Resin film for graphite sheet, graphite sheet, and production methods of these
A laminated resin film with a phenolic resin layer on a non-thermoplastic polyimide layer addresses the cost and thermal diffusivity issues in graphite sheet manufacturing, achieving high thermal conductivity and low production costs by leveraging the thermal stability difference between the layers.
Patent Information
- Application Number
- JP2023059456
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for manufacturing graphite sheets using laminated polyimide films are costly and do not efficiently produce graphite sheets with high thermal diffusivity.
A resin film for graphite sheets with a laminated structure comprising a phenolic resin layer on a non-thermoplastic polyimide layer, where the non-thermoplastic polyimide layer has a birefringence of 0.095 or more, is used to create a graphite sheet with improved thermal diffusivity by leveraging the thermal stability difference between the two layers during carbonization and graphitization.
The method results in a graphite sheet with excellent thermal diffusivity and reduced manufacturing costs, as the phenolic resin layer is pseudo-stretched and fixed by the thermally stable non-thermoplastic polyimide layer, enhancing crystal orientation and thermal conductivity.
Smart Images

Figure 2024146506000004 
Figure 2024146506000001 
Figure 2024146506000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin film for a graphite sheet, a graphite sheet, and methods for producing the same. [Background technology]
[0002] Graphite sheets have excellent thermal conductivity and are therefore used as heat dissipation members in various electronic devices such as computers, semiconductor elements mounted in electrical devices, and other heat-generating parts.
[0003] As a method for producing such a graphite sheet, a method is known in which a polyimide film is subjected to a heat treatment in an inert gas at a high temperature of, for example, 2400° C. or higher to carbonize and graphitize the polyimide constituting the polyimide film, and then, optionally, a rolling treatment is performed.
[0004] In recent years, there has been an increasing demand for thick graphite sheets that are advantageous in terms of heat transport. As a method for producing such graphite sheets, for example, a method is known in which a laminated polyimide film formed by laminating two or more polyimide films is used as a raw material (see Patent Documents 1 to 3, etc.). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2022 / 158526 Brochure [Patent Document 2] JP 2017-114098 A [Patent Document 3] Special Publication No. 2022-512190 Summary of the Invention [Problem to be solved by the invention]
[0006] However, the above-mentioned technique for producing a graphite sheet using a laminated polyimide film has room for improvement in terms of producing a graphite sheet at low production costs.
[0007] An object of the present invention is to provide a graphite sheet that has excellent thermal diffusivity and can be produced at low cost, and a resin film for graphite sheet that is the raw material for the graphite sheet. [Means for solving the problem]
[0008] In order to solve the above problems, one embodiment of the present invention includes the following configuration.
[0009] That is, one embodiment of the present invention relates to a resin film for graphite sheet having a laminated structure in which a phenolic resin layer is laminated on at least one surface of a non-thermoplastic polyimide layer, wherein the non-thermoplastic polyimide layer has a birefringence of 0.095 or more in a single layer film.
[0010] Moreover, one embodiment of the present invention relates to a method for producing a resin film for a graphite sheet, the method comprising a step of preparing a laminate by forming a phenolic resin layer on at least one surface of a non-thermoplastic polyimide layer, wherein the non-thermoplastic polyimide layer has a birefringence of 0.095 or more in a single layer film. Effect of the Invention
[0011] According to a resin film for graphite sheet according to one embodiment of the present invention, it is possible to realize a graphite sheet that has excellent thermal diffusivity and low production costs, and a resin film for graphite sheet that can be used to produce the graphite sheet. [Brief description of the drawings]
[0012] [Figure 1]FIG. 2 is a schematic diagram showing an example of a method for carrying out a step of preparing a laminate using a press in a manufacturing method of a resin film for a graphite sheet according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] An embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to each configuration described below, and various modifications are possible within the scope of the claims, and embodiments and examples obtained by appropriately combining the technical means disclosed in different embodiments and examples are also included in the technical scope of the present invention. In addition, all academic literature and patent documents described in this specification are incorporated herein by reference. In addition, unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more and B or less."
[0014] <1. Technical idea of the present invention> In order to use a graphite sheet as a heat dissipation member, the graphite sheet is required to have excellent thermal diffusivity. The thermal diffusivity of a graphite sheet depends on the crystal orientation of the graphite sheet, and the higher the crystal orientation, the higher the thermal diffusivity of the graphite sheet.
[0015] When highly oriented polyimide film is carbonized and graphitized, crystallization proceeds well, making it possible to produce a graphite sheet with high crystal orientation and excellent thermal diffusivity. For this reason, in the past, in order to produce a thick graphite sheet with high crystal orientation, a resin film for graphite sheet having a laminated structure composed only of highly oriented polyimide film has been used as the raw material.
[0016] However, a resin film for a graphite sheet having a laminated structure composed only of the highly oriented polyimide film has a problem in that it is disadvantageous in terms of cost.
[0017] A graphite sheet with low manufacturing costs is, for example, a graphite sheet manufactured from a film made of a resin that is less expensive than polyimide. However, such a graphite sheet has a low thermal diffusivity.
[0018] In the course of investigations, the present inventors used a phenolic resin which is low in production cost but which is expected to produce a graphite sheet with a low thermal diffusivity. They carbonized and graphitized a resin film for graphite sheet having a laminate structure in which the phenolic resin layer is laminated on a non-thermoplastic polyimide film with high birefringence. They found that, contrary to expectations, a graphite sheet with excellent thermal diffusivity was obtained, which led to the completion of the present invention.
[0019] This is presumably due to the action described below. When the resin film for graphite sheet according to one embodiment of the present invention is heated and carbonized / graphitized, the phenolic resin constituting the phenolic resin layer undergoes thermal decomposition, and as a result, a force acts in the direction in which the phenolic resin layer tends to shrink. On the other hand, the non-thermoplastic polyimide layer on which the phenolic resin layer is laminated is known to have a constituent non-thermoplastic polyimide that is more thermally stable than the phenolic resin and has a higher thermal decomposition temperature. Specifically, it is known that the "thermal decomposition temperature" of the phenolic resin is usually 10°C or more lower than the "thermal decomposition temperature" of the non-thermoplastic polyimide. The "thermal decomposition temperature" is also known as the "thermal decomposition peak temperature (T pThe term "temperature at the peak position of a differential thermogravimetry (DTG) curve obtained by differentiating a thermogravimetry (TG) curve with respect to time, which is called "temperature at the peak position of a differential thermogravimetry (DTG) curve," is intended. Thus, when the phenolic resin is thermally decomposed, the non-thermoplastic polyimide is not thermally decomposed, and the shape of the non-thermoplastic polyimide layer does not change. Therefore, the phenolic resin layer is laminated and fixed by the non-thermoplastic polyimide layer during thermal decomposition, and as a result, the phenolic resin layer does not shrink against the force acting in the direction of shrinkage, but is pseudo-stretched, improving its orientation. As a result, it is considered to change into a graphite sheet with high crystal orientation and excellent thermal diffusivity.
[0020] It has not been known in the past and is a surprising finding that a graphite sheet having excellent thermal diffusivity can be obtained from a resin film for graphite sheet having such a laminated structure including a phenolic resin layer with low orientation.
[0021] <2. Resin film for graphite sheets> A resin film for graphite sheet according to one embodiment of the present invention (hereinafter, sometimes referred to as the present resin film) will be described in detail below. The present resin film is a resin film for graphite sheet having a laminated structure in which a phenolic resin layer is laminated on at least one surface of a non-thermoplastic polyimide layer, and the non-thermoplastic polyimide layer has a birefringence of 0.095 or more in a single layer film. In this specification, the non-thermoplastic polyimide layer is also referred to as a "polyimide film."
[0022] The present resin film has a low production cost, and by including a phenolic resin layer, a graphite sheet can be provided that can be produced at low cost.
[0023] As described above, the phenolic resin layer in the present resin film is laminated on at least one surface of the non-thermoplastic polyimide layer, and is therefore pseudo-stretched during carbonization and graphitization, improving its orientation and changing into a graphite layer with excellent thermal diffusivity. Furthermore, the non-thermoplastic polyimide layer in the present resin film has a birefringence of 0.095 or more in a single layer film and is highly oriented, so that it changes into a graphite layer with excellent thermal diffusivity through carbonization and graphitization. Thus, a graphite sheet with excellent thermal diffusivity can be produced from the present resin film through carbonization and graphitization.
[0024] Thus, the present resin film has the effect of providing a graphite sheet that has excellent thermal diffusivity and can be produced at low costs.
[0025] <2.1. Non-thermoplastic polyimide layer> (Birefringence) The non-thermoplastic polyimide layer constituting the present resin film has a birefringence of 0.095 or more in a monolayer film. Here, the "birefringence in a monolayer film" means the birefringence of the monolayer when the non-thermoplastic polyimide layer is formed as a monolayer, and can be determined, for example, by measuring the birefringence of the non-thermoplastic polyimide layer before laminating the phenolic resin layer.
[0026] Since the orientation of the non-thermoplastic polyimide layer does not change even when the phenolic resin layer is laminated thereon, the birefringence of the non-thermoplastic polyimide layer does not change substantially either. Therefore, in the present resin film having a laminated structure, the "birefringence in a single layer film" of the non-thermoplastic polyimide layer can be determined, for example, by removing the phenolic resin layer and the like from the present resin film and then measuring the birefringence of the remaining non-thermoplastic polyimide layer.
[0027] In one embodiment of the present invention, the birefringence can be measured by the method described in JIS K0062: 1992. Specifically, the birefringence can be measured using a commercially available refractive index measuring device, and more specifically, can be measured by the method described in the examples below.
[0028] When the birefringence is high, the non-thermoplastic polyimide layer is converted into a graphite layer having superior thermal diffusivity by carbonization and graphitization, so the higher the birefringence, the better. Specifically, the birefringence is more preferably 0.1 or more. In addition, the birefringence may usually be 0.2 or less, and is preferably 0.16 or less.
[0029] (Composition of Non-Thermoplastic Polyimide Layer) The non-thermoplastic polyimide layer has a birefringence of 0.095 or more in a single layer film, and the composition is not particularly limited as long as the layer contains a non-thermoplastic polyimide. The non-thermoplastic polyimide layer preferably contains a non-thermoplastic polyimide made mainly of an acid dianhydride component and a diamine component.
[0030] (Acid dianhydride component) The acid dianhydride component is not particularly limited. The acid dianhydride component preferably contains 50 mol% or more of pyromellitic dianhydride (hereinafter also referred to as "PMDA") in the total amount of the acid dianhydride component (100 mol%). The amount of PMDA contained in the acid dianhydride component is preferably 50 mol% or more, more preferably 70 mol% or more, and even more preferably 90 mol% or more, based on the total amount of the acid dianhydride component (100 mol%), from the viewpoint of being able to provide the non-thermoplastic polyimide layer having appropriate orientation and birefringence. The amount of PMDA contained in the acid dianhydride component may be 95 mol% or more, or may be 100 mol%.
[0031] The non-thermoplastic polyimide may contain an acid dianhydride other than the PMDA as the acid dianhydride component. Examples of the other acid dianhydrides include 3,3',4,4'-benzophenonetetracarboxylic dianhydride (hereinafter referred to as "BTDA"), 4,4'-oxydiphthalic dianhydride (hereinafter referred to as "ODPA"), naphthalenetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, 1,1-(dicarboxyphenyl)ethane dianhydride, bis(dicarboxyphenyl)methane dianhydride, bis(3,4-dicarboxyphenyl)sulfone dianhydride, p-phenylene bis(trimellitic acid monoester dianhydride), ethylene bis(trimellitic acid monoester dianhydride), bisphenol A bis(trimellitic acid monoester dianhydride), and the like. As the other acid dianhydrides, these acid dianhydrides may be used alone, or a plurality of these acid dianhydrides may be mixed in any ratio.
[0032] The content of the other acid dianhydrides in the acid dianhydride component that is the raw material of the non-thermoplastic polyimide can be 50 mol % or less, preferably 30 mol % or less, and more preferably 10 mol % or less, in 100 mol % of the total amount of the acid dianhydride components.
[0033] (Diamine component) The diamine component, which is a raw material of the non-thermoplastic polyimide, preferably contains 50 mol % or more of 4,4'-diaminodiphenyl ether (hereinafter, referred to as "ODA").
[0034] In one embodiment of the present invention, from the viewpoint of providing the non-thermoplastic polyimide layer having appropriate orientation and birefringence, the amount of ODA contained in the diamine component is preferably 50 mol% or more, more preferably 60 mol% or more, and even more preferably 70 mol% or more, based on 100 mol% of the total amount of the diamine component. The amount of ODA contained in the diamine component may be 80 mol% or more, 90 mol% or more, 95 mol% or more, or even 100 mol%.
[0035] In particular, it is preferable that the diamine component contains 50 mol % or more of ODA and the acid dianhydride component contains 50 mol % or more of PMDA. With this configuration, the orientation and birefringence of the non-thermoplastic polyimide layer are improved, and as a result, the thermal diffusivity of the finally obtained graphite sheet is improved.
[0036] The non-thermoplastic polyimide may contain other diamines as the diamine component other than the ODA. Examples of the other diamines include 2,2-bis[4-(4-aminophenoxy)phenyl]propane (hereinafter referred to as "BAPP"), p-phenylenediamine (PDA), 4,4'-diaminodiphenylmethane, benzidine, 3,3'-dichlorobenzidine, 4,4'-diaminodiphenyl sulfide, diaminodiphenyl sulfone, diaminodiphenyl ether, 1,5-diaminonaphthalene, 4,4'-diaminodiphenyl diethyl silane, 4,4'-diaminodiphenyl silane, 4,4'-diaminodiphenyl ethyl phosphine oxide, 4,4'-diaminodiphenyl N-methylamine, 4,4'-diaminodiphenyl N-phenylamine, 1,3-diaminobenzene, and the like. As the other diamines, these diamines may be used alone, or a plurality of these diamines may be used in any ratio.
[0037] The content of the other diamine in the diamine component that is the raw material of the non-thermoplastic polyimide can be 50 mol % or less, preferably 30 mol % or less, and more preferably 10 mol % or less, in 100 mol % of the total amount of the diamine component.
[0038] The non-thermoplastic polyimide is a non-thermoplastic polyimide made from substantially equimolar amounts of the acid dianhydride component and the diamine component. In this specification, the term "substantially equimolar amounts" means that the molar ratio of two or more different substances (e.g., the acid dianhydride component and the diamine component) is within the range of 100:98 to 100:102, and preferably 100:100.
[0039] (Physical properties of non-thermoplastic polyimide layer) The thickness of the non-thermoplastic polyimide layer is preferably 5 μm or more, and more preferably 12 μm or more. When the thickness of the non-thermoplastic polyimide layer is 5 μm or more, the phenolic resin layer can be more suitably laminated and fixed by the non-thermoplastic polyimide layer during carbonization and graphitization of the present resin film, and can be changed into a graphite layer having superior thermal diffusivity.
[0040] If the thickness of the non-thermoplastic polyimide layer is too large, problems such as a decrease in productivity of the non-thermoplastic polyimide layer and an increase in cost may occur, etc. Therefore, the thickness of the non-thermoplastic polyimide layer is preferably 75 μm or less, and more preferably 50 μm or less.
[0041] <2.2. Phenol resin layer> The phenolic resin layer constituting the present resin film is not particularly limited as long as it is a layer containing a phenolic resin. The phenolic resin layer may contain one type of phenolic resin, or may contain two or more types of phenolic resin. The phenolic resin contained in the phenolic resin layer constituting the present resin film may be in a cured state, a partially cured state, or an uncured state.
[0042] It is known that the birefringence of a layer containing a phenolic resin is generally lower than that of the non-thermoplastic polyimide layer. Therefore, a graphite sheet obtained by carbonizing and graphitizing a resin film for graphite sheet having a laminated structure containing a phenolic resin usually has a low thermal diffusivity. However, as described above, the phenolic resin layer constituting the present resin film is laminated and fixed to the non-thermoplastic polyimide layer, and when carbonized and graphitized, it is pseudo-stretched, has improved orientation, and is changed into a graphite layer with excellent thermal diffusivity. Therefore, by using the present resin film as a raw material, a graphite sheet having excellent thermal diffusivity and low production cost can be provided.
[0043] (Composition of phenolic resin layer) The content of the phenolic resin in the phenolic resin layer is preferably 50% by weight or more, more preferably 70% by weight or more, and even more preferably 90% by weight or more, based on the total weight of the phenolic resin layer. When the phenolic resin layer contains two or more kinds of phenolic resins, the total content of each phenolic resin is the content of the phenolic resin in the phenolic resin layer.
[0044] Here, the phenolic resin means a polymer obtained by polymerizing a phenol and an aldehyde compound.
[0045] The phenols that are monomers constituting the phenol-based resin are not particularly limited, and examples thereof include phenol and cresol.
[0046] The aldehyde compound, which is a monomer constituting the phenol-based resin, is not particularly limited, and examples thereof include formaldehyde, glutaraldehyde, and the like.
[0047] Phenolic resins are generally classified into novolac resins and resol resins, but both novolac resins and resol resins can be used. In addition, other phenolic resins different from novolac resins and resol resins can also be used. Specific examples of the novolac resins include Phenolite (manufactured by DIC), etc. Specific examples of the resol resins include Sumilite Resin (manufactured by Sumitomo Bakelite), etc. Specific examples of the other phenolic resins include Bellpearl (registered trademark) (manufactured by Air Water Bellpearl Co., Ltd.), etc.
[0048] The phenol resin layer may contain additives such as an organic phosphorus compound and inorganic particles, as long as the object of the present invention is not impaired.
[0049] (Physical properties of phenolic resin layer) The thickness of the phenolic resin layer is preferably 100 μm or less, more preferably 50 μm or less. When the thickness of the phenolic resin layer is 100 μm or less, the phenolic resin layer is more suitably laminated and fixed by the non-thermoplastic polyimide layer during carbonization and graphitization of the present resin film, and is more strongly pseudo-stretched, so that the phenolic resin layer can be converted into a graphite layer having superior thermal diffusivity.
[0050] The thickness of the phenolic resin layer is preferably more than 1 μm, and more preferably 10 μm or more. When the thickness of the phenolic resin layer is more than 1 μm, a thick graphite sheet that is advantageous in terms of thermal diffusivity can be suitably produced.
[0051] In addition, the ratio of the thickness of the adjacent phenolic resin layer to the thickness of the non-thermoplastic polyimide layer (thickness of phenolic resin layer / thickness of non-thermoplastic polyimide layer) is preferably 0.1 or more and 10.0 or less, more preferably 0.2 or more and 8.0 or less. Here, the "phenolic resin layer adjacent to the non-thermoplastic polyimide layer" refers to the ratio of the thickness of one phenolic resin layer to the thickness of one adjacent non-thermoplastic polyimide layer in the portion where the non-thermoplastic polyimide layer and the phenolic resin layer are adjacent when multiple non-thermoplastic polyimide layers and multiple phenolic resin layers are laminated. When the resin film has multiple portions where the non-thermoplastic polyimide layer and the phenolic resin layer are adjacent, it is preferable that the ratio of the thickness of one phenolic resin layer to the thickness of the adjacent non-thermoplastic polyimide layer in at least one portion is within the above range, and it is more preferable that the ratio of the thickness of one phenolic resin layer to the thickness of one non-thermoplastic polyimide layer in all portions is within the above range. In addition, the term "adjacent" includes cases where the non-thermoplastic polyimide layer and the phenolic resin layer are laminated directly to each other in the resin film, and cases where they are laminated to each other via an adhesive layer, which will be described later.
[0052] By setting the ratio (phenolic resin layer thickness / non-thermoplastic polyimide layer thickness) to 10.0 or less, the phenolic resin layer can be changed into a graphite layer having superior thermal diffusivity. Also, by setting the ratio (phenolic resin layer thickness / non-thermoplastic polyimide layer thickness) to 0.1 or more, a graphite sheet having a large thickness that is advantageous in terms of thermal diffusivity can be suitably produced, and the production cost of the graphite sheet can be reduced.
[0053] The arithmetic mean roughness (Ra) of the surface of the non-thermoplastic polyimide layer on the phenolic resin layer side and the arithmetic mean roughness (Ra) of the surface of the phenolic resin layer on the non-thermoplastic polyimide layer side are not particularly limited. In addition, the surface of the non-thermoplastic polyimide layer and / or the surface of the phenolic resin layer may be subjected to a treatment for improving adhesion.
[0054] <2.3. Structure of this resin film> The present resin film is not particularly limited as long as it has a laminated structure in which a phenolic resin layer is laminated on at least one surface of the non-thermoplastic polyimide layer. The laminated structure in the present resin film is preferably a laminated structure in which the non-thermoplastic polyimide layer and the phenolic resin layer are directly laminated without the presence of other layers such as an adhesive layer.
[0055] The laminated structure has the non-thermoplastic polyimide layer and the phenolic resin layer directly laminated thereon, and therefore can be changed into a graphite sheet having superior thermal diffusivity.
[0056] The laminated structure may be a three-layer structure or a four-layer structure including, in addition to the non-thermoplastic polyimide layer and the phenolic resin layer, another non-thermoplastic polyimide layer and another phenolic resin layer, or may further include another layer. The non-thermoplastic polyimide layers and the phenolic resin layers each included in the resin film may be the same or different non-thermoplastic polyimide layers and phenolic resin layers, respectively.
[0057] <3. Graphite sheet> One embodiment of the present invention also includes a graphite sheet containing the present resin film as a raw material (hereinafter, referred to as the present graphite sheet). The present graphite sheet contains the present resin film as a raw material, and therefore has high crystal orientation and excellent thermal diffusivity. The present resin film also contains a phenolic resin layer that has a low manufacturing cost. Therefore, the present graphite sheet has a low manufacturing cost. In this specification, the present graphite sheet refers to both the graphite sheet before being subjected to the rolling process described below (graphite sheet before rolling) and the graphite sheet after being subjected to the rolling process (graphite sheet after rolling), but unless otherwise specified, refers to the graphite sheet after rolling.
[0058] The density of this graphite sheet is 0.90g / cm 3 It is preferable that the content is 1.10 g / cm or more. 3 More preferably, it is 1.30 g / cm or more. 3 More preferably, it is 1.50 g / cm or more. 3 The upper limit of the density is not particularly limited, but is usually 2.20 g / cm. 3 The density is 0.90 g / cm 3 The graphite sheet described above can realize efficient heat dissipation. In addition, a plurality of the graphite sheets can be laminated with a resin layer interposed therebetween to form a graphite plate having a block shape such as a cube or a rectangular parallelepiped. The graphite plate can be made of anisotropic graphite having a desired shape using a wire saw or the like. The density of the graphite sheet can be measured by the method described in the examples below.
[0059] (Thermal Conductivity) In this specification, the thermal conductivity of the graphite sheet can be evaluated by the thermal diffusivity of the graphite sheet. The thermal diffusivity of the graphite sheet is 2.0 cm 2 / s or more is sufficient, and 4.0 cm 2 / s or more is preferable, and 7.0 cm 2 / s or more is preferable, and 8.0m 2 More preferably, it is 9.0 cm / s or more. 2 It is even more preferable that the thermal diffusivity is 4.0 cm / s or more. 2 A graphite sheet having a thermal conductivity of 100 / s or more has excellent thermal conductivity.
[0060] The thermal diffusivity is measured using the method described in JIS R7240: 2018. Specific examples of the method for measuring the thermal diffusivity include the method described in the (Thermal diffusivity) section of the Examples described later.
[0061] The lower limit of the thickness of the graphite sheet is preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 20 μm or more, from the viewpoint of enabling efficient heat dissipation. The upper limit of the thickness of the graphite sheet after rolling is preferably 150 μm or less, and more preferably 100 μm or less, from the viewpoint of enabling arrangement in a small space.
[0062] <4. Manufacturing method of graphite sheet> The method for producing a graphite sheet according to one embodiment of the present invention (hereinafter sometimes referred to as the method for producing the graphite sheet) is not particularly limited as long as it is possible to heat-treat the resin film and provide a graphite sheet, and is preferably a method including a step of heat-treating the resin film at 2400°C or higher. The method for producing the graphite sheet will be described in detail below. In the following description, with regard to the resin film, the descriptions in the above section <2. Resin film for graphite sheet> and the below-mentioned section <5. Method for producing resin film for graphite sheet> are appropriately cited.
[0063] The method for producing the graphite sheet is preferably a so-called polymer pyrolysis method in which the resin film is heat-treated in an inert gas atmosphere or under reduced pressure. Specifically, the method preferably includes a carbonization step in which the resin film is preheated at a temperature of about 1000°C to obtain a carbonized resin film, and a graphitization step in which the carbonized resin film produced in the carbonization step is heat-treated (heated) at a temperature of 2400°C or higher to graphitize the resin film. The method may further include a rolling step in which the graphite sheet obtained in the graphitization step is rolled. In the method for producing the graphite sheet, the carbonization step and the graphitization step may be performed consecutively, or the graphitization step may be performed separately after the carbonization step is completed.
[0064] (carbonization process) The carbonization step is a step of carbonizing the present resin film by heat treatment up to a temperature of about 1000°C. The carbonization method of the present resin film in the carbonization step is not particularly limited, and for example, a sheet of the present resin film may be carbonized, a roll of the present resin film may be carbonized while still in the roll, or the film may be unrolled from the roll of the present resin film and continuously carbonized. The carbonization step is preferably carried out in a vacuum atmosphere, under reduced pressure, or in an inert gas, and nitrogen is preferably used as the inert gas. In this specification, the carbonized present resin film obtained by the carbonization step may be referred to as a carbonaceous film.
[0065] (Graphitization process) The graphitization step is a step of graphitizing the carbonaceous film obtained in the carbonization step by heat treatment at a temperature of 2400°C or higher to obtain a graphite sheet before rolling. In the graphitization step, the temperature (maximum temperature) during heat treatment is preferably 2400°C or higher, 2600°C or higher, 2800°C or higher, 2900°C or higher, or 3000°C or higher, since the thermal diffusivity of the obtained graphite sheet is good. The upper limit of the maximum temperature is not particularly limited, but is preferably 3300°C or lower, and more preferably 3200°C or lower, since sublimation of the graphite member in the graphitization furnace can be suppressed. The graphitization step is performed under reduced pressure or in an inert gas, and argon or helium can be suitably used as the inert gas.
[0066] In the graphitization step, a sheet of carbonaceous film may be graphitized, a roll of carbonaceous film may be graphitized while still in the roll state, or the film may be unwound from the roll of carbonaceous film and continuously graphitized.
[0067] In the graphitization step, the temperature rise rate when the carbonaceous film is heated to the maximum temperature is not particularly limited, but from the viewpoint of providing a graphite sheet with good productivity, the temperature rise rate is preferably 0.2° C. / min or more, more preferably 0.3° C. / min or more, even more preferably 0.4° C. / min or more, and even more preferably 0.5° C. / min or more.
[0068] (Rolling process) The rolling step is a step of rolling the graphite sheet obtained in the graphitization step before rolling. The graphite sheet before rolling is in a foamed state due to the influence of outgassing generated in the graphitization step and may have an excessive thickness that is unsuitable for practical use. However, by carrying out the rolling step, the thickness of the graphite sheet can be adjusted and flexibility can be imparted to the graphite sheet. In the rolling step, the method of rolling the graphite sheet is not particularly limited, and examples thereof include roll rolling in which the graphite sheet is rolled using a metal roll and a resin roll, and pressing. The rolling step may be carried out in a state in which the produced graphite sheet has been cooled to room temperature, or may be carried out continuously with the graphitization step.
[0069] <5. Manufacturing method of resin film for graphite sheet> A manufacturing method of a resin film for graphite sheet according to one embodiment of the present invention (hereinafter may be referred to as the manufacturing method of the present resin film) is a manufacturing method of a resin film for graphite sheet comprising a step of preparing a laminate by forming a phenolic resin layer on at least one side of a non-thermoplastic polyimide layer, wherein the non-thermoplastic polyimide layer has a birefringence of 0.095 or more in a single layer film.
[0070] The method for producing the present resin film is not particularly limited as long as it includes a step of preparing the laminate. For example, the method for producing the present resin film includes preparing the non-thermoplastic polyimide layer in advance, forming a pre-cured phenolic resin layer on the non-thermoplastic polyimide layer, and heating and curing the pre-cured phenolic resin layer to produce the present resin film.
[0071] The method for preparing the non-thermoplastic polyimide layer in advance may include a method of using a commercially available non-thermoplastic polyimide film having a birefringence of 0.095 or more as the non-thermoplastic polyimide layer, a chemical imidization method (chemical cure) in which a polyamic acid solution containing an imidization accelerator is heated to imidize the polyamic acid, and a thermal imidization method (thermal cure) in which a polyamic acid solution is heated to imidize without using an imidization accelerator, and a method of combining the non-thermoplastic polyimide layer with other known operations that can improve the orientation of the prepared polyimide film (non-thermoplastic polyimide layer).
[0072] The method for preparing a laminate by forming a phenolic resin layer on at least one surface of the non-thermoplastic polyimide layer is not particularly limited, and for example, the following methods (a) to (c) can be adopted. (a) A method of preparing a laminate by uniformly scattering particles of the phenolic resin (phenolic resin particles) on a surface of the non-thermoplastic polyimide layer, and then using a heat press to spread the phenolic resin particles on one surface of the non-thermoplastic polyimide layer to form a pre-cured phenolic resin layer, and at the same time, heating and curing the pre-cured phenolic resin layer. (b) A method of preparing a laminate by applying a coating liquid containing the phenolic resin onto a surface of the non-thermoplastic polyimide layer to form a coating layer, and then heating the coating layer to form a phenolic resin layer. (c) A method of preparing a laminate by thermocompression bonding a separately prepared phenolic resin layer onto the surface of the non-thermoplastic polyimide layer.
[0073] Hereinafter, the methods for producing a resin film for a graphite sheet will be described by taking the methods (a) to (c) as examples.
[0074] The method (a) can be adopted when a phenolic resin that is solid at room temperature is used as the phenolic resin. Hereinafter, an example of the method (a) will be described with reference to FIG. 1. As shown in FIG. 1, a press machine is used that is provided with a pair of opposing press plates 1 and a cylinder 6 on the lower side of the lower press plate 1. A stainless steel (SUS) plate 2 is placed on the lower press plate 1, a protective film 5 is placed on the SUS plate 2, and a non-thermoplastic polyimide layer 3 is placed on the protective film 5. Then, the phenolic resin particles 4 are uniformly scattered on the non-thermoplastic polyimide layer 3. Then, a non-thermoplastic polyimide layer 3' is placed on the phenolic resin particles 4, a protective film 5 is placed on the non-thermoplastic polyimide layer 3', and a SUS plate 2 is placed on the protective film 5. Then, the cylinder 6 is moved upward (in the direction of the arrow in FIG. 1) to move the lower press plate 1 upward so that the upper SUS plate 2 and the upper press plate 1 come into contact with each other. Next, pressure is applied to the phenolic resin particles 4 while heating, so that the phenolic resin particles 4 are spread and the phenolic resin particles 4 are changed into a pre-cured phenolic resin layer. As a result, a laminate of the non-thermoplastic polyimide layer 3 / the pre-cured phenolic resin layer / another non-thermoplastic polyimide layer 3' is prepared. The method (a) may also include applying pressure to the pre-cured phenolic resin layer while heating.
[0075] In the method (a), an example of a method of applying pressure to the phenolic resin particles 4 and the pre-cured phenolic resin layer while heating it is to apply pressure while controlling the temperature of the upper press plate 1 and / or the lower press plate 1 (hereinafter referred to as the "heat press set temperature") to a high temperature. The "heat press set temperature" can be appropriately set and used as a temperature at which the phenolic resin particles 4 can be suitably spread and cured without thermally decomposing the non-thermoplastic polyimide layer 3, the other non-thermoplastic polyimide layer 3', the phenolic resin particles 4, and the pre-cured / cured phenolic resin layer. The "heat press set temperature" is, for example, 50°C to 250°C, preferably 100°C to 200°C.
[0076] In the method (a), the pressure applied to the phenolic resin particles 4 and / or the phenolic resin layer before curing can be appropriately set and adopted so that the phenolic resin particles 4 can be suitably pushed and cured without damaging the members used in the method (a) and each layer constituting the present resin film. In addition, the method of applying the pressure is preferably a method of gradually increasing the magnitude of the applied pressure from the viewpoint of suitably preventing damage to the members. Note that pressure can be applied to the phenolic resin particles 4 and / or the phenolic resin layer before curing by applying a load of a predetermined magnitude to the phenolic resin particles 4 and / or the phenolic resin layer before curing. The magnitude of the load can be controlled, for example, by adjusting the cylinder pressure of the cylinder 6 when the method (a) is carried out using a press machine shown in FIG. 1. Hereinafter, the final magnitude of the load when the magnitude of the load applied is increased in order to increase the pressure applied is referred to as the "set load". The "set load" may be appropriately selected depending on the type and thickness of the material constituting the member, and is, for example, 1 kgf to 10,000 kgf, and preferably 10 kgf to 5,000 kgf.
[0077] In the method (a), from the viewpoint of suppressing bubbles that may occur during the heat pressing, it is preferable to preheat the member by heating before the heat pressing. After preheating for a predetermined time at a predetermined heat pressing temperature, it is preferable to gradually increase the magnitude of the load applied, and after the magnitude of the load reaches the set load, to maintain the magnitude of the load at the set load for a predetermined time.
[0078] There is no particular limitation on the protective film 5, and for example, a polytetrafluoroethylene (PTFE) film, a rubber sheet, etc. may be used. In the above-mentioned heat pressing, the protective film 5 does not have to be used.
[0079] The coating liquid in the method (b) contains the phenolic resin and may be a coating liquid made of the phenolic resin in a liquid state, or may be a coating liquid in which the phenolic resin is dissolved in a solvent.
[0080] When the coating liquid is a coating liquid in which the phenolic resin is dissolved in a solvent, the solvent is not particularly limited as long as it can dissolve the phenolic resin without adversely affecting the non-thermoplastic polyimide layer. Specific examples of the solvent include methanol. The solvent may be one of the above-mentioned solvents, or a mixture of two or more of the above-mentioned solvents.
[0081] The method for applying the coating liquid onto the non-thermoplastic polyimide layer is not particularly limited, and an appropriate method can be selected and adopted from among methods generally known as methods for applying a coating liquid onto a substrate.
[0082] In the method (b), the coating layer is heated to form the phenolic resin layer on the surface of the non-thermoplastic polyimide layer, and the laminate is prepared. The precipitated phenolic resin may be at least partially cured. In this case, the heating conditions may be appropriately adjusted so that at least a part of the phenolic resin is cured and / or the solvent is removed from the coating layer, and the heating temperature may be, for example, 30°C to 400°C, preferably 50°C to 350°C, and the heating time may be, for example, 5 minutes to 120 minutes, preferably 10 minutes to 60 minutes.
[0083] The coating liquid is applied to the surface of the non-thermoplastic polyimide layer opposite to the surface on which the uncured phenolic resin layer is laminated, and the phenolic resin layer is formed in the same manner as described above, thereby obtaining a laminate having a structure in which uncured phenolic resin layers are laminated on both sides of the non-thermoplastic polyimide layer.
[0084] In the method (c), the method for separately preparing the uncured phenolic resin layer is not particularly limited, and for example, the following method can be adopted. In the method (a) and the method (b), a different substrate is used instead of the non-thermoplastic polyimide layer, and the phenolic resin layer is laminated on the different substrate to prepare a different laminate. Then, the phenolic resin layer is peeled off from the different substrate in the different laminate to prepare the phenolic resin layer.
[0085] The other substrate is not particularly limited, and for example, a release film, a glass plate, an aluminum foil, an endless stainless steel belt, a stainless steel drum, etc. can be suitably used.
[0086] The method of the thermocompression bonding in the method (c) is not particularly limited as long as the non-thermoplastic polyimide layer and the separately prepared phenolic resin layer are not damaged. As the method of the thermocompression bonding, for example, a method can be adopted in which a laminate formed by laminating the non-thermoplastic polyimide layer and the separately prepared phenolic resin layer is subjected to a pressure of 0.1 kgf to 100 kgf, preferably 1 kgf to 10 kgf from both sides of the laminate while controlling the temperature of the laminate to 50°C to 200°C, preferably 80°C to 120°C.
[0087] In the methods (a), (b) and (c), a gel film, which is a precursor of the non-thermoplastic polyimide layer, can be used in place of the non-thermoplastic polyimide layer.
[0088] The phenolic resin layer in the laminate prepared in the step of preparing the laminate may be incompletely cured. In that case, after the step of preparing the laminate, a step of further heating the phenolic resin layer in the laminate to completely cure the phenolic resin layer (hereinafter referred to as an "additional curing step") may be carried out. The method of further heating the phenolic resin layer in the laminate is not particularly limited, and for example, a method of heating the entire laminate using an oven or the like may be mentioned.
[0089] The method for producing the resin film may appropriately include a step of forming another layer, such as an adhesive layer, in the resin film, as a step other than the step of preparing the laminate and the additional curing step. The method for forming the other layer may be a method appropriately selected from known methods commonly used by those skilled in the art.
[0090] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention.
[0091] That is, one embodiment of the present invention includes the following inventions. <1> A resin film for graphite sheet having a laminated structure in which a phenolic resin layer is laminated on at least one surface of a non-thermoplastic polyimide layer, The resin film for a graphite sheet, wherein the non-thermoplastic polyimide layer has a birefringence of 0.095 or more in a single layer film. <2> the laminated structure is a laminated structure in which the non-thermoplastic polyimide layer and the phenolic resin layer are directly laminated to each other; <1> 2. The resin film for graphite sheet according to claim 1 . <3> The thickness of the phenolic resin layer is greater than 1 μm; <1> or <2> 2. The resin film for graphite sheet according to claim 1 . <4> The thickness of the non-thermoplastic polyimide layer is 5 μm or more. <1> ~ <3> 10. A resin film for a graphite sheet according to any one of the above. <5> a ratio of a thickness of the adjacent phenolic resin layer to a thickness of the non-thermoplastic polyimide layer (thickness of the phenolic resin layer / thickness of the non-thermoplastic polyimide layer) is 0.1 or more and 10.0 or less; <2> ~ <4> 10. A resin film for a graphite sheet according to any one of the above. <6> <1> ~ <5> A graphite sheet comprising, as a raw material, the resin film for graphite sheet according to any one of the above items. <7> Thermal diffusivity is 2.0cm 2 / s or more, <6> Graphite sheet according to claim 1. <8> The thickness is 10 μm or more. <6> or <7> Graphite sheet according to claim 1. <9> Density is 0.9g / cm 3 That's all. <6> ~ <8> 13. The graphite sheet according to any one of claims 1 to 12. <10> <1> ~ <5> 1. A method for producing a graphite sheet, comprising: a step of heat treating the resin film according to any one of the above items at a temperature of 2400° C. or higher. <11> A method for producing a resin film for a graphite sheet, comprising a step of forming a phenolic resin layer on at least one surface of a non-thermoplastic polyimide layer to prepare a laminate, the non-thermoplastic polyimide layer has a birefringence of 0.095 or more in a single layer film. EXAMPLES
[0092] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0093] <Evaluation method> The evaluation methods used in the examples and comparative examples will be described below.
[0094] (Thickness) The thickness of the non-thermoplastic polyimide layer described in Examples 1 to 12 was measured by the following method. In the non-thermoplastic polyimide layer, the thicknesses of four points 7 mm from each of the four corners of the non-thermoplastic polyimide layer along the diagonal line toward the center and one point in the center were measured using a micrometer model MDC-PX (measurement surface diameter φ6.3 mm) manufactured by Mitutoyo Corporation. Here, the "diagonal line" refers to a straight line drawn from each corner of the non-thermoplastic polyimide layer to a corner located diagonally, and there are two of them. In addition, the "center" refers to the position of the intersection of the two diagonal lines. The average value of the thickness measurements obtained at a total of five points was taken as the thickness of the non-thermoplastic polyimide layer. In addition, when the non-thermoplastic polyimide layer to be measured is a rectangle, the corner refers to the vertex of the rectangle.
[0095] In addition, the thickness of the resin film for graphite sheet described in Comparative Example 1, that is, the thickness of the phenol resin layer, was measured by the same method as the method for measuring the thickness of the non-thermoplastic polyimide layer described above.
[0096] Furthermore, the thickness of the resin film for graphite sheet having the structure of non-thermoplastic polyimide layer / phenolic resin layer / non-thermoplastic polyimide layer described in Examples 1 to 7, 10 and 11 was measured by the same method as the method for measuring the thickness of the non-thermoplastic polyimide layer shown above. Then, the thickness of the non-thermoplastic polyimide layer constituting the resin film was subtracted from the thickness of the resin film for graphite sheet, and the difference was calculated. As a result, the calculated difference was taken as the thickness of the phenolic resin layer constituting the resin film for graphite sheet.
[0097] Furthermore, the thicknesses of the resin film for graphite sheet having a structure of phenolic resin layer / non-thermoplastic polyimide layer / phenolic resin layer described in Examples 8 and 9, and the resin film for graphite sheet having a structure of non-thermoplastic polyimide layer / phenolic resin layer / non-thermoplastic polyimide layer / phenolic resin layer / non-thermoplastic polyimide layer described in Example 12 were measured by the same method as the method for measuring the thickness of the non-thermoplastic polyimide layer shown above. Then, the thickness of the non-thermoplastic polyimide layer constituting the resin film was subtracted from the thickness of the resin film for graphite sheet, and the difference was calculated. Here, it was assumed that the thicknesses of the two phenolic resin layers constituting the resin film for graphite sheet were the same, and 1 / 2 of the calculated difference was taken as the thickness of one of the phenolic resin layers.
[0098] Furthermore, the thicknesses of the graphite sheets described in Examples 13 to 24 and Comparative Example 2 were measured by carrying out the same method as the above-described method for measuring the thickness of the non-thermoplastic polyimide layer on measurement samples prepared in the same manner as the method for preparing samples for density measurement described below.
[0099] (Birefringence) The birefringence of the non-thermoplastic polyimide layers used in Examples 1 to 12 was measured by the method described below. The measured birefringence was taken as the "birefringence in a single layer film" for each of the non-thermoplastic polyimide layers described in Examples 1 to 12.
[0100] The birefringence was measured using a Metricon refractive index / thickness measurement system (model number: 2010 Prism Coupler). The measurement was performed in an atmosphere of 23° C. using a light source with a wavelength of 594 nm, measuring the refractive index in each mode in TE mode and TM mode, and calculating the birefringence as "(refractive index in TE mode) - (refractive index in TM mode)".
[0101] (density) The center of each of the graphite sheets described in Examples 13 to 24 and Comparative Example 2 was cut out into a square shape measuring 30 mm in length and 30 mm in width to obtain a sample for density measurement. The volume (unit: cm) of the sample for density measurement was 3 ) was calculated based on the formula: (volume of density measurement sample) = (vertical length of density measurement sample) x (horizontal length of density measurement sample) x (thickness of graphite sheet). Next, the weight (unit: g) of the density measurement sample was measured using a weighing scale (product name: electromagnetic scale, manufacturer: Kensei Kogyo Co., Ltd.). The measured weight of the density measurement sample was divided by the volume of the density measurement sample to obtain the density of the graphite sheet (unit: g / cm 3 Here, the "central portion" refers to a portion of the graphite sheet that is at the center in the width direction and also at the center in the longitudinal direction.
[0102] (Thermal diffusivity) The thermal diffusivity in the planar direction of the graphite sheets was measured by the method described below. Each of the graphite sheets described in Examples 1 to 12 and Comparative Example 1 was cut into a square shape of 30 mm x 30 mm to obtain a sample for thermal diffusivity measurement. Each of the samples for thermal diffusivity measurement was measured using a "Thermowave Analyzer TA3" manufactured by Bethel Corporation under conditions of an atmosphere of 23°C and 10 to 75 Hz to obtain the thermal diffusivity (unit: cm) of each graphite sheet. 2The thermal diffusivity (TDI) was measured by cutting out the central portion of the graphite sheet. The "central portion" refers to the portion of the graphite sheet that is in the center in both the width direction and the length direction.
[0103] (Measurement of thermal decomposition temperature) A comparative graphite sheet resin film (1) made of a phenolic resin layer prepared in Comparative Example 1, a commercially available polyimide film (Kaneka, product name: Apical NPI, thickness 12.5 μm) and a commercially available polyimide film (Kaneka, product name: Apical AH, thickness 12.5 μm) used as a non-thermoplastic polyimide layer in the Examples were weighed and cut out in 10 mg portions to obtain a thermal decomposition temperature measurement sample 1, a thermal decomposition temperature measurement sample 2, and a thermal decomposition temperature measurement sample 3. Each of the thermal decomposition temperature measurement sample 1, the thermal decomposition temperature measurement sample 2, and the thermal decomposition temperature measurement sample 3 was heated under a nitrogen flow (flow rate: 400 mL / min) from 35 to 1000 ° C. at a rate of 10 ° C. / min using a thermal analyzer (Hitachi High-Tech Science (SII), EXSTAR6000 series TG / DTA6300), and the thermal decomposition temperature was measured. As a result, it was found that the thermal decomposition temperature of the phenolic resin constituting the phenolic resin layer was 543°C. In addition, it was found that the thermal decomposition temperature of the polyimide constituting the commercially available polyimide film (manufactured by Kaneka, product name: Apical NPI, thickness 12.5 μm) was 608°C. In addition, it was found that the thermal decomposition temperature of the polyimide constituting the commercially available polyimide film (manufactured by Kaneka, product name: Apical AH, thickness 12.5 μm) was 605°C. The phenolic resin constituting the phenolic resin layer was the same as the phenolic resin constituting the phenolic resin layers in the resin films for graphite sheet (1) to (12) produced in Examples 1 to 12, and the thermal decomposition temperatures were also the same. In the examples, the polyimide film used as the non-thermoplastic polyimide layer was a commercially available polyimide film (manufactured by Kaneka, product name: Apical NPI, thickness 25 μm), and the polyimide constituting the polyimide film was the same as that of the polyimide film (manufactured by Kaneka, product name: Apical NPI, thickness 12.5 μm), and the thermal decomposition temperature was also the same.Furthermore, in the examples, the polyimide film used as the non-thermoplastic polyimide layer was a commercially available polyimide film (manufactured by Kaneka, product name: Apical AH, thickness 25 μm), and the polyimide constituting the polyimide film was the same as that of the polyimide film (manufactured by Kaneka, product name: Apical AH, thickness 12.5 μm), and the thermal decomposition temperature was also the same.
[0104] [Example 1] (Preparation of resin film for graphite sheet) As the non-thermoplastic polyimide layer, a polyimide film with a size of 50 mm square cut out from a commercially available polyimide film (Kaneka, product name: Apical NPI, thickness 12.5 μm) was used. As the phenolic resin, a commercially available phenolic resin (Air Water Bellpearl, product name: Bellpearl (registered trademark) S899) was used. As the polytetrafluoroethylene (PTFE) sheet, a PTFE sheet with a size of 10 cm square cut out from a commercially available PTFE sheet (Nitto Denko, product name: Nitoflon Film No. 900UL, 0.05 mmt) was used. As the stainless steel (SUS) plate, a SUS plate with a thickness of 2 mm and a size of 20 cm square made of SUS304 was used.
[0105] A SUS plate, a PTFE sheet, and a non-thermoplastic polyimide layer were laminated in this order to prepare a laminate A(1) having a configuration of SUS plate / PTFE sheet / non-thermoplastic polyimide layer. 0.1 g of phenolic resin was spread on the surface of the non-thermoplastic polyimide layer in the laminate A(1), and then spread evenly. A non-thermoplastic polyimide layer, a PTFE sheet, and a SUS plate were further laminated in this order on the phenolic resin that had been spread evenly to prepare a laminate B(1) having a configuration of SUS plate / PTFE sheet / non-thermoplastic polyimide layer / phenolic resin / non-thermoplastic polyimide layer / PTFE sheet / SUS plate.
[0106] A pressure was applied from the two SUS plates constituting the outermost surface of the laminate B(1) toward the inside using a compression molding machine AYSR-10 manufactured by Shinto Metal Industries Co., Ltd., and a resin film for graphite sheets was produced by hot pressing. Specifically, the temperature of the two press plates of the compression molding machine AYSR-10 was set to 180°C. Next, the laminate B1 was placed on one of the two press plates of the compression molding machine AYSR-10, and the laminate B1 was heated for one minute to perform preheating. After the preheating, the press plate of the compression molding machine AYSR-10 was moved so that the other press plate of the compression molding machine AYSR-10 and the SUS plate located on the opposite side to the SUS plate in contact with the one press plate in the laminate B(1) were in contact with each other, and a load was applied stepwise in the direction from the two SUS plates constituting the outermost surface of the laminate B(1) toward the inside, thereby applying pressure to the phenolic resin constituting the laminate B(1). At this time, a load was applied to the laminate B(1) so that the magnitude of the applied load was gradually increased. (Hereinafter, this operation is referred to as the "initial pressing operation"). After that, when the magnitude of the applied load reached 255.75 kgf, the magnitude of the load was reduced, and the other press plate was separated from the SUS plate located on the opposite side of the SUS plate in contact with the one press plate in the laminate B(1) (Hereinafter, this operation is referred to as the "releasing operation"). Next, pressing was performed in this order until the load reached 2 / 4, 3 / 4, and 4 / 4 with a set load of 1023 kgf in the same manner as the "initial pressing operation", and a releasing operation was performed each time the pressing was completed. In the last pressing, after the load reached 4 / 4, i.e., the set load, the load was held at the set load for 10 minutes before the releasing operation was performed. In the remaining pressings, the releasing operation was performed when the load reached 2 / 4 or 3 / 4. By the above-mentioned operation, a laminate C(1) was obtained. The laminate C(1) had a structure of the SUS plate / the PTFE sheet / the non-thermoplastic polyimide layer / the partially cured phenolic resin layer / the non-thermoplastic polyimide layer / the PTFE sheet / the SUS plate.
[0107] The obtained laminate C(1) was sandwiched between plates through which cooling water was flowing, cooled to room temperature, and then placed in an oven with an air atmosphere, heated at a heating temperature of 180°C for 60 minutes, and then heated at a heating temperature of 200°C for 60 minutes, to carry out an additional curing step. As a result, the phenolic resin in the phenolic resin layer before curing in the laminate C(1) was completely cured. Next, the SUS plate and the PTFE sheet were peeled off from the laminate C(1) after the additional curing step to obtain a resin film for graphite sheet. The obtained resin film for graphite sheet is referred to as a resin film for graphite sheet (1). The resin film for graphite sheet (1) has a configuration of a non-thermoplastic polyimide layer / phenolic resin layer / non-thermoplastic polyimide layer.
[0108] [Example 2] (Preparation of resin film for graphite sheet) A resin film for graphite sheet was produced in the same manner as in Example 1, except that the amount of the phenolic resin used was changed from 0.1 g to 0.2 g. The resin film for graphite sheet produced is referred to as resin film for graphite sheet (2).
[0109] [Example 3] (Preparation of resin film for graphite sheet) A resin film for graphite sheet was produced in the same manner as in Example 1, except that the amount of the phenolic resin used was changed from 0.1 g to 0.5 g. The resin film for graphite sheet produced is referred to as resin film for graphite sheet (3). Resin film for graphite sheet (3) has a configuration of non-thermoplastic polyimide layer / phenolic resin layer / non-thermoplastic polyimide layer.
[0110] [Example 4] (Preparation of resin film for graphite sheet) A resin film for graphite sheet was produced in the same manner as in Example 1, except that the amount of the phenolic resin used was changed from 0.1 g to 1.0 g. The resin film for graphite sheet produced is referred to as resin film for graphite sheet (4). Resin film for graphite sheet (4) has a configuration of non-thermoplastic polyimide layer / phenolic resin layer / non-thermoplastic polyimide layer.
[0111] [Example 5] (Preparation of resin film for graphite sheet) A resin film for graphite sheet was produced in the same manner as in Example 2, except that a commercially available polyimide film (manufactured by Kaneka, product name: Apical AH, thickness 12.5 μm) was used as the non-thermoplastic polyimide layer instead of a commercially available polyimide film (manufactured by Kaneka, product name: Apical NPI, thickness 12.5 μm). The produced resin film for graphite sheet is referred to as resin film for graphite sheet (5). Resin film for graphite sheet (5) has a configuration of non-thermoplastic polyimide layer / phenolic resin layer / non-thermoplastic polyimide layer.
[0112] [Example 6] (Preparation of resin film for graphite sheet) A resin film for graphite sheet was produced in the same manner as in Example 2, except that a commercially available polyimide film (manufactured by Kaneka, product name: Apical NPI, thickness 25 μm) was used as the non-thermoplastic polyimide layer instead of a commercially available polyimide film (manufactured by Kaneka, product name: Apical NPI, thickness 12.5 μm). The produced resin film for graphite sheet is referred to as resin film for graphite sheet (6). Resin film for graphite sheet (6) has a configuration of non-thermoplastic polyimide layer / phenolic resin layer / non-thermoplastic polyimide layer.
[0113] [Example 7] (Preparation of resin film for graphite sheet) A resin film for graphite sheet was produced in the same manner as in Example 2, except that a commercially available polyimide film (manufactured by Kaneka, product name: Apical AH, thickness 25 μm) was used as the non-thermoplastic polyimide layer instead of a commercially available polyimide film (manufactured by Kaneka, product name: Apical NPI, thickness 12.5 μm). The produced resin film for graphite sheet is referred to as resin film for graphite sheet (7). Resin film for graphite sheet (7) has a configuration of non-thermoplastic polyimide layer / phenolic resin layer / non-thermoplastic polyimide layer.
[0114] [Example 8] (Preparation of resin film for graphite sheet) A laminate A(1) having a structure of SUS plate / PTFE sheet / non-thermoplastic polyimide layer was prepared by the same method as in Example 1. 0.2 g of phenolic resin was sprayed on the surface of the non-thermoplastic polyimide layer in the laminate 1, and then spread evenly. A PTFE sheet and a SUS plate were further laminated in this order on the phenolic resin that had been spread evenly, to prepare a laminate B(8') having a structure of SUS plate / PTFE sheet / non-thermoplastic polyimide layer / phenolic resin / PTFE sheet / SUS plate.
[0115] Except for using the laminate B (8') instead of the laminate B (1), the heat pressing was carried out in the same manner as in Example 1 to produce a resin film (8'). The resin film (8') has a structure of a non-thermoplastic polyimide layer / phenolic resin layer.
[0116] Next, a resin film for graphite sheet was produced by carrying out the heat pressing and additional curing steps in the same manner as in Example 1, except that a resin film (8') was used instead of the non-thermoplastic polyimide layer, and a phenolic resin was sprayed on the surface of the non-thermoplastic polyimide layer in the resin film (8') opposite to the surface on which the phenolic resin layer was laminated. The resin film for graphite sheet produced is referred to as resin film for graphite sheet (8). Resin film for graphite sheet (8) has a configuration of phenolic resin layer / non-thermoplastic polyimide layer / phenolic resin layer.
[0117] [Example 9] (Preparation of resin film for graphite sheet) A resin film for graphite sheet was produced in the same manner as in Example 8, except that a commercially available polyimide film (manufactured by Kaneka, product name: Apical AH, thickness 25 μm) was used as the non-thermoplastic polyimide layer instead of a commercially available polyimide film (manufactured by Kaneka, product name: Apical NPI, thickness 12.5 μm). The produced resin film for graphite sheet is referred to as resin film for graphite sheet (9). Resin film for graphite sheet (9) has a configuration of a phenolic resin layer / non-thermoplastic polyimide layer / phenolic resin layer.
[0118] [Example 10] (Preparation of resin film for graphite sheet) A resin film for graphite sheet was produced in the same manner as in Example 1, except that the amount of the phenolic resin used was changed from 0.1 g to 0.2 g. The resin film for graphite sheet produced is referred to as resin film for graphite sheet (10). Resin film for graphite sheet (10) has a configuration of a non-thermoplastic polyimide layer / phenolic resin layer / non-thermoplastic polyimide layer.
[0119] [Example 11] (Preparation of resin film for graphite sheet) A resin film for graphite sheet was produced in the same manner as in Example 5, except that the amount of the phenolic resin used was changed from 0.1 g to 0.2 g. The produced resin film for graphite sheet is referred to as resin film for graphite sheet (11). Resin film for graphite sheet (11) has a configuration of non-thermoplastic polyimide layer / phenolic resin layer / non-thermoplastic polyimide layer.
[0120] [Example 12] (Preparation of resin film for graphite sheet) Except for changing the amount of the phenolic resin used from 0.1 g to 0.2 g, heat pressing was performed in the same manner as in Example 1 to produce a resin film (12'). The resin film (12') has a structure of a non-thermoplastic polyimide layer / phenolic resin layer / non-thermoplastic polyimide layer.
[0121] Next, a resin film for graphite sheet was produced in the same manner as that for producing the resin film (12'), except that a resin film (12') was used instead of one of the non-thermoplastic polyimide layers, and a phenolic resin was sprayed on the surface of the resin film (12') opposite to the surface on which the phenolic resin layer was laminated of one of the non-thermoplastic polyimide layers. In detail, a laminate D (12) having a configuration of SUS plate / PTFE sheet / non-thermoplastic polyimide layer / phenolic resin layer / non-thermoplastic polyimide layer / phenolic resin / non-thermoplastic polyimide layer / PTFE sheet / SUS plate was prepared, and the laminate D (12) was subjected to a heat press and additional curing process in the same manner as in Example 1 to produce a resin film for graphite sheet. The non-thermoplastic polyimide layer / phenolic resin layer / non-thermoplastic polyimide layer portion of the laminate D (12) is the resin film (12'). The produced resin film for graphite sheet is referred to as a resin film for graphite sheet (12). The resin film for graphite sheet (12) has a structure of non-thermoplastic polyimide layer / phenolic resin layer / non-thermoplastic polyimide layer / phenolic resin layer / non-thermoplastic polyimide layer.
[0122] [Comparative Example 1] (Preparation of resin film for graphite sheet) A resin film for graphite sheet was produced in the same manner as in Example 1, except that a non-thermoplastic polyimide layer was not used and the amount of phenolic resin used was changed from 0.1 g to 0.2 g. The resin film for graphite sheet produced is referred to as comparative resin film for graphite sheet (1). Comparative resin film for graphite sheet (1) has a configuration consisting of only a phenolic resin layer.
[0123] [Examples 13 to 24, Comparative Example 2] (Preparation of graphite sheets) The following operations were carried out on each of the resin films for graphite sheet (1) to (12) produced in Examples 1 to 12 and Comparative Example 1, and the comparative resin film for graphite sheet (1). The resin film for graphite sheet was sandwiched between graphite sheets (Perma-Foil PF, manufactured by Toyo Tanso) with a size of 60 mm x 60 mm and a thickness of 200 μm to obtain a laminated sheet. At this time, the resin film for graphite sheet and the graphite sheets were laminated one by one alternately. The obtained laminated sheet was heated to 1000°C in a nitrogen atmosphere and heat-treated to be carbonized. After that, the carbonized laminated sheet was heated to 2900°C and heat-treated to produce a graphitized resin film for graphite sheet, i.e., a graphite sheet.
[0124] The graphite sheets thus produced were designated graphite sheets (1) to (12) and comparative graphite sheet (1), respectively.
[0125] [result] The birefringence of the non-thermoplastic polyimide layers used in Examples 1 to 12 was measured by the above-mentioned method, and the results are shown in Table 1 below.
[0126] [Table 1]
[0127] As shown in Table 1, the birefringence of the non-thermoplastic polyimide layers used in Examples 1 to 12 was 0.095 or more. As described above, the resin films for graphite sheet (1) to (12) produced in Examples 1 to 12 had a laminate structure in which a phenol resin layer was laminated on at least one surface of the non-thermoplastic polyimide layer. Thus, the resin films for graphite sheet (1) to (12) are resin films for graphite sheet according to one embodiment of the present invention.
[0128] The layer structures of the resin films for graphite sheet (1) to (12) and the comparative resin film for graphite sheet (1) produced in Examples 1 to 12 and Comparative Example 1, as well as the thicknesses of the non-thermoplastic polyimide layer and the phenolic resin layer, are shown in Table 2 below. In Table 2, "NPI" represents a commercially available polyimide film (manufactured by Kaneka, product name: Apical NPI) as the non-thermoplastic polyimide layer, "AH" represents a commercially available polyimide film (manufactured by Kaneka, product name: Apical A) as the non-thermoplastic polyimide layer, and "PF" represents a phenolic resin layer. When the resin films for graphite sheet (1) to (12) have two non-thermoplastic polyimide layers and / or two phenolic resin layers, the thicknesses of the respective non-thermoplastic polyimide layers are all the same, and the thicknesses of the respective phenolic resin layers are considered to be the same, and the film thickness of one non-thermoplastic polyimide layer and / or one phenolic resin layer was calculated.
[0129] Furthermore, the ratio of (phenolic resin layer thickness / non-thermoplastic polyimide layer thickness) in each of the resin films for graphite sheet (1) to (12) was calculated, and the values are shown in the following Table 2. Note that when each of the resin films for graphite sheet (1) to (12) had two phenolic resin layers, the calculated ratio for each of the phenolic resin layers was the same.
[0130] [Table 2]
[0131] The physical properties of the graphite sheets (1) to (12) produced in Examples 13 to 24 and Comparative Example 2, and the comparative graphite sheet (1) were measured by the above-mentioned methods. The results are shown in Table 3 below.
[0132] [Table 3]
[0133] As shown in Table 3, comparative graphite sheet (1) produced in Comparative Example 2 using resin film (1) for comparative graphite sheet consisting only of a phenolic resin layer as its raw material has a very low thermal diffusivity. On the other hand, graphite sheets (1) to (12) produced in Examples 13 to 24 have high thermal diffusivities, despite being made from resin films for graphite sheet (1) to (12) containing a phenolic resin layer as their raw material. In addition, a phenolic resin layer is known to have a lower production cost than a non-thermoplastic polyimide layer.
[0134] From the above, it has been found that by using the resin film for graphite sheet according to one embodiment of the present invention as a raw material, it is possible to provide a graphite sheet that has excellent thermal diffusivity and low production costs. [Industrial Applicability]
[0135] INDUSTRIAL APPLICABILITY The resin film for graphite sheet according to one embodiment of the present invention has excellent thermal diffusivity and can be used to produce a graphite sheet at low production costs. [Explanation of symbols]
[0136] 1 Press plate 2 Stainless steel (SUS) plate 3 Non-thermoplastic polyimide layer 3' Another non-thermoplastic polyimide layer 4. Phenolic resin particles 5 Protective film 6 cylinders
Claims
1. A resin film for graphite sheet having a laminated structure in which a phenolic resin layer is laminated on at least one surface of a non-thermoplastic polyimide layer, The resin film for a graphite sheet, wherein the non-thermoplastic polyimide layer has a birefringence of 0.095 or more in a single layer film.
2. 2. The resin film for graphite sheet according to claim 1, wherein the laminate structure is a laminate structure in which the non-thermoplastic polyimide layer and the phenolic resin layer are directly laminated together.
3. 2. The resin film for graphite sheet according to claim 1, wherein the phenolic resin layer has a thickness of more than 1 μm.
4. 2. The resin film for graphite sheet according to claim 1, wherein the non-thermoplastic polyimide layer has a thickness of 5 μm or more.
5. 3. The resin film for graphite sheet according to claim 2, wherein a ratio of a thickness of the adjacent phenolic resin layer to a thickness of the non-thermoplastic polyimide layer (thickness of the phenolic resin layer / thickness of the non-thermoplastic polyimide layer) is 0.1 or more and 10.0 or less.
6. A graphite sheet comprising the resin film for graphite sheet according to any one of claims 1 to 5 as a raw material.
7. Thermal diffusivity is 2.0 cm 2 7. The graphite sheet according to claim 6, wherein the tensile strength is 1 / s or more.
8. 7. The graphite sheet according to claim 6, having a thickness of 10 μm or more.
9. Density is 0.9g / cm 3 The graphite sheet according to claim 6 .
10. A method for producing a graphite sheet, comprising a step of heat-treating the resin film for a graphite sheet according to any one of claims 1 to 5 at a temperature of 2400°C or higher.
11. A method for producing a resin film for a graphite sheet, comprising a step of forming a phenolic resin layer on at least one surface of a non-thermoplastic polyimide layer to prepare a laminate, the non-thermoplastic polyimide layer has a birefringence of 0.095 or more in a single layer film.
Citation Information
Patent Citations
Laminated film
JP2017114098A
Multilayer polyimide film for graphite sheet, its manufacturing method, and graphite sheet manufactured from the same
JP2022512190A