Heat radiation insulation resin sheet, laminate and semiconductor device
A balanced formulation of boron nitride agglomerated particles and solid filler in the resin sheet addresses the trade-off between thermal conductivity and insulation, ensuring effective heat dissipation and insulation in semiconductor devices under low-pressure molding.
Patent Information
- Application Number
- JP2023059607
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Insulating resin sheets used in power devices face a trade-off between thermal conductivity and insulation properties when pressed under low pressure to accommodate heat sinks with complex shapes, leading to potential damage and reduced insulation.
A heat dissipating insulating resin sheet is formulated with boron nitride agglomerated particles and a solid filler, where the average particle diameters of both components are closely matched, allowing for a balanced blend that maintains excellent insulation and thermal conductivity even under low-pressure molding.
The resin sheet achieves high thermal conductivity and insulation properties without damaging heat sinks, ensuring effective heat dissipation and electrical safety in semiconductor devices.
Smart Images

Figure 2024146604000005 
Figure 2024146604000006 
Figure 2024146604000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a heat dissipation insulation resin sheet, a laminate including the heat dissipation insulation resin sheet, and a semiconductor device including the laminate. [Background technology]
[0002] 2. Description of the Related Art Equipment equipped with semiconductor elements such as power devices often uses insulating heat dissipation substrates to dissipate heat generated during use. Insulating heat dissipation substrates used in power devices are required to have high thermal conductivity as a heat dissipation substrate and high insulation to prevent electrical conduction to the metals provided above and below the substrate. For this reason, the use of insulating resin sheets containing insulating heat dissipation fillers as insulating heat dissipation substrates has been considered, but there is a trade-off between thermal conductivity and insulation, and for example, when the insulating heat dissipation filler is highly filled, the thermal conductivity improves but the insulation tends to deteriorate. Therefore, from the viewpoint of effectively improving thermal conductivity with a small amount of insulating heat dissipation filler, there has also been consideration of improving the thermal conductivity of the insulating heat dissipation filler itself to be used.
[0003] For example, Patent Document 1 discloses a resin sheet containing 30 to 75 volume % of boron nitride agglomerated particles having an average particle size of 33 μm or 40 μm and 5 to 35 volume % of alumina having an average particle size of 8 μm, as a specific example of a resin sheet having excellent insulation and thermal conductivity and excellent adhesion to a metal plate. Patent Document 1 also discloses that the resin sheet is pressed at a pressure of 18 MPa. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2022 / 255450 Summary of the Invention [Problem to be solved by the invention]
[0005] Incidentally, when mounting an insulating resin sheet on a power device, the insulating resin sheet has been placed between a heat generating body and a heat sink and pressed at high pressure, but in recent years, heat sinks having various shapes, such as cooling fins with protrusions, have also been used. When mounting an insulating resin sheet on a power device using such a heat sink, pressing the insulating resin sheet at a relatively low pressure is required because pressing the insulating resin sheet at a high pressure may cause the heat sink to be damaged, such as by breaking the protrusions. Furthermore, the insulating resin sheet may be required to be press-molded under a relatively low pressure while curing, and then bonded to a metal base plate or copper foil. However, when the insulating resin sheet is pressed at a relatively low pressure and the boron nitride agglomerated particles are highly loaded, the thermal conductivity is improved but the insulating properties are reduced.
[0006] Therefore, an object of the present invention is to provide a heat dissipation insulation resin sheet that has excellent insulating properties and thermal conductivity even when press-molded at low pressure when highly loaded with boron nitride agglomerated particles. [Means for solving the problem]
[0007] The present inventors have discovered that the above problems can be solved by using boron nitride agglomerated particles and a solid filler in a thermal insulation resin sheet, which have a relatively small difference in average particle size, adjusting the blending balance of the boron nitride agglomerated particles and the solid filler, and setting the content of the boron nitride agglomerated particles within a predetermined range. That is, the present invention provides the following [1] to [7].
[0008] [1] A thermal insulation resin sheet comprising a resin, boron nitride agglomerated particles, and a solid filler, wherein an average particle diameter (d50)A of the boron nitride agglomerated particles and an average particle diameter (d50)B of the solid filler satisfy the following formula (1), the content of the boron nitride agglomerated particles is, by volume, from 4 to 50 times the content of the solid filler, and the content of the boron nitride agglomerated particles is from 40 to 70 volume% of the total amount of the thermal insulation resin sheet.
number
[0009] According to the present invention, when boron nitride agglomerated particles are highly loaded, a heat dissipation insulation resin sheet having excellent electrical insulation properties and thermal conductivity can be provided even when press-molded at a low pressure. [Brief description of the drawings]
[0010] [Figure 1] 1 is a schematic cross-sectional view showing a laminate including a heat dissipation insulation resin sheet of the present invention. [Diagram 2] 1 is a schematic cross-sectional view showing a laminate including a heat dissipation insulation resin sheet of the present invention. [Diagram 3]1 is a schematic cross-sectional view showing a semiconductor device provided with a heat dissipation and insulation resin sheet of the present invention. [Figure 4] 1 is a schematic cross-sectional view showing a semiconductor device provided with a heat dissipation and insulation resin sheet of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] [Heat dissipation and insulation resin sheet] The thermal insulation resin sheet of the present invention is a thermal insulation resin sheet containing resin, boron nitride agglomerated particles, and solid filler, in which the average particle size A of the boron nitride agglomerated particles and the average particle size B of the solid filler satisfy the following formula (1). By satisfying the following formula (1), the difference in average particle size between the boron nitride agglomerated particles and the solid filler becomes small, and when the thermal insulation resin sheet is press-molded at low pressure, both thermal conductivity and insulation properties can be achieved. The principle behind this is unclear, but is presumed to be as follows. By having the average particle size of the solid filler be somewhat close to that of the boron nitride agglomerated particles, the boron nitride agglomerated particles are prevented from being crushed sideways and becoming oriented horizontally even when compressed, and a decrease in thermal conductivity can be suppressed. Therefore, even if the content of the boron nitride agglomerated particles is 70 volume % or less, sufficient thermal conductivity can be ensured, making it possible to achieve both insulation and thermal conductivity.
[0012]
number
[0013] In order to make it easier for the heat dissipation and insulation resin sheet of the present invention to have both thermal conductivity and insulation properties, the value of AB is preferably in the range of -15 μm to +15 μm, and more preferably in the range of -10 μm to +10 μm.
[0014] In addition, in the thermal insulation resin sheet of the present invention, the content of the boron nitride agglomerated particles is 4 to 50 times the content of the solid filler in volume ratio. If the content of the boron nitride agglomerated particles is less than 4 times the content of the solid filler in volume ratio, the content of the boron nitride agglomerated particles becomes insufficient, making it difficult to suppress a decrease in thermal conductivity while suppressing a decrease in insulation. If the content of the boron nitride agglomerated particles is more than 50 times the content of the solid filler in volume ratio, it becomes difficult to improve thermal conductivity without decreasing insulation. From these viewpoints, the content of the boron nitride agglomerated particles is preferably 4.5 to 40 times, more preferably 5 to 35 times, and even more preferably 7 to 20 times the content of the solid filler, by volume ratio.
[0015] Furthermore, the content of the boron nitride agglomerated particles is 40% by volume or more and 70% by volume or less based on the total volume of the thermal insulation resin sheet. If the content of the boron nitride agglomerated particles is less than 40% by volume, the content of the boron nitride agglomerated particles is insufficient, making it difficult to sufficiently improve thermal conductivity. If the content of the boron nitride agglomerated particles exceeds 70% by volume, voids increase during press molding at low pressure, making it difficult to impart excellent insulation to the thermal insulation resin sheet. From these viewpoints, the content of the boron nitride agglomerated particles is preferably 42% by volume or more and 67% by volume or less, and more preferably 45% by volume or more and 65% by volume or less.
[0016] (Boron nitride agglomerated particles) The boron nitride agglomerated particles are agglomerated particles formed by agglomerating primary particles of boron nitride particles. Generally, whether or not a boron nitride agglomerated particle is an agglomerated particle can be determined by, for example, observing a cross section by SEM. Note that, when the boron nitride agglomerated particle undergoes various processes such as press molding, it may maintain the shape of the boron nitride agglomerated particle, or it may be deformed, collapsed, or crushed. However, when the boron nitride agglomerated particle undergoes a process such as press molding after being mixed with a resin, it is not generally oriented even if it is deformed, collapsed, or crushed, and it exists in a certain degree of aggregation, so that, for example, by observing the above-mentioned cross section, it is suggested that it is a boron nitride agglomerated particle, and it can be determined whether or not it is a boron nitride agglomerated particle.
[0017] From the viewpoint of effectively enhancing the insulating properties and thermal conductivity, the boron nitride agglomerated particles blended into the thermal insulation resin sheet preferably have an average particle size of 15 μm or more and 50 μm or less, more preferably 20 μm or more and 45 μm or less, and even more preferably 25 μm or more and 40 μm or less. The average particle size of the aggregated particles can be measured using a laser diffraction particle size distribution analyzer. The average particle size is calculated by taking the particle size (d50) of the aggregated particles when the cumulative volume is 50%.
[0018] The method for producing the boron nitride aggregated particles is not particularly limited, and they can be produced by a known method. For example, they can be obtained by aggregating (granulating) the primary particles prepared in advance, and specifically, the spray drying method and the fluidized bed granulation method can be mentioned. The spray drying method (also called spray drying) can be classified into a two-fluid nozzle method, a disk method (also called rotary method), and an ultrasonic nozzle method, etc., depending on the spray method, and any of these methods can be applied. The method for producing agglomerated particles of boron nitride does not necessarily require a granulation step. For example, agglomerated particles may be formed by natural aggregation of primary particles of boron nitride as crystals of boron nitride crystallized by a known method grow. Examples of boron nitride agglomerated particles include "UHP-G1H" manufactured by Showa Denko KK and "HP-40" manufactured by Mizushima Ferroalloy Co., Ltd.
[0019] The average major axis of the primary particles of the boron nitride agglomerated particles is not particularly limited, but is preferably 1 μm or more, more preferably 1.5 μm or more, even more preferably 2.0 μm or more, and is preferably 20 μm or less, more preferably 15 μm or less, even more preferably 10 μm or less. The average aspect ratio, determined by the major axis and minor axis of the primary particles of the boron nitride agglomerated particles, is preferably 1 or more, more preferably 2 or more, and is preferably 7 or less, more preferably 6 or less. The average aspect ratio and the average major axis are determined from the major axis and minor axis of the primary particle diameter of the boron nitride agglomerated particles measured on a cross section exposed by a cross section polisher. First, a cross section of the cured resin sheet is exposed by a cross section polisher, and the exposed cross section is observed by a scanning electron microscope (SEM) at 400 to 1200 times to obtain an observation image. In the observation image, the major axis and minor axis of 200 randomly selected primary particles of boron nitride particles are measured using image analysis software, and the aspect ratio of each particle is calculated from the major axis / minor axis, and the average value of the 200 particles is taken as the average aspect ratio. The average value of the major axes of the measured 200 primary particles is taken as the average major axis. The major axis is the length of the longest part of the primary particle of the boron nitride particles observed in the observation image. The minor axis is the length in the direction perpendicular to the major axis direction in the observation image.
[0020] (Solid filler) As the solid filler, a thermally conductive filler other than the above-mentioned boron nitride agglomerated particles may be used. The thermally conductive filler has, for example, a thermal conductivity of 10 W / (m·K) or more, preferably 15 W / (m·K) or more, and more preferably 20 W / (m·K) or more. The upper limit of the thermal conductivity of the thermally conductive filler is not particularly limited, but may be, for example, 1000 W / (m·K) or less, 300 W / (m·K) or less, or 200 W / (m·K) or less. Furthermore, as described above, by using a solid filler whose average particle size differs from the average particle size of the boron nitride agglomerated particles by 20 μm or less, it is possible to impart excellent thermal conductivity and insulation properties to the heat dissipation insulation resin sheet even when the sheet is pressed at low pressure. The thermal conductivity of the solid filler can be measured, for example, by a periodic heating thermoreflectance method using a thermal microscope manufactured by Bethel Corporation on a cross section of the filler machined with a cross section polisher.
[0021] The solid filler is preferably at least one selected from the group consisting of silicon oxide (silica), alumina, aluminum nitride, magnesium oxide, zinc oxide, aluminum hydroxide, and silicon carbide, more preferably at least one selected from the group consisting of aluminum nitride and alumina, and even more preferably aluminum nitride. By using these solid fillers, it becomes easier to prevent the insulation from decreasing while maintaining the thermal conductivity more favorably. The solid filler may be used alone or in combination of two or more kinds.
[0022] A solid filler is a filler that has substantially no voids inside, and is different from an agglomerated particle that is formed by agglomerating primary particles and has voids inside. The solid filler preferably has a rounded shape, which makes it easier to impart excellent thermal conductivity and insulating properties to the heat dissipation and insulation resin sheet.
[0023] The rounded filler is a filler having a sphericity of 0.75 or more, for example, a spherical filler. The spherical filler may be a perfect sphere, but is not limited to a perfect sphere. In this specification, a filler having a sphericity of 0.95 or more is defined as a spherical filler. The upper limit of the sphericity of the spherical filler or the rounded filler is 1. In addition to spherical fillers, polyhedral fillers may be rounded fillers. Examples of polyhedral fillers include hexahedrons such as cubes, octahedrons, and polyhedrons with octahedrons or more such as truncated octahedrons. Of course, the solid filler may be other than a spherical filler or a filler having a multi-faceted shape. The solid filler may be a filler other than a rounded filler having a sphericity of less than 0.75. Specific examples of fillers other than rounded fillers include fillers having an irregular shape such as a crushed shape, a plate shape, a needle shape, a fiber shape, a tube shape, and the like.
[0024] The average particle size of the solid filler is preferably 5 μm or more and 70 μm or less, more preferably 10 μm or more and 65 μm or less, and even more preferably 15 μm or more and 45 μm or less. When the average particle size is within these ranges, the difference with the average particle size of the boron nitride agglomerated particles is kept to a certain level or less, and it becomes easy to impart excellent thermal conductivity and insulation properties to the heat dissipation insulation resin sheet. In addition, when the average particle size is equal to or more than the above lower limit, it becomes easy to appropriately prevent the agglomerated particles from being compressed and deformed by pressing. The average particle size of the solid filler can be measured using a laser diffraction particle size distribution analyzer. The average particle size is calculated by taking the particle size (d50) of the aggregated particles when the cumulative volume is 50%.
[0025] The solid filler content is preferably 0.8% by volume or more and 17% by volume or less, more preferably 1% by volume or more and 15% by volume or less, and even more preferably 1.5% by volume or more and 10% by volume or less, based on the total volume of the thermal insulation resin sheet. When the solid filler content is within these ranges, the compounding ratio with the boron nitride agglomerated particles is appropriately controlled, making it easier to impart excellent thermal conductivity and insulation properties to the thermal insulation resin sheet.
[0026] (resin) The type of resin contained in the heat dissipation insulation resin sheet of the present invention is not particularly limited, but it preferably contains a thermosetting resin, and more preferably contains a thermosetting resin and a curing agent.
[0027] <Thermosetting resin> The thermosetting resin is not particularly limited, but examples thereof include amino resins such as urea resins and melamine resins, phenolic resins, thermosetting urethane resins, epoxy resins, phenoxy resins, thermosetting polyimide resins, aminoalkyd resins, and benzoxazine resins. The thermosetting resins used in the heat dissipation insulation resin sheet may be used alone or in combination of two or more. Among the above, the thermosetting resin is preferably an epoxy resin.
[0028] The epoxy resin may be, for example, a compound containing two or more epoxy groups in the molecule, and may have a weight average molecular weight of less than 5,000. Specific examples of epoxy resins include styrene skeleton-containing epoxy resins, resorcinol type epoxy resins, bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, phenol novolac type epoxy resins, biphenol type epoxy resins, phenoxy type epoxy resins, naphthalene type epoxy resins, biphenyl type epoxy resins, phenylene ether type epoxy resins, fluorene type epoxy resins, phenol aralkyl type epoxy resins, naphthol aralkyl type epoxy resins, dicyclopentadiene type epoxy resins, anthracene type epoxy resins, epoxy resins having an adamantane skeleton, epoxy resins having a tricyclodecane skeleton, epoxy resins having a triazine nucleus in the skeleton, and glycidylamine type epoxy resins.
[0029] The epoxy equivalent of the epoxy resin is not particularly limited, but is, for example, 70 g / eq or more and 500 g / eq or less. The epoxy equivalent of the epoxy resin is preferably 80 g / eq or more, and preferably 400 g / eq or less, more preferably 350 g / eq or less. The epoxy equivalent can be measured, for example, according to the method specified in JIS K 7236. The above-mentioned epoxy resins may be used alone or in combination of two or more kinds.
[0030] The content of the thermosetting resin in the heat dissipation insulation resin sheet is preferably 10 vol% or more, more preferably 15 vol% or more, even more preferably 20 vol% or more, and is preferably 35 vol% or less, more preferably 30 vol% or less.
[0031] <Hardening agent> The above-mentioned thermosetting resin is preferably cured with a curing agent to bind the agglomerated particles of boron nitride and the solid filler. Examples of the curing agent include phenol compounds (phenolic heat curing agents), amine compounds (amine heat curing agents), imidazole compounds, and acid anhydrides. Among these, curing agents other than phenol compounds are preferred. The curing agents may be used alone or in combination of two or more.
[0032] Examples of the phenol compound include novolak type phenol, biphenol type phenol, naphthalene type phenol, dicyclopentadiene type phenol, aralkyl type phenol, and dicyclopentadiene type phenol. Examples of the amine compound include dicyandiamide, diaminodiphenylmethane, and diaminodiphenylsulfone.
[0033] Examples of the imidazole compound include 2-undecylimidazole, 2-heptadecylimidazole, 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1,2-dimethylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole trimellitate, and 1-cyanoethyl-2-phenylimidazolium trimethylate. Examples of the compound include melitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-methylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-dihydroxymethylimidazole.
[0034] Examples of acid anhydrides include styrene / maleic anhydride copolymer, benzophenone tetracarboxylic anhydride, pyromellitic anhydride, trimellitic anhydride, 4,4'-oxydiphthalic anhydride, phenylethynylphthalic anhydride, glycerol bis(anhydrotrimellitate) monoacetate, ethylene glycol bis(anhydrotrimellitate), methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, and trialkyltetrahydrophthalic anhydride.
[0035] The content of the curing agent in the heat dissipation insulation resin sheet is not particularly limited, but is preferably 0.1 vol. % or more, more preferably 0.2 vol. % or more, even more preferably 0.5 vol. % or more, and is preferably 15 vol. % or less, more preferably 12 vol. % or less, even more preferably 10 vol. % or less.
[0036] <Curing accelerator> The resin may further include a curing accelerator. The use of the curing accelerator increases the curing speed, allowing the thermosetting resin to be cured quickly, and the crosslinked structure in the heat dissipation insulation resin sheet to be uniform. In addition, the number of unreacted functional groups is reduced, resulting in a high crosslink density. The curing accelerator is not particularly limited, and conventionally known curing accelerators can be used. Specific examples include anionic curing accelerators such as imidazole compounds, cationic curing accelerators such as amine compounds, curing accelerators other than anionic and cationic curing accelerators such as phosphorus compounds and organometallic compounds, and radical curing accelerators such as peroxides. The content of the curing accelerator in the heat dissipation insulation resin sheet is, for example, 0.1 to 8 volume %, preferably 0.3 to 5 volume %. The curing accelerator may be used alone or in combination of two or more kinds.
[0037] The resin content in the heat dissipation insulation resin sheet is not particularly limited, but is preferably 10% by volume or more, more preferably 15% by volume or more, even more preferably 20% by volume or more, and preferably 55% by volume or less, more preferably 50% by volume or less, and even more preferably 45% by volume or less. If the resin content is equal to or greater than these lower limits, the boron nitride agglomerated particles and solid filler can be sufficiently bound after curing to obtain a sheet of a desired shape. If the resin content is equal to or less than these upper limits, a certain amount or more of the boron nitride agglomerated particles and solid filler can be contained, so that the thermal conductivity and insulation properties can be excellent.
[0038] (Other ingredients) In addition to the above-mentioned components, the thermal insulation resin sheet of the present invention may contain other additives such as a dispersant, a coupling agent such as a silane coupling agent, a flame retardant, an antioxidant, an ion scavenger, a tackifier, a plasticizer, a thixotropy imparting agent, and a colorant.
[0039] (Thickness) The thickness of the heat dissipation insulation resin sheet of the present invention is not particularly limited, but is, for example, 50 μm or more and 500 μm or less. If the thickness is 50 μm or more, it is easy to ensure a certain level of insulation and heat dissipation, and if the thickness is 500 μm or less, it is easy to make the circuit board and semiconductor device described below thinner. The thickness of the heat dissipation insulation resin sheet is preferably 60 μm or more, more preferably 70 μm or more, and preferably 400 μm or less, more preferably 200 μm or less.
[0040] The thermal conductivity of the heat dissipation insulation resin sheet is preferably 5 W / (m·K) or more. By setting the thermal conductivity to 5 W / (m·K) or more, the heat dissipation performance is excellent, and when used as a circuit board, the heat generated by the elements mounted on the circuit board can be efficiently released to the outside. Therefore, even if an element with a large amount of heat dissipation, such as a power element used in a power module, is mounted, the temperature of the element can be prevented from becoming too high. The thermal conductivity of the cured product of the heat dissipation insulation resin sheet is more preferably 10 W / (m·K) or more. In addition, the upper limit of the thermal conductivity of the heat dissipation insulation resin sheet is not particularly limited, but in practical use, it is about 30 W / (m·K). The thermal conductivity of the cured product of the heat dissipation insulation resin sheet can be measured by measuring the thermal conductivity in the thickness direction using the laser flash method.
[0041] The heat dissipation insulation resin sheet of the present invention can be cured by heating at a temperature equal to or higher than the curing temperature of the resin, as described below, to form a cured product of the heat dissipation insulation resin sheet. The curing is preferably performed by heating under pressure. The cured product of the heat dissipation insulation resin sheet can constitute a part of the laminate described below.
[0042] [Laminate] The heat dissipation insulation resin sheet of the present invention may be used in a laminate. As the laminate, for example, as shown in Fig. 1, a metal base plate 11 and a metal plate 12 are provided in addition to the heat dissipation insulation resin sheet 10 of the present invention, and a laminate 13 is provided in which the heat dissipation insulation resin sheet 10 and the metal plate 12 are provided on the metal base plate 11 in this order. The heat dissipation insulation resin sheet 10 is preferably a cured product in the laminate.
[0043] Since the metal base plate 11 and the metal plate 12 each function as a thermal conductor, it is preferable that they have a thermal conductivity of 10 W / (m·K) or more. Materials used for these include metals such as aluminum, copper, gold, and silver, as well as graphite sheets. From the viewpoint of more effectively increasing thermal conductivity, aluminum, copper, or gold is preferable, and aluminum or copper is more preferable. The thickness of the metal base plate 11 is preferably 0.1 to 5 mm, and the thickness of the metal plate 12 is preferably 10 to 3000 μm, and more preferably 10 to 1500 μm. The metal plate may be a plate such as a copper plate or a foil such as a copper foil.
[0044] The laminate 13 is preferably used as a circuit board. When used as a circuit board, the metal plate 12 in the laminate 13 may have a circuit pattern. The circuit pattern may be appropriately patterned according to the elements to be mounted on the circuit board. The circuit pattern is not particularly limited, but may be formed by etching or the like. In the circuit board, the metal base plate 11 is used as a heat sink or the like. The laminate 13 may include a metal base plate 21 having a convex shape as the metal base plate, as shown in Fig. 2. As the metal base plate 21 having a convex shape, for example, a heat sink formed of a heat dissipation fin or the like may be used. The specific shape of the metal base plate 21 having the convex shape is not particularly limited, and for example, pin fins, comb fins, corrugated fins, etc. can be suitably used.
[0045] (Breakdown voltage) The laminate of the present invention preferably has a breakdown voltage of 5 kV or more, more preferably 5.5 kV or more, and even more preferably 6.5 kV or more. When the breakdown voltage is equal to or more than the lower limit, it is possible to exhibit excellent insulation while maintaining good thermal conductivity. The higher the breakdown voltage, the better, and the upper limit is not particularly limited, but in practice, it is, for example, 20 kV or less, preferably 15 kV or less. The breakdown voltage can be obtained by the measurement method described in the examples.
[0046] [Method of manufacturing the heat dissipation and insulation resin sheet and laminate] The heat dissipation insulating resin sheet can be obtained by forming a curable resin composition containing a resin (for example, a thermosetting resin and a curing agent), boron nitride aggregated particles, a solid filler, and other components blended as necessary into a sheet. For example, the curable resin composition may be formed into a sheet by coating or laminating it on a support such as a release sheet. Here, the sheet-like refers to a thin, flat product whose thickness is small compared to its length and width, and the concept of a sheet also includes a film or layer formed on another member such as a support or a metal base plate. In this way, a heat dissipation insulating resin sheet before curing can be obtained by forming the curable resin composition into a sheet. The curable resin composition can be obtained by mixing the components by a known method. The curable resin composition may be diluted with a dilution solvent as necessary. In this case, the curable resin composition applied to a support or the like may be dried.
[0047] The curable resin composition formed into a sheet by coating, lamination, or the like (the heat dissipation insulating resin sheet before curing) may be cured by applying heat and pressure by press molding or the like. The press molding may be performed, for example, while the laminate is being manufactured. Specifically, the heat dissipation and insulation resin sheet may be placed between a metal base plate and a metal plate, and heated and pressurized to bond the metal base plate and the metal plate via the heat dissipation and insulation resin sheet. From the viewpoint of improving the production yield, two or more sheets of the curable resin composition may be prepared and disposed between the metal base plate and the metal plate. That is, two or more sheets of the curable resin composition may be laminated to form the heat dissipation insulation resin sheet.
[0048] The press molding may be performed at a pressure of, for example, 1 MPa to 12 MPa, preferably 3 MPa to 10 MPa. The press temperature may be, for example, 120°C to 230°C, preferably 140°C to 220°C, and the press time may be, for example, 30 minutes to 240 minutes, preferably 50 minutes to 200 minutes. In the press molding, pressing may be performed two or more times at different temperatures, for example, after hot pressing at 120°C to 160°C, hot pressing may be performed again at 170°C to 230°C. In the above press molding, by lowering the press pressure, even when a laminate is formed having a metal base plate with a convex shape, the metal base plate can be prevented from being damaged during pressing. Furthermore, by relatively lowering the press pressure as described above, the thermal insulation resin sheet of the present invention can prevent the boron nitride aggregate particles from being compressed and oriented in the lateral direction, thereby exhibiting excellent thermal conductivity.
[0049] The heat dissipation insulation resin sheet is preferably cured by heating during the press molding described above, but may be partially cured before press molding. When partially cured before press molding, the curing may be performed, for example, at 60°C to 130°C, preferably 70°C to 110°C, and the curing time may be, for example, 20 minutes to 120 minutes, preferably 30 minutes to 100 minutes. When partially cured before press molding, the partial curing may be performed while applying pressure, and the pressure in this case is preferably 1 MPa to 12 MPa, more preferably 3 MPa to 10 MPa.
[0050] [Semiconductor Devices] The laminate including the heat dissipation insulation resin sheet of the present invention is preferably used in a semiconductor device. Specifically, as shown in Fig. 3, a semiconductor device 15 includes a laminate 13 including a heat dissipation insulation resin sheet 10, a metal base plate 11, and a metal plate 12, and a semiconductor element 14 provided on the metal plate 12 of the laminate 13. The metal plate 12 is preferably patterned by etching or the like to have a circuit pattern.
[0051] Although two semiconductor elements 14 are shown in FIG. 3, the number of semiconductor elements 14 is not limited and may be any number as long as it is one or more. In addition to the semiconductor elements 14, other electronic components such as transistors (not shown) may be mounted on the metal plate 12. Each semiconductor element 14 is connected to the metal plate 12 via a connection conductive part 16 formed on the metal plate 12. The connection conductive part 16 is preferably formed of solder. Furthermore, a sealing resin 19 is provided on the surface of the laminate 13 on the metal plate 12 side. At least the semiconductor elements 14 are sealed with the sealing resin 19, and if necessary, the metal plate 12 may also be sealed with the sealing resin 19 together with the semiconductor elements 14. Although the semiconductor elements 14 are not particularly limited, it is preferable that at least one of them is a power element (i.e., a power semiconductor element), and thus the semiconductor device 15 is preferably a power module. The power module is used, for example, in an inverter or the like. Furthermore, the power module is used in industrial equipment such as elevators and uninterruptible power supplies (UPS), but its use is not particularly limited.
[0052] Leads 20 are connected to the metal plate 12. The leads 20 extend, for example, from the sealing resin 19 to the outside and connect the metal plate 12 to an external device or the like. Wires 17 may also be connected to the semiconductor element 14. The wires 17 may connect the semiconductor element 14 to another semiconductor element 14, the metal plate 12, or the like, as shown in FIG. 3. The semiconductor element 14 generates heat when power is supplied via the leads 20 or the like to operate, and the heat generated by the semiconductor element 14 is transmitted to the metal base plate 11 via the heat dissipating and insulating resin sheet 10 and dissipated from the metal base plate 11. The metal base plate 11 may be connected to a heat sink consisting of heat dissipating fins or the like as necessary. Moreover, the semiconductor device 15 may include, instead of the metal base plate 11, a metal base plate 21 having the above-mentioned convex shape, as shown in FIG.
[0053] The semiconductor device 15 may be manufactured through a reflow process in the manufacturing process. Specifically, in the manufacturing method of the semiconductor device 15, first, the laminate 13 is prepared, and the connection conductive portion 16 is formed on the metal plate 12 of the laminate 13 by solder printing or the like, and the semiconductor element 14 is mounted on the connection conductive portion 16. Thereafter, the laminate 13 on which the semiconductor element 14 is mounted is passed through the inside of a reflow furnace and heated in the reflow furnace, and the semiconductor element 14 is connected to the metal plate 12 by the connection conductive portion 16. The temperature in the reflow furnace is not particularly limited, but is, for example, about 200 to 300°C. In the manufacturing method of the semiconductor device 15, after the reflow process, the sealing resin 19 may be laminated on the laminate 13 to seal the semiconductor element 14. In addition, before sealing with the sealing resin 19, the wires 17, the leads 20, and the like may be attached as appropriate. Although the above describes an embodiment in which the semiconductor element 14 is connected to the metal plate 12 by a reflow process, the present invention is not limited to such an embodiment. For example, the laminate 13 (i.e., a circuit board) may be connected to another board (not shown) by a reflow process. EXAMPLES
[0054] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0055] [Various physical properties] Various physical properties were measured and evaluated by the following methods.
[0056] (Thermal Conductivity) The heat dissipation insulation resin sheets obtained in the examples and comparative examples were cut into 1 cm squares, and carbon black was sprayed on both sides to prepare measurement samples. The thermal conductivity of these samples was measured by the laser flash method using a measuring device called "Nanoflash" (NETZSCH, model number: LFA447) and evaluated according to the following criteria. <Evaluation criteria> ◎:10W / m·K or more ○: 5 W / m K or more and less than 10 W / m K ×: Less than 5 W / m K
[0057] (Breakdown voltage) A circular electrode of φ2 was formed on each laminate (6 cm × 6 cm) produced in the examples and comparative examples, and a voltage was applied to the electrode at a rate of 20 kV / min. The voltage at which the measurement sample caused dielectric breakdown was taken as the dielectric breakdown voltage.
[0058] [Ingredients used] The components used in each of the examples and comparative examples are as follows. (resin) <Thermosetting resin> Biphenyl type epoxy resin "YL6121HA" manufactured by Mitsubishi Chemical Corporation Bisphenol A epoxy resin "YD-127" manufactured by Nippon Steel Chemical & Material Co., Ltd. <Hardening agent> Amine compound: "Dicyandiamide" manufactured by Tokyo Chemical Industry Co., Ltd. Imidazole compound: Isocyanuric modified solid dispersion type imidazole "2MZA-PW" manufactured by Shikoku Kasei Co., Ltd.
[0059] (Boron nitride agglomerated particles) Mizushima Ferroalloy "HP-40", average particle size of agglomerated particles: 35μm (Aluminum Nitride (AIN)) "HF20a" manufactured by Tokuyama Corporation, average particle size 20 μm (used in Examples 1 and 3) Showa Denko "AlN3001", average particle size 30 μm (used in Example 2) "ANF-A-02" manufactured by Maruwa Co., Ltd., average particle size 3 μm (used in Comparative Example 1) (alumina) "DAW-20" manufactured by Denka Co., Ltd., average particle size 20 μm (used in Example 4) "AA3" manufactured by Sumitomo Chemical Co., Ltd., average particle size 3 μm (used in Comparative Example 2)
[0060] [Example 1] The thermosetting resin, curing agent, boron nitride aggregated particles, and solid filler shown in Table 1 were mixed in the amounts shown in Table 1 to obtain a curable resin composition. The curable resin composition was applied to a release PET sheet (thickness 40 μm) to a thickness of 200 μm, and dried in an oven at 50 ° C. for 10 minutes to form a heat dissipation insulation resin sheet made of the curable resin composition on the release PET sheet. Thereafter, the release PET sheet was peeled off, and both sides of the heat dissipation insulation resin sheet were sandwiched between a first metal layer (copper plate, thickness 500 μm) and a second metal layer (aluminum plate, thickness 1.0 mm), and vacuum pressed under conditions of a temperature of 195 ° C. and a pressure of 10 MPa to produce a laminate in which the first metal layer, the heat dissipation insulation resin sheet, and the second metal layer were laminated in this order.
[0061] [Examples 2 to 4, Comparative Examples 1 to 2] A laminate was produced in the same manner as in Example 1, except that the types and amounts of each component contained in the curable resin composition were changed as shown in Table 1.
[0062] [Table 1] *The content [volume %] of boron nitride agglomerated particles and solid filler shown in Table 1 is the content based on the total amount of the thermal insulation resin sheet.
[0063] As is clear from the above examples, the heat dissipation and insulation resin sheets of the respective examples which satisfy the requirements of the present invention had good thermal conductivity and insulation properties even when molded by low pressure pressing. In contrast, the resin sheet produced in Comparative Example 1 had a larger than predetermined difference in average particle size between the boron nitride agglomerated particles and the solid filler, resulting in reduced thermal conductivity. Also, the resin sheet produced in Comparative Example 2 had an excessively high content of boron nitride agglomerated particles, resulting in good thermal conductivity but reduced insulation. [Explanation of symbols]
[0064] 10 Insulating resin sheet 11 Metal base plate 12 metal plate 13 Laminate 14 Semiconductor elements 15 Semiconductor Devices 16 Conductive connection 17 Wire 19 Sealing resin 20 Lead 21 Metal base plate having a convex shape
Claims
1. A thermal insulation resin sheet comprising a resin, boron nitride agglomerated particles, and a solid filler, The average particle size (d50) A of the boron nitride agglomerated particles and the average particle size (d50) B of the solid filler satisfy the following formula (1), The content of the boron nitride agglomerated particles is 4 to 50 times the content of the solid filler by volume ratio; The thermal insulation resin sheet has a content of the boron nitride agglomerated particles of 40 volume % or more and 70 volume % or less based on the total volume of the thermal insulation resin sheet. [0010]
2. 2. The thermal insulation resin sheet according to claim 1, wherein the average particle diameter (d50) of the boron nitride agglomerated particles is 15 μm or more and 50 μm or less.
3. The thermal insulation resin sheet according to claim 1 , wherein the solid filler particles are rounded.
4. 3. A laminate comprising: the heat dissipation insulation resin sheet according to claim 1; a metal base plate; and a metal plate, the insulating resin sheet and the metal plate being disposed in this order on the metal base plate.
5. The laminate according to claim 4 , which is a circuit board.
6. The laminate according to claim 4 , wherein the metal plate has a circuit pattern.
7. A semiconductor device comprising the laminate according to claim 4 and a semiconductor element provided on the metal plate.
Citation Information
Patent Citations
Resin sheet, laminate, and semiconductor device
WO2022255450A1
Cited By
Insulation heat dissipation sheet
WO2026100666A1