By employing a specific solvent ratio and reactant combination in the polymerization of cyclic organosiloxane, the method effectively produces polysiloxanes with a controlled number of silicon atoms between 3 and 15 per molecule, overcoming the challenges of high molecular weight polysiloxanes in existing technologies.
Patent Information
- Application Number
- JP2023059119
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing methods for producing polysiloxane struggle to control the molecular weight in the low molecular region, resulting in high molecular weight polysiloxanes with more than 15 silicon atoms per molecule, making it difficult to achieve low molecular weight polysiloxanes with a controlled number of silicon atoms.
A method involving the ring-opening polymerization of cyclic organosiloxane using a predetermined ratio of aprotic polar solvents and nonpolar solvents, specifically combining lithium silanolate and organosiloxane in specific molar ratios, to produce polysiloxanes with controlled silicon atom counts between 3 and 15 per molecule.
This approach allows for the production of low molecular weight polysiloxanes with a controlled number of silicon atoms, achieving a range of 3 to 15 silicon atoms per molecule, thereby addressing the limitations of previous methods.
Smart Images

Figure 2024146307000001 
Figure 2024146307000002 
Figure 2024146307000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polysiloxane and a method for producing the same. [Background technology]
[0002] As a method for producing polysiloxane, a method for obtaining linear polysiloxane by anionically polymerizing cyclic organosiloxane using a lithium catalyst has been proposed (Patent Document 1). Patent Document 1 states that the solvent used in this anionic polymerization is "preferably a polar solvent having no active hydrogen, and the polymerization reaction is inhibited in a solvent having active hydrogen, and the polymerization reaction does not proceed at all in the case of a non-polar solvent." In the examples of Patent Document 1, tetrahydrofuran is used. In the examples of Patent Document 1, the catalyst component butyllithium is used as a hexane solution, and the reaction system contains tetrahydrofuran, which is a polar solvent, and hexane, which is a non-polar solvent, and the ratio (molar ratio) is [hexane / tetrahydrofuran] = 0.002 in Example 1 of Patent Document 1, and [hexane / tetrahydrofuran] = 0.001 in Example 2.
[0003] In the production method of Patent Document 1, it is difficult to obtain a low molecular weight polysiloxane in which the number of silicon atoms in one molecule is 15 or less by controlling the molecular weight in the low molecular weight region. For this reason, the polysiloxane produced in Example 1 of Patent Document 1 is a high molecular weight polysiloxane in which the number of silicon atoms in one molecule is 20 in Example 1 and 32 in Example 2. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 1-98631 Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a method for producing low molecular weight polysiloxanes having a small number of silicon atoms per molecule, in particular a method for producing low molecular weight polysiloxanes in which the number of silicon atoms per molecule is controlled to 3 or more, preferably 5 or more, more preferably 6 or more, and 15 or less, preferably 13 or less, more preferably 11 or less, even more preferably 9 or less, and most preferably 7 or less, and a low molecular weight polysiloxane in which the number of silicon atoms per molecule is controlled to 3 or more, preferably 5 or more, more preferably 6 or more, and 15 or less, preferably 13 or less, more preferably 11 or less, even more preferably 9 or less, and most preferably 7 or less. [Means for solving the problem]
[0006] As a result of intensive research conducted by the present inventors in order to solve the above problems, it has been found that the above problems can be solved by using an aprotic polar solvent and a nonpolar solvent in a predetermined ratio when carrying out ring-opening polymerization of a cyclic organosiloxane. That is, the present invention relates to the following.
[0007] [1] A method for producing a polysiloxane, comprising polymerizing a lithium silanolate (I) represented by the following formula (2) with an organosiloxane (D3) represented by the following formula (1) in the presence of an aprotic polar solvent and a nonpolar solvent to produce a polysiloxane represented by the following formula (3): A method for producing a polysiloxane, wherein the molar ratio of the aprotic polar solvent to the nonpolar solvent ([nonpolar solvent] / [aprotic polar solvent]) is 5 to 100, and the molar ratio of the organosiloxane (D3) to the lithium silanolate (I) ([D3] / [I]) is 0.01 to 2.
[0008] [ka]
[0009] (In the formula, R1 and R2 each independently represent an optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, an optionally substituted aromatic group, or an optionally substituted z-linear alkenyl group having 2 to 12 carbon atoms (wherein z is a number indicating the position of the double bond in the alkenyl group and is an integer equal to the number of carbon atoms in the alkenyl group minus 1).)
[0010] [ka]
[0011] (In the formula, R3 represents a hydrogen atom, an optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, an optionally substituted aromatic group, or an optionally substituted z-linear alkenyl group having 2 to 12 carbon atoms (wherein z is a number indicating the position of the double bond in the alkenyl group and is an integer equal to the number of carbon atoms in the alkenyl group minus 1). R4 represents an optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms.)
[0012] [ka]
[0013] (In the formula, R1 and R2 are defined as R1 and R2 in the formula (1), and R3 and R4 are defined as R3 and R4 in the formula (2). R5 represents a hydrogen atom, an optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, an optionally substituted aromatic group, or an optionally substituted z-linear alkenyl group having 2 to 12 carbon atoms (wherein z is a number indicating the position of the double bond in the alkenyl group and is an integer equal to the number of carbon atoms in the alkenyl group minus 1). n is an integer from 1 to 13.)
[0014] [2] A polysiloxane represented by the following formula (3), which contains 3 to 15 silicon atoms in one molecule.
[0015] [ka]
[0016] (In the formula, R1 and R2 each independently represent an optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, an optionally substituted aromatic group, or an optionally substituted z-straight-chain alkenyl group having 2 to 12 carbon atoms (wherein z is a number indicating the position of the double bond in the alkenyl group and is an integer equal to the number of carbon atoms in the alkenyl group minus 1). R3 represents a hydrogen atom, an optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, an optionally substituted aromatic group, or an optionally substituted z-straight-chain alkenyl group having 2 to 12 carbon atoms (wherein and z is a number indicating the position of the double bond in the alkenyl group and is an integer equal to the number of carbon atoms in the alkenyl group minus 1.) R4 represents a saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms which may be substituted. R5 represents a hydrogen atom, a saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms which may be substituted, an aromatic group which may be substituted, or a z-straight-chain alkenyl group having 2 to 12 carbon atoms which may be substituted (wherein z is a number indicating the position of the double bond in the alkenyl group and is an integer equal to the number of carbon atoms in the alkenyl group minus 1). n is an integer equal to 1 to 13.) Effect of the Invention
[0017] According to the present invention, when carrying out ring-opening polymerization of cyclic organosiloxane, aprotic polar solvent and nonpolar solvent are used in combination in a prescribed ratio, thereby making it possible to obtain a low molecular weight polysiloxane having a small number of silicon atoms per molecule, in particular a polysiloxane in which the number of silicon atoms per molecule is controlled within a small molecular weight range. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The present invention will be described in detail below. However, the description of the constituent elements described below is a representative example of an embodiment of the present invention, and the present invention is not limited to these contents as long as it does not exceed the gist of the present invention.
[0019] The method for producing a polysiloxane of the present invention comprises polymerizing a lithium silanolate (I) represented by the following formula (2) with an organosiloxane (D3) represented by the following formula (1) in the presence of an aprotic polar solvent and a nonpolar solvent to produce a polysiloxane represented by the following formula (3): The molar ratio of the aprotic polar solvent to the nonpolar solvent ([nonpolar solvent] / [aprotic polar solvent]) is 5 to 100, and the molar ratio of the organosiloxane (D3) to the lithium silanolate (I) ([D3] / [I]) is 0.01 to 2.
[0020] [ka]
[0021] (In the formula, R1 and R2 each independently represent an optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, an optionally substituted aromatic group, or an optionally substituted z-linear alkenyl group having 2 to 12 carbon atoms (wherein z is a number indicating the position of the double bond in the alkenyl group and is an integer equal to the number of carbon atoms in the alkenyl group minus 1).)
[0022] [ka]
[0023] (In the formula, R3 represents a hydrogen atom, an optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, an optionally substituted aromatic group, or an optionally substituted z-linear alkenyl group having 2 to 12 carbon atoms (wherein z is a number indicating the position of the double bond in the alkenyl group and is an integer equal to the number of carbon atoms in the alkenyl group minus 1). R4 represents an optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms.)
[0024] [ka]
[0025] (In the formula, R1 and R2 are defined as R1 and R2 in the formula (1), and R3 and R4 are defined as R3 and R4 in the formula (2). R5 represents a hydrogen atom, an optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, an optionally substituted aromatic group, or an optionally substituted z-linear alkenyl group having 2 to 12 carbon atoms (wherein z is a number indicating the position of the double bond in the alkenyl group and is an integer equal to the number of carbon atoms in the alkenyl group minus 1). n is an integer from 1 to 13.)
[0026] <Organosiloxane (D3)> The organosiloxane (D3) used in the present invention is a compound represented by the following formula (1).
[0027] [ka]
[0028] (In the formula, R1 and R2 each independently represent an optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, an optionally substituted aromatic group, or an optionally substituted z-linear alkenyl group having 2 to 12 carbon atoms (wherein z is a number indicating the position of the double bond in the alkenyl group and is an integer equal to the number of carbon atoms in the alkenyl group minus 1).)
[0029] Examples of the optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms for R1 and R2 include linear or branched alkyl groups having 1 to 12 carbon atoms, specifically, methyl, ethyl, n-propyl, i-propyl, n-butyl, i-butyl, t-butyl, n-hexyl, n-octyl, n-decyl, n-dodecyl, 2-ethylhexyl, etc. Among these, the methyl group is preferred because it has little steric hindrance. Examples of the substituents which these saturated aliphatic hydrocarbon groups may have include a phenyl group, a halogen group, a nitro group, a hydroxyl group, and an ether group.
[0030] The aromatic group which may be substituted for R1 and R2 has an aromatic ring which is directly bonded to a silicon atom, and the aromatic ring may have a substituent such as an alkyl group such as a methyl group, a halogen group, a nitro group, a hydroxyl group, etc. Preferred is an aromatic group which has no polarity, such as an aromatic group substituted with an alkyl group or an unsubstituted aromatic group, and more preferably an unsubstituted phenyl group.
[0031] The z-linear alkenyl group having 2 to 12 carbon atoms which may be substituted for R1 and R2 (where z is a number indicating the position of the double bond in the alkenyl group and is an integer equal to the number of carbon atoms in the alkenyl group minus 1) is an alkenyl group having a double bond at the end opposite to the bond with the silicon atom, which may have a substituent and preferably has 2 to 12 carbon atoms, more preferably an alkenyl group having 2 to 7 carbon atoms, i.e., 0 to 5 methylene groups linked in series and having a vinyl group at the end. Specific examples include a vinyl group (ethenyl group), a vinylmethyl group (2-propenyl group), and a 2-vinylethyl group (3-butenyl group). In addition, when these alkenyl groups have a substituent, examples of the substituent include an alkyl group, an alkenyl group, a phenyl group, a halogen group, a nitro group, a hydroxy group, an ether group, and the like. Preferably, the alkenyl group has no substituent, and more preferably, the vinyl group (ethenyl group) has no substituent.
[0032] Specific examples of the organosiloxane (D3) represented by the formula (1) include hexamethylcyclotrisiloxane, hexaethylcyclotrisiloxane, trimethyltrivinylcyclotrisiloxane, and hexaphenylcyclotrisiloxane. Among them, hexamethylcyclotrisiloxane, hexaethylcyclotrisiloxane, and trimethyltrivinylcyclotrisiloxane are preferred, and hexamethylcyclotrisiloxane is more preferred. Thus, when R1 and R2, which are groups bonded to silicon atoms, are low bulk such as methyl, ethyl, and vinyl groups, the ring-opening equilibrium reaction is inclined toward the ring-opening side, and the polymerization reaction is likely to proceed.
[0033] <Lithium silanolate(I)> The lithium silanolate (I) used in the present invention is a compound represented by the following formula (2).
[0034] [ka]
[0035] (In the formula, R3 represents a hydrogen atom, an optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, an optionally substituted aromatic group, or an optionally substituted z-linear alkenyl group having 2 to 12 carbon atoms (wherein z is a number indicating the position of the double bond in the alkenyl group and is an integer equal to the number of carbon atoms in the alkenyl group minus 1). R4 represents an optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms. Me is a methyl group.)
[0036] Examples of the optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, the optionally substituted aromatic group, and the optionally substituted z-straight-chain alkenyl group having 2 to 12 carbon atoms (where z is a number indicating the position of the double bond of the alkenyl group and is an integer that is the number of carbon atoms in the alkenyl group minus 1) for R3 include those exemplified as the optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, the optionally substituted aromatic group, and the optionally substituted z-straight-chain alkenyl group having 2 to 12 carbon atoms (where z is a number indicating the position of the double bond of the alkenyl group and is an integer that is the number of carbon atoms in the alkenyl group minus 1) for R1 and R2 in formula (1), and preferred examples thereof are also the same. Examples of the optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms for R4 include those exemplified as the optionally substituted saturated aliphatic hydrocarbon groups having 1 to 12 carbon atoms for R1 and R2. Among these, a methyl group, an ethyl group, an n-butyl group, and a t-butyl group are preferred because raw material reagents are easily available.
[0037] The lithium silanolate (I) used in the present invention can be produced by known methods, for example, by directly reacting an equivalent or more of a lithium metal compound or lithium metal with a cyclic siloxane such as cyclotrisiloxane. Examples of the lithium metal compound include methyllithium, n-butyllithium, sec-butyllithium, t-butyllithium, and phenylbutyllithium. These compounds may be used after diluting with an appropriate solvent. The lithium metal compound may also be obtained by reacting a halogenated compound with lithium metal in-situ.
[0038] Since lithium silanolate (I) is unstable, it is preferable to prepare it in-situ. For example, it is preferable to add 3 equivalents of lithium metal compound to 1 equivalent of cyclotrisiloxane to generate 3 equivalents of lithium silanolate. Whether less than 3 equivalents of lithium metal compound are added to 1 equivalent of cyclotrisiloxane or whether more than 3 equivalents of lithium metal compound are added, the molar amount of lithium silanolate generated is equal to the molar amount of lithium metal compound added.
[0039] <Molar ratio of organosiloxane (D3) to lithium silanolate (I)> The molar ratio ([D3] / [I]) of organosiloxane (D3) and lithium silanolate (I) used in the ring-opening polymerization reaction of organosiloxane (D3) according to the present invention is 0.01 or more, preferably 0.05 or more, more preferably 0.1 or more. On the other hand, it is 2 or less, preferably 1.5 or less, more preferably 1 or less, and even more preferably 0.5 or less. If this ratio is too small, there is a tendency that the amount of unreacted organosiloxane (D3) is insufficient and the polymerization reaction is difficult to proceed. On the other hand, if this ratio is too large, the amount of organosiloxane (D3) relative to the solvent becomes excessive, so that some organosiloxane (D3) remains undissolved, and the control of the amount ratio tends to become ineffective.
[0040] The method for calculating the [D3] / [I] molar ratio will be explained in the Examples section below.
[0041] <Aprotic polar solvent> An aprotic solvent is a solvent that has no substrate that can act as a proton donor in the molecule and has a dipole moment in the molecule.
[0042] Examples of the aprotic polar solvent used in the present invention include tetrahydrofuran, 1,4-dioxane, dimethylformamide, dimethylsulfoxide, acetone, acetonitrile, ethyl acetate, and hexamethylphosphoric acid triamide. Among these, tetrahydrofuran, dimethylsulfoxide, dimethylformamide, and acetonitrile are preferred. These aprotic polar solvents may be used alone or in combination of two or more.
[0043] <Non-polar solvent> A non-polar solvent refers to a simple compound that is liquid at room temperature and normal pressure and has a relative dielectric constant of less than 6. Examples of the non-polar solvent used in the present invention include n-hexane, cyclohexane, benzene, toluene, o-xylene, m-xylene, p-xylene, diethyl ether, and diphenyl ether. Among them, n-hexane, benzene, toluene, o-xylene, and diethyl ether are preferred, and n-hexane, toluene, and diethyl ether are particularly preferred. These non-polar solvents may be used alone or in combination of two or more.
[0044] <Molar ratio of non-polar solvent to aprotic polar solvent> In the present invention, a non-polar solvent and an aprotic polar solvent are used in combination so that the molar ratio of the non-polar solvent to the aprotic polar solvent ([non-polar solvent] / [aprotic polar solvent]) is in the range of 5 to 100. If this molar ratio exceeds 100, that is, the amount of the non-polar solvent is large and the amount of the aprotic polar solvent is small, the organosiloxane (D3) as the raw material tends not to dissolve and the reaction does not proceed. On the other hand, if this molar ratio is less than 5, that is, the amount of the non-polar solvent is small and the amount of the aprotic polar solvent is large, the reaction tends to be too fast, and it tends to be difficult to obtain a polysiloxane in which the number of silicon atoms is controlled in the low molecular weight range. From this viewpoint, [non-polar solvent] / [aprotic polar solvent] is 5 to 100, preferably 5 to 60, and more preferably 5 to 50.
[0045] The method for calculating the molar ratio of [nonpolar solvent] / [aprotic polar solvent] will be explained in the Examples section below.
[0046] <Reaction temperature> The reaction temperature in the present invention is preferably from -20 to 80°C, more preferably from -10 to 40°C, and further preferably from 0 to 30°C.
[0047] <Response time> The reaction time in the present invention is preferably from 5 to 48 hours, more preferably from 5 to 24 hours.
[0048] <Polysiloxane> According to the method for producing a polysiloxane of the present invention, in which a nonpolar solvent and an aprotic polar solvent are used in combination in a predetermined molar ratio, it is possible to produce a polysiloxane having a small molecular weight and a controlled number of silicon atoms per molecule, and it is possible to produce a polysiloxane of the present invention represented by the following formula (3), which preferably contains 3 to 15 silicon atoms per molecule.
[0049] [ka]
[0050] (In the formula, R1 and R2 are defined as R1 and R2 in the formula (1), and R3 and R4 are defined as R3 and R4 in the formula (2). R5 represents a hydrogen atom, an optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, an optionally substituted aromatic group, or an optionally substituted z-linear alkenyl group having 2 to 12 carbon atoms (wherein z is a number indicating the position of the double bond in the alkenyl group and is an integer equal to the number of carbon atoms in the alkenyl group minus 1). n is an integer from 1 to 13.)
[0051] R1, R2, R3, and R4 in formula (3) are as defined above.
[0052] Examples of the optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, the optionally substituted aromatic group, and the optionally substituted z-straight-chain alkenyl group having 2 to 12 carbon atoms (where z is a number indicating the position of the double bond of the alkenyl group and is an integer that is the number of carbon atoms in the alkenyl group minus 1) for R5 include those exemplified as the optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, the optionally substituted aromatic group, and the optionally substituted z-straight-chain alkenyl group having 2 to 12 carbon atoms (where z is a number indicating the position of the double bond of the alkenyl group and is an integer that is the number of carbon atoms in the alkenyl group minus 1) for R1 and R2 in formula (1), and preferred examples thereof are also the same. In view of ease of functional group conversion, R5 is particularly preferably a hydrogen atom or an optionally substituted z-straight-chain alkenyl group having 2 to 12 carbon atoms (wherein z is a number indicating the position of the double bond in the alkenyl group and is an integer equal to the number of carbon atoms in the alkenyl group minus 1), and more preferably a hydrogen atom or an unsubstituted z-straight-chain alkenyl group having 2 to 12 carbon atoms (wherein z is a number indicating the position of the double bond in the alkenyl group and is an integer equal to the number of carbon atoms in the alkenyl group minus 1). n is 1 or more, preferably 3 or more, more preferably 4 or more, and is 13 or less, preferably 11 or less, more preferably 9 or less, even more preferably 7 or less, and most preferably 5 or less.
[0053] The number of silicon atoms contained in one molecule of the polysiloxane of the present invention represented by the formula (3) is 3 or more, preferably 5 or more, more preferably 6 or more, and is 15 or less, preferably 13 or less, more preferably 11 or less, even more preferably 9 or less, and most preferably 7 or less. Here, the number of silicon atoms contained in one molecule of polysiloxane is 1 It is a value calculated from the integral ratio of the peaks of the terminal functional group and the substituent on the silicon atom in a H-NMR chart, and more specifically, it can be determined by the method described in the Examples section below. However, when all of R1 to R5 are methyl groups, 1 Because it is difficult to calculate the number of silicon atoms in one molecule using H-NMR, it is preferable to use other methods. EXAMPLES
[0054] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples in any way as long as the gist of the present invention is not exceeded.
[0055] [Measurement / calculation method] The measurement and calculation methods for various parameters are as follows:
[0056] <Number of silicon atoms in one molecule> 7 mg of the obtained sample was dissolved in 0.98 g of deuterated chloroform and subjected to a 400 MHz magnetic field using a JEOL nuclear magnetic resonance apparatus at room temperature. 1 H-NMR measurement was carried out. The obtained chart was assigned, and the integral ratio (a:b) of the peaks of the substituents on the terminal silicon atoms and the substituents on the silicon atoms of the repeating units was calculated. The integral ratio of the peaks was divided by the number of hydrogen atoms (c, d) assigned to each substituent to calculate the ratio of the number of substituents contained in one molecule (a / c:b / d). The number of silicon atoms (x) in one molecule of polysiloxane was determined from the following formula using a, b, c, d, and the constant m determined from R1 and R2 in formula (1). Here, m is 2 when R1 and R2 in formula (1) are the same, and m is 1 when R1 and R2 in formula (1) are different. x=1 / m(b / d / a / c -1)+1
[0057] <Lithium silanolate amount> In the following examples, n-butyllithium was selected as the lithium metal compound and reacted with cyclotrisiloxane to obtain lithium silanolate in situ. The amount of n-butyllithium added in each example was converted into the amount of substance and used as the amount of lithium silanolate (mol).
[0058] <[D3] / [I] molar ratio> The molar ratio ([D3] / [I]) was calculated by dividing the molar amount of the added organosiloxane (D3) by the molar amount of the added lithium metal compound.
[0059] <[Non-polar solvent] / [Aprotic polar solvent] molar ratio> If the volume of the aprotic polar solvent is v1mL and the volume of the nonpolar solvent is v2mL, the molar ratio of the aprotic polar solvent to the nonpolar solvent ([nonpolar solvent] / [aprotic polar solvent]) (y) is expressed by the following formula. Here, ρ1, ρ2, n1, and n2 respectively represent the density of the aprotic polar solvent at room temperature and normal pressure, the density of the nonpolar solvent at room temperature and normal pressure, the molecular weight of the aprotic polar solvent, and the molecular weight of the nonpolar solvent. Note that, for tetrahydrofuran used in the following examples, ρ1 = 0.889 g / mL, n1 = 72.11 g / mol, for n-hexane, ρ2 = 0.655 g / mL, n2 = 86.18 g / mol, for toluene, ρ2 = 0.867 g / mL, n2 = 92.14 g / mol, and for diethyl ether, ρ2 = 0.713 g / mL, n2 = 74.12 g / mol.
[0060]
number
[0061] [Example 1] Trimethyltrivinylcyclotrisiloxane (1.10 mL, 4.1 mmol) and dehydrated toluene (1.23 mL) were placed in a 100 mL three-necked eggplant flask and dissolved under an argon atmosphere. Methyllithium (1.04 M diethyl ether solution, 12.80 mL, 13.3 mmol) was slowly added dropwise at room temperature, and stirring was continued for 30 minutes after the completion of the addition to allow the reaction to proceed. Then, hexamethylcyclotrisiloxane (D3) (620 mg, 2.8 mmol) and dehydrated tetrahydrofuran (THF) (0.192 mL, 2.4 mmol) were added in this order at room temperature. This reaction solution was stirred at room temperature for 5 hours, and dimethylchlorosilane (1.40 mL, 12.8 mmol) was added to cap the Li terminal, and then stirred at room temperature overnight. The reaction solution was extracted three times with diethyl ether, and the resulting organic layer was washed three times with saturated saline, and then dehydrated using anhydrous sodium sulfate. The solvent was removed from the resulting solution using a rotary evaporator over 1.5 hours, yielding a colorless, transparent liquid (0.64 g).
[0062] The resulting colorless and transparent liquid 1 H-NMR measurement confirmed the formation of the target product. In addition, the integral ratio of the peak at 5.73-6.10 ppm attributable to the terminal vinyl group and the peak at 0.06-0.19 ppm attributable to the methyl group on the silicon was 3.00:37.92, which means that one molecule of this polysiloxane contains an average of 6.8 silicon atoms. The amount of lithium silanolate (I), the amount of organosiloxane (D3), [D3] / [I], the amount of toluene, the amount of diethyl ether, the amount of THF, [nonpolar solvent] / [aprotic polar solvent], and the number of silicon atoms per molecule in this example are shown in Table 1.
[0063] [Example 2] Trimethyltrivinylcyclotrisiloxane (0.54 mL, 2.0 mmol) and dehydrated toluene (0.60 mL) were placed in a 100 mL three-necked eggplant flask and dissolved under an argon atmosphere. Methyllithium (1.04 M diethyl ether solution, 5.77 mL, 6.00 mmol) was slowly added dropwise at room temperature, and stirring was continued for 30 minutes after the completion of the addition to allow the reaction to proceed. Then, hexamethylcyclotrisiloxane (D3) (300 mg, 1.3 mmol) and dehydrated tetrahydrofuran (THF) (0.93 mL, 11.5 mmol) were added in this order at room temperature. This reaction solution was stirred at room temperature for 24 hours, and dimethylchlorosilane (0.67 mL, 6.1 mmol) was added to cap the Li terminal, and then stirred at room temperature overnight. The reaction solution was extracted three times with diethyl ether, and the resulting organic layer was washed three times with saturated saline, and then dehydrated using anhydrous sodium sulfate. The solvent was removed from the resulting solution using a rotary evaporator over a period of 2 hours, yielding a colorless, transparent liquid (0.50 g).
[0064] The resulting colorless and transparent liquid 1 H-NMR measurement confirmed the formation of the target product. In addition, the integral ratio of the peak at 5.73-6.10 ppm attributable to the terminal vinyl group and the peak at 0.06-0.19 ppm attributable to the methyl group on the silicon was 3.01:35.09, which means that one molecule of this polysiloxane contains an average of 6.3 silicon atoms. The amount of lithium silanolate (I), the amount of organosiloxane (D3), [D3] / [I], the amount of toluene, the amount of diethyl ether, the amount of THF, [nonpolar solvent] / [aprotic polar solvent], and the number of silicon atoms per molecule in this example are shown in Table 1.
[0065] [Example 3] Trimethyltrivinylcyclotrisiloxane (0.54 mL, 2.0 mmol) and dehydrated toluene (0.60 mL) were placed in a 100 mL three-necked eggplant flask and dissolved under an argon atmosphere. Methyllithium (1.04 M diethyl ether solution, 5.77 mL, 6.00 mmol) was slowly added dropwise at room temperature, and stirring was continued for 30 minutes after the completion of the addition to allow the reaction to proceed. Then, hexamethylcyclotrisiloxane (D3) (300 mg, 1.3 mmol) and dehydrated tetrahydrofuran (THF) (0.09 mL, 1.1 mmol) were added in this order at room temperature. This reaction solution was stirred at room temperature for 24 hours, and dimethylchlorosilane (0.70 mL, 6.4 mmol) was added to cap the Li terminal, and then stirred at room temperature overnight. The reaction solution was extracted three times with diethyl ether, and the resulting organic layer was washed three times with saturated saline, and then dehydrated using anhydrous sodium sulfate. The solvent was removed from the resulting solution using a rotary evaporator over a period of 2 hours, yielding a colorless, transparent liquid (0.28 g).
[0066] The resulting colorless and transparent liquid 1 H-NMR measurement confirmed the formation of the target product. In addition, the integral ratio of the peak at 5.73-6.10 ppm attributable to the terminal vinyl group and the peak at 0.06-0.19 ppm attributable to the methyl group on the silicon was 3.00:33.17, which means that one molecule of this polysiloxane contains an average of 6.0 silicon atoms. The amount of lithium silanolate (I), the amount of organosiloxane (D3), [D3] / [I], the amount of toluene, the amount of diethyl ether, the amount of THF, [nonpolar solvent] / [aprotic polar solvent], and the number of silicon atoms per molecule in this example are shown in Table 1.
[0067] [Example 4] Polysiloxane was synthesized in the same manner as in Example 3, except that the amount of hexamethylcyclotrisiloxane (D3) used was changed to 0.67 g, 3.0 mmol, and the amount of tetrahydrofuran (THF) used was changed to 0.50 mL, 6.2 mmol. The resulting colorless and transparent liquid 1H-NMR measurement confirmed the formation of the target product. In addition, the integral ratio of the peak at 5.74-6.10 ppm attributable to the terminal vinyl group to the peak at 0.05-0.19 ppm attributable to the methyl group on the silicon was 3:31.05, which means that one molecule of this polysiloxane contains an average of 5.7 silicon atoms. The amount of lithium silanolate (I), the amount of organosiloxane (D3), [D3] / [I], the amount of toluene, the amount of n-hexane, the amount of THF, [nonpolar solvent] / [aprotic polar solvent], and the number of silicon atoms per molecule in this example are shown in Table 1.
[0068] [Example 5] Polysiloxane was synthesized in the same manner as in Example 3, except that the amount of hexamethylcyclotrisiloxane (D3) used was changed to 1.33 g, 6.0 mmol, and the amount of tetrahydrofuran (THF) used was changed to 0.30 mL, 3.7 mmol. The resulting colorless and transparent liquid 1 H-NMR measurement confirmed the formation of the target product. In addition, the integral ratio of the peak at 5.74-6.10 ppm attributable to the terminal vinyl group to the peak at 0.05-0.19 ppm attributable to the methyl group on the silicon was 3:51.06, which means that one molecule of this polysiloxane contains an average of 9.0 silicon atoms. The amount of lithium silanolate (I), the amount of organosiloxane (D3), [D3] / [I], the amount of toluene, the amount of n-hexane, the amount of THF, [nonpolar solvent] / [aprotic polar solvent], and the number of silicon atoms per molecule in this example are shown in Table 1.
[0069] [Example 6] Trimethyltrivinylcyclotrisiloxane (0.54 mL, 2.0 mmol) and dehydrated toluene (2.20 mL) were placed in a 100 mL three-necked eggplant flask and dissolved under an argon atmosphere. Methyllithium (1.04 M diethyl ether solution, 5.77 mL, 6.0 mmol) was slowly added dropwise at room temperature, and stirring was continued for 30 minutes after the completion of the addition to allow the reaction to proceed. Then, hexamethylcyclotrisiloxane (D3) (2.00 g, 9.0 mmol) and dehydrated dimethylformamide (DMF) (0.19 mL, 2.5 mmol) were added in this order at room temperature. This reaction solution was stirred at room temperature for 5 hours, and dimethylchlorosilane (0.70 mL, 6.4 mmol) was added to cap the Li terminal, and then stirred at room temperature overnight. The reaction solution was extracted three times with diethyl ether, and the resulting organic layer was washed three times with saturated saline, and then dehydrated using anhydrous sodium sulfate. The solvent was removed from the resulting solution using a rotary evaporator over a period of 1.5 hours, yielding a colorless, transparent liquid.
[0070] The resulting colorless and transparent liquid 1 H-NMR measurement confirmed the formation of the target product. In addition, the integral ratio of the peak at 5.73-6.10 ppm attributable to the terminal vinyl group to the peak at 0.06-0.19 ppm attributable to the methyl group on the silicon was 3:48.25, which means that one molecule of this polysiloxane contains an average of 8.5 silicon atoms. The amount of lithium silanolate (I), the amount of organosiloxane (D3), [D3] / [I], the amount of toluene, the amount of diethyl ether, the amount of THF, [nonpolar solvent] / [aprotic polar solvent], and the number of silicon atoms per molecule in this example are shown in Table 1.
[0071] [Example 7] Trimethyltrivinylcyclotrisiloxane (0.54 mL, 2.0 mmol) and dehydrated toluene (1.60 mL) were placed in a 100 mL three-necked eggplant flask and dissolved under an argon atmosphere. Methyllithium (1.04 M diethyl ether solution, 5.77 mL, 6.0 mmol) was slowly added dropwise at room temperature, and dehydrated normal hexane (2.00 mL) was added after completion of the dropwise addition. Stirring was continued for 30 minutes to allow the reaction to proceed, after which hexamethylcyclotrisiloxane (D3) (1.33 g, 6.0 mmol) and dehydrated tetrahydrofuran (THF) (0.30 mL, 3.7 mmol) were added in this order at room temperature. This reaction solution was stirred at room temperature for 5 hours, and dimethylchlorosilane (0.70 mL, 6.4 mmol) was added to cap the Li terminal, followed by stirring at room temperature overnight. The reaction solution was extracted three times with diethyl ether, and the resulting organic layer was washed three times with saturated saline, and then dehydrated using anhydrous sodium sulfate. The solvent was removed from the resulting solution using a rotary evaporator for 1.5 hours. A colorless, transparent liquid was obtained by this operation.
[0072] The resulting colorless and transparent liquid 1 H-NMR measurement confirmed the formation of the target product. In addition, the integral ratio of the peak at 5.73-6.10 ppm attributable to the terminal vinyl group to the peak at 0.06-0.19 ppm attributable to the methyl group on the silicon was 3:42.32, which means that one molecule of this polysiloxane contains an average of 7.6 silicon atoms. The amount of lithium silanolate (I), the amount of organosiloxane (D3), [D3] / [I], the amount of toluene, the amount of diethyl ether, the amount of THF, [nonpolar solvent] / [aprotic polar solvent], and the number of silicon atoms per molecule in this example are shown in Table 1.
[0073] [Example 8] Trimethyltrivinylcyclotrisiloxane (0.54 mL, 2.0 mmol) and dehydrated toluene (0.60 mL) were placed in a 100 mL three-necked eggplant flask and dissolved under an argon atmosphere. Normal butyl lithium (1.6 M normal hexane solution, 3.80 mL, 6.0 mmol) was slowly added dropwise at room temperature. After the completion of the addition, stirring was continued for 30 minutes to proceed with the reaction, and then hexamethylcyclotrisiloxane (D3) (0.67 g, 3.0 mmol) and dehydrated tetrahydrofuran (THF) (0.28 mL, 3.4 mmol) were added in this order at room temperature. This reaction solution was stirred at room temperature for 5 hours, and dimethylchlorosilane (0.70 mL, 6.4 mmol) was added to cap the Li terminal, and then stirred at room temperature overnight. The reaction solution was extracted three times with diethyl ether, and the resulting organic layer was washed three times with saturated saline, and then dehydrated using anhydrous sodium sulfate. The solvent was removed from the resulting solution using a rotary evaporator over a period of 1.5 hours, yielding a colorless, transparent liquid.
[0074] The resulting colorless and transparent liquid 1 H-NMR measurement confirmed the formation of the target product. In addition, the integral ratio of the peak at 5.73-6.10 ppm attributable to the terminal vinyl group to the peak at 0.06-0.19 ppm attributable to the methyl group on the silicon was 3:19.6, which means that one molecule of this polysiloxane contains an average of 3.8 silicon atoms. The amount of lithium silanolate (I), the amount of organosiloxane (D3), [D3] / [I], the amount of toluene, the amount of diethyl ether, the amount of THF, [nonpolar solvent] / [aprotic polar solvent], and the number of silicon atoms per molecule in this example are shown in Table 1.
[0075] [Example 9] Polysiloxane was synthesized in the same manner as in Example 8, except that the amount of hexamethylcyclotrisiloxane (D3) used was changed to 1.33 g, 6.0 mmol, and the amount of tetrahydrofuran (THF) used was changed to 0.16 mL, 2.0 mmol. The resulting colorless and transparent liquid 1H-NMR measurement confirmed the formation of the target product. In addition, the integral ratio of the peak at 5.74-6.10 ppm attributable to the terminal vinyl group to the peak at 0.05-0.19 ppm attributable to the methyl group on the silicon was 3:35.94, which means that one molecule of this polysiloxane contains an average of 6.5 silicon atoms. The amount of lithium silanolate (I), the amount of organosiloxane (D3), [D3] / [I], the amount of toluene, the amount of n-hexane, the amount of THF, [nonpolar solvent] / [aprotic polar solvent], and the number of silicon atoms per molecule in this example are shown in Table 1.
[0076] [Example 10] Trimethyltrivinylcyclotrisiloxane (0.54 mL, 2.0 mmol) and dehydrated toluene (2.20 mL) were placed in a 100 mL three-necked eggplant flask and dissolved under an argon atmosphere. Normal butyl lithium (1.6 M normal hexane solution, 3.80 mL, 6.0 mmol) was slowly added dropwise at room temperature. After the completion of the addition, stirring was continued for 30 minutes to allow the reaction to proceed, and then hexamethylcyclotrisiloxane (D3) (2.00 g, 9.0 mmol) and dehydrated dimethylformamide (DMF) (0.15 mL, 1.9 mmol) were added in this order at room temperature. This reaction solution was stirred at room temperature for 5 hours, and dimethylchlorosilane (0.70 mL, 6.4 mmol) was added to cap the Li terminal, and then stirred at room temperature overnight. The reaction solution was extracted three times with diethyl ether, and the resulting organic layer was washed three times with saturated saline, and then dehydrated using anhydrous sodium sulfate. The solvent was removed from the resulting solution using a rotary evaporator over a period of 1.5 hours, yielding a colorless, transparent liquid.
[0077] The resulting colorless and transparent liquid 1 H-NMR measurement confirmed the formation of the target product. In addition, the integral ratio of the peak at 5.73-6.10 ppm attributable to the terminal vinyl group to the peak at 0.06-0.19 ppm attributable to the methyl group on the silicon was 3:26.28, which means that one molecule of this polysiloxane contains an average of 4.9 silicon atoms. The amount of lithium silanolate (I), the amount of organosiloxane (D3), [D3] / [I], the amount of toluene, the amount of diethyl ether, the amount of THF, [nonpolar solvent] / [aprotic polar solvent], and the number of silicon atoms per molecule in this example are shown in Table 1.
[0078] [Example 11] Trimethyltrivinylcyclotrisiloxane (0.54mL, 2.0mmol) and dehydrated toluene (1.60mL) were placed in a 100mL three-necked eggplant flask and dissolved under an argon atmosphere. Normal butyl lithium (1.6M normal hexane solution, 3.80mL, 6.0mmol) was slowly added dropwise at room temperature, and after completion of the addition, dehydrated normal hexane (2.00mL) was added. Stirring was continued for 30 minutes to allow the reaction to proceed, and then hexamethylcyclotrisiloxane (D3) (1.33g, 6.0mmol) and dehydrated tetrahydrofuran (THF) (0.16mL, 2.0mmol) were added in this order at room temperature. This reaction solution was stirred at room temperature for 5 hours, and dimethylchlorosilane (0.70mL, 6.4mmol) was added to cap the Li terminal, and then stirred at room temperature overnight. The reaction solution was extracted three times with diethyl ether, and the resulting organic layer was washed three times with saturated saline, and then dehydrated using anhydrous sodium sulfate. The solvent was removed from the resulting solution using a rotary evaporator for 1.5 hours. A colorless, transparent liquid was obtained by this operation.
[0079] The resulting colorless and transparent liquid 1 H-NMR measurement confirmed the formation of the target product. In addition, the integral ratio of the peak at 5.73-6.10 ppm attributable to the terminal vinyl group to the peak at 0.06-0.19 ppm attributable to the methyl group on the silicon was 3:20.41, which means that one molecule of this polysiloxane contains an average of 3.9 silicon atoms. The amount of lithium silanolate (I), the amount of organosiloxane (D3), [D3] / [I], the amount of toluene, the amount of diethyl ether, the amount of THF, [nonpolar solvent] / [aprotic polar solvent], and the number of silicon atoms per molecule in this example are shown in Table 1.
[0080] [Table 1]
[0081] From Table 1, it can be seen that by carrying out the synthesis under the conditions of the present invention, it is possible to obtain a polysiloxane in which the number of silicon atoms in one molecule is controlled to be 3 or more, preferably 5 or more, more preferably 6 or more, and 15 or less, preferably 13 or less, more preferably 11 or less, even more preferably 9 or less, and most preferably 7 or less.
Claims
1. A method for producing a polysiloxane, comprising polymerizing a lithium silanolate (I) represented by the following formula (2) with an organosiloxane (D3) represented by the following formula (1) in the presence of an aprotic polar solvent and a nonpolar solvent to produce a polysiloxane represented by the following formula (3): A method for producing a polysiloxane, wherein the molar ratio of the aprotic polar solvent to the nonpolar solvent ([nonpolar solvent] / [aprotic polar solvent]) is 5 to 100, and the molar ratio of the organosiloxane (D3) to the lithium silanolate (I) ([D3] / [I]) is 0.01 to 2. 【Chemistry 1】 (In the formula, R1 and R2 each independently represent an optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, an optionally substituted aromatic group, or an optionally substituted z-linear alkenyl group having 2 to 12 carbon atoms (wherein z is a number indicating the position of the double bond in the alkenyl group and is an integer equal to the number of carbon atoms in the alkenyl group minus 1).) 【Chemistry 2】 (In the formula, R3 represents a hydrogen atom, an optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, an optionally substituted aromatic group, or an optionally substituted z-linear alkenyl group having 2 to 12 carbon atoms (wherein z is a number indicating the position of the double bond in the alkenyl group and is an integer equal to the number of carbon atoms in the alkenyl group minus 1). R4 represents an optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms.) 【Chemistry 3】 (In the formula, R1 and R2 are defined as R1 and R2 in formula (1), and R3 and R4 are defined as R3 and R4 in formula (2). R5 represents a hydrogen atom, an optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, an optionally substituted aromatic group, or an optionally substituted z-linear alkenyl group having 2 to 12 carbon atoms (wherein z is a number indicating the position of the double bond in the alkenyl group and is an integer equal to the number of carbon atoms in the alkenyl group minus 1). n is an integer from 1 to 13.)
2. A polysiloxane represented by the following formula (3), which contains 3 to 15 silicon atoms in one molecule. 【Chemistry 4】 (In the formula, R1 and R2 each independently represent an optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, an optionally substituted aromatic group, or an optionally substituted z-straight-chain alkenyl group having 2 to 12 carbon atoms (wherein z is a number indicating the position of the double bond in the alkenyl group and is an integer equal to the number of carbon atoms in the alkenyl group minus 1). R3 represents a hydrogen atom, an optionally substituted saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, an optionally substituted aromatic group, or an optionally substituted z-straight-chain alkenyl group having 2 to 12 carbon atoms (wherein , z is a number indicating the position of the double bond in the alkenyl group and is an integer equal to the number of carbon atoms in the alkenyl group minus 1. R4 represents a saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms which may be substituted. R5 represents a hydrogen atom, a saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms which may be substituted, an aromatic group which may be substituted, or a z-linear alkenyl group having 2 to 12 carbon atoms which may be substituted (wherein z is a number indicating the position of the double bond in the alkenyl group and is an integer equal to the number of carbon atoms in the alkenyl group minus 1). n is an integer equal to 1 to 13.
Citation Information
Patent Citations
Production of polysiloxane
JP1986275329A
Thermally conductive silicone composition and cured product thereof
JP2022185620A
Non-aqueous electrolyte and non-aqueous electrolyte battery
WO2021251472A1
Oil-bleeding silicone rubber composition
WO2022163365A1
Production of polysiloxane
JP1989098631A