Resin fine particle

Resin fine particles with tailored storage modulus and molecular weight characteristics enhance image durability in water-based inks for inkjet printing on low or non-ink-absorbing media, addressing issues of bending and blocking resistance.

JP2024146214AInactive Publication Date: 2024-10-15NIPPON KAYAKU CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023058989
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Water-based inks used in inkjet printing on low or non-ink-absorbing media face challenges with image durability due to slow film formation of fine resin particles, leading to issues with image bending resistance and blocking resistance.

Method used

Development of resin fine particles with specific storage modulus ranges (1.0×10^4 Pa to 1.0×10^8 Pa) and molecular weight characteristics, combined with acrylic and acrylic styrene resins, to enhance film formation and durability.

Benefits of technology

The resin fine particles provide inkjet inks with improved image bending resistance and blocking resistance, ensuring high-quality printed films with good folding and blocking properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146214000001
    Figure 2024146214000001
  • Figure 2024146214000002
    Figure 2024146214000002
Patent Text Reader

Abstract

To provide resin fine particles with enhanced image bending resistance and blocking resistance, and to provide inkjet ink.SOLUTION: Resin fine particles include at least any resin selected from a group consisting of an acrylic resin and an acrylic styrene resin. The resin fine particles have a storage modulus G1 of 1.0×104 Pa or more and 1.0×108 Pa or less at 20°C as determined by a dynamic viscoelasticity measurement method. The resin fine particles have a storage modulus G2 of 1.0×104 Pa or less at 70°C as determined by the dynamic viscoelasticity measurement method.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to resin fine particles. [Background technology]

[0002] Among various color recording methods, the recording method using an inkjet printer (inkjet recording method), which is one of the most representative methods, generates small droplets of ink and deposits them on a printing medium such as paper to perform recording. In recent years, demand has increased for commercial and industrial applications, and there is a demand for inks that can be printed on a variety of printing media.

[0003] In commercial fields such as catalogs and pamphlets, printing media with lower ink absorption than plain paper (hereinafter also referred to as "low-ink-absorbency media"), such as coated paper and art paper, are often used. In industrial fields such as outdoor signage and soft food packaging, printing media with low ink absorption (hereinafter also referred to as "low-ink-absorbency media"), such as polyvinyl chloride film, PET (polyethylene terephthalate) film, and polyolefin film, are often used.

[0004] For poorly ink-absorbent media and non-ink-absorbent media, development has been promoted of solvent inks using organic solvents as the main solvent, curable inks containing polymerizable monomers, etc. However, these inks have many safety issues for the natural environment and the human body. Therefore, in recent years, development of water-based inks using water as the main solvent has become more active.

[0005] Since water-based inks do not use polymerizable monomers, resin particles are generally used as a binder to ensure the quality of image durability. However, particles dispersed in water are slow to form a film when dried, and the particles need to be fused together, which tends to reduce image durability compared to polymerizable monomers, and various methods have been used to improve image durability. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2014-65826 A [Patent Document 2] JP 2017-88850 A Summary of the Invention [Problem to be solved by the invention]

[0007] An object of the present invention is to provide resin fine particles and an ink-jet ink that are excellent in image folding resistance and blocking resistance. [Means for solving the problem]

[0008] As a result of intensive research conducted by the present inventors to solve the above problems, the present inventors have discovered a resin microparticle containing at least one resin selected from the group consisting of an acrylic resin and an acrylic styrene resin, the resin microparticle having a storage modulus G1 at 20° C. as measured by a dynamic viscoelasticity measurement method of 1.0×10 4 Pa or more 1.0×10 8 The storage modulus G2 of the resin fine particles at 70°C as measured by a dynamic viscoelasticity measurement method is 1.0 x 10 4 The present invention has been completed based on the discovery that resin fine particles having a viscosity of 100 Pa or less can solve the above problems.

[0009] That is, the present invention relates to the following 1) to 5). 1) Resin fine particles containing at least one resin selected from the group consisting of an acrylic resin and an acrylic styrene resin, the resin fine particles having a storage modulus G1 at 20° C. as measured by a dynamic viscoelasticity measurement method of 1.0×10 4 Pa or more 1.0×10 8 The storage modulus G2 of the resin fine particles at 70°C as measured by a dynamic viscoelasticity measurement method is 1.0 x 10 4 Resin particles characterized by a viscosity of 0.01 Pa or less. 2) 1) The resin fine particles according to 1), wherein the acid value of the resin fine particles is 10 to 120 mgKOH / g. 3) The resin fine particles according to 1) or 2), wherein the relationship between the acid value and the hydroxyl value of the resin fine particles satisfies the condition that the value calculated by acid value / hydroxyl value is in the range of 0.5 to 2.0. 4) The resin fine particles according to any one of 1) to 3), wherein the average particle diameter of the resin fine particles is in the range of 20 to 400 nm. 5) The resin fine particles according to any one of 1) to 4), containing monomers having C4 to C19 side chain components in an amount of 50 to 90% by mass relative to 100% by total mass of constituent monomers of the resin fine particles. Effect of the Invention

[0010] The present invention provides an ink having excellent image folding resistance and blocking resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, specific embodiments to which the present invention is applied will be described in detail. In this specification, "CI" means "color index." "(Meth)acrylic" is used to mean both "acrylic" and "methacrylic." The same applies to "(meth)acrylate." In addition, the above resin fine particles may be abbreviated to resin fine particles or fine particles.

[0012] <Resin fine particles> The resin microparticles according to the present embodiment contain at least one resin selected from the group consisting of acrylic resins and acrylic styrene resins, and the storage modulus G1 of the resin microparticles at 20° C. as measured by a dynamic viscoelasticity measurement method is 1.0×10 4 Pa or more 1.0×10 8 The storage modulus G2 of the resin fine particles at 70°C as measured by a dynamic viscoelasticity measurement method is 1.0 x 10 4 It is characterized in that the tensile strength is less than or equal to Pa.

[0013] <Resin> The acrylic resin and the acrylic styrene resin are resins obtained from radical polymerizable monomers. The acrylic resin is a resin obtained by radical polymerization of (meth)acrylic acid or (meth)acrylic acid ester monomers, and examples thereof include methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, stearyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, lauryl methacrylate, 2-ethylhexyl methacrylate, and stearyl methacrylate. In particular, (meth)acrylic acid having C4 to C19 is preferable. The acrylic styrene resin is a resin obtained by radical polymerization of the acrylic acid esters and styrenes, and examples of the styrenes include styrene, parachlorostyrene, and α-methylstyrene. In particular, styrene and α-methylstyrene are preferable. In addition, an acid value-imparting monomer or a hydroxyl group-imparting monomer may be copolymerized. Examples of the acid value-imparting monomer include acrylic acid, methacrylic acid, carboxyethyl acrylate, and carboxypropyl acrylate. The acid value of the resin fine particles is preferably 5 to 150 mgKOH / g, more preferably 10 to 120 mgKOH / g, and even more preferably 15 to 100 mgKOH / g from the viewpoint of particle stability. Examples of the hydroxyl group-imparting monomer include 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, and hydroxybutyl methacrylate. From the viewpoint of polymerizability, 2-hydroxyethyl methacrylate or (meth)acrylic acid esters having a hydroxyl group chain length of C3 to C5 are preferable. In addition, when the resin fine particles have hydroxyl groups, it is preferable that the relationship between the acid value and the hydroxyl value satisfies the condition that the value calculated by acid value / hydroxyl value falls within the range of 0.5 to 2.0. The hydroxyl value refers to the number of milligrams of potassium hydroxide required to neutralize acetic acid bonded to hydroxyl groups when 1 g of a sample is acetylated, and is measured according to JIS K0070.

[0014] <Storage modulus G1, G2> In this embodiment, the storage moduli G1 and G2 are measured by a sine wave vibration method using an ARES-GII measuring device manufactured by TA Instruments. The resin fine particles for inkjet are freeze-dried and powdered as a sample for measurement. The powder is compressed and solidified to form a pellet of about 0.5 g to be used as a sample. The sample is sandwiched between parallel plates with a diameter of 8 mm, and heat of 30°C to 120°C is applied to adhere to the parallel plates. The sample adhered to the parallel plates is cooled to 10°C and held at 10°C for 1 minute. The sample is then heated from 30°C to 90°C at a heating rate of 2°C / min. During this time, sine wave vibration is applied at a frequency of 1 Hz continuously from the point when the sample temperature reaches 10°C. Based on the results, the storage modulus at 30°C is defined as G1, and the storage modulus at 70°C is defined as G2. The G1 of the above resin particles is 7.0×10 4 Pa or more 1.0×10 7 It is preferable that the pressure is 0.1 Pa or less. The G2 of the above resin particles is 1.0×10 3 Pa or less is preferable.

[0015] By setting the storage modulus G1 and G2 of the resin fine particles to the above ranges, it is possible to provide an inkjet ink having excellent image folding resistance and blocking properties. 8 Pa or less and G2 is 1.0×10 4 When the pressure is lower than Pa, a printed film with good image folding properties is obtained. That is, the printed film stretches and conforms to the substrate when the image is folded, resulting in good folding properties. On the other hand, G1 is 1.0×10 4 When the resistivity is equal to or higher than Pa, a printing film having good blocking properties can be obtained.

[0016] The average particle size of the resin fine particles is not particularly limited, but is preferably in the range of 20 to 400 nm, and more preferably in the range of 50 to 250 nm.

[0017] Examples of methods for obtaining the resin microparticles include a method in which synthesis and microparticle formation are carried out simultaneously in a resin emulsion state dispersed in water as a dispersion medium, such as an emulsion polymerization method or a suspension polymerization method, a method in which a resin is synthesized in advance, dissolved in a solvent, and then emulsified using a surfactant, such as a phase inversion emulsification method or a suspension emulsification method, or a method in which a surfactant is added to a thermally melted mixture, kneaded, and then water is added to the mixture, and the like. These methods may be used alone or in combination of two or more types of resin particles.

[0018] The present invention also includes an inkjet ink (hereinafter sometimes abbreviated to "ink") containing the above-mentioned resin microparticles, an ink set containing a plurality of such inks, an ink set containing such ink and other inks, a printed matter obtained using such ink, and a printing method for obtaining a printed matter using such ink.

[0019] The inkjet ink containing the resin fine particles may further contain a colorant in addition to the resin fine particles. The colorant is not particularly limited, but examples thereof include pigments and disperse dyes.

[0020] The ink may contain a colorant. The colorant is not particularly limited, but examples thereof include pigments and disperse dyes.

[0021] Examples of the pigment include inorganic pigments, organic pigments, extender pigments, hollow particles, and the like. Examples of inorganic pigments include carbon black, metal oxides, metal hydroxides, metal sulfides, metal ferrocyanides, and metal chlorides.

[0022] When the ink according to the present embodiment is a black ink and the colorant is an inorganic pigment, the inorganic pigment contained in the black ink is preferably carbon black such as thermal black, acetylene black, oil furnace black, gas furnace black, lamp black, gas black, channel black, etc. Specific examples of carbon black include the Raven series manufactured by Columbia Carbon Co., the Monarch series, Regal series, and Mogul series manufactured by Cabot Corporation, the HiBlack series, ColorBlack series, Printex series, SpecialBlack series, and Nerox series manufactured by Orion Engineered Carbons, and the MA series, MCF series, No. 25, No. 33, No. 40, No. 47, No. 52, No. 900, and No. 2300 manufactured by Mitsubishi Chemical Corporation.

[0023] When the ink according to the present embodiment is a white ink and the colorant is an inorganic pigment, examples of the inorganic pigment contained in the white ink include oxides, nitrides, and oxynitrides of metals such as zinc, silicon, aluminum, titanium, strontium, and zirconium; inorganic compounds such as glass and silica; etc. Among these, titanium dioxide and zinc oxide are preferred.

[0024] Examples of organic pigments include various pigments such as azo, disazo, phthalocyanine, quinacridone, isoindolinone, dioxazine, perylene, perinone, thioindigo, anthraquinone, and quinophthalone.

[0025] Specific examples of organic pigments include yellow pigments such as CI Pigment Yellow 1, 2, 3, 12, 13, 14, 16, 17, 24, 55, 73, 74, 75, 83, 93, 94, 95, 97, 98, 108, 114, 128, 129, 138, 139, 150, 151, 154, 155, 180, 185, 193, 199, 202, and 213; Red pigments such as 5, 7, 12, 48, 48:1, 57, 88, 112, 122, 123, 146, 149, 150, 166, 168, 177, 178, 179, 184, 185, 202, 206, 207, 254, 255, 257, 260, 264, 269, 272; blue pigments such as CI Pigment Blue 1, 2, 3, 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 22, 25, 60, 66, 80; violet pigments such as CI Pigment Violet 19, 23, 29, 37, 38, 50; orange pigments such as CI Pigment Orange 13, 16, 43, 68, 69, 71, 73; CI Pigment Green 7, 36, 54, and other green pigments; and CI Pigment Black 1, and other black pigments. Among these, CI Pigment Blue 15:4 is preferred.

[0026] Examples of the extender pigment include silica, calcium carbonate, talc, clay, barium sulfate, white carbon, etc. The extender pigment is often used in combination with other colorants.

[0027] As the hollow particles, known hollow particles described in, for example, U.S. Pat. No. 4,880,465, Japanese Patent No. 3,562,754, Japanese Patent No. 6,026,234, Japanese Patent No. 5,459,460, JP-A-2003-268694, Japanese Patent No. 4,902,216, etc. can be used, and they are particularly preferably used as white pigments.

[0028] As disperse dyes, for example, dyes selected from CI Dispers are preferred. Specific examples thereof include yellow dyes such as CI Dispers Yellow 9, 23, 33, 42, 49, 54, 58, 60, 64, 66, 71, 76, 79, 83, 86, 90, 93, 99, 114, 116, 119, 122, 126, 149, 160, 163, 165, 180, 183, 186, 198, 200, 211, 224, 226, 227, 231, and 237; red dyes such as CI Dispers Red 60, 73, 88, 91, 92, 111, 127, 131, 143, 145, 146, 152, 153, 154, 167, 179, 191, 192, 206, 221, 258, and 283; and CI Dispers Orange. Orange dyes such as 9, 25, 29, 30, 31, 32, 37, 38, 42, 44, 45, 53, 54, 55, 56, 61, 71, 73, 76, 80, 96, 97, etc.; violet dyes such as CI Dispers Violet 25, 27, 28, 54, 57, 60, 73, 77, 79, 79:1, etc.; blue dyes such as CI Dispers Blue 27, 56, 60, 79:1, 87, 143, 165, 165:1, 165:2, 181, 185, 197, 202, 225, 257, 266, 267, 281, 341, 353, 354, 358, 364, 365, 368, etc.;

[0029] The average particle size of the colorant is preferably 30 to 300 nm, and more preferably 50 to 250 nm. In this specification, the average particle size refers to the average particle size of particles measured by a laser light scattering method.

[0030] The content of the colorant relative to the total mass of the ink according to this embodiment is preferably 1 to 30 mass %, more preferably 1 to 10 mass %, and even more preferably 2 to 8 mass %.

[0031] The colorant may further contain other dyes in addition to the pigment and the disperse dye. Examples of the other dyes include solvent dyes, direct dyes, acid dyes, and reactive dyes.

[0032] When the ink contains a plurality of types of colorants, the mixing ratio of the colorants can be set arbitrarily according to the purpose. When the ink contains other dyes in addition to the colorants, the mixing ratio of the total amount of the colorants to the total amount of the other dyes can also be set arbitrarily.

[0033] The ink may contain an organic solvent, and the organic solvent is not particularly limited, but is preferably a water-soluble organic solvent, such as polyhydric alcohols, ethers such as polyhydric alcohol alkyl ethers and polyhydric alcohol aryl ethers, nitrogen-containing heterocyclic compounds, amides, amines, and sulfur-containing compounds. Specific examples of the water-soluble organic solvent include ethylene glycol, diethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 3-methyl-1,3-butanediol, triethylene glycol, polyethylene glycol, polypropylene glycol, 1,2-pentanediol, 1,3-pentanediol, 1,4-pentanediol, 2,4-pentanediol, 1,5-pentanediol, and the like. polyhydric alcohols such as pentanediol, 1,2-hexanediol, 1,6-hexanediol, 1,3-hexanediol, 2,5-hexanediol, 1,5-hexanediol, glycerin, 1,2,6-hexanetriol, 2-ethyl-1,3-hexanediol, ethyl-1,2,4-butanetriol, 1,2,3-butanetriol, 2,2,4-trimethyl-1,3-pentanediol, and petriol; ethylene glycol monoethyl ether; ethylene glycol monobutyl ether; Examples of the alkyl ether include polyhydric alcohol alkyl ethers such as diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, tetraethylene glycol monomethyl ether, and propylene glycol monoethyl ether; polyhydric alcohol aryl ethers such as ethylene glycol monophenyl ether and ethylene glycol monobenzyl ether; nitrogen-containing heterocyclic compounds such as 2-pyrrolidone, N-methyl-2-pyrrolidone, N-hydroxyethyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, ε-caprolactam, and γ-butyrolactone; amides such as formamide, N-methylformamide, N,N-dimethylformamide, 3-methoxy-N,N-dimethylpropionamide, and 3-butoxy-N,N-dimethylpropionamide; amines such as monoethanolamine, diethanolamine, and triethylamine; sulfur-containing compounds such as dimethyl sulfoxide, sulfolane, and thiodiethanol; propylene carbonate; and ethylene carbonate. It is preferable to use an organic solvent having a boiling point of 250° C. or less, since this not only functions as a wetting agent but also provides good drying properties.

[0034] Polyol compounds having 8 or more carbon atoms and glycol ether compounds are also suitably used. Specific examples of polyol compounds having 8 or more carbon atoms include 2-ethyl-1,3-hexanediol and 2,2,4-trimethyl-1,3-pentanediol. Specific examples of glycol ether compounds include polyhydric alcohol alkyl ethers such as ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, tetraethylene glycol monomethyl ether, and propylene glycol monoethyl ether; and polyhydric alcohol aryl ethers such as ethylene glycol monophenyl ether and ethylene glycol monobenzyl ether.

[0035] Polyol compounds having 8 or more carbon atoms and glycol ether compounds can improve the permeability of ink when paper is used as the recording medium.

[0036] The content of the organic solvent in the ink is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoints of the drying property and ejection reliability of the ink, however, the content is preferably from 10% by mass to 60% by mass, and more preferably from 20% by mass to 60% by mass.

[0037] The ink may contain a resin. The resin is not particularly limited as long as it is other than the above-mentioned resin particles, but examples thereof include polyester resin and polyurethane resin.

[0038] The ink may contain water. The water is preferably water with a low content of impurities such as metal ions, i.e., ion-exchanged water, distilled water, etc. The water content is not particularly limited and can be appropriately selected depending on the purpose, but from the viewpoint of the drying property and ejection reliability of the ink, it is preferably 10% by mass or more and 90% by mass or less, and more preferably 20% by mass or more and 60% by mass or less.

[0039] The ink may contain, as other components, ink preparation agents such as wax, dispersants, moisturizers, preservatives and antifungals, pH adjusters, chelating agents, rust inhibitors, water-soluble ultraviolet absorbers, water-soluble polymeric compounds, antioxidants and / or surfactants.

[0040] [wax] The ink may contain wax.

[0041] The form of the wax is preferably a wax emulsion, and particularly preferably an aqueous wax emulsion. As the wax emulsion, natural wax and chemically synthesized wax can be used. As the natural wax, an emulsion in which petroleum wax such as paraffin wax and microcrystalline wax, lignite wax such as montan wax, or vegetable wax such as carnauba wax and candelilla wax, animal and vegetable wax such as beeswax and lanolin are dispersed in an aqueous medium, and as the chemically synthesized wax, an emulsion in which homopolymer wax such as polyalkylene waxes such as polyethylene wax and polypropylene wax, and their oxidized forms such as polyalkylene oxide waxes, Fischer-Trop, copolymer waxes such as ethylene vinyl acetate, ethylene acrylic acid, and ester wax are dispersed in an aqueous medium can be mentioned. Among these waxes, polyalkylene waxes, oxidized polyalkylene waxes, and paraffin waxes are preferred. These waxes may be used alone or in combination.

[0042] The amount of wax added is usually 0.01 to 3.0% by mass, and more preferably 0.1 to 1.5% by mass.

[0043] [Dispersant] The ink preferably contains one or more dispersants to disperse the colorant. Another embodiment of the present invention is to use a self-dispersing colorant as the colorant, thereby dispersing the colorant without using a dispersant. The dispersant is not particularly limited, and known dispersants such as polymer dispersants can be used. The polymer dispersant is other than the binder and wax, and examples thereof include copolymers composed of at least two monomers (preferably at least one of which is a hydrophilic monomer) selected from monomers such as styrene and its derivatives; vinyl naphthalene and its derivatives; aliphatic alcohol esters of α,β-ethylenically unsaturated carboxylic acids; (meth)acrylic acid and its derivatives; maleic acid and its derivatives; itaconic acid and its derivatives; faric acid and its derivatives; vinyl acetate, vinyl alcohol, vinyl pyrrolidone, acrylamide, and their derivatives. Examples of such copolymers include styrene-(meth)acrylic acid copolymers, styrene-(meth)acrylic acid-(meth)acrylic acid ester copolymers, (meth)acrylic acid ester-(meth)acrylic acid copolymers, polyethylene glycol (meth)acrylate-(meth)acrylic acid copolymers, and styrene-maleic acid copolymers. Among these, styrene-(meth)acrylic acid copolymers, styrene-(meth)acrylic acid-(meth)acrylic acid ester copolymers, and (meth)acrylic acid ester-(meth)acrylic acid copolymers are preferred, (meth)acrylic acid ester-(meth)acrylic acid copolymers are more preferred, and methacrylic acid ester-methacrylic acid copolymers are even more preferred. Examples of types of copolymers include block copolymers, random copolymers, and graft copolymers. These copolymers may be in the form of a salt.

[0044] Dispersants can be commercially available or synthesized.

[0045] Examples of commercially available dispersants include Joncyrl 62, 67, 68, 678, and 687 (styrene-acrylic copolymers manufactured by BASF); Movinyl S-100A (modified vinyl acetate copolymer manufactured by Japan Coating Resins Co., Ltd.); and Julimer AT-210 (polyacrylic acid ester copolymer manufactured by Toa Gosei Co., Ltd.).

[0046] Examples of dispersants obtained by synthesis include the AB block polymer disclosed in WO 2013 / 115071. The monomer constituting the A block of the AB block polymer disclosed in WO 2013 / 115071 is at least one monomer selected from (meth)acrylic acid and linear or branched C4 alkyl (meth)acrylate, preferably at least one monomer selected from methacrylic acid and n-butyl methacrylate, and more preferably these two monomers are used in combination. The monomer constituting the B block of the AB block polymer disclosed in WO 2013 / 115071 is at least one monomer selected from benzyl methacrylate and benzyl acrylate, preferably benzyl methacrylate. Specific examples of the AB block polymer include the block copolymers disclosed in Synthesis Examples 3 to 8 of WO 2013 / 115071.

[0047] The acid value of the dispersant is usually from 90 to 200 mgKOH / g, preferably from 100 to 150 mgKOH / g, and more preferably from 100 to 120 mgKOH / g.

[0048] A neutralizing agent may be used to disperse the dispersant uniformly in water. Examples of the neutralizing agent include ammonia, hydroxides of alkali metals, hydroxides of alkaline earth metals, aliphatic amine compounds, and alkanolamine compounds. Among these, ammonia and hydroxides of alkali metals are preferred, and ammonia is more preferred. The amount of the neutralizing agent to be used is usually 30 to 300% neutralization degree, preferably 50 to 200%, assuming that the neutralization degree is 100% when the dispersant is neutralized with the theoretical equivalent of the acid value of the dispersant.

[0049] The mass average molecular weight of the dispersant is usually 10,000 to 60,000, preferably 10,000 to 40,000, more preferably 15,000 to 30,000, and further preferably 20,000 to 25,000. The mass average molecular weight of the dispersant can be measured by gel permeation chromatography (GPC). Specifically, the measurement can be performed using HLC-8320GPC (manufactured by Tosoh Corporation) as a GPC device, two TSK gel Super Multipore HZ-H (manufactured by Tosoh Corporation, inner diameter 4.6 mm x 15 cm) columns, tetrahydrofuran as an eluent, and TSK Standard (manufactured by Tosoh Corporation) as a standard sample.

[0050] The PDI (mass average molecular weight / number average molecular weight) of the dispersant is preferably about 1.29 to 1.49. By setting it in this range, the dispersibility and storage stability of the ink tend to be improved.

[0051] The dispersant may be used in a state where it is mixed with the colorant, or in a state where a part or the whole of the surface of the colorant is coated with the dispersant, or both of these states may be used in combination.

[0052] The ratio of the total mass of the dispersants to the total mass of the colorants is preferably from 0.01 to 1.0, more preferably from 0.05 to 0.6, and even more preferably from 0.1 to 0.5.

[0053] Specific examples of moisturizing agents include polyols such as glycerin, ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, propylene glycol, dipropylene glycol, polypropylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,2,6-hexanetriol, and pentaerythritol; cyclic amides such as 2-pyrrolidone and N-methyl-2-pyrrolidone; ureas such as urea, thiourea, ethyleneurea, and 1,3-dimethylimidazolidinones; lactams such as ε-caprolactam; solid glycerins such as trimethylolpropane and trimethylolethane; and sugars such as maltitol, sorbitol, gluconolactone, and maltose.

[0054] Specific examples of antiseptic and antifungal agents include organic sulfur-based, organic nitrogen sulfur-based, organic halogen-based, haloarylsulfone-based, iodopropargyl-based, haloalkylthio-based, nitrile-based, pyridine-based, 8-oxyquinoline-based, benzothiazole-based, isothiazolin-based, dithiol-based, pyridine oxide-based, nitropropane-based, organic tin-based, phenol-based, quaternary ammonium salt-based, triazine-based, thiazine-based, anilide-based, adamantane-based, dithiocarbamate-based, brominated indanone-based, benzyl bromoacetate-based, and inorganic salt-based compounds.

[0055] A specific example of the organic halogen compound is sodium pentachlorophenol, and a specific example of the pyridine oxide compound is sodium 2-pyridinethiol-1-oxide.

[0056] Examples of isothiazoline compounds include 1,2-benzisothiazolin-3-one, 2-n-octyl-4-isothiazolin-3-one, 5-chloro-2-methyl-4-isothiazolin-3-one, 5-chloro-2-methyl-4-isothiazolin-3-one magnesium chloride, 5-chloro-2-methyl-4-isothiazolin-3-one calcium chloride, and 2-methyl-4-isothiazolin-3-one calcium chloride.

[0057] Other specific examples of antiseptic and antifungal agents include anhydrous sodium acetate, sodium sorbate, sodium benzoate, ethyl p-hydroxybenzoate, and Arch Chemical's trade names Proxel GXL(S) and Proxel XL-2(S).

[0058] Any substance can be used as the pH adjuster as long as it can control the pH of the ink within the above range without adversely affecting the ink being prepared. Specific examples of the pH adjuster include the neutralizing agents mentioned above; alkali metal carbonates such as lithium carbonate, sodium carbonate, sodium hydrogencarbonate, and potassium carbonate; alkali metal salts of organic acids such as sodium silicate and potassium acetate; and inorganic bases such as disodium phosphate.

[0059] Specific examples of the chelating agent include disodium ethylenediaminetetraacetate, sodium nitrilotriacetate, sodium hydroxyethylethylenediaminetriacetate, sodium diethylenetriaminepentaacetate, and sodium uracildiacetate.

[0060] Specific examples of the rust inhibitor include acid sulfite, sodium thiosulfate, ammonium thioglycolate, diisopropylammonium nitrite, pentaerythritol tetranitrate, and dicyclohexylammonium nitrite.

[0061] Examples of the water-soluble ultraviolet absorber include sulfonated benzophenone compounds, benzotriazole compounds, salicylic acid compounds, cinnamic acid compounds, and triazine compounds.

[0062] Specific examples of the water-soluble polymer compound include those other than the above-mentioned binders, waxes, and dispersants, such as polyethylene glycol, polyvinyl alcohol, cellulose derivatives, polyamines, and polyimines.

[0063] Examples of the antioxidant include various organic and metal complex-based anti-fading agents. Examples of the organic anti-fading agents include hydroquinones, alkoxyphenols, dialkoxyphenols, phenols, anilines, amines, indanes, chromans, alkoxyanilines, and heterocycles.

[0064] Examples of the surfactant include known anionic, cationic, amphoteric, nonionic, silicone-based and fluorine-based surfactants, and one or more of these can be selected and used.

[0065] Examples of anionic surfactants include alkyl sulfocarboxylates, α-olefin sulfonates, polyoxyethylene alkyl ether acetates, N-acylamino acids or salts thereof, N-acyl methyl taurines, alkyl sulfates, polyoxyalkyl ether sulfates, alkyl sulfates, polyoxyethylene alkyl ether phosphates, rosin acid soaps, castor oil sulfates, lauryl alcohol sulfates, alkylphenol phosphates, alkyl phosphates, alkylaryl sulfonates, diethyl sulfosuccinates, diethylhexyl sulfosuccinates, and dioctyl sulfosuccinates.

[0066] Examples of the cationic surfactant include 2-vinylpyridine derivatives and poly(4-vinylpyridine) derivatives.

[0067] Examples of amphoteric surfactants include lauryl dimethylaminoacetate betaine, 2-alkyl-N-carboxymethyl-N-hydroxyethyl imidazolinium betaine, coconut oil fatty acid amidopropyl dimethylaminoacetate betaine, polyoctyl polyaminoethyl glycine, and imidazoline derivatives.

[0068] Examples of nonionic surfactants include ether surfactants such as polyoxyethylene nonylphenyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene dodecylphenyl ether, polyoxyethylene oleyl ether, polyoxyethylene lauryl ether, and polyoxyethylene alkyl ether; polyoxyethylene oleate, polyoxyethylene distearate, sorbitan laurate, sorbitan monostearate, sorbitan monooleate, sorbitan sesquioleate, and polyoxyethylene monooleate. ester-based compounds such as ester acetate, polyoxyethylene stearate, and the like; acetylene glycol (alcohol)-based compounds such as 2,4,7,9-tetramethyl-5-decyne-4,7-diol, 3,6-dimethyl-4-octyne-3,6-diol, and 3,5-dimethyl-1-hexyne-3-ol; trade names Surfynol 104, 105PG50, 82, 420, 440, 465, 485, DF-110D, and Olfin STG manufactured by Nissin Chemical Industry Co., Ltd.; and polyglycol ether-based compounds such as TergItol 15-S-7 manufactured by SIGMA-ALDRICH.

[0069] Examples of silicone surfactants include polyether-modified siloxane, polyether-modified polydimethylsiloxane, etc. Examples of such surfactants include Dynol 960 and Dynol 980 manufactured by Air Products Co., Ltd., Silface SAG001, Silface SAG002, Silface SAG003, Silface SAG005, Silface SAG503A, Silface SAG008, Silface SAG009, Silface SAG010 manufactured by Nissin Chemical Industry Co., Ltd., and BYK-345, BYK-347, BYK-348, BYK-349, BYK-3450, BYK-3451, BYK-3455, etc. manufactured by BYK-Chemie Japan Co., Ltd., and various types of products can be easily purchased.

[0070] Examples of fluorine-based surfactants include perfluoroalkyl sulfonic acid compounds, perfluoroalkyl carboxylic acid compounds, perfluoroalkyl phosphate compounds, perfluoroalkyl ethylene oxide adducts, and polyoxyalkylene ether polymer compounds having perfluoroalkyl ether groups on the side chains, etc. Examples of such surfactants include Zonyl TBS, FSP, FSA, FSN-100, FSN, FSO-100, FSO, FS-300, and Capstone, manufactured by DuPont. FS-30, FS-31; PF-151N, PF-154N manufactured by Omnova; F-114, F-410, F-444, EXP.TF-2066, EXP.TF-2148, EXP.TF-2149, F-430, F-477, F-552, F-553, F-554, F-555, F-556, F-557, F-558, F-559, F-561, F-562, R-40, R-41, RS-72-K, RS-75, RS-76-E, RS-76-NS, RS-77, EXP.TF-1540, EXP.TF-1760 manufactured by DIC; and BYK-3440, BYK-3441 manufactured by BYK Japan Co., Ltd.

[0071] Among these, it is preferable to select at least one surfactant selected from nonionic or silicone surfactants.

[0072] In all of the above-mentioned components, contents, content ratios, etc., a combination of preferred components is more preferable, and a combination of more preferred components is even more preferable. The same applies to combinations of preferred components and more preferred components.

[0073] The method for preparing the ink is not particularly limited. One example is a method in which a dispersion liquid is prepared from a colorant and a dispersant, the binder and the organic solvent are added thereto, and water and the ink preparation agent are further added as necessary to prepare the ink.

[0074] The ink may be prepared using only one type of dispersion liquid, or two or more types of dispersion liquids.

[0075] When the ink contains a colorant, the method of dispersing the colorant to prepare a dispersion liquid includes a method using a sand mill (bead mill), a roll mill, a ball mill, a paint shaker, an ultrasonic disperser, a microfluidizer, etc., among which a sand mill (bead mill) is preferable. In addition, when preparing a colorant dispersion liquid using a sand mill (bead mill), it is preferable to use small beads (0.01 to 1 mm in diameter) and treat under conditions that increase the dispersion efficiency by increasing the bead packing rate, etc. By carrying out dispersion under such conditions, the particle size of the colorant can be reduced, and a dispersion liquid with good dispersibility can be obtained. In addition, after preparing the dispersion liquid, it is also preferable to remove components such as pigments with large particle sizes by filtration and / or centrifugation. In addition, in order to suppress foaming during the preparation of the dispersion liquid, a very small amount of a silicone-based, acetylene glycol-based, or other defoaming agent may be added. However, some defoaming agents inhibit dispersion and microparticulation, and it is preferable to use one that does not affect dispersion or stability after dispersion.

[0076] The colorant in the dispersion may be a microencapsulated colorant in which the surface of the colorant is coated with a dispersant, or may not be microencapsulated, but is preferably a microencapsulated colorant in which the colorant is uniformly coated with a dispersant.

[0077] The methods of uniformly covering the colorant surface with a dispersant to form a microencapsulation are roughly divided into two methods: physical / mechanical methods and chemical methods. As the latter chemical methods, surface precipitation, kneading, interfacial polymerization, etc. have been proposed. The surface precipitation method is a method of precipitating a dispersant on the colorant surface by utilizing pH adjustment or differences in solubility in a medium, and includes acid precipitation and phase inversion emulsification. The interfacial polymerization method is a method of adsorbing a monomer, oligomer, or pigment derivative on the colorant surface and then carrying out a polymerization reaction, and is also called the surface polymerization method. In the present invention, either method may be used, but the surface precipitation method is preferred, and the colored dispersion obtained by the phase inversion emulsification method is more preferred.

[0078] The phase inversion emulsification method is a method in which a colorant, a dispersant, and an organic solvent are mixed and dispersed, and water is further added to uniformly adsorb the dispersant onto the colorant surface. Specific manufacturing methods include the following five types of manufacturing methods.

[0079] 1. A manufacturing method in which a solution of a dispersant that disperses or dissolves in water and has a colorant dispersed in it is mixed with a liquid whose main component is water, and then the solvent is removed. 2. A manufacturing method in which a solution of a colorant dispersed in a hydrophilic organic solvent and a dispersant that disperses or dissolves in water by neutralization is mixed with a mixed liquid containing water and a neutralizing agent, and then the solvent is removed. 3. A manufacturing method in which a mixed solution of a hydrophilic organic solvent and a hydrophobic organic solvent in which a colorant is dispersed and a dispersant that disperses or dissolves in water is mixed with a liquid whose main component is water, and then the solvent is removed. 4. A manufacturing method in which a solution of a mixed solvent of a hydrophilic organic solvent and a hydrophobic organic solvent in which a colorant is dispersed and in which the dispersant disperses or dissolves in water by neutralization is mixed with a mixed liquid containing water and a neutralizing agent, and then the solvent is removed. 5. A manufacturing method in which a colorant is mixed with a solution of a mixed solvent whose main components are water and a hydrophilic organic solvent of a dispersant that disperses or dissolves in water, the pigment is dispersed in the solution, and then the solvent is removed.

[0080] The above-mentioned dispersion can be obtained by the above-mentioned manufacturing method, but a coated colorant dispersion can also be obtained by a different manufacturing method. An example of the manufacturing method is a manufacturing method in which a solution of a hydrophobic organic solvent in which a dispersant is dissolved is mixed with a liquid mainly composed of water containing a neutralizing agent to prepare an emulsion (emulsion or microemulsion), a colorant is added thereto and mixed / dispersed, and then water is further added to remove the solvent.

[0081] Although the dispersion liquid composed of colorant particles whose surfaces are covered with a dispersant has been described in detail, by using the above method, it is possible to easily obtain a dispersion liquid composed of colorant particles having a dispersant on the surface and an average particle size of 200 nm or less. In particular, it is more preferable to set the average particle size to 50 to 180 nm by selecting the type of colorant and the type of dispersant used, the acid value, the molecular weight, etc. Here, in this specification, the average particle size refers to the average particle size of particles measured using a laser light scattering method.

[0082] In preparing the dispersion, a neutralizing agent can be used, such as an alkali metal hydroxide, an alkaline earth metal hydroxide, an aliphatic amine compound, or an alcohol amine compound. These neutralizing agents can be used alone or in combination. In preparing the dispersion, the amount of the neutralizing agent is not limited. The degree of neutralization is 100% when the neutralization is performed with the theoretical equivalent of the acid value of the dispersing agent, and the neutralizing agent can be used in an amount exceeding the theoretical amount. The degree of neutralization is usually 0 to 150%, preferably 30 to 100%, and more preferably 50 to 70%.

[0083] Alkali metal hydroxides include, for example, lithium hydroxide, sodium hydroxide, and potassium hydroxide. Examples of the hydroxides of alkaline earth metals include beryllium hydroxide, magnesium hydroxide, calcium hydroxide, and strontium hydroxide. Of these, lithium hydroxide or sodium hydroxide is preferred.

[0084] Examples of the alcohol amine compound include monoethanolamine, diethanolamine, triethanolamine, monopropanolamine, dipropanolamine, tripropanolamine, methylethanolamine, dimethylethanolamine, and N-methyldiethanolamine. Among these, tertiary amines are preferred, and triethanolamine is more preferred.

[0085] Examples of the aliphatic amine compound include ammonia, monomethylamine, dimethylamine, trimethylamine, monoethylamine, dimethylamine and trimethylamine. Of these, ammonia or triethylamine is preferred.

[0086] The pH of the ink is usually pH 5 to 11, preferably pH 7 to 10, for the purpose of improving storage stability. The surface tension of the ink is usually 10 to 50 mN / m, preferably 20 to 40 mN / m. The viscosity of the ink is usually 30 mPa s or less, preferably 20 mPa s or less. The pH and surface tension of the ink can be appropriately adjusted by using ink regulators such as a pH adjuster and a surfactant.

[0087] The ink is excellent in circulation stability, storage stability, ejection stability, wet spreadability on a recording material, and drying property, and a printed matter obtained using the ink of the present invention is excellent in image folding resistance, blocking resistance, abrasion resistance, adhesion, color development, etc. Furthermore, in terms of abrasion resistance, it is excellent in dry abrasion resistance and wet abrasion resistance.

[0088] When the ink is used as an inkjet ink, it is preferable to reduce the content of inorganic impurities such as chlorides of metal cations (e.g., sodium chloride) and sulfates (e.g., sodium sulfate). The content of inorganic impurities is preferably 1% or less based on the total mass of the colorant, and the lower limit may be below the detection limit of an analytical instrument, i.e., 0%. Examples of methods for producing colorants with low inorganic impurities include a method of exchanging and adsorbing inorganic impurities with an ion exchange resin.

[0089] The present invention also includes an ink set that combines two or more of the above inks, an ink set that combines the above ink with an ink other than the above inks, an inkjet recording method in which droplets of the above inks are ejected from an inkjet head to record on a printing medium, and a printed matter printed using the above ink.

[0090] As the inkjet recording method, there is mentioned an inkjet recording method in which droplets of the ink are ejected in response to a recording signal and adhered to a recording material, thereby performing recording. The ink is poured into a container called an "ink tank" or an "ink cartridge", which is then loaded into a predetermined position of an inkjet printer and used for inkjet recording.

[0091] Examples of the inkjet method include a charge control method; a drop-on-demand method (pressure pulse method) that uses the vibration pressure of a piezoelectric element; an acoustic inkjet method; and a thermal inkjet, ie, a bubble jet (registered trademark) method. The ink can be used in any of these systems.

[0092] The recording material is not particularly limited, but a recording material that is non-absorbent or poorly absorbent to ink is preferred. Specific examples include coated paper such as lightly coated paper, art paper, coated paper, matte paper, and cast paper. Coated paper is paper that has a coating applied to its surface to enhance its aesthetic appearance and smoothness. Examples of the coating include various clays such as talc, pyrophyllite, and kaolin; mixtures of titanium oxide, magnesium carbonate, calcium carbonate, and the like with starch and / or polyvinyl alcohol; and the like. For example, paint can be applied to paper using a coater during the paper manufacturing process. There are two types of coaters: in-line type, which is directly connected to the papermaking machine to combine papermaking and coating in one process, and offline type, which is a separate process from papermaking. Lightly coated paper is paper with a coating weight of 12 g / m2. 2 The following paper is referred to. Art paper is a high-quality paper made of 100% chemical pulp with a thickness of 40 g / m2 This refers to paper that has been coated with paint on the front and back. Coated paper and matte paper are 20 to 40 g / m 2 It refers to paper that has been coated with a coating of paint to a degree of gloss. Cast paper refers to paper that has been finished by applying pressure to the surface of art paper or coated paper using a machine such as a casting drum to enhance its gloss and recording effect. The above ink exhibits the effects of the present invention extremely favorably when used for recording on such non-absorbent or poorly absorbent recording materials.

[0093] Examples of the recording material include ordinary paper, none of which has an ink-receiving layer, media used in gravure printing or offset printing, etc.; paper and film exclusively for inkjet printing, which have an inkjet receiving layer, glossy paper and glossy film, etc.; fibers and cloths such as cellulose, nylon, and wool; leather; and substrates for color filters. Here, among plain papers not having an ink receiving layer, there are those that have low ink receiving properties similar to the non-absorbent non-recording materials described above. Even when such plain papers are used, the effects obtained by the present invention are extremely effectively exhibited. EXAMPLES

[0094] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the following examples. In the text, "parts" and "%" are based on mass unless otherwise specified. In the examples, when quantitative determination of the pigment solid content in the dispersion was required, it was determined by the dry weight method using MS-70 manufactured by A&D Co., Ltd. The pigment solid content is a converted value calculated from the total amount of solids, i.e., the pigment solid content alone.

[0095] <Preparation of Dispersion 1> A block copolymer described in Synthesis Example 3 of International Publication No. 2013 / 115071 was prepared. 4.95 parts of the obtained polymer dispersant was dissolved in 19.5 parts of 2-butanone to obtain a uniform solution. A solution in which 0.15 parts of 28% ammonia water, 0.41 parts of PROXELGXL(S) (manufactured by Lonza), and 0.25 parts of BYK1770 (manufactured by BYK Japan Co., Ltd.) were dissolved in 56 parts of ion-exchanged water was added to this solution, and the mixture was stirred for 1 hour to prepare an emulsified solution. 16.5 parts of copper phthalocyanine blue (CHROMOFINE BLUE 4851 manufactured by Dainichi Seikagaku Co., Ltd.) were added thereto, and dispersion was performed using a sand grinder. Dispersion was performed for 6 hours under conditions of 1500 rpm. Subsequently, 58.3 parts of ion-exchanged water was dropped, and the dispersion beads were separated by filtration. Further, 2-butanone and water were distilled off under reduced pressure using an evaporator so that the pigment solid content was 11.7%, thereby obtaining a dispersion having a pigment solid content of 11.7% and an average pigment particle size of 110 nm. This is designated as "Dispersion 1".

[0096] <Synthesis example of resin particle dispersion> (Resin fine particles 1) A mixture consisting of 6.12 parts by weight of methyl methacrylate, 55.63 parts by weight of 2-ethylhexyl acrylate, 25.03 parts by weight of lauryl acrylate, 5.01 parts by weight of methacrylic acid, 7.79 parts by weight of 2-hydroxyethyl methacrylate, 0.42 parts by weight of dodecanethiol, 3.0 parts by weight of Neopelex G65 (manufactured by Kao Corporation), and 100 parts by weight of ion-exchanged water was emulsified using a homomixer to obtain a uniform milky white emulsion. In a 1L flask equipped with a stirrer, a thermometer, a nitrogen gas inlet tube, and a reflux tube, 250 parts by weight of ion-exchanged water and 3.0 parts by weight of Neopelex G65 (manufactured by Kao Corporation) were charged in advance, and the temperature was raised to 65°C while introducing nitrogen. Next, 3.0 parts by weight of ammonium persulfate was added, and the previously prepared emulsion was continuously dropped over 3.0 hours. After the dropwise addition was completed, the mixture was aged for 2 hours and then cooled, whereby resin particle dispersion 1 was obtained. (Resin fine particles 2) A mixture consisting of 8.25 parts by weight of methyl methacrylate, 78.13 parts by weight of 2-ethylhexyl acrylate, 5.01 parts by weight of methacrylic acid, 7.79 parts by weight of 2-hydroxyethyl methacrylate, 0.82 parts by weight of dodecanethiol, 3.0 parts by weight of Neopelex G65 (manufactured by Kao Corporation), and 100 parts by weight of ion-exchanged water was emulsified using a homomixer to obtain a uniform milky white emulsion. 250 parts by weight of ion-exchanged water and 3.0 parts by weight of Neopelex G65 (manufactured by Kao Corporation) were charged in a 1L flask equipped with a stirrer, a thermometer, a nitrogen gas inlet tube, and a reflux tube, and the temperature was raised to 65°C while introducing nitrogen. Next, 3.0 parts by weight of ammonium persulfate was added, and the previously prepared emulsion was continuously dropped over 3.0 hours. After the end of the dropwise addition, the mixture was aged for 2 hours and then cooled to obtain a resin fine particle dispersion 2. (Resin fine particles 3) A mixture consisting of 1.2 parts by weight of styrene, 68.28 parts by weight of 2-ethylhexyl acrylate, 15.2 parts by weight of lauryl acrylate, 6.00 parts by weight of methacrylic acid, 8.50 parts by weight of 2-hydroxyethyl methacrylate, 0.82 parts by weight of dodecanethiol, 3.0 parts by weight of Neopelex G65 (manufactured by Kao Corporation), and 100 parts by weight of ion-exchanged water was emulsified using a homomixer to obtain a uniform milky white emulsion. In a 1L flask equipped with a stirrer, a thermometer, a nitrogen gas inlet tube, and a reflux tube, 250 parts by weight of ion-exchanged water and 3.0 parts by weight of Neopelex G65 (manufactured by Kao Corporation) were charged in advance, and the temperature was raised to 65°C while introducing nitrogen. Next, 3.0 parts by weight of ammonium persulfate was added, and the previously prepared emulsion was continuously added dropwise over 3.0 hours. After the dropwise addition was completed, the mixture was aged for 2 hours and then cooled to obtain resin particle dispersion 3. (Resin fine particles 4) A mixture consisting of 25 parts by weight of methyl methacrylate, 60.79 parts by weight of 2-ethylhexyl acrylate, 4.00 parts by weight of methacrylic acid, 10.00 parts by weight of 2-hydroxyethyl methacrylate, 0.21 parts by weight of dodecanethiol, 3.0 parts by weight of Neopelex G65 (manufactured by Kao Corporation), and 100 parts by weight of ion-exchanged water was emulsified using a homomixer to obtain a uniform milky white emulsion. 250 parts by weight of ion-exchanged water and 3.0 parts by weight of Neopelex G65 (manufactured by Kao Corporation) were charged in a 1L flask equipped with a stirrer, a thermometer, a nitrogen gas inlet tube, and a reflux tube, and the temperature was raised to 65°C while introducing nitrogen. Next, 3.0 parts by weight of ammonium persulfate was added, and the previously prepared emulsion was continuously dropped over 3.0 hours. After the end of the dropwise addition, the mixture was aged for 2 hours and then cooled to obtain resin fine particle dispersion 4. (Resin fine particles 5) A mixture consisting of 15 parts by weight of methyl methacrylate, 69.90 parts by weight of 2-ethylhexyl acrylate, 6.00 parts by weight of methacrylic acid, 9.00 parts by weight of 2-hydroxyethyl methacrylate, 0.21 parts by weight of dodecanethiol, 3.0 parts by weight of Neopelex G65 (manufactured by Kao Corporation), and 100 parts by weight of ion-exchanged water was emulsified using a homomixer to obtain a uniform milky white emulsion. 250 parts by weight of ion-exchanged water and 3.0 parts by weight of Neopelex G65 (manufactured by Kao Corporation) were charged in a 1L flask equipped with a stirrer, a thermometer, a nitrogen gas inlet tube, and a reflux tube, and the temperature was raised to 65°C while introducing nitrogen. Next, 3.0 parts by weight of ammonium persulfate was added, and the previously prepared emulsion was continuously dropped over 3.0 hours. After the end of the dropwise addition, the mixture was aged for 2 hours and then cooled to obtain resin fine particle dispersion 5. (Resin fine particles 6) A mixture consisting of 8 parts by weight of methyl methacrylate, 78.36 parts by weight of 2-ethylhexyl acrylate, 5.01 parts by weight of methacrylic acid, 7.79 parts by weight of 2-hydroxyethyl methacrylate, 0.82 parts by weight of dodecanethiol, 3.0 parts by weight of Neopelex G65 (manufactured by Kao Corporation), and 100 parts by weight of ion-exchanged water was emulsified using a homomixer to obtain a uniform milky white emulsion. 250 parts by weight of ion-exchanged water and 3.0 parts by weight of Neopelex G65 (manufactured by Kao Corporation) were charged in a 1L flask equipped with a stirrer, a thermometer, a nitrogen gas inlet tube, and a reflux tube, and the temperature was raised to 65°C while introducing nitrogen. Next, 3.0 parts by weight of ammonium persulfate was added, and the previously prepared emulsion was continuously dropped over 3.0 hours. After the end of the dropwise addition, the mixture was aged for 2 hours and then cooled to obtain resin fine particle dispersion 6. (Resin fine particles 7) A mixture consisting of 76.38 parts by weight of 2-ethylhexyl acrylate, 10 parts by weight of n-butyl methacrylate, 5.01 parts by weight of methacrylic acid, 7.79 parts by weight of 2-hydroxyethyl methacrylate, 0.82 parts by weight of dodecanethiol, 3.0 parts by weight of Neopelex G65 (manufactured by Kao Corporation), and 100 parts by weight of ion-exchanged water was emulsified using a homomixer to obtain a uniform milky white emulsion. 250 parts by weight of ion-exchanged water and 3.0 parts by weight of Neopelex G65 (manufactured by Kao Corporation) were charged in a 1L flask equipped with a stirrer, a thermometer, a nitrogen gas inlet tube, and a reflux tube, and the temperature was raised to 65°C while introducing nitrogen. Next, 3.0 parts by weight of ammonium persulfate was added, and the previously prepared emulsion was continuously dropped over 3.0 hours. After the end of the dropwise addition, the mixture was aged for 2 hours and then cooled to obtain resin fine particle dispersion 7. (Resin fine particles 8) A mixture consisting of 40 parts by weight of methyl methacrylate, 51.30 parts by weight of 2-ethylhexyl acrylate, 4.00 parts by weight of methacrylic acid, 3.5 parts by weight of 2-hydroxyethyl methacrylate, 1.2 parts by weight of dodecanethiol, 3.0 parts by weight of Neopelex G65 (manufactured by Kao Corporation), and 100 parts by weight of ion-exchanged water was emulsified using a homomixer to obtain a uniform milky white emulsion. 250 parts by weight of ion-exchanged water and 3.0 parts by weight of Neopelex G65 (manufactured by Kao Corporation) were charged in a 1L flask equipped with a stirrer, a thermometer, a nitrogen gas inlet tube, and a reflux tube, and the temperature was raised to 65°C while introducing nitrogen. Next, 3.0 parts by weight of ammonium persulfate was added, and the previously prepared emulsion was continuously dropped over 3.0 hours. After the end of the dropwise addition, the mixture was aged for 2 hours and then cooled to obtain a resin fine particle dispersion 8.

[0097] [Table 1]

[0098] The abbreviations in Table 1 above are as follows. In addition, blanks in Table 1 indicate 0 parts. MMA: Methyl methacrylate ST: styrene 2EHA: 2-Ethylhexyl acrylate BMA: n-Butyl acrylate LA: Lauryl acrylate MAA: Methacrylic acid HEMA: 2-hydroxyethyl methacrylate DDT: Dodecanethiol

[0099] <Ink Preparation> The dispersion 1 and each of the fine particles obtained above were added and stirred to obtain a liquid having the composition shown in Table 2 below. The resulting liquid was filtered through a membrane filter with a pore size of 3 μm to obtain the inks of Examples 1 to 3 and Comparative Examples 1 to 5. In Table 2, blanks indicate 0 parts.

[0100] [Table 2]

[0101] The abbreviations in Table 2 above represent the following. 1,5-PD: 1,5 pentanediol In Table 2 above, the numbers for each component represent the number of parts.

[0102] <Evaluation of bending properties> 50 μl of each of the inks obtained in the Examples and Comparative Examples was measured out and coated onto Toyobo PET film E5100 at a speed of 200 mm / sec using a No. 3 bar coater on a PI-1210 automatic coating device (manufactured by Tester Sangyo Co., Ltd.). The image area of ​​the resulting printed film was observed under a zoom microscope to observe the density of the solid image and cracks. The image quality was evaluated according to the following evaluation criteria. A score of 4 or higher is a tolerable level for a product, and a score of 3 or lower is a quality defect. -Evaluation criteria- 5: A dense, uniform solid image is formed. 4: The color is slightly pale, but a uniform solid image is formed. 3: There are some cracks in the solid image 2: Cracks are visible throughout the image 1: Image cracks are visible overall, and the base is clearly visible <Blocking evaluation> 50 μl of each ink obtained in the examples and comparative examples was measured out and coated on Toyobo PET film E5100 at a speed of 200 mm / sec using a No. 3 bar coater on a PI-1210 automatic coating device (manufactured by Tester Sangyo Co., Ltd.). The printed portion was cut into 2 x 3 cm pieces, and the printed surface and the back side of the unprinted film were placed on top of each other and subjected to a pressure of 7 MPa for 30 seconds using a compression tester. The pieces were then peeled off and the color transfer to the unprinted film side and image loss on the printed surface were evaluated. A score of 4 or higher is a low issue in terms of print quality, while a score of 3 or lower is a quality defect. -Evaluation criteria- 5: No color transfer at all 4: There is some dot-like color transfer, but no image loss on the printed surface. 3: There are more than 10 dot-like color transfers or color transfers in lines, and image loss is observed on the printed surface. 2: Approximately half of the print has been discolored and approximately 50% of the image is missing from the printed surface. 1: Over 50% of the printed surface has completely transferred to the non-printed surface

[0103] The results in Table 2 show that the prints obtained using the inks of the examples have excellent image folding resistance and blocking resistance. [Industrial Applicability]

[0104] The resin fine particles of the present invention make it possible to provide an ink-jet ink having excellent image folding resistance and blocking resistance.

Claims

1. Resin fine particles containing at least one resin selected from the group consisting of an acrylic resin and an acrylic styrene resin, the resin fine particles having a storage modulus G1 at 20° C. as measured by a dynamic viscoelasticity measurement method of 1.0×10 4 Pa or more 1.0×10 8 The storage modulus G2 of the resin fine particles at 70° C. as measured by a dynamic viscoelasticity measurement method is 1.0×10 4 The resin particles have a viscosity of 0.1 Pa or less.

2. 2. The resin particles according to claim 1, wherein the acid value of the resin particles is 10 to 120 mgKOH / g.

3. 3. The resin fine particles according to claim 1, wherein the relationship between the acid value and the hydroxyl value of the resin fine particles satisfies the condition that the value calculated by acid value / hydroxyl value is in the range of 0.5 to 2.

0.

4. 3. The resin fine particles according to claim 1, wherein the average particle diameter of the resin fine particles is in the range of 20 to 400 nm.

5. 3. The resin fine particles according to claim 1, wherein the resin fine particles contain monomers having C4 to C19 side chain components in an amount of 50 to 90% by mass, based on 100% by total mass of monomers constituting the resin fine particles.

Citation Information

Patent Citations

  • Aqueous pigment dispersion and aqueous recording liquid

    JP2000219749A

  • Polymer binder for ink-jet ink

    JP2001240622A

  • Ink for ink jet printer

    JP2002338863A

  • Flame retardant coating film

    JP2020007534A

  • Aqueous ink set for inkjet recording

    JP2014065826A