Acrylic resin emulsion for coating

The acrylic resin emulsion with layered resin particles and specific glass transition temperature differences addresses the limitations of existing emulsions, achieving superior performance in weather resistance, low-temperature film-forming, extensibility, water resistance, and frost damage resistance.

JP2024146370APending Publication Date: 2024-10-15NIPPON SHOKUBAI CO LTD

Patent Information

Application Number
JP2023059220
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing acrylic resin emulsions for paints lack comprehensive excellence in weather resistance, low-temperature film-forming properties, extensibility, water resistance, frost damage resistance, and stain resistance.

Method used

The acrylic resin emulsion is formulated with emulsion particles having at least two resin layers, containing an organosilane compound and monomer components, with a specific glass transition temperature difference between layers to enhance properties such as weather resistance, low-temperature film-forming properties, extensibility, water resistance, and frost damage resistance.

Benefits of technology

The formulation results in a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming properties, extensibility, water resistance, and frost damage resistance, with improved stain resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146370000001
    Figure 2024146370000001
  • Figure 2024146370000002
    Figure 2024146370000002
  • Figure 2024146370000003
    Figure 2024146370000003
Patent Text Reader

Abstract

To provide: a coating which forms a coating film having comprehensively excellent weather resistance, low-temperature film-forming property, elongation, water resistance, frost resistance, and stain resistance; an acrylic resin emulsion which can be used suitably for the coating and a production method thereof; and an inorganic base material having a coating film formed of the coating.SOLUTION: A resin emulsion for coating comprises emulsion particles having at least two resin layers. As raw materials for the resin layers constituting the emulsion particles, there are comprised an organosilane compound and a monomer component. The monomer-containing component used has an organosilane compound content of 20 to 100 pts.mass per 100 pts.mass of the monomer component. The glass transition temperature of the resin constituting the inner layer is 40°C or more higher than the glass transition temperature of the resin constituting the resin layer present on the inner layer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an acrylic resin emulsion for paint. More specifically, the present invention relates to an acrylic resin emulsion for paint and a method for producing the same, a paint containing the acrylic resin emulsion for paint, and an inorganic substrate having a coating film made of the paint. [Background technology]

[0002] As a coating composition capable of forming a coating film excellent in stain resistance, flexibility, water resistance, weather resistance, durability, pigment dispersibility, gloss retention, adhesion and rust prevention, a highly durable coating composition has been proposed which comprises a silicone-containing polymer emulsion comprising a silicone modifier, at least one ethylenically unsaturated monomer having a carboxyl group, and at least one other ethylenically unsaturated monomer, wherein the silicone modifier contains at least one silane having a specific silicone structure and / or a cyclic silane, and a photocatalyst (see, for example, Patent Document 1).

[0003] However, the highly durable coating composition has the drawback of being poor in extensibility and frost resistance.

[0004] In recent years, there has been a demand for the development of a coating material which forms a coating film which is comprehensively excellent in terms of weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance and stain resistance, and an acrylic resin emulsion which can be suitably used for such a coating material. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2008-038113 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in view of the above-mentioned conventional techniques, and an object of the present invention is to provide a coating material which forms a coating film which is comprehensively excellent in weather resistance, low-temperature film-forming properties, extensibility, water resistance, frost resistance and stain resistance, an acrylic resin emulsion which can be suitably used for the coating material and a method for producing the same, and an inorganic substrate having a coating film made of the coating material. [Means for solving the problem]

[0007] The present invention relates to (1) An acrylic resin emulsion for paint containing emulsion particles having at least two resin layers, the emulsion particles being made of a resin layer containing an organosilane compound and a monomer component, the monomer component containing an organosilane compound in an amount of 20 to 100 parts by mass per 100 parts by mass of the monomer component, and the glass transition temperature of the resin constituting the inner layer being 40° C. or more higher than the glass transition temperature of the resin constituting the resin layer present on the inner layer. (2) The acrylic resin emulsion for paint according to (1) above, wherein the content of the alicyclic structure-containing (meth)acrylate in all monomer components used in the emulsion particles is 20 to 80 mass%. (3) The acrylic resin emulsion for paint according to (1) above, wherein the monomer-containing component contains a piperidine compound. (4) The acrylic resin emulsion for paint according to (1) above, wherein the emulsion particles have an inner layer, an intermediate layer and an outer layer. (5) The acrylic resin emulsion for paint according to (4) above, wherein the glass transition temperature of the resin constituting the inner layer is at least 40° C. higher than the glass transition temperature of the resin constituting the intermediate layer. (6) A method for producing a resin emulsion for paint containing emulsion particles having at least two resin layers, the method comprising using a monomer-containing component containing an organosilane compound and a monomer component as raw materials for the resin layers constituting the emulsion particles, the amount of the organosilane compound being 20 to 100 parts by mass per 100 parts by mass of the monomer component, and adjusting the glass transition temperature of the inner layer to be 40°C or more higher than the glass transition temperature of the resin of an outer layer present on the inner layer; (7) A paint comprising the acrylic resin emulsion for paint according to any one of (1) to (5) above, and (8) An inorganic substrate having a coating film made of the coating material according to (7) above. Regarding. Effect of the Invention

[0008] According to the present invention, there are provided a coating material which forms a coating film which is comprehensively excellent in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance and stain resistance, an acrylic resin emulsion which can be suitably used for said coating material and a method for producing the same, and an inorganic substrate having a coating film made of said coating material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The acrylic resin emulsion for paint of the present invention is a resin emulsion for paint containing emulsion particles having at least two resin layers, as described above. The acrylic resin emulsion for paint of the present invention is characterized in that it contains an organosilane compound and a monomer component as raw materials for the resin layer constituting the emulsion particles, a monomer-containing component is used in which the amount of the organosilane compound is 20 to 100 parts by mass per 100 parts by mass of the monomer component, and the glass transition temperature of the resin constituting the inner layer is 40°C or more higher than the glass transition temperature of the resin constituting the resin layer present on the inner layer.

[0010] In the present invention, the monomer component means a component composed of a monomer. The monomer-containing component is a component that contains at least the monomer component, and may be composed of only the monomer component, or may be a component that contains the monomer component and an organosilane compound.

[0011] The acrylic resin emulsion for paint of the present invention and the paint containing the acrylic resin emulsion for paint have the above-mentioned constituent requirements, and therefore form a coating film that is comprehensively excellent in weather resistance, low-temperature film-formability, extensibility, water resistance, frost resistance and stain resistance.

[0012] The above-mentioned minimum film-forming temperature, weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance and stain resistance all refer to properties measured based on the methods described in the following examples.

[0013] [Emulsion particles] The emulsion particle has at least two resin layers. The resin layers are present in the emulsion particle in a layered form, and the boundaries between adjacent resin layers may be clear, but are not necessarily clear. It is preferable that the resins (polymers) used in each resin layer are different from each other in order to fully express the physical properties of each layer.

[0014] As described later in detail, emulsion particles having at least two resin layers can be formed by emulsion polymerizing a monomer-containing component containing an organosilane compound and a monomer component by a two-stage or more emulsion polymerization method. The number of resin layers constituting the emulsion particles is two or more layers, but from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance, and stain resistance, it is preferably 2 to 5 layers, more preferably 2 or 3 layers, and even more preferably 3 layers.

[0015] [Monomer-containing components] As a raw material for the resin layer constituting the emulsion particle, a monomer-containing component containing an organosilane compound and a monomer component is used.

[0016] [Organosilane Compound] The organosilane compound may be an organosilane compound that does not have a carbon-carbon unsaturated double bond (hereinafter referred to as a non-polymerizable organosilane compound), or an organosilane compound that has a carbon-carbon unsaturated double bond (hereinafter referred to as a polymerizable organosilane compound).

[0017] In the present invention, the polymerizable organosilane compound has a carbon-carbon unsaturated double bond, but since it is an organosilane compound, it is not included in the concept of the monomer component.

[0018] The non-polymerizable organosilane compound and the polymerizable organosilane compound may be used alone or in combination. The non-polymerizable organosilane compound and the polymerizable organosilane compound are preferably used in combination from the viewpoint of improving the water resistance and extensibility of the coating film. When the non-polymerizable organosilane compound and the polymerizable organosilane compound are used in combination, the mass ratio of the non-polymerizable organosilane compound to the polymerizable organosilane compound (non-polymerizable organosilane compound / polymerizable organosilane compound) is preferably 80 / 20 or more, more preferably 90 / 10 or more, from the viewpoint of improving the extensibility of the coating film, and is preferably 99 / 1 or less, more preferably 98 / 2 or less, and even more preferably 97 / 3 or less, from the viewpoint of improving the water resistance of the coating film.

[0019] Examples of the non-polymerizable organosilane compound include those represented by the formula (I): (R 1 ) x -Si-(R 2 ) y (I) (In the formula, R 1 is an alkyl group having 1 to 8 carbon atoms, a cycloalkyl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms; R 2 represents an alkoxy group having 1 to 4 carbon atoms, x and y each represent an integer of 1 to 3, and the sum of x and y is 4. Examples of the non-polymerizable organosilane compounds include those represented by the formula: R 1 Among these, from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance, and stain resistance, alkyl groups having 1 to 8 carbon atoms and aryl groups having 6 to 12 carbon atoms are preferred, and alkyl groups having 1 to 4 carbon atoms and aryl groups having 6 to 8 carbon atoms are more preferred. 1 From the viewpoint of further improving the low-temperature film-forming property and extensibility, the aryl group is preferably an aryl group having 6 to 12 carbon atoms, more preferably an aryl group having 6 to 8 carbon atoms, and even more preferably a phenyl group.

[0020] In the organosilane compound, R of formula (I) 1 The content of the non-polymerizable organosilane compound, which is preferably an aryl group having 6 to 12 carbon atoms, more preferably an aryl group having 6 to 8 carbon atoms, and even more preferably a phenyl group, is preferably 5 mass % or more, more preferably 10 mass % or more from the viewpoint of improving the water resistance of the coating film, and is preferably 50 mass % or less, more preferably 40 mass % or less, from the viewpoint of improving the extensibility of the coating film.

[0021] Specific examples of the non-polymerizable organosilane compound represented by formula (I) include methyltrimethoxysilane, dimethyldimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, phenyltrimethoxysilane, diphenyldimethoxysilane, phenyltriethoxysilane, diphenyldiethoxysilane, phenylmethyldimethoxysilane, cyclohexyltrimethoxysilane, dicyclohexyldimethoxysilane, cyclohexyltriethoxysilane, dicyclohexyldiethoxysilane, etc., but the present invention is not limited to these examples. Among these non-polymerizable organosilane compounds, from the viewpoint of improving the water resistance of the coating film, phenyltrimethoxysilane, diphenyldimethoxysilane, phenyltriethoxysilane, diphenyldiethoxysilane, and phenylmethyldimethoxysilane are preferred. Each of these non-polymerizable organosilane compounds may be used alone, or two or more types may be used in combination.

[0022] The polymerizable organosilane compound may, for example, be a compound represented by the formula (II): H2C=C(R 3 )-COO-R 4 -Si(R 5 )3(II) (In the formula, R 3 is a hydrogen atom or a methyl group, R 4 is an alkylene group having 1 to 8 carbon atoms, R 5 represents an alkoxy group having 1 to 4 carbon atoms. Examples of the polymerizable organosilane compounds include those represented by the formula: R 3 R is a hydrogen atom or a methyl group, but from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance and stain resistance, a methyl group is preferable. 4 is an alkylene group having 1 to 8 carbon atoms, but from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance, and stain resistance, it is preferably an alkylene group having 2 to 4 carbon atoms. 5 is an alkoxy group having 1 to 4 carbon atoms, but from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-formability, extensibility, water resistance, frost resistance, and stain resistance, it is preferably a methoxy group or an ethoxy group.

[0023] Specific examples of the polymerizable organosilane compound include γ-(meth)acryloyloxymethyltrimethoxysilane, γ-(meth)acryloyloxyethyltrimethoxysilane, γ-(meth)acryloyloxypropyltrimethoxysilane, γ-(meth)acryloyloxypropylhydroxysilane, γ-(meth)acryloyloxypropylmethylhydroxysilane, etc., but the present invention is not limited to these examples. Among these polymerizable organosilane compounds, from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming property, elongation, water resistance, frost resistance, and stain resistance, γ-(meth)acryloyloxymethyltrimethoxysilane, γ-(meth)acryloyloxyethyltrimethoxysilane, and γ-(meth)acryloyloxypropyltrimethoxysilane are preferred, and γ-(meth)acryloyloxypropyltrimethoxysilane is more preferred. These polymerizable organosilane compounds may be used alone or in combination of two or more kinds.

[0024] In the present invention, "(meth)acryloyl" means "acryloyl" or "methacryloyl", "(meth)acrylate" means "acrylate" or "methacrylate", and "(meth)acrylic" means "acrylic" or "methacrylic".

[0025] The amount of the organosilane compound per 100 parts by mass of the monomer component is 20 parts by mass or more, and preferably 25 parts by mass or more, from the viewpoint of forming a coating film which is comprehensively excellent in weather resistance, low-temperature film-formability, elongation, water resistance, frost resistance, and stain resistance, and is 100 parts by mass or less, preferably 95 parts by mass or less, more preferably 90 parts by mass or less, and even more preferably 85 parts by mass or less, from the viewpoint of suppressing gelation of the resin emulsion.

[0026] [Monomer components] Examples of the monomer component include alkyl (meth)acrylates, alicyclic structure-containing (meth)acrylates, hydroxyl group-containing (meth)acrylates, carboxyl group-containing monomers, aromatic monomers, nitrogen atom-containing monomers, oxo group-containing monomers, fluorine atom-containing monomers, epoxy group-containing monomers, ultraviolet absorbing monomers, and ultraviolet stable monomers, but the present invention is not limited to these examples. Each of these monomers may be used alone, or two or more of them may be used in combination.

[0027] Examples of alkyl (meth)acrylates include alkyl (meth)acrylates having 1 to 18 carbon atoms in the alkyl group, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, sec-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-octyl (meth)acrylate, tridecyl (meth)acrylate, n-octyl (meth)acrylate, n-lauryl (meth)acrylate, and 2-(acetoacetoxy)ethyl (meth)acrylate, but the present invention is not limited to these examples. Among alkyl (meth)acrylates, alkyl (meth)acrylates having 1 to 8 carbon atoms in the alkyl group are preferred from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance, and stain resistance. These monomers may be used alone or in combination of two or more kinds.

[0028] The content of alkyl (meth)acrylate in all monomer components used in the emulsion particles is preferably 20% by mass or more, more preferably 25% by mass or more, and even more preferably 30% by mass or more, from the viewpoint of improving the weather resistance and extensibility of the coating film, and is preferably 80% by mass or less, more preferably 75% by mass or less, and even more preferably 70% by mass or less, from the viewpoint of improving the weather resistance of the coating film.

[0029] Examples of the alicyclic structure-containing (meth)acrylate include cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, and other alicyclic structure-containing (meth)acrylates having an alicyclic structure with a carbon number of 3 to 12. These alicyclic structure-containing (meth)acrylates may be used alone or in combination of two or more kinds.

[0030] The content of the alicyclic structure-containing (meth)acrylate in all monomer components used in the emulsion particles is preferably 20 mass% or more, more preferably 25 mass% or more, and even more preferably 30 mass% or more from the viewpoint of improving the weather resistance of the coating film, and is preferably 80 mass% or less, more preferably 75 mass% or less, and even more preferably 70 mass% or less from the viewpoint of improving the low-temperature film-formability and extensibility.

[0031] Examples of hydroxyl group-containing (meth)acrylates include hydroxyl group-containing (meth)acrylates having a hydroxyalkyl group with 1 to 18 carbon atoms, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate, but the present invention is not limited to these examples. These monomers may be used alone or in combination of two or more kinds. The content of the hydroxyl group-containing monomer in the total monomer components used in the emulsion particles is preferably adjusted appropriately depending on the application of the coating material of the present invention.

[0032] Examples of the carboxyl group-containing monomer include carboxyl group-containing aliphatic monomers such as (meth)acrylic acid, maleic acid, fumaric acid, crotonic acid, itaconic acid, and maleic anhydride, but the present invention is not limited to these examples. These monomers may be used alone or in combination of two or more. The content of the carboxyl group-containing monomer in the total monomer components used in the emulsion particles is preferably adjusted appropriately depending on the application of the coating material of the present invention.

[0033] Examples of aromatic monomers include styrene monomers such as styrene, α-methylstyrene, p-methylstyrene, tert-methylstyrene, chlorostyrene, and vinyltoluene, and aralkyl (meth)acrylates, but the present invention is not limited to these examples. Examples of aralkyl (meth)acrylates include aralkyl (meth)acrylates having an aralkyl group with 7 to 18 carbon atoms, such as benzyl (meth)acrylate, phenylethyl (meth)acrylate, methylbenzyl (meth)acrylate, and naphthylmethyl (meth)acrylate, but the present invention is not limited to these examples. These aromatic monomers may be used alone or in combination of two or more. The content of aromatic monomers in the total monomer components used in the emulsion particles is preferably adjusted appropriately depending on the application of the coating material of the present invention.

[0034] Examples of the nitrogen atom-containing monomer include (meth)acrylamide, diacetone (meth)acrylamide, N-monomethyl (meth)acrylamide, N-monoethyl (meth)acrylamide, N,N-dimethyl (meth)acrylamide, Nn-propyl (meth)acrylamide, N-isopropyl (meth)acrylamide, methylene bis (meth)acrylamide, N-methylol (meth)acrylamide, N-butoxymethyl (meth)acrylamide, dimethylaminoethyl (meth)acrylamide, N,N-dimethylaminopropyl (meth)acrylamide, and diacetone (meth)acrylamide (meth)acrylamide and other (meth)acrylamide compounds, dimethylaminoethyl (meth)acrylate, and diethylaminoethyl (meth)acrylate (meth)acrylamide and other nitrogen atom-containing (meth)acrylate compounds, N-vinylpyrrolidone, and (meth)acrylonitrile, but the present invention is not limited to these examples. These nitrogen atom-containing monomers may be used alone or in combination of two or more. The content of the nitrogen atom-containing monomer in all the monomer components used in the emulsion particles is preferably adjusted appropriately depending on the application of the coating material of the present invention.

[0035] Examples of oxo group-containing monomers include (di)ethylene glycol (methoxy) (meth) acrylates such as ethylene glycol (meth) acrylate, ethylene glycol methoxy (meth) acrylate, diethylene glycol (meth) acrylate, and diethylene glycol methoxy (meth) acrylate, but the present invention is not limited to these examples. These monomers may be used alone or in combination of two or more kinds. The content of the oxo group-containing monomer in the total monomer components used in the emulsion particles is preferably adjusted appropriately according to the application of the coating material of the present invention.

[0036] Examples of fluorine atom-containing monomers include fluorine atom-containing alkyl (meth)acrylates having 2 to 6 carbon atoms in the fluoroalkyl group, such as trifluoroethyl (meth)acrylate, tetrafluoropropyl (meth)acrylate, and octafluoropentyl (meth)acrylate, but the present invention is not limited to these examples. These monomers may be used alone or in combination of two or more kinds. The content of the fluorine atom-containing monomer in the total monomer components used in the emulsion particles is preferably adjusted appropriately depending on the application of the coating material of the present invention.

[0037] Examples of epoxy group-containing monomers include epoxy group-containing (meth)acrylates such as glycidyl (meth)acrylate, but the present invention is not limited to these examples. The content of the epoxy group-containing monomer in the total monomer components used in the emulsion particles is preferably adjusted appropriately depending on the application of the coating material of the present invention.

[0038] Examples of ultraviolet absorbing monomers include benzotriazole-based ultraviolet absorbing monomers, benzophenone-based ultraviolet absorbing monomers, etc., but the present invention is not limited to these examples. These monomers may be used alone or in combination of two or more kinds.

[0039] Examples of the benzotriazole-based ultraviolet absorbing monomer include 2-[2'-hydroxy-5'-(meth)acryloyloxymethylphenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxyethylphenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxymethylphenyl]-5-tert-butyl-2H-benzotriazole, and 2-[2'-hydroxy-5'-(meth)acryloyloxymethylphenyl]-5-tert-butyl-2H-benzotriazole. ) Acryloylaminomethyl-5'-tert-octylphenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxypropylphenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxyhexylphenyl]-2H-benzotriazole, 2-[2'-hydroxy-3'-tert-butyl-5'-(meth)acryloyloxyethylphenyl]-2H-benzotriazole , 2-[2'-hydroxy-3'-tert-butyl-5'-(meth)acryloyloxyethylphenyl]-5-chloro-2H-benzotriazole, 2-[2'-hydroxy-5'-tert-butyl-3'-(meth)acryloyloxyethylphenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxyethylphenyl]-5-chloro-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxyethylphenyl]-5-chloro-2H-benzotriazole, Examples of the benzotriazole-based ultraviolet absorbing monomer include 2-[2'-hydroxy-5'-(meth)acryloyloxyethylphenyl]-5-cyano-2H-benzotriazole, 2-[2'-hydroxy-5'-(β-(meth)acryloyloxyethoxy)-3'-tert-butylphenyl]-5-tert-butyl-2H-benzotriazole, but the present invention is not limited to these examples. These benzotriazole-based ultraviolet absorbing monomers may be used alone or in combination of two or more kinds.

[0040] Benzophenone-based ultraviolet absorbing monomers include, for example, 2-hydroxy-4-(meth)acryloyloxybenzophenone, 2-hydroxy-4-[2-hydroxy-3-(meth)acryloyloxy]propoxybenzophenone, 2-hydroxy-4-[2-(meth)acryloyloxy]ethoxybenzophenone, 2-hydroxy-4-[3-(meth)acryloyloxy-2-hydroxypropoxy]benzophenone, 2-hydroxy-3-tert-butyl-4-[2-(meth)acryloyloxy]butoxybenzophenone, but the present invention is not limited to these examples. These benzophenone-based ultraviolet absorbing monomers may be used alone or in combination of two or more kinds.

[0041] Examples of the ultraviolet ray stable monomer include 4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidine, 4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 4-(meth)acryloyloxy-1,2,2,6,6-pentamethylpiperidine, 4-(meth)acryloyl-1-methoxy-2,2,6,6-tetramethylpiperidine, 4-cyano-4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidine, 1-(meth)acryloyl-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 4-(meth)acryloylamino-1,2,2,6,6-pentamethylpiperidine, Examples of the polymerizable piperidine compound include lysine, 4-cyano-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 1-(meth)acryloyl-4-cyano-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, and other (meth)acryloyloxy group-containing piperidines, and 4-crotonoylamino-2,2,6,6-tetramethylpiperidine, 4-crotonoyloxy-2,2,6,6-tetramethylpiperidine, and other crotonoyl group-containing piperidines, but the present invention is not limited to these examples. These ultraviolet stable monomers may be used alone or in combination of two or more kinds.

[0042] In the present invention, from the viewpoint of forming a coating film that is excellent in weather resistance, low-temperature film-forming property, elongation, water resistance, frost resistance and stain resistance, it is preferable that a polymerizable piperidine compound is contained as an ultraviolet stable monomer in the raw material of the resin layer that constitutes the emulsion particle.Among the polymerizable piperidine compounds, from the viewpoint of forming a coating film that is excellent in weather resistance, low-temperature film-forming property, elongation, water resistance, frost resistance and stain resistance, it is more preferable that the piperidine that contains (meth)acryloyloxy group is contained.

[0043] In the present invention, from the viewpoint of improving the weather resistance of the coating film, it is preferable that the raw material of the resin layer constituting the emulsion particles contains a piperidine compound.

[0044] The piperidine compound includes the above-mentioned polymerizable piperidine compound and the non-polymerizable piperidine compound that does not have a polymerizable group.The polymerizable piperidine compound and the non-polymerizable piperidine compound may be used alone or in combination.Among the piperidine compounds, the polymerizable piperidine compound is preferred from the viewpoint of maintaining the weather resistance of the coating film.The polymerizable piperidine compound is used as the above-mentioned monomer component and is also used as the piperidine compound.

[0045] Examples of non-polymerizable piperidine compounds include tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)butane-1,2,3,4-tetracarboxylate, tetrakis(2,2,6,6-tetramethyl-4-piperidyl)butane-1,2,3,4-tetracarboxylate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(1-undecanoxy-2,2,6,6-tetramethylpiperidin-4-yl)carbonate, but the present invention is not limited to these examples.These non-polymerizable piperidine compounds may be used alone or in combination.

[0046] The amount of the piperidine compound per 100 parts by mass of the total monomer components used in the emulsion particles is preferably 0.5 to 10 parts by mass, more preferably 1 to 5 parts by mass, from the viewpoint of forming a coating film which is comprehensively excellent in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance and stain resistance.

[0047] [Weight average molecular weight of resin (polymer) constituting each resin layer] The weight average molecular weight of the resin (polymer) constituting each resin layer is preferably 100,000 or more, more preferably 300,000 or more, even more preferably 550,000 or more, and particularly preferably 600,000 or more, from the viewpoint of improving the water permeability of the coating film. The upper limit of the weight average molecular weight of the resin (polymer) is not particularly limited when it has a crosslinked structure, since it is difficult to measure the weight average molecular weight, but when it does not have a crosslinked structure, it is preferably 5,000,000 or less from the viewpoint of improving film-forming properties.

[0048] In the present invention, the weight average molecular weight of a resin (polymer) refers to the weight average molecular weight (polystyrene equivalent) measured using gel permeation chromatography (manufactured by Tosoh Corporation, product number: HLC-8120GPC, columns: TSKgel G-5000HXL and TSKgel GMHXL-L in series).

[0049] [Resin Layer Constituting Emulsion Particle] The resin layers constituting the emulsion particles will be described below. As described above, the emulsion particles have at least two resin layers.

[0050] [Inner layer] The inner layer is a resin layer constituting the center of an emulsion particle having at least two resin layers. The monomer-containing component used as the raw material for the inner layer preferably contains a monomer component and an organosilane compound from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance, and stain resistance.

[0051] The monomer component may be any of the various monomers described above. From the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming properties, extensibility, water resistance, frost resistance, and stain resistance, it is preferable to use an alicyclic structure-containing (meth)acrylate as an essential component.

[0052] The content of the alicyclic structure-containing (meth)acrylate in the monomer component is preferably 65 to 100 mass%, more preferably 70 to 100 mass%, and even more preferably 75 to 100 mass%, from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-formability, extensibility, water resistance, frost resistance, and stain resistance.

[0053] As the monomer other than the alicyclic structure-containing (meth)acrylate, from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance and stain resistance, at least one monomer selected from the group consisting of alkyl (meth)acrylates, hydroxyl group-containing (meth)acrylates and carboxyl group-containing monomers can be preferably used.

[0054] The content of monomers other than the alicyclic structure-containing (meth)acrylate in the monomer component is preferably 0 to 35 mass %, more preferably 0 to 30 mass %, and even more preferably 0 to 25 mass %, from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-formability, extensibility, water resistance, frost resistance, and stain resistance.

[0055] The content of the monomer component in the monomer-containing component is preferably 30 to 90 mass %, and more preferably 35 to 85 mass %, from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance, and stain resistance.

[0056] From the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance, and stain resistance, it is preferable that the organosilane compound is a combination of a polymerizable organosilane compound and a non-polymerizable organosilane compound. From the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance, and stain resistance, it is preferable that the mass ratio of the polymerizable organosilane compound to the non-polymerizable organosilane compound (polymerizable organosilane compound / non-polymerizable organosilane compound) is 1 / 99 to 20 / 80.

[0057] In the organosilane compound, R 1 The content of the non-polymerizable organosilane compound, in which the aryl group is preferably an aryl group having 6 to 12 carbon atoms, more preferably an aryl group having 6 to 8 carbon atoms, and even more preferably a phenyl group, is preferably 5 mass % or more, more preferably 10 mass % or more, from the viewpoint of improving low-temperature film-formability and extensibility, and is preferably 50 mass % or less, more preferably 40 mass % or less, and even more preferably 30 mass % or less, from the viewpoint of improving weather resistance.

[0058] The content of the organosilane compound in the monomer-containing component is preferably 10 to 70 mass %, and more preferably 15 to 65 mass %, from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-formability, extensibility, water resistance, frost resistance, and stain resistance.

[0059] The glass transition temperature of the resin (polymer) constituting the inner layer is preferably 40°C or higher, more preferably 45°C or higher, and even more preferably 50°C or higher, from the viewpoint of forming a coating film which is comprehensively excellent in weather resistance, low-temperature film-formability, elongation, water resistance, frost resistance, and stain resistance, and is preferably 130°C or lower, more preferably 100°C or lower, and even more preferably 90°C or lower, from the viewpoint of forming a coating film which is comprehensively excellent in weather resistance, low-temperature film-formability, elongation, water resistance, frost resistance, and stain resistance.

[0060] In this specification, the glass transition temperature of a resin (polymer) is expressed by the glass transition temperature of a homopolymer of a monomer used in a monomer component constituting the resin (polymer) as shown in formula (III): 1 / Tg=Σ(Wm / Tgm) / 100 (III) (In the formula, Wm represents the content (mass%) of monomer m in the monomer components constituting the polymer, and Tgm represents the glass transition temperature (absolute temperature: K) of a homopolymer of monomer m.) This refers to the temperature calculated based on the Fox formula,

[0061] In the present invention, the glass transition temperature of the resin (polymer) constituting the emulsion particles means the glass transition temperature calculated based on the formula (III), unless otherwise specified.

[0062] The glass transition temperature of the entire resin layers constituting an emulsion particle having a plurality of resin layers means a glass transition temperature calculated from the mass fraction of each monomer in all the monomer components used in the multistage emulsion polymerization and the glass transition temperature of the homopolymer of the corresponding monomer.

[0063] For monomers with unknown glass transition temperatures such as special monomers and polyfunctional monomers, if the total amount of monomers with unknown glass transition temperatures in the monomer component is 10% by mass or less, the glass transition temperature is determined using only monomers with known glass transition temperatures. If the total amount of monomers with unknown glass transition temperatures in the monomer component exceeds 10% by mass, the glass transition temperature of the polymer is determined by differential scanning calorimetry (DSC), differential thermal analysis (DTA), thermomechanical analysis (TMA), etc.

[0064] The glass transition temperature of the resin (polymer) can be easily adjusted by adjusting the composition of the monomer components. The composition of the monomer components can be determined taking into account the glass transition temperature of the resin (polymer) constituting the emulsion particles.

[0065] The glass transition temperature of the resin (polymer) is, for example, 83°C for a homopolymer of cyclohexyl methacrylate, 105°C for a homopolymer of methyl methacrylate, -70°C for a homopolymer of 2-ethylhexyl acrylate, -56°C for a homopolymer of n-butyl acrylate, -44°C for a homopolymer of 2-octyl acrylate, -25°C for a homopolymer of 2-octyl methacrylate, 55°C for a homopolymer of 2-hydroxyethyl methacrylate, 106°C for a homopolymer of acrylic acid, 130°C for a homopolymer of methacrylic acid, 165°C for a homopolymer of acrylamide, 130°C for a homopolymer of 4-methacryloyloxy-1,2,2,6,6-pentamethylpiperidine, and 130°C for a monomer of 4-methacryloyloxy-2,2,6,6-tetramethylpiperidine.

[0066] In the present invention, from the viewpoint of forming a coating film which is comprehensively excellent in weather resistance, low-temperature film-formability, extensibility, water resistance, frost resistance and stain resistance, the glass transition temperature of the resin constituting the inner layer is at least 40° C. higher than the glass transition temperature of the resin constituting the resin layer present on the inner layer.

[0067] Therefore, when the emulsion particles have a two-layer structure consisting of an inner layer and an outer layer, from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-formability, extensibility, water resistance, frost resistance, and stain resistance, the glass transition temperature of the resin constituting the inner layer is preferably at least 40°C higher than the glass transition temperature of the resin constituting the outer layer, more preferably at least 50°C higher than the glass transition temperature of the resin constituting the outer layer, and even more preferably at least 60°C higher than the glass transition temperature of the resin constituting the outer layer. Furthermore, when the emulsion particles have a three-layer structure consisting of an inner layer, an intermediate layer, and an outer layer, from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-formability, extensibility, water resistance, frost resistance, and stain resistance, the glass transition temperature of the resin constituting the inner layer is preferably at least 40°C higher than the glass transition temperature of the resin constituting the intermediate layer present on the inner layer, more preferably at least 50°C higher than the glass transition temperature of the resin constituting the intermediate layer, and even more preferably at least 60°C higher than the glass transition temperature of the resin constituting the intermediate layer.

[0068] [Middle class] The intermediate layer is a resin layer that exists between the inner layer and the outer layer of an emulsion particle having at least three resin layers. Therefore, when an emulsion particle is composed of two resin layers, there is no intermediate layer in the emulsion particle.

[0069] When the emulsion particle is composed of two resin layers, a resin layer made of another polymer may be formed between the inner layer and the outer layer, if necessary, within the scope of the present invention. When the emulsion particle is composed of three or more resin layers, a resin layer made of another polymer may be formed between the inner layer and the intermediate layer, if necessary, within the scope of the present invention.

[0070] From the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance, and stain resistance, the monomer-containing component used as the raw material for the intermediate layer preferably contains the monomer component at a content of 95% by mass or more and the organosilane compound at a content of 5% by mass or less, and more preferably contains the monomer component at a content of 97% by mass or more and the organosilane compound at a content of 3% by mass or less. Note that the upper limit of the monomer component in the monomer-containing component is 100% by mass, and the lower limit of the organosilane compound is 0% by mass.

[0071] From the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance, and stain resistance, the monomer component may be a monomer such as an alkyl (meth)acrylate, an alicyclic structure-containing (meth)acrylate, a hydroxyl group-containing (meth)acrylate, a carboxyl group-containing monomer, a nitrogen atom-containing monomer, etc. These monomers may be used alone or in combination of two or more kinds.

[0072] From the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance, and stain resistance, it is preferable that the monomer component contains an alicyclic structure-containing (meth)acrylate as an essential component. From the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance, and stain resistance, the content of the alicyclic structure-containing (meth)acrylate in the monomer component is preferably 15 to 50 mass%, more preferably 20 to 45 mass%, from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance, and stain resistance.

[0073] From the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming properties, extensibility, water resistance, frost resistance, and stain resistance, the monomer other than the alicyclic structure-containing (meth)acrylate is preferably at least one monomer selected from the group consisting of alkyl (meth)acrylates, hydroxyl group-containing (meth)acrylates, carboxyl group-containing monomers, and nitrogen atom-containing monomers, and more preferably at least one monomer selected from the group consisting of alkyl (meth)acrylates, hydroxyl group-containing (meth)acrylates, (meth)acrylic acid, and (meth)acrylamide.

[0074] The content of monomers other than the alicyclic structure-containing (meth)acrylate in the monomer component is preferably 50 to 85 mass %, more preferably 55 to 80 mass %, from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-formability, extensibility, water resistance, frost resistance, and stain resistance.

[0075] The glass transition temperature of the resin constituting the intermediate layer is preferably -10°C or lower, more preferably -15°C or lower, from the viewpoint of forming a coating film that is excellent in low-temperature film-forming properties and elongation, and is preferably -60°C or higher, more preferably -55°C or higher, and even more preferably -50°C or higher, from the viewpoint of forming a coating film that is excellent in water resistance, frost resistance, and stain resistance.

[0076] [Outer layer] The outer layer is a resin layer constituting the outermost layer of the emulsion particle. When the emulsion particle has at least three resin layers, a resin layer made of another polymer may be formed between the intermediate layer and the outer layer as necessary within a range that does not impair the object of the present invention.

[0077] The monomer-containing component used as a raw material for the outer layer preferably contains a monomer component and an organosilane compound, from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-formability, extensibility, water resistance, frost resistance, and stain resistance.

[0078] From the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance, and stain resistance, the monomer component may be a monomer such as an alkyl (meth)acrylate, an alicyclic structure-containing (meth)acrylate, a hydroxyl group-containing (meth)acrylate, a carboxyl group-containing monomer, an ultraviolet ray-stable monomer, etc. Each of these monomers may be used alone, or two or more kinds may be used in combination.

[0079] It is preferable that the monomer component contains an alicyclic structure-containing (meth)acrylate as an essential component, from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming properties, extensibility, water resistance, frost resistance, and stain resistance.

[0080] The content of the alicyclic structure-containing (meth)acrylate in the monomer component is preferably 20 to 60 mass %, more preferably 25 to 55 mass %, from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance and stain resistance.

[0081] From the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming properties, extensibility, water resistance, frost resistance, and stain resistance, it is preferable that the monomer other than the alicyclic structure-containing (meth)acrylate is at least one monomer selected from the group consisting of alkyl (meth)acrylates, hydroxyl group-containing (meth)acrylates, and ultraviolet-stable monomers.

[0082] The content of the monomer other than the alicyclic structure-containing (meth)acrylate in the monomer component is preferably 40 to 80 mass %, more preferably 45 to 75 mass %, from the viewpoint of forming a coating film that is excellent overall in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance, and stain resistance. The monomer other than the alicyclic structure-containing (meth)acrylate may contain, for example, a carboxyl group-containing monomer such as (meth)acrylic acid, within a range that does not impair the object of the present invention.

[0083] The content of the monomer component in the monomer-containing component is preferably 30 to 90 mass %, and more preferably 35 to 85 mass %, from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance, and stain resistance.

[0084] From the viewpoint of forming a coating film which is comprehensively excellent in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance and stain resistance, it is preferable that a polymerizable organosilane compound and a non-polymerizable organosilane compound are used in combination.

[0085] The mass ratio of the polymerizable organosilane compound to the non-polymerizable organosilane compound (polymerizable organosilane compound / non-polymerizable organosilane compound) is preferably 1 / 99 to 25 / 75, and more preferably 3 / 97 to 10 / 90, from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance, and stain resistance.

[0086] In the organosilane compound, R 1 The content of the non-polymerizable organosilane compound, in which the aryl group is preferably an aryl group having 6 to 12 carbon atoms, more preferably an aryl group having 6 to 8 carbon atoms, and even more preferably a phenyl group, is preferably 5 mass % or more, more preferably 10 mass % or more, from the viewpoint of improving low-temperature film-formability and extensibility, and is preferably 50 mass % or less, more preferably 40 mass % or less, and even more preferably 30 mass % or less, from the viewpoint of improving weather resistance.

[0087] The content of the organosilane compound in the monomer-containing component is preferably 10 to 70 mass %, and more preferably 15 to 65 mass %, from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-formability, extensibility, water resistance, frost resistance, and stain resistance.

[0088] In addition, the monomer-containing component used as the raw material of the resin layer of the outer layer preferably contains the piperidine compound from the viewpoint of improving the weather resistance of the coating film.Among the piperidine compounds, from the viewpoint of maintaining the weather resistance of the coating film, polymerizable piperidine compounds are preferred, and from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance and stain resistance, (meth)acryloyloxy group-containing piperidines are more preferred.

[0089] The content of the piperidine compound in the monomer component used in the monomer-containing component is preferably 1.5 mass % or more, more preferably 2 mass % or more, and even more preferably 2.5 mass % or more, from the viewpoint of improving the weather resistance of the coating film, and is preferably 10 mass parts or less, more preferably 8 mass parts or less, from the viewpoint of forming a coating film that is comprehensively excellent not only in weather resistance but also in low-temperature film-formability, elongation, water resistance, frost resistance and stain resistance.

[0090] The glass transition temperature of the resin constituting the outer layer is preferably -40°C or higher, more preferably -35°C or higher, from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, water resistance, frost resistance, and stain resistance, and is preferably 40°C or lower, more preferably 20°C or lower, and even more preferably 10°C or lower, from the viewpoint of forming a coating film that is excellent in low-temperature film-forming properties and elongation.

[0091] [Ratio of each resin layer of emulsion particles] When the emulsion particles have two resin layers, the mass ratio of the resin layer constituting the inner layer to the resin layer constituting the outer layer (resin layer constituting the inner layer / resin layer constituting the outer layer) is preferably 20 / 80 or more, more preferably 30 / 70 or more, and even more preferably 40 / 60 or more, from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-formability, elongation, water resistance, frost resistance and contamination resistance, and is preferably 80 / 20 or less, more preferably 70 / 30 or less, and even more preferably 60 / 40 or less, from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-formability, elongation, water resistance, frost resistance and contamination resistance.

[0092] When the emulsion particles have three resin layers, from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-formability, extensibility, water resistance, frost resistance, and stain resistance, the content of the resin layer constituting the inner layer in the emulsion particles is preferably 10% by mass or more, more preferably 15% by mass or more, the content of the resin layer constituting the middle layer in the emulsion particles is preferably 20% by mass or more, more preferably 25% by mass or more, and the content of the resin layer constituting the outer layer in the emulsion particles is preferably 10% by mass or more, more preferably 15% by mass or more. In addition, from the viewpoint of forming a coating film that is comprehensively excellent in weather resistance, low-temperature film-formability, extensibility, water resistance, frost resistance, and stain resistance, the content of the resin layer constituting the inner layer in the emulsion particle is preferably 50 mass % or less, more preferably 45 mass % or less, the content of the resin layer constituting the intermediate layer in the emulsion particle is preferably 60 mass % or less, more preferably 55 mass % or less, and the content of the polymer constituting the outer layer in the emulsion particle is preferably 50 mass % or less, more preferably 45 mass % or less.

[0093] [Glass transition temperature of entire emulsion particles] The glass transition temperature of the entire emulsion particles is preferably -20°C or higher, more preferably -15°C or higher, from the viewpoint of forming a coating film that is excellent in water resistance, frost resistance, and stain resistance, and is preferably 50°C or lower, more preferably 30°C or lower, and even more preferably 20°C or lower, from the viewpoint of forming a coating film that is excellent in low-temperature film-forming properties and elongation.

[0094] [Preparation of resin emulsion for paint] The resin emulsion for paint containing emulsion particles contains an organosilane compound and a monomer component as raw materials for the resin layer constituting the emulsion particles, and can be prepared by using a monomer-containing component in which the amount of the organosilane compound is 20 to 100 parts by mass per 100 parts by mass of the monomer component, and by adjusting the glass transition temperature of the inner layer to be 40°C or more higher than the glass transition temperature of the resin constituting the outer layer present on the inner layer.

[0095] Examples of the method for emulsion-polymerizing the monomer-containing component containing the organosilane compound and the monomer component include a method of dissolving an emulsifier in a medium such as an aqueous medium containing water and a water-soluble organic solvent such as water or a lower alcohol such as methanol, and dropping the monomer-containing component and the polymerization initiator, and a method of dropping the monomer-containing component that has been emulsified in advance using an emulsifier and water into water or an aqueous medium, but the present invention is not limited to only such a method. The amount of the medium may be appropriately set in consideration of the amount of non-volatile matter contained in the resulting resin emulsion.

[0096] Examples of the emulsifier include anionic emulsifiers, nonionic emulsifiers, cationic emulsifiers, amphoteric emulsifiers, and polymeric emulsifiers. These emulsifiers may be used alone or in combination of two or more kinds.

[0097] Examples of the anionic emulsifier include alkyl sulfate salts such as ammonium dodecyl sulfate and sodium dodecyl sulfate; alkyl sulfonate salts such as ammonium dodecyl sulfonate and sodium dodecyl sulfonate; alkyl aryl sulfonate salts such as ammonium dodecyl benzene sulfonate and sodium dodecyl naphthalene sulfonate; polyoxyethylene alkyl sulfate salts; polyoxyethylene alkyl aryl sulfate salts; dialkyl sulfosuccinates; aryl sulfonic acid-formalin condensates; and fatty acid salts such as ammonium laurate and sodium stearate, but the present invention is not limited to these examples.

[0098] Examples of nonionic emulsifiers include polyoxyethylene alkyl ethers, polyoxyethylene alkylaryl ethers, condensates of polyethylene glycol and polypropylene glycol, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, fatty acid monoglycerides, and condensates of ethylene oxide and aliphatic amines; however, the present invention is not limited to these examples.

[0099] Examples of cationic emulsifiers include alkyl ammonium salts such as dodecyl ammonium chloride, but the present invention is not limited to these examples.

[0100] Examples of amphoteric emulsifiers include betaine ester emulsifiers, but the present invention is not limited to these examples.

[0101] Examples of polymeric emulsifiers include poly(meth)acrylates such as sodium polyacrylate; polyvinyl alcohol; polyvinylpyrrolidone; polyhydroxyalkyl(meth)acrylates such as polyhydroxyethyl acrylate; and polymers containing one or more of the monomers constituting these polymers as copolymerization components, but the present invention is not limited to these examples.

[0102] As the emulsifier, from the viewpoint of improving the mechanical stability of the emulsion particles, an emulsifier having a reactive group, i.e., a so-called reactive emulsifier, is preferred, and from the viewpoint of environmental protection, a non-nonylphenyl type emulsifier is preferred.

[0103] Examples of reactive emulsifiers include propenyl-alkyl sulfosuccinate salts, (meth)acrylic acid polyoxyethylene sulfonate salts, (meth)acrylic acid polyoxyethylene phosphonate salts (e.g., Sanyo Chemical Industries, Ltd., product name: ELEMINOL RS-30, etc.), polyoxyethylene alkylpropenyl phenyl ether ammonium sulfate (e.g., Daiichi Kogyo Seiyaku Co., Ltd., product name: AQUALON HS-10, AQUALON BC-10, etc.), allyloxymethyl alkyloxy polyoxyethylene sulfonate salts (e.g., Daiichi Kogyo Seiyaku Co., Ltd., product name: AQUALON KH-10, etc.), allyloxymethyl nonyl phenoxyethyl hydroxy polyoxyethylene sulfonate salts (e.g., ADEKA Corporation, product name: ADEKA REASOAP SE-10, etc.), allyloxymethyl alkoxyethyl hydroxy polyoxyethylene sulfate salts (e.g., ADEKA Corporation, product name: ADEKA REASOAP SR-10, SR-20, SR-30, etc.), biphenylsulfonates, Examples of suitable polyoxyethylene methacrylated sulfonate salts include polyoxyethylene polycyclic phenyl ether methacrylated sulfonate salts (e.g., trade name: Antox MS-60, manufactured by Nippon Nyukazai Co., Ltd.), allyloxymethylalkoxyethylhydroxypolyoxyethylene (e.g., trade name: Adeka Reasoap ER-20, manufactured by ADEKA Corporation), polyoxyethylene alkylpropenylphenyl ether (e.g., trade name: Aqualon RN-20, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.), allyloxymethylnonylphenoxyethylhydroxypolyoxyethylene (e.g., trade name: Adeka Reasoap NE-10, manufactured by ADEKA Corporation), polyoxyethylene styrenated propenylphenyl ether sulfate salts (e.g., trade name: Aqualon AR-10, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.), and polyoxyethylene styrenated propenylphenyl ether sulfate (e.g., trade name: Aqualon AN-10, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.), but the present invention is not limited to these examples.

[0104] The amount of emulsifier per 100 parts by mass of the monomer-containing component is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, from the viewpoint of improving the homopolymerization stability, and is preferably 10 parts by mass or less, more preferably 7 parts by mass or less, and even more preferably 5 parts by mass or less, from the viewpoint of improving the water permeability resistance of the coating film.

[0105] Examples of the polymerization initiator include azo compounds such as azobisisobutyronitrile, 2,2-azobis(2-methylbutyronitrile), 2,2-azobis(2,4-dimethylvaleronitrile), 2,2-azobis(2-diaminopropane) hydrochloride, 4,4-azobis(4-cyanovaleric acid), and 2,2-azobis(2-methylpropionamidine); persulfates such as potassium persulfate and ammonium persulfate; and peroxides such as hydrogen peroxide, benzoyl peroxide, parachlorobenzoyl peroxide, lauroyl peroxide, and ammonium peroxide, but the present invention is not limited to these examples. These polymerization initiators may be used alone or in combination of two or more.

[0106] The amount of polymerization initiator per 100 parts by mass of the monomer component is preferably 0.01 part by mass or more, more preferably 0.03 part by mass or more, from the viewpoint of increasing the polymerization rate and reducing the amount of remaining unreacted monomer, and is preferably 1 part by mass or less, more preferably 0.5 part by mass or less, from the viewpoint of improving the water permeability of the coating film.

[0107] The method of adding the polymerization initiator is not particularly limited. Examples of the method of addition include batch charging, divided charging, continuous dropwise addition, etc. In addition, in order to hasten the end of the polymerization reaction, a part of the polymerization initiator may be added to the flask before or after the addition of the monomer-containing component to the reaction system.

[0108] In order to promote the decomposition of the polymerization initiator, a suitable amount of a decomposer for the polymerization initiator, such as a reducing agent such as sodium hydrogen sulfite, or a transition metal salt such as ferrous sulfate, may be added to the reaction system. In addition, a suitable amount of an additive, such as a chain transfer agent, such as a compound having a thiol group, such as tert-dodecyl mercaptan, a pH buffer, a chelating agent, or a film-forming aid, may be added to the reaction system in the flask, if necessary.

[0109] The atmosphere in which the monomer-containing components are emulsion-polymerized is not particularly limited, but from the viewpoint of increasing the efficiency of the polymerization initiator, an inert gas such as nitrogen gas is preferable.

[0110] The polymerization temperature when emulsion-polymerizing the monomer-containing component is not particularly limited, but is usually preferably 50 to 100° C., more preferably 60 to 95° C. The polymerization temperature may be constant or may be changed during the polymerization reaction.

[0111] The polymerization time for emulsion-polymerizing the monomer-containing components is not particularly limited and may be appropriately set depending on the progress of the polymerization reaction, but is usually about 2 to 9 hours.

[0112] By repeating the procedure of emulsion polymerizing the monomer-containing component to prepare a resin emulsion containing emulsion particles as described above two or more times, a resin emulsion for paint containing emulsion particles having at least two resin layers can be prepared.

[0113] [Performance of resin emulsion for paint] From the viewpoint of improving the low-temperature film-formability and extensibility of the coating film, it is preferable that the solubility parameter (hereinafter referred to as SP value) of the resin (polymer) constituting the outer layer of the emulsion particle is higher than the SP value of the polymer constituting the inner layer.

[0114] The SP value is a value defined by the regular solution theory introduced by Hildebrand, and is also a measure of the solubility of a two-component solution. In general, substances with similar SP values ​​tend to mix easily with each other. Therefore, the SP value is also a measure of how easily a solute and a solvent mix.

[0115] The average particle size of the emulsion particles is not particularly limited, but from the viewpoint of improving the mechanical stability of the emulsion particles themselves, it is preferably 50 nm or more, more preferably 100 nm or more, and from the viewpoint of improving the water resistance of the coating film, it is preferably 300 nm or less, more preferably 200 nm or less.

[0116] In this specification, the average particle size of emulsion particles means the volume average particle size measured using a particle size distribution measuring device (manufactured by Particle Sizing Systems, product name: NICOMP Model 380) using the dynamic light scattering method.

[0117] The nonvolatile content in the resin emulsion is preferably 30% by mass or more, more preferably 35% by mass or more, from the viewpoint of improving productivity, and is preferably 70% by mass or less, more preferably 60% by mass or less, from the viewpoint of improving handleability.

[0118] The amount of non-volatile matter in the resin emulsion was determined by weighing 1 g of the resin emulsion, drying it in a hot air dryer at a temperature of 110° C. for 1 hour, and calculating the non-volatile matter from the resulting residue using the formula (IV): [Non-volatile content in resin emulsion (mass%)] = ([mass of residue] ÷ [1 g of resin emulsion]) × 100 (IV) This means the value calculated based on

[0119] From the viewpoint of improving the film-forming properties of the coating film, the minimum film-forming temperature (MFT) of the resin emulsion is preferably 0 to 30° C. The minimum film-forming temperature of the resin emulsion can be adjusted, for example, by adjusting the glass transition temperature of the entire emulsion particle or the glass transition temperature of the outermost layer.

[0120] The minimum film-forming temperature of a resin emulsion means the boundary temperature between the film-formed and non-film-formed areas when the resin emulsion is applied in a band shape on a flat plate having an appropriate temperature gradient, and is defined as "the minimum temperature at which a uniform coating film without cracks is formed."

[0121] The minimum film-forming temperature of the resin emulsion can be measured, for example, according to JIS K6828-2 (2003). More specifically, using an MFT tester (manufactured by Tester Sangyo Co., Ltd., product number: TP-801 LT), a coating film of the resin emulsion having a thickness of 250 μm after drying is formed on a grooveless stainless steel plate with an applicator, and the minimum temperature (°C) at which a crack-free, uniform coating film is formed is measured. The presence or absence of cracks in the coating film can be visually determined according to JIS K6828-2. Note that, when the minimum film-forming temperature of the coating film is 0°C or lower, the minimum film-forming temperature of the coating film is considered to be 0°C.

[0122] 〔paint〕

[0123] The paint of the present invention contains the acrylic resin emulsion for paint. The acrylic resin emulsion for paint can be used as a clear paint as it is, or can be used as an enamel paint by adding an appropriate amount of a colorant such as a dye or pigment to the acrylic resin emulsion for paint.

[0124] The coating material of the present invention may contain additives as necessary. Examples of additives include dispersants, defoamers, thickeners, rheology control agents, foaming agents, plasticizers, wetting agents, antiblocking agents, antiaging agents, preservatives, polymerization inhibitors, antistatic agents, UV absorbers, UV stabilizers, silane coupling agents, flame retardants, leveling agents, plasticizers, and antioxidants, but the present invention is not limited to these examples. These additives may be used alone or in combination of two or more types. The amount of additives contained in the coating material varies depending on the type of additive, so it is preferable to appropriately adjust it depending on the type of additive.

[0125] The paint obtained as described above uses the acrylic resin emulsion for paint of the present invention, and therefore forms a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance, and stain resistance, and can be suitably used as a topcoat paint. In addition, since the paint forms a coating film that is comprehensively excellent in weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance, and stain resistance, it can be suitably used as a paint to be applied to the front or back surface of an inorganic building material as the substrate.

[0126] Examples of inorganic substrates include ceramic substrates and metal substrates. Ceramic substrates are used for applications such as roofing tiles and exterior wall materials. Ceramic substrates are obtained by adding inorganic fillers, fibrous materials, etc. to a hydraulic adhesive material that is the raw material of an inorganic hardened body, molding the resulting mixture, and curing and hardening the resulting molded body. Examples of inorganic substrates include slate boards, flexible boards, calcium silicate boards, gypsum slag perlite boards, wood chip cement boards, precast concrete boards, ALC boards, gypsum boards, etc., but the present invention is not limited to these examples.

[0127] Examples of methods for applying the coating material of the present invention to an inorganic substrate include spray coating, roll coating, brush coating, trowel coating, bar coating, die coating, comma coating, gravure coating, kiss coating, spin coating, dip coating, curtain coating, doctor blade coating, knife coating, air knife coating, microgravure coating, offset gravure coating, and lip coating, but the present invention is not limited to these examples. Among these methods, the sealer of the present invention can also be suitably used for the roll coating method.

[0128] The coating material of the present invention may be applied in a single layer by itself, or may be applied by overcoating two or more layers. When applying two or more layers, only some of the layers may be formed by the coating material of the present invention, or all of the layers may be formed by the coating material of the present invention. When applying the coating material of the present invention to a substrate, the substrate may be previously coated with an undercoat such as a sealer, if necessary.

[0129] The thickness of the coating film of the coating material of the present invention formed on the surface of an inorganic substrate after drying is not particularly limited, but is usually preferably about 0.5 to 200 μm, more preferably about 1 to 150 μm.

[0130] By applying the coating material of the present invention onto the surface of an inorganic substrate as described above, an inorganic substrate having a coating film made of the coating material can be obtained.

[0131] The inorganic substrate having the coating film has excellent weather resistance, low-temperature film-forming properties, extensibility, water resistance, frost resistance and stain resistance, because the coating film contains the acrylic resin emulsion for paint of the present invention. EXAMPLES

[0132] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples. In the following examples, "parts" means "parts by mass" unless otherwise specified.

[0133] Example 1 Into a flask equipped with a dropping funnel, a stirrer, a nitrogen gas inlet tube, a thermometer and a reflux condenser, 773 parts of deionized water was placed at room temperature.

[0134] Into the dropping funnel A were added 156 parts of deionized water, 100 parts of a 25% aqueous solution of an emulsifier (manufactured by ADEKA Corporation, product name: ADEKA REASOAP SR-20), 45 parts of 2-ethylhexyl acrylate, 335 parts of methyl methacrylate, 50 parts of cyclohexyl methacrylate, 55 parts of butyl acrylate, 10 parts of acrylic acid and 5 parts of methacrylic acid as monomer components, and 5 parts of γ-methacryloyloxypropyltrimethoxysilane as an organosilane compound, to prepare a pre-emulsion for dropping at room temperature.

[0135] 92 parts of the pre-emulsion for dropping was added to the flask, and the temperature was raised to 80° C. while slowly blowing nitrogen gas into the flask. 57 parts of a 3.5% aqueous ammonium persulfate solution was added to the flask to initiate the polymerization reaction.

[0136] Thereafter, 90 parts of methyltrimethoxysilane was added to dropping funnel B, which was different from dropping funnel A, and 25 parts of a 2% aqueous solution of ammonium persulfate was added to dropping funnel C. The pre-emulsion for dropping remaining in dropping funnel A, methyltrimethoxysilane, and the 2% aqueous solution of ammonium persulfate were each dropped uniformly into the flask from dropping funnels A to C over a period of 120 minutes.

[0137] After the dropwise addition was completed, the contents of the flask were maintained at 80°C for 60 minutes, and 25% aqueous ammonia was added to the flask to adjust the pH of the contents of the flask (measured at 23°C using a product name: Ph meter F-23, manufactured by Horiba Ltd.; the same applies below) to 6 or higher.

[0138] Next, a second pre-emulsion was prepared consisting of 184 parts of deionized water, 100 parts of a 25% aqueous solution of an emulsifier (ADEKA Corporation, trade name: Adeka Reasoap SR-20), 250 parts of 2-ethylhexyl acrylate, 70 parts of methyl methacrylate, 150 parts of cyclohexyl methacrylate, and 30 parts of n-butyl acrylate as monomer components, and 10 parts of γ-methacryloyloxypropyltrimethoxysilane as an organosilane compound, and the obtained second pre-emulsion, 210 parts of methyltrimethoxysilane, and 25 parts of an aqueous solution of 2% ammonium persulfate were uniformly dropped into the flask over a period of 120 minutes in the same manner as above. After the dropwise addition, the contents of the flask were maintained at 80°C for 120 minutes to terminate the polymerization reaction, and a reaction mixture was obtained. The reaction mixture obtained above was cooled to room temperature (about 23°C) and then filtered through a 300 mesh (JIS mesh, the same applies below) wire mesh to obtain an acrylic resin emulsion with a non-volatile content of 42% by mass.

[0139] Table 2 shows information regarding the emulsion particles contained in the acrylic resin emulsion obtained above.

[0140] Example 2 An acrylic resin emulsion having a non-volatile content of 42% by mass was obtained in the same manner as in Example 1, except that the components having the composition shown in Table 1 were used in Example 1. Information regarding the emulsion particles contained in the acrylic resin emulsion obtained above is shown in Table 2.

[0141] Example 3 Into a flask equipped with a dropping funnel, a stirrer, a nitrogen gas inlet tube, a thermometer and a reflux condenser, 775 parts of deionized water was placed at room temperature.

[0142] Into the dropping funnel A, 96 parts of deionized water, 51 parts of a 20% aqueous solution of an emulsifier (manufactured by Kao Corporation, product name: Ramtel PD-104), 40 parts of a 25% aqueous solution of an emulsifier (manufactured by ADEKA Corporation, product name: Adeka Reasop SR-20), 10 parts of 2-ethylhexyl acrylate, 40 parts of methyl methacrylate, 230 parts of cyclohexyl methacrylate, and 20 parts of n-butyl acrylate as monomer components, and 7 parts of γ-methacryloyloxypropyltrimethoxysilane as an organosilane compound were added at room temperature to prepare a pre-emulsion for dropping.

[0143] 96 parts of the pre-emulsion for dropping was added to the flask, and the temperature was raised to 80° C. while slowly blowing nitrogen gas into the flask. 57 parts of a 3.5% aqueous ammonium persulfate solution was added to the flask to initiate the polymerization reaction.

[0144] Thereafter, 120 parts of methyltrimethoxysilane and 30 parts of dimethyldimethoxysilane were added to dropping funnel B, which was different from dropping funnel A, and 130 parts of a 2% aqueous solution of ammonium persulfate were added to dropping funnel C. The pre-emulsion for dropping remaining in dropping funnel A, methyltrimethoxysilane, dimethyldimethoxysilane, and the 2% aqueous solution of ammonium persulfate were each dropped uniformly into the flask from dropping funnels A to C over a period of 60 minutes.

[0145] Next, the contents of the flask were maintained at 80°C for 60 minutes, and a second pre-emulsion was prepared consisting of 147 parts of deionized water, 50 parts of a 20% aqueous solution of an emulsifier (manufactured by Kao Corporation, trade name: Ramtel PD-104), 40 parts of a 25% aqueous solution of an emulsifier (manufactured by ADEKA Corporation, trade name: Adeka Reasoap SR-20), 153 parts of 2-ethylhexyl acrylate as monomer components, 50 parts of methyl methacrylate, 100 parts of cyclohexyl methacrylate, 80 parts of butyl acrylate, 10 parts of acrylic acid, 5 parts of methacrylic acid, and 2 parts of acrylamide, and the obtained second pre-emulsion and 25 parts of an aqueous solution of 2% ammonium persulfate were uniformly dropped into the flask over 120 minutes in the same manner as above. After the dropwise addition, the contents of the flask were maintained at 80°C for 60 minutes, and 25% ammonia water was added to the flask to adjust the pH of the contents of the flask to 6 or more.

[0146] Next, a third-stage pre-emulsion was prepared at room temperature consisting of 111 parts of deionized water, 38 parts of a 20% aqueous solution of an emulsifier (manufactured by Kao Corporation, trade name: Ramtel PD-104), 30 parts of a 25% aqueous solution of an emulsifier (manufactured by ADEKA Corporation, trade name: Adeka Reasoap SR-20), 190 parts of 2-ethylhexyl acrylate, 30 parts of methyl methacrylate, 100 parts of cyclohexyl methacrylate, 60 parts of butyl acrylate, 10 parts of 2-hydroxyethyl methacrylate, and 10 parts of 1,2,2,6,6-pentamethylpiperidine-4-methacrylate as monomer components, and 10 parts of γ-methacryloyloxypropyltrimethoxysilane as an organosilane compound.

[0147] The third-stage pre-emulsion obtained above was mixed with 100 parts of methyltrimethoxysilane and 40 parts of dimethyldimethoxysilane as organosilane compounds to prepare a mixed solution. The mixed solution obtained above and 13 parts of an aqueous solution of 2% ammonium persulfate were uniformly dropped into the flask over 60 minutes in the same manner as above. After the dropping was completed, the contents of the flask were maintained at 80°C for 120 minutes to terminate the polymerization reaction and obtain a reaction mixture. The reaction mixture obtained above was cooled to room temperature (about 23°C) and then filtered through a 300-mesh wire net to obtain an acrylic resin emulsion with a non-volatile content of 42% by mass.

[0148] Table 2 shows information regarding the emulsion particles contained in the acrylic resin emulsion obtained above.

[0149] Examples 4 to 10 An acrylic resin emulsion having a non-volatile content of 42% by mass was obtained in the same manner as in Example 3, except that the components having the composition shown in Table 1 were used in Example 3. Information regarding the emulsion particles contained in the acrylic resin emulsion obtained above is shown in Table 2.

[0150] Comparative Examples 1 and 2 An acrylic resin emulsion having a non-volatile content of 42% by mass was obtained in the same manner as in Example 1, except that the components having the composition shown in Table 1 were used in Example 1. Information regarding the emulsion particles contained in the acrylic resin emulsion obtained above is shown in Table 2.

[0151] Comparative Example 3 An acrylic resin emulsion was prepared in the same manner as in Example 1, except that the components having the composition shown in Table 1 were used. However, the obtained acrylic resin emulsion was gelled, and therefore evaluation of the physical properties of the acrylic resin emulsion was abandoned.

[0152] The meanings of the abbreviations in Table 1 are as follows: [Monomer components] CHMA: Cyclohexyl methacrylate MMA: Methyl methacrylate 2EHA: 2-Ethylhexyl acrylate ·BA: n-Butyl acrylate 2OA: 2-octyl acrylate 2OMA: 2-octyl methacrylate HEMA: 2-hydroxymethyl methacrylate ·AA: Acrylic acid ·MAA: Methacrylic acid ·AAm: Acrylamide HALS1: 1,2,2,6,6-pentamethylpiperidine-4-methacrylate ·HALS2: 2,2,6,6-Tetramethylpiperidine-4-methacrylate

[0153] [Organosilane Compound] SCA: 3-Methacryloyloxypropyltrimethoxysilane ·SCB: Methyltrimethoxysilane ·SCC: Dimethyldimethoxysilane ·SCD: Phenyltrimethoxysilane ·SCE: Diphenyldimethoxysilane

[0154] Furthermore, the terms listed in Table 2 have the following meanings. Layer ratio: Mass ratio of inner layer, middle layer, and outer layer Inner layer Tg (℃): Glass transition temperature of the polymer that composes the inner layer (℃) Intermediate layer Tg (℃): Glass transition temperature of the polymer that composes the intermediate layer (℃) Outer layer Tg (℃): Glass transition temperature of the polymer that composes the outer layer (℃) Difference between inner layer Tg and middle layer Tg (℃): The temperature difference between the glass transition temperature of the polymer constituting the inner layer and the glass transition temperature of the polymer constituting the middle layer (℃) Total Tg (℃): The glass transition temperature (℃) of all polymers that make up the emulsion particles Amount of silicon charged (parts by mass): Amount of organosilane compound per 100 parts by mass of monomer component (parts by mass) Silicon content in each layer: The amount (parts by mass) of organosilane compound used in each of the inner / middle / outer layers per 100 parts by mass of monomer component. A "-" in the middle layer column means that there is no middle layer. ·Si ratio: Mass ratio of SCA / SCB / SCC / SCD / SCE used as organosilane compounds in emulsion particles. "-" in the intermediate layer column means that there is no intermediate layer. CHMA content (mass%): The cyclohexyl methacrylate content (mass%) of the monomer components used in each of the inner / middle / outer layers. A "-" in the middle layer column means that there is no middle layer. Total CHMA content (mass%): Content of cyclohexyl methacrylate in all monomer components (mass%) ·MFT(℃): Minimum film-forming temperature of resin emulsion (℃)

[0155] [Table 1]

[0156] [Table 2]

[0157] Next, the physical properties of the acrylic resin emulsion and its coating material obtained above were examined by the following methods, including glass transition temperature, minimum film-forming temperature, weather resistance, low-temperature film-forming property, extensibility, water resistance, frost resistance, and stain resistance. The results are shown in Table 3.

[0158] [Glass transition temperature (Tg)] The glass transition temperature was calculated as a temperature obtained based on the Fox formula represented by the above formula (III) using the glass transition temperature of a homopolymer of a monomer used in the monomer component constituting the polymer. When the emulsion has a multi-layer structure, the glass transition temperature of the entire polymer constituting the emulsion of the multi-layer structure was calculated from the mass fraction of each monomer in all the monomer components used in the multi-stage emulsion polymerization and the glass transition temperature of the homopolymer of the corresponding monomer.

[0159] [Minimum film forming temperature] The minimum film-forming temperature of the acrylic resin emulsion was measured in accordance with JIS K6828-2 (2003). More specifically, an MFT tester (manufactured by Tester Sangyo Co., Ltd., product number: TP-801 LT) was used to apply the acrylic resin emulsion to a stainless steel grooveless flat plate with an applicator to a thickness of 250 μm, and the minimum temperature (°C) at which a crack-free, uniform coating film was formed was measured. The presence or absence of cracks in the coating film was visually determined in accordance with JIS K6828-2.

[0160] (A) Preparation of clear paint To 100 parts of the acrylic resin emulsion obtained in each Example or Comparative Example, 10 parts of 2,2,4-trimethyl-1,3-pentanediol isobutyrate was added as a film-forming assistant, and the mixture was mixed in a homodisper at a rotation speed of 1500 min -1 The mixture was stirred at RT for 10 minutes to obtain a dispersion.

[0161] A BH type viscometer (manufactured by Tokyo Keiki Co., Ltd.) was used at a rotation speed of 20 min -1 A thickener (ADEKA CORPORATION, product name: ADEKA NOL UH-420) was added to the dispersion obtained above so that the viscosity at 25°C was 4000 mPa s. The mixture obtained was stirred for 30 minutes and then filtered through a 300 mesh wire screen to obtain a clear coating material.

[0162] (B) Preparation of enamel paint 100 parts of deionized water, 15 parts of dispersant (manufactured by BYK Japan, product name: DisperBYK-190), 210 parts of titanium dioxide (manufactured by Ishihara Sangyo Kaisha), 2 parts of defoamer (manufactured by BYK Japan, product number: BYK-024), and 2 parts of a 15% aqueous solution of thickener (manufactured by ADEKA, product name: Adekanol UH-420) were mixed in a homodisper at a rotation speed of 300 min. -1 After dispersing for 60 minutes, the mixture was filtered through a 300 mesh wire screen to obtain a white paste.

[0163] To 100 parts of the acrylic resin emulsion obtained in each Example or Comparative Example, 10 parts of 2,2,4-trimethyl-1,3-pentanediol isobutyrate was added as a film-forming assistant, and the mixture was mixed in a homodisper at a rotation speed of 1500 min -1 The mixture was stirred at RT for 30 minutes to obtain a dispersion.

[0164] To the dispersion obtained above, 80 parts of the white paste obtained above and 0.6 parts of a defoaming agent (manufactured by BYK Japan Co., Ltd., product number: BYK-024) were added to obtain a mixture. -1 A thickener (ADEKA Corporation, product name: Adekanol UH-420) was added to the mixture obtained above so that the viscosity at 25°C was 4000 mPa·s, and the mixture was stirred for 30 minutes and then filtered through a 300 mesh wire screen to obtain an enamel paint.

[0165] [Weather resistance] Apply a sealer (SK Chemical Co., Ltd., product name: EX Sealer) with an air spray at a rate of 150 g / m 2 The coating was evenly applied to a slate board (manufactured by Nippon Test Panel Co., Ltd.) so that the coating was as shown in the figure, and the board was dried in the air at room temperature (about 23° C.) for one week to prepare a test board.

[0166] Next, enamel paint was applied to the sealer surface of the test plate with an 8 mil applicator, and after drying for one week in the air at room temperature (approximately 23°C), the 60° specular gloss of the enamel paint-coated surface of the test plate was measured with a gloss meter (product number: VG2000, manufactured by Nippon Denshoku Industries Co., Ltd.) Subsequently, a weather resistance test was conducted for 2500 hours on the test plate coated with enamel paint under the following weather resistance test conditions, and then the 60° specular gloss of the enamel paint-coated surface of the test plate was measured with the gloss meter in the same manner as above.

[0167] (Weather resistance test conditions) Testing machine: Weather resistance testing machine (manufactured by Daipla Wintes Co., Ltd., product name: Metal Weather KU-R5) Irradiation: 4 hours in air at 65°C and 50% relative humidity (irradiation intensity: 80mW / cm 2 ) Humidity: 4 hours in air at 35°C and 98% relative humidity Shower: 30 seconds before and after wetting

[0168] The gloss retention of the enamel paint surface of the test plate was calculated using the formula: [Gloss retention rate (%)] = [[Gloss after weather resistance test] ÷ [Gloss before weather resistance test]] × 100 The weather resistance was evaluated based on the following evaluation criteria.

[0169] (Evaluation Criteria) ◎: Gloss retention is 90% or more ○: Gloss retention is 80% or more but less than 90% △: Gloss retention is between 60% and 80% ×: Gloss retention is less than 60%

[0170] [Low temperature film forming property] The enamel paint obtained above was applied to a slate board (manufactured by Nippon Test Panel Co., Ltd.) using a 10 mil applicator, and dried for 24 hours in a thermostatic chamber whose temperature was adjusted to 0°C.

[0171] Next, the slate boards coated with the enamel paint described above were immersed in water at 23° C. for 24 hours, then removed from the water and dried in air at 23° C. for 24 hours. The enamel paint-coated surfaces of the dried slate boards were visually observed at 10x magnification with a loupe, and the low-temperature film-forming stability was evaluated based on the following evaluation criteria.

[0172] (Evaluation Criteria) ○: No cracks were observed. ◯: No cracks were observed, but swelling or blisters were observed in the coating film. △: Small cracks (less than 5 mm in length) are observed in the coating. ×: Large cracks (length 5 mm or more) are observed in the coating film.

[0173] [Extensibility] A test substrate was prepared by attaching release paper to one surface of a square glass plate with sides measuring 15 cm, and then attaching cloth tape to the edge of the surface to which the release paper was attached.

[0174] Next, the clear coating obtained above was applied to the release paper surface of a test substrate so that the coating thickness after drying was 0.3 mm, and after drying in air at 23°C for one week, the formed coating film was peeled off from the test substrate and the resulting coating film was cut into a dumbbell shape as specified in JIS K 6909 (2014) to prepare a test specimen. The short side of the test specimen was held in the chuck of a tensile tester (manufactured by Shimadzu Corporation, product name: Autograph AGS-100D) in air at room temperature (approximately 23°C) and a tensile test was performed under conditions of an initial gauge length of 60 mm and a tensile speed of 200 mm / min, and the formula: [Elongation rate (%)] = [(elongation at break) ÷ (60 mm)] × 100 The elongation rate of the coating film was examined based on the above, and the elongation was evaluated based on the following evaluation criteria.

[0175] (Evaluation Criteria) ○: Elongation rate is 100% or more ○: Elongation rate is 80% or more but less than 100% △: Elongation rate is 40% or more but less than 80% ×: Elongation rate is less than 40%

[0176] [Water whitening resistance] The clear coating obtained above was applied to a black acrylic plate (manufactured by Nippon Test Panel Co., Ltd.) using a 6 mil applicator, and dried in air at room temperature (about 23° C.) for one week to prepare a test plate.

[0177] The L value (L0) of the color difference of the clear coating surface of the test plate was measured using a color difference meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name: Spectroscopic Color Difference Meter SE-2000).

[0178] Next, the test plate was immersed in water at 23°C for 24 hours, then removed from the water and wiped dry with Kimtowel (manufactured by Nippon Paper Crecia Co., Ltd.). Within 1 minute, the L value (L1) of the color difference was measured using the color difference meter.

[0179] Based on the color difference L0 and L1 measured above, the change in L value (△L) is calculated using the formula: [Change in L value (△L)] = L1 - L0 The water resistance was evaluated based on the following criteria.

[0180] (Evaluation Criteria) ○: △L is less than 10 ○: △L is 10 or more and less than 20 △:△L is 20 or more and less than 30 ×: △L is 30 or more

[0181] [Freeze resistance (freeze-thaw resistance)] A test plate was prepared in the same manner as described in the "Weather Resistance" section above, and the sides and back other than the enamel paint-coated surface were sealed with a two-component curing solvent-based resin. The test plate was then subjected to a cycle of freezing in air at -20°C for 2 hours and immersing in water at 10°C for 1 hour using a freeze-thaw tester (manufactured by Marui Co., Ltd.). After 50 cycles of this procedure, the enamel paint-coated surface of the test plate was visually observed to determine the number of cycles until cracks appeared on the paint surface. The frost resistance was evaluated based on the following evaluation criteria.

[0182] (Evaluation Criteria) ○: No cracks observed after 300 cycles ○: Cracks occurred after 200 cycles and before 300 cycles △: Cracks appear after more than 100 cycles and up to 200 cycles ×: Cracks occurred within 100 cycles

[0183] [Stain resistance] Glass beads with a diameter of 1 mm were added to deionized water at a ratio of 5 parts per 95 parts of deionized water, and the deionized water was rotated in a homodisper at a speed of 500 min -1 Add 5 parts of carbon black (manufactured by Mitsubishi Chemical Corporation) to deionized water while stirring at a rotation speed of 2500 min -1 The deionized water was further stirred at 50° C. for 30 minutes to obtain a dispersion. The dispersion obtained above was filtered through a 300-mesh wire screen to obtain a dispersion of carbon black.

[0184] Next, the enamel paint obtained above was applied to a white acrylic plate (manufactured by Nippon Test Panel Co., Ltd.) with an 8 mil applicator and dried in air at room temperature (about 23°C) for one week. After drying, the initial L value (L0) of the enamel paint-coated surface of the test plate was measured with a color difference meter (manufactured by Nippon Denshoku Kogyo Co., Ltd., product name: Spectroscopic Color Difference Meter SE-2000).

[0185] Subsequently, the carbon black dispersion obtained above was applied to the enamel paint-coated surface of the test plate with a 20 mil applicator and dried for 24 hours at room temperature (about 23° C.). After drying, the carbon black adhering to the enamel paint-coated surface of the test plate was washed away with running water and a brush (pig bristles with 40 mm bristles), and the L value (L1) of the carbon black dispersion-coated surface was measured with the color difference meter.

[0186] Next, the change in L value (△L) is calculated using the formula: △L=L1-L0 The stain resistance was evaluated based on the following evaluation criteria.

[0187] (Evaluation Criteria) ○: △L is less than 20 ○: △L is 20 or more and less than 40 △: △L is 40 or more and less than 60 ×: △L is 60 or more

[0188] [Table 3]

[0189] From the results shown in Table 3, it can be seen that the acrylic resin emulsions for paint obtained in each Example all had excellent coating film elongation and frost resistance, despite the use of an organosilane compound, and formed coating films that were excellent overall in weather resistance, low-temperature film-forming properties, elongation, water resistance, frost resistance, and stain resistance. [Industrial Applicability]

[0190] The acrylic resin emulsion for paint of the present invention can be suitably used for coating objects such as inorganic substrates such as slate boards, flexible boards, calcium silicate boards, gypsum slag perlite boards, wood-chip cement boards, precast concrete boards, ALC boards, and gypsum boards.

Claims

1. The acrylic resin emulsion for paint contains emulsion particles having at least two resin layers, the resin layers constituting the emulsion particles contain an organosilane compound and a monomer component, the monomer-containing component contains 20 to 100 parts by mass of the organosilane compound per 100 parts by mass of the monomer component, and the glass transition temperature of the resin constituting the inner layer is 40° C. or more higher than the glass transition temperature of the resin used in the resin layer present on the inner layer.

2. 2. The acrylic resin emulsion for paint according to claim 1, wherein the content of the alicyclic structure-containing (meth)acrylate in all monomer components used in the emulsion particles is 20 to 80 mass %.

3. 2. The acrylic resin emulsion for paint according to claim 1, wherein the monomer-containing component contains a piperidine compound.

4. 2. The acrylic resin emulsion for paint according to claim 1, wherein the emulsion particles have an inner layer, an intermediate layer and an outer layer.

5. 5. The acrylic resin emulsion for paint according to claim 4, wherein the glass transition temperature of the resin constituting the inner layer is at least 40[deg.] C. higher than the glass transition temperature of the resin constituting the intermediate layer.

6. A method for producing an acrylic resin emulsion for paint containing emulsion particles having at least two resin layers, the method comprising the steps of: using a monomer-containing component containing an organosilane compound and a monomer component as raw materials for the resin layers constituting the emulsion particles, the monomer component having an amount of the organosilane compound of 20 to 100 parts by mass per 100 parts by mass of the monomer component; and adjusting the glass transition temperature of the inner layer to be 40° C. or more higher than the glass transition temperature of a resin constituting an outer layer present on the inner layer.

7. A paint comprising the acrylic resin emulsion for paint according to any one of claims 1 to 5.

8. An inorganic substrate having a coating film formed from the coating material according to claim 7.

Citation Information

Patent Citations

  • Method for manufacturing aqueous polymer dispersion for coating material and the dispersion

    JP2002012601A

  • Aqueous resin composition

    JP2004292541A

  • Aqueous resin dispersion

    JP2006249183A

  • Water-based resin composition

    JP2009270034A

  • Highly durable acrylic emulsion

    JP2010059379A

Cited By

  • Resin composition for coating material

    WO2025197917A1