Foam and laminate
A foam made from ethylene/α-olefin copolymer with controlled residual nitrogen and using physical foaming with carbon dioxide addresses odor and discoloration issues, ensuring high performance for footwear applications.
Patent Information
- Application Number
- JP2023059373
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing ethylene/α-olefin copolymer foams face issues with odor and discoloration due to the use of organic chemical blowing agents like azodicarbonamide (ADCA), and there is a need for a foam that suppresses these issues while maintaining excellent performance.
The foam is formulated with an ethylene/α-olefin copolymer containing specific properties, including a residual nitrogen content of 200 ppm or less, and is produced using a physical foaming method with safer gases like carbon dioxide, reducing the reliance on ADCA.
The solution effectively suppresses odor and discoloration while maintaining excellent foam performance, making it suitable for applications in footwear and footwear parts.
Smart Images

Figure 2024146464000001 
Figure 2024146464000002 
Figure 2024146464000003
Abstract
Description
[Technical field]
[0001] The present invention relates to foams and laminates, and more particularly to foams and laminates comprising an ethylene-α-olefin copolymer. [Background technology]
[0002] Crosslinked foams, which have a low specific gravity, i.e., are lightweight and flexible, and have high mechanical strength, have been widely used for interior and exterior building materials, interior materials, automobile parts such as door glass runs, packaging materials, daily necessities, etc. Foams obtained by simply foaming resin to reduce weight have low mechanical strength, so it is a known technique to suppress the decrease in mechanical strength by further bonding molecular chains within the foam through a crosslinking reaction of the resin.
[0003] Resin crosslinked foams are also used in footwear or footwear parts, such as the soles (mainly midsoles) of sports shoes, etc. This is because footwear or footwear parts are required to be lightweight, to be resistant to deformation due to long-term use, and to have mechanical strength and resilience sufficient to withstand severe use conditions.
[0004] It is widely known that crosslinked foams of ethylene-vinyl acetate copolymer have been conventionally used for shoe soles. However, crosslinked foams molded using this ethylene-vinyl acetate copolymer composition have a high specific gravity and a large compression set. Therefore, when used for shoe soles, for example, there are problems in that the soles are heavy and the soles are compressed over long-term use, causing a loss of mechanical strength such as rebound resilience.
[0005] On the other hand, crosslinked foams using ethylene-α-olefin copolymers have high mechanical strength, light weight and flexibility, and therefore are used in building exterior and interior materials, automobile parts such as door glass runs, packaging materials, daily necessities, etc., and attempts have been made to use them in footwear or footwear parts, such as soles (mainly midsoles) of sports shoes, etc. In this regard, Patent Documents 1 and 2 respectively describe inventions relating to crosslinked foams using ethylene-α-olefin copolymers and crosslinked foams using a mixture of ethylene-vinyl acetate copolymer and ethylene-α-olefin copolymer, but although these inventions improve the low specific gravity and compression set properties, sufficient performance is not obtained.
[0006] Various attempts have been made to obtain a foam with a low specific gravity and a small compression set. For example, Patent Document 4 discloses a foam usable for footwear and footwear parts, which is obtained by crosslinking and foaming a composition containing an ethylene-α-olefin copolymer, a small amount of an ethylene-α-olefin-non-conjugated polyene copolymer, azodicarbonamide (ADCA), and a crosslinking agent. Patent Document 4 also discloses that, while having a low specific gravity, this foam has a small compression set compared to foams obtained from a composition that does not contain an ethylene-α-olefin-non-conjugated polyene copolymer. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Special Publication No. 9-501447 [Patent Document 2] Japanese Patent Application Publication No. 11-206406 [Patent Document 3] Japanese Patent Application Publication No. 11-5818 [Patent Document 4] International Publication No. 2007 / 132731 Brochure Summary of the Invention [Problem to be solved by the invention]
[0008] Ethylene-α-olefin copolymer foams are produced by expanding ethylene-α-olefin copolymers with gas. Representative methods for expanding ethylene-α-olefin copolymers include physical foaming and chemical foaming.
[0009] Physical foaming is a method of foaming plastics by dissolving a gas or supercritical fluid in plastics such as ethylene-α-olefin copolymers under high pressure, and then reducing the solubility of the gas by lowering the pressure or heating to generate bubbles. The gas or supercritical fluid used in physical foaming is called a physical foaming agent. When physically foaming plastics such as ethylene-α-olefin copolymers, liquefied gases that are highly soluble in plastics, such as fluorocarbons and hydrocarbons, have traditionally been used as physical foaming agents to ensure sufficient foaming. However, fluorocarbons and hydrocarbons have problems such as ozone layer destruction, global warming, and flammability, so safer substances such as carbon dioxide and nitrogen are being considered as replacements. However, carbon dioxide and nitrogen tend to be less soluble in plastics than fluorocarbons and hydrocarbons in their normal gaseous state.
[0010] On the other hand, chemical foaming is a method of foaming plastics by compounding a chemical substance that generates gas through a chemical reaction with plastics such as ethylene-α-olefin copolymers, and generating bubbles with the gas generated by the chemical reaction of the chemical substance. Here, the chemical substance used in chemical foaming is called a chemical foaming agent. Such chemical foaming agents include organic chemical foaming agents such as azodicarbonamide (ADCA) and inorganic chemical foaming agents such as baking soda.
[0011] Here, in the past, when producing foams of ethylene-α-olefin copolymers, organic chemical blowing agents such as azodicarbonamide (ADCA) have been widely used because the foams can be easily produced using general-purpose molding machines and a large amount of gas is generated during thermal decomposition. However, when producing foams using organic chemical blowing agents such as azodicarbonamide (ADCA), the resulting foams may have problems such as odor and discoloration due to the organic chemical blowing agent. When such foams are used in footwear and footwear parts, it is necessary to reduce problems such as odor and discoloration as much as possible.
[0012] Therefore, an object of the present invention is to provide a foam that can suppress odors and discoloration caused by chemical foaming agents such as azodicarbonamide (ADCA) while also achieving excellent foam performance. [Means for solving the problem]
[0013] As a result of intensive research into solving the above-mentioned problems, the inventors have found that the above-mentioned problems can be solved by adjusting the content of a certain specific component in an ethylene-α-olefin copolymer foam to a certain level or less, and have thus completed the present invention.
[0014] The present invention relates to the following [1] to
[13] . [1] An ethylene-α-olefin copolymer (A) obtained by copolymerizing only ethylene and an α-olefin having 3 to 20 carbon atoms, Residual nitrogen measured by chemiluminescence method is 200ppm or less Foam.
[0015] [2] The foam according to [1], comprising an ethylene-polar monomer copolymer (B). [3] The foam according to [1] or [2], further comprising a crosslinking agent (C).
[0016] [4] The foam according to any one of [1] to [3], wherein the ethylene-α-olefin copolymer (A) satisfies the following requirements (Aa) and (Ab): (Aa) Density 0.850-0.910g / cm 3 in the range of; (Ab) Melt flow rate (MFR) measured at 190°C under a load of 2.16 kg according to the method of ASTM D1238 2.16 ) is in the range of 0.01 to 200 g / 10 min.
[0017] [5] The foam according to any one of [1] to [4], wherein the ethylene / α-olefin copolymer (A) satisfies the following requirements (Ac) and (Ad): (Ac) 1 The vinyl group content per 1,000 carbon atoms as determined by H-NMR is in the range of 0.025 to 0.3; (Ad)MFR 10 / MFR 2.16 is in the range of 7 to 20 (but MFR 10 is the melt flow rate measured at 190°C under a load of 10 kg according to the method of ASTM D1238, and MFR 2.16 is the melt flow rate measured at 190°C under a load of 2.16 kg according to the method of ASTM D1238.
[0018] [6] A layer made of the foam according to any one of [1] to [5], A layer made of at least one material selected from the group consisting of polyolefin, polyurethane, rubber, leather and artificial leather; A laminate having the following structure:
[0019] [7] Footwear comprising the foam according to any one of [1] to [5] or the laminate according to [6]. [8] A footwear part comprising the foam according to any one of [1] to [5] or the laminate according to [6].
[0020] [9] The footwear part according to [8], which is a midsole, an insole or a sole.
[0021]
[10] A method for producing a foam, comprising a step of physically foaming an ethylene-α-olefin copolymer (A) obtained by copolymerizing only ethylene and an α-olefin having 3 to 20 carbon atoms.
[0022]
[11] A method for producing a foam, comprising a step of physically foaming a composition containing an ethylene-α-olefin copolymer (A) obtained by copolymerizing only ethylene and an α-olefin having 3 to 20 carbon atoms and a crosslinking agent (C).
[0023]
[12] A method for producing a foam, comprising a step of impregnating an ethylene-α-olefin copolymer (A) obtained by copolymerizing only ethylene and an α-olefin having 3 to 20 carbon atoms with a supercritical fluid.
[0024]
[13] A method for producing a foam, comprising a step of impregnating a composition containing an ethylene-α-olefin copolymer (A) obtained by copolymerizing only ethylene and an α-olefin having 3 to 20 carbon atoms and a crosslinking agent (C) with a supercritical fluid. [Effect of the Invention]
[0025] According to the present invention, it is possible to provide a foam capable of achieving both suppression of odor and discoloration and excellent foam performance. [Embodiments for Carrying Out the Invention]
[0026] Hereinafter, the present invention will be specifically described. Here, in this specification, "~" indicating a numerical range means "not less than M and not more than N" when expressed as, for example, "M~N" (M and N are numerical values satisfying M < N) without particular notice.
[0027] Furthermore, in this specification, when an olefin constituting a certain polymer is represented by M, the expression "structural unit derived from M" is sometimes used, which means a "structural unit corresponding to M", that is, a structural unit having a pair of bonds formed by opening the π bond constituting the double bond of M. For example, a "structural unit derived from ethylene" means a structural unit represented by -CH2-CH2-, and a "structural unit derived from an α-olefin" specifically means a structural unit represented by -CH2-CRR'- (R and R' are each independently a hydrogen atom or an alkyl group).
[0028] [Foam] The foam of the present invention contains an ethylene-α-olefin copolymer (A) obtained by copolymerizing only ethylene with an α-olefin having 3 to 20 carbon atoms, and has a residual nitrogen amount of 200 ppm or less as measured by a chemiluminescence method.
[0029] <Ethylene-α-olefin copolymer (A)> The ethylene-α-olefin copolymer (A) constituting the foam of the present invention is a copolymer obtained by copolymerizing only ethylene and an α-olefin having 3 to 20 carbon atoms. That is, the ethylene-α-olefin copolymer (A) is a copolymer comprising structural units derived from ethylene and structural units derived from an α-olefin having 3 to 20 carbon atoms. The ethylene and the α-olefin having 3 to 20 carbon atoms may be, for example, monomers derived from fossil fuels or monomers derived from biomass, and these monomers may be used alone or in combination of two or more kinds.
[0030] The α-olefin constituting the ethylene-α-olefin copolymer (A) is an α-olefin having 3 to 20 carbon atoms, specifically, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-hexadecene, 1-octadecene, 1-nonadecene, 1-eicosene, 4-methyl-1-pentene, etc. Among these, α-olefins having 3 to 10 carbon atoms are preferred, and propylene, 1-butene, 1-hexene, and 1-octene are particularly preferred. These α-olefins may be used alone or in combination of two or more.
[0031] The ethylene-α-olefin copolymer (A) preferably contains 75 to 95 mol % and more preferably 80 to 95 mol % of structural units derived from ethylene and 5 to 25 mol % and more preferably 5 to 20 mol % of structural units derived from an α-olefin having 3 to 20 carbon atoms, the total amount of ethylene and α-olefin being 100 mol %.
[0032] The ethylene / α-olefin copolymer (A) preferably satisfies the following requirements (Aa) and (Ab).
[0033] (Aa) Density 0.850-0.910g / cm 3 is in the range. The ethylene-α-olefin copolymer (A) used in the present invention usually has a density of 0.850 g / cm 3 More than 0.855 g / cm 3 More preferably, 0.857 g / cm 3 More preferably, 0.858 g / cm 3 More than 0.910g / cm 3 Less than 0.909 g / cm 3 Less than or equal to 0.908 g / cm 3 More preferably, 0.907 g / cm 3The density of the ethylene-α-olefin copolymer (A) is a value measured at 23° C. in accordance with ASTM D1505. When the density satisfies such a range, the resulting foam is preferred because it has an excellent balance between flexibility and strength, and a good balance between rigidity and impact strength.
[0034] (Ab) Melt flow rate (MFR) measured at 190°C under a load of 2.16 kg according to the method of ASTM D1238 2.16 ) is in the range of 0.01 to 200 g / 10 min. The ethylene-α-olefin copolymer (A) used in the present invention has an MFR 2.16 The melt flow rate (measured at 190° C. under a load of 2.16 kg according to the method of ASTM D1238) is preferably in the range of 0.01 to 200 g / 10 min.
[0035] In the ethylene / α-olefin copolymer (A) used in the present invention, the MFR can be appropriately selected according to the application, preferably within this range. 2.16 is not particularly limited, but is usually 0.01 g / 10 min or more, preferably 0.08 g / 10 min or more, more preferably 0.05 g / 10 min or more, even more preferably 0.1 g / 10 min or more, particularly preferably 0.2 g / 10 min, and is usually 200 g / 10 min or less, preferably 100 g / 10 min or less, more preferably 40 g / 10 min or less, even more preferably 25 g / 10 min or less, particularly preferably 5 g / 10 min or less. The larger the molecular weight of the ethylene-α-olefin copolymer (A), the higher the MFR 2.16 tends to be smaller.
[0036] MFR 2.16 It is preferable that the MFR is equal to or less than the above upper limit in that the strength of the obtained molded article is improved. 2.16 It is preferable that the above lower limit value or more since the fluidity of the ethylene / α-olefin copolymer (A) during melt molding is improved.
[0037] The ethylene-α-olefin copolymer (A) satisfying the above requirements (Aa) and (Ab) may be in the form of a thermoplastic elastomer or a thermoplastic resin.
[0038] In addition to the above requirements (Aa) and (Ab), the ethylene / α-olefin copolymer (A) preferably further satisfies either the following requirement (Ac) or the following requirement (Ad), and more preferably satisfies both the following requirement (Ac) and the following requirement (Ad).
[0039] (Ac) 1 The vinyl group content per 1000 carbon atoms determined by 1 H-NMR is in the range of 0.025 to 0.3. The lower limit of the vinyl group content per 1000 carbon atoms of the ethylene-α-olefin copolymer (A) used in the present invention is usually 0.025, preferably 0.026, more preferably 0.027, even more preferably 0.028, and particularly preferably 0.03. The upper limit of the vinyl group content per 1000 carbon atoms of the ethylene-α-olefin copolymer (A) used in the present invention is usually 0.3, preferably 0.2, more preferably 0.15, even more preferably 0.1, and particularly preferably 0.09. The vinyl group content in the above range is preferred in terms of improving the mechanical strength of the resulting molded article.
[0040] The specific method for measuring the vinyl group content will be described in detail in the section "Amount of Double Bonds" in the Examples described later. In the ethylene-α-olefin copolymer (A) used in the present invention, the vinyl group is usually present at the terminal of the copolymer. The ethylene-α-olefin copolymer (A) used in the present invention has a vinyl group content per 1000 carbon atoms in the above range and has crosslinkability. When the vinyl group content is within the above range, the mechanical strength of the resulting molded article is excellent, which is preferable. When the vinyl group content is 0.3 or less per 1000 carbon atoms in the ethylene-α-olefin copolymer (A), crosslinking and polymer main chain scission during heat molding are reduced, resulting in excellent moldability. When the vinyl group content is 0.025 or more per 1000 carbon atoms in the ethylene-α-olefin copolymer (A), crosslinking is facilitated, and the compression set (CS) and mechanical strength of the molded article or crosslinked foam are excellent.
[0041] (Ad)MFR 10 / MFR 2.16 is in the range of 7 to 20. The ethylene-α-olefin copolymer (A) used in the present invention has an MFR 10 / MFR 2.16 is preferably in the range of 7 to 20, more preferably 7.2 to 15, and even more preferably 7.5 to 12. 10 is the melt flow rate (g / 10 min) measured at 190°C under a load of 10 kg according to the method of ASTM D1238, and MFR 2.16 is the melt flow rate (g / 10 min) measured at 190° C. under a load of 2.16 kg according to the method of ASTM D1238.
[0042] MFR 10 / MFR 2.16 is a value that is considered to be one of the indicators of the degree of long chain branching of a copolymer, and MFR 10 / MFR 2.16 A value in the above range is specified as having long chain branching. 10 / MFR 2.16 A lower value indicates less long chain branching. 10 / MFR 2.16When the MFR value is 7 or more, when a crosslinked foam is produced from a composition containing a large amount of the copolymer, the crosslinked foam has high shape precision and excellent dimensional stability. 10 / MFR 2.16 When the value is 20 or less, the physical properties such as strength are excellent.
[0043] MFR of ethylene-α-olefin copolymer (A) 10 / MFR 2.16 If the value is less than the above lower limit, for example, when the ethylene-α-olefin copolymer (A) is combined with components such as a foaming agent and a crosslinking agent to form a composition, and then injection molding and foaming are performed to produce a foam, the shape of the obtained foam may be low in precision, and the dimensions of the foam may vary. 10 / MFR 2.16 If the value exceeds the upper limit and is too large, the degree of dimensional variation is improved slightly, but the physical properties such as strength of the obtained foamed molded article may decrease, which is undesirable.
[0044] In the present invention, by using the ethylene-α-olefin copolymer (A) as the polymer component constituting the foam, a foam having a smaller compression set tends to be obtained more easily than when an ethylene-vinyl acetate copolymer is used as the polymer component instead of the ethylene-α-olefin copolymer (A). Among the ethylene-α-olefin copolymers (A), the ethylene-α-olefin copolymers (A) that satisfy the requirements (Aa) to (Ad) tend to give foams having a smaller compression set more easily than the ethylene-α-olefin copolymers (A) that satisfy only the requirements (Aa) and (Ab).
[0045] The ethylene / α-olefin copolymer preferably satisfies the following requirements (Ae) and / or (Af) in addition to the requirements (Aa) and (Ab). (Ae)Mw / Mn The ethylene-α-olefin copolymer (A) used in the present invention is not particularly limited, but the molecular weight distribution (Mw / Mn) calculated as the ratio of the weight average molecular weight Mw to the number average molecular weight Mn measured by gel permeation chromatography (GPC) is preferably 1.5 to 3.5, more preferably 1.5 to 3.0. Mw / Mn can be adjusted to the above range by appropriately selecting the polymerization catalyst as described in the section on olefin polymerization catalyst. In addition, it is preferable that Mw / Mn is within the above range in terms of improving the melt moldability and the strength of the obtained molded article.
[0046] (Af) Melting point (Tm) The ethylene / α-olefin copolymer (A) used in the present invention is not particularly limited, but has a melting point (Tm) determined from a DSC endothermic curve of preferably 40° C. or higher, more preferably 50° C. or higher, even more preferably 55° C. or higher, and preferably 130° C. or lower, more preferably 120° C. or lower, even more preferably 110° C. or lower. A melting point of the ethylene copolymer (A) within the above range is preferred in terms of the balance between rebound resilience and heat shrinkage.
[0047] <Production method of ethylene-α-olefin copolymer (A)> The method for producing the ethylene-α-olefin copolymer (A) is not particularly limited, but it can be suitably produced, for example, by copolymerizing ethylene with at least one α-olefin having 3 to 20 carbon atoms in the presence of an olefin polymerization catalyst.
[0048] Olefin polymerization catalyst The ethylene-α-olefin copolymer (A) used in the present invention has the above-mentioned properties. There is no limitation on the production method thereof. For example, it can be produced by copolymerizing ethylene and one or more selected from the group consisting of α-olefins having 3 to 20 carbon atoms in the presence of an olefin polymerization catalyst comprising the following catalytic components [A] and [B]:
[0049] [A] A bridged metallocene compound represented by the following general formula [I]:
[0050] [ka]
[0051] In formula [I], M represents a transition metal, p represents the valence of the transition metal, e.g., 4, X may be the same or different, and each represents a hydrogen atom, a halogen atom, or a hydrocarbon group, e.g., a chlorine atom, R 1 and R 2 represents a π-electron conjugated ligand coordinated to M, which may be the same or different, and Q represents R 1 and R 2 represents a divalent group that crosslinks [B] (b-1) organoaluminum oxy compound, (b-2) a compound that reacts with the bridged metallocene compound [A] to form an ion pair, and (b-3) Organoaluminum compounds At least one compound selected from the group consisting of:
[0052] The copolymerization can be carried out, for example, by solution polymerization of one or more monomers selected from the group consisting of ethylene and α-olefins in the presence of such an olefin polymerization catalyst at a temperature of 0 to 200° C. in the presence of a solvent.
[0053] However, the ethylene-α-olefin copolymer (A) used in the present invention is not limited to the above-mentioned production method as long as it satisfies the above-mentioned properties. For example, a metallocene compound having a structure different from the structure represented by the above formula [I] may be used in the copolymerization, a co-catalyst other than the catalyst component [B] may be used, or two or more known types of ethylene-based copolymers may be used to prepare the copolymer by a technique such as reactor blending or physical blending.
[0054] The above-mentioned method for producing an ethylene-α-olefin copolymer (A), which comprises copolymerizing ethylene with one or more selected from the group consisting of α-olefins having 3 to 20 carbon atoms in the presence of an olefin polymerization catalyst containing the catalyst components [A] and [B], will be further described below.
[0055] Catalyst component [A] The catalyst component [A] is a bridged metallocene compound represented by the above formula [I]. In the above formula [I], examples of the transition metal represented by M include Zr, Ti, Hf, V, Nb, Ta and Cr, and the preferred transition metal is Zr, Ti or Hf, and the more preferred transition metal is Zr or Hf.
[0056] In general formula [I], R 1 and R 2 Examples of the π-electron conjugated ligand represented by the formula (1) include ligands having an η-cyclopentadienyl structure, an η-benzene structure, an η-cycloheptatrienyl structure, and an η-cyclooctatetraene structure, and particularly preferred ligands are those having an η-cyclopentadienyl structure. Examples of the ligand having an η-cyclopentadienyl structure include a cyclopentadienyl group, an indenyl group, a hydrogenated indenyl group, and a fluorenyl group. These groups may be further substituted with a halogen atom, a hydrocarbon group such as an alkyl, an aryl, an aralkyl, an alkoxy, or an aryloxy group, a hydrocarbon-containing silyl group such as a trialkylsilyl group, or a linear or cyclic alkylene group. R 1 and R 2 In one preferred and exemplary embodiment of the present invention, the π-electron conjugated ligands represented by R 1 and R 2 The π-electron conjugated ligands represented by R 1 The π-electron conjugated ligand represented by the formula 2 The π-electron conjugated ligand represented by the formula (I) may be an octamethyloctahydrodibenzofluorenyl group.
[0057] The octamethyloctahydrodibenzofluorenyl group is 1,1,4,4,7,7,10,10-octamethyl-(5a,5b,11a,12,12a-η 5 )-1,2,3,4,7,8,9,10-octahydrodibenzo[b,H]fluorenyl group.
[0058] In the general formula [I], R represented by Q 1 and R 2 The group bridging R represented by Q is not particularly limited as long as it is a divalent group, and examples thereof include a linear or branched alkylene group, an unsubstituted or substituted cycloalkylene group, an alkylidene group, an unsubstituted or substituted cycloalkylidene group, an unsubstituted or substituted phenylene group, a silylene group, a dialkyl-substituted silylene group, a germyl group, and a dialkyl-substituted germyl group. 1 and R 2 The group bridging between is a di(p-tolyl)methylene group.
[0059] Specific examples of catalyst component [A] include the metallocene complexes used in the examples described below, but the catalyst component [A] is not limited to these compounds. Such a catalyst component [A] is preferably used together with a catalyst component [B] as a catalyst for olefin polymerization.
[0060] Catalyst component [B] When the catalyst component [A] is used as a component of an olefin polymerization catalyst for producing an ethylene-α-olefin copolymer (A), the olefin polymerization catalyst preferably contains a catalyst component [B] composed of at least one compound selected from the group consisting of (b-1) an organoaluminum oxy compound, (b-2) a compound that reacts with the catalyst component [A] to form an ion pair, and (b-3) an organoaluminum compound. From the viewpoints of polymerization activity and properties of the resulting olefin polymer, the catalyst component [B] is preferably used in any one of the following embodiments [c1] to [c4].
[0061] [c1] (b-1) Organoaluminum oxy compounds only [c2] (b-1) organoaluminum oxy compounds and (b-3) organoaluminum compounds, [c3] (b-2) a compound that reacts with the catalyst component [A] to form an ion pair, and (b-3) an organoaluminum compound, [c4] (b-1) an organoaluminum oxy compound and (b-2) a compound which reacts with the catalyst component [A] to form an ion pair.
[0062] However, when a bridged metallocene compound in which Q in the general formula [I] is a silylene group is used as the catalyst component [A], (b-2) a compound that reacts with the catalyst component [A] to form an ion pair is not used as the component [B], and only [c1] and [c2] are employed in the above-mentioned preferred [B] components; [c1] to [c4].
[0063] Each component that may constitute the catalyst component [B] will be specifically described below. (b-1) Organoaluminum oxy compounds As the organoaluminum oxy compound (b-1), a conventionally known aluminoxane can be used as it is. Specific examples include compounds represented by the following general formula [II] and / or general formula [III].
[0064] [ka]
[0065] (In formula [II] or [III], R is a hydrocarbon group having 1 to 10 carbon atoms, and n is an integer of 2 or more.) In particular, methylaluminoxanes in which R is a methyl group and n is 3 or more, preferably 10 or more, are used. (An organoaluminumoxy compound in which R is a methyl group in general formula [II] or [III] may be referred to as "methylaluminoxane" hereinafter.) As the organoaluminum oxy compound (b-1), it is also preferable to use a methylaluminoxane analogue that is soluble in a saturated hydrocarbon, such as a modified methylaluminoxane represented by the following general formula [IV].
[0066] [ka]
[0067] (In formula [IV], R represents a hydrocarbon group having 2 to 20 carbon atoms, and m and n represent integers of 2 or more.) The modified methylaluminoxane represented by the general formula [IV] is prepared using trimethylaluminum and an alkylaluminum other than trimethylaluminum (the manufacturing method is disclosed in, for example, US4960878, US5041584, etc.), and is commercially produced by manufacturers such as Tosoh Finechem Corporation under the trade names MMAO and TMAO, which are prepared using trimethylaluminum and triisobutylaluminum, where R is an isobutyl group (see, for example, "Tosoh Research and Technology Report," Vol. 47, p. 55 (2003)).
[0068] Furthermore, as the organoaluminum oxy compound (b-1), a benzene-insoluble organoaluminum oxy compound exemplified in JP-A-2-78687 may be used, or a boron-containing organoaluminum oxy compound represented by the following general formula [V] may be used.
[0069] [ka]
[0070] (In formula [V], R c R represents a hydrocarbon group having 1 to 10 carbon atoms. d may be the same or different and represent a hydrogen atom, a halogen atom, or a hydrocarbon group having 1 to 10 carbon atoms.) Incidentally, there is no problem if a small amount of an organoaluminum compound is mixed into the above-mentioned (b-1) organoaluminum oxy-compound.
[0071] (b-2) A compound that reacts with the catalyst component [A] to form an ion pair Examples of the compound (b-2) that reacts with the catalyst component [A] to form an ion pair (hereinafter, sometimes abbreviated as "ionic compound (b-2)") include Lewis acids, ionic compounds, borane compounds, and carborane compounds described in JP-T-1-501950, JP-T-1-502036, JP-A-3-179005, JP-A-3-179006, JP-A-3-207703, JP-A-3-207704, and USP 5321106. Furthermore, examples of the ionic compound (b-2) include heteropoly compounds and isopoly compounds.
[0072] In the present invention, the ionic compound (b-2) preferably used is a compound represented by the following general formula [VI].
[0073] [ka]
[0074] In formula [VI], R e+ As for H + , carbenium cation, oxonium cation, ammonium cation, phosphonium cation, cycloheptyltrienyl cation, ferrocenium cation having a transition metal, etc. f ~R i may be the same or different and are organic groups, preferably aryl groups.
[0075] Specific examples of the carbenium cation include tri-substituted carbenium cations such as triphenylcarbenium cation, tris(methylphenyl)carbenium cation, and tris(dimethylphenyl)carbenium cation.
[0076] Specific examples of the ammonium cation include trialkylammonium cations such as trimethylammonium cation, triethylammonium cation, tri(n-propyl)ammonium cation, triisopropylammonium cation, tri(n-butyl)ammonium cation, and triisobutylammonium cation; N,N-dialkylanilinium cations such as N,N-dimethylanilinium cation, N,N-diethylanilinium cation, and N,N-2,4,6-pentamethylanilinium cation; and dialkylammonium cations such as diisopropylammonium cation and dicyclohexylammonium cation.
[0077] Specific examples of the phosphonium cation include triarylphosphonium cations such as triphenylphosphonium cation, tris(methylphenyl)phosphonium cation, and tris(dimethylphenyl)phosphonium cation.
[0078] Of the above, R e+ As the cation, a carbenium cation, an ammonium cation, etc. are preferred, and in particular, a triphenylcarbenium cation, an N,N-dimethylanilinium cation, and an N,N-diethylanilinium cation are preferred.
[0079] Specific examples of the ionic compound (b-2) which is a carbenium salt include triphenylcarbenium tetraphenylborate, triphenylcarbenium tetrakis(pentafluorophenyl)borate, triphenylcarbenium tetrakis(3,5-ditrifluoromethylphenyl)borate, tris(4-methylphenyl)carbenium tetrakis(pentafluorophenyl)borate, and tris(3,5-dimethylphenyl)carbenium tetrakis(pentafluorophenyl)borate.
[0080] Examples of the ionic compound (b-2) which is an ammonium salt include trialkyl-substituted ammonium salts, N,N-dialkylanilinium salts, and dialkylammonium salts.
[0081] Specific examples of the ionic compound (b-2) which is a trialkyl-substituted ammonium salt include triethylammonium tetraphenylborate, tripropylammonium tetraphenylborate, tri(n-butyl)ammonium tetraphenylborate, trimethylammonium tetrakis(p-tolyl)borate, trimethylammonium tetrakis(o-tolyl)borate, tri(n-butyl)ammonium tetrakis(pentafluorophenyl)borate, triethylammonium tetrakis(pentafluorophenyl)borate, tripropylammonium tetrakis(pentafluorophenyl)borate, tripropylammonium tetrakis(2,4-dimethylphenyl)borate, tri(n-butyl)ammonium tetrakis(3,5-dimethylphenyl)borate, tri(n-butyl)ammonium tetrakis(4-trifluoromethylphenyl)borate, tri (n-butyl)ammonium tetrakis(3,5-ditrifluoromethylphenyl)borate, tri(n-butyl)ammonium tetrakis(o-tolyl)borate, dioctadecylmethylammonium tetraphenylborate, dioctadecylmethylammonium tetrakis(p-tolyl)borate, dioctadecylmethylammonium tetrakis(o-tolyl)borate, dioctadecylmethylammonium tetrakis(pentafluorophenyl)borate, dioctadecylmethylammonium tetrakis(2,4-dimethylphenyl)borate, dioctadecylmethylammonium tetrakis(3,5-dimethylphenyl)borate, dioctadecylmethylammonium tetrakis(4-trifluoromethylphenyl)borate, dioctadecylmethylammonium tetrakis(3,5-ditrifluoromethylphenyl)borate, dioctadecylmethylammonium and the like.
[0082] Specific examples of the ionic compound (b-2) which is an N,N-dialkylanilinium salt include N,N-dimethylanilinium tetraphenylborate, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis(3,5-ditrifluoromethylphenyl)borate, N,N-diethylanilinium tetraphenylborate, N,N-diethylanilinium tetrakis(pentafluorophenyl)borate, N,N-diethylanilinium tetrakis(3,5-ditrifluoromethylphenyl)borate, N,N-2,4,6-pentamethylanilinium tetraphenylborate, and N,N-2,4,6-pentamethylanilinium tetrakis(pentafluorophenyl)borate.
[0083] Specific examples of dialkylammonium salts include di(1-propyl)ammonium tetrakis(pentafluorophenyl)borate, dicyclohexylammonium tetraphenylborate, and the like.
[0084] As other ionic compounds (b-2), ionic compounds disclosed by the present applicant (JP-A-2004-51676) can also be used without any restrictions. The above ionic compounds (b-2) may be used alone or in combination of two or more.
[0085] (b-3) Organoaluminum compounds Examples of the organoaluminum compound (b-3) include an organoaluminum compound represented by the following general formula [VII] and an alkyl complex of a Group 1 metal and aluminum represented by the following general formula [VIII].
[0086] R a m Al(OR b ) n H p X q … [VII] (In formula [VII], R a and Rb may be the same as or different from each other, and represents a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms; X represents a halogen atom; m is a number where 0 < m ≦ 3, n is a number where 0 ≦ n < 3, p is a number where 0 ≦ p < 3, q is a number where 0 ≦ q < 3, and m + n + p + q = 3.) Specific examples of the organoaluminum compound represented by the general formula [VII] include tri-n-alkylaluminums such as trimethylaluminum, triethylaluminum, tri-n-butylaluminum, trihexylaluminum, and trioctylaluminum; tri-branched chain alkylaluminums such as triisopropylaluminum, triisobutylaluminum, tri-sec-butylaluminum, tri-t-butylaluminum, tri-2-methylbutylaluminum, tri-3-methylhexylaluminum, and tri-2-ethylhexylaluminum; tricycloalkylaluminums such as tricyclohexylaluminum and tricyclooctylaluminum; triarylaluminums such as triphenylaluminum and tritolylaluminum; dialkylaluminum hydrides such as diisopropylaluminum hydride and diisobutylaluminum hydride; General formula (i-C4H9) x Al y (C5H 10 ) z (wherein x, y, and z are positive numbers, and z ≦ 2x.) such as isoprenylaluminum represented by the formula; alkenylaluminums; alkylaluminum alkoxides such as isobutylaluminum methoxide and isobutylaluminum ethoxide; dialkylaluminum alkoxides such as dimethylaluminum methoxide, diethylaluminum ethoxide, and dibutylaluminum butoxide; alkylaluminum sesquialkoxides such as ethylaluminum sesquiethoxide and butylaluminum sesquibutoxide; General formula R a 2.5 Al(ORb ) 0.5 Partially alkoxylated alkylaluminum having an average composition represented by the formula: Alkylaluminum aryloxides such as diethylaluminum phenoxide and diethylaluminum (2,6-di-t-butyl-4-methylphenoxide); Dialkylaluminum halides such as dimethylaluminum chloride, diethylaluminum chloride, dibutylaluminum chloride, diethylaluminum bromide, and diisobutylaluminum chloride; Alkyl aluminum sesquihalides such as ethyl aluminum sesquichloride, butyl aluminum sesquichloride, and ethyl aluminum sesquibromide; partially halogenated alkylaluminums, such as alkylaluminum dihalides, such as ethylaluminum dichloride; Dialkylaluminum hydrides such as diethylaluminum hydride and dibutylaluminum hydride; Other partially hydrogenated alkylaluminums, such as alkylaluminum dihydrides, such as ethylaluminum dihydride, propylaluminum dihydride, etc.; Examples of the aluminum compounds include partially alkoxylated and halogenated alkylaluminum compounds such as ethylaluminum ethoxy chloride, butylaluminum butoxy chloride, and ethylaluminum ethoxy bromide.
[0087] M 2 AlR a 4. [VIII] (In formula [VIII], M 2 indicates Li, Na or K, and R a represents a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms.) and aluminum alkyl complexes of metals in Group 1 of the Periodic Table. Examples of such compounds include LiAl(C2H5)4, LiAl(C7H 15 ) 4 can be given as an example.
[0088] Compounds similar to the compound represented by the above general formula [VII] can also be used, such as organoaluminum compounds in which two or more aluminum compounds are bonded via nitrogen atoms, such as (C2H5)2AlN(C2H5)Al(C2H5)2.
[0089] As the (b-3) organoaluminum compound, trimethylaluminum and triisobutylaluminum are preferably used from the viewpoint of easy availability. -Production of ethylene-α-olefin copolymer (A) The ethylene / α-olefin copolymer (A) used in the present invention can be suitably produced by copolymerizing ethylene with at least one α-olefin having 3 to 20 carbon atoms in the presence of the above-mentioned olefin polymerization catalyst. The copolymerization can be carried out, for example, by solution polymerization in the presence of a solvent. The polymerization temperature is not particularly limited, but can be, for example, 80° C. or higher, preferably 90° C. or higher. When the copolymerization reaction is carried out at such a temperature, the MFR of the obtained ethylene / α-olefin copolymer (A) is 10 / MFR 2.16 This is preferable because it is possible to increase the vinyl group content.
[0090] In the polymerization, the method of using each component and the order of addition may be selected arbitrarily. For example, the catalyst component [A] and the catalyst component [B] may be added to the polymerization vessel in any order. In the above process, two or more of each catalyst component may be pre-contacted.
[0091] When the ethylene-α-olefin copolymer (A) used in the present invention is produced by copolymerizing ethylene with at least one α-olefin having 3 to 20 carbon atoms using the above-mentioned olefin polymerization catalyst, the catalyst component [A] is usually used in an amount of 10 -9 ~10 -1 Molar, preferably 10 -8 ~10 -2It is used in molar amounts.
[0092] Component (b-1) is used in an amount such that the molar ratio [(b-1) / (M)] of component (b-1) to the total transition metal atoms (M) in component [A] is usually 1 to 10,000, preferably 10 to 5,000. Component (b-2) is used in an amount such that the molar ratio [(b-2) / (M)] of component (b-2) to the total transition metal atoms (M) in component [A] is usually 0.5 to 50, preferably 1 to 20. Component (b-3) is used in an amount such that the amount is usually 0 to 5 mmol, preferably about 0 to 2 mmol, per liter of polymerization volume.
[0093] Here, the molar ratio of ethylene to an α-olefin having 3 to 20 carbon atoms may be appropriately selected depending on the properties of the desired ethylene-α-olefin copolymer (A) and is not particularly limited. Generally, the molar ratio of ethylene:α-olefin is 10:90 to 99.9:0.1, preferably ethylene:α-olefin is 30:70 to 99.9:0.1, and more preferably ethylene:α-olefin is 50:50 to 95.0:5.0.
[0094] Examples of the α-olefin having 3 to 20 carbon atoms include linear or branched α-olefins, such as propylene, 1-butene, 2-butene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3-methyl-1-pentene, 1-octene, 1-decene, and 1-dodecene. Among these α-olefins, 1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene are particularly preferably used. In the present invention, among these, α-olefins having 3 to 10 carbon atoms are more preferably used.
[0095] "Solution polymerization" preferably used for producing the ethylene-α-olefin copolymer (A) is a general term for a method in which polymerization is carried out in a state where the polymer is dissolved in a hydrocarbon solvent inert to the copolymerization reaction. The polymerization temperature in the solution polymerization according to the present invention can usually be in the range of about 0 to 200°C, but is preferably 140°C or higher, and more preferably 150°C or higher.
[0096] In the solution polymerization of the present invention, if the polymerization temperature is less than 0°C, the polymerization activity drops drastically, making it impractical in terms of productivity, and the vinyl group content of the ethylene-α-olefin copolymer (A) may also drop. In addition, in the polymerization temperature range of 0°C or higher, as the temperature increases, the solution viscosity during polymerization drops, the heat of polymerization is easily removed, and the vinyl group content of the ethylene-α-olefin copolymer (A) increases. However, if the polymerization temperature exceeds 200°C, the polymerization activity may also drop drastically. The ethylene-α-olefin copolymer (A) used in the present invention has a relatively high MFR 10 / MFR 2.16 Since the vinyl group content is relatively high, it is preferable to carry out the copolymerization at a relatively high temperature of 80° C. or higher, preferably 90° C. or higher.
[0097] The polymerization pressure is usually normal pressure to 10 MPa gauge pressure, preferably normal pressure to 8 MPa gauge pressure, and the copolymerization can be carried out by any of batch, semi-continuous, and continuous methods. The reaction time (average residence time when the copolymerization reaction is carried out by a continuous method) varies depending on conditions such as catalyst concentration and polymerization temperature and can be appropriately selected, but is usually 1 minute to 3 hours, preferably 10 minutes to 2.5 hours. It is also possible to carry out the polymerization in two or more stages with different reaction conditions. The molecular weight of the obtained ethylene-α-olefin copolymer (A) can be adjusted by changing the hydrogen concentration in the polymerization system or the polymerization temperature. It can also be adjusted by the amount of the catalyst component [B] used. When hydrogen is added to the polymerization system, the amount is suitably about 0.001 to 5,000 NL per kg of the ethylene copolymer produced. The amount of vinyl groups in the obtained ethylene-α-olefin copolymer (A) can be increased by increasing the polymerization temperature and minimizing the amount of hydrogen added. The MFR of the obtained ethylene-α-olefin copolymer (A) can be adjusted by changing the polymerization temperature and the amount of hydrogen added as much as possible. 10 / MFR 2.16is an index that indicates that the larger the value, the more the long-chain branched structure is contained, but in the case of coordination polymerization such as in the examples described later, it is believed that the long-chain branched structure in the ethylene-α-olefin copolymer (A) is formed by the reinsertion of molecular chains (macromonomers) with terminal vinyl groups generated by β-hydrogen elimination reactions. Therefore, the MFR of the ethylene-α-olefin copolymer (A) can be adjusted by increasing or decreasing the ratio of the macromonomer concentration to the ethylene concentration in the solution ([macromonomer] / [ethylene]). 10 / MFR 2.16 The value of can be controlled. In general, when the [macromonomer] / [ethylene] ratio is high, the amount of long chain branches in the ethylene polymer increases, and when the [macromonomer] / [ethylene] ratio is low, the amount of long chain branches in the ethylene polymer decreases. Specific methods for increasing or decreasing the [macromonomer] / [ethylene] ratio in the solution include the following methods [1] to [4].
[0098] [1] Polymerization temperature The higher the polymerization temperature, the easier the β-hydrogen elimination reaction occurs. Therefore, by increasing the polymerization temperature, the ratio of [macromonomer] / [ethylene] increases, and the amount of long chain branches in the ethylene copolymer increases.
[0099] [2] Polymer concentration If the polymer concentration in the solution is increased, the macromonomer concentration also increases relatively, so that the ratio [macromonomer] / [ethylene] increases and the amount of long chain branches in the ethylene copolymer increases.
[0100] [3] Ethylene conversion rate When the ethylene conversion rate is increased, the ethylene concentration in the solution decreases, so that the ratio [macromonomer] / [ethylene] increases and the amount of long chain branches in the ethylene copolymer increases.
[0101] [4] Solvent type When a polymerization solvent with a low boiling point is used, the ethylene concentration in the solution decreases, so that the ratio [macromonomer] / [ethylene] increases and the amount of long chain branches in the ethylene copolymer increases.
[0102] In addition, by controlling the chain transfer reaction to Al in addition to controlling the β-hydrogen elimination reaction, it is possible to increase or decrease the ratio (macromonomer / ethylene) and change the amount of long chain branches in the ethylene polymer.
[0103] The solvent used in the solution polymerization is usually an inert hydrocarbon solvent, preferably a saturated hydrocarbon having a boiling point of 50°C to 200°C under normal pressure. Specifically, aliphatic hydrocarbons such as pentane, hexane, heptane, octane, decane, dodecane, and kerosene; alicyclic hydrocarbons such as cyclopentane, cyclohexane, and methylcyclopentane can be mentioned. Aromatic hydrocarbons such as benzene, toluene, and xylene, and halogenated hydrocarbons such as ethylene chloride, chlorobenzene, and dichloromethane also fall within the category of "inert hydrocarbon solvents" related to the high-temperature solution polymerization of the present invention, and the use thereof is not limited thereto. As described above, in the high-temperature solution polymerization according to the present invention, not only the organic aluminum oxy compounds that dissolve in aromatic hydrocarbons, which have been frequently used in the past, but also modified methylaluminoxanes such as MMAO that dissolve in aliphatic and alicyclic hydrocarbons can be used. As a result, by adopting aliphatic and alicyclic hydrocarbons as the solvent for solution polymerization, it is possible to almost completely eliminate the possibility of aromatic hydrocarbons being mixed into the polymerization system or the ethylene-based polymer produced. In other words, the high-temperature solution polymerization method according to the present invention has the advantage of being able to reduce the environmental load and minimize the impact on human health.
[0104] In order to suppress variations in physical properties, the ethylene-α-olefin copolymer (A) obtained by the polymerization reaction and other components added as desired are preferably melted by any method and then kneaded, granulated, or the like.
[0105] <Ethylene-polar monomer copolymer (B)> The foam of the present invention may contain an ethylene-polar monomer copolymer (B) in addition to the ethylene-α-olefin copolymer (A). In this case, the foam of the present invention is formed from a composition containing the ethylene-α-olefin copolymer (A) and the ethylene-polar monomer copolymer (B).
[0106] Examples of the polar monomer of the ethylene-polar monomer copolymer (B) include unsaturated carboxylic acids, their salts, their esters, their amides, vinyl esters, carbon monoxide, etc. More specifically, examples include unsaturated carboxylic acids such as acrylic acid, methacrylic acid, fumaric acid, itaconic acid, monomethyl maleate, monoethyl maleate, maleic anhydride, itaconic anhydride, etc., salts of these unsaturated carboxylic acids with monovalent metals such as lithium, sodium, potassium, etc., and salts of polyvalent metals such as magnesium, calcium, zinc, etc., unsaturated carboxylic acid esters such as methyl acrylate, ethyl acrylate, isopropyl acrylate, isobutyl acrylate, n-butyl acrylate, isooctyl acrylate, methyl methacrylate, ethyl methacrylate, isobutyl methacrylate, dimethyl maleate, etc., vinyl esters such as vinyl acetate and vinyl propionate, carbon monoxide, sulfur dioxide, etc., which may be one or more of these.
[0107] More specifically, representative examples of the ethylene-polar monomer copolymer (B) include ethylene-unsaturated carboxylic acid copolymers such as ethylene-acrylic acid copolymers and ethylene-methacrylic acid copolymers, ionomers in which the carboxyl groups of the ethylene-unsaturated carboxylic acid copolymers have been partially or entirely neutralized with the above-mentioned metals, ethylene-unsaturated carboxylic acid ester copolymers such as ethylene-methyl acrylate copolymers, ethylene-ethyl acrylate copolymers, ethylene-methyl methacrylate copolymers, ethylene-isobutyl acrylate copolymers and ethylene-n-butyl acrylate copolymers, ethylene-unsaturated carboxylic acid ester-unsaturated carboxylic acid copolymers such as ethylene-isobutyl acrylate-methacrylic acid copolymers and ethylene-n-butyl acrylate-methacrylic acid copolymers, and ionomers in which the carboxyl groups of the ethylene-unsaturated carboxylic acid ester-unsaturated carboxylic acid copolymers have been partially or entirely neutralized with the above-mentioned metals, and ethylene-vinyl ester copolymers such as ethylene-vinyl acetate copolymer.
[0108] Among these, copolymers of ethylene with a polar monomer selected from the group consisting of unsaturated carboxylic acids, their salts, and their esters, and vinyl acetate are particularly preferred, and ethylene-(meth)acrylic acid copolymers or ionomers thereof, ethylene-(meth)acrylic acid-(meth)acrylic acid ester copolymers or ionomers thereof, and ethylene-vinyl acetate copolymers are particularly preferred, with ethylene-vinyl acetate copolymers being most preferred.
[0109] The ethylene and polar monomer constituting the ethylene-polar monomer copolymer (B) may be, for example, a monomer derived from a fossil fuel or a monomer derived from biomass, and these monomers may be used alone or in combination of two or more kinds.
[0110] The ethylene-polar monomer copolymer (B) preferably has a polar monomer content of usually 1 to 50 mass%, particularly 5 to 45 mass%, although this varies depending on the type of polar monomer. In addition, in consideration of moldability, mechanical strength, etc., the ethylene-polar monomer copolymer preferably has an MFR 2.16It is preferable to use one with a viscosity of 0.05 to 500 g / 10 min, and particularly 0.1 to 100 g / 10 min. Copolymers of ethylene and unsaturated carboxylic acids, unsaturated carboxylic acid esters, vinyl esters, etc. can be obtained by radical copolymerization under high temperature and high pressure. Copolymers of ethylene and metal salts of unsaturated carboxylic acids (ionomers) can be obtained by reacting ethylene-unsaturated carboxylic acid copolymers with the corresponding metal compounds.
[0111] In the present invention, when the ethylene-polar monomer copolymer (B) is an ethylene-vinyl acetate copolymer, the vinyl acetate content in the ethylene-vinyl acetate copolymer is usually 10 to 30% by mass, preferably 15 to 30% by mass, and more preferably 15 to 25% by mass. In addition, the ethylene-vinyl acetate copolymer has an MFR 2.16 is preferably 0.1 g / 10 min or more, more preferably 0.3 g / 10 min or more, even more preferably 0.5 g / 10 min or more, and is preferably 50 g / 10 min or less, more preferably 20 g / 10 min or less, even more preferably 5 g / 10 min or less.
[0112] In the foam of the present invention, the ethylene-polar monomer copolymer (B) is an optional component, but when the foam of the present invention contains the ethylene-polar monomer copolymer (B), when the foam is made into a laminate, the obtained foam layer tends to have excellent adhesion to other layers made of polyurethane, rubber, leather, etc. Therefore, the foam of the present invention can be preferably used as a layer constituting a laminate.
[0113] When the foam of the present invention is formed from a composition containing ethylene-α-olefin copolymer (A) and ethylene-polar monomer copolymer (B), the composition contains the above-mentioned ethylene-α-olefin copolymer (A) and ethylene-polar monomer copolymer (B) in a ratio of 100 to 20 parts by mass of (A) and 0 to 80 parts by mass of (B), and it is one of the preferred embodiments that (A) is 100 parts by mass and (B) is 0 parts by mass. When (B) is contained, it is preferable that (A) is 99 to 20 parts by mass and (B) is 1 to 80 parts by mass (here, the total of (A) and (B) is 100 parts by mass). That is, in the composition containing ethylene-α-olefin copolymer (A) and ethylene-polar monomer copolymer (B), the mass ratio ((A) / (B)) of the ethylene-α-olefin copolymer (A) to the ethylene-polar monomer copolymer (B) is 100 / 0 to 20 / 80, and it is one of the preferred embodiments that it is 100 / 0. When (B) is contained, the ratio is preferably in the range of 99 / 1 to 20 / 80, more preferably 80 / 20 to 40 / 60.
[0114] <Other polymer components> When the foam of the present invention is formed from a composition containing the ethylene-α-olefin copolymer (A) and the ethylene-polar monomer copolymer (B), the composition may contain other polymer components (hereinafter referred to as "other polymer components") that do not fall under either the ethylene-α-olefin copolymer (A) or the ethylene-polar monomer copolymer (B) as necessary. The other polymer components are not particularly limited, but may include, for example, ethylene-α-olefin-non-conjugated polyene copolymers. When the composition of the present invention contains polymer components other than the ethylene-α-olefin copolymer (A) and the ethylene-polar monomer copolymer (B), the content thereof is usually 30 parts by mass or less, preferably about 1 to 20 parts by mass, based on 100 parts by mass of the total of (A) and (B).
[0115] In this specification, the ethylene-α-olefin copolymer (A), the optional ethylene-polar monomer copolymer (B), and the optional other polymer components may be collectively referred to as the "polymer components".
[0116] <Crosslinking agent (C)> The foam of the present invention may be composed only of a polymer component such as the ethylene-α-olefin copolymer (A), but in a typical embodiment, the foam of the present invention is formed from a composition containing a polymer component such as the ethylene-α-olefin copolymer (A) and a crosslinking agent (C).
[0117] As the crosslinking agent (C), any radical generator that acts as a crosslinking agent can be used without any particular limitation. When the polymer used to form the crosslinked body of the present invention contains a crosslinking agent (C), the content thereof is generally within the range of 0.1 to 1.5 parts by mass, preferably 0.2 to 1.0 parts by mass, and more preferably 0.2 to 0.7 parts by mass, per 100 parts by mass of the total of the ethylene-α-olefin copolymer (A), the optional ethylene-polar monomer copolymer (B), and the optional other polymer components (i.e., 100 parts by mass of all polymer components). By using a composition containing the crosslinking agent (C) in such an amount, a foam having an appropriate crosslinked structure can be produced.
[0118] As the crosslinking agent (C), an organic peroxide is preferably used. Specifically, Dicumyl peroxide (DCP), di-t-butyl peroxide, 2,5-dimethyl-2,5-di-(t-butylperoxy)hexane, 2,5-Dimethyl-2,5-di-(t-butylperoxy)hexyne-3, 1,3-bis(t-butylperoxyisopropyl)benzene, 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane, n-butyl-4,4-bis(t-butylperoxy)valerate, Benzoyl peroxide, p-Chlorobenzoyl peroxide, 2,4-dichlorobenzoyl peroxide, t-butyl peroxybenzoate, t-butyl perbenzoate, t-Butyl peroxy isopropyl carbonate, Diacetyl peroxide, Lauroyl peroxide, and organic peroxides such as t-butylcumyl peroxide. Of these, dicumyl peroxide (DCP) is preferred.
[0119] When the composition according to the present invention contains a crosslinking agent (C), it is also preferable to contain a crosslinking assistant, if necessary, together with the crosslinking agent (C). Examples of the crosslinking assistant include peroxy crosslinking assistants such as sulfur, p-quinone dioxime, p,p'-dibenzoylquinone dioxime, N-methyl-N-4-dinitrosoaniline, nitrosobenzene, diphenyl guanidine, and trimethylolpropane-N,N'-m-phenylenedimaleimide; or divinylbenzene, triallyl cyanurate (TAC), and triallyl isocyanurate (TAIC).
[0120] Examples of the crosslinking aid include polyfunctional methacrylate monomers such as ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, and allyl methacrylate; polyfunctional vinyl monomers such as vinyl butyrate and vinyl stearate. Among these, triallyl cyanurate (TAC) and triallyl isocyanurate (TAIC) are preferred.
[0121] In the composition according to the present invention, it is desirable to use such a crosslinking aid in an amount such that the mass ratio of the crosslinking aid to the crosslinking agent (C) [crosslinking aid / crosslinking agent (C)] is 1 / 30 to 5 / 1, preferably 1 / 20 to 3 / 1, more preferably 1 / 15 to 2 / 1, and particularly preferably 1 / 10 to 1 / 1.
[0122] <Physical foaming agent (D)> The foam of the present invention may be composed only of a polymer component such as the ethylene-α-olefin copolymer (A). The foam of the present invention is usually obtained by foaming a polymer component such as the ethylene-α-olefin copolymer (A), and this foaming is often carried out using a foaming agent. Therefore, the polymer component such as the ethylene-α-olefin copolymer (A) that gives the foam of the present invention is often used in the form of a composition containing the polymer component such as the ethylene-α-olefin copolymer (A) and a foaming agent. This composition may further contain the crosslinking agent (C), or may further contain the crosslinking coagent in addition to the crosslinking agent (C).
[0123] In the present invention, a physical foaming agent (D) can be used as the foaming agent. The physical foaming agent (D) is a substance that generates bubbles in a polymer component such as the ethylene-α-olefin copolymer (A) by utilizing the change in solubility in the polymer component depending on temperature and / or pressure, and does not necessarily involve a chemical reaction during foaming.
[0124] Examples of the physical blowing agent (D) include organic physical blowing agents such as various aliphatic hydrocarbons such as methanol, ethanol, propane, butane, pentane, hexane, etc., various chlorinated hydrocarbons such as dichloroethane, dichloromethane, carbon tetrachloride, etc., various fluorochlorohydrocarbons such as chlorofluorocarbons, etc., and further inorganic physical blowing agents such as air, carbon dioxide, nitrogen, argon, water, etc. Among these, carbon dioxide, nitrogen, and argon are excellent because they do not need to be converted into steam, are inexpensive, and have very little possibility of environmental pollution and ignition, and among these, carbon dioxide is particularly excellent.
[0125] The physical foaming agent (D) can be used in the form of a gas in many cases. However, the physical foaming agent (D) may be used in the form of a supercritical fluid in order to sufficiently increase the solubility in polymer components such as the ethylene-α-olefin copolymer (A). Carbon dioxide has a critical pressure of 7.38 MPa and a critical temperature of 31.1°C, and can be relatively easily converted into a supercritical fluid.
[0126] In the present invention, since the physical foaming agent (D) is used as the foaming agent, there is no decomposition residue of the foaming agent in the obtained foam. Therefore, it is possible to prevent mold staining during crosslinking and foaming of the composition. Moreover, since the physical foaming agent is not powdery, it has excellent kneadability. In addition, the use of this physical foaming agent can prevent the obtained foam from having an unpleasant odor (for example, the ammonia odor generated during the decomposition of azodicarbonamide (ADCA)).
[0127] As a method of storing the physical blowing agent (D), in the case of small-scale production, carbon dioxide, nitrogen, etc., can be used in a cylinder and supplied to the injection molding machine, extrusion molding machine, etc. through a pressure reducing valve, or the pressure can be increased by a pump or the like and supplied to the injection molding machine, extrusion molding machine, etc.
[0128] In addition, in the case of a facility for manufacturing foamed products on a large scale, storage tanks for liquefied carbon dioxide, liquefied nitrogen, etc. are installed, and the liquefied carbon dioxide, liquefied nitrogen, etc. are vaporized through a heat exchanger and supplied to an injection molding machine, extrusion molding machine, etc. through piping and a pressure reducing valve.
[0129] When a liquid physical blowing agent is used as the physical blowing agent (D), the storage pressure is preferably in the range of 0.13 to 100 MPa. When a physical foaming agent (D) is used, the amount of the physical foaming agent (D) added is appropriately determined depending on the desired expansion ratio, and is usually 0.1 to 15 parts by mass, and preferably 0.5 to 10 parts by mass, per 100 parts by mass of the total of the ethylene-α-olefin copolymer (A), the optional ethylene-polar monomer copolymer (B), and the optional other polymer components.
[0130] On the other hand, in relation to the physical foaming agent (D), in the prior art, a chemical foaming agent (D') is often used as a foaming agent when producing plastic foams. This chemical foaming agent (D') is a chemical substance that generates gas by thermal decomposition or other chemical reactions. Specific examples of the chemical foaming agent (D') include: Azodicarbonamide (ADCA), 1,1'-azobis(1-acetoxy-1-phenylethane), Dimethyl-2,2'-azobisbutyrate, Dimethyl-2,2'-azobisisobutyrate, 2,2'-azobis(2,4,4-trimethylpentane), 1,1'-azobis(cyclohexane-1-carbonitrile), Azo compounds such as 2,2'-azobis[N-(2-carboxyethyl)-2-methyl-propionamidine]; Nitroso compounds such as N,N'-dinitrosopentamethylenetetramine (DPT); 4,4'-oxybis(benzenesulfonylhydrazide), Hydrazine derivatives such as diphenylsulfone-3,3'-disulfonylhydrazide; Semicarbazide compounds such as p-toluenesulfonylsemicarbazide; Organic thermal decomposition type blowing agents such as trihydrazinotriazine, Bicarbonates such as sodium hydrogen carbonate and ammonium hydrogen carbonate, carbonates such as sodium carbonate and ammonium carbonate; Nitrites such as ammonium nitrite, Examples of inorganic thermal decomposition type blowing agents include hydrogen compounds. Among these, azodicarbonamide (ADCA) tends to be used frequently because of the large amount of gas that is generated during thermal decomposition.
[0131] In addition, when a chemical foaming agent (D') is used as a foaming agent, a foaming assistant may be used in combination with the chemical foaming agent (D'). The foaming assistant acts to lower the decomposition temperature of the chemical foaming agent (D'), promote decomposition, and make bubbles uniform. Examples of such foaming assistants include zinc oxide (ZnO), zinc stearate, organic acids such as salicylic acid, phthalic acid, stearic acid, and oxalic acid, urea, or derivatives thereof, and the like.
[0132] However, when a foam is produced using azodicarbonamide (ADCA) or the like as a foaming agent, the resulting foam may have an odor (unpleasant odor) derived from the foaming agent, such as the odor of ammonia generated during decomposition of ADCA, and the presence of such an odor (unpleasant odor) is undesirable for using the foam as footwear and footwear parts. In addition, when ADCA or the like is used as a foaming agent, problems such as discoloration may occur in the resulting foam, and such discoloration is undesirable from the viewpoint of aesthetics, etc. Therefore, in the present invention, a chemical foaming agent (D') is not usually used.
[0133] <Other ingredients> The foam of the present invention may contain optional components other than the above-mentioned components, such as various additives such as fillers, heat stabilizers, weather stabilizers, flame retardants, hydrochloric acid absorbents, and pigments, as necessary. Examples of various additives include those known as additives that can be added to general olefin resins. These may be included in the foam of the present invention as long as they do not impair the object of the present invention.
[0134] [Method of manufacturing foam] The foam of the present invention can be produced by using the ethylene-α-olefin copolymer (A) together with, for example, the optional components such as the ethylene-polar monomer copolymer (B), the other polymer components, the crosslinking agent (C), the crosslinking aid, the physical foaming agent (D), and the other components (hereinafter, the olefin polymer and these optional components may be collectively referred to as "a component containing the ethylene-α-olefin copolymer (A)"), for example, by a method such as the following, but is not limited to these methods.
[0135] The ethylene-α-olefin copolymer (A) or the composition containing the ethylene-α-olefin copolymer (A) used in the present invention is in an uncrosslinked and unfoamed state. In the step (S1), molding is performed using the uncrosslinked and unfoamed ethylene-α-olefin copolymer (A) or the composition containing the ethylene-α-olefin copolymer (A).
[0136] Morphology of ethylene-α-olefin copolymer (A) etc. The ethylene / α-olefin copolymer (A) or a composition containing the ethylene / α-olefin copolymer (A) may be in a state as it is, or in a molten state. Alternatively, the ethylene / α-olefin copolymer (A) or a composition containing the ethylene / α-olefin copolymer (A) may be in the form of pellets or a sheet obtained by once melting and plasticizing the ethylene / α-olefin copolymer (A) or the composition containing the ethylene / α-olefin copolymer (A) and then cooling and solidifying it.
[0137] The pellets of the "component containing ethylene-α-olefin copolymer (A)" can be prepared, for example, by mixing the ethylene-α-olefin copolymer (A) and, if necessary, the ethylene-polar monomer copolymer (B), the other polymer components, the crosslinking agent (C), the crosslinking aid, and the physical foaming agent (D) in the above-mentioned ratios in a Henschel mixer or the like, melting and plasticizing the mixture in a kneader such as a Banbury mixer, a roll (a roll mill such as a two-roll mill or a three-roll mill), or an extruder at a temperature at which the crosslinking agent (C) does not decompose, uniformly mixing and dispersing the mixture, and then using a granulator. As a method for crosslinking and foaming, for example, crosslinking by heat treatment and ionizing radiation crosslinking can be mentioned as described later. In the case of crosslinking by heat treatment, it is preferable that the composition contains the crosslinking agent (C) and the crosslinking aid. In the case of crosslinking by ionizing radiation, a crosslinking aid may be added.
[0138] In addition to the ethylene / α-olefin copolymer (A), the above-mentioned other components may be used as necessary within the scope of not impairing the object of the present invention. The sheet of the "component containing ethylene-α-olefin copolymer (A)" can be prepared, for example, from the pellets obtained as described above using an extruder or a calendar molding machine. Alternatively, the ethylene-α-olefin copolymer (A) or the composition containing the ethylene-α-olefin copolymer (A) can be kneaded in a kneader such as a roll mill at a temperature at which the crosslinking agent (C) does not decompose, and molded into a sheet. When the kneading is carried out using a roll mill, the ethylene-α-olefin copolymer (A) or the composition containing the ethylene-α-olefin copolymer (A) after kneading can be in the form of a sheet. The sheet of the "component containing ethylene-α-olefin copolymer (A)" can also be obtained by kneading the various components containing the ethylene-α-olefin copolymer (A) with a Brabender or the like, and then molding them into a sheet with a calendar roll, forming them into a sheet with a press molding machine, or kneading them using an extruder and then forming them into a sheet through a T-die or annular die.
[0139] By these methods, an uncrosslinked and unfoamed expandable sheet can be prepared. <Preparation of foam> The foam of the present invention can be prepared by any method, for example, as follows, although there is no particular limitation on the method for producing the foam.
[0140] The foam of the present invention can be obtained, for example, by a production method including a step of physically foaming the ethylene-α-olefin copolymer (A) or a composition containing the ethylene-α-olefin copolymer (A). Here, the composition containing the ethylene-α-olefin copolymer (A) often contains the crosslinking agent (C). The physically foaming step may be performed by first impregnating the ethylene-α-olefin copolymer (A) or a composition containing the ethylene-α-olefin copolymer (A) in a gaseous physical foaming agent under pressure, and then releasing the pressure. The physically foaming step may also be performed by impregnating the ethylene-α-olefin copolymer (A) or a composition containing the ethylene-α-olefin copolymer (A) in a supercritical fluid.
[0141] The production method typically includes: a step (S1) of molding the ethylene-α-olefin copolymer (A) or a composition containing the ethylene-α-olefin copolymer (A); A step (S2) of crosslinking the precursor molded body obtained by the molding; and A step (S3) of physically foaming the crosslinked body obtained by the crosslinking. Includes.
[0142] Here, the composition containing the ethylene-α-olefin copolymer (A) often contains the crosslinking agent (C). The step (S2) may be carried out after the step (S1) or simultaneously with the step (S1).
[0143] In the step (S1), the ethylene-α-olefin copolymer (A) or a composition containing the ethylene-α-olefin copolymer (A) is molded by a suitable molding method to obtain a precursor molded body. The ethylene-α-olefin copolymer (A) or a composition containing the ethylene-α-olefin copolymer (A) used here may be in the form of pellets or sheets as described above.
[0144] For example, when a sheet-like molded product is obtained as the precursor molded product, a sheet containing the ethylene-α-olefin copolymer (A) can be obtained using a calendar molding machine, a press molding machine, or a T-die extruder. Preferably, a sheet of the ethylene-based polymer composition can be obtained using a calendar molding machine, a press molding machine, or a T-die extruder. In forming the sheet, it is preferable to perform the sheet molding at a temperature lower than the decomposition temperature of the crosslinking agent (C), and specifically, it is preferable to perform the sheet molding under conditions set so that the temperature of the component containing the ethylene-α-olefin copolymer (A) in a molten state is, for example, 100 to 130°C.
[0145] The precursor molded body may also be obtained by other molding methods such as injection molding, for example, by injecting the ethylene / α-olefin copolymer (A) or a composition containing the ethylene / α-olefin copolymer (A) into a mold at a temperature lower than the decomposition temperature of the crosslinking agent (C).
[0146] In the step (S2), the precursor molded body is crosslinked to produce a corresponding crosslinked body. This crosslinking is usually carried out in the presence of the crosslinking agent (C) at a temperature equal to or higher than the decomposition temperature of the crosslinking agent (C), for example, at 130 to 200°C. When the sheet molding is carried out using a press molding machine, the components containing the ethylene-α-olefin copolymer (A) are heated in the press molding machine at a temperature equal to or higher than the decomposition temperature of the crosslinking agent (C), whereby the steps (S1) and (S2) can be carried out in a single step.
[0147] In the step (S3), the crosslinked body obtained in the step (S2) is physically foamed using a physical foaming agent. This leads to the crosslinked body being transformed into a foam. The physical foaming agent used here can be the above-mentioned physical foaming agent (D).
[0148] The step (S3) may be performed by first impregnating the ethylene-α-olefin copolymer (A) or a composition containing the ethylene-α-olefin copolymer (A) in a gaseous physical blowing agent under pressure and then releasing the pressure, or by impregnating the ethylene-α-olefin copolymer (A) or a composition containing the ethylene-α-olefin copolymer (A) in a supercritical fluid.
[0149] The conditions for physical foaming, such as temperature and pressure, are not particularly limited as long as the object of the present invention can be achieved, and can be appropriately set depending on the properties and applications of the foam to be obtained. When step (S3) is carried out in a supercritical fluid, it is carried out at a temperature equal to or higher than the critical temperature of the physical foaming agent (D) and at a pressure equal to or higher than the critical pressure of the physical foaming agent (D).
[0150] For example, when carbon dioxide is used as the physical foaming agent (D), the temperature at which step (S3) is performed can be, for example, 40 to 200°C, and the pressure can be, for example, 2 to 50 MPa. Carbon dioxide has a critical pressure of 7.38 MPa and a critical temperature of 31.1°C, and is relatively easy to convert into a supercritical fluid. Therefore, when carbon dioxide is used as the supercritical fluid, the temperature at which step (S3) is performed can be, for example, 40 to 200°C, and the pressure can be, for example, 7.4 to 50 MPa.
[0151] Step (S3) can be carried out in a pressure-resistant and heat-resistant reaction apparatus such as an autoclave. Examples of the foam product shape include a sheet, a thick board, a net, a molded product, and the like.
[0152] The foam obtained as described above may be used as it is as a primary foam, or the foam may be compressed to give a desired shape to produce a secondary foam. Examples of compression molding conditions are a mold temperature of 130 to 200°C and a mold clamping pressure of 30 to 300 kgf / cm. 2, the compression time is in the range of 5 to 60 minutes, and the compression ratio is in the range of 1.1 to 3.0.
[0153] Among the above-mentioned production methods, it is preferable to obtain a foam by heat treating the component containing the olefin polymer (preferably an ethylene polymer composition). Another foam of the present invention, which is obtained by foaming the ethylene polymer composition, preferably has a specific gravity of 0.03 to 0.30. This foam of another embodiment is also preferably used for laminates, footwear, or footwear parts described below.
[0154] [Laminate] The laminate of the present invention is a laminate having a layer made of the foam of the present invention described above and a layer made of at least one material selected from the group consisting of polyolefins, polyurethanes, rubber, leather and artificial leather.
[0155] The polyolefin, polyurethane, rubber, leather and artificial leather are not particularly limited, and conventionally known polyolefin, polyurethane, rubber, leather and artificial leather can be used. Such a laminate is particularly suitable for use in footwear or footwear parts.
[0156] [Footwear and footwear parts] The footwear and footwear parts of the present invention are both made using the foam or laminate of the present invention. That is, it can be said that the footwear and footwear parts of the present invention both include the foam or laminate of the present invention. Examples of footwear parts include shoe soles, shoe midsoles, innersoles, soles, sandals, etc.
[0157] The footwear or footwear part of the present invention uses the foam or laminate of the present invention, and therefore is lightweight and can be prevented from deforming due to long-term use. EXAMPLES
[0158] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring various physical properties described in the examples are as follows.
[0159] [Evaluation of copolymer properties] 1-Butene Content The 1-butene content of ethylene-1-butene copolymer is as follows: 13 C-NMR measurements were performed, and the values were calculated by analyzing the obtained spectra.
[0160] Equipment: Bruker Biospin AVANCE III cryo-500 nuclear magnetic resonance spectrometer Measurement nuclei: 13 C(125MHz) Measurement mode: Single pulse proton broadband decoupling Pulse width: 45° (5.00μsec) Number of points: 64k Measurement range: 250 ppm (-55 to 195 ppm) Repeat time: 5.5 seconds Number of times accumulated: 128 times Measurement solvent: orthodichlorobenzene / benzene-d6 (4 / 1 [v / v]) Sample concentration: ca. 60mg / 0.6mL Measurement temperature: 120℃ Window function: exponential (BF: 1.0Hz) Chemical shift reference: δδ signal (29.73 ppm)
[0161] Double bond amount The amount of double bonds in ethylene-α-olefin copolymers is determined by the following method. 1The measurements were carried out by H-NMR (JEOL Ltd., "ECX400P Nuclear Magnetic Resonance Spectrometer"). Here, vinyl double bonds, vinylidene double bonds, di-substituted olefin double bonds, and tri-substituted olefin double bonds are observed as signals derived from double bonds. The amount of double bonds was quantified from the integrated intensity of each signal. The main chain methylene signal of the ethylene-α-olefin copolymer was used as the chemical shift standard (1.2 ppm).
[0162] [ka]
[0163] In each formula, * indicates a bond to an atom other than a hydrogen atom. The peaks of the hydrogen atoms a to e are observed near the following positions. Hydrogen atom a peak: 4.60 ppm Hydrogen atom b peak: 4.85 ppm Hydrogen atom c peak: 5.10 ppm Hydrogen atom d peak: 5.25 ppm Hydrogen atom e peak: 5.70 ppm
[0164] The quantitative formula for the amount of double bonds is as follows: Amount of vinyl double bonds = {(integral intensity of signal b) + (integral intensity of signal e)} / 3 Amount of vinylidene double bonds = (integral intensity of signal a) / 2 Amount of disubstituted olefinic double bonds = (integral intensity of signal d) / 2 Amount of trisubstituted olefinic double bonds = (integral intensity of signal c) From these results, the vinyl group content (amount of vinyl double bonds) per 1000 carbon atoms (1000C) was calculated.
[0165] density d Density d(kg / m 3 ) was determined at 23°C according to ASTM D1505.
[0166] MFR The MFR (melt flow rate, g / 10 min) was determined at 190°C according to ASTM D1238. The measured value under a load of 2.16 kg was used as the MFR 2.16 , the measured value with a 10 kg load is MFR 10 It was decided.
[0167] Molecular weight distribution (Mw / Mn) The chromatographic properties were determined by gel permeation chromatography (GPC) in an orthodichlorobenzene solvent at 140°C. A gel permeation chromatograph Alliance GPC-2000 manufactured by Waters was used, and the measurements were performed as follows. The separation columns were two TSKgel GNH6-HT and two TSKgel GNH6-HTL, each with a diameter of 7.5 mm and a length of 300 mm, the column temperature was 140°C, the mobile phase was o-dichlorobenzene (Wako Pure Chemical Industries) and 0.025 mass% BHT (Takeda Pharmaceuticals) as an antioxidant, and the mobile phase was moved at 1.0 ml / min, the sample concentration was 15 mg / 10 ml, the sample injection amount was 500 μl, and a differential refractometer was used as the detector. The standard polystyrene had molecular weights of Mw<1000 and Mw>4×10 6 For the 1000≦Mw≦4×10 6 The material used was manufactured by Pressure Chemical Company.
[0168] Melting point (Tm) Using a differential scanning calorimeter (SII DSC220), approximately 5.0 mg of the sample was heated from 30°C to 200°C at a heating rate of 10°C / min under a nitrogen atmosphere and held at that temperature for 10 minutes. It was then cooled to 30°C at a heating rate of 10°C / min, held at that temperature for 5 minutes, and then heated to 200°C at a heating rate of 10°C / min. The endothermic peak observed during this second heating was taken as the melting peak, and the temperature at which the melting peak appeared was determined as the melting point (Tm).
[0169] [Evaluation of physical properties of crosslinked foam] specific gravity The specific gravity was measured according to JIS K7222. If the foam is cubic, the sample was taken from 20 mm or more inside each of the four sides of the maximum area plane, and from the surface of the parallel plane with the skin remaining. For example, in the case of a midsole, the sample was prepared from 20 mm or more inside each end, and from both surfaces of the approximately parallel plane with the skin remaining.
[0170] The measurement is the average of five parts of the foam. The difference between the maximum and minimum values of the specific gravity measurements of the five parts, which is a measure of the uniformity of the foam quality, is preferably 0.08 or less, more preferably 0.06 or less. If the difference exceeds 0.08, it means that the molded product quality (hardness, mechanical properties, compression set, etc.) is not uniform.
[0171] Asker C hardness The Asker C hardness was measured in a 23°C environment according to the "Spring hardness test type C test method" described in JIS K7312-1996, Appendix 2.
[0172] Rebound elasticity The impact resilience was measured in accordance with JIS K 6255. Samples were prepared in the same manner as the samples used for the above (2) Compression set (CS), and measurements were performed in an atmosphere of 23°C.
[0173] Interlaminar tear strength The interlaminar tear strength was measured at a test temperature of 23°C using an Intescor 205X test machine. A rectangular sample 25 mm wide and 15 mm thick was set with a chuck distance of 30 mm and peeled in the thickness direction at a test speed of 50 mm / min. The interlaminar tear strength S (N / mm) was calculated using the following formula. S=S0 / S1 S0: Tearing stress (N) S1: Sample width (mm)
[0174] Compression set (CS) Compression set (CS) was measured according to JIS K 6262. The samples were prepared by cutting the foam into a cylindrical shape with a diameter of 30 mm and a thickness of 15 mm or more, and extracting a thickness of 10 mm from each of two parallel flat surfaces of the cylinder while leaving a skin on one side.
[0175] In addition, even when the foam to be sampled was a three-dimensional object of various shapes, it was cut into a cylindrical shape with a diameter of 30 mm and a thickness of 15 mm or more, and a sample was prepared by extracting a sample from the surface of each of the two parallel planes of the cylinder, leaving a skin on one side to make a thickness of 10 mm.
[0176] A cylindrical dumbbell cutter can be used to cut a foam into a cylindrical shape and to cut a foam from the surface of a parallel plane. The sample was compressed by 50% and left at rest in a 50°C environment for 6 hours, and then measured 30 minutes after releasing the compression. The compression set (CS) (%) was calculated using the following formula.
[0177] CS=(t0-t1) / (t0-t2)×100 t0: sample thickness (mm) t1: Thickness (mm) 30 minutes after removing the sample from the compression device t2: Spacer thickness (mm)
[0178] Residual nitrogen The amount of residual nitrogen was quantified by chemiluminescence using a total nitrogen trace analyzer (TN-2100H manufactured by Mitsubishi Chemical Analytech Co., Ltd.) 5 mg of solid foam was used as the sample, and quantification by chemiluminescence was performed based on the chemiluminescence intensity when NO generated by thermal decomposition of the sample reacted with ozone.
[0179] Here, when no chemiluminescence was observed, or when the chemiluminescence intensity was weaker than the detection limit of the trace total nitrogen analyzer, the result was evaluated as "ND" (not detected).
[0180] [Ethylene-α-olefin copolymer (A)] <Ethylene-1-butene copolymer (A-1)> Ethylene-1-butene copolymer (A-1): Ethylene-1-butene copolymer (density 0.885 g / cm 3 The polymer used was Tafmer DF810 (manufactured by Mitsui Chemicals, Inc.), with a MFR of 190°C, 2.16 kg, and a melting point of 66°C.
[0181] <Production of ethylene-1-butene copolymer (A-2)> Copolymerization of ethylene and 1-butene was carried out continuously at a polymerization temperature of 130°C and a polymerization pressure of 2.5MPaG in a 100L stainless steel polymerization vessel equipped with an impeller (agitation speed: 250 rpm). Dehydrated and purified hexane was continuously fed from the side of the vessel at a rate of 39L, ethylene at 9.0kg, 1-butene at 8.3kg per hour, hydrogen at 13NL, di(p-tolyl)methylene(cyclopentadienyl)(octamethyloctahydrodibenzofluorenyl)zirconium dichloride at 0.02mmol, methylaluminoxane at 10.0mmol in terms of aluminum, and triisobutylaluminum at 4mmol per hour. The hexane solution of the ethylene-1-butene copolymer thus produced was continuously discharged through an outlet provided on the side wall of the vessel while adjusting the opening of the liquid level control valve to maintain the amount of solution in the vessel at 30L. The resulting hexane solution of ethylene-1-butene copolymer was introduced into a heater and heated to 180°C. 80 mL of methanol was added every hour as a catalyst deactivator to terminate the polymerization. The solution was then continuously transferred to a degassing process under reduced pressure and dried to obtain ethylene-1-butene copolymer (A-2).
[0182] The resulting ethylene-1-butene copolymer (A-2) had a 1-butene content of 11.2 mol%, a vinyl group content of 0.060 per 1,000 carbon atoms, and an MFR 2.16 0.5g / 10min, MFR 10 4.2 / 10 min, MFR 10 / MFR 2.16 is 8.4, and density d is 0.885g / cm 3, Mw / Mn was 2.0, the melting point was 66°C, and the yield was 17.2 kg per hour.
[0183] [Method of manufacturing physical foam] [Example 1] A mixture consisting of 100 parts by weight of ethylene-1-butene copolymer (A-1), 0.5 parts by weight of talc, and 0.5 parts by weight of dicumyl peroxide (DCP) was kneaded for 3 minutes at a roll surface temperature of 100°C (two-roll mill manufactured by Daejung Co., Ltd.) and then formed into a sheet.
[0184] The obtained sheet was filled into a press mold and subjected to a pressure of 150 kg / cm 2 The crosslinked body was obtained by applying pressure and heating at 170°C for 10 minutes. This press mold had a cavity that was 5 mm thick, 50 mm long, and 50 mm wide when the sheet was press molded, and the crosslinked body obtained also had a thickness of 5 mm, length of 50 mm, and width of 50 mm.
[0185] The obtained crosslinked body was put into an autoclave (PARTICLE foamtec, internal volume 40 L), and then the inside of the autoclave was pressurized with carbon dioxide, and the crosslinked body was impregnated with carbon dioxide for 1 hour under the conditions of a temperature of 110°C and a pressure of 55 bar (about 5.5 MPa). After that, the pressure inside the autoclave was returned to a pressure of 6 bar (about 0.6 MPa) at a rate of 50 bar / min (about 5.0 MPa / min) (during this process, carbon dioxide was discharged outside the autoclave), and the crosslinked body was left to stand for 1 hour to foam, thereby obtaining a foam sheet.
[0186] Table 1 shows the composition of each component in the mixture used to mold the sheet, the molding conditions used when molding the sheet, and the results regarding the physical properties (foam performance) of the obtained foam sheet.
[0187] [Examples 2 to 4 and Comparative Example 1] Examples 2 to 4 and Comparative Example 1 were carried out in the same manner as Example 1, except that the composition of each component in the mixture used for forming the sheets was changed as shown in Table 1 below.
[0188] Here, in Table 1 below, "EVA (VA = 28%)" refers to ethylene-vinyl acetate copolymer (vinyl acetate content 28% by mass) [product name EVA FLEX EV270], which corresponds to ethylene-polar monomer copolymer (B).
[0189] Also, "TAC 50" as used in Example 3 refers to Rhenogran® TAC-50: a 50% by weight triallyl cyanurate and 50% by weight ethylene-propylene-diene elastomer composition. The results are shown in Table 1.
[0190] [Table 1]
[0191] [Method of manufacturing chemical foam] [Comparative Example 2] As Comparative Example 2, a comparative example for a foam obtained using a chemical foaming agent (azodicarbonamide (ADCA)) is shown below.
[0192] A mixture consisting of 50 parts by weight of ethylene-vinyl acetate copolymer (vinyl acetate content 25% by weight) [product name EVAFlex EV360] (hereinafter referred to as "EVA (VA = 25%)"), 50 parts by weight of copolymer (A-1), 3.0 parts by weight of titanium oxide (TiO2), 3.0 parts by weight of zinc oxide (ZnO), 1.0 part by weight of stearic acid, 0.7 parts by weight of dicumyl peroxide (DCP), 0.1 part by weight of triallylisocyanurate (TAIC), and 2.7 parts by weight of azodicarbonamide (ADCA) was kneaded with a roll at a roll surface temperature of 120°C for 10 minutes and then formed into a sheet.
[0193] The obtained sheet was filled into a press mold and pressed at 150 kg / cm 2 The mixture was pressurized and heated at 170°C for 15 minutes to obtain a crosslinked foam. The size of this press mold was 10 mm thick, 151.5 mm long, and 76.5 mm wide.
[0194] Table 2 shows the composition of each component in the mixture used to form the sheet, and the results regarding the physical properties (foam performance) of the obtained foam sheet.
[0195] [Table 2]
Claims
1. It contains an ethylene / α-olefin copolymer (A) obtained by copolymerizing only ethylene and an α-olefin having 3 to 20 carbon atoms, Residual nitrogen amount measured by chemiluminescence method is 200 ppm or less Foam.
2. 2. The foam of claim 1, comprising an ethylene-polar monomer copolymer (B).
3. The foam of claim 1 further comprising a crosslinking agent (C).
4. The foam according to claim 1, wherein the ethylene / α-olefin copolymer (A) satisfies the following requirements (A-a) and (A-b): (A-a) density is 0.850 to 0.910 g / cm 3 in the range of; (A-b) Melt flow rate (MFR) measured at 190°C under a load of 2.16 kg according to the method of ASTM D1238 2.16 ) is in the range of 0.01 to 200 g / 10 min.
5. The foam according to claim 1, wherein the ethylene / α-olefin copolymer (A) satisfies the following requirements (Ac) and (Ad): (A-c) 1 The vinyl group content per 1,000 carbon atoms as determined by H-NMR is in the range of 0.025 to 0.3; (A-d) MFR 10 / M.F.R. 2.16 is in the range of 7 to 20 (where MFR 10 is the melt flow rate measured at 190°C under a load of 10 kg according to the method of ASTM D1238, and MFR 2.16 is the melt flow rate measured at 190° C. under a load of 2.16 kg according to the method of ASTM D1238.
6. A layer comprising the foam according to claim 1; a layer made of at least one material selected from the group consisting of polyolefin, polyurethane, rubber, leather and artificial leather; A laminate having the following structure:
7. Footwear comprising the foam of claim 1 or the laminate of claim 6.
8. 10. A footwear component comprising the foam of claim 1 or the laminate of claim 6.
9. The footwear part according to claim 8, wherein the footwear part is a midsole, an innersole or a sole.
10. A method for producing a foam, comprising a step of physically foaming an ethylene / α-olefin copolymer (A) obtained by copolymerizing only ethylene with an α-olefin having 3 to 20 carbon atoms.
11. A method for producing a foam, comprising a step of physically foaming a composition containing an ethylene / α-olefin copolymer (A) obtained by copolymerizing only ethylene and an α-olefin having 3 to 20 carbon atoms, and a crosslinking agent (C).
12. A method for producing a foam, comprising the step of impregnating an ethylene / α-olefin copolymer (A) obtained by copolymerizing only ethylene with an α-olefin having 3 to 20 carbon atoms, with a supercritical fluid.
13. A method for producing a foam, comprising the step of impregnating a composition containing an ethylene / α-olefin copolymer (A) obtained by copolymerizing only ethylene and an α-olefin having 3 to 20 carbon atoms, and a crosslinking agent (C) into a supercritical fluid.
Citation Information
Patent Citations
Process for making cross-linked ethylene-based polymer foam structures
JP1997501447A
Ethylenic random copolymer and its production
JP1999005818A
Foam for shoe sole
JP1999206406A
Foam, composition for foam, and use of the foam
WO2007132731A1