Laminated film and package
A three-layer laminated film with a thermoplastic base, polyolefin seal adjacent, and surfactant-enhanced polyester seal layer addresses film residue and fuzzing issues, ensuring clean peeling and antifogging for improved packaging aesthetics.
Patent Information
- Application Number
- JP2023059308
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing laminated films using polyester resins for sealing layers suffer from issues such as film residue and fuzzing during peeling, poor transparency, and inadequate antifogging properties, particularly when used for packaging containers.
A laminated film with three layers: a base layer of thermoplastic resin, a seal adjacent layer of polyolefin resin, and a seal layer of polyester resin containing isophthalic acid and specific diol residues, with a surfactant addition to enhance peeling and antifogging properties.
The film provides a clean peeling surface without residue or fuzz, maintains transparency, and ensures antifogging properties, enhancing the aesthetic appearance and visibility of packaged contents.
Smart Images

Figure 2024146422000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate film and a packaging material. [Background technology]
[0002] Polyolefin resin containers have been used for individually packaged cup-shaped products containing jellies, chawanmushi, side dishes, etc., deep-draw packaging, medical products such as disposable syringes, daily necessities, and blister packs containing stationery, and films having a sealing layer made of polyolefin resin have been used as the lid material for the containers. For example, polyolefin resins such as polyethylene, polypropylene, ethylene-vinyl acetate copolymer (EVA), and ethylene-acrylic acid ester copolymer are mainly used for the sealing layer of the lid material film.
[0003] In recent years, there has been a demand for high functionality in food packaging container materials, and containers made of polyester-based resin using unstretched polyester sheets (A-PET sheets) made of polyester-based resins are being used from the standpoints of transparency, heat resistance, oxygen gas barrier properties, non-adsorption, aroma retention, formability, etc., and as lid materials for these containers, films for lid material using polyester-based resins in the sealing layer are being considered.
[0004] Patent Document 1 discloses a three-layer coextruded film consisting of a heat-sealable polyester layer, a film layer made of a copolymer resin of olefin and maleic anhydride, and a polyolefin layer. However, the film disclosed in Patent Document 1 uses a polyester resin with a low glass transition temperature of -20°C for the purpose of improving the heat sealability in the fusion state with the polyester resin of the container made of polyester resin, but since the polyester resin itself is opaque, there is room for further improvement in appearance.
[0005] Patent Document 2 discloses an easy-open packaging material that undergoes delamination via a seal layer made of a crystalline polyester having a glass transition temperature of 40°C or lower and an amorphous polyester having a glass transition temperature of 45 to 90°C. However, in the case of the sealing layer disclosed in Patent Document 2, the elastic modulus of the sealing layer is low, so that the stress generated when opening and peeling the package may cause the sealing layer to stretch and break, raising concerns that the sealing layer resin may leave a film residue or become frayed.
[0006] Patent Document 3 discloses a laminated film in which a heat seal layer containing a polyester resin and an antifogging agent is laminated. Various amorphous or low crystalline polyester resins are described as the resin for the heat seal layer, but the amorphous polyethylene terephthalate resin described in Example 1 has insufficient seal adhesion, and the crystalline polyester resin described in Example 8 has a concern of poor transparency in the sealed portion. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Unexamined Patent Publication No. 4-94933 [Patent Document 2] JP 2001-328221 A [Patent Document 3] International Publication No. 2015 / 046132 Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made in consideration of the above problems, and provides a laminated film which can be easily peeled when opening a package sealed by heat sealing with a molded body made of a resin composition containing a polyester-based resin as a main component, and which can form a clean peeled surface (peeled appearance) without leaving any resin residue or fuzz at the opened area after peeling, and which also has good transparency and anti-fogging properties. In the present invention, the term "molded article made of a resin composition containing a polyester-based resin as a main component" refers to a film, sheet, container, etc., which are formed by molding a resin composition containing a polyester-based resin as a main component. The molded article may be formed entirely from a resin composition containing a polyester-based resin as a main component, or may be formed from a laminate in which a layer made of the resin composition containing a polyester-based resin as a main component and another resin layer are laminated. [Means for solving the problem]
[0009] As a result of extensive research, the inventors have invented a laminated film having at least three layers, namely a base layer, a seal adjacent layer, and a seal layer, in which the seal layer has the function of forming a clean peel surface (peel appearance) without leaving any film residue or fuzz, and the seal adjacent layer has the function of being able to peel off at the layer interface with the seal layer (interlayer peeling), and a packaging body using said film, thereby solving the above-mentioned problems.
[0010] The present invention has the following aspects. [1] A laminated film having at least three layers, namely, a base layer (I), a seal adjacent layer (II), and a seal layer (III), which satisfies the following (1) to (4): (1) The resin composition forming the substrate layer (I) contains a thermoplastic resin as a main component. (2) The resin composition forming the seal adjacent layer (II) contains a polyolefin resin as a main component. (3) The resin composition forming the seal layer (III) contains a polyester resin as a main component, and the polyester resin contains isophthalic acid as a dicarboxylic acid residue and at least two kinds of residues as a diol residue. (4) The resin composition forming the sealing layer (III) contains a surfactant in an amount of 0.1 to 10% by mass when the resin composition is taken as 100% by mass. [2] The laminate film according to [1], wherein the polyester resin contains ethylene glycol as the first diol residue and at least one selected from the group consisting of diethylene glycol, neopentyl glycol, hexanediol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, pentamethylene glycol, and 1,4-cyclohexanedimethanol as the second diol residue. [3] The laminate film according to [1] or [2], wherein the contact angle of the sealing layer (III) measured in accordance with JIS K6768 (1999) is 50° or less. [4] The laminate film according to any one of [1] to [3], wherein the sealing layer (III) has a tensile breaking stress in the machine direction of the film of 85 MPa or less, measured in accordance with JIS K7127 (1999). [5] The laminate film according to any one of [1] to [4], wherein the thermoplastic resin contained in the resin composition forming the base layer (I) is at least one selected from polyolefin-based resins, polyamide-based resins, polyester-based resins, polystyrene-based resins, and ethylene-vinyl acetate copolymers. [6] The laminate film according to any one of [1] to [5], wherein the polyolefin resin contained in the resin composition forming the seal adjacent layer (II) is a polyethylene resin. [7] A package formed by heat-sealing the seal layer (III) of the laminated film according to any one of [1] to [6] and a container made of a resin composition containing a polyester-based resin as a main component. Effect of the Invention
[0011] According to the present invention, it is possible to provide a sealant film that can firmly adhere to a molded body (e.g., a container) made of a resin composition containing a polyester resin as a main component. Therefore, even if the contents contain moisture such as yogurt, jelly, or side dishes and there is a possibility that the sealed portion may become wet, or even if there is a possibility that minute impurities are present at the sealed portion, it is possible to obtain a package in which the sealant film and the molded body are reliably sealed.
[0012] In addition, when opening the package, the seal layer and the peel layer have easy peeling properties that allow the layers to be peeled off at the interface, and the resin of the seal layer is unlikely to remain on the surface after peeling, so that the contents can be taken out without getting caught on the sealed area. In addition, the laminated film of the present invention is unlikely to cause the resin of the seal layer to tear, so that the torn resin can be prevented from mixing with the contents as a foreign matter. Furthermore, since the laminated film of the present invention is a transparent film, the visibility of the contents is good, and it is effective in improving the aesthetic appearance of the product and increasing the product value. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The laminated film of the present invention (hereinafter, referred to as "the present film") will be described below as one example of an embodiment of the present invention. However, the scope of the present invention is not limited to the embodiment described below.
[0014] <Terminology explanation> In the present invention, the term "film" encompasses the meaning of "sheet", and the term "sheet" encompasses the meaning of "film". In the present invention, "MD" means the machine direction of the film, and "TD" means the direction perpendicular to the machine direction of the film. In the present invention, when it is described as "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as the meaning of "preferably larger than X" and "preferably smaller than Y". Furthermore, when it is stated that the amount is "X or more" (X is any number), it also means that the amount is "preferably greater than X" unless otherwise specified, and when it is stated that the amount is "Y or less" (Y is any number), it also means that the amount is "preferably smaller than Y" unless otherwise specified.
[0015] The upper and lower limit values of the numerical ranges specified in the present invention are included in the equivalent range of the present invention even if they are slightly outside the numerical ranges specified in the present invention, as long as they have the same action and effect as those within the numerical range.
[0016] In the present invention, the term "main component" refers to a component that occupies the largest mass% of the components contained in the target. With regard to the content of the main component, when the content of the components contained in the target is 100 mass%, the mass of the component may be 50 mass% or more, 60 mass% or more, 70 mass% or more, 80 mass% or more, 90 mass% or more, 99 mass%, or 100 mass%.
[0017] <Laminated film> A laminated film according to an embodiment of the present invention (hereinafter referred to as "the film") has at least three resin layers, namely, a base layer (I), a seal adjacent layer (II), and a seal layer (III). Each layer of the film will be described below.
[0018] [Base material layer (I)] The resin composition forming the base layer (I) of the present film contains a thermoplastic resin as a main component. The thermoplastic resin may be selected depending on the application and required properties of the film, such as oxygen gas barrier property, water vapor barrier property, impact resistance, pinhole resistance, and handling properties during production and transportation, in food packaging applications. Specific examples of the thermoplastic resin include polyolefin resins such as polyethylene resins, polypropylene resins, polystyrene resins, and ethylene copolymers, and gas barrier resins such as polyamide resins, polyester resins, and ethylene-vinyl acetate copolymers. These may be used alone or in combination of two or more. Among these, at least one selected from the group consisting of polyolefin resins, polyamide resins, polyester resins, polystyrene resins, and ethylene-vinyl acetate copolymers is preferred, and polyethylene resins are particularly preferred.
[0019] Examples of the polyethylene resin include high density polyethylene (HDPE), linear low density polyethylene (LLDPE), low density polyethylene (LDPE), etc. These may be used alone or in combination of two or more. Among them, linear low density polyethylene and low density polyethylene are preferred.
[0020] The polyethylene resin may be a homopolymer of ethylene or a copolymer of ethylene and another monomer (polyethylene copolymer resin).
[0021] Examples of the other monomer include α-olefins having 3 to 8 carbon atoms, such as propylene and butene, which may be used alone or in combination of two or more kinds.
[0022] The melt flow rate (MFR) of the polyethylene resin (JIS K7210-1A method (2014), 230° C., load 2.16 kg) is usually 0.1 to 50 g / 10 min, and preferably 1 to 40 g / 10 min, from the viewpoint of film-forming properties.
[0023] The melting point of the polyethylene resin is usually 95 to 175° C., preferably 100 to 170° C., and more preferably 115 to 168° C. By setting the melting point within the above range, the mechanical properties such as moldability and pinhole resistance of the present film tend to be improved.
[0024] The storage modulus E' of the polyethylene resin at 20° C. is usually 10 to 1000 MPa, preferably 50 to 800 MPa, and more preferably 100 to 700 MPa. By setting the storage modulus E' at 20° C. within the above range, the mechanical properties such as formability and pinhole resistance of the present film tend to be improved.
[0025] In the present invention, the storage modulus of the polyethylene resin can be calculated by measuring the temperature dispersion of tensile vibration at a frequency of 10 Hz based on the JIS K7244-4 (1999) method. The storage modulus of a polyethylene resin is influenced by the copolymer composition, the degree of modification, the molecular weight, the molecular weight distribution, the molecular structure such as branching, and the three-dimensional structure such as crystallinity and orientation.
[0026] The substrate layer (I) may be a single layer or a multi-layer. When the substrate layer (I) is a multi-layer, an adhesive layer, a vapor deposition layer, a printing layer, a coating layer, etc. may be appropriately provided between the substrate layers.
[0027] Furthermore, a biaxially oriented film can also be used as the base layer (I). Examples of the biaxially oriented film include a biaxially oriented polyethylene terephthalate film (OPET), a biaxially oriented nylon film (ONy), a biaxially oriented polypropylene film (OPP), and a biaxially oriented polystyrene film (OPS).
[0028] [Seal adjacent layer (II)] The resin composition forming the seal adjacent layer (II) of the present film contains a polyolefin resin as a main component. The seal adjacent layer (II) is a layer that has sufficient adhesion to the seal layer (III) when the film is formed, and has a function of peeling after the seal layer (III) is heat-sealed to the adherend. That is, the seal adjacent layer (II) is a layer that has interlayer adhesion with the seal layer (III) when the package is sealed, and has easy peelability when opened.
[0029] The polyolefin resin has a low viscosity in a high-temperature molten state, and when opened after sealing, its storage modulus under the usage environment (room temperature) is lower than that of the polyester resin used in the seal layer (III), so it is suitable as a resin for forming the seal adjacent layer (II). Among them, polyolefin resins are preferably polypropylene resins and polyethylene resins, and polyethylene resins are particularly preferred from the viewpoint of lower storage modulus than polyester resins.
[0030] (Polyethylene resin) Examples of the polyethylene resin include linear low density polyethylene (LLDPE) resin, low density polyethylene (LDPE) resin, medium density polyethylene (MDPE) resin, high density polyethylene (HDPE) resin, etc. These may be used alone or in combination of two or more. Among them, linear low density polyethylene (LLDPE) resin and low density polyethylene (LDPE) resin are preferred from the viewpoint of low storage modulus.
[0031] The polyethylene resin may be a homopolymer of ethylene or a copolymer of ethylene and another monomer (polyethylene copolymer resin). Among these, polyethylene copolymer resins are preferred in the present invention.
[0032] Examples of the other monomer include alkenes having 3 to 8 carbon atoms, such as propylene and butene, (meth)acrylic acid esters, vinyl acetate, vinyl alcohol, etc. These may be used alone or in combination of two or more. Among these, propylene and butene are preferred.
[0033] Examples of the (meth)acrylic acid ester component include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, lauryl (meth)acrylate, octyl (meth)acrylate, dodecyl (meth)acrylate, and stearyl (meth)acrylate.
[0034] From the viewpoint of adhesion to the seal layer (III), the polyethylene resin is more preferably a modified polyethylene resin.
[0035] The modification is preferably an acid-modified polyethylene resin with an unsaturated carboxylic acid component. By using an acid-modified polyethylene resin, there is a tendency that the film has sufficient adhesion to the seal layer during film formation, and that the seal layer has sufficient peeling function after heat sealing to the adherend.
[0036] Examples of the unsaturated carboxylic acid component include acrylic acid, methacrylic acid, maleic acid, maleic anhydride, itaconic acid, itaconic anhydride, fumaric acid, crotonic acid, etc., as well as half esters and half amides of unsaturated dicarboxylic acids. These may be used alone or in combination of two or more. Among these, acrylic acid, methacrylic acid, maleic acid, and maleic anhydride are preferred, and maleic anhydride is particularly preferred. The unsaturated carboxylic acid component may be copolymerized with the ethylene, and the form is not limited, and examples of the copolymerization state include random copolymerization, block copolymerization, and graft copolymerization.
[0037] The acid-modified rate of the acid-modified polyethylene resin is preferably from 0.1 to 10%, and more preferably from 0.2 to 5%, from the viewpoint of good adhesiveness.
[0038] As the polyolefin resin contained in the resin composition forming the seal adjacent layer (II), maleic anhydride modified ethylene-butene copolymer, maleic anhydride modified ethylene-propylene-butene copolymer, and maleic anhydride modified ethylene-propylene-butene copolymer are preferred.
[0039] The density of the polyolefin resin contained in the resin composition forming the seal adjacent layer (II) is 920 kg / m 3 It is preferable that the resistance is less than 910 kg / m 3 More preferably, the density is 920 kg / m 3 By ensuring that the content is equal to or less than this, the amount of crystalline components in the polyethylene resin is reduced, and coextrusion adhesion with adjacent layers tends to be improved.
[0040] The storage modulus E' at 20°C of the polyolefin resin contained in the resin composition forming the seal adjacent layer (II) is preferably 500MPa or less, more preferably 300MPa or less, and even more preferably 100MPa or less. By being 500MPa or less, when the present film is peeled off from the adherend in a room temperature environment, the seal adjacent layer (II) tends to peel off at the layer interface with the seal layer (III) while the seal layer (III) remains firmly attached, and it is easy to open. In addition, the lower limit is not particularly limited, but generally 10MPa or more is preferable.
[0041] The seal adjacent layer (II) may contain other resins in an amount of less than 50% of the resin composition in order to not significantly impair interlayer adhesion and easy peeling or to improve them. In particular, when an acid-modified ethylene copolymer is used, it is preferable to use a polyethylene resin or a polyolefin resin modified or copolymerized with maleic anhydride (excluding polyethylene resins) as the other resin in terms of mixability with the acid-modified ethylene copolymer and co-extrudability in film formation.
[0042] [Sealing layer (III)] The sealing layer (III) of the present film is preferably disposed at the outermost surface position on one side of the present film for the functional purpose of heat sealing to an adherend, and is made of a resin composition containing a polyester resin as a main component and further containing 0.1 to 10 mass % of a surfactant.
[0043] (Polyester resin) The polyester resin is usually a polyester resin derived from a dicarboxylic acid residue and a diol residue, and in the present invention, contains isophthalic acid as the dicarboxylic acid residue and at least two kinds of residues as the diol residue. In the present invention, the diol residue that accounts for the largest mol % relative to 100 mol % of all diol residues is referred to as the "first diol residue", and hereinafter, in descending order of mol %, the diol residues are referred to as the "second diol residue", the "third diol residue", ... (hereinafter, these may be collectively referred to as the "second or subsequent diol residues"). Furthermore, when the dicarboxylic acid residue is composed of two or more types of residues, the dicarboxylic acid residue that occupies the greatest amount of mole percent relative to 100 mole percent of all dicarboxylic acid residues is referred to as the "first dicarboxylic acid residue", and the following are referred to in order of mole percent as the "second dicarboxylic acid residue", the "third dicarboxylic acid residue", ... (hereinafter, these may be collectively referred to as the "second or subsequent dicarboxylic acid residues").
[0044] In addition to isophthalic acid residues, the dicarboxylic acid residues include aromatic dicarboxylic acid residues such as terephthalic acid, furandicarboxylic acid, 2-chloroterephthalic acid, 2,5-dichloroterephthalic acid, 2-methylterephthalic acid, 4,4-stilbene dicarboxylic acid, 4,4-biphenyl dicarboxylic acid, orthophthalic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, bisbenzoic acid, bis(p-carboxyphenyl)methane, anthracene dicarboxylic acid, 4,4-diphenyl ether dicarboxylic acid, 4,4-diphenoxyethane dicarboxylic acid, 5-Na sulfoisophthalic acid, and ethylene-bis-p-benzoic acid, dimer acid, hydrogenated dimer acid, adipic acid, sebacic acid, succinic acid, azelaic acid, dodecanedioic acid, 1,3-cyclohexanedicarboxylic acid, and 1,4-cyclohexanedicarboxylic acid, and ester derivatives thereof. These dicarboxylic acid residues may be contained alone or in combination.
[0045] Among these, it is preferable that the dicarboxylic acid residue contains terephthalic acid as the first dicarboxylic acid residue and isophthalic acid as the second or subsequent dicarboxylic acid residues.
[0046] Examples of the diol residue include aliphatic glycols such as ethylene glycol, diethylene glycol, neopentyl glycol, hexanediol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, and pentamethylene glycol, alicyclic glycols such as cyclohexanedimethanol, and aromatic dihydroxy compound derivatives such as bisphenol A and bisphenol S. These diol residues may be contained alone or in combination of two or more kinds.
[0047] In particular, the diol residue preferably contains ethylene glycol as the first diol residue and at least one selected from the group consisting of diethylene glycol, neopentyl glycol, hexanediol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, pentamethylene glycol, and 1,4-cyclohexanedimethanol as the second diol residue, and particularly preferably contains at least one selected from the group consisting of diethylene glycol, 1,4-butanediol, and 1,4-cyclohexanedimethanol as the second diol residue.
[0048] The polyester resin is preferably a mixture of two or more types from the viewpoint of obtaining desired physical properties, and from the viewpoint of transparency, it is preferably a mixture of polyester resins having high compatibility. When using two or more types of polyester resins that are incompatible with each other, it is preferable to combine polyester resins having a small refractive index difference or a small viscosity difference at the extrusion molding temperature from the viewpoint of dispersibility.
[0049] As a preferred polyester-based resin of the present invention, from the viewpoint of being able to produce a clean peeled surface (peeling appearance) without leaving any film residue or fuzz during peeling, a mixture of a polyethylene terephthalate / isophthalate copolymer and a polyester-based resin other than a polyethylene terephthalate / isophthalate copolymer is preferred, and a mixture of a polyethylene terephthalate / isophthalate copolymer and at least one selected from the group consisting of polybutylene terephthalate and glycol-modified polyethylene terephthalate is particularly preferred. In other words, by mixing a polyethylene terephthalate / isophthalate copolymer, which is a hard and brittle resin, with polybutylene terephthalate or glycol-modified polyethylene terephthalate, the stress required for breaking is reduced while maintaining the same breaking elongation as polybutylene terephthalate and glycol-modified polyethylene terephthalate, which tends to result in a clean peeling surface (peeling appearance) without leaving any residual film or fuzz. The breaking stress and breaking elongation of polyester resins are influenced by the copolymer composition, molecular weight, molecular weight distribution, molecular structure such as branching, and three-dimensional structure such as crystallinity and orientation.
[0050] In addition, when a mixture of a polyethylene terephthalate / isophthalate copolymer and a polyester resin other than polyethylene terephthalate / isophthalate copolymer is used as the polyester resin, the ratio [polyethylene terephthalate / isophthalate copolymer: polyester resin other than polyethylene terephthalate / isophthalate copolymer] is usually 99:1 to 1:99, preferably 95:5 to 20:80, more preferably 90:10 to 40:60, based on mass. When the ratio of the polyethylene terephthalate / isophthalate copolymer and the polyester resin other than polyethylene terephthalate / isophthalate copolymer is within the above range, anti-fogging properties tend to be excellent.
[0051] The melting point of the polyester resin is usually 280° C. or less. The upper limit of the melting point is preferably 260° C. or less, more preferably 240° C. or less, and even more preferably 220° C. or less. The lower limit of the melting point is not particularly limited, but the lower the better, and it is most preferable that the resin does not exhibit a melting point. By setting the melting point within the above range, the mechanical properties of the present film tend to be good.
[0052] The storage modulus E' of the polyester resin at 20° C. is usually 100 to 5000 MPa, preferably 500 to 4000 MPa, and more preferably 1000 to 3000 MPa. By setting the storage modulus E' at 20° C. within the above range, there is a tendency for a clean peeled surface (peeling appearance) to be obtained without film residue or fluffing.
[0053] The glass transition temperature (Tg) of the polyester resin is usually 30 to 120° C., preferably 40 to 100° C., and more preferably 50 to 90° C. By setting the glass transition temperature within the above range, there is a tendency for a clean peeled surface (peeling appearance) to be obtained without any film residue or fluffing.
[0054] As described above, the resin composition forming the seal layer (III) contains 0.1 to 10% by mass of a surfactant when the resin composition is taken as 100% by mass. Usually, when a polyester film is used as a lid for a container, for example, if the contents contain some moisture and there is a space between the contents in the base container and the lid, the surface of the lid facing the contents, i.e., the surface of the seal layer, may become cloudy due to the moisture in the contents depending on the outside air temperature, and the visibility of the contents may become poor. On the other hand, in this film, the resin composition forming the seal layer (III) contains a specific amount of a surfactant, so that the deterioration of visibility can be suppressed. In addition, when this film is used as a lid material, by containing a specific amount of surfactant in the sealing layer (III), the surfactant continuously bleeds onto the surface of the sealing layer (III) of the lid material, thereby enabling the effect to be sustained continuously.
[0055] The surfactant is not particularly limited, and examples thereof include nonionic surfactants, cationic surfactants, and anionic surfactants. Among these, from the viewpoints of compatibility with the polyester resin and not impairing the anti-fogging effect or sealability, nonionic surfactants and anionic surfactants are preferred, with anionic surfactants being more preferred. The surfactants may be used in combination. For example, it is preferable to use a nonionic surfactant and an anionic surfactant in combination.
[0056] Conventionally, when a seal layer is formed from a resin composition containing a polyester resin and a surfactant, the compatibility between the polyester resin and the surfactant is poor, and kneading is insufficient, resulting in problems such as the seal layer becoming opaque and not exhibiting sufficient antifogging properties. Therefore, a method of applying a surfactant solution to the surface of the seal layer, rather than kneading the surfactant with the polyester resin, is often used. On the other hand, it has been found that the present film tends to have both anti-fogging properties and transparency by using a specific polyester resin and a specific type of surfactant, and further tends to have excellent anti-fogging properties (low-temperature anti-fogging properties) that prevent the film surface from fogging even when stored at low temperatures such as in a refrigerator.
[0057] (anionic surfactant) Examples of the anionic surfactant include alkali metal salts or alkaline earth metal salts of alkylsulfonic acid, alkylarylsulfonic acid, arylsulfonic acid, alkylsulfuric acid, alkylarylsulfuric acid, and arylsulfuric acid. These may be used alone or in combination of two or more. Among them, metal salts such as sodium, potassium, lithium, magnesium, and calcium of alkylsulfonic acid, alkylarylsulfonic acid, and alkylsulfuric acid having 8 to 30 carbon atoms, more preferably having 12 to 16 carbon atoms, are preferred, and sodium and potassium salts are particularly preferred.
[0058] (cationic surfactant) Examples of the cationic surfactant include alkylamine salts, quaternary ammonium salts, etc. The cationic surfactant is preferable from the viewpoint of surface activity and compatibility with the resin.
[0059] (Nonionic surfactant) The nonionic surfactant may be, for example, an ethylene oxide adduct or polyethylene glycol, and may be used alone or in combination of two or more kinds. The ethylene oxide adduct is a compound obtained by adding ethylene oxide to alcohol, fatty acid, their esters, oils, etc., and the lipophilic-hydrophilic parameter (HLB) is adjusted to a desired value by adjusting the chain length of the polymerized portion of ethylene oxide. Specific examples of the ethylene oxide adduct include polyoxyethylene alkyl ether, polyoxyethylene sorbitan fatty acid ester, polyoxyethylene fatty acid ester, etc. The polyethylene glycol has a structure in which ethylene glycol is polymerized, and has a similar structure to polyethylene oxide, but the molecular weight of polyethylene glycol is about 20,000, whereas the molecular weight of polyethylene oxide is several tens of thousands or more. Among these, polyoxyethylene alkyl ether is preferred because it combines antifogging properties and transparency when used in combination with an anionic surfactant, and the alkyl group more preferably has 8 to 30 carbon atoms, and even more preferably has 12 to 16 carbon atoms.
[0060] The content of the surfactant relative to the resin composition is 0.1 to 10% by mass, preferably 0.2 to 8% by mass, and particularly preferably 0.3 to 6% by mass. If the content of the surfactant is equal to or greater than the above-mentioned numerical value, even when a content containing moisture is packaged with the present film and stored in a low-temperature environment, the moisture inside the package is likely to form a uniform water film without forming droplets on the surface of the sealant film. In addition, since the film has excellent antifogging properties from room temperature to low temperatures, the visibility of the contents is good and the aesthetic appearance of the product is excellent. Furthermore, since the film has an excellent antistatic effect, film-forming problems such as blocking and triboelectric charging can be suppressed. In addition, if the content of the surfactant is equal to or less than the above-mentioned numerical value, the transparency can be made good.
[0061] In order to improve the transparency of the present film, it is more preferable to use anionic surfactants and nonionic surfactants in combination. Specifically, when the content of anionic surfactants in the seal layer is increased in order to improve anti-fogging properties, the seal strength, peelability, and transparency may be reduced, but by using anionic surfactants and nonionic surfactants in combination, it is possible to achieve both anti-fogging properties, seal strength, peelability, and transparency.
[0062] When a nonionic surfactant and an anionic surfactant are used in combination, the ratio (nonionic surfactant:anionic surfactant) is usually 5:95 to 50:50, preferably 10:90 to 40:60, on a mass basis.
[0063] The polyester resin and the surfactant can be mixed by a known method. For example, a master batch having a high surfactant concentration, which is prepared by kneading the polyester resin and the surfactant in advance with a twin-screw extruder or the like, may be dry-blended with the polyester resin, or a master batch prepared to a predetermined concentration may be used. In addition, the polyester resin and the surfactant may be dry-blended directly in an extruder for film formation. Among them, it is preferable to prepare the master batch with a twin-screw extruder from the viewpoint of the dispersibility of the surfactant in the polyester resin.
[0064] (Other Ingredients) The resin composition forming each layer of the present film need only contain the above-mentioned resin as its main component, and may contain other resins or the following additives within the scope that does not impair the function of the present invention.
[0065] Examples of the additives include colorants, inorganic fillers, organic fillers, ultraviolet absorbers, light stabilizers, heat stabilizers, antioxidants, lubricants, hydrolysis inhibitors, plasticizers, flame retardants, mold release agents, etc. The amounts of these additives to be added are not particularly limited, and can be appropriately determined within the range that does not impair the desired physical properties of the present invention.
[0066] <Manufacturing method of this film> The method for producing the present film is not particularly limited, so long as the film can be produced so that the seal layer (III) is located on the outermost surface of one side of the present film and the seal layer (III) and the seal adjacent layer (II) are arranged directly adjacent to each other. For example, the seal layer (III) and the seal adjacent layer (II) may be co-extruded using a known T-die method or inflation method, a feed block method, a multi-manifold method, or a combination thereof, or each layer may be produced as a single layer film and then thermally laminated, or one layer may be extrusion laminated to the other.
[0067] The base layer (I) may be co-extruded with the seal layer (III) and the seal adjacent layer (II), or the base layer (I) may be formed on the laminate film of the seal layer (III) / seal adjacent layer (II) by dry lamination, wet lamination, sand lamination, thermal lamination, or extrusion lamination. When laminating, anchor coat treatment or surface treatment such as plasma or corona discharge may be performed as necessary. In dry lamination or wet lamination, various adhesives such as known urethane adhesives, acrylic adhesives, and polyester adhesives may be used. Alternatively, the substrate layer (I), the seal adjacent layer (II) and the seal layer (III) may be prepared by co-extrusion, and the biaxially stretched film may be laminated on the substrate layer (I) as the substrate layer (I). The lamination method and surface treatment method are as described above. The present film may be unstretched, or may be uniaxially or biaxially stretched by a known method, and the biaxial stretching may be simultaneous or sequential. When a biaxially stretched film is further laminated as the base layer (I) as described above, the present film may be stretched as necessary before lamination.
[0068] <Thickness of each layer and film> The thickness of the seal adjacent layer (II) and the seal layer (III) of the present film is preferably 1.0 to 50 μm, more preferably 1.5 to 40 μm, and particularly preferably 2.0 to 30 μm, for each of the layers, taking into consideration the balance between the total thickness of the film and the thicknesses of the other layers. If the thickness of the seal adjacent layer (II) and the seal layer (III) is 1.0 μm or more, the film formability of the film tends to be improved, and if it is 50 μm or less, it is preferable from the viewpoint of economic efficiency.
[0069] The total thickness of the present film is preferably 10 to 100 μm, and more preferably 15 to 50 μm. If the total thickness of the present film is 10 μm or more, the film strength tends to be sufficient, and if it is 100 μm or less, the heat transfer property in the heat sealing step and the film transparency tend to be excellent.
[0070] The film thus produced can have the following physical properties:
[0071] <Total light transmittance> The total light transmittance of the present film is preferably 85% or more, and more preferably 88% or more, from the viewpoints of visibility of contents, aesthetics, design, etc. The lower limit is not particularly limited, and a larger value is preferable since transparency is good. The total light transmittance is a value measured based on JIS K7136 (2000).
[0072] <All Haze> The total haze of the present film is preferably 50% or less, more preferably 45% or less, from the viewpoints of visibility of contents, aesthetics, design, etc. The lower limit is not particularly limited, and a smaller value is preferable since transparency is good. The total haze is a value measured based on JIS K7136 (2000).
[0073] <Internal haze> The internal haze of the present film is preferably 50% or less, more preferably 45% or less, from the viewpoints of visibility of contents, aesthetics, design, etc. The lower limit is not particularly limited, and a smaller value is preferable since transparency is good. The internal haze is a value measured based on JIS K7136 (2000).
[0074] <External haze> The external haze of the present film is preferably 20% or less, more preferably 10% or less, from the viewpoints of visibility of contents, aesthetics, design, etc. The lower limit is not particularly limited, and a smaller value is preferable since transparency is good. The external haze is a value measured based on JIS K7136 (2000).
[0075] <Contact angle> A drop of 1 μL of distilled water is dropped on the surface of the sealing layer (III) of the present film at 23° C., and the contact angle (wettability) after 20 seconds is preferably 50° or less, more preferably 45° or less, from the viewpoint of the anti-fogging properties of the film. The lower limit of the contact angle is not particularly limited, and a smaller value means that the water wets and spreads on the sealing layer surface, which is preferable.
[0076] <Anti-fogging properties> Since the present film contains a surfactant in the sealing layer (III), it exhibits excellent anti-fogging properties, and further exhibits good anti-fogging properties even in a low temperature environment. For example, when 80 mL of water at a specified temperature (90°C, 40°C) or 100 mL of water at room temperature (25°C) is placed in a cylindrical polypropylene container having a bottom diameter of 50 mm and a depth of 80 mm, the film is attached to the opening of the container with double-sided tape with the sealing layer (III) of the film facing the container, and the container is allowed to stand for a specified period of time (10 seconds, 1 minute, or 48 hours), water vapor does not condense on the surface of the film sealing layer, and even if moisture condenses on the film surface, a uniform water film is formed rather than becoming lenticular, allowing the contents to be clearly observed.
[0077] <Tensile breaking stress> The tensile breaking stress of the seal layer (III) of the present film in the machine direction (MD) of the film is preferably 85 MPa or less, more preferably 82 MPa or less, even more preferably 78 MPa or less, and most preferably 71 MPa or less. By being in the above range, when the present film is peeled off at the interface between the seal adjacent layer (II) and the seal layer (III), the seal layer (III) in close contact with the adherend is pulled toward the peel layer (seal adjacent layer (II)) and does not stretch too much, so that the easy peelability is good. The lower limit is not particularly limited, but is generally 20 MPa or more.
[0078] In addition, the tensile breaking stress of the seal layer (III) of this film in the direction perpendicular to the flow direction of the film (TD) is preferably 78 MPa or less, more preferably 75 MPa or less, even more preferably 73 MPa or less, and most preferably 65 MPa or less. By being in the above range, when this film is peeled off at the interface between the seal adjacent layer (II) and the seal layer (III), the seal layer (III) in close contact with the adherend is pulled toward the peel layer (seal adjacent layer (II)) side and does not stretch too much, so that the easy peelability is good. The lower limit is not particularly limited, but is generally 20 MPa or more.
[0079] <Tensile elongation at break> The tensile elongation at break of the seal layer (III) of the present film is preferably 10% or less, more preferably 8% or less, even more preferably 5% or less, and most preferably 3% or less. By being in the above range, when the present film is peeled off at the interface between the seal adjacent layer (II) and the seal layer (III), the seal layer (III) in close contact with the adherend is pulled toward the peel layer (seal adjacent layer (II)) and does not stretch too much, so that the easy peelability is good. The lower limit is not particularly limited, but is generally 0.5% or more.
[0080] The tensile stress at break of the sealing layer (III) can be determined by measuring at a speed of 200 mm / sec according to JIS K 7127 (1999). The measurement may be performed by peeling only the sealing layer (III) from the present film and measuring the sealing layer (III) alone, or by producing a single film from the resin composition forming the sealing layer (III) and measuring the same.
[0081] <Package> The present film can be made into a package by heat-sealing the sealing layer (III) of the present film to a container made of a resin composition containing a polyester-based resin as a main component. Specific examples of the container form include cups, deep-drawn bodies, blister packs, etc., formed from non-oriented polyester sheets (A-PET sheets) made of polyester-based resins. The packages thus obtained are suitable for packaging foods, medicines, medical products, industrial parts, etc., for which visibility of contents and aesthetic appearance are important. EXAMPLES
[0082] The present invention will be described in more detail with reference to the following examples and comparative examples, but the present invention is not limited to the following examples. Prior to the examples, the following raw materials were prepared.
[0083] [Base material layer (I)] PO-1: Linear low-density polyethylene (melting point: 121°C, storage modulus at 20°C: 499MPa) PO-2: Low density polyethylene (melting point: 107℃, storage modulus at 20℃: 226MPa)
[0084] [Seal adjacent layer (II)] MAPO-1: Maleic anhydride modified ethylene-butene copolymer (density: 902 kg / m 3 , 20℃ storage modulus: 41MPa) MAPO-2: Maleic anhydride modified ethylene-propylene-butene copolymer (density: 888 kg / m 3 , 20℃ storage modulus: 25MPa) MAPO-3: Maleic anhydride modified ethylene-propylene-butene copolymer (density: 903 kg / m 3 , 20℃ storage modulus: 64MPa)
[0085] [Sealing layer (III)] [Polyester resin] PS-1: Polyethylene terephthalate / isophthalate copolymer (glass transition temperature: 73°C, melting point: none, storage modulus at 20°C: 2241MPa) PS-2: Glycol-modified polyethylene terephthalate (glass transition temperature: 71°C, melting point: none, storage modulus at 20°C: 1802MPa)
[0086] [Surfactants] S-1: Sodium alkylsulfonate S-2: Mixture of sodium alkylsulfonate and polyoxyethylene alkyl ether
[0087] <Examples 1 to 7, Comparative Examples 1 and 2> The raw materials having the composition shown in Table 1 below were fed to each extruder, and the base layer (I), seal adjacent layer (II), and seal layer (III) were melt-extruded in contact with each other using a T-die coextrusion method at an extrusion temperature of 220°C, and then cooled with a water-cooled metal cooling roll at 60°C to obtain a laminated film.
[0088] <Evaluation method> The laminated films obtained in the examples and comparative examples were measured and evaluated by the following methods. The results are shown in Table 1 below.
[0089] [Transparency (total light transmittance, total haze, internal haze, external haze)] Based on JIS K7136 (2000), the total light transmittance and total haze of each laminate film were measured using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name: NDH5000) under conditions of light source D65 and temperature 25°C. After measuring the total haze, each laminate film was immersed in a cell containing ethanol (purity 99.5% by mass) to measure the internal haze. The external haze was calculated from the difference between the total haze and the internal haze.
[0090] [Contact angle (wettability)] A droplet of 1 μL of distilled water was dropped onto the surface of the seal layer (III) of each laminate film at 23° C., and the contact angle was measured 20 seconds later.
[0091] [Tensile stress at break and tensile elongation at break] The tensile breaking stress and tensile breaking elongation of the seal layer (III) of each laminated film were measured at a speed of 200 mm / sec in accordance with JIS K 7127 (1999).
[0092] [Anti-fogging properties] 80 mL of hot water adjusted to 90°C or 40°C was poured into a cylindrical polypropylene container having a bottom diameter of 50 mm and a depth of 80 mm. Next, the sealing layer (III) side of each laminated film was attached to the opening of the container with double-sided tape facing the container, and the container was sealed. The film was left to stand for a predetermined time, and the degree of cloudiness of the film was observed and evaluated according to the following criteria. In addition, the anti-fogging property in a low-temperature environment was evaluated by pouring 100 mL of water at room temperature (25°C) into the cylindrical polypropylene container, sealing the opening of the container with the sealing layer (III) side of the film facing the container using double-sided tape, and leaving the film in a thermostatic chamber at 5°C for 48 hours. The degree of fogging of the film was observed and evaluated according to the following criteria. [Evaluation Criteria] ◯: Moisture spreads evenly over the entire surface of the film facing the contents, allowing the contents to be clearly seen. △: The surface of the film facing the contents was wet (uneven) without forming droplets, and the contents were visible. ×: Moisture condenses on the surface of the film facing the contents, forming fine droplets that make the film cloudy and the contents invisible.
[0093] [Film residue (appearance), easy peeling] The base layer (I) side of the laminated film obtained in the examples and comparative examples was heat-laminated with the LDPE side of a commercially available PA6 / LDPE laminated film (total thickness 75 μm, PA6: 15 μm, LDPE: 60 μm), and then the seal layer (III) of the laminated film was heat-sealed with a commercially available non-oriented polyester sheet (A-PET sheet, thickness 250 μm) using a packaging machine (R530 manufactured by Multipack) at 150 ° C. for 2.0 sec. Strip test pieces 15 mm wide x 50 mm long were taken in the flow direction of the film (machine direction, MD) and in the direction perpendicular to the flow direction of the film (transverse direction, TD). A tensile test (test temperature 23°C, tensile speed 300mm / min, peel angle 180°) was performed on the strip test pieces using a tensile tester (Shimadzu AG-X plus) in accordance with JIS K6854-2 (1999), and the peel strength was measured in the film flow direction (machine direction, MD) and in the direction perpendicular to the film flow direction (transverse direction, TD), and evaluated according to the following criteria. In addition, the appearance after peeling was visually observed and evaluated according to the following criteria. [Easy peelability (peel strength) evaluation criteria] ○: Peel strength is 400g·f / 15mm or more and 1500g·f / 15mm or less △: Peel strength is 100g·f / 15mm or more but less than 400g·f / 15mm, or 1500g·f / 15mm or more but less than 2500g·f / 15mm ×: Peel strength is less than 100g·f / 15mm or more than 2500g·f / 15mm [Film Remaining (Appearance) Evaluation Criteria] ◎: No film residue or fluffing ○: There is a small amount of film remaining or fuzzing △: There is some film remaining or fuzz in some areas ×: Film remains or fuzz is present on the entire surface
[0094] [Table 1]
[0095] As can be seen from Table 1, the multilayer films of Examples 1 to 7 had good peelability, good appearance after peeling, and good transparency.
[0096] The films of Comparative Examples 1 and 2 had high tensile breaking stress, and film residue and fluffing occurred. Moreover, the multilayer film of Comparative Example 1, which did not contain a surfactant, had poor anti-fogging properties. [Industrial Applicability]
[0097] This film has good easy-opening properties, transparency, and anti-fogging properties for containers and other products made of a resin composition containing a polyester resin as the main component, and forms a clean peel-off surface (peeling appearance) without leaving any residual film or fuzz on the sealing layer, making it ideal for packaging foods, medicines, medical supplies, industrial parts, and other products where visibility of the contents and aesthetics are important. Specifically, the packaging form is a laminated film that can be suitably used as a lid for containers such as cups, deep-drawn bodies, and blister packs, which are made of a non-oriented polyester sheet (A-PET sheet) made of polyester-based resin.
Claims
1. A laminated film having at least three layers, namely, a substrate layer (I), a seal adjacent layer (II), and a seal layer (III), and satisfying the following (1) to (4): (1) The resin composition forming the substrate layer (I) contains a thermoplastic resin as a main component. (2) The resin composition forming the seal adjacent layer (II) contains a polyolefin resin as a main component. (3) The resin composition forming the seal layer (III) contains a polyester resin as a main component, and the polyester resin contains isophthalic acid as a dicarboxylic acid residue and at least two kinds of residues as a diol residue. (4) The resin composition forming the seal layer (III) contains a surfactant in an amount of 0.1 to 10% by mass when the resin composition is taken as 100% by mass.
2. The polyester resin contains ethylene glycol as the first diol residue, and contains at least one selected from the group consisting of diethylene glycol, neopentyl glycol, hexanediol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, pentamethylene glycol, and 1,4-cyclohexanedimethanol as the second diol residue. The laminated film according to claim 1.
3. 3. The laminated film according to claim 1 or 2, wherein the contact angle of the sealing layer (III) measured in accordance with JIS K6768 (1999) is 50° or less.
4. 3. The laminated film according to claim 1, wherein the sealing layer (III) has a tensile breaking stress in the machine direction of the film of 85 MPa or less, measured in accordance with JIS K7127 (1999).
5. The thermoplastic resin contained in the resin composition forming the base layer (I) is at least one selected from polyolefin-based resins, polyamide-based resins, polyester-based resins, polystyrene-based resins, and ethylene-vinyl acetate copolymers. The laminate film according to claim 1 or 2.
6. 3. The laminated film according to claim 1, wherein the polyolefin resin contained in the resin composition forming the seal adjacent layer (II) is a polyethylene resin.
7. 3. A package formed by heat-sealing the seal layer (III) of the laminated film according to claim 1 or 2 with a container made of a resin composition containing a polyester resin as a main component.
Citation Information
Patent Citations
Sealant film and packaging material
JP2019171792A
Peelable film
JP1992094933A
Easy opening packaging material
JP2001328221A
Antifogging multilayer film, laminate using same, and packaging material
WO2015046132A1