Resin film for graphite sheet, graphite sheet, and production method of graphite sheet
A laminated resin film with controlled holes in a non-thermoplastic polyimide layer and resin layers addresses non-uniform curing and gas retention issues, enhancing the reliability and productivity of thick graphite sheets by preventing peeling and ensuring efficient heat dissipation.
Patent Information
- Application Number
- JP2023059457
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for manufacturing thick graphite sheets face challenges such as non-uniform curing, internal gas residue leading to brittleness, and localized gas retention causing peeling between layers, which compromises the reliability of graphite sheets as heat dissipation members.
A laminated resin film with a non-thermoplastic polyimide layer and one or more resin layers, featuring predetermined holes on one side to distribute gas generated during thermal decomposition, preventing localized residue and peeling between graphite layers.
The resin film effectively prevents peeling between graphite layers by distributing gas throughout the sheet, ensuring high thermal diffusivity and productivity in producing reliable graphite sheets.
Smart Images

Figure 2024146507000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin film for a graphite sheet, a graphite sheet, and a method for producing a graphite sheet. [Background technology]
[0002] Graphite sheets have excellent thermal conductivity and are therefore used as heat dissipation members in various electronic devices such as computers, semiconductor elements mounted in electrical devices, and other heat-generating parts.
[0003] As a method for producing such a graphite sheet, a method is known in which a polyimide film is subjected to a heat treatment in an inert gas at a high temperature of, for example, 2400° C. or higher to carbonize and graphitize the polyimide constituting the polyimide film, and then, optionally, a rolling treatment is performed.
[0004] In recent years, there has been an increasing demand for thick graphite sheets, which are advantageous in terms of heat transport. In order to manufacture such graphite sheets, a method of heat treating a thick polyimide film is usually adopted. However, in the manufacture of thick polyimide films, there is a problem that it is difficult to uniformly harden the inside and outside of the polyimide film. In addition, in the manufacture of graphite sheets by the above method, there is a problem that gas generated by thermal decomposition of polyimide remains inside the graphite sheet to be manufactured, making the graphite sheet brittle.
[0005] As a technique for solving the problems in the graphite sheet production by the above-mentioned method, a graphite sheet production method is known that includes the steps of impregnating a hollow-formed sheet made of a material that loses 80% or more of its weight by firing during graphite sheet production with polyamic acid to form a sheet, imidizing the polyamic acid to produce a polyimide sheet, and firing the polyimide sheet to produce a graphite sheet (Patent Document 1). However, the production method described in Patent Document 1 does not solve the above-mentioned problems in producing a polyimide film with a large thickness.
[0006] On the other hand, another method for producing a thick graphite sheet is known, for example, which uses a laminated polyimide film formed by laminating two or more polyimide films as a raw material (see Patent Documents 2 and 3, etc.). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. 2013 / 140724 Brochure [Patent Document 2] JP 2017-114098 A [Patent Document 3] Special Publication No. 2022-512190 Summary of the Invention [Problem to be solved by the invention]
[0008] However, in the graphite sheet made from the above-mentioned laminated polyimide film, gas generated by thermal decomposition of polyimide may remain locally at the interface between the graphite layers derived from each polyimide layer. As a result, peeling may occur between the graphite layers in the obtained graphite sheet. As a result, the reliability of the graphite sheet when used as a heat dissipation member may decrease, and improvement was required.
[0009] An object of the present invention is to provide a graphite sheet in which peeling between graphite layers is prevented, and a resin film for graphite sheet which is a raw material for the graphite sheet and has excellent productivity. [Means for solving the problem]
[0010] As a result of intensive investigations to solve the above-mentioned problems, the present inventors have found that when a graphite sheet is produced using as a raw material a laminate resin film formed by laminating a plurality of resin layers including a non-thermoplastic polyimide layer, in which at least one resin layer has one or more holes with openings on one side forming an interface with other layers, the laminate resin film has a predetermined amount of holes. This hole has been found to be effective in preventing gas generated by thermal decomposition of a resin contained in a resin layer from remaining locally at the interface between the graphite layers derived from each of the resin layers, and as a result, peeling between the graphite layers can be prevented, which has led to the completion of the present invention.
[0011] That is, one embodiment of the present invention relates to a resin film for graphite sheet having a multilayer structure in which a non-thermoplastic polyimide layer and one or more resin layers are laminated, wherein at least one of the non-thermoplastic polyimide layer and the one or more resin layers has one or more holes formed therein, the one or more holes having openings on one side forming an interface between the layer in which the one or more holes are formed and another layer, and the ratio of a total area of the openings to an area of the one side having the openings, of the layer in which the one or more holes are formed, is 0.05% to 5%. Regarding. Effect of the Invention
[0012] ADVANTAGEOUS EFFECTS OF THE PRESENT EMBODIMENT The resin film for graphite sheet according to one embodiment of the present invention can provide a graphite sheet in which peeling between graphite layers is prevented, and has excellent productivity. [Brief description of the drawings]
[0013] [Figure 1] FIG. 2 is a schematic diagram showing a pore structure in an example of a resin film for a graphite sheet according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram illustrating an example of a method for preparing a laminate using a press in a method for producing a resin film for a graphite sheet according to one embodiment of the present invention. [Diagram 3] 1 is a micrograph showing a cross section in a thickness direction of a graphite sheet produced in Example 1 of the present invention. [Figure 4] 1 is a photomicrograph showing a cross section in a thickness direction of a graphite sheet produced in Comparative Example 3 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] An embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to each configuration described below, and various modifications are possible within the scope of the claims, and embodiments and examples obtained by appropriately combining the technical means disclosed in different embodiments and examples are also included in the technical scope of the present invention. In addition, all academic literature and patent documents described in this specification are incorporated herein by reference. In addition, unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more and B or less."
[0015] <1. Technical idea of the present invention> As described above, the present inventors conducted intensive studies to solve the above problems, and as a result, they found that when a graphite sheet was produced using as a raw material a laminate resin film formed by laminating a plurality of resin layers including a non-thermoplastic polyimide layer, in which at least one resin layer has one or more holes with openings on one side forming an interface with the other layers, the gas generated by thermal decomposition of the resin contained in the resin layer can be prevented from remaining locally at the interface between the graphite layers derived from each resin layer, and as a result, peeling between the graphite layers can be prevented.
[0016] This is believed to be due to the following action. When the resin film for graphite sheet according to one embodiment of the present invention is carbonized and graphitized, the resin contained in the resin layer is thermally decomposed, generating gas. The resin film for graphite sheet according to one embodiment of the present invention has a multilayer structure, and in at least one layer constituting the layer structure, one or more holes having openings with a ratio of a total area to an area of one side within a range of 0.05% to 5% are formed on one side forming an interface between the other layers. As a result, the gas does not remain locally at the interface, but is dispersed throughout the graphite sheet through the one or more holes. Therefore, in the resin film for graphite sheet according to one embodiment of the present invention, peeling between graphite layers caused by the gas remaining locally at the interface is prevented. As a result, the resin film for graphite sheet according to one embodiment of the present invention has an effect of being usable for producing a graphite sheet in which peeling between graphite layers is prevented.
[0017] In addition, in the resin film for graphite sheet according to one embodiment of the present invention, it is more preferable that the one or more holes communicate with one surface of the resin film for graphite sheet, and it is even more preferable that the one or more holes communicate with both surfaces. When the one or more holes communicate with at least one surface of the resin film for graphite sheet, the gas can be directly discharged to the outside through the one or more holes, and it is more preferable that the gas does not remain locally at the interface. In addition, it is particularly preferable that the one or more holes penetrate from one surface to the other surface of the resin film for graphite sheet. In that case, the gas can be more preferably discharged to the outside from all interfaces in the resin film for graphite sheet through the one or more holes, and it is more preferable that the gas does not remain locally at all interfaces.
[0018] <2. Resin film for graphite sheets> Hereinafter, a resin film for graphite sheet according to one embodiment of the present invention (hereinafter, sometimes referred to as the present resin film) will be described in detail. The present resin film is a resin film for graphite sheet having a multilayer structure in which a non-thermoplastic polyimide layer and one or more resin layers are laminated, in which at least one layer of the non-thermoplastic polyimide layer and the one or more resin layers has one or more holes formed therein, the one or more holes have openings on one side forming an interface between the layer in which the one or more holes are formed and another layer, and the ratio of the total area of the openings to the area of the one side having the openings of the layer in which the one or more holes are formed is 0.05% to 5%.
[0019] As described above, the present resin film can suppress the gas generated during production of the graphite sheet from remaining locally at the interface between the graphite layers derived from each resin layer of the present resin film, thereby preventing delamination between the graphite layers due to such localized remainder.
[0020] <2.1. Non-thermoplastic polyimide layer> (Birefringence) From the viewpoint of producing a graphite sheet having excellent thermal diffusivity, the non-thermoplastic polyimide layer constituting the present resin film preferably has a birefringence of 0.1 or more in a monolayer film. Usually, the birefringence may be 0.2 or less, and is preferably 0.16 or less. Here, the "birefringence in a monolayer film" means the birefringence of the monolayer when the non-thermoplastic polyimide layer is formed as a monolayer, and can be determined, for example, by measuring the birefringence of the non-thermoplastic polyimide layer before laminating the one or more resin layers.
[0021] Since the orientation of the non-thermoplastic polyimide layer does not change even when the one or more resin layers are laminated thereon, the birefringence of the non-thermoplastic polyimide layer does not change substantially. Therefore, in the present resin film having a multilayer structure, the "birefringence in a single layer film" of the non-thermoplastic polyimide layer can be determined, for example, by removing the one or more resin layers from the present resin film and then measuring the birefringence of the remaining non-thermoplastic polyimide layer.
[0022] In one embodiment of the present invention, the birefringence can be measured by the method described in JIS K0062: 1992. Specifically, the birefringence can be measured using a commercially available refractive index measuring device.
[0023] (Composition of Non-Thermoplastic Polyimide Layer) The composition of the non-thermoplastic polyimide layer is not particularly limited as long as it is a layer containing a non-thermoplastic polyimide. The non-thermoplastic polyimide layer preferably contains a non-thermoplastic polyimide containing an acid dianhydride component and a diamine component as main raw materials.
[0024] (Acid dianhydride component) The acid dianhydride component is not particularly limited. The acid dianhydride component preferably contains 50 mol% or more of pyromellitic dianhydride (hereinafter also referred to as "PMDA") in the total amount of the acid dianhydride component (100 mol%). The amount of PMDA contained in the acid dianhydride component is preferably 50 mol% or more, more preferably 70 mol% or more, and even more preferably 90 mol% or more, based on the total amount of the acid dianhydride component (100 mol%), from the viewpoint of being able to provide the non-thermoplastic polyimide layer having appropriate orientation and birefringence. The amount of PMDA contained in the acid dianhydride component may be 95 mol% or more, or may be 100 mol%.
[0025] The non-thermoplastic polyimide may contain an acid dianhydride other than the PMDA as the acid dianhydride component. Examples of the other acid dianhydrides include 3,3',4,4'-benzophenonetetracarboxylic dianhydride (hereinafter referred to as "BTDA"), 4,4'-oxydiphthalic dianhydride (hereinafter referred to as "ODPA"), naphthalenetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, 1,1-(dicarboxyphenyl)ethane dianhydride, bis(dicarboxyphenyl)methane dianhydride, bis(3,4-dicarboxyphenyl)sulfone dianhydride, p-phenylene bis(trimellitic acid monoester dianhydride), ethylene bis(trimellitic acid monoester dianhydride), bisphenol A bis(trimellitic acid monoester dianhydride), and the like. As the other acid dianhydrides, these acid dianhydrides may be used alone, or a plurality of these acid dianhydrides may be mixed in any ratio.
[0026] The content of the other acid dianhydrides in the acid dianhydride component that is the raw material of the non-thermoplastic polyimide can be 50 mol % or less, preferably 30 mol % or less, and more preferably 10 mol % or less, in 100 mol % of the total amount of the acid dianhydride components.
[0027] (Diamine component) The diamine component, which is a raw material of the non-thermoplastic polyimide, preferably contains 50 mol % or more of 4,4'-diaminodiphenyl ether (hereinafter, referred to as "ODA").
[0028] In one embodiment of the present invention, from the viewpoint of providing the non-thermoplastic polyimide layer having appropriate orientation and birefringence, the amount of ODA contained in the diamine component is preferably 50 mol% or more, more preferably 60 mol% or more, and even more preferably 70 mol% or more, based on 100 mol% of the total amount of the diamine component. The amount of ODA contained in the diamine component may be 80 mol% or more, 90 mol% or more, 95 mol% or more, or even 100 mol%.
[0029] In particular, it is preferable that the diamine component contains 50 mol % or more of ODA and the acid dianhydride component contains 50 mol % or more of PMDA. With this configuration, the orientation and birefringence of the non-thermoplastic polyimide layer are improved, and as a result, the thermal diffusivity of the finally obtained graphite sheet is improved.
[0030] The non-thermoplastic polyimide may contain other diamines as the diamine component other than the ODA. Examples of the other diamines include 2,2-bis[4-(4-aminophenoxy)phenyl]propane (hereinafter referred to as "BAPP"), p-phenylenediamine (PDA), 4,4'-diaminodiphenylmethane, benzidine, 3,3'-dichlorobenzidine, 4,4'-diaminodiphenyl sulfide, diaminodiphenyl sulfone, diaminodiphenyl ether, 1,5-diaminonaphthalene, 4,4'-diaminodiphenyl diethyl silane, 4,4'-diaminodiphenyl silane, 4,4'-diaminodiphenyl ethyl phosphine oxide, 4,4'-diaminodiphenyl N-methylamine, 4,4'-diaminodiphenyl N-phenylamine, 1,3-diaminobenzene, and the like. As the other diamines, these diamines may be used alone, or a plurality of these diamines may be used in any ratio.
[0031] The content of the other diamine in the diamine component that is the raw material of the non-thermoplastic polyimide can be 50 mol % or less, preferably 30 mol % or less, and more preferably 10 mol % or less, in 100 mol % of the total amount of the diamine component.
[0032] The non-thermoplastic polyimide is a non-thermoplastic polyimide made from substantially equimolar amounts of the acid dianhydride component and the diamine component. In this specification, the term "substantially equimolar amounts" means that the molar ratio of two or more different substances (e.g., the acid dianhydride component and the diamine component) is within the range of 100:98 to 100:102, and preferably 100:100.
[0033] (Physical properties of non-thermoplastic polyimide layer) The thickness of the non-thermoplastic polyimide layer is preferably 5 μm or more, more preferably 12 μm or more, and by having the thickness of the non-thermoplastic polyimide layer be 5 μm or more, a graphite sheet having a large thickness and excellent heat transport properties can be suitably produced, and a thick present resin film can be more easily obtained.
[0034] If the thickness of the non-thermoplastic polyimide layer is too large, problems such as a decrease in productivity of the non-thermoplastic polyimide layer and an increase in cost may occur, etc. Therefore, the thickness of the non-thermoplastic polyimide layer is preferably 75 μm or less, and more preferably 50 μm or less.
[0035] <2.2. Resin layer> (Composition of resin layer) The resin layer constituting the present resin film is not particularly limited as long as it is a layer containing a resin that changes to graphite by carbonization and graphitization. The resin layer may contain one type of resin, or may contain two or more types of resin. The resin may be a non-thermoplastic polyimide, and the resin layer may be a non-thermoplastic polyimide layer other than the non-thermoplastic polyimide layer described above. The non-thermoplastic polyimide contained in the non-thermoplastic polyimide layer and the non-thermoplastic polyimide contained in the other non-thermoplastic polyimide layer may be the same non-thermoplastic polyimide or different non-thermoplastic polyimides. In addition, the preferred physical properties of the other non-thermoplastic polyimide layer may be those described in the above section <2.1. Non-thermoplastic polyimide layer>.
[0036] The resin may be a resin other than non-thermoplastic polyimide. Hereinafter, the "resin other than non-thermoplastic polyimide" is referred to as a "different resin." Specific examples of the different resin include polyacrylonitrile, polyvinyl chloride, and phenol resin.
[0037] When the resin layer is a layer containing different resins, the resin layer may contain one type of different resin, or may contain two or more types of different resins. When the different resin contained in the different resin layer constituting the present resin film is a thermosetting resin, it may be in a cured state, a partially cured state, or an uncured state.
[0038] The content of the heterogeneous resin in the heterogeneous resin layer is preferably 50% by weight or more, more preferably 70% by weight or more, and even more preferably 90% by weight or more, based on the total weight of the heterogeneous resin layer. When the heterogeneous resin layer contains two or more types of heterogeneous resin, the total content of each of the heterogeneous resins is the content of the heterogeneous resin in the heterogeneous resin layer.
[0039] As an example of the different resins, a phenolic resin will be described in detail below. Here, the phenolic resin refers to a polymer obtained by polymerizing a phenol and an aldehyde compound.
[0040] The phenols that are monomers constituting the phenol-based resin are not particularly limited, and examples thereof include phenol and cresol.
[0041] The aldehyde compound, which is a monomer constituting the phenol-based resin, is not particularly limited, and examples thereof include formaldehyde, glutaraldehyde, and the like.
[0042] Phenolic resins are generally classified into novolac resins and resol resins, but both novolac resins and resol resins can be used. In addition, other phenolic resins different from novolac resins and resol resins can also be used. Specific examples of the novolac resins include Phenolite (manufactured by DIC Corporation). Specific examples of the resol resins include Sumilite Resin (manufactured by Sumitomo Bakelite Co., Ltd.). Specific examples of the other phenolic resins include Bellpearl (registered trademark) (manufactured by Air Water Bellpearl Co., Ltd.).
[0043] The resin layer may contain additives such as an organic phosphorus compound and inorganic particles, as long as the object of the present invention is not impaired.
[0044] (Physical properties of different resin layers) The thickness of the heterogeneous resin layer is preferably 75 μm or less, and more preferably 50 μm or less. In general, the graphite layer formed by carbonizing and graphitizing the heterogeneous resin layer has a lower thermal diffusivity than the graphite layer formed by carbonizing and graphitizing the non-thermoplastic polyimide layer. Therefore, if the thickness of the heterogeneous resin layer is excessively large, the proportion of the heterogeneous resin layer in the resin film increases, and the thermal diffusivity of the resulting graphite sheet may decrease.
[0045] The thickness of the heterogeneous resin layer is preferably more than 1 μm, and more preferably 10 μm or more. When the thickness of the heterogeneous resin layer is more than 1 μm, a thick graphite sheet having excellent heat transport properties can be suitably produced.
[0046] <2.3. Structure of this resin film> The resin film of the present invention may have a multilayer structure (lamination structure) in which the non-thermoplastic polyimide layer and one or more resin layers are laminated, and the laminate structure is not particularly limited. The multilayer structure in the resin film of the present invention is preferably a laminate structure in which the non-thermoplastic polyimide layer and one of the one or more resin layers are directly laminated without the presence of other layers such as an adhesive layer having a high thermal resistance.
[0047] The multilayer structure is a two-layer structure consisting of at least the non-thermoplastic polyimide layer and the resin layer, and may be a three-layer structure or a four-layer structure. When the multilayer structure is composed of a plurality of non-thermoplastic polyimide layers and / or a plurality of resin layers, the non-thermoplastic polyimide layers and / or the one resin layer constituting the multilayer structure may be the same or different.
[0048] In the present resin film, at least one of the non-thermoplastic polyimide layer and the one or more resin layers has one or more holes formed on one side forming an interface with another layer, the holes having openings whose ratio of the total area to the area of the one side is within a range of 0.05% to 5%. Here, the total area of the openings refers to the total area of the openings on one side of the layer in which the one or more holes are formed, which forms the interface with the other layer and has the openings.
[0049] In the present resin film, the one or more holes are holes having an opening on one side that forms an interface between the layer in which the one or more holes are formed and another layer. The presence of the one or more holes allows gas generated during the preparation of the graphite sheet to disperse throughout the graphite sheet through the one or more holes. Thus, the present resin film prevents peeling between the graphite layers caused by the gas remaining locally at the interface between the graphite layers derived from the respective resin layers, and a graphite sheet in which peeling between the graphite layers is prevented can be obtained.
[0050] In the present resin film, it is more preferable that the one or more holes communicate with one surface of the resin film for graphite sheet, and even more preferable that the one or more holes communicate with both surfaces. When the one or more holes communicate with at least one surface of the resin film for graphite sheet, the gas can be directly discharged to the outside through the one or more holes, and the gas can be more preferably prevented from remaining locally at the interface. In addition, it is particularly preferable that the one or more holes penetrate from one surface to the other surface of the resin film for graphite sheet. In that case, the gas can be more preferably discharged to the outside from all interfaces in the resin film for graphite sheet through the one or more holes, and the gas can be more preferably prevented from remaining locally at all interfaces.
[0051] The lower limit of the ratio of the total area of the openings to the area of one side of the layer in which the one or more holes are formed that forms the interface with another layer and that has the openings is not less than 0.05%, more preferably not less than 0.1%, and even more preferably not less than 0.2%. When the total area of the openings is not less than the aforementioned lower limit, the gas is dispersed throughout the graphite sheet through the one or more holes, and as a result, the resin film can more effectively prevent peeling between graphite layers in the resulting graphite sheet.
[0052] If the total area of the openings is excessively large, the thermal diffusivity of the graphite sheet obtained from the resin film decreases. Also, the total volume of the holes increases, the strength of the graphite sheet decreases, and the reliability of the graphite sheet when used as a heat dissipation member decreases. Therefore, the upper limit of the ratio of the total area of the openings to the area of one side of the layer in which the one or more holes are formed, which forms the interface with another layer and has the openings, is 5% or less, more preferably 3% or less, and even more preferably 1% or less.
[0053] When the diameter of the one or more pores is larger, the gas is more suitably dispersed throughout the graphite sheet through the one or more pores. From the above viewpoint, the lower limit of the diameter of the one or more pores is preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 30 μm or more.
[0054] On the other hand, if the size of the one or more pores is excessively large, the graphite sheet will have problems of reduced thermal diffusivity and reduced strength, as described above. Therefore, the diameter of the one or more pores is preferably 200 μm or less, more preferably 150 μm or less, and even more preferably 100 μm or less.
[0055] When the one or more holes are uniformly distributed over the entire surface of the layer in which the one or more holes are formed, which surface includes the opening, the gas is more suitably dispersed over the entire graphite sheet through the one or more holes. From the same viewpoint, the number of the one or more holes per unit area on the surface of the layer in which the one or more holes are formed, which surface includes the opening, is preferably 1 / 9 holes / mm 2 More preferably, it is 1 / 4 (=0.25) pieces / mm 2 More preferably, 1 / mm 2 From the same viewpoint, in the surface of the layer in which the one or more holes are formed and which has the opening, the one or more holes are preferably a plurality of holes, and all of the plurality of holes are preferably formed at a pitch of 3 mm or less, more preferably 2 mm or less, and further preferably 1 mm or less. The pitch means the distance between the center of one hole of the plurality of holes and the center of another hole that is closest to the one hole.
[0056] Furthermore, when the one or more holes are a plurality of holes on the surface of the layer having the opening, and the pitch between the plurality of holes is excessively small, the thermal diffusivity and strength of the graphite sheet are also reduced, as described above. Therefore, on the surface of the layer having the opening, the one or more holes are preferably a plurality of holes, and the plurality of holes are preferably formed at a pitch of 0.1 mm or more, more preferably 0.2 mm or more, and even more preferably 0.3 mm or more.
[0057] In addition, when the resin film has a plurality of surfaces having the openings, it is preferable that the total area of the openings, hole diameter, number per unit area and / or pitch of the plurality of holes of the one or more holes are within the above-mentioned preferred ranges on at least one of the surfaces having the openings of the layer in which the one or more holes are formed, and it is particularly preferable that the total area of the openings, hole diameter, number per unit area and / or pitch of the plurality of holes of the one or more holes are within the above-mentioned ranges on all of the surfaces having the openings of the layer in which the one or more holes are formed.
[0058] The total area value of the openings, the hole diameter, the number per unit area, and the pitch of the plurality of holes in the surface having the openings of the layer in which the one or more holes are formed can be determined, for example, by observing the surface having the openings of the layer in which the one or more holes are formed with a microscope. If the surface having the openings of the layer in which the one or more holes are formed is in contact with another layer and cannot be observed with a microscope, the surface having the openings may be observed with a microscope after removing the other layer. The observation of the surface having the openings of the layer may be performed using a method of image processing a microscope image using a computer, etc. A commercially available program may be used for the image processing.
[0059] In the present resin film, the one or more holes are holes having an opening on one side that forms an interface between the layer in which the one or more holes are formed and another layer. The shape of the one or more holes may be straight or curved. The direction of the holes is not particularly limited, and may be perpendicular or oblique to the surface direction of the layer. From the viewpoint of preventing peeling in the surface direction of the graphite layer, the direction is preferably 30° or more, more preferably 45° or more, to the surface direction of the layer. The shape of the opening and cross section of the one or more holes is not particularly limited, and may be, for example, a circle, an ellipse, an irregular shape, etc. The shape, direction, and opening (cross section) shape of each of the one or more holes may be the same or different.
[0060] The mode of the one or more holes in the present resin film will be described with reference to Fig. 1. Fig. 1 is a schematic diagram showing a hole structure in one example of a resin film for graphite sheet according to one embodiment of the present invention. All of the three present resin films shown in 100 to 102 in Fig. 1 are formed by laminating a resin layer 1 and a non-thermoplastic polyimide layer 2 in this order, and at least one layer has one or more holes 3 with openings formed on one side forming an interface with the other layer. Note that the resin layer 1 and the non-thermoplastic polyimide layer 2 may be the same layer or different layers.
[0061] In the example shown in 100 of Fig. 1, the non-thermoplastic polyimide layer constituting the present resin film has the above-mentioned holes formed therein, which extend in a direction perpendicular to one or more planar directions. The above-mentioned holes do not communicate with the surface of the present resin film.
[0062] In the example shown in 101 of Fig. 1, the non-thermoplastic polyimide layer and the resin layer constituting the present resin film have the above-mentioned holes extending in one or more directions perpendicular to the surface direction at the same positions in the surface direction. The holes existing at the same positions are connected to each other and penetrate from one surface to the other surface of the present resin film.
[0063] In the example shown in 102 of Fig. 1, the non-thermoplastic polyimide layer and the resin layer constituting the present resin film have one or more holes formed therein. Meanwhile, the directions of the holes vary. Furthermore, the holes are formed at different positions in the surface direction in each layer.
[0064] <3. Graphite sheet> One embodiment of the present invention also includes a graphite sheet containing the present resin film as a raw material (hereinafter referred to as the present graphite sheet). Since the present graphite sheet contains the present resin film as a raw material, peeling between graphite layers is prevented. In this specification, the present graphite sheet refers to both the graphite sheet before being subjected to the rolling step described below (graphite sheet before rolling) and the graphite sheet after being subjected to the rolling step (graphite sheet after rolling), but unless otherwise specified, the graphite sheet after rolling is intended.
[0065] The density of this graphite sheet is 1.2g / cm 3 It is preferable that the content is 1.3 g / cm or more. 3 More preferably, it is 1.4 g / cm or more. 3 The upper limit of the density is not particularly limited, but the density of the graphite sheet is usually 2.2 g / cm or more. 3 The density is 1.2g / cm 3 The graphite sheet having the above structure can realize efficient heat dissipation. The density of the graphite sheet can be measured by the method described in the Examples section below.
[0066] In addition, a plurality of the graphite sheets can be laminated with a resin layer interposed therebetween to form a graphite plate having a block shape such as a cube or a rectangular parallelepiped. The graphite plate can be made of anisotropic graphite having a desired shape using a wire saw or the like.
[0067] (Thermal Conductivity) In this specification, the thermal conductivity of the graphite sheet can be evaluated by the thermal diffusivity of the graphite sheet. The thermal diffusivity of the graphite sheet is 6.0 cm 2 / s or more is preferable, and 7.0 cm 2 / s or more is preferable, and 8.0 cm 2 More preferably, it is 9.0 cm / s or more. 2 It is even more preferable that the thermal diffusivity is 6.0 cm / s or more. 2 A graphite sheet having a thermal conductivity of 100 / s or more has excellent thermal conductivity.
[0068] The thermal diffusivity is measured by a flash method. Specific examples of the method for measuring the thermal diffusivity include the methods described in the (Thermal diffusivity) section of the Examples described later.
[0069] In this specification, the thermal conductivity of the graphite sheet can also be evaluated using the thermal conductivity λ calculated by the method described below. The thermal conductivity λ of the graphite sheet is preferably 600 W·m / k or more, more preferably 800 W·m / k or more, even more preferably 1000 W·m / k or more, and even more preferably 1400 W·m / k or more. A graphite sheet having a thermal conductivity λ of 600 W·m / k or more has excellent thermal conductivity. The thermal conductivity λ is calculated by the following formula (1). Thermal conductivity λ{W / (m·k)}={thermal diffusivity α(cm 2 / s)×density ρ(g / cm 3 ) × constant pressure specific heat capacity Cp(J·kg / k)} / 10 (1) The thermal diffusivity α and density ρ in the above formula (1) can be the values of thermal diffusivity and density measured by the above method. The specific heat capacity at constant pressure Cp in the above formula (1) is a value specific to the target material, and here, the specific heat capacity at constant pressure of graphite Cp = 850 (J kg / k) is used.
[0070] The lower limit of the thickness of the graphite sheet is preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 20 μm or more, from the viewpoint of enabling efficient heat transport, and the upper limit of the thickness of the graphite sheet is preferably 150 μm or less, and more preferably 100 μm or less, from the viewpoint of enabling arrangement in a small space.
[0071] <4. Manufacturing method of graphite sheet> The method for producing a graphite sheet according to one embodiment of the present invention (hereinafter sometimes referred to as the method for producing the graphite sheet) is not particularly limited as long as it is possible to heat-treat the resin film and provide a graphite sheet, and is preferably a method including a step of heat-treating the resin film at 2400°C or higher. The method for producing the graphite sheet will be described in detail below. In the following description, with regard to the resin film, the descriptions in the above section <2. Resin film for graphite sheet> and the below-mentioned section <5. Method for producing resin film for graphite sheet> are appropriately cited.
[0072] The method for producing the graphite sheet is preferably a so-called polymer pyrolysis method in which the resin film is heat-treated in an inert gas atmosphere or under reduced pressure. Specifically, the method preferably includes a carbonization step in which the resin film is preheated at a temperature of about 1000°C to obtain a carbonized resin film, and a graphitization step in which the carbonized resin film produced in the carbonization step is heat-treated (heated) at a temperature of 2400°C or higher to graphitize the resin film. The method may further include a rolling step in which the graphite sheet obtained in the graphitization step is rolled. In the method for producing the graphite sheet, the carbonization step and the graphitization step may be performed consecutively, or the graphitization step may be performed separately after the carbonization step is completed.
[0073] (carbonization process) The carbonization step is a step of carbonizing the present resin film by heat treatment up to a temperature of about 1000°C. The carbonization method of the present resin film in the carbonization step is not particularly limited, and for example, a sheet of the present resin film may be carbonized, a roll of the present resin film may be carbonized while still in the roll, or the film may be unrolled from the roll of the present resin film and continuously carbonized. The carbonization step is preferably carried out in a vacuum atmosphere, under reduced pressure, or in an inert gas, and nitrogen is preferably used as the inert gas. In this specification, the carbonized present resin film obtained by the carbonization step may be referred to as a carbonaceous film.
[0074] (Graphitization process) The graphitization step is a step of graphitizing the carbonaceous film obtained in the carbonization step by heat treatment at a temperature of 2400°C or higher to obtain a graphite sheet before rolling. In the graphitization step, the temperature (maximum temperature) during heat treatment is preferably 2400°C or higher, 2600°C or higher, 2800°C or higher, 2900°C or higher, or 3000°C or higher, since the thermal diffusivity of the obtained graphite sheet is good. The upper limit of the maximum temperature is not particularly limited, but is preferably 3300°C or lower, and more preferably 3200°C or lower, since sublimation of the graphite member in the graphitization furnace can be suppressed. The graphitization step is performed under reduced pressure or in an inert gas, and argon or helium can be suitably used as the inert gas.
[0075] In the graphitization step, a sheet of carbonaceous film may be graphitized, a roll of carbonaceous film may be graphitized while still in the roll state, or the film may be unwound from the roll of carbonaceous film and continuously graphitized.
[0076] In the graphitization step, the temperature rise rate when the carbonaceous film is heated to the maximum temperature is not particularly limited, but from the viewpoint of providing a graphite sheet with good productivity, the temperature rise rate is preferably 0.2° C. / min or more, more preferably 0.3° C. / min or more, even more preferably 0.4° C. / min or more, and even more preferably 0.5° C. / min or more.
[0077] (Rolling process) The rolling step is a step of rolling the graphite sheet obtained in the graphitization step before rolling. The graphite sheet before rolling is in a foamed state due to the influence of outgassing generated in the graphitization step and may have an excessive thickness that is unsuitable for practical use. However, by carrying out the rolling step, the thickness of the graphite sheet can be adjusted and flexibility can be imparted to the graphite sheet. In the rolling step, the method of rolling the graphite sheet is not particularly limited, and examples thereof include roll rolling in which the graphite sheet is rolled using a metal roll and a resin roll, and pressing. The rolling step may be carried out in a state in which the produced graphite sheet has been cooled to room temperature, or may be carried out continuously with the graphitization step.
[0078] <5. Manufacturing method of resin film for graphite sheet> A method for producing a resin film for graphite sheet according to one embodiment of the present invention (hereinafter, sometimes referred to as the method for producing the resin film) can include a method including a step of preparing a laminate by forming one or more resin layers on at least one surface of a non-thermoplastic polyimide layer (hereinafter, referred to as the "laminate preparation step"), and a step of forming one or more holes with openings on one surface that forms an interface with other layers in at least one layer of the non-thermoplastic polyimide layer and the one or more resin layers that constitute the laminate (hereinafter, referred to as the "hole formation step"). In addition, a method for producing the resin film can also include a method including, instead of the hole formation step, a step of forming one or more holes with openings on one surface that forms an interface with other layers in at least one layer of the non-thermoplastic polyimide layer and the one or more resin layers to be subjected to the laminate preparation step before carrying out the laminate preparation step (hereinafter, referred to as the "pre-hole formation step").
[0079] The specific method of the laminate preparation step is not particularly limited. The laminate preparation step may be, for example, a step of preparing the non-thermoplastic polyimide layer in advance, forming a pre-cured resin layer on the non-thermoplastic polyimide layer, and heating and curing the pre-cured resin layer to prepare the laminate.
[0080] As a method for preparing the non-thermoplastic polyimide layer in advance, a method of using a commercially available non-thermoplastic polyimide film as the non-thermoplastic polyimide layer, a chemical imidization method (chemical cure) in which a polyamic acid solution containing an imidization accelerator is heated to imidize the polyamic acid, and a thermal imidization method (thermal cure) in which a polyamic acid solution is heated to imidize without using an imidization accelerator, and a method of combining the above-mentioned non-thermoplastic polyimide layer with other known operations that can improve the orientation of the prepared polyimide film (non-thermoplastic polyimide layer) may be adopted.
[0081] The method for preparing a laminate by forming one or more resin layers on at least one surface of the non-thermoplastic polyimide layer is not particularly limited, and for example, the following methods (a) and (b) can be adopted. (a) A method for preparing a laminate, comprising: uniformly scattering resin particles constituting the resin layer on a surface of the non-thermoplastic polyimide layer; using a heat press, spreading the resin constituting the resin layer onto one surface of the non-thermoplastic polyimide layer to form an uncured resin layer; and heating and curing the uncured resin layer. (b) A method of preparing a laminate by applying a coating liquid containing a resin that constitutes the resin layer onto a surface of the non-thermoplastic polyimide layer to form a coating layer, and then heating the coating layer to form the resin layer.
[0082] The laminate preparation step will be described below by taking the methods (a) and (b) as examples.
[0083] The method (a) can be adopted when a resin that is solid at room temperature is used as the resin constituting the resin layer. Hereinafter, an example of the method (a) will be described with reference to FIG. 2. More specifically, the method described in FIG. 2 is a method for preparing a laminate having a three-layer structure of a non-thermoplastic polyimide layer / resin layer / another non-thermoplastic polyimide layer by using another non-thermoplastic polyimide layer as one of the one or more resin layers. As shown in FIG. 2, a press machine is used that is provided with a pair of opposing press plates 4 and a cylinder 9 on the lower side of the lower press plate 4. A stainless steel (SUS) plate 5 is placed on the lower press plate 4, a protective film 8 is placed on the SUS plate 5, and a non-thermoplastic polyimide layer 6 is placed on the protective film 8. Next, resin particles 7 that constitute the resin layer are uniformly scattered on the non-thermoplastic polyimide layer 6. Further, another non-thermoplastic polyimide layer 6' is placed on the resin particles 7, a protective film 8 is placed on the other non-thermoplastic polyimide layer 6', and a SUS plate 5 is placed on the protective film 8. Thereafter, the cylinder 9 is moved upward (in the direction of the arrow in FIG. 1), thereby moving the lower press plate 4 upward so that the upper SUS plate 5 and the upper press plate 4 come into contact with each other. Next, the resin particles 7 are spread by applying pressure to them while heating them, and the resin particles 7 are changed into a pre-cured resin layer. As a result, a laminate of a non-thermoplastic polyimide layer 6 / a pre-cured resin layer / another non-thermoplastic polyimide layer 6' is prepared. The method (a) may also include applying pressure to the pre-cured resin layer while heating it.
[0084] In the method (a), an example of a method of applying pressure to the resin particles 7 and the uncured resin layer while heating it is to apply pressure while controlling the temperature of the upper press plate 4 and / or the lower press plate 4 (hereinafter referred to as the "heat press set temperature") to a high temperature. The "heat press set temperature" can be appropriately set and used as a temperature at which the resin particles 7 can be suitably spread and cured without thermally decomposing the non-thermoplastic polyimide layer 6, the other non-thermoplastic polyimide layer 6', the resin particles 7, and the uncured / cured resin layer. The "heat press set temperature" is, for example, 50°C to 250°C, preferably 100°C to 200°C.
[0085] In the method (a), the pressure applied to the resin particles 7 and / or the resin layer before curing can be appropriately set and adopted so that the resin particles 7 can be appropriately spread and cured without damaging the members used in the method (a) and each layer constituting the present resin film. In addition, the method of applying the pressure is preferably a method of gradually increasing the magnitude of the applied pressure from the viewpoint of appropriately preventing damage to the members. Note that pressure can be applied to the resin particles 7 and / or the resin layer before curing by applying a load of a predetermined magnitude to the resin particles 7 and / or the resin layer before curing. The magnitude of the load can be controlled by adjusting the cylinder pressure of the cylinder 9, for example, when the method (a) is carried out using a press machine shown in FIG. 1. Hereinafter, the final magnitude of the load when the magnitude of the load applied is increased in order to increase the pressure applied is referred to as the "set load". The "set load" may be appropriately selected depending on the type and thickness of the material constituting the member, and is, for example, 1 kgf to 10,000 kgf, and preferably 10 kgf to 5,000 kgf.
[0086] In the method (a), from the viewpoint of suppressing bubbles that may occur during the heat pressing, it is preferable to preheat the member by heating before the heat pressing. After preheating for a predetermined time at a predetermined heat pressing temperature, it is preferable to gradually increase the magnitude of the load applied, and after the magnitude of the load reaches the set load, to maintain the magnitude of the load at the set load for a predetermined time.
[0087] There is no particular limitation on the protective film 8, and for example, a polytetrafluoroethylene (PTFE) film, a rubber sheet, etc. may be used. In the above-mentioned heat pressing, the protective film 8 does not have to be used.
[0088] The coating fluid in the method (b) contains the resin and may be a coating fluid made of the resin in a liquid state, or may be a coating fluid in which the resin is dissolved in a solvent.
[0089] When the coating liquid is a coating liquid in which the resin constituting the resin layer is dissolved in a solvent, the solvent is not particularly limited as long as it can dissolve the resin constituting the resin layer without adversely affecting the non-thermoplastic polyimide layer. The solvent can be appropriately selected depending on the type of resin constituting the resin layer. For example, when the resin constituting the resin layer is a phenolic resin, methanol or the like can be used as the solvent. The solvent may be one type of solvent or a mixture of two or more types of solvents.
[0090] The method for applying the coating liquid onto the non-thermoplastic polyimide layer is not particularly limited, and an appropriate method can be selected and adopted from among methods generally known as methods for applying a coating liquid onto a substrate.
[0091] In the method (b), the coating layer is heated to form the resin layer on the surface of the non-thermoplastic polyimide layer, and the laminate is prepared. The resin constituting the precipitated resin layer may be at least partially cured. In this case, the heating conditions may be appropriately adjusted so that at least a part of the resin constituting the resin layer is cured and / or the solvent can be removed from the coating layer. The heating temperature may be, for example, 30°C to 400°C, preferably 50°C to 350°C, and the heating time may be, for example, 5 minutes to 120 minutes, preferably 10 minutes to 60 minutes.
[0092] The coating liquid is applied to the surface of the non-thermoplastic polyimide layer opposite to the surface on which the uncured resin layer is laminated, and the resin layer is formed in the same manner as described above, thereby obtaining a laminate having a structure in which uncured resin layers are laminated on both sides of the non-thermoplastic polyimide layer.
[0093] In the methods (a) and (b), a gel film, which is a precursor of the non-thermoplastic polyimide layer, can also be used in place of the non-thermoplastic polyimide layer.
[0094] The resin layer in the laminate prepared in the step of preparing the laminate may not have all of the resin contained therein cured, in other words, may be incompletely cured. In that case, after the step of preparing the laminate, it is preferable to carry out a step of heating the resin layer in the laminate to cure all of the resin contained in the resin layer and completely cure the resin layer (hereinafter referred to as an "additional curing step"). The method of heating the resin layer in the laminate is not particularly limited, and for example, a method of heating the entire laminate using an oven or the like can be mentioned.
[0095] The hole forming step is a step of forming holes in at least one layer of the laminate or the laminate after the additional curing step. The method of forming the holes is not particularly limited, and examples thereof include a method of irradiating the laminate or the laminate after the additional curing step with a laser.
[0096] The specific method of irradiating the laser is not particularly limited, and examples of the method include a method in which a laser of a predetermined size is irradiated onto one side of the laminate or the laminate after the additional curing process, to form one hole at the location irradiated with the laser, and then a laser of a predetermined size is irradiated onto another location on the laminate or the laminate after the additional curing process, to form another hole at the other location, and a method in which a plurality of lasers of a predetermined size are irradiated at predetermined intervals onto one side of the laminate or the laminate after the additional curing process, to form holes at the plurality of locations irradiated with the laser.
[0097] In the method of irradiating a laser, the type and intensity of the laser are not particularly limited, and can be appropriately adjusted as long as it can melt the non-thermoplastic polyimide and resin present in the portion of the laminate or the laminate after the additional curing step where the laser is irradiated, and form the one or more holes, and does not adversely affect the laminate or the laminate after the additional curing step.
[0098] In addition, the direction of the holes to be formed and the shape of the openings can be appropriately adjusted by the direction of irradiation of the laser, the shape of the laser, the operation method, etc. Furthermore, the diameter of the holes to be formed can be appropriately adjusted by the type, intensity, irradiation time, etc. of the laser.
[0099] Furthermore, by adjusting the position of the spot where the laser is irradiated, etc., it is possible to appropriately control the pitch between the multiple holes when there are multiple holes of one or more.
[0100] Here, when the hole forming step is carried out by employing the laser irradiation method, the laser usually penetrates the laminate or the laminate after the additional curing step in the thickness direction, and one or more holes are formed as shown in 101 in FIG. 1.
[0101] The pre-hole forming step is a step of forming one or more holes in advance in at least one layer of the non-thermoplastic polyimide layer and one or more resin layers to be subjected to the laminate preparation step. When the pre-hole forming step is performed, the laminate prepared in the laminate preparation step has the one or more holes formed in at least one layer of the non-thermoplastic polyimide layer and one or more resin layers constituting the laminate, and corresponds to the present resin film. Therefore, when the pre-hole forming step is performed, the laminate preparation step can be a step of manufacturing the present resin film.
[0102] The specific method of the pre-hole formation step is not particularly limited, and an example thereof can be mentioned, in the method of irradiating a laser given above as an example of the hole formation step, in which the target of laser irradiation is changed from the laminate or the laminate after the additional curing step to at least one layer of the non-thermoplastic polyimide layer and one or more resin layers to be subjected to the laminate preparation step.
[0103] Here, when the pre-hole formation step is carried out to produce the present resin film by laminating a plurality of layers, consisting of a layer in which the one or more holes are formed and a layer in which the one or more holes are not formed, as the non-thermoplastic polyimide layer and the one or more resin layers, the present resin film produced has one or more holes as shown in 100 in Figure 1.
[0104] Another method of the pre-hole forming step may be, for example, a method using a filler that functions as a hole forming agent.Specifically, the other method may be, for example, a method in which a mixture of the non-thermoplastic polyimide or the resin constituting the resin layer and the filler is used as the raw material of the non-thermoplastic polyimide layer or the resin layer, a sheet containing the non-thermoplastic polyimide or the resin and the filler is formed, the sheet is stretched, and then the filler is removed using a suitable solvent.
[0105] The one or more holes formed by the method using the filler may have irregular directions and shapes. Therefore, when the present resin film is manufactured by laminating a plurality of layers in which one or more holes are formed using the method using the filler as the pre-hole forming step, the present resin film manufactured has one or more holes as shown in 102 in FIG.
[0106] The method for producing the resin film may include a step of forming other layers, such as an adhesive layer, in the resin film, other than the step of preparing the laminate, the step of additional curing, the step of forming holes, and the step of preforming holes. The method for forming the other layers may be appropriately selected from known methods commonly used by those skilled in the art.
[0107] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention.
[0108] That is, one embodiment of the present invention includes the following inventions. <1> A resin film for graphite sheet having a multilayer structure in which a non-thermoplastic polyimide layer and one or more resin layers are laminated, At least one of the non-thermoplastic polyimide layer and the one or more resin layers has one or more holes formed therein; the one or more holes have an opening on one side of the layer in which the one or more holes are formed that forms an interface with another layer; a ratio of a total area of the openings to an area of one side of the layer having the one or more holes formed therein is 0.05% to 5%. <2> the one or more holes communicate with at least one surface of the resin film for graphite sheet; <1> 2. The resin film for a graphite sheet according to claim 1 . <3> The multilayer structure is a multilayer structure in which the non-thermoplastic polyimide layer and one of the one or more resin layers are directly laminated to each other. <1> or <2> 2. The resin film for graphite sheet according to claim 1 . <4> On the surface of the layer in which the one or more holes are formed that includes the opening, The pore size of the one or more pores is 5 μm to 200 μm. <1> ~ <3> 10. A resin film for a graphite sheet according to any one of the above. <5> On the surface of the layer in which the one or more holes are formed that includes the opening, The number of the one or more holes per unit area is 1 / 9 holes / mm 2 That's all. <1> ~ <4> 10. A resin film for a graphite sheet according to any one of the above. <6> On the surface of the layer in which the one or more holes are formed that includes the opening, the one or more holes are a plurality of holes, The plurality of holes are formed at a pitch of 3 mm or less. <1> ~ <5> 10. A resin film for a graphite sheet according to any one of the above. <7> <1> ~ <6> A graphite sheet comprising, as a raw material, the resin film for graphite sheet according to any one of the above items. <8> <1> ~ <6> 1. A method for producing a graphite sheet, comprising: a step of heat-treating the resin film for a graphite sheet according to any one of claims 1 to 9 at a temperature of 2400°C or higher. EXAMPLES
[0109] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0110] <Evaluation method> The evaluation methods used in the examples and comparative examples will be described below.
[0111] (Thickness) The thickness of the non-thermoplastic polyimide layer described in Examples 1 to 3 and Comparative Examples 1 to 3 was measured by the method shown below. In the non-thermoplastic polyimide layer, the thickness was measured at four points 7 mm from each of the four corners of the non-thermoplastic polyimide layer along the diagonal line toward the center and at one point in the center using a micrometer (product name: MDC-PX, manufacturer: Mitutoyo Corporation, measurement surface diameter φ6.3 mm). Here, the "diagonal line" refers to a straight line drawn from each corner of the non-thermoplastic polyimide layer to a corner located diagonally opposite, and there were two of them. In addition, the "center" refers to the position of the intersection of the two diagonal lines. The average value of the thickness measurements obtained at a total of five points was taken as the thickness of the non-thermoplastic polyimide layer. Note that, when the non-thermoplastic polyimide layer to be measured is rectangular, the corner refers to the apex of the rectangle. Note that the resin film for graphite sheet described in Examples 1 to 3 and Comparative Examples 1 to 3 was configured as a non-thermoplastic polyimide layer / phenolic resin layer / non-thermoplastic polyimide layer, and both non-thermoplastic polyimide layers were the same layer.
[0112] Furthermore, the thickness of each of the resin films for graphite sheets described in Examples 1 to 3 and Comparative Examples 1 to 3 was measured by the same method as the method for measuring the thickness of the non-thermoplastic polyimide layer shown above.
[0113] In addition, the thickness of the graphite sheet before rolling and the thickness of the rolled graphite sheet described in Examples 1 to 3 and Comparative Examples 1 to 3 were measured by the same method as the method for measuring the thickness of the non-thermoplastic polyimide layer described above.
[0114] Next, the thickness retention rate (%) in the graphitization step and the thickness retention rate (%) in the rolling step were calculated using the thickness of the obtained resin film for graphite sheet, the thickness of the graphite sheet before rolling, and the thickness of the rolled graphite sheet based on the following formulas (2) and (3). Thickness retention rate in graphitization process (%) = {(thickness of graphite sheet before rolling) / (thickness of resin film for graphite sheet)}*100 (2) Thickness retention rate in rolling process (%) = {(thickness of rolled graphite sheet) / (thickness of resin film for graphite sheet)} * 100 (3) (density ρ) The graphite sheets described in Examples 1 to 3 and Comparative Examples 1 to 3 had a rectangular shape. The graphite sheets were used as samples for density measurement as they were. The volume (unit: cm) of the samples for density measurement was 3 ) was calculated based on the formula: (volume of density measurement sample) = (vertical length of density measurement sample) x (horizontal length of density measurement sample) x (thickness of graphite sheet). Next, the weight (unit: g) of the density measurement sample was measured using a weighing scale (product name: electromagnetic scale, manufacturer: Kensei Kogyo Co., Ltd.). The measured weight of the density measurement sample was divided by the volume of the density measurement sample to obtain the density of the graphite sheet (unit: g / cm 3 The measured density is referred to as "density ρ."
[0115] (thermal diffusivity α) The thermal diffusivity in the plane direction of the graphite sheets was measured by the method described below. Each of the graphite sheets described in Examples 1 to 3 and Comparative Examples 1 to 3 was punched out into a circle with a diameter of 25 mm to obtain a sample for thermal diffusivity measurement. Each of the samples for thermal diffusivity measurement was measured by an in-plane method using a thermal diffusivity measurement device (product name: LFA467 Hyper Flash, manufacturer: NETZSCH), to obtain the thermal diffusivity α (unit: cm 2The thermal diffusivity measurement sample was prepared by punching out the center of the graphite sheet. Here, the "center" refers to the portion of the graphite sheet that is in the center in both the width direction and the length direction.
[0116] (Thermal conductivity λ) Using the "density ρ" and "thermal diffusivity α" of the graphite sheets described in Examples 1 to 3 and Comparative Examples 1 to 3 obtained by the above-mentioned methods, and the specific heat capacity at constant pressure of graphite Cp = 850 (J kg / k), the thermal conductivity λ {W / (m k)} of the graphite sheets was calculated based on the following formula (1). Thermal conductivity λ{W / (m·k)}={thermal diffusivity α(cm 2 / s)×density ρ(g / cm 3 ) × constant pressure specific heat capacity Cp(J·kg / k)} / 10 (1) (surface and cross-sectional observation) Each of the graphite sheets was cut into a 5 mm x 5 mm square to obtain a sample for cross-sectional observation. The obtained sample for cross-sectional observation was clamped between clips and embedded in epoxy resin. The sample embedded in epoxy resin was polished using a rotary polisher (trade name: low peripheral speed doctor wrap, manufactured by Maruto Co., Ltd.) and a simple drive arm (manufactured by Maruto Co., Ltd.) first with JIS standard #220 waterproof abrasive paper (manufactured by Maruto Co., Ltd.), then with JIS standard #800 waterproof abrasive paper (manufactured by Maruto Co., Ltd.), then with JIS standard #1500 waterproof abrasive paper (manufactured by Maruto Co., Ltd.), then with a polishing cloth (trade name: TOUCH LAM 2TS4, manufactured by LAM PLAN Co., Ltd.) and an alumina suspension with an average particle size of 1 μm (trade name: Baikalox, manufactured by BAIKOWSKI Co., Ltd.), and finally with an alumina suspension with an average particle size of 0.1 μm (manufactured by BAIKOWSKI Co., Ltd.). As a result of the polishing, a cross section in the thickness direction of the graphite sheet was obtained. The cross section was observed using a laser microscope (product name: LEXT OLS4100, manufacturer: Olympus Corporation) in color observation mode with a 50x objective lens, and a micrograph of the cross section was obtained. From the obtained micrograph, the presence or absence of peeling between the graphite layers was confirmed. Among the obtained micrographs, micrographs obtained for the graphite sheets described in Example 1 and Comparative Example 3 are shown in Figures 3 and 4.
[0117] (Percentage of total opening area) An interface between the non-thermoplastic polyimide layer and the other layer, a phenolic resin layer, was formed, and the ratio of the total area of the openings to the area of one side having the openings of the holes was calculated by the following methods (a) to (c). The hole diameter on the surface of the non-thermoplastic polyimide layer having the openings was measured by observing the surface on which the resin layer of the non-thermoplastic polyimide layer after the pre-hole forming step was laminated using the same laser microscope as that used for the above-mentioned cross-sectional observation. In addition, as described later, the holes in the resin film for graphite sheet were formed by irradiating a laser from above vertically to the surface of the non-thermoplastic polyimide layer constituting the resin film for graphite sheet, and penetrating the non-thermoplastic polyimide layer. Therefore, the hole diameter and the pitch of the holes do not change in the thickness direction of the non-thermoplastic polyimide layer. Therefore, the hole diameter on the surface of the non-thermoplastic polyimide layer having the openings can also be obtained by observing the surface of the resin film for graphite sheet. (a) The total number of the openings present on the surface of the resin film for graphite sheet was calculated from the surface area of the resin film and the pitch set when the holes were formed. (b) The total area of the openings was calculated from the total number of openings obtained in (a) and the hole diameter measured above. (c) The ratio of the total area of the hole openings on the surface obtained in (b) to the area of the entire surface of the resin film for graphite sheet was calculated, and this ratio was defined as the ratio of the total area of the openings to the area of one side that forms an interface between the non-thermoplastic polyimide layer and the other layer, the phenolic resin layer, and is provided with the hole openings (hereinafter referred to as the "ratio of the total area of the openings").
[0118] [Example 1] (Preparation of resin film for graphite sheet) As materials, a commercially available polyimide film (product name: Apical (registered trademark) AH, manufactured by Kaneka Corporation, thickness 25 μm) and a commercially available fine particle phenolic resin (product name: Bellpearl (registered trademark) S899, manufactured by Air Water Bellpearl Co., Ltd.) were used. After cutting the polyimide film into a 90 mm x 90 mm square, a laser processing machine (product name: MD-T1000, manufactured by Keyence Corporation) was used to irradiate a 80 mm x 80 mm square area of the cut polyimide film with a laser under conditions of 100% laser power, 55 kHz Q-switch frequency, and 40 mm / s scan speed, forming 6400 holes of Φ60 μm at a pitch of 1 mm. Here, "6400 holes of Φ60μm were formed at a pitch of 1mm" means that the size of one laser irradiated area was Φ60μm, the number of laser irradiated areas was 6400, and the pitch between the multiple laser irradiated areas was 1mm, and the conditions for irradiating the laser were controlled. The polyimide film with holes was cut into four pieces of 40mm x 40mm square. Each of the cut pieces was used as a non-thermoplastic polyimide layer. 0.1g of the phenolic resin was spread on one of the four non-thermoplastic polyimide layers, and another non-thermoplastic polyimide layer of the four non-thermoplastic polyimide layers was placed on top of it to obtain a laminate A. The laminate A was subjected to thermocompression bonding for 10 minutes using a heat press machine (product name: compression molding machine AYSR-10, manufacturer: Shinto Metal Industries Co., Ltd.) under the conditions of a set load of 1023 kgf and a heat press set temperature of 180°C. Specifically, from the bottom, a SUS plate (20 mm x 20 mm square), a PTFE sheet (10 mm x 10 mm square), the one non-thermoplastic polyimide layer, the phenolic resin, the other one non-thermoplastic polyimide layer, another PTFE sheet, and another SUS plate were stacked to obtain a laminate B. The laminate B was placed on one of the press plates of the heat press machine. Next, the temperature of the two press plates of the heat press machine was set to 180°C, and the laminate B was heated for 1 minute to perform preheating.After that, after the preheating, the press plate of the heat press machine was moved so that the other press plate of the heat press machine was in contact with the SUS plate located on the opposite side of the SUS plate in contact with the one press plate in the laminate B, and a load was applied stepwise in a direction from the two SUS plates constituting the outermost surface of the laminate B toward the inside, and pressure was applied to the phenolic resin constituting the laminate B. At this time, a load was applied to the laminate B so that the magnitude of the load was gradually increased. (Hereinafter, this operation is referred to as "initial pressing operation"). Then, when the magnitude of the load applied reached 255.75 kgf, the magnitude of the load was reduced, and the other press plate was separated from the SUS plate located on the opposite side of the SUS plate in contact with the one press plate in the laminate B (Hereinafter, this operation is referred to as "releasing operation"). Next, pressing was performed in this order with a set load of 1023 kgf in the same manner as the "initial pressing operation" until the load reached 2 / 4, 3 / 4, and 4 / 4, and a releasing operation was performed each time the pressing was completed. In the last press, after the applied load reached 4 / 4 load, i.e., the set load, the applied load was maintained at the set load for 10 minutes before performing the release operation. In the remaining presses, the release operation was performed when the applied load reached 2 / 4 load or 3 / 4 load. By the above-mentioned operation, a laminate C was obtained. The laminate C had a configuration of the SUS plate / the PTFE sheet / the non-thermoplastic polyimide layer / the partially cured phenolic resin layer / the non-thermoplastic polyimide layer / the PTFE sheet / the SUS plate.
[0119] The obtained laminate C was sandwiched between plates through which cooling water was flowing, cooled, and then placed in an oven with an air atmosphere, heated at a heating temperature of 180°C for 60 minutes, and then heated at a heating temperature of 200°C for 60 minutes, to carry out an additional curing step. As a result, the phenolic resin in the phenolic resin layer before curing in the laminate C was completely cured. Next, the SUS plate and the PTFE sheet were peeled off from the laminate C after the additional curing step, and the ends were cut off to obtain a resin film for graphite sheet having a thickness of 70 μm and a size of 30 mm x 30 mm. The obtained resin film for graphite sheet is referred to as a resin film for graphite sheet (1). The resin film for graphite sheet (1) had a configuration of a non-thermoplastic polyimide layer / phenolic resin layer / non-thermoplastic polyimide layer.
[0120] (Preparation of graphite sheets) The graphite sheet resin film (1) was sandwiched between graphite sheets of 200 μm thickness and 60 mm×60 mm square to obtain a laminated sheet. At this time, the graphite sheet resin film (1) and the graphite sheets were laminated alternately one by one. The obtained laminated sheet was heated to 1000° C. in a nitrogen atmosphere and carbonized by heat treatment. Thereafter, the carbonized laminated sheet was graphitized by heating it to 2900° C. to produce a graphitized graphite sheet resin film, that is, a graphite sheet before rolling. Thereafter, the graphite sheet before rolling was rolled using a roll rolling machine (product name: 3-ton air hydro type roll press, manufacturer: Thank Metal Co., Ltd.) under conditions of a pressure of 4 MPa and a roll rotation speed of 2 m / min to produce a rolled graphite sheet. The rolled graphite sheet is referred to as the graphite sheet (1).
[0121] [Example 2] (Preparation of resin film for graphite sheet) A resin film for graphite sheet was produced in the same manner as in Example 1, except that, in the conditions of laser irradiation by the laser processing machine, the scan speed was changed to 80 mm / s, the size of one spot irradiated with the laser was set to Φ40 μm, and a hole of Φ40 μm was formed. The produced resin film for graphite sheet is referred to as resin film for graphite sheet (2).
[0122] (Preparation of graphite sheets) A graphite sheet was produced in the same manner as in Example 1, except that the resin film for graphite sheet (2) was used instead of the resin film for graphite sheet (1). The produced graphite sheet is referred to as graphite sheet (2).
[0123] [Example 3] (Preparation of resin film for graphite sheet) A resin film for graphite sheet was produced in the same manner as in Example 1, except that under the conditions of laser irradiation by the laser processing machine, the scan speed was changed to 2 mm / s, the size of one point irradiated with the laser was set to Φ160 μm to form a hole of Φ160 μm, and the laser was irradiated such that the pitch between the multiple points irradiated with the laser was 2 mm. The produced resin film for graphite sheet is referred to as resin film for graphite sheet (3).
[0124] (Preparation of graphite sheets) A graphite sheet was produced in the same manner as in Example 1, except that the resin film for graphite sheet (3) was used instead of the resin film for graphite sheet (1). The produced graphite sheet is referred to as graphite sheet (3).
[0125] [Comparative Example 1] (Preparation of resin film for graphite sheet) A resin film for graphite sheet was produced in the same manner as in Example 1, except that the laser was irradiated under the laser irradiation conditions using the laser processing machine such that the pitch between the multiple laser irradiated points was 4 mm. The produced resin film for graphite sheet is referred to as comparative resin film for graphite sheet (1).
[0126] (Preparation of graphite sheets) A graphite sheet was produced in the same manner as in Example 1, except that the resin film for graphite sheet (1) was used instead of the resin film for graphite sheet (1). The produced graphite sheet is referred to as the comparative graphite sheet (1).
[0127] [Comparative Example 2] (Preparation of resin film for graphite sheet) A resin film for graphite sheet was produced in the same manner as in Example 1, except that the laser was irradiated using the laser processing machine under the conditions such that the pitch between the multiple laser irradiated points was 8 mm. The produced resin film for graphite sheet is referred to as comparative resin film for graphite sheet (2).
[0128] (Preparation of graphite sheets) A graphite sheet was produced in the same manner as in Example 1, except that the resin film for graphite sheet (2) for comparison was used instead of the resin film for graphite sheet (1). The produced graphite sheet is referred to as the comparative graphite sheet (2).
[0129] [Comparative Example 3] (Preparation of resin film for graphite sheet) A resin film for graphite sheet was produced in the same manner as in Example 1, except that a non-thermoplastic polyimide layer not having holes formed therein was used as the non-thermoplastic polyimide layer. Here, the non-thermoplastic polyimide layer not having holes formed therein was a non-thermoplastic polyimide layer prepared in the same manner as in Example 1, except that the commercially available polyimide film was not irradiated with a laser. The produced resin film for graphite sheet is referred to as comparative resin film for graphite sheet (3).
[0130] (Preparation of graphite sheets) A graphite sheet was produced in the same manner as in Example 1, except that the resin film for graphite sheet (3) for comparison was used instead of the resin film for graphite sheet (1). The produced graphite sheet is referred to as the comparative graphite sheet (3).
[0131] [result] The physical properties of the resin films for graphite sheets described in Examples 1 to 3 and Comparative Examples 1 to 3, the resin films for graphite sheets before rolling, and the graphite sheets after rolling were measured by the methods described above, and the results are shown in Tables 1 and 2 below. In "Whether or not peeling occurs in cross-sectional observation" in Table 2, "no peeling" means that no gaps can be confirmed at the interface between the graphite layers constituting the graphite sheet, as shown in FIG. 3, and peeling does not occur. In addition, "peeling occurs" means that gaps exist at the interface between the graphite layers constituting the graphite sheet, as shown in FIG. 4, and peeling has occurred.
[0132] [Table 1]
[0133] [Table 2]
[0134] From the descriptions in Examples 1 to 3, Comparative Examples 1 and 2, and Table 1, the "pitch between holes" in the obtained resin films for graphite sheet (1) to (3) and comparative resin films for graphite sheet (1) to (2) was the same as the pitch between the positions irradiated with a laser when the surface of the layer in which holes were formed was irradiated with the laser to form the holes. Therefore, it was found that the "pitch between holes" and the number of holes per unit area in the resin film for graphite sheet can be controlled by adjusting the pitch between the positions irradiated with the laser.
[0135] As shown in Examples 1 to 3 and Table 1, resin films for graphite sheet (1) to (3) described in Examples 1 to 3 are resin films for graphite sheet having a multilayer structure in which a non-thermoplastic polyimide layer and one or more resin layers are laminated, in which at least one layer of the non-thermoplastic polyimide layer and the one or more resin layers has one or more holes formed therein, the one or more holes have openings on one side forming an interface between the layer in which the one or more holes are formed and another layer, and the ratio of the total area of the openings to the area of the one side having the openings of the layer in which the one or more holes are formed is within a range of 0.05% to 5%. Thus, resin films for graphite sheet (1) to (3) correspond to the present resin film. On the other hand, as shown in Table 1, the comparative resin films for graphite sheet (1) to (3) described in Comparative Examples 1 to 3 do not have the one or more holes, or even if the one or more holes are formed and the one or more holes have openings on one side forming the interface between the layer in which the one or more holes are formed and another layer, the ratio of the total area of the openings to the area of the one side having the openings of the layer in which the one or more holes are formed is less than 0.05%. Thus, the comparative resin films for graphite sheet (1) to (3) do not fall under the category of the present resin film.
[0136] When the graphite sheet resin films (1) to (3) were used as the raw material, no peeling occurred between the graphite layers. However, when the comparative graphite sheet resin films (1) to (3) were used as the raw material, peeling between the graphite layers could not be prevented.
[0137] From the above, it has been found that the resin film for graphite sheet according to one embodiment of the present invention can be used to manufacture a graphite sheet in which peeling between graphite layers is prevented, and has the effect of providing excellent productivity. [Industrial Applicability]
[0138] A resin film for a graphite sheet according to an embodiment of the present invention can be used to manufacture a graphite sheet in which peeling between graphite layers is prevented. [Explanation of symbols]
[0139] 100, 101, 102 Resin film for graphite sheet 1 Resin layer 2. Non-thermoplastic polyimide layer 3 holes 4 Press plate 5 Stainless steel (SUS) plate 6 Non-thermoplastic polyimide layer 6' Another non-thermoplastic polyimide layer 7 Resin particles 8 Protective Film 9 Cylinders
Claims
1. A resin film for graphite sheet having a multilayer structure in which a non-thermoplastic polyimide layer and one or more resin layers are laminated, At least one of the non-thermoplastic polyimide layer and the one or more resin layers has one or more holes formed therein; the one or more holes have an opening on one side of the layer in which the one or more holes are formed that forms an interface with another layer; a ratio of a total area of the openings to an area of one side of the layer having the one or more holes formed therein is 0.05% to 5%.
2. 2. The resin film for a graphite sheet according to claim 1, wherein the one or more holes communicate with at least one surface of the resin film for a graphite sheet.
3. 2. The resin film for graphite sheet according to claim 1, wherein the multilayer structure is a multilayer structure in which the non-thermoplastic polyimide layer and one of the one or more resin layers are directly laminated together.
4. On the surface of the layer having the one or more holes formed therein, the surface has the opening.
2. The resin film for graphite sheet according to claim 1, wherein the one or more holes have a pore size of 5 μm to 200 μm.
5. On the surface of the layer having the one or more holes formed therein, the surface has the opening. The number of the one or more holes per unit area is 1 / 9 holes / mm 2 2. The resin film for graphite sheet according to claim 1 .
6. On the surface of the layer having the one or more holes formed therein, the surface has the opening. the one or more holes is a plurality of holes, 2. The resin film for graphite sheet according to claim 1, wherein the plurality of holes are formed at a pitch of 3 mm or less.
7. A graphite sheet comprising the resin film for graphite sheet according to any one of claims 1 to 6 as a raw material.
8. A method for producing a graphite sheet, comprising a step of heat-treating the resin film for a graphite sheet according to any one of claims 1 to 6 at a temperature of 2400°C or higher.
Citation Information
Patent Citations
Laminated film
JP2017114098A
Multilayer polyimide film for graphite sheet, its manufacturing method, and graphite sheet manufactured from the same
JP2022512190A
Method for producing graphite sheet
WO2013140724A1