Styrene-based resin composition

The styrenic resin composition with styrene, polyester, and acrylic resin components addresses melt tension and foaming issues, enhancing extrudability and producing high-quality foam sheets for various applications.

JP2024146542AInactive Publication Date: 2024-10-15TOYO STYRENE CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023059514
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing styrenic resin compositions face difficulties in maintaining melt tension and foaming properties during extrusion, leading to poor extrudability and foaming characteristics.

Method used

A styrenic resin composition comprising styrene resin, a polarity imparting material, and an acrylic resin, with specific mass ratios and properties, such as a styrene homopolymer, polyester resin, and acrylic resin with controlled molecular weights and monomer compositions, to enhance melt tension and foaming properties.

Benefits of technology

The composition achieves improved extrudability, melt tension, and foaming properties, resulting in high-quality foam sheets suitable for applications like food containers and packaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146542000001
    Figure 2024146542000001
  • Figure 2024146542000002
    Figure 2024146542000002
Patent Text Reader

Abstract

To provide a styrene-based resin composition having excellent extrudability, melt tension and foaming characteristics, a foamed sheet which is a foamed body of the styrene-based resin composition, and a food container which is a molding of the foamed sheet.SOLUTION: A styrene-based resin composition contains a styrene-based resin (A), a polarity-imparting material (B) and an acrylic resin (C). When the total of the styrene-based resin (A), the polarity-imparting material (B) and the acrylic resin (C) is 100 pts.mass, the styrene-based resin composition contains the styrene-based resin (A) by 80 to 90 pts.mass, the polarity-imparting material (B) by 5 to 10 pts.mass, and the acrylic resin (C) by 5 to 10 pts.mass, and the polarity-imparting material (B) is a polyester-based resin and / or styrene-methacrylic acid copolymer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a styrenic resin composition containing a polarizing agent and an acrylic resin. [Background technology]

[0002] Extruded foam sheets of styrene resins are excellent in light weight, rigidity, and moldability, and are therefore widely used for food packaging containers such as food trays, lunch boxes, instant noodle containers, natto containers, cups, etc. In addition, plate-shaped extruded foams of styrene resins have excellent heat insulation properties and mechanical strength, and are therefore used in various fields such as flooring, wall materials, ceiling materials, and core materials for tatami mats in general buildings.

[0003] Patent Document 1 discloses a styrene-based resin composition containing a polyester-based resin, which has an excellent balance between heat resistance and sheet strength. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] WO2021 / 039400 [Patent Document 2] WO2020 / 054536 Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the styrene-based resin compositions disclosed in Patent Documents 1 and 2, there are cases where extrusion is difficult, where the melt tension is reduced, and where the foaming properties are deteriorated. Therefore, the conditions for producing a styrene-based resin composition having good foaming properties while maintaining high extrudability and melt tension have been unknown.

[0006] An object of the present invention is to provide a styrene-based resin composition having excellent extrudability, melt tension and foaming characteristics, a foamed sheet which is a foam of the styrene-based resin composition, and a food container which is a molded article of the foamed sheet. [Means for solving the problem]

[0007] (1) A styrene-based resin composition containing a styrene-based resin (A), a polarity-imparting material (B) and an acrylic resin (C), the styrene-based resin composition containing 80 to 90 parts by mass of the styrene-based resin (A), 5 to 10 parts by mass of the polarity-imparting material (B) and 5 to 10 parts by mass of the acrylic resin (C) when the total amount of the styrene-based resin (A), the polarity-imparting material (B) and the acrylic resin (C) is 100 parts by mass. (2) The styrene-based resin composition according to (1), wherein the polarizing agent (B) is a polyester-based resin and / or a styrene-methacrylic acid copolymer. (3) The styrene-based resin composition according to any one of (1) to (2), wherein the styrene-based resin (A) comprises a homopolymer of styrene. (4) The styrene-based resin composition according to any one of (1) to (3), wherein the acrylic resin (C) has a mass average molecular weight (Mw) of 1.5 million or more and 6 million or less. (5) The styrene-based resin composition according to any one of (1) to (4), wherein the acrylic resin (C) contains 60% by mass or more of methyl methacrylate as a structural unit. (6) A foamed sheet which is a foam of the styrene-based resin composition according to any one of (1) to (5). (7) A food container which is a molded product of the foamed sheet according to (6). Effect of the Invention

[0008] The resin composition of the present invention has improved melt tension even when a small amount of the polarizing agent (B) and the acrylic resin (C) is added, and the melt tension is easily controlled. The resin composition of the present invention has excellent processability due to its high extrudability and melt tension, and is advantageous for producing a foamed sheet due to its excellent foaming characteristics. The molded product of the foamed sheet can be advantageously used for applications such as food containers and packaging, office automation equipment, home appliance parts, and miscellaneous goods. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, embodiments of the present invention will be described. The features of the embodiments described below can be combined with each other. Also, each feature can be an invention independently.

[0010] [Styrene-based resin composition] A styrene-based resin composition according to one embodiment of the present invention contains a styrene-based resin (A), a polarity-imparting agent (B) and an acrylic resin (C).

[0011] When the total of the styrene resin (A), the polarity imparting material (B) and the acrylic resin (C) is 100 parts by mass, the content of the styrene resin (A) is 80 to 90 parts by mass. Specifically, for example, it may be within the range of any two values ​​among 80, 81, 82, 83, 84, 85, 86, 87, 88, 89 and 90 parts by mass. In addition, when the styrene resin (A) is used in combination, the amount of the styrene resin (A) used means the total amount of the styrene resin (A) used in combination.

[0012] When the total of the styrene resin (A), the polarity imparting material (B) and the acrylic resin (C) is 100 parts by mass, the content of the polarity imparting material (B) is 5 to 10 parts by mass. Specifically, for example, it may be within the range of any two values ​​among 5, 6, 7, 8, 9 and 10 parts by mass. In addition, when the polarity imparting material (B) is used in combination, the amount of the polarity imparting material (B) used means the total amount of the polarity imparting material (B) used in combination. When the content of the polarity imparting material (B) exceeds 15 parts by mass, the closed cell ratio of the styrene resin composition decreases (the foaming characteristics deteriorate). When the content of the polarity imparting material (B) is less than 3 parts by mass, the melt tension of the styrene resin composition decreases.

[0013] When the total of the styrene resin (A), the polarity imparting material (B) and the acrylic resin (C) is 100 parts by mass, the content of the acrylic resin (C) is 5 to 10 parts by mass. Specifically, for example, it may be within the range of any two values ​​among 5, 6, 7, 8, 9 and 10 parts by mass. In addition, when the acrylic resin (C) is used in combination, the amount of the acrylic resin (C) used means the total amount of the acrylic resin (C) used in combination. When the content of the acrylic resin (C) exceeds 15 parts by mass, the extrudability of the styrene resin composition decreases. When the content of the acrylic resin (C) is less than 5 parts by mass, the melt tension of the styrene resin composition decreases and the closed cell ratio decreases (the foaming characteristics deteriorate), or the melt tension of the styrene resin composition decreases.

[0014] <Styrene-based resin (A)> The styrene-based resin (A) is obtained by radical polymerization of an aromatic vinyl compound monomer, and may be modified into rubber by adding a conjugated diene rubber-like polymer as necessary. The polymerization method may be a known method, such as bulk polymerization, two-stage bulk / suspension polymerization, or solution polymerization. The aromatic vinyl compound monomer is a monocyclic or polycyclic aromatic vinyl monomer, such as styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, 2,5-dimethylstyrene, 3,4-dimethylstyrene, 3,5-dimethylstyrene, p-ethylstyrene, m-ethylstyrene, o-ethylstyrene, p-tert-butylstyrene, 1-vinylnaphthalene, 2-vinylnaphthalene, 1,1-diphenylethylene, isopropenylbenzene (α-methylstyrene), isopropenyltoluene, isopropenylethylbenzene, and the like. The aromatic vinyl monomer may be used alone or in combination of two or more of styrene, isopropenylpropylbenzene, isopropenylbutylbenzene, isopropenylpentylbenzene, isopropenylhexylbenzene, isopropenyloctylbenzene, etc., and preferably styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, 2,5-dimethylstyrene, 3,4-dimethylstyrene, 3,5-dimethylstyrene, p-ethylstyrene, m-ethylstyrene, o-ethylstyrene, p-tert-butylstyrene. The aromatic vinyl monomer may be used alone or in combination of two or more. The homopolymer of the styrene monomer is obtained by polymerizing a styrene monomer, which is an aromatic vinyl monomer. The homopolymer of the styrene monomer means a polymer of only a styrene monomer, and may be a copolymer of two or more styrene monomers.

[0015] Conjugated diene rubbery polymers used for rubber modification of the styrene resin (A) include polybutadiene, random or block copolymers of styrene-butadiene, polyisoprene, polychloroprene, random, block or graft copolymers of styrene-isoprene, ethylene-propylene rubber, ethylene-propylene-diene rubber, etc., with polybutadiene and random, block or graft copolymers of styrene-butadiene being particularly preferred. These may also be partially hydrogenated.

[0016] The styrene-based resin (A) is preferably a homopolymer of a styrene-based monomer, and more preferably a homopolymer of styrene (polystyrene). In one embodiment, the styrene-based resin (A) does not include a styrene-methacrylic acid copolymer.

[0017] <Mass average molecular weight (Mw)> From the viewpoint of strength and moldability, the styrene resin (A) preferably has a mass average molecular weight (Mw) of 50,000 to 700,000, more preferably 150,000 to 400,000. Specifically, for example, it may be 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, or 700,000, and may be within a range between any two of the numerical values ​​exemplified here. By setting it in such a range, a styrene resin composition having an excellent balance of extrudability, melt tension, and foaming properties can be obtained. The mass average molecular weight (Mw) of the homopolymer of the styrene monomer can be controlled by the reaction temperature and residence time in the polymerization step, the type and amount of the polymerization initiator, the type and amount of the chain transfer agent, the type and amount of the solvent used during polymerization, and the like.

[0018] The weight average molecular weight (Mw) can be measured, for example, by using gel permeation chromatography (GPC) under the following conditions. GPC model: Showa Denko Co., Ltd. Shodex GPC-101 Column: Polymer Laboratories PLgel 10 μm MIXED-B Mobile phase: Tetrahydrofuran Sample concentration: 0.2% by mass Temperature: oven 40℃, injection port 35℃, detector 35℃ Detector: Differential refractometer

[0019] The molecular weight is calculated as a polystyrene-equivalent molecular weight by calculating the molecular weight at each elution time from the elution curve of monodisperse polystyrene.

[0020] <Glass transition temperature (Tg)> From the viewpoints of heat resistance and moldability, the homopolymer of the styrene-based monomer according to this embodiment preferably has a glass transition temperature (Tg) of 50 to 160° C., more preferably 70 to 120° C. The glass transition temperature (Tg) can be controlled, for example, by adjusting the mass average molecular weight of the monomer and copolymer constituting the homopolymer. The glass transition temperature (Tg) can be measured, for example, using an EXTER DSC6200 manufactured by SII Corporation, by raising the temperature from 20° C. at a rate of 10° C. / min.

[0021] The polymerization method of the styrene-based resin (A) may be a known styrene polymerization method such as bulk polymerization, solution polymerization, suspension polymerization, or emulsion polymerization. In terms of quality and productivity, bulk polymerization and solution polymerization are preferred, and continuous polymerization is preferred. As the solvent, for example, alkylbenzenes such as benzene, toluene, ethylbenzene, and xylene, ketones such as acetone and methyl ethyl ketone, and aliphatic hydrocarbons such as hexane and cyclohexane can be used.

[0022] In the case of continuous polymerization, first, a known complete mixing tank type stirring tank or tower type reactor is used in the polymerization process, and the polymerization reaction is controlled by adjusting the polymerization temperature, etc., so as to achieve the target molecular weight, molecular weight distribution, and reaction conversion rate. The polymer solution containing the polymer that has left the polymerization process is transferred to a devolatilization process, where unreacted monomers and polymerization solvent are removed. The devolatilization process is composed of a vacuum devolatilization tank equipped with a heater or a devolatilization extruder equipped with a vent. The molten polymer that has left the devolatilization process is transferred to a granulation process. In the granulation process, the molten resin is extruded in the form of strands from a multi-hole die, and processed into pellets by a cold cut method, an air hot cut method, or an underwater hot cut method.

[0023] During polymerization of the styrene-based resin (A), a polymerization initiator and a chain transfer agent can be used as necessary. As the polymerization initiator, a radical polymerization initiator is preferable, and examples of the polymerization initiator include peroxyketals such as 1,1-di(t-butylperoxy)cyclohexane, 2,2-di(t-butylperoxy)butane, 2,2-di(4,4-di-t-butylperoxycyclohexyl)propane, and 1,1-di(t-amylperoxy)cyclohexane, hydroperoxides such as cumene hydroperoxide and t-butyl hydroperoxide, alkyl peroxides such as t-butyl peroxyacetate and t-amyl peroxy isononanoate, t-butyl cumyl peroxide, di-t-butyl peroxide, dicumyl peroxide, and di-t-hexyl peroxide. Examples of the dialkyl peroxide include dialkyl peroxides such as t-butyl peroxyacetate, t-butyl peroxybenzoate, and t-butyl peroxyisopropyl monocarbonate; peroxyesters such as t-butyl peroxyisopropyl carbonate and polyether tetrakis(t-butyl peroxycarbonate); peroxycarbonates such as N,N'-azobis(cyclohexane-1-carbonitrile), N,N'-azobis(2-methylbutyronitrile), N,N'-azobis(2,4-dimethylvaleronitrile), and N,N'-azobis[2-(hydroxymethyl)propionitrile], and these may be used alone or in combination of two or more. Examples of the chain transfer agent include aliphatic mercaptans, aromatic mercaptans, pentaphenylethane, α-methylstyrene dimer, and terpinolene.

[0024] <Polarizing material (B)> The polarizing agent (B) may be a polyester resin and / or a styrene-methacrylic acid copolymer.

[0025] [Polyester resin] The polyester resin used in the present invention is a general term for polymers having an ester bond obtained by polymerizing a monomer containing a carboxylic acid and an alcohol.

[0026] Polyester-based resins can be obtained, for example, by polymerization of dicarboxylic acids and diols. Examples of such polyester-based resins include polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, polybutylene naphthalate, polyhexamethylene terephthalate, and polyhexamethylene naphthalate, but the present invention is not limited to these.

[0027] From the viewpoint of reducing carbon dioxide emissions, the polyester resin is preferably polylactic acid, which is a plant-derived raw material.

[0028] In the case of poly(L-lactic acid), the crystallization speed varies depending on the ratio of the D-lactic acid component. Considering the heat resistance and moldability of the resin composition of the present invention, the ratio of the D-lactic acid component is preferably 0.01 mol% or more and 5.0 mol% or less. The range of 0.01 mol% or more and 1.5 mol% or less is particularly preferable.

[0029] The molecular weight of the polyester resin is preferably in the range of mass average molecular weight (Mw) of 50,000 or more and 400,000 or less, and particularly preferably in the range of 100,000 or more and 300,000 or less.

[0030] [Styrene-methacrylic acid copolymer] Styrene-methacrylic acid copolymers can be obtained by copolymerizing styrene monomers and methacrylic acid monomers by radical polymerization using heat or a peroxide catalyst. As the polymerization method, known styrene polymerization methods such as bulk polymerization, solution polymerization, and suspension polymerization can be used.

[0031] The content of methacrylic acid in the styrene-methacrylic acid copolymer is preferably 1 to 15 mass%, more preferably 2 to 12 mass%, and particularly preferably 2 to 10 mass%. The content of methacrylic acid can be adjusted by the concentration of methacrylic acid in the raw material liquid in the polymerization step.

[0032] The mass average molecular weight (Mw) of the styrene-methacrylic acid copolymer of the present invention is preferably 160,000 or more. When Mw is 160,000 or more, a styrene-based resin composition having a good balance between strength and moldability can be obtained. The Mw of the styrene-methacrylic acid copolymer can be adjusted by the reaction temperature and residence time in the polymerization process, the type and amount of polymerization initiator, the type and amount of chain transfer agent, the type and amount of solvent used during polymerization, etc.

[0033] The mass average molecular weight (Mw) of the styrene-methacrylic acid copolymer can be calculated by the method for calculating the mass average molecular weight (Mw) of the styrene-based resin (A).

[0034] <Acrylic resin (C)> The acrylic resin (C) refers to a polymer obtained by polymerization of an acrylic monomer or the like.

[0035] The mass average molecular weight (Mw) of the acrylic resin (C) is preferably 1.5 million or more and 6 million or less, and more preferably 1.5 million or more and 4.5 million or less.

[0036] The type of monomer for the acrylic resin (C) is not particularly limited as long as it does not impair the effects of the present invention. For example, homopolymers of acrylate monomers such as methyl acrylate, ethyl acrylate, isopropyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, benzyl acrylate, cyclohexyl acrylate, phenyl acrylate, and chloroethyl acrylate, and homopolymers of methacrylate monomers such as methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, benzyl methacrylate, cyclohexyl methacrylate, phenyl methacrylate, and chloroethyl methacrylate, and copolymers obtained by copolymerizing two or more of these monomers can be used.

[0037] The constituent units of the acrylic resin (C) may be mainly composed of methyl methacrylate units. The content of methyl methacrylate units in the acrylic resin (C) is preferably 60% by mass or more, and may be 70% by mass or more, 80% by mass or more, 90% by mass or more, 95% by mass or more, 99% by mass or more, 99.9% by mass or more, or 100% by mass or more. The content of methyl methacrylate units in the acrylic resin (C) can be adjusted by the concentration of methyl methacrylate in the raw material liquid in the polymerization step.

[0038] The acrylic resin (C) may be one obtained by adding and polymerizing, in addition to these acrylic monomers, vinyl monomers (excluding aromatic vinyl compound monomers) copolymerizable therewith, so long as the effects of the present invention are not impaired. For example, monomers such as α-olefins, unsaturated nitriles, unsaturated carboxylic acid esters, and polyunsaturated compounds such as ethylene glycol di(meth)acrylate may be added.

[0039] Examples of the polymerization method for the acrylic resin (C) include known polymerization methods such as emulsion polymerization, soap-free emulsion polymerization, fine suspension polymerization, suspension polymerization, bulk polymerization, solution polymerization, etc. Among these polymerization methods, emulsion polymerization is preferred because it is easy to produce a high molecular weight substance.

[0040] When the acrylic resin (C) is produced by emulsion polymerization, a known emulsifier can be used, such as an anionic emulsifier, a nonionic emulsifier, a polymer emulsifier, or a reactive emulsifier having a radically polymerizable unsaturated double bond in the molecule.

[0041] <Other ingredients> To the resin composition of the present invention, other additives, for example, known additives such as reinforcing materials, flame retardants, dyes and pigments, coloring inhibitors, lubricants, antioxidants, antiaging agents, light stabilizers, antistatic agents, fillers, crystallization nucleating agents, and compatibilizers, and modifiers such as colorants such as titanium oxide and carbon black, can be added within the scope of the present invention. The method of adding these is not particularly limited, and they may be added by known methods. For example, a method of adding them in the raw material charging process, polymerization process, and finishing process during the production of the styrene-based resin (A), the polarizing agent (B), or the acrylic resin (C), or a method of adding them in the process of mixing the resin composition using an extruder or a molding machine can be applied.

[0042] <Method of producing resin composition> The method for mixing the resin composition of the present invention is not particularly limited, and known mixing techniques can be applied. For example, a homogeneous resin composition can be produced by mixing various raw materials in advance using a mixing device such as a mixer-type mixer, a V-type blender, and a tumbler-type mixer, and melt-kneading the mixture. The melt-kneading device is also not particularly limited, and examples thereof include a Banbury-type mixer, a kneader, a roll, a single-screw extruder, a special single-screw extruder, and a twin-screw extruder. Furthermore, there is also a method in which additives such as a flame retardant are added separately from the middle of a melt-kneading device such as an extruder.

[0043] The molding method for obtaining a molded article, film, sheet, or foam from the resin composition of the present invention is not particularly limited, and known molding methods such as extrusion molding methods such as calendar molding, blow molding, extrusion foam molding, profile extrusion molding, lamination molding, inflation molding, T-die film molding, sheet molding, vacuum molding, and pressure molding, and injection molding methods such as injection molding, RIM molding, and injection foam molding can be suitably used.

[0044] <Melt tension> The melt tension (MT) of the styrene resin composition measured at 200° C. is preferably 13 gf or more, more preferably 14 gf or more. If the melt tension is less than 13 gf, the thickness deviation of the styrene resin composition increases, and the compressive strength and drop strength of the food container decrease.

[0045] The melt tension value was measured using a Toyo Seiki "Capillograph 1B type" with a barrel temperature of 200°C, barrel diameter of 9.55 mm, capillary length: L = 10 mm, capillary diameter: D = 1 mm (L / D = 10), and extrusion speed in the barrel of 10 mm / min. The load measurement section was set 60 cm below the die, and the strand-like resin flowing out of the capillary was set on a winder. The winding linear speed was gradually increased from 4 m / min, and the load was measured until the strand broke. As the load was increased, it stabilized at a constant value, so the melt tension value was determined by averaging the range where the load was stable.

[0046] <Foam sheet> The foamed sheet of the present invention is a foamed product of the above-mentioned styrene-based resin composition.

[0047] Thickness The thickness of the foamed sheet of the present invention is 0.5 mm or more and 3.5 mm or less, preferably 1.5 mm or more and 2.5 mm or less, and more preferably 1.5 mm or more and 2.3 mm or less. When the thickness of the foamed sheet is within the above range, the sheet has excellent sheet strength and is easy to handle. When the thickness of the foamed sheet is equal to or more than the lower limit, the strength, heat resistance, and heat insulation are excellent. When the thickness of the foamed sheet is equal to or less than the upper limit, the thermoformability is good.

[0048] [Expansion ratio] The expansion ratio of the foamed sheet of the present invention is 1.1 times or more and 20.0 times or less, preferably 1.5 times or more and 15.0 times or less, and more preferably 1.7 times or more and 12.0 times or less. When the expansion ratio of the foamed sheet is within the above range, the sheet has excellent sheet strength and is easy to handle. When the expansion ratio of the foamed sheet is equal to or more than the lower limit, the sheet has excellent heat insulation properties, and when the expansion ratio of the foamed sheet is equal to or less than the upper limit, the sheet has excellent sheet strength.

[0049] [Average bubble diameter] The average bubble diameter of the foamed sheet of the present invention is 30 μm or more and 500 μm or less, preferably 50 μm or more and 350 μm or less, and more preferably 50 μm or more and 300 μm or less. If the average bubble diameter of the foamed sheet is within the above range, the foamed sheet has excellent sheet strength and is easy to handle. If the average bubble diameter of the foamed sheet is equal to or more than the above lower limit, the foamed sheet has good moldability and a good molded product can be obtained. If the average bubble diameter of the foamed sheet is equal to or less than the above upper limit, the foamed sheet becomes soft and is less likely to crack.

[0050] [Closed bubble rate] The closed cell ratio of the foamed sheet of the present invention is 50% or more, preferably 60% or more, and more preferably 70% or more. When the closed cell ratio of the foamed sheet is within the above range, the foamed sheet has excellent sheet strength and is easy to handle.

[0051] [Method of manufacturing foam sheet] The method for producing the foamed sheet of the present invention is not particularly limited, and examples thereof include a method in which the above-mentioned styrene-based resin composition, a nucleating agent, and the like are supplied to an extruder, heated and melted, a foaming agent is added and kneaded, extrusion foaming is performed through a die attached to the tip of the extruder, and the obtained foamed sheet is wound up and recovered.

[0052] The foaming agent may be any commonly used one, including chemical foaming agents such as azodicarbonamide, dinitrosopentamethylenetetramine, hydrazoyldicarbonamide, and sodium bicarbonate, and physical foaming agents such as saturated aliphatic hydrocarbons such as propane, normal butane, isobutane, normal pentane, isopentane, and hexane, ethers such as dimethyl ether, methyl chloride, carbon dioxide, and nitrogen.

[0053] Examples of the nucleating agent include talc, sodium hydrogen carbonate, ammonium hydrogen carbonate, calcium carbonate, clay, and citric acid. Among them, talc is preferable as the nucleating agent. The nucleating agent may be used alone or in combination of two or more. The amount of the nucleating agent to be added is preferably 0.01 parts by mass or more and 5 parts by mass or less with respect to 100 parts by mass of the styrene-based resin composition.

[0054] Examples of the die attached to the tip of the extruder include an annular die (circular die) having an annular opening, a T-die, etc. A specific embodiment when an annular die is used is, for example, a cylindrical foam extruded from the annular die is aligned along a cooling mandrel, and cut into two foam sheets by making slits in the axial direction of the cylindrical foam using cutters provided on both sides of the tip of the cooling mandrel.

[0055] There is no particular limitation on the method for controlling the thickness, expansion ratio, average cell diameter and closed cell ratio of the foamed sheet. For example, the expansion ratio increases by increasing the amount of the nucleating agent used. Also, the expansion ratio decreases by decreasing the amount of the foaming agent used. The thickness of the foamed sheet can be controlled by changing the amount and type of the foaming agent used. Also, the average cell diameter increases by decreasing the amount of the nucleating agent used.

[0056] [Thickness measurement method] The foam sheet was measured at 21 points at 50 mm intervals in the width direction, excluding 20 mm at both ends in the width direction. The thickness at these measurement points was measured to the minimum unit of 0.1 mm using a dial thickness gauge Peacock Model G (manufactured by Ozaki Seisakusho Co., Ltd.). The average of these measurements was taken as the thickness T (mm) of the foam sheet.

[0057] [Expansion ratio] Excluding 20 mm on both ends of the foam sheet in the width direction, cut out 10 pieces of 10 cm x 10 cm at equal intervals in the width direction and measure the mass (g) of each piece to the nearest 0.001 g. Average the mass (g) of each piece over 1 m. 2 The value converted to the mass per unit is called the basis weight M (g / m 2 From the thickness T (mm) and basis weight M, the apparent density ρ can be calculated using the following formula (1), and the expansion ratio can be calculated using the following formula (2). Apparent density ρ(g / cm 3 )=M / (T×10 3 ) · · · (1) Expansion ratio = true density / apparent density ρ (2)

[0058] [Method of measuring average bubble diameter] The average bubble diameter in the thickness direction of the sheet is determined. A vertical cross section of the foamed sheet in the extrusion direction is observed using a scanning electron microscope (JSM-6510, manufactured by JEOL Ltd.). A vertical line is drawn across the entire thickness of the foamed sheet, and the average chord length is calculated from the length of the line and the number of bubbles intersecting the line according to ASTM D2842-06 using the following formula (3), and the average bubble diameter can be calculated using the following formula (4). Average chord length = length of straight line / number of bubbles (3) Average bubble diameter (μm) = average chord length / 0.616 (4)

[0059] [Method for measuring closed cell ratio] The foam sheet is cut into test pieces measuring 25 mm long x 25 mm wide, and the number of test pieces is prepared so that when stacked, the thickness is approximately 25 mm. The volume (V1) of the prepared test pieces is measured using an air type specific gravity meter (Shimadzu Corporation, Accupyc II 1340TC-100cc). The total mass (M0) and apparent volume (V0) of each test piece are measured, and the closed cell ratio can be calculated using the following formula (5). Closed cell ratio (%) = (V0-V1) / (V0-M0 / true density) × 100 (5)

[0060] <Food containers> The food container of the present invention is a molded article of the foamed sheet of the present invention, and is a container for storing food.

[0061] The shape and dimensions of the food container of the present invention are not particularly limited, and examples thereof include a cup for instant noodles and a bowl. The food container of the present invention can be obtained by thermoforming the foamed sheet of the present invention.

[0062] Examples of thermoforming methods include conventionally known general forming methods such as vacuum forming, compressed air forming, and applications of these methods such as free drawing forming, plug and ridge forming, ridge forming, matched mold forming, straight forming, drape forming, reverse draw forming, air slip forming, plug assist forming, and plug assist reverse load forming. EXAMPLES

[0063] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to these.

[0064] The materials used in the examples and comparative examples are as follows.

[0065] [Styrene-based resin (A)] GPPS (Polystyrene, weight average molecular weight (Mw) 350,000, glass transition temperature (Tg) 105°C)

[0066] [Polarity imparting material (B)] PLA (“REVODA190” manufactured by Zhejiang Hisun Biomaterials Co., Ltd. D-lactic acid component ratio 0.5 mol%, mass average molecular weight (Mw) 200,000) Styrene-methacrylic acid copolymer (mass average molecular weight (Mw) 200,000, glass transition temperature (Tg) 122°C, methacrylic acid monomer 10 parts by mass)

[0067] [Acrylic resin (C)] An acrylic resin was prepared by the following manufacturing method. - Manufacturing method of acrylic resin (Mw: 1.5 million) - In a separable flask (capacity 5 liters) equipped with a thermometer, a nitrogen inlet tube, a cooling tube and a stirrer, 300 parts by mass of ion-exchanged water as a dispersion medium, 1.1 parts by mass of sodium dodecylbenzenesulfonate as an emulsifier, 0.007 parts by mass of n-octyl mercaptan as a chain transfer agent, 85 parts by mass of methyl methacrylate as a monomer, and 15 parts by mass of butyl acrylate were added. The atmosphere in the flask was replaced with nitrogen by passing a nitrogen stream through the separable flask. Next, the internal temperature was raised to 60°C, and 0.15 parts by mass of potassium persulfate and 5 parts by mass of ion-exchanged water were added. After that, the polymerization was terminated by continuing heating and stirring for 2 hours, and an acrylic resin latex was obtained. The obtained acrylic resin latex was cooled to 25°C, then dropped into 500 parts by mass of 70°C warm water containing 5 parts by mass of calcium acetate, and then heated to 90°C to cause coagulation. The obtained coagulated material was separated and washed, and then dried at 60°C for 12 hours to obtain an acrylic resin. The peak top molecular weight (Mp) of the acrylic resin was 1.5 million.

[0068] - Manufacturing method of acrylic resin (Mw: 4.5 million) - An acrylic resin (Mw: 4.5 million) was obtained under the same manufacturing conditions as the above-mentioned acrylic resin (Mw: 1.5 million), except that the peak top molecular weight (Mp) was changed by adjusting the amounts of various raw materials charged.

[0069] (Examples 1 to 6, Comparative Examples 1 to 7) The components were premixed in the amounts shown in Tables 1 and 2 in a Henschel mixer (Mitsui Miike Chemical Co., Ltd., FM20B), fed to a twin-screw extruder (Toshiba Machine Co., Ltd., TEM26SS) to make strands, cooled with water, and then fed to a pelletizer to be pelletized. The main operating conditions were as follows: Cylinder temperature setting: 180℃ (transport area) - 230℃ (mixing - weighing area) Screw rotation speed: 300 rpm Extrusion speed: 30kg / h Resin temperature: 240~250℃

[0070] [Extrusion] It was checked whether the resin overflowed from the vent during the pelletization. Resin compositions that were prone to overflowing were rated as x.

[0071] Extrudability: ○ (Can be manufactured), × (Problems such as bent-up and strand breakage occur. Cannot be manufactured)

[0072] [Melt tension] The pelletized resin composition was extruded using a Toyo Seiki Co., Ltd. "Capillograph Type 1B" (barrel temperature: 200°C, barrel diameter: 9.55 mm, capillary length: L = 10 mm, capillary diameter: D = 1 mm (L / D = 10), extrusion speed in barrel: 10 mm / min, load measurement section: set 60 cm below the die), and the strand-like resin flowing out of the capillary was set on a winder, and the winding linear speed was gradually increased from 4 m / min, and the load until the strand broke was measured. In Tables 1 and 2, "-" means that measurement was not possible.

[0073] The melt tension value stabilizes at a constant value when the load is increased by increasing the winding linear speed, so the melt tension value was determined by averaging the range in which the load was stable.

[0074] [Production of foam sheets] 0.6 parts by mass of a nucleating agent (manufactured by Toyo Styrene Co., Ltd.: "DSM1401A") was added to 100 parts by mass of the pelletized resin composition, and the mixture was put into a first extruder (manufactured by Plastics Engineering Research Institute Co., Ltd., diameter 40 mm) and heated at a cylinder temperature of 210 ° C. to knead and melt. Next, 1.6 parts by mass of carbon dioxide was injected as a foaming agent from an injection port provided in the middle of the first extruder, relative to 100 parts by mass of the resin composition, and mixed with the resin composition. Then, the resin composition kneaded with the nucleating agent and the foaming agent was fed from the first extruder to a second extruder (manufactured by Plastics Engineering Research Institute Co., Ltd., diameter 50 mm), cooled to a resin temperature of 150 ° C. near the die outlet, and extrusion foamed using a circular die, to obtain a cylindrical body at a discharge rate of 10 kg / h. The obtained cylindrical body was cut at one point along the extrusion direction and taken up at 2.0 m / min to obtain a foamed sheet.

[0075] [Method for measuring closed cell ratio] The foamed sheet was cut into test pieces measuring 25 mm long x 25 mm wide, and the number of test pieces was prepared so that when stacked, the test pieces were approximately 25 mm thick. The volume (V1) of the test pieces was determined using an air type specific gravity meter (Shimadzu Corporation, Accupyk II 1340TC-100cc). The total mass (M0) and apparent volume (V0) of each test piece were measured, and the closed cell ratio was calculated using the following formula (1). Closed cell ratio (%) = (V0-V1) / (V0-M0 / true density) × 100 (1) In addition, "-" in Tables 1 and 2 means that measurement was not possible.

[0076] [Table 1]

[0077] [Table 2]

[0078] It was found from the Examples in Table 1 that the resin compositions of the present invention are excellent in extrudability, melt tension and foaming properties. On the other hand, from the Comparative Examples in Table 2, the resin compositions not satisfying the requirements of the present invention were inferior in melt tension and / or foaming properties, and the resin compositions with inferior extrudability were impossible to mold. [Industrial Applicability]

[0079] The resin composition of the present invention has excellent processability due to its high extrudability and melt tension, and is advantageous for producing a foamed sheet due to its excellent foaming properties. Furthermore, the molded product of the foamed sheet can be advantageously used for applications such as food containers and packaging, office automation equipment, home appliance parts, and miscellaneous goods, and has industrial applicability.

Claims

1. The styrene-based resin composition contains a styrene-based resin (A), a polarity-imparting material (B), and an acrylic resin (C), and the styrene-based resin composition contains 80 to 90 parts by mass of the styrene-based resin (A), 5 to 10 parts by mass of the polarity-imparting material (B), and 5 to 10 parts by mass of the acrylic resin (C), when the total of the styrene-based resin (A), the polarity-imparting material (B), and the acrylic resin (C) is 100 parts by mass.

2. 2. The styrene-based resin composition according to claim 1, wherein the polarizing agent (B) is a polyester-based resin and / or a styrene-methacrylic acid copolymer.

3. The styrene-based resin composition according to any one of claims 1 to 2, wherein the styrene-based resin (A) comprises a homopolymer of styrene.

4. The styrene-based resin composition according to any one of claims 1 to 3, characterized in that the mass average molecular weight (Mw) of the acrylic resin (C) is 1.5 million or more and 6 million or less.

5. The styrene-based resin composition according to any one of claims 1 to 4, characterized in that the acrylic resin (C) contains 60 mass% or more of methyl methacrylate as a structural unit.

6. A foamed sheet which is a foam of the styrene-based resin composition according to any one of claims 1 to 5.

7. A food container which is a molded article of the foamed sheet according to claim 6.

Citation Information