Low thermal expansion block
A ceramic block with SiC-replaced fused silica powder addresses the need for high thermal conductivity and low expansion, ensuring stability in heated applications.
Patent Information
- Application Number
- JP2023059635
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Ceramic blocks used in heated environments require both high thermal conductivity and low thermal expansion to maintain dimensional accuracy and prevent deformation.
A low thermal expansion block composed of fused silica powder with a portion replaced by SiC powder, specifically 25 to 50% SiC by mass, to enhance thermal conductivity while controlling thermal expansion.
The block achieves improved thermal conductivity and reduced thermal expansion, minimizing deformation and thermal shock, making it suitable for molds and mounting tables in heated conditions.
Smart Images

Figure 2024146615000003 
Figure 2024146615000001 
Figure 2024146615000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a low thermal expansion block. [Background technology]
[0002] Ceramics are made by sintering raw material powders and are generally known as heat-resistant materials. Ceramic blocks have high strength and are used as components that are used at high temperatures. In recent years, they have been increasingly used as high-strength components with heat resistance, for example, for forming dies and mounting tables that form objects in a heated state. When used as a mold, a silica block mainly made of fused quartz, which has low thermal expansion, is used to maintain the dimensional accuracy of the molded object. For example, Patent Document 1 discloses a high-strength compound refractory material with heat resistance, mainly made of fused quartz, which has a low thermal expansion coefficient. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 56-78476 Summary of the Invention [Problem to be solved by the invention]
[0004] However, since the material to be molded is molded in a heated state, the ceramic block is required to have high thermal conductivity as well as high heat resistance. The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a low thermal expansion block which is made of ceramics and has excellent thermal conductivity. [Means for solving the problem]
[0005] The low thermal expansion block of the present invention, which solves the above-mentioned problems, is a low thermal expansion block obtained by molding and sintering a fused silica powder consisting of a coarse powder consisting of powder with a particle diameter of 100 μm or more, a medium powder consisting of powder with a particle diameter of 10 μm or more and less than 100 μm, and a fine powder consisting of powder with a particle diameter of less than 10 μm, and is characterized in that at least a portion of the fine powder is replaced with SiC powder, and the SiC powder is contained in an amount of 25 to 50 mass% when the whole is taken as 100 mass%. The low thermal expansion block of the present invention has improved thermal conductivity due to the SiC powder mixed with fused silica. The SiC powder content of 25 to 50 mass % prevents the coefficient of thermal expansion from becoming excessively large. [Brief description of the drawings]
[0006] [Figure 1] 4 is a cross-sectional photograph of the low thermal expansion blocks of samples A to G. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] The present invention will be specifically described below using embodiments.
[0008] [Embodiment] The low thermal expansion block of this embodiment is formed by sintering fused silica powder consisting of a coarse powder having a particle diameter of 100 μm or more, a medium powder having a particle diameter of 10 μm or more but less than 100 μm, and a fine powder having a particle diameter of less than 10 μm.
[0009] Fused silica powder is a powder made of particles whose main component is fused silica. Fused silica is a substance also known as quartz glass. In general, it is made of a glass-like amorphous material made by melting a high-purity siliceous material. In particular, fused silica is a material whose coefficient of thermal linear expansion at 1000°C is as low as about 0.05%. Incidentally, "made mainly of fused silica" refers to a state in which the content of fused silica is the highest, and preferably consists of only fused silica.
[0010] Fused silica is a material with low thermal expansion. Fused quartz, the main component of fused silica, is a material with a smaller thermal linear expansion coefficient than SiC. In other words, it reduces the volume change when exposed to high temperatures. Therefore, the low thermal expansion block of this embodiment is less susceptible to weakening of the structure and cracking, is less susceptible to damage due to thermal shock, and has improved heat resistance.
[0011] In this embodiment, coarse powder refers to powder with a particle diameter of 100 μm or more. Medium powder refers to powder with a particle diameter of 10 μm or more and less than 100 μm. Fine powder refers to powder with a particle diameter of less than 10 μm. These boundary values (especially the upper limit of fine powder) are values in this embodiment and may be changed within the scope of the technical common sense of a person skilled in the art. In the low thermal expansion block of this embodiment, at least a part of the fine powder is replaced with SiC powder, and the SiC powder is contained in an amount of 25 to 50 mass % when the whole is taken as 100 mass %.
[0012] SiC powder is a powder made up of particles whose main component is SiC. SiC is a material with high thermal conductivity of 270 (W / m K), and the inclusion of SiC powder improves the thermal conductivity of the low thermal expansion block. Note that "mainly made of SiC" refers to a state in which the SiC content is the highest, and preferably consists of only SiC.
[0013] The SiC powder is contained in an amount of 25 to 50 mass% when the entire low thermal expansion block is taken as 100 mass%. When the SiC powder is contained in an amount of 25 mass% or more, the thermal conductivity of the low thermal expansion block is improved. When the SiC powder is contained in an amount of less than 25 mass%, it becomes difficult to obtain the effect of improving the thermal conductivity. Furthermore, when the SiC powder is contained in an amount of more than 50 mass%, the thermal expansion coefficient of the low thermal expansion block becomes large, and deformation occurs easily. Furthermore, the thermal shock resistance is reduced.
[0014] The SiC powder replaces at least a portion of the fine powder. Here, the SiC powder that replaces a portion of the fine powder has a particle diameter of less than 10 μm (powder with a particle diameter included in the particle size distribution of the fine powder). By replacing at least a portion of the fine powder with the SiC powder, the dispersibility of the coarse powder, medium powder, and fine powder in the low thermal expansion block is improved.
[0015] It is preferable that the SiC powder replaces the powder with a small particle size (fine particle side powder) of the fused silica powder. It is preferable that the SiC powder does not replace the coarse particle powder. If the SiC powder replaces the coarse particle powder, the obtained low thermal expansion block will have an uneven distribution of SiC particles with a particle size of 100 μm or more. It is preferable to substitute the SiC powder from the powder with the smallest particle size (the powder on the finer side) of the fused silica powder. Substitution from the powder with the smallest particle size prevents the SiC powder from substituting the coarse powder. Substitution from the powder with the smallest particle size (the powder on the finer side) indicates that, when the SiC powder is substituted, the fine powder is substituted first, followed by the medium powder, and finally the coarse powder.
[0016] The low thermal expansion block of this embodiment is produced by molding and sintering a mixed powder in which at least a part of the fused silica powder is replaced with SiC powder. The sintering conditions are not limited as long as the mixed powder particles can be sintered. For example, the mixed powder can be heated and sintered under the conditions of 1000°C x 6 hours in an air atmosphere. The mixed powder can be molded by any method as long as it is moldable. For example, a castable made of the mixed powder can be prepared and placed in a mold of a predetermined shape.
[0017] In the low thermal expansion block of this embodiment, when the particle size distribution of the SiC powder contained in the mixed powder is measured, it is preferable that the SiC powder has a peak in the range of particle diameters of less than 10 μm (the range of particle diameters of the fine powder). By having a peak in the particle size distribution in this range, a sufficient amount of fine powder is contained to achieve the above-mentioned effects. Here, having a peak means having at least one sharp peak, and it is also possible to have multiple peaks in this particle size range.
[0018] The low thermal expansion block of this embodiment preferably has a thermal conductivity of 0.6 (W / m K) or more, and more preferably 0.8 (W / m K) or more. When the thermal conductivity is in this range, the effect of the SiC powder substitution can be more clearly confirmed.
[0019] The low thermal expansion block of this embodiment has a thermal expansion coefficient of preferably 0.1% or less, and more preferably 0.09% or less. Here, the thermal expansion coefficient is the thermal expansion coefficient at 600° C. When the thermal expansion coefficient is in this range, the effect of the SiC powder substitution can be more clearly confirmed. EXAMPLES
[0020] The present invention will now be described in detail with reference to examples. (Example) As an example, castables of samples A to G were prepared by thoroughly wet-mixing the mixed powders having the following compositions, adding a specified amount of water and kneading them in a mortar mixer, pouring them into a specified formwork on a vibration table, removing them from the formwork after natural curing for 48 hours, and drying them at 110°C for 24 hours. After that, they were heated and fired in the air at 1000°C for 6 hours to produce ceramic blocks (low thermal expansion blocks) of samples A to G. The mixed powder of sample A is a powder consisting of fused silica powder only, with the following components: coarse powder: 35 mass%, medium powder: 25 mass%, fine powder: 40 mass%. This sample corresponds to the reference sample.
[0021] The mixed powder of sample B is a powder consisting of fused silica powder with a coarse grain powder: 10 mass%, medium grain powder: 25 mass%, fine grain powder: 40 mass%, and SiC powder with a coarse grain powder: 25 mass%, medium grain powder: 0 mass%, fine grain powder: 0 mass%.
[0022] The mixed powder of sample C is a powder consisting of fused silica powder with a coarse grain powder: 15 mass%, medium grain powder: 10 mass%, fine grain powder: 25 mass%, and SiC powder with a coarse grain powder: 20 mass%, medium grain powder: 15 mass%, fine grain powder: 15 mass%.
[0023] The mixed powder of sample D is a powder consisting of fused silica powder with a coarse grain powder: 0 mass%, medium grain powder: 5 mass%, fine grain powder: 20 mass%, and SiC powder with a coarse grain powder: 35 mass%, medium grain powder: 20 mass%, fine grain powder: 20 mass%.
[0024] The mixed powder of sample E was composed of fused silica powder with a coarse powder content of 35 mass%, medium powder content of 25 mass%, and fine powder content of 15 mass%, and SiC powder with a coarse powder content of 0 mass%, medium powder content of 0 mass%, and fine powder content of 25 mass%.
[0025] The mixed powder of sample F was composed of fused silica powder with a coarse grain size of 25 mass%, medium grain size of 10 mass%, and fine grain size of 15 mass%, and SiC powder with a coarse grain size of 10 mass%, medium grain size of 15 mass%, and fine grain size of 25 mass%.
[0026] The mixed powder of sample G was composed of fused silica powder with a coarse powder content of 15 mass%, medium powder content of 5 mass%, and fine powder content of 5 mass%, and SiC powder with a coarse powder content of 20 mass%, medium powder content of 20 mass%, and fine powder content of 35 mass%. The particle size distribution of the SiC powder contained in the mixed powder of Samples A to G was measured (N=3), and the measurement results are shown in Table 1. The measurement of the particle size distribution was performed using a measuring device.
[0027] [Table 1]
[0028] The thermal conductivity, thermal expansion coefficient, porosity, bulk density, bending strength, and compressive strength of the produced ceramic blocks of samples A to G were measured, and the measurement results are shown in Table 2. In addition, cross-sectional photographs of the ceramic blocks of samples A to G were taken and shown in Figure 1. The thermal conductivity was measured by the laser flash method using a thermal conductivity measuring device. The temperature range for measuring thermal conductivity was set from room temperature to 1000°C, and the measurement was performed in an argon atmosphere. Table 2 shows the values at 600°C. The thermal expansion coefficient was measured using a thermal dilatometer from room temperature to 1000°C, and expressed as a percentage of the length at 50°C. (Table 2 shows the value at 600°C.) The porosity was measured by a method in accordance with JIS-R-2205 (underwater gravimetric method). The bulk density was measured by a method according to JIS-R-2205. The compressive strength was measured by a method according to JIS-R-2206. The bending strength was measured by a method conforming to JIS-R-2213.
[0029] [Table 2]
[0030] As shown in Figure 1, the more the SiC powder substitution ratio increases, the more particles (black dots) derived from the SiC powder can be confirmed. In particular, it was confirmed that the particles (black dots) derived from the SiC powder were unevenly distributed in the block of sample B. On the other hand, in samples E to F, it was confirmed that the particles (black dots) derived from the SiC powder were uniformly dispersed in a fine state. As shown in Table 2, the thermal conductivity increases as the substitution ratio of SiC powder increases. In addition, when the SiC powder is replaced with fine powder, the thermal expansion coefficient can be kept lower compared to the case of coarse powder. On the other hand, no significant changes were observed in the porosity and bulk density. When a large amount of coarse grain powder is substituted for SiC powder, the bending strength and compressive strength are increased significantly.
[0031] As described above, the ceramic blocks (low thermal expansion blocks) of samples E to F, which are made by replacing the fine powder without replacing the coarse powder so that the SiC powder content is 25 to 50 mass%, are blocks with high thermal conductivity and low thermal expansion coefficient. Due to these characteristics, the ceramic blocks (low thermal expansion blocks) of samples E to F are suitable materials for use in molds and mounting tables that mold the object to be molded in a heated state.
Claims
[Claim 1] A low thermal expansion block obtained by molding and sintering a fused silica powder including a coarse powder having a particle size of 100 μm or more, a medium powder having a particle size of 10 μm or more but less than 100 μm, and a fine powder having a particle size of less than 10 μm, A low thermal expansion block, characterized in that at least a portion of the fine powder is replaced with SiC powder, and the SiC powder is contained in an amount of 25 to 50 mass % when the whole is taken as 100 mass %.
Citation Information
Patent Citations
Refractory blend mainly consisting of fused quartz
JP1981078476A