0.60, which exhibits an absolute value of the anomalous Nernst coefficient of 5.0 μV/K or more under a 2T magnetic field at 300K, allowing for the creation of inexpensive and efficient thermoelectric conversion modules and heat flow sensors.

Benefits of technology

The proposed material and module design enable cost-effective power generation performance in the temperature range from room temperature to 100°C, facilitating large-area deployment and film integration with enhanced power generation efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146186000001_ABST
    Figure 2024146186000001_ABST
Patent Text Reader

Abstract

To provide an anomalous Nernst effect material which is inexpensive and has a high absolute value of anomalous Nernst coefficient.SOLUTION: An anomalous Nernst effect material is represented by a compositional formula of Fe3AlxGa1-x and satisfies 0.25<x<0.60.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an anomalous Nernst effect material, a thermoelectric conversion module, and a heat flow sensor. [Background technology]

[0002] Thermoelectric conversion modules are being actively developed to utilize unused thermal energy. Well-known thermoelectric conversion modules use the Seebeck effect, which can generate voltage from a temperature gradient.

[0003] In the Seebeck effect, a voltage is generated in the same direction as the temperature gradient, so a thermoelectric conversion module using the Seebeck effect has a complex three-dimensional structure. For this reason, it is difficult to make a thermoelectric conversion module using the Seebeck effect large-area or into a film. In addition, thermoelectric conversion modules using the Seebeck effect use rare materials, which poses the issue of high manufacturing costs.

[0004] In recent years, thermoelectric conversion modules using anomalous Nernst effect materials that generate electromotive force due to the anomalous Nernst effect have been proposed in addition to thermoelectric conversion modules that utilize the Seebeck effect. The anomalous Nernst effect is a phenomenon in which, when a temperature difference occurs due to a heat flow in a magnetic material, a voltage is generated in a direction perpendicular to both the magnetization direction and the temperature gradient.

[0005] The anomalous Nernst effect generates a voltage in a direction perpendicular to the temperature gradient. Therefore, a thermoelectric conversion module utilizing the anomalous Nernst effect has the advantage that it can be deployed along the heat source and can be easily made into a large area and a film.

[0006] For example, in Patent Document 1, the Fermi energy E F The thermoelectric conversion element is made of a ferromagnetic material having a band structure with a Weyl point in the vicinity of the ferromagnetic material and has a thermoelectric mechanism that generates an electromotive force by the anomalous Nernst effect.

Prior Art Documents

Patent Documents

[0007]

Patent Document 1

Summary of the Invention

Problems to be Solved by the Invention

[0008] Materials such as Co2MnGa disclosed in Patent Document 1 exhibit high power generation performance in the temperature range from room temperature to 100°C, but there is a problem that expensive raw materials such as Co are used. Therefore, there is a demand for a material that is inexpensive and exhibits high power generation performance in the temperature range from room temperature to 100°C.

[0009] The present invention has been made in view of the above circumstances, and an object thereof is to provide an anomalous Nernst effect material, a thermoelectric conversion module, and a heat flux sensor that are inexpensive and exhibit high power generation performance in the temperature range from room temperature to 100°C.

Means for Solving the Problems

[0010] In order to solve the above problems, the present invention proposes the following means. <1>The anomalous Nernst effect material according to Aspect 1 of the present invention is represented by the composition formula of Fe3Al x Ga 1-x satisfying 0.25 ≦ x ≦ 0.60, and the absolute value of the anomalous Nernst coefficient when a magnetic field of magnetic flux density 2T is applied under the temperature condition of 300K is 5.0 μV / K or more. <2>Aspect 2 of the present invention may satisfy 0.25 < x ≦ 0.45 in the anomalous Nernst effect material according to Aspect 1. <3>Aspect 3 of the present invention may be a polycrystal in the anomalous Nernst effect material according to Aspect 1 or Aspect 2. <4>Aspect 4 of the present invention may have a D03 structure in the polycrystal in the anomalous Nernst effect material according to Aspect 3. <5> A thermoelectric conversion module according to a fifth aspect of the present invention comprises the anomalous Nernst effect material according to any one of the first to fourth aspects, and the absolute value of the anomalous Nernst coefficient of the anomalous Nernst effect material when a magnetic field with a magnetic flux density of 2 T is applied at a temperature condition of 300 K is 5.0 μV / K or more. <6> A heat flow sensor according to a sixth embodiment of the present invention includes the thermoelectric conversion module according to the fifth embodiment. Effect of the Invention

[0011] According to the above-mentioned aspects of the present invention, it is possible to provide an anomalous Nernst effect material, a thermoelectric conversion module, and a heat flow sensor which are inexpensive and have a high absolute value of the anomalous Nernst coefficient. [Brief description of the drawings]

[0012] [Figure 1] 1 is a perspective view illustrating a schematic configuration of a thermoelectric conversion module according to a first embodiment. [Diagram 2] FIG. 1 is a schematic diagram showing the crystal structure of Fe3AlxGa1-x. [Diagram 3] FIG. 6 is a perspective view illustrating a schematic configuration of a thermoelectric conversion module according to a second embodiment. [Figure 4] FIG. 11 is a plan view showing the configuration of a thermoelectric conversion module according to a third embodiment. [Diagram 5] FIG. 11 is a perspective view illustrating a schematic configuration of a thermoelectric conversion module according to a fourth embodiment. [Figure 6] 1 shows XRD spectra of Comparative Example 1 (Fe3Ga0.25Al0.75), Example 6 (Fe3Ga0.50Al0.50), Example 1 (Fe3Ga0.75Al0.25), Fe3Ga, and Fe3Al. [Figure 7] 4 shows the anomalous Nernst coefficients of Examples 1 to 7 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] [First embodiment] Hereinafter, with reference to the drawings, a thermoelectric conversion module 100 according to an embodiment of the present invention will be described. FIG. 1 is a schematic diagram showing the configuration of the thermoelectric conversion module 100 according to the first embodiment. As shown in FIG. 1, the thermoelectric conversion module 100 includes an anomalous Nernst effect material 1, a first electrode 11, a second electrode 12, and a magnetic field applying means 20. Hereinafter, each part will be described.

[0014] (Anomalous Nernst effect material) In this embodiment, the anomalous Nernst effect material 1 is a mixed crystal of Fe3Al and Fe3Ga, Fe3Al x Ga 1-x represented by the composition formula of. In this specification, the anomalous Nernst effect material refers to a material in which the absolute value of the anomalous Nernst coefficient S ANE described later is 1.0 μV / K or more.

[0015] "Fe3Al x Ga 1-x " The anomalous Nernst effect material 1 is a mixed crystal of Fe3Al and Fe3Ga, Fe3Al x Ga 1-x represented by the composition formula of, and satisfies 0.25 ≦ x ≦ 0.60. More preferably, it preferably satisfies 0.25 < x ≦ 0.45. By the anomalous Nernst effect material satisfying 0.25 ≦ x ≦ 0.60, the content of inexpensive Al can be increased, and the absolute value of the anomalous Nernst coefficient of the anomalous Nernst effect material 1 can be made as high as that of Fe3Ga.

[0016] The anomalous Nernst effect material 1 is preferably a polycrystal of Fe3Al x Ga 1-x or a single crystal of Fe3Al x Ga 1-x . The anomalous Nernst effect material 1 is more preferably a polycrystal of Fe3Al x Ga 1-x . It is more preferable that the polycrystal of Fe3Al x Ga 1-x or the single crystal of Fe3Al x Ga 1-xThe anomalous Nernst effect material 1 has an anomalous Nernst coefficient S when a magnetic field of 300K and a magnetic flux density of 2T is applied. ANE As long as the absolute value of is 5.0 μV / K or more, the anomalous Nernst effect material 1 may contain other components.

[0017] "D03 structure" Anomalous Nernst effect material 1 is Fe3Al x Ga 1-x If the polycrystalline form is Fe3Al x Ga 1-x It is preferable that the anomalous Nernst effect material 1 has a D03 structure as shown in FIG. 2. When the anomalous Nernst effect material 1 is a polycrystalline material and has a D03 structure, the anomalous Nernst coefficient S ANE The absolute value of tends to be 5.0 μV / K or more. The unit cell of the D03 structure has eight body-centered cubic (bcc) type subcells. In each subcell, Fe atoms (Fe(II)) occupy the corner points, and each Fe(II) is shared by the eight adjacent subcells. Four of the eight subcells have four Fe atoms (Fe(I)) occupying the body center points, and the remaining four subcells have four X atoms (X atoms are Ga or Al) occupying the body center points. For example, Fe3Al in the D03 structure x Ga 1-x The lattice constant a of Fe3Al is 5.826 Å to 5.842 Å when 0.25≦x≦0.60. x Ga 1-x The lattice constants of can be derived from the XRD data.

[0018] The thickness of the anomalous Nernst effect material 1 is preferably 200 nm or more. By making the thickness 200 nm or more, an appropriate temperature difference can be easily formed in the temperature range from room temperature (for example, 20°C) to 100°C.

[0019] "The absolute value of the anomalous Nernst coefficient of the anomalous Nernst effect material when a magnetic field with a magnetic flux density of 2 T is applied at a temperature of 300 K is 5.0 μV / K or more." In this embodiment, the absolute value of the anomalous Nernst coefficient of the anomalous Nernst effect material 1 is 5.0 μV / K or more when a magnetic field with a magnetic flux density of 2 T is applied under a temperature condition of 300 K. Since the absolute value of the anomalous Nernst coefficient of the anomalous Nernst effect material 1 when a magnetic field of 2 T is applied is 5.0 μV / K or more, the thermoelectric conversion module 100 of the present disclosure can efficiently generate power in a temperature range from room temperature (e.g., 20°C) to 100°C.

[0020] "Anomalous Nernst coefficient S ANE " Anomalous Nernst coefficient S ANE is expressed by the following formula (1). yy means the longitudinal resistance. α in Equation (1) yx means the transverse thermoelectric coefficient. σ in Eq. (1) yx means the Hall conductivity. S in formula (1) SE means the Seebeck coefficient.

[0021] Transverse thermoelectric coefficient α yx is expressed by the following formula (2). Here, ∂σ in the following formula (2) yx / ∂ε is the value at the Fermi level. k in the following equation (2) B is the Boltzmann constant. In the following formula (2), ε means energy, and in the following formula (2), e means elementary charge. In the following formula (2), T means the absolute temperature (K) of the measurement sample.

[0022] S ANE =ρ yy α yx -σ yx ρ yy S SE (1) α yx =-(π 2 / 3)·{(k B 2 T) / e}(∂σ yx / ∂ε) (2)

[0023] "Method for measuring the anomalous Nernst coefficient" The anomalous Nernst coefficient S of the anomalous Nernst effect material 1 when a magnetic field with a magnetic flux density of 2 T is applied under the above-mentioned temperature condition of 300 K is ANE Specifically, is measured as follows: A sample is cut into a flat plate (length L: 7 mm, width W: 2 mm, thickness t: 1 mm). One longitudinal end of the cut sample is heated with a heater (temperature 300 K), and the other longitudinal end is brought into contact with a heat sink, creating a temperature difference along the side L of the sample. A uniform temperature gradient is given to the rectangular sample, and the temperature difference ΔT (K) is measured at two points separated by L_temp (mm). A magnetic field is applied in a direction perpendicular to this temperature difference, and the voltage (V) generated at two points separated by a distance W (mm) in a direction perpendicular to both the temperature difference and the magnetic field is measured. Anomalous Nernst coefficient S ANE is calculated from the obtained voltage (V) and other information using the following formula (3).

[0024] S ANE =(V / ΔT)×(L_temp / W)···(3)

[0025] (1st electrode 11) In the thermoelectric conversion module 100, the first electrode 11 is electrically connected to the anomalous Nernst effect material 1. The material of the first electrode is not particularly limited as long as it has electrical conductivity. For example, the material of the first electrode may be metals such as Au, Ag, Cu, and Al.

[0026] (2nd electrode 12) In the thermoelectric conversion module 100, the second electrode 12 is electrically connected to the anomalous Nernst effect material 1. The material of the second electrode is not particularly limited as long as it has electrical conductivity. For example, the material of the second electrode may be metals such as Au, Ag, Cu, and Al.

[0027] There is no particular limitation on the arrangement of the first electrode 11 and the second electrode 12. However, if there is a difference in temperature between the first electrode 11 and the second electrode 12, the Seebeck effect will be superimposed in addition to the anomalous Nernst effect, so for the heat flow sensor, it is preferable that the first electrode 11 and the second electrode 12 are arranged so that they are the same distance from the heat source.

[0028] (Magnetic field application means 20) The magnetic field application means 20 is not particularly limited as long as it can apply a magnetic field in a direction perpendicular to the direction in which the temperature difference occurs and the direction in which the electromotive force is generated (the direction connecting the electrodes 11 and 12). Examples of the magnetic field application means 20 include a permanent magnet and an electromagnet.

[0029] (Thermoelectric Conversion Using Thermoelectric Conversion Module 100) 1, the thermoelectric conversion module 100 of this embodiment has a rectangular parallelepiped anomalous Nernst effect material 1 extending in one direction (Y direction in this embodiment), has a thickness of 0.1 μm or more in the thickness direction (X direction in this embodiment), and is magnetized in the +X direction. A magnetic field is applied by magnetic field application means 20. A known method can be used for applying the magnetic field.

[0030] When a heat flow Q flows in a direction (+Z direction in this embodiment) perpendicular to the direction of magnetization M (+X direction) through the anomalous Nernst effect material 1 of this embodiment, a temperature difference ΔT occurs in the +Z direction.

[0031] As a result, in the anomalous Nernst effect material 1, an electromotive force is generated in a direction (Y direction in this embodiment) perpendicular to both the direction of the heat flow Q (+Z direction) and the direction of the magnetization M (+X direction) due to the anomalous Nernst effect. As a result, the anomalous Nernst effect material 1 of this embodiment is capable of performing thermoelectric conversion.

[0032] (Method of manufacturing anomalous Nernst effect material 1) Anomalous Nernst effect material 1 is Fe3Al x Ga 1-xThe manufacturing method of the anomalous Nernst effect material 1 will be described using the polycrystalline Fe3Al as an example. x Ga 1-x The polycrystalline body of can be produced, for example, by the following method. Fe, Ga, and Al in an appropriate ratio are placed in a mono-arc furnace (step 1). A vacuum is drawn using a rotary pump and a turbo molecular pump until the ultimate pressure reaches 0.2 Pa, and then Ar purging is performed three times. Then, argon gas is filled into the furnace until the pressure reaches 0.08 MPa, and arc discharge is started (step 2). After step 2, an arc discharge is performed under a condition of 4 amperes to melt the metal, and the molten state is maintained for 10 to 15 seconds (step 3). After waiting about 1 minute after step 3, the top and bottom surfaces of the obtained metal material are inverted (step 4). The process from step 2 to step 4 is repeated 6 to 7 times. Using this procedure, Fe3Al having a D03 structure is obtained. x Ga 1-x The Fe3Al polycrystalline body obtained by the above-mentioned manufacturing method can be produced. x Ga 1-x The polycrystalline body has an anomalous Nernst coefficient of 5.0 μV / K or more as an absolute value of the anomalous Nernst effect material when a magnetic field with a magnetic flux density of 2 T is applied. Therefore, the thermoelectric conversion module of the present disclosure exhibits excellent power generation characteristics when used in a temperature range from room temperature to 100° C. or less.

[0033] The above describes the thermoelectric conversion module 100 according to the first embodiment. Since the anomalous Nernst effect material 1 in the thermoelectric conversion module 100 contains Fe and Al, the thermoelectric conversion module 100 is inexpensive and suitable for use in a temperature range from room temperature to 100° C. or lower.

[0034] Although the thermoelectric conversion module 100 includes the magnetic field application means 20, the thermoelectric conversion module 100 does not necessarily need to include the magnetic field application means 20.

[0035] Second Embodiment Next, a thermoelectric conversion module 100A according to the second embodiment will be described. Fig. 3 is a schematic diagram of the thermoelectric conversion module 100A.

[0036] As shown in FIG. 3, the thermoelectric conversion module 100A includes a substrate 30 and a power generating body 40 disposed on the substrate 30. As shown in FIG.

[0037] (Substrate 30) The substrate 30 has a first surface 30a on which the power generating body 40 is disposed, and a second surface 30b opposite to the first surface 30a. For example, the second surface 30b receives heat from a heat source (not shown). The material of the substrate 30 is not particularly limited. The material of the substrate 30 is preferably one having high thermal conductivity. Examples of the material of the substrate 30 include AlN, Al2O3, MgO, and BN.

[0038] (1st electrode 11A) In the thermoelectric conversion module 100A, the first electrode 11A is electrically connected to one end of the power generation body 40. The material of the first electrode is not particularly limited as long as it has electrical conductivity. For example, the material of the first electrode may be metals such as Au, Ag, Cu, and Al.

[0039] (2nd electrode 12A) In the thermoelectric conversion module 100A, the second electrode 12A is electrically connected to the other end of the power generation body 40. The material of the second electrode is not particularly limited as long as it has electrical conductivity. For example, the material of the second electrode may be a metal such as Au, Ag, Cu, or Al.

[0040] (Power Generator 40) The power generating body 40 has one or more first anomalous Nernst effect materials 41 and one or more second anomalous Nernst effect materials 42. The first anomalous Nernst effect materials 41 and the second anomalous Nernst effect materials 42 may be the same as the anomalous Nernst effect material 1 described above.

[0041] One or more first anomalous Nernst effect materials 41 and one or more second anomalous Nernst effect materials 42 extend in one direction (here, the Y direction) within the plane of the first surface 30a and are arranged alternately in another direction (here, the X direction) that intersects with this one direction (orthogonal in the second embodiment).

[0042] The first anomalous Nernst effect material 41 has a first connection portion 41a protruding from one end (end on the +Y side) in one direction (Y direction) toward one side (-X side) in the other direction (X direction). On the other hand, the second anomalous Nernst effect material 42 has a second connection portion 42a protruding from the other end (end on the -Y side) in the one direction (Y direction) toward one side (-X side) in the other direction (X direction).

[0043] The first anomalous Nernst effect material 41 is electrically connected to one end (end on the +Y side) in one direction (Y direction) of the second anomalous Nernst effect material 42 via a first connection portion 41a. On the other hand, the second anomalous Nernst effect material 42 is electrically connected to the other end (end on the -Y side) of the first anomalous Nernst effect material 41 via a second connection portion 42a.

[0044] As a result, in the power generating body 40, the first anomalous Nernst effect material 41 and the second anomalous Nernst effect material 42 adjacent to each other are electrically connected in series, so that the power generating body 40 has a meandering shape.

[0045] The power generating body 40 and the first anomalous Nernst effect material 41 are arranged such that the direction of magnetization M1 (-X direction in the second embodiment) is opposite to the direction of magnetization M2 (+X direction in the second embodiment) of the second anomalous Nernst effect material 42. Furthermore, both the first anomalous Nernst effect material 41 and the second anomalous Nernst effect material 42 have negative anomalous Nernst coefficients.

[0046] In the thermoelectric conversion module 100A, when a heat flow Q flows from the second surface 30b side of the substrate 30 toward the power generator 40, a temperature difference occurs in the power generator 40 in the direction of the heat flow, and a voltage V is generated in the power generator 40 due to the anomalous Nernst effect.

[0047] When the second surface 30b of the substrate 30 receives heat from the heat source, a heat flow Q flows in the +Z direction toward the power generator 40. At this time, in the first anomalous Nernst effect material 41, an electromotive force E1 is generated in a direction (+Y direction) perpendicular to both the direction of the magnetization M1 (-X direction) and the direction of the heat flow Q (+Z direction). On the other hand, in the second anomalous Nernst effect material 42, an electromotive force E2 is generated in a direction (-Y direction) perpendicular to both the direction of the magnetization M2 (+X direction) and the direction of the heat flow Q (+Z direction).

[0048] In the power generating body 40, the first anomalous Nernst effect material 41 and the second anomalous Nernst effect material 42 adjacent to each other are electrically connected in series. Therefore, the electromotive force E1 generated in the first anomalous Nernst effect material 41 and the electromotive force E2 generated in the second anomalous Nernst effect material 42 are added together, and the output voltage V can be increased.

[0049] In the thermoelectric conversion module 100A of the present embodiment, the temperature gradient, the magnetization direction, and the voltage direction are perpendicular to each other, so that it is possible to use the first anomalous Nernst effect material 41 and the second anomalous Nernst effect material 42 in thin sheet form.

[0050] Here, assuming that the length in the longitudinal direction (extension direction) of the first anomalous Nernst effect material 41 and the second anomalous Nernst effect material 42 is L1 and the thickness (height) is H1, when the temperature difference in the first anomalous Nernst effect material 41 and the second anomalous Nernst effect material 42 is constant, the voltage V generated by the anomalous Nernst effect is proportional to L1 / H1. In other words, the longer and thinner the first anomalous Nernst effect material 41 and the second anomalous Nernst effect material 42 are, the larger the obtained voltage V becomes.

[0051] Third Embodiment Next, a thermoelectric conversion module 100B according to a third embodiment will be described. Fig. 4 is a plan view of the thermoelectric conversion module 100B. The thermoelectric conversion module 100B includes a substrate 30 and a power generation body 40B disposed on the substrate 30.

[0052] (Power generating body 40B) The power generating body 40B has a plurality of anomalous Nernst effect materials 45 and wiring 50.

[0053] "Abnormal Nernst effect material 45" The anomalous Nernst effect material 45 may be made of the same material as the anomalous Nernst effect material 1. The anomalous Nernst effect materials 45 are arranged in parallel on the substrate 30 in a direction (X direction) perpendicular to the extension direction (Y direction) so that the directions of the magnetization M1A are the same (-X direction).

[0054] "Wiring 50" In the thermoelectric conversion module 100B, one end of the wiring 50 is electrically connected to one end side (-Y side) of the anomalous Nernst effect material 45, and the other end is electrically connected to the other end side (+Y side) of another adjacent anomalous Nernst effect material 45. This electrically connects the anomalous Nernst effect materials 45 in series. The material of the wiring 50 is not particularly limited as long as it has conductivity. For example, the material of the wiring 50 may be metal such as Au, Ag, Cu, or Al.

[0055] The heat flow Q flows from the substrate 30 side to the power generating body 40B side (flows in the +Z direction). The thermoelectric conversion module 100B can be manufactured more easily than the thermoelectric conversion module 100A because the adjacent anomalous Nernst effect materials 45 are connected via the wiring 50.

[0056] [Fourth embodiment] Next, a thermoelectric conversion module 100C according to a fourth embodiment will be described. Fig. 5 is a schematic diagram showing the configuration of the thermoelectric conversion module 100C.

[0057] 5, the thermoelectric conversion module 100C includes a substantially cylindrical hollow member 31 and a long sheet-like anomalous Nernst effect material 32 spirally wound around the outer circumferential surface of the hollow member 31. The anomalous Nernst effect material 32 may be the same as the anomalous Nernst effect material 1. The anomalous Nernst effect material 32 is magnetized in a direction parallel to the axial direction (X direction) of the hollow member 31.

[0058] In the thermoelectric conversion module 100C, when the inside of the hollow member 31 is hotter than the outside, the heat flow P flows from the inside to the outside of the hollow member 31, and a temperature gradient (temperature difference) occurs from the inside to the outside of the hollow member 31. In this embodiment, an electromotive force is generated along the longitudinal direction of the anomalous Nernst effect material 32 (the direction perpendicular to both the magnetization direction and the heat flow direction).

[0059] In the thermoelectric conversion module 100C of this embodiment, the temperature gradient, the magnetization direction, and the voltage direction are perpendicular to each other, so that it is possible to use a thin sheet-like anomalous Nernst effect material 32.

[0060] Therefore, as shown in formula (4), the electromotive force generated by the anomalous Nernst effect increases as the length of the anomalous Nernst effect material increases. In the thermoelectric conversion module 100C of this embodiment, the long sheet-like anomalous Nernst effect material 32 is wound in a spiral shape around the outer circumferential surface of the hollow member 31 described above. This makes it possible to increase the length of the anomalous Nernst effect material, and a further increase in the voltage V can be expected.

[0061] The present invention is not limited to the configurations of the above-described embodiments, and various modifications can be made without departing from the spirit of the present invention. For example, the above-mentioned thermoelectric conversion modules 100, 100A, 100B, and 100C can be applied to various devices. For example, by providing the thermoelectric conversion modules 100, 100A, 100B, and 100C in a heat flow sensor, it is possible to determine whether the thermal insulation performance of a building is good or bad.

[0062] In addition, by installing thermoelectric conversion modules 100, 100A, 100B, and 100C in an exhaust device of a motorcycle or the like, electricity can be generated by utilizing the heat (waste heat) of the exhaust gas, and the thermoelectric conversion modules 100, 100A, 100B, and 100C can be effectively used as auxiliary power sources.

[0063] Furthermore, the thermoelectric conversion modules 100, 100A, 100B, and 100C of the present embodiment can be provided with not only the function as the thermoelectric conversion element described above, but also the function of temperature modulation (particularly cooling) by supplying electric power, like a Peltier element. EXAMPLES

[0064] The effects of the present invention will be more clearly understood by the following examples. Note that the present invention is not limited to the following examples, and can be modified as appropriate without departing from the spirit and scope of the present invention.

[0065] Example 1 Fe3Al 0.25 Ga 0.75 The raw materials were melted in a mono-arc furnace so that the composition ratio was as follows: the melted state was maintained for 10-15 seconds, and then the material was cooled for about 1 minute. The upper and lower surfaces of the resulting metal material were then inverted. This procedure was repeated 6-7 times to produce the anomalous Nernst effect material of Example 1.

[0066] Example 2 Fe3Al 0.30 Ga 0.70 The raw materials were melted in a mono-arc furnace so that the composition ratio was as follows: the melted state was maintained for 10-15 seconds, and then the material was cooled for about 1 minute. The upper and lower surfaces of the resulting metal material were then inverted. This procedure was repeated 6-7 times to produce the anomalous Nernst effect material of Example 2.

[0067] Example 3 Fe3Al 0.35 Ga 0.65 The raw materials were melted in a mono-arc furnace so that the composition ratio was as follows: the melted state was maintained for 10-15 seconds, and then the material was cooled for about 1 minute. The upper and lower surfaces of the resulting metal material were then inverted. This procedure was repeated 6-7 times to produce the anomalous Nernst effect material of Example 3.

[0068] Example 4 Fe3Al 0.40 Ga 0.60The raw materials were melted in a mono-arc furnace so that the composition ratio was as follows: the melted state was maintained for 10-15 seconds, and then the material was cooled for about 1 minute. The upper and lower surfaces of the resulting metal material were then inverted. This procedure was repeated 6-7 times to produce the anomalous Nernst effect material of Example 4.

[0069] Example 5 Fe3Al 0.45 Ga 0.55 The raw materials were melted in a mono-arc furnace so that the composition ratio was as follows: the melted state was maintained for 10-15 seconds, and then the material was cooled for about 1 minute. The upper and lower surfaces of the resulting metal material were then inverted. This procedure was repeated 6-7 times to produce the anomalous Nernst effect material of Example 5.

[0070] Example 6 Fe3Al 0.50 Ga 0.50 The raw materials were melted in a Monoark furnace so as to obtain the composition ratio of the above, and the melted state was maintained for 10-15 seconds, after which the material was cooled for about 1 minute, and the upper and lower surfaces of the obtained metal material were inverted. This procedure was repeated 6-7 times to produce the anomalous Nernst effect material of Example 6.

[0071] Example 7 Fe3Al 0.60 Ga 0.40 The raw materials were melted in a mono-arc furnace so that the composition ratio was as follows: the melted state was maintained for 10-15 seconds, and then the material was cooled for about 1 minute. The upper and lower surfaces of the resulting metal material were then inverted. This procedure was repeated 6-7 times to produce the anomalous Nernst effect material of Example 7.

[0072] Comparative Example 1 Fe3Al 0.75 Ga 0.25 The raw materials were melted in a mono-arc furnace so that the composition ratio was as follows: the melted state was maintained for 10-15 seconds, and then the material was cooled for about 1 minute. The upper and lower surfaces of the resulting metal material were then inverted. This procedure was repeated 6-7 times to produce the anomalous Nernst effect material of Comparative Example 1.

[0073] (XRD) XRD measurements of the anomalous Nernst effect materials of Examples 1 to 7 and Comparative Example 1 were carried out using a Rigaku Smart-Lab device. XRD measurements were carried out by crushing the materials into powder, filling them in a holder, and measuring them. Similarly, measurements were also carried out on polycrystalline Fe3Ga and Fe3Al.

[0074] (Anomalous Nernst coefficient) The anomalous Nernst coefficient was calculated as follows. A flat sample (L=7mm, W=2mm, t=1mm) for evaluation was cut out from the anomalous Nernst effect material. One end of the sample was heated with a heater (300K) and the other end was contacted with a heat sink, creating a temperature difference along the edge L of the sample. Thermocouples were placed at two points separated by L_temp (1-4mm) on the sample to measure the temperature difference ΔT. A magnetic field with a magnetic flux density of 2T was applied in a direction perpendicular to this temperature difference and perpendicular to the surface of the flat sample. The voltage V generated at two points separated by a distance W was measured in a direction perpendicular to both the temperature difference and the magnetic field. The anomalous Nernst coefficient was calculated based on the above formula (3) from the voltage when a magnetic field of 2T was applied.

[0075] The results of the XRD measurement are shown in Figure 6. The horizontal axis of Figure 6 is 2θ (°) and the vertical axis is intensity. From the XRD spectrum in Figure 6, it was confirmed that the anomalous Nernst effect materials of Examples 1 to 7 and Comparative Example 1 were polycrystalline and had a crystal structure of D03.

[0076] The measurement results of the anomalous Nernst coefficient of the anomalous Nernst effect material obtained above are shown in Table 1 and Fig. 7. As shown in Table 1 and Fig. 7, the anomalous Nernst effect materials of Examples 1 to 7 had absolute values ​​of the anomalous Nernst coefficient of 5 μV / K or more at 300 K. Therefore, it was found that the thermoelectric conversion modules using the anomalous Nernst effect materials of Examples 1 to 7 exhibited excellent power generation performance in the range from room temperature to 100°C. On the other hand, Comparative Example 1, which did not satisfy 0.25≦x≦0.60, had an absolute value of the anomalous Nernst coefficient of less than 5.0 μV / K even though the crystal structure was D03.

[0077] [Table 1] [Explanation of symbols]

[0078] 1 anomalous Nernst effect material, 11 first electrode, 12 second electrode, 20 magnetic field application means, 100 thermoelectric conversion module

Claims

1. Fe 3 A x G 1-x wherein the composition formula is represented by the formula: and 0.25≦x≦0.60 is satisfied, and the absolute value of the anomalous Nernst coefficient when a magnetic field with a magnetic flux density of 2 T is applied at a temperature condition of 300K is 5.0 μV / K or more.

2. The anomalous Nernst effect material according to claim 1 , wherein 0.25<x≦0.45 is satisfied.

3. 2. The anomalous Nernst effect material of claim 1, which is polycrystalline.

4. The polycrystalline body is D0 3 4. The anomalous Nernst effect material of claim 3, which has a structure.

5. The anomalous Nernst effect material according to any one of claims 1 to 4 is provided, A thermoelectric conversion module, wherein the absolute value of the anomalous Nernst coefficient of the anomalous Nernst effect material when a magnetic field with a magnetic flux density of 2 T is applied at a temperature condition of 300 K is 5.0 μV / K or more.

6. A heat flow sensor comprising the thermoelectric conversion module according to claim 5 .

Citation Information

Patent Citations

  • Thermoelectric conversion element and thermoelectric conversion device

    EP3961733A1

  • Thermoelectric conversion element and thermoelectric conversion device

    US20220246820A1

  • Thermoelectric conversion element and thermoelectric conversion device

    WO2020218613A1

  • Thermoelectric conversion element

    WO2023013702A1

  • Thermoelectric conversion element and thermoelectric conversion device

    WO2019009308A1

Cited By

  • Magnetic domain detection method using light-induced abnormal Nernst effect

    CN119716684A