Thermally conductive resin composition, electronic device and semiconductor device

The thermally conductive resin composition with a disulfide-bonded curing agent and inorganic filler self-heals to maintain thermal conductivity, addressing cracking issues in electronic devices.

JP2024146529AInactive Publication Date: 2024-10-15PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023059495
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing thermally conductive materials experience a decrease in thermal conductivity due to cracking when repeatedly heated, which affects their efficiency in heat dissipation in electronic devices.

Method used

A thermally conductive resin composition containing a thermosetting resin, a curing agent with an aromatic compound having a disulfide bond, and an inorganic filler, with the aromatic compound comprising at least 40% of the total mass, which allows for self-healing and maintains thermal conductivity.

Benefits of technology

The composition maintains high thermal conductivity and self-repairs cracks, ensuring consistent heat dissipation performance in electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146529000001_ABST
    Figure 2024146529000001_ABST
Patent Text Reader

Abstract

To provide a thermally conductive resin composition that yields a thermally conductive material including a cured product with high thermal conductivity, while preventing its thermal conductivity from deteriorating, and also to provide an electronic device and a semiconductor device each including a cured product of the thermally conductive resin composition.SOLUTION: A thermally conductive resin composition includes a thermosetting resin (A), a curing agent (B), and an inorganic filler (C). The curing agent (B) includes an aromatic compound (B1) with a disulfide bond in each molecule. The proportion of the aromatic compound (B1) to the total of the thermosetting resin (A) and the curing agent (B) is more than 40 mass%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a thermally conductive resin composition, an electronic device, and a semiconductor device, and more specifically, to a thermally conductive resin composition that can be used in electronic devices and the like to produce a useful thermally conductive material, and an electronic device and a semiconductor device containing a cured product of the thermally conductive resin composition. [Background technology]

[0002] Patent Document 1 discloses a heat dissipation sheet that contains at least an alkyl group-introduced silicone oil (component A), an α-olefin (component B), and a thermally conductive filler (component D), and may also contain a silicone gel (component C). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 4149846 Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present disclosure is to provide a thermally conductive resin composition capable of obtaining a thermally conductive material containing a cured product having high thermal conductivity and capable of suppressing a decrease in the thermal conductivity, and to provide an electronic device and a semiconductor device containing a cured product of the thermally conductive resin composition. [Means for solving the problem]

[0005] A thermally conductive resin composition according to an embodiment of the present disclosure contains a thermosetting resin (A), a curing agent (B), and an inorganic filler (C). The curing agent (B) contains an aromatic compound (B1) having a disulfide bond in the molecule. The proportion of the aromatic compound (B1) to the total of the thermosetting resin (A) and the curing agent (B) is more than 40 mass%.

[0006] According to an embodiment of the present disclosure, there is provided an electronic device comprising an electronic component, a shell member covering the electronic component, and a thermally conductive layer interposed between the electronic component and the shell member, the thermally conductive layer including a cured product of the thermally conductive resin composition.

[0007] A semiconductor device according to an embodiment of the present disclosure includes a semiconductor element, a lid covering the semiconductor element, and a thermally conductive layer interposed between the semiconductor element and the lid, the thermally conductive layer including a cured product of the thermally conductive resin composition. Effect of the Invention

[0008] According to the present disclosure, it is possible to provide a thermally conductive resin composition that can obtain a thermally conductive material containing a cured product having high thermal conductivity and that can suppress a decrease in the thermal conductivity, and an electronic device and a semiconductor device that contain a cured product of the thermally conductive resin composition. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an electronic device according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] (1) Overview The process by which the thermally conductive resin composition of the present disclosure (hereinafter, also referred to as composition (X)) was completed will be described.

[0011] By placing a thermal interface material (TIM) between electronic / electrical components such as transistors and computer CPUs (central processing units) and a heat sink, the heat generated from the electronic / electrical components is conducted to the heat sink. In addition, with the high integration of electronic / electrical components, the amount of heat generated from electronic / electrical components tends to increase, and for this reason, there is a demand for efficient conduction of the heat generated by each electronic / electrical component using thermally conductive materials.

[0012] However, according to the inventors' research, when a thermally conductive material is repeatedly heated due to heat generated from electronic or electrical components, etc., cracks can occur inside the thermally conductive material, which can reduce the thermal conductivity of the thermally conductive material.

[0013] Therefore, the inventors conducted extensive research to obtain a thermally conductive resin composition that can produce a thermally conductive material with enhanced thermal conductivity and suppress a decrease in the thermal conductivity of the material, and as a result, have arrived at the present disclosure.

[0014] (2) Implementation form An embodiment will be described. Note that the following embodiment is merely a part of various embodiments of the present disclosure. In addition, the following embodiment can be modified in various ways depending on the design, etc., as long as the object of the present disclosure can be achieved. The figures referred to below are all schematic diagrams, and the dimensional ratios of the components in the figures do not necessarily reflect the actual dimensional ratios.

[0015] First, the outline of the composition (X) will be described. As described above, the composition (X) contains a thermosetting resin (A), a curing agent (B), and an inorganic filler (C). The curing agent (B) contains an aromatic compound (B1) having a disulfide bond in the molecule (hereinafter, simply referred to as an aromatic compound (B1)). The ratio of the aromatic compound (B1) to the total of the thermosetting resin (A) and the curing agent (B) is more than 40 mass%. This makes it possible to prepare a thermally conductive material with high thermal conductivity, and to suppress a decrease in the enhanced thermal conductivity of the thermally conductive material.

[0016] More specifically, the composition (X) contains a thermosetting resin (A), a curing agent (B), and an inorganic filler (C), which can enhance the thermal conductivity of a thermally conductive material made from the composition (X).

[0017] And, the composition (X) contains an aromatic compound (B1) having a specific functional group in a specific ratio. Therefore, the enhanced thermal conductivity of the thermally conductive material made from the composition (X) can be maintained. Although the above-mentioned effect of the thermally conductive material made from the composition (X) by containing the aromatic compound (B1) in a specific ratio has not been precisely clarified, it is believed to be due to the following reasons.

[0018] A thermally conductive material containing a cured product of the composition (X) may crack when it is cooled after it has been heated once. In contrast, since the composition (X) contains the aromatic compound (B1) having a disulfide bond as described above, the cured product of the composition (X) also has a disulfide bond in its composition structure, and the thermally conductive material produced by curing the composition (X) may experience disulfide bond cleavage when cracks occur. When the temperature of the thermally conductive material in which the cracks have occurred rises again, the cleaved disulfide bond may recombine. In other words, the thermally conductive material produced from the composition (X) containing the aromatic compound (B1) having a disulfide bond may have a self-repairing function that allows scratches and cracks to be repaired when the thermally conductive material is used in a normal manner, even if scratches or cracks occur.

[0019] Here, JP-A-2006-028476 describes that a semiconductor encapsulation resin composition used for semiconductor encapsulation contains diphenyl disulfide. However, JP-A-2006-028476 describes that a diphenyl disulfide compound is applied to enhance adhesion between the cured product of the semiconductor encapsulation resin composition and a lead frame, and does not describe that the cured product of the semiconductor encapsulation resin composition can self-repair. In addition, JP-A-2006-028476 describes that the content of diphenyl disulfide in the semiconductor encapsulation resin composition is about 0.01 to 1 mass %. In other words, the semiconductor encapsulation resin composition described in JP-A-2006-028476 does not contain diphenyl disulfide to an extent that it can fully exhibit self-repairing properties.

[0020] In contrast, the composition (X) of the present disclosure contains the aromatic compound (B1) at a specific ratio, i.e., more than 40 mass %, relative to the total of the thermosetting resin (A) and the curing agent (B). This can ensure sufficient self-repairing function of the cured product of the composition (X). As a result, the thermal conductivity of the thermally conductive material containing the cured product of the composition (X) can be maintained without decreasing. Due to this mechanism, the decrease in thermal conductivity can be suppressed in the thermally conductive material made from the composition (X).

[0021] As described above, the composition (X) can be used to prepare a thermally conductive material. The thermally conductive material is used, for example, by being interposed between an electronic component 3 included in an electronic device 1 and an outer shell member 4 covering the electronic component 3 (see FIG. 1). Then, the heat generated inside the electronic device 1 can be smoothly transferred to the outside of the electronic device 1 via the thermally conductive material. Note that the use of the composition (X) is not limited to being installed in the electronic device 1. The composition (X) can be applied to various uses.

[0022] (2.1) Composition The components of composition (X) will be described in detail below.

[0023] (thermosetting resin) The thermosetting resin (A) has a functional group that exhibits reactivity upon heating. The functional group of the thermosetting resin (A) includes, for example, at least one selected from the group consisting of an epoxy group, a (meth)acryloyl group, a vinyl group, an allyl group, and the like.

[0024] The molecular form of the thermosetting resin (A) is not particularly limited as long as its curing reactivity is not impaired, and examples of preferred forms include monomers, oligomers, prepolymers, etc. In particular, when the thermosetting resin (A) contains at least one of a monomer and an oligomer, the viscosity of the composition (X) can be reduced.

[0025] The thermosetting resin (A) contains at least one selected from the group consisting of, for example, an epoxy resin (A1), a phenolic resin, a styrene-based resin, a bismaleimide resin, a modified polyphenylene ether resin, a benzoxazine resin, etc. Among these, it is preferable that the thermosetting resin (A) contains an epoxy resin (A1).

[0026] The epoxy resin (A1) contains at least one component selected from the group consisting of, for example, glycidyl ether type epoxy resins, glycidyl amine type epoxy resins, glycidyl ester type epoxy resins, and olefin oxide type (alicyclic) epoxy resins. More specifically, the epoxy resin (A1) contains at least one component selected from the group consisting of, for example, alkylphenol novolac type epoxy resins such as phenol novolac type epoxy resins and cresol novolac type epoxy resins; naphthol novolac type epoxy resins; phenol aralkyl type epoxy resins having a phenylene skeleton, a biphenylene skeleton, or the like; biphenyl aralkyl type epoxy resins; naphthol aralkyl type epoxy resins having a phenylene skeleton, a biphenylene skeleton, or the like; polyfunctional type epoxy resins such as triphenol methane type epoxy resins and alkyl modified triphenol methane type epoxy resins; triphenyl methane type epoxy resins; tetrakisphenol ethane type epoxy resins; dicyclo The epoxy resin contains at least one component selected from the group consisting of pentadiene type epoxy resins; stilbene type epoxy resins; bisphenol type epoxy resins such as bisphenol A type epoxy resins and bisphenol F type epoxy resins; biphenyl type epoxy resins; naphthalene type epoxy resins; alicyclic epoxy resins; bromine-containing epoxy resins such as bisphenol A type bromine-containing epoxy resins; glycidyl amine type epoxy resins obtained by reacting polyamines such as diaminodiphenylmethane or isocyanuric acid with epichlorohydrin; and glycidyl ester type epoxy resins obtained by reacting polybasic acids such as phthalic acid or dimer acid with epichlorohydrin.

[0027] In addition, it is preferable that the epoxy resin (A1) has fluidity at room temperature, specifically at 25°C. In this case, the viscosity of the composition (X) can be reduced. This can improve the applicability of the composition (X). Here, the epoxy resin (A1) has fluidity means that the epoxy resin (A1) is liquid or pasty, and when the epoxy resin (A1) contains a plurality of components, the epoxy resin (A1), which is a mixture of a plurality of components, has fluidity as a whole. Preferably, the viscosity of the epoxy resin (A1) is 3000 Pa·s or less at 25°C. The viscosity of the epoxy resin (A1) is measured using an E-type rotational viscometer under the measurement conditions of a temperature of 25°C, a rotation speed of 0.3 rpm, and a measurement time of 200 seconds. In addition, the "applicability" of the composition (X) means the ease with which the composition (X) can be discharged from an applicator such as a dispenser and applied to any desired location.

[0028] Furthermore, it is particularly preferable that the epoxy resin (A1) contains at least one of a monomer and an oligomer of a bisphenol type epoxy resin having fluidity at room temperature (25° C.), in which case the viscosity of the composition (X) can be further reduced. The bisphenol type epoxy resin contains at least one selected from the group consisting of, for example, bisphenol A type epoxy resins and bisphenol F type epoxy resins.

[0029] The thermosetting resin (A) may contain only one type of component, or may contain two or more types of components.

[0030] (hardening agent) As described above, the composition (X) contains the curing agent (B) as a component. This curing agent (B) can react with the thermosetting resin (A), thereby curing the composition (X).

[0031] The curing agent (B) has one or more functional groups selected from the group consisting of, for example, an epoxy group, a hydroxyl group, an amino group, a thiol group, a carboxyl group, a silyl group, a carbon-carbon double bond (-C=C-), and the like. In this case, the reactivity of the thermosetting resin (A) with the curing agent (B) can be improved. In particular, when the thermosetting resin (A) contains an epoxy resin (A1), the curing agent (B) preferably contains at least one of a hydroxyl group and an amino group. In this case, the reactivity of the thermosetting resin (A) with the curing agent (B) can be further improved. This can further enhance the curability of the composition (X). The functional group of the curing agent (B) may be located at any position in the molecule, but is preferably located at the molecular end. The curability of the composition (X) can be enhanced by the functional group of the curing agent (B) being located at the molecular end.

[0032] When the composition (X) contains an epoxy resin (A1), the equivalent ratio of the curing agent (B) to the epoxy resin (A1) can be appropriately set in consideration of the reactivity between the epoxy resin (A1) and the curing agent (B). Specifically, the equivalent ratio of the curing agent (B) to the epoxy resin (A1) is preferably 0.6 or more and 1.5 or less, and more preferably 0.7 or more and 1.2 or less.

[0033] As described above, the curing agent (B) contains a specific ratio of aromatic compound (B1) having a disulfide bond (-SS-) in the molecule. This allows the cured product of the composition (X) to self-repair even if scratches or cracks occur, so that the thermal conductivity of the cured product can be prevented from decreasing. This allows the thermal conductivity of the thermally conductive material containing the cured product of the composition (X) to be prevented from decreasing. In other words, the thermal conductivity of the thermally conductive material produced from the composition (X) can be prevented from decreasing.

[0034] The aromatic compound (B1) includes, for example, at least one selected from the group consisting of a monomer, an oligomer, and a prepolymer. In particular, it is particularly preferable that the aromatic compound (B1) includes a monomer. In this case, the viscosity of the composition (X) can be reduced. The aromatic compound (B1) may have only one disulfide bond, or may have two or more disulfide bonds. The disulfide bond may or may not be directly bonded to a carbon atom of an aromatic ring in the aromatic compound (B1).

[0035] In addition, the aromatic compound (B1) having a disulfide bond (-SS-) in the molecule preferably contains a diphenyl disulfide compound (b1). In this case, the decrease in thermal conductivity of the cured product of the composition (X) can be further suppressed.

[0036] The diphenyl disulfide compound (b1) has, for example, a structure represented by formula (1) in the molecule and has a reactive group at the molecular end that reacts with the thermosetting resin (A).

[0037] [ka]

[0038] In formula (1), n ​​represents the number of substituents X bonded to the aromatic ring in formula (1), each n is independently an integer of 0 to 4, and each X is independently an alkyl group. The alkyl group may be linear or branched. The number of carbon atoms in the alkyl group is not particularly limited as long as it is 1 or more, but the upper limit is preferably 20 or less in consideration of the effect on the reactivity due to the increase in viscosity caused by the increase in molecular weight and the steric hindrance. When n is 0, the aromatic ring in formula (1) does not have a substituent. In this case, a hydrogen atom is bonded to each of the carbon atoms of the aromatic ring in formula (1). The reactive group of the diphenyl disulfide compound (b1) may be the same as the functional group of the curing agent (B), and includes, for example, one or more selected from the group consisting of an epoxy group, a hydroxyl group, an amino group, a thiol group, a carboxyl group, a silyl group, and a carbon-carbon double bond (-C=C-).

[0039] The diphenyl disulfide compound (b1) contains at least one component selected from the group consisting of aromatic disulfide diols such as 4,4'-dihydroxydiphenyl disulfide; aromatic disulfide diamines such as 4,4'-diaminodiphenyl disulfide (4,4'-dithioaniline); and aromatic disulfide dicarboxylic acids such as 2,2'-dicarboxydiphenyl disulfide. When the thermosetting resin (A) contains an epoxy resin (A1), it is particularly preferable that the diphenyl disulfide compound (b1) contains either 4,4'-dihydroxydiphenyl disulfide or 4,4'-diaminodiphenyl disulfide. In other words, when the thermosetting resin (A) contains an epoxy resin (A1), it is particularly preferable that the reactive group of the diphenyl disulfide compound (b1) contains at least one of a hydroxyl group and an amino group. In this case, the decrease in thermal conductivity of the thermally conductive material containing the cured product of the composition (X) is particularly suppressed, and the reactivity between the thermosetting resin (A) and the curing agent (B) can be particularly improved.

[0040] The cured product (B) may further contain a compound having a disulfide bond other than the aromatic compound (B1). Examples of the compound having a disulfide bond other than the aromatic compound (B1) include aliphatic compounds having a disulfide bond.

[0041] The ratio of the aromatic compound (B1) to the total of the thermosetting resin (A) and the curing agent (B) is more than 40 mass%. In this case, self-repair can occur in the cured product of the composition (X). This can maintain the enhanced thermal conductivity of the cured product of the composition (X). In addition, when the ratio of the aromatic compound (B1) to the total of the thermosetting resin (A) and the curing agent (B) is more than 40 mass%, the reactivity of the thermosetting resin (A) with the curing agent (B) can be enhanced. This can enhance the curability of the composition (X). In addition, when the thermosetting resin (A) contains an epoxy resin (A1), the reactivity of the thermosetting resin (A) with the curing agent (B) can be particularly enhanced.

[0042] The ratio of the aromatic compound (B1) to the total of the thermosetting resin (A) and the curing agent (B) is more preferably more than 41% by mass, and even more preferably more than 43% by mass. The upper limit of the ratio of the aromatic compound (B1) to the total of the thermosetting resin (A) and the curing agent (B) is not particularly limited, but it is preferable that the self-repairing function of the cured product of the composition (X) is not saturated, and the reactivity between the thermosetting resin (A) and the curing agent (B) is good, and the curability of the composition (X) is sufficiently ensured. Such an upper limit may be, for example, 70% by mass or less, 65% by mass or less, or 60% by mass or less.

[0043] The curing agent (B) may be used in the form of one kind of component or in the form of a combination of two or more kinds of components.

[0044] (Inorganic filler) As described above, the composition (X) contains an inorganic filler (C) as a component. This inorganic filler (C) preferably contains a thermally conductive filler (C1) (hereinafter, also referred to as a first inorganic filler (C1)). The thermally conductive filler (C1) can have high thermal conductivity. This can impart high thermal conductivity to the cured product of the composition (X).

[0045] As described above, the thermally conductive filler (C1) can have high thermal conductivity. The thermal conductivity of the thermally conductive filler (C1) is, for example, 15 W / m·K or more at 25° C., and preferably 20 W / m·K or more at 25° C.

[0046] The thermally conductive filler (C1) contains at least one component selected from the group consisting of metals such as silver, aluminum, and copper; metal oxides such as aluminum oxide, zinc oxide, and magnesium oxide; nitrides such as aluminum nitride, silicon nitride, and boron nitride; carbides such as silicon carbide; hydroxides such as aluminum hydroxide; carbonates such as magnesium carbonate and anhydrous magnesium carbonate; and carbon-based materials such as graphite, graphene, carbon nanotubes, and diamond. The thermally conductive filler (C1) preferably contains at least one of aluminum oxide and aluminum nitride. In this case, the thermal conductivity of the cured product of the composition (X) can be further increased. These components may be used alone or in combination of two or more.

[0047] The volume ratio of the thermally conductive filler (C1) is preferably 30% by volume or more and 90% by volume or less with respect to the entire composition (X). When the volume ratio of the thermally conductive filler (C1) is 30% by volume or more with respect to the entire composition (X), the thermal conductivity of the cured product of the composition (X) can be particularly enhanced. When the volume ratio of the thermally conductive filler (C1) is 90% by volume or less with respect to the entire composition (X), the fluidity of the composition (X) can be ensured. This can enhance the applicability of the composition (X). The volume ratio of the thermally conductive filler (C1) is more preferably 40% by volume or more, and even more preferably 50% by volume or more with respect to the entire composition (X).

[0048] The inorganic filler (C) may contain a second inorganic filler (C2) different from the first inorganic filler (C1) (thermally conductive filler (C1)). That is, the inorganic filler (C) may contain only the first inorganic filler (C1), or may contain the first inorganic filler (C1) and the second inorganic filler (C2). Specific examples of the second inorganic filler (C2) include inorganic compound powders such as talc, mica, kaolin, diatomaceous earth, silica, titania, and zeolite, and glass fibers. These components may be used alone or in combination of two or more.

[0049] (Cure accelerator) The composition (X) may contain a curing accelerator as a component. In this case, the curing property of the composition (X) may be further improved. Examples of the curing accelerator include phosphorus compounds such as triphenylphosphine and amine compounds such as imidazole. The curing accelerator may be used alone or in combination of two or more types.

[0050] (Dispersant) The composition (X) may contain a dispersant as a component. The dispersant may be a commercially available product. Specific examples of commercially available products include Marialim SC-050K (manufactured by NOF Corporation). The dispersant may be used alone or in combination of two or more types.

[0051] (Additives) The composition (X) may contain additives other than the above-mentioned thermosetting resin (A), curing agent (B), inorganic filler (C), dispersant and curing accelerator, as long as the effects of the present disclosure are not impaired. The additives may contain at least one selected from the group consisting of, for example, coupling agents, pigments, flame retardants, colorants, and adhesion promoters.

[0052] (2.2) Physical Properties (Self-repair) As described above, even if the cured product of the composition (X) is scratched or cracked, it can be self-repaired to a state without scratches or cracks. This self-repair of the cured product of the composition (X) can occur, for example, when the cured product of the composition (X) is heated. Specifically, the self-repair of the cured product of the composition (X) can occur when the cured product of the composition (X) is heated at a temperature equal to or higher than its glass transition temperature.

[0053] (viscosity) The composition (X) is preferably in a paste form, and therefore preferably has a low viscosity at 25°C. More specifically, the composition (X) is preferably in a paste form at 25°C. The viscosity of the composition (X) at 25°C is preferably 3000 Pa·s or less, and more preferably 2000 Pa·s or less. In this case, the applicability of the composition (X) can be particularly improved. The lower limit of the viscosity of the composition (X) at 25°C is not particularly limited, but is, for example, 50 Pa·s or more. In this case, the composition (X) can be easily handled while ensuring the applicability of the composition (X). The viscosity of the composition (X) was measured using an E-type viscometer (manufactured by Toki Sangyo Co., Ltd., model number: RC-215) at a temperature of 25°C, a rotation speed of 0.3 rpm, and a measurement time of 200 seconds.

[0054] (thermal resistance) As described above, the cured product of the composition (X) can have high thermal conductivity. For example, the thermal conductivity of the cured product of the composition (X) can be evaluated using the thermal resistance value as an index.

[0055] For example, when the thickness of the cured product of composition (X) is 150 μm, the thermal resistance in the direction of the pressing pressure is preferably 2.0 K / W or less, and more preferably 1.5 K / W or less. In this case, the thermally conductive material containing the cured product of composition (X) can exhibit excellent thermal conductivity and can transmit heat efficiently.

[0056] The method for measuring the thermal resistance will be described in detail in the Examples section below.

[0057] (2.3) Application Examples (Thermal Conductive Materials) In this embodiment, the thermally conductive material can be produced by curing the composition (X) by heating it, i.e., a thermally conductive material containing a cured product of the composition (X) is obtained.

[0058] The composition (X) according to this embodiment can be used by being interposed between a heat generating body such as an electronic component 3, such as a semiconductor element, and a heat dissipating body such as a heat sink 7, and then cured to produce a thermally conductive material capable of promoting heat dissipation from the electronic component 3 to the heat sink 7. That is, the thermally conductive material according to this embodiment can form a thermally conductive layer 5 interposed between the electronic component 3 and the outer shell member 4 of an electronic device 1 (see FIG. 1). The thermally conductive material according to this embodiment can be particularly suitably applied to a semiconductor device among electronic devices 1, and can be used as the thermally conductive layer 5 interposed between a semiconductor element and a lid of the semiconductor device.

[0059] When preparing a thermally conductive material from the composition (X), the composition (X) may be placed at the desired location and then cured by heating. It may also be molded into a component of a predetermined shape depending on the intended use. For example, the composition (X) may be molded into a film by a suitable method such as press molding, extrusion molding, or calendar molding, or may be molded into a film using a dispenser and then cured by heating to prepare a film-shaped thermally conductive material.

[0060] The method for producing the thermally conductive material from the composition (X) is not limited to the above-mentioned method, and various production methods can be adopted depending on the application and purpose.

[0061] (electronic equipment) As described above, the thermally conductive material made from the composition (X) can be used to make a thermally conductive layer 5 for transferring heat generated from an electronic device 1 as shown in FIG. 1 to the outside of the electronic device 1. Specifically, the electronic device 1 includes an electronic component 3, an outer shell member 4 covering the electronic component 3, and a thermally conductive layer 5 interposed between the electronic component 3 and the outer shell member 4. The thermally conductive layer 5 is made from a thermally conductive material made from the composition (X), that is, it contains a cured product of the composition (X). Therefore, the thermal conductivity of the thermally conductive layer 5 is particularly enhanced, and the heat generated from the electronic device 1 can be suitably transferred to the outer shell member 4 through the thermally conductive layer 5. This allows the heat generated inside the electronic device 1 to be dissipated to the outside.

[0062] Furthermore, since the thermally conductive layer 5 is made of a thermally conductive material made of the composition (X), it has high thermal conductivity and can have a high self-repairing function. Therefore, even if the thermally conductive layer 5 is scratched or cracked, the thermally conductive layer 5 can self-repair during normal use. This allows the thermally conductive layer 5 to be repaired to a state free of scratches and cracks. In this way, the thermal conductivity of the thermally conductive layer 5 can be prevented from decreasing due to scratches or cracks.

[0063] As described above, the thermally conductive material made from the composition (X) is particularly suitable for use in semiconductor devices, among other electronic devices 1. Specifically, the semiconductor device, which is the electronic device 1, comprises a semiconductor element, which is an electronic component 3, a lid, which is an outer shell member 4 covering the semiconductor element, and a thermally conductive layer 5 interposed between the semiconductor element and the lid. The thermally conductive layer 5 is made of the thermally conductive material made from the composition (X) and contains a cured product of the composition (X).

[0064] The configuration of the electronic device 1 will now be described in more detail.

[0065] The electronic device 1 includes a substrate 2, an electronic component 3, an outer shell member 4 covering the electronic component 3, and a thermally conductive layer 5 containing a cured product of a composition (X) interposed between the electronic component 3 and the outer shell member 4.

[0066] The substrate 2 may be, for example, a mother substrate, a package substrate, an interposer substrate, etc. The substrate 2 may be made of, for example, glass epoxy, polyimide, polyester, ceramic, etc.

[0067] The electronic component 3 includes at least one selected from the group consisting of active elements such as transistors and diodes; passive elements such as resistors, capacitors, inductors, reactors, memristors, and transformers; CPUs, MPUs, driver ICs, and memories. The electronic component 3 may also be a semiconductor element, and the semiconductor element includes at least one selected from the group consisting of transistors, diodes, thyristors, and modules. Furthermore, a plurality of electronic components 3 may be mounted on the substrate 2. In this case, the electronic components 3 may have different thicknesses.

[0068] As described above, the outer shell member 4 is mounted on the substrate 2 so as to cover the electronic component 3. The outer shell member 4 is, for example, a housing of the electronic device 1 such as a lid, and is a member having high thermal conductivity. The electronic device 1 may include a heat spreader and a heat sink 7. In the present embodiment, the heat spreader and the heat sink 7 are preferably disposed on the outer shell member 4 of the electronic device 1, but are not particularly limited thereto. For example, the heat spreader and the heat sink 7 may be disposed on the surface of the substrate 2 opposite to the surface on which the outer shell member 4 is mounted. In this case, the heat spreader may be interposed between the substrate 2 and the heat sink 7. Furthermore, a thermally conductive layer 8 may be interposed between the heat spreader and the heat sink 7, and the thermally conductive layer 8 may be a thermally conductive material made of the composition (X).

[0069] The thermally conductive layer 5 of the electronic device 1 is produced, for example, by the following method. First, the composition (X) is filled in the gap between the electronic component 3 and the outer shell member 4 located on the outside thereof, and cured by heating. In this manner, the thermally conductive layer 5 containing the cured product of the composition (X) can be produced in the gap between the electronic component 3 and the outer shell member 4 located on the outside thereof. In this embodiment, the composition (X) is preferably in a paste form at room temperature, specifically at 25° C., and in this case, the composition (X) can be easily applied by a dispenser device. This allows the composition (X) to be easily filled in the gap between the electronic component 3 and the outer shell member 4 located on the outside thereof.

[0070] Furthermore, the composition (X) is formed into a film, and then the film-like composition (X) is heated and cured under conditions according to its composition to obtain a film-like thermally conductive material. The film-like thermally conductive material may be interposed between the electronic component 3 and the outer shell member 4 to produce the thermally conductive layer 5.

[0071] (3) Summary As is apparent from the above embodiment, the present disclosure includes the following aspects. In the following, reference symbols are given in parentheses only to clarify the correspondence with the embodiment.

[0072] The thermally conductive resin composition according to the first embodiment of the present disclosure contains a thermosetting resin (A), a curing agent (B), and an inorganic filler (C). The curing agent (B) contains an aromatic compound (B1) having a disulfide bond in the molecule. The proportion of the aromatic compound (B1) to the total of the thermosetting resin (A) and the curing agent (B) is more than 40 mass%.

[0073] According to the first aspect, it is possible to provide a thermally conductive resin composition that can obtain a thermally conductive material containing a cured product having high thermal conductivity and can suppress a decrease in the thermal conductivity.

[0074] In the thermally conductive resin composition according to the second embodiment of the present disclosure, in the first embodiment, the aromatic compound (B1) contains a diphenyl disulfide compound (b1). The diphenyl disulfide compound (b1) has a structure represented by formula (1) in the molecule and has a reactive group at the molecular end that reacts with the thermosetting resin (A).

[0075] [ka]

[0076] In formula (1), n ​​represents the number of substituents X, and each n is independently an integer of 0 to 4, and each X is independently an alkyl group.

[0077] According to the second aspect, the decrease in thermal conductivity of the cured product of the composition (X) can be further suppressed.

[0078] In the thermally conductive resin composition according to the third aspect of the present disclosure, in the second aspect, the thermosetting resin (A) includes an epoxy resin (A1). The reactive group includes at least one of a hydroxyl group and an amino group.

[0079] According to the third embodiment, the reactivity between the thermosetting resin (A) and the curing agent (B) can be further improved, which can further enhance the curability of the composition (X).

[0080] In the thermally conductive resin composition according to the fourth aspect of the present disclosure, in the third aspect, the epoxy resin (A1) has flowability at 25°C.

[0081] According to the fourth aspect, the viscosity of the composition (X) can be reduced, thereby improving the applicability of the composition (X).

[0082] In the thermally conductive resin composition according to the fifth aspect of the present disclosure, in any one of the first to fourth aspects, the inorganic filler (C) includes a thermally conductive filler (C1). The thermal conductivity of the thermally conductive filler (C1) is 15 W / m·K or more.

[0083] According to the fifth embodiment, a thermally conductive material having higher thermal conductivity can be produced from the composition (X).

[0084] In the thermally conductive resin composition according to the sixth aspect of the present disclosure, in the fifth aspect, the proportion of the thermally conductive filler (C1) is 30 vol % or more and 90 vol % or less with respect to the entire composition (X).

[0085] According to the sixth embodiment, the thermal conductivity of the cured product of the composition (X) can be particularly increased.

[0086] The thermally conductive resin composition according to the seventh aspect of the present disclosure, in any one of the first to sixth aspects, is in a paste form having a viscosity of 3000 Pa·s or less at 25° C.

[0087] According to the seventh embodiment, the coatability of the composition (X) can be improved.

[0088] An electronic device (1) according to an eighth aspect of the present disclosure includes an electronic component (3), an outer shell member (4) that covers the electronic component (3), and a thermally conductive layer (5) that is interposed between the electronic component (3) and the outer shell member (4). The thermally conductive layer (5) includes a cured product of the thermally conductive resin composition according to any one of the first to seventh aspects.

[0089] According to the eighth aspect, it is possible to obtain an electronic device (1) including a thermally conductive material that has enhanced thermal conductivity and can maintain the enhanced thermal conductivity.

[0090] A semiconductor device according to a ninth aspect of the present disclosure includes a semiconductor element, a lid covering the semiconductor element, and a thermally conductive layer interposed between the semiconductor element and the lid, the thermally conductive layer including a cured product of the thermally conductive resin composition according to any one of the first to seventh aspects.

[0091] According to the ninth aspect, a semiconductor device can be obtained that includes a thermally conductive material that can enhance and maintain the enhanced thermal conductivity. EXAMPLES

[0092] More specific examples of the present embodiment will be described below, but the present embodiment is not limited to the following examples.

[0093] 1. Method for producing thermally conductive resin composition Methods for producing the thermally conductive resin compositions of Examples 1 to 6 and Comparative Examples 1 to 3 will be described.

[0094] [component] The components used to prepare the thermally conductive resin compositions of Examples 1 to 6 and Comparative Examples 1 to 3 are shown below. The components were mixed in the ratios shown in Tables 1 and 2 to obtain the thermally conductive resin compositions.

[0095] (thermosetting resin) Epoxy resin: bisphenol F type epoxy resin (manufactured by DIC Corporation, product name Epicron 830S, viscosity 3000 to 4500 mPa·s (25°C)).

[0096] (hardening agent) Aromatic compound having a disulfide bond 1: 4,4'-dithioaniline (Tokyo Chemical Industry Co., Ltd.).

[0097] Aromatic compound having a disulfide bond 2: bis(4-hydroxyphenyl) disulfide (Tokyo Chemical Industry Co., Ltd.).

[0098] Aliphatic compound having a disulfide bond: dithiodipropionic acid (Tokyo Chemical Industry Co., Ltd.).

[0099] (Inorganic filler) Thermally conductive filler 1: Alumina (manufactured by Sumitomo Chemical Co., Ltd., product name Advanced Alumina AA-5, median particle size 6.6 μm, thermal conductivity 35 W / m·K).

[0100] Thermally conductive filler 2: Alumina (manufactured by Sumitomo Chemical Co., Ltd., product name Advanced Alumina AA-05, central particle size 0.58 μm, thermal conductivity 35 W / m·K).

[0101] Thermally conductive filler 3: Aluminum nitride (manufactured by Combustion Synthesis Co., Ltd., product name AN-HF50LGL-HTZ, average particle size 50 μm, thermal conductivity 170 W / m·K).

[0102] (Cure accelerator) Curing accelerator 1: Triphenylphosphine (manufactured by Tokyo Chemical Industry Co., Ltd.).

[0103] (Dispersant) Dispersant 1: Dispersant (manufactured by NOF Corporation, product name Marialim SC0505K).

[0104] 2. Evaluation The resin compositions of the examples and comparative examples prepared according to the method described in "1. Method for preparing resin composition" were evaluated by the following tests.

[0105] (1) Viscosity The viscosity of the composition was measured using an E-type viscometer (model RC-215) manufactured by Toki Sangyo Co., Ltd. as the measuring device under conditions of a measurement temperature of 25° C., a rotation speed of 0.3 rpm, and a measurement time of 200 seconds.

[0106] (2) Thermal resistance The thermally conductive resin composition was filled between two copper plates having a thickness of 1 mm, and in the sandwiched state, it was directly pressed under a pressure of 1060 kPa, and the thickness of the thermally conductive resin composition was adjusted to 150 μm. In this state, it was cured in a dryer at 120 ° C for 3 hours to prepare a sheet-like sample having a thickness of 150 μm, which is a cured product of the thermally conductive resin composition. In this state, the thermal resistance of the sample in the direction of the pressing pressure at room temperature under the pressing pressure of 1060 kPa was measured using a DynTIM Tester manufactured by Mentor Graphics. The thermal resistance was evaluated as an index of thermal conductivity.

[0107] (3) Self-repairability evaluation A sheet-shaped sample, which is a cured product of the thermally conductive resin composition, was prepared in the same manner as in "(2) Thermal resistance" except that the thickness of the sample was set to 500 μm. Next, a groove of about 20 mm in length was made on the surface of the sheet-shaped sample with a cutter knife. The groove was set to a depth of 50 to 100 μm so as not to penetrate the sample. Then, the sample was heated at 120° C. for 10 minutes, and whether the damage was repaired was visually confirmed using a magnifying glass, and the confirmation result was judged according to the following criteria. A: After heating, the groove closed to the sample surface and healed. B: After heating, the groove did not close to the surface of the sample, but it was fixed and repaired halfway inside. C: The groove remained the same after heating.

[0108] [Table 1]

[0109] [Table 2]

[0110] As shown in Table 1, suitable heat resistance was obtained in Examples 1 to 6, and the self-repairing property was confirmed. On the other hand, as shown in Table 2, the self-repairing property was not confirmed in Comparative Examples 1 to 3. In Comparative Example 3, the viscosity was too high to perform stable measurements, and a sample could not be produced. [Explanation of symbols]

[0111] 1 Electronic equipment 3. Electronic Components 4. Shell Materials 5. Thermal Conduction Layer

Claims

1. Contains a thermosetting resin (A), a curing agent (B), and an inorganic filler (C), The curing agent (B) contains an aromatic compound (B1) having a disulfide bond in the molecule, The ratio of the aromatic compound (B1) to the total of the thermosetting resin (A) and the curing agent (B) is more than 40 mass%. A thermally conductive resin composition.

2. The aromatic compound (B1) includes a diphenyl disulfide compound (b1), The diphenyl disulfide compound (b1) has a structure represented by formula (1) in the molecule and has a reactive group at the molecular end which reacts with the thermosetting resin (A), 【Chemistry 1】 In formula (1), n ​​represents the number of substituents X, each n is independently an integer of 0 to 4, and each X is independently an alkyl group. The thermally conductive resin composition according to claim 1 .

3. The thermosetting resin (A) contains an epoxy resin (A1), The reactive group includes at least one of a hydroxyl group and an amino group. The thermally conductive resin composition according to claim 2 .

4. The epoxy resin (A1) has fluidity at 25°C. The thermally conductive resin composition according to claim 3 .

5. The inorganic filler (C) contains a thermally conductive filler (C1), The thermal conductivity of the thermally conductive filler (C1) is 15 W / m K or more. The thermally conductive resin composition according to claim 1 .

6. The volume ratio of the thermally conductive filler (C1) is 30 vol% or more and 90 vol% or less with respect to the entire thermally conductive resin composition. The thermally conductive resin composition according to claim 5 .

7. It is a paste having a viscosity of 3000 Pa s or less at 25 ° C. The thermally conductive resin composition according to claim 1 .

8. The electronic component includes an outer shell member that covers the electronic component, and a heat conductive layer that is interposed between the electronic component and the outer shell member, The thermally conductive layer comprises a cured product of the thermally conductive resin composition according to any one of claims 1 to 7. Electronic equipment equipment.

9. a semiconductor element; a lid covering the semiconductor element; and a thermally conductive layer interposed between the semiconductor element and the lid; The thermally conductive layer comprises a cured product of the thermally conductive resin composition according to any one of claims 1 to 7. Semiconductor device.

Citation Information

Patent Citations

  • Heat dissipation sheet

    JP4149846B2